High-strength cold-rolled steel sheet, hot-dip galvanized steel sheet, and alloyed hot-dip galvanized steel sheet, and methods for producing the same
A high-strength cold-rolled steel sheet with optimized chemical composition and manufacturing process addresses the workability issues of existing steel sheets, achieving enhanced stretch flangeability and bendability for improved impact resistance.
Patent Information
- Application Number
- JP2021120210
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-10-06
- Filing Date
- 2021-07-21
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2041-07-21
AI Technical Summary
High-strength steel sheets used in automobile and transportation machinery parts face challenges with reduced workability, such as ductility and stretch flangeability, leading to cracking during impact deformation, especially in complex shapes and severe bending deformations.
A high-strength cold-rolled steel sheet with a specific chemical composition and microstructure, including C, Si, and Mn, and a controlled manufacturing process involving hot rolling, cold rolling, and annealing, results in a structure with a high area ratio of bainite, tempered martensite, and MA phases, optimized for stretch flangeability and bendability.
The solution provides steel sheets with tensile strength of 900 MPa or more, excellent stretch flangeability, and bendability, effectively preventing cracking during impact deformation.
Smart Images

Figure 0007572332000004 
Figure 0007572332000005 
Figure 0007572332000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a high-strength cold-rolled steel sheet, a hot-dip galvanized steel sheet and a hot-dip galvannealed steel sheet using the high-strength cold-rolled steel sheet, and methods for producing these steel sheets. [Background technology]
[0002] In recent years, as the strength of automobile parts and transport machinery parts and the like has increased, the strength of the steel sheets used for these parts has also increased. In such high-strength steel sheets, the workability such as ductility and stretch flangeability has decreased due to the increased strength. Therefore, it has become difficult to press-form parts having complex shapes using high-strength steel sheets such as automobile steel sheets and transport machinery steel sheets.
[0003] Furthermore, the high-strength steel sheets have reduced local ductility such as bendability and stretch flangeability, etc. Therefore, when the high-strength steel sheets are used in body structural members intended to absorb impact energy during a collision, there is a problem that the high-strength steel sheets may crack during deformation due to the collision.
[0004] In order to address these problems, there is a demand for the development of high-strength steel plates that are excellent in workability and resistance to cracking during collision deformation (hereinafter referred to as "collision properties").
[0005] When automotive steel sheets are used in body structural members for the purpose of absorbing impact energy, the steel sheets are required to be resistant to cracking when subjected to large loads and high-speed deformation due to collision. Such members are subjected to severe bending deformation due to buckling during deformation. Therefore, high-strength steel sheets with excellent local ductility, such as bendability and stretch flangeability, are considered to be suitable for use in such members.
[0006] Examples of documents disclosing techniques relating to the above-mentioned properties of steel sheets include Patent Document 1 and Patent Document 2.
[0007] Patent Document 1 discloses a high-strength plated steel sheet having excellent workability including elongation, bendability, and hole expandability (stretch flangeability), in which, when the metallographic structure is observed with a scanning electron microscope, the low-temperature transformation formed phase accounts for 70 area % or more of the entire metallographic structure, and pearlite, quenched martensite, and an MA mixed phase which is a composite phase of quenched martensite and retained austenite account for 15 area % or less of the entire metallographic structure.
[0008] Patent Document 2 describes a high-strength cold-rolled steel sheet that is excellent in both workability, as evaluated by ductility and stretch flangeability, and crashworthiness, and has an equivalent circle diameter of 2.0 μm or less in an MA structure in which quenched martensite and retained austenite are combined, and a volume fraction of retained austenite V γ Area ratio of MA structure to V MA Ratio of V MA / V γ However, 0.50≦V MA / V γ A high strength cold rolled steel sheet satisfying the condition of ≦1.50 is disclosed. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Patent No. 6085348 [Patent Document 2] Patent No. 6554396 Summary of the Invention [Problem to be solved by the invention]
[0010] However, the inventors of the present application have conducted studies and found that the steel sheets disclosed in Patent Documents 1 and 2 have room for further improvement in stretch flangeability and bendability.
[0011] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a high-strength cold-rolled steel sheet excellent in stretch flangeability and bendability, and a hot-dip galvanized steel sheet and an alloyed hot-dip galvanized steel sheet having a hot-dip galvanized layer or an alloyed hot-dip galvanized layer on the surface of the high-strength cold-rolled steel sheet, and to provide a method for manufacturing the high-strength cold-rolled steel sheet, the hot-dip galvanized steel sheet, and the alloyed hot-dip galvanized steel sheet. [Means for solving the problem]
[0012] As a result of extensive investigations, the present inventors have found that the above object can be achieved by the following invention.
[0013] A high-strength cold-rolled steel sheet according to one aspect of the present invention contains, by mass%, C: 0.070 to 0.140%, Si: 0.80 to 1.80%, and Mn: 1.80 to 2.80%, with the balance being iron and unavoidable impurities; in terms of area fraction in a structure observed with a scanning electron microscope, a total of hard phases consisting of bainite, tempered martensite, and at least one of MA and cementite in which quenched martensite and retained austenite are combined is 85% or more; the hard phases each having a short diameter of 0.4 μm or less and a long diameter of 1.2 μm or more account for 0.5% or more; the hard phases each having a short diameter of 1.2 μm or more account for 5.0% or less; and a structure other than the bainite, the tempered martensite, and the hard phases accounts for 15% or less; and the retained austenite is 3.0% or more and 7.0% or less in terms of volume fraction measured by X-ray diffraction.
[0014] A hot-dip galvanized steel sheet and an alloyed hot-dip galvanized steel sheet according to another aspect of the present invention have the above-mentioned high-strength cold-rolled steel sheet and a hot-dip galvanized layer or an alloyed hot-dip galvanized layer provided on the surface of the high-strength cold-rolled steel sheet.
[0015] A method for producing a high-strength cold-rolled steel sheet according to another aspect of the present invention includes a rolling step of successively performing hot rolling and cold rolling on a steel slab satisfying the above-mentioned chemical composition, a heating step of heating the steel sheet obtained by cold rolling the steel slab to a temperature range of (Ac3 point + 200°C) or lower at a temperature rise rate of 1.5°C / sec to 30°C / sec at 700°C or higher, and a soaking step of holding the steel sheet after the heating step for 10 seconds to 100 seconds. the steel plate that has undergone the soaking step having a first cooling temperature of 100°C or more and 410°C or less at a cooling rate of 10°C / sec or more and 50°C / sec or less; a holding step of holding the steel plate that has been cooled to the first cooling temperature at a holding temperature of 100°C or more and 410°C or less for 10 seconds or more and 80 seconds or less; and a second cooling step of cooling the steel plate that has undergone the holding step to approximately room temperature at a cooling rate of 15°C / sec or more, in this order.
[0016] According to another aspect of the present invention, there is provided a method for producing a hot-dip galvanized steel sheet and a method for producing an alloyed hot-dip galvanized steel sheet, in which, in the above-described method for producing a high-strength cold-rolled steel sheet, the steel sheet is further subjected to a galvanizing treatment before the second cooling step, or is subjected to an alloying treatment following the galvanizing treatment. Effect of the Invention
[0017] Effects of the Invention According to the present invention, it is possible to provide a high-strength cold-rolled steel sheet having excellent stretch flangeability and bendability, a hot-dip galvanized steel sheet having a hot-dip galvanized layer on the surface of the high-strength cold-rolled steel sheet, and an alloyed hot-dip galvanized steel sheet having a hot-dip galvanized layer on the surface of the high-strength cold-rolled steel sheet.
[0018] Moreover, according to the present invention, it is possible to provide methods for producing these high-strength cold-rolled steel sheets, hot-dip galvanized steel sheets, and galvannealed steel sheets. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a schematic diagram for explaining the size and shape of the hard phase defined in this embodiment. [Diagram 2]FIG. 2 is a schematic diagram of the heat pattern of the annealing process, where (A) is a basic pattern, (B) is a pattern having a reheating process, (C) is a pattern having a plating (alloying) process, and (D) is a pattern having both a reheating process and a plating (alloying) process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The present inventors have conducted extensive research focusing on the chemical composition, structural structure, volume fraction of retained austenite, and the size and shape of MA and cementite in order to provide a high-strength cold-rolled steel sheet having a tensile strength of 900 MPa or more and excellent stretch flangeability and bendability. Specifically, they considered that the structural structure of the steel sheet and the size and shape of MA and cementite dispersed in the structure affect the stretch flangeability and bendability, and investigated these structures in detail.
