Method for manufacturing barrier-metal-free metal wiring structure, and barrier-metal-free metal wiring structure
By filling narrow wiring trenches with an intermetallic compound and using selective CMP to remove excess material, the method addresses the high resistivity issue of conventional copper wiring structures, achieving low resistance copper wiring without barrier metals.
Patent Information
- Application Number
- JP2020085049
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-14
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2040-05-14
AI Technical Summary
Conventional copper wiring structures with barrier metals exhibit high electrical resistivity due to the higher resistivity of barrier metals, making it difficult to achieve fine wiring with low resistance as the ratio of barrier metal increases with narrower widths.
A method for manufacturing a barrier metal-free metal wiring structure by filling narrow wiring trenches with an intermetallic compound, followed by chemical mechanical polishing (CMP) using selective polishing liquids to control the removal rates, ensuring no barrier metal is present in the narrow trenches.
This approach allows for the realization of low resistance wiring by eliminating the barrier metal in narrow trenches, achieving lower electrical resistivity than conventional copper and barrier metal combinations, particularly in wiring widths less than 7 nm.
Smart Images

Figure 0007572795000001 
Figure 0007572795000002 
Figure 0007572795000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a metal wiring structure for a semiconductor device or the like and a method for manufacturing the same, and more particularly to a metal wiring structure that does not contain a barrier metal and a method for manufacturing the same. [Background technology]
[0002] Copper (Cu) is commonly used as a wiring material. Copper is filled into wiring grooves formed in insulating layers such as oxide films by plating to form copper wiring. If copper is deposited directly on an insulating layer, it will diffuse into the insulating layer. Therefore, to prevent copper diffusion, a barrier metal layer is formed on the insulating layer, and copper is deposited on the barrier metal layer.
[0003] 11(a) and 11(b) are cross-sectional views showing an example of a conventional wiring structure. As shown in FIG. 11(a), a barrier metal 205 is deposited on an insulating layer (e.g., a silicon oxide film) 201 in which a wiring groove 200 is formed. A seed layer 207 that functions as a plating electrode is formed on the barrier metal 205. Copper 208 is further deposited on the seed layer 207 by plating. A part of the copper 208 is embedded in the wiring groove 200. Thereafter, the excess copper 208 and the seed layer 207, and a part of the insulating layer 201 are removed by CMP (chemical mechanical polishing), and a wiring made of the copper 208 and the seed layer 207 is formed as shown in FIG. 11(b).
[0004] 12(a) and 12(b) are cross-sectional views showing another example of a conventional wiring structure. As shown in FIG. 12(a), a barrier metal 205 is deposited on an insulating layer (e.g., a silicon oxide film) 201 in which a wiring groove 200 is formed. A seed layer 207 is deposited on the barrier metal 205, and the wiring groove 200 is filled with the seed layer 207. Copper 208 is further deposited on the seed layer 207. After that, the excess copper 208 and the seed layer 207, and a part of the insulating layer 201 are removed by CMP (chemical mechanical polishing), and a wiring made of the seed layer 207 is formed as shown in FIG. 12(b). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 2010-536175 Summary of the Invention [Problem to be solved by the invention]
[0006] However, as can be seen from Figures 11 and 12, as the wiring width becomes narrower, the ratio of barrier metal to the wiring metal increases. Because the electrical resistivity of barrier metal is much higher than that of copper, the resistance of the entire wiring increases. For these reasons, it has been difficult to realize fine wiring with low resistance.
[0007] Therefore, the present invention provides a method for manufacturing a low-resistance barrier-metal-free metal wiring structure, and also provides such a barrier-metal-free metal wiring structure. [Means for solving the problem]
[0008] In one embodiment, there is provided a method for manufacturing a barrier-metal-free metal wiring structure, comprising: depositing an intermetallic compound on an insulating layer in which a first wiring groove and a second wiring groove wider than the first wiring groove are formed, thereby filling at least the first wiring groove with the intermetallic compound; performing a planarization step of polishing the intermetallic compound until the insulating layer is exposed; and then performing a height adjustment step of polishing the intermetallic compound and the insulating layer until the height of the intermetallic compound in the first wiring groove reaches a predetermined height.
[0009] In one embodiment, the intermetallic compound is deposited on the insulating layer, thereby filling the first wiring trench and the second wiring trench with the intermetallic compound. In one embodiment, the planarization step is performed using a first polishing liquid having a removal rate selectivity ratio in which the removal rate of the intermetallic compound is higher than the removal rate of the insulating layer, and the height adjustment step is performed using a second polishing liquid having a removal rate selectivity ratio in which the removal rate of the intermetallic compound is the same as or lower than the removal rate of the insulating layer.
[0010] In one embodiment, the method further includes, after filling the first wiring trench with the intermetallic compound, depositing a second metal, different from the intermetallic compound, on the intermetallic compound to fill the second wiring trench with the second metal. In one embodiment, the planarization process is a process of polishing the second metal and the intermetallic compound until the insulating layer is exposed, and the height adjustment process is a process of polishing the second metal, the intermetallic compound, and the insulating layer until the height of the intermetallic compound in the first wiring groove reaches the predetermined height. In one embodiment, the planarization step is performed using a first polishing liquid having a removal rate selectivity ratio in which the removal rate of the second metal and the intermetallic compound is higher than the removal rate of the insulating layer, and the height adjustment step is performed using a second polishing liquid having a removal rate selectivity ratio in which the removal rate of the second metal and the intermetallic compound is the same as or lower than the removal rate of the insulating layer.
