Foaming calming material and foaming calming method using same
A mixture of organic and inorganic materials, tailored to generate a controlled gas volume and density, addresses the inefficiencies of conventional calming agents by effectively suppressing slag foaming during high-speed slag removal, enhancing operational efficiency and reducing costs.
Patent Information
- Application Number
- JP2021004772
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-15
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2041-01-15
AI Technical Summary
Conventional calming materials fail to effectively suppress slag foaming during high-speed slag removal operations, leading to increased costs and operational inefficiencies due to the need for continuous addition and potential overflow, which is exacerbated by the rapid reaction of carbon in granulated iron with FeO in the slag.
A foaming suppressing material composed of a mixture of organic compounds and inorganic materials, designed to generate a specific gas volume and apparent density, effectively suppressing slag foaming by controlling the volumetric expansion energy and settling properties.
The material efficiently and quickly calms slag foaming, reducing costs and extending the slag drainage time, while minimizing the risk of overflow and equipment damage.
Smart Images

Figure 0007572621000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a foaming suppression material for suppressing foaming of slag discharged from a converter into a slag ladle, and a foaming suppression method using the same. [Background technology]
[0002] During or after the refining process of molten iron, the slag foams due to CO bubbles generated by the reaction of C in the molten iron with FeO (iron oxide) in the slag at the interface between the molten iron and steelmaking slag (hereinafter referred to as slag), or CO bubbles generated by the reaction of FeO in the slag with C in the iron particles contained in the slag inside the slag itself (hereinafter referred to as foaming). If this foaming of the slag is severe, the 1300-1500°C slag may overflow from the refining equipment or the transport vessel, and if the refining equipment or the transport vessel is damaged, it will take a lot of time and effort to restore it. If the FeO concentration in the slag is high, a large amount of CO bubbles will be generated, so slag with a high FeO concentration has a strong foaming tendency (it expands rapidly and easily overflows).
[0003] In order to calm the foaming of the slag, it is necessary to destroy the layer in which the CO bubbles remain (hereafter referred to as the foam layer) and shrink the slag. A commonly known method for this purpose is to add a mass of material (calming material) that gasifies inside the slag to the slag, and to use the volume expansion energy generated when the mass gasifies through pyrolysis to destroy the foam layer.
[0004] Here, as one of the smelting processes for molten iron, a multi-function converter process is generally known in which after dephosphorization in a converter, a part of the slag is discharged (intermediate discharge) into a slag ladle outside the furnace, and the decarburization process is continued in the same converter. In this multi-function converter process, if the foaming of the slag becomes so severe during the dephosphorization blow that the slag is about to overflow from the throat of the converter, the dephosphorization blow must be interrupted, and the progress of the dephosphorization reaction becomes insufficient. Therefore, in order to increase the dephosphorization rate in the next decarburization blow, it is necessary to add extra CaO to the converter, which leads to an increase in refining costs and an increase in the amount of slag generated. In addition, when slag foaming progresses in the slag ladle that receives the slag during intermediate slag removal, if the slag is about to overflow from the slag ladle, intermediate slag removal must be interrupted. As a result, the weight of P2O5 in the slag remaining in the converter increases, and phosphorus is re-recovered during decarburization blowing, so extra CaO must be added to the converter. Furthermore, in decarburization blowing, if slag foaming progresses too rapidly, there is a concern that the slag will flow out of the converter throat when the converter is tilted during tapping. For these reasons, it is necessary to add a silencing material to the converter during dephosphorization and decarburization, and to the slag ladle during intermediate slag removal. Usually, such agglomerates that have a destructive effect are called silencing materials, and examples of such silencing materials are disclosed in Patent Documents 1 to 8. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 54-32116 [Patent Document 2] Japanese Patent Application Publication No. 4-180507 [Patent Document 3] Japanese Patent Application Publication No. 5-287347 [Patent Document 4] Japanese Patent Application Publication No. 7-145417 [Patent Document 5] Japanese Patent Application Publication No. 11-50124 [Patent Document 6] JP 2008-255446 A [Patent Document 7] JP 2009-270178 A [Patent Document 8] JP 2009-287050 A Summary of the Invention [Problem to be solved by the invention]
[0006] On the other hand, in recent years, in order to improve the production capacity of converters, high-speed slag disposal operation has been performed in which the intermediate slag disposal time has been shortened to within 4 minutes, which is 3 / 4 or less of the conventional slag disposal time. Under such operating conditions, slag containing a large amount of iron granules falls into the slag ladle, and the carbon in the iron granules reacts with FeO in the slag to generate CO gas, which promotes slag foaming. Therefore, the conventional silencing materials described in the above Patent Documents 1 to 8 cannot sufficiently suppress the outflow of foamed slag from the slag ladle. In addition, in order to suppress slag foaming under such operation, a large amount of silencing material needs to be added continuously, which increases the cost of the silencing material.
