Release agent composition and release film
A release agent composition using a polyester resin and (meth)acrylic copolymer with a block structure addresses silicone migration and peel force issues, providing a release layer with low peeling force, high residual adhesion, and improved abrasion resistance for electrical components.
Patent Information
- Application Number
- JP2020111203
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-29
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2040-06-29
AI Technical Summary
Release films using silicone resins face issues with silicone compound migration, leading to conductivity problems in electrical components and high peel forces, along with low residual adhesion rates and abrasion resistance in release layers formed from (meth)acrylic polymers with long-chain alkyl groups.
A release agent composition comprising a polyester resin, a (meth)acrylic copolymer with a block structure, and a crosslinking agent, where the copolymer segregates to the surface during curing, forming a release layer with low peeling force, improved residual adhesion, and enhanced abrasion resistance.
The composition forms a release layer with reduced silicone migration, ensuring low peeling force, high residual adhesion, and excellent appearance and strength, suitable for electrical components without conductivity issues.
Smart Images

Figure 0007572799000001 
Figure 0007572799000002 
Figure 0007572799000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a release agent composition and a release film. [Background technology]
[0002] Electrical components such as semiconductors, various connectors, capacitors, resistors, printed wiring boards, etc. are widely used in various products, and adhesive films are attached to these electrical components for the purpose of temporary fixing during assembly, etc. A release film is used for the adhesive film to protect the surface of the adhesive layer that comes into contact with the adherend (hereinafter sometimes referred to as the "adhesive surface").
[0003] The release film comprises a substrate and a release layer laminated on at least one side of the substrate, and the surface of the release layer opposite to the substrate (hereinafter sometimes referred to as "release surface") is laminated on the adhesive surface of the adhesive film. The release film is also used when producing an adhesive film. For example, an adhesive layer is formed by applying an adhesive composition onto the release surface of the release film and drying the resulting coating. Subsequently, an adhesive film with a release film can be produced by laminating a substrate for the adhesive film on the surface of the adhesive layer opposite to the release film. It is also used in the production of a so-called non-carrier adhesive film in which release films are arranged on both sides of the adhesive layer.
[0004] In such a release film, a silicone resin is usually used in the release layer to reduce the release force. However, in a release film using a silicone resin, silicone compounds such as low molecular weight silicone resin and silicone oil in the release layer may migrate to the adhesive layer. In addition, the release film is wound into a roll after production, and at this time, the silicone compounds may also migrate to the back surface of the release film. The silicone compounds that have migrated to the back surface of the release film may further migrate to the adhesive film substrate when the release film is applied to the adhesive film and then wound into a roll. When the adhesive film is peeled off from the release sheet and applied to an electrical component, the silicone compounds that have migrated to the adhesive layer or adhesive film substrate may gradually vaporize after application and accumulate near the electrical contacts of the electronic components, causing electrical component conduction defects.
[0005] As a release agent that solves the problem of poor conduction caused by silicone compounds, so-called non-silicone release agents that do not contain silicone compounds are known. For example, Patent Document 1 describes a long-chain alkyl release agent having 12 or more carbon atoms. In addition, Patent Document 2 proposes a release agent composition that contains a polyester resin, a (meth)acrylic polymer having a long-chain alkyl group having 12 to 16 carbon atoms, and a crosslinking agent. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2005-23255 A [Patent Document 2] International Publication No. 2012 / 020673 Summary of the Invention [Problem to be solved by the invention]
[0007] The release agent using the (meth)acrylic polymer having a long-chain alkyl group does not contain a silicone compound, and therefore the problem of poor electrical conduction caused by the silicone compound is eliminated. However, the release layer formed from the release agent using the (meth)acrylic polymer having a long-chain alkyl group tends to have a high peeling force, and the release agent is likely to migrate, which tends to reduce the residual adhesion rate. In addition, the release agent using the (meth)acrylic polymer having a long-chain alkyl group tends to cause unevenness in the release layer formed, and has low abrasion resistance.
[0008] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a release agent composition that has a small peel strength, can suppress a decrease in the residual adhesion rate, and can form a release layer that is excellent in appearance and strength (abrasion resistance). [Means for solving the problem]
[0009] The release agent composition of the present invention, which has been able to solve the above problems, contains a polyester resin, a (meth)acrylic copolymer, and a crosslinking agent, and is characterized in that the (meth)acrylic copolymer is a block copolymer having an A block having a structural unit represented by general formula (1) and a B block having a structural unit derived from a vinyl monomer having a reactive functional group.
