Nitride materials and piezoelectric bodies made of the same, as well as MEMS devices, transistors, inverters, transducers, SAW devices, and ferroelectric memories using the piezoelectric bodies
Scandium-doped aluminum nitride materials with controlled composition and layered structures address the limitations of existing piezoelectric materials, achieving higher piezoelectricity and frequency compatibility for 5G applications in MEMS devices and transistors.
Patent Information
- Application Number
- JP2021027147
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-24
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2041-02-24
AI Technical Summary
Existing aluminum nitride-based piezoelectric materials face challenges in achieving high piezoelectricity, polarization direction control, and performance limitations in high-frequency filters, particularly for 5G applications, due to issues with germanium-doped aluminum nitride and scandium-doped aluminum nitride materials.
Development of scandium-doped aluminum nitride materials with specific compositional ratios of Sc, C, Si, Ge, or Sn, and an X/Y ratio of 0.2 to 5, which exhibit nitrogen polarity and improved piezoelectricity, along with optional intermediate layers and multi-layer structures to enhance crystallinity and frequency performance.
The proposed nitride materials and piezoelectric bodies achieve higher piezoelectricity, enabling high-frequency vibration, wider bandwidth, and lower loss, supporting advanced MEMS devices, transistors, and ferroelectric memories with enhanced performance.
Smart Images

Figure 0007572048000001 
Figure 0007572048000002 
Figure 0007572048000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a nitride material to which scandium is added and at least one of carbon, silicon, germanium, and tin, a piezoelectric body made thereof, and a MEMS device, a transistor, an inverter, a transducer, a SAW device, and a ferroelectric memory that use the piezoelectric body. [Background technology]
[0002] Aluminum nitride (AlN) is used in high-frequency filters for mobile phones and other devices because of its excellent elastic wave propagation velocity, quality factor (Q), and frequency temperature characteristics.
[0003] However, as the fifth generation mobile communication system (5G) has begun operation and 5G systems are being gradually introduced, there is a demand for high-frequency filters with wider bandwidth, lower loss, and improved Q values. For example, the frequency band allocated to 5G in each country is several GHz. Therefore, the thickness of the AlN piezoelectric thin film that constitutes the high-frequency filter has been thinned to enable the high-frequency filter to vibrate in this frequency band. However, this method has already reached its limit.
[0004] Meanwhile, a high-frequency filter has been proposed that can vibrate at twice the frequency compared to a nitride piezoelectric thin film of the same thickness by using a two-layer structure in which a nitride piezoelectric thin film with the polarity reversed is laminated on top of the nitride piezoelectric thin film (see Non-Patent Document 1).
[0005] As a nitride material with reversed polarity, an aluminum nitride piezoelectric thin film with a specific concentration of germanium (Ge) added has been proposed (see Patent Document 1).
[0006] Furthermore, as a piezoelectric material for a piezoelectric thin film used in a high frequency filter, for example, aluminum nitride doped with scandium (Sc) (see Patent Document 2) has been proposed. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2017-45749 A [Patent Document 2] JP 2009-10926 A [Non-patent literature]
[0008] [Non-Patent Document 1] Mizuno, t. et al. in 2017 19th International Conference on Solid-State Sensors, Actuators and Microsystems (TRANSDUCERS). 1891-1894 Summary of the Invention [Problem to be solved by the invention]
[0009] However, the above-mentioned germanium-doped aluminum nitride does not have a high piezoelectricity. As a result, even if the above-mentioned two-layered nitride piezoelectric body is formed using germanium-doped aluminum nitride, a wide passband width cannot be ensured, and high performance cannot be achieved in terms of insertion loss and guaranteed attenuation, making it difficult to use the material as a high-frequency filter for 5G.
[0010] On the other hand, there is a problem that only aluminum nitride with scandium added has been obtained that has aluminum polarity (Al polarity). For example, paragraph
[0006] of Patent Document 1 states that a piezoelectric thin film with nitrogen polarity (N polarity) having a polarization direction opposite to the thin film growth direction has not been obtained, and it has been said that there is no aluminum nitride with scandium added that has a polarity (nitrogen polarity) with a polarization direction opposite to that of aluminum polarity.
