Transition metal doped silica sol and method for producing same
A transition metal-doped silica sol with optimized particle size and doping levels addresses transparency and light resistance issues, ensuring effective color retention in various applications.
Patent Information
- Application Number
- JP2024515941
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-11-30
- Filing Date
- 2023-11-30
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2043-11-30
AI Technical Summary
Existing transition metal-containing silica particles face challenges in achieving both transparency and light resistance due to insufficient tinting power, large particle diameters leading to light scattering, and poor coloring power due to transition metals not being present in porous or hollow structures.
A transition metal-doped colored silica sol with specific particle size, density, and surface area characteristics, along with controlled doping levels and particle distribution, ensuring excellent transparency, light resistance, and colorability.
The solution provides a silica sol with high light resistance and colorability, suitable for use in paints, inks, glazes, and molded objects, maintaining color integrity under UV exposure.
Smart Images

Figure 0007572662000004 
Figure 0007572662000005 
Figure 0007572662000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a colored silica sol containing colloidal silica particles, the colloidal silica particles being doped with a transition metal (hereinafter referred to as a transition metal-doped colored silica sol), and a method for producing the same. [Background technology]
[0002] Conventionally, pigments have been widely used as colorants for applications such as inks, paints, plastics, rubber, fibers, and toners. These pigments are broadly classified into two types: organic pigments and inorganic pigments. In general, organic pigments are superior in color clarity, coloring power, and chemical resistance compared to inorganic pigments, but tend to have lower light resistance, heat resistance, and solvent resistance (see Non-Patent Document 1). In addition, for applications such as color filters and inkjet inks, high transparency is required for pigments as colorants, and the particle size of organic pigments is reduced by various methods to reduce light scattering and increase transparency (see Non-Patent Documents 2 and 3).
[0003] One method for coloring silica-based glass is known to be doping the glass with a transition metal. Many of these colored glasses have high light resistance and are used for, for example, highly designed crafts such as stained glass and cut glass, ornaments, containers, furniture, and building materials (see Non-Patent Document 4).
[0004] Similarly, various techniques for providing silica particles containing transition metals have been proposed. For example, Patent Document 1 discloses a method of obtaining a silica sol having a mass ratio of Cu to silica (Cu / silica) of about 0.0007 by adding an active silicic acid aqueous solution as a feed liquid to a heel liquid having a silica / alkali (molar ratio) of 44.9, which is obtained by adding an active silicic acid aqueous solution and Cu(NO3)2·3H2O to a sodium silicate aqueous solution. Patent Document 2 discloses a method of obtaining a silica sol having a mass ratio of Cu to silica (Cu / silica) of about 0.0005 and a mean particle diameter of 89 nm by using a transition metal-free silica sol having a mean particle diameter of 76 nm as a core and coating a mixed layer in which Cu is dispersed in silica using a CuSO4-containing active silicic acid aqueous solution. Patent Document 3 discloses a method of obtaining amorphous silica particles having a volume average particle diameter of 0.15 μm and a mass ratio of Fe to silica (Fe / silica) of about 0.009 by burning metal silicon and an Fe source in an atmosphere in the presence of oxygen. Patent Document 4 discloses a method for obtaining silica particles having a mass ratio of Cu to silica (Cu / silica) of about 0.04 by contacting silica particles having an average particle size of 0.75 μm produced by a sol-gel method with a CuSO4 aqueous solution. Patent Document 5 discloses a method for obtaining silica particles having a mass ratio of Co to silica (Co / silica) of about 0.01 and a specific surface area of 1000 m 2 Patent Document 6 discloses a method for obtaining a porous silica powder having an average particle diameter of 61 nm or more by contacting a hollow silica sol with an aqueous CuSO4 solution to obtain silica particles having a mass ratio of Cu to silica (Cu / silica) of about 0.05. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 8-005657 [Patent Document 2] Patent Publication No. 2022-106677 [Patent Document 3] Patent No. 5389374 [Patent Document 4] Patent No. 3400826 [Patent Document 5] JP 2017-132687 A [Patent Document 6] JP 2022-115605 A [Non-patent literature]
[0006] [Non-Patent Document 1] Katsuhiko Matsuura, “Inorganic Pigments (II) Chromatic Pigments”, Color Materials, 55(8), p590-599 (1982) [Non-Patent Document 2] Shoji Funakura, "Pigments for Color Filters", Journal of the Japan Color Materials Association, 84(5), p179-183 (2011) [Non-Patent Document 3] Kyoichi Okada, "Current Status of Organic Pigments for Inkjet Printing", Journal of the Imaging Society of Japan, 49(1), p40-47 (2010) [Non-Patent Document 4] Hirokazu Kato, “Material Science of Artistic Glass (Revised Edition)” (2017) Summary of the Invention [Problem to be solved by the invention]
[0007] It is generally known that the transparency of organic pigments increases when the particle size is reduced, but in that case, the light resistance is also likely to decrease, and it is difficult to achieve both transparency and light resistance. On the other hand, the silica particles containing transition metals proposed in the above Patent Documents 1 and 2 have a small amount of transition metal and insufficient coloring power. The silica particles containing transition metals proposed in the above Patent Documents 3 and 4 have a large particle size, so light scattering is large and the transparency is insufficient. The silica particles containing transition metals proposed in the above Patent Documents 5 and 6 tend to have insufficient coloring power because the transition metals, which are coloring components, cannot exist in the pores of the porous structure or hollow structure.
[0008] The present invention has been made to solve the above problems, and an object of the present invention is to provide a transition metal-doped colored silica sol having excellent transparency, light resistance, and colorability, a method for producing the same, and a pigment composition, paint, ink, glaze, film, or molded article containing at least the transition metal-doped colored silica sol. [Means for solving the problem]
[0009] As a result of intensive research into solving the above problems, the present inventors have completed the present invention. A first aspect of the present invention provides a transition metal-doped colored silica sol that satisfies the following (1) to (4): (1) The mass ratio of the transition metal T to silica (T / silica) is 0.0001 or more and 0.05 or less; (2) the number average particle diameter (D1) of the particles in the silica sol calculated by image analysis of an electron microscope image is 5 nm or more and less than 50 nm; (3) the BET particle diameter (D2) of the particles in the silica sol calculated by the nitrogen adsorption method is 5 nm or more and less than 50 nm; (4) the ratio of the number average particle size to the BET particle size (D1 / D2) is 1.5 or less; As a second aspect, the transition metal-doped colored silica sol according to the first aspect, wherein the transition metal T is one or more selected from V, Cr, Mn, Fe, Co, Ni, and Cu; As a third aspect, the transition metal-doped colored silica sol has a specific surface area (SSA) of particles in the silica sol obtained by a nitrogen adsorption method of 50 m 2 / g or more, 550m 2 / g or less, As a fourth aspect, the transition metal-doped colored silica sol has a particle density PD of particles in the sol of at least 2.10 g / cm 3 The transition metal-doped colored silica sol according to any one of the first to third aspects, As a fifth aspect, the transition metal-doped colored silica sol according to any one of the first to fourth aspects, wherein a dried powder obtained by drying the transition metal-doped colored silica sol at 100° C. under air is amorphous. As a sixth aspect, the transition metal-doped colored silica sol according to any one of the first to fifth aspects, characterized in that particles in the sol are dispersed in an aqueous dispersion medium at a silica concentration of 1 mass % or more and 50 mass % or less. As a seventh aspect, the transition metal-doped colored silica sol according to any one of the first to sixth aspects, in which an average particle diameter (D3) of particles in the silica sol measured by a dynamic light scattering method is 5 nm or more and less than 100 nm. As an eighth aspect, the transition metal-doped colored silica sol according to any one of the first to seventh aspects, in which an apparent concentration of the transition metal T present in a dispersion medium of the transition metal-doped colored silica sol is less than 0.002 mass %. As a ninth aspect, the transition metal-doped colored silica sol is subjected to UV irradiation with a UVA-340 lamp at a UV irradiation intensity of 0.89 W / m 2 The transition metal-doped colored silica sol according to any one of the first to eighth aspects, wherein, before and after a UV irradiation test under conditions of a temperature of 50° C. and an irradiation time of 500 hours, a rate of change in absorbance at an absorption wavelength that causes coloring of the colored silica sol, as represented by the following formula (3), is 50 to 100%, as determined by visible-ultraviolet spectrum analysis: Absorbance change rate (%) = [absorbance after UV irradiation / absorbance before UV irradiation] × 100 (3), As a tenth aspect, the following steps (a), (b), (c), (d) and (e); (a) contacting an aqueous alkali silicate solution with a cation exchange resin to prepare an aqueous activated silicic acid solution; (b) mixing one or more selected from an aqueous alkali silicate solution, an aqueous activated silicic acid solution, an aqueous alkali solution, and a transition metal salt compound to prepare a heel liquid having a silica / alkali (molar ratio) of less than 30; (c) preparing a feed liquid comprising one or more kinds selected from an aqueous solution of active silicic acid, a transition metal salt compound, and an aqueous alkali solution; (d) adding the feed liquid to the heel liquid while maintaining the heel liquid in the vessel at a temperature of 60° C. or higher and 105° C. or lower; the mass ratio of transition metal T to silica (T / silica) is 0.0001 or more and 0.05 or less, the number average particle diameter D1 calculated from an electron microscope image by image analysis is 5 nm or more and less than 50 nm, the BET particle diameter D2 calculated from a nitrogen adsorption method is 5 nm or more and less than 50 nm, and the number average particle diameter / BET particle diameter (D1 / D2) ratio is 1.5 or less, A step of synthesizing a transition metal-doped colored silica sol, (e) (d) a step of obtaining a sizing liquid by maintaining the temperature at 60°C or more and 105°C or less for a certain period of time after the step; Including, a method for producing a transition metal-doped colored silica sol, wherein the transition metal salt compound is added during preparation of the heel solution, during preparation of the feed solution, or during preparation of both, and / or the transition metal salt compound is contained in at least one of the aqueous alkali silicate solution, the aqueous active silicic acid solution, and the aqueous alkali solution; As an eleventh aspect, the method for producing a transition metal-doped colored silica sol according to the tenth aspect, further comprising a step (f) of concentrating the transition metal-doped colored silica sol to obtain a concentrated liquid after the step (e). As a twelfth aspect, the method for producing a transition metal-doped colored silica sol according to the tenth aspect or the eleventh aspect, in which the aqueous alkali silicate solution is one or more selected from an aqueous lithium silicate solution, an aqueous sodium silicate solution, and an aqueous potassium silicate solution; As a thirteenth aspect, the method for producing a transition metal-doped colored silica sol according to any one of the tenth to twelfth aspects, in which the alkaline aqueous solution is one or more selected from the group consisting of aqueous solutions of lithium hydroxide, sodium hydroxide, potassium hydroxide, and ammonia. As a fourteenth aspect, the method for producing a transition metal-doped colored silica sol according to any one of the tenth to thirteenth aspects, in which a metal of the transition metal salt compound is one or more selected from V, Cr, Mn, Fe, Co, Ni, and Cu; As a fifteenth aspect, the transition metal-doped colored silica sol is characterized in that the specific surface area of the particles in the silica sol obtained by a nitrogen adsorption method is 50 m 2 / g or more, 550m 2 The method for producing a transition metal-doped colored silica sol according to any one of the tenth to fourteenth aspects, In a sixteenth aspect, the transition metal-doped colored silica sol has a particle density of particles in the sol of at least 2.10 g / cm. 3 The method for producing a transition metal-doped colored silica sol according to any one of the tenth to fifteenth aspects, As a seventeenth aspect, the method for producing a transition metal-doped colored silica sol according to any one of the tenth to sixteenth aspects, in which a dried powder obtained by drying the transition metal-doped colored silica sol at 100° C. under air is amorphous. As an eighteenth aspect, the method for producing a transition metal-doped colored silica sol according to any one of the tenth to seventeenth aspects, characterized in that the transition metal-doped colored silica sol is dispersed in an aqueous dispersion medium at a silica concentration of 1 mass % or more and 50 mass % or less. As a 19th aspect, the method for producing a transition metal-doped colored silica sol according to any one of the 10th to 18th aspects, in which the transition metal-doped colored silica sol has an average particle size (D3) of particles in the silica sol measured by a dynamic light scattering method of 5 nm or more and less than 100 nm; As a twentieth aspect, the method for producing a transition metal-doped colored silica sol according to any one of the tenth to nineteenth aspects, in which an apparent concentration of the transition metal T dissolved in a dispersion medium of the transition metal-doped colored silica sol is less than 0.002 mass %; According to a twenty-first aspect, there is provided a pigment composition comprising at least the transition metal-doped colored silica sol according to any one of the first to ninth aspects. According to a twenty-second aspect, there is provided a paint, ink, or glaze comprising at least the pigment composition according to the twenty-first aspect. As a 23rd aspect, a printed matter, a film, or a molded body comprising at least the pigment composition according to the 21st aspect; As a twenty-fourth aspect, there is provided the production method according to the tenth aspect, further comprising, after the step of adding the feed liquid of the step (d) to the heel liquid to synthesize particles of the transition metal-doped colored silica sol, and before the step (e), a step of adding an active silicic acid aqueous solution to the heel liquid while maintaining the heel liquid in the vessel at 60° C. or more and 105° C. or less to form a shell layer on the surfaces of the silica particles in the transition metal-doped colored silica sol. Effect of the Invention
[0010] According to the present invention, it is possible to provide a transition metal-doped colored silica sol having excellent transparency, light resistance and colorability, and a method for producing the same.
[0011] Furthermore, the transition metal-doped colored silica sol of the present invention can be used as a pigment composition as a colorant for various applications. This pigment composition can be mixed with a resin or the like to produce paints, inks, glazes, printed matter, films, molded bodies, etc. Furthermore, the transition metal-doped colored silica sol of the present invention has high light resistance, so it is resistant to discoloration and fading, and can be expected to be used for a long time in various applications. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 shows transmission electron microscope images (observation magnification: 100,000 times) of the Co-doped colored silica sol obtained in Example 1, the Cr-doped colored silica sol obtained in Example 13, the Mn-doped colored silica sol obtained in Example 14, the Cu-doped colored silica sol obtained in Example 15, the Ni-doped colored silica sol obtained in Example 16, and the silica sol obtained in Comparative Example 1. [Diagram 2]FIG. 2 shows the appearance of the UF concentrate of the Co-doped colored silica sol obtained in Example 1, the Cr-doped colored silica sol obtained in Example 13, the Mn-doped colored silica sol obtained in Example 14, the Cu-doped colored silica sol obtained in Example 15, the Ni-doped colored silica sol obtained in Example 16, and the UF concentrate of the silica sol obtained in Comparative Example 1. [Diagram 3] FIG. 3 shows the appearance of powders obtained by drying the UF concentrate of the Co-doped colored silica sol obtained in Example 1, the Cr-doped colored silica sol obtained in Example 13, the Mn-doped colored silica sol obtained in Example 14, the Cu-doped colored silica sol obtained in Example 15, the Ni-doped colored silica sol obtained in Example 16, and the UF concentrate of the silica sol obtained in Comparative Example 1 at 100° C. in air. [Figure 4] FIG. 4 shows X-ray diffraction patterns of powders obtained by drying the UF concentrate of the Co-doped colored silica sol obtained in Example 1, the Cr-doped colored silica sol obtained in Example 13, the Mn-doped colored silica sol obtained in Example 14, the Cu-doped colored silica sol obtained in Example 15, the Ni-doped colored silica sol obtained in Example 16, and the UF concentrate of the silica sol obtained in Comparative Example 1 at 100° C. in air. [Diagram 5] FIG. 5 shows the visible-ultraviolet transmission spectrum and the visible-ultraviolet absorption spectrum of the UF concentrate of the Co-doped colored silica sol obtained in Example 1, the Cr-doped colored silica sol obtained in Example 13, the Mn-doped colored silica sol obtained in Example 14, the Cu-doped colored silica sol obtained in Example 15, the Ni-doped colored silica sol obtained in Example 16, and the UF concentrate of the silica sol obtained in Comparative Example 1. [Figure 6] FIG. 6 is an evaluation of the light resistance of each of the Co-doped colored silica sols obtained in Examples 1 to 4, the Cr-doped colored silica sol obtained in Example 13, the Mn-doped colored silica sol obtained in Example 14, the Cu-doped colored silica sol obtained in Example 15, and the Ni-doped colored silica sol obtained in Example 16, showing the transition of the rate of change in absorbance at each absorption wavelength after 500 hours of UV irradiation. [Figure 7]FIG. 7 is an evaluation of the light resistance of each of the PGME diluted organic pigment dispersions of Comparative Examples 2 to 5, showing the transition of the rate of change in absorbance at each absorption wavelength after 500 hours of UV irradiation. [Figure 8] FIG. 8 shows a) the appearance of the colored film containing the Co-doped colored silica sol obtained in Example 18, b) a cross-sectional SEM image (magnification: 2000 times), and c) a visible-ultraviolet transmission spectrum. [Figure 9] FIG. 9 shows the appearances of the molded body containing the Co-doped colored silica sol obtained in Example 20, the molded body containing the silica sol obtained in Comparative Example 14, and the molded body obtained in Comparative Example 15. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described in detail below. [Transition metal doped colored silica sol] The present invention relates to a transition metal-doped colored silica sol that satisfies the following (1) to (4). (1) The mass ratio of the transition metal T to silica (T / silica) is 0.0001 or more and 0.05 or less; (2) the number average particle diameter (D1) of the particles in the silica sol calculated by image analysis of an electron microscope image is 5 nm or more and less than 50 nm; (3) the BET particle diameter (D2) of the particles in the silica sol calculated by the nitrogen adsorption method is 5 nm or more and less than 50 nm; (4) The ratio of the number average particle size to the BET particle size (D1 / D2) is 1.5 or less.
[0014] Regarding the above (1), the transition metal-doped colored silica sol of the present invention is a sol of particles in which a transition metal T is doped into colloidal silica particles, and the transition metal T is doped at a mass ratio (T / silica) of 0.0001 or more and 0.05 or less to the silica. Preferably, the mass ratio (T / silica) is 0.001 or 0.005 or more and 0.02 or less. If the mass ratio (T / silica) is less than 0.0001, the coloring property becomes insufficient, and if it is more than 0.05, it is difficult to dope the transition metal T into the silica particles, which is not preferable. The doped amount of the transition metal T can be quantified by analyzing the silica sol by inductively coupled plasma optical emission spectroscopy (ICP-OES), inductively coupled plasma mass spectrometry (ICP-MS), atomic absorption spectrometry (AA), X-ray fluorescence spectrometry (XRF), or the like after performing a known appropriate pretreatment. The transition metal T may be doped unevenly in the colloidal silica particles, or may be doped uniformly.
[0015] Regarding (2), the particle diameter of the particles in the transition metal-doped colored silica sol is 5 nm or more and less than 50 nm in number average particle diameter (D1) calculated from an electron microscope image by image analysis. Preferably, the number average particle diameter (D1) is 7 nm or more and 30 nm or less. If the number average particle diameter (D1) is smaller than 5 nm, the particles tend to aggregate with each other, resulting in poor dispersibility when made into a dispersion, and if it is larger than 50 nm, it is not preferable because the transparency is deteriorated due to strong light scattering such as Rayleigh scattering and Mie scattering. The number average particle diameter (D1) of the particles in the silica sol can be obtained by the following procedure. That is, the silica sol is subjected to a known appropriate pretreatment, and then observed with a transmission electron microscope (TEM), a scanning electron microscope (SEM), or a scanning transmission electron microscope (STEM), and the area of the particles is calculated from the obtained electron microscope image of the silica sol by image analysis, and the circle equivalent diameter, which is the diameter of a perfect circle equal to the area, is obtained. The number average value of this circle equivalent diameter can be the number average particle diameter (D1).
[0016] Regarding (3), the particle diameter of the particles in the transition metal-doped colored silica sol is further calculated by the nitrogen adsorption method (BET method) such that the BET particle diameter (D2) is 5 nm or more and less than 50 nm. Preferably, the BET particle diameter (D2) is 7 nm or more and 30 nm or less. If the BET particle diameter (D2) is less than 5 nm, the particles tend to aggregate with each other, resulting in poor dispersibility when made into a dispersion, whereas if it is more than 50 nm, it is not preferable because the transparency is deteriorated due to strong light scattering such as Rayleigh scattering and Mie scattering. The BET particle diameter of the particles in the silica sol is calculated by the specific surface area SSA (m 2 / g) and particle density PD (g / cm 3 ) by the following formula (1), and means the diameter of a spherical particle having the same specific surface area: BET particle diameter D2 (nm) = 6000 / [particle density PD (g / cm 3 )×specific surface area SSA(m 2 / g)] (1)
[0017] Regarding (4), the transition metal-doped colored silica sol has a ratio of the number average particle size to the BET particle size (D1 / D2) of 1.5 or less. Preferably, D1 / D2 is 1.3 or less. The lower limit of D1 / D2 can be selected from the range of 0.1 or more, 0.3 or more, 0.5 or more, 0.8 or more, or 1.0 or more. The silica particles in the silica sol preferably have a non-porous and non-hollow structure and are substantially solid particles. If D1 / D2 is greater than 1.5, the silica particles become highly porous or hollow, and the transition metal, which is a coloring component, cannot exist in the pores of the porous or hollow structure, which is undesirable since the coloring power tends to be insufficient. It is considered that the smaller the number-average particle size / BET particle size (D1 / D2) ratio, the more solid the particles become.
