Dry etching method, semiconductor device manufacturing method and etching apparatus

A dry etching method using β-diketone and nitrogen dioxide enables low-temperature etching of high dielectric constant materials like hafnium oxide without plasma, addressing the challenges of existing etching technologies and reducing equipment costs.

JP7572633B2Active Publication Date: 2024-10-24CENT GLASS CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021554123
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-23
Filing Date
2020-09-01
Publication Date
2024-10-24
Estimated Expiration
2040-09-01

AI Technical Summary

Technical Problem

Existing etching methods for high dielectric constant materials like hafnium oxide are difficult to perform at low temperatures without causing damage to semiconductor devices, and existing technologies are expensive due to the need for plasma-based etching.

Method used

A dry etching method using β-diketone and nitrogen dioxide as additives to etch metal oxides with an M-O bond energy of 5 eV or more without plasma, allowing etching at temperatures of 400°C or lower.

Benefits of technology

The method effectively etches challenging metal oxides like hafnium oxide at low temperatures, preventing damage and eliminating the need for plasma-based equipment, thus reducing costs and improving process reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572633000004
    Figure 0007572633000004
  • Figure 0007572633000001
    Figure 0007572633000001
  • Figure 0007572633000002
    Figure 0007572633000002
Patent Text Reader

Abstract

A dry etching method according to the embodiments of the present disclosure is characterized in that etching is performed without a plasma state by reacting β-diketone and nitrogen dioxide on a film to be etched, which is formed on a surface of a workpiece and includes a metal having an M-O binding energy of at least 5 eV or an oxide of the metal.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a dry etching method, a method for manufacturing a semiconductor device, and an etching apparatus. [Background technology]

[0002] As the circuit patterns of semiconductor devices become finer, field effect transistors are also becoming smaller. As a result, it is being considered to form the gate insulating film from HfO2 (dielectric constant k=25), a type of high-k material, rather than SiO2 (dielectric constant k=3.9).

[0003] In order to form a gate insulating film using a high dielectric constant material, it is necessary to etch the film after deposition to form it into a predetermined shape.

[0004] Patent Document 1, in relation to a method for manufacturing a MOS transistor or the like, describes a method for etching a metal film and a metal oxide film containing at least one of Al, Zr, Hf, Y, La, Ce, and Pr formed on a substrate, in which an etching gas containing β-diketone is used to reduce damage to the substrate, and an example discloses a method in which the wafer temperature is set to about 450° C. and oxygen is added to hexafluoroacetylacetone gas to etch an HfO2 film.

[0005] Patent Document 2 discloses a method for manufacturing a semiconductor device, in which a high dielectric constant film sample such as hafnium oxide formed on a Si film is etched by exciting a CH-based etching gas containing C and H into a plasma state.

[0006] Patent Document 3 discloses a method for cleaning a metal film adhering to a film formation device that forms a film of a metal gate material, an electrode material, or a magnetic material on a substrate surface, by using a gas containing β-diketone and NO or NO. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2004-91829 A [Patent Document 2] JP 2006-310676 A [Patent Document 3] JP 2013-194307 A Summary of the Invention [Problem to be solved by the invention]

[0008] In response to the trend toward finer circuit patterns in semiconductor devices, technologies have been developed that use high-dielectric-constant materials as gate insulating films. However, many high-dielectric-constant materials, such as hafnium oxide, are difficult to etch.

[0009] The invention described in Patent Document 1 discloses that the etching gas preferably contains at least one of water and alcohol in addition to oxygen, and that etching does not proceed at a low wafer temperature of 400° C. or less. That is, FIG. 9 of Patent Document 1 shows that in the case of a mixed gas of hexafluoroacetylacetone and oxygen, etching does not proceed at a wafer temperature of 400° C. or less. When the etching process is performed at a wafer temperature exceeding 400° C., damage to the semiconductor device is significant, and therefore a method capable of etching hafnium oxide at a low temperature of 400° C. or less, more preferably 300° C. or less, has been desired.

[0010] Patent Document 2 discloses that an etching rate of 1.0 nm / min was obtained by using C2H2 as a plasma etching gas, but in plasma etching, the plasma damages the parts of the semiconductor device that are not the target of etching, and the RF power source for generating the plasma makes the equipment expensive, so a method that does not use plasma is desired. Furthermore, Patent Document 3 only describes a method for cleaning metal films, and does not disclose an example of etching HfO2.

[0011] In view of the above-mentioned problems, the present disclosure aims to provide a dry etching method using a gas composition capable of etching a specific type of metal oxide film or metal film, including a hafnium oxide film, without plasma and at a low temperature. Further, the present disclosure aims to provide a method for manufacturing a semiconductor device using the dry etching method. [Means for solving the problem]

[0012] The inventors have discovered that when nitrogen dioxide is used as an additive gas for β-diketone, etching of specific metal oxide films such as hafnium oxide and metal films proceeds specifically at temperatures of 400° C. or lower, and even 300° C. or lower, compared to the use of other additive gases, and have arrived at the present disclosure.

[0013] The dry etching method disclosed herein is characterized in that a film to be etched, which is formed on the surface of a workpiece and contains a metal having an MO bond energy of 5 eV or more or an oxide of the above metal, is reacted with β-diketone and nitrogen dioxide to etch the film without creating a plasma state.

[0014] The MO bond energy is the difference in potential energy between the state in which a metal exists and the state in which it exists as oxygen. It can be said that the larger the bond energy, the stronger the bond between the metal and oxygen. In the case of metals having an MO bond energy of 5 eV or more, the bond between the metal and oxygen is strong and the metal oxide is stable, making the material difficult to etch. Since the metal itself is easily oxidized by nitrogen dioxide, the metal oxide is essentially etched, making etching difficult, but the dry etching method of the present disclosure makes it possible to etch at 300° C. or less.

[0015] In the dry etching method of the present disclosure, examples of the metals having an MO bond energy of 5 eV or more include hafnium, zirconium, titanium, and aluminum, and examples of the oxides of these metals include hafnium oxide, zirconium oxide, titanium oxide, and aluminum oxide. These metals can be used alone or as an alloy containing two or more of them. Therefore, the oxides of these metals can be either an oxide of one metal or an oxide of an alloy of these metals.