[0011] In one embodiment, the planarization step includes a first planarization step of polishing the second metal until the intermetallic compound is exposed, and a second planarization step of polishing the second metal and the intermetallic compound until the insulating layer is exposed. In one embodiment, the first planarization step is performed using a first polishing liquid having a removal rate selectivity ratio in which the removal rate of the second metal is higher than the removal rate of the intermetallic compound, the second planarization step is performed using a second polishing liquid having a removal rate selectivity ratio in which the removal rates of the second metal and the intermetallic compound are higher than the removal rate of the insulating layer, and the height adjustment step is performed using a third polishing liquid having a removal rate selectivity ratio in which the removal rates of the second metal and the intermetallic compound are the same as or lower than the removal rate of the insulating layer.
[0012] In one embodiment, the method further includes, after filling the first wiring trench with the intermetallic compound, forming a seed layer on the intermetallic compound and depositing a second metal, different from the intermetallic compound, on the seed layer to fill the second wiring trench with the second metal. In one embodiment, the planarization process is a process of polishing the second metal, the seed layer, and the intermetallic compound until the insulating layer is exposed, and the height adjustment process is a process of polishing the second metal, the seed layer, the intermetallic compound, and the insulating layer until the height of the intermetallic compound in the first wiring groove reaches the predetermined height. In one embodiment, the planarization step is performed using a first polishing liquid having a removal rate selectivity ratio in which the removal rates of the second metal, the seed layer, and the intermetallic compound are higher than the removal rate of the insulating layer, and the height adjustment step is performed using a second polishing liquid having a removal rate selectivity ratio in which the removal rates of the second metal, the seed layer, and the intermetallic compound are the same as or lower than the removal rate of the insulating layer.
[0013] In one embodiment, the planarization step includes a first planarization step of polishing the second metal and the seed layer until the intermetallic compound is exposed, and a second planarization step of polishing the second metal, the seed layer, and the intermetallic compound until the insulating layer is exposed. In one embodiment, the first planarization step is performed using a first polishing liquid in which the removal rates of the second metal and the seed layer have a higher removal rate selectivity than the removal rate of the intermetallic compound, the second planarization step is performed using a second polishing liquid in which the removal rates of the second metal, the seed layer, and the intermetallic compound have a higher removal rate selectivity than the removal rate of the insulating layer, and the height adjustment step is performed using a third polishing liquid in which the removal rates of the second metal, the seed layer, and the intermetallic compound have a removal rate selectivity that is the same as or lower than the removal rate of the insulating layer. In one embodiment, the intermetallic compound is CuAl 2 Or NiAl.
[0014] In one embodiment, a barrier-metal-free metal wiring structure is provided, comprising an insulating layer in which a first wiring trench and a second wiring trench wider than the first wiring trench are formed, and an intermetallic compound filling the first wiring trench.
[0015] In one embodiment, the barrier-metal-free metal wiring structure further comprises an intermetallic compound filling the second wiring trench. In one embodiment, the barrier-metal-free metal wiring structure further includes an intermetallic compound and a second metal filling the second wiring trench. In one embodiment, the second metal is copper, titanium, or titanium nitride. In one embodiment, the width of the first wiring trench is less than 7 nm. In one embodiment, the intermetallic compound filling the first wiring groove is CuAl 2 Or NiAl. Effect of the Invention
[0016] According to the present invention, the narrow first wiring trench is filled with the intermetallic compound, and no barrier metal is present in the first wiring trench, thereby realizing a low-resistance wiring made of the intermetallic compound in the first wiring trench. [Brief description of the drawings]
[0017] [Figure 1] 1(a) to 1(d) are diagrams illustrating one embodiment of a method for manufacturing a barrier-metal-free metal wiring structure. [Diagram 2] 1 is a graph showing the relationship between electrical resistivity and wiring width. [Diagram 3] 3(a) to 3(e) are diagrams illustrating another embodiment of a method for manufacturing a barrier-metal-free metal wiring structure. [Figure 4] 4(a) to 4(f) are diagrams illustrating still another embodiment of a method for manufacturing a barrier-metal-free metal wiring structure. [Diagram 5]5(a) to 5(d) are diagrams illustrating still another embodiment of the method for manufacturing a barrier-metal-free metal wiring structure. [Figure 6] Figures 6(a) and 6(b) are further explanatory diagrams of the embodiment shown in Figures 5(a) to 5(d). [Figure 7] 7(a) to 7(d) are diagrams illustrating still another embodiment of the method for manufacturing a barrier-metal-free metal wiring structure. [Figure 8] Figures 8(a) to 8(c) are further explanatory diagrams of the embodiment shown in Figures 7(a) to 7(d). [Figure 9] FIG. 1 is a schematic diagram showing a manufacturing system for manufacturing a barrier-metal-free metal wiring structure. [Figure 10] FIG. 10 is a perspective view showing a schematic view of the first CMP apparatus shown in FIG. [Figure 11] 11(a) and 11(b) are cross-sectional views showing an example of a conventional wiring structure. [Figure 12] 12(a) and 12(b) are cross-sectional views showing another example of a conventional wiring structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. 1(a) to 1(d) are diagrams for explaining one embodiment of a method for manufacturing a barrier-metal-free metal wiring structure. As shown in FIG. 1(a), an insulating layer 3 having a first wiring groove 1 and a second wiring groove 2 formed therein is prepared. The insulating layer 3 is formed on a workpiece such as a wafer, a substrate, or a panel. The material constituting the insulating layer 3 is, for example, silicon dioxide (SiO 2 ) and the insulating layer 3 is, for example, a silicon oxide film. The width W1 of the first wiring groove 1 is narrower than the width W2 of the second wiring groove 2, and in one embodiment, the width W1 of the first wiring groove 1 is smaller than 7 nm.