[0011] As a result, there was a problem in that it was not possible to fabricate a two-layered piezoelectric body in which scandium-doped aluminum nitride and a thin film of the same nitride piezoelectric body with reversed polarity were laminated.
[0012] In view of the above circumstances, an object of the present invention is to provide scandium-doped aluminum nitride having a nitrogen polarity in the polarization direction, a piezoelectric body made thereof, and a MEMS device, a transistor, an inverter, a transducer, a SAW device, and a ferroelectric memory using the piezoelectric body. [Means for solving the problem]
[0013] As a result of intensive research into the above-mentioned problems, the inventors of the present invention have discovered the following revolutionary nitride material, a piezoelectric body made of the nitride material, and a MEMS device using the piezoelectric body.
[0014] The first aspect of the present invention for solving the above problem is a compound represented by the chemical formula Sc X M Y Al 1-X-Y The nitride material is represented by N, where M is at least one element selected from the group consisting of C, Si, Ge, and Sn, X is greater than 0 and less than or equal to 0.4, Y is greater than 0 and less than or equal to 0.2, and X / Y is less than or equal to 5.
[0015] In the first aspect, it is possible to provide a nitride material having piezoelectricity with a nitrogen polarity direction.
[0016] A second aspect of the present invention resides in the nitride material according to the first aspect, characterized in that M is any one element of C, Si, Ge and Sn.
[0017] In the second aspect, a nitride material having a nitrogen polarity in the polarization direction and higher piezoelectricity can be provided.
[0018] A third aspect of the present invention resides in the nitride material according to the second aspect, characterized in that X is greater than 0 and less than or equal to 0.35, Y is greater than 0 and less than or equal to 0.2, and X / Y is less than or equal to 5.
[0019] In the third aspect, a nitride material having a nitrogen polarity and higher piezoelectricity is provided.
[0020] A fourth aspect of the present invention is a nitride material comprising the nitride material according to any one of the first to third aspects provided on a substrate, and at least one intermediate layer provided between the nitride material and the substrate.
[0021] In the fourth aspect, since the crystallinity (degree of crystallinity) of the nitride material is improved, it is possible to provide a nitride material whose polarization direction is nitrogen polarity and which has higher piezoelectricity.
[0022] A fifth aspect of the present invention resides in the nitride material according to the fourth aspect, characterized in that the intermediate layer comprises at least one of aluminium nitride, gallium nitride, indium nitride, titanium nitride, scandium nitride, ytterbium nitride, molybdenum, tungsten, hafnium, titanium, ruthenium, ruthenium oxide, chromium, chromium nitride, platinum, gold, silver, copper, aluminium, tantalum, iridium, palladium and nickel.
[0023] In the fifth aspect, since the crystallinity (degree of crystallinity) of the nitride material is further improved, it is possible to provide a nitride material whose polarization direction is nitrogen polarity and which has even higher piezoelectricity.
[0024] The sixth aspect of the present invention is a piezoelectric body made of a nitride material according to any one of the first to fifth aspects.
[0025] In such a sixth aspect, a piezoelectric body having a polarization direction with nitrogen polarity piezoelectricity can be provided.
[0026] The seventh aspect of the present invention is that on the surface of a scandium-containing nitride material represented by the chemical formula Sc Z Al 1-Z N (0 < Z ≤ 0.4), there is a piezoelectric body characterized in that the nitride material according to any one of the first to fifth aspects is provided.
[0027] In such a seventh aspect, a piezoelectric body that can vibrate at a high frequency and has high piezoelectricity can be provided.
[0028] The eighth aspect of the present invention is a piezoelectric body characterized in that at least two or more of the piezoelectric bodies according to the seventh aspect are laminated.
