Resin composition, resin film, metal-clad laminate, and printed wiring board
A resin composition combining fibrous liquid crystal polymer and particulate metal oxide fillers addresses the limitations of existing materials by enhancing dielectric properties and dimensional stability in circuit boards, ensuring flexibility and toughness, suitable for high-frequency applications.
Patent Information
- Application Number
- JP2020213772
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-23
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-12-23
AI Technical Summary
Existing resin materials for circuit boards, such as liquid crystal polymers and fluororesins, face issues with low heat resistance, adhesion to metal foils, and significant thermal expansion, while adding fillers to improve dielectric properties compromises flexibility and toughness.
A resin composition comprising fibrous liquid crystal polymer fillers and particulate metal oxide fillers, with specific ratios and properties, is used to enhance dielectric properties and dimensional stability without impairing flexibility and toughness.
The resin composition achieves low dielectric loss tangent and thermal expansion, suitable for high-frequency signal transmission and maintaining dimensional stability, making it suitable for flexible printed circuits and printed wiring boards.
Smart Images

Figure 0007572234000001 
Figure 0007572234000002 
Figure 0007572234000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition useful, for example, as a circuit board material, and to a resin film, a metal-clad laminate, and a printed wiring board each using the same. [Background technology]
[0002] Flexible printed circuit boards (FPCs) are capable of three-dimensional, high-density mounting even in a limited space, and their applications have expanded to include wiring for moving parts of electronic devices, cables, connectors, and other components, and they are now installed in devices in many fields. As a result, the environments in which FPCs are used are becoming more diverse, and the performance required is becoming more advanced. For example, in information processing and communications, efforts are being made to increase the transmission frequency in order to transmit and process large volumes of information, and there is a strong demand for circuit boards to reduce transmission loss by improving the dielectric properties of the insulating resin layer.
[0003] As one approach to improving the dielectric properties of the insulating resin layer, it has been considered to use a resin with a low dielectric tangent as the base material of the insulating resin layer. For example, liquid crystal polymer is a resin characterized by a low dielectric constant and a low dielectric tangent, and by using this as the base material, the dielectric properties of the insulating resin layer can be greatly improved. However, a film using liquid crystal polymer as the base material has problems such as low heat resistance and low adhesion to metal foil, and does not satisfy all of the properties required as a circuit board material. In addition, fluororesin, polyolefin, polystyrene, polyester, etc. are also known as resin materials with excellent dielectric properties. However, these resins have a very large thermal expansion coefficient, and there is a problem that the dimensional stability of the circuit board is significantly impaired when used in the insulating resin layer.
[0004] As another approach, the incorporation of a filler capable of lowering the relative dielectric constant and dielectric loss tangent into the base material constituting the insulating resin layer has been considered. However, the addition of an inorganic filler to the insulating resin layer tends to cause problems such as a decrease in the flexibility and toughness of the resin film, impairing the physical properties required for circuit board materials.
[0005] Meanwhile, the method of adding a filler to an insulating resin layer to compound it and improve its functionality is widely known, not limited to the improvement of dielectric properties. For example, Patent Document 1 proposes that an insulating resin with excellent mechanical strength and low thermal expansion coefficient can be obtained by adding aramid fiber or glass fiber to an epoxy resin to be injection molded. Patent Document 1 also describes that the anisotropy of the thermal expansion coefficient specific to fibrous fillers can be eliminated by further adding granular fillers, but does not consider dielectric properties or flexibility. Also, Patent Document 2 proposes the preparation of a high-strength molding material with little anisotropy in the thermal expansion coefficient by adding fibrous fillers and spherical fillers to an epoxy resin. However, Patent Document 2 uses inorganic fibers, which makes it difficult to mold into a flexible resin film, and no consideration is given to improving the dielectric properties. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 11-273456 [Patent Document 2] Patent No. 6547277 Summary of the Invention [Problem to be solved by the invention]
[0007] Therefore, an object of the present invention is to provide a resin film which has both dielectric properties and dimensional stability without impairing physical properties such as flexibility and toughness. [Means for solving the problem]
[0008] As a result of intensive research to solve the above problems, it was discovered that by combining and blending a fibrous liquid crystal polymer filler and a particulate metal oxide filler into the base resin, it is possible to simultaneously improve the dielectric properties and dimensional stability without compromising the physical properties of the resin film, and thus the present invention was completed.
[0009] That is, the resin composition of the present invention comprises the following components (A) to (C); (A) a fibrous liquid crystal polymer filler; (B) Particulate metal oxide filler and (C) Thermoplastic resin and / or thermosetting resin Contains:
[0010] In the resin composition of the present invention, the total content of the fillers of the (A) component and the (B) component may be within a range of 10 to 90 volume % relative to the solid content in the resin composition, and the content of the (C) component may be within a range of 10 to 90 volume %.
[0011] The resin composition of the present invention is characterized in that the average length L of the major axis of the fibrous liquid crystal polymer filler of the component (A) and the average length R of the major axis of the fibrous liquid crystal polymer filler are Orthogonal The ratio L / D of the minor axis to the average diameter D of the minor axis may be 2.5 or more.
[0012] In the resin composition of the present invention, the component (A) fibrous liquid crystal polymer filler may have an average major axis length L in the range of 0.1 mm to 5 mm, and an average minor axis diameter D in the range of 5 μm to 50 μm.
[0013] In the resin composition of the present invention, the fibrous liquid crystal polymer filler of the component (A) may have a melting point of 290° C. or higher.
[0014] In the resin composition of the present invention, the content of the fibrous liquid crystal polymer filler of the component (A) may be within a range of 5 to 60% by volume relative to the content of the solid content in the resin composition.
[0015] In the resin composition of the present invention, the particulate metal oxide filler of the component (B) has a volume average particle diameter D 50 may be within a range of 1 μm to 100 μm.
[0016] In the resin composition of the present invention, the particulate metal oxide filler of component (B) may be silica particles in which the ratio of the total area of peaks derived from the cristobalite crystal phase and the quartz crystal phase to the total area of all peaks derived from SiO2 in the range of 2θ=10° to 90° in an X-ray diffraction analysis spectrum using CuKα rays is 20% by weight or more.
[0017] In the resin composition of the present invention, the content of the particulate metal oxide filler of the component (B) may be within a range of 20 to 80% by volume relative to the content of the solid content in the resin composition.
[0018] The resin composition of the present invention may have a volume ratio of the content of the fibrous liquid crystal polymer filler in the (A) component to the content of the particulate metal oxide filler in the (B) component [(A) component / (B) component] within a range of 0.1 to 10.
[0019] The resin composition of the present invention has a volume average particle diameter D 50 The ratio of the average minor axis diameter D of the fibrous liquid crystal polymer filler of the component (A) to the average minor axis diameter D [D / D 50 ] may be in the range of 1 to 50.
[0020] The resin composition of the present invention has a volume average particle diameter D 50 The ratio of the average length L of the major axis of the fibrous liquid crystal polymer filler of the component (A) to the average length L / D 50 ] may be in the range of 10 to 1000.
[0021] In the resin composition of the present invention, the component (C) may be at least one selected from thermoplastic polyimides, liquid crystal polymers, and fluororesins.
[0022] In the resin composition of the present invention, the component (C) may be a polyimide that uses a diamine component as a raw material, and the diamine component may contain 30 mol % or more of a dimer diamine composition mainly composed of a dimer diamine in which two terminal carboxylic acid groups of a dimer acid are substituted with primary aminomethyl groups or amino groups, relative to the total diamine components.
[0023] The resin film of the present invention is a resin film having a single or multiple resin layers, and at least one of the resin layers is a filler-containing resin layer formed using any of the above-mentioned resin compositions.
[0024] In the resin film of the present invention, the filler-containing resin layer may have a relative dielectric constant of 3 or less and a dielectric loss tangent of 0.003 or less at 10 GHz measured by a split post dielectric resonator (SPDR) after being conditioned for 24 hours under constant temperature and humidity conditions of 23°C and 50% RH.
[0025] In the resin film of the present invention, the filler-containing resin layer may have an absolute value of an average coefficient of thermal expansion (CTE) in the MD direction at 10°C to 20°C of 50 ppm / K or less, and an absolute value of an average coefficient of thermal expansion (CTE) in the TD direction of 100 ppm / K or less.
[0026] The metal-clad laminate of the present invention is a metal-clad laminate comprising an insulating resin layer consisting of a single layer or multiple layers, and a metal layer laminated on at least one side of the insulating resin layer, and at least one layer constituting the insulating resin layer is made of any of the resin films described above.
[0027] The printed wiring board of the present invention is a printed wiring board comprising an insulating resin layer consisting of a single layer or multiple layers, and a circuit wiring layer laminated on at least one surface of the insulating resin layer, and at least one layer constituting the insulating resin layer is made of any of the resin films described above. Effect of the Invention
[0028] The resin composition of the present invention contains components (A) to (C), and thus can form a resin film that has both excellent dielectric properties and dimensional stability without impairing physical properties such as flexibility and toughness. The resin film of the present invention has a low dielectric tangent, which effectively reduces the transmission loss of high-frequency signals (particularly high-frequency signals of 10 GHz or higher), and has excellent dimensional stability, so that it can be suitably used as a circuit board material for FPCs and the like in various electronic devices. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] Hereinafter, an embodiment of the present invention will be described. The resin composition according to one embodiment of the present invention comprises the following components (A) to (C); (A) a fibrous liquid crystal polymer filler; (B) Particulate metal oxide filler and (C) Thermoplastic resin and / or thermosetting resin Contains:
[0030] [Component (A): Fibrous liquid crystal polymer filler] The fibrous liquid crystal polymer filler of component (A) is a fibrous filler having shape anisotropy, and since the average coefficient of thermal expansion (hereinafter sometimes simply referred to as "CTE") in the major axis direction of the filler is low, it contributes to lowering the CTE of the resin film. In addition, since the fibrous liquid crystal polymer filler has flexibility, it is effective in maintaining the flexibility of the resin film. In the present invention, "fibrous" refers to the average length L of the major axis of the filler and the average length R of the filler relative to the major axis. Orthogonal This means that the ratio L / D of the average diameter D of the minor axis of the fibrous liquid crystal polymer filler to the average diameter D of the minor axis of the fibrous liquid crystal polymer filler is 2.5 or more. The L / D of the fibrous liquid crystal polymer filler is preferably 4.5 or more, more preferably 15.0 or more, and even more preferably 30.0 or more. If the L / D is less than 2.5, the fibrous liquid crystal polymer filler is likely to be arranged in a disorderly manner in the resin film, and the effect of improving the CTE is reduced. In addition, problems such as the fibrous liquid crystal polymer filler being likely to aggregate with each other occur.