[0016] The dry etching method of the present disclosure may employ a first dry etching method in which an etching gas A containing the β-diketone and the nitrogen dioxide is brought into contact with the film to be etched, or may employ a second dry etching method including a first etching step in which an etching gas B containing the nitrogen dioxide is brought into contact with the film to be etched, and a second etching step in which an etching gas C containing the β-diketone is brought into contact with the film to be etched.

[0017] The method for manufacturing a semiconductor device according to the present disclosure is characterized by comprising a step of reacting a β-diketone and nitrogen dioxide with a film to be etched, the film containing a metal or an oxide of the metal having an MO bond energy of 5 eV or more on a substrate, to perform etching without using a plasma state. In the method for manufacturing a semiconductor device according to the present disclosure, either the first dry etching method or the second dry etching method described above may be adopted.

[0018] The etching apparatus disclosed herein is characterized in that it is provided in a heatable processing container and includes a mounting section for mounting a workpiece having an etching film formed on its surface, the etching film containing a metal having an MO bond energy of 5 eV or more or an oxide of the metal, a β-diketone supply section for supplying β-diketone to the workpiece, and a nitrogen dioxide gas supply section for supplying nitrogen dioxide to the workpiece. Effect of the Invention

[0019] According to the dry etching method of the present disclosure, it is possible to provide a dry etching method capable of etching a difficult-to-etch film containing the above-mentioned metal having an MO bond energy of 5 eV or more or an oxide of the above-mentioned metal, without involving a plasma state, even at a temperature of 400° C. or less, or even 300° C. or less. According to the dry etching method of the present disclosure, whether the above-mentioned first dry etching method or the above-mentioned second dry etching method is adopted, a dry etching method having the same effect as described above can be provided.

[0020] According to the semiconductor device manufacturing method of the present disclosure, it is possible to provide a semiconductor device manufacturing method capable of etching a difficult-to-etch film on a substrate, the film containing the above-mentioned metal having an MO bond energy of 5 eV or more or an oxide of the above-mentioned metal, without involving a plasma state, even at a temperature of 400° C. or less, or even 300° C. or less. According to the semiconductor device manufacturing method of the present disclosure, whether the first dry etching method or the second dry etching method is adopted, a semiconductor device manufacturing method having the same effects as those described above can be provided.

[0021] According to the etching apparatus of the present disclosure, by using this etching apparatus, it becomes possible to etch a difficult-to-etch film containing the above-mentioned metal having an MO bond energy of 5 eV or more or an oxide of the above-mentioned metal without involving a plasma state, even at a temperature of 400° C. or less, or even 300° C. or less. By using the etching apparatus of the present disclosure, the same effects as described above can be obtained whether the above-mentioned first dry etching method or the above-mentioned second dry etching method is adopted. [Brief description of the drawings]

[0022] [Figure 1]FIG. 1 is a schematic diagram illustrating an etching apparatus according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, embodiments of the present disclosure will be described in detail. However, the present disclosure is not limited to the following embodiments, and can be modified and applied as appropriate within the scope that does not change the gist of the present disclosure.

[0024] [Dry etching method] The dry etching method of the present disclosure is a dry etching method characterized by reacting a β-diketone and nitrogen dioxide with an etched film formed on the surface of a workpiece, the film containing a metal having an MO bond energy of 5 eV or more or an oxide of the above metal, to etch the film without involving a plasma state.

[0025] The metal having an MO bond energy of 5 eV or more or the oxide of the metal is desirably at least one selected from the group consisting of hafnium oxide, zirconium oxide, titanium oxide, aluminum oxide, hafnium metal, zirconium metal, titanium metal, and aluminum metal. Furthermore, the film to be etched containing the above-mentioned metal having an MO bond energy of 5 eV or more or an oxide of the above-mentioned metal is desirably at least one film selected from the group consisting of a hafnium oxide film, a zirconium oxide film, a titanium oxide film, an aluminum oxide film, a hafnium metal film, a zirconium metal film, a titanium metal film, and an aluminum metal film. The film to be etched may be a film of the above-mentioned single metal or metal oxide, or may be a film of an alloy containing two or more of the above-mentioned metals or an oxide of the alloy.

[0026] According to the dry etching method of the present disclosure, it is possible to provide a dry etching method capable of etching a difficult-to-etch film containing the above-mentioned metal having an MO bond energy of 5 eV or more or an oxide of the above-mentioned metal, without involving a plasma state, even at a temperature of 400° C. or less, or even 300° C. or less.

[0027] Hexafluoroacetylacetone (hereinafter, also referred to as HFAc), which is a type of β-diketone, has a decomposition temperature of 375° C., and therefore, when the etching temperature described in Patent Document 1 exceeds 400° C., it is fully expected that HFAc will decompose and carbon components will deposit on the film to be etched, which is the etching target, causing problems in the subsequent processes. On the other hand, in the dry etching method of the present disclosure, HFAc and NO2 are used as the etching gas, so that the etching temperature can be reduced to 375°C or lower, thereby suppressing the formation of a carbon film due to the decomposition of HFAc. The reason why the etching temperature can be lowered is presumably because NO2, which constitutes the etching gas, is adsorbed onto the surface of the film to be etched, weakening the bonding strength between the metal and oxygen that constitutes the above-mentioned metal oxide, improving the reactivity with HFAc, and making it possible to etch at a low temperature.

[0028] [First dry etching method] First, as the dry etching method of the present disclosure, a first dry etching method in which an etching gas A containing the β-diketone and the nitrogen dioxide is brought into contact with the film to be etched will be described.

[0029] In the first dry etching method of the present disclosure, examples of the object to be processed include a silicon substrate, a compound semiconductor substrate, a quartz substrate, and a glass substrate. On the surface of the object to be processed, in addition to the film containing a metal having an M-O bond energy of 5 eV or more or an oxide of the metal described above, a silicon film, a silicon oxide film, a silicon nitride film, a metal wiring film other than the above metals, etc. may be formed. The object to be processed is placed on the placement part, and by heating the placement part, the object to be processed and the etching film containing a metal having an M-O bond energy of 5 eV or more or an oxide of the metal formed on the surface of the object to be processed are heated.