[0018] In addition, solid particles can be distinguished from porous or hollow particles by the difference in particle contrast when observed with a transmission electron microscope (TEM).
[0019] The particle shape of the silica particles in the silica sol is not particularly limited. For example, it may be spherical, ellipsoidal (rugby ball), cocoon-like, confetti-like, chain-like, or dice-like. Among them, spherical particles are preferred because they have high dispersibility and little light scattering.
[0020] The particle size distribution of the silica particles in the silica sol is not particularly limited. For example, a particle size distribution with one peak, a particle size distribution with two or more peaks, a particle size distribution with a narrow half-value width, a particle size distribution with a wide half-value width, etc. are included. Among them, a particle size distribution with one peak and a narrow half-value width is preferred because it causes less light scattering.
[0021] The transition metal T is preferably one or more selected from elements existing between Group 3 and Group 11 of the periodic table, and can be appropriately selected according to the absorption wavelength band. The transition metal T may be doped singly into the colloidal silica particles in the silica sol, or a plurality of transition metals T may be doped simultaneously into the colloidal silica particles in the silica sol. Alternatively, a silica sol in which one type of transition metal T is doped singly into the colloidal silica particles may be produced, and then a plurality of silica sols doped with another type of transition metal T may be mixed. The transition metal T is preferably one or more selected from the transition metals of the first transition series, and more preferably one or more selected from V, Cr, Mn, Fe, Co, Ni, and Cu.
[0022] The transition metal-doped colored silica sol has a specific surface area (SSA) of particles in the silica sol obtained by a nitrogen adsorption method of 50 m 2 / g or more, 550m 2 The specific surface area SSA is preferably 90 m 2 / g or more, 400m 2 / g or less. The specific surface area is 50m 2 If the specific surface area is less than 550 m / g, the transparency is likely to be lost when the silica sol is used in a resin composite material or the like. 2If the silica content is greater than 1 / g, the silica particles may have poor dispersibility in the dispersion medium or resin, making it difficult to add the silica particles at high concentrations.
[0023] The transition metal doped colored silica sol has a particle density PD of at least 2.10 g / cm 3 The upper limit of the particle density PD is preferably 3.0 g / cm. 3 , or 2.80 g / cm 3 , or 2.70 g / cm 3 , or 2.60 g / cm 3 , or 2.50 g / cm 3 , or 2.40 g / cm 3 , or 2.30 g / cm 3 , or 2.25 g / cm 3 The true density of bulk silica is generally 2.2 to 2.3 g / cm 3 Therefore, 2.10 g / cm 3 If it is smaller than this, closed pores resulting from the porous or hollow structure are present, and the transition metals that serve as coloring components cannot exist, which is undesirable since the coloring power is likely to be insufficient. This particle density PD is obtained, for example, by measuring the silica sol that has been heat-treated (dried) at 100°C in the atmosphere using a dry automatic density meter (Micromeritics, AccuPycII 1340TEC) with He gas.
[0024] The transition metal-doped colored silica sol is preferably dried in an amorphous form by heat-treating (drying) the sol at 100° C. in air. The crystallinity of the dried powder can be confirmed by X-ray diffraction, and when no crystalline phase derived from the transition metal T is confirmed by X-ray diffraction, the transition metal T is considered to be doped in the silica particles. In addition, cristobalite, tridymite, quartz, etc. are known as crystalline phases derived from silica, but crystalline silica is toxic, and from the viewpoint of safety, it is preferable that these crystalline phases cannot be confirmed (the powder is amorphous).
[0025] The transition metal-doped colored silica sol is preferably a silica sol in which transition metal-doped colloidal silica particles are dispersed in an aqueous dispersion medium at a silica concentration of 1% by mass or more and 50% by mass or less. The silica concentration is preferably 2% by mass or more and 40% by mass or less. If it is less than 1% by mass, the productivity may be low and the transportation cost may be low, and if it is more than 50% by mass, the dispersibility may be easily deteriorated due to the increase in the number of particles. The silica concentration can be calculated by removing metal elements such as transition metal T in oxide form from the solid residue obtained by heat-treating (drying) the transition metal-doped colored silica sol at a predetermined temperature and time. The water can be pure water such as ion-exchanged water, ultrafiltered water, reverse osmosis water, distilled water, or ultrapure water, and can be appropriately selected according to the purpose of use.
[0026] The transition metal-doped colored silica sol is preferably such that the average particle size (D3) of the particles in the silica sol measured by dynamic light scattering is 5 nm or more and less than 100 nm. The average particle size (D3) is preferably 10 nm or more and less than 80 nm. The measurement principle of the average particle size (D3) by dynamic light scattering is dynamic light scattering. For example, the silica sol can be measured by a dynamic light scattering particle size measuring device (Spectris, Zetasizer Nano) after performing a known appropriate pretreatment. If it is smaller than 5 nm, the dispersibility in the dispersion medium or resin is likely to decrease. On the other hand, if it is larger than 100 nm, it is not preferable because the transparency is deteriorated due to the strong light scattering such as Rayleigh scattering and Mie scattering.
[0027] The transition metal-doped colored silica sol desirably has a pH of 2 or more and 12 or less. The pH is preferably 2 or more and 4 or less, or 8 or more and 11 or less. If the pH of the silica sol is less than 2, the dispersibility may be easily deteriorated, and in addition, the transition metal T may be easily dissolved into the dispersion medium. If the pH is higher than 12, the silica may be easily dissolved and gelled, and in addition, the dissolved silica may easily dissolve the transition metal T into the dispersion medium.
[0028] The transition metal-doped colored silica sol preferably has an apparent concentration of the transition metal T dissolved in the dispersion medium of the silica sol of less than 0.002% by mass (less than 20 ppm by mass). The apparent concentration is preferably less than 0.0002% by mass (less than 2 ppm by mass). More preferably, it is less than 0.0001% by mass (less than 1 ppm by mass). If the apparent concentration is greater than 0.002% by mass, there are concerns about safety to the body and environmental impact. The apparent concentration of the transition metal T dissolved in the dispersion medium of the silica sol can be quantified by analyzing the filtrate obtained by treating the silica sol with an ultrafiltration (UF) membrane or reverse osmosis (RO) membrane having an appropriate molecular weight cutoff, and then analyzing it with inductively coupled plasma optical emission spectrometry (ICP-OES), inductively coupled plasma mass spectrometry (ICP-MS), atomic absorption spectrometry (AA), or the like after performing a known appropriate pretreatment.
[0029] The transition metal-doped colored silica sol was exposed to UV irradiation intensity of 0.89 W / m using a UVA-340 lamp. 2 It is desirable that the rate of change in absorbance, as represented by the following formula (3), at the absorption wavelength that causes coloring of the colored silica sol, before and after a UV irradiation test under conditions of a temperature of 50°C and an irradiation time of 500 hours (equivalent to 3.6 months of sunlight), as determined by visible-ultraviolet spectrum analysis, is 50 to 100%. Absorbance change rate (%) = [absorbance after UV irradiation / absorbance before UV irradiation] x 100 (3) The rate of change in absorbance before and after the UV irradiation test is preferably 60 to 100%, 70 to 100%, 75 to 100%, or 80 to 100%. The UV irradiation test can be carried out, for example, by placing the transition metal-doped colored silica sol in a quartz cell with a lid and an optical path length of 10 mm, placing it in a QUV accelerated weathering tester (manufactured by Q-Lab Co., Ltd., product name QUV / se), and using a UVA-340 type lamp. In addition, the absorption wavelengths for comparing the absorbance change vary depending on the color of the colored silica sol, that is, the type of transition metal T doped into the silica particles. When there are multiple absorption wavelengths derived from the transition metal T, the absorption wavelengths to be compared may be appropriately selected in consideration of the small influence of absorption due to other factors and the magnitude of absorption. For example, but not limited to, the absorbance can be compared at absorption wavelengths of around 640 nm for Co, around 590 nm for Cr, around 455 nm for Mn, around 640 nm for Cu, around 670 nm for Ni, around 425 nm and around 625 nm for V, and around 400 nm for Fe. The rate of change in absorbance can be calculated from the absorbance thus obtained using the following formula (3). The closer the absorbance change rate (%) is to 100%, the less the absorbance changes due to UV irradiation, and the silica sol can be judged to have high light resistance. In the present invention, the transition gold-doped colored silica sol has an absorbance change rate of 50 to 100%, which makes it a suitable silica sol that can maintain its color even when used in an environment exposed to sunlight.
[0030] The silica particles in the transition metal-doped colored silica sol may have a shell layer formed on the particle surface (in this case, the silica particles may be referred to as core particles). The shell layer is a shell layer coated with a metal oxide that does not intentionally contain a transition metal T (excluding unavoidable impurities). Note that the "shell layer formed on the particle surface" includes both an embodiment in which the surface of the silica particle is coated with a shell layer, and an embodiment in which the components constituting the shell layer are bonded to the surface of the silica particle. The former "embodiment in which the surface of the silica particle is covered with a shell layer" may be any embodiment in which the shell layer covers at least a part of the surface of the silica particle, that is, it includes an embodiment in which the shell layer covers a part of the surface of the silica particle (an embodiment in which the shell layer exists on a part of the surface of the silica particle) and an embodiment in which the shell layer covers the entire surface of the silica particle (an embodiment in which the shell layer exists on the entire surface of the silica particle).In this embodiment, it does not matter whether the shell layer is bonded to the surface of the silica particle or not. The latter "embodiment in which the component constituting the shell layer is bonded to the surface of the silica particle" may mean any embodiment in which the component constituting the shell layer is bonded to at least a portion of the surface of the silica particle, i.e., it includes an embodiment in which the component constituting the shell layer is bonded to a portion of the surface of the silica particle, an embodiment in which the component constituting the shell layer is bonded to a portion of the surface of the silica particle and covers at least a portion of the surface, and even an embodiment in which the component constituting the shell layer is bonded to the entire surface of the silica particle and covers the entire surface.
[0031] In the transition metal-doped colored silica sol, when the silica particles have a shell layer on the particle surface, the thickness of the shell layer (shell thickness) can be, for example, 0.3 nm or more and 5 nm or less, and can be, for example, 0.4 nm or more and 4 nm or less. By making the shell thickness, for example, 0.3 nm or more, the core region doped with the transition metal can be sufficiently covered, which can lead to the realization of improved light resistance. In addition, by making the shell thickness, for example, 5 nm or less, it is possible to ensure the coloring power of the transition metal doped in the core region, which can lead to the realization of a sol with excellent coloring properties.
[0032] As described above, in this embodiment, the surface of the silica particles may be partially or completely covered with a shell layer, but it is preferable that the surface is completely covered and has a non-porous structure. The shell thickness of the silica particles in the colored silica sol in this embodiment can be calculated by the following formula (2): Shell thickness = (number average particle size (D1) of silica particles having a shell layer formed thereon - number average particle size (D1) of core particles (silica particles having no shell layer) (used to produce silica particles having a shell layer)) ÷ 2 (2) The shell thickness may be calculated using the BET particle diameter (D2) instead of the number average particle diameter (D1).
[0033] [Method for producing transition metal-doped silica sol] The transition metal-doped silica sol of the present invention can be produced based on a silica sol production method generally called the water glass method, specifically, the following steps (a), (b), (c), (d) and (e); (a) contacting an aqueous alkali silicate solution with a cation exchange resin to prepare an aqueous activated silicic acid solution; (b) mixing one or more selected from an aqueous alkali silicate solution, an aqueous activated silicic acid solution, an aqueous alkali solution, and a transition metal salt compound to prepare a heel liquid having a silica / alkali (molar ratio) of less than 30; (c) preparing a feed liquid comprising one or more kinds selected from an aqueous solution of active silicic acid, a transition metal salt compound, and an aqueous alkali solution; (d) adding the heel liquid in the vessel, and while maintaining the heel liquid at 60° C. or more and 105° C. or less, adding the feed liquid to the heel liquid; the mass ratio of transition metal T to silica (T / silica) is 0.0001 or more and 0.05 or less, the number average particle diameter D1 calculated from an electron microscope image by image analysis is 5 nm or more and less than 50 nm, the BET particle diameter D2 calculated from a nitrogen adsorption method is 5 nm or more and less than 50 nm, and the number average particle diameter / BET particle diameter (D1 / D2) ratio is 1.5 or less, A step of synthesizing a transition metal-doped colored silica sol, (e) (d) a step of obtaining a sizing liquid by maintaining the temperature at 60°C or more and 105°C or less for a certain period of time after the step; Including, provided that the transition metal salt compound is added during preparation of the heel solution, during preparation of the feed solution, or during preparation of both, and / or the transition metal salt compound is contained in at least one of the aqueous alkali silicate solution, the aqueous active silicic acid solution, and the aqueous alkali solution; It can be manufactured.
[0034] The aqueous alkali silicate solution used in the step (a) is preferably one or more selected from an aqueous lithium silicate solution, an aqueous sodium silicate solution, and an aqueous potassium silicate solution. The aqueous alkali silicate solution may be used alone or in combination of two or more. From the viewpoint of economy, an aqueous sodium silicate solution called water glass is preferred. These aqueous alkali silicate solutions may be used by diluting them with water as necessary.
[0035] The cation exchange resin used in the step (a) can be appropriately selected from known ones and is not particularly limited. A strongly acidic cation exchange resin is preferable. For example, in the step of contacting an aqueous alkali silicate solution with a cation exchange resin, the aqueous solution is diluted with water to a silica concentration of 1% by mass or more and less than 10% by mass, and the aqueous solution is contacted with a strongly acidic cation exchange resin for decationization (dealkalization). If necessary, the aqueous solution can be contacted with a strongly basic anion exchange resin before or after contact with the cation exchange resin for deanionization. Various details of the contact conditions have been proposed in the past, and any of those known conditions can be adopted in the present invention.
[0036] Specific examples of strongly acidic cation exchange resins include Amberlite IR-120B (trade name), Amberjet 1020 (trade name, manufactured by Organo Corporation), DOWEX MARATHON GH (trade name, manufactured by The Dow Chemical Company), Diaion SK104 (trade name), Diaion PK208 (trade name, manufactured by Mitsubishi Chemical Group Corporation), and Duolite C20J (trade name, manufactured by Sumika Chemtex Corporation).
[0037] Specific examples of strongly basic anion exchange resins include Amberlite IRA400J, Amberlite IRA410J, Amberjet 4400 (manufactured by Organo Corporation), Diaion SA10A, Diaion SA20A (manufactured by Mitsubishi Chemical Group Corporation), and Duolite UBA120 (manufactured by Sumika Chemtex Corporation).
[0038] The concentration of the active silicic acid aqueous solution obtained in step (a) is preferably 1% by mass or more and 6% by mass or less, more preferably 3% by mass or more and 4% by mass or less, as silica. If the concentration is less than 1% by mass as silica, the productivity deteriorates, and if it is higher than 6% by mass, the active silicic acid aqueous solution becomes unstable and tends to gel. The pH of the active silicic acid aqueous solution is preferably 1 to 5, or pH 7 to 12, more preferably 2 to 4, or pH 8 to 11. If the pH is outside this range, the active silicic acid aqueous solution becomes unstable and tends to gel.
[0039] The heel liquid obtained in step (b) is prepared by mixing one or more types selected from an aqueous alkali silicate solution, an aqueous active silicic acid solution, an aqueous alkali solution, and a transition metal salt compound, so that the silica / alkali (molar ratio) is less than 30. If the silica / alkali (molar ratio) is greater than 30, the particles in the silica sol tend to fuse together during particle synthesis, which is undesirable as it tends to reduce dispersibility. When preparing the heel liquid, there are no particular limitations on the order of mixing and adding these aqueous solutions, etc., as long as they do not adversely affect the effects of the present invention. The aqueous alkali silicate solution and the aqueous active silicic acid solution in the step (b) may be the same as or different from those used and prepared in the step (a).
[0040] The alkaline aqueous solution used in the step (b) is preferably one or more selected from aqueous solutions of lithium hydroxide, sodium hydroxide, potassium hydroxide, and ammonia. The alkaline aqueous solution may be used alone or in combination of two or more. Aqueous alkaline solutions are commercially available in various concentrations, and these commercially available products may be used, or may be diluted with water as necessary.
[0041] The transition metal salt compound used in the step (b) is not particularly limited, and may be an organic salt or an inorganic salt, but is preferably at least one selected from chloride salts, nitrates, sulfates, borates, and phosphates. One type of transition metal salt compound may be used alone, or two or more types may be used. The transition metal salt compound is preferably used after being dissolved in water.
[0042] The metal of the transition metal salt compound used in step (b) is preferably one or more selected from V, Cr, Mn, Fe, Co, Ni, and Cu. The metal of these transition metal salt compounds may be used alone or in combination of two or more.
[0043] The feed liquid obtained in the step (c) is composed of one or more selected from an active silicic acid aqueous solution, a transition metal salt compound, and an alkaline aqueous solution. It may be used alone or in combination of two or more. In preparing the feed liquid, the order of mixing these aqueous solutions is not particularly limited as long as it does not adversely affect the effects of the present invention. If necessary, an acid aqueous solution such as hydrochloric acid, nitric acid, or sulfuric acid, or the alkaline aqueous solution may be added to adjust the pH to a level at which the active silicic acid aqueous solution is easily stabilized. The aqueous activated silicic acid solution in step (c) may be the same as or different from those used and prepared in step (a) and / or step (b), and the aqueous alkali solution and transition metal salt compound in step (c) may be the same as or different from those used in step (b). The transition metal salt compound may be added during preparation of the heel solution or feed solution, or may be originally contained in the aqueous alkali silicate solution, the aqueous active silicic acid solution, or the aqueous alkali solution, or both. That is, the transition metal salt compound is added during preparation of the heel solution in step (b), during preparation of the feed solution in step (c), or during preparation of both, and / or the transition metal salt compound is contained in at least one of the aqueous alkali silicate solution, the aqueous active silicic acid solution, and the aqueous alkali solution.
[0044] The liquid temperature of the heel liquid in the step (d) is 60° C. or higher and 105° C. or lower, and preferably 70° C. or higher and 100° C. or lower. If it is lower than 60° C., the reactivity of particle synthesis is low, which is not preferable. In this step, when multiple feed liquids are used, one type may be added alone, or two or more types may be added simultaneously. The rate at which the feed liquids are added to the heel liquid can be appropriately set for each.
[0045] Furthermore, after the step of adding the feed liquid in step (d) to the heel liquid to synthesize the transition metal-doped colored silica sol particles, and before the step (e) described below, a step of adding an aqueous solution of active silicic acid to the heel liquid while maintaining the heel liquid in the vessel at 60°C or higher and 105°C or lower to form a silica shell layer on the surface of the particles in the transition metal-doped colored silica sol may be included. In the step of forming the shell layer, the temperature of the heel liquid is 60°C or higher and 105°C or lower, preferably 70°C or higher and 100°C or lower. If it is lower than 60°C, the reactivity of the active silicic acid may be low, making it difficult to form a shell layer on the particle surface. The rate at which the active silicic acid aqueous solution is added to the heel liquid can be appropriately set. After the step (d) is completed, the mixture may be cooled to room temperature once and then heated again to form a shell layer. If necessary, the acid aqueous solution or the alkali aqueous solution may be further added to adjust the pH to a level at which a shell layer is easily formed on the particle surface, and then the shell layer may be formed.
[0046] In step (e), after step (d), the mixture is maintained at a temperature of 60°C or more and 105°C or less for a certain period of time to obtain a sizing liquid. The maintenance time is preferably between 0.5 hours and 24 hours. If it is shorter than 0.5 hours, unreacted active silicic acid remains in the system, which tends to deteriorate the dispersibility, and it is not preferable. If it is longer than 24 hours, it is not preferable from the viewpoint of productivity. Before carrying out step (e), if necessary, an aqueous acid solution such as hydrochloric acid, nitric acid, or sulfuric acid, or the above-mentioned aqueous alkali solution may be added to adjust the pH.
[0047] Furthermore, after the step (e), a step (f) of concentrating the silica sol to obtain a concentrated solution can be included. The concentration step (f) can adjust the silica concentration to 1% by mass or more and 50% by mass or less, for example, by concentration using an ultrafiltration (UF) membrane or evaporation concentration under reduced pressure or normal pressure.
