Alumina powder, resin composition, heat dissipation part, and method for producing coated alumina particles

Coated alumina particles with controlled sphericity and aluminum nitride coating address the viscosity and thermal conductivity issues of alumina particles, achieving high thermal conductivity and moldability in resin compositions.

JP7572356B2Active Publication Date: 2024-10-23DENKA CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021522835
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-30
Filing Date
2020-05-27
Publication Date
2024-10-23
Estimated Expiration
2040-05-27

AI Technical Summary

Technical Problem

Existing alumina particles with high specific surface area and distorted shapes lead to increased viscosity when filled into resins, resulting in low moldability and thermal conductivity of heat dissipation components.

Method used

Development of alumina powder with coated alumina particles having a specific projected area circle equivalent diameter, average sphericity, and a coating layer of aluminum nitride to suppress viscosity increase and enhance thermal conductivity.

Benefits of technology

The alumina powder effectively reduces resin viscosity and enhances thermal conductivity, enabling efficient formation of thermal paths and improved heat dissipation components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572356000002
    Figure 0007572356000002
  • Figure 0007572356000001
    Figure 0007572356000001
Patent Text Reader

Abstract

The purpose of the present invention is to provide alumina particles which are capable of suppressing an increase in viscosity when included in a resin, and which make a resin composition containing the resin highly heat conductive. An alumina powder according to the present invention contains coated alumina particles that each comprise an alumina particle and a coating layer coating the alumina particle, and that each have a projected area equivalent circle diameter of 1 µm or greater as determined by microscopy. The coating layer contains aluminum nitride, and the average sphericity of the coated alumina particles is 0.85 to 0.97.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an alumina powder, a resin composition, a heat dissipation part, and a method for producing coated alumina particles. [Background technology]

[0002] In recent years, electrical devices have become smaller and more powerful. As a result of this miniaturization and higher performance, the packaging density of electronic components that make up the electrical devices has increased, increasing the need to effectively dissipate heat generated by the electronic components.

[0003] In addition, in power device applications such as electric vehicles that can reduce environmental load, high voltages may be applied to electronic components or large currents may flow. In this case, a large amount of heat is generated, and in order to deal with the large amount of heat generated, there is an increasing demand for more effective heat release than before. As a technology to meet such demands, for example, Patent Document 1 discloses a resin composition containing three types of alumina fillers. In addition, Patent Document 2 discloses alumina blend particles containing spherical alumina particles and non-spherical alumina particles, and a resin composition containing the particles. Furthermore, Patent Document 3 discloses aluminum nitride particles as a thermally conductive filler, which include a core made of at least one of alumina and aluminum oxynitride, and a surface layer made of aluminum nitride having a thickness of 1.1 μm or more formed on the surface of the core. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2009-164093 A [Patent Document 2] JP 2009-274929 A [Patent Document 3] JP 2012-41253 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in Patent Documents 1 and 2, the alumina particles have a high specific surface area, low average sphericity, and distorted shape, so that the resin thickens when filled with the alumina particles, making it difficult to fill the resin with the alumina particles at a high ratio. As a result, the moldability is low and the thermal conductivity of the resulting heat dissipation component is also low.

[0006] In addition, in Patent Document 3, aluminum nitride particles are obtained by microwave irradiation, but this manufacturing method does not allow spherical particles to be obtained. Therefore, as described above, the aluminum nitride particles described in Patent Document 3 also have a poor shape, so there is a problem that the resin thickens when filled with the aluminum nitride particles, making it difficult to highly fill the resin with the aluminum nitride particles. In the end, even if the aluminum nitride particles described in Patent Document 3 are used, the moldability is low and the thermal conductivity of the obtained heat dissipation part is low.

[0007] The present invention has been made in consideration of such problems, and aims to provide an alumina powder containing specific coated alumina particles that can suppress an increase in viscosity when filled into a resin and can achieve high thermal conductivity in a resin composition containing the resin, as well as a resin composition, a heat dissipation part, and a method for producing coated alumina particles that contain the alumina powder. [Means for solving the problem]

[0008] As a result of extensive research to achieve the above-mentioned object, the inventors have discovered that an alumina powder containing specific coated alumina particles can suppress an increase in viscosity when filled into a resin, and that by containing this alumina powder, a resin composition and a heat dissipation part can be obtained that can achieve high thermal conductivity, and have thus completed the present invention.

[0009] That is, the present invention is as follows. [1] An alumina powder containing coated alumina particles having alumina particles and a coating layer coating the alumina particles, the coated alumina particles having a projected area equivalent circle diameter measured by a microscope of 1 μm or more and 300 μm or less, the coating layer containing aluminum nitride, and the coated alumina particles having an average sphericity of 0.85 or more and 0.97 or less. [2] The alumina powder according to [1], wherein the alumina powder has a plurality of peaks in a particle size range of 2 μm or more and 200 μm or less in a volume-based frequency particle size distribution measured by a laser diffraction scattering method. [3] The alumina powder according to [1] or [2], wherein the proportion of the coated alumina particles having a sphericity of 0.80 or less is 15% or less on a number basis. [4] The alumina powder according to any one of [1] to [3], wherein the average particle size of the coated alumina particles is 30 μm or more and 150 μm or less, as measured by a laser diffraction / scattering particle size distribution measuring device. [5] The alumina powder according to any one of [1] to [4], wherein the content of aluminum nitride in the coated alumina particles is 10% by mass or more and 40% by mass or less.

[0010] [6] The alumina powder according to any one of [1] to [5], wherein the total content of alumina and aluminum nitride in the alumina powder is 80 mass % or more. [7] The alumina powder according to any one of [1] to [6], wherein the amount of carbon in the coated alumina particles is 0.3 mass % or less. [8] A resin composition comprising a resin and the alumina powder according to any one of [1] to [7]. [9] The resin composition according to [8], wherein the resin includes at least one selected from the group consisting of a silicone resin, an epoxy resin, a urethane resin, and an acrylic resin.

[0011]

[10] A heat dissipation part comprising the alumina powder according to any one of [1] to [7], or the resin composition according to [8] or [9].

[11] The method for producing a coated alumina powder according to [1], comprising: a first step of sintering a mixture containing raw material alumina powder and carbon powder at a temperature of 1500°C or more and 1700°C or less in a reducing atmosphere containing nitrogen gas to obtain a first sintered powder; and a second step of further sintering the first sintered powder at a temperature of 600°C or more and 900°C or less in an air atmosphere to obtain the coated alumina particles, wherein the carbon powder has an average particle size of 30 nm or more and 70 nm or less and a bulk density of 0.10 g / cm. 3 More than 0.20g / cm 3 The specific surface area is 20m or less. 2 / g or more 60m 2 / g or less. Effect of the Invention

[0012] According to the present invention, it is possible to provide an alumina powder that can suppress an increase in viscosity when filled into a resin and can achieve high thermal conductivity in a resin composition containing the resin, as well as a resin composition, a heat dissipation part, and a method for producing coated alumina particles that contain the alumina powder. [Brief description of the drawings]

[0013] [Figure 1] 1 is an image of a cross-sectional EPMA analysis of the coated alumina particles according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment for carrying out the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. Note that the following present embodiment is an example for explaining the present invention, and the present invention is not limited to only this embodiment.

[0015] [Alumina powder] The alumina powder of this embodiment contains one or more types of coated alumina particles according to this embodiment described later. The alumina powder of this embodiment may contain a filler other than the coated alumina particles, particularly an inorganic filler, as described later. When the alumina powder of this embodiment contains a filler other than the coated alumina particles and a filler other than the inorganic filler, it should be referred to as a simple powder rather than an alumina powder. Furthermore, when the alumina powder of this embodiment contains an inorganic filler other than the coated alumina particles (but does not contain a filler other than the inorganic filler), it should be referred to as an inorganic powder. However, in this specification, "alumina powder" is used as a concept that includes them.

[0016] (Coated alumina particles) The coated alumina particles according to this embodiment have alumina particles and a coating layer containing aluminum nitride that coats the alumina particles, and have a projected area equivalent circle diameter measured by a microscope of 1 μm to 300 μm and an average sphericity of 0.85 to 0.97. Hereinafter, unless otherwise specified, the coated alumina particles according to this embodiment will also be simply referred to as "coated alumina particles".

[0017] The coated alumina particles are derived from alumina particles contained in a raw material alumina powder (hereinafter simply referred to as "raw alumina powder") which will be described later.