[0021] As a result, the inventors have found that, if the chemical composition, structural structure, volume fraction of retained austenite, and area fraction of MA and cementite of specified sizes and shapes in the structure of a steel sheet satisfy the specified requirements described below, good stretch flangeability and bendability can be achieved in a high-strength cold-rolled steel sheet, and have completed the present invention.
[0022] In the following description, "high strength" for steel sheet, hot-dip galvanized steel sheet, and alloyed hot-dip galvanized steel sheet means "tensile strength of 900 MPa or more." Furthermore, "MA" as defined in the present invention is an abbreviation for "Martensite-Austenite Constituent," and refers to a structure in which quenched martensite and retained austenite are combined.
[0023] Hereinafter, a high-strength cold-rolled steel sheet and a manufacturing method thereof according to one embodiment of the present invention will be described.
[0024] (Metal structure of high-strength cold-rolled steel sheet) In the high-strength cold-rolled steel sheet according to the present embodiment, the total area ratio of hard phases consisting of bainite, tempered martensite, and at least one of MA and cementite, which are a combination of quenched martensite and retained austenite, is 85% or more, the hard phase having a short diameter of 0.4 μm or less and a long diameter of 1.2 μm or more is 0.5% or more, the hard phase having a short diameter of 1.2 μm or more is 5.0% or less, and the structure other than bainite, tempered martensite, and hard phase is 15% or less, and the volume ratio of retained austenite measured by X-ray diffraction is 3.0% or more and 7.0% or less. This makes it possible to obtain a high-strength cold-rolled steel sheet with excellent stretch flangeability and bendability.
[0025] (Hard phase) The hard phase defined in this embodiment is composed of at least one of MA and cementite. MA is a combination of quenched martensite and retained austenite. In the high-strength cold-rolled steel sheet according to this embodiment, the area ratio of a hard phase having a minor axis of 0.4 μm or less and a major axis of 1.2 μm or more (hereinafter also referred to as a "first hard phase") is 0.5% or more, and the area ratio of a hard phase having a minor axis of 1.2 μm or more (hereinafter also referred to as a "second hard phase") is 5.0% or more in terms of the area ratio in the structure observed by a scanning electron microscope (SEM).
[0026] 1 is a schematic diagram for explaining the size and shape of the hard phase defined in this embodiment. In this embodiment, a photograph of the cross section of a steel sheet taken with an SEM is subjected to image processing by a computer, and the minor axis, major axis and area of each hard phase in the cross section are measured.
[0027] As shown in FIG. 1, in the structure of the high-strength cold-rolled steel sheet according to the present embodiment, a hard phase exists together with bainite or tempered martensite. The hard phase 1 shown in FIG. 1 has a major axis of 2.5 μm and a minor axis of 0.3 μm, and corresponds to the first hard phase. The hard phase 2 has a minor axis of 1.4 μm and corresponds to the second hard phase. The hard phase 3 shown in FIG. 1 has a major axis of 0.9 μm and a minor axis of 0.3 μm, and corresponds to neither the first hard phase nor the second hard phase. The hard phase 4 has a minor axis of 0.7 μm, and corresponds to neither the first hard phase nor the second hard phase.
[0028] When the area ratio of the first hard phase is lower than 0.5%, the stretch flange formability and bendability of the steel sheet are reduced. Although the reason for this has not been clarified, it can probably be considered as follows. That is, it is presumed that when the area ratio of the first hard phase is lower than 0.5%, microcracks and fissures are likely to propagate in the steel sheet structure when the steel sheet is subjected to stretch flange formability or bending deformation, and the stretch flange formability and bendability of the steel sheet are deteriorated. The area ratio of the first hard phase is preferably 0.55% or more, more preferably 0.60% or more.
[0029] The reason for specifying the area ratio for the first hard phase, i.e., the hard phase with a "minor axis of 0.4 μm or less and a major axis of 1.2 μm or more" is as follows. It is believed that if the hard phase has a minor axis of 0.4 μm or less, it can deform in the same way as the surrounding structure when the steel sheet is deformed. Also, if the major axis is 1.2 μm or more, it is believed that it acts as a sufficiently large obstacle to the propagation of microcracks and fissures in the structure. Therefore, it is believed that the stretch flangeability and bendability of a steel sheet can be evaluated by the area ratio of the hard phase with a "minor axis of 0.4 μm or less and a major axis of 1.2 μm or more."
[0030] Furthermore, when the area ratio of the second hard phase is higher than 5.0%, the stretch flangeability and bendability of the steel sheet are reduced. Although the reason for this has not been clarified, it can probably be considered as follows. That is, when the area ratio of the second hard phase is higher than 5.0%, it is presumed that microcracks are likely to occur when the steel sheet is subjected to stretch flange deformation or bending deformation, and the stretch flangeability and bendability of the steel sheet are deteriorated. The area ratio of the second hard phase is preferably 4.8% or less, more preferably 4.6% or less.
[0031] The reason for specifying the area ratio for the second hard phase, i.e., the hard phase with a "minor axis of 1.2 μm or more" is as follows. If the hard phase has a minor axis of 1.2 μm or more, it cannot deform in the same way as the surrounding structure when the material is deformed, and it is thought that it can become a source of microcracks. Therefore, it is thought that the stretch flangeability and bendability of a steel sheet can be evaluated by the area ratio of the hard phase with a "minor axis of 1.2 μm or more".
[0032] (Residual austenite) Since the influence of the retained austenite in the microstructure on the properties of the high-strength cold-rolled steel sheet is clear, the volume fraction of the retained austenite relative to the entire structure is specified to be 3.0% or more and 7.0% or less in the high-strength cold-rolled steel sheet according to the present embodiment, as measured by an X-ray diffraction method. The volume fraction of the retained austenite is preferably 3.5% or more, more preferably 4.0% or more. Moreover, the volume fraction of the retained austenite is preferably 6.5% or less, more preferably 6.0% or less.
[0033] If the volume fraction of retained austenite is less than 3.0%, the effect of improving ductility due to the transformation-induced plasticity of retained austenite during processing of the steel sheet is reduced, resulting in a decrease in the ductility of the steel sheet. On the other hand, if the volume fraction of retained austenite exceeds 7.0%, the retained austenite transforms into martensite due to processing-induced transformation under stress, becoming a source of microcracks and fissures, which deteriorates the stretch flangeability and bendability of the steel sheet.
[0034] Since retained austenite is included in bainite in the structure observed by SEM and cannot be observed independently, the area ratio of retained austenite in the structure observed by SEM is not specified in the high-strength cold-rolled steel sheet according to this embodiment.
[0035] (Bainite, tempered martensite) In the high-strength cold-rolled steel sheet according to the present embodiment, the bainite structure and tempered martensite constitute the base structure of the high-strength cold-rolled steel sheet. In order to satisfy the above-mentioned area ratio of the hard phase and the volume ratio of the retained austenite, the total area ratio of the bainite and tempered martensite in the structure observed by SEM is set to 85% or more. The total area ratio of the bainite and tempered martensite is preferably 90% or more, more preferably 95% or more. The high-strength steel sheet according to the present embodiment may not contain both the bainite structure and the tempered martensite, but may contain only one of them.
[0036] (Other organizations) In the high-strength cold-rolled steel sheet according to the present embodiment, the area ratio of the phases other than bainite, tempered martensite, and hard phase (hereinafter also referred to as "remaining structure") in the structure observed by SEM is set to 15% or less in total. The main structures constituting the remaining structure include as-quenched martensite (in the present embodiment, as-quenched martensite includes self-tempered martensite), and unavoidably formed ferrite and pearlite.
[0037] The reason why the area ratio of the remaining structure is specified to be 15% or less in total is that if the structure of the steel sheet contains a large amount of structures with different hardness, such as hard as-quenched martensite, soft ferrite, and pearlite with intermediate hardness between them, the stretch flangeability and bendability will deteriorate due to the difference in hardness between the structures. The area ratio of the remaining structure is preferably 10% or less in total, and more preferably 5% or less.
[0038] (Chemical composition) In the high-strength cold-rolled steel sheet according to this embodiment, the chemical composition is not particularly limited as long as it can obtain the above-mentioned structural structure, the area ratio of the hard phase of a predetermined size and shape, and the volume ratio of the retained austenite. However, since C, Si, and Mn have a large effect on the strength of the steel sheet and the amount of retained austenite, they are specified in the following composition ranges. The reasons for specifying the composition ranges of each element are explained below. In the following explanation of the chemical composition, "%" always means "mass%".