[0010] [ka] [In formula (1), R 11 R represents an alkyl group having 17 to 28 carbon atoms. 12 represents a hydrogen atom or a methyl group. Effect of the Invention
[0011] Use of the release agent composition of the present invention makes it possible to form a release layer that has a small peel strength, is capable of suppressing a decrease in the residual adhesion rate, and is excellent in appearance and strength (abrasion resistance). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, a preferred embodiment of the present invention will be described. However, the following embodiment is merely an example, and the present invention is not limited to the following embodiment.
[0013] <1. Stripping agent composition> The release agent composition of the present invention contains a polyester resin, a (meth)acrylic copolymer, and a crosslinking agent. The release layer formed by curing (crosslinking reaction) the release agent composition has components derived from the copolymer segregated near its surface (release surface). The segregation is considered to occur because the molecular structure, molecular polarity, etc. of the copolymer are different from those of the polyester resin, and are pushed up to the surface of the release layer before the release layer is cured (crosslinked reaction). Since the copolymer pushed up to the surface is a block copolymer, a crosslinked structure can be efficiently formed uniformly near the surface of the polyester resin, and further, the alkyl chains of the copolymer (R 11 It is believed that the cations of the groups represented by the formula (I) are oriented to the surface.
[0014] Each component of the release agent composition is described below. In this specification, "(meth)acrylic" means "at least one of acrylic and methacrylic". "(meth)acrylate" means "at least one of acrylate and methacrylate". "(meth)acryloyl" means "at least one of acryloyl and methacryloyl". "Vinyl monomer" means a monomer having a radically polymerizable carbon-carbon double bond in the molecule, and "(meth)acrylic monomer" is also included in "vinyl monomer". "Structural unit derived from vinyl monomer" means a structural unit in which the radically polymerizable carbon-carbon double bond of a vinyl monomer is polymerized to become a carbon-carbon single bond. "Structural unit derived from (meth)acrylic monomer" means a structural unit in which the radically polymerizable carbon-carbon double bond of a (meth)acrylic monomer is polymerized to become a carbon-carbon single bond. "~" in the numerical range means greater than or equal to and less than or equal to, that is, α~β means greater than or equal to α and less than or equal to β.
[0015] (1-1. Polyester resin) The polyester resin is not particularly limited, and can be appropriately selected from known polyester resins known for paints. The polyester resin is preferably one obtained by a condensation reaction between a polyhydric alcohol and a polybasic acid, and a linear polyester resin is preferable. The polyester resin includes a non-convertible polyester resin which is a condensate of a dibasic acid and a dihydric alcohol or modified with a non-drying oil fatty acid, and a convertible polyester resin which is a condensate of a dibasic acid and a trihydric or higher alcohol. The polyester resin may be used alone or in combination of two or more.
[0016] Examples of polyhydric alcohols used as raw materials for the polyester resin include dihydric alcohols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, trimethylene glycol, tetramethylene glycol, and neopentyl glycol; trihydric alcohols such as glycerin, trimethylolethane, and trimethylolpropane; and polyhydric alcohols having tetrahydric or higher valences such as diglycerin, triglycerin, pentaerythritol, dipentaerythritol, mannitol, and sorbitol. The polyhydric alcohols may be used alone or in combination of two or more.
[0017] Examples of polybasic acids used as raw materials for the polyester resin include aromatic polybasic acids such as phthalic anhydride, terephthalic acid, isophthalic acid, and trimellitic anhydride; aliphatic saturated polybasic acids such as succinic acid, adipic acid, and sebacic acid; aliphatic unsaturated polybasic acids such as maleic acid, maleic anhydride, fumaric acid, itaconic acid, and citraconic anhydride; and polybasic acids produced by Diels-Alder reaction such as cyclopentadiene-maleic anhydride adduct, terpene-maleic anhydride adduct, and rosin-maleic anhydride adduct. The polybasic acids may be used alone or in combination of two or more.
