Anisotropic Conductive Film

The anisotropic conductive film with controlled lattice point arrangements and a transfer process addresses particle aggregation and dropout issues, ensuring reliable conductivity and reduced short circuits in electronic connections.

JP7572638B2Active Publication Date: 2024-10-24DEXERIALS CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022171547
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2014-10-28
Filing Date
2022-10-26
Publication Date
2024-10-24
Estimated Expiration
2035-10-28

AI Technical Summary

Technical Problem

Conventional anisotropic conductive films face challenges in maintaining regular particle arrangements due to conductive particle aggregation and dropout, leading to short circuits and poor conduction, especially with narrower pitch terminals in electronic devices.

Method used

The anisotropic conductive film is designed with a planar lattice pattern where the ratio of missing and aggregated lattice points is controlled, with conductive particles placed at lattice points and attached to the tips of columnar convex parts, ensuring minimal dropout and aggregation, and a manufacturing method involving a transfer process is used.

Benefits of technology

This design achieves good initial conductivity and reliability with reduced short circuits, making it suitable for connections between electronic components with narrow pitches.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572638000006
    Figure 0007572638000006
  • Figure 0007572638000007
    Figure 0007572638000007
  • Figure 0007572638000008
    Figure 0007572638000008
Patent Text Reader

Abstract

Provided is an anisotropic conductive film that has regularly arranged conductive particles and significantly reduces the occurrence of short circuits and poor conduction. [Solution] An anisotropic conductive film having an insulating adhesive base layer and conductive particles arranged at the lattice points of a planar lattice pattern has a structure in which the proportion of lattice points where no conductive particles are arranged relative to all lattice points of the planar lattice pattern assumed in any reference area is less than 20%, the proportion of lattice points where multiple conductive particles are arranged in agglomerates relative to all lattice points of the planar lattice pattern is 15% or less, and the sum of missing particles and agglomerates is less than 20%.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an anisotropic conductive film. [Background technology]

[0002] Anisotropic conductive films in which conductive particles are dispersed in an insulating resin binder are widely used when mounting electronic components such as IC chips on wiring boards, etc., but it is known that the conductive particles exist in a linked or aggregated state in such anisotropic conductive films. For this reason, when anisotropic conductive films are used to connect terminals of IC chips and terminals of wiring boards, which are becoming narrower in pitch as electronic devices become lighter and smaller, there have been cases where short circuits have occurred between adjacent terminals due to the conductive particles existing in a linked or aggregated state in the anisotropic conductive film.

[0003] Conventionally, as an anisotropic conductive film corresponding to such narrow pitch, a film in which conductive particles are regularly arranged in the film has been proposed. For example, an anisotropic conductive film has been proposed in which an adhesive layer is formed on a stretchable film, conductive particles are densely packed in a single layer on the surface of the adhesive layer, and then the film is biaxially stretched until the distance between the conductive particles becomes a desired distance to arrange the conductive particles regularly, and then an insulating adhesive base layer that is a component of the anisotropic conductive film is pressed against the conductive particles, and the conductive particles are transferred to the insulating adhesive base layer (Patent Document 1). In addition, an anisotropic conductive film has been proposed in which conductive particles are scattered on a recess-forming surface of a transfer mold having a recess on its surface, the recess-forming surface is squeegeeed to hold the conductive particles in the recess, an adhesive film on which an adhesive layer for transfer is formed is pressed from above, the conductive particles are primarily transferred to the adhesive layer, and then an insulating adhesive base layer that is a component of the anisotropic conductive film is pressed against the conductive particles attached to the adhesive layer, and the conductive particles are transferred to the insulating adhesive base layer (Patent Document 2). In these anisotropic conductive films, an insulating adhesive cover layer is generally laminated on the surface on the conductive particle side so as to cover the conductive particles. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] WO2005 / 054388 [Patent Document 2] JP 2010-33793 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, because conductive particles tend to aggregate and turn into secondary particles due to static electricity and the like, it is difficult to keep conductive particles present alone as primary particles all the time. For this reason, the techniques of Patent Document 1 and Patent Document 2 have the following problems. That is, in the case of Patent Document 1, it is difficult to densely pack conductive particles in a single layer without defects over the entire surface of the stretchable film, and the conductive particles are packed into the stretchable film in an aggregated state, which can cause short circuits or generate unfilled areas (so-called "voids"), which can cause poor electrical continuity. In the case of Patent Document 2, when the recesses of the transfer mold are covered with conductive particles having a large particle diameter, these are subsequently removed by a squeegee, resulting in recesses that do not hold the conductive particles, causing conductive particles to be "missing" in the anisotropic conductive film and resulting in poor conductivity; conversely, when a large number of small conductive particles are pushed into the recesses, the conductive particles may aggregate when transferred to the insulating adhesive base layer; and, since the conductive particles located on the bottom side of the recesses are not in contact with the insulating adhesive base layer, they may be scattered on the surface of the insulating adhesive base layer, disrupting the regular arrangement and causing short circuits or poor conductivity.

[0006] As described above, Patent Documents 1 and 2 do not fully consider how to control the "loosening" and "aggregation" of conductive particles that are to be arranged in a regular pattern on an anisotropic conductive film.

[0007] The object of the present invention is to solve the problems of the conventional technology described above, and to provide an anisotropic conductive film in which the occurrence of short circuits and poor conductivity is greatly suppressed from the viewpoint of "missing" and "aggregation" of conductive particles that should be arranged in a regular pattern. [Means for solving the problem]

[0008] The inventors have found that when arranging conductive particles at the lattice points of a planar lattice, the above-mentioned object can be achieved by controlling the "proportion of lattice points where conductive particles are not arranged" and the "proportion of lattice points where conductive particles are arranged in an aggregated manner" with respect to all lattice points of a planar lattice pattern assumed in any reference region of an anisotropic conductive film, and have completed the present invention. In addition, the inventors have found that such an anisotropic conductive film can be manufactured by attaching conductive particles to the tips of the convex portions of a transfer body having columnar convex portions formed on the surface thereof and transferring the conductive particles, rather than arranging conductive particles in the concave portions of the transfer body, and have completed the manufacturing method of the present invention.