[0039] (C:0.070~0.140%) C is an element necessary to ensure the strength of the steel sheet. If the C content is insufficient, the tensile strength of the steel sheet decreases, so the C content is set to 0.070% or more. The lower limit of the C content is preferably 0.080% or more, and more preferably 0.090% or more. However, if the C content is excessive, the area ratio of coarse MA and the volume ratio of retained austenite increase, and the stretch flangeability and bendability of the steel sheet decrease. Therefore, the upper limit of the C content is set to 0.140% or less. The upper limit of the C content is preferably 0.130% or less, and more preferably 0.120% or less. It is further preferably 0.110% or less.
[0040] (Si: 0.80 to 1.80%) Silicon is known as a solid solution strengthening element, and is an element that effectively acts to improve the tensile strength while suppressing the decrease in ductility of the steel sheet. It is also an element that is effective in ensuring the volume fraction of retained austenite. In order to effectively exert such effects, the amount of silicon must be 0.80% or more. The lower limit of the amount of silicon is preferably 1.10% or more, and more preferably 1.40% or more.
[0041] However, if the amount of Si is excessive, the volume fraction of retained austenite also increases, and the stretch flangeability and bendability of the steel sheet deteriorate. Therefore, the upper limit of the amount of Si is set to 1.80% or less. The upper limit of the amount of Si is preferably 1.70% or less, and more preferably 1.60% or less.
[0042] (Mn: 1.80~2.80%) Mn is an element that contributes to increasing the strength of steel sheets. To effectively exert such effects, the Mn content needs to be 1.80% or more. The lower limit of the Mn content is preferably 1.9% or more, and more preferably 2.0% or more. However, if the Mn content is excessive, the ductility and stretch flangeability of the steel sheet are reduced. Therefore, the upper limit of the Mn content is set to 2.80% or less. The upper limit of the Mn content is preferably 2.70% or less, and more preferably 2.60% or less.
[0043] The basic components of the high-strength cold-rolled steel sheet according to this embodiment are as described above, with the remainder being substantially iron. However, it is of course acceptable that the steel contains impurities that are inevitably introduced due to the conditions of raw materials, materials, manufacturing equipment, etc. Examples of such inevitable impurities include P and S, which will be described below.
[0044] (P: more than 0%, less than 0.015%) P is an element that is inevitably contained, and it segregates at grain boundaries to promote grain boundary embrittlement, and since it deteriorates the bendability of the steel sheet, it is recommended that the P content be reduced as much as possible. Therefore, the P content is preferably 0.015% or less, more preferably 0.013% or less, and even more preferably 0.010% or less. Note that P is an impurity that is inevitably mixed into steel, and it is impossible in industrial production to reduce the content to 0%.
[0045] (S: more than 0%, less than 0.0050%) Like P, S is an element that is inevitably contained, and since it generates inclusions and reduces the stretch flangeability of steel sheets, it is recommended to reduce the S content as much as possible. Therefore, the S content is preferably 0.0050% or less, more preferably 0.0040% or less, and even more preferably 0.0030% or less. Note that S is an impurity that is inevitably mixed into steel, and it is impossible in industrial production to reduce the content to 0%.
[0046] In addition to P and S, inevitable impurities contained in steel include, for example, N and O. The contents of N and O are preferably within the following ranges.
[0047] (N: more than 0%, less than 0.0100%) N is inevitably present as an impurity element and deteriorates the bendability of steel sheet. For this reason, the N content is preferably 0.0100% or less, more preferably 0.0060% or less, and even more preferably 0.0050% or less. The lower the N content, the better. However, it is difficult to reduce the N content to 0% in industrial production.
[0048] (O: more than 0%, less than 0.0020%) O is inevitably present as an impurity element and deteriorates the bendability of steel sheet. For this reason, the O content is preferably 0.0020% or less, more preferably 0.0015% or less, and even more preferably 0.0010% or less. The smaller the O content, the better. However, it is difficult in industrial production to reduce the O content to 0%.
[0049] The high-strength cold-rolled steel sheet according to the present embodiment may contain one or more elements selected from the group consisting of Al, Cr, Ti, B, Cu, Ni, Cr, Mo, V, Nb, and Ca in the ranges shown below, as necessary. By containing these elements alone or in appropriate combination, the properties of the steel sheet are further improved according to the types of elements contained.
[0050] (Al: 0.015~0.60%) Al is an element that acts as a deoxidizer. To effectively exert this function, the Al content is preferably 0.015% or more, more preferably 0.025% or more, and even more preferably 0.030% or more. Furthermore, Al is an effective element for ensuring the volume fraction of retained austenite. However, if the Al content is excessive, there is a risk of excessively increasing the Ac3 point and increasing the manufacturing cost. Therefore, the upper limit of the Al content is preferably 0.60% or less, more preferably 0.55% or less, and even more preferably 0.50% or less.
[0051] (Cr: more than 0%, less than 0.60%) Cr is an element that contributes to increasing the strength of steel sheets, and may be contained as necessary. The effect increases as the content increases, but in order to effectively exert the above effect, the Cr content is preferably 0.05% or more, more preferably 0.10% or more, and even more preferably 0.15% or more. However, if the Cr content is excessive, it may cause bare spots in hot-dip galvanized steel sheets and alloyed hot-dip galvanized steel sheets. Therefore, the upper limit of the Cr content is preferably 0.60% or less, more preferably 0.55% or less, even more preferably 0.50% or less, and even more preferably 0.45% or less.
[0052] (Ti: 0.010~0.040%) Ti is an element that forms carbides and nitrides to improve the strength of steel sheet. It is also an effective element for effectively exerting the hardenability improving effect of B described later. That is, Ti reduces N in steel by forming nitrides. As a result, the formation of B nitrides in steel is suppressed, and B in steel is in a solid solution state, so that the hardenability improving effect of B can be effectively exerted. In this way, Ti contributes to increasing the strength of steel sheet by improving hardenability. In order to effectively exert such effects, the Ti amount is preferably 0.010% or more, more preferably 0.013% or more, and even more preferably 0.015% or more.
[0053] However, if the Ti content is excessive, Ti carbides and Ti nitrides become excessive, which deteriorates the stretch flangeability of the steel sheet, so the upper limit of the Ti content is preferably 0.040% or less, more preferably 0.035% or less, and further preferably 0.030% or less.
[0054] (B: 0.0015~0.0040%) B is an element that improves hardenability and contributes to increasing the strength of steel sheets. To effectively exert such effects, the B content is preferably 0.0015% or more, more preferably 0.0020% or more, and even more preferably 0.0025% or more. However, if the B content is excessive, the effect becomes saturated and the cost only increases. Therefore, the B content is preferably 0.0040% or less, and more preferably 0.0035% or less.
[0055] (Cu: more than 0%, less than 0.30%) Cu is an element effective in improving the corrosion resistance of steel sheets, and may be contained as necessary. The effect increases as the content increases, but in order to effectively exert the above effect, the Cu content is preferably 0.03% or more, and more preferably 0.05% or more. However, if the Cu content is excessive, the effect saturates and the cost increases. Therefore, the upper limit of the Cu content is preferably 0.30% or less, more preferably 0.20% or less, and even more preferably 0.15% or less.
[0056] (Ni: more than 0%, less than 0.30%) Ni is an element effective in improving the corrosion resistance of steel sheets, and may be contained as necessary. The effect increases as the content increases, but in order to effectively exert the above effect, the Ni content is preferably 0.03% or more, and more preferably 0.05% or more. However, if the Ni content is excessive, the effect saturates and the cost increases. Therefore, the upper limit of the Ni content is preferably 0.30% or less, more preferably 0.20% or less, and even more preferably 0.15% or less.
[0057] (Mo: more than 0%, less than 0.30%) Mo is an element that contributes to increasing the strength of steel sheets, and may be contained as necessary. The effect increases as the content increases, but in order to effectively exert the above effect, the Mo content is preferably 0.03% or more, and more preferably 0.05% or more. However, if the Mo content is excessive, the effect saturates and the cost increases. Therefore, the upper limit of the Mo content is preferably 0.30% or less, more preferably 0.25% or less, and even more preferably 0.20% or less.
[0058] (V: more than 0%, less than 0.30%) V is an element that contributes to increasing the strength of steel sheets, and may be contained as necessary. The effect increases as the content increases, but in order to effectively exert the above effect, the V content is preferably 0.005% or more, and more preferably 0.010% or more. However, if the V content is excessive, the effect saturates and the cost increases. Therefore, the upper limit of the V content is preferably 0.30% or less, more preferably 0.25% or less, even more preferably 0.20% or less, and even more preferably 0.15% or less.