[0030] The temperature of the object to be processed is substantially equal to the temperature of the etching film. When an etching gas containing β-diketone and nitrogen dioxide is brought into contact with the heated etching film, β-diketone, nitrogen dioxide, and a metal having an M-O bond energy of 5 eV or more or an oxide of the metal react to form a complex on the etching film. Since this complex has a high vapor pressure, the etching film can be etched by vaporizing the complex.

[0031] Examples of the hafnium oxide constituting the oxide of a metal having an M-O bond energy of 5 eV or more include hafnium oxide (HfO x (where x is 1 or more and 3 or less), particularly HfO2), hafnium silicon oxide, and hafnium aluminum oxide. Examples of hafnium silicon oxide include Hf 1-x Si x O y 、Hf 1-x Si x O y N z And examples of hafnium aluminum oxide include Hf 1-x Al x O m 、Hf 1-x Al x O m N n However, x, y, z, m, and n represent 0 < x < 1, 0 < y ≤ 2, 0 < z ≤ 1.33, 0 < m ≤ 1.5, and 0 < n ≤ 1.

[0032] Zirconium oxide includes zirconium oxide (ZrO u (u is 1 or more and 3 or less), especially ZrO2). Aluminum oxides include aluminum oxide (AlO v (v is 1 or more and 2 or less), especially Al2O3). Titanium oxides include titanium oxide (TiO w (w is 1 or more and 3 or less), especially TiO2).

[0033] The method of forming the film to be etched containing a metal having an MO bond energy of 5 eV or more or an oxide of the above metal on the surface of the workpiece is not particularly limited, but examples thereof include chemical vapor deposition (CVD) and sputtering. The thickness of the film to be etched containing a metal having an MO bond energy of 5 eV or more or an oxide of the above metal is also not particularly limited, but can be, for example, 0.1 nm to 1 μm.

[0034] The type of β-diketone is not particularly limited, and examples thereof include hexafluoroacetylacetone (HFAc, 1,1,1,5,5,5-hexafluoro-2,4-pentanedione), trifluoroacetylacetone (1,1,1-trifluoro-2,4-pentanedione), etc. As the β-diketone, one type of compound may be used, or two or more types of compounds may be used.

[0035] The volume ratio of β-diketone to nitrogen dioxide contained in the etching gas A is preferably β-diketone:nitrogen dioxide=10:0.001 to 100, more preferably β-diketone:nitrogen dioxide=10:0.01 to 10, and even more preferably β-diketone:nitrogen dioxide=10:0.1 to 10. If the amount of β-diketone in the etching gas is too small, the etching rate tends to decrease, and if there is too much, the etching gas becomes too expensive. Also, if the amount of nitrogen dioxide in the etching gas is too small or too large, etching does not proceed easily.

[0036] The etching gas A may be composed of only β-diketone and nitrogen dioxide, or may further contain at least one additive gas selected from the group consisting of O2, NO, N2O, CO, CO2, H2O, H2O2, and alcohol, or may further contain at least one inert gas selected from the group consisting of N2, Ar, He, Ne, and Kr. As the alcohol, methanol, ethanol, propanol, isopropyl alcohol, etc. can be used.

[0037] When the etching gas A contains an additive gas other than nitrogen dioxide, the total content of nitrogen dioxide and the other additive gas contained in the etching gas A can be the same as the above-mentioned content of nitrogen dioxide.

[0038] When the etching gas A contains an inert gas, the content of the inert gas in the etching gas A is preferably 1 vol.% or more and 90 vol.% or less, more preferably 10 vol.% or more and 80 vol.% or less, and even more preferably 30 vol.% or more and 50 vol.% or less.

[0039] [Second dry etching method] Next, a second dry etching method according to the present disclosure will be described, which includes a first etching step in which an etching gas B containing nitrogen dioxide is brought into contact with the film to be etched, and a second etching step in which an etching gas C containing a β-diketone is brought into contact with the film to be etched.

[0040] In the second dry etching method of the present disclosure, the object to be processed may be a silicon substrate, a compound semiconductor substrate, a quartz substrate, or a glass substrate, as in the first dry etching method. In addition to the above-mentioned metal film having an MO bond energy of 5 eV or more or an oxide of the above-mentioned metal, a silicon film, a silicon oxide film, a silicon nitride film, a metal wiring film other than the above-mentioned metal, or the like may be formed on the surface of the object to be processed. The object to be processed is placed on a mounting part, and the mounting part is heated to heat the object to be processed and the etched film formed on the surface of the object to be processed, which includes a metal having an MO bond energy of 5 eV or more or an oxide of the above-mentioned metal.

[0041] The temperature of the workpiece is substantially equal to the temperature of the film to be etched. When the etching gas B containing nitrogen dioxide is brought into contact with the film to be etched in a heated state as the first etching step, the nitrogen dioxide is adsorbed on the surface of the film to be etched. Thereafter, when the etching gas C containing β-diketone is brought into contact with the film to be etched as the second etching step, the metal or the oxide of the metal having an MO bond energy of 5 eV or more, on whose surface the nitrogen dioxide is adsorbed, reacts with the β-diketone, and a complex is generated on the film to be etched, as in the first dry etching method. Since the vapor pressure of this complex is high, the film to be etched containing the metal or the oxide of the metal having an MO bond energy of 5 eV or more can be etched by vaporizing the complex. In the second dry etching method of the present disclosure, the above steps may be repeated multiple times to repeatedly etch the film to be etched. Since it is possible to etch a constant thickness in one cycle of etching steps, a layer of a desired thickness can be precisely etched by specifying the number of cycles.

[0042] As the hafnium oxide constituting the oxide of the metal having an MO bond energy of 5 eV or more, the same one as in the first dry etching method can be used.