[0007] In view of the above-mentioned problems, the present invention aims to provide a foaming calming material that efficiently, quickly, and inexpensively calms the foaming of slag discharged from a converter into a slag ladle, and a foaming calming method using the same. [Means for solving the problem]
[0008] In order to solve the above problems, the inventors of the present invention have investigated important factors for quenching the foaming of slag. As a result, it was found that the foaming quenching effect obtained by adding a quenching agent is related to the gas generation volume (Nm) of the quenching agent at high temperature. 3 / kg) and the apparent density of the sedative (kg / m 3 It was found that the gas generation volume and the apparent density of the quenching material are related to each other, and that the foaming of the slag can be quickly quenched by designing the quenching material to control the gas generation volume and the apparent density of the quenching material to specified conditions.
[0009] Here, in order to control the gas generation volume to an appropriate condition, it is important that the sedative contains an organic compound, and in order to increase the apparent density, it is important that the sedative contains an inorganic material. Therefore, the inventors have conducted extensive research and found that a sedative consisting of a mixture of an organic compound and an inorganic material has a gas generation volume of 0.4 Nm3 when completely combusted. 3 / kg or more, 2.0Nm 3 / kg or less and an apparent density of 1300kg / m 3 It has been discovered that adding the above-mentioned calming agent to the foaming slag makes it possible to calm the foaming of the slag efficiently, quickly, and inexpensively.
[0010] Here, the gas generation volume is the volume of gas (Nm3) generated per 1 kg of silencing material when the silencing material comes into contact with the foamed slag and is completely combusted. 3 / kg), and can be measured, for example, by heating a sample in an oxygen-containing atmosphere and collecting the generated gas in a bag, and the gas generation volume can be calculated using the components and composition of the quenching material. In addition, the apparent density is the density of the molded product including the volume of the pores contained inside the molded product when the quenching material is solid. In the case where the foaming quenching material is made of multiple solids made of different materials, the apparent densities are averaged using the apparent densities and ratios of each solid, and the average value may be used as the apparent density of the foamed slag. In the present invention, since there is almost no difference between the apparent density and the bulk density, the apparent density may be used as the bulk density. The apparent density can be measured, for example, by the method described in JIS Z8807:2012.
[0011] The present invention has been made based on the above findings, and the gist of the present invention is as follows. (1) A foaming calming material for calming foaming of slag discharged into a slag ladle, comprising: A mixture of an organic compound and at least one inorganic material, The volume of gas generated when the mixture is completely combusted is V g T In this case, the gas generation volume V is calculated using the following formulas (1) and (2). g T 0.4Nm 3 / kg or more, 2.0Nm 3 / kg, apparent density is 2000 kg / m 3 A foaming calming material characterized by the above. V g T =V g O +V g I 1 +V g I 2 +V g I 3 +···+V g I n ···(1) V g O =22.4·W O / 100 (a+0.5 b) / (12 a+b+16 c) ···(2) Here, V g O is the gas generation volume (Nm m) generated when the organic compound in the mixture is completely combusted. 3 / kg), and V g I 1 、V g I 2 、V g I 3 、···V g I n is the gas generation volume (Nm) generated when the hydrogen contained in each inorganic material is completely combusted when the mixture contains n types of inorganic materials. 3 / kg). Also, W O represents the proportion (mass%) of the organic compound in the foaming calming material, and a represents the chemical formula C a H b O c represents the total number of carbon atoms in the organic compound represented by the chemical formula C a H b O c represents the total number of hydrogen atoms in the organic compound represented by the chemical formula C a H bO c represents the total number of oxygen atoms in
[0013] (2) The inorganic material includes at least one of slag, dust, refractory, and concrete. (1) The foaming calming material described in.
