Foaming calming material and foaming calming method using same

A mixture of organic and inorganic materials with specific gas generation and density properties effectively suppresses slag foaming in steelmaking converters, addressing the inefficiencies of conventional sedatives and enhancing operational stability.

JP7572622B2Active Publication Date: 2024-10-24NIPPON STEEL CORPORATION
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2021004789
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-15
Publication Date
2024-10-24
Estimated Expiration
2041-01-15

AI Technical Summary

Technical Problem

Conventional sedative materials fail to effectively suppress slag foaming during high-speed oxygen supply in steelmaking converters, leading to increased costs and operational disruptions, and the need for continuous large-scale sedative addition.

Method used

A foaming suppressant material composed of a mixture of organic compounds and inorganic materials, with a gas generation volume of 1.0 Nm³/kg or more and an apparent density of 1000 kg/m³, designed to quickly destroy the foam layer by generating sufficient volumetric expansion energy.

Benefits of technology

The material efficiently and quickly suppresses slag foaming, reducing operational disruptions and costs by ensuring effective settling and gasification within the slag, thereby extending blowing time and improving production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572622000001
    Figure 0007572622000001
Patent Text Reader

Abstract

To provide a foaming suppressor that can suppress the foaming of the slag generated during blowing efficiently and quickly, and a foaming suppressing method using the same.SOLUTION: A foaming suppressor is to suppress the foaming of the slag in a converter. The foaming suppressor is a mixture of an organic compound and at least one inorganic material. The volume of a gas generated in burning completely it is 1.0 Nm3 / kg or more. The apparent density is 1000 kg / m3 or more. Preferably the inorganic material includes one or more of slag, dust, refractory, and concrete.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a foaming suppression material for suppressing foaming of slag in a converter and a foaming suppression method using the same. [Background technology]

[0002] During or after the refining process of molten iron, the slag foams due to CO bubbles generated by the reaction of C in the molten iron with FeO (iron oxide) in the slag at the interface between the molten iron and steelmaking slag (hereinafter referred to as slag), or CO bubbles generated by the reaction of FeO in the slag with C in the iron particles contained in the slag inside the slag itself (hereinafter referred to as foaming). If this foaming of the slag is severe, the 1300-1500°C slag may overflow from the refining equipment or the transport vessel, and if the refining equipment or the transport vessel is damaged, it will take a lot of time and effort to restore it. If the FeO concentration in the slag is high, a large amount of CO bubbles will be generated, so slag with a high FeO concentration has a strong foaming tendency (it expands rapidly and easily overflows).

[0003] In order to calm the foaming of the slag, it is necessary to destroy the layer in which the CO bubbles remain (hereafter referred to as the foam layer) and shrink the slag. A commonly known method for this purpose is to add a mass of material (calming material) that gasifies inside the slag to the slag, and to use the volume expansion energy generated when the mass is gasified by pyrolysis to destroy the foam layer.

[0004] Here, as one of the smelting processes for molten iron, a multi-function converter process is generally known in which after dephosphorization in a converter, a part of the slag is discharged (intermediate discharge) into a slag ladle outside the furnace, and the decarburization process is continued in the same converter. In this multi-function converter process, if the foaming of the slag becomes so severe during the dephosphorization blow that the slag is about to overflow from the throat of the converter, the dephosphorization blow must be interrupted, and the progress of the dephosphorization reaction becomes insufficient. Therefore, in order to increase the dephosphorization rate in the next decarburization blow, it is necessary to add extra CaO to the converter, which leads to an increase in refining costs and an increase in the amount of slag generated. In addition, when slag foaming progresses in the slag ladle that receives the slag during intermediate slag removal, if the slag is about to overflow from the slag ladle, intermediate slag removal must be interrupted. As a result, the weight of P2O5 in the slag remaining in the converter increases, and phosphorus is re-recovered during decarburization blowing, so extra CaO must be added to the converter. Furthermore, in decarburization blowing, if slag foaming progresses too rapidly, there is a concern that the slag will flow out of the converter throat when the converter is tilted during tapping. For these reasons, it is necessary to add a silencing material to the converter during dephosphorization and decarburization, and to the slag ladle during intermediate slag removal. Usually, such agglomerates that have a destructive effect are called silencing materials, and examples of such silencing materials are disclosed in Patent Documents 1 to 8. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 54-32116 [Patent Document 2] Japanese Patent Application Publication No. 4-180507 [Patent Document 3] Japanese Patent Application Publication No. 5-287347 [Patent Document 4] Japanese Patent Application Publication No. 7-145417 [Patent Document 5] Japanese Patent Application Publication No. 11-50124 [Patent Document 6] JP 2008-255446 A [Patent Document 7] JP 2009-270178 A [Patent Document 8] JP 2009-287050 A Summary of the Invention [Problem to be solved by the invention]