[0031] The average length L of the long axis of the fibrous liquid crystal polymer filler can be appropriately selected depending on the method of compounding the fibrous liquid crystal polymer filler with the (C) component, but considering the dispersibility when dispersing the fibrous liquid crystal polymer filler in the (C) component, for example, it is preferably in the range of 0.1 mm to 5 mm, more preferably in the range of 0.2 mm to 1 mm. If the average length L of the long axis is less than 0.1 mm, when the resin composition is cast to form a resin film, the proportion of the fibrous liquid crystal polymer filler oriented in the thickness direction of the film increases, and the effect of lowering the CTE is achieved. On the other hand, if the average length L of the long axis exceeds 5 mm, the fibrous liquid crystal polymer filler becomes entangled with each other, making it difficult to cast the resin composition to form a resin film. If the average length L of the long axis is within the above range, a resin film with good appearance can be obtained without impairing the handleability and without deteriorating the surface smoothness when the resin film is formed.
[0032] The average minor axis diameter D of the fibrous liquid crystal polymer filler is, for example, preferably in the range of 5 μm to 50 μm, more preferably in the range of 10 μm to 30 μm. If the average minor axis diameter D is within the above range, the surface smoothness of the formed resin film is not deteriorated, and a resin film with good appearance can be obtained.
[0033] The liquid crystal polymer constituting the fibrous liquid crystal polymer filler is a resin that exhibits liquid crystallinity when melted, and may be a wholly aromatic liquid crystal polymer or a semi-aromatic liquid crystal polymer. The liquid crystal polymer is not particularly limited, but is preferably one having a polyester structure such as known thermotropic liquid crystal polyesters and polyesteramides derived from compounds classified into the following (1) to (4) and their derivatives. (1) Aromatic or aliphatic dihydroxy compounds (2) Aromatic or aliphatic dicarboxylic acids (3) Aromatic hydroxycarboxylic acids (4) Aromatic diamines, aromatic hydroxyamines, or aromatic aminocarboxylic acids
[0034] Representative examples of liquid crystal polymers obtained from these raw material compounds are copolymers having a combination of two or more structural units selected from the structural units shown in the following formulas (a) to (n), and preferably contain either the structural unit shown in formula (a) or the structural unit shown in formula (e), and more preferably contain the structural unit shown in formula (a) and the structural unit shown in formula (e). In addition, since the more aromatic rings in the liquid crystal polymer, the more the effect of improving dielectric properties and flame retardancy can be expected, it is preferable to use an aromatic dihydroxy compound as the above (1) and an aromatic dicarboxylic acid as the above (2).
[0035] [ka]
[0036] There are various methods for producing the fibrous liquid crystal polymer filler, such as melt spinning, melt extrusion, solution casting, and flow casting. In order to effectively orient the liquid crystal polymer molecules, it is preferable to carry out molding by a melting process and an extrusion process. In particular, the maximum shear rate u during extrusion calculated by the following formula is preferably 10 2 sec -1 More than 10, more preferably 4 sec -1 It is better to do this. u = 4Q / {π×(d / 2) 3} [However, Q is the amount of polymer passing through the extrusion outlet cross section per unit time (cm 3 / sec), d is the length (cm) of the shortest diameter of the cross section of the extrusion outlet, but in the case of a circular extrusion outlet such as a tubular nozzle or a fine hole, it is the diameter (cm). At such a maximum shear rate, the liquid crystal polymer molecules are sufficiently oriented, and it becomes easier to obtain controllability of the CTE when used as a fibrous liquid crystal polymer filler.
[0037] In particular, by discharging the resin through fine holes, it is possible to obtain liquid crystal polymer fibers in which the liquid crystal polymer molecules are strongly oriented in the longitudinal direction. Fine holes refer to holes with a diameter of 1 mm or less, more preferably 0.5 mm or less.
[0038] The obtained fibers may be combined into a composite material. Examples of the composite material include twisted yarn, woven fabric, knitted fabric, and nonwoven fabric. The composite material may be cut, crushed, or otherwise subdivided for use. In addition, the composite material may be combined into an aggregate material by combining a plurality of fillers exhibiting shape anisotropy. For example, the aggregate material may be prepared by heating or chemical action. The aggregate material may be cut, crushed, or otherwise subdivided for use. It is sufficient to grasp the shape anisotropy of the composite material or aggregate material in the state of the fiber, not in terms of their overall shape.
[0039] For example, the liquid crystal polymer fibers produced by the above method can be bundled and cut to a predetermined length to obtain a short fiber (also called chopped fiber or cut fiber) liquid crystal polymer filler. Furthermore, milled fiber filler can be produced by pulverizing the fibers. At this time, the fibers may be frozen, which allows the liquid crystal polymer filler to be efficiently divided into smaller pieces.
[0040] The cross-sectional shape of the fibrous liquid crystal polymer filler is not limited to a circle, and may be a star, flower, cross, or hollow shape. By changing the cross-sectional shape of the fibrous liquid crystal polymer filler, the surface area of the fibrous liquid crystal polymer filler can be adjusted to control the adhesion to the component (C) and the viscosity of the resin solution.
[0041] The fibrous liquid crystal polymer filler may be surface-modified to improve dispersibility and adhesion to the component (C). Examples of surface-modifying treatments include plasma treatment and coating treatment. The fibrous liquid crystal polymer filler may have a multilayer structure or a core-sheath structure. Examples of the multilayer structure include hollow liquid crystal polymer fillers and porous liquid crystal polymer fillers, and examples of the core-sheath structure include those in which the core is a liquid crystal polymer and the sheath is a resin that is highly adhesive to the component (C). Examples of the resin that is highly adhesive to the component (C) include thermoplastic resins such as polyimide, polyamide, perfluoroalkoxy fluororesin (PFA), and polyolefin.
[0042] Liquid crystal polymers have very good dielectric properties, and by blending them as fibrous fillers, it is possible to prevent the deterioration of the dielectric properties of the resin film. % The dielectric constant at 20 GHz under a RH environment is preferably within a range of 2 to 3.5, more preferably within a range of 2.7 to 3.2, and the dielectric loss tangent is preferably 0.002 or less, more preferably 0.0015 or less. By setting the dielectric properties of the fibrous liquid crystal polymer filler within the above ranges, deterioration of the dielectric properties of the resin film obtained by using the fibrous liquid crystal polymer filler can be prevented.
[0043] The dielectric properties of the fibrous liquid crystal polymer filler can be measured by using only the fibrous liquid crystal polymer filler as an aggregate or by melt molding. When it is necessary to separate the fibrous liquid crystal polymer filler from other components from a resin film, the separation method can be appropriately selected and used based on the difference in melting point or solubility between the fibrous liquid crystal polymer filler and other components. For example, the resin film can be dissolved in a solvent in which the fibrous liquid crystal polymer filler is insoluble and components other than the fibrous liquid crystal polymer filler are soluble, and unnecessary materials can be separated by filtration and centrifugation. The liquid crystal polymer can also be separated by crushing the resin film and treating it at a temperature at which only the fibrous liquid crystal polymer filler melts.
[0044] The melting point of the liquid crystal polymer constituting the fibrous liquid crystal polymer filler is sometimes called the liquid crystal transition temperature or liquid crystallization temperature, and is preferably 290° C. or higher, more preferably 300° C. or higher, and even more preferably 310° C. or higher. If the melting point is lower than 290° C., the polymer may melt during the manufacturing process of electronic devices, etc., causing changes in the properties.
[0045] [Component (B): Particulate metal oxide filler] The particulate metal oxide filler of component (B) is a filler that is mainly composed of metal oxide and has a particulate shape. "Particulate" refers to the shape of the major axis of the filler, with the length of the major axis being X and the length of the filler relative to that axis being X. Orthogonal When the length of the shortest axis among the axes is defined as Y, X / Y is less than 2.5, preferably 2 or less, more preferably 1.5 or less, and may be, for example, plate-like, spherical, polyhedral, etc. In addition, the term "plate-like" is used to mean, for example, flat, plate-like, flaky, scaly, etc., and refers to a particulate metal oxide filler whose thickness is sufficiently smaller than the major axis or minor axis of the flat portion, preferably 1 / 2 or less. By blending the particulate metal oxide filler, the CTE and dielectric loss tangent when the resin film is formed can be reduced. In addition, since the particulate metal oxide filler does not thermally decompose at normal combustion temperatures, the addition of the particulate metal oxide filler can improve flame retardancy.
[0046] It is most preferable to use a spherical particulate metal oxide filler. The spherical shape refers to a particle whose shape is close to a perfect sphere and whose average major axis and average minor axis ratio is 1 or close to 1. In addition, it is preferable that 90% by weight or more of the particulate metal oxide filler has a circularity of 0.7 or more, more preferably 0.9 or more. The circularity of the particulate metal oxide filler can be determined by an image analysis method, assuming a circle having the same projected area as the photographed particle, and calculating the ratio of the perimeter of the circle to the perimeter of the particle. If the circularity is less than 0.7, the surface area increases, which may adversely affect the dielectric properties, and further increases the viscosity when blended into a resin solution, making it difficult to handle. In addition, a value substantially corresponding to the circularity value is preferable for the three-dimensionally determined sphericity.
[0047] The particulate metal oxide filler preferably contains 50% by weight or more of metal oxide, more preferably 70% by weight or more. Examples of metal oxides constituting the particulate metal oxide filler include amorphous silica, crystalline silica, aluminum oxide, magnesium oxide, beryllium oxide, niobium oxide, and titanium oxide. Among these, crystalline silica particles having a cristobalite crystal phase or a quartz crystal phase, as described below, are most preferred from the viewpoint of achieving a low dielectric loss tangent when a resin film is formed.