[0018] Examples of the non-drying oil fatty acid, which is a modifier for the polyester resin, include octylic acid, lauric acid, palmitic acid, stearic acid, oleic acid, linoleic acid, linoleic acid, eleostearic acid, ricinoleic acid, dehydrated ricinoleic acid, as well as coconut oil, linseed oil, tung oil, castor oil, dehydrated castor oil, soybean oil, safflower oil, and fatty acids thereof. The modifier may be used alone or in combination of two or more.
[0019] The polyester resin preferably has a reactive functional group (first reactive functional group) for reacting with a reactive functional group (third reactive functional group) of the crosslinking agent. The content of the first reactive functional group in the polyester resin is preferably 0.05 mmol / g to 8.9 mmol / g, more preferably 0.2 mmol / g to 5.3 mmol / g, and further preferably 0.3 mmol / g to 1.8 mmol / g.
[0020] The first reactive functional group is preferably a hydroxy group. When the polyester resin has a hydroxy group, the hydroxy value (also referred to as a hydroxyl value) of the polyester resin is preferably 1 mgKOH / g to 500 mgKOH / g, more preferably 10 mgKOH / g to 300 mgKOH / g, and even more preferably 15 mgKOH / g to 100 mgKOH / g. In this case, the acid value of the polyester resin is preferably less than 2 mgKOH / g. The acid value and hydroxyl value of the polyester resin are measured according to JIS K0070 (1992).
[0021] The number average molecular weight (Mn) of the polyester resin, as calculated using polystyrene standards by gel permeation chromatography (GPC), is preferably 500 to 30,000, and more preferably 1,000 to 5,000. Because the polyester resin has such a relatively low number average molecular weight, the network structure tends to become dense when the release agent composition is crosslinked with a crosslinking agent, and segregation of the copolymer described below to the release surface tends to occur.
[0022] The content of the polyester resin in the solid content of the release agent composition is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, and is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less.
[0023] (1-2. (Meth)acrylic copolymer) The (meth)acrylic copolymer (hereinafter, sometimes simply referred to as "copolymer") is a block copolymer having an A block having a structural unit (a-1) represented by general formula (1) and a B block having a structural unit (b-1) derived from a vinyl monomer having a reactive functional group.
[0024] The copolymer may be a copolymer containing structural units derived from (meth)acrylic monomers as the main component (50% by mass or more), and may contain structural units derived from vinyl monomers other than (meth)acrylic monomers. The content of structural units derived from (meth)acrylic monomers in the copolymer is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, based on 100% by mass of the entire copolymer. The copolymer may be composed only of structural units derived from (meth)acrylic monomers.
[0025] The content of the structural unit (a-1) in the copolymer is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, and is preferably 99.99% by mass or less, more preferably 99.9% by mass or less, and even more preferably 99.5% by mass or less, in 100% by mass of the copolymer. If the content of the structural unit (a-1) is 80% by mass or more, the peelability of the formed release layer becomes better, and if it is 99.99% by mass or less, the solubility in various solvents and the compatibility with polyester resins become better.
[0026] The content of the structural unit (b-1) in the copolymer is preferably 0.01% by mass or more, more preferably 0.2% by mass or more, even more preferably 0.5% by mass or more, and is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on 100% by mass of the copolymer. If the content of the structural unit (b-1) is 0.01% by mass or more, the effect of improving the strength of the release layer by crosslinking becomes greater, and if it is 20% by mass or less, the viscosity increase of the release agent composition is suppressed, and the coatability is improved.
[0027] The total content of the structural unit (a-1) and the structural unit (b-1) in the copolymer is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, based on 100% by mass of the copolymer. The copolymer may be composed of only the structural unit (a-1) and the structural unit (b-1).
[0028] The mass ratio ((a-1) / (b-1)) of the structural unit (a-1) to the structural unit (b-1) in the copolymer is preferably 4 or more, more preferably 5 or more, and even more preferably 10 or more, and is preferably 10,000 or less, more preferably 500 or less, even more preferably 200 or less, and particularly preferably 100 or less. When the mass ratio ((a-1) / (b-1)) is 4 or more, it is possible to suppress deterioration of coatability due to an increase in viscosity while maintaining releasability, and when it is 10,000 or less, it is possible to impart solubility in various solvents, compatibility with polyester resins, and strength to the release layer by crosslinking.
