Method for producing porous carbon structures having increased surface area and total pore volume and porous carbon structures produced using the same
The method of using a halogenated carbon precursor with a mesoporous template significantly increases the surface area and pore volume of porous carbon structures, addressing the limitations of conventional methods and improving the performance of adsorbents and electrochemical devices.
Patent Information
- Application Number
- JP2023533368
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-04-14
- Filing Date
- 2022-03-30
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2042-03-30
AI Technical Summary
Conventional methods for producing porous carbon structures fail to achieve the higher levels of surface area and total pore volume required by advanced technological applications, limiting their performance in adsorbents, electrochemical devices, and fuel cells.
A method involving the use of a template with a mesoporous shell, injection of a carbon precursor comprising a polymer precursor with a halogen functional group, and a crosslinking agent, followed by polymerization and carbonization to create a template-carbon composite, which is then treated to produce a porous carbon structure with significantly increased surface area and pore volume.
The method results in porous carbon structures with BET surface areas ranging from 2,000 to 5,000 m²/g and total pore volumes from 2.0 to 7.2 cm³/g, enhancing the performance of adsorbents and electrochemical devices such as fuel cells.
Smart Images

Figure 0007572557000002 
Figure 0007572557000003 
Figure 0007572557000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a porous carbon structure having an increased surface area and total pore volume, and a porous carbon structure produced using the same, and more particularly, to a method for producing a porous carbon structure that can dramatically increase the surface area and total pore volume of the porous carbon structure, and a porous carbon structure produced using the same. [Background technology]
[0002] Porous carbon structures, due to their high surface area, high pore volume, excellent conductivity, and excellent chemical stability, are used in various technical fields, such as (i) the adsorbent field, and (ii) electrochemical fields such as fuel cells, secondary batteries, capacitors, etc. In an effort to precisely control the microstructure of a porous carbon structure and further increase its surface area and total pore volume, the porous carbon structure is generally manufactured using a template. For example, a carbon precursor (e.g., a monomer) is injected into a template having spherical inorganic particles and a mesoporous shell formed thereon, followed by polymerization and carbonization to manufacture a template-carbon complex. Then, the template is removed from the template-carbon complex to manufacture a hollow type porous carbon structure.
[0003] However, the surface area and total pore volume of the porous carbon structure produced by the above-mentioned conventional methods are not as high as those required in the industry (e.g., 2,000 m 2 / g or greater BET surface area and 2.0 cm 3 / g or more). Furthermore, in some technical fields, increasingly higher levels of BET surface area and total pore volume are required for porous carbon structures. Summary of the Invention [Problem to be solved by the invention]
[0004] Therefore, the present invention relates to a method for manufacturing a porous carbon structure, which can avoid problems caused by the limitations and shortcomings of the related art as described above, and a porous carbon structure manufactured using the same.
[0005] One aspect of the present invention is to provide a method by which porous carbon structures can be produced having dramatically increased surface area and total pore volume. Another aspect of the present invention is to provide a porous carbon structure having dramatically increased surface area and total pore volume. Another aspect of the present invention is to provide an adsorbent with superior performance by incorporating a porous carbon structure with dramatically increased surface area and total pore volume. Another aspect of the present invention is to provide electrodes for electrochemical devices having superior performance by incorporating porous carbon structures having dramatically increased surface area and total pore volume. Another aspect of the present invention is to provide a membrane electrode assembly with superior performance by including a porous carbon structure in the anode and / or cathode that has dramatically increased surface area and total pore volume. Another aspect of the present invention is to provide a fuel cell having superior performance by including said membrane electrode assembly. In addition to the above-described aspects of the present invention, other features and advantages of the present invention will be described below or will become apparent to those skilled in the art from the description. [Means for solving the problem]
[0006] According to one aspect of the present invention, there is provided a method for producing a porous carbon structure, the method including the steps of: preparing a template having a mesoporous shell; injecting a carbon precursor into the template, the carbon precursor including a polymer precursor and a crosslinking agent, the polymer precursor including a first component having a halogen functional group and a second component not having a halogen functional group, the content of the first component in the polymer precursor being 20 to 80 wt %; polymerizing the polymer precursor to form a polymer; carbonizing the polymer to obtain a template-carbon composite; and removing the template from the template-carbon composite.