[0048] Among particulate metal oxide fillers, silica particles having a cristobalite crystal phase have extremely superior dielectric properties compared to general silica particles (for example, silica particles containing 90% or more by weight of the cristobalite crystal phase have a dielectric tangent of approximately 0.0001 at 20 GHz by themselves), and can greatly contribute to lowering the dielectric tangent of resin films. Therefore, from the viewpoint of achieving a low dielectric tangent when a resin film is formed, silica particles in which the ratio of the total area of the peaks derived from the cristobalite crystal phase and the quartz crystal phase to the total area of all peaks derived from SiO2 in the range of 2θ=10° to 90° in the X-ray diffraction analysis spectrum using CuKα rays is 20% by weight or more, more preferably 40% by weight or more, and more preferably 80% by weight or more. By increasing the ratio of the cristobalite crystal phase and / or the quartz crystal phase in the entire silica particles, it is possible to further reduce the dielectric tangent of the resin film. If the ratio of the area of the peaks derived from the cristobalite crystal phase and the quartz crystal phase in the entire silica particles is less than 20% by weight, the effect of improving the dielectric properties becomes unclear. Note that when the target peak in the X-ray diffraction analysis spectrum is difficult to separate from the broad peak of the amorphous material or overlaps with the peak of another crystal phase, various known analysis methods, such as the internal standard method and the PONKCS method, can be used.
[0049] The particulate metal oxide filler has a volume average particle diameter D 50 In this regard, the volume average particle diameter D is preferably in the range of 1 μm to 100 μm, and more preferably in the range of 2 to 50 μm. 50 " is the value at which the cumulative value reaches 50% on the frequency distribution curve obtained by measuring the volume-based particle size distribution using the laser diffraction scattering method. 50 If the volume average particle diameter D is less than 1 μm, the specific surface area of the particulate metal oxide filler increases, and the adsorbed water and polar groups on the particle surface may affect the dielectric properties. 50 If the volume average particle diameter D of the particulate metal oxide filler exceeds 100 μm, it will appear as unevenness on the surface of the resin film, and the smoothness of the film surface may be deteriorated. 50If the diameter is within the range of 1 μm to 100 μm, it will be approximately the same as the average diameter D of the minor axis of the fibrous liquid crystal polymer filler of component (A), and therefore the orientation and alignment of the fibrous liquid crystal polymer filler can be effectively inhibited by the particulate metal oxide filler without affecting the smoothness of the film surface. In addition, an appropriate particle diameter reduces the amount of adsorbed water and surface functional groups, and effectively improves the dielectric properties. Therefore, when a resin film is formed from the resin composition, the surface smoothness is not deteriorated, and a resin film with a good appearance and a low dielectric loss tangent with a mitigated CTE anisotropy can be obtained.
[0050] In addition, the average minor axis diameter D of the fibrous liquid crystal polymer filler of component (A) and the volume average particle diameter D of the particulate metal oxide filler of component (B) 50 The relationship between the ratio [D / D 50 The ratio [D / D 50 If the value of ] is within the range of 1 to 50, the particulate metal oxide filler has a strong effect of preventing the orientation and alignment of the fibrous liquid crystal polymer filler, and the CTE difference between the MD and TD directions when the resin film is formed can be reduced.
[0051] Furthermore, the average length L of the long axis of the fibrous liquid crystal polymer filler of component (A) and the volume average particle diameter D of the particulate metal oxide filler of component (B) 50 The relationship between the ratio [L / D 50 The ratio [L / D] is preferably in the range of 10 to 1000, and more preferably in the range of 20 to 500. 50 If ] is within the range of 10 to 1000, the particulate metal oxide filler has a strong effect of preventing the orientation and alignment of the fibrous liquid crystal polymer filler, and the CTE difference between the MD and TD directions when the resin film is formed can be reduced.
[0052] The particulate metal oxide filler may be selected from commercially available products. For example, spherical cristobalite silica powder (manufactured by Nippon Steel Chemical & Material Co., Ltd., product name: CR10-20) and spherical amorphous silica powder (manufactured by Nippon Steel Chemical & Material Co., Ltd., product name: SC70-2) may be preferably used. Furthermore, particles of two or more different metal oxides may be used in combination as the particulate metal oxide filler.
[0053] [Component (C): Thermoplastic resin and / or thermosetting resin] The component (C) is a component that becomes a matrix resin when the resin film is formed. Examples of thermoplastic resins that can be used as the component (C) include thermoplastic polyimide, thermoplastic bismaleimide resin, thermoplastic epoxy resin, thermoplastic polyamide, liquid crystal polymer, fluororesin, polyolefin, polystyrene, polyether, polyether ketone, and polyester. Examples of thermosetting resins that can be used as the component (C) include non-thermoplastic polyimide, thermosetting epoxy resin, thermosetting polyphenylene ether, and phenolic resin. The above thermoplastic resins and thermosetting resins can be used in combination of two or more. In this specification, the term "thermoplastic resin" generally refers to a resin that can be softened by heating and solidified by cooling, and this can be repeated, and the glass transition temperature (Tg) can be clearly confirmed, and the term "non-thermoplastic resin" generally refers to a resin that does not soften even when heated.
[0054] As the component (C), a precursor of the polymer exemplified above can be used. The precursor refers to a substance in a stage before the substance is generated, and in this specification, the precursor of the resin also includes an oligomer. For example, in the case of polyimide, polyamic acid corresponds to the precursor. A case where it is preferable to use a precursor is when the precursor is soluble even in a polymer that is insoluble in a solvent. Specifically, most of the wholly aromatic polyimides are insoluble in general-purpose solvents, but the precursor polyamic acid is easily soluble in an amide-based solvent. In addition, even if a polyester is insoluble in a solvent in a high molecular weight form, its oligomer can be soluble in the solvent. In general, an oligomer refers to a polymer with a low degree of polymerization, and in this specification, it refers to a polymer with a repeat number in the range of 2 to 50 and a molecular weight of 5000 or less. When an oligomer has an active site, it is possible to react and increase the degree of polymerization by applying energy such as heating, increasing the solution concentration, or adding an activator or crosslinking agent.
[0055] Among the resins that can be used as the component (C), particularly preferred resins, namely polyimides (thermoplastic and non-thermoplastic), liquid crystal polymers and fluororesins, will be described below.
[0056] [Polyimide] Polyimide is a polymer having an imide group represented by the following general formula (1). When it further has an amide group or an ether bond, it may be called polyamideimide or polyetherimide, but in this specification, these are generally described as polyimide. Such polyimide can be produced by known methods such as a method of polymerizing a maleimide component with a diamine or triamine component, a method of crosslinking a bismaleimide with an aromatic cyanate ester, or a method of using substantially equimolar amounts of a diamine component and an acid dianhydride component and polymerizing them in an organic polar solvent. At this time, heating may be performed. In this case, in order to set the viscosity in the desired range, the molar ratio of the acid dianhydride component to the diamine component may be adjusted, and the range is preferably within a molar ratio of, for example, 0.98 to 1.03.
[0057] [ka]
[0058] In general formula (1), Ar1 represents a tetravalent group derived from an acid anhydride containing a tetracarboxylic dianhydride residue, R2 represents a divalent diamine residue derived from a diamine, and n is an integer of 1 or more.
[0059] As the acid dianhydride, for example, an aromatic tetracarboxylic acid dianhydride represented by O(OC)2-Ar1-(CO)2O is preferable, and examples thereof include those which give the following aromatic acid anhydride residue as Ar1.
[0060] [ka]
[0061] In addition, it is preferable to contain a total of 50 molar parts or more, and more preferably 80 molar parts or more, of tetracarboxylic acid anhydrides represented by the following general formula (2) and / or (3) per 100 molar parts of the total tetracarboxylic acid anhydride components.
[0062] [ka]
[0063] In general formula (2), X represents a single bond or a divalent group selected from the following formulas, and in general formula (3), the cyclic moiety represented by Y represents the formation of a cyclic saturated hydrocarbon group selected from a 4-membered ring, a 5-membered ring, a 6-membered ring, a 7-membered ring, or an 8-membered ring.
[0064] [ka]
[0065] In the above formula, Z represents -C6H4-, -(CH2)n-, or -CH2-CH(-OC(=O)-CH3)-CH2-, where n represents an integer of 1 to 20.
[0066] As the diamine, for example, a diamine represented by H2N-R2-NH2 is preferable, and examples thereof include diamines having the following diamine residue as R2.
[0067] [ka]
[0068] Among these diamines, preferred examples include diaminodiphenyl ether (DAPE), 2,2'-dimethyl-4,4'-diaminobiphenyl (m-TB), paraphenylenediamine (p-PDA), 1,3-bis(4-aminophenoxy)benzene (TPE-R), 1,3-bis(3-aminophenoxy)benzene (APB), 1,4-bis(4-aminophenoxy)benzene (TPE-Q), 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), 2,2-bis(trifluoromethyl)benzidine (TFMB), dimer diamines in which the two terminal carboxylic acid groups of a dimer acid (dimer fatty acid) are substituted with primary aminomethyl groups or amino groups, and dimer diamine compositions containing them as the main component.
[0069] In particular, since the dimer diamine composition can not only reduce the dielectric loss tangent but also increase the toughness of the resin film, it is preferable that the dimer diamine composition contains structural units derived from a diamine component that contains 30 mol % or more, preferably 40 mol % or more of the diamine composition relative to the total diamine components. Here, the dimer diamine composition is a refined product that contains the following component (a) as the main component and also contains controlled amounts of components (b) and (c). (a) Dimer diamine (b) Monoamine compounds obtained by substituting the terminal carboxylic acid group of a monobasic acid compound having 10 to 40 carbon atoms with a primary aminomethyl group or an amino group. (c) Amine compounds obtained by substituting the terminal carboxylic acid group of a polybasic acid compound having a hydrocarbon group having 41 to 80 carbon atoms with a primary aminomethyl group or an amino group (excluding the above dimer diamine).
[0070] The dimer diamine of the component (a) means a diamine in which two terminal carboxylic acid groups (-COOH) of a dimer acid are replaced with a primary aminomethyl group (-CH2-NH2) or an amino group (-NH2), and can be defined as a diamine compound obtained by replacing the terminal carboxylic acid groups of a dibasic acid compound having a carbon number of 18 to 54, preferably 22 to 44, with a primary aminomethyl group or an amino group. The dimer diamine composition is preferably one in which the dimer diamine content of the component (a) is increased to 96% by weight or more, preferably 97% by weight or more, more preferably 98% by weight or more by a purification method such as molecular distillation. By making the dimer diamine content of the component (a) 96% by weight or more, the spread of the molecular weight distribution of the polyimide can be suppressed. If technically possible, it is best that the entire dimer diamine composition (100% by weight) is composed of the dimer diamine of the component (a).
[0071] The dimer diamine composition is available as a commercially available product, and is preferably purified to reduce the amount of components other than the dimer diamine of the component (a), for example, it is preferable to make the component (a) 96% by weight or more. The purification method is not particularly limited, but known methods such as distillation and precipitation purification are suitable. Examples of commercially available dimer diamine compositions include PRIAMINE 1073 (trade name), PRIAMINE 1074 (trade name), and PRIAMINE 1075 (trade name) manufactured by Croda Japan.