[0029] The structure of the copolymer is preferably a linear block copolymer. The linear block copolymer may have any structure (arrangement), but from the viewpoint of the physical properties of the linear block copolymer or the physical properties of the composition, when the A block is represented as A and the B block is represented as B, the structure (arrangement) of the linear block copolymer is preferably (AB) m Type, (AB) m - Type A, (BA) mIt is preferable that the copolymer has at least one structure selected from the group consisting of -B type (m is an integer of 1 or more, for example, an integer of 1 to 3). Among these, it is preferable that the copolymer is an AB type diblock copolymer from the viewpoint of handling during processing and physical properties of the composition. By forming an AB type diblock copolymer, the structural unit (a-1) in the A block and the structural unit (b-1) in the B block are localized, and the structural unit (a-1) in the A block is efficiently oriented and crystallized on the air surface (release surface), thereby improving the release property, and the structural unit (b-1) in the B block is oriented on the substrate surface, thereby improving the crosslinking efficiency and improving the strength of the release layer. The copolymer may have blocks other than the A block and the B block.
[0030] The content of the A block is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 85% by mass or more, and preferably 99.9% by mass or less, more preferably 99% by mass or less, and even more preferably 95% by mass or less, based on 100% by mass of the entire copolymer. The content of the B block is preferably 0.1% by mass or more, more preferably 1% by mass or more, even more preferably 5% by mass or more, and preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less, based on 100% by mass of the entire copolymer. By adjusting the contents of the A block and the B block within the above ranges, the compatibility of the copolymer with the polyester resin is increased, the coatability of the release agent composition is improved, and the release property of the formed release layer is further improved.
[0031] The mass ratio of the A block to the B block in the copolymer (A block / B block) is preferably 70 / 30 or more, more preferably 80 / 20 or more, and even more preferably 85 / 15 or more, and is preferably 99.9 / 0.1 or less, more preferably 99 / 1 or less, and even more preferably 95 / 5 or less. When the mass ratio of the A block to the B block is within the above range, the compatibility of the copolymer with the polyester resin is increased, the coatability of the release agent composition is improved, and the releasability of the formed release layer is further improved.
[0032] The molecular weight of the copolymer is measured by gel permeation chromatography (hereinafter referred to as "GPC"). The weight average molecular weight (Mw) of the copolymer is preferably 5,000 or more, more preferably 10,000 or more, even more preferably 20,000 or more, and is preferably 2,000,000 or less, more preferably 600,000 or less, even more preferably 150,000 or less, and particularly preferably less than 70,000. By adjusting the weight average molecular weight within the above range, segregation of the copolymer to the release surface occurs easily, and the release performance of the formed release layer is further improved.
[0033] The molecular weight distribution (PDI) of the copolymer is preferably 3.0 or less, more preferably 2.0 or less, even more preferably 1.6 or less, and particularly preferably 1.5 or less. In this specification, the molecular weight distribution (PDI) is calculated by (weight average molecular weight (Mw) of the copolymer) / (number average molecular weight (Mn) of the copolymer). The smaller the PDI, the narrower the molecular weight distribution width, and the more uniform the molecular weight of the copolymer is. When the PDI value is 1.0, the molecular weight distribution width is the narrowest. In other words, the lower limit of the PDI is 1.0. When the molecular weight distribution (PDI) of the copolymer exceeds 3.0, it includes both low molecular weight and high molecular weight.
[0034] In the release agent composition, the mass ratio of the polyester resin to the (meth)acrylic copolymer (polyester resin / (meth)acrylic copolymer) is preferably 5 / 95 or more, more preferably 15 / 85 or more, and even more preferably 30 / 70 or more, and is preferably 95 / 5 or less, more preferably 90 / 10 or less, and even more preferably 85 / 15 or less. When the mass ratio (polyester resin / (meth)acrylic copolymer) is within the above range, the release performance and abrasion resistance of the formed release layer can be further improved.
[0035] The various constituent components of the copolymer will be described below.
[0036] (1-2-1.A Block) The A block is a polymer block having a structural unit (a-1) represented by the following general formula (1): The structural unit (a-1) may be of one type, or of two or more types.
[0037] [ka] [In formula (1), R 11 R represents an alkyl group having 17 to 28 carbon atoms. 12 represents a hydrogen atom or a methyl group.