[0029] In such an eighth aspect, a piezoelectric body that can vibrate at a higher frequency and has higher piezoelectricity can be provided.
[0030] The ninth aspect of the present invention is a MEMS device using the piezoelectric body according to any one of the sixth to eighth aspects.
[0031] Here, the "MEMS device" is not particularly limited as long as it is a microelectromechanical system, and examples include physical sensors such as pressure sensors, acceleration sensors, and gyro sensors, actuators, microphones, fingerprint authentication sensors, vibration generators, and the like.
[0032] In such a ninth aspect, by using a piezoelectric body that can vibrate at a high frequency and has high piezoelectricity, a MEMS device can be provided that can contribute to further high-frequency compatibility, miniaturization, and power saving of portable devices.
[0033] A tenth aspect of the present invention resides in a transistor, an inverter, a transducer, a SAW device or a ferroelectric memory using the nitride material according to any one of the first to fifth aspects.
[0034] Here, a "transducer" refers to an element or device that converts a physical quantity carrying a signal into another type of physical quantity that is convenient for transmission, processing, storage, recording, display, operation, etc. Additionally, a "SAW device" refers to an electronic device that applies surface acoustic waves (SAW), such as an IDT-SAW device (Inter Digital Transducer-SAW device).
[0035] In the tenth aspect, a transistor can be provided that can be operated at a higher speed than conventional transistors and has low loss and high output. Also, a transistor can be provided that has a higher dielectric strength and low loss than conventional inverters. Furthermore, a ferroelectric memory can be provided that has a higher spontaneous polarization and higher memory performance than conventional ferroelectric memories. Also, a high-frequency wideband transducer can be provided that uses nitride materials with different polarities. Furthermore, by configuring the IDT using a piezoelectric body made of nitride materials with different polarities, a SAW device that vibrates at a higher frequency than a general IDT-SAW device can be provided. [Brief description of the drawings]
[0036] [Figure 1] FIG. 1 is a schematic cross-sectional view of a piezoelectric thin film according to the first embodiment. [Diagram 2] FIG. 2 is a table showing the composition and piezoelectric constant (d33) of each piezoelectric thin film when Si is used as an additive substance and the Sc concentration is fixed at approximately 10 mol %. [Diagram 3] FIG. 3 is a table showing the composition and piezoelectric constant (d33) of each piezoelectric thin film when Si is used as an additive substance and the Sc concentration is fixed at approximately 20 mol %. [Figure 4]FIG. 4 is a table showing the composition and piezoelectric constant (d33) of each piezoelectric thin film when Si is used as an additive substance and the Sc concentration is fixed at approximately 30 mol %. [Diagram 5] FIG. 5 is a graph showing the relationship between the Si concentration and d33 in each piezoelectric thin film when Si is used as an additive substance. [Figure 6] FIG. 6 is a graph showing the relationship between the Si concentration and the Sc concentration at which the piezoelectric polarity is inverted in each piezoelectric thin film when Si is used as an additive substance. [Figure 7] FIG. 7 is a table showing the composition and piezoelectric constant (d33) of each piezoelectric thin film when Ge is used as an additive substance and the Sc concentration is fixed at approximately 10 mol %. [Figure 8] FIG. 8 is a table showing the composition and piezoelectric constant (d33) of each piezoelectric thin film when Ge is used as an additive substance and the Sc concentration is fixed at approximately 20 mol %. [Figure 9] FIG. 9 is a table showing the composition and piezoelectric constant (d33) of each piezoelectric thin film when Ge is used as an additive substance and the Sc concentration is fixed at about 30 mol %. [Figure 10] FIG. 10 is a graph showing the relationship between the Ge concentration and d33 in each piezoelectric thin film when Ge is used as an additive substance. [Figure 11] FIG. 11 is a graph showing the relationship between the Ge concentration and the Sc concentration at which the piezoelectric polarity is