[0072] The synthesized polyamic acid or polyimide is usually advantageously used as a reaction solvent solution, but if necessary, it can be concentrated, diluted, or replaced with another organic solvent to form a resin solution (varnish). The method for imidizing the polyamic acid is not particularly limited, and for example, a heat treatment in which the polyamic acid is heated in the above-mentioned solvent at a temperature within a range of 80 to 400°C for 1 to 24 hours is preferably used.
[0073] In addition, when the polyimide has a ketone group, the ketone group can be reacted with the amino group of an amino compound having at least two primary amino groups as functional groups (hereinafter, sometimes referred to as "amino compound for crosslinking") to form a C=N bond, thereby forming a crosslinked structure. The formation of the crosslinked structure can improve the heat resistance of the polyimide. A preferred example of a tetracarboxylic anhydride for forming a polyimide having a ketone group is 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), and a preferred example of a diamine compound is an aromatic diamine such as 4,4'-bis(3-aminophenoxy)benzophenone (BABP) or 1,3-bis[4-(3-aminophenoxy)benzoyl]benzene (BABB).
[0074] Examples of the amino compound for crosslinking include (I) dihydrazide compounds, (II) aromatic diamines, and (III) aliphatic amines. Among these, dihydrazide compounds are preferred because they can achieve both the storage stability of the varnish and a shortened curing time. Examples of the dihydrazide compounds include oxalic acid dihydrazide, malonic acid dihydrazide, succinic acid dihydrazide, glutaric acid dihydrazide, adipic acid dihydrazide, pimelic acid dihydrazide, suberic acid dihydrazide, azelaic acid dihydrazide, sebacic acid dihydrazide, dodecanedioic acid dihydrazide, maleic acid dihydrazide, fumaric acid dihydrazide, diglyceryl dihydrazide, ... Preferred are dihydrazide compounds such as cholic acid dihydrazide, tartaric acid dihydrazide, malic acid dihydrazide, phthalic acid dihydrazide, isophthalic acid dihydrazide, terephthalic acid dihydrazide, 2,6-naphthoedioic acid dihydrazide, 4,4-bisbenzene dihydrazide, 1,4-naphthoic acid dihydrazide, 2,6-pyridine diacid dihydrazide, itaconic acid dihydrazide, etc. The above dihydrazide compounds may be used alone or in combination of two or more.
[0075] When crosslinking a ketone group in a polyimide with an amino compound for crosslinking, the amino compound for crosslinking is added to a resin solution containing a polyimide to cause a condensation reaction between the ketone group in the polyimide and the primary amino group of the amino compound for crosslinking. This condensation reaction causes the resin solution to harden and become a hardened product. In this case, the amount of the amino compound for crosslinking can be 0.004 mol to 1.5 mol, preferably 0.005 mol to 1.2 mol, of the primary amino group per mol of the ketone group. If the amount of the amino compound for crosslinking is less than 0.004 mol of the primary amino group per mol of the ketone group, crosslinking by the amino compound for crosslinking is insufficient, and the heat resistance after curing tends to be difficult to be expressed. If the amount of the amino compound for crosslinking exceeds 1.5 mol, the unreacted amino compound for crosslinking acts as a thermoplasticizer, which tends to reduce the heat resistance of the adhesive layer.
[0076] The conditions of the condensation reaction for forming crosslinks are not particularly limited as long as the ketone group in the polyimide reacts with the primary amino group of the amino compound for forming crosslinks to form an imine bond (C=N bond). The temperature of the heat condensation is preferably within the range of, for example, 120 to 220°C, more preferably within the range of 140 to 200°C, for the purpose of releasing water produced by condensation out of the system, or for the purpose of simplifying the condensation step when the heat condensation reaction is carried out subsequently to the synthesis of the polyimide. The reaction time is preferably about 30 minutes to 24 hours. The end point of the reaction can be determined by measuring the infrared absorption spectrum using, for example, a Fourier transform infrared spectrophotometer (commercially available: FT / IR620 manufactured by JASCO Corporation) at 1670 cm. -1 The decrease or disappearance of the absorption peak due to the ketone group in the polyimide resin near 1635 cm -1 This can be confirmed by the appearance of an absorption peak derived from a nearby imine group.
[0077] In the above, examples of crosslinked polyimides in which a crosslinked structure is formed by the formation of imine bonds in order to impart heat resistance to polyimides have been described, but the present invention is not limited to this. As a method for curing polyimides, it is also possible to mix and cure them with compounds having unsaturated bonds, such as epoxy resins, epoxy resin curing agents, maleimides, activated ester resins, and resins having a styrene skeleton.
[0078] Polyimide films generally have excellent heat resistance, and there are also polyimide films with low CTE. However, due to the polarity of the imide structure, the dielectric loss tangent and water absorption are high, and in terms of resin composition design, there is a trade-off between low CTE and low dielectric loss tangent. In the present invention, by compounding with components (A) and (B), it is possible to achieve a low dielectric loss tangent while maintaining the above properties for a resin film with polyimide as the matrix resin.
[0079] [Fluororesin] The fluororesin that can be used as component (C) is not particularly limited as long as it is a polymer obtained by polymerizing a monomer containing fluorine, and examples thereof include polytetrafluoroethylene and polymers obtained by polymerizing ethylene in which one or more hydrogen groups have been replaced with fluorine groups as part of the raw material. For example, copolymers of tetrafluoroethylene and olefins are preferable, and examples thereof include tetrafluoroethylene-perfluoroalkyl vinyl ether copolymers, tetrafluoroethylene-ethylene copolymers, and tetrafluoroethylene-hexafluoropropylene copolymers. Fluororesins that have excellent heat resistance, dielectric properties, and low water absorption are preferable.
[0080] Fluororesin films generally have excellent heat resistance, dielectric properties, and low water absorption, and in particular, their dielectric properties are superior to those of films made of liquid crystal polymers alone. However, since fluororesin films generally have a CTE of more than 100 ppm / K, when used in combination with different materials, particularly metal materials, they are prone to warping, peeling, and displacement due to stress caused by temperature changes. In the present invention, by compounding the fluororesin with components (A) and (B), it is possible to achieve a low CTE for a resin film containing a fluororesin as a matrix resin while maintaining the above properties.
[0081] [Liquid crystal polymer] As the liquid crystal polymer usable as the (C) component, the liquid crystal polymer described for the liquid crystal polymer filler of the (A) component can be used. Although liquid crystal polymer films generally have excellent dielectric properties, they require a special manufacturing method such as an inflation method to reduce the difference in CTE between the MD and TD directions. In the present invention, by compounding the liquid crystal polymer with the (A) component and the (B) component, it is possible to reduce the difference in CTE between the MD and TD directions of a resin film having a liquid crystal polymer as a matrix resin in a simple manner without using a special manufacturing method, and it is also possible to further improve the dielectric properties and reduce the dielectric loss tangent.
[0082] [Optional ingredients] The resin composition of the present embodiment may contain optional components in addition to the components (A) to (C) within a range that does not impair the effects of the invention. Examples of the optional components include solvents such as organic solvents, organic fillers other than the component (A), inorganic fillers other than the component (B), catalysts, plasticizers, elastomers, coupling agents, curing agents, pigments, flame retardants, and heat dissipation agents. Examples of the organic solvents include N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N,N-diethylacetamide, N-methyl-2-pyrrolidone (NMP), 2-butanone, dimethylsulfoxide (DMSO), hexamethylphosphoramide, N-methylcaprolactam, dimethyl sulfate, cyclohexanone, dioxane, tetrahydrofuran, diglyme, triglyme, and cresol. Two or more of these solvents may be used in combination, and aromatic hydrocarbons such as xylene and toluene may also be used in combination. The content of the organic solvent is not particularly limited, but it is preferable to adjust the amount used so that the concentration of the (C) component is about 5 to 50% by weight. Examples of organic fillers other than the (A) component include elastomer particles and rubber particles. Examples of inorganic fillers other than the (B) component include nitrides such as boron nitride, aluminum nitride, and silicon nitride, fluorides such as aluminum fluoride, calcium fluoride, magnesium fluoride, and potassium silicofluoride, and metal salts such as metal phosphinates. These can be used alone or in combination of two or more.
[0083] [Mixing ratio] In the resin composition, the blending ratio of each component can be appropriately set according to the type of these, but it is preferable that the total content of the fillers of the (A) and (B) components is within the range of 10 to 90 volume % and the content of the (C) component is within the range of 10 to 90 volume % relative to the content of the solid content (meaning the remainder excluding the solvent) in the resin composition, and it is more preferable that the total content of the fillers of the (A) and (B) components is within the range of 20 to 70 volume % and the content of the (C) component is within the range of 30 to 90 volume %. If the total content of the fillers of the (A) and (B) components is less than 10 volume %, the effect of improving the dielectric properties and dimensional stability is difficult to be expressed, and if it exceeds 90 volume %, the filler is exposed on the film surface, and smoothness may be impaired.
[0084] The content of the fibrous liquid crystal polymer filler of the component (A) is preferably within the range of 5 to 60 volume % relative to the solid content in the resin composition, and more preferably within the range of 10 to 50 volume %. If the content of the component (A) is less than 5 volume %, the effect of improving the dielectric properties is difficult to manifest, and if it is too high, exceeding 60 volume %, the fibrous liquid crystal polymer filler becomes entangled with each other and tends to form lumps, which reduces the handleability and impairs the surface smoothness.
[0085] The content of the particulate metal oxide filler of component (B) is preferably within the range of 20 to 80 volume % relative to the solid content in the resin composition, and more preferably within the range of 30 to 70 volume %. If the content of component (B) is less than 20 volume %, the effect of improving the dielectric properties and the effect of inhibiting the orientation of the fibrous liquid crystal polymer filler of component (A) are not fully exhibited, and if it exceeds 80 volume %, the resin film becomes easily embrittled and the surface smoothness is impaired.
[0086] Furthermore, the ratio of the content of component (A) to the content of component (B) [component (A) / component (B)] is preferably within a range of 0.1 to 10 on a volume basis. When the ratio [component (A) / component (B)] is within a range of 0.1 to 10, the orientation and alignment of the fibrous liquid crystal polymer filler of component (A) can be effectively inhibited by the particulate metal oxide filler of component (B), and the CTE difference between the MD and TD directions when a resin film is formed can be reduced.