[0009] That is, the present invention provides an anisotropic conductive film having a structure in which conductive particles are arranged at lattice points of a planar lattice pattern on an insulating adhesive base layer, The ratio of lattice points at which conductive particles are not arranged to all lattice points of a planar lattice pattern assumed in a reference region of the anisotropic conductive film is less than 20%; The present invention provides an anisotropic conductive film in which the ratio of lattice points where a plurality of conductive particles are arranged in an aggregated manner to the total lattice points of the planar lattice pattern is 15% or less, and the sum of the voids and aggregates is less than 20%.

[0010] In addition, the present invention provides a method for manufacturing an anisotropic conductive film, the ratio of lattice points at which conductive particles are not arranged to all lattice points of a planar lattice pattern assumed in a reference region of the anisotropic conductive film being less than 5%; The present invention provides an anisotropic conductive film in which the ratio of lattice points where a plurality of conductive particles are arranged in an aggregated manner to the total lattice points of the planar lattice pattern is more than 10% and less than 15%. In this case, too, the sum of the voids and the aggregates is preferably less than 20%.

[0011] The present invention also provides a method for producing the above-mentioned anisotropic conductive film having a structure in which an insulating adhesive base layer and an insulating adhesive cover layer are laminated and conductive particles are arranged at lattice points of a planar lattice pattern in the vicinity of the interface between them, the method comprising the steps of: <Process (a)> preparing a transfer body having a surface on which columnar protrusions corresponding to the lattice points of the planar lattice pattern are formed; <Process (b)> a step of forming a weak adhesive layer on at least the top surface of the convex portion of the transfer body; <Process (C)> a step of attaching conductive particles to the slightly adhesive layer on the convex portions of the transfer body; <Step (D)> A step of transferring the conductive particles to the insulating adhesive base layer by superposing and pressing an insulating adhesive base layer on the surface of the transfer body on which the conductive particles are attached; and <Process (e)> A process of laminating an insulating adhesive cover layer on the insulating adhesive base layer to which the conductive particles have been transferred from the conductive particle transfer surface side. The present invention provides a method for producing the same.

[0012] The present invention further provides a connection structure in which a terminal of a first electronic component and a terminal of a second electronic component are anisotropically conductively connected by the anisotropic conductive film of the present invention. Effect of the Invention

[0013] In the anisotropic conductive film of the present invention, the ratio of "grid points where conductive particles are not arranged" to all lattice points of the planar lattice pattern assumed in the reference region is set to less than 20%, the ratio of lattice points where a plurality of conductive particles are arranged in agglomeration to all lattice points of the planar lattice pattern is set to 15% or less, and the sum of missing and agglomeration is set to less than 20%. Therefore, when the anisotropic conductive film of the present invention is applied to an anisotropic conductive connection, good initial conductivity (initial conduction resistance value) and good conduction reliability after aging can be realized, and the occurrence of short circuits can be suppressed. In addition, it is economically excellent not only for COG but also for electronic components with sufficiently large bump area and distance, such as FOG.

[0014] In a preferred anisotropic conductive film of the present invention, the ratio of "lattice points where no conductive particles are arranged" to all lattice points of a planar lattice pattern assumed in any reference region is set to less than 5%, and the ratio of "lattice points where a plurality of conductive particles are arranged in an aggregate" is set to more than 10% and less than 15%. Therefore, when the anisotropic conductive film of the present invention is applied to an anisotropic conductive connection, a good initial conductive resistance value and good conductive reliability after aging can be achieved, and the occurrence of short circuits can also be suppressed.

[0015] In addition, in the manufacturing method of the anisotropic conductive film of the present invention, a transfer body having a surface formed with columnar convex portions corresponding to the lattice points of a planar lattice pattern is used, and conductive particles are attached to a micro-adhesive layer formed on the top surface of the convex portions, and then the conductive particles are transferred to an insulating adhesive base layer. Therefore, the ratio of "lattice points where no conductive particles are arranged" to all lattice points of a planar lattice pattern assumed in any reference region of the anisotropic conductive film can be made less than 5%, and the ratio of "lattice points where a plurality of conductive particles are arranged in an aggregate" to all lattice points of the planar lattice pattern can be made more than 10% and less than 15%. Therefore, the manufacturing method of the present invention can manufacture an anisotropic conductive film economically, and by using this anisotropic conductive film, an anisotropic conductive connection can be made between a narrow-pitched IC chip and a wiring board while greatly suppressing the occurrence of short circuits and poor conduction. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a cross-sectional view of an anisotropic conductive film of the present invention. [Figure 2A] FIG. 2A is a plan view perspective view of an anisotropic conductive film of the present invention. [Figure 2B] FIG. 2B is a partially enlarged plan view of the anisotropic conductive film of the present invention. [Figure 3A] FIG. 3A is a process explanatory diagram of the production method of the present invention. [Figure 3B] FIG. 3B is a process explanatory diagram of the manufacturing method of the present invention. [Figure 3C]FIG. 3C is a process explanatory diagram of the manufacturing method of the present invention. [Figure 3D] FIG. 3D is a process explanatory diagram of the production method of the present invention. [Figure 3E] FIG. 3E is a process explanatory diagram of the manufacturing method of the present invention. [Figure 3F] FIG. 3F is a process explanatory diagram of the manufacturing method of the present invention and is also a schematic cross-sectional view of the anisotropic conductive film of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The anisotropic conductive film of the present invention has a structure in which an insulating adhesive base layer and an insulating adhesive cover layer are laminated, and conductive particles are arranged at the lattice points of a planar lattice pattern near the interface between them. The ratio of lattice points where no conductive particles are arranged to all lattice points of the planar lattice pattern assumed in the reference region of this anisotropic conductive film is less than 20%, and the ratio of lattice points where multiple conductive particles are arranged in an aggregated manner to all lattice points of the planar lattice pattern is 15% or less, and the total of missing and aggregated particles is less than 20%. Hereinafter, the anisotropic conductive film of the present invention will be described in detail with reference to the drawings.