inverted in each piezoelectric thin film when Ge is used as an additive substance. [Figure 12] FIG. 12 is a table showing the composition and piezoelectric constant (d33) of each piezoelectric thin film when Sn is used as an additive substance and the Sc concentration is fixed at about 10 mol %. [Figure 13] FIG. 13 is a table showing the composition and piezoelectric constant (d33) of each piezoelectric thin film when Sn is used as an additive substance and the Sc concentration is fixed at about 20 mol %. [Figure 14] FIG. 14 is a table showing the composition and piezoelectric constant (d33) of each piezoelectric thin film when Sn is used as an additive substance and the Sc concentration is fixed at about 30 mol %. [Figure 15] FIG. 15 is a graph showing the relationship between the Sn concentration and d33 in each piezoelectric thin film when Sn is used as an additive substance. [Figure 16] FIG. 16 is a graph showing the relationship between the Sn concentration and the Sc concentration at which the piezoelectric polarity is inverted in each piezoelectric thin film when Sn is used as an additive substance. [Figure 17] FIG. 17 is a schematic cross-sectional view of a piezoelectric thin film according to the second embodiment. [Figure 18] FIG. 18 is a schematic cross-sectional view of a piezoelectric thin film according to the third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0037] Hereinafter, an embodiment of a piezoelectric thin film according to the present invention will be described with reference to the accompanying drawings. Note that the present invention is not limited to the following embodiment, and for example, the shape is not limited, and it goes without saying that it does not have to be a thin film. (Embodiment 1)
[0038] 1 is a schematic cross-sectional view of a piezoelectric thin film according to this embodiment. As shown in this figure, a piezoelectric thin film 1 is formed on a substrate 10. There are no particular limitations on the thickness of the piezoelectric thin film 1, but a thickness in the range of 0.1 to 30 μm is preferable, and a thickness in the range of 0.1 to 2 μm is particularly preferable since this provides excellent adhesion.
[0039] The thickness and material of the substrate 10 are not particularly limited as long as the piezoelectric thin film 1 can be formed on the surface of the substrate 10. Examples of the substrate 10 include heat-resistant alloys such as silicon and Inconel, and resin films such as polyimide.
[0040] The piezoelectric thin film 1 is a material with the chemical formula Sc X M Y Al 1-X-YThe nitride material is represented by N, M represents at least one element selected from carbon (C), silicon (Si), germanium (Ge) and tin (Sn), X is greater than 0 and less than 0.4, Y is greater than 0 and less than 0.2, and X / Y is less than 5. When M is composed of multiple elements, it goes without saying that Y is the molar concentration of the total of these elements, and the concentration of each element is not particularly limited as long as it is within the above range.
[0041] Such a piezoelectric thin film 1 has a piezoelectricity with a nitrogen polarity (N polarity) in the polarization direction, unlike conventional aluminum nitride doped with scandium (Sc). Note that M may be only one of carbon, silicon, germanium, and tin. Such a nitride material has a nitrogen polarity in the polarization direction and has higher piezoelectricity.
[0042] In addition, when M is only Si, X is greater than 0 and 0.35 or less, Y is greater than 0 and 0.2 or less, and X / Y is preferably 5 or less, and Y is more preferably 0.03 or more. In addition, when M is only Ge, X is greater than 0 and 0.35 or less, Y is greater than 0 and 0.2 or less, and X / Y is preferably 5 or less, and X / Y is more preferably 4 or less, and Y is particularly preferably 0.05 or more. Furthermore, when M is only Sn, X is greater than 0 and 0.35 or less, Y is greater than 0 and 0.2 or less, and X / Y is preferably 5 or less, and Y is more preferably 0.05 or more. Such a piezoelectric thin film has a nitrogen polarity in the polarization direction and has a more stable piezoelectricity.
[0043] In the case of a nitride material having the above-described structure, the main crystals constituting the nitride material are wurtzite-type crystals having nitrogen polarity, and therefore the nitride material as a whole is considered to have nitrogen polarity.