[0007] The first component may be a halogenated monomer or NH4F. The halogenated monomer may be a fluorinated monomer. The first component may be a fluorophenol, the second component may be a phenol, and the cross-linking agent may be paraformaldehyde. The fluorophenol may be 4-fluorophenol. The first component may be NH4F, the second component may be phenol, and the cross-linking agent may be paraformaldehyde. The method may further include treating the template with an acid prior to the carbon precursor injection step. The acid may include AlCl3.
[0008] According to another aspect of the present invention, 2 / g and 2.0-7.2 cm 3 A porous carbon structure is provided having a total pore volume of about 1000 nm / g. The porous carbon structure has a thickness of 2,300 to 5,000 m 2 / g and a BET surface area of 2.8–7.2 cm 3 / g total pore volume. The porous carbon structure has a thickness of 3,100 to 5,000 m 2 / g and a BET surface area of 5.0–7.2 cm 3 / g total pore volume. The porous carbon structure has a thickness of 3,400 to 5,000 m 2 / g and a BET surface area of 5.7–7.2 cm 3 / g total pore volume. The porous carbon structure may be a hollow structure. According to another aspect of the present invention there is provided an adsorbent comprising the porous carbon structure described above. According to another aspect of the present invention there is provided an electrode for an electrochemical device comprising the porous carbon structure described above.
[0009] According to another aspect of the present invention, there is provided a membrane electrode assembly comprising an anode, a cathode, and an electrolyte membrane between the anode and the cathode, wherein at least one electrode selected from the group consisting of the anode and the cathode comprises the porous carbon structure and catalytic metal particles dispersed on the porous carbon structure. According to another aspect of the present invention, there is provided a fuel cell comprising the membrane electrode assembly described above. The above general description of the present invention is intended to illustrate or explain the present invention, and is not intended to limit the scope of the present invention. Effect of the Invention
[0010] The present invention overcomes the limitations of the prior art and provides a porous carbon structure having a significantly increased surface area and total pore volume, thus satisfying the demand for a porous carbon structure having a higher level of surface area and total pore volume due to the technological development in the related fields. Furthermore, the porous carbon structure of the present invention can not only improve the performance of an adsorbent containing it, but also improve the performance of an electrochemical device (e.g., a fuel cell, a secondary battery, a capacitor, etc.) containing it. [Brief description of the drawings]
[0011] The accompanying drawings, which are intended to aid in the understanding of the invention and are incorporated in and constitute a part of this specification, illustrate embodiments of the invention and, together with the description, serve to explain the principles of the invention. [Figure 1] 1 is a schematic diagram showing a method for fabricating a porous carbon structure according to one embodiment of the present invention. [Diagram 2] 1 shows BET adsorption / desorption isotherm curves of a carbon precursor containing a "component having a halogen functional group" of the present invention and a carbon structure obtained by polymerization and carbonization of a conventional carbon precursor, respectively. [Figure 3a] 1 is a transmission electron microscope (TEM) photograph of a mold of Production Example 2. [Figure 3b] 1 is a TEM photograph of the porous carbon structure of Comparative Example 2a. [Figure 3c] 1 is a TEM photograph of the porous carbon structure of Example 2a. [Figure 3d] 4 is a TEM image of the porous carbon structure of Example 2b. [Figure 3e] 4 is a TEM photograph of the porous carbon structure of Example 2c. [Figure 3f] 1 is a TEM photograph of the porous carbon structure of Comparative Example 2b. [Figure 4] 1 shows BET adsorption / desorption isothermal curves of the porous carbon structures of Examples 1a to 1c and the porous carbon structures of Comparative Examples 1a and 1b. [Diagram 5] 1 shows BET adsorption / desorption isothermal curves of the porous carbon structures of Examples 2a to 2c and the porous carbon structures of Comparative Examples 2a and 2b. MODE FOR CARRYING OUT THEINVENTION
[0012] Hereinafter, the embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, the embodiments described below are presented for illustrative purposes to help a clear understanding of the present invention, and do not limit the scope of the present invention. FIG. 1 is a schematic diagram showing a method for producing a porous carbon structure according to one embodiment of the present invention. As shown in FIG. 1, the method of the present invention includes the steps of providing a template (10) having a mesoporous shell (12), injecting a carbon precursor (20) into the template (10), polymerizing the carbon precursor (20) to form a polymer, carbonizing the polymer to obtain a template-carbon complex, and removing the template (10) from the template-carbon complex.