[0048] [Pigment composition] The pigment composition of the present invention is not particularly limited as long as it contains at least the transition metal-doped colored silica sol of the present invention. The pigment composition may be prepared as a pigment composition in the form of a dispersion liquid by using the transition metal-doped colored colloidal silica particles in the transition metal-doped colored silica sol as a pigment as it is, or may be prepared as a powdered pigment composition by using the solid residue obtained by heat-treating (drying) the transition metal-doped colored silica sol at an appropriate treatment temperature and for an appropriate treatment time. The powder may be pulverized by a known technique and further classified before use. In addition, the pigment composition may be color-matched by mixing a plurality of transition metal-doped colored silica sols having different elements in an arbitrary mixing ratio, or may be color-matched by adding another type of pigment.
[0049] As another type of pigment, inorganic pigments and organic pigments can be used. The above pigments include inorganic white pigments such as titanium oxide, zinc oxide, and mica; inorganic black pigments such as carbon black, graphite, iron black, copper-chrome black, cobalt-chrome black, and copper-manganese-iron black; inorganic red and orange pigments such as red iron oxide; inorganic yellow pigments such as yellow iron oxide, titanium yellow, and titanium-antimony-chrome yellow; inorganic green pigments such as chrome green, dichromium trioxide, cobalt green, cobalt-titanium-nickel-zinc green, and cobalt-aluminum-chrome blue green; inorganic blue pigments such as ultramarine blue, Berlin blue, and cobalt blue; permanent red 4R, brilliant carmine FB, permanent red F5RK, pyrazolone orange, pyrazolone red, benzimidazolone orange, permanent red 2B, lake red R, Bordeaux 10B, Bonn maroon light, and thioindigo Bordeaux. , anthraquinone red, anthranthrone red, perylene red, perylene scarlet, perylene maroon, quinacridone red, dichloroquinacridone magenta, quinacridone magenta, and other organic red-orange pigments; organic yellow pigments such as fast yellow FGL, benzimidazolone yellow H3G, benzimidazolone yellow H4G, diarylide yellow HR, isoindoline yellow, anthrapyrimidine yellow, nickel azo yellow, and quinophthalone yellow; organic green pigments such as chlorinated phthalocyanine green and brominated phthalocyanine green; organic blue pigments such as phthalocyanine blue α, metal-free phthalocyanine blue, and threne blue; organic purple pigments such as dioxane violet and quinacridone violet; and extender pigments such as calcium carbonate, kaolin, diatomaceous earth, silica, talc, barium sulfate, and barium carbonate. In terms of light resistance, inorganic pigments are particularly preferred.
[0050] Furthermore, the pigment composition can be mixed with a dispersion medium such as water and / or a water-soluble organic solvent, a resin (plastic), glass raw materials, additives, etc. as necessary. The order of mixing can be any order as long as it does not affect the effects of the present invention. The pigment composition after mixing may be used while maintaining the state of a dispersion liquid (liquid state), or may be used in powder form after heat treatment (drying) at an appropriate treatment temperature and treatment time. Alternatively, the transition metal-doped colored silica sol may be first powdered, and then the resin, additives, etc. may be mixed therewith, and the powder may be used as is, or the dispersion medium, etc. may be added thereto, followed by dispersion treatment, and the powder may be used as a dispersion liquid. From the viewpoint of transparency, it is particularly preferred that the pigment composition be used while maintaining the state of a dispersion.
[0051] The water-soluble organic solvent may be an alcohol, an ether, an ester, or a ketone. Examples of the water-soluble organic solvent include monoalcohol solvents such as methanol, ethanol, 1-propanol, 2-propanol, tert-butanol, and diacetone alcohol; polyhydric alcohol solvents such as ethylene glycol and propylene glycol; aromatic alcohol solvents such as furfuryl alcohol; ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoisopropyl ether, ethylene glycol monotert-butyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, diethylene glycol dimethyl ...ethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, diethylene glycol dimethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, diethylene glycol dimethyl ether, diethylene glycol monoethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, diethylene glycol dimethyl ether, diethylene glycol monoethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, diethylene glycol dimethyl ether, diethylene glycol monoethyl ether, diethylene glycol monoethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, diethylene glycol dimethyl ether, diethylene glycol monoethyl ether, diethylene glycol monoethyl ether, diethylene glycol Examples of the solvent include ether and ester solvents such as ethylene glycol diethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol dimethyl ether, 3-methoxybutanol, 3-methyl-3-methoxybutanol, ethylene glycol monomethyl ether acetate, ethyl 2-hydroxypropionate, ethyl hydroxyacetate, γ-butyrolactone, tetrahydrofuran, and 1,4-dioxane; ketone solvents such as acetone and 4-hydroxy-4-methyl-2-pentanone; and nitrogen-containing solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone. These may be used alone or in combination of two or more.
[0052] The resin (plastic) may be a known resin. For example, it may be a thermoplastic resin, a thermosetting resin, a photocurable resin, etc. Examples of the thermoplastic resin include polyvinyl chloride (PVC) resin, polyethylene (PE) resin, polypropylene (PP) resin, polystyrene (PS) resin, acrylonitrile-butadiene-styrene (ABS) resin, acrylonitrile-styrene (AS) resin, thermoplastic acrylic (e.g., polymethyl methacrylate: PMMA) resin, polyvinyl alcohol (PVA) resin, vinyl acetate (PVAc) resin, polyvinylidene chloride (PVDC) resin, polyethylene terephthalate (PET) resin, polyamide (PA) resin, polyacetal (POM) resin, polycarbonate (PC) resin, modified polyphenylene ether (m-PPE) resin, polybutylene terephthalate (PBT) resin, ultra-high molecular weight polyethylene (U-PE) resin, polyvinylidene fluoride (PVDF) resin, polysulfone (PSU) resin, polyethersulfone (PESU) resin, polyphenylene sulfone (P ... Examples of suitable polyphenylene sulfide (PPS) resins include polyarylate (PAR) resins, polyamide-imide (PAI) resins, polyetherimide (PEI) resins, polyetheretherketone (PEEK) resins, thermoplastic polyimide (TPI) resins, liquid crystal polymer (LCP) resins, polytetrafluoroethylene (PTFE) resins, polymethylterpene (PMP) resins, polyphenylene oxide (NORYL, PPO) resins, thermoplastic polyurethane (TPU) resins, coumarone resins, ionomer (ION) resins, polyester-based thermoplastic elastomers, rosin, cellulose acetate (CA) resins, polylactic acid (PLA) resins, polybutylene succinate (PBS) resins, polycaprolactone (PCL) resins, polyglycolic acid (PGA) resins, polyhydroxyalkanoic acid (PHA) resins, polyvinyl butyral resins (PVB), and polyacrylonitrile (PAN) resins.Examples of the thermosetting resin include phenol (PF) resin, urea (UF) resin, melamine (MF) resin, unsaturated polyester (UP) resin, epoxy (EP) resin, silicone (SI) resin, polyurethane (PU) resin, diallyl phthalate (PDAP) resin, polyimide (PI) resin, thermosetting acrylic (TPA) resin, liquid polybutadiene, silicone rubber, shellac, furan resin, casein resin, etc. Examples of the photocurable resin include vinyl-based photocurable resin, acrylic-based photocurable resin, epoxy-based photocurable resin, urethane-based photocurable resin, polyester-based photocurable resin, etc. These resins may be used alone or in combination of two or more kinds, or may be used as a copolymer or modified product of two or more kinds.
[0053] The resin is preferably a soluble resin that dissolves in water and / or a water-soluble organic solvent, or a dispersed resin that is dispersed in the form of a colloid or emulsion.
[0054] The glass raw material may be any known glass raw material. For example, silica sand, feldspar, cullet, sodium silicate, calcium carbonate, lithium carbonate, sodium carbonate, sodium sulfate, sodium nitrate, potassium carbonate, potassium nitrate, barium carbonate, barium nitrate, limestone, dolomite, magnesium oxide, borax, boric acid, phosphoric acid, aluminum hydroxide, red lead, litharge, fluorite, creolite, sodium silicofluoride, zinc oxide, titanium oxide, zirconium oxide, etc. may be used alone or in combination of two or more. The glass raw material may also be used as a raw material for glazes.
[0055] The additives may be any known additive. Examples of the additives include wetting agents, dispersants, penetrants, drying agents, drying inhibitors, defoamers, viscosity adjusters, pH adjusters, chelating agents, plasticizers, crosslinking agents, curing catalysts, radical generators, acid generators, sensitizers, polymerization inhibitors, antioxidants, ultraviolet absorbers, leveling agents, lubricants, flame retardants, antistatic agents, rust inhibitors, preservatives, algae inhibitors, antibacterial agents, antifungal agents, and antiviral agents. These additives may be used alone or in combination of two or more.
[0056] These mixing and dispersion steps can be carried out in a container using a mixing and dispersing machine such as a stirring blade, a paint shaker, a bead mill, a ball mill, a dissolver, a kneader, etc. If the mixing or dispersing properties are poor at room temperature, heating may be carried out as necessary.
[0057] Furthermore, before or after mixing, the pigment composition may be subjected to classification using a sieve, centrifugation, filtration, or the like to remove unnecessary foreign matter.
[0058] When the pigment composition is used as a dispersion, the concentration of the pigment (the transition metal-doped colored colloidal silica particles in the transition metal-doped colored silica sol, and other pigments as desired) in the pigment composition can be 1% by mass or more and 50% by mass or less in 100% by mass of the pigment composition. It is preferably 2% by mass or more and 40% by mass or less. If the pigment concentration in the pigment composition (dispersion) is less than 1% by mass, the coloring property is low due to the small amount of coloring components, and if it is more than 50% by mass, the dispersibility is likely to deteriorate due to the increase in the number of particles, which is not preferable. On the other hand, when the pigment composition is used as a powder, the pigment concentration can be 1% by mass or more and 100% by mass or less in 100% by mass of the pigment composition. It is preferably 5% by mass or more and 90% by mass or less. If the pigment concentration in the pigment composition (powder) is less than 1% by mass, the coloring component is small, and the coloring property is low, which is not preferable.
[0059] The proportion of the dispersion medium, such as water and a water-soluble organic solvent, in the pigment composition may be 50% by mass or more and 99% by mass or less in 100% by mass of the pigment composition when the pigment composition is used as a dispersion liquid. On the other hand, when the pigment composition is used as a powder, it is preferable that the pigment composition contains as few of these dispersion media as possible.
[0060] The proportion of the resin in the pigment composition is not particularly limited, but is 0% by mass or more and 50% by mass or less in 100% by mass of the pigment composition. Preferably, it is 1% by mass or more and 50% by mass or less. When a resin is blended in the pigment composition, it is preferably 1% by mass or more.
[0061] When the pigment composition contains a resin, the mass ratio of the pigment to the resin (pigment / resin) is 1 / 99 or more and 99 / 1 or less, and preferably 5 / 95 or more and 95 / 5 or less.
[0062] The proportion of the additive in the pigment composition is the remainder in 100% by mass of the pigment composition, specifically, from 0% by mass to 10% by mass of 100% by mass of the pigment composition.
[0063] [Paints, inks, glazes] The pigment composition of the present invention can be used as a paint, ink, or glaze. That is, the present invention is also directed to the paint, ink, or glaze that contains at least the pigment composition.
[0064] [Printed matter, film, molded object] The present invention also relates to a printed matter, a film, or a molded article that contains at least the pigment composition.
[0065] The printed matter or film of the present invention is not particularly limited as long as it contains at least the pigment composition of the present invention. Here, the printed matter refers to an item on which images such as letters, pictures, photographs, etc. are printed with ink on a substrate. The film may be a coating film applied to a substrate or a free-standing film. Here, the coating film means a film formed by applying a coating material or the like onto a substrate, and the free-standing film means a film that does not require the support of a substrate.
[0066] The thickness of the film is not particularly limited, but can be selected from the range of about 0.01 μm to 10 mm. For example, the thickness of the coating film is 0.05 μm or more and 20 μm or less, and preferably 0.1 μm or more and 10 μm or less. The thickness of the free-standing film is 5 μm or more and 10 mm or less, and preferably 50 μm or more and 1 mm or less.
[0067] Examples of the method for applying the pigment composition of the present invention to a substrate include brush coating, roller coating, spatula coating, aerosol, air spray coating, airless spray coating, dip coating, electrodeposition coating, electrostatic coating, powder coating, flow coating, curtain coating, shower coating, spray coating, roll coating, bar coating, gravure coating, slit coater method, dipping, spin coating, casting, screen printing, and inkjet methods. The pigment composition may be applied once or twice or more. When applying, the pigment composition and / or the substrate may be applied while being heated, or may be heated after application. After drying, the substrate to which the pigment composition is applied may be subjected to a heat treatment (post-baking). When a photocurable resin is used, a light source of an appropriate wavelength may be irradiated at a predetermined intensity for a predetermined time.
[0068] The substrate may be a known substrate. Examples of the substrate include metal, ceramics, glass, pottery, porcelain, refractory material, concrete, mortar, slate, wood, paper, cotton, hemp, silk, wool, and plastic. Preferred substrates are transparent in the visible range, such as glass, polyethylene terephthalate resin, acrylic resin, polycarbonate resin, cellulose acetate resin, vinyl chloride resin, polyethylene resin, polyolefin resin, fluororesin, and polyimide resin.
[0069] The shape of the substrate is not particularly limited and includes any shape, such as fibers, mesh fabrics, knitted fabrics, woven fabrics, nonwoven fabrics, films, sheets, plates, rods, pipes, plates, bowls, cups, boxes, and the like.
[0070] The molded article of the present invention is not particularly limited as long as it contains at least the pigment composition of the present invention. Here, the term "molded body" refers to a material obtained by processing a raw material into a desired shape, surface, or design, and may be various shaped bodies including, but not limited to, resin, metal, glass, etc.
[0071] Examples of methods for molding the pigment composition of the present invention include injection molding, blow molding, extrusion molding, cast molding, hand lay-up molding, press molding, compression molding, vacuum molding, compressed air molding, T-die method, inflation method, calendar molding, droplet molding method, direct dissolution method, marble melt method, overflow method, float method, and the like.
[0072] The shape of the molded product is not particularly limited and includes any shape, such as fibers, mesh fabrics, knitted fabrics, woven fabrics, nonwoven fabrics, films, sheets, plates, rods, pipes, plates, bowls, cups, boxes, and the like. EXAMPLES
[0073] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples in any way. In addition, when explaining the procedures of the following examples, the silica particles may be referred to simply as "silica particles" or "silica sol" regardless of whether or not they have a shell layer or are doped with a transition metal.
[0074] The measurement procedures and devices for physical properties in the examples and comparative examples are as follows.
[0075] <ph> The pH of the sample was measured at room temperature (20±5° C.) using a pH meter (manufactured by DKK Toa Corporation).
[0076] <Silica concentration> The silica concentration of the sample was measured by a mass method. Specifically, the silica sol of a given mass to be measured was calcined in an electric furnace at 1000°C, and the mass of the calcination residue was subtracted from the mass of the metal elements of 0.0001 mass% or more (1 mass ppm or more) converted into oxides, excluding silica (measured as silicon in the analysis and converted into oxides), among the inorganic elements measured by the metal element analysis described below, to obtain the silica mass, and the silica concentration (%) was calculated by [(silica mass / silica sol mass) x 100].
[0077] <Metal elemental analysis (inorganic elemental analysis)> Metal element analysis (including silica) was performed using an inductively coupled plasma optical emission spectrometer (ICP-OES, Agilent Technologies, product name Agilent 5110). Specifically, the sample was treated with a microwave decomposition device, then appropriately diluted and measured with ICP-OES. A calibration curve was created using a calibration solution prepared in the range of 0-1 ppm by mass. The mass ratio of transition metal T to silica (T / silica) was calculated from the measured metal element amount and the above silica mass.
[0078] <Number average particle size (D1) calculated by image analysis from electron microscope images> An electron microscope image of the particles was obtained using a multi-function electron microscope (manufactured by JEOL Ltd., product name JEM-F200). The observation conditions were TEM mode and an accelerating voltage of 200 kV. Next, a small general-purpose image processing and analysis system (manufactured by Nireco Corporation, product name Luzex AP) was used to determine the particle area from the obtained electron microscope image by image analysis, and the circle equivalent diameter, which is the diameter of a perfect circle equal to the area, was calculated. The number-average particle diameter (D1) was taken as the number-average value of the circle equivalent diameters of at least 500 or more arbitrary particles. The standard deviation was 1σ, and the number-average particle diameter (D1) was calculated as the average value ± standard deviation.
[0079] <BET particle size (D2) calculated by nitrogen adsorption method> The specific surface area (SSA) measured by the nitrogen adsorption method (BET method) was measured using a nitrogen adsorption specific surface area measuring device (Monosorb MS-22, manufactured by Yuasa Ionics Co., Ltd.). 2 The sample was prepared by contacting the silica sol to be measured with a hydrogen-type strong acid cation exchange resin, drying it at 300°C in air for 1 hour, and then grinding it in a mortar to prepare a powder. Next, the BET particle diameter D2 (nm) was calculated by multiplying the specific surface area SSA (m 2 / g) and the particle density PD (g / cm 3 ) was calculated using equation (1). BET particle diameter D2 (nm) = 6000 / [particle density PD (g / cm 3 )×specific surface area SSA(m 2 / g)] (1)
[0080] <Number average particle size / BET particle size (D1 / D2) ratio> The number average particle size / BET particle size (D1 / D2) ratio was calculated by taking the ratio of the above-mentioned number average particle size (D1) to the BET particle size (D2).
[0081] <Average particle size by dynamic light scattering method (D3)> The average particle size (D3) measured by dynamic light scattering was measured using a dynamic light scattering particle size measuring device (manufactured by Spectris Corporation, trade name: Zetasizer Nano S).
[0082] <Shell thickness> In the embodiment in which a shell layer is formed on the particle surface, the shell thickness was calculated from the number average particle diameter (D1) of the transition metal-doped colored silica sol before the formation of the shell layer and the number average particle diameter (D1) of the transition metal-doped colored silica sol after the formation of the shell layer according to the following formula (2). Shell thickness = (number average particle size of particles after shell layer formation (D1) - number average particle size of particles before shell layer formation (D1)) ÷ 2 (2) The shell thickness may be calculated using the BET particle diameter (D2) instead of the number average particle diameter (D1).
[0083] <Dispersibility> The silica sol to be evaluated was irradiated with a green laser pointer with a wavelength of 532 nm, and the occurrence of the Tyndall phenomenon was visually confirmed to evaluate the dispersibility of the silica particles. If the Tyndall phenomenon was observed and no sedimentation occurred, the dispersibility was evaluated as ○, and if the Tyndall phenomenon was not observed or sedimentation occurred, the dispersibility was evaluated as ×.
[0084] <Particle density PD> Particle density (g / cm 3 ) was measured using a dry automatic density meter (Micromeritics, product name AccuPyc 1340 TEC). The measurement conditions were He gas, introduction pressure of 134 kPaG, and the average value of 10 measurements. The sample was dried at 100°C in air and then ground in a mortar to prepare a powder.
[0085] <Identification of crystalline phase> The crystal phase was identified using a desktop X-ray diffractometer (XRD, Rigaku Corporation, product name MiniFlex600). The measurement conditions were CuKα radiation (=0.15418 nm), θ-2θ method, and a measurement range of 3°-80°. The sample was dried at 100°C in air and then ground in a mortar to obtain a powder.
[0086] <Visible UV Spectral Analysis> The UV-visible near-infrared spectrophotometer (Shimadzu Corporation, product name UV-3600) was used to measure the UV-visible spectrum of the silica sol to be measured. Specifically, a quartz cell with a lid and an optical path length of 10 mm was used, and water or propylene glycol monomethyl ether (PGME) was used as a control. The UV-visible transmission spectrum and the UV-visible absorption spectrum were measured in the measurement wavelength range of 250-800 nm.
[0087] <Light resistance evaluation> The light resistance of the transition metal-doped colored silica sol was evaluated using a QUV accelerated weathering tester (manufactured by Q-Lab Co., Ltd., product name QUV / se). Specifically, the target silica sol sample was placed in a quartz cell with a lid and an optical path length of 10 mm, and placed in the QUV accelerated weathering tester. The measurement conditions were a UVA-340 lamp, UV irradiation intensity of 0.89 W / m 2 The irradiation was performed at 50°C for 500 hours (equivalent to 3.6 months of sunlight). The mass loss of the sample after 500 hours of UV irradiation was less than 1%, and there was no problem with the airtightness of the quartz cell with lid. In addition, UV irradiation was performed on the target silica sol in the same manner under conditions of 100 or 250 hours of UV irradiation only. After UV irradiation for a predetermined period of time (100 hours, 250 hours, 500 hours), the absorption spectrum of the silica sol was measured by visible-ultraviolet spectrum analysis, and the rate of absorbance change before and after UV irradiation at any absorption wavelength was calculated using the following formula (3). Absorbance change rate (%) = [absorbance after UV irradiation / absorbance before UV irradiation] x 100 (3) The closer the absorbance change rate (%) is to 100%, the less the absorbance changes upon UV irradiation, and the higher the light resistance is determined to be.