[0087] [Method of producing resin composition] The method for producing the resin composition of the present embodiment is not particularly limited since it can be appropriately selected according to the types and combinations of the (A) to (C) components, but as a preferred method, the particulate metal oxide filler of the (B) component is first added to the resin solution in which the (C) component is dissolved in an organic solvent, and after uniform mixing, the fibrous liquid crystal polymer filler of the (A) component is added and uniformly mixed. If the order of addition of the (B) and (A) components is reversed and the (A) component is added before the (B) component to the resin solution in which the (C) component is dissolved in an organic solvent, entanglement and aggregation of the fibrous liquid crystal polymer filler occurs, making it difficult to form a uniform resin composition.
[0088] [Resin film] The resin film of the present embodiment may be a resin film having a single or multiple resin layers, and at least one of the resin layers may be a filler-containing resin layer formed using the above resin composition. However, the filler-containing resin layer is preferably the main layer of the resin film. Here, the "main layer" means a layer having a thickness of more than 50% of the total thickness of the resin film. Therefore, it is more preferable that the entire resin film is composed of the filler-containing resin layer. In addition, the resin film may be, for example, a part of the insulating resin layer as an adhesive layer, or it can be used in the film state as, for example, a bonding sheet. Here, the "bonding sheet" is used for the purpose of bonding films to each other, a film to a metal, and a metal to a metal. The form of use is not limited to lamination and bonding in the film state, and it can also be applied as an adhesive layer in the form of a varnish and cured.
[0089] In addition, the filler-containing resin layer preferably has a relative dielectric constant of 3 or less at 10 GHz measured by a split post dielectric resonator (SPDR) after 24 hours of humidity control under constant temperature and humidity conditions of 23°C and 50% RH, and a dielectric loss tangent of 0.003 or less. In order to improve the transmission loss of the circuit board, it is particularly important to control the dielectric loss tangent of the insulating resin layer, and by setting the dielectric loss tangent to the above value or less, the effect of reducing the transmission loss is increased. Therefore, for example, when the resin film is used as an insulating resin layer of a high-frequency circuit board, the transmission loss can be efficiently reduced. If the dielectric loss tangent at 10 GHz exceeds 0.003, when the resin film is used as an insulating resin layer of the circuit board, inconveniences such as increased loss of electrical signals on the transmission path of high-frequency signals are likely to occur.
[0090] The filler-containing resin layer preferably has an absolute value of CTE in the MD direction of 50 ppm / K or less and a CTE in the TD direction of 100 ppm / K or less at 10° C. to 20° C. By having the CTE in the MD direction and the TD direction of the above values or less, dimensional changes in the film surface before and after heating can be suppressed, so that warping can be suppressed and misalignment during bonding of wires on a printed wiring board can be prevented.
[0091] Thickness The overall thickness of the resin film is preferably within the range of 15 to 250 μm, and more preferably within the range of 25 to 200 μm. If the thickness of the resin film is less than 15 μm, the surface smoothness of the film may deteriorate, and the metal foil may wrinkle during the transport process during the production of the metal-clad laminate, and the resin film may easily break. On the other hand, if the thickness of the resin film exceeds 250 μm, there is a tendency for it to be disadvantageous in that the foldability of the resin film decreases.
[0092] [Manufacturing method of resin film] The method for producing the resin film is not particularly limited, as it can be appropriately selected depending on the types and combination of the components (A) to (C). A preferred method is a casting method in which a resin composition containing the components (A) to (C) and an organic solvent is applied to any substrate, and then dried or otherwise molded into a film.
[0093] [Effect] In this embodiment, the resin composition contains the component (B) together with the components (A) and (C), thereby alleviating the anisotropy of the CTE when the resin film is formed. This is because when the resin composition is cast to form a film, the particulate metal oxide filler of the component (B) moderately prevents the fibrous liquid crystal polymer filler of the component (A) from aligning in the MD direction, thereby alleviating the anisotropy of the filler-containing resin layer. As a result, dimensional changes after heating can be suppressed, and by using the resin film of this embodiment, it is possible to manufacture a printed wiring board with finer and higher definition.
[0094] [Metal-clad laminate] The metal-clad laminate of the present embodiment is a metal-clad laminate including an insulating resin layer and a metal layer laminated on at least one surface of the insulating resin layer, at least one of the insulating resin layers being made of the above-mentioned resin film. The metal-clad laminate may be a single-sided metal-clad laminate having a metal layer only on one surface of the insulating resin layer, or a double-sided metal-clad laminate having metal layers on both surfaces of the insulating resin layer.
[0095] [Insulating resin layer] The insulating resin layer is composed of a single layer or multiple layers, and includes a layer made of the resin film. For example, the resin film may form a non-thermoplastic resin layer as a main layer of the insulating resin layer to ensure mechanical properties and thermal properties. The resin film may also form a thermoplastic resin layer as an adhesive layer that is responsible for the adhesive strength with a metal layer such as copper foil. The "main layer" means a layer that occupies more than 50% of the total thickness of the insulating resin layer. In addition, the metal-clad laminate of this embodiment does not exclude the use of an adhesive for bonding the resin film and the metal foil. However, when an adhesive layer is interposed in a double-sided metal-clad laminate having metal layers on both sides of the insulating resin layer, the thickness of the adhesive layer is preferably less than 30% of the thickness of the entire insulating resin layer, and more preferably less than 20%, so as not to impair the dielectric properties. Furthermore, when an adhesive layer is interposed in a single-sided metal-clad laminate having a metal layer on only one side of an insulating resin layer, the thickness of the adhesive layer is preferably less than 15% of the thickness of the entire insulating resin layer, and more preferably less than 10%, so as not to impair the dielectric properties. For example, the thickness of the insulating resin layer for use in a high-frequency circuit is preferably within a range of 35 to 200 μm, more preferably within a range of 50 to 150 μm, which allows for both the flexibility of the metal-clad laminate and the suppression of transmission loss of high-frequency signals when used in a circuit board.
[0096] Examples of methods for producing a metal-clad laminate having a resin film as an insulating resin layer include a method of applying a resin composition onto a metal foil and performing a vacuum and / or heat treatment, a method of heat-pressing a metal foil directly or via an arbitrary adhesive to a resin film, a method of forming a metal layer on a resin film by a technique such as metal vapor deposition, etc. Note that a double-sided metal-clad laminate can be obtained by, for example, forming a single-sided metal-clad laminate, and then forming the resin layers by facing each other and pressing them together by hot pressing, or by pressing a metal foil onto the resin layer of a single-sided metal-clad laminate.
[0097] [Metal layer] The material of the metal layer is not particularly limited, and examples thereof include copper, stainless steel, iron, nickel, beryllium, aluminum, zinc, indium, silver, gold, tin, zirconium, tantalum, titanium, lead, magnesium, manganese, and alloys thereof. Among these, copper, silver, or alloys thereof are particularly preferred. In particular, a copper-clad laminate (CCL) using copper for the metal layer is preferred from the viewpoints of electrical conductivity and cost. The metal layer may be made of metal foil, or may be a film on which metal has been vapor-deposited or a paste or the like has been printed. In addition, since the resin composition can be directly applied, either a metal foil or a metal plate can be used, and copper foil or copper plate is preferred.
[0098] The thickness of the metal layer is not particularly limited since it is appropriately set according to the purpose of use of the metal-clad laminate, but is preferably within the range of 5 μm to 3 mm, and more preferably within the range of 12 μm to 1 mm. If the thickness of the metal layer is less than 5 μm, there is a risk of problems such as wrinkles occurring during transportation in the manufacture of the metal-clad laminate. On the other hand, if the thickness of the metal layer exceeds 3 mm, it becomes hard and difficult to process. Regarding the thickness of the metal layer, a thick metal layer is generally suitable for applications such as in-vehicle circuit boards, and a thin metal layer is suitable for applications such as LED circuit boards.
[0099] [Printed wiring board] The printed wiring board is formed by forming a circuit using the metal layer of the metal-clad laminate as a conductor. That is, the printed wiring board includes an insulating resin layer composed of a single layer or multiple layers, and a circuit wiring layer laminated on at least one surface of the insulating resin layer, and at least one layer constituting the insulating resin layer is made of the above-mentioned resin film. In particular, it is preferable to use copper for the circuit wiring in terms of electrical conductivity and cost. Considering the transmission loss due to high-frequency signals, the roughness Rz of the copper side at the interface between the copper and the insulating resin layer is preferably 1.5 μm or less, more preferably 1 μm or less. Here, high frequency refers to a frequency of 10 GHz or more.
[0100] As described above, the resin film and metal-clad laminate of the present embodiment have excellent dielectric properties and dimensional stability due to the inclusion of components (A) to (C). Therefore, the resin film and metal-clad laminate can reduce loss in high-frequency signal transmission and maintain dimensional stability, and can be suitably used as circuit board materials such as FPCs in various electronic devices. EXAMPLES
[0101] The features of the present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to the examples. In the following examples, various measurements and evaluations are as follows, unless otherwise specified.
[0102] [Method for measuring amine value] Approximately 2 g of the dimer diamine composition is weighed into a 200-250 mL Erlenmeyer flask, and phenolphthalein is used as an indicator. A 0.1 mol / L ethanolic potassium hydroxide solution is dropped into the solution until the solution turns light pink, and the solution is dissolved in approximately 100 mL of neutralized butanol. 3-7 drops of phenolphthalein solution are added thereto, and titration is performed with 0.1 mol / L ethanolic potassium hydroxide solution while stirring until the sample solution turns light pink. Five drops of bromophenol blue solution are added thereto, and titration is performed with 0.2 mol / L hydrochloric acid / isopropanol solution while stirring until the sample solution turns yellow. The amine value is calculated according to the following formula (1). Amine value = {(V2 × C2) - (V1 × C1)} × MKOH / m (1) Here, the amine value is expressed in mg-KOH / g, MKOH is the molecular weight of potassium hydroxide, 56.1, V and C are the volume and concentration of the solution used, respectively, and the subscripts 1 and 2 represent a 0.1 mol / L ethanolic potassium hydroxide solution and a 0.2 mol / L hydrochloric acid / isopropanol solution, respectively, and m is the sample weight in grams.
[0103] [Calculation of GPC and chromatogram area percentage] For GPC, 20 mg of the dimer diamine composition was pretreated with 200 μL of acetic anhydride, 200 μL of pyridine, and 2 mL of THF (tetrahydrofuran), and 100 mg of the solution was diluted with 10 mL of THF (containing 1000 ppm of cyclohexanone) to prepare a sample. The prepared sample was measured using Tosoh Corporation's product name: HLC-8220GPC under the following conditions: column: TSK-gel G2000HXL, G1000HXL, flow rate: 1 mL / min, column (oven) temperature: 40° C., injection volume: 50 μL. Cyclohexanone was treated as a standard substance to correct the elution time.