[0013] The step of preparing the template (10) may include a step of forming a mesoporous shell (12) on spherical inorganic particles (11). The inorganic particles (11) may include inorganic oxides such as zirconia, alumina, titania, silica, and ceria. For example, commercially available silica particles having a diameter of 10 nm to 1000 nm may be used as the inorganic particles (11). Alternatively, the silica particles may be prepared by adding tetraethyl orthosilicate (TEOS) (also called "tetraethoxysilane") to a mixed solution of aqueous ammonia, ethanol, and deionized water, and stirring for a sufficient period of time. For the sake of convenience, a method for preparing the template (10) containing silica particles as the inorganic particles (11) will be specifically described below. First, silica particles (11) are placed in a dispersion medium (e.g., a mixed dispersion medium of ethanol and water) and TEOS and octadecyltrimethoxysilane (C 18 -TMS) is added and stirred for a sufficient period of time. 18 -TMS functions as a silane coupling agent.18 By adjusting the molar ratio of TEOS to -TMS, the pore size of the mesoporous shell (12) formed through the calcination process described below can be adjusted to within a range of 2 to 50 nm, and for example, the molar ratio may be 3 to 50. 18 The larger the molar ratio of TEOS to -TMS, the smaller the pore size of the mesoporous shell (12) tends to be.
[0014] Subsequently, the silica particles (11) are separated from the dispersion liquid, for example, by centrifugation, and then placed in a furnace and baked at 500°C to 600°C (for example, about 550°C) for 5 to 7 hours. By such a baking step, the silane coupling agent (i.e., C 18 The organic functional groups of the silane (-TMS) are removed to form the mesoporous shell (12) on the silica particles (11). As an optional process, the template (10) thus obtained can be treated with an acid. For example, the template (10) can be immersed in an acid solution containing AlCl3, dried, and then calcined at 500°C to 600°C (e.g., about 550°C) for 2 to 4 hours to prepare a template (10) having an aluminosilica mesoporous shell (12). The acid treatment provides acid sites on the surface of the template (10) to induce a surface reaction, thereby maximizing the surface area and total pore volume of the porous carbon structure (100) manufactured using the template (10). Next, as shown in Fig. 1, a carbon precursor (20) is injected into the template (10). The method of injecting the carbon precursor (20) is not particularly limited in the present invention. For example, the carbon precursor (20) may be injected into the mesopores of the template (10) by a method such as vacuum-filling.
[0015] According to the present invention, the carbon precursor (20) comprises a polymeric precursor and a cross-linking agent, the polymeric precursor comprising a first component having a halogen functional group and a second component not having a halogen functional group. Each of the first and second components may be monomeric. Alternatively, the first component may be a halogenating agent and the second component may be exclusively a monomeric component. Optionally, the carbon precursor (20) may further comprise an initiator for polymerization of the monomeric component(s). The monomer component(s) can form a polymer through condensation polymerization or addition polymerization. For example, the carbon precursor 20 can include phenolic monomer(s) as monomer component(s) that can form a phenolic resin through condensation polymerization, and paraformaldehyde as a cross-linking agent. The first component having a halogen functional group may be a halogenated monomer and / or NH4F. The halogenated monomer is the same monomer as the second component substituted with a halogen functional group, and may be a fluorinated monomer, a chlorinated monomer, a brominated monomer, or an iodinated monomer, preferably a fluorinated monomer.