[0088] <Preparation of active silicic acid aqueous solution> 304 g of commercially available JIS No. 3 sodium silicate aqueous solution (silica concentration 28.8 mass%, Na2O concentration 9.5 mass%, silica / Na2O molar ratio 3.1) was added to 2196 g of pure water and mixed uniformly to prepare 2500 g of sodium silicate aqueous solution diluted to a silica concentration of 3.5 mass%. This diluted sodium silicate aqueous solution was passed through a column packed with 1 L of hydrogen-type strong acid cation exchange resin (manufactured by Organo Corporation, product name Amberlite IR-120B) at a rate of 250 mL / min to contact with the cation exchange resin, thereby preparing 1684 g of active silicic acid aqueous solution with a silica concentration of 3.5 mass% and pH of 2.9. The concentrations of V, Cr, Mn, Fe, Co, Ni, and Cu in this active silicic acid aqueous solution were all below the lower detection limit (less than 0.0001 mass%). The obtained aqueous solution of activated silicic acid was appropriately used in the preparation of the feed liquid and the heel liquid, and also in the coating (shell layer) of silica particles in the production process of each silica sol shown below.
[0089] [Example 1] <Production of Co-doped Colored Silica Sol> To 780 g of pure water, 28 g of a commercially available aqueous sodium silicate solution of JIS No. 3 (silica concentration 28.8% by mass, Na2O concentration 9.5% by mass, silica / Na2O molar ratio 3.1) was added and uniformly mixed to prepare 808 g of a heel liquid having a silica concentration of 1.0% by mass, a Na2O concentration of 0.33% by mass, a silica / Na2O molar ratio of 3.1, and a pH of 11.0. Next, 7.9 g of a 10% by mass CoSO4 aqueous solution prepared by previously mixing and dissolving CoSO4·7H2O powder in pure water was added to 1684 g of the above-mentioned aqueous solution of activated silicic acid and uniformly mixed to prepare 1692 g of a feed liquid. 808 g of the prepared heel liquid was charged into a 3 L glass reaction vessel equipped with a stirrer and a condenser, and the liquid temperature in the vessel was maintained at 80 °C with an oil bath. Next, 1692 g of the feed liquid was continuously supplied into this vessel under stirring at a constant rate over 100 minutes to perform particle synthesis. After the supply of this feed liquid was completed, the liquid temperature in the vessel was maintained at 80 °C for 6 hours under stirring to obtain 2500 g of a sizing liquid of Co-doped colored silica sol.
[0090] The obtained sizing liquid of Co-doped colored silica sol was highly transparent and blue-violet, and no sediment was generated. Further, when irradiated with a green laser pointer having a wavelength of 532 nm, the Tyndall phenomenon was observed and the dispersibility was good. This obtained sizing liquid of Co-doped colored silica sol had a pH of 10.4, a silica concentration of 2.7% by mass, an average particle diameter (D3) of 13 nm by the dynamic light scattering method, a Co concentration of 0.012% by mass (120 ppm by mass), and a mass ratio of Co to silica (Co / silica) of 0.0044. When the particles were observed with an electron microscope in the TEM mode, they were solid spherical particles. The electron micrograph of this particle is shown in Fig. 1. The number average particle diameter (D1) calculated by the image analysis method from this electron micrograph of the particle was 9.3 ± 2.8 nm.
[0091] Next, 2300 g of the resulting sized liquid of Co-doped colored silica sol was concentrated by pressure filtration with compressed air at room temperature under stirring using an ultrafiltration (UF) membrane with a molecular weight cutoff of 200,000, and 238 g of a highly transparent, blue-purple UF concentrate of Co-doped colored silica sol and 2062 g of a colorless, transparent UF filtrate were recovered. The appearance of this UF concentrate of Co-doped colored silica sol is shown in Figure 2. The UF concentrated solution of the obtained Co-doped colored silica sol had a pH of 9.9, a silica concentration of 26.1 mass%, a Co concentration of 0.12 mass% (1200 mass ppm), and a mass ratio of Co to silica (Co / silica) of 0.0046. The UF filtrate obtained during UF concentration had a pH of 10.4 and a Co concentration of 0.0004 mass% (4 mass ppm). Since almost no Co was present in the UF filtrate side, but was present in the UF concentrated solution side, it was confirmed that the colloidal silica particles were doped with Co and colored. The obtained UF concentrated solution of the Co-doped colored silica sol was dried at 100°C in air to obtain a transparent blue-purple powder of the Co-doped colored silica sol. The appearance of the powder of the Co-doped colored silica sol is shown in Figure 3. The powder was then crushed in a mortar and the particle density PD was measured using a dry density meter, which was 2.17 g / cm 3 Similarly, when the crushed powder was measured by X-ray diffraction, the XRD pattern was broad, indicating that the powder was amorphous. The XRD pattern is shown in Figure 4.
[0092] The UF concentrate of the obtained Co-doped colored silica sol was then contacted with a hydrogen-type strong acid cation exchange resin to obtain an acidic Co-doped colored silica sol with a pH of 2.6 and a silica concentration of 22.1% by mass. This acidic Co-doped colored silica sol was dried in air at 300°C for 1 hour to obtain a transparent blue-purple acidic Co-doped colored silica sol powder. Furthermore, the powder was crushed in a mortar and measured by nitrogen adsorption, and the specific surface area (SSA) was 377 m 2 The BET particle diameter (D2) calculated by the nitrogen adsorption method using formula (1) was 7.3 nm, and the number-average particle diameter / BET particle diameter (D1 / D2) ratio was 1.27.
[0093] After filtering the UF concentrate of the obtained Co-doped colored silica sol through a nylon membrane filter with a pore size of 0.45 μm, the visible-ultraviolet spectrum of the UF concentrate of the Co-doped colored silica sol was measured using pure water as a control. As a result, Co-derived absorption was confirmed at wavelengths of 540 nm, 590 nm, and 640 nm. This visible-ultraviolet transmission spectrum and visible-ultraviolet absorption spectrum are shown in Fig. 5.
[0094] <Lightfastness evaluation> The Co-doped colored silica sol obtained in Example 1 was placed in a quartz cell with a lid and an optical path length of 10 mm, and installed in a QUV accelerated weathering tester to evaluate its lightfastness. When the situation before UV irradiation was set as 100%, the absorbance change rate after 500 h of UV irradiation at an absorption wavelength of 640 nm was 78%. The results are shown in Table 2 and Fig. 6.
[0095] [Example 2] <Production of Co-doped colored silica sol> After the completion of the feed liquid supply, except that the step of maintaining the liquid temperature in the container at 80 °C for 6 hours under stirring was changed to 1 hour, the same operation as in Example 1 was performed to obtain 2500 g of the sizing liquid of the Co-doped colored silica sol.
[0096] The obtained sizing liquid of the Co-doped colored silica sol was highly transparent and bluish-purple, and no sediment was generated. Furthermore, when irradiated with a green laser pointer with a wavelength of 532 nm, the Tyndall phenomenon was observed, and the dispersibility was good. The obtained sizing liquid of the Co-doped colored silica sol had a pH of 10.5, a silica concentration of 2.7% by mass, an average particle diameter (D3) of 13 nm by the dynamic light scattering method, a Co concentration of 0.012% by mass (120 ppm by mass), and a mass ratio of Co to silica (Co / silica) of 0.0045. When the particles were observed with an electron microscope in TEM mode, they were solid spherical particles. The number average particle diameter (D1) calculated by the image analysis method from the electron microscope image of these particles was 9.5 ± 2.6 nm.
[0097] Next, 2,300 g of the resulting sized liquid of Co-doped colored silica sol was concentrated by pressure filtration with compressed air at room temperature under stirring using an ultrafiltration (UF) membrane with a molecular weight cutoff of 200,000, and 220 g of a highly transparent, blue-purple Co-doped colored silica sol UF concentrate and 2,080 g of a colorless, transparent UF filtrate were recovered. The UF concentrated solution of the obtained Co-doped colored silica sol had a pH of 9.9, a silica concentration of 28.2 mass%, a Co concentration of 0.13 mass% (1300 mass ppm), and a mass ratio of Co to silica (Co / silica) of 0.0046. The UF filtrate obtained during UF concentration had a pH of 10.4 and a Co concentration of 0.0003 mass% (3 mass ppm). Since almost no Co was present in the UF filtrate side, but was present in the UF concentrated solution side, it was confirmed that the colloidal silica particles were doped with Co and colored. The obtained UF concentrated solution of Co-doped colored silica sol was dried at 100°C under air to obtain a transparent blue-purple powder of Co-doped colored silica sol. The powder was then crushed in a mortar and the particle density PD was measured with a dry densitometer, which was 2.13 g / cm. 3 Similarly, when the crushed powder was measured by X-ray diffraction, the XRD pattern was broad, indicating that the powder was amorphous.
[0098] The UF concentrate of the obtained Co-doped colored silica sol was then contacted with a hydrogen-type strong acid cation exchange resin to obtain an acidic Co-doped colored silica sol with a pH of 2.4 and a silica concentration of 22.1% by mass. This acidic Co-doped colored silica sol was dried in air at 300°C for 1 hour to obtain a transparent blue-purple acidic Co-doped colored silica sol powder. Furthermore, the powder was crushed in a mortar and measured by nitrogen adsorption, and the specific surface area (SSA) was 372 m 2 The BET particle size (D2) calculated by the nitrogen adsorption method using formula (1) was 7.6 nm, and the number-average particle size / BET particle size (D1 / D2) ratio was 1.26.
[0099] The UF concentrate of the obtained Co-doped colored silica sol was filtered through a nylon membrane filter with a pore size of 0.45 μm, and then the visible ultraviolet spectrum of the UF concentrate of the Co-doped colored silica sol was measured using pure water as a control. As a result, Co-derived absorption was confirmed at wavelengths of 540 nm, 590 nm, and 640 nm.
[0100] <Lightfastness evaluation> The obtained Co-doped colored silica sol was placed in a quartz cell with a lid and an optical path length of 10 mm, and installed in a QUV accelerated weathering tester to evaluate the lightfastness. When the state before UV irradiation was set as 100%, the absorbance change rates after 100 h, 250 h, and 500 h of UV irradiation at an absorption wavelength of 640 nm were 96%, 88%, and 83%, respectively. The results are shown in Table 2 and Figure 6.
[0101] [Example 3] <Production of Co-doped colored silica sol> The heel liquid was changed to 808 g of a heel liquid (silica concentration 1.0 mass%, NH3 concentration 1.1 mass%, silica / NH3 molar ratio 0.28, pH 10.9) obtained by adding 544 g of pure water, 231 g of the above-mentioned active silica aqueous solution (silica concentration 3.5 mass%, pH 2.9), and 33 g of aqueous ammonia (ammonia concentration 27 mass%) and mixing them uniformly. Except for this change, the same operation as in Example 1 was performed to obtain 2500 g of a sizing liquid for Co-doped colored silica sol.
[0102] The obtained sizing liquid of Co-doped colored silica sol was highly transparent and blue-violet, and no sediment was generated. Furthermore, when irradiated with a green laser pointer with a wavelength of 532 nm, the Tyndall phenomenon was observed, indicating good dispersibility. The obtained sizing liquid of Co-doped colored silica sol had a pH of 10.4, a silica concentration of 2.7 mass%, an average particle diameter (D3) of 17 nm by the dynamic light scattering method, a Co concentration of 0.013 mass% (130 mass ppm), and a mass ratio of Co to silica (Co / silica) of 0.0049. When the particles were observed with an electron microscope in TEM mode, they were solid spherical particles. The number average particle diameter (D1) calculated by the image analysis method from the electron microscope image of these particles was 11.6 ± 4.3 nm.
[0103] Next, 2,300 g of the resulting sized liquid of Co-doped colored silica sol was concentrated by pressure filtration with compressed air at room temperature under stirring using an ultrafiltration (UF) membrane with a molecular weight cutoff of 200,000, and 201 g of a highly transparent, blue-purple Co-doped colored silica sol UF concentrate and 2,099 g of a colorless, transparent UF filtrate were recovered. The UF concentrate of the obtained Co-doped colored silica sol had a pH of 9.8, a silica concentration of 30.9 mass%, a Co concentration of 0.14 mass% (1400 mass ppm), and a mass ratio of Co to silica (Co / silica) of 0.0045. The UF filtrate obtained during UF concentration had a pH of 10.5 and a Co concentration below the lower detection limit (less than 0.0001 mass%). Since almost no Co was present in the UF filtrate side but was present in the UF concentrate side, it was confirmed that the colloidal silica particles were doped with Co and colored. The obtained UF concentrated solution of Co-doped colored silica sol was dried at 100°C under air to obtain a transparent blue-purple powder of Co-doped colored silica sol. The powder was then crushed in a mortar and the particle density PD was measured with a dry densitometer, which was 2.18 g / cm. 3 Similarly, when the crushed powder was measured by X-ray diffraction, the XRD pattern was broad, indicating that the powder was amorphous.
[0104] The UF concentrate of the obtained Co-doped colored silica sol was then contacted with a hydrogen-type strong acid cation exchange resin to obtain an acidic Co-doped colored silica sol with a pH of 2.4 and a silica concentration of 25.2% by mass. This acidic Co-doped colored silica sol was dried in air at 300°C for 1 hour to obtain a transparent blue-purple acidic Co-doped colored silica sol powder. Furthermore, the powder was crushed in a mortar and measured by nitrogen adsorption, and the specific surface area (SSA) was found to be 271 m 2 The BET particle diameter (D2) calculated by the nitrogen adsorption method using formula (1) was 10.1 nm, and the number-average particle diameter / BET particle diameter (D1 / D2) ratio was 1.14.
[0105] After filtering the sizing solution of the obtained Co-doped colored silica sol through a nylon membrane filter with a pore size of 0.45 μm, the visible-ultraviolet spectrum of the sizing solution of the Co-doped colored silica sol was measured using pure water as a control. As a result, Co-derived absorption was confirmed at wavelengths of 525 nm, 580 nm, and 640 nm.
[0106] <Lightfastness evaluation> The obtained Co-doped colored silica sol was placed in a quartz cell with a lid and an optical path length of 10 mm, and installed in a QUV accelerated weathering tester to evaluate its lightfastness. When the absorbance before UV irradiation was set to 100%, the change rates of absorbance after 100 h, 250 h, and 500 h of UV irradiation at an absorption wavelength of 640 nm were 84%, 81%, and 76%, respectively. The results are shown in Table 2 and Figure 6.
[0107] [Example 4] <Production of Co-doped colored silica sol> A sizing solution of Co-doped colored silica sol (2527 g) was obtained in the same manner as in Example 3, except that 7.9 g of a 10% by mass aqueous CoSO4 solution used for preparing the feed solution was changed to 35.3 g, and 1719 g of the prepared feed solution was used.
[0108] The obtained sizing solution of Co-doped colored silica sol was highly transparent and blue-violet, and no sediment was generated. Furthermore, when irradiated with a green laser pointer with a wavelength of 532 nm, the Tyndall phenomenon was observed, indicating good dispersibility. The obtained sizing solution of Co-doped colored silica sol had a pH of 10.3, a silica concentration of 2.7% by mass, an average particle diameter (D3) of 27 nm by the dynamic light scattering method, a Co concentration of 0.054% by mass (540 ppm by mass), and a mass ratio of Co to silica (Co / silica) of 0.020. When the particles were observed with an electron microscope in TEM mode, they were solid spherical particles. The number average particle diameter (D1) calculated by the image analysis method from the electron microscope image of these particles was 9.6 ± 3.0 nm.
[0109] Next, 2,300 g of the resulting sized liquid of Co-doped colored silica sol was concentrated by pressure filtration with compressed air at room temperature under stirring using an ultrafiltration (UF) membrane with a molecular weight cutoff of 200,000, and 190 g of a highly transparent, blue-purple Co-doped colored silica sol UF concentrate and 2,110 g of a colorless, transparent UF filtrate were recovered. The UF concentrate of the obtained Co-doped colored silica sol had a pH of 9.6, a silica concentration of 27.5 mass%, a Co concentration of 0.56 mass% (5600 mass ppm), and a mass ratio of Co to silica (Co / silica) of 0.020. The UF filtrate obtained during UF concentration had a pH of 10.2 and a Co concentration below the lower detection limit (less than 0.0001 mass%). Since almost no Co was present in the UF filtrate side but was present in the UF concentrate side, it was confirmed that the colloidal silica particles were doped with Co and colored. The obtained UF concentrated solution of Co-doped colored silica sol was dried at 100°C under air to obtain a transparent blue-purple powder of Co-doped colored silica sol. The powder was then crushed in a mortar and the particle density PD was measured with a dry densitometer, which was 2.21 g / cm. 3 Similarly, when the crushed powder was measured by X-ray diffraction, the XRD pattern was broad, indicating that the powder was amorphous.
[0110] The UF concentrate of the obtained Co-doped colored silica sol was then contacted with a hydrogen-type strong acid cation exchange resin to obtain an acidic Co-doped colored silica sol with a pH of 2.8 and a silica concentration of 20.0 mass%. This acidic Co-doped colored silica sol was dried in air at 300°C for 1 hour to obtain a transparent blue-purple acidic Co-doped colored silica sol powder. Furthermore, the powder was crushed in a mortar and measured by nitrogen adsorption, and the specific surface area (SSA) was found to be 282 m 2 The BET particle size (D2) calculated by the nitrogen adsorption method using formula (1) was 9.6 nm, and the number-average particle size / BET particle size (D1 / D2) ratio was 1.00.
[0111] The sizing solution of the obtained Co-doped colored silica sol was filtered through a nylon membrane filter with a pore size of 0.45 μm, and then the visible-ultraviolet spectrum of the sizing solution of the Co-doped colored silica sol was measured using pure water as a control. As a result, Co-derived absorption was confirmed at wavelengths of 525 nm, 580 nm, and 640 nm.
[0112] <Lightfastness evaluation> The obtained Co-doped colored silica sol was placed in a quartz cell with a lid and an optical path length of 10 mm, and installed in a QUV accelerated weathering tester to evaluate its lightfastness. When the situation before UV irradiation was set as 100%, the absorbance change rates after 100 h, 250 h, and 500 h of UV irradiation at an absorption wavelength of 640 nm were 94%, 90%, and 87% respectively. The results are shown in Table 2 and Figure 6.
[0113] [Example 5] <Production of Co-doped colored silica sol> Except that the heel solution was changed to 808 g of a heel solution (silica concentration 1.0 mass%, Na2O concentration 0.32 mass%, NH3 concentration 0.50 mass%, silica / alkali molar ratio 0.48, pH 11.2) obtained by adding 765 g of pure water, 28 g of a commercially available aqueous sodium silicate solution of JIS No. 3, and 15 g of aqueous ammonia and mixing them uniformly, the same operations as in Example 1 were carried out to obtain 2500 g of a sizing solution of Co-doped colored silica sol.
[0114] The obtained sizing solution of Co-doped colored silica sol was highly transparent and bluish-purple, and no sediment was generated. Furthermore, when irradiated with a green laser pointer with a wavelength of 532 nm, the Tyndall phenomenon was observed and the dispersibility was good. The obtained sizing solution of Co-doped colored silica sol had a pH of 10.7, a silica concentration of 2.7 mass%, an average particle diameter (D3) of 20 nm by the dynamic light scattering method, a Co concentration of 0.012 mass% (120 mass ppm), and a mass ratio of Co to silica (Co / silica) of 0.0045. When the particles were observed with an electron microscope in TEM mode, they were solid spherical particles. The number average particle diameter (D1) calculated by the image analysis method from the electron microscope image of these particles was 9.2 ± 3.0 nm.
[0115] Next, 2,300 g of the resulting sized liquid of Co-doped colored silica sol was concentrated by pressure filtration with compressed air at room temperature under stirring using an ultrafiltration (UF) membrane with a molecular weight cutoff of 200,000, and 216 g of a highly transparent, blue-purple Co-doped colored silica sol UF concentrate and 2,084 g of a colorless, transparent UF filtrate were recovered. The UF concentrate of the obtained Co-doped colored silica sol had a pH of 10.3, a silica concentration of 28.8 mass%, a Co concentration of 0.13 mass% (1300 mass ppm), and a mass ratio of Co to silica (Co / silica) of 0.0045. The UF filtrate obtained during UF concentration had a pH of 10.8 and a Co concentration below the lower detection limit (less than 0.0001 mass%). Since almost no Co was present in the UF filtrate side, but was present in the UF concentrate side, it was confirmed that the colloidal silica particles were doped with Co and colored. The obtained UF concentrated solution of Co-doped colored silica sol was dried at 100°C under air to obtain a transparent blue-purple powder of Co-doped colored silica sol. The powder was then crushed in a mortar and the particle density PD was measured with a dry densitometer, which was 2.18 g / cm. 3 Similarly, when the crushed powder was measured by X-ray diffraction, the XRD pattern was broad, indicating that the powder was amorphous.