[0043] The method of forming the film to be etched containing a metal having an MO bond energy of 5 eV or more or an oxide of the above metal on the surface of the workpiece is not particularly limited, but examples thereof include chemical vapor deposition (CVD) and sputtering. The thickness of the film to be etched containing a metal having an MO bond energy of 5 eV or more or an oxide of the above metal is not particularly limited, but may be, for example, 0.1 nm to 1 μm.

[0044] As the β-diketone, the same ones as in the above-mentioned first dry etching method can be used.

[0045] The etching gas C may consist only of β-diketone, and the etching gas B may consist only of nitrogen dioxide, but may further contain at least one additive gas selected from the group consisting of O2, NO, N2O, CO, CO2, H2O, H2O2, and alcohol, or may further contain at least one inert gas selected from the group consisting of N2, Ar, He, Ne, and Kr. Also, examples of the alcohol that can be used include methanol, ethanol, propanol, and isopropyl alcohol.

[0046] When etching gas B contains an additive gas other than nitrogen dioxide, the total volume ratio of nitrogen dioxide and the other additive gas contained in etching gas A can be the same as the volume ratio of β-diketone and nitrogen dioxide contained in etching gas A described above. In addition, when etching gas C contains an additive gas other than β-diketone, the total volume ratio of the β-diketone contained in etching gas C to the other additive gas can be the same as the volume ratio of the β-diketone to nitrogen dioxide contained in the above-mentioned etching gas A.

[0047] When etching gas B and etching gas C contain an inert gas, the content of the inert gas contained in etching gas B and etching gas C is preferably 1 vol.% or more and 90 vol.% or less, more preferably 10 vol.% or more and 80 vol.% or less, and even more preferably 30 vol.% or more and 50 vol.% or less.

[0048] [Etching equipment] The dry etching method of the present disclosure can be realized, for example, by using a general etching apparatus used in the semiconductor manufacturing process. Such an etching apparatus also constitutes part of the present disclosure.

[0049] FIG. 1 is a schematic diagram illustrating an etching apparatus according to an embodiment of the present disclosure. 1 includes a processing vessel 110 for accommodating a processing target object 10 having a metal with an MO bond energy of 5 eV or more or an oxide of the above metal formed on the surface thereof, a β-diketone supply unit 140 connected to the processing vessel 110 for supplying gaseous β-diketone, a nitrogen dioxide gas supply unit 150 for supplying gaseous nitrogen dioxide, an inert gas supply unit 160 for supplying an inert gas, and a heating means 170 for heating the processing vessel 110. Note that the etching apparatus 100 does not necessarily have to include the inert gas supply unit 160.

[0050] The etching apparatus 100 further includes a control unit (not shown). This control unit is, for example, a computer, and includes a program, a memory, and a CPU. The program incorporates a group of steps to perform a series of operations in the first etching method or the second etching method, and performs the following operations in accordance with the program: adjusting the temperature of the workpiece 10, opening and closing the valves of each supply unit, adjusting the flow rate of each gas, adjusting the pressure inside the processing vessel 110, and the like. This program is stored in a computer storage medium, for example, a compact disc, a hard disk, a magneto-optical disc, a memory card, or the like, and is installed in the control unit.

[0051] The processing vessel 110 includes a mounting portion 111 for mounting the object to be processed 10. The processing vessel 110 is not particularly limited as long as it is resistant to the β-diketone used and can be depressurized to a predetermined pressure, but typically, a general processing vessel provided in a semiconductor etching device is used. In addition, a supply pipe for supplying an etching gas and other piping are also not particularly limited as long as they are resistant to β-diketone, and general piping can be used.

[0052] The β-diketone supply unit 140 supplies β-diketone from pipes 141 and 142 to the pipe 121 by adjusting the supply amount using valves V1 and V2 and flow rate adjustment means MFC1.

[0053] Nitrogen dioxide gas supply unit 150 supplies nitrogen dioxide from pipes 151 and 152 to pipe 121 by adjusting the supply amount using valves V3 and V4 and flow rate adjustment means MFC2.

[0054] The inert gas supply unit 160 supplies the inert gas from pipes 161 and 162 to the pipe 121 by adjusting the supply amount using valves V5 and V6 and flow rate adjustment means MFC3.

[0055] A heating unit 170 for heating the processing vessel 110 is disposed outside the processing vessel 110. A heater (not shown) may be provided inside the mounting unit 111 as a second heating unit. When multiple mounting units are disposed in the processing vessel 110, a heater is provided for each mounting unit, so that the temperature of the workpiece on each mounting unit can be set to a predetermined temperature individually.

[0056] A gas exhaust means for exhausting gas after reaction is provided on one side of the processing vessel 110. A vacuum pump 173 of the gas exhaust means exhausts the gas after reaction from the processing vessel 110 through a pipe 171. The gas after reaction is collected by a liquid nitrogen trap 174 provided between the pipes 171 and 172. Valves V7 and V8 are provided on the pipes 171 and 172 to adjust the pressure. In addition, in FIG. 1, PI1 and PI2 are pressure gauges, and a control unit can control each flow rate adjustment means and each valve based on the indicated value.

[0057] The etching method will be specifically described using the etching apparatus 100 as an example. [First dry etching method using the etching apparatus described above] In the first dry etching method of the present disclosure, an etching gas A containing a β-diketone and nitrogen dioxide is brought into contact with a film to be etched.

[0058] In the first dry etching method, first, the object 10 to be processed, on which a film to be etched containing a metal having an MO bond energy of 5 eV or more or an oxide of the above metal is formed, is placed in the processing vessel 110. Next, the inside of the processing vessel 110, the pipe 121, the pipes 141 and 142, the pipes 151 and 152, the pipes 161 and 162, the liquid nitrogen trap 174, and the pipes 171 and 172 are evacuated to a predetermined pressure by the vacuum pump 173, and then the object 10 to be processed is heated by the heating means 170. When the workpiece 10 reaches a predetermined temperature, β-diketone and nitrogen dioxide gas are supplied at predetermined flow rates from β-diketone supply unit 140 and nitrogen dioxide gas supply unit 150 to pipe 121. Note that an inert gas may be supplied from inert gas supply unit 160 to pipe 121 at a predetermined flow rate.