[0038] An alkyl group is introduced into the A block by the structural unit (a-1) represented by general formula (1). Thus, the copolymer is a (meth)acrylic polymer having an alkyl group. When the number of carbon atoms in the alkyl group of the (meth)acrylic polymer having an alkyl group is too small, it is generally difficult for the (meth)acrylic polymer to exhibit the peelability (releasability) and the residual adhesive strength tends to decrease. When the number of carbon atoms in the alkyl group is too large, the peel strength becomes too high due to high crystallinity, etc., and the peel performance decreases. Therefore, in the structural unit (a-1), R 11 By making the carbon number of R 17 to 28, the release performance becomes excellent. 11 The carbon number of the alkyl group is preferably 17 to 24, and more preferably 17 to 22.
[0039] R 11 Examples of the alkyl group include a linear alkyl group, a branched alkyl group, and a cyclic alkyl group, with the linear alkyl group and / or the branched alkyl group being preferred. Examples of the linear alkyl group include an n-heptadecyl group, an n-octadecyl group (an n-stearyl group), an n-nonadecyl group, an n-icosyl group, an n-heicosyl group, an n-docosyl group, an n-tricosyl group, an n-tetracosyl group, an n-heptacosyl group, an n-hexacosyl group, an n-heptacosyl group, and an n-octacosyl group. Examples of the branched alkyl group include an isooctadecyl group (isostearyl group), an isononadecyl group, an isoicosyl group, an isoheicosyl group, an isodocosyl group, an isotricosyl group, an isotetracosyl group, an isoheptacosyl group, an isohexacosyl group, an isoheptacosyl group, and an isooctacosyl group. The cyclic alkyl group includes a cyclic alkyl group having a monocyclic structure (for example, a cycloalkyl group), and specific examples thereof include an n-undecylcyclohexyl group and an n-dodecylcyclohexyl group.
[0040] Specific examples of vinyl monomers forming the structural unit represented by general formula (1) include n-heptadecyl (meth)acrylate, n-stearyl (meth)acrylate, n-nonadecyl (meth)acrylate, n-icosyl (meth)acrylate, n-heicosyl (meth)acrylate, n-docosyl (meth)acrylate, n-tricosyl (meth)acrylate, n-tetracosyl (meth)acrylate, n-heptacosyl (meth)acrylate, n-hexacosyl (meth)acrylate, n-heptacosyl (meth)acrylate, n-octacosyl (meth)acrylate, and isoheptadecyl (meth)acrylate. n-Undecylcyclohexyl (meth)acrylate, n-Dodecylcyclohexyl (meth)acrylate, n-Dodecylcyclohexyl (meth)acrylate, and the like.
[0041] The A block may be composed of only the structural unit (a-1), or may contain other structural units. From the viewpoint of maintaining excellent releasability, the content of the structural unit (a-1) is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, in 100% by mass of the A block. In addition, it is preferable that the A block does not substantially contain the structural unit (b-1) described below. That is, the content of the structural unit (b-1) is preferably 5% by mass or less, more preferably 2% by mass or less, and even more preferably 1% by mass or less, in 100% by mass of the A block.
[0042] Specific examples of vinyl monomers that can form other structural units of the A block include (meth)acrylates having a linear alkyl group having 1 to 16 carbon atoms, (meth)acrylates having a branched alkyl group having 3 to 16 carbon atoms, (meth)acrylates having a cyclic alkyl group having 6 to 16 carbon atoms, (meth)acrylates having an aromatic group, (meth)acrylates having a polyalkylene glycol structural unit, (meth)acrylates having an alkoxy group, (meth)acrylates having an oxygen-containing heterocyclic group, α-olefins, aromatic vinyl monomers, vinyl monomers containing a heterocycle, vinyl amides, vinyl carboxylates, and dienes.
[0043] The (meth)acrylate having a linear alkyl group having 1 to 16 carbon atoms is preferably a (meth)acrylate having a linear alkyl group having 1 to 10 carbon atoms, and more preferably a (meth)acrylate having a linear alkyl group having 1 to 5 carbon atoms. Examples of the (meth)acrylate having a linear alkyl group having 1 to 16 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, and decyl (meth)acrylate.
[0044] The (meth)acrylate having a branched alkyl group having 3 to 16 carbon atoms is preferably a (meth)acrylate having a branched alkyl group having a carbon number of 3 to 10. Examples of the (meth)acrylate having a branched alkyl group include isopropyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isononyl (meth)acrylate, and isodecyl (meth)acrylate.