[0018] <Anisotropic conductive film> As shown in FIG. 1 (cross-sectional view) and FIG. 2A and FIG. 2B (planar perspective views), the anisotropic conductive film 10 of the present invention has a structure in which an insulating adhesive base layer 11 and an insulating adhesive cover layer 12 are laminated, and conductive particles 13 are arranged at the lattice points of a planar lattice pattern (dotted lines in FIG. 2A and FIG. 2B) near the interface between them. In FIG. 1, FIG. 2A and FIG. 2B, the planar lattice pattern is assumed to be along the longitudinal direction of the anisotropic conductive film 10 and the direction perpendicular thereto (short side direction), but it may be assumed to be inclined as a whole with respect to the longitudinal direction and short side direction. Here, arrow A indicates a position where a conductive particle is not arranged at a lattice point of the planar lattice, that is, a position where a conductive particle is "missing". Note that arrow B indicates a position where conductive particles are in contact with each other and aggregated (connected), and arrow C indicates a position where conductive particles are aggregated without contact. Here, "aggregated without contact" means that conductive particles are close to each other within a range not exceeding 25% of the average particle diameter of the conductive particles.

[0019] (Loss of conductive particles) In the anisotropic conductive film of the present invention, the ratio of "lattice points where no conductive particles are arranged" (A in FIG. 2A) (the ratio of lattices where conductive particles are missing) to all lattice points of a planar lattice pattern assumed in any reference region of the anisotropic conductive film is set to less than 5%, preferably 4% or less, and more preferably 1% to 4%. This makes it possible to achieve good initial conductive resistance and good conductive reliability after aging, and also to suppress the occurrence of short circuits, when the anisotropic conductive film of the present invention is applied to an anisotropic conductive connection.

[0020] (Plane grid pattern) Examples of planar lattice patterns include an oblique lattice, a hexagonal lattice, a square lattice, a rectangular lattice, and a parallelepiped lattice. Among these, a hexagonal lattice that allows closest packing is preferred.

[0021] Here, it is possible to select the entire surface of the anisotropic conductive film as the reference region of the anisotropic conductive film, but it is usually preferable to select an approximately rectangular region consisting of sides X and Y at the planar central portion of the anisotropic conductive film, which satisfies the following relational formula (A), preferably relational formula (1) and relational formulas (2) and (3), as the reference region.

[0022]

number

[0023] When applied to c-connection, which allows for a relatively large connection area, it is possible to reduce the amount of conductive particles in the film. In such a case, as shown below, it is preferable to increase the values ​​of X and Y, preferably to set them to 20D or more, and it is also preferable to set the value of "X+Y" to a value between 100D and about 400D, and ultimately to 400D.

[0024]

number

[0025] In the formulas (A) and (1) to (3), D is the average particle diameter of the conductive particles. The average particle diameter of the conductive particles can be measured by an image-type particle size distribution analyzer. It may also be measured by surface observation. Side Y is a straight line within a range of less than ±45° with respect to the longitudinal direction of the anisotropic conductive film (see FIG. 2A), and side X is a straight line perpendicular to side Y.

[0026] By defining the reference area in this way, the reference area can be made similar or approximate to the shape of the bump against which the conductive particles are pressed, and as a result, the allowable range of deviation of the conductive particles from the planar lattice pattern can be increased, making it possible to economically and stably perform anisotropic conductive connection. In other words, by making the minimum side of this reference area 5 times or more the conductive particle diameter, even if the conductive particles are displaced, missing, or close to each other within an expected range within this range, they will be captured by one of the bumps and will not excessively aggregate in the space between the bumps, so that anisotropic conductive connection can be reliably performed.

[0027] The reason why the minimum side is set to 5 times or more the conductive particle diameter is that, in general, at least one side of the bump connected by anisotropic conductive connection needs to be larger than the average particle diameter of the conductive particles to ensure capture, and the space between the bumps needs to be preferably 2 times or more the average particle diameter of the conductive particles to prevent short circuits. In other words, when focusing on a circular conductive particle as a standard, if no unexpected defects occur within a concentric circle having a diameter equal to the average particle diameter D of the conductive particles plus 4 times the length (4D) of the diameter (i.e., 5D), the above requirement can be satisfied. Also, the minimum distance between bumps in the case of fine pitch is, for example, less than 4 times the conductive particle diameter.

[0028] (Agglomeration of conductive particles) In the anisotropic conductive film of the present invention, the ratio of the lattice points (arrows B and C in FIG. 2A) where a plurality of conductive particles are arranged in an aggregated manner to all the lattice points of the planar lattice pattern is preferably 15% or less, and may be more than 10% and less than 15%, and there is no practical problem if it is 11% or more and 14% or less. If the ratio of the aggregated arrangement lattice points is within this range, even when the anisotropic conductive film of the present invention is applied to an anisotropic conductive connection, better initial conductivity and conductive reliability after aging can be realized, and the occurrence of short circuits can be further suppressed. Here, the state in which conductive particles are aggregated together includes not only the case where they are directly connected as shown by arrow B in FIG. 2A, but also the case where conductive particles are not directly connected to each other but are very close to each other as shown by arrow C in FIG. 2A. The distance between the conductive particles is preferably within 25% of the average particle diameter of the conductive particles. In addition, the degree of aggregation of conductive particles at one lattice point may be such that more than two conductive particles are connected in a chain shape, but from the viewpoint of suppressing short circuits, it is preferable that the aggregation is small, and it is preferable that more than two conductive particles do not aggregate.

[0029] In the present invention, the direction of aggregation of the conductive particles arranged in an aggregated state (usually the direction of a line connecting the centers of gravity of each of the two aggregated conductive particles) is shifted in the thickness direction, and is inclined toward the plane direction of the anisotropic conductive film, as indicated by arrows B and C in FIG. 1. The degree of inclination is preferably 5 to 45°, more preferably 10 to 40°, so as not to impede the pushing-in at the time of connection. The reason for this inclination is that if the conductive particles are present at the end of the bump at the time of connection, they can be captured at least on one side (if they overlap without being inclined, it will affect the pushing-in). There is no particular problem even if the aggregation is horizontal.