[0018] By using the alumina powder of this embodiment, which contains coated alumina particles containing aluminum nitride in the coating layer, in a resin composition and a heat dissipating part, the thermal conductivity of the resin composition and the heat dissipating part is particularly increased, in combination with the average sphericity being set to a predetermined numerical range, as described below. The coating layer may contain unavoidable components such as aluminum oxynitride that are generated in the process of generating the coating layer.

[0019] The thickness of the coating layer according to this embodiment is preferably 0.8 μm or more and 12 μm or less, and more preferably 1.5 μm or more and 7.5 μm or less, because the viscosity increase during filling into the resin can be suppressed favorably, or the resin composition containing the resin can be more highly thermally conductive. When using an alumina powder in which the thickness of the coating layer in the coated alumina particles is within the above range, the heat path can be efficiently formed, and the heat tends to be sufficiently conducted. The thickness of the coating layer is measured by the method described in the examples.

[0020] The coated alumina particles according to this embodiment have a projected area circle equivalent diameter of 1 μm or more and 300 μm or less, and an average sphericity of 0.85 or more and 0.97 or less, as measured by the following microscopy method. If the coated alumina particles are spherical and have an average sphericity within the above range, the resin is less likely to thicken when filled with the coated alumina particles. By including the coated alumina particles in the alumina powder according to this embodiment, it is possible to fill the resin with the alumina powder at a high ratio. As a result, a heat path can be efficiently and satisfactorily formed in the resin, and a resin composition and a heat dissipation part having high thermal conductivity can be obtained. The average sphericity is preferably 0.87 or more and 0.96 or less, more preferably 0.89 or more and 0.95 or less, in terms of a reduction in frictional resistance when filled in the resin and an increase in the contact area between the particles. By including coated alumina particles having the average sphericity in the above range, the alumina powder of the present embodiment can improve the fluidity of the alumina powder including the coated alumina particles in the resin, reduce the frictional resistance with the resin, and suppress the increase in viscosity when the alumina powder is filled into the resin. In addition, the contact between the alumina particles including the coated alumina particles becomes more sufficient and the contact area becomes larger, which results in efficient formation of a heat path, and therefore tends to result in a resin composition and a heat dissipation part with higher thermal conductivity. The average sphericity is measured, for example, by the following microscopic method. That is, particle images taken with a scanning electron microscope, a transmission electron microscope, or the like are input into an image analyzer, and the projected area (A) and perimeter (PM) of the particle are measured from the photograph. If the area of ​​a perfect circle having the same perimeter as the perimeter (PM) is (B), the sphericity of the particle is A / B. Therefore, assuming a perfect circle having the same perimeter as the perimeter (PM) of the sample, PM=2πr, B=πr 2 Therefore, B = π × (PM / 2π) 2 The sphericity of each particle is given by: Sphericity = A / B = A × 4π / (PM) 2 The sphericity of any 200 particles having a projected area circle equivalent diameter of 1 μm or more and 300 μm or less is determined as above, and the arithmetic mean value is taken as the average sphericity. The specific measurement method is as described in the Examples. The projected area circle equivalent diameter refers to the diameter of a perfect circle having the same projected area as the projected area (A) of the particle.

[0021] In the coated alumina powder of this embodiment, the ratio of coated alumina particles having a sphericity of 0.80 or less is preferably 15% or less by number, more preferably 10% or less by number. The ratio of coated alumina particles having a sphericity of 0.80 or less by number of 15% or less means that the alumina powder contains coated alumina particles with fewer coalescence particles and cracked particles that cause thickening when the alumina powder is filled into a resin, and is therefore preferable. In addition, there is a tendency to reduce wear of the device and the mold. The ratio of the coated alumina particles is, for example, 0.5% or more by number. In addition, the projected area circle equivalent diameter measured by a microscope is usually 200 μm or less.

[0022] In the coated alumina powder of this embodiment, the ratio of coated alumina particles having a sphericity of more than 0.80 and not more than 0.83 is preferably 10% or less by number, more preferably 5% or less by number. The ratio of coated alumina particles having a sphericity in the above range of 10% or less means that the alumina powder contains coated alumina particles with fewer coalescence particles and cracked particles that cause thickening when the alumina powder is filled into a resin, and is therefore preferable in that respect. In addition, there is a tendency to reduce wear of the device and the mold. The ratio of the coated alumina particles is, for example, 0.5% or more by number. In addition, the projected area circle equivalent diameter measured by a microscope is usually 200 μm or less.

[0023] The coated alumina particles according to this embodiment tend to have better contact between alumina powders containing the coated alumina particles, and thus a heat path can be efficiently and well formed, resulting in a resin composition and a heat dissipation component with higher thermal conductivity. Furthermore, from the viewpoint of surface smoothness when the resin composition is prepared, the average particle size is preferably 30 μm or more and 150 μm or less, more preferably 30 μm or more and 130 μm or less, and more preferably 40 μm or more and 120 μm or less. When the average particle size is 30 μm or more, the heat path can be formed more efficiently in the resin composition and the heat dissipation component, and the heat tends to be conducted more sufficiently. In addition, when the average particle size is 150 μm or less, the surface smoothness of the heat dissipation component is further improved, and the thermal resistance at the interface between the heat dissipation component and the heat source is reduced, so that the thermal conductivity tends to be more sufficiently improved. In this embodiment, the particle size and the average particle size are measured by a laser diffraction scattering type particle size distribution measuring instrument. The specific measurement method is as described in the examples.

[0024] The content of aluminum nitride in the coated alumina particles according to the present embodiment is preferably 10% by mass or more and 40% by mass or less, and more preferably 15% by mass or more and 35% by mass or less, since the resin composition can be more highly thermally conductive. When coated alumina particles having an aluminum nitride content within the above range are used, the heat path can be formed more efficiently, and the heat tends to be conducted more sufficiently. When the content is 10% by mass or more, the coating layer of aluminum nitride becomes thicker, and the effect of improving the thermal conductivity by coating with aluminum nitride tends to be further enhanced. When the content is 40% by mass or less, the fine unevenness of the coating layer can be further reduced, and the moldability of the resin composition and the heat dissipation component is further improved, and the voids in the heat dissipation component tend to be further reduced. The content of aluminum nitride is measured by the method described in the examples.

[0025] The carbon content in the coated alumina particles according to the present embodiment is preferably 0.3% by mass or less, more preferably 0.2% by mass or less, and even more preferably 0.1% by mass or less. The carbon content in the coated alumina particles is, for example, 0.01% by mass or more. When the carbon content is within the above range, the resin composition and heat dissipation part having high insulation and thermal conductivity can be obtained more effectively and reliably because the carbon content, which is a conductive material, is reduced as much as possible. The carbon content in the coated alumina particles is measured by the method described in the examples. The carbon in the coated alumina particles is mainly derived from the carbon powder mixed with the raw alumina powder. The carbon powder is used when producing the coated alumina particles according to the present embodiment, as described later in the method for producing the coated alumina particles.

[0026] The specific surface area of ​​the coated alumina particles according to this embodiment is 0.02 m 2 / g or more 0.15m 2 / g or less, and 0.03m 2 / g or more 0.12m 2 / g or less is more preferable. When the specific surface area is in the above range, it is easy to suppress the increase in viscosity when the alumina powder containing the specific coated alumina particles is filled into the resin, and it is possible to obtain a resin composition and a heat dissipation part having higher thermal conductivity. In this embodiment, the specific surface area is measured by the BET flow method, and the specific measurement method is as described in the examples.

[0027] (Alumina powder) In the alumina powder of this embodiment, the total content of alumina and aluminum nitride is preferably 80% by mass or more, more preferably 85% by mass or more, even more preferably 90% by mass or more, and even more preferably 99% by mass or more. The upper limit of the total content is, for example, 100% by mass. Alumina powder having a total content of alumina and aluminum nitride within the above range has even less unavoidable components such as aluminum oxynitride that tend to block heat paths, so that it tends to be possible to obtain a resin composition and a heat dissipation part with higher thermal conductivity. The total content of alumina and aluminum nitride is measured by the method described in the examples.

[0028] The alumina powder of this embodiment preferably has multiple peaks in the particle size range of 2 μm or more and 200 μm or less in the volume-based frequency particle size distribution by the laser diffraction scattering method. As a result, the alumina powder of this embodiment can be efficiently filled into the resin to form a heat path, achieve high thermal conductivity, and further suppress the increase in viscosity of the resin composition. Here, in this embodiment, the peak refers to a maximum point detected in the particle size range of 0.01 μm or more and 3500 μm or less in the volume-based frequency particle size distribution by the laser diffraction scattering method, which is divided into 100. In addition, if there is a shoulder in the detected peak, the shoulder is also counted as a peak. The shoulder is detected by the curvature of the peak given by the second derivative coefficient, and means that there is an inflection point in the peak, that is, that there are more particle components of a specific particle size.