[0016] For example, when the carbon precursor (20) includes phenol as the second component and paraformaldehyde as the cross-linking agent, the first component may be a halogenated phenol such as fluorophenol, chlorophenol, bromophenol, and iodophenol, preferably fluorophenol, and more preferably 4-fluorophenol. That is, the carbon precursor (20) according to one embodiment of the present invention may include 4-fluorophenol, phenol, and paraformaldehyde. Alternatively, instead of or in addition to a halogenated monomer, the carbon precursor (20) of the present invention may include NH4F as the first component having a halogen functionality. For example, the carbon precursor (20) according to one embodiment of the present invention may include NH4F, phenol, and paraformaldehyde. The inventors of the present invention have found that the “first component having a halogen functional group” contained in the carbon precursor (20) significantly increases the surface area of the carbon structure obtained by polymerization and carbonization of the carbon precursor (20). FIG. 2 shows BET adsorption / desorption isotherm curves of a carbon precursor containing the “first component having a halogen functional group” of the present invention and a carbon structure obtained by polymerization and carbonization of a conventional carbon precursor.
[0017] Specifically, the graph in FIG. 2 shows (i) a BET adsorption / desorption isothermal curve of a first carbon precursor obtained by heating a carbon precursor containing 4-fluorophenol together with phenol and paraformaldehyde (phenol: 0.2 g, 4-fluorophenol: 0.2 g) at 160° C. for 6 hours to polymerize the carbon precursor, followed by carbonization at 1000° C. for 6 hours under an Ar atmosphere; (ii) a BET adsorption / desorption isothermal curve of a second carbon precursor obtained by heating a carbon precursor containing NHF together with phenol and paraformaldehyde (phenol: 0.3 g, NHF: 0.1 g) at 160° C. for 6 hours to polymerize the carbon precursor, followed by carbonization at 1000° C. for 6 hours under an Ar atmosphere; and (iii) a BET adsorption / desorption isothermal curve of a third carbon precursor obtained by heating a carbon precursor containing phenol and paraformaldehyde (phenol: 0.4 g) at 160° C. for 6 hours to polymerize the carbon precursor, followed by carbonization at 1000° C. for 6 hours under an Ar atmosphere. As evidenced by FIG. 2, the carbon structures (i.e., the first and second carbon structures) obtained from the carbon precursor (20) of the present invention, which further comprises a "first component having a halogen functional group" such as 4-fluorophenol or NHF in addition to the second component which is a monomer, have a much larger surface area than the carbon structures (i.e., the third carbon structure) obtained from a carbon precursor which comprises only the second component which is a monomer component and does not comprise any "component having a halogen functional group".
[0018] According to one embodiment of the present invention, the content of the first component having a halogen functional group in the polymer precursor containing the first and second components is 20-80% by weight, more preferably 25-75% by weight. If the content of the first component having a halogen functional group in the polymer precursor is less than 20% by weight, the effect of increasing the surface area of the carbon structure intended by the present invention may be insignificant. On the other hand, if the content of the first component having a halogen functional group in the polymer precursor exceeds 80% by weight, the structure of the carbon structure is destroyed, resulting in a decrease in its surface area. Referring again to FIG. 1, after the carbon precursor (20) is injected into the mold (10), the carbon precursor (20) (more specifically, a polymer precursor, and even more specifically, a monomer component(s)) is polymerized to form a polymer. The temperature and time of the polymerization reaction can be determined depending on the components constituting the carbon precursor (20). For example, when the carbon precursor (20) contains a phenolic monomer(s) and paraformaldehyde, the polymerization reaction can be carried out at a temperature of 150 to 200° C. for 5 to 7 hours.