[0030] (Arrangement of conductive particles) It is preferable that 11 or more conductive particles are arranged in a row in a direction perpendicular to the longitudinal direction of the film, and more preferably 13 or more conductive particles are arranged in a row. This is because if conductive particles are missing in the longitudinal direction of the bump, this may cause problems with the anisotropic conductive connection. In this case, it is preferable that the above condition be satisfied in all three consecutive rows along the longitudinal direction of the film, and more preferably that the above condition be satisfied in all five rows. This allows the number of conductive particles captured by the bump to be greater than a certain level, and a stable anisotropic conductive connection can be achieved.

[0031] When the conductive particles are aggregated, it is preferable that there are three or less pairs of two-connected conductive particles around each two-aggregated conductive particle, more preferably two or less, and even more preferably one or less. This is because the presence of two-aggregated conductive particles close together can cause a short circuit. It is preferable that the two-aggregated conductive particles are not more than three consecutive in one direction of arrangement while satisfying the above conditions.

[0032] In addition, it is preferable that the conductive particle voids are such that four or more consecutive ones in the longitudinal direction of the film do not intersect with four or more consecutive ones in the direction perpendicular to the longitudinal direction of the film, it is more preferable that any of the four or more consecutive voids are not adjacent to each other via conductive particles that are one or more lattice points, and it is even more preferable that any of the four or more consecutive voids are not adjacent to each other via conductive particles that are two or more lattice points. There is no problem even if up to three rows of such voids intersect simultaneously with voids in one direction. If the voids are not continuous beyond this, they will be captured by the bumps by the conductive particles nearby.

[0033] Although it is generally not desirable to have multiple adjacent areas where consecutive gaps intersect, there is no problem with the stability of the anisotropic conductive connection if there is an arrangement of conductive particles in the same number or more as the number of gaps.

[0034] Furthermore, as shown in FIG. 2B, it is preferable in terms of preventing short circuits that the distance L between the lattice point P1 at which the aggregated conductive particles 13 are located and the center P2 of the circle inscribed in the aggregated conductive particles 13 be 25% or less of the average particle diameter of the conductive particles.

[0035] (particle area occupancy) Furthermore, the particle area occupancy rate of all conductive particles present in an arbitrary reference region of the anisotropic conductive film is usually 0.15% or more, preferably 0.35% or more, and more preferably 1.4% or more, when the bump size and the distance between the bumps are relatively large, such as in FOG connection. In this case, the upper limit is preferably 35% or less, more preferably 32% or less. In addition, when the bump size and the distance between the bumps are relatively small (for example, COG connection), it is more preferably 15 to 35%, particularly preferably 20 to 25%. Within this range, even when the anisotropic conductive film of the present invention is applied to an anisotropic conductive connection, better initial conductivity and conductivity reliability after aging can be achieved, and the occurrence of short circuits can be further suppressed. Here, the particle area occupancy rate is the ratio of the area occupied by all conductive particles present in an arbitrary reference region to the area S of the reference region. The area occupied by all conductive particles is expressed as (R / 2) where R is the average particle diameter of the conductive particles and n is the number of conductive particles. 2 ×π×n. Therefore, particle area occupancy rate (%) = [{(R / 2) 2 ×π×n} / S]×100.

[0036] By the way, the average particle diameter of the conductive particles is 2 μm and the particle density is 500 particles / mm 2 (0.0005 pieces / μm 2 ), X = Y = 200D, and X + Y = 400D, the calculated particle area occupancy is 0.157%. The average particle diameter of the conductive particles is 3 μm, and the particle density is 500 particles / mm 2 (0.0005 pieces / μm 2 ), X = Y = 200D, and X + Y = 400D, the calculated particle area occupancy is 0.35325%. The average particle diameter of the conductive particles is 3 μm, and the particle density is 2000 particles / mm 2 (0.002 pieces / μm2 ), X = Y = 200D, and X + Y = 400D, the calculated particle area occupancy is 1.413%. In addition, the average particle diameter of the conductive particles is 30 μm, and the particle density is 500 particles / mm 2 (0.0005 pieces / μm 2 ), X = Y = 200D, and X + Y = 400D, the calculated particle area occupancy rate is 35.325%.

[0037] (Conductive particles) The conductive particles may be appropriately selected from those used in known anisotropic conductive films. For example, metal particles such as nickel, copper, silver, gold, and palladium, and metal-coated resin particles in which the surface of resin particles such as polyamide and polybenzoguanamine is coated with a metal such as nickel, may be mentioned. In addition, the average particle size is preferably 1 to 30 μm, more preferably 1 to 10 μm, and particularly preferably 2 to 6 μm, from the viewpoint of ease of handling during production. The average particle size can be measured by an image type or laser type particle size distribution meter as described above.

[0038] The amount of conductive particles in the anisotropic conductive film depends on the lattice pitch of the planar lattice pattern and the average particle size of the conductive particles, and is usually 300 to 40,000 particles / mm 2 It is.

[0039] (distance between adjacent lattice points) Furthermore, the distance between adjacent lattice points in a planar lattice pattern assumed for the anisotropic conductive film is preferably greater than 0.5 times the average particle size of the conductive particles, more preferably at least 1 time, and even more preferably from 1 to 20 times. Within this range, even when the anisotropic conductive film of the present invention is applied to an anisotropic conductive connection, better initial conductivity and conductive reliability after aging can be achieved, and the occurrence of short circuits can be further suppressed.

[0040] (Insulating adhesive base layer) As the insulating adhesive base layer 11, those used as insulating adhesive base layers in known anisotropic conductive films can be appropriately selected and used. For example, a photoradical polymerizable resin layer containing an acrylate compound and a photoradical polymerization initiator, a thermal radical polymerizable resin layer containing an acrylate compound and a thermal radical polymerization initiator, a thermal cationic polymerizable resin layer containing an epoxy compound and a thermal cationic polymerization initiator, a thermal anionic polymerizable resin layer containing an epoxy compound and a thermal anionic polymerization initiator, or the like, or a cured resin layer thereof can be used. In addition, these resin layers can contain appropriately selected silane coupling agents, pigments, antioxidants, ultraviolet absorbers, etc., as necessary.