[0059] (Nb: more than 0%, less than 0.040%) Nb is an element that contributes to increasing the strength of steel sheets, and may be contained as necessary. The effect increases as the content increases, but in order to effectively exert the above effect, the Nb content is preferably 0.003% or more, and more preferably 0.005% or more. However, if the Nb content is excessive, the bendability is deteriorated. Therefore, the upper limit of the Nb content is preferably 0.040% or less, more preferably 0.035% or less, and even more preferably 0.030% or less.
[0060] (Ca: more than 0%, less than 0.0050%) Ca is an element that is effective in spheroidizing sulfides in steel and improving bendability, and may be contained as necessary. The effect increases as the content increases, but in order to effectively exert the above effect, the Ca content is preferably 0.0005% or more, and more preferably 0.0010% or more. However, if the Ca content is excessive, the effect saturates and the cost increases. Therefore, the upper limit of the Ca content is preferably 0.0050% or less, more preferably 0.0030% or less, and even more preferably 0.0025% or less.
[0061] (Characteristics of high-strength cold-rolled steel sheets) The high-strength cold-rolled steel sheet according to this embodiment, which satisfies the above-described chemical composition, structural structure, volume fraction of retained austenite, and area fraction of hard phase of a specified size and shape, has a tensile strength of 900 MPa or more, and, depending on the strength level, is excellent in both ductility and stretch flangeability.
[0062] The high-strength cold-rolled steel sheet according to this embodiment preferably has a tensile strength of 900 MPa or more and also satisfies, for example, all of the following properties.
[0063] The elongation EL is preferably 12% or more, more preferably 13% or more. The stretch flangeability (hole expansion ratio λ) is preferably 60% or more, more preferably 70% or more. The VDA bending angle is preferably 100° or more, more preferably 105° or more. The upper limit of the elongation EL is not particularly specified, but is usually about 18%. The higher the hole expansion ratio λ, the better the stretch flangeability, and the upper limit is not particularly limited, but is usually about 100%.
[0064] (Hot-dip galvanized steel sheet and galvannealed steel sheet) The hot-dip galvanized steel sheet according to the present embodiment includes the high-strength cold-rolled steel sheet described above and a hot-dip galvanized layer provided on the surface of the high-strength cold-rolled steel sheet. The alloyed hot-dip galvanized steel sheet according to the present embodiment includes the high-strength cold-rolled steel sheet described above and a hot-dip galvanized layer provided on the surface of the high-strength cold-rolled steel sheet.
[0065] These hot-dip galvanized steel sheets and galvannealed steel sheets also have a tensile strength of 900 MPa or more, as well as excellent ductility and stretch flangeability, similar to the high-strength cold-rolled steel sheet according to this embodiment.
[0066] Hereinafter, the high-strength cold-rolled steel sheet, the hot-dip galvanized steel sheet, and the alloyed hot-dip galvanized steel sheet according to the present embodiment will be collectively referred to as "high-strength steel sheet".
[0067] (Method of manufacturing high-strength cold-rolled steel sheets) Next, a method for producing a high-strength cold-rolled steel sheet according to this embodiment will be described.
[0068] The manufacturing method of the high-strength cold-rolled steel sheet according to the present embodiment includes a rolling step in which a steel slab is subjected to hot rolling and cold rolling in sequence, and an annealing step in which the steel sheet obtained by cold rolling the steel slab is heated to a predetermined temperature range and cooled at a predetermined rate. The high-strength cold-rolled steel sheet according to the present embodiment that satisfies the above-mentioned requirements can be manufactured by appropriately controlling the manufacturing method, particularly the annealing step after cold rolling.
[0069] Hereinafter, the manufacturing method of the high strength cold rolled steel sheet according to the present embodiment will be described in the order of the rolling process (hot rolling, cold rolling) and the annealing process. Note that the hot rolling and cold rolling do not necessarily have to be performed under the following conditions.
[0070] (Rolling process) In the rolling process, the steel slab satisfying the above-mentioned composition is subjected to hot rolling and cold rolling in this order. The hot rolling conditions are, for example, as follows.
[0071] [Hot rolling conditions] In hot rolling, a steel slab heated to a predetermined temperature is rolled at least once until it has a predetermined thickness. If the heating temperature before hot rolling is low, carbides such as TiC may not easily dissolve in austenite. Therefore, the heating temperature before hot rolling is preferably 1200°C or higher, more preferably 1250°C or higher. However, if the heating temperature before hot rolling is too high, the cost increases. Therefore, the upper limit of the heating temperature before hot rolling is preferably 1350°C or lower, more preferably 1300°C or lower.
[0072] In this embodiment, the temperature of the steel slab at the time of performing the final rolling (finish rolling) in hot rolling is referred to as the "finish rolling temperature". If the finish rolling temperature of hot rolling is low, the rolling will not be performed in the austenite single phase region, and the deformation resistance during rolling will increase, which may make operation difficult. Therefore, the finish rolling temperature is preferably 850°C or higher, and more preferably 870°C or higher. However, if the finish rolling temperature is too high, there is a risk of the crystals becoming coarse. Therefore, the finish rolling temperature is preferably 980°C or lower, and more preferably 950°C or lower.
[0073] The average cooling rate from the end of finish rolling in hot rolling to the start of coiling is preferably 10°C / sec or more, more preferably 20°C / sec or more, in consideration of productivity. On the other hand, if the average cooling rate is too fast, the equipment cost increases. Therefore, the average cooling rate is preferably 100°C / sec or less, more preferably 50°C / sec or less.
[0074] Next, the conditions of the steps after the hot rolling will be described.
[0075] [Coiling temperature after hot rolling] The steel sheet obtained by hot rolling (hot rolled steel sheet) is wound into a coil. If the coiling temperature after hot rolling is less than 570°C, the strength of the hot rolled steel sheet increases, making it difficult to roll down by cold rolling. Therefore, the coiling temperature after hot rolling is preferably 570°C or higher, more preferably 580°C or higher, and even more preferably 590°C or higher. On the other hand, if the coiling temperature after hot rolling is too high, pickling properties for removing scale deteriorate. Therefore, the coiling temperature is preferably 700°C or lower, more preferably 690°C or lower, and even more preferably 680°C or lower.
[0076] [Reduction ratio during cold rolling] The hot-rolled steel sheet wound into a coil is unwound, pickled to remove scale, and then cold-rolled. The rolling ratio (synonymous with "rolling reduction") during cold rolling is preferably 20% or more and 60% or less. In order to obtain a steel sheet of a predetermined thickness with a rolling ratio during cold rolling of less than 20%, the thickness of the hot-rolled steel sheet must be thinned in the hot rolling process. If the thickness of the hot-rolled steel sheet is thinned, the length of the steel sheet increases, so that pickling takes time and productivity decreases. Therefore, the rolling ratio during cold rolling is preferably 20% or more, more preferably 25% or more. On the other hand, if the rolling ratio during cold rolling exceeds 60%, a high-capacity cold rolling machine is required. Therefore, the upper limit of the rolling ratio during cold rolling is preferably 60% or less, more preferably 55% or less, and even more preferably 50% or less.
[0077] (Annealing process) In the annealing process, the steel sheet obtained by hot rolling and cold rolling the steel slab is annealed using an annealing furnace. In order to obtain the high-strength cold-rolled steel sheet according to this embodiment, it is important to appropriately adjust the conditions in each process included in the annealing process after cold rolling. In the manufacturing method of the high-strength cold-rolled steel sheet according to this embodiment, the annealing process includes (a) a heating process, (b) a soaking process performed following the heating process, (c) a first cooling process performed following the soaking process, (d) a holding process performed following the first cooling process, and (e) a second cooling process performed following the holding process. The heat pattern (time change in the temperature of the steel sheet) of the annealing process including each of these processes (a) to (e) is shown in FIG. 2(A) as a schematic diagram. Each of the processes (a) to (e) will be described below in order.
[0078] (a) Heating process In the heating step according to the present embodiment, the cold-rolled steel sheet obtained by cold rolling the steel slab is heated to a temperature range of (Ac3 point + 200 ° C) or less, that is, the soaking temperature described later, at a heating rate (i.e., heating rate) of 1.5 ° C / sec or more and 30 ° C / sec or less at 700 ° C or more. The lower limit of the temperature range to be heated is preferably the lower of the Ac3 point and 950 ° C. In other words, when the Ac3 point is less than 950 ° C, it is preferable to heat to a temperature range of the Ac3 point or more (Ac3 point + 200 ° C) or less, and when the Ac3 point is 950 ° C or more, it is preferable to heat to a temperature range of 950 ° C or more (Ac3 point + 200 ° C). If the heating rate at 700 ° C or more is less than 1.5 ° C / sec, the time to reach the soaking temperature will be long, and the equipment cost will be high. Therefore, the lower limit of the heating rate at 700 ° C or more is set to 1.5 ° C / sec or more.