[0029] The alumina powder of this embodiment has one or more peaks derived from the coated alumina particles in a particle size range of 0.01 μm or more and 3500 μm or less in a volume-based frequency particle size distribution measured by a laser diffraction scattering method. The alumina powder of this embodiment may have multiple peaks derived from the coated alumina particles of this embodiment in a particle size range of 0.01 μm or more and 3500 μm or less in a volume-based frequency particle size distribution measured by a laser diffraction scattering method.

[0030] An alumina powder having such a particle size distribution can be obtained by, for example, containing two or more types of coated alumina particles each having one peak in the above particle size range and having different average particle sizes.

[0031] Furthermore, the alumina powder of this embodiment may contain a filler other than the coated alumina particles of this embodiment. Even in this case, usually, in the volume-based frequency particle size distribution by the laser diffraction scattering method, two or more peaks are detected in the particle size range of 0.01 μm or more and 3500 μm or less, namely, a peak derived from the coated alumina particles of this embodiment and a peak derived from a filler other than the coated alumina particles. Examples of the filler include inorganic fillers. Specifically, examples of the filler include coated alumina particles other than the coated alumina particles of this embodiment, alumina particles not having a coating layer (i.e., uncoated), magnesia, aluminum nitride, silicon nitride, yttrium oxide, boron nitride, calcium oxide, iron oxide, and boron oxide. Note that the alumina powder of this embodiment includes inorganic materials other than alumina, such as aluminum nitride, as described above, and in this respect corresponds to an inorganic powder.

[0032] The coated alumina particles other than the coated alumina particles include, for example, coated alumina particles having a coating layer that coats the alumina particles and a projected area equivalent circle diameter measured by a microscope of less than 1 μm. In this case, the coating layer may be, for example, aluminum nitride or silicon nitride.

[0033] In addition, the coated alumina particles other than the coated alumina particles according to the present embodiment include coated alumina particles having a coating layer that coats the alumina particles, a projected area equivalent circle diameter measured by a microscope of 1 μm to 300 μm, and the coating layer does not contain aluminum nitride. In this case, the coating layer may be, for example, silicon nitride.

[0034] These fillers may be fillers that have been surface-treated with a known silane coupling agent or the like. The alumina powder of the present embodiment may contain one or more of these fillers in addition to the coated alumina particles of the present embodiment.

[0035] In the alumina powder of this embodiment, the content of the coated alumina particles according to this embodiment is preferably 20% by volume or more and 80% by volume or less, and more preferably 25% by volume or more and 75% by volume or less, based on the total amount of the alumina powder. In this embodiment, when the alumina powder contains two or more types of coated alumina particles according to this embodiment having different average particle sizes, the content of the coated alumina particles is the total amount of the coated alumina particles. By containing the coated alumina particles within the above range, the alumina powder according to this embodiment can further suppress the increase in viscosity when filled into a resin, and can further realize high thermal conductivity of a resin composition containing the resin.

[0036] In the alumina powder of this embodiment, from the viewpoint of improving thermal conductivity, the total content of the coated alumina particles according to this embodiment, coated alumina particles other than the coated alumina particles according to this embodiment, and uncoated alumina particles (hereinafter referred to as "coated alumina particles, etc.") relative to the total amount of the alumina powder is preferably 80 volume % or more and 100 volume % or less, and more preferably 85 volume % or more and 100 volume % or less. By containing the coated alumina particles, etc. within the above range, the alumina powder of this embodiment exhibits the effect of increasing the thermal conductivity of the resin composition.

[0037] The alumina powder of the present embodiment preferably has a plurality of peaks, i.e., two or more peaks, more preferably two or more and four or less peaks, and even more preferably three peaks, in the particle size range of 2 μm to 200 μm in particle size, as described above. For each peak, in the volume-based frequency particle size distribution by the laser diffraction scattering method, the particle having the first peak detected from the fine particle side (i.e., the 0.01 μm side) in the particle size range of 0.01 μm to 3500 μm in particle size is called the first particle, the particle having the second peak is called the second particle, and the particle having the nth peak is called the nth particle. That is, the number of peaks detected is n. The detected particles may be only the coated alumina particles according to the present embodiment, or may be a filler other than the coated alumina particles in addition to the coated alumina particles. However, the filler other than the coated alumina particles according to the present embodiment is preferably one or more of the coated alumina particles other than the coated alumina particles according to the present embodiment and the uncoated alumina particles.

[0038] In the alumina powder of this embodiment, when the number of peaks n is 2, the position of the peak derived from the first particle is preferably detected in the particle size range of 3 μm to 15 μm, and the position of the peak derived from the second particle is preferably detected in the particle size range of 30 μm to 150 μm. In addition, it is preferable that the second particle is the coated alumina particle according to this embodiment, and in addition, it is more preferable that the first particle is an uncoated alumina particle. The content of the first particles in the alumina powder of this embodiment is 25% by volume or more and 55% by volume or less, preferably 30% by volume or more and 50% by volume or less, and more preferably 35% by volume or more and 45% by volume or less, from the viewpoint of suppressing the increase in viscosity of the resin composition. The content of the second particles is 45% by volume or more and 75% by volume or less, preferably 50% by volume or more and 70% by volume or less, and more preferably 55% by volume or more and 65% by volume or less, from the viewpoint of suppressing the increase in viscosity of the resin composition. The total of the first particles and the second particles is 100% by volume. The average particle size of the first particles is preferably 4.0 μm or more and 12 μm or less, and more preferably 5.0 μm or more and 10 μm or less, from the viewpoint of suppressing an increase in viscosity of the resin composition. The average particle size of the second particles is preferably 35 μm or more and 140 μm or less, and more preferably 40 μm or more and 130 μm or less, from the viewpoint of suppressing an increase in viscosity of the resin composition.

[0039] When the number of peaks n is 3, it is preferable that the position of the peak derived from the first particle is detected in the particle size range of 0.3 μm or more and 1.0 μm or less, the position of the peak derived from the second particle is detected in the particle size range of 3.0 μm or more and 15 μm or less, and the position of the peak derived from the third particle is detected in the particle size range of 30 μm or more and 150 μm or less. The content of the first particles in the alumina powder of this embodiment is 10% by volume or more and 25% by volume or less, preferably 12% by volume or more and 18% by volume or less, and more preferably 13% by volume or more and 17% by volume or less. The content of the second particles is 20% by volume or more and 55% by volume or less, preferably 25% by volume or more and 41% by volume or less, and more preferably 30% by volume or more and 39% by volume or less. Furthermore, the content of the third particles is 35% by volume or more and 55% by volume or less, preferably 47% by volume or more and 57% by volume or less, and more preferably 48% by volume or more and 53% by volume or less. When the content of each particle is within the above range, the alumina powder can be filled in the resin at a high rate, and is preferable from the viewpoint of suppressing the viscosity increase of the resin composition. The total of the first particles, the second particles, and the third particles is 100% by volume.

[0040] In this case, the average particle diameter of the first particles is preferably 0.3 μm or more and 1.0 μm or less, more preferably 0.4 μm or more and 0.9 μm or less, and more preferably 0.5 μm or more and 0.8 μm or less. When the average particle diameter of the first particles is 0.3 μm or more, the gaps between the particles are efficiently filled, the thermal conductivity can be improved, and the effect of suppressing the increase in viscosity of the resin composition tends to be obtained. In addition, when the average particle diameter of the first particles is 1.0 μm or less, the number of particles tends to increase and the number of heat paths between the particles tends to increase when the content of the first particles is about the same, compared to when the average particle diameter exceeds 1.0 μm. On the other hand, when the average particle diameter exceeds 1.0 μm, the number of heat paths between the particles tends to decrease. In addition, when the average particle diameter exceeds 1.0 μm, the heat conduction within the first particles is fast, but the heat conduction in the few heat paths becomes rate-limiting, and the heat conductivity when viewed as a whole powder tends to be low. However, when the average particle size is 1.0 μm or less, the particle size of each particle is small and the number of thermal paths is large, so that a large difference is unlikely to occur between the thermal conduction within the first particle and the thermal conduction in the thermal paths between particles, and as a result of the high uniformity of thermal conduction, the thermal conductivity tends to be high.