[0104] In this case, the retention times were adjusted so that the peak top of the cyclohexanone main peak was at a retention time of 27 to 31 minutes, and the period from the peak start to the peak end of the cyclohexanone main peak was 2 minutes, and the peak top of the main peak excluding the cyclohexanone peak was at a retention time of 18 to 19 minutes, and the period from the peak start to the peak end of the main peak excluding the cyclohexanone peak was at a retention time of 2 minutes to 4 minutes 30 seconds, (a) Component represented by the main peak; (b) A component represented by a GPC peak detected at a time later than the minimum retention time of the main peak; (c) Components represented by GPC peaks detected at earlier retention times than the minimum value of the main peak on the earlier side; was detected.
[0105] [Measurement of weight average molecular weight (Mw) of polyimide] The weight average molecular weight was measured by gel permeation chromatography (HLC-8220GPC, manufactured by Tosoh Corporation). Polystyrene was used as a standard substance, and tetrahydrofuran was used as a developing solvent.
[0106] [Evaluation of dielectric properties] <Silica particles> A vector network analyzer (Keysight Technologies, product name: Vector Network Analyzer E8363C) and a dielectric constant measurement device manufactured by Kanto Electronics Application Development Co., Ltd. using a cavity resonator perturbation method were used, and the dielectric constant (ε1) and dielectric loss tangent (Tanδ1) of the silica particles at a frequency of 10 GHz were measured using a dielectric constant measurement mode of TM020. The silica particles were in powder form and were filled into a sample tube (inner diameter 1.68 mm, outer diameter 2.28 mm, height 8 cm) for measurement.
[0107] <Liquid crystal polymer short fiber> A dimethylacetamide dispersion of liquid crystal polymer short fibers adjusted to a solid content of 10% by weight was applied to the smooth surface of a copper foil and dried for 20 minutes at 120° C. Then, a new copper foil was laminated so that its smooth surface was in contact with the coated liquid crystal polymer short fiber layer, and vacuum pressure bonding was performed for 10 minutes at the melting point of the liquid crystal polymer +20° C. The copper foil of the obtained laminate was etched and removed to obtain a liquid crystal polymer film. The liquid crystalline polymer film obtained was left for 24 hours under conditions of temperature: 23°C and humidity: 50%, and then the relative dielectric constant and dielectric loss tangent at a frequency of 10 GHz were measured using a vector network analyzer (manufactured by Keysight Technologies, product name: Vector Network Analyzer E8363C) and a split post dielectric resonator (SPDR resonator).
[0108] <Resin film> Using a vector network analyzer (manufactured by Keysight Technologies, product name: Vector Network Analyzer E8363C) and an SPDR resonator, a resin film was pressed under conditions of a temperature of 160°C, a pressure of 3.5 MPa, and a time of 60 minutes, and then left for 24 hours under conditions of a temperature of 23°C and a humidity of 50%, after which the relative dielectric constant and dielectric loss tangent at a frequency of 10 GHz were measured.
[0109] [How to measure CTE] The resin film was cut into a size of 3 mm x 20 mm, and using a thermomechanical analyzer (manufactured by Bruker, product name: 4000SA) in tensile mode, the temperature was raised from 5°C to 300°C at a constant heating rate while applying a load of 5.0 g, and the average thermal expansion coefficient from 10°C to 20°C (average coefficient of linear thermal expansion: CTE) was measured in the MD and TD directions of the film.
[0110] [Melt point measurement] The melting point was measured by using a differential scanning calorimeter (DSC, manufactured by SII, product name: DSC-6200) in an inert gas atmosphere, raising the temperature from room temperature to 450° C. at a rate of 1.5° C. / min.
[0111] [Method of measuring the average length of the major axis and the average length of the minor axis] Ten fibrous fillers were randomly selected and observed independently using a stereomicroscope. The major axis length and minor axis length of each of the selected fillers were measured and averaged.
[0112] [Measurement of true specific gravity] The true density was measured by the pycnometer method (liquid phase displacement method) using a continuous automatic powder true density measuring device (manufactured by Seishin Enterprise Co., Ltd., product name: AUTO TRUE DENSERMAT‐7000).
[0113] [Circularity measurement] The average circularity of the silica particles was measured by dynamic flow particle image analysis using a wet flow type particle size / shape analyzer (manufactured by Sysmex Corporation, product name: FPIA-3000).
[0114] [Volume average particle size D 50 Measurement of Using a laser diffraction particle size distribution analyzer (Malvern Instruments, product name: Master Sizer 3000), the volume average particle diameter of silica particles was measured by a laser diffraction / scattering measurement method under conditions of water as the dispersion medium and a particle refractive index of 1.54.
[0115] [Measurement of cristobalite crystal phase] Using an X-ray diffraction measuring device (manufactured by Bruker, product name: D2PHASER), the total area of all peaks derived from SiO2 is calculated from all diffraction patterns (peak positions, peak widths, and peak intensities) derived from SiO2 in the range of diffraction angles (Cu, Kα)2θ = 10° to 90°. Next, the peak positions derived from the cristobalite crystal phase were identified, the total area of all peaks of the cristobalite crystal phase was calculated, and the ratio (wt%) to the total area of all peaks derived from SiO2 was obtained. The attribution of each peak was made by referring to the database of the International Centre for Diffraction Data (ICDD).
[0116] [Peel strength measurement] The peel strength was measured as follows: A copper-clad laminate was cut into a test piece with a width of 3 mm, and the peel strength between the resin layer and the copper foil was measured using a tensile tester (Strograph VE, manufactured by Toyo Seiki Seisakusho) when the test piece was pulled in the 90° direction at a speed of 50 mm / min.
[0117] [Evaluation of moisture-controlled solder heat resistance] The roughened surface of the copper foil was laminated to the resin side of the prepared copper-clad laminate, and the laminate was heated and pressed to prepare a double-sided copper-clad laminate. The obtained double-sided copper-clad laminate was cut into 30 mm squares, and the test pieces were left at 23°C and 50% relative humidity for 72 hours, and then immersed in a solder bath set at 288°C for 10 seconds, and the adhesion state was observed to check for defects such as foaming, swelling, and peeling. The case where no defects occurred was rated as good, and the case where defects occurred was rated as bad.
[0118] The abbreviations used in the examples and comparative examples represent the following compounds. PI: Polyimide PMDA: Pyromellitic dianhydride BTDA: 3,3',4,4'-benzophenonetetracarboxylic dianhydride BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride DDA: Product name: PRIAMINE 1075 manufactured by Croda Japan Co., Ltd., distilled and purified (component a: 99.2% by weight, component b: 0%, component c: 0.8%, amine value: 210 mg KOH / g) BAPP: 2,2-bis[4-(4-aminophenoxy)phenyl]propane BAFL: 9,9-bis(4-aminophenyl)fluorene m-TB: 2,2'-dimethyl-4,4'-diaminobiphenyl N-12: Dodecanedioic acid dihydrazide LCP: Liquid crystal polymer NMP: N-methyl-2-pyrrolidone DMAc: N,N-dimethylacetamide
[0119] LCP1: Liquid crystal polymer with polyester structure, melting point (Tm): 350°C, true specific gravity: 1.4, relative dielectric constant: 3.1, dielectric tangent: 0.0010 LCP2: Liquid crystal polymer with polyester structure, melting point (Tm); 330°C, true specific gravity; 1.4, relative dielectric constant; 3.4, dielectric tangent; 0.0020 LCP3: Liquid crystal polymer with polyester structure, melting point (Tm); 320°C, true specific gravity; 1.4, relative dielectric constant; 3.4, dielectric tangent; 0.0008
[0120] Shape 1: Short fiber, average major axis length: 0.5 mm, average minor axis length: 28 μm, manufacturing method: melt spinning, then cut Shape 2: Short fiber, average major axis length: 3 mm, average minor axis length: 28 μm, manufacturing method: melt spinning, then cut
[0121] Particle 1: Nippon Steel Chemical & Material Co., Ltd. Product name: CR10-20 (spherical cristobalite silica powder, circularity: 0.98, cristobalite crystal phase: 98% by weight, true specific gravity: 2.33, D 50 10.8μm, relative dielectric constant at 10GHz: 3.16, dielectric tangent at 10GHz: 0.0008) Particle 2: Admatec Co., Ltd. Product name: SE4050 (spherical amorphous silica powder, true sphere, true specific gravity: 2.21, D 50 1.5μm, relative dielectric constant at 10GHz: 2.92, dielectric tangent at 10GHz: 0.0052) Particle 3: Manufactured by Nippon Steel Chemical & Material Co., Ltd. Product name: SC70-2 (spherical amorphous silica powder, circularity: 0.98, true specific gravity: 2.21, D 50 11.7μm, relative dielectric constant at 10GHz: 3.08, dielectric tangent at 10GHz: 0.0015)
[0122] (Synthesis Example 1) In a 500mL separable flask, 33.84g of BTDA (0.1048 mol) as an acid anhydride, 56.16g of DDA (0.1051 mol) as a diamine, 126g of NMP, and 84g of xylene were charged and mixed well at 40°C for 1 hour to prepare a polyamic acid solution. The polyamic acid solution was heated to 190°C and heated and stirred for 8 hours to complete the imidization, and 64g of xylene was added to dilute the solution to prepare polyimide solution 1 (solid content: 30% by weight, weight average molecular weight: 58,500). This polyimide composition is called PI1.
[0123] (Synthesis Examples 2-3) Polyimide solutions 2 and 3 were prepared in the same manner as in Synthesis Example 1, except that the acid anhydride and diamine were changed as shown in Table 1. The resulting polyimide compositions are designated PI2 and PI3.
[0124] [Table 1]
[0125] (Synthesis Example 4) 19g of m-TB (90mmol) and 230g of DMAc were placed in a 300ml separable flask and stirred at room temperature under a nitrogen stream. After complete dissolution, 16g of PMDA (72mmol) and 5.3g of BPDA (18mmol) were added and stirred at room temperature for 18 hours to obtain polyamic acid solution 1. The viscosity of the obtained polyamic acid solution 1 was 22,400cps. The polyimide obtained by curing polyamic acid solution 1 was designated as PI4.