[0019] As shown in FIG. 1(b), an intermetallic compound 6 is deposited on the insulating layer 3. The first wiring groove 1 and the second wiring groove 2 are entirely filled with the intermetallic compound 6. There is no particular limitation on the method for depositing the intermetallic compound 6, but in this embodiment, sputtering is used. Specific examples of the intermetallic compound 6 include CuAl 2 , NiAl, etc. For example, CuAl 2 In one embodiment of a method for forming a CuAl by sputtering, a voltage is applied between a target made of copper (Cu) and aluminum (Al) and a workpiece while flowing an inert gas (typically argon gas). 2 is deposited on the insulating layer 3.
[0020] As shown in FIG. 1(c), a planarization step is performed in which the intermetallic compound 6 is polished until the insulating layer 3 is exposed. This planarization step is a CMP (chemical mechanical polishing) step, and is performed by a CMP device. More specifically, the intermetallic compound 6 is brought into sliding contact with a first polishing pad (not shown) while a first polishing liquid is supplied onto the first polishing pad. The intermetallic compound 6 is planarized by the chemical action of the first polishing liquid and the mechanical action of the abrasive grains contained in the first polishing liquid and / or the first polishing pad.
[0021] The first polishing liquid has a removal rate selectivity where the removal rate of the intermetallic compound 6 is higher than the removal rate of the insulating layer 3. The removal rate is the rate at which the thickness of a material is reduced per unit time. When the first polishing liquid having such a removal rate selectivity is used, the exposed surface of the insulating layer 3 functions as a polishing stopper. Thus, when the insulating layer 3 is exposed, the polishing of the intermetallic compound 6 can be substantially stopped. The planarization process may be performed while measuring the thickness of the intermetallic compound 6 with a film thickness sensor. Based on the measured value of the thickness of the intermetallic compound 6, the time when the insulating layer 3 is exposed can be estimated. The configuration of the film thickness sensor is not particularly limited, but for example, an eddy current sensor can be used as the film thickness sensor.
[0022] As shown in FIG. 1(d), after the planarization step, a height adjustment step is performed in which the intermetallic compound 6 and the insulating layer 3 are polished until the height of the intermetallic compound 6 in the first wiring groove 1 reaches a predetermined height. This height adjustment step is also a CMP (chemical mechanical polishing) step, and is performed by a CMP device. More specifically, the intermetallic compound 6 and the insulating layer 3 are brought into sliding contact with a second polishing pad (not shown) while a second polishing liquid is supplied onto the second polishing pad. The intermetallic compound 6 and the insulating layer 3 are polished by the chemical action of the second polishing liquid and the mechanical action of the abrasive grains contained in the second polishing liquid and / or the second polishing pad.
[0023] The height adjustment step is performed using a second polishing liquid having a removal rate selectivity such that the removal rate of the intermetallic compound 6 is equal to or lower than the removal rate of the insulating layer 3. Specifically, when dishing is expected to occur when polishing the intermetallic compound 6 in the second wiring groove 2, a second polishing liquid having a removal rate selectivity such that the removal rate of the intermetallic compound 6 is lower than the removal rate of the insulating layer 3 is used. On the other hand, when dishing is expected not to occur when polishing the intermetallic compound 6 in the second wiring groove 2, a second polishing liquid having a removal rate selectivity such that the removal rate of the intermetallic compound 6 is equal to the removal rate of the insulating layer 3 is used.
[0024] The height adjustment step is performed while measuring the height of the intermetallic compound 6 in the first wiring trench 1 (i.e., the wiring height) with the film thickness sensor. When the height of the intermetallic compound 6 in the first wiring trench 1 measured by the film thickness sensor reaches a predetermined height, the height adjustment step is stopped. In this manner, a barrier-metal-free metal wiring structure is manufactured.
[0025] As shown in Fig. 1(d), the barrier-metal-free metal wiring structure manufactured according to the above-mentioned method includes an insulating layer 3 in which a first wiring groove 1 and a second wiring groove 2 are formed, and an intermetallic compound 6 filling the first wiring groove 1 and the second wiring groove 2. The first wiring groove 1 having a small width is filled with the intermetallic compound 6, and no barrier metal exists in the first wiring groove 1. Therefore, a low-resistance wiring made of the intermetallic compound 6 in the first wiring groove 1 can be realized.
[0026] The intermetallic compound 6 used in this embodiment is CuAl 2 FIG. 2 is a graph showing the relationship between electrical resistivity and wiring width. As shown in FIG. 2, when the wiring width is small to a certain extent, the electrical resistivity of the intermetallic compound 6 is smaller than the electrical resistivity of the combination of copper, which is a conventional wiring material, and a barrier metal layer. In the graph shown in FIG. 2, when the wiring width is smaller than 7 nm, 2 The electrical resistivity of the intermetallic compound 6 made of copper is smaller than the electrical resistivity of a combination of copper and a barrier metal layer. Therefore, when the width of the first wiring groove 1 is smaller than 7 nm, the wiring made of the intermetallic compound 6 exhibits lower electrical efficiency than the conventional wiring made of copper and a barrier metal layer. From this viewpoint, the width of the first wiring groove 1 in this embodiment is set to be less than 7 nm.
[0027] On the other hand, the width of the second wiring groove 2 is 7 nm or more. In one embodiment, the width of the second wiring groove 2 may be 0.1 μm or more, or may be 1 μm or more. According to the graph shown in FIG. 2, when the wiring width is 7 nm or more, CuAl 2 Although the electrical resistivity of the second wiring groove 2 is larger than that of the combination of copper and a barrier metal layer, the electrical resistance is small because the cross-sectional area of the wiring is large. Therefore, the wiring in the second wiring groove 2 can have a low resistance, similar to the wiring in the first wiring groove 1.