[0044] Moreover, high frequency filters using these piezoelectric thin films 1 have lower loss and can operate over a wider band than conventional high frequency filters. As a result, portable devices can be made to handle higher frequencies, be more compact, and consume less power. The configuration of the high frequency filter is not particularly limited, and it can be manufactured with a known configuration, for example.
[0045] Next, a method for manufacturing the piezoelectric thin film 1 according to this embodiment will be described. The piezoelectric thin film 1 can be manufactured using a manufacturing method such as a sputtering method or a deposition method, like a general piezoelectric thin film. Specifically, for example, the piezoelectric thin film 1 can be manufactured by simultaneously sputtering a target made of scandium, a target made of an additive substance M (including a case where the additive substance M is made of a plurality of elements), and a target made of aluminum (Al) on a substrate 10 (for example, a silicon (Si) substrate) in a nitrogen gas (N2) atmosphere or a mixed atmosphere of nitrogen gas (N2) and argon gas (Ar) (gas pressure 1 Pa or less). Note that an alloy containing scandium, M, and aluminum in a predetermined ratio may be used as the target.
[0046] A layer containing the material constituting the substrate and the material constituting the piezoelectric thin film may be formed between the substrate and the piezoelectric thin film. Such a layer can be formed, for example, by forming the piezoelectric thin film on the substrate and then applying heat thereto. <When Si is used as an additive>
[0047] An example of the nitride material (piezoelectric thin film) according to this embodiment in which Si is used as the additive substance M will be described.
[0048] Using the following equipment and sputtering targets, a piezoelectric thin film (ScN) of 0.4 to 1.5 μm thick aluminum nitride doped with scandium and silicon (M=Si) was deposited on an n-type silicon substrate with a resistivity of 0.02 Ωcm. X S Y Al 1-X-Y N) was prepared. Multi-target simultaneous sputtering deposition equipment (manufactured by Eiko Engineering Co., Ltd.) Scandium sputtering target material (purity: 99.999%) Silicon sputtering target material (purity: 99.999%) Aluminum sputtering target material (purity: 99.999%) Gas: Mixture of nitrogen (purity: 99.99995% or more) and argon gas (purity: 99.9999% or more) (mixture ratio (nitrogen:argon) 30:70) Substrate heating temperature: 200℃
[0049] The deposition experiment was carried out with the air pressure in the sputtering chamber at 10 -5 The experiment was performed after lowering the pressure to a high vacuum of less than 1 Pa using a vacuum pump. In order to prevent the inclusion of impurities such as oxygen, the target surface was cleaned immediately after the target was attached and immediately before each film formation experiment.
[0050] The composition of each piezoelectric thin film obtained is shown in Fig. 2 to Fig. 4. Fig. 2 shows the composition and piezoelectric constant (d 33 ) and Fig. 3 shows the composition and piezoelectric constant (d 33 ) and Fig. 4 shows the composition and piezoelectric constant (d 33 ) is shown.
[0051] FIG. 5 shows the relationship between the Si concentration and the piezoelectric constant (d 33 ) indicates the relationship between
[0052] In these figures, d 33 If the value of is positive, it indicates that the polarization direction of the piezoelectric thin film is aluminum polarity, and d 33 If the value is negative, it indicates that the polarization direction of the piezoelectric thin film is nitrogen polarity.
[0053] Next, from a graph like Figure 5, d 33The Si concentration and Sc concentration when becomes 0 were obtained by interpolation, extrapolation, etc. The results are shown in Figure 6.
[0054] As can be seen from this figure, when the Sc concentration (X) is greater than 0 and less than 0.35 (35 mol%), the Si concentration (Y) is greater than 0 and less than 0.2 (20 mol%), and X / Y is less than 5, the polarization direction of the piezoelectric thin film becomes nitrogen polarity. The dotted line in this figure indicates X / Y=5. <When Ge is used as an additive material>
[0055] An example of the nitride material (piezoelectric thin film) according to this embodiment in which Ge is used as the additive substance M will be described.