[0041] From the viewpoint of suppressing the increase in viscosity of the resin composition, the average particle size of the second particles is preferably 3.0 μm or more and 15 μm or less, more preferably 4.0 μm or more and 12 μm or less, and even more preferably 5.0 μm or more and 10 μm or less. When the average particle size of the second particles is within the above range, the second particles are efficiently filled into the gaps between the particles, the thermal conductivity can be improved, and the effect of suppressing the increase in viscosity of the resin composition tends to be obtained.

[0042] From the viewpoint of suppressing the increase in viscosity of the resin composition, the average particle diameter of the third particles is preferably 30 μm or more and 140 μm or less, more preferably 35 μm or more and 135 μm or less, even more preferably 45 μm or more and 130 μm or less, and even more preferably 60 μm or more and 120 μm or less. When the average particle diameter of the third particles is 30 μm or more, the particles can efficiently form a heat path by contact with each other, so that the thermal conductivity tends to be improved. Furthermore, the specific surface area of ​​the particles tends to be reduced, so that the filling rate can be increased. In addition, when the average particle diameter of the third particles is 140 μm or less, the surface smoothness of the obtained heat dissipation component can be maintained, and further, the contact resistance of the particle interface can be reduced, so that the thermal conductivity tends to be increased.

[0043] In addition, the average sphericity of the first particles is preferably 0.82 or more and 0.94 or less, and more preferably 0.84 or more and 0.92 or less, from the viewpoints of reducing frictional resistance when filled into a resin and increasing the contact area between particles. The average sphericity of the second particles is preferably 0.82 or more and 0.94 or less, and more preferably 0.84 or more and 0.92 or less, from the viewpoints of reducing frictional resistance when filled in a resin and increasing the contact area between particles. The average sphericity of the third particles is preferably 0.82 or more and 0.94 or less, and more preferably 0.84 or more and 0.92 or less, from the viewpoints of reducing frictional resistance when filled in a resin and increasing the contact area between particles.

[0044] The content of the α crystal phase in the first particles is preferably 80% by mass or more, and more preferably 90% by mass or more, from the viewpoint of improving thermal conductivity. The upper limit is, for example, 100% by mass. The content of the α crystal phase in the second particles is preferably 80% by mass or more, and more preferably 90% by mass or more, from the viewpoint of improving thermal conductivity. The upper limit is, for example, 100% by mass. The content of the α crystal phase in the third particles is preferably 80% by mass or more, and more preferably 90% by mass or more, from the viewpoint of improving thermal conductivity. The upper limit is, for example, 100% by mass.

[0045] In this embodiment, the first particles are preferably uncoated alumina particles from the viewpoint of further improving flowability. As the second particles, from the viewpoint of improving fluidity and thermal conductivity, uncoated alumina particles, coated alumina particles other than the coated alumina particles according to this embodiment, and coated alumina particles according to this embodiment are preferable, and uncoated alumina particles are more preferable. From the viewpoint of improving thermal conductivity, the third particles are preferably the coated alumina particles according to this embodiment, uncoated alumina particles, and coated alumina particles other than the coated alumina particles according to this embodiment, and are more preferably the coated alumina particles according to this embodiment. The uncoated alumina particles include, for example, spherical alumina particles.

[0046] When the number of peaks n is 4, it is preferable that the position of the peak derived from the first particle is detected in the particle size range of 0.05 μm or more and 0.2 μm or less, the position of the peak derived from the second particle is detected in the particle size range of 0.3 μm or more and 1.0 μm or less, the position of the peak derived from the third particle is detected in the particle size range of 3.0 μm or more and 15 μm or less, and the position of the peak derived from the fourth particle is detected in the particle size range of 30 μm or more and 150 μm or less. In the alumina powder of this embodiment, from the viewpoint of suppressing the increase in viscosity of the resin composition, it is more preferable that the position of the peak derived from the first particle is detected in the particle size range of 0.07 μm to 0.1 μm, the position of the peak derived from the second particle is detected in the particle size range of 0.4 μm to 0.9 μm, the position of the peak derived from the third particle is detected in the particle size range of 4.0 μm to 12 μm, and the position of the peak derived from the fourth particle is detected in the particle size range of 35 μm to 140 μm. It is also preferable that the fourth particle is the coated alumina particle according to this embodiment, and in addition, it is more preferable that the first particle, the second particle, and the third particle are uncoated alumina particles.

[0047] The content of the first particles in the alumina powder of this embodiment is 0.5 vol% or more and 5.0 vol% or less, preferably 1.0 vol% or more and 4.0 vol% or less, and more preferably 1.5 vol% or more and 3.0 vol% or less, from the viewpoint of suppressing the viscosity increase of the resin composition. The content of the second particles is 9 vol% or more and 20 vol% or less, preferably 11 vol% or more and 18 vol% or less, and more preferably 12 vol% or more and 17 vol% or less, from the viewpoint of suppressing the viscosity increase of the resin composition. The content of the third particles is 19 vol% or more and 45 vol% or less, preferably 24 vol% or more and 41 vol% or less, and more preferably 29 vol% or more and 39 vol% or less, from the viewpoint of suppressing the viscosity increase of the resin composition. The content of the fourth particles is 43 vol% or more and 60 vol% or less, preferably 45 vol% or more and 57 vol% or less, and more preferably 46 vol% or more and 53 vol% or less, from the viewpoint of suppressing the viscosity increase of the resin composition. The total volume of the first particles, the second particles, the third particles, and the fourth particles is 100% by volume.

[0048] In addition, the average particle diameter of the first particles is preferably 0.05 μm or more and 0.2 μm or less, and more preferably 0.07 μm or more and 0.1 μm or less, from the viewpoint of suppressing the viscosity increase of the resin composition. The average particle diameter of the second particles is preferably 0.3 μm or more and 1.0 μm or less, and more preferably 0.4 μm or more and 0.9 μm or less, from the viewpoint of suppressing the viscosity increase of the resin composition. The average particle diameter of the third particles is preferably 3.0 μm or more and 15 μm or less, and more preferably 4.0 μm or more and 12 μm or less, from the viewpoint of suppressing the viscosity increase of the resin composition. The average particle diameter of the fourth particles is preferably 30 μm or more and 150 μm or less, and more preferably 35 μm or more and 140 μm or less, from the viewpoint of suppressing the viscosity increase of the resin composition.

[0049] In this embodiment, the total content of all the first to nth particles in the alumina powder is preferably 98% by volume or more, and more preferably 99% by volume or more, from the viewpoint of improving thermal conductivity. The upper limit of the content is 100% by volume.

[0050] (Method of manufacturing coated alumina particles) The method for producing the coated alumina particles according to the present embodiment includes a first step of sintering a mixture containing raw alumina powder and carbon powder at a temperature of 1500°C to 1700°C in a reducing atmosphere containing nitrogen gas to obtain a first sintered powder, and a second step of further sintering the first sintered powder at a temperature of 600°C to 900°C in an air atmosphere to obtain the coated alumina particles according to the present embodiment. This production method can obtain coated alumina particles that contain aluminum nitride in the coating layer and have a predetermined high average sphericity. By including the coated alumina particles according to the present embodiment, thickening can be suppressed, and a resin composition and a heat dissipation part having high thermal conductivity can be obtained. The method will be described in detail below.

[0051] In the first step, a predetermined mixer is used to mix the raw alumina powder and the carbon powder to a predetermined mixing ratio. The mixing method is not particularly limited as long as the raw alumina powder and the carbon powder can be mixed uniformly, and either wet mixing or dry mixing may be used. An example of such a mixing method is ball mill mixing. The mixing ratio of the raw alumina powder and the carbon powder is preferably 10 parts by mass or more and 50 parts by mass or less of the carbon powder, and more preferably 15 parts by mass or more and 45 parts by mass or less, per 100 parts by mass of the raw alumina powder, in consideration of the stoichiometric mixing ratio of the raw alumina powder and the carbon powder, from the viewpoint of forming a reaction atmosphere.

[0052] As the raw alumina powder, various alumina particles having, for example, α, γ, θ, and η crystal structures can be used. The alumina particles are usually spherical. Specifically, the average sphericity of the alumina particles contained in the raw alumina powder and having a projected area circle equivalent diameter of 1 μm or more and 300 μm or less by the above-mentioned microscopic method is usually 0.90 or more, preferably 0.91 or more and 0.99 or less, and more preferably 0.92 or more and 0.98 or less. The upper limit of the average sphericity is, for example, 1.00. By having the average sphericity in the above range, the raw alumina powder and the carbon powder are mixed more uniformly, and the reaction is promoted.