[0006] On the other hand, in recent years, in order to improve the production capacity of converters, the oxygen supply rate from the top blowing lance of the converter has been increased. Under such operating conditions, the generation rate of CO gas, which causes foaming, increases, and the conventional silencing materials described in the above Patent Documents 1 to 8 cannot sufficiently suppress the outflow of foaming slag from the converter. In addition, in order to suppress foaming in such a high-speed oxygen supply operation, a large amount of silencing material needs to be added continuously, which increases the cost of the silencing material.

[0007] In view of the above-mentioned problems, the present invention has an object to provide a foaming suppression material that efficiently and quickly suppresses slag foaming that occurs during blowing, and a foaming suppression method using the same. [Means for solving the problem]

[0008] In order to solve the above problems, the inventors of the present invention have investigated important factors for quenching the foaming of slag. As a result, it was found that the foaming quenching effect obtained by adding a quenching agent is related to the gas generation volume (Nm) of the quenching agent at high temperature. 3 / kg) and the apparent density of the sedative (kg / m 3 It was found that the foaming of slag can be rapidly suppressed by satisfying certain conditions for the gas generation volume and the apparent density of the suppressing material.

[0009] In addition, in order to increase the gas generation volume, it is important that the tranquilizer contains an organic compound, and in order to increase the apparent density, it is important that the tranquilizer contains an inorganic material. Therefore, assuming that the gas generation volume from a tranquilizer consisting of a mixture of organic compounds and inorganic materials is complete combustion, it is assumed that the gas generation volume is 1.0 Nm 3 / kg or more and the apparent density is 1000kg / m 3 The inventors have discovered that adding the above-mentioned calming agent to the foaming slag makes it possible to quickly calm the foaming of the slag.

[0010] Here, the gas generation volume is the volume of gas (Nm3) generated per 1 kg of silencing material when the silencing material comes into contact with the foamed slag and is completely combusted. 3 / kg), and can be measured, for example, by heating a sample in an oxygen-containing atmosphere and collecting the generated gas in a bag, and the gas generation volume can be calculated using the components and composition of the quenching material. In addition, the apparent density is the density of the molded product including the volume of the pores contained inside the molded product when the quenching material is solid. In the case where the foaming quenching material is made of multiple solids made of different materials, the apparent densities are averaged using the apparent densities and ratios of each solid, and the average value may be used as the apparent density of the foamed slag. In the present invention, since there is almost no difference between the apparent density and the bulk density, the apparent density may be used as the bulk density. The apparent density can be measured, for example, by the method described in JIS Z8807:2012.

[0011] The present invention has been made based on the above findings, and the gist of the present invention is as follows. (1) A foaming calming material for calming slag foaming in a converter, comprising: A mixture of an organic compound and at least one inorganic material, The volume of gas generated when the mixture is completely combusted is V g T In this case, it is calculated using the following formulas (1) and (2). Gas generation volume V g T is 1.5 Nm 3 / kg or more, and the apparent density is 1000kg / m 3 A foaming calming material characterized by the above. V g T =V g O +V g I 1 +V g I 2 +V g I 3 +···+V g I n ···(1) V g O =22.4·W O / 100 (a+0.5 b) / (12 a+b+16 c) ···(2) Here, V g O is the gas generation volume (Nm m) generated when the organic compound in the mixture is completely combusted. 3 / kg), and V g I 1 、V g I 2 、V g I 3 、···V g I n is the gas generation volume (Nm m) generated when the hydrogen contained in each inorganic material is completely combusted when the mixture contains n types of inorganic materials. 3 / kg). Also, W O represents the proportion (mass%) of the organic compound in the foaming calming material, and a represents the chemical formula C a H b O c represents the total number of carbon atoms in the organic compound represented by the chemical formula C a H b O c represents the total number of hydrogen atoms in the organic compound represented by the chemical formula C a H b O c represents the total number of oxygen atoms in

[0013] (2) The inorganic material includes at least one of slag, dust, refractory, and concrete. (1) The foaming calming material described in.