[0056] The manufacturing method was the same as for the nitride material using Si as an additive substance, except that the following Ge sputtering target was used instead of the Si sputtering target material. Ge sputtering target material (purity: 99.999%)
[0057] The composition and d 33 7 to 9 are shown in Fig. 7. Fig. 7 shows the relationship between the composition and d of each piezoelectric thin film when the Sc concentration is fixed at about 10 mol%. 33 Fig. 8 shows the composition and d of each piezoelectric thin film when the Sc concentration is fixed at about 20 mol%. 33 Fig. 9 shows the composition and d of each piezoelectric thin film when the Sc concentration is fixed at about 30 mol%. 33 Shows.
[0058] FIG. 10 shows the relationship between the Ge concentration and d 33 Furthermore, in the same way as in Figure 6, from the graph in Figure 10, d 33 The Ge concentration and Sc concentration when becomes 0 were obtained by interpolation, extrapolation, etc. The results are shown in FIG.
[0059] As can be seen from this figure, when the Sc concentration (X) is greater than 0 and less than 0.35 (35 mol%), the Ge concentration (Y) is greater than 0 and less than 0.2 (20 mol%), and X / Y is less than 5, the polarization direction of the piezoelectric thin film becomes nitrogen polarity. The dotted line in this figure indicates X / Y=5. <When Sn is used as an additive>
[0060] An example of the nitride material (piezoelectric thin film) according to this embodiment in which Sn is used as the additive substance M will be described.
[0061] The manufacturing method was the same as for the nitride material using Si as an additive substance, except that the following Sn sputtering target was used instead of the Si sputtering target material. Sn sputtering target material (purity: 99.999%)
[0062] The composition and d 33 12 to 14. Fig. 12 shows the relationship between the composition and d of each piezoelectric thin film when the Sc concentration is fixed at about 10 mol%. 33 Fig. 13 shows the composition and d of each piezoelectric thin film when the Sc concentration is fixed at about 20 mol%. 33 Fig. 14 shows the composition and d of each piezoelectric thin film when the Sc concentration is fixed at about 30 mol%. 33 Shows.
[0063] FIG. 15 shows the relationship between the Sn concentration and d 33 Furthermore, in the same way as in Fig. 6, from the graph in Fig. 15, d 33 The Sn concentration and Sc concentration when becomes 0 were obtained by interpolation, extrapolation, etc. The results are shown in FIG.
[0064] As can be seen from this figure, when the concentration (X) of Sc is greater than 0 and 0.35 (35 mol%) or less, the concentration (Y) of Sn is greater than 0 and 0.2 (20 mol%) or less, and X / Y is 5 or less, it was found that the polarization direction of the piezoelectric thin film becomes nitrogen polar. The dotted line in this figure indicates X / Y = 5. <When using C as an additive substance>
[0065] Even when using C as an additive substance, it can be produced in the same manner as the nitride material using Si as an additive substance, except that a sputtering target of C is used instead of the sputtering target material of Si. (Embodiment 2)
[0066] In Embodiment 1, the piezoelectric body was constituted only by the nitride material according to the present invention, but the present invention is not limited thereto. For example, as shown in FIG. 17, on the nitride material (first layer) of Embodiment 1, a scandium-containing nitride material having aluminum polarity (Sc Z Al 1-Z N (0 <Z ≦ 0.4), second layer 20) is formed, and a piezoelectric thin film (piezoelectric body) 100 composed of these two layers may be constituted. Note that the second layer 20 may be formed below the first layer 1. Also, the thickness of the first layer 1 and the thickness of the second layer 20 may be the same or different.