[0079] On the other hand, if the heating rate exceeds 30°C / sec at 700°C or higher, it becomes difficult to control the steel sheet temperature, and the equipment cost increases. Therefore, the upper limit of the heating rate at 700°C or higher is set to 30°C / sec or lower. The upper limit of the heating rate at 700°C or higher is preferably 25°C / sec or lower, and more preferably 20°C / sec or lower. In the heating step according to this embodiment, the heating rate in the temperature range below 700°C may be any rate.
[0080] (b) Soaking process In the soaking step according to this embodiment, the steel sheet that has been through the heating step is held at a predetermined temperature for a predetermined time. Specifically, in the heating step, the steel sheet is heated to a temperature range of (Ac3 point + 200°C) or lower, and then held at that temperature for a predetermined time to soak. Hereinafter, the temperature at which the steel sheet is soaked is referred to as the "soaking temperature" and the time for soaking is referred to as the "soaking time". By setting the soaking temperature to (Ac3 point + 200°C) or lower and holding for a predetermined soaking time, a steel sheet with excellent stretch flangeability can be produced in the subsequent steps without consuming excessive energy.
[0081] If the soaking temperature is less than the Ac3 point when the Ac3 point is less than 950°C, or if the soaking temperature is less than 950°C when the Ac3 point is 950°C or more, ferrite may be generated in the structure during the soaking process, and it may be difficult to ensure the desired stretch flangeability. Therefore, the lower limit of the soaking temperature is preferably the lower of the Ac3 point or 950°C or more. By setting the lower limit of the soaking temperature to the lower of the Ac3 point or 950°C or more and holding for a predetermined soaking time, the area ratio of austenite in the entire structure can be 85% or more. The lower limit of the soaking temperature is more preferably the lower of the Ac3 point + 10°C or more or 960°C or more.
[0082] On the other hand, if the soaking temperature is too high and exceeds Ac3 point + 200°C, excessive energy is required to industrially produce high-strength cold-rolled steel sheets. Therefore, the upper limit of the soaking temperature is set to Ac3 point + 200°C or less. The upper limit of the soaking temperature is preferably Ac3 point + 150°C or less.
[0083] Here, the Ac3 point of the steel sheet is calculated based on the following formula (1). Note that (% [element name]) in the formula is the content (mass%) of each element, and the content of elements not contained in the steel sheet is calculated as 0%. The following formula (1) is quoted from "Leslie Steel Materials Science" (published by Maruzen Co., Ltd., written by William C. Leslie, p. 273). Ac3 points=910-203(%C) 1 / 2-15.2(%Ni)+44.7(%Si)+104(%V)+31.5(%Mo)+13.1(%W)-30(%Mn)-11(%Cr)-20(%Cu)+700(%P)+400(%Al)+120(%As)+400(%Ti) …(1)
[0084] In the soaking step according to the present embodiment, the soaking time is set to 10 seconds or more and 100 seconds or less. By setting the soaking time to 10 seconds or more and 100 seconds or less and holding at the above-mentioned soaking temperature, the area ratio of austenite in the entire structure can be set to 85% or more, and a steel sheet with excellent stretch flangeability can be produced with high productivity by the subsequent steps. If the soaking time is less than 10 seconds, it becomes difficult to ensure the desired stretch flangeability due to the generation of excessive ferrite. Therefore, the lower limit of the soaking time is set to 10 seconds or more. The lower limit of the soaking time is preferably 13 seconds or more. On the other hand, if the soaking time exceeds 100 seconds, the productivity decreases. Therefore, the upper limit of the soaking time is set to 100 seconds or less. The upper limit of the soaking time is preferably 80 seconds or less.
[0085] In the soaking step, the soaking temperature is preferably kept constant at the temperature when the heating step is completed, i.e., the temperature when the temperature increase of the steel sheet is stopped, but it may vary as long as it is in a temperature range below (Ac3 point + 200°C) (preferably above the lower of Ac3 point or 950°C) and at a temperature increase rate slower than the temperature increase rate at 700°C or higher, and the temperature at the start and end of the soaking step may be different. The gradual increase in temperature in the soaking step in Fig. 2(A) means that even when the temperature increase of the annealing furnace is stopped, the temperature inside the furnace and the steel sheet continues to increase slightly.
[0086] (c) First cooling step In the first cooling step according to the present embodiment, the steel sheet that has been through the soaking step is cooled at a predetermined cooling rate to a predetermined cooling stop temperature (hereinafter referred to as the "first cooling temperature"). The cooling rate from the soaking temperature to the first cooling temperature (hereinafter referred to as the "first cooling rate") is set to 10°C / sec or more and 50°C / sec or less.
[0087] If the first cooling rate is less than 10°C / sec, the area ratio of the first hard phase decreases and the area ratio of the second hard phase increases, which is thought to result in a decrease in stretch flangeability. Therefore, the lower limit of the first cooling rate is set to 10°C / sec or more. The lower limit of the first cooling rate is preferably 15°C / sec or more, more preferably 18°C / sec or more.
[0088] On the other hand, if the first cooling rate exceeds 50°C / sec, it becomes difficult to control the steel sheet temperature, and the equipment cost increases. Therefore, the upper limit of the first cooling rate is set to 50°C / sec or less. The upper limit of the first cooling rate is preferably 40°C / sec or less, and more preferably 30°C / sec or less.
[0089] The first cooling temperature is 100° C. or more and 410° C. or less. By cooling to a temperature range of 100° C. or more and 410° C. or less at the above-mentioned first cooling rate, it is possible to obtain a steel sheet structure mainly composed of bainite or mainly composed of as-quenched martensite.
[0090] If the first cooling temperature is less than 100°C, the volume fraction of the retained austenite decreases, and the ductility decreases. Therefore, the lower limit of the first cooling temperature is set to 100°C or more. The lower limit of the first cooling temperature is preferably 150°C or more, and more preferably 200°C or more.
[0091] On the other hand, if the first cooling temperature exceeds 410°C, the area ratio of the first hard phase becomes lower than 0.5%, or the area ratio of the second hard phase becomes higher than 5.0%, and the stretch flangeability and bendability of the steel sheet deteriorate. Therefore, the upper limit of the first cooling temperature is set to 410°C or less. The upper limit of the first cooling temperature is preferably 400°C or less.
[0092] In the first cooling step, the structure of the steel sheet can be controlled by controlling the first cooling temperature. Specifically, the steel sheet structure can be made mainly of bainite (area ratio of 85% or more) by setting the first cooling temperature to 350°C or more and 410°C or less. In addition, the steel sheet structure can be made mainly of as-quenched martensite by setting the first cooling temperature to 100°C or more and less than 350°C. Furthermore, the as-quenched martensite can be tempered to make the steel sheet structure mainly of tempered martensite (area ratio of 85% or more) by providing a reheating step described later after the first cooling step.
[0093] (d) Holding process In the holding step after the first cooling step, the holding temperature is 100° C. or higher and 410° C. or lower, and the holding time is 80 seconds or shorter.
[0094] If the holding temperature in the holding step is less than 100°C, the volume fraction of the retained austenite decreases and the ductility decreases. Therefore, the lower limit of the holding temperature in the holding step is set to 100°C or higher, preferably 150°C or higher, and more preferably 200°C or higher.
[0095] On the other hand, if the holding temperature in the holding step exceeds 410°C, the area ratio of the first hard phase will be lower than 0.5%, or the area ratio of the second hard phase will be higher than 5.0%, and the stretch flangeability and bendability of the steel sheet will decrease, so the upper limit of the holding temperature in the holding step is set to 410°C or less. The upper limit of the holding temperature in the holding step is preferably 400°C or less.
[0096] Furthermore, if the holding time in the holding step is less than 10 seconds, the concentration of C due to diffusion from the bainite or martensite generated in the first cooling step to the untransformed austenite does not proceed sufficiently, and the martensite transformation of the untransformed austenite proceeds excessively in the second cooling step, which is thought to reduce the volume fraction of the retained austenite and reduce ductility. On the other hand, if the holding time in the holding step exceeds 80 seconds, the bainite or martensite transformation of the untransformed austenite proceeds excessively, which is thought to reduce the volume fraction of the retained austenite and reduce ductility, and at the same time, reduce productivity. Therefore, the upper limit of the holding time is set to 80 seconds or less.
[0097] In the holding step, the holding temperature is preferably kept constant at the temperature at the end of the first cooling step, but the holding temperature may be different between the start and end of the holding step. Specifically, the holding temperature may vary as long as it is in the temperature range of 100°C or more and 410°C or less, and the temperature drop rate is slower than the first cooling rate. The gradual decrease in temperature in the holding step in Fig. 2(A) means that even if the temperature drop in the annealing furnace is stopped, the temperature inside the furnace and the steel sheet will continue to decrease slightly.