[0116] The UF concentrate of the obtained Co-doped colored silica sol was then contacted with a hydrogen-type strong acid cation exchange resin to obtain an acidic Co-doped colored silica sol with a pH of 2.5 and a silica concentration of 19.4% by mass. This acidic Co-doped colored silica sol was dried in air at 300°C for 1 hour to obtain a transparent blue-purple acidic Co-doped colored silica sol powder. Furthermore, the powder was crushed in a mortar and measured by nitrogen adsorption, and the specific surface area (SSA) was 332 m 2 The BET particle size (D2) calculated by the nitrogen adsorption method using formula (1) was 8.3 nm, and the number-average particle size / BET particle size (D1 / D2) ratio was 1.11.
[0117] The sizing solution of the obtained Co-doped colored silica sol was filtered through a nylon membrane filter with a pore size of 0.45 μm, and then the visible ultraviolet spectrum of the sizing solution of the Co-doped colored silica sol was measured using pure water as a control. As a result, Co-derived absorption was confirmed at wavelengths of 525 nm, 580 nm, and 640 nm.
[0118] <Lightfastness evaluation> The obtained Co-doped colored silica sol was placed in a quartz cell with a lid and an optical path length of 10 mm, and installed in a QUV accelerated weathering tester to evaluate its lightfastness. When the absorbance before UV irradiation was set to 100%, the change rates of absorbance after 100 h, 250 h, and 500 h of UV irradiation at an absorption wavelength of 640 nm were 77%, 69%, and 64%, respectively. The results are shown in Table 2.
[0119] [Example 6] <Production of Co-doped colored silica sol> To 284 g of pure water, 10 g of a commercially available aqueous sodium silicate solution of JIS No. 3 was added and mixed uniformly to prepare 294 g of a heel solution with a silica concentration of 1.0% by mass, a Na2O concentration of 0.33% by mass, a silica / Na2O molar ratio of 3.1, and a pH of 11.0. Next, 10.3 g of a 10% by mass CoSO4 aqueous solution was added to 2205 g of the active silicic acid aqueous solution and mixed uniformly to prepare 2215 g of a feed solution. 294 g of the prepared heel solution was charged into a 3 L glass reaction vessel equipped with a stirrer and a condenser, and the liquid temperature in the vessel was maintained at 80 °C with an oil bath. Then, 2215 g of the feed solution was continuously supplied into this vessel at a constant rate over 360 minutes under stirring to perform particle synthesis. After the supply of this feed solution was completed, the liquid temperature in the vessel was maintained at 80 °C for 6 hours under stirring to obtain 2509 g of a sizing solution of Co-doped colored silica sol.
[0120] The resulting Co-doped colored silica sol was highly transparent and blue-purple in color, and no sediment was observed. Furthermore, when a green laser pointer with a wavelength of 532 nm was irradiated, the Tyndall phenomenon was observed, and the dispersibility was good. The resulting Co-doped colored silica sol had a pH of 9.4, a silica concentration of 3.2 mass%, an average particle size (D3) of 16 nm measured by dynamic light scattering, a Co concentration of 0.0066 mass% (66 mass ppm), and a mass ratio of Co to silica (Co / silica) of 0.0020. When the particles were observed with a TEM mode electron microscope, they were solid spherical particles. The number-average particle size (D1) calculated from the electron microscope image of the particles by image analysis was 9.7 ± 3.2 nm.
[0121] Next, 2,233 g of the resulting sized liquid of Co-doped colored silica sol was concentrated by pressure filtration with compressed air at room temperature under stirring using an ultrafiltration (UF) membrane with a molecular weight cutoff of 200,000, and 216 g of a highly transparent, blue-purple Co-doped colored silica sol UF concentrate and 2,017 g of a colorless, transparent UF filtrate were recovered. The UF concentrate of the obtained Co-doped colored silica sol had a pH of 8.6, a silica concentration of 32.6 mass%, a Co concentration of 0.066 mass% (660 mass ppm), and a mass ratio of Co to silica (Co / silica) of 0.0020. The UF filtrate obtained during UF concentration had a pH of 9.2 and a Co concentration below the lower detection limit (less than 0.0001 mass%). Since almost no Co was present in the UF filtrate side, but was present in the UF concentrate side, it was confirmed that the colloidal silica particles were doped with Co and colored. The obtained UF concentrated solution of Co-doped colored silica sol was dried at 100° C. in air to obtain a transparent blue-purple powder of Co-doped colored silica sol. The powder was then crushed in a mortar and the particle density PD was measured using a dry density meter, which was 2.17 g / cm 3 Similarly, when the crushed powder was measured by X-ray diffraction, the XRD pattern was broad, indicating that the powder was amorphous.
[0122] Next, the UF concentrate of the Co-doped colored silica sol obtained was contacted with a hydrogen-type strongly acidic cation exchange resin to obtain an acidic Co-doped colored silica sol having a pH of 2.1 and a silica concentration of 23.2% by mass. This acidic Co-doped colored silica sol was dried at 300 °C for 1 hour in air to obtain a transparent blue-violet powder of the acidic Co-doped colored silica sol. Furthermore, the powder further pulverized in a mortar was measured by the nitrogen adsorption method. As a result, the specific surface area SSA was 313 m 2 / g. The BET particle size (D2) calculated from the nitrogen adsorption method using Equation (1) was 8.8 nm, and the ratio of the number average particle size to the BET particle size (D1 / D2) was 1.10.
[0123] The UF concentrate of the obtained Co-doped colored silica sol was filtered through a nylon membrane filter with a pore size of 0.45 μm, and then the visible ultraviolet spectrum of the UF concentrate of the Co-doped colored silica sol was measured using pure water as a control. As a result, Co-derived absorption was confirmed at wavelengths of 540 nm, 590 nm, and 640 nm.
[0124] <Light resistance evaluation> The obtained Co-doped colored silica sol was placed in a quartz cell with a lid having an optical path length of 10 mm and installed in a QUV accelerated weathering tester to evaluate the light resistance. When the state before UV irradiation was taken as 100%, the absorbance change rates after 100 h, 250 h, and 500 h of UV irradiation at an absorption wavelength of 640 nm were 100%, 100%, and 100%, respectively. The results are shown in Table 2.
[0125] [Example 7] <Production of Co-doped colored silica sol (with a shell layer)> Particle synthesis of the Co-doped colored silica sol was carried out under the same conditions as in Example 1. That is, first, 10 g of a commercially available aqueous sodium silicate solution of JIS No. 3 was added to 284 g of pure water and uniformly mixed to prepare 294 g of a heel solution having a silica concentration of 1.0% by mass, a Na2O concentration of 0.32% by mass, a silica / Na2O molar ratio of 3.1, and a pH of 11.0. Next, 2.9 g of a 10 mass % CoSO4 aqueous solution, which had been prepared in advance by mixing and dissolving CoSO4·7H2O powder in pure water, was added to 613 g of the activated silicic acid aqueous solution and mixed uniformly to prepare 616 g of a feed liquid. 294 g of the prepared heel liquid was charged into a 3 L glass reaction vessel equipped with a stirrer and a condenser, and the liquid temperature in the vessel was kept at 80° C. in an oil bath. Next, 616 g of the feed liquid was continuously fed into the vessel under stirring at a constant rate over 100 minutes to synthesize particles. Thereafter, 1,593 g of the above aqueous active silicic acid solution was continuously fed at a constant rate over 260 minutes at 80° C. to form a shell layer on the particle surfaces. After the supply of the active silicic acid solution was completed, the liquid temperature in the vessel was maintained at 80° C. for 6 hours with stirring to obtain 2503 g of a sized liquid of Co-doped colored silica sol (with a shell layer).
[0126] The resulting Co-doped colored silica sol was highly transparent and blue-purple in color, and no sediment was observed. Furthermore, when a green laser pointer with a wavelength of 532 nm was irradiated, the Tyndall phenomenon was observed, and the dispersibility was good. The resulting Co-doped colored silica sol had a pH of 9.7, a silica concentration of 3.1% by mass, an average particle size (D3) of 14 nm measured by dynamic light scattering, a Co concentration of 0.0043% by mass (43 ppm by mass), and a mass ratio of Co to silica (Co / silica) of 0.0014. When the particles were observed with a TEM mode electron microscope, they were solid spherical particles. The number-average particle size (D1) calculated from the electron microscope image of the particles by image analysis was 12.9 ± 3.8 nm.
[0127] When the shell thickness was calculated from the number average particle diameter (D1) of the particles in Example 1, which was 9.5±2.6 nm, according to formula (2), the shell thickness was 1.7 nm.
[0128] Next, 2300 g of the obtained Co-doped colored silica sol was concentrated by pressure filtration with compressed air at room temperature under stirring using an ultrafiltration (UF) membrane with a molecular weight cutoff of 200,000, and 217 g of a highly transparent and blue-purple Co-doped colored silica sol UF concentrate and 2082 g of a colorless and transparent UF filtrate were recovered. The obtained UF concentrate of the Co-doped colored silica sol had a pH of 8.9, a silica concentration of 32.8 mass%, a Co concentration of 0.046 mass% (460 mass ppm), and a mass ratio of Co to silica (Co / silica) of 0.0014. The UF filtrate obtained during UF concentration had a pH of 9.7 and a Co concentration of 0.0001 mass% (1 mass ppm). Since Co was almost absent on the UF filtrate side and present on the UF concentrate side, it was confirmed that the colloidal silica particles were doped with Co and colored. The obtained UF concentrated solution of Co-doped colored silica sol was dried at 100° C. in air to obtain a transparent blue-purple powder of Co-doped colored silica sol. The powder was then crushed in a mortar and the particle density PD was measured using a dry density meter, which was 2.21 g / cm 3 Similarly, when the crushed powder was measured by X-ray diffraction, the XRD pattern was broad, indicating that the powder was amorphous.
[0129] The UF concentrate of the obtained Co-doped colored silica sol was then contacted with a hydrogen-type strong acid cation exchange resin to obtain an acidic Co-doped colored silica sol with a pH of 2.2 and a silica concentration of 26.2 mass%. This acidic Co-doped colored silica sol was dried in air at 300°C for 1 hour to obtain a transparent blue-purple acidic Co-doped colored silica sol powder. Furthermore, the powder was crushed in a mortar and measured by nitrogen adsorption, and the specific surface area (SSA) was found to be 255 m 2 The BET particle size (D2) calculated by the nitrogen adsorption method using formula (1) was 10.6 nm, and the number-average particle size / BET particle size (D1 / D2) ratio was 1.21.
[0130] The UF concentrate of the obtained Co-doped colored silica sol was filtered through a nylon membrane filter with a pore size of 0.45 μm, and then the visible-ultraviolet spectrum of the UF concentrate of the Co-doped colored silica sol was measured using pure water as a control. As a result, Co-derived absorption was confirmed at wavelengths of 540 nm, 590 nm, and 640 nm.
[0131] <Lightfastness evaluation> The obtained Co-doped colored silica sol was placed in a quartz cell with a lid and an optical path length of 10 mm, and installed in a QUV accelerated weathering tester to evaluate its lightfastness. When the state before UV irradiation was set as 100%, the absorbance change rates after 100 h, 250 h, and 500 h of UV irradiation at an absorption wavelength of 640 nm were 100%, 100%, and 100%, respectively. By forming a shell layer of silica on the particle surface, the lightfastness was improved compared with Example 1. The results are shown in Table 2.
[0132] [Example 8] <Production of Co-doped colored silica sol (with shell layer)> After synthesizing the particles in Example 7, in order to form a shell layer on the particle surface, the liquid temperature in the container during the continuous supply of the active silicic acid aqueous solution at a constant rate was changed from 80 °C to 100 °C, and further, after the supply of the active silicic acid aqueous solution was completed, the liquid temperature in the container was also changed from 80 °C to 100 °C. Otherwise, the operation was the same as in Example 7 to obtain 2503 g of a sizing liquid of Co-doped colored silica sol (with shell layer).
[0133] The obtained sizing liquid of Co-doped colored silica sol was highly transparent and blue-violet, and no sediment was generated. Further, when irradiated with a green laser pointer with a wavelength of 532 nm, the Tyndall phenomenon was observed and the dispersibility was good. This obtained sizing liquid of Co-doped colored silica sol had a pH of 9.7, a silica concentration of 3.3% by mass, an average particle diameter (D3) of 12 nm by the dynamic light scattering method, a Co concentration of 0.0044% by mass (44 ppm by mass), and a mass ratio of Co to silica (Co / silica) of 0.0013. When the particles were observed with an electron microscope in TEM mode, they were solid spherical particles. The number average particle diameter (D1) calculated by the image analysis method from the electron microscope image of these particles was 12.7 ± 2.9 nm.
[0134] When the shell thickness was calculated from the number average particle diameter (D1) of the particles in Example 1, which was 9.5±2.6 nm, according to formula (2), the shell thickness was 1.6 nm.
[0135] Next, 2,300 g of the resulting sized liquid of Co-doped colored silica sol was concentrated by pressure filtration with compressed air at room temperature under stirring using an ultrafiltration (UF) membrane with a molecular weight cutoff of 200,000, and 258 g of a highly transparent, blue-purple Co-doped colored silica sol UF concentrate and 2,042 g of a colorless, transparent UF filtrate were recovered. The UF concentrated solution of the obtained Co-doped colored silica sol had a pH of 8.9, a silica concentration of 29.4 mass%, a Co concentration of 0.038 mass% (380 mass ppm), and a mass ratio of Co to silica (Co / silica) of 0.0013. The UF filtrate obtained during UF concentration had a pH of 9.5 and a Co concentration of 0.0001 mass% (1 mass ppm). Since almost no Co was present in the UF filtrate side, but was present in the UF concentrated solution side, it was confirmed that the colloidal silica particles were doped with Co and colored. The obtained UF concentrated solution of Co-doped colored silica sol was dried at 100° C. in air to obtain a transparent blue-purple powder of Co-doped colored silica sol. The powder was then crushed in a mortar and the particle density PD was measured using a dry density meter, which was 2.22 g / cm 3 Similarly, when the crushed powder was measured by X-ray diffraction, the XRD pattern was broad, indicating that the powder was amorphous.
[0136] The resulting UF concentrate of the Co-doped colored silica sol was then contacted with a hydrogen-type strong acid cation exchange resin to obtain an acidic Co-doped colored silica sol with a pH of 2.1 and a silica concentration of 27.9% by mass. This acidic Co-doped colored silica sol was dried in air at 300°C for 1 hour to obtain a transparent blue-purple acidic Co-doped colored silica sol powder. Furthermore, the powder was crushed in a mortar and measured by nitrogen adsorption, and the specific surface area (SSA) was found to be 252 m 2 It was / g. The BET particle diameter (D2) calculated from the nitrogen adsorption method using Equation (1) was 10.7 nm, and the ratio of the number average particle diameter to the BET particle diameter (D1 / D2) was 1.19.
[0137] The UF concentrate of the obtained Co-doped colored silica sol was filtered through a nylon membrane filter with a pore size of 0.45 μm, and then the visible-ultraviolet spectrum of the UF concentrate of the Co-doped colored silica sol was measured using pure water as a control. As a result, Co-derived absorption was confirmed at wavelengths of 540 nm, 590 nm, and 640 nm.
[0138] <Light resistance evaluation> The obtained Co-doped colored silica sol was placed in a quartz cell with a lid and an optical path length of 10 mm, and installed in a QUV accelerated weathering tester to evaluate its light resistance. When the absorbance before UV irradiation was set as 100%, the change rates of absorbance after 100 h, 250 h, and 500 h of UV irradiation at an absorption wavelength of 640 nm were 100%, 100%, and 100%, respectively. By forming a shell layer of silica on the particle surface, the light resistance was improved compared to Example 1. The results are shown in Table 2.
[0139] [Example 9] <Production of Co-doped colored silica sol (with shell layer)> 343 g of the sizing liquid of the Co-doped colored silica sol prepared in Example 1 and 9.2 g of a 10 mass% aqueous NaOH solution were charged into a 3 L glass reaction vessel equipped with a stirrer and a condenser, and the liquid temperature in the vessel was maintained at 80 °C with an oil bath. Next, 2029 g of the active silicic acid aqueous solution was continuously supplied to this vessel under stirring at a constant rate over 900 minutes to form a shell layer on the particle surface. After the supply of this active silicic acid aqueous solution was completed, the liquid temperature in the vessel was maintained at 80 °C for 6 hours under stirring to obtain 2381 g of the sizing liquid of the Co-doped colored silica sol (with shell layer).
[0140] The resulting Co-doped colored silica sol was highly transparent and blue-purple in color, and no sediment was observed. Furthermore, when a green laser pointer with a wavelength of 532 nm was irradiated, the Tyndall phenomenon was observed, and the dispersibility was good. The resulting Co-doped colored silica sol had a pH of 10.0, a silica concentration of 3.4 mass%, an average particle size (D3) of 17 nm measured by dynamic light scattering, a Co concentration of 0.0017 mass% (17 mass ppm), and a mass ratio of Co to silica (Co / silica) of 0.0005. When the particles were observed with a TEM mode electron microscope, they were solid spherical particles. The number-average particle size (D1) calculated from the electron microscope image of the particles by image analysis was 16.8 ± 3.7 nm.
[0141] When the shell thickness was calculated from the number average particle diameter (D1) of the particles in Example 1, which was 9.5±2.6 nm, according to formula (2), the shell thickness was 3.7 nm.
[0142] Next, 2,300 g of the resulting sized liquid of Co-doped colored silica sol was concentrated by pressure filtration with compressed air at room temperature under stirring using an ultrafiltration (UF) membrane with a molecular weight cutoff of 200,000, and 238 g of a highly transparent, blue-purple Co-doped colored silica sol UF concentrate and 2,062 g of a colorless, transparent UF filtrate were recovered. The UF concentrated solution of the obtained Co-doped colored silica sol had a pH of 9.4, a silica concentration of 32.8 mass%, a Co concentration of 0.016 mass% (160 mass ppm), and a mass ratio of Co to silica (Co / silica) of 0.0005. The UF filtrate obtained during UF concentration had a pH of 9.8 and a Co concentration of 0.0001 mass% (1 mass ppm). Since almost no Co was present in the UF filtrate side, but was present in the UF concentrated solution side, it was confirmed that the colloidal silica particles were doped with Co and colored. The obtained UF concentrated solution of Co-doped colored silica sol was dried at 100° C. in air to obtain a transparent blue-purple powder of Co-doped colored silica sol. The powder was then crushed in a mortar and the particle density PD was measured using a dry density meter, which was 2.23 g / cm 3 It was the same. As a result of measuring the pulverized powder by X-ray diffraction method, since the XRD pattern was broad, the crystallinity of the powder was amorphous.
[0143] Next, the UF concentrate of the obtained Co-doped colored silica sol was brought into contact with a hydrogen-type strongly acidic cation exchange resin to obtain an acidic Co-doped colored silica sol having a pH of 2.2 and a silica concentration of 25.4% by mass. This acidic Co-doped colored silica sol was dried at 300 °C for 1 hour in the air to obtain a powder of a transparent blue-violet acidic Co-doped colored silica sol. Furthermore, as a result of measuring the powder pulverized in a mortar by the nitrogen adsorption method, the specific surface area SSA was 186 m 2 / g. The BET particle size (D2) calculated from the nitrogen adsorption method using Equation (1) was 14.5 nm, and the ratio of the number average particle size to the BET particle size (D1 / D2) was 1.16.
[0144] The UF concentrate of the obtained Co-doped colored silica sol was filtered through a nylon membrane filter with a pore size of 0.45 μm, and then the visible ultraviolet spectrum of the UF concentrate of the Co-doped colored silica sol was measured using pure water as a control. As a result, Co-derived absorption was confirmed at wavelengths of 540 nm, 590 nm, and 640 nm.
[0145] <Light resistance evaluation> The obtained Co-doped colored silica sol was placed in a quartz cell with a lid having an optical path length of 10 mm and installed in a QUV accelerated weathering tester to evaluate the light resistance. When the state before UV irradiation was set as 100%, the absorbance change rates after 100 h, 250 h, and 500 h of UV irradiation at an absorption wavelength of 640 nm were 100%, 100%, and 100%, respectively. By forming a shell layer of silica on the particle surface, the light resistance was improved compared with Example 1. The results are shown in Table 2.
[0146] [Example 10] [Production of Co-doped colored silica sol (with shell layer)] In Example 9, in order to form a shell layer on the particle surface, the liquid temperature in the container when the active silicic acid aqueous solution was continuously supplied at a constant rate was changed from 80°C to 100°C, and after the supply of the active silicic acid aqueous solution was completed, the liquid temperature in the container was also changed from 80°C to 100°C. Except for this, the same procedure as in Example 9 was repeated to obtain 2,381 g of a sized solution of Co-doped colored silica sol (with shell layer).