[0015] (3) Apparent density 1500kg / m 3 The above (1) characterized in that Or (2) 2. The foaming calming material according to claim 1 .

[0016] (4) Above (1)~ (3) 13. A foaming stabilization method, comprising adding the foaming stabilization material according to any one of claims 1 to 12 to slag undergoing foaming in a converter. Effect of the Invention

[0017] According to the present invention, it is possible to provide a foaming suppression material that efficiently and quickly suppresses slag foaming that occurs during blowing, and a foaming suppression method using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described. The foaming calming material according to this embodiment is a mixture of an organic compound and at least one inorganic material, and the volume of gas generated when completely combusted is Vg T (Nm 3 / kg) is 1.0 or more, and the apparent density of the mixture is 1000 kg / m 3 The present invention is characterized in that:

[0019] As mentioned above, it is known that the sedative material destroys the foam layer by utilizing the volume expansion energy generated when gasifying in the foamed slag. Therefore, it is considered that the larger the gas generation volume of the sedative material, the larger the volume expansion energy becomes, and the easier it is to destroy the foam layer of the foamed slag. Therefore, it is necessary to select a material for the sedative material that will generate a large gas volume when it gasifies.

[0020] However, the method for accurately calculating the actual gas generation volume when the tranquilizer gasifies is unclear, and it has been difficult to design a tranquilizer with an appropriate composition. One of the reasons is that it is not clear under what conditions the gas generated by the tranquilizer in the foaming slag is generated. This is because the foaming slag into which the tranquilizer is added contains inert CO gas, and the gas generation volume from the tranquilizer added to such an inert gas atmosphere changes continuously depending on the progress of the decomposition reaction of the gas generated from the tranquilizer, making it difficult to identify.

[0021] Therefore, the inventors of the present invention have studied a method for clarifying the gas generation volume from the silencing material added to the foamed slag. As a result, taking into consideration the oxygen supplied from the foamed slag, the inventors have found the gas generation volume generated when the hydrogen, carbon, etc. in the silencing material are completely burned by the oxygen, and have confirmed that there is a statistically high correlation between the gas generation volume generated in the case of complete combustion and the slag silencing effect of the silencing material.

[0022] Considering the oxygen supply from the foamed slag is extremely important in searching for materials with high gas generation volumes. The gas generated by the thermal decomposition of the quenching agent supplied into the foamed slag comes into contact with the molten slag over a wide area, and oxygen is instantly shared by the lower oxides, such as FeO and MnO, contained in the molten slag.

[0023] Here, a method for calculating the gas generation volume will be described. The foaming calming material according to this embodiment is a mixture of an organic compound and one or more inorganic materials. Here, the gas generation volume from the calming material is mainly the volume of gas from the organic compound, but the inorganic material may also contain a gas generating component. The gas generating component contained in the inorganic material is typically hydrogen, and is contained in water, hydrates, hydroxides, etc. These also effectively act on the slag calming effect. Therefore, in this embodiment, when the calming material contains n types of inorganic materials, the gas generation volume from each of the inorganic materials when the hydrogen contained in each of the inorganic materials is completely combusted is summed up to calculate the gas generation volume (Nm 3 / kg) can be calculated.