[0041] The insulating adhesive base layer 11 is formed by coating a coating composition containing the above-mentioned resin. The coating is formed by a cloth method, dried, and then cured, or by a known method. The film can be formed by forming the film by a method.

[0042] The thickness of such an insulating adhesive base layer 11 is preferably 1 to 30 μm, and more preferably 2 to 15 μm.

[0043] (Insulating adhesive cover layer) The insulating adhesive cover layer 12 may be appropriately selected from those used as insulating adhesive cover layers in known anisotropic conductive films, or may be made of the same material as the insulating adhesive base layer 11 described above.

[0044] The insulating adhesive cover layer 12 can be formed by forming a film of a coating composition containing the resin described above by a coating method and drying or further curing the film, or by forming the film into a film in advance by a known method.

[0045] The thickness of such an insulating adhesive cover layer 12 is preferably 1 to 30 μm, and more preferably 2 to 15 μm.

[0046] Furthermore, insulating fillers such as silica fine particles, alumina, and aluminum hydroxide may be added to the insulating adhesive base layer 11 and the insulating adhesive cover layer 12 as necessary. The amount of the insulating filler is preferably 3 to 40 parts by mass per 100 parts by mass of the resin constituting these layers. This makes it possible to suppress unnecessary movement of the conductive particles 2 by the molten resin even if the insulating adhesive layer 10 melts during anisotropic conductive connection.

[0047] (Lamination of insulating adhesive base layer and insulating adhesive cover layer, embedding conductive particles) In addition, when the insulating adhesive base layer 11 and the insulating adhesive cover layer 12 are laminated with the conductive particles 13 sandwiched therebetween, this can be done by a known method. In this case, the conductive particles 13 are present near the interface between these layers. Here, "present near the interface" means that a part of the conductive particles is embedded in one layer, and the remaining part is embedded in the other layer. The conductive particles may also be embedded in the insulating adhesive base layer. In this case, it can be formed without laminating the insulating adhesive cover layer.

[0048] <Production of anisotropic conductive film> Next, the insulating adhesive base layer and the insulating adhesive cover layer are laminated, and a conductive layer is formed near the interface between them. The anisotropic conductive film of the present invention has a structure in which conductive particles are arranged at the lattice points of a planar lattice pattern. The manufacturing method will be described. This manufacturing method includes the following steps (a) to (e). Each step will be described in detail below, however, the present invention is not limited to this production method.

[0049] (Step (a)) First, as shown in FIG. 3A, a transfer body 100 is prepared, on whose surface columnar convex portions 101 corresponding to the lattice points of a planar lattice pattern are formed. The columnar shape includes a cone. It is preferably a cylindrical shape. The height of the convex portions 101 can be determined according to the terminal pitch to be anisotropically conductively connected, the terminal width, the space width, the average particle diameter of the conductive particles, etc., and is preferably 2 to 4 times the average particle diameter of the conductive particles used. In addition, the width of the convex portions 101 (width at half height) is preferably 1.4 to 3.6 times the average particle diameter of the conductive particles. If the height and width are within these ranges, the effect of preventing excessive falling off and only sporadic falling off can be obtained.

[0050] Furthermore, the protrusions 101 are substantially flat to such a level that the conductive particles can be stably attached. It has a top surface.

[0051] *Examples of transcripts The transfer body to be prepared in this step (a) can be produced by using a known method, for example, by processing a metal plate to produce a master, applying a curable resin to it, and curing it. Specifically, a transfer body master having recesses corresponding to the protrusions is also produced by cutting a flat metal plate, and the resin composition constituting the transfer body is applied to the recessed surface of this master, cured, and then separated from the master to obtain the transfer body.

[0052] (Step (b)) Next, as shown in FIG. 3B, at least the top surfaces of the convex portions 101 of the transfer body 100 having a surface on which a plurality of convex portions 101 are formed in a planar grid pattern are made into a weakly adhesive layer 102.

[0053] *Slightly adhesive layer of transfer material The weakly adhesive layer 102 is a layer that exhibits an adhesive force capable of temporarily holding the conductive particles until the conductive particles are transferred to the insulating adhesive base layer that constitutes the anisotropic conductive film, and is formed on at least the top surface of the convex portion 101. Therefore, the entire convex portion 101 may be weakly adhesive. The thickness of the weakly adhesive layer 102 can be appropriately determined depending on the material of the weakly adhesive layer 102, the particle diameter of the conductive particles, and the like. In addition, "weakly adhesive" means that when the conductive particles are transferred to the insulating adhesive base layer, the adhesive force is weaker than that of the insulating adhesive base layer.

[0054] A weak adhesive layer used in a known anisotropic conductive film can be applied to such a weak adhesive layer 102. For example, it can be formed by applying a silicone-based adhesive composition or an adhesive layer made of the same material as the insulating adhesive base layer or the insulating adhesive cover layer to the top surface of the protrusion 101.

[0055] (Step (C)) 3C, conductive particles 103 are attached to the weak adhesive layer 102 of the convex portions 101 of the transfer body 100. Specifically, the conductive particles 103 are scattered from above the convex portions 101 of the transfer body 100, and the conductive particles 103 that do not adhere to the weak adhesive layer 102 are blown away with a blower. In this case, in some of the convex portions 101, the conductive particles adhere to the side surfaces due to the action of static electricity or the like with a certain frequency, and furthermore, it occurs that the conductive particles cannot be removed by the blower.

[0056] It is also possible to reverse the direction of the surface from FIG. 3C and attach the top surface of the protrusion to the surface that is covered with conductive particles. This is to avoid applying unnecessary stress to the conductive particles. By attaching only the conductive particles necessary for placement to the top surface of the protrusion in this way, the conductive particles can be easily collected and reused, and this is more economical than a method in which conductive particles are filled into an opening and then removed. However, when filling conductive particles into an opening and then removing them, there is a concern that unnecessary stress may be applied to the conductive particles that are not filled.