[0015] (3) (1) Above Or (2) A foaming stabilization method, comprising adding the foaming stabilization material described in claim 1 to foaming slag discharged in a slag ladle. Effect of the Invention
[0016] According to the present invention, it is possible to provide a foaming calming material that efficiently and quickly calms the foaming of slag that occurs during slag discharge, and a foaming calming method using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described. The foaming calming material according to this embodiment is a mixture of an organic compound and at least one inorganic material, and the volume of gas generated when completely combusted is Vg T (Nm 3 / kg) is 0.4 or more and less than 2.0, and the apparent density of the mixture is 1300 kg / m 3 The present invention is characterized in that:
[0018] As described above, it is known that the calming material destroys the foam layer by utilizing the volume expansion energy generated when gasifying in the foaming slag. Therefore, it is considered that the larger the gas generation volume of the calming material, the larger the volume expansion energy, and the easier it is to destroy the foam layer of the foaming slag. On the other hand, the inventors have confirmed that when suppressing foaming of slag discharged from a converter to a slag pan, a substance with an excessively large gas generation volume has a small apparent density, cannot settle in the foaming slag, and reacts on the surface layer of the foaming slag, so that a clear calming effect cannot be obtained. In addition, even if the apparent density is increased and the substance is allowed to settle in the foaming slag, it may cause re-foaming of the slag, which leads to an extension of the slag discharge time. In other words, it has been found that when suppressing foaming of slag discharged from a converter to a slag pan, it is necessary to control the gas generation volume of the calming material to an appropriate range.
[0019] However, the method for accurately calculating the actual gas generation volume when the tranquilizer gasifies is unclear, and it has been difficult to design a tranquilizer with an appropriate composition. One of the reasons for this is that it is not clear under what conditions the gas generated by the tranquilizer in the foaming slag is generated. This is because the foaming slag into which the tranquilizer is added contains inert CO gas, and the gas generation volume from the tranquilizer added to such an inert gas atmosphere changes continuously depending on the progress of the decomposition reaction of the gas generated from the tranquilizer, making it difficult to identify.
[0020] Therefore, the inventors of the present invention have studied a method for clarifying the gas generation volume from the silencing material added to the foamed slag. As a result, taking into consideration the oxygen supplied from the foamed slag, the inventors have found the gas generation volume generated when the hydrogen, carbon, etc. in the silencing material are completely burned by the oxygen, and have confirmed that there is a statistically high correlation between the gas generation volume generated in the case of complete combustion and the slag silencing effect of the silencing material.
[0021] Considering the oxygen supply from the foamed slag is extremely important in searching for materials with high gas generation volumes. The gas generated by the thermal decomposition of the quenching agent supplied into the foamed slag comes into contact with the molten slag over a wide area, and oxygen is instantly shared by the lower oxides, such as FeO and MnO, contained in the molten slag.
[0022] Here, a method for calculating the gas generation volume will be described. The foaming calming material according to this embodiment is a mixture of an organic compound and one or more inorganic materials. Here, the gas generation volume from the calming material is mainly the volume of gas from the organic compound, but the inorganic material may also contain a gas generating component. The gas generating component contained in the inorganic material is typically hydrogen, and is contained in water, hydrates, hydroxides, etc. These also effectively act on the slag calming effect. Therefore, in this embodiment, when the calming material contains n types of inorganic materials, the gas generation volume from each of the inorganic materials when the hydrogen contained in each of the inorganic materials is completely combusted is summed up to calculate the gas generation volume (Nm 3 / kg) can be calculated.
[0023] In other words, the volume of gas generated from an organic compound when it is completely burned is V g O (Nm 3 / kg), and the gas generation volume when hydrogen contained in each of the n inorganic materials is completely combusted is V g I 1. V g I 2. V g I 3. V g I n (Nm 3 / kg), the volume of gas generated from the sedative V g T (Nm 3 / kg) can be calculated using the following formula (1). V g T =V g O +V gI 1+V g I 2+V g I 3+···+V g I n ) ···(1)
[0024] Also, the chemical formula of the organic compound is C a H b O c (For polymer compounds, the values are in parentheses.) When completely combusted, the volume of gas generated from the organic compound is V g 0 can be calculated using the following equation (2). V g O =22.4 W O / 100 (a+0.5 b) / (12 a+b+16 c) (2)
[0025] Here, W O represents the percentage (mass%) of organic compounds in the sedative. In addition, a represents the total number of carbon atoms in the chemical formula of the organic compound, b represents the total number of hydrogen atoms in the chemical formula of the organic compound, and c represents the total number of oxygen atoms in the chemical formula of the organic compound. For organic compounds that do not contain oxygen, c = 0. For example, cellulose (C6H 10 O5) n In the case of a sedative material containing 50% by mass, the gas generation volume V from cellulose in the case of complete combustion is g O is 0.8Nm 3 / kg.