[0045] The (meth)acrylate having a cyclic alkyl group having 6 to 16 carbon atoms is preferably a (meth)acrylate having a cyclic alkyl group having 6 to 12 carbon atoms in the cyclic alkyl group. Examples of the cyclic alkyl group include a cyclic alkyl group having a monocyclic structure (for example, a cycloalkyl group). Specific examples of the (meth)acrylate having a cyclic alkyl group having a monocyclic structure having 6 to 16 carbon atoms include cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, and cyclododecyl (meth)acrylate.
[0046] The (meth)acrylate having an aromatic group is preferably a (meth)acrylate having an aromatic group having 6 to 12 carbon atoms, and more preferably a (meth)acrylate having an aromatic group having 6 to 9 carbon atoms. Examples of the aromatic group include an aryl group, and may have a chain portion such as an alkylaryl group, an aralkyl group, or an aryloxyalkyl group. Specific examples of the (meth)acrylate having an aromatic group include benzyl (meth)acrylate, phenyl (meth)acrylate, and phenoxyethyl (meth)acrylate.
[0047] Examples of the (meth)acrylate having a polyalkylene glycol structural unit include (meth)acrylates having a polyethylene glycol structural unit such as polyethylene glycol (degree of polymerization = 2 to 10) methyl ether (meth)acrylate, polyethylene glycol (degree of polymerization = 2 to 10) ethyl ether (meth)acrylate, and polyethylene glycol (degree of polymerization = 2 to 10) propyl ether (meth)acrylate; and (meth)acrylates having a polypropylene glycol structural unit such as polypropylene glycol (degree of polymerization = 2 to 10) methyl ether (meth)acrylate, polypropylene glycol (degree of polymerization = 2 to 10) ethyl ether (meth)acrylate, and polypropylene glycol (degree of polymerization = 2 to 10) propyl ether (meth)acrylate.
[0048] Examples of the (meth)acrylate having an alkoxy group include methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate.
[0049] The (meth)acrylate having an oxygen-containing heterocyclic group is preferably a (meth)acrylate having a 4- to 6-membered oxygen-containing heterocyclic group.Specific examples of the (meth)acrylate having an oxygen-containing heterocyclic group include glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, (3-ethyloxetan-3-yl)methyl (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, cyclic trimethylolpropaneformal (meth)acrylate, 2-[(2-tetrahydropyranyl)oxy]ethyl (meth)acrylate, and 1,3-dioxane-(meth)acrylate.
[0050] Examples of the α-olefin include 1-hexene, 1-octene, and 1-decene. Examples of the aromatic vinyl monomer include styrene, α-methylstyrene, 4-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methoxystyrene, 2-hydroxymethylstyrene, and 1-vinylnaphthalene. Examples of the vinyl monomer containing a heterocycle include 2-vinylthiophene, N-methyl-2-vinylpyrrole, 1-vinyl-2-pyrrolidone, 2-vinylpyridine, 4-vinylpyridine, N-phenylmaleimide, N-benzylmaleimide, and N-cyclohexylmaleimide. Examples of the vinyl amide include N-vinylformamide, N-vinylacetamide, and N-vinyl-ε-caprolactam. Examples of the vinyl carboxylate include vinyl acetate, vinyl pivalate, and vinyl benzoate. Examples of the dienes include butadiene, isoprene, 4-methyl-1,4-hexadiene, and 7-methyl-1,6-octadiene.
[0051] It is preferable that the A block does not have a reactive functional group capable of reacting with a reactive functional group (third reactive functional group) possessed by a crosslinking agent described later. If the A block does not have a reactive functional group, the A block of the copolymer is more likely to segregate on the surface of the release layer formed from the release agent composition, and the release force is further reduced.
[0052] When two or more types of structural units are contained in the A block, the various structural units contained in the A block may be contained in the A block in any form such as random copolymerization, block copolymerization, etc., and from the viewpoint of uniformity, it is preferable that they are contained in the A block in the form of random copolymerization. For example, the A block may be formed of a copolymer of structural units consisting of the a1 block and structural units consisting of the a2 block.
[0053] (1-2-2.B Block) The B block is a polymer block having a structural unit (b-1) derived from a vinyl monomer having a reactive functional group. The structural unit (b-1) may be of one type or of two or more types.