[0059] β-diketone and nitrogen dioxide are mixed in a predetermined composition and supplied to the processing vessel 110. While the mixed etching gas is introduced into the processing vessel 110, the inside of the processing vessel 110 is controlled to a predetermined pressure. The etching gas is reacted with a film to be etched, which contains a metal having an MO bond energy of 5 eV or more or an oxide of the above metal, for a predetermined time to form a complex, and etching is performed. In this etching method, etching can be performed without a plasma state, and excitation of the etching gas by plasma or the like is not required during etching. The flow rate of the etching gas can be appropriately set based on the volume and pressure of the processing vessel.

[0060] Etching accompanied by a plasma state refers to a process in which a gas or the like at about 0.1 to 10 Torr is introduced into a reaction device, high-frequency power is applied to an outer coil or a counter electrode to generate low-temperature gas plasma in the reaction device, and etching is performed by active chemical species such as ions and radicals that are generated in the plasma. In the dry etching method of the present disclosure, the gas is brought into contact without being in a plasma state, and dry etching is performed without generating the above-mentioned gas plasma.

[0061] After the etching process is completed, the heating by the heating means 170 is stopped to lower the temperature, and the vacuum pump 173 is stopped and replaced with an inert gas to release the vacuum. As described above, by the first dry etching method using the above etching apparatus, it is possible to etch a film to be etched that contains a metal having an MO bond energy of 5 eV or more or an oxide of the above metal.

[0062] (Etching conditions in the first dry etching method) In the first dry etching method of the present disclosure, the temperature of the film to be etched when the etching gas A is brought into contact with the film to be etched may be any temperature at which the complex can be vaporized, and in particular, the temperature of the film to be etched to be removed is preferably 250°C or higher and 375°C or lower, more preferably 275°C or higher and 375°C or lower, more preferably 275°C or higher and 350°C or lower, and even more preferably 275°C or higher and 325°C or lower.

[0063] In addition, when the etching gas A is brought into contact with the film to be etched, the pressure inside the processing vessel in which the object to be etched on which the film to be etched is formed is placed is not particularly limited, but is usually in the pressure range of 0.1 kPa or more and 101.3 kPa or less.

[0064] From the viewpoint of obtaining a sufficient etching rate, the pressure in the processing vessel in the etching step is preferably 20 Torr or more and 300 Torr or less (2.67 kPa or more and 39.9 kPa or less), more preferably 20 Torr or more and 200 Torr or less (2.67 kPa or more and 26.7 kPa or less), and even more preferably 20 Torr or more and 100 Torr or less (2.67 kPa or more and 13.3 kPa or less).

[0065] The processing time of the etching step is not particularly limited, but is preferably within 60 minutes in consideration of the efficiency of the semiconductor device manufacturing process. Here, the processing time of the etching step refers to the time from when the etching gas is introduced into the processing vessel in which the object to be processed is placed until the etching gas in the processing vessel is exhausted by a vacuum pump or the like to finish the etching process.

[0066] [Second dry etching method using the etching apparatus 100] The second dry etching method of the present disclosure includes a first etching step in which an etching gas B containing nitrogen dioxide is brought into contact with a film to be etched, and a second etching step in which an etching gas C containing a β-diketone is brought into contact with the film to be etched.

[0067] In the second dry etching method, first, the object 10 to be processed, on which a film to be etched containing a metal having an MO bond energy of 5 eV or more or an oxide of the above metal is formed, is placed in the processing vessel 110. Next, the inside of the processing vessel 110, the pipe 121, the pipes 141 and 142, the pipes 151 and 152, the pipes 161 and 162, the liquid nitrogen trap 174, and the pipes 171 and 172 are evacuated to a predetermined pressure by the vacuum pump 173, and then the object 10 to be processed is heated by the heating means 170.

[0068] When the workpiece 10 reaches a predetermined temperature, first, nitrogen dioxide gas is supplied from the nitrogen dioxide gas supply unit 150 to the pipe 121 at a predetermined flow rate. Alternatively, an inert gas may be supplied from the inert gas supply unit 160 to the pipe 121 at a predetermined flow rate. While nitrogen dioxide gas or nitrogen dioxide gas and an inert gas are being introduced into the processing vessel 110, the pressure inside the processing vessel 110 is controlled to a predetermined value. By introducing the nitrogen dioxide gas into the processing vessel 110 for a predetermined time, the nitrogen dioxide is adsorbed to the film to be etched. After the gas containing nitrogen dioxide gas is evacuated to a vacuum, β-diketone gas is supplied from β-diketone supply unit 140 to pipe 121 at a predetermined flow rate. Alternatively, inert gas may be supplied from inert gas supply unit 160 to pipe 121 at a predetermined flow rate. While β-diketone gas or β-diketone gas and inert gas are being introduced into processing vessel 110, the pressure inside processing vessel 110 is controlled to a predetermined pressure. By introducing β-diketone gas into processing vessel 110 for a predetermined time, the previously adsorbed nitrogen dioxide and β-diketone react to form a complex, and the complex further reacts with the film to be etched, thereby etching the film to be etched.

[0069] In the second dry etching method of the present disclosure, a cycle consisting of a first etching step of introducing nitrogen dioxide gas into the processing vessel 110 and a second etching step of introducing β-diketone into the processing vessel 110 can be repeated multiple times. In the second dry etching method of the present disclosure, the etching conditions for one cycle are set to predetermined conditions, thereby making it possible to control the thickness of the film to be etched in one cycle. Therefore, by setting the thickness of the film to be etched in one cycle to a thin value, it is possible to precisely control the thickness to be etched.

[0070] In addition, the second dry etching method also allows etching without plasma, and does not require excitation of the etching gas with plasma, etc. The flow rates of nitrogen dioxide and β-diketone can be appropriately set based on the volume and pressure of the processing vessel.

[0071] In this manner, in the second dry etching method of the present disclosure using the above-mentioned etching apparatus, the gas can be brought into contact without a plasma state, and dry etching can be performed without generating the above-mentioned gas plasma.

[0072] After the etching process is completed, the heating by the heating means 170 is stopped to lower the temperature, and the vacuum pump 173 is stopped and replaced with an inert gas to release the vacuum. In this manner, the film to be etched containing a metal having an MO bond energy of 5 eV or more or an oxide of the above metal can be etched.