[0057] In Fig. 3C, the width of the weak adhesive layer 102 of the left half of the convex portion 101 is adjusted to be narrower than that of the weak adhesive layer 102 of the right half of the convex portion 101. As a result, as shown in Fig. 3C, there may be a difference in the aggregation state of the conductive particles 103 between the left half and the right half.

[0058] (Step (D)) Next, as shown in Fig. 3D, the insulating adhesive base layer 104 that is to constitute the anisotropic conductive film is placed on the surface of the transfer body 100 on which the conductive particles 103 are attached and pressed, thereby transferring the conductive particles 103 to one side of the insulating adhesive base layer 104 (Fig. 3E). In this case, it is preferable to place the transfer body 100 on the insulating adhesive base layer 104 and press it so that the convex parts 101 face downward. By blowing with the transfer body facing downward, it is possible to easily remove the conductive particles that are not attached to the top surfaces of the convex parts.

[0059] (Step (E)) 3F, an insulating adhesive cover layer 105 is laminated on the conductive particle-transferred surface side of the insulating adhesive base layer 104 to which the conductive particles 103 have been transferred, thereby obtaining an anisotropic conductive film 200 of the present invention.

[0060] <Connection structure> The anisotropic conductive film of the present invention is disposed between a terminal (e.g., a bump) of a first electronic component (e.g., an IC chip) and a terminal (e.g., a bump, pad) of a second electronic component (e.g., a wiring board), and is fully cured by thermocompression bonding from the first or second electronic component side to form an anisotropic conductive connection, thereby providing a connection structure such as a so-called COG (chip on glass) or FOG (film on glass) in which short circuits and poor conductivity are suppressed. EXAMPLES

[0061] The present invention will be specifically described below.

[0062] Example 1 A nickel plate with a thickness of 2 mm was prepared, and cylindrical recesses (inner diameter 6 μm, depth 8 μm) were formed in a square lattice pattern to prepare a transfer master. The distance between the centers of adjacent recesses was 8 μm. Therefore, the density of the recesses is 16,000 pieces / mm 2 It was.

[0063] A photopolymerizable resin composition containing 60 parts by mass of phenoxy resin (YP-50, Nippon Steel & Sumikin Chemical Co., Ltd.), 29 parts by mass of acrylate resin (M208, Toagosei Co., Ltd.), and 2 parts by mass of photopolymerization initiator (IRGACURE184, BASF Japan Ltd.) was applied onto the obtained transfer master on a PET (polyethylene terephthalate) film to a dry thickness of 30 μm, and after drying at 80°C for 5 minutes, a transfer master was produced by irradiating it with 1000 mJ of light from a high-pressure mercury lamp.

[0064] The transfer body was peeled off from the master and wound around a stainless steel roll with a diameter of 20 cm so that the convex parts were on the outside. While rotating the roll, a weak adhesive composition containing 70 parts by mass of epoxy resin (jER828, Mitsubishi Chemical Corporation) and 30 parts by mass of phenoxy resin (YP-50, Nippon Steel & Sumikin Chemical Co., Ltd.) was brought into contact with the adhesive sheet impregnated into the nonwoven fabric, and the weak adhesive composition was adhered to the top surface of the convex parts, forming a weak adhesive layer with a thickness of 1 μm, thereby obtaining a transfer body.

[0065] Conductive particles (nickel-plated resin particles (AUL704, Sekisui Chemical Co., Ltd.)) with an average particle size of 4 μm were sprayed onto the surface of this transfer body, and then the conductive particles that were not attached to the slightly adhesive layer were removed by blowing.

[0066] The transfer body with the conductive particles attached was pressed from the conductive particle-attached surface against an insulating adhesive base layer, which was a 5 μm-thick sheet-like thermosetting insulating adhesive film (a film formed from an insulating adhesive composition containing 60 parts by mass of phenoxy resin (YP-50, Nippon Steel & Sumikin Chemical Co., Ltd.), 40 parts by mass of epoxy resin (jER828, Mitsubishi Chemical Co., Ltd.), 2 parts by mass of cationic curing agent (SI-60L, Sanshin Chemical Industry Co., Ltd.), and 20 parts by mass of silica microparticles (Aerosil RY200, Nippon Aerosil Co., Ltd.)) at a temperature of 50°C and a pressure of 0.5 MPa, thereby transferring the conductive particles to the insulating adhesive base layer.

[0067] On the conductive particle transfer surface of the obtained insulating adhesive base layer, another insulating adhesive film in sheet form having a thickness of 15 μm was superimposed as a transparent insulating adhesive cover layer (a film formed from an insulating adhesive composition containing 60 parts by mass of phenoxy resin (YP-50, Nippon Steel & Sumikin Chemical Co., Ltd.), 40 parts by mass of epoxy resin (jER828, Mitsubishi Chemical Co., Ltd.), and 2 parts by mass of cationic curing agent (SI-60L, Sanshin Chemical Industry Co., Ltd.)), and laminated at a temperature of 60° C. and a pressure of 2 MPa. This produced an anisotropic conductive film.

[0068] Example 2 An anisotropic conductive film was obtained by repeating Example 1, except that the amount of conductive particles dispersed and the number of blower cycles were doubled compared to Example 1.

[0069] Example 3 The cylindrical recesses of the transfer master have an inner diameter of 4.5 μm and a depth of 7.5 μm. The distance between the centers of adjacent recesses is 6 μm, and the density of the recesses is 28,000 pieces / mm. 2 An anisotropic conductive film was obtained by repeating Example 1, except that the conductive particles having an average particle diameter of 4 μm were replaced with conductive particles having an average particle diameter of 3 μm (AUL703, Sekisui Chemical Co., Ltd.).

[0070] Example 4 An anisotropic conductive film was obtained by repeating Example 3, except that the amount of conductive particles dispersed and the number of blower cycles were doubled compared to Example 3.

[0071] Comparative Example 1 The depth of the recesses on the transfer master is 4.4 μm, the inner diameter of the recesses is 4.8 μm, the center distance between adjacent recesses is 5.6 μm, and the density of the recesses is 32,000 pieces / mm 2 An anisotropic conductive film was obtained by repeating Example 1 except for the above.