[0028] 3(a) to 3(e) are diagrams for explaining another embodiment of the method for manufacturing a barrier-metal-free metal wiring structure. The configuration and steps of this embodiment that are not specifically explained are the same as those of the embodiment explained with reference to FIG. 1(a) to FIG. 1(d), so that the overlapping explanations will be omitted.
[0029] As shown in Fig. 3(a), an insulating layer 3 having a first wiring groove 1 and a second wiring groove 2 formed therein is prepared. Next, as shown in Fig. 3(b), an intermetallic compound 6 is deposited on the insulating layer 3. The first wiring groove 1 is entirely filled with the intermetallic compound 6, and a film of the intermetallic compound 6 is formed in the second wiring groove 2. The surface of the insulating layer 3 constituting the second wiring groove 2 is covered with the intermetallic compound 6, but the second wiring groove 2 is not entirely filled with the intermetallic compound 6.
[0030] After the first wiring groove 1 is filled with the intermetallic compound 6, a second metal 10 different from the intermetallic compound 6 is deposited on the intermetallic compound 6, and the second wiring groove 2 is filled with the second metal 10, as shown in FIG. 3(c). Examples of the second metal 10 include copper, titanium, titanium nitride, etc. The method for depositing the second metal 10 is not particularly limited, but electrolytic plating can be used, for example.
[0031] As shown in FIG. 3(d), a planarization step is performed in which the second metal 10 and the intermetallic compound 6 are polished until the insulating layer 3 is exposed. This planarization step is a CMP (chemical mechanical polishing) step, and is performed by a CMP device. More specifically, the second metal 10 and the intermetallic compound 6 are brought into sliding contact with the first polishing pad while a first polishing liquid is supplied onto the first polishing pad. The second metal 10 and the intermetallic compound 6 are planarized by the chemical action of the first polishing liquid and the mechanical action of the abrasive grains contained in the first polishing liquid and / or the first polishing pad. The first polishing liquid has a removal rate selectivity such that the removal rate of the second metal 10 and the intermetallic compound 6 is higher than the removal rate of the insulating layer 3.
[0032] As shown in FIG. 3(e), after the planarization step, a height adjustment step is performed in which the second metal 10, the intermetallic compound 6, and the insulating layer 3 are polished until the height of the intermetallic compound 6 in the first wiring groove 1 reaches a predetermined height. This height adjustment step is also a CMP (chemical mechanical polishing) step, and is performed by a CMP device. More specifically, the second metal 10, the intermetallic compound 6, and the insulating layer 3 are brought into sliding contact with the second polishing pad while a second polishing liquid is supplied onto the second polishing pad. The second metal 10, the intermetallic compound 6, and the insulating layer 3 are polished by the chemical action of the second polishing liquid and the mechanical action of the abrasive grains contained in the second polishing liquid and / or the second polishing pad.
[0033] The height adjustment step is performed using a second polishing liquid having a removal rate selectivity ratio in which the removal rate of the second metal 10 and the intermetallic compound 6 is the same as or lower than the removal rate of the insulating layer 3. Specifically, when dishing is expected to occur when polishing the second metal 10 and the intermetallic compound 6 in the second wiring groove 2, a second polishing liquid having a removal rate selectivity ratio in which the removal rate of the second metal 10 and the intermetallic compound 6 is lower than the removal rate of the insulating layer 3 is used. On the other hand, when dishing is expected not to occur when polishing the second metal 10 and the intermetallic compound 6 in the second wiring groove 2, a second polishing liquid having a removal rate selectivity ratio in which the removal rate of the second metal 10 and the intermetallic compound 6 is the same as the removal rate of the insulating layer 3 is used.
[0034] The height adjustment process is performed while measuring the height of the intermetallic compound 6 in the first wiring trench 1 (i.e., the wiring height) by the film thickness sensor. When the height of the intermetallic compound 6 in the first wiring trench 1 measured by the film thickness sensor reaches a predetermined height, the height adjustment process is stopped. In this manner, a barrier-metal-free metal wiring structure is manufactured. The narrow first wiring trench 1 is filled with the intermetallic compound 6, and no barrier metal is present in the first wiring trench 1. Therefore, a low-resistance wiring made of the intermetallic compound 6 in the first wiring trench 1 can be realized. The second wiring trench 2 is filled with the intermetallic compound 6 and the second metal 10, which form a wide wiring.
[0035] 4(a) to 4(f) are diagrams for explaining yet another embodiment of a method for manufacturing a barrier-metal-free metal wiring structure. The configuration and steps of this embodiment that are not specifically explained are the same as those of the embodiment explained with reference to FIG. 3(a) to FIG. 3(e), and therefore the overlapping explanations will be omitted.
[0036] The steps shown in FIG. 4(a) to FIG. 4(c) are the same as the steps shown in FIG. 3(a) to FIG. 3(c). As shown in FIG. 4(d), a first planarization step is performed in which the second metal 10 is polished until the intermetallic compound 6 is exposed. More specifically, the second metal 10 is brought into sliding contact with the first polishing pad while a first polishing liquid is supplied onto the first polishing pad. The second metal 10 is planarized by the chemical action of the first polishing liquid and the mechanical action of the abrasive grains contained in the first polishing liquid and / or the first polishing pad. The first polishing liquid has a removal rate selectivity ratio in which the removal rate of the second metal 10 is higher than the removal rate of the intermetallic compound 6. Therefore, the intermetallic compound 6 functions as a polishing stopper.