[0147] The resulting Co-doped colored silica sol was highly transparent and blue-purple in color, and no sediment was observed. Furthermore, when a green laser pointer with a wavelength of 532 nm was irradiated, the Tyndall phenomenon was observed, and the dispersibility was good. The resulting Co-doped colored silica sol had a pH of 10.1, a silica concentration of 3.6 mass%, an average particle size (D3) of 25 nm measured by dynamic light scattering, a Co concentration of 0.0017 mass% (17 mass ppm), and a mass ratio of Co to silica (Co / silica) of 0.0005. When the particles were observed with a TEM mode electron microscope, they were solid spherical particles. The number-average particle size (D1) calculated from the electron microscope image of the particles by image analysis was 17.3 ± 4.1 nm.
[0148] When the shell thickness was calculated from the number average particle diameter (D1) of the particles in Example 1, which was 9.5±2.6 nm, according to formula (2), the shell thickness was 3.9 nm.
[0149] Next, 2,300 g of the resulting sized liquid of Co-doped colored silica sol was concentrated by pressure filtration with compressed air at room temperature under stirring using an ultrafiltration (UF) membrane with a molecular weight cutoff of 200,000, and 268 g of a highly transparent, blue-purple Co-doped colored silica sol UF concentrate and 2,032 g of a colorless, transparent UF filtrate were recovered. The UF concentrate of the obtained Co-doped colored silica sol had a pH of 9.6, a silica concentration of 30.9 mass%, a Co concentration of 0.014 mass% (140 mass ppm), and a mass ratio of Co to silica (Co / silica) of 0.0005. The UF filtrate obtained during UF concentration had a pH of 10.0 and a Co concentration below the lower detection limit (less than 0.0001 mass%). Since almost no Co was present in the UF filtrate side but was present in the UF concentrate side, it was confirmed that the colloidal silica particles were doped with Co and colored. The obtained UF concentrated solution of Co-doped colored silica sol was dried at 100° C. in air to obtain a transparent blue-purple powder of Co-doped colored silica sol. The powder was then crushed in a mortar and the particle density PD was measured using a dry density meter, which was 2.24 g / cm 3 Similarly, when the crushed powder was measured by X-ray diffraction, the XRD pattern was broad, indicating that the powder was amorphous.
[0150] The UF concentrate of the obtained Co-doped colored silica sol was then contacted with a hydrogen-type strong acid cation exchange resin to obtain an acidic Co-doped colored silica sol with a pH of 2.1 and a silica concentration of 24.2% by mass. This acidic Co-doped colored silica sol was dried in air at 300°C for 1 hour to obtain a transparent blue-purple acidic Co-doped colored silica sol powder. Furthermore, the powder was crushed in a mortar and measured by nitrogen adsorption, and the specific surface area (SSA) was 174 m 2 The BET particle size (D2) calculated by the nitrogen adsorption method using formula (1) was 15.4 nm, and the number-average particle size / BET particle size (D1 / D2) ratio was 1.13.
[0151] The UF concentrated solution of the Co-doped colored silica sol was filtered through a nylon membrane filter with a pore size of 0.45 μm, and the visible-ultraviolet spectrum of the UF concentrated solution of the Co-doped colored silica sol was measured using pure water as a control. As a result, absorption due to Co was confirmed at wavelengths of 540 nm, 590 nm, and 640 nm.
[0152] <Light resistance evaluation> The obtained Co-doped colored silica sol was placed in a quartz cell with a lid and an optical path length of 10 mm, and installed in a QUV accelerated weathering tester to evaluate its light resistance. When the absorbance before UV irradiation was set to 100%, the absorbance change rates after 100 h, 250 h, and 500 h of UV irradiation at an absorption wavelength of 640 nm were 100%, 100%, and 100%, respectively. By forming a shell layer of silica on the particle surface, the light resistance was improved compared to Example 1. The results are shown in Table 2.
[0153] [Example 11] <Production of Co-doped Colored Silica Sol> 1108 g of a heel solution (silica concentration: 1.0% by mass, NH3 concentration: 1.1% by mass, silica / NH3 molar ratio: 0.26, pH: 10.8) was prepared by adding 745 g of pure water, 317 g of the above-mentioned active silicic acid aqueous solution, and 46 g of aqueous ammonia and mixing them uniformly. Next, 29.0 g of a 10% by mass CoSO4 aqueous solution prepared by previously mixing and dissolving CoSO4·7H2O powder in pure water and 1384 g of the above-mentioned active silicic acid aqueous solution were uniformly mixed to prepare 1413 g of a feed solution. 1108 g of the prepared heel solution was charged into a 3 L glass reaction vessel equipped with a stirrer and a condenser, and the liquid temperature in the vessel was maintained at 80 °C with an oil bath. Then, 1413 g of the feed solution was continuously supplied into this vessel under stirring at a constant rate over 60 minutes to perform particle synthesis. After the completion of the supply of this feed solution, the liquid temperature in the vessel was maintained at 80 °C for 6 hours under stirring to obtain 2521 g of a sizing solution of Co-doped colored silica sol.
[0154] The resulting Co-doped colored silica sol was highly transparent and blue-purple in color, and no sediment was observed. Furthermore, when a green laser pointer with a wavelength of 532 nm was irradiated, the Tyndall phenomenon was observed, and the dispersibility was good. The resulting Co-doped colored silica sol had a pH of 10.4, a silica concentration of 2.4 mass%, an average particle size (D3) of 27 nm measured by dynamic light scattering, a Co concentration of 0.045 mass% (450 mass ppm), and a mass ratio of Co to silica (Co / silica) of 0.019. When the particles were observed with a TEM mode electron microscope, they were solid spherical particles. The number-average particle size (D1) calculated from the electron microscope image of the particles by image analysis was 10.5 ± 3.3 nm.
[0155] Next, 2,360 g of the resulting sized liquid of Co-doped colored silica sol was concentrated by pressure filtration with compressed air at room temperature under stirring using an ultrafiltration (UF) membrane with a molecular weight cutoff of 200,000, and 193 g of a highly transparent, blue-purple Co-doped colored silica sol UF concentrate and 2,167 g of a colorless, transparent UF filtrate were recovered. The UF concentrate of the obtained Co-doped colored silica sol had a pH of 9.7, a silica concentration of 29.4 mass%, a Co concentration of 0.57 mass% (5700 mass ppm), and a mass ratio of Co to silica (Co / silica) of 0.019. The UF filtrate obtained during UF concentration had a pH of 10.4 and a Co concentration below the lower detection limit (less than 0.0001 mass%). Since almost no Co was present in the UF filtrate side, but was present in the UF concentrate side, it was confirmed that the colloidal silica particles were doped with Co and colored. The obtained UF concentrated solution of Co-doped colored silica sol was dried at 100°C under air to obtain a transparent blue-purple powder of Co-doped colored silica sol. The powder was then crushed in a mortar and the particle density PD was measured with a dry densitometer, which was 2.21 g / cm. 3 Similarly, when the crushed powder was measured by X-ray diffraction, the XRD pattern was broad, indicating that the powder was amorphous.
[0156] Next, the UF concentrate of the Co-doped colored silica sol obtained was contacted with a hydrogen-type strongly acidic cation exchange resin to obtain an acidic Co-doped colored silica sol having a pH of 2.0 and a silica concentration of 20.5% by mass. This acidic Co-doped colored silica sol was dried at 300 °C for 1 hour under the atmosphere to obtain a transparent blue-violet powder of the acidic Co-doped colored silica sol. Furthermore, the powder further pulverized in a mortar was measured by the nitrogen adsorption method. As a result, the specific surface area SSA was 296 m 2 / g. The BET particle size (D2) calculated from the nitrogen adsorption method using Equation (1) was 9.2 nm, and the ratio of the number average particle size to the BET particle size (D1 / D2) was 1.14.
[0157] The sizing liquid of the obtained Co-doped colored silica sol was filtered through a nylon membrane filter with a pore size of 0.45 μm, and then the visible ultraviolet spectrum of the sizing liquid of the Co-doped colored silica sol was measured using pure water as a control. As a result, Co-derived absorption was confirmed at wavelengths of 525 nm, 580 nm, and 640 nm.
[0158] <Lightfastness evaluation> The obtained Co-doped colored silica sol was placed in a quartz cell with a lid having an optical path length of 10 mm and installed in a QUV accelerated weathering tester to evaluate the lightfastness. When the situation before UV irradiation was set as 100%, the absorbance change rates after 100 h, 250 h, and 500 h of UV irradiation at an absorption wavelength of 640 nm were 89%, 80%, and 74%, respectively. The results are shown in Table 2.
[0159] [Example 12] <Production of Co-doped colored silica sol (with shell layer)> Particle synthesis of the Co-doped colored silica sol was carried out under the same conditions as in Example 11. That is, first, 315 g of pure water, 134 g of the active silicic acid aqueous solution, and 19 g of aqueous ammonia were added and uniformly mixed to prepare 468 g of a heel liquid (silica concentration 1.0% by mass, NH3 concentration 1.1% by mass, silica / NH3 molar ratio 0.26, pH 10.8). Next, 12.3 g of a 10 mass % CoSO4 aqueous solution, which had been prepared in advance by mixing and dissolving CoSO4·7H2O powder in pure water, and 585 g of the above-mentioned active silicic acid aqueous solution were uniformly mixed to prepare 597 g of a feed liquid. 468 g of the prepared heel liquid was charged into a 3 L glass reaction vessel equipped with a stirrer and a condenser, and the liquid temperature in the vessel was kept at 80° C. in an oil bath. Next, 597 g of the feed liquid was continuously fed into the vessel under stirring at a constant rate over 60 minutes to synthesize particles. Thereafter, 1,454 g of the above aqueous active silicic acid solution was continuously fed at a constant rate over 144 minutes at 80° C. to form a shell layer on the particle surfaces. After the supply of the active silicic acid solution was completed, the liquid temperature in the vessel was maintained at 80° C. for 6 hours with stirring to obtain 2,519 g of a sized liquid of Co-doped colored silica sol (with a shell layer).
[0160] The granulation liquid of the Co-doped colored silica sol was highly transparent and blue-purple, and no sediment was generated. Furthermore, when a green laser pointer with a wavelength of 532 nm was irradiated, the Tyndall phenomenon was observed, and the dispersibility was good. The granulation liquid of the Co-doped colored silica sol obtained had a pH of 10.1, a silica concentration of 3.0 mass%, an average particle size (D3) of 24 nm by dynamic light scattering method, a Co concentration of 0.019 mass% (190 mass ppm), and a mass ratio of Co to silica (Co / silica) of 0.0063. When the particles were observed with an electron microscope in TEM mode, they were solid spherical particles. The number-average particle size (D1) calculated by image analysis from the electron microscope image of the particles was 11.1 ± 3.8 nm.
[0161] When the shell thickness was calculated from the formula (2) using the number average particle diameter (D1) of the particles of Comparative Example 2, which was 10.5±3.3 nm, the shell thickness was 0.3 nm.
[0162] Next, 2,340 g of the resulting sized liquid of Co-doped colored silica sol was concentrated by pressure filtration with compressed air at room temperature under stirring using an ultrafiltration (UF) membrane with a molecular weight cutoff of 200,000, and 232 g of a highly transparent, blue-purple Co-doped colored silica sol UF concentrate and 2,108 g of a colorless, transparent UF filtrate were recovered. The UF concentrate of the obtained Co-doped colored silica sol had a pH of 9.4, a silica concentration of 30.3 mass%, a Co concentration of 0.19 mass% (1900 mass ppm), and a mass ratio of Co to silica (Co / silica) of 0.0063. The UF filtrate obtained during UF concentration had a pH of 10.2 and a Co concentration below the lower detection limit (less than 0.0001 mass%). Since almost no Co was present in the UF filtrate side but was present in the UF concentrate side, it was confirmed that the colloidal silica particles were doped with Co and colored. The obtained UF concentrated solution of Co-doped colored silica sol was dried at 100° C. in air to obtain a transparent blue-purple powder of Co-doped colored silica sol. The powder was then crushed in a mortar and the particle density PD was measured using a dry density meter, which was 2.20 g / cm 3 Similarly, when the crushed powder was measured by X-ray diffraction, the XRD pattern was broad, indicating that the powder was amorphous.
[0163] The UF concentrate of the obtained Co-doped colored silica sol was then contacted with a hydrogen-type strong acid cation exchange resin to obtain an acidic Co-doped colored silica sol having a pH of 2.2 and a silica concentration of 21.5% by mass. This acidic Co-doped colored silica sol was dried in air at 300°C for 1 hour to obtain a transparent blue-purple acidic Co-doped colored silica sol powder. Furthermore, the powder was crushed in a mortar and measured by nitrogen adsorption, and the specific surface area (SSA) was found to be 275 m 2 The BET particle size (D2) calculated by the nitrogen adsorption method using formula (1) was 9.9 nm, and the number-average particle size / BET particle size (D1 / D2) ratio was 1.12.
[0164] The resulting sized liquid of the Co-doped colored silica sol was filtered through a nylon membrane filter with a pore size of 0.45 μm, and then the visible-ultraviolet spectrum of the sized liquid of the Co-doped colored silica sol was measured using pure water as a control. As a result, absorption due to Co was confirmed at wavelengths of 525 nm, 580 nm, and 640 nm.
[0165] <Light resistance evaluation> The obtained Co-doped colored silica sol was placed in a quartz cell with a lid and an optical path length of 10 mm, and installed in a QUV accelerated weathering tester to evaluate its light resistance. When the state before UV irradiation was set as 100%, the absorbance change rates after 100 h, 250 h, and 500 h of UV irradiation at an absorption wavelength of 640 nm were 95%, 92%, and 90%, respectively. By forming a silica shell layer on the particle surface, the light resistance was improved compared to Example 11. The results are shown in Table 2.
[0166] [Example 13] <Production of Cr-doped colored silica sol> 808 g of a heel liquid (silica concentration 1.0 mass%, NH3 concentration 1.1 mass%, silica / NH3 molar ratio 0.26, pH 10.9) was prepared by adding 543 g of pure water, 231 g of the above-mentioned active silicic acid aqueous solution (silica concentration 3.5 mass%, pH 2.9), and 34 g of aqueous ammonia (ammonia concentration 27 mass%) and mixing them uniformly. Next, 13.9 g of a 10 mass% Cr(NO3)3 aqueous solution prepared by previously mixing and dissolving Cr(NO3)3·9H2O in pure water was added to 1684 g of the above-mentioned active silicic acid aqueous solution and mixed uniformly to prepare 1698 g of a feed liquid. 808 g of the prepared heel liquid was charged into a 3 L glass reaction vessel equipped with a stirrer and a condenser, and the liquid temperature in the vessel was maintained at 80 °C with an oil bath. Then, 1698 g of the feed liquid was continuously supplied into this vessel at a constant rate over 100 minutes with stirring to perform particle synthesis. After the completion of the supply of this feed liquid, the liquid temperature in the vessel was maintained at 80 °C for 6 hours with stirring to obtain 2506 g of a sizing liquid of Cr-doped colored silica sol.
[0167] The granulated liquid of the Cr-doped colored silica sol obtained was highly transparent and blue-green, and no sediment was generated. Furthermore, when a green laser pointer with a wavelength of 532 nm was irradiated, the Tyndall phenomenon was observed, and the dispersibility was good. The granulated liquid of the Cr-doped colored silica sol obtained had a pH of 10.4, a silica concentration of 2.7 mass%, an average particle size (D3) of 23 nm by dynamic light scattering method, a Cr concentration of 0.012 mass% (120 mass ppm), and a mass ratio of Cr to silica (Cr / silica) of 0.0044. When the particles were observed with an electron microscope in TEM mode, they were solid spherical particles. The electron microscope image is shown in Figure 1. The number average particle size (D1) calculated by image analysis from the electron microscope image of the particles was 9.3 ± 3.0 nm.
[0168] Next, 2340 g of the resulting sized liquid of Cr-doped colored silica sol was concentrated by pressure filtration with compressed air at room temperature under stirring using an ultrafiltration (UF) membrane with a molecular weight cutoff of 200,000, and 210 g of a highly transparent, blue-green UF concentrate of Cr-doped colored silica sol and 2130 g of a colorless, transparent UF filtrate were recovered. The appearance of this UF concentrate of Cr-doped colored silica sol is shown in Figure 2. The UF concentrated solution of the obtained Cr-doped colored silica sol had a pH of 9.7, a silica concentration of 30.1 mass%, a Cr concentration of 0.13 mass% (1300 mass ppm), and a mass ratio of Cr to silica (Cr / silica) of 0.0043. The UF filtrate obtained during UF concentration had a pH of 10.5 and a Cr concentration below the lower detection limit (less than 0.0001 mass%). Since Cr was almost absent in the UF filtrate and present in the UF concentrated solution, it was confirmed that the colloidal silica particles were doped with Cr and colored. The UF concentrated solution of the Cr-doped colored silica sol was dried at 100°C in air to obtain a transparent blue-green powder of Cr-doped colored silica sol. The appearance of this powder of Cr-doped colored silica sol is shown in Figure 3. The powder was then pulverized in a mortar and the particle density PD was measured with a dry densitometer, which was 2.16 g / cm. 3 Similarly, when the crushed powder was measured by X-ray diffraction, the XRD pattern was broad, indicating that the powder was amorphous. The XRD pattern is shown in Figure 4.
[0169] Next, the UF concentrate of the obtained Cr-doped colored silica sol was brought into contact with a hydrogen-type strongly acidic cation exchange resin to obtain an acidic Cr-doped colored silica sol having a pH of 2.5 and a silica concentration of 21.2% by mass. This acidic Cr-doped colored silica sol was dried at 300 °C for 1 hour under the atmosphere to obtain a transparent blue-green acidic Cr-doped colored silica sol powder. Furthermore, as a result of measuring the powder further pulverized in a mortar by the nitrogen adsorption method, the specific surface area SSA was 307 m 2 / g. The BET particle size (D2) calculated from the nitrogen adsorption method using Equation (1) was 9.0 nm, and the ratio of the number average particle size to the BET particle size (D1 / D2) was 1.07.
[0170] After filtering the UF concentrate of the obtained Cr-doped colored silica sol with a nylon membrane filter having a pore size of 0.45 μm, the visible ultraviolet spectrum of the UF concentrate of the Cr-doped colored silica sol was measured using pure water as a control. As a result, Cr-derived absorption was confirmed at wavelengths of 425 nm and 590 nm. This visible ultraviolet transmission spectrum and visible ultraviolet absorption spectrum are shown in FIG. 5.
[0171] <Lightfastness evaluation> The obtained Cr-doped colored silica sol was placed in a quartz cell with a lid having an optical path length of 10 mm and installed in a QUV accelerated weathering tester to evaluate the lightfastness. When the state before UV irradiation was set to 100%, the absorbance change rates after 100 h, 250 h, and 500 h of UV irradiation at an absorption wavelength of 590 nm were 99%, 98%, and 97%, respectively. The results are shown in Table 2 and FIG. 6.
[0172] [Example 14] <Production of Mn-doped colored silica sol> 808 g of a heel liquid (silica concentration: 1.0% by mass, NH3 concentration: 1.1% by mass, silica / NH3 molar ratio: 0.26, pH: 10.9) was prepared by adding 543 g of pure water, 231 g of the above-mentioned active silicic acid aqueous solution (silica concentration: 3.5% by mass, pH: 2.9), and 34 g of aqueous ammonia (ammonia concentration: 27% by mass) and mixing them uniformly. Next, 8.3 g of a 10 mass % MnSO4 aqueous solution, which had been prepared in advance by mixing and dissolving MnSO4·5H2O in pure water, was added to 1,684 g of the activated silicic acid aqueous solution and mixed uniformly to prepare 1,692 g of a feed liquid. 808 g of the prepared heel liquid was charged into a 3 L glass reaction vessel equipped with a stirrer and a condenser, and the liquid temperature in the vessel was kept at 80° C. in an oil bath. Next, 1692 g of the feed liquid was continuously fed into the vessel under stirring at a constant rate over 100 minutes to synthesize particles. After the feed liquid was fed, the liquid temperature in the vessel was kept at 80° C. for 6 hours under stirring to obtain 2500 g of a granulated liquid of Mn-doped colored silica sol.
[0173] The obtained Mn-doped colored silica sol was highly transparent and reddish brown, and no sediment was generated. Furthermore, when a green laser pointer with a wavelength of 532 nm was irradiated, the Tyndall phenomenon was observed, and the dispersibility was good. The obtained Mn-doped colored silica sol had a pH of 10.4, a silica concentration of 2.7 mass%, an average particle size (D3) of 19 nm by dynamic light scattering, a Mn concentration of 0.012 mass% (120 mass ppm), and a mass ratio of Mn to silica (Mn / silica) of 0.0045. When the particles were observed with an electron microscope in TEM mode, they were solid spherical particles. The electron microscope image is shown in Figure 1. The number-average particle size (D1) calculated from the electron microscope image of the particles by image analysis was 10.0 ± 2.8 nm.