[0072] Comparative Example 2 The depth of the recesses on the transfer master is 3.3 μm, the inner diameter of the recesses is 3.3 μm, the center distance between adjacent recesses is 4.2 μm, and the density of the recesses is 57,000 pieces / mm 2 An anisotropic conductive film was obtained by repeating Example 1, except that the conductive particles having an average particle diameter of 4 μm were replaced with conductive particles having an average particle diameter of 3 μm (AUL703, Sekisui Chemical Co., Ltd.).

[0073] <Evaluation> (Disappearance and aggregation of conductive particles) For the anisotropic conductive films of Examples 1 to 4 and Comparative Examples 1 and 2, a 1 cm square area was observed from the transparent insulating adhesive cover layer side with an optical microscope (MX50, Olympus Corporation), and the ratio of lattice points to all lattice points to which no conductive particles were attached (missing [%]) in an assumed planar lattice pattern and the ratio of lattice points to all lattice points to which two or more conductive particles were aggregated were examined. The results are shown in Table 1.

[0074] In addition, the maximum distance between the aggregated conductive particles (aggregation distance) was measured and is also shown in Table 1. Note that the "aggregation" direction was the horizontal direction of the anisotropic conductive film in all cases.

[0075] (particle area occupancy) The particle area occupancy was calculated from the average particle diameter of the conductive particles and the density of the recesses on the transfer body master (= the density of the protrusions on the transfer body), taking into account the "dropout" and "aggregation" of the conductive particles. The results are shown in Table 1.

[0076] (Initial Conduction Resistance) Using the anisotropic conductive films of the examples and comparative examples, an IC chip having gold bumps of 15 μm height and 30 μm×50 μm with a 12 μm space between the bumps was anisotropically conductively connected to a glass substrate having wiring spaced 12 μm apart at 180° C., 60 MPa, and 5 seconds to obtain a connection structure. The initial conduction resistance of the connection structure obtained was measured using a resistance measuring device (digital multimeter 7565, Yokogawa Electric Corporation). The results are shown in Table 1. It is desirable that the resistance be 0.5Ω or less.

[0077] (Continuity reliability) The connection structure used for measuring the initial conduction resistance value was placed in an aging tester set at a temperature of 85°C and a humidity of 85%, and the conduction resistance value after leaving it for 500 hours was measured in the same manner as the initial conduction resistance. The results are shown in Table 1. It is desirable that the conduction resistance value be 5 Ω or less.

[0078] (Short circuit occurrence rate) The same connection structure as that used for the initial conduction resistance was created, and the occurrence of short circuits between adjacent wirings was examined. The results are shown in Table 1. It is desirable that the rate of short circuit occurrence is 50 ppm or less.

[0079] [Table 1]

[0080] The results in Table 1 show that the connection structures using the anisotropic conductive films of Examples 1 to 4 showed good results in terms of the evaluation items of initial conduction resistance, conduction reliability, and short circuit occurrence rate.

[0081] On the other hand, in the case of the anisotropic conductive films of Comparative Examples 1 and 2, although the rate of "lost" conductive particles was low, the rate of "aggregation" was too high, resulting in a short circuit occurrence rate that far exceeded 50 ppm.

[0082] Example 5 The recess density is 500 pieces / mm 2A transfer body was produced in the same manner as in Example 2, except that the distance between the centers of adjacent recesses was adjusted in order to use a transfer master having a thickness of 100 nm or less, and an anisotropic conductive film was also produced. For the obtained anisotropic conductive film, the "missing" and "aggregation" of conductive particles were measured in the same manner as in Example 2, and the particle area occupancy was calculated. As a result, the "missing" and "aggregation" of conductive particles were found to be the same as in Example 2. The particle area occupancy was also 0.7%.

[0083] The anisotropic conductive film obtained was sandwiched between a glass substrate (ITO solid electrode) and a flexible wiring substrate (bump width: 200 μm, L (line) / S (space) = 1, wiring height 10 μm), and anisotropic conduction was performed under conditions of 180 ° C, 80 MPa, and 5 seconds so that the connection bump length was 1 mm, to obtain a connection structure for evaluation. The "initial conduction resistance value" of the obtained connection structure and its "conductivity reliability" after being placed in a thermostatic chamber at a temperature of 85 ° C and a humidity of 85% RH for 500 hours were measured by a four-terminal method at a current of 1 A using a digital multimeter (34401A, manufactured by Agilent Technologies, Inc.). In the case of the "initial conduction resistance value", a measured value of 2 Ω or less was evaluated as good, and a measured value exceeding 2 Ω was evaluated as bad. In the case of the "conductivity reliability", a measured value of 5 Ω or less was evaluated as good, and a measured value of 5 Ω or more was evaluated as bad. As a result, all of the connection structures of Example 5 were evaluated as "good". Moreover, when the "rate of occurrence of short circuits" was measured in the same manner as in Example 2, good results were obtained, similar to those in Example 2.

[0084] Example 6 The recess density is 2000 pieces / mm 2 A transfer body was produced in the same manner as in Example 2, except that the distance between the centers of adjacent recesses was adjusted in order to use a transfer master having a thickness of 100 nm or less, and an anisotropic conductive film was also produced. For the obtained anisotropic conductive film, the "missing" and "aggregation" of conductive particles were measured in the same manner as in Example 2, and the particle area occupancy was calculated. As a result, the "missing" and "aggregation" of conductive particles were found to be the same as in Example 2. The particle area occupancy was also 2.7%.