[0054] The reactive functional group (second reactive functional group) possessed by the structural unit (b-1) is a functional group that can react with a reactive functional group (third reactive functional group) possessed by a crosslinking agent described later. Examples of the vinyl monomer having a reactive functional group that forms the structural unit (b-1) include a (meth)acrylic monomer having a reactive functional group and a vinyl monomer having a reactive functional group other than a (meth)acrylic monomer.
[0055] Examples of the second reactive functional group include a hydroxy group, an acid group, and an epoxy group, and are preferably a hydroxy group and / or an acid group. Examples of the acid group include a carboxy group (-COOH), a sulfonic acid group (-SO3H), a phosphoric acid group (-OPO3H2), a phosphonic acid group (-PO3H2), and a phosphinic acid group (-PO2H2), and are preferably a carboxy group (-COOH).
[0056] Examples of the vinyl monomer forming the structural unit (b-1) include (meth)acrylic monomers having a hydroxyl group, (meth)acrylic monomers having an acidic group, (meth)acrylic monomers having an epoxy group, vinyl monomers other than (meth)acrylic monomers having a hydroxyl group, vinyl monomers other than (meth)acrylic monomers having an acidic group, vinyl monomers other than (meth)acrylic monomers having an epoxy group, etc. Among these, at least one selected from the group consisting of (meth)acrylic monomers having a hydroxyl group and (meth)acrylic monomers having an acidic group is preferred.
[0057] Examples of the (meth)acrylic monomer having a hydroxy group include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, and 12-hydroxylauryl (meth)acrylate; caprolactone adducts of hydroxyalkyl (meth)acrylates, etc. Among these, hydroxyalkyl (meth)acrylates are preferred, and (meth)acrylates having a hydroxyalkyl group having 1 to 5 carbon atoms are more preferred.
[0058] Examples of the (meth)acrylic monomer having an acidic group include a (meth)acrylic monomer having a carboxy group, a (meth)acrylic monomer having a sulfonic acid group, a (meth)acrylic monomer having a phosphoric acid group, etc. Among these, a (meth)acrylic monomer having a carboxy group is preferred.
[0059] Examples of the (meth)acrylic monomer having a carboxy group include monomers obtained by reacting (meth)acrylates having a hydroxy group, such as 2-(meth)acryloyloxyethyl succinate and 2-(meth)acryloyloxyethyl maleate, with acid anhydrides, such as maleic anhydride and succinic anhydride, (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, etc. Among these, (meth)acrylic acid is preferred. Examples of the (meth)acrylic monomer having a sulfonic acid group include ethyl sulfonate (meth)acrylate. Examples of the (meth)acrylic monomer having a phosphoric acid group include 2-(phosphonooxy)ethyl (meth)acrylate.
[0060] Examples of the (meth)acrylic acid ester having an epoxy group include glycidyl (meth)acrylate and 3,4-epoxycyclohexylmethyl (meth)acrylate.
[0061] Examples of vinyl monomers other than the (meth)acrylic monomer having a hydroxy group include allyl alcohol.
[0062] Examples of vinyl monomers other than the (meth)acrylic monomer having an acidic group include vinyl monomers having a carboxy group, vinyl monomers having a sulfonic acid group, and vinyl monomers having a phosphoric acid group. Among these, vinyl monomers having a carboxy group are preferred. Examples of vinyl monomers having a carboxy group include crotonic acid, maleic acid, itaconic acid, citraconic acid, and cinnamic acid.
[0063] Examples of the vinyl monomer other than the (meth)acrylic monomer containing an epoxy group include 2-allyloxirane, glycidyl vinyl ether, and 3,4-epoxycyclohexyl vinyl ether.
[0064] The B block may be composed of only the structural unit (b-1), or may contain other structural units. From the viewpoint of maintaining excellent releasability, the content of the structural unit (b-1) is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, in 100% by mass of the B block.
[0065] Specific examples of vinyl monomers capable of forming other structural units of the B block include the same as those exemplified as specific examples of vinyl monomers capable of forming the A block and vinyl monomers capable of forming other structural units of the A block, and preferred are vinyl monomers capable of forming the A block.
[0066] When two or more types of structural units are contained in the B block, the various structural units contained in the B block may be contained in the B block in any form such as random copolymerization, block copolymerization, etc., and from the viewpoint of uniformity, it is preferable that they are contained in the B block in the form of random copolymerization. For example, the B block may be formed of a copolymer of structural units consisting of the b1 block and structural units consisting of the b2 block.