[0024] In other words, the volume of gas generated from an organic compound when it is completely burned is V g O (Nm 3 / kg), and the gas generation volume when hydrogen contained in each of n types of inorganic materials is completely combusted is V g I 1. V g I 2. V g I 3. V g I n (Nm 3 / kg), the volume of gas generated from the sedative V g T (Nm 3 / kg) can be calculated using the following formula (1). V g T =V g O +V g I 1+V g I 2+V g I 3+···+V g I n ) ···(1)

[0025] Also, the chemical formula of the organic compound is C a Hb O c (For polymer compounds, the values ​​are in parentheses.) When completely combusted, the volume of gas generated from the organic compound is V g 0 can be calculated using the following equation (2). V g O =22.4 W O / 100 (a+0.5 b) / (12 a+b+16 c) (2)

[0026] Here, W O represents the percentage (mass%) of organic compounds in the sedative. Also, a represents the total number of carbon atoms in the chemical formula of the organic compound, b represents the total number of hydrogen atoms in the chemical formula of the organic compound, and c represents the total number of oxygen atoms in the chemical formula of the organic compound. For organic compounds that do not contain oxygen, c = 0. For example, cellulose (C6H 10 O5) n In the case of a sedative material containing 50% by mass, the gas generation volume V from cellulose in the case of complete combustion is g O is 0.8Nm 3 / kg.

[0027] In addition, when a sedative contains multiple types of organic compounds, it may be difficult to identify, quantify, and estimate the types and compositions of all the organic compounds. Therefore, the chemical formula of one representative organic compound contained in the sedative is used, and the W o The total ratio of multiple organic compounds in the sedative is used to calculate the gas generation volume V from the organic compounds. g O The standard for defining a representative organic compound here is, for example, that an organic compound that has the highest ratio (mass%) and accounts for 25 mass% or more of the total of the multiple organic compounds is regarded as a representative organic compound. On the other hand, if the sedative contains multiple organic compounds and each organic compound can be identified, the gas generation volume from each organic compound is calculated using formula (1) for each organic compound, and the sum of these is calculated as the gas generation volume V from the organic compounds contained in the sedative.g O It may be calculated as:

[0028] If the main composition of the organic compound is unknown, you can use the following procedure to find the compound with formula C a H b O c It is also possible to estimate a, b, and c and obtain them. For example, in a combustion tube, a sample of the organic compound is burned together with CuO, an oxidizing agent that promotes complete combustion, and then, in two subsequent U-shaped tubes, a calcium chloride tube absorbs H2O and a soda lime tube absorbs CO2, and the masses of absorbed H2O and CO2 are obtained. In this case, instead of directly quantifying O alone, the masses of all elements other than O are subtracted from the mass of the sample, and the molar ratio of each element is obtained by dividing the mass [g] of each element by its atomic weight. Since the ratio of the amounts of substance of each element represents the ratio of the number of atoms, it is possible to obtain a, b, and c in the chemical formula by obtaining the simplest integer ratio and making it into a composition formula that represents the organic compound. Alternatively, the chemical formula may be obtained by analyzing spectral data obtained by physical techniques such as nuclear magnetic resonance, mass spectrometry, infrared spectroscopy, and ultraviolet-visible spectroscopy.

[0029] On the other hand, the gas generation volume when hydrogen contained in inorganic materials is completely burned can be measured by the temperature programming method or the thermal conductivity method. When the contained substance is water or a hydrate, it can be measured by the Karl Fischer method or the like as specified in JIS K 0068: 2001.

[0030] Next, the organic compounds and inorganic materials contained in the foaming calming material according to this embodiment will be described. As described above, in this embodiment, the gas generation volume V from the calming material in the case of complete combustion is calculated based on the gas generation volume calculated using the formula (2). g T is 1.0Nm 3 / kg or more. As can be seen from formula (2), the more hydrogen there is in the chemical formula, the more the volume of gas generated is likely to be large. In addition, from the viewpoint of producing the sedative at low cost, it is preferable to use recyclable waste materials such as PET bottles and discarded plastics.

[0031] In addition, the inorganic material contained in the tranquilizer according to this embodiment is mainly non-combustible, and the apparent density of the tranquilizer is 1000 kg / m 3 There is no particular limitation on the type of material, so long as it can be mixed to achieve the above results. However, from the viewpoint of inexpensively producing the sedative, it is preferable that the sedative be a waste or by-product that can be obtained inexpensively in a steelworks, such as slag, dust, concrete, or refractory material. Here, refractory material refers to waste of composite inorganic materials, such as bricks, generated in various processes, such as pig iron making, steel making, and rolling processes, and concrete refers to waste of composite inorganic materials generated during demolition work, etc. In addition, slag is a by-product of composite inorganic materials that contain various oxides and is generated in the pig iron making or steel making process, and dust is a by-product of composite inorganic materials that contain various substances attached to filters, etc.