[0126] (Synthesis Example 5) 24 g of BAPP (60 mmol) and 230 g of DMAc were placed in a 300 ml separable flask and stirred at room temperature under a nitrogen stream. After complete dissolution, 6.5 g of PMDA (30 mmol) and 8.7 g of BPDA (30 mmol) were added and stirred at room temperature for 18 hours to obtain polyamic acid solution 2. The viscosity of the obtained polyamic acid solution 2 was 21,074 cps. The polyimide obtained by curing polyamic acid solution 2 was designated PI5.
[0127] [Example 1] 1.1 g of N-12 was mixed as a crosslinking agent into 100 g of the polyimide solution 1 obtained in Synthesis Example 1, 115 g of particles 1 was added, and after stirring, 11.7 g of LCP1 of shape 1 was added, and the mixture was diluted with xylene to a total solids concentration of 45% by weight, and stirred to prepare polyimide varnish 1. The volume-based content of LCP1 relative to the total solids in this polyimide varnish 1 was 10% and that of particles 1 was 60%.
[0128] The prepared polyimide varnish 1 was cast onto electrolytic copper foil (12 μm), dried at 80° C. for 20 minutes, and then treated at 160° C. for 1 hour to prepare a copper-clad laminate 1. The copper foil was further etched to prepare a resin film 1 (thickness: 145 μm). The various evaluation results of Resin Film 1 are as follows. Dielectric constant: 2.5, dissipation factor: 0.0009, CTE(TD): 58ppm / K, CTE(MD): 17ppm / K, peel strength: 1.3kN / m, humidity controlled solder heat resistance: good
[0129] [Example 2] To 100 g of the polyimide solution 1 obtained in Synthesis Example 1, 1.1 g of N-12 was mixed as a crosslinking agent, 19.2 g of particles 1 was added, and after stirring, 11.7 g of LCP1 of shape 1 was added, and the mixture was diluted with xylene to a total solids concentration of 45% by weight, and stirred to prepare polyimide varnish 2. The volumetric content of LCP1 and particles 1 relative to the total solids in this polyimide varnish 2 was 20% and 20%, respectively.
[0130] The prepared polyimide varnish 2 was cast onto electrolytic copper foil (12 μm), dried at 80° C. for 20 minutes, and then treated at 160° C. for 1 hour to prepare a copper-clad laminate 2. The copper foil was further etched to prepare a resin film 2 (thickness: 113 μm). The various evaluation results of the resin film 2 are as follows. Dielectric constant: 1.9, dissipation factor: 0.0015, CTE(TD): 91ppm / K, CTE(MD): 20ppm / K, humidity controlled solder heat resistance: good
[0131] [Example 3] To 100 g of the polyimide solution 1 obtained in Synthesis Example 1, 1.1 g of N-12 was mixed as a crosslinking agent, 57.5 g of particles 1 was added, and after stirring, 17.5 g of LCP1 of shape 1 was added, and the mixture was diluted with xylene to a total solids concentration of 45% by weight, and stirred to prepare polyimide varnish 3. The volumetric content of LCP1 relative to the total solids in this polyimide varnish 3 was 20% and that of particles 1 was 40%.
[0132] The prepared polyimide varnish 3 was cast onto electrolytic copper foil (12 μm), dried at 80° C. for 20 minutes, and then treated at 160° C. for 1 hour to prepare a copper-clad laminate 3. The copper foil was further etched to prepare a resin film 3 (thickness: 135 μm). The various evaluation results of the resin film 3 are as follows. Dielectric constant: 2.0, dissipation factor: 0.0013, CTE(TD): 70ppm / K, CTE(MD): 17ppm / K
[0133] [Example 4] To 100 g of the polyimide solution 1 obtained in Synthesis Example 1, 1.1 g of N-12 was mixed as a crosslinking agent, 28.8 g of particles 1 was added, and after stirring, 35 g of LCP1 of shape 1 was added, and the mixture was diluted with xylene to a total solids concentration of 45% by weight, and stirred to prepare polyimide varnish 4. The volumetric content of LCP1 relative to the total solids in this polyimide varnish 4 was 40% and that of particles 1 was 20%.
[0134] The prepared polyimide varnish 4 was cast onto electrolytic copper foil (12 μm), dried at 80° C. for 20 minutes, and then treated at 160° C. for 1 hour to prepare a copper-clad laminate 4. The copper foil was further etched to prepare a resin film 4 (thickness: 58 μm). The various evaluation results of Resin Film 1 are as follows. Dielectric constant: 1.8, dissipation factor: 0.0009, CTE(TD): 69ppm / K, CTE(MD): 30ppm / K, peel strength: 1.2kN / m, humidity controlled solder heat resistance: good
[0135] [Example 5] To 100 g of the polyimide solution 1 obtained in Synthesis Example 1, 1.1 g of N-12 was mixed as a crosslinking agent, 18.3 g of particles 2 was added, and after stirring, 11.7 g of LCP1 of shape 1 was added, and the mixture was diluted with xylene to a total solids concentration of 45% by weight, and stirred to prepare polyimide varnish 5. The volumetric content of LCP1 and particles 2 relative to the total solids in this polyimide varnish 5 was 20% and 20%, respectively.
[0136] The prepared polyimide varnish 5 was cast onto electrolytic copper foil (12 μm), dried at 80° C. for 20 minutes, and then treated at 160° C. for 1 hour to prepare a copper-clad laminate 5. The copper foil was further etched to prepare a resin film 5 (thickness: 158 μm). The various evaluation results of the resin film 5 are as follows. Dielectric constant: 2.0, dissipation factor: 0.0015, CTE(TD): 87ppm / K, CTE(MD): 15ppm / K, humidity controlled solder heat resistance: good
[0137] [Example 6] 1.1 g of N-12 was mixed as a crosslinking agent into 100 g of the polyimide solution 1 obtained in Synthesis Example 1, 55 g of particles 2 were added, and the mixture was stirred, after which 17.5 g of LCP1 of shape 1 was added, and the mixture was diluted with xylene to a total solids concentration of 45% by weight, and stirred to prepare polyimide varnish 6. The volumetric content of LCP1 relative to the total solids in this polyimide varnish 5 was 20% and that of particles 2 was 40%.
[0138] The prepared polyimide varnish 6 was cast onto electrolytic copper foil (12 μm), dried at 80° C. for 20 minutes, and then treated at 160° C. for 1 hour to prepare a copper-clad laminate 6. The copper foil was further etched to prepare a resin film 6 (thickness: 178 μm). The various evaluation results of the resin film 6 are as follows. Dielectric constant: 2.2, dissipation factor: 0.0016, CTE(TD): 57ppm / K, CTE(MD): 15ppm / K, peel strength: 1.1kN / m, humidity controlled solder heat resistance: good
[0139] [Example 7] To 100 g of the polyimide solution 1 obtained in Synthesis Example 1, 1.1 g of N-12 was mixed as a crosslinking agent, 33 g of particles 3 was added, and after stirring, 14 g of LCP1 of shape 1 was added, and the mixture was diluted with xylene to a total solids concentration of 45% by weight, and stirred to prepare polyimide varnish 7. The volume-based content of LCP1 relative to the total solids in this polyimide varnish 7 was 20% and that of particles 3 was 30%.
[0140] The prepared polyimide varnish 7 was cast onto electrolytic copper foil (12 μm), dried at 80° C. for 20 minutes, and then treated at 160° C. for 1 hour to prepare a copper-clad laminate 7. The copper foil was further etched to prepare a resin film 7 (thickness: 108 μm). The various evaluation results of the resin film 7 are as follows. Dielectric constant: 1.9, dissipation factor: 0.0016, CTE(TD): 80ppm / K, CTE(MD): 23ppm / K, humidity controlled solder heat resistance: good
[0141] [Example 8] To 100 g of the polyimide solution 2 obtained in Synthesis Example 2, 1.1 g of N-12 was mixed as a crosslinking agent, 19.2 g of particles 1 was added, and after stirring, 11.7 g of LCP1 of shape 1 was added, and the mixture was diluted with xylene to a total solids concentration of 45% by weight, and stirred to prepare polyimide varnish 8. The volume-based content of LCP1 and particles 1 relative to the total solids in this polyimide varnish 8 was 20% and 20%, respectively.
[0142] The prepared polyimide varnish 8 was cast onto electrolytic copper foil (12 μm), dried at 80° C. for 20 minutes, and then treated at 160° C. for 1 hour to prepare a copper-clad laminate 8. Furthermore, the copper foil was etched to prepare a resin film 8 (thickness: 102 μm). The various evaluation results of the resin film 8 are as follows. Dielectric constant: 1.9, dissipation factor: 0.0011, CTE(TD): 70ppm / K, CTE(MD): 22ppm / K
[0143] [Example 9] To 100 g of the polyimide solution 3 obtained in Synthesis Example 3, 1.1 g of N-12 was mixed as a crosslinking agent, 19.2 g of particles 1 was added, and after stirring, 11.7 g of LCP1 of shape 1 was added, and the mixture was diluted with xylene to a total solids concentration of 45% by weight, and stirred to prepare polyimide varnish 9. The volume-based content of LCP1 and particles 1 relative to the total solids in this polyimide varnish 9 was 20% and 20%, respectively.
[0144] The prepared polyimide varnish 9 was cast onto electrolytic copper foil (12 μm), dried at 80° C. for 20 minutes, and then treated at 160° C. for 1 hour to prepare a copper-clad laminate 9. The copper foil was further etched to prepare a resin film 9 (thickness: 97 μm). The various evaluation results of the resin film 9 are as follows. Dielectric constant: 2.0, dissipation factor: 0.0014, CTE(TD): 75ppm / K, CTE(MD): 20ppm / K, peel strength: 1.5kN / m, humidity controlled solder heat resistance: good
[0145] [Example 10] To 100 g of the polyamic acid solution 1 obtained in Synthesis Example 4, 7 g of particles 1 were added and stirred, and then 2.1 g of LCP1 of shape 2 was added, and the mixture was diluted with DMAc to a total solids concentration of 20% by weight, and stirred to prepare polyamic acid varnish 1. The volumetric content of LCP1 relative to the total solids in this polyamic acid varnish 1 was 10% and that of particles 1 was 20%.