[0026] In addition, when a sedative contains multiple types of organic compounds, it may be difficult to identify, quantify, and estimate the types and compositions of all the organic compounds. Therefore, the chemical formula of one representative organic compound contained in the sedative is used, and the W o The total ratio of multiple organic compounds in the sedative is used to calculate the gas generation volume V from the organic compounds. g OThe standard for defining a representative organic compound here is, for example, that an organic compound that has the highest ratio (mass%) and accounts for 25 mass% or more of the total of the multiple organic compounds is regarded as a representative organic compound. On the other hand, if the sedative contains multiple organic compounds and each organic compound can be identified, the gas generation volume from each organic compound is calculated using formula (1) for each organic compound, and the sum of these is calculated as the gas generation volume V from the organic compounds contained in the sedative. g O It may be calculated as:
[0027] If the main composition of the organic compound is unknown, you can use the following procedure to find the compound with formula C a H b O c It is also possible to estimate a, b, and c and obtain them. For example, in a combustion tube, a sample of the organic compound is burned together with CuO, an oxidizing agent that promotes complete combustion, and then, in two subsequent U-shaped tubes, a calcium chloride tube absorbs H2O and a soda lime tube absorbs CO2, and the masses of absorbed H2O and CO2 are obtained. In this case, instead of directly quantifying O alone, the masses of all elements other than O are subtracted from the mass of the sample, and the molar ratio of each element is obtained by dividing the mass [g] of each element by its atomic weight. Since the ratio of the amounts of substance of each element represents the ratio of the number of atoms, it is possible to obtain a, b, and c in the chemical formula by obtaining the simplest integer ratio and making it into a composition formula that represents the organic compound. Alternatively, the chemical formula may be obtained by analyzing spectral data obtained by physical techniques such as nuclear magnetic resonance, mass spectrometry, infrared spectroscopy, and ultraviolet-visible spectroscopy.
[0028] On the other hand, the gas generation volume when hydrogen contained in inorganic materials is completely burned can be measured by the temperature programming method or the thermal conductivity method. When the contained substance is water or a hydrate, it can be measured by the Karl Fischer method or the like as specified in JIS K 0068: 2001.
[0029] Next, the organic compounds and inorganic materials contained in the foaming calming material according to this embodiment will be described. As described above, in this embodiment, the gas generation volume V from the calming material in the case of complete combustion is calculated based on the gas generation volume calculated using the formula (2). g T 0.4Nm 3 An organic compound is selected that satisfies the above-mentioned solubility requirement of 1.0 to 2.0 / kg. As can be seen from formula (2), the more hydrogen there is in the chemical formula, the more preferable it is, and the less oxygen there is, the more the gas generation volume tends to increase. In addition, from the viewpoint of producing the sedative at low cost, it is preferable to use recyclable waste materials such as PET bottles and discarded plastics.
[0030] In addition, the inorganic material contained in the tranquilizer according to this embodiment is mainly non-combustible, and the apparent density of the tranquilizer is 1300 kg / m 3 There is no particular limitation on the type of material, so long as it can be mixed to achieve the above results. However, from the viewpoint of inexpensively producing the sedative, it is preferable that the sedative be a waste or by-product that can be obtained inexpensively in a steelworks, such as slag, dust, concrete, or refractory material. Here, refractory material refers to waste of composite inorganic materials, such as bricks, generated in various processes, such as pig iron making, steel making, and rolling processes, and concrete refers to waste of composite inorganic materials generated during demolition work, etc. In addition, slag is a by-product of composite inorganic materials that contain various oxides and is generated in the pig iron making or steel making process, and dust is a by-product of composite inorganic materials that contain various substances attached to filters, etc.