[0085] A connection structure for evaluation was obtained by sandwiching the obtained anisotropic conductive film between a glass substrate and a flexible wiring substrate and connecting the anisotropically conductive film in the same manner as in Example 5. The obtained connection structure was evaluated for "initial conductive resistance value," "conductivity reliability," and "rate of occurrence of short circuit" in the same manner as in Example 5, and good results were obtained for all of them. [Industrial Applicability]

[0086] In a preferred anisotropic conductive film of the present invention, the ratio of "lattice points where no conductive particles are arranged" to all lattice points of a planar lattice pattern assumed in any reference region is set to less than 5%, and the ratio of "lattice points where a plurality of conductive particles are arranged in an aggregate" to all lattice points of the planar lattice pattern is more than 10% and less than 15%. Therefore, when the anisotropic conductive film of the present invention is applied to an anisotropic conductive connection, good initial conductivity and good conductive reliability after aging can be achieved, and the occurrence of short circuits can be suppressed, making it useful when an anisotropic conductive connection is made between a narrow-pitched IC chip and a wiring board. [Explanation of symbols]

[0087] 10, 200 Anisotropic Conductive Film 11, 104 Insulating adhesive base layer 12, 105 Insulating adhesive cover layer 13, 103 Conductive particles 100 Transcripts 101 Convex 102 Slight adhesive layer A: A position where no conductive particle is placed at the lattice point (a position where a conductive particle is missing). B: Position where conductive particles are in contact with each other and aggregate C: Position where conductive particles are agglomerated without contacting each other P1 Lattice point where aggregated conductive particles are arranged P2 Center of a circle inscribed in the agglomerated conductive particles L Distance between P1 and P2

Claims

1. An anisotropic conductive film having a structure in which conductive particles are arranged at lattice points of a planar lattice pattern on an insulating adhesive base layer, the ratio of lattice points at which conductive particles are not arranged to all lattice points of a planar lattice pattern assumed in a reference region of the anisotropic conductive film is less than 20%; the ratio of lattice points where a plurality of conductive particles are arranged in an aggregated manner to all lattice points of the planar lattice pattern is 15% or less, and the sum of the voids and the aggregates is less than 20%, When the conductive particles are aggregated, the number of pairs of two connected conductive particles around two aggregated conductive particles is three or less; In each of three consecutive rows along the longitudinal direction of the anisotropic conductive film in a planar grid pattern, 11 or more conductive particles are consecutively arranged in a direction perpendicular to the longitudinal direction of the film, The reference region is a region at the center of the plane of the anisotropic conductive film that satisfies the following relations (A), (2), and (3): [0010] wherein D is the average particle diameter of the conductive particles, side Y is a straight line within a range of less than ±45° with respect to the longitudinal direction of the anisotropic conductive film, and side X is a straight line perpendicular to side Y.

2. An anisotropic conductive film having a structure in which conductive particles are arranged at lattice points of a planar lattice pattern on an insulating adhesive base layer, The ratio of lattice points at which conductive particles are not arranged to all lattice points of a planar lattice pattern assumed in any reference region of the anisotropic conductive film is less than 5%; a ratio of lattice points at which a plurality of conductive particles are arranged in an aggregated manner to all lattice points of the planar lattice pattern is more than 10% and less than 15%; When the conductive particles are aggregated, the number of pairs of two connected conductive particles around two aggregated conductive particles is three or less; In each of three consecutive rows along the longitudinal direction of the anisotropic conductive film in a planar grid pattern, 11 or more conductive particles are consecutively arranged in a direction perpendicular to the longitudinal direction of the film, The reference region is a region at the center of the plane of the anisotropic conductive film that satisfies the following relations (A), (2), and (3): [0010] wherein D is the average particle diameter of the conductive particles, side Y is a straight line within a range of less than ±45° with respect to the longitudinal direction of the anisotropic conductive film, and side X is a straight line perpendicular to side Y.

3. 3. The anisotropic conductive film according to claim 1, wherein the sum of X and Y is 100D.

4. 4. The anisotropic conductive film according to claim 1, wherein the particle area occupancy rate of all conductive particles present in an arbitrary reference region of the anisotropic conductive film is 15 to 35% of the area of ​​the reference region.

5. 5. The anisotropic conductive film according to claim 1, wherein the conductive particles have an average particle size of 1 to 10 μm, and the distance between adjacent lattice points in the planar lattice pattern is greater than 0.5 times the average particle size of the conductive particles.

6. 6. The anisotropic conductive film according to claim 1, wherein the direction of aggregation of the conductive particles arranged in an aggregated state is inclined with respect to the planar direction of the anisotropic conductive film.

7. 7. The anisotropic conductive film according to claim 1, wherein the distance between the lattice points at which the agglomerated conductive particles are arranged and the center of a circle inscribed in the agglomerated conductive particles is 25% or less of the average particle diameter of the conductive particles.

8. 4. The anisotropic conductive film according to claim 1, wherein the particle area occupancy rate of all conductive particles present in an arbitrary reference region of the anisotropic conductive film is 0.15% or more.

9. 9. The anisotropic conductive film according to claim 8, wherein the conductive particles have an average particle size of 1 to 30 μm, and the distance between adjacent lattice points in the planar lattice pattern is greater than 0.5 times the average particle size of the conductive particles.

10. 10. The anisotropic conductive film according to claim 1, further comprising an insulating adhesive cover layer laminated on the insulating adhesive base layer.

11. 11. The anisotropic conductive film according to claim 10, wherein conductive particles are arranged at lattice points of a planar lattice pattern in the vicinity of the interface between the insulating adhesive base layer and the insulating adhesive cover layer.

12. An anisotropic conductive film as described in any one of claims 1 to 11, wherein, when conductive particles are missing, four or more consecutive missing particles in the longitudinal direction of the anisotropic conductive film and four or more consecutive missing particles in a direction perpendicular to the longitudinal direction of the anisotropic conductive film do not intersect.

13. A connection structure in which a terminal of a first electrical component and a terminal of a second electrical component are anisotropically conductively connected by the anisotropic conductive film according to any one of claims 1 to 12.

14. A method for manufacturing a connection structure, comprising: disposing the anisotropic conductive film according to any one of claims 1 to 12 between a terminal of a first electrical component and a terminal of a second electrical component; and crimping the anisotropic conductive connection.

Citation Information

Patent Citations

  • Fine-pitch anisotropic conductive adhesive

    JP2002519473A

  • Anisotropic conductive adhesive sheet and its manufacturing method

    JP2003286457A

  • Method for manufacturing particle transfer film

    JP2010033793A

  • Anisotropic conductive adhesive sheet and coupling structure

    WO2005054388A1