[0053] The average particle diameter of the raw material alumina powder is preferably 25 μm or more and 140 μm or less, and more preferably 30 μm or more and 130 μm or less, because if the average particle diameter is larger than that of the carbon powder described below, the above-mentioned carbon reduction-nitridation reaction proceeds more easily.

[0054] The specific surface area of ​​the raw alumina powder is 0.03 m 2 / g or more 0.30m 2 / g or less, and 0.05m 2 / g or more 0.25m 2 When the specific surface area is within the above range, the raw material alumina powder and carbon powder are mixed more uniformly, and the reaction is promoted.

[0055] The carbon powder according to this embodiment has an average particle size of 30 nm or more and 70 nm or less and a bulk density of 0.10 g / cm 3 More than 0.20g / cm 3 The specific surface area is 20m or less. 2 / g or more 60m 2 By using such carbon powder, the carbon powder adheres to the surfaces of the alumina particles in a large amount, and in the reaction between the raw material alumina powder and nitrogen at high temperatures, the carbon powder acts as a spacer to suppress adhesion between the alumina particles, thereby making it possible to suitably produce coated alumina particles with high sphericity.

[0056] The average particle size of the carbon powder is preferably 35 nm or more and 65 nm or less from the viewpoint of improving the effect of preventing adhesion between alumina particles.

[0057] The bulk density of the carbon powder is 0.10 g / cm 3 More than 0.20g / cm 3 Less than or equal to 0.12 g / cm 3 More than 0.18g / cm 3 It is preferable that the bulk density is not more than 1000 g / mol. When the bulk density is in the above range, the carbon powder adheres more uniformly to the surface of the alumina particles, and the reaction is promoted. In this embodiment, the bulk density is measured by the method described in the Examples.

[0058] Furthermore, the specific surface area of ​​carbon powder is 20m 2 / g or more 60m 2 / g or less, 25m 2 / g or more 55m 2 When the specific surface area is in the above range, an effect of preventing adhesion between alumina particles is improved.

[0059] The carbon powder preferably has a total pore volume of 1 mL / g or more and 4 mL / g or less, and more preferably 1.5 mL / g or more and 3 mL / g or less. When the total pore volume is in the above range, nitrogen gas can easily penetrate into the carbon, and the above-mentioned carbon reduction-nitridation reaction can more easily proceed in the carbon powder. In this embodiment, the total pore volume is measured by the method described in the Examples.

[0060] Examples of carbon powders include carbon blacks such as acetylene black, furnace black, and thermal black, and powdered graphite. As the carbon powder, acetylene black is preferred in terms of purity and the like.

[0061] In the first step, the mixture is fired in a reducing atmosphere containing nitrogen gas at a temperature of 1500° C. to 1700° C. to obtain a first fired powder. The formation of a coating layer containing aluminum nitride on the surface of the raw alumina powder proceeds based on the following formula showing a carbon-reduction-nitridation reaction. Al 2 O 3 +3C+N 2 →2AlN+3CO The gas reducing atmosphere containing nitrogen gas can be obtained, for example, by using a reducing atmosphere furnace in which oxygen and moisture are removed by circulating the gas through a refining device. In addition, the gas may contain inevitable components such as carbon dioxide gas in addition to nitrogen gas.

[0062] During firing of the mixture, it is preferable to supply nitrogen gas to the mixture at a rate of 1 L / min to 10 L / min in terms of reaction promotion and productivity, and more preferably at a rate of 3 L / min to 7 L / min.

[0063] The firing temperature in the first step is preferably 1550° C. or more and 1650° C. or less in terms of controlling the coating layer and sphericity of the coated alumina particles according to this embodiment. In addition, the firing time is usually 4 hours or more and 12 hours or less in consideration of productivity. Note that the coating layer tends to become thicker as the amount of nitrogen gas increases, the firing temperature increases, and the firing time increases.

[0064] In the second step, the first calcined powder obtained in the first step is further calcined in an air atmosphere at a temperature of 600° C. to 900° C. to obtain coated alumina particles. By calcining the first calcined powder in the second step, the remaining carbon powder can be removed, and the coated alumina particles according to the present embodiment can be obtained. The firing temperature in the second step is preferably 650° C. or more and 850° C. or less from the viewpoint of controlling the carbon content of the coated alumina particles according to the present embodiment. In addition, the firing time is preferably 2 hours or more and 6 hours or less from the viewpoint of efficiently removing the carbon powder.

[0065] In the second step, when the first calcined powder is calcined, it is preferable to supply air to the first calcined powder at 1 L / min to 3 L / min from the viewpoint of controlling the carbon content of the coated alumina particles according to the present embodiment, and more preferably at 1.5 L / min to 2.5 L / min.

[0066] (Method of manufacturing alumina powder) The alumina powder according to the present embodiment may be obtained by using one type of coated alumina particles according to the present embodiment as it is. The alumina powder according to the present embodiment may also be obtained by appropriately mixing two or more types of coated alumina particles. Furthermore, the alumina powder according to the present embodiment may also be obtained by appropriately mixing at least one type of coated alumina particles according to the present embodiment with other fillers and the like. For example, ball mill mixing can be used as a mixing method.

[0067] [Resin composition and method for producing same] The resin composition according to the present embodiment includes at least a resin and the alumina powder according to the present embodiment. By including the alumina powder, the resin composition according to the present embodiment can suppress thickening and have high thermal conductivity.

[0068] (resin) As the resin, various polymer compounds such as thermoplastic resins and their oligomers, elastomers, etc. can be used, for example, epoxy resin, phenol resin, melamine resin, urea resin, unsaturated polyester, urethane resin, acrylic resin, and fluororesin; polyamide such as polyimide, polyamideimide, and polyetherimide; polyester such as polybutylene terephthalate and polyethylene terephthalate; polyphenylene sulfide, aromatic polyester, polysulfone, liquid crystal polymer, polyethersulfone, polycarbonate, maleimide-modified resin, ABS (acrylonitrile-butadiene-styrene) resin, AAS (acrylonitrile-acrylic rubber-styrene) resin, AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resin, EVA (ethylene-vinyl acetate copolymer) resin, and silicone resin can be used. These resins can be used alone or in a suitable mixture of two or more.

[0069] Among these resins, from the viewpoint of obtaining high heat dissipation characteristics, preferred are epoxy resins, phenol resins, urethane resins, acrylic resins, fluororesins, polyimides, polyphenylene sulfide, polycarbonates, ABS resins, and silicone resins, more preferred are silicone resins, epoxy resins, urethane resins, and acrylic resins, and even more preferred is silicone resin. As the silicone resin, it is preferable to use a rubber or gel obtained from a one-liquid or two-liquid addition reaction type liquid silicone having an organic group such as a methyl group and a phenyl group. Examples of such rubber or gel include "YE5822A Liquid / YE5822B Liquid (trade name)" manufactured by Momentive Performance Materials Japan LLC, and "SE1885A Liquid / SE1885B Liquid (trade name)" manufactured by Dow Corning Toray Co., Ltd.

[0070] (Alumina powder and resin content) In the resin composition of this embodiment, from the viewpoint of improving thermal conductivity, the content of the alumina powder according to this embodiment is preferably 67 volume % or more and 88 volume % or less, and more preferably 71 volume % or more and 85 volume % or less, relative to the total amount of the resin composition. Since the alumina powder according to this embodiment is unlikely to thicken even when filled into a resin, even if it is contained in the resin composition within the above range, it is possible to suppress thickening of the resin composition.

[0071] In the resin composition of the present embodiment, from the viewpoint of moldability of the resin composition, the content of the resin according to the present embodiment is preferably 12 volume % or more and 33 volume % or less, and more preferably 15 volume % or more and 29 volume % or less, relative to the total amount of the resin composition.

[0072] (Other Ingredients) In addition to the alumina powder and resin according to the present embodiment, the resin composition according to the present embodiment may contain inorganic fillers such as fused silica, crystalline silica, zircon, calcium silicate, calcium carbonate, silicon carbide, aluminum nitride, boron nitride, beryllia, and zirconia, as necessary, nitrogen-containing compounds such as melamine and benzoguanamine, oxazine ring-containing compounds, and phosphorus-based phosphate compounds, aromatic condensed phosphate esters, and halogen-containing condensed phosphate esters, and other flame-retardant compounds. Examples of additives include reaction retarders such as dimethyl maleate, curing agents, curing accelerators, flame retardant assistants, flame retardants, colorants, tackifiers, ultraviolet absorbers, antioxidants, fluorescent brighteners, photosensitizers, thickeners, lubricants, defoamers, surface conditioners, gloss agents, and polymerization inhibitors, as long as the properties of the present embodiment are not impaired. These components may be used alone or in appropriate mixtures of two or more. In the resin composition according to the present embodiment, the content of other components is usually 0.1% by mass or more and 5% by mass or less.