[0031] Although some of these wastes or by-products can be recycled within the plant or used as roadbed materials, the demand is small compared to the amount generated, and most of the remaining wastes are disposed of in landfills at great expense. Therefore, if these can be used as foaming sedation materials, raw material costs and disposal costs can be reduced. For example, refractories can be easily obtained by collecting refractories dismantled due to deterioration or wear, and then crushing and magnetically separating them. In addition, concrete generated during construction work within the plant is often difficult to reuse, and it has been confirmed that it can be reused by mixing it with this sedation material. These have a relatively high density and are effective in increasing the apparent density. In addition, they can be used regardless of their composition. This is because the density does not depend much on the composition. In addition, not only one type of inorganic material but two or more types may be mixed.
[0032] Next, the conditions for the foaming suppression material made of the mixture of the organic compound and inorganic material described above will be described. As described above, in order to obtain the foaming suppression effect, the suppression material must be a mixture of the organic compound and inorganic material described above, and the volume of gas generated when completely combusted must be less than V. g T But 0.4Nm 3 / kg or more, 2.0Nm 3 The volume of gas generated during complete combustion must be less than V / kg. g T But 0.4Nm 3 If the volume expansion energy is less than 1 / kg, the foam layer of the foamed slag cannot be destroyed sufficiently due to insufficient volume expansion energy. g T is 2.0Nm 3When the molten iron is discharged with the slag into the slag ladle, the iron pellets contained in the slag and the molten iron discharged with the slag into the slag ladle are vigorously stirred by the large amount of gas generated, and the carbon in the molten iron and the iron pellets react with the FeO and MnO components in the slag, increasing the rate of CO gas generation. g T is 1.0Nm 3 / kg.
[0033] However, the inventors have found that even if the gas generation volume of the sedative is appropriately controlled, if the apparent density is low, a sufficient sedative effect cannot be obtained. 3 / kg or more, 2.0Nm 3 / kg, and the apparent density must be increased to a certain value or more. This is because when the foamed slag, which has become hot in the converter, is discharged into the slag ladle at room temperature, the foamed slag cools and a solidified, high-density slag layer covers the surface of the foamed slag. Also, the viscosity of the foamed slag increases as it cools, so the apparent density must be increased in order to increase the settling speed of the settling material.
[0034] In this embodiment, the apparent density of the sedative is 1300 kg / m 3 By setting the density to 1,800 kg / m or more, the foaming slag in the slag ladle can be quickly settled during intermediate slag removal. 3 More preferably, it is 2000 kg / m 3 That's all. In general, the density of organic compounds that are burned and gasified is low, so the apparent density of the sedative tends to decrease as the ratio of organic compounds increases. Therefore, it is preferable that the inorganic material to be mixed with the organic compound is a material with a relatively high apparent density.
[0035] Regarding the particle size of the tranquilizer, when the tranquilizer is added directly to the foamed slag without being placed in a container such as a hemp bag or a plastic bag, it is preferable that the ratio of particles with a particle size of 5 mm or more is 50% by mass or more. By making the ratio of particles with a particle size of 5 mm or more 50% by mass, scattering of the tranquilizer due to gases, etc., ejected from the foamed slag is suppressed, and the ratio of particles that can reach deeper into the slag is increased, resulting in a higher tranquilizing effect. More preferably, the ratio of particles with a particle size of 5 mm or more is 60% by mass or more. Also, if the ratio of particles with a large particle size is too large, the time required for the tranquilizer to react in the foamed slag increases, and the foamed slag cannot be efficiently tranquilized, so it is preferable that the ratio of particles with a particle size of 60 mm or less is 50% by mass or more, and more preferably, 60% by mass or more.
[0036] Furthermore, when the sedative is added in a container such as a hemp bag or a plastic bag, the risk of scattering of the sedative until it reaches the foamed slag is small, so particles of fine particle size may be included, but it is preferable that the ratio of particles with particle sizes of 1 mm or more is 50 mass % or more. Also, it is preferable that the ratio of particles with particle sizes of 60 mm or less is 50 mass % or more, and more preferably 60 mass % or more. Here, the above-mentioned particle size and its distribution can be measured, for example, using a sieve such as JIS Z 8801.