[0037] As shown in FIG. 4(e), the second planarization step is performed after the first planarization step. In this second planarization step, the second metal 10 and the intermetallic compound 6 are polished until the insulating layer 3 is exposed. More specifically, the second metal 10 and the intermetallic compound 6 are brought into sliding contact with the second polishing pad while supplying a second polishing liquid onto the second polishing pad. The second metal 10 and the intermetallic compound 6 are planarized by the chemical action of the second polishing liquid and the mechanical action of the abrasive grains contained in the second polishing liquid and / or the second polishing pad. The second polishing liquid has a removal rate selectivity ratio in which the removal rate of the second metal 10 and the intermetallic compound 6 is higher than the removal rate of the insulating layer 3. Therefore, the insulating layer 3 functions as a polishing stopper.
[0038] As shown in FIG. 4(f), after the second planarization step, a height adjustment step is performed in which the second metal 10, the intermetallic compound 6, and the insulating layer 3 are polished until the height of the intermetallic compound 6 in the first wiring groove 1 reaches a predetermined height. More specifically, the second metal 10, the intermetallic compound 6, and the insulating layer 3 are brought into sliding contact with the third polishing pad while a third polishing liquid is supplied onto the third polishing pad. The second metal 10, the intermetallic compound 6, and the insulating layer 3 are polished by the chemical action of the third polishing liquid and the mechanical action of the abrasive grains contained in the third polishing liquid and / or the third polishing pad.
[0039] The height adjustment step is performed using a third polishing liquid having a removal rate selectivity ratio in which the removal rate of the second metal 10 and the intermetallic compound 6 is the same as or lower than the removal rate of the insulating layer 3. Specifically, when dishing is expected to occur when polishing the second metal 10 and the intermetallic compound 6 in the second wiring groove 2, a third polishing liquid having a removal rate selectivity ratio in which the removal rate of the second metal 10 and the intermetallic compound 6 is lower than the removal rate of the insulating layer 3 is used. On the other hand, when dishing is expected not to occur when polishing the second metal 10 and the intermetallic compound 6 in the second wiring groove 2, a third polishing liquid having a removal rate selectivity ratio in which the removal rate of the second metal 10 and the intermetallic compound 6 is the same as the removal rate of the insulating layer 3 is used.
[0040] 5(a) to 5(d) and 6(a) and 6(b) are diagrams for explaining yet another embodiment of a method for manufacturing a barrier-metal-free metal wiring structure. The configuration and steps of this embodiment that are not specifically explained are the same as those of the embodiment explained with reference to Figs. 1(a) to 1(d), and therefore the overlapping explanations will be omitted.
[0041] As shown in Fig. 5(a), an insulating layer 3 having a first wiring groove 1 and a second wiring groove 2 formed therein is prepared. Next, as shown in Fig. 5(b), an intermetallic compound 6 is deposited on the insulating layer 3. The first wiring groove 1 is entirely filled with the intermetallic compound 6, and a film of the intermetallic compound 6 is formed in the second wiring groove 2. The surface of the insulating layer 3 constituting the second wiring groove 2 is covered with the intermetallic compound 6, but the second wiring groove 2 is not entirely filled with the intermetallic compound 6.
[0042] After the first wiring groove 1 is filled with the intermetallic compound 6, a seed layer 12 is formed on the intermetallic compound 6 as shown in FIG. 5(c). The seed layer 12 functions as an electrode for the subsequent electrolytic plating. The seed layer 12 is made of, for example, copper. The seed layer 12 can be formed by electroless plating, sputtering, or the like.
[0043] 5(d), a second metal 10 different from the intermetallic compound 6 is deposited on the seed layer 12, and the second wiring trench 2 is filled with the second metal 10. Examples of the second metal 10 include copper, titanium, titanium nitride, etc. In this embodiment, copper is used as the second metal 10, and electrolytic plating is used as a method for forming the second metal 10.
[0044] As shown in FIG. 6(a), a planarization process is performed in which the second metal 10, the seed layer 12, and the intermetallic compound 6 are polished until the insulating layer 3 is exposed. This planarization process is a CMP (chemical mechanical polishing) process, and is performed by a CMP device. More specifically, the second metal 10, the seed layer 12, and the intermetallic compound 6 are brought into sliding contact with the first polishing pad while a first polishing liquid is supplied onto the first polishing pad. The second metal 10, the seed layer 12, and the intermetallic compound 6 are planarized by the chemical action of the first polishing liquid and the mechanical action of the abrasive grains contained in the first polishing liquid and / or the first polishing pad. The first polishing liquid has a removal rate selectivity ratio in which the removal rate of the second metal 10, the seed layer 12, and the intermetallic compound 6 is higher than the removal rate of the insulating layer 3. Therefore, the insulating layer 3 functions as a polishing stopper.
[0045] As shown in FIG. 6(b), after the planarization step, a height adjustment step is performed in which the second metal 10, the seed layer 12, the intermetallic compound 6, and the insulating layer 3 are polished until the height of the intermetallic compound 6 in the first wiring groove 1 reaches a predetermined height. This height adjustment step is also a CMP (chemical mechanical polishing) step, and is performed by a CMP device. More specifically, the second metal 10, the seed layer 12, the intermetallic compound 6, and the insulating layer 3 are brought into sliding contact with the second polishing pad while a second polishing liquid is supplied onto the second polishing pad. The second metal 10, the seed layer 12, the intermetallic compound 6, and the insulating layer 3 are polished by the chemical action of the second polishing liquid and the mechanical action of the abrasive grains contained in the second polishing liquid and / or the second polishing pad.