[0032] Although some of these wastes or by-products can be recycled within the plant or used as roadbed materials, the demand is small compared to the amount generated, and most of the remaining wastes are disposed of in landfills at great expense. Therefore, if these can be used as foaming sedation materials, raw material costs and disposal costs can be reduced. For example, refractories can be easily obtained by collecting refractories dismantled due to deterioration or wear, and then crushing and magnetically separating them. In addition, concrete generated during construction work within the plant is often difficult to reuse, and it has been confirmed that it can be reused by mixing it with this sedation material. These have a relatively high density and are effective in increasing the apparent density. In addition, they can be used regardless of their composition. This is because the density does not depend much on the composition. In addition, not only one type of inorganic material but two or more types may be mixed.

[0033] Next, the conditions for the foaming suppression material made of the mixture of the organic compound and inorganic material described above will be described. As described above, in order to obtain the foaming suppression effect, the suppression material must be a mixture of the organic compound and inorganic material described above, and the volume of gas generated when completely combusted must be less than V. g T But 1.0Nm 3 The volume of gas generated during complete combustion must be V / kg or more. g T But 1.0Nm 3 If the volume expansion energy is less than 1 / kg, the foam layer of the foamed slag cannot be sufficiently destroyed due to insufficient volume expansion energy. g T is 1.5Nm 3 / kg or more, more preferably 1.7 Nm 3 / kg or more. The volume of gas generated during complete combustion is V g T There is no particular upper limit to the gas generation volume. However, if the gas generation volume is too large, the expansion energy may cause part of the foaming slag to erupt from the throat of the converter. Therefore, the upper limit should be 3.0 Nm. 3 It is preferable to set the concentration to 1 / kg or less.

[0034] However, the inventors have found that even if the gas generation volume of the sedative is increased, if its apparent density is low, a sufficient sedative effect cannot be obtained. In other words, it is necessary to increase both the gas generation volume and the apparent density of the sedative to a certain value or more. This is because, when the sedative is added to the foamed slag, the higher the apparent density of the sedative, the deeper the slag sinks, and the deeper the slag gasifies and expands, so that the foam layer of the foamed slag is easily destroyed.

[0035] In this embodiment, the apparent density of the sedative is 1000 kg / m 3 By setting the apparent density at 1500 kg / m or more, foaming slag generated during blowing in a refining furnace can be quickly calmed down. 3More preferably, it is 1800 kg / m 3 That's all. In general, the density of organic compounds that are burned and gasified is low, so the apparent density of the sedative tends to decrease as the ratio of organic compounds increases. Therefore, it is preferable that the inorganic material to be mixed with the organic compound is a material with a relatively high apparent density.

[0036] In addition, as the particle size distribution of the calming agent, the ratio of particles having a particle size of 5 mm or more is preferably 50% by mass or more. By making the ratio of particles having a particle size of 5 mm or more 50% by mass, when the calming agent is added to the foaming slag of the converter, scattering of the calming agent caused by gases and the like ejected from the throat as the slag metal reaction in the converter progresses is suppressed, and the ratio of the calming agent that can reach a deeper part of the slag is increased, so that a higher calming effect can be obtained. More preferably, the ratio of particles having a particle size of 5 mm or more is 60% by mass or more. Also, if the ratio of particles having a large particle size is too large, the time required for the calming agent to react in the foaming slag is extended, and the foaming slag cannot be efficiently calmed, so that the ratio of particles having a particle size of 100 mm or less is preferably 50% by mass or more, more preferably 60% by mass or more. Here, the above-mentioned particle size and its distribution can be measured, for example, using a sieve such as JIS Z 8801.