[0067] Such a piezoelectric thin film having a two-layer structure can vibrate at a higher frequency compared to a piezoelectric thin film composed only of the piezoelectric thin film of Embodiment 1 described above or a piezoelectric thin film composed only of Sc Z Al 1-Z N (0 <Z ≦ 0.4), provided that the thicknesses are the same. Needless to say, in order to vibrate this piezoelectric thin film, for example, an upper electrode needs to be attached to the upper surface of this piezoelectric thin film and a lower electrode needs to be attached to the lower surface, and a voltage needs to be applied to these electrodes. (Embodiment 3)
[0068] In Embodiment 2, a scandium-containing nitride material (second layer 20) with a polarization direction of aluminum polarity is formed on a nitride material (first layer 1) with a polarization direction of nitrogen polarity to form a two-layer piezoelectric thin film, but the present invention is not limited thereto. For example, as shown in FIG. 18, on a thin film having the same configuration as that of Embodiment 2, a thin film of two layers (third layer 30 and fourth layer 40) having the same configuration may be further formed to form a four-layer piezoelectric thin film (piezoelectric body) 100A.
[0069] That is, the first layer 1 is a nitride material with a polarization direction of nitrogen polarity, the second layer 20 is a scandium-containing nitride material with a polarization direction of aluminum polarity, the third layer 30 is a nitride material with a polarization direction of nitrogen polarity, and the fourth layer 40 is a scandium-containing nitride material with a polarization direction of aluminum polarity, and a four-layer piezoelectric thin film 100A may be formed. Note that the stacking order is not particularly limited as long as the polarization directions of the adjacent nitride materials are different.
[0070] Such a four-layer piezoelectric thin film 100A can extend the bandwidth of the frequency that can be vibrated over a wider range compared to the piezoelectric thin film composed only of the piezoelectric thin film of Embodiment 1 described above, the piezoelectric thin film composed only of Sc Z Al 1-Z N (0 < Z ≦ 0.4), or the piezoelectric thin film of Embodiment 2, as long as the thicknesses are the same.
[0071] Note that a diffusion layer containing the substance constituting the first layer and the substance constituting the second layer may be formed between the first layer and the second layer. Such a diffusion layer can be formed, for example, by applying heat to them after forming the second layer on the first layer. (Embodiment 4)
[0072] In Embodiment 1, the piezoelectric thin film was directly formed on the substrate, but the present invention is not limited thereto. For example, an intermediate layer may be provided between the substrate and the piezoelectric thin film. The intermediate layer can be formed by sputtering or the like.
[0073] Here, the intermediate layer is not particularly limited in terms of material or thickness, etc., as long as a piezoelectric thin film can be formed on the intermediate layer. Examples of the intermediate layer include those made of aluminum nitride (AlN), gallium nitride (GaN), indium nitride (InN), titanium nitride (TiN), scandium nitride (ScN), ytterbium nitride (YbN), molybdenum (Mo), tungsten (W), hafnium (Hf), titanium (Ti), ruthenium (Ru), ruthenium oxide (RuO2), chromium (Cr), chromium nitride (CrN), platinum (Pt), gold (Au), silver (Ag), copper (Cu), aluminum (Al), tantalum (Ta), iridium (Ir), palladium (Pd), nickel (Ni), etc., and having a thickness of 50 to 200 nm.
[0074] By providing such an intermediate layer on the substrate, the crystallinity (degree of crystallization) of the piezoelectric thin film is improved, and thus the piezoelectric constant d 33 It is possible to manufacture a piezoelectric thin film having the above structure. (Other embodiments)
[0075] Although the piezoelectric body in the third embodiment has a four-layer structure, the present invention is not limited to this structure. The piezoelectric thin film may be formed by stacking a large number of layers made of a nitride material having a polarization direction different from that of the adjacent nitride material.
[0076] Such a piezoelectric thin film can vibrate at a higher frequency than the piezoelectric thin film of the third embodiment, and the bandwidth of the frequencies at which it can vibrate can be expanded to a wider range.
[0077] In addition, the piezoelectric thin film may be formed by laminating an odd number of layers (for example, a three-layer structure piezoelectric thin film) instead of an even number of layers made of a nitride material having a polarization direction different from that of the adjacent nitride material.