[0046] The height adjustment step is performed using a second polishing liquid having a removal rate selectivity such that the removal rate of the second metal 10, the seed layer 12, and the intermetallic compound 6 is the same as or lower than the removal rate of the insulating layer 3. Specifically, when dishing is expected to occur when polishing the second metal 10, the seed layer 12, and the intermetallic compound 6 in the second wiring groove 2, a second polishing liquid having a removal rate selectivity such that the removal rate of the second metal 10, the seed layer 12, and the intermetallic compound 6 is lower than the removal rate of the insulating layer 3 is used. On the other hand, when dishing is expected not to occur when polishing the second metal 10, the seed layer 12, and the intermetallic compound 6 in the second wiring groove 2, a second polishing liquid having a removal rate selectivity such that the removal rate of the second metal 10, the seed layer 12, and the intermetallic compound 6 is the same as the removal rate of the insulating layer 3 is used.
[0047] The height adjustment process is performed while measuring the height of the intermetallic compound 6 in the first wiring trench 1 (i.e., the wiring height) by the film thickness sensor. When the height of the intermetallic compound 6 in the first wiring trench 1 measured by the film thickness sensor reaches a predetermined height, the height adjustment process is stopped. In this manner, a barrier-metal-free metal wiring structure is manufactured. The narrow first wiring trench 1 is filled with the intermetallic compound 6, and no barrier metal is present in the first wiring trench 1. Therefore, a low-resistance wiring made of the intermetallic compound 6 in the first wiring trench 1 can be realized. The second wiring trench 2 is filled with the intermetallic compound 6, the second metal 10, and the seed layer 12, which form a wide wiring.
[0048] Figures 7(a) to 7(d) and 8(a) to 8(c) are diagrams for explaining yet another embodiment of a method for manufacturing a barrier-metal-free metal wiring structure. The configuration and steps of this embodiment that are not specifically explained are the same as those of the embodiment explained with reference to Figures 5(a) to 5(d) and Figures 6(a) and 6(b), and therefore the overlapping explanations will be omitted.
[0049] 7(a) to 7(d) are performed in the same manner as in FIG. 5(a) to FIG. 5(d). As shown in FIG. 8(a), a first planarization step is performed in which the second metal 10 and the seed layer 12 are polished until the intermetallic compound 6 is exposed. More specifically, the second metal 10 and the seed layer 12 are brought into sliding contact with the first polishing pad while a first polishing liquid is supplied onto the first polishing pad. The second metal 10 and the seed layer 12 are planarized by the chemical action of the first polishing liquid and the mechanical action of the abrasive grains contained in the first polishing liquid and / or the first polishing pad. The first polishing liquid has a removal rate selectivity ratio in which the removal rate of the second metal 10 and the seed layer 12 is higher than the removal rate of the intermetallic compound 6. Therefore, the intermetallic compound 6 functions as a polishing stopper.
[0050] As shown in FIG. 8(b), the second planarization step is performed after the first planarization step. In this second planarization step, the second metal 10, the seed layer 12, and the intermetallic compound 6 are polished until the insulating layer 3 is exposed. More specifically, the second metal 10, the seed layer 12, and the intermetallic compound 6 are brought into sliding contact with the second polishing pad while supplying the second polishing liquid onto the second polishing pad. The second metal 10, the seed layer 12, and the intermetallic compound 6 are planarized by the chemical action of the second polishing liquid and the mechanical action of the abrasive grains contained in the second polishing liquid and / or the second polishing pad. The second polishing liquid has a removal rate selectivity ratio in which the removal rate of the second metal 10, the seed layer 12, and the intermetallic compound 6 is higher than the removal rate of the insulating layer 3. Therefore, the insulating layer 3 functions as a polishing stopper.
[0051] As shown in FIG. 8(c), after the second planarization step, a height adjustment step is performed in which the second metal 10, the seed layer 12, the intermetallic compound 6, and the insulating layer 3 are polished until the height of the intermetallic compound 6 in the first wiring groove 1 reaches a predetermined height. More specifically, the second metal 10, the seed layer 12, the intermetallic compound 6, and the insulating layer 3 are brought into sliding contact with the third polishing pad while a third polishing liquid is supplied onto the third polishing pad. The second metal 10, the seed layer 12, the intermetallic compound 6, and the insulating layer 3 are polished by the chemical action of the third polishing liquid and the mechanical action of the abrasive grains contained in the third polishing liquid and / or the third polishing pad.
[0052] The height adjustment step is performed using a third polishing liquid having a removal rate selectivity such that the removal rate of the second metal 10, the seed layer 12, and the intermetallic compound 6 is equal to or lower than the removal rate of the insulating layer 3. Specifically, when dishing is expected to occur when polishing the second metal 10, the seed layer 12, and the intermetallic compound 6 in the second wiring groove 2, a third polishing liquid having a removal rate selectivity such that the removal rate of the second metal 10, the seed layer 12, and the intermetallic compound 6 is lower than the removal rate of the insulating layer 3 is used. On the other hand, when dishing is expected not to occur when polishing the second metal 10, the seed layer 12, and the intermetallic compound 6 in the second wiring groove 2, a third polishing liquid having a removal rate selectivity such that the removal rate of the second metal 10, the seed layer 12, and the intermetallic compound 6 is equal to the removal rate of the insulating layer 3 is used.
[0053] According to each of the above-mentioned embodiments, the wiring in the narrow first wiring trench 1 is composed only of the intermetallic compound 6. Therefore, a barrier metal-free metal wiring structure can be realized.