[0037] As mentioned above, the volume of gas generated during complete combustion is V g T is 1.0Nm 3 / kg or more and the apparent density is 1000kg / m 3 In order to achieve the above, the foaming calming effect can be maintained at a high level by mixing 25 to 75 mass% of slag, dust, refractory material, or concrete with the organic compound. It is preferable that the organic compound and inorganic material are mixed in a state of adhesion, and in this case, there are a method of adhering them with a binder such as cement, a method of compressing powdered materials, and a method of fusing materials together. In addition, the organic compound and other inorganic materials may be used as a calming material in a state where they are placed in a container.

[0038] Next, a method for foaming and settling slag using the above-mentioned settling material will be described in detail. Although the present embodiment will be described taking converter operation as an example, the converter operation is not limited to the temperature of the slag.

[0039] The addition of the tranquilizing agent to the refining furnace is performed, for example, through a hopper installed near the refining furnace. This hopper is connected to a bunker that stores the tranquilizing agent, and it is possible to add any amount of tranquilizing agent set by an operator. As for the timing of adding the tranquilizing agent, it is preferable to add the tranquilizing agent of the material described later when the slag formed in the refining furnace reaches a height of about 4 / 5 of the height of the refining furnace. The method of measuring the slag height includes, for example, a method of measuring using vibration information of a lance, a method of measuring using μ-waves, and a method of predicting the height from the sound level in the furnace.

[0040] The silencing agent may be added under the condition that the slag height is lower than 4 / 5 of the height of the refining furnace, but the silencing effect of the silencing agent may decrease and the amount of silencing agent required may increase if the slag is not sufficiently foamed. On the other hand, if the slag height reaches 4 / 5 or more of the height of the refining furnace, the slag may flow out of the furnace throat due to foaming. It is preferable to add the silencing agent before the slag flows out of the furnace throat due to foaming, but the effect is also achieved when the silencing agent is added after the slag flows out of the furnace throat of the refining furnace due to foaming.

[0041] Although the preferred embodiment of the present invention has been described above, the present invention is not limited to such an example. It is clear that a person skilled in the art can come up with various modified or revised examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention. EXAMPLES

[0042] Next, an embodiment of the present invention will be described, but the conditions in the embodiment are merely an example of conditions adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to this example of conditions. Various conditions can be adopted in the present invention as long as they do not deviate from the gist of the present invention and achieve the object of the present invention.

[0043] 250t of molten iron was charged into a 300t converter, auxiliary materials were added, and 4Nm of molten iron was blown from the top lance. 3 Dephosphorization was performed by blowing oxygen into the molten iron at a rate of 1 / min / t.

[0044] Five minutes after the start of the dephosphorization blowing, a mixture of organic compounds and inorganic materials was added to the converter from above at a rate of 50 kg / min under the conditions shown in Table 1, and the blowing was interrupted just before the slag overflowed from the converter throat.

[0045] Here, each sample was made by mixing the organic compound and inorganic material in Table 1 and molding the mixture. Molded PET bottles, polyethylene resin, and soap were used as the organic compounds in Table 1. Representative organic compounds contained in these are polyethylene terephthalate, polyethylene, and soap, respectively, and the gas generation volume V was calculated using the chemical formulas of the representative organic compounds. g O was calculated.

[0046] In addition, slag, refractories, dust, and concrete were used as inorganic materials, and the moisture content of each was measured to determine the gas generation volume V g I 1~V g I 4 was calculated. V in Table 1 g T is the sum of the gas generation volumes of each sample. The apparent density was measured by the method described in JIS Z8807:2012.

[0047] The molten iron temperature measured after the completion of dephosphorization blowing was 1330-1380°C, and the slag composition was CaO = 30-40 mass%, SiO2 = 20-35 mass%, T.Fe = 10-20 mass%, MgO = 5-10 mass%, MnO = 5-10 mass%, P2O5 = 2-5 mass%, and Al2O3 = 0-5 mass%.

[0048] In addition, under conditions where the foaming stabilization effect is high, the foaming of the slag in the converter quickly settles, and the blowing time becomes longer. Therefore, the slag stabilization effect under those conditions was evaluated from the blowing time.