[0019] The polymer formed by polymerization of the carbon precursor 20 is then carbonized to obtain a template-carbon composite. The carbonization process can be carried out in the presence of a non-reactive gas such as Ar or N2 at a temperature of 800 to 1200°C for 5 to 7 hours. Subsequently, the template (10) can be removed from the template-carbon composite to obtain the porous carbon structure (100) of the present invention. For example, the template (10) can be dissolved in a strong base (e.g., NaOH, KOH, etc.) or a strong acid (e.g., HF), and the remaining structure can be washed with ethanol, water, or a mixture thereof, and dried at or above the boiling point of the washing liquid for a sufficient time to obtain the porous carbon structure (100).
[0020] The porous carbon structure (100) of the present invention obtained by the above-mentioned method has a length of 2,000 to 5,000 m. 2 / g, more preferably 2,300 to 5,000m 2 High BET surface area of 2.0-7.2 cm / g 3 / g, and more preferably 2.8 to 7.2 cm 3 / g. In particular, when the template (10) is subjected to acid treatment (e.g., using AlCl3) and calcination before the carbon precursor (20) is poured into the template (10), the final porous carbon structure (100) has a thickness of 3,100 to 5,000 m. 2 / g, more preferably 3,400 to 5,000 m2 Higher BET surface area of 5.0~7.2cm / g and 3 / g, and more preferably 5.7 to 7.2 cm 3 / g. The porous carbon structure (100) of the present invention may be a hollow structure as shown in FIG. The porous carbon structure (100) of the present invention may be used in the manufacture of adsorbents and / or electrodes for electrochemical devices to improve their performance. For example, the porous carbon structure (100) of the present invention can be used to manufacture a membrane electrode assembly for a fuel cell, that is, in a membrane electrode assembly including an anode, a cathode, and an electrolyte membrane between the anode and the cathode, at least one electrode selected from the group consisting of the anode and the cathode can include the porous carbon structure (100) of the present invention and catalytic metal particles dispersed on the porous carbon structure (100). The present invention will be described in detail with reference to the following Preparation Examples, Examples, and Comparative Examples. However, the following Preparation Examples and Examples are provided to aid in the understanding of the present invention and should not be construed as limiting the scope of the present invention.
[0021] [Mold manufacturing] Manufacturing Example 1 Commercially available silica nanoparticles were dispersed in a mixed dispersion medium of ethanol and water to obtain a mixture. 18 -TMS was added and stirred for 4 hours. The silica nanoparticles separated from the mixture by centrifugation were then calcined at 550°C for 6 hours to produce a template in which a mesoporous shell was formed on each of the silica nanoparticles. Manufacturing Example 2 The template obtained in Production Example 1 was immersed in 0.2 g of an AlCl3-containing solution, then dried and fired at 550°C for 3 hours to produce a template having an aluminosilica mesoporous shell.
[0022] [Production of a porous carbon structure using the mold of Production Example 1] Example 1a A carbon precursor was injected into the mesopores of the template obtained in Preparation Example 1 by a vacuum-filling method. The carbon precursor contained a polymer precursor (4-fluorophenol + phenol) and a crosslinking agent (paraformaldehyde). The amounts of 4-fluorophenol and phenol in the polymer precursor were 0.1 g and 0.3 g, respectively. The template into which the carbon precursor was injected was then heated at 160°C for 6 hours to polymerize the carbon precursor. The polymer was then carbonized at 1000°C for 6 hours under an Ar atmosphere to obtain a template-carbon composite. The template (10) was then removed from the template-carbon composite by dissolving it with HF, and the remaining structure was washed and dried to complete a porous carbon structure. Example 1b A porous carbon structure was prepared in the same manner as in Example 1a, except that the amounts of 4-fluorophenol and phenol in the polymer precursor were both 0.2 g. Example 1c A porous carbon structure was prepared in the same manner as in Example 1a, except that the amounts of 4-fluorophenol and phenol in the polymer precursor were 0.3 g and 0.1 g, respectively. Comparative Example 1a A porous carbon structure was prepared in the same manner as in Example 1a, except that the polymer precursor contained only phenol (0.4 g) and no 4-fluorophenol. Comparative example 1b A porous carbon structure was prepared in the same manner as in Example 1a, except that the polymer precursor contained only 4-fluorophenol (0.4 g) and no phenol.