[0098] Furthermore, when the first cooling temperature is set to 350°C or more and 410°C or less, the holding temperature is also preferably set to 350°C or more and 410°C or less. This allows the steel sheet structure mainly composed of bainite generated in the first cooling step to be maintained in the holding step. Similarly, when the first cooling temperature is set to 100°C or more and less than 350°C, the holding temperature is also preferably set to 100°C or more and less than 350°C. This allows the steel sheet structure mainly composed of martensite as quenched generated in the first cooling step to be maintained in the holding step.
[0099] (e) Second cooling step In the second cooling step, after the holding step, cooling is performed at a cooling rate of 15°C / sec or more from the holding temperature at the end of the holding step. In the high-strength cold-rolled steel sheet according to the present embodiment, the C content is as low as 0.140% or less, so that it is difficult to obtain retained austenite. Therefore, if the cooling rate in the second cooling step (hereinafter also referred to as the "second cooling rate") is less than 15°C / sec, it is considered that the volume fraction of retained austenite decreases and ductility decreases. Therefore, the lower limit of the second cooling rate is 15°C / sec or more. The lower limit of the second cooling rate is preferably 18°C / sec or more. The upper limit of the second cooling rate is not particularly limited, and is, for example, 30°C / sec or less. The cooling stop temperature in the second cooling step is also not particularly limited, and it is usually sufficient to cool to room temperature.
[0100] In the annealing step of the method for producing a high-strength steel sheet according to this embodiment, in addition to the steps (a) to (e) described above, one or both of a reheating step (f) and a plating step (g) may be added. In addition, an alloying step (h) may be added to the plating step (g). Each of the steps (f) to (h) will be described below.
[0101] (f) Reheating process In the manufacturing method of a high-strength steel plate according to this embodiment, as shown in FIG. 2(B), a reheating step (f) of reheating the steel plate to a temperature of 400° C. or more and 500° C. or less and holding the temperature for 10 seconds or more may be provided between the holding step (d) and the second cooling step (e).
[0102] In the reheating step, the as-quenched martensite generated in the first cooling step and held in the holding step can be tempered, and a steel sheet structure mainly composed of tempered martensite (area ratio of 85% or more) can be obtained. When the reheating step is provided, in order to generate as-quenched martensite in the first cooling step, the first cooling temperature in the first cooling step is set to 100°C or more and less than 350°C, and the holding temperature in the holding step is set to 100°C or more and less than 350°C. After the reheating step, the above-mentioned second cooling step is performed.
[0103] (g) Plating process, (h) Alloying process In the manufacturing method of the high-strength steel sheet according to the present embodiment, a step of subjecting the steel sheet to a zinc plating treatment (plating step) is provided before the second cooling step, thereby making it possible to manufacture the hot-dip galvanized steel sheet according to the present embodiment. In addition, in the manufacturing method of the high-strength steel sheet according to the present embodiment, a step of subjecting the steel sheet to a zinc plating treatment and an alloying treatment in sequence (plating step and alloying step) is provided before the second cooling step, thereby making it possible to manufacture the hot-dip galvanized steel sheet according to the present embodiment. Specifically, as shown in FIG. 2(C), a plating step (g), or a plating step (g) and an alloying step (h) are performed before the second cooling step (e).
[0104] The hot-dip galvanized steel sheet according to this embodiment can be produced by subjecting the steel sheet that has been subjected to the above-mentioned holding step (d) to a galvanizing treatment (immersion in a galvanizing bath at about 460°C for about 1 to 5 seconds) by a conventional method (plating step (g)), and then cooling in the above-mentioned second cooling step (e).
[0105] The galvannealed steel sheet according to this embodiment can be produced by subjecting the steel sheet that has been subjected to the above-mentioned holding step (d) to a galvanizing treatment (immersion in a galvanizing bath at about 460°C for about 1 to 5 seconds) by a conventional method (plating step (g)), further subjecting it to an alloying treatment of the galvanized steel with the galvanized steel (heating to 430 to 550°C and holding for 20 to 40 seconds) (alloying step (h)), and then cooling in the above-mentioned second cooling step (e).
[0106] When the plating step (g) is provided, the first cooling temperature in the first cooling step (c) is set to 350°C or higher and 410°C or lower, and the holding temperature in the holding step (d) is set to 350°C or higher and 410°C or lower, whereby a hot-dip galvanized steel sheet or an alloyed hot-dip galvanized steel sheet having a steel sheet structure mainly composed of bainite can be obtained.
[0107] In the manufacturing method of the hot-dip galvanized steel sheet and the manufacturing method of the alloyed hot-dip galvanized steel sheet according to the present embodiment, the above-mentioned reheating step (f) may be performed before the plating step (g). Specifically, as shown in Fig. 2(D) , after the holding step (d) and before the second cooling step (e), the reheating step (f) is performed, and the plating step (g) is performed following the reheating step (f). After the plating step (g), the alloying step (h) may be performed.
[0108] When the reheating step (f) and the plating step (g) are provided, the first cooling temperature in the first cooling step is set to 100°C or more and less than 350°C, and the holding temperature in the holding step is set to 100°C or more and less than 350°C, whereby a hot-dip galvanized steel sheet or an alloyed hot-dip galvanized steel sheet having a steel sheet structure mainly composed of tempered martensite can be obtained.
[0109] The high-strength steel plate according to the present embodiment is not limited to the one obtained by the above-mentioned manufacturing method, and may be the one obtained by another manufacturing method as long as it satisfies the requirements defined in the present invention.
[0110] As described above, this specification discloses various aspects of the technology, the main technologies of which are summarized below.
[0111] As described above, the high-strength cold rolled steel sheet according to one aspect of the present invention contains, by mass%, C: 0.070 to 0.140%, Si: 0.80 to 1.80%, and Mn: 1.80 to 2.80%, with the balance being iron and inevitable impurities; in terms of area fraction in a structure observed with a scanning electron microscope, a total of hard phases consisting of bainite, tempered martensite, and at least one of MA in which quenched martensite and retained austenite are combined, and cementite, is 85% or more; in the hard phase, a hard phase having a short diameter of 0.4 μm or less and a long diameter of 1.2 μm or more is 0.5% or more; in the hard phase, a hard phase having a short diameter of 1.2 μm or more is 5.0% or less; and a structure other than the bainite, the tempered martensite, and the hard phase is 15% or less; and in terms of volume fraction measured by an X-ray diffraction method, the retained austenite is 3.0% or more and 7.0% or less.
[0112] According to this configuration, a high-strength cold-rolled steel sheet excellent in stretch flangeability and bendability can be obtained.
[0113] The high-strength cold rolled steel sheet having the above configuration may further contain, by mass%, one or more selected from the group consisting of Al: 0.015 to 0.60%, Cr: more than 0% and 0.60% or less, Ti: 0.010 to 0.040%, B: 0.0015 to 0.0040%, Cu: more than 0% and 0.30% or less, Ni: more than 0% and 0.30% or less, Mo: more than 0% and 0.30% or less, V: more than 0% and 0.30% or less, Nb: more than 0% and 0.040% or less, and Ca: more than 0% and 0.0050% or less.
[0114] According to this configuration, it is possible to obtain a high-strength cold-rolled steel sheet that is excellent not only in stretch flangeability and bendability but also in other properties.
[0115] The high-strength cold-rolled steel sheet having the above configuration may further contain, as the unavoidable impurities, P: more than 0% and 0.015% or less, and S: more than 0% and 0.0050% or less, in mass %.
[0116] According to this configuration, it is possible to obtain a high-strength cold-rolled steel sheet that is excellent in stretch flangeability and bendability and in which the influence of unavoidable impurities is suppressed.
[0117] A hot-dip galvanized steel sheet and an alloyed hot-dip galvanized steel sheet according to another aspect of the present invention have the above-mentioned high-strength cold-rolled steel sheet and a hot-dip galvanized layer or an alloyed hot-dip galvanized layer provided on the surface of the high-strength cold-rolled steel sheet.
[0118] According to this configuration, it is possible to obtain a hot-dip galvanized steel sheet or a hot-dip galvannealed steel sheet having excellent stretch flangeability and bendability.