[0174] Next, 2340 g of the resulting Mn-doped colored silica sol was concentrated by pressure filtration with compressed air at room temperature under stirring using an ultrafiltration (UF) membrane with a molecular weight cutoff of 200,000, and 238 g of a highly transparent, reddish-brown UF concentrate of Mn-doped colored silica sol and 2102 g of a colorless, transparent UF filtrate were recovered. The appearance of this UF concentrate of Mn-doped colored silica sol is shown in Figure 2. The UF concentrated solution of the obtained Mn-doped colored silica sol had a pH of 9.8, a silica concentration of 26.5 mass%, a Mn concentration of 0.12 mass% (1200 mass ppm), and a mass ratio of Mn to silica (Mn / silica) of 0.0045. The UF filtrate obtained during UF concentration had a pH of 10.5 and a Mn concentration below the lower detection limit (less than 0.0001 mass%). Since Mn was almost absent in the UF filtrate and present in the UF concentrated solution, it was confirmed that the colloidal silica particles were doped with Mn and colored. The obtained UF concentrated solution of Mn-doped colored silica sol was dried at 100°C in air to obtain a transparent reddish brown powder of Mn-doped colored silica sol. The appearance of this powder of Mn-doped colored silica sol is shown in Figure 3. The powder was then pulverized in a mortar, and the particle density PD was measured with a dry densitometer, which was 2.18 g / cm. 3 Similarly, when the crushed powder was measured by X-ray diffraction, the XRD pattern was broad, indicating that the powder was amorphous. The XRD pattern is shown in Figure 4.
[0175] Next, the obtained UF concentrate of Mn-doped colored silica sol was contacted with a hydrogen-type strong acid cation exchange resin to obtain an acidic Mn-doped colored silica sol having a pH of 2.3 and a silica concentration of 19.6 mass%. This acidic Mn-doped colored silica sol was dried in air at 300°C for 1 hour to obtain a transparent reddish brown acidic Mn-doped colored silica sol powder. Furthermore, the powder was crushed in a mortar and measured by nitrogen adsorption, and the specific surface area (SSA) was found to be 271 m 2 The BET particle size (D2) calculated by the nitrogen adsorption method using formula (1) was 10.2 nm, and the number-average particle size / BET particle size (D1 / D2) ratio was 0.98.
[0176] The obtained UF concentrated solution of Mn-doped colored silica sol was filtered through a nylon membrane filter with a pore size of 0.45 μm, and then the visible-ultraviolet spectrum of the UF concentrated solution of Mn-doped colored silica sol was measured using pure water as a control. As a result, absorption due to Mn was confirmed at a wavelength of 455 nm. The visible-ultraviolet transmission spectrum and the visible-ultraviolet absorption spectrum are shown in Figure 5.
[0177] <Light resistance evaluation> The obtained Mn-doped colored silica sol was placed in a quartz cell with a lid and an optical path length of 10 mm, and installed in a QUV accelerated weathering tester to evaluate its light resistance. When the absorbance before UV irradiation was set to 100%, the change rates of absorbance after 100 h, 250 h, and 500 h of UV irradiation at an absorption wavelength of 455 nm were 100%, 100%, and 100%, respectively. The results are shown in Table 2 and Figure 6.
[0178] [Example 15] <Production of Cu-doped colored silica sol> 808 g of a heel solution (silica concentration 1.0 mass%, NH3 concentration 1.1 mass%, silica / NH3 molar ratio 0.26, pH 10.9) was prepared by adding 543 g of pure water, 231 g of the above-mentioned active silicic acid aqueous solution (silica concentration 3.5 mass%, pH 2.9), and 34 g of aqueous ammonia (ammonia concentration 27 mass%) and mixing them uniformly. Next, 7.6 g of a 10 mass% CuSO4 aqueous solution prepared by previously mixing and dissolving CuSO4·5H2O in pure water was added to 1684 g of the above-mentioned active silicic acid aqueous solution and mixed uniformly to prepare 1692 g of a feed solution. 808 g of the prepared heel solution was charged into a 3 L glass reaction vessel equipped with a stirrer and a condenser, and the liquid temperature in the vessel was maintained at 80 °C with an oil bath. Then, 1692 g of the feed solution was continuously supplied into this vessel at a constant rate over 100 minutes with stirring to perform particle synthesis. After the supply of this feed solution was completed, the liquid temperature in the vessel was maintained at 80 °C for 6 hours with stirring to obtain 2500 g of a sizing solution of Cu-doped colored silica sol.
[0179] The resulting Cu-doped colored silica sol was highly transparent and sky blue, and no sediment was generated. Furthermore, when a green laser pointer with a wavelength of 532 nm was irradiated, the Tyndall phenomenon was observed, and the dispersibility was good. The resulting Cu-doped colored silica sol had a pH of 10.4, a silica concentration of 2.7 mass%, an average particle size (D3) of 19 nm by dynamic light scattering, a Cu concentration of 0.011 mass% (110 mass ppm), and a mass ratio of Cu to silica (Cu / silica) of 0.0041. When the particles were observed with a TEM mode electron microscope, they were solid spherical particles. The electron microscope image is shown in Figure 1. The number-average particle size (D1) calculated from the electron microscope image of the particles by image analysis was 9.7 ± 2.9 nm.
[0180] Next, 2340 g of the resulting Cu-doped colored silica sol was concentrated by pressure filtration with compressed air at room temperature under stirring using an ultrafiltration (UF) membrane with a molecular weight cutoff of 200,000, and 207 g of a highly transparent, sky blue Cu-doped colored silica sol UF concentrate and 2133 g of a colorless, transparent UF filtrate were recovered. The appearance of this Cu-doped colored silica sol UF concentrate is shown in Figure 2. The UF concentrated solution of the obtained Cu-doped colored silica sol had a pH of 9.7, a silica concentration of 30.5 mass%, a Cu concentration of 0.13 mass% (1300 mass ppm), and a mass ratio of Cu to silica (Cu / silica) of 0.0043. The UF filtrate obtained during UF concentration had a pH of 10.6 and a Cu concentration below the lower detection limit (less than 0.0001 mass%). Since almost no Cu was present in the UF filtrate side, but was present in the UF concentrated solution side, it was confirmed that the colloidal silica particles were doped with Cu and colored. The obtained UF concentrated solution of Cu-doped colored silica sol was dried at 100°C in air to obtain a transparent sky blue powder of Cu-doped colored silica sol. The appearance of this powder of Cu-doped colored silica sol is shown in Figure 3. The powder was then crushed in a mortar and the particle density PD was measured with a dry densitometer, which was 2.17 g / cm. 3 Similarly, when the crushed powder was measured by X-ray diffraction, the XRD pattern was broad, indicating that the powder was amorphous. The XRD pattern is shown in Figure 4.
[0181] Next, the UF concentrate of the obtained Cu-doped colored silica sol was contacted with a hydrogen-type strongly acidic cation exchange resin to obtain an acidic Cu-doped colored silica sol having a pH of 2.2 and a silica concentration of 19.8% by mass. This acidic Cu-doped colored silica sol was dried at 300 °C for 1 hour under the atmosphere to obtain a transparent sky-blue acidic Cu-doped colored silica sol powder. Furthermore, the powder pulverized in a mortar was measured by the nitrogen adsorption method. As a result, the specific surface area SSA was 280 m 2 / g. The BET particle size (D2) calculated from the nitrogen adsorption method using Equation (1) was 9.9 nm, and the ratio of the number average particle size to the BET particle size (D1 / D2) was 0.98.
[0182] After filtering the UF concentrate of the obtained Cu-doped colored silica sol through a nylon membrane filter with a pore size of 0.45 μm, the visible-ultraviolet spectrum of the UF concentrate of the Cu-doped colored silica sol was measured using pure water as a control. As a result, absorption derived from Cu was confirmed at a wavelength of 640 nm. The visible-ultraviolet transmission spectrum and the visible-ultraviolet absorption spectrum are shown in Fig. 5.
[0183] <Light resistance evaluation> The obtained Cu-doped colored silica sol was placed in a quartz cell with a lid having an optical path length of 10 mm and installed in a QUV accelerated weathering tester to evaluate the light resistance. When the state before UV irradiation was set as 100%, the absorbance change rates after 100 h, 250 h, and 500 h of UV irradiation at an absorption wavelength of 640 nm were 99%, 99%, and 99%, respectively. The results are shown in Table 2 and Fig. 6.
[0184] [Example 16] <Production of Ni-doped colored silica sol> 284 g of pure water, 10 g of a commercially available aqueous sodium silicate solution of JIS No. 3, and 10 g of an aqueous sodium hydroxide solution (NaOH concentration: 10% by mass) were added and uniformly mixed to prepare 304 g of a heel solution (silica concentration: 1.0% by mass, N2O concentration: 0.57% by mass, silica / N2O molar ratio: 1.8, pH: 12.0). Next, 19.6 g of a 10 mass % NiSO4 aqueous solution, which had been prepared in advance by mixing and dissolving NiSO4·6H2O in pure water, was added to 2205 g of the activated silicic acid aqueous solution and mixed uniformly to prepare 2225 g of a feed liquid. 304 g of the prepared heel liquid was charged into a 3 L glass reaction vessel equipped with a stirrer and a condenser, and the liquid temperature in the vessel was kept at 80° C. in an oil bath. Next, 2225 g of the feed liquid was continuously fed into the vessel under stirring at a constant rate over 100 minutes, and then heated to 100° C. and continuously fed at a constant rate over 260 minutes to synthesize particles. After the feed liquid was fed, the liquid temperature in the vessel was kept at 100° C. for 6 hours under stirring to obtain 2529 g of a sized liquid of Ni-doped colored silica sol.
[0185] The Ni-doped colored silica sol obtained was highly transparent and green, and no precipitate was generated. Furthermore, when a green laser pointer with a wavelength of 532 nm was irradiated, the Tyndall phenomenon was observed, and the dispersibility was good. The Ni-doped colored silica sol obtained had a pH of 9.4, a silica concentration of 3.1 mass%, an average particle size (D3) of 14 nm by dynamic light scattering, a Ni concentration of 0.031 mass% (310 mass ppm), and a mass ratio of Ni to silica (Ni / silica) of 0.0099. When the particles were observed with a TEM mode electron microscope, they were solid spherical particles. The electron microscope image is shown in Figure 1. The number-average particle size (D1) calculated from the electron microscope image of the particles by image analysis was 11.3 ± 2.4 nm.
[0186] Next, 2340 g of the Ni-doped colored silica sol was concentrated by pressure filtration with compressed air at room temperature under stirring using an ultrafiltration (UF) membrane with a molecular weight cutoff of 200,000, and 236 g of a highly transparent and green Ni-doped colored silica sol UF concentrate and 2104 g of a colorless and transparent UF filtrate were recovered. The appearance of this Ni-doped colored silica sol UF concentrate is shown in Figure 2. The UF concentrated solution of the obtained Ni-doped colored silica sol had a pH of 8.8, a silica concentration of 30.7 mass%, a Ni concentration of 0.29 mass% (2900 mass ppm), and a mass ratio of Ni to silica (Ni / silica) of 0.0095. The UF filtrate obtained during UF concentration had a pH of 9.1 and a Ni concentration of 0.0002 mass% (2 mass ppm). Since Ni was almost absent in the UF filtrate side and present in the UF concentrated solution side, it was confirmed that the colloidal silica particles were doped with Ni and colored. The obtained UF concentrated solution of Ni-doped colored silica sol was dried at 100°C in air to obtain a transparent green Ni-doped colored silica sol powder. The appearance of this Ni-doped colored silica sol powder is shown in Figure 3. The powder was then crushed in a mortar and the particle density PD was measured with a dry densitometer, which was 2.17 g / cm. 3 Similarly, when the crushed powder was measured by X-ray diffraction, the XRD pattern was broad, indicating that the powder was amorphous. The XRD pattern is shown in Figure 4.
[0187] Next, the UF concentrate of the Ni-doped colored silica sol obtained was contacted with a hydrogen-type strong acid cation exchange resin to obtain an acidic Ni-doped colored silica sol having a pH of 2.3 and a silica concentration of 24.0 mass%. This acidic Ni-doped colored silica sol was dried in air at 300°C for 1 hour to obtain a transparent green powder of acidic Cr-doped colored silica sol. Furthermore, the powder was crushed in a mortar and measured by nitrogen adsorption, and the specific surface area (SSA) was found to be 262 m 2 The BET particle size (D2) calculated by the nitrogen adsorption method using formula (1) was 10.6 nm, and the number-average particle size / BET particle size (D1 / D2) ratio was 1.07.
[0188] The obtained UF concentrated solution of Ni-doped colored silica sol was filtered through a nylon membrane filter with a pore size of 0.45 μm, and then the visible-ultraviolet spectrum of the UF concentrated solution of Ni-doped colored silica sol was measured using pure water as a control. As a result, absorption due to Ni was confirmed at wavelengths of 395 nm, 670 nm, and 750 nm. The visible-ultraviolet transmission spectrum and the visible-ultraviolet absorption spectrum are shown in Figure 5.
[0189] <Light resistance evaluation> The obtained Ni-doped colored silica sol was placed in a quartz cell with a lid and a light path length of 10 mm, and placed in a QUV accelerated weathering tester to evaluate light resistance. When the absorbance before UV irradiation was taken as 100%, the absorbance change rate after 100 hours, 250 hours, and 500 hours of UV irradiation at an absorption wavelength of 670 nm was 100%, 100%, and 100%, respectively. The results are shown in Table 2 and Figure 6.
[0190] [Comparative Example 1] 2,300 g of an aqueous solution of active silicic acid was prepared by the same procedure as in <Preparation of an aqueous solution of active silicic acid>.
[0191] <Production of Silica Sol> 10 g of a commercially available JIS No. 3 aqueous sodium silicate solution (silica concentration 28.8% by mass, Na2O concentration 9.5% by mass, silica / Na2O molar ratio 3.1) was added to 284 g of pure water and mixed uniformly to prepare 294 g of heel liquid with a silica concentration of 1.0% by mass, Na2O concentration 0.33% by mass, silica / Na2O molar ratio 3.1, and pH 11.0. No transition metal compound was added, and 2206 g of the aqueous activated silicic acid solution was used as the feed liquid. 294 g of the prepared heel liquid was charged into a 3 L glass reaction vessel equipped with a stirrer and a condenser, and the liquid temperature in the vessel was kept at 80° C. in an oil bath. Next, 2206 g of the feed liquid was continuously fed into the vessel under stirring at a constant rate over 360 minutes. During the course of the feed liquid feeding, the liquid temperature in the vessel was raised and changed to 100° C. for particle synthesis. After the feed liquid feeding was completed, the liquid temperature in the vessel was kept at 100° C. for 6 hours under stirring to obtain 2500 g of a silica sol granulation liquid.
[0192] The silica sol sieving liquid obtained was highly transparent and no sediment was generated. Furthermore, when a green laser pointer with a wavelength of 532 nm was irradiated, the Tyndall phenomenon was observed, and the dispersibility was good. Although a slight colloidal color was observed, the liquid was colorless and transparent and not colored. The silica sol sieving liquid obtained had a pH of 10.1, a silica concentration of 3.3 mass%, and an average particle size (D3) of 20 nm as determined by dynamic light scattering. The transition metal compounds were below the lower detection limit (less than 0.0001 mass%). When the particles were observed with a TEM mode electron microscope, they were solid spherical particles. The electron microscope image is shown in Figure 1. The number-average particle size (D1) calculated from the electron microscope image of the particles by image analysis was 12.5 ± 3.7 nm.
[0193] Next, 2300 g of the silica sol sized liquid obtained was concentrated by pressure filtration with compressed air at room temperature under stirring using an ultrafiltration (UF) membrane with a molecular weight cutoff of 200,000, and 265 g of a colorless and transparent silica sol UF concentrate and 2034 g of a colorless and transparent UF filtrate were recovered. The appearance of this silica sol UF concentrate is shown in Figure 2. The obtained UF concentrated solution of silica sol had a pH of 9.5 and a silica concentration of 28.6% by mass. The transition metal T was below the lower detection limit (less than 0.0001% by mass). No precipitate was observed in the UF concentrated solution of the obtained silica sol. Furthermore, when a green laser pointer with a wavelength of 532 nm was irradiated, the Tyndall phenomenon was observed, indicating good dispersibility. The UF filtrate obtained during UF concentration had a pH of 9.9. The transition metal T was below the detection limit (less than 0.0001% by mass). The obtained UF concentrated solution of silica sol was dried at 100°C in air to obtain a colorless and transparent silica sol powder. The appearance of this silica sol powder is shown in Figure 3. The powder was then crushed in a mortar and the particle density PD was measured using a dry density meter, which was 2.26 g / cm 3 Similarly, when this powder was measured by X-ray diffraction, the XRD pattern was broad, indicating that the powder was amorphous. The XRD pattern is shown in Figure 4.
[0194] The UF concentrate of the obtained silica sol was then contacted with a hydrogen-type strong acid cation exchange resin to obtain an acidic silica sol having a pH of 2.4 and a silica concentration of 24.1% by mass. This acidic silica sol was dried in air at 300°C for 1 hour to obtain a colorless and transparent acidic silica sol powder. Furthermore, the powder was crushed in a mortar and measured by nitrogen adsorption, and the specific surface area (SSA) was found to be 224 m 2 The BET particle size (D2) calculated by the nitrogen adsorption method using formula (1) was 11.9 nm, and the number-average particle size / BET particle size (D1 / D2) ratio was 1.05.
[0195] The UF concentrated silica sol was filtered through a nylon membrane filter with a pore size of 0.45 μm, and the visible-ultraviolet spectrum of the UF concentrated silica sol was measured using pure water as a control. As a result, in the measurement wavelength range of 250 nm to 800 nm, only absorption due to light scattering by colloidal silica particles with wavelengths of 400 nm or less was observed. The visible-ultraviolet transmission spectrum and visible-ultraviolet absorption spectrum are shown in Figure 5.
[0196] [Comparative Example 2] A red organic pigment dispersion (manufactured by TOKUSHIKI CORPORATION, product name MT-120 Red, pigment Pigment Violet 19, pigment concentration 15% by mass) was diluted with propylene glycol monomethyl ether (PGME) to a pigment concentration of 0.01% by mass to prepare a PGME-diluted red organic pigment dispersion. Note that the red organic pigment dispersion diluted with pure water was not suitable for lightfastness evaluation because the particles aggregated and sediment occurred. Using PGME as a control, the visible-ultraviolet spectrum of this PGME diluted red organic pigment dispersion was measured, and absorption was confirmed at wavelengths of 490 nm, 525 nm, and 560 nm. <Light resistance evaluation> This PGME diluted red organic pigment dispersion was placed in a quartz cell with a lid and an optical path length of 10 mm, and placed in a QUV accelerated weathering tester to evaluate light resistance. When the absorbance before UV irradiation was taken as 100%, the absorbance change rates after 100 hours, 250 hours, and 500 hours of UV irradiation at an absorption wavelength of 560 nm were 35%, 0.3%, and 0.2%, respectively. The results are shown in Table 3 and Figure 7.
[0197] [Comparative Example 3] A yellow organic pigment dispersion (manufactured by TOKUSHIKI CORPORATION, product name MT-150 Yellow, pigment Pigment Yellow 110, pigment concentration 15% by mass) was diluted with propylene glycol monomethyl ether (PGME) to a pigment concentration of 0.01% by mass to prepare a PGME-diluted yellow organic pigment dispersion. Note that the yellow organic pigment dispersion diluted with pure water was not suitable for lightfastness evaluation because the particles aggregated and sediment occurred. Using PGME as a control, the visible-ultraviolet spectrum of this PGME diluted yellow organic pigment dispersion was measured, and absorption was confirmed at wavelengths of 325 nm and 440 nm. <Light resistance evaluation> The PGME diluted yellow organic pigment dispersion was placed in a quartz cell with a lid and a light path length of 10 mm, and placed in a QUV accelerated weathering tester to evaluate light resistance. When the absorbance before UV irradiation was taken as 100%, the absorbance change rates after 100 hours, 250 hours, and 500 hours of UV irradiation at an absorption wavelength of 440 nm were 35%, 0.4%, and 0.4%, respectively. The results are shown in Table 3 and Figure 7.
[0198] [Comparative Example 4] A green organic pigment dispersion (manufactured by TOKUSHIKI CORPORATION, product name MT-160 Green, pigment Pigment Green 7, pigment concentration 25% by mass) was diluted with propylene glycol monomethyl ether (PGME) to a pigment concentration of 0.01% by mass to prepare a PGME-diluted green organic pigment dispersion. Note that the green organic pigment dispersion diluted with pure water was not suitable for lightfastness evaluation because the particles aggregated and sediment occurred. Using PGME as a control, the visible-ultraviolet spectrum of this PGME diluted green organic pigment dispersion was measured, and absorption was confirmed at wavelengths of 320 nm, 365 nm, and 650 nm. <Light resistance evaluation> This PGME diluted green organic pigment dispersion was placed in a quartz cell with a lid and an optical path length of 10 mm, and placed in a QUV accelerated weathering tester to evaluate light fastness. When the value before UV irradiation was taken as 100%, the absorbance change rates after 100 hours, 250 hours, and 500 hours of UV irradiation at an absorption wavelength of 650 nm were 74%, 33%, and 5%, respectively. The results are shown in Table 3 and Figure 7. The results are shown in Table 3 and Figure 7.