[0078] Moreover, the nitride material (piezoelectric body) according to the present invention described above can be used in MEMS. The MEMS using the nitride material according to the present invention can vibrate at high frequencies, and by using a piezoelectric body having high piezoelectricity, it is possible to provide a MEMS device that can contribute to making portable devices more compatible with high frequencies, smaller in size, and more energy-efficient. Note that, for example, a known MEMS configuration can be used for the MEMS.
[0079] Furthermore, in the first embodiment, the piezoelectric thin film using the nitride material according to the present invention has been described as an example, but the present invention is not limited thereto. For example, the nitride material according to the present invention can be applied to MEMS devices, transistors, inverters, transducers, SAW devices, or ferroelectric memories. A transistor using the nitride material according to the present invention can be operated at a higher speed than a conventional transistor, and has a low loss and high output. In addition, an inverter using the nitride material according to the present invention has a higher dielectric strength and a low loss than a conventional inverter. Furthermore, a ferroelectric memory using the nitride material according to the present invention has a higher spontaneous polarization and a higher memory performance than a conventional ferroelectric memory. Furthermore, a high-frequency wideband transducer using nitride materials with different polarities can be provided. In addition, by constructing an IDT using a piezoelectric made of nitride materials with different polarities, a SAW device that vibrates at a higher frequency than a general IDT-SAW device can be provided. Note that the configuration of such a transistor, inverter, transducer, SAW device, or ferroelectric memory can be, for example, a known one. [Explanation of symbols]
[0080] 1 Piezoelectric thin film (first layer) 10 Substrate 20 2nd layer 30 3rd layer 40 4th layer 100, 100A Piezoelectric thin film
Claims
1. Chemical formula Sc X M Y A 1-X-Y A nitride material represented by N, M is at least one element selected from the group consisting of Si, Ge, and Sn; X is greater than 0 and less than or equal to 0.4; Y is greater than 0 and less than or equal to 0.2; X / Y is 5 or less A nitride material characterized by:
2. 2. The nitride material according to claim 1, wherein M is any one of elements Si, Ge and Sn.
3. X is greater than 0 and less than or equal to 0.35; Y is greater than 0 and less than or equal to 0.2; X / Y is 5 or less The nitride material of claim 2 .
4. The nitride material according to any one of claims 1 to 3 is provided on a substrate, A nitride material, characterized in that at least one intermediate layer is provided between the nitride material and the substrate.
5. 5. The nitride material of claim 4, wherein the intermediate layer comprises at least one of aluminum nitride, gallium nitride, indium nitride, titanium nitride, scandium nitride, ytterbium nitride, molybdenum, tungsten, hafnium, titanium, ruthenium, ruthenium oxide, chromium, chromium nitride, platinum, gold, silver, copper, aluminum, tantalum, iridium, palladium, and nickel.
6. A piezoelectric body made of the nitride material according to any one of claims 1 to 5.
7. Chemical formula Sc Z A 1-Z 6. A piezoelectric body comprising the nitride material according to claim 1 provided on a surface of a scandium-containing nitride material represented by Z=N (0<Z≦0.4).
8. A piezoelectric body comprising at least two piezoelectric bodies according to claim 7 stacked together.
9. A MEMS device using the piezoelectric body according to any one of claims 6 to 8.
10. A transistor, an inverter, a transducer, a SAW device or a ferroelectric memory using the nitride material according to any one of claims 1 to 5.
Citation Information
Patent Citations
Piezoelectric thin film, piezoelectric material, fabrication method of piezoelectric thin film and piezoelectric material, and piezoelectric resonator, actuator element and physical sensor using piezoelectric thin film
JP2009010926A
Piezoelectric thin film resonator and manufacturing method of piezoelectric thin film
JP2013128267A
Piezoelectric element, manufacturing method of the same, and piezoelectric sensor
JP2013148562A
Piezoelectric thin film and method for producing the same
JP2014236051A
Aluminum nitride piezoelectric thin film, method of manufacturing the same, piezoelectric member and piezoelectric component
JP2017045749A