[0119] A method for producing a high-strength cold-rolled steel sheet according to another aspect of the present invention includes a rolling step of successively performing hot rolling and cold rolling on a steel slab satisfying the above-mentioned chemical composition, a heating step of heating the steel sheet obtained by cold rolling the steel slab to a temperature range of (Ac3 point + 200°C) or lower at a temperature rise rate of 1.5°C / sec to 30°C / sec at 700°C or higher, and a soaking step of holding the steel sheet after the heating step for 10 seconds to 100 seconds. the steel plate that has undergone the soaking step having a first cooling temperature of 100°C or more and 410°C or less at a cooling rate of 10°C / sec or more and 50°C / sec or less; a holding step of holding the steel plate that has been cooled to the first cooling temperature at a holding temperature of 100°C or more and 410°C or less for 10 seconds or more and 80 seconds or less; and a second cooling step of cooling the steel plate that has undergone the holding step to approximately room temperature at a cooling rate of 15°C / sec or more, in this order.
[0120] According to this configuration, a high-strength cold-rolled steel sheet excellent in stretch flangeability and bendability can be produced.
[0121] In the method for producing a high-strength cold-rolled steel sheet having the above configuration, a first cooling temperature in the first cooling step may be 350°C or more and 410°C or less, and a holding temperature in the holding step may be 350°C or more and 410°C or less.
[0122] According to this configuration, a high-strength cold-rolled steel sheet having a steel sheet structure mainly composed of bainite can be produced.
[0123] In the manufacturing method of the high-strength cold-rolled steel sheet having the above configuration, the first cooling temperature in the first cooling step is 100°C or more and less than 350°C, the holding temperature in the holding step is 100°C or more and less than 350°C, and a reheating step may be provided between the holding step and the second cooling step, in which the steel sheet is reheated to a temperature of 400°C or more and 500°C or less and held for 10 seconds or more.
[0124] According to this configuration, a high-strength cold-rolled steel sheet having a steel sheet structure mainly composed of tempered martensite can be manufactured.
[0125] According to another aspect of the present invention, there is provided a method for producing a hot-dip galvanized steel sheet and a method for producing an alloyed hot-dip galvanized steel sheet, in which, in the above-described method for producing a high-strength cold-rolled steel sheet, the steel sheet is further subjected to a galvanizing treatment before the second cooling step, or is subjected to an alloying treatment following the galvanizing treatment.
[0126] According to this configuration, it is possible to obtain a hot-dip galvanized steel sheet or a hot-dip galvannealed steel sheet having excellent stretch flangeability and bendability.
[0127] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples, and may be modified within the scope of the above and below-described aims, and all such modifications are included in the technical scope of the present invention. EXAMPLES
[0128] Slabs were produced having the chemical composition (steel types: steels 1 to 8) shown in Table 1. The slabs were hot-rolled, and the hot-rolling was performed at a coiling temperature of 660° C. The obtained hot-rolled steel sheets were pickled and then cold-rolled.
[0129] Thereafter, heat treatment was performed under the conditions (heat treatments 1 to 14) shown in Table 2 based on the heat pattern shown in FIG. 2. In Table 1, the column "-" means that no addition was made. In Table 1, the V, Nb, and Ca contents are shown as values rounded off to two decimal places, so "0.00" for these contents means that the measured values were 0.004% or less. Also, "N / A" means that the values were below the detection limit. Also, P, S, N, and O are unavoidable impurities as mentioned above, and the values shown in the columns for P, S, N, and O mean the amounts that were unavoidably contained.
[0130] [Table 1]
[0131] [Table 2]
[0132] Under heat treatment conditions 1 to 14 shown in Table 2, the same thermal history as that of galvannealed steel sheet was given. In Table 2, "holding temperature" is the temperature at the end of the holding process, and is hereinafter also referred to as "holding end temperature." "Soaking temperature" is the average value of the temperature range in the soaking process that can be estimated from the actual measured value. In Table 2, the column "-" indicates that the reheating process was not performed.
[0133] For each of the cold-rolled steel sheets thus obtained, the structure fraction (area fraction), the volume fraction of retained austenite, the size and shape of the hard phase, and various properties (tensile properties, stretch flangeability, bendability) were measured according to the following procedures.
[0134] [Tissue fraction] The metal structure of the base steel sheet that constitutes the steel sheet was observed using the following procedure. The area ratios of ferrite, pearlite, bainite, tempered martensite, and as-quenched martensite (including self-tempered martensite) in the metal structure were calculated based on the results of observation using a scanning electron microscope (SEM).
[0135] Observation by SEM was carried out as follows: the surface of the cross section parallel to the rolling direction of the base steel sheet was polished, further electrolytically polished, and then the polished surface was corroded with nital, and three fields of view were observed at a magnification of 5000 times by SEM at a position of 1 / 4 of the sheet thickness. The observation field was about 30 μm × about 30 μm.
[0136] For steel plates that were clearly composed only of bainite or tempered martensite in the images observed in this manner, the area ratio was not calculated. Only when ferrite, as-quenched martensite, etc. were present, the area ratio was calculated by image processing.
[0137] When observed by SEM, bainite and tempered martensite are observed as structures in which MA and cementite (hard phase) are dispersed among the crystal grains of bainite or tempered martensite. Bainite or tempered martensite is observed mainly in gray, MA is observed in white or light gray, and cementite is observed in white. In this case, it is difficult to distinguish between the retained austenite and quenched martensite that make up MA, and they are observed as one body.
[0138] When observed by SEM, bainite also contains retained austenite and carbides, so the area ratio of bainite is calculated as the area ratio including the retained austenite and carbides.
[0139] In addition, ferrite is observed mainly in a gray color close to white, and no MA or cementite is present in the ferrite grains. Pearlite is observed as a structure in which carbides and ferrite are layered. As-quenched martensite (including self-tempered martensite) is observed mainly in a gray color, and as-quenched martensite grains have extremely fine carbides dispersed therein.
[0140] [Volume fraction of retained austenite] The volume fraction of the retained austenite was measured by cutting test pieces of each plate thickness × 10 to 20 mm × 10 to 20 mm from the cold rolled steel sheets after the annealing, grinding them to t / 4 of the plate thickness t, and then chemically polishing them, and then measuring the volume fraction of the retained austenite by X-ray diffraction (ISIJ Int. Vol. 33. (1993), No. 7, P. 776).
[0141] [Measurement of size and shape of hard phases] The observation images obtained by the SEM observation performed when calculating the above-mentioned structure fraction were subjected to image processing and then image analysis to calculate the minor axis, major axis, and area of the hard phase. The "major axis" was the longest axis of the hard phase, and the "minor axis" was the longest axis in the direction perpendicular to the major axis. Using the calculated minor axis, major axis, and area of the hard phase, the area ratio of the hard phase (first hard phase) with a minor axis of 0.4 μm or less and a major axis of 1.2 μm or more, and the hard phase (second hard phase) with a minor axis of 1.2 μm or more were calculated.
[0142] [Tensile properties] JIS No. 5 test pieces (plate-shaped test pieces) were taken so that the longitudinal direction of the test piece was perpendicular to the rolling direction in a plane parallel to the cold-rolled rolling surface of the steel plate. Tensile tests were performed using the test pieces to measure the tensile strength (TS) and elongation (EL). The ductility of the steel plate was evaluated based on the measured elongation (EL).
[0143] [Stretch flangeability] Test pieces measuring 90 mm x 90 mm were taken from each cold-rolled steel sheet. Using the test pieces, a hole expansion test was performed based on JIS Z 2256:2010 to measure the hole expansion ratio λ. The stretch flangeability of the steel sheets was evaluated based on the measured hole expansion ratio λ.
[0144] [VDA bending angle] Test pieces measuring 60 mm x 60 mm x thickness were taken from the cold-rolled steel sheets and subjected to bending tests under the following conditions based on the VDA standard (VDA238-100) prescribed by the German Association of the Automotive Industry. The displacement at the maximum load measured in the bending test was converted to an angle according to the VDA standard to determine the bending angle.
[0145] (Measurement conditions) Test method: Roll support, punch press Roll diameter: φ30mm Punch shape: Tip R = 0.4 mm Distance between rolls: Sheet thickness x 2 + 0.5 mm Punch pressing speed: 20mm / min Test piece size: 60mm x 60mm Bending direction: Perpendicular to the rolling direction Testing machine: SHIMADZU AUTOGRAPH 20kN The pass criteria for each test item are as follows:
[0146] A tensile strength of 900 MPa or more, ductility (elongation EL) of 12% or more, stretch flangeability (hole expansion ratio λ) of 60% or more, and VDA bend angle of 100° or more were deemed to pass, and anything else was deemed to fail. The higher the elongation EL, the better the ductility, and the higher the hole expansion ratio λ, the better the stretch flangeability. Also, the higher the VDA bend angle, the better the bendability.