[0073] (Method of producing resin composition) The resin composition of the present embodiment can be produced, for example, by thoroughly stirring a resin, an alumina powder, and other components as necessary. The resin composition of the present embodiment can be produced, for example, by blending predetermined amounts of each component using a blender and a Henschel mixer, kneading the mixture using a heating roll, a kneader, and a single-screw or twin-screw extruder, cooling, and then pulverizing the mixture.

[0074] [Heat dissipation parts] The heat dissipation part according to the present embodiment includes the alumina powder or resin composition according to the present embodiment. The heat dissipation part according to the present embodiment can achieve high thermal conductivity, that is, can have high heat dissipation, by using the alumina powder or resin composition. Examples of the heat dissipation part include a heat dissipation sheet, a heat dissipation grease, a heat dissipation spacer, a semiconductor encapsulant, and a heat dissipation paint (heat dissipation coating agent).

[0075] The heat dissipation sheet is usually an insulating heat conductive sheet for removing heat generated from heat generating electronic components and electronic devices. The heat dissipation sheet is not particularly limited as long as it contains the alumina powder or resin composition according to the present embodiment. Examples of materials other than the alumina powder contained in the heat dissipation sheet of the present embodiment include silicone rubber. The heat dissipation sheet is mainly used by attaching it to a heat dissipation fin or a metal plate. The heat dissipation sheet can be obtained, for example, by forming the alumina powder according to the present embodiment and silicone rubber into a sheet shape by a method such as a solvent casting method or an extrusion film formation method. When forming into a sheet shape, it is preferable to defoam it. The thickness of the heat dissipation sheet is usually preferably 10 μm or more and 300 μm or less.

[0076] The heat dissipating grease is usually applied between a heat generating member and a heat dissipating member, and is used to efficiently conduct heat generated in the heat dissipating member to the heat dissipating member, thereby promoting heat dissipation. The heat dissipating grease is not particularly limited as long as it contains the alumina powder or resin composition of the present embodiment. Examples of materials other than the alumina powder contained in the heat dissipating grease of the present embodiment include organosilicon compounds such as silicone oil and hydrocarbon-based synthetic oils such as poly-α-olefin oil. The heat dissipating grease can be obtained, for example, by dispersing the alumina powder of the present embodiment in an organosilicon compound or a hydrocarbon-based synthetic oil to make it semi-solid. The heat dissipating grease may also be obtained by using a resin composition in which the alumina powder of the present embodiment is dispersed in an organosilicon compound or a hydrocarbon-based synthetic oil, and making the resin composition semi-solid.

[0077] The heat dissipation spacer is usually used to fill the space between the heat-generating electronic components and electronic devices and the case that houses them. By using this heat dissipation spacer, the heat generated from the heat-generating electronic components and electronic devices can be directly transferred to the case of the electronic device and dissipated. The heat dissipation spacer is not particularly limited as long as it contains the alumina powder or resin composition of this embodiment. Examples of materials other than the alumina powder contained in the heat dissipation spacer of this embodiment include silicone rubber. The heat dissipation spacer can usually be obtained by the same method as the heat dissipation sheet, but its thickness is thicker than that of the heat dissipation sheet.

[0078] The semiconductor encapsulant is used to remove heat generated from electronic components such as semiconductor elements and to protect the electronic components from external stimuli. The semiconductor encapsulant is not particularly limited as long as it contains the alumina powder or resin composition of the present embodiment. The semiconductor encapsulant can be produced, for example, by mixing the alumina powder or resin composition of the present embodiment with various known additives or solvents that are generally used in encapsulating material applications using a known mixer. The method of adding various components and solvents during mixing can be appropriately applied by generally known methods and is not particularly limited.

[0079] The heat dissipation paint is applied to mechanical parts, electrical products, and electrical parts having a heat source, and is used to enhance the heat dissipation of these parts. The heat dissipation paint is not limited as long as it contains the alumina powder or resin composition of this embodiment and a solvent. The alumina powder of this embodiment can suppress the increase in viscosity when the alumina powder is filled into the resin, so that it can maintain a suitable viscosity even in the solvent. Examples of the solvent include water, methyl ethyl ketone, methyl isobutyl ketone, ethyl acetate, propyl acetate, butyl acetate, cyclohexanone, ethylbenzene, xylene, methyl methacrylate, and 1-butanol. These solvents can be used alone or in an appropriate mixture of two or more. Examples of the mechanical parts include engines, boilers, blowers, and pumps. Examples of the electrical products include lighting, solar cell modules, and refrigerators. Examples of the electrical parts include circuit boards. EXAMPLES

[0080] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these examples in any way.

[0081] [Evaluation method] (1) Average sphericity and percentage of coated alumina particles The coated alumina particles were separated from the alumina powder using a sieve made of stainless steel test sieve conforming to the JIS standard with a mesh size of 53 μm. As in the above microscopy method, particle images taken with a scanning electron microscope (JSM-6301F manufactured by JEOL Ltd.) were imported into an image analyzer (MacView Ver.4 (product name) manufactured by Mountec Co., Ltd.), and the projected area (A) and perimeter (PM) of the particles were measured from the photograph. Using these values, the sphericity and its ratio of each particle were calculated, and the arithmetic mean value of the sphericity of each particle was taken as the average sphericity. For reference, an SEM image (500x) of the coated alumina particles according to this embodiment is shown in FIG. 1.

[0082] (2) Average particle size and particle size distribution (number of peaks) The average particle size and particle size distribution (number of peaks) were measured using a laser diffraction light scattering particle size distribution measuring device (Malvern, product name "Mastersizer 3000", wet dispersion unit: Hydro MV attached). In the measurement, water was used as the solvent, and dispersion treatment was performed for 2 minutes as a pretreatment by applying 200W output using an ultrasonic generator UD-200 (with ultra-micro tip TP-040 attached) (product name) manufactured by Tommy Seiko Co., Ltd. The particles after dispersion treatment were dropped into the dispersion unit so that the laser scattering intensity was 10 to 15%. The stirring speed of the dispersion unit stirrer was 1750 rpm, and there was no ultrasonic mode. The particle size distribution was analyzed by dividing the particle size range of 0.01 to 3500 μm into 100 parts. The refractive index of water was 1.33, and the refractive index of alumina particles and coated alumina particles was 1.768. In the measured mass-based particle size distribution, the particles with a cumulative mass of 50% were taken as the average particle size. The peak was determined as the maximum point detected within the above particle size range.

[0083] (3) Content of aluminum nitride in the coated alumina particles The coated alumina particles were separated from the alumina powder using a sieve made of stainless steel test sieve conforming to the JIS standard with a mesh size of 53 μm. The content of aluminum nitride in the coated alumina particles (hereinafter also referred to as "AlN content") was measured by Rietveld analysis of the powder X-ray diffraction pattern. The coated alumina particles were packed in a sample holder and measured using an X-ray diffractometer (Bruker's "D8 ADVANCE" (product name), detector: LynxEye (product name)). The measurement conditions were as follows: X-ray source: CuKα (λ = 1.5406 Å), measurement method: continuous scan method, scan speed: 0.017° / 2.0 sec, tube voltage: 45 kV, tube current: 360 mA, divergence slit: 0.5°, solar slit: 4°, measurement range: 2θ = 10 to 70°. Based on the obtained X-ray diffraction pattern, the content of aluminum nitride was determined by quantitative analysis by Rietveld analysis using the analysis software TOPAS.

[0084] (4) Carbon content The coated alumina particles were separated from the alumina powder using a sieve made of stainless steel test sieve conforming to the JIS standard with a mesh size of 53 μm. Thereafter, the carbon amount in the coated alumina particles was measured using a carbon / sulfur simultaneous analyzer (CS-444LS (product name) manufactured by LECO Corporation), and the carbon amount was quantified by a calibration curve method. Specifically, first, a calibration curve was obtained using 63 carbon steel, a Japanese steel standard sample, as the standard substance. Thereafter, 0.3 g of the coated alumina particles obtained in the examples and comparative examples was mixed with metallic iron (product name "IRON CHIP" manufactured by LECO Corporation) and metallic tungsten (product name "CECOCEL II" manufactured by LECO Corporation) as a combustion improver under an oxygen atmosphere until the carbon-containing material was completely decomposed and all carbon was converted to CO. 2 The resulting CO 2 The amount of carbon was determined by measuring the amount with an infrared detector.