[0023] [Production of a porous carbon structure using the mold of Production Example 2] Example 2a A porous carbon structure was prepared in the same manner as in Example 1a, except that the template of Preparation Example 2 was used instead of the template of Preparation Example 1. Example 2b A porous carbon structure was prepared in the same manner as in Example 2a, except that the amounts of 4-fluorophenol and phenol in the polymer precursor were both 0.2 g. Example 2c A porous carbon structure was prepared in the same manner as in Example 2a, except that the amounts of 4-fluorophenol and phenol in the polymer precursor were 0.3 g and 0.1 g, respectively. Comparative example 2a A porous carbon structure was prepared in the same manner as in Example 2a, except that the polymer precursor contained only phenol (0.4 g) and no 4-fluorophenol. Comparative Example 2b A porous carbon structure was prepared in the same manner as in Example 2a, except that the polymer precursor contained only 4-fluorophenol (0.4 g) and no phenol.
[0024] [Transmission electron microscope (TEM) analysis] Transmission electron microscope photographs of the template of Preparation Example 2 having an aluminosilica mesoporous shell, and the porous carbon structures of Examples 2a to 2c and Comparative Examples 2a and 2b are shown in Figure 3. Figure 3a is a TEM photograph of the template of Preparation Example 2, Figure 3b is a TEM photograph of the porous carbon structure of Comparative Example 2a in which the content of 4-fluorophenol in the carbon precursor was 0% by weight, Figure 3c is a TEM photograph of the porous carbon structure of Example 2a in which the weight ratio of 4-fluorophenol to phenol in the carbon precursor was 1:3, Figure 3d is a TEM photograph of the porous carbon structure of Example 2b in which the weight ratio of 4-fluorophenol to phenol in the carbon precursor was 1:1, Figure 3e is a TEM photograph of the porous carbon structure of Example 2c in which the weight ratio of 4-fluorophenol to phenol in the carbon precursor was 3:1, and Figure 3f is a TEM photograph of the porous carbon structure of Comparative Example 2b in which the content of phenol in the carbon precursor was 0% by weight. 3b to 3e show that as the content of the component having a halogen functional group (i.e., 4-fluorophenol) in the polymer precursor (or the weight ratio of the first component having a halogen functional group to the second component not having a halogen functional group) increases, the porosity of the mesoporous shell of the hollow carbon structure increases. On the other hand, as can be seen from FIG. 3f, when the content of the component having a halogen functional group (i.e., 4-fluorophenol) in the polymer precursor is too high, collapse of the carbon structure structure is caused.
[0025] [BET (Brunauer-Emmett-Teller) surface area analysis] Using a BET analyzer (Micromeritics, ASAP-2020), BET adsorption / desorption isothermal curves of the porous carbon structures of the examples and comparative examples were obtained. Figure 4 shows the BET adsorption / desorption isothermal curves of the porous carbon structures of Examples 1a to 1c and the porous carbon structures of Comparative Examples 1a and 1b, and Figure 5 shows the BET adsorption / desorption isothermal curves of the porous carbon structures of Examples 2a to 2c and the porous carbon structures of Comparative Examples 2a and 2b. It was confirmed from FIGS. 4 and 5 that the porous carbon structure of the embodiment of the present invention, which was prepared using a carbon precursor containing an appropriate amount of a component having a halogen functional group (i.e., 4-fluorophenol), had a much larger surface area than the porous carbon structures of Comparative Examples 1a and 2a, which were prepared using a carbon precursor not containing the component having a halogen functional group. On the other hand, when a porous carbon structure is prepared using a carbon precursor containing an excessive amount of a component having a halogen functional group, the structure of the carbon structure is destroyed and its surface area is reduced, as can be seen from the BET adsorption / desorption isotherms of Comparative Examples 1b and 2b. In addition, the BET surface area (S BET ), micropore volume (V MICRO ), mesopore volume (V MESO ), total pore volume (V TOTALSpecifically, five samples were randomly selected, and the physical properties were measured. The average values of the measured values for each physical property were calculated and shown in Table 1 below. [Table 1]