[0073] (Etching conditions in the second dry etching method) In the second dry etching method of the present disclosure, the temperature of the film to be etched during the etching step may be any temperature at which the complex can be vaporized, and in particular, the temperature of the film to be etched to be removed is preferably 250° C. or higher and 375° C. or lower, more preferably 275° C. or higher and 375° C. or lower, more preferably 275° C. or higher and 350° C. or lower, and more preferably 275° C. or higher and 325° C. The temperature of the film to be etched in the first etching step and the second etching step is desirably the same.

[0074] The pressure within the processing vessel during the etching process is not particularly limited, but is usually within the range of 0.1 kPa to 101.3 kPa.

[0075] From the viewpoint of obtaining a sufficient etching rate, the pressure in the processing vessel in the first etching step and the second etching step is preferably 20 Torr to 300 Torr (2.67 kPa to 39.9 kPa), more preferably 20 Torr to 200 Torr (2.67 kPa to 26.7 kPa), and further preferably 20 Torr to 100 Torr (2.67 kPa to 13.3 kPa). The pressure in the processing vessel in the second etching step is desirably higher than the pressure in the processing vessel in the first etching step.

[0076] The processing time in the first etching step and the second etching step is not particularly limited, but the processing time in one cycle of the first etching step is preferably within 60 minutes, and the processing time in one cycle of the second etching step is preferably within 60 minutes. Here, the processing time in the etching step refers to the time from when an etching gas is introduced into a processing vessel in which a workpiece is placed until the etching gas in the processing vessel is exhausted by a vacuum pump or the like to finish the etching process.

[0077] [Method of manufacturing semiconductor devices] The above-described dry etching method of the present disclosure can be used as an etching method for forming a predetermined pattern on a hafnium oxide film, hafnium metal, etc., of a conventional semiconductor device. By etching a hafnium oxide film, hafnium metal, etc., on a substrate using the dry etching method of the present disclosure, a semiconductor device can be manufactured at low cost. EXAMPLES

[0078] EXAMPLES Hereinafter, examples that more specifically disclose the present disclosure will be described, but the present disclosure is not limited to these examples.

[0079] Example 1 Using the etching apparatus 100 shown in FIG. 1, an object to be processed 10 having an etching film made of a hafnium oxide (HfO2) film (shape: 1 cm x 1 cm, film thickness: 5 nm) formed on the surface of a silicon wafer was etched.

[0080] The inside of the processing vessel 110, the pipe 121, the pipes 141 and 142, the pipes 151 and 152, the pipes 161 and 162, the liquid nitrogen trap 174, and the pipes 171 and 172 were evacuated to less than 10 Pa. Then, the object 10 placed on the placement part 111 was heated by the heater disposed inside the heating means 170 and the placement part 111. After it was confirmed that the temperature of the object 10 reached 300°C, the pressure inside the processing vessel 110 was controlled to 90 Torr while the etching gas was introduced into the processing vessel 110 by supplying gaseous hexafluoroacetylacetone (HFAc) from the β-diketone supply part 140 and NO2 gas from the nitrogen dioxide gas supply part 150 to the pipe 121 at a predetermined flow rate, and an etching process was performed. The temperature of the object was set to 300°C, and the flow rates of the etching gas were set to HFAc=10 sccm and NO2=1 sccm. Thirty minutes after the introduction of the etching gas was started, the introduction of the etching gas was stopped. Then, the inside of the processing vessel 110 was evacuated to less than 10 Pa, and the inside pressure was replaced with N2 gas supplied from the inert gas supply unit 160. Then, the processing object 10 was taken out, the film thickness was measured, and the amount of etching was evaluated.

[0081] In the following Examples 1 to 22, including Examples 2 to 20, the first dry etching method is employed in which an etching gas A containing β-diketone and nitrogen dioxide is brought into contact with a film to be etched, and in Comparative Examples 1 to 17, except for Comparative Examples 4, 7, 10, 12, and 17, an etching gas containing β-diketone and a gas shown in Tables 1 and 2 is brought into contact with a film to be etched. In Comparative Examples 4, 7, 10, 12, and 17, an etching gas containing only β-diketone is brought into contact with a film to be etched.

[0082] (Examples 2 to 4, Comparative Examples 1 to 4) Table 1 below shows the type of additive gas, the flow rate of HFAc, the flow rate of the additive gas, the pressure inside the processing vessel, the temperature during etching, the etching time, and whether or not etching is possible in the above-mentioned etching. The etching rate was rated as ◯ if the etching rate was 0.1 nm / min or more, and rated as × if the etching rate was less than 0.1 nm / min. The etching rate is the value obtained by dividing the change in film thickness before and after etching by the time required for etching. Differences between Examples 2 to 4 and Comparative Examples 1 to 4 and Example 1 will be described. In Example 2, the flow rate of NO2, which is an additive gas, was changed. In Example 3, the flow rate of NO2, which is an additive gas, the etching time, and the temperature of the workpiece 10 were changed. In Example 4, the temperature of the workpiece 10 was changed. In Comparative Examples 1 to 3, nitric oxide (NO), oxygen (O2), and dinitrogen oxide (N2O) were used as additive gases, respectively, and in Comparative Example 4, processing was performed without using an additive gas. In other respects, the same operation as in Example 1 was performed, and whether or not a hafnium oxide (HfO2) film could be etched was evaluated.

[0083] [Table 1]

[0084] (Examples 5 to 22, Comparative Examples 5 to 17) Using the etching apparatus 100 shown in FIG. 1, an object to be processed having an etching film formed on the surface of a silicon wafer, the etching film being made of an aluminum oxide (Al2O3) film, a zirconium oxide (ZrO2) film, a hafnium oxide (HfO2) film, and a titanium oxide (TiO2) film, each having a size of 1 cm x 1 cm and a thickness of 60 nm, was etched.