[0054] 9 is a schematic diagram showing a manufacturing system for manufacturing the above-mentioned barrier-metal-free metal wiring structure. The manufacturing system includes a sputtering device 20 for forming an intermetallic compound 6, a plating device 22 for forming a second metal 10, a film forming device 23 for forming a seed layer 12, a plurality of CMP devices (chemical mechanical polishing devices) 24, 25, 26, a cleaning device 31 for cleaning the polished workpiece, a drying device 33 for drying the cleaned workpiece, and a transport device 35 for transporting the workpiece. The metal wiring structure is formed on a workpiece such as a wafer, a substrate, or a panel.
[0055] The configuration of the manufacturing system shown in Fig. 9 is an example, and may be appropriately changed based on the metal wiring structure to be manufactured. For example, in the embodiment described with reference to Fig. 1(a) to Fig. 1(d), the second metal 10 and the seed layer 12 may not be formed. In such a case, the plating device 22 and the film forming device 23 may be omitted. The manufacturing system shown in Fig. 9 includes three CMP devices 24, 25, and 26, but may include only two CMP devices 24 and 25 when only two types of polishing liquid are used.
[0056] The first CMP apparatus 24, the second CMP apparatus 25, and the third CMP apparatus 26 basically have the same configuration. Therefore, the first CMP apparatus 24 will be described below with reference to Fig. 10. As shown in Fig. 10, the first CMP apparatus 24 includes a first polishing table 41 that supports a first polishing pad 40, a first polishing head 42 that presses a workpiece W against the first polishing pad 40, a first table motor 44 that rotates the first polishing table 41, and a first polishing liquid supply nozzle 45 for supplying a first polishing liquid onto the first polishing pad 40. The upper surface of the first polishing pad 40 constitutes a polishing surface 40a that polishes the workpiece W.
[0057] The first polishing head 42 is connected to a head shaft 48, and the head shaft 48 is connected to a first polishing head motor (not shown). The first polishing head motor rotates the first polishing head 42 together with the head shaft 48 in the direction indicated by the arrow. The first polishing table 41 is connected to a first table motor 44, and the first table motor 44 is configured to rotate the first polishing table 41 and the first polishing pad 40 in the direction indicated by the arrow.
[0058] The workpiece W is polished as follows. While the first polishing table 41 and the first polishing head 42 are rotated in the direction indicated by the arrows in Fig. 10, a first polishing liquid is supplied from a first polishing liquid supply nozzle 45 to the polishing surface 40a of the first polishing pad 40 on the first polishing table 41. While the workpiece W is rotated by the first polishing head 42, the workpiece W is pressed against the polishing surface 40a of the first polishing pad 40 by the first polishing head 42 with the first polishing liquid present on the first polishing pad 40. The metal wiring structure formed on the workpiece W is polished by the chemical action of the first polishing liquid and the mechanical action of the abrasive grains contained in the first polishing liquid and / or the first polishing pad 40.
[0059] The first CMP device 24 is equipped with a first film thickness sensor 50 for measuring the film thickness of the metal wiring structure formed on the workpiece W. The configuration of the first film thickness sensor 50 is not particularly limited, but an eddy current sensor is used in this embodiment. The first film thickness sensor 50 is attached to the first polishing table 41 and rotates together with the first polishing table 41 and the first polishing pad 40. The position of the first film thickness sensor 50 is a position where the first polishing table 41 and the first polishing pad 40 cross the surface of the workpiece W on the first polishing pad 40 every time the first polishing table 41 and the first polishing pad 40 rotate once. The thickness of the intermetallic compound 6 formed on the workpiece W is measured by the first film thickness sensor 50.
[0060] Although not shown, the second CMP apparatus 25 includes a second polishing table supporting a second polishing pad, a second polishing head pressing the workpiece W against the second polishing pad, a second table motor rotating the second polishing table, a second polishing liquid supply nozzle for supplying a second polishing liquid onto the second polishing pad, and a second film thickness sensor for measuring the film thickness of the workpiece W. Similarly, the third CMP apparatus 26 includes a third polishing table supporting a third polishing pad, a third polishing head pressing the workpiece W against the third polishing pad, a third table motor rotating the third polishing table, a third polishing liquid supply nozzle for supplying a third polishing liquid onto the third polishing pad, and a third film thickness sensor for measuring the film thickness of the workpiece W. The third CMP apparatus 26 may not be provided.
[0061] The cleaning device 31 is configured to clean the workpiece W polished by the CMP devices 24, 25, 26. In this embodiment, the cleaning device 31 is a roll cleaner that scrubs both sides of the workpiece W with a roll scrubber while supplying a cleaning liquid to the workpiece W. In one embodiment, the cleaning device 31 may be a pen sponge cleaner that scrubs one side of the workpiece W with a pen sponge while supplying a cleaning liquid to the workpiece W.
[0062] The drying device 33 is configured to dry the workpiece W cleaned by the cleaning device 31. In this embodiment, the drying device 33 is an IPA drying device that supplies isopropyl alcohol to the workpiece W while rotating the workpiece W. In one embodiment, the drying device 33 may be a spin drying device that rotates the workpiece W at a high speed.
[0063] The transport apparatus 35 is configured to transport workpieces between the CMP apparatuses 24 , 25 , 26 , the cleaning apparatus 31 , and the drying apparatus 33 .
[0064] The film forming apparatus 23 for forming the seed layer 12 is composed of a sputtering apparatus, an electroless plating apparatus, a PVD apparatus, a CVD apparatus, etc. When manufacturing a metal wiring structure without the seed layer 12, the film forming apparatus 23 may be omitted.