[0085] (5) Thickness of the coating layer The coated alumina particles were separated from the alumina powder using a sieve made of stainless steel test sieve conforming to the JIS standard with a mesh size of 53 μm. As shown in Figure 1, the thickness of the coating layer on the coated alumina particles was measured by cross-sectional EPMA analysis. First, the coated alumina particles were embedded in G-2 epoxy resin (Gatan), cross-sectional milled, and then osmium-coated. The coated sample was subjected to N element mapping analysis using an electron beam microanalyzer (JXA-8230 (product name) manufactured by JEOL Ltd.). The accelerating voltage was 15 kV, and the probe current was 5 × 10 -8 A. The obtained mapping image was imported into an image analyzer (Mountech Co., Ltd.'s "MacView Ver.4" (product name)) to determine the thickness of the coating layer. The thicknesses were determined at 10 points for one particle, and the arithmetic mean value was used as the thickness of the coating layer for one particle. The thicknesses of the coating layers of 200 random particles thus obtained were determined, and the arithmetic mean value was used as the thickness of the coating layer for the coated alumina particles.

[0086] (6) Specific surface area The coated alumina particles were separated from the alumina powder using a sieve made of stainless steel test sieve conforming to the JIS standard with a mesh size of 53 μm. The specific surface area was measured using a Macsorb HM-Model 1208. Prior to the measurement, the coated alumina particles were pretreated by heating in a nitrogen gas atmosphere at 300°C for 18 minutes. The adsorption gas used was a mixture of 30% nitrogen and 70% helium, and the flow rate was adjusted so that the flow meter reading was 25 ml / min.

[0087] (7) Bulk density The bulk density of the carbon powder was measured in accordance with JIS K 5101-12-2.

[0088] (8) Total pore volume The total pore volume of the carbon powder was measured by mercury intrusion porosimetry using a pore distribution measuring device (Shimadzu Corporation, AutoPore IV 9520 (trade name)).

[0089] (9) Total content of alumina and aluminum nitride in the alumina powder The total content of alumina and aluminum nitride in the alumina powder (hereinafter also referred to as "total content") was measured by Rietveld analysis of the powder X-ray diffraction pattern. X-ray diffraction measurement was performed in the same manner as for the content of aluminum nitride in the alumina powder described above, and the content of alumina and aluminum nitride was determined by quantitative analysis by Rietveld analysis using the analysis software TOPAS based on the obtained X-ray diffraction pattern.

[0090] (10) Viscosity The alumina powder obtained in the examples and comparative examples was added to silicone oil (product name "KF96-100cs" manufactured by Shin-Etsu Chemical Co., Ltd.) so that the filling rate of the alumina powder was 75 vol%. This was mixed for 30 seconds at a rotation speed of 2200 rpm using a planetary centrifugal mixer (product name "Awatori Rentaro ARE-310" manufactured by Thinky Corporation), and then vacuum degassed to obtain a resin composition. The shear viscosity of the obtained resin composition was measured using a rheometer (product name "MCR102" manufactured by Anton-Paar). The measurement conditions were temperature: 30°C, plate: φ25 mm parallel plate, gap: 1 mm. The shear rate was 0.01 s -1 From 10s -1 Measure while continuously changing from -1 The viscosity was read at this time.

[0091] (11) Thermal conductivity The alumina powder obtained in the examples and comparative examples was added to silicone resin (Toray Dow Corning SE-1885 Liquid A and Liquid B) so that the filling rate of the alumina powder was 80 vol%. After stirring and mixing, the mixture was vacuum degassed and processed to a thickness of 3 mm, and then heated at 120°C for 5 hours to obtain a resin composition. The thermal conductivity of the obtained resin composition was measured using a thermal conductivity measuring device (Hitachi Technology and Services Resin Material Thermal Resistance Measuring Device "TRM-046RHHT" (product name)) by a steady method in accordance with ASTM D5470. The resin composition was processed to a width of 10 mm x 10 mm, and measurements were performed while applying a load of 2 N.

[0092] [Example 1] In Example 1, the raw alumina powder used to produce the coated alumina particles was DAW-90 (product name) manufactured by Denka Co., Ltd. (average sphericity: 0.91, average particle size: 91 μm, specific surface area: 0.1 m 2 / g) was used. In addition, acetylene black, which is a carbon powder, was used. HS-100 (product name) (average particle size: 46 nm, bulk density: 0.15 g / cm) manufactured by Denka Co., Ltd. was used. 3 , Specific surface area: 40m 2 / g, total pore volume: 2.1 mL / g) was used. 50 g of raw material alumina powder and 20 g of carbon powder were mixed in a ball mill, and nitrogen gas was supplied at a rate of 7 L / min, and the mixture was fired in a nitrogen atmosphere at a firing temperature of 1650°C for a firing time of 12 hours (first step). Thereafter, air was supplied at a rate of 2 L / min, and the mixture was fired in an air atmosphere at a firing temperature of 700°C for a firing time of 4 hours to obtain coated alumina particles A. For the coated alumina particles A, the average sphericity of the coated alumina particles of 1 μm or more and 300 μm or less, the proportion of coated alumina particles with a sphericity of 0.80 or less, the average sphericity, the content of AlN relative to the total, and the thickness of the coating layer were measured, and the results are shown in Table 1. An alumina powder was prepared by blending AA-05 (product name) manufactured by Sumitomo Chemical Co., Ltd. as ultrafine alumina powder 1, DAW-07 (product name) manufactured by Denka Co., Ltd. as fine alumina powder 2, and coated alumina particles A as coarse alumina powder 3 in the proportions (volume %) shown in Table 1. The physical properties of the obtained alumina powder were evaluated, and the results are shown in Table 1.

[0093] [Example 2] In Example 2, alumina powder used as a raw material for producing coated alumina particles was DAW-70 (product name) manufactured by Denka Co., Ltd. (average sphericity: 0.92, average particle size: 70 μm, specific surface area: 0.1 m 2 Coated alumina particles B were produced in the same manner as in Example 1, except that a 100% aqueous solution of 1,550% by weight per 1000 g of cellulose acetate was used, and the firing temperature in the first step was changed to 1,550° C. and the firing time to 4 hours. The same measurements as in Example 1 were carried out, and the results are shown in Table 1. An alumina powder was obtained in the same manner as in Example 1 with the composition (volume %) shown in Table 1, except that DAW-05 (product name) manufactured by Denka Co., Ltd. was used as the fine alumina 2 and the coated alumina particles B were used as the coarse alumina 3. The same measurements as in Example 1 were also carried out, and the results are shown in Table 1.

[0094] [Example 3] In Example 3, alumina powder used as a raw material for producing coated alumina particles was DAS-30 (product name) (average sphericity: 0.93, average particle size: 30 μm, specific surface area: 0.2 m) manufactured by Denka Co., Ltd. 2Coated alumina particles C were produced in the same manner as in Example 1, except that a 100% sintered alumina powder (1.0 g / g) was used, and the firing temperature in the first step was changed to 1500° C. and the firing time to 4 hours. The same measurements as in Example 1 were carried out, and the results are shown in Table 1. An alumina powder was obtained in the same manner as in Example 1 with the composition (volume %) shown in Table 1, except that DAW-05 (product name) manufactured by Denka Co., Ltd. was used as the fine alumina 2 and coated alumina particles C were used as the coarse alumina 3. The same measurements as in Example 1 were also carried out, and the results are shown in Table 1.

[0095] [Example 4] In Example 4, the raw alumina powder used to produce the coated alumina particles was DAW-120 (product name) manufactured by Denka Co., Ltd. (average sphericity: 0.91, average particle size: 115 μm, specific surface area: 0.1 m 2 Coated alumina particles D were produced in the same manner as in Example 1, except that 1,2-dichlorophenyl ether (COOH) was used instead of 1,2-dichlorophenyl ether (COOH) and ...). An alumina powder was obtained in the same manner as in Example 1 with the composition (volume %) shown in Table 1, except that DAW-10 (product name) manufactured by Denka Co., Ltd. was used as the fine alumina 2 and coated alumina particles D were used as the coarse alumina 3. The same measurements as in Example 1 were also carried out, and the results are shown in Table 1.

[0096] [Example 5] In Example 5, coated alumina particles E were produced in the same manner as in Example 1, except that the firing temperature in the first step was changed to 1600° C. The same measurements as in Example 1 were carried out, and the results are shown in Table 1. Except for using the coated alumina particles E as the coarse alumina powder 3, an alumina powder was obtained in the same manner as in Example 1 with the composition (volume %) shown in Table 1. In addition, the same measurements as in Example 1 were carried out, and the results are shown in Table 1.