[0147] These results are shown in Table 3 together with the applied steel grades and heat treatment conditions. In Table 3, a "-" column indicates that the corresponding item was not measured. Additionally, the "remaining structure" in Table 3 refers to the structure other than bainite, tempered martensite, and hard phases, and is mainly pearlite, ferrite, and as-quenched martensite (including self-tempered martensite).
[0148] [Table 3]
[0149] The results shown in Table 3 can be interpreted as follows.
[0150] Test Nos. 1, 3, 5 to 8, 13, and 14 are examples (examples of the present invention) manufactured using steel types (steels 1 to 4, 7, and 8 in Table 1) that satisfy the chemical composition specified in the present invention, under appropriate heat treatment conditions (heat treatment Nos. 1, 3, 5 to 8, 13, and 14 in Table 2; all of these are thermal histories used in manufacturing galvannealed steel sheets).
[0151] All of these examples had a tensile strength of 900 MPa or more, an elongation EL of 12% or more, a hole expansion ratio λ of 60% or more, and a VDA bending angle of 100° or more, which satisfied the pass criteria. In the high-strength steel plates of Test Nos. 1, 3, 5 to 8, 13, and 14, the microstructures satisfied the area fractions of bainite and tempered martensite, the volume fraction of retained austenite, the area fractions of the first hard phase and the second hard phase, and the area fraction of the remaining structure, all of which are specified in the present invention.
[0152] In contrast, Test Nos. 2, 4, and 9 were examples (comparative examples) in which steel types (steels 1 to 4 in Table 1) that satisfied the chemical composition specified in the present invention were used, but which were manufactured under heat treatment conditions (heat treatments 2, 4, and 9 in Table 2) that were outside the appropriate range, and the desired properties were not obtained and the pass criteria were not met.
[0153] Specifically, in Test No. 2, the first cooling temperature and holding temperature (holding stop temperature) were high (heat treatment 2), the area fraction of the first hard phase was lower than 0.5%, the area fraction of the second hard phase was higher than 5.0%, the hole expansion ratio λ was less than 60%, and the VDA bend angle was less than 100°.
[0154] In Test No. 4, the first cooling temperature and the holding end temperature were high (Heat Treatment 4). The obtained steel sheet had an area ratio of the second hard phase higher than 5.0% and a hole expansion ratio λ of less than 60%.
[0155] In Test No. 9, the first cooling temperature and the holding end temperature were high (Heat Treatment 9). The obtained steel sheet had an area ratio of the residual structure higher than 15%, an area ratio of the first hard phase less than 0.5%, a volume fraction of the retained austenite less than 3%, a hole expansion ratio λ less than 60%, and a VDA bending angle less than 100°.
[0156] On the other hand, Test No. 12 is an example (comparative example) produced using a steel type (steel type 6 in Table 1) that does not satisfy the chemical composition specified in the present invention and is produced under appropriate heat treatment conditions (heat treatment type 12 in Table 2), and the desired properties were not obtained and the pass criteria were not met. Specifically, in Test No. 12, the C content was high (steel type 6), the volume fraction of retained austenite was higher than 7%, and the hole expansion ratio λ was less than 60%.
[0157] Test Nos. 10 and 11 are examples (comparative examples) produced using a steel type (steel 5 in Table 1) that does not satisfy the chemical composition specified in the present invention and under heat treatment conditions (heat treatments 10 and 11 in Table 2) that are outside the appropriate range. The desired properties were not obtained and the pass criteria were not met.
[0158] Specifically, in Test No. 10, the Si content was low (Steel Type 5), and the heating rate and first cooling rate at 700°C or higher were low, and the first cooling temperature and holding stop temperature were high (Heat Treatment 10). The obtained steel sheet had a hole expansion ratio λ of less than 60% and an elongation of less than 12%.
[0159] In test No. 11, the Si content was low (steel type 5), and the heating rate and first cooling rate at 700°C or higher were low, and the first cooling temperature and holding stop temperature were high (heat treatment 11). The obtained steel sheet had a hole expansion ratio λ of less than 60%. [Explanation of symbols]
[0160] 1 Hard phase (first hard phase) 2 Hard phase (second hard phase)
Claims
1. In mass percent, C: 0.070-0.140%, Si: 0.80 to 1.80%, and Mn: 1.80-2.80%, and the balance being iron and unavoidable impurities, The area ratio in the structure observed with a scanning electron microscope. The total content of hard phases consisting of bainite, tempered martensite, and at least one of MA, which is a combination of quenched martensite and retained austenite, and cementite is 85% or more; The hard phase has a minor axis of 0.4 μm or less and a major axis of 1.2 μm or more, and the minor axis of the hard phase is 0.5% or more; The hard phase has a minor axis of 1.2 μm or more in an amount of 5.0% or less, a structure other than the bainite, the tempered martensite, and the hard phase is 15% or less; A high-strength cold-rolled steel sheet having a volume fraction of retained austenite of 3.0% or more and 7.0% or less, as measured by an X-ray diffraction method.
2. Further, in mass%, Al: 0.015-0.60%, Cr: more than 0%, 0.60% or less, Ti: 0.010-0.040%, B: 0.0015-0.0040%, Cu: more than 0%, 0.30% or less, Ni: more than 0%, less than 0.30%, Mo: more than 0%, less than 0.30%, V: more than 0%, less than 0.30%, Nb: more than 0% and 0.040% or less, and Ca: one or more selected from the group consisting of more than 0% and 0.0050% or less; The high strength cold rolled steel sheet according to claim 1, which contains
3. Further, as the unavoidable impurities, in mass %, P: more than 0% and 0.015% or less, and S: more than 0%, less than 0.0050%, The high strength cold rolled steel sheet according to claim 1, which contains
4. A hot-dip galvanized steel sheet comprising: the high-strength cold-rolled steel sheet according to any one of claims 1 to 3; and a hot-dip galvanized layer provided on a surface of the high-strength cold-rolled steel sheet.
5. A galvannealed steel sheet comprising: the high-strength cold-rolled steel sheet according to any one of claims 1 to 3; and a galvannealed layer provided on a surface of the high-strength cold-rolled steel sheet.
6. A rolling step of sequentially subjecting a steel slab having a chemical composition according to any one of claims 1 to 3 to hot rolling and cold rolling; The steel slab is cold-rolled to obtain a steel sheet, and the temperature rise rate at 700° C. or higher is set to 1.5° C. / sec or more and 30° C. / sec or less, (Ac 3 a heating step of heating the material to a temperature range of 0.1% or less (temperature range of 0.1% or less +200°C); a soaking step of holding the steel sheet after the heating step for 10 seconds or more and 100 seconds or less; A first cooling step of cooling the steel sheet having been subjected to the soaking step to a first cooling temperature of 100° C. or more and 410° C. or less at a cooling rate of 10° C. / sec or more and 50° C. / sec or less; A holding step of holding the steel sheet cooled to the first cooling temperature at a holding temperature of 100° C. or more and 410° C. or less for 10 seconds or more and 80 seconds or less; The method for producing a high strength cold rolled steel sheet according to claim 1 or 2, further comprising: a second cooling step of cooling the steel sheet that has been subjected to the holding step to room temperature at a cooling rate of 15°C / sec or more.
7. The method for producing a high strength cold rolled steel sheet according to claim 6, wherein a first cooling temperature in the first cooling step is 350°C or more and 410°C or less, and a holding temperature in the holding step is 350°C or more and 410°C or less.
8. The first cooling temperature in the first cooling step is 100° C. or more and less than 350° C.; The holding temperature in the holding step is 100° C. or more and less than 350° C., The method for producing a high strength cold rolled steel sheet according to claim 6, further comprising a reheating step between the holding step and the second cooling step, of reheating the steel sheet to a temperature of 400°C or more and 500°C or less and holding the temperature for 10 seconds or more.
9. The method for producing a high-strength cold-rolled steel sheet according to any one of claims 6 to 8, further comprising the step of: subjecting the steel sheet to a galvanizing treatment before the second cooling step. The method for producing a hot-dip galvanized steel sheet according to claim 4.
10. The method for producing a high-strength cold-rolled steel sheet according to any one of claims 6 to 8, further comprising the steps of: subjecting the steel sheet to a zinc plating treatment and an alloying treatment in this order before the second cooling step.
Citation Information
Patent Citations
Stave-damage detecting method
JP1985085348A
High-strength cold-rolled steel sheet with excellent workability and crashworthiness and tensile strength of 980 MPa or more, and its manufacturing method
JP6554396B2
Steel sheet and manufacturing method therefor
WO2020080407A1
High-strength steel sheet having excellent moldability and impact resistance, and method for manufacturing high-strength steel sheet having excellent moldability and impact resistance
WO2020121418A1