[0037] As mentioned above, the volume of gas generated during complete combustion is V g T 0.4Nm 3 / kg or more, 2.0Nm 3 / kg and an apparent density of 1300kg / m 3 In order to achieve the above, the foaming calming effect can be maintained at a high level by mixing 20 to 95 mass% of slag, dust, refractory material, or concrete with the organic compound. It is preferable that the organic compound and inorganic material are mixed in a state of adhesion, and in this case, there are a method of adhering them with a binder such as cement, a method of compressing powdered materials, and a method of fusing materials together. In addition, the organic compound and other inorganic materials may be used as a calming material in a state where they are placed in a container.
[0038] Next, the foaming and settling method of slag using the above-mentioned settling material will be described in detail. In this embodiment, foaming slag in a slag ladle during intermediate slag removal operation will be described as an example, but the present invention can also be applied to operations in other refining vessels. In addition, the temperature of the slag is not limited.
[0039] The slag ladle is added, for example, via a hopper installed near the slag ladle. This hopper is connected to a bunker that stores the slag, and any amount of slag can be added as set by the operator. The timing of adding the slag is preferably when the slag formed in the slag ladle reaches a height of about 4 / 5 of the height of the refining furnace. The slag height may be determined by video observation or visual inspection of the slag ladle. When adding the slag to the converter, for example, there are methods of measuring the lance vibration information, using μ-waves, and predicting the sound level in the furnace.
[0040] Although the slag may be added when the slag height is less than 4 / 5 of the height of the slag ladle, the slag may not be sufficiently foamed, and the slag may not be effective, requiring a larger amount of slag. On the other hand, when the slag height reaches 4 / 5 or more of the height of the slag, the slag may flow out of the slag ladle due to foaming. The effect of the slag can also be achieved when the slag is added after the slag has flowed out of the slag ladle due to foaming.
[0041] Although the preferred embodiment of the present invention has been described above, the present invention is not limited to such an example. It is clear that a person skilled in the art can come up with various modified or revised examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention. EXAMPLES
[0042] Next, an embodiment of the present invention will be described, but the conditions in the embodiment are merely an example of conditions adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to this example of conditions. Various conditions can be adopted in the present invention as long as they do not deviate from the gist of the present invention and achieve the object of the present invention.
[0043] 250t of molten pig iron was charged into a 300t converter, and after adding auxiliary materials and carrying out dephosphorization treatment, the converter was tilted and about 10t of foaming slag in the converter was discharged into a slag ladle outside the furnace. The slag temperature at this time was 1300-1450℃, and the slag composition was CaO = 30-40 mass%, SiO2 = 20-35 mass%, T.Fe = 10-20 mass%, MgO = 5-10 mass%, MnO = 5-10 mass%, P2O5 = 2-5 mass%, and Al2O3 = 0-5 mass%.
[0044] In this experiment, the calming agent, which was a mixture of organic compounds and inorganic materials, was added to the foaming slag in the slag ladle at a rate of 20 kg / min under the conditions shown in Table 1, and the time required for the converter to finish discharging slag was investigated. The time required for the converter to finish discharging slag was measured. The time required for the converter to finish discharging slag was measured from the time the converter started tilting for intermediate discharging to the time the converter was restarted after the completion of discharging. If the foaming calming was insufficient, the converter stopped discharging slag temporarily to prevent the slag from flowing out, and the time required for the converter to finish discharging slag was longer. In other words, the shorter the time required for the foaming calming in the slag ladle, the greater the calming effect of the foaming in the slag ladle. The calming agent was added by a worker who threw the bagged calming agent directly into the center of the foaming slag in the slag ladle.
[0045] Here, each sample was prepared by mixing the organic compounds and inorganic materials in Table 1 in a given ratio and placing them in a 5 kg bag in a vinyl container. Molded PET bottles, polyethylene resin, and soap were used as the organic compounds in Table 1. Representative organic compounds contained in these were polyethylene terephthalate, polyethylene, and soap, respectively, and the gas generation volume V was calculated using the chemical formulas of the representative organic compounds. g O was calculated.
[0046] In addition, slag, refractories, dust, and concrete were used as inorganic materials, and the moisture content of each was measured to determine the gas generation volume V g I 1~V g I 4 was calculated. V in Table 1 g T is the sum of the gas generation volumes of each sample. The apparent density was measured by the method described in JIS Z8807:2012.
[0047] The molten iron temperature measured after the completion of dephosphorization blowing was 1330-1380°C, and the slag composition was CaO = 30-40 mass%, SiO2 = 20-35 mass%, T.Fe = 10-20 mass%, MgO = 5-10 mass%, MnO = 5-10 mass%, P2O5 = 2-5 mass%, and Al2O3 = 0-5 mass%.