[0097] [Example 6] In Example 6, alumina powder as a raw material used for producing coated alumina particles was DAW-45 (product name) manufactured by Denka Co., Ltd. (average sphericity: 0.92, average particle size: 43 μm, specific surface area: 0.2 m 2Coated alumina particles F were produced in the same manner as in Example 1, except that a 100% sintered alumina powder (1.0 g / g) was used, and the firing temperature in the first step was changed to 1600° C. and the firing time to 8 hours. The same measurements as in Example 1 were carried out, and the results are shown in Table 1. An alumina powder was obtained in the same manner as in Example 1 with the composition (volume %) shown in Table 1, except that DAW-05 (product name) manufactured by Denka Co., Ltd. was used as the fine alumina 2 and coated alumina particles F were used as the coarse alumina 3. The same measurements as in Example 1 were also carried out, and the results are shown in Table 1.

[0098] [Example 7] In Example 7, the raw alumina powder used to produce the coated alumina particles was DAW-70 (product name) manufactured by Denka Co., Ltd. (average sphericity: 0.92, average particle size: 70 μm, specific surface area: 0.1 m 2 Coated alumina particles G were produced in the same manner as in Example 1, except that 1,2-dichloro-1,2-tetrafluoroethylene (CO) was used and the firing temperature in the first step was changed to 1600° C. The same measurements as in Example 1 were carried out, and the results are shown in Table 1. An alumina powder was obtained in the same manner as in Example 1 with the composition (volume %) shown in Table 1, except that DAW-05 (product name) manufactured by Denka Co., Ltd. was used as the fine alumina 2 and coated alumina particles G were used as the coarse alumina 3. The same measurements as in Example 1 were also carried out, and the results are shown in Table 1.

[0099] [Example 8] In Example 8, the raw alumina powder used to produce the coated alumina particles was DAW-120 (product name) manufactured by Denka Co., Ltd. (average sphericity: 0.91, average particle size: 115 μm, specific surface area: 0.1 m 2 Coated alumina particles H were produced in the same manner as in Example 1, except that 1,2-dichloro-1,2-tetrafluoroethylene (CO) was used and the firing temperature in the first step was changed to 1600° C. The same measurements as in Example 1 were carried out, and the results are shown in Table 1. An alumina powder was obtained in the same manner as in Example 1 with the composition (volume %) shown in Table 1, except that DAW-10 (product name) manufactured by Denka Co., Ltd. was used as the fine alumina 2 and coated alumina particles H were used as the coarse alumina 3. The same measurements as in Example 1 were also carried out, and the results are shown in Table 1.

[0100] [Example 9] Alumina powders were produced and evaluated in the same manner as in Example 7, except that the compounding ratio of alumina was changed to the ratio (volume %) shown in Table 1. The results are shown in Table 1.

[0101] [Example 10] Alumina powders were produced and evaluated in the same manner as in Example 7, except that the compounding ratio of alumina was changed to the ratio (volume %) shown in Table 1. The results are shown in Table 1.

[0102] [Comparative Example 1] In Comparative Example 1, DAW-05 (product name) manufactured by Denka Co., Ltd. was used as the fine powder of alumina 2, and DAW-45 (product name) manufactured by Denka Co., Ltd. (average sphericity: 0.92, average particle size: 43 μm, specific surface area: 0.2 m) was used as the coarse powder of alumina 3 instead of the coated alumina particles A. 2 Except for using 1,000 mol / g of alumina powder was obtained in the same manner as in Example 1 with the composition (volume %) shown in Table 1. The same measurements as in Example 1 were also carried out, and the results are shown in Table 1.

[0103] [Comparative Example 2] In Comparative Example 2, alumina powder as a raw material used for producing coated alumina particles was DAW-45 (product name) manufactured by Denka Co., Ltd. (average sphericity: 0.92, average particle size: 43 μm, specific surface area: 0.2 m 2 Coated alumina particles a were produced in the same manner as in Example 1, except that a 100% sintered product (1.0 g / g) was used, and the firing temperature in the first step was changed to 1650° C. and the firing time to 30 hours. Measurements were performed in the same manner as in Example 1, and the results are shown in Table 1. The coated alumina particles a did not correspond to the coated alumina particles according to this embodiment. An alumina powder was obtained in the same manner as in Example 1 with the composition (volume %) shown in Table 1, except that DAW-05 manufactured by Denka Co., Ltd. was used as the fine alumina 2 and the coated alumina particles a were used as the coarse alumina 3. The same measurements as in Example 1 were also carried out, and the results are shown in Table 1.

[0104] [Table 1]

[0105] This application is based on a Japanese patent application (Patent Application No. 2019-101604) filed on May 30, 2019, the contents of which are incorporated herein by reference. [Industrial Applicability]

[0106] According to the coated alumina powder of the present invention, the increase in viscosity during filling into a resin can be suppressed, and the resin composition containing the resin can have high thermal conductivity. Therefore, the coated alumina powder is particularly useful for applications of heat dissipation parts such as heat dissipation sheets, heat dissipation greases, heat dissipation spacers, semiconductor encapsulants, and heat dissipation paints (heat dissipation coating agents).

Claims

1. An alumina powder containing coated alumina particles having alumina particles and a coating layer coating the alumina particles, the coated alumina particles having a projected area equivalent circle diameter measured by a microscope of 1 μm or more and 300 μm or less, the coating layer comprises aluminum nitride; The average sphericity of the coated alumina particles is 0.85 or more and 0.97 or less, The average particle size of the coated alumina particles, as measured by a laser diffraction / scattering particle size distribution measuring device, is 72 μm or more and 150 μm or less; The content of aluminum nitride in the coated alumina particles is 15% by mass or more and 40% by mass or less. Alumina powder.

2. The alumina powder according to claim 1 , wherein the alumina powder has a plurality of peaks in a particle size range of 2 μm or more and 200 μm or less in a volume-based frequency particle size distribution measured by a laser diffraction scattering method.

3. 3. The alumina powder according to claim 1, wherein the proportion of the coated alumina particles having a sphericity of 0.80 or less is 15% or less on a number basis.

4. The alumina powder according to any one of claims 1 to 3, wherein the total content of alumina and aluminum nitride in the alumina powder is 80 mass% or more.

5. The alumina powder according to any one of claims 1 to 4, wherein the carbon content in the coated alumina particles is 0.3 mass% or less.

6. A resin composition comprising a resin and the alumina powder according to any one of claims 1 to 5.

7. The resin composition according to claim 6, wherein the resin comprises at least one resin selected from the group consisting of a silicone resin, an epoxy resin, a urethane resin, and an acrylic resin.

8. A heat dissipation part comprising the alumina powder according to any one of claims 1 to 5, or the resin composition according to claim 6 or 7.

9. A method for producing coated alumina particles, comprising the steps of: the coated alumina particles have alumina particles and a coating layer coating the alumina particles, a projected area equivalent circle diameter measured by a microscope is 1 μm or more and 300 μm or less, the coating layer contains aluminum nitride, and the average sphericity of the coated alumina particles is 0.85 or more and 0.97 or less, The manufacturing method includes a first step of sintering a mixture containing raw material alumina powder and carbon powder at a temperature of 1500° C. to 1700° C. in a reducing atmosphere containing nitrogen gas to obtain a first sintered powder; A second step of further calcining the first calcined powder at a temperature of 600° C. or more and 900° C. or less in an air atmosphere to obtain the coated alumina particles, The carbon powder has an average particle size of 30 nm or more and 70 nm or less and a bulk density of 0.10 g / cm 3 0.20g / cm or more 3 The specific surface area is 20 m or less. 2 / g or more 60m 2 / g or less.

10. The average particle diameter of the coated alumina particles measured by a laser diffraction scattering type particle size distribution measuring device is 72 μm or more and 150 μm or less, The method according to claim 9 , wherein the content of aluminum nitride in the coated alumina particles is from 15% by mass to 40% by mass.

Citation Information

Patent Citations

  • Spherical aluminum nitride and its manufacturing method

    JP2005162555A

  • Insulating sheet and multilayer structure

    JP2009164093A

  • Alumina blend particle and resin molding

    JP2009274929A

  • Aluminum nitride-based particle, method for producing the same, and apparatus for producing aluminum nitride-based particle

    JP2012041253A

  • Aluminum nitride powder for filler, aluminum nitride powder for sub-filler and manufacturing method therefor

    JP2017114706A