[0085] The etching rate of the film to be etched was measured in the same manner as in Example 1, except that the material of the film to be etched, the type and flow rate of the etching gas, the pressure in the processing vessel, and the temperature of the object to be etched during etching were changed as shown in Table 2 (275°C, 300°C, 350°C). The results are shown in Table 2. In Table 2, etching rates of 0.1 nm / min or more and less than 1.0 nm / min are indicated as A, 1.0 nm / min or more and less than 10.0 nm / min as B, 10.0 nm / min or more and less than 50.0 nm / min as C, and less than 0.1 nm as X.

[0086] [Table 2]

[0087] From the above results, when HFAc and NO2 were used as the etching gas, it was possible to etch aluminum oxide films, zirconium oxide films, hafnium oxide films, hafnium metal films, and titanium oxide films at a rate of 0.1 nm / min or more at a temperature of the treated object of 350° C. or less, and in particular, etching was possible even at a temperature of the treated object of 300° C. Furthermore, since etching was possible at a temperature of the treated object of 300° C. or less, which is the decomposition temperature of HFAc (375° C.), no carbon film was formed on the surface of the treated object in Examples 1 to 4. On the other hand, when NO, O2, or NO was used as the additive gas, or when no additive gas was used, the aluminum oxide film, zirconium oxide film, hafnium oxide film, hafnium metal film, and titanium oxide film could not be etched even when the temperature of the treated object was 350°C.

[0088] (Examples 23 to 26) In these examples, a second dry etching method was adopted in which a first etching step in which an etching gas B containing nitrogen dioxide is brought into contact with the film to be etched and a second etching step in which an etching gas C containing β-diketone is brought into contact with the film to be etched were repeatedly performed to etch a film to be etched, which was a hafnium oxide (HfO2) film (size 1 cm x 1 cm, film thickness 60 nm) formed on the surface of a silicon wafer.

[0089] First, the inside of the processing vessel 110, the pipe 121, the pipes 141 and 142, the pipes 151 and 152, the pipes 161 and 162, the liquid nitrogen trap 174, and the pipes 171 and 172 were evacuated to less than 10 Pa. Thereafter, the workpiece 10 having the hafnium oxide (HfO2) film placed on the placement part 111 was heated by the heating means 170 and a heater disposed inside the placement part 111.

[0090] After it was confirmed that the temperature of the workpiece 10 reached 350°C, NO2 gas was supplied from the nitrogen dioxide gas supply unit 150 to the pipe 121, and NO2 gas was allowed to flow into the inside of the processing vessel 110 while controlling the pressure inside the processing vessel 110 to 30 Torr. The temperature of the workpiece was set to 350°C, the flow rate of the etching gas was set to NO2=5 sccm, and the NO2 gas was allowed to flow for the time shown in Table 3 and come into contact with the film to be etched. Thereafter, the introduction of the etching gas was stopped, and the inside of the processing vessel 110 was evacuated to less than 10 Pa.

[0091] Next, hexafluoroacetylacetone (HFAc) gas was supplied from β-diketone supply unit 140 to pipe 121, and HFAc gas was flowed into processing vessel 110 while controlling the pressure inside processing vessel 110 to 60 Torr. The temperature of the processing target was set to 350° C., the flow rate of the etching gas was set to HFAc=10 sccm, and the HFAc gas was flowed for the time shown in Table 3 to contact with the film to be etched. Thereafter, the introduction of the etching gas was stopped, and the inside of processing vessel 110 was evacuated to less than 10 Pa.

[0092] After repeating the above-mentioned process of flowing NO2 gas into the inside of the processing vessel 110 and the process of flowing HFAc gas into the inside of the processing vessel 110 as one cycle for the number of times (number of cycles) shown in Table 3, the inside of the processing vessel 110 was evacuated to less than 10 Pa, the inside of the processing vessel 110 was replaced with N2 gas supplied from the inert gas supply unit 160, the workpiece 10 was removed, the film thickness was measured, the total etching thickness was measured, and the etching thickness per cycle was calculated. The results are shown in Table 3.

[0093] [Table 3]

[0094] As is clear from the results shown in Table 3, by keeping the etching conditions constant, the thickness of the film to be etched per cycle becomes almost constant, and it was found that by setting the number of cycles, the film to be etched can be etched to the required thickness with almost exact accuracy. [Explanation of symbols]

[0095] 10 Object to be treated 100 Etching equipment 110 Processing vessel 111 Placement section 121 Piping 140 β-diketone supply unit 141, 142 Piping 150 Nitrogen dioxide gas supply unit 151, 152 Piping 160 Inert gas supply section 161, 162 Piping 170 Heating means 171, 172 Piping 173 Vacuum Pump 174 Liquid Nitrogen Trap MFC1, MFC2, MFC3 flow rate adjustment means PI1, PI2 pressure gauges V1, V2, V3, V4, V5, V6, V7, V8 Valves

Claims

1. A dry etching method characterized by reacting a β-diketone and nitrogen dioxide with a film to be etched, the film containing a metal or an oxide of the metal having an M-O bond energy of 5 eV or more, formed on a surface of a workpiece, to perform etching without involving a plasma state.

2. 2. The dry etching method according to claim 1, wherein the metal having an M-O bond energy of 5 eV or more or the oxide of the metal is at least one selected from the group consisting of hafnium oxide, zirconium oxide, titanium oxide, aluminum oxide, hafnium metal, zirconium metal, titanium metal, and aluminum metal.

3. 3. The dry etching method according to claim 1, wherein the film to be etched is at least one film selected from the group consisting of a hafnium oxide film, a zirconium oxide film, a titanium oxide film, an aluminum oxide film, a hafnium metal film, a zirconium metal film, a titanium metal film, and an aluminum metal film.

4. 4. The dry etching method according to claim 1, wherein the β-diketone is hexafluoroacetylacetone or trifluoroacetylacetone.

5. 5. The dry etching method according to claim 1, wherein an etching gas A containing the β-diketone and the nitrogen dioxide is brought into contact with the film to be etched.

6. 6. The dry etching method according to claim 5, wherein the temperature of the film to be etched when the etching gas A is brought into contact with the film to be etched is 250° C. or more and 375° C. or less.