[0048] [Table 1]
[0049] The slag in Table 1 was steel slag generated in the converter process, and the refractory material was a mixture of refractory powder and slag powder generated from equipment such as tundishes, blast furnace troughs, converter furnace bodies, KR (Kanbara Reactor) impellers, and RH-type vacuum degassing equipment. The dust was collected dust generated in the sintering, blast furnace, and steelmaking processes, and the concrete was concrete rubble generated as construction waste. The particle size of these inorganic materials and organic compounds was 50% by mass with a particle size of 5 mm or more. The calming material O, No. 15, is a paper waste molding product, which is a mixture of 50% by mass of paper waste and 50% by mass of steel slag, and is formed into a cylindrical mass with a diameter of about 50 mm and a height of about 50 mm. In addition, calming material P No. 16 is made by bagging paper waste and steel slag in ratios of 10% by mass paper waste and 90% by mass steel slag, respectively.
[0050] As shown in Table 1, the gas generation volume Vg T is 0.4Nm 3 / kg or more, 2.0Nm 3 / kg, and the apparent density is 1300kg / m 3 The apparent density of No. 13 and No. 15 was 1300 kg / m 3 The gas generation volume of No. 14 is less than V g T is 2.0Nm 3 / kg or more, No.16 gas generation volume V g T is 0.4Nm 3 / kg.
[0051] The invention examples in Table 1 No.2, No.3, No.6~No.8, No. 12 had a shorter slag draining time and a higher slag settling effect than the comparative examples No. 13 to No. 16. This is because No.2, No.3, No.6~No.8, Gas generation volume V of No. 12 g T is 0.4Nm 3 / kg or more, 2.0Nm 3 / kg, and the apparent density is 2000 kg / m 3 The above is the appropriate gas generation volume V so that the sedative does not settle in the foaming slag and cause reforming of the slag. g T This is thought to be because the sedative reacted quickly and efficiently by controlling the temperature. No.3, No.6~No.8 、 No.12 is, reference The example No.1, No.4, The draining time was shorter than that of No. 5, No. 9 to No. 11. This is because the invention example No. 2 , No.3, No.6~No.8 、 No.12 has an apparent density of 2000 kg / m 3 From the above, it is considered that the reaction occurred after sinking to a deeper part of the foaming slag.
Claims
1. A foaming calming material for calming foaming of slag discharged into a slag ladle, comprising: A mixture of an organic compound and at least one inorganic material, in which the gas generation volume V g T generated when the mixture is completely combusted is 0.4 Nm or less, as calculated by the following formulas (1) and (2): 3 / kg or more, 2.0Nm 3 / kg, and apparent density is 2000kg / m 3 A foaming calming material characterized by the above. V g T =V g O +V g I 1 +V g I 2 +V g I 3 +...+V g I n...(1) V g O =22.4・W O / 100・(a+0.5・b) / (12・a+b+16・c) ... (2) Here, VgO represents the gas generation volume (Nm3 / kg) generated when the organic compound in the mixture is completely combusted, and VgI1, VgI2, VgI3, ... VgIn represent the gas generation volume (Nm3 / kg) generated when hydrogen contained in each inorganic material is completely combusted when n types of inorganic materials are contained in the mixture. Also, WO represents the ratio (mass%) of the organic compound in the foaming calming material, a represents the total number of carbon atoms in the chemical formula C aHbOc of the composition representative of the organic compound, b represents the total number of hydrogen atoms in the chemical formula C aHbOc of the composition representative of the organic compound, and c represents the total number of oxygen atoms in the chemical formula C aHbOc of the organic compound.
2. 2. The foaming calming material of claim 1, wherein the inorganic material comprises one or more of slag, dust, refractory, and concrete.
3. A foaming calming method, comprising adding the foaming calming material according to claim 1 or 2 to foaming slag discharged in a slag ladle.
Citation Information
Patent Citations
Killing material for foaming of converter slag
JP1979032116A
Method for restraining slopping
JP1992180507A
Method for injecting carbonaceous material for restraining slag foaming
JP1993287347A
Foaming supressor for slag
JP1995145417A
Repressing material of foaming slag in containing vessel for molten metal and molten slag
JP1999050124A