[0146] The prepared polyamic acid varnish 1 was cast onto electrolytic copper foil (12 μm) and dried at 130° C. for 3 minutes. Then, it was subjected to stepwise heat treatment from 155° C. to 360° C. to imidize it, and a copper-clad laminate 10 was prepared. Furthermore, the copper foil was etched to prepare a resin film 10 (thickness: 40 μm). The results of various evaluations of the resin film 10 are as follows. Dielectric constant: 2.8, dissipation factor: 0.0028, CTE(TD): 10ppm / K, CTE(MD): 4ppm / K
[0147] [Example 11] To 100 g of the polyamic acid solution 1 obtained in Synthesis Example 4, 7 g of particles 1 were added and stirred, and then 2.1 g of LCP2 of shape 2 was added, and DMAc was added to dilute the total solids concentration to 20% by weight, followed by stirring to prepare polyamic acid varnish 2. The volumetric content of LCP2 relative to the total solids in this polyamic acid varnish 2 was 10% and that of particles 1 was 20%.
[0148] The prepared polyamic acid varnish 2 was cast onto electrolytic copper foil (12 μm) and dried at 130° C. for 3 minutes. Then, stepwise heat treatment was performed from 155° C. to 360° C. to imidize the copper foil, thereby preparing a copper-clad laminate 11. Furthermore, the copper foil was etched to prepare a resin film 11 (thickness: 48 μm). The various evaluation results of the resin film 11 are as follows. Dielectric constant: 2.9, dissipation factor: 0.0028, CTE(TD): 18ppm / K, CTE(MD): 17ppm / K, humidity controlled solder heat resistance: good
[0149] [Example 12] To 100 g of the polyamic acid solution 2 obtained in Synthesis Example 5, 6.9 g of particles 2 were added and stirred, and then 4.2 g of LCP1 of shape 2 was added, and DMAc was added to dilute the total solids concentration to 15 wt %, followed by stirring to prepare polyamic acid varnish 3. The volumetric content of LCP1 relative to the total solids in this polyamic acid varnish 3 was 20% and that of particles 2 was 20%.
[0150] The prepared polyamic acid varnish 3 was cast onto electrolytic copper foil (12 μm) and dried at 130° C. for 3 minutes. Then, stepwise heat treatment was performed from 155° C. to 360° C. to imidize the copper foil, thereby preparing a copper-clad laminate 12. Furthermore, the copper foil was etched to prepare a resin film 12 (thickness: 55 μm). The results of various evaluations of the resin film 12 are as follows. Dielectric constant: 3.0, dissipation factor: 0.0040, CTE(TD): 42ppm / K, CTE(MD): 30ppm / K, humidity controlled solder heat resistance: good
[0151] [Example 13] 24.6 g of Particle 2 was added to 50 g of DMAc liquid in which 50 wt% of LCP3 fine powder was dispersed, and after stirring, 10 g of LCP1 of shape 1 was added, diluted with DMAc to a total solids concentration of 50 wt%, and stirred to prepare LCP varnish 1. The volumetric content of LCP1 relative to the total solids in this LCP varnish 1 was 20% and Particle 2 was 30%.
[0152] The prepared LCP varnish 1 was cast onto electrolytic copper foil (12 μm) and dried at 130° C. for 3 minutes. Then, stepwise heat treatment was performed from 155° C. to 340° C. to prepare a copper-clad laminate 13. Furthermore, the copper foil was etched to prepare a resin film 13 (thickness: 45 μm). The various evaluation results of the resin film 13 are as follows. Dielectric constant: 2.8, dissipation factor: 0.0015, CTE(TD): 40ppm / K, CTE(MD): 38ppm / K
[0153] [Comparative Example 1] A copper-clad laminate 14 and a resin film 14 (thickness: 50 μm) were prepared in the same manner as in Example 1, except that the particles 1 and the LCP 1 of shape 1 were not added. The various evaluation results of the resin film 14 are as follows. Dielectric constant: 2.6, dissipation factor: 0.0019, CTE(TD): 150ppm / K, CTE(MD): 150ppm / K, peel strength: 1.3kN / m, humidity controlled solder heat resistance: good
[0154] [Comparative Example 2] A copper-clad laminate 15 and a resin film 15 (thickness: 49 μm) were prepared in the same manner as in Example 3, except that LCP 1 of Form 1 was not added. The various evaluation results of the resin film 15 are as follows. Dielectric constant: 2.8, dissipation factor: 0.0013, CTE(TD): 90ppm / K, CTE(MD): 90ppm / K, humidity controlled solder heat resistance: good
[0155] [Comparative Example 3] A copper-clad laminate 16 and a resin film 16 (thickness: 48 μm) were prepared in the same manner as in Example 6, except that LCP 1 of Form 1 was not added. The various evaluation results of the resin film 16 are as follows. Dielectric constant: 2.9, dissipation factor: 0.0020, CTE(TD): 72ppm / K, CTE(MD): 72ppm / K, humidity controlled solder heat resistance: good
[0156] [Comparative Example 4] A copper-clad laminate 17 and a resin film 17 (thickness: 53 μm) were prepared in the same manner as in Example 7, except that LCP 1 of Form 1 was not added. The various evaluation results of the resin film 17 are as follows. Dielectric constant: 2.8, dissipation factor: 0.0016, CTE(TD): 129ppm / K, CTE(MD): 129ppm / K, humidity controlled solder heat resistance: good
[0157] [Reference example 1] A copper-clad laminate 18 and a resin film 18 (thickness: 63 μm) were prepared in the same manner as in Example 2, except that the particles 1 were not added. The various evaluation results of the resin film 18 are as follows. Dielectric constant: 1.9, dissipation factor: 0.0017, CTE(TD): 120ppm / K, CTE(MD): 16ppm / K, humidity controlled solder heat resistance: good
[0158] Although the embodiment of the present invention has been described in detail above for the purpose of illustration, the present invention is not limited to the above embodiment, and various modifications are possible.
Claims
1. The following components (A) to (C): (A) a fibrous liquid crystal polymer filler, (B) Particulate metal oxide filler and (C) At least one selected from polyimide, its precursor, liquid crystal polymer, and fluororesin and a total content of the fillers of the (A) component and the (B) component is within a range of 10 to 90 volume % relative to the content of solids in the resin composition, and a content of the (C) component is within a range of 10 to 90 volume %.
2. 2. The resin composition according to claim 1, wherein the ratio L / D of the average length L of the major axis of the fibrous liquid crystal polymer filler of the component (A) to the average diameter D of the minor axis perpendicular to the major axis is 2.5 or more.
3. The resin composition according to claim 2, wherein the average length L of the major axis of the fibrous liquid crystal polymer filler of the component (A) is within the range of 0.1 mm to 5 mm, and the average diameter D of the minor axis is within the range of 5 μm to 50 μm.
4. 4. The resin composition according to claim 1, wherein the melting point of the fibrous liquid crystal polymer filler of the component (A) is 290° C. or higher.
5. The resin composition according to any one of claims 1 to 4, wherein the content of the fibrous liquid crystal polymer filler of the component (A) is within the range of 5 to 60 volume % relative to the solid content in the resin composition.
6. The particulate metal oxide filler of the component (B) has a volume average particle diameter D 50 The resin composition according to any one of claims 1 to 5, wherein the particle size is in the range of 1 µm to 100 µm.
7. The particulate metal oxide filler of the component (B) is SiO in the range of 2θ=10° to 90° in an X-ray diffraction analysis spectrum using CuKα radiation. 2 7. The resin composition according to claim 1, wherein the ratio of the total area of peaks derived from the cristobalite crystal phase and the quartz crystal phase to the total area of all peaks derived from the cristobalite crystal phase is 20% by weight or more.
8. The resin composition according to any one of claims 1 to 7, wherein the content of the particulate metal oxide filler of the component (B) is within the range of 20 to 80 volume % relative to the content of solids in the resin composition.
9. The resin composition according to any one of claims 1 to 8, wherein the ratio of the content of the fibrous liquid crystal polymer filler of the (A) component to the content of the particulate metal oxide filler of the (B) component [(A) component / (B) component] is within the range of 0.1 to 10 on a volume basis.
10. The volume average particle diameter D of the particulate metal oxide filler of the component (B) 50 The ratio of the average minor axis diameter D of the fibrous liquid crystal polymer filler of the component (A) to the average minor axis diameter D [D / D 50 10. The resin composition according to claim 1, wherein the value of [R] is in the range of 1 to 50.
11. The volume average particle diameter D of the particulate metal oxide filler of the component (B) 50 The ratio of the average length L of the major axis of the fibrous liquid crystal polymer filler of the component (A) to the average length L / D 50 11. The resin composition according to claim 1, wherein the molecular weight of the polymer is 10 to 1,000.
12. 2. The resin composition according to claim 1, wherein the polyimide of component (C) is a thermoplastic polyimide.
13. The resin composition described in claim 12, wherein the thermoplastic polyimide is a polyimide that uses a diamine component as a raw material, and the diamine component is a polyimide that contains 30 mol% or more of a dimer diamine composition mainly composed of a dimer diamine in which the two terminal carboxylic acid groups of a dimer acid are substituted with primary aminomethyl groups or amino groups, relative to the total diamine component.
14. A resin film having a single or multiple resin layers, A resin film, wherein at least one of the resin layers is a filler-containing resin layer formed using the resin composition according to any one of claims 1 to 13.
15. The resin film according to claim 14, wherein the filler-containing resin layer has a relative dielectric constant of 3 or less and a dielectric loss tangent of 0.003 or less at 10 GHz, as measured by a split post dielectric resonator (SPDR) after being conditioned for 24 hours under constant temperature and humidity conditions of 23°C and 50% RH.
16. The filler-containing resin layer has an absolute value of an average coefficient of thermal expansion (CTE) in an MD direction at 10°C to 20°C of 50 ppm / K or less, and an absolute value of an average coefficient of thermal expansion (CTE) in a TD direction of 100 ppm / K or less.
17. A metal-clad laminate comprising an insulating resin layer composed of a single layer or multiple layers, and a metal layer laminated on at least one surface of the insulating resin layer, A metal-clad laminate, wherein at least one layer constituting the insulating resin layer is made of the resin film according to any one of claims 14 to 16.
18. A printed wiring board comprising an insulating resin layer composed of a single layer or multiple layers, and a circuit wiring layer laminated on at least one surface of the insulating resin layer, A printed wiring board, wherein at least one layer constituting the insulating resin layer is made of the resin film according to any one of claims 14 to 16.
Citation Information
Patent Citations
Fishing line
JP1994046726A
Epoxy resin composition for apparatus insulated with sulfur hexafluoride gas
JP1996193164A
Sliding resin molding
JP1997227695A
Electrical insulating resin composition and printed wiring board
JP1999273456A
Composite material and production method therefor
JP2005179631A