[0065] The above-described embodiments have been described for the purpose of enabling a person having ordinary skill in the art to practice the present invention. Various modifications of the above-described embodiments are naturally possible for a person skilled in the art, and the technical idea of the present invention can be applied to other embodiments. Therefore, the present invention is not limited to the described embodiments, but is to be interpreted in the broadest scope according to the technical idea defined by the claims. [Explanation of symbols]
[0066] 1 1st wiring groove 2 2nd wiring groove 3. Insulation layer 6 Intermetallic compounds 10 Second metal 12 Seed layer 20 Sputtering Equipment 22 Plating equipment 23 Film deposition equipment 24,25,26 CMP equipment (chemical mechanical polishing equipment) 31 Cleaning Equipment 33 Drying equipment 35 Transport equipment 40 First Polishing Pad 41 First Polishing Table 42 No. 1 Polishing Head 44 First table motor 45 First polishing liquid supply nozzle 48 Head Shaft 50 First film thickness sensor
Claims
1. A method for manufacturing a barrier-metal-free metal interconnect structure, comprising: depositing an intermetallic compound on an insulating layer in which a first wiring groove having a width smaller than 7 nm and a second wiring groove wider than the first wiring groove are formed, thereby filling the first wiring groove with the intermetallic compound, the intermetallic compound being CuAl 2 or NiAl; After filling the first wiring trench with the intermetallic compound, a second metal different from the intermetallic compound is deposited on the intermetallic compound to fill the second wiring trench with the second metal; A planarization step is performed in which the second metal and the intermetallic compound are polished until the insulating layer is exposed, and then performing a height adjustment step of polishing the second metal, the intermetallic compound, and the insulating layer until a height of the intermetallic compound in the first wiring trench reaches a predetermined height.
2. the planarization step is performed using a first polishing liquid having a removal rate selectivity ratio in which the removal rate of the second metal and the intermetallic compound is higher than the removal rate of the insulating layer; 2. The method of claim 1, wherein the height adjustment step is performed using a second polishing liquid having a removal rate selectivity ratio in which the removal rate of the second metal and the intermetallic compound is equal to or lower than the removal rate of the insulating layer.
3. The planarization step includes: a first planarization step of polishing the second metal until the intermetallic compound is exposed; 2. The method of claim 1, further comprising a second planarization step of polishing said second metal and said intermetallic compound until said insulating layer is exposed.
4. the first planarization step is performed using a first polishing liquid having a removal rate selectivity ratio in which the removal rate of the second metal is higher than the removal rate of the intermetallic compound; the second planarization step is performed using a second polishing liquid having a removal rate selectivity ratio in which the removal rate of the second metal and the intermetallic compound is higher than the removal rate of the insulating layer; 4. The method of claim 3, wherein the height adjustment step is performed using a third polishing liquid having a removal rate selectivity ratio in which the removal rate of the second metal and the intermetallic compound is equal to or lower than the removal rate of the insulating layer.
5. A method for manufacturing a barrier-metal-free metal interconnect structure, comprising: depositing an intermetallic compound on an insulating layer in which a first wiring groove having a width smaller than 7 nm and a second wiring groove wider than the first wiring groove are formed, thereby filling the first wiring groove with the intermetallic compound, the intermetallic compound being CuAl 2 or NiAl; forming a seed layer on the intermetallic compound after filling the first wiring trench with the intermetallic compound; depositing a second metal different from the intermetallic compound on the seed layer to fill the second wiring trench with the second metal; a planarization step of polishing the second metal, the seed layer, and the intermetallic compound until the insulating layer is exposed; and performing a height adjustment step of polishing the second metal, the seed layer, the intermetallic compound, and the insulating layer until a height of the intermetallic compound in the first wiring trench reaches a predetermined height.
6. the planarization step is performed using a first polishing solution having a removal rate selectivity that is higher than a removal rate of the second metal, the seed layer, and the intermetallic compound than a removal rate of the insulating layer; 6. The method of claim 5, wherein the height adjustment step is performed using a second polishing fluid having a removal rate selectivity ratio in which the removal rates of the second metal, the seed layer, and the intermetallic compound are equal to or lower than a removal rate of the insulating layer.
7. The planarization step includes: a first planarization step of polishing the second metal and the seed layer until the intermetallic compound is exposed; 6. The method of claim 5, further comprising a second planarization step of polishing the second metal, the seed layer, and the intermetallic compound until the insulating layer is exposed.
8. the first planarization step is performed using a first polishing solution having a removal rate selectivity ratio in which the removal rates of the second metal and the seed layer are higher than the removal rate of the intermetallic compound; the second planarization step is performed using a second polishing solution having a removal rate selectivity ratio in which the removal rate of the second metal, the seed layer, and the intermetallic compound is higher than the removal rate of the insulating layer; 8. The method of claim 7, wherein the height adjustment step is performed using a third polishing liquid having a removal rate selectivity ratio in which the removal rates of the second metal, the seed layer, and the intermetallic compound are equal to or lower than a removal rate of the insulating layer.
9. An insulating layer in which a first wiring groove having a width smaller than 7 nm and a second wiring groove having a width wider than the first wiring groove are formed; an intermetallic compound filling the first wiring groove; A barrier-metal-free metal wiring structure comprising an intermetallic compound and a second metal filling the second wiring trench, the intermetallic compound being CuAl 2 or NiAl.
10. 10. The barrier-metal-free metal wiring structure of claim 9, wherein the second metal is copper, titanium, or titanium nitride.
Citation Information
Patent Citations
Method for manufacturing semiconductor device
JP2007081113A
Wiring of semiconductor device, and method of forming wiring of semiconductor device
JP2008270545A
Intermetallic compound conductors
JP2010536175A
Method of manufacturing semiconductor device
JP2012253121A
Wiring structure and semiconductor device
JP2019212892A