[0049] [Table 1]

[0050] The slag in Table 1 was steel slag generated in the converter process, and the refractory material was a mixture of refractory powder and slag powder generated from equipment such as tundishes, blast furnace runners, converter furnace bodies, KR (Kanbara Reactor) impellers, and RH-type vacuum degassing equipment. The dust was collected dust generated in the sintering, blast furnace, and steelmaking processes, and the concrete was concrete rubble generated as construction waste. The particle size of these inorganic materials and organic compounds was 50% by mass with a particle size of 5 mm or more. The calming material N, No. 14, is a paper waste molding product, which is a mixture of 50% by mass of paper waste and 50% by mass of steel slag, and is formed into a cylindrical mass with a diameter of about 50 mm and a height of about 50 mm.

[0051] As shown in Table 1, the gas generation volume V g T is 1.0Nm 3 / kg or more, and the gas generation volume V g T The apparent density of No. 1 to No. 11 and No. 13 was less than 1000 kg / m 3 However, the apparent density of No. 12 was 1000 kg / m 3 It was less than.

[0052] The invention examples in Table 1 No.4, No.6 No. 11 had a longer blowing time than No. 14, which was a comparative example, and showed a high slag stabilization effect. No.4, No.6 The blowing time of No. 11 was longer than that of the comparative example No. 12. This is because the apparent density of No. 12 was 1000 kg / m 3 It is considered that the reaction occurred because the amount of the slag was less than 100g, and the slag did not sink sufficiently in the foaming slag. No.4, No.6 No. 11 had a longer blowing time than No. 13, which was a comparative example. This is because the gas generation volume V g T is 1.0Nm 3 / kg, which is thought to be because the actual volume of gas generated was small.

[0053] Also, examples of inventions N Gas generation volume V when No.4 and No.6 to No.11 are completely burned g T is 1.5Nm 3 No. 2, No. 5 to No. 7, No. 9 and No. 11 had an apparent density of 1500 kg / m 3 Among them, No. 6, No. 7, No. 9 and No. 11 have the highest gas generation volume V g T is 1.5Nm 3 / kg or more and an apparent density of 1500kg / m 3 Therefore, the blowing time was longer than the other invention examples. This is thought to be because the slag settled deeper in No.6, No.7, No.9 and No.11, and a larger amount of gas was generated, which improved the slag settling effect.

Claims

1. A foaming calming material for calming slag foaming in a converter, comprising: A mixture of an organic compound and at least one inorganic material, in which the gas generation volume V g T generated when the mixture is completely combusted is 1.5 Nm 3 / kg or more, and the apparent density is 1000 kg / m 3 A foaming calming material characterized by the above. V g T =V g O +V g I 1 +V g I 2 +V g I 3 +...+V g I n...(1) V g O =22.4・W O / 100・(a+0.5・b) / (12・a+b+16・c) ・・・(2) Here, VgO represents the gas generation volume (Nm3 / kg) generated when the organic compound in the mixture is completely combusted, and VgI1, VgI2, VgI3, ... VgIn represent the gas generation volume (Nm3 / kg) generated when hydrogen contained in each inorganic material is completely combusted when n types of inorganic materials are contained in the mixture. Also, WO represents the ratio (mass%) of the organic compound in the foaming calming material, a represents the total number of carbon atoms in the chemical formula C aHbOc of the composition representative of the organic compound, b represents the total number of hydrogen atoms in the chemical formula C aHbOc of the composition representative of the organic compound, and c represents the total number of oxygen atoms in the chemical formula C aHbOc of the organic compound.

2. 2. The foaming calming material of claim 1, wherein the inorganic material comprises one or more of slag, dust, refractory, and concrete.

3. Apparent density: 1500 kg / m 3 The foaming calming material according to claim 1 or 2, characterized in that:

4. A method for stabilizing foaming, comprising adding the foaming stabilizing material according to any one of claims 1 to 3 to slag undergoing foaming in a converter.

Citation Information

Patent Citations

  • Killing material for foaming of converter slag

    JP1979032116A

  • Foaming suppressing agent for steel making slag

    JP1988250412A

  • Method for restraining slopping

    JP1992180507A

  • Method for injecting carbonaceous material for restraining slag foaming

    JP1993287347A

  • Foaming supressor for slag

    JP1995145417A