7. 7. The dry etching method according to claim 5, wherein a volume ratio of said β-diketone to said nitrogen dioxide in said etching gas A is β-diketone:nitrogen dioxide=10:0.001 or more and 100 or less.

8. 8. The dry etching method according to claim 7, wherein a volume ratio of said β-diketone to said nitrogen dioxide in said etching gas A is β-diketone:nitrogen dioxide=10:0.01 or more and 10 or less.

9. 9. The dry etching method according to claim 5, wherein when the etching gas A is brought into contact with the film to be etched, a pressure in a processing vessel in which a workpiece on which the film to be etched is formed is placed is in a pressure range of 0.1 kPa or more and 101.3 kPa or less.

10. The film to be etched is hafnium oxide (HfO x (x is 1 or more and 3 or less)), zirconium oxide (ZrO u (u is 1 or more and 3 or less)), aluminum oxide (AlO v (v is 1 or more and 2 or less)), and titanium oxide (TiO w (w is 1 or more and 3 or less), the β-diketone is hexafluoroacetylacetone; the temperature of the film to be etched when the β-diketone and the nitrogen dioxide are brought into contact with the film to be etched is 250° C. or higher and 375° C. or lower; a volume ratio of β-diketone to nitrogen dioxide in the etching gas A is β-diketone:nitrogen dioxide=10:0.001 or more and 100 or less; when the etching gas A is brought into contact with the film to be etched, a pressure in a processing vessel in which a workpiece on which the film to be etched is formed is placed is in a pressure range of 0.1 kPa or more and 101.3 kPa or less; 6. The dry etching method according to claim 5, wherein the etching rate of the film to be etched is 0.1 nm / min or more.

11. The etching gas A is N 2 11. The dry etching method according to claim 5, further comprising at least one inert gas selected from the group consisting of Ar, He, Ne and Kr.

12. 12. The dry etching method according to claim 11, wherein the content of the inert gas in the etching gas A is 1% by volume or more and 90% by volume or less.

13. 12. The dry etching method according to claim 11, wherein the content of the inert gas in the etching gas A is 30% by volume or more and 50% by volume or less.

14. a first etching step of contacting the etching gas B containing nitrogen dioxide with the film to be etched; 5. The dry etching method according to claim 1, further comprising a second etching step of contacting the etching gas C containing the β-diketone with the film to be etched.

15. 15. The dry etching method according to claim 14, wherein the first etching step and the second etching step are repeated a plurality of times.

16. 16. The dry etching method according to claim 14, wherein the temperature of the film to be etched when the etching gas B is brought into contact with the film to be etched and the temperature of the film to be etched when the etching gas C is brought into contact with the film to be etched are 250° C. or higher and 375° C. or lower.

17. The dry etching method according to any one of claims 14 to 16, wherein when the etching gas B is brought into contact with the etching film and when the etching gas C is brought into contact with the etching film, a pressure in a processing vessel in which a processing object on which the etching film is formed is placed is in a pressure range of 0.1 kPa or more and 101.3 kPa or less.

18. The film to be etched is hafnium oxide (HfO x (x is 1 or more and 3 or less)), zirconium oxide (ZrO u (u is 1 or more and 3 or less)), aluminum oxide (AlO V (v is 1 or more and 2 or less)), and titanium oxide (TiO w (w is 1 or more and 3 or less), the β-diketone is hexafluoroacetylacetone; a temperature of the film to be etched when the etching gas B is brought into contact with the film to be etched and a temperature of the film to be etched when the etching gas C is brought into contact with the film to be etched are 250° C. or more and 375° C. or less; 15. The dry etching method according to claim 14, wherein when the etching gas B is brought into contact with the etching film and when the etching gas C is brought into contact with the etching film, a pressure in a processing vessel in which a processing object on which the etching film is formed is placed is in a pressure range of 0.1 kPa or more and 101.3 kPa or less.

19. The etching gas B and the etching gas C are N 2 The dry etching method according to any one of claims 14 to 18, further comprising at least one inert gas selected from the group consisting of Ar, He, Ne and Kr.

20. 20. The dry etching method according to claim 19, wherein the etching gas B and the etching gas C each have a content of the inert gas of 1 volume % or more and 90 volume % or less.

21. 21. The dry etching method according to claim 20, wherein the content of the inert gas in the etching gas B and the etching gas C is 30% by volume or more and 50% by volume or less.

22. A method for manufacturing a semiconductor device, comprising the steps of reacting a β-diketone and nitrogen dioxide with a film to be etched, the film containing a metal or an oxide of the metal having an M-O bond energy of 5 eV or more on a substrate, to etch the film without using a plasma state.

23. 23. The method for manufacturing a semiconductor device according to claim 22, wherein the film to be etched is at least one film selected from the group consisting of a hafnium oxide film, a zirconium oxide film, a titanium oxide film, an aluminum oxide film, a hafnium metal film, a zirconium metal film, a titanium metal film, and an aluminum metal film.

24. a mounting part provided in a heatable processing container, on which a processing object having a film to be etched, the film containing a metal having an M-O bond energy of 5 eV or more or an oxide of the metal, is mounted; A β-diketone supply unit that supplies β-diketone to the object to be treated; a nitrogen dioxide gas supply unit that supplies nitrogen dioxide to the object to be treated; An etching apparatus comprising:

25. 25. The etching apparatus according to claim 24, further comprising an inert gas supply unit that supplies an inert gas to the object to be processed.

26. 26. The etching apparatus according to claim 24, wherein the film to be etched is at least one film selected from the group consisting of a hafnium oxide film, a zirconium oxide film, a titanium oxide film, an aluminum oxide film, a hafnium metal film, a zirconium metal film, a titanium metal film, and an aluminum metal film.

Citation Information

Patent Citations

  • Method of etching high-permittivity multicomponent oxide film and refractory metal film, manufacture of thin-film capacitor, and plasma apparatus for film formation

    JP1994151383A

  • Etching method and etching apparatus

    JP2004091829A

  • Method for etching sample

    JP2006310676A

  • Method for dry-cleaning metallic film in film deposition apparatus

    JP2013194307A

  • Dry etching method and etching device

    JP2018110229A