[0199] [Comparative Example 5] A blue organic pigment dispersion (manufactured by TOKUSHIKI CORPORATION, product name MT-170 Blue, pigment Pigment Blue 15, pigment concentration 15% by mass) was diluted with propylene glycol monomethyl ether (PGME) to a pigment concentration of 0.01% by mass to prepare a PGME-diluted blue organic pigment dispersion. Note that the blue organic pigment dispersion diluted with pure water was not suitable for lightfastness evaluation because the particles aggregated and precipitated. Using PGME as a control, the visible-ultraviolet spectrum of this PGME diluted blue organic pigment dispersion was measured, and absorption was confirmed at wavelengths of 345 nm, 630 nm, and 710 nm. <Light resistance evaluation> This PGME diluted blue organic pigment dispersion was placed in a quartz cell with a lid and a light path length of 10 mm, and placed in a QUV accelerated weathering tester to evaluate light resistance. When the absorbance before UV irradiation was taken as 100%, the absorbance change rates after 100 hours, 250 hours, and 500 hours of UV irradiation at an absorption wavelength of 630 nm were 77%, 31%, and 6%, respectively. The results are shown in Table 3 and Figure 7.
[0200] As shown in Table 3 and Figure 7, the organic pigments of Comparative Example 2 to Comparative Example 5 had an absorbance change rate of 0.2-6% after 500 hours of UV irradiation, and absorption almost disappeared, whereas the transition metal-doped colored silica sols of Examples 1 to 16 had an absorbance change rate of 64-100% after 500 hours of UV irradiation, as shown in Table 2 and Figure 6, which means that there was no decrease (100%) or only a decrease of about 40%, and it was clear that the transition metal-doped silica sol of the present invention has excellent light resistance. In particular, as shown in Examples 7 to 10 and 12, it was confirmed that light resistance was improved by forming a shell layer on the particle surface.
[0201] [Table 1]
[0202] [Table 2]
[0203] [Table 3]
[0204] [Comparative Example 6] To 10 g of the UF concentrated solution of the silica sol obtained in Comparative Example 1 (silica concentration: 28.6% by mass), 0.46 g of a 10% by mass CoSO4 aqueous solution was added under stirring so that the mass ratio of Co to silica (Co / silica) was 0.005. The silica nanoparticles aggregated, causing a precipitate to form, and then gelled.
[0205] [Comparative Example 7] To 10 g of the UF concentrated solution of the silica sol obtained in Comparative Example 1 (silica concentration: 28.6% by mass), 0.80 g of a 10% by mass Cr(NO3)3 aqueous solution was added under stirring so that the mass ratio of Cr to silica (Cr / silica) was 0.005, and gelation occurred immediately.
[0206] [Comparative Example 8] To 10 g of the UF concentrated solution of the silica sol obtained in Comparative Example 1 (silica concentration: 28.6% by mass), 0.48 g of a 10% by mass MnSO4 aqueous solution was added under stirring so that the mass ratio of Mn to silica (Mn / silica) was 0.005. The silica nanoparticles aggregated, generating a precipitate, which then gelled.
[0207] [Comparative Example 9] To 10 g of the UF concentrate of the silica sol obtained in Comparative Example 1 (silica concentration: 28.6% by mass), 0.44 g of a 10% by mass aqueous CuSO4 solution was added with stirring such that the mass ratio of Cu to silica (Cu / silica) was 0.005. As a result, the silica nanoparticles aggregated to form a precipitate, which then gelled.
[0208] [Comparative Example 10] To 10 g of the UF concentrate of the silica sol obtained in Comparative Example 1 (silica concentration: 28.6% by mass), 0.54 g of a 10% by mass aqueous NiSO4 solution was added with stirring such that the mass ratio of Ni to silica (Ni / silica) was 0.005. As a result, the silica nanoparticles aggregated to form a precipitate, which then gelled.
[0209] As shown in Comparative Examples 6 - 10, when a transition metal compound was added later to the silica sol obtained in Comparative Example 1 (without doping of the transition metal compound to the silica particles), the dispersion stability was low. The cationic transition metal ions constituting the transition metal compound added later aggregated the anionic silica particles contained in the silica sol, resulting in precipitation or gelation. On the other hand, in the transition metal-doped colored silica sols of Examples 1 - 16 described above, since the transition metal was mainly doped inside the silica particles, a high dispersion stability was obtained without aggregation, precipitation, or gelation.
[0210] [Example 17] <Production of a Pigment Composition Containing a Co-Doped Colored Silica Sol> The UF concentrate of the Co-doped colored silica sol obtained in Example 1 was dried at 100 °C in air and then heat-treated at 600 °C for 1 hour to obtain a transparent blue-violet powder of the Co-doped colored silica sol. Then, it was further pulverized in a mortar to form a powder. As a result of measuring this pulverized powder by X-ray diffraction, the XRD pattern was broad, indicating that the crystallinity of the powder was amorphous. 1 g of this pulverized powder was mixed with 4 g of a commercially available aqueous sodium silicate solution of JIS No. 3 to obtain a pigment composition. <Production of Colored Glass Containing a Co-Doped Colored Silica Sol> 0.5 g of the obtained pigment composition was used as a glaze, placed in a magnetic crucible, dried at 100 °C for 30 minutes, and then heat-treated at 1000 °C for 60 minutes to obtain a blue-violet colored glass.
[0211] [Comparative Example 11] 0.5 g of a commercially available aqueous sodium silicate solution of JIS No. 3 was used as a glaze, placed in a magnetic crucible, dried at 100 °C for 30 minutes, and then heat-treated at 1000 °C for 60 minutes to obtain a colorless and transparent glass.
[0212] [Example 18] [Production of a Pigment Composition Containing Co-Doped Colored Silica Sol] 2.7 g of a UF concentrate of the Co-doped colored silica sol obtained in Example 4 (silica concentration: 27.5% by mass), 2.1 g of an aqueous polyester-based urethane resin (trade name: Hydran HW-171, manufactured by DIC Corporation, solid content: 35% by mass), and 0.2 g of water were mixed to obtain 5.0 g of a pigment composition composed of a blue-violet dispersion having a silica concentration of 15% by mass, a solid content of the aqueous polyester-based urethane resin of 15% by mass, and a total solid content of 30% by mass in 100% by mass of the pigment composition. [Production of a Colored Film Containing Co-Doped Colored Silica Sol] 2 g of the obtained pigment composition was used as a paint, applied onto a blue plate glass substrate with a doctor blade, and heat-treated at 100 °C for 5 minutes to form a blue-violet transparent film. The appearance is shown in Fig. 8(a). The film was cut with a cutter, and the film thickness of the cross-section of the film was measured with a scanning electron microscope (SEM, manufactured by JEOL Ltd., trade name: JSM-6010LV). As a result, the film thickness was 14 μm. The SEM image is shown in Fig. 8(b). The visible-ultraviolet spectrum of the obtained film was measured with air as a control. As a result, absorption was confirmed at wavelengths of 525 nm, 580 nm, and 640 nm. The transmission spectrum is shown in Fig. 8(c).
[0213] [Comparative Example 12] 4.3 g of an aqueous polyester-based urethane resin (trade name: Hydran HW-171, manufactured by DIC Corporation, solid content: 35% by mass) and 0.7 g of water were mixed to obtain 5.0 g of a colorless and transparent pigment composition having a solid content of 30% by mass of the aqueous polyester-based urethane resin and a total solid content of 30% by mass in 100% by mass of the pigment composition. 2 g of the obtained pigment composition was used as a paint, applied onto a blue glass substrate with a doctor blade, and heat-treated at 100 °C for 5 minutes to form a colorless and transparent film.
[0214] [Example 19] <Production of Pigment Composition Containing Co-Doped Colored Silica Sol> 2.4 g of a UF concentrate of the Co-doped colored silica sol obtained in Example 3 (silica concentration: 30.9% by mass), 2.1 g of an aqueous polyester-based urethane resin (trade name: Hydran AP-40N, manufactured by DIC Corporation, solid content: 35% by mass), and 0.5 g of water were mixed to obtain 5.0 g of a pigment composition composed of a blue-violet dispersion having a silica concentration of 15% by mass, a solid content of the aqueous polyester-based urethane resin of 15% by mass, and a total solid content of 30% by mass in 100% by mass of the pigment composition. <Production of Colored Film Containing Co-Doped Colored Silica Sol> 3 g of the obtained pigment composition was used as a paint, applied onto a PET film with a thickness of 125 μm at a speed of 4 m / s with a bar coater to achieve a wet film thickness of 150 μm, and heat-treated at 100 °C for 5 minutes to form a blue-violet transparent film. When the film thickness was measured with a scanning electron microscope (SEM), it was 35 μm. The visible-ultraviolet spectrum of the obtained film was measured with air as a control. As a result, absorption was confirmed at wavelengths of 525 nm, 580 nm, and 640 nm.
[0215] [Comparative Example 13] 4.3 g of an aqueous polyester-based urethane resin (trade name: Hydran AP-40N, manufactured by DIC Corporation, solid content: 35% by mass) and 0.7 g of water were mixed to obtain 5.0 g of a colorless and transparent pigment composition having a solid content of 30% by mass of the aqueous polyester-based urethane resin and a total solid content of 30% by mass in 100% by mass of the pigment composition. 3 g of the obtained pigment composition was used as a paint and applied onto a PET film with a thickness of 125 μm at a speed of 4 m / s with a bar coater to obtain a wet film thickness of 150 μm, and then heat-treated at 100 °C for 5 minutes to form a colorless and transparent film. When the film thickness was measured with a scanning electron microscope (SEM), it was 34 μm.
[0216] [Example 20] <Production of a Pigment Composition Containing Co-Doped Colored Silica Sol> 2.4 g of a UF concentrate of the Co-doped colored silica sol obtained in Example 3 (silica concentration: 30.9% by mass), 2.1 g of an aqueous polyester-based urethane resin (trade name: Hydran AP-40N, manufactured by DIC Corporation, solid content: 35% by mass), and 0.5 g of water were mixed to obtain 5.0 g of a pigment composition composed of a blue-violet dispersion having a silica concentration of 15% by mass, a solid content of 15% by mass of the aqueous polyester-based urethane resin, and a total solid content of 30% by mass in 100% by mass of the pigment composition. <Production of a Molded Body Containing Co-Doped Colored Silica Sol> 3 g of the obtained pigment composition was placed in a Teflon (registered trademark) petri dish and dried at 60 °C for 24 hours to form a blue-violet transparent molded body. The appearance is shown in Fig. 9. When the thickness of the molded body was measured with a vernier caliper, it was 1 mm.
[0217] [Comparative Example 14] <Production of a Pigment Composition Containing Silica Sol> 2.6 g of a UF concentrate of the silica sol obtained in Comparative Example 1 (silica concentration: 28.6% by mass), 2.1 g of an aqueous polyester-based urethane resin (trade name: Hydran AP-40N, manufactured by DIC Corporation, solid content: 35% by mass), and 0.3 g of water were mixed to obtain 5.0 g of a pigment composition composed of a white dispersion having a silica concentration of 15% by mass, a solid content of 15% by mass of the aqueous polyester-based urethane resin, and a total solid content of 30% by mass in 100% by mass of the pigment composition. <Production of Molded Article Containing Silica Sol> 3 g of the obtained pigment composition was placed in a Teflon (registered trademark) petri dish and dried at 60° C. for 24 hours to form a colorless and transparent molded product. The appearance is shown in Figure 9. The thickness of the molded product was measured with a vernier caliper and found to be 1 mm.
[0218] [Comparative Example 15] 4.3 g of an aqueous polyester-based urethane resin (product name Hydran AP-40N, manufactured by DIC Corporation, solid content 35% by mass) and 0.7 g of water were mixed to obtain 5.0 g of a colorless and transparent pigment composition having a solid content of 30% by mass of the aqueous polyester-based urethane resin and a total solid content of 30% by mass in 100% by mass of the pigment composition. 3 g of the obtained pigment composition was placed in a Teflon (registered trademark) petri dish and dried at 60° C. for 24 hours to form a colorless and transparent molded product. The appearance is shown in Figure 9. The thickness of the molded product was measured with a vernier caliper and found to be 1 mm.
[0219] 9, the molded product obtained in Example 20 was colored, whereas the molded products obtained in Comparative Examples 14 and 15 were not colored. As described above, it has become clear that the transition metal-doped colored silica sol of the present invention has excellent colorability. [Industrial Applicability]
[0220] Examples of pigment compositions incorporating the transition metal-doped colored silica sol of the present invention include bicycles, motorbikes, automobiles, railroad vehicles, ships, aircraft, rockets, buildings, building materials, roofing materials, exterior wall materials, wall materials, flooring materials, ceiling materials, undercoats, signs, bulletin boards, signs, traffic lights, utility poles, electric wires, street lights, mailboxes, roads, bridges, window glass, glasswork, industrial electrical appliances, household electrical appliances, furniture, kitchen equipment, sanitary equipment, cooking utensils, tableware, containers, stationery, clothing, decorative items, etc. In particular, it is preferably used in applications requiring transparency and light resistance. In addition, a pigment composition containing the transition metal-doped colored silica sol of the present invention can be applied to glass and then heated and cooled, or added to glass raw materials and then melted, cooled, and vitrified, thereby producing colored glass. The pigment composition containing the transition metal-doped colored silica sol of the present invention can also be used in various other products for the purpose of coloring.< / ph>
Claims
1. A transition metal-doped colored silica sol, which satisfies the following (1) to (4): (1) the mass ratio of the transition metal T to silica (T / silica) is 0.0001 or more and 0.05 or less; (2) the number average particle diameter (D1) of the particles in the transition metal-doped colored silica sol calculated by image analysis of an electron microscope image is 5 nm or more and less than 50 nm; (3) the BET particle diameter (D2) of the particles in the transition metal-doped colored silica sol calculated by a nitrogen adsorption method is 5 nm or more and less than 50 nm; (4) The ratio of the number average particle size to the BET particle size (D1 / D2) is 1.5 or less.
2. 2. The transition metal-doped colored silica sol according to claim 1, wherein the transition metal T is one or more selected from the group consisting of V, Cr, Mn, Fe, Co, Ni, and Cu.
3. The transition metal-doped colored silica sol has a specific surface area (SSA) of 50 m2 or less of the particles in the transition metal-doped colored silica sol obtained by a nitrogen adsorption method. 2 / g or more, 550m 2 2. The transition metal-doped colored silica sol according to claim 1, wherein the transition metal doping ratio is 1:1 or less.
4. The transition metal-doped colored silica sol has a particle density PD of at least 2.10 g / cm 3 The transition metal-doped colored silica sol according to claim 1 .
5. 2. The transition metal-doped colored silica sol according to claim 1, wherein the dried powder obtained by drying the transition metal-doped colored silica sol at 100° C. in air is amorphous.
6. 2. The transition metal-doped colored silica sol according to claim 1, wherein the particles in the transition metal-doped colored silica sol are dispersed in an aqueous dispersion medium at a silica concentration of 1% by mass or more and 50% by mass or less.
7. 2. The transition metal-doped colored silica sol according to claim 1, wherein the average particle diameter (D3) of particles in the transition metal-doped colored silica sol is 5 nm or more and less than 100 nm as measured by a dynamic light scattering method.
8. 2. The transition metal-doped colored silica sol according to claim 1, wherein the transition metal T present in the dispersion medium of the transition metal-doped colored silica sol has an apparent concentration of less than 0.002 mass %.
9. The transition metal doped colored silica sol is UVA-340 lamp, UV irradiation intensity 0.89 W / m 2 Before and after the UV irradiation test under the conditions of a temperature of 50°C and an irradiation time of 500 hours, The rate of absorbance change at an absorption wavelength that causes coloring of the transition metal-doped colored silica sol, as determined by visible / ultraviolet spectrum analysis, is 50 to 100%, as represented by the following formula (3):
2. The transition metal-doped colored silica sol according to claim 1. Absorbance change rate (%) = [absorbance after UV irradiation / absorbance before UV irradiation] × 100 (3)
10. The following steps (a), (b), (c), (d) and (e); (a) contacting an aqueous alkali silicate solution with a cation exchange resin to prepare an aqueous activated silicic acid solution; (b) mixing one or more selected from an aqueous alkali silicate solution, an aqueous active silicic acid solution, an aqueous alkali solution, and a transition metal salt compound to prepare a heel liquid having a silica / alkali (molar ratio) of less than 30; (c) preparing a feed liquid comprising one or more kinds selected from an active silicic acid aqueous solution, a transition metal salt compound, and an alkaline aqueous solution; (d) adding the feed liquid to the heel liquid in the vessel while maintaining the heel liquid at 60° C. or more and 105° C. or less; a mass ratio of transition metal T to silica (T / silica) of 0.0001 or more and 0.05 or less, a number average particle diameter D1 calculated from an electron microscope image by image analysis method of 5 nm or more and less than 50 nm, a BET particle diameter D2 calculated from a nitrogen adsorption method of 5 nm or more and less than 50 nm, and a number average particle diameter / BET particle diameter (D1 / D2) ratio of 1.5 or less, A step of synthesizing a transition metal-doped colored silica sol, (e) (d) after the step, a step of maintaining the temperature at 60 ° C. or more and 105 ° C. or less for a certain period of time to obtain a sizing liquid; Including, provided that the transition metal salt compound is added during preparation of the heel solution, during preparation of the feed solution, or during preparation of both, and / or the transition metal salt compound is contained in at least one of the aqueous alkali silicate solution, the aqueous active silicic acid solution, and the aqueous alkali solution. A method for producing a transition metal doped colored silica sol.
11. 11. The method for producing a transition metal-doped colored silica sol according to claim 10, further comprising a step (f) of concentrating the transition metal-doped colored silica sol to obtain a concentrated liquid after the step (e).
12. 11. The method for producing a transition metal-doped colored silica sol according to claim 10, wherein the aqueous alkali silicate solution is one or more selected from the group consisting of an aqueous lithium silicate solution, an aqueous sodium silicate solution, and an aqueous potassium silicate solution.
13. 11. The method for producing a transition metal-doped colored silica sol according to claim 10, wherein the aqueous alkali solution is one or more selected from the group consisting of aqueous solutions of lithium hydroxide, sodium hydroxide, potassium hydroxide, and ammonia.
14. 11. The method for producing a transition metal-doped colored silica sol according to claim 10, wherein the metal of the transition metal salt compound is one or more selected from the group consisting of V, Cr, Mn, Fe, Co, Ni, and Cu.
15. The transition metal-doped colored silica sol has a specific surface area of 50 m2 or less of the particles in the transition metal-doped colored silica sol obtained by a nitrogen adsorption method. 2 / g or more, 550m 2 The method for producing a transition metal-doped colored silica sol according to claim 10, wherein the transition metal doping ratio is 1:1 or less.
16. The transition metal doped colored silica sol has a particle density of at least 2.10 g / cm 3 The method for producing a transition metal-doped colored silica sol according to claim 10,
17. 11. The method for producing a transition metal-doped colored silica sol according to claim 10, wherein the dried powder obtained by drying the transition metal-doped colored silica sol at 100° C. in air is amorphous.
18. The method for producing a transition metal-doped colored silica sol according to claim 10, characterized in that the particles in the transition metal-doped colored silica sol are dispersed in an aqueous dispersion medium at a silica concentration of 1% by mass or more and 50% by mass or less.
19. The method for producing a transition metal-doped colored silica sol according to claim 10, wherein the average particle diameter (D3) of particles in the transition metal-doped colored silica sol measured by dynamic light scattering method is 5 nm or more and less than 100 nm.
20. 11. The method for producing a transition metal-doped colored silica sol according to claim 10, wherein the transition metal T dissolved in the dispersion medium of the transition metal-doped colored silica sol has an apparent concentration of less than 0.002 mass%.
21. A pigment composition comprising at least the transition metal-doped colored silica sol according to any one of claims 1 to 9.
22. A paint, ink or glaze comprising at least the pigment composition according to claim 21.
23. A printed matter, a film or a molded article comprising at least the pigment composition according to claim 21.
Citation Information
Patent Citations
Silica gel containing foreign element
JP2003267720A
Silica gel carrying heteroelement
JP2005022896A
Silica gel carrying heteroelement
JP2005022897A
Hollow silica sol and hollow silica fine particle
JP2006342023A
Manufacturing method of slurry containing porous silica doped with metal
JP2021187732A