[0026] As can be seen from Table 1, the porous carbon structure of the comparative example had a 1500m 2 Relatively low BET surface area (S BET ) and 2.0 cm 3 Relatively low total pore volume (V TOTAL ), whereas the porous carbon structure of the embodiment of the present invention has a thickness of 2,000 to 4,400 m 2 / g, more specifically 2,300-4,400m 2 High BET surface area (S BET ) and 2.0~6.8cm 3 / g, and more specifically, 2.8 to 6.8 cm 3 High total pore volume (V TOTAL ). In particular, the porous carbon structures of Examples 2a to 2c were produced using the molds of Production Example 2 obtained by immersing the mold of Production Example 1 in an acid solution containing AlCl3, followed by drying and firing. 2 / g, more specifically 3,400-4,400m 2 The remarkably high BET surface area (S BET ) and 5.0~6.8cm 3 / g, and more specifically, 5.7-6.8 cm 3 Much higher total pore volume (V TOTAL ) can be confirmed. On the other hand, Examples 2a-2c each exhibited two pore size values, which means that the pores of these carbon structures have a bimodal morphology.
Claims
1. providing a template having a mesoporous shell; injecting a carbon precursor into the mold, the carbon precursor including a polymer precursor and a crosslinking agent, the polymer precursor including a first component having a halogen functional group and a second component not having a halogen functional group, the content of the first component in the polymer precursor being 20-80 wt %; polymerizing the polymer precursor to form a polymer; carbonizing the polymer to obtain a template-carbon composite; and Removing the template from the template-carbon composite. Including, A method for producing a porous carbon structure.
2. The first component is a halogenated monomer or NH 4 F. A method for producing the porous carbon structure according to claim 1.
3. The halogenated monomer is a fluorinated monomer. A method for producing the porous carbon structure according to claim 2.
4. the first component is a fluorophenol; the second component is a phenol; The crosslinking agent is paraformaldehyde. A method for producing the porous carbon structure according to claim 1.
5. The fluorophenol is 4-fluorophenol. A method for producing the porous carbon structure according to claim 4.
6. The first component is NH 4 F, the second component is a phenol; The crosslinking agent is paraformaldehyde. A method for producing the porous carbon structure according to claim 1.
7. The method further comprises treating the template with an acid prior to the carbon precursor injection step. A method for producing the porous carbon structure according to any one of claims 1 to 6.
8. The acid is AlCl 3 Including, A method for producing the porous carbon structure according to claim 7.
9. 3,100 to 5,000m 2 / g and 5.0-7.2 cm 3 / g of total pore volume.
10. The porous carbon structure has a thickness of 3,400 to 5,000 m 2 / g and a BET surface area of 5.7–7.2 cm 3 / g total pore volume, 10. The porous carbon structure of claim 9.
11. The porous carbon structure is a hollow structure. The porous carbon structure according to any one of claims 9 to 10.
12. An adsorbent comprising the porous carbon structure according to any one of claims 9 to 10.
13. An electrode for an electrochemical device comprising the porous carbon structure according to any one of claims 9 to 10.
14. anode, A cathode, and An electrolyte membrane between the anode and the cathode Including, At least one electrode selected from the group consisting of the anode and the cathode, The porous carbon structure according to any one of claims 9 to 10, and Catalytic metal particles dispersed on said porous carbon structure Including, Membrane electrode assembly.
15. A fuel cell comprising the membrane electrode assembly according to claim 14.
Citation Information
Patent Citations
Method for producing nanoporous carbide-derived carbon with high specific surface area
JP2009517314A
Nanoporous capsule-structure body having hollow core with mesoporous shell(HCMS) and manufacturing method thereof
KR1020030068765A
Method of surface area enhancement for nano-structuredhollow carbon material containing mesoporous shell
KR1020050117112A