[0067] (1-2-3. Method for producing copolymer) Examples of methods for producing the copolymer include a method in which an A block is first produced by a polymerization reaction of a vinyl monomer, and then a monomer for a B block is polymerized onto the A block; a method in which a B block is first produced, and then a monomer for an A block is polymerized onto the B block; and a method in which the A block and the B block are produced separately, and then the A block and the B block are coupled together.
[0068] The polymerization method is not particularly limited, but living radical polymerization is preferred. That is, the copolymer is preferably one polymerized by living radical polymerization. The living radical polymerization method is preferred in that it maintains the simplicity and versatility of conventional radical polymerization methods, while being less susceptible to termination reactions and chain transfer, and grows without being hindered by side reactions that deactivate the growing end, making it easy to precisely control the molecular weight distribution and produce a polymer with a uniform composition.
[0069] Living radical polymerization methods include, depending on the method of stabilizing the polymer growing end, a method using a transition metal catalyst (ATRP method), a method using a sulfur-based reversible chain transfer agent (RAFT method), a method using an organic tellurium compound (TERP method), etc. Among these, the TERP method is preferred from the viewpoints of the variety of monomers that can be used, molecular weight control in the polymer region, uniform composition, and coloring.
[0070] The TERP method is a method in which an organic tellurium compound is used as a chain transfer agent to polymerize a radically polymerizable compound (vinyl monomer), and is a method described, for example, in WO 2004 / 14848, WO 2004 / 14962, WO 2004 / 072126, and WO 2004 / 096870.
[0071] Specific polymerization methods of the TERP method include the following (a) to (d). (a) A method of polymerizing a vinyl monomer using an organotellurium compound represented by the general formula (6): (b) A method of polymerizing a vinyl monomer using a mixture of an organotellurium compound represented by the general formula (6) and an azo-based polymerization initiator. (c) A method of polymerizing a vinyl monomer using a mixture of an organotellurium compound represented by general formula (6) and an organic ditelluride compound represented by general formula (7). (d) A method of polymerizing a vinyl monomer using a mixture of an organotellurium compound represented by general formula (6), an azo-based polymerization initiator, and an organic ditelluride compound represented by general formula (7).
[0072] [ka] [In formula (6), R 61 R represents an alkyl group having 1 to 8 carbon atoms, an aryl group, or an aromatic heterocyclic group. 62 and R 63 R each independently represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. 64 represents an alkyl group having 1 to 8 carbon atoms, an aryl group, a substituted aryl group, an aromatic heterocyclic group, an alkoxy group, an acyl group, an amido group, an oxycarbonyl group, a cyano group, an allyl group, or a propargyl group. In formula (7), R 61 represents an alkyl group having 1 to 8 carbon atoms, an aryl group, or an aromatic heterocyclic group.]
[0073] Specific examples of the organic tellurium compound represented by the general formula (6) include ethyl-2-methyl-2-n-butyltellanyl-propionate, ethyl-2-n-butyltellanyl-propionate, (2-hydroxyethyl)-2-methyl-methyltellanyl-propionate, and the organic tellurium compounds described in WO 2004 / 14848, WO 2004 / 14962, WO 2004 / 072126, and WO 2004 / 096870. Specific examples of the organic ditelluride compound represented by the general formula (7) include dimethyl ditelluride, dibutyl ditelluride, and the like. The azo polymerization initiator can be any azo polymerization initiator used in normal radical polymerization without any particular limitation. Examples of the azo polymerization initiator include 2,2'-azobis(isobutyronitrile) (AIBN), 2,2'-azobis(2,4-dimethylvaleronitrile) (ADVN), 1,1'-azobis(1-cyclohexanecarbonitrile) (ACHN), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) (V-70), and the like.
[0074] In the polymerization step, a vinyl monomer and an organic tellurium compound of general formula (6) are mixed in a vessel purged with an inert gas, and for the purpose of promoting the reaction and controlling the molecular weight and molecular weight distribution depending on the type of vinyl monomer, an azo polymerization initiator and / or an organic ditelluride compound of general formula (7) are further mixed. Examples of the inert gas include nitrogen, argon, and helium. Argon and nitrogen are preferable. The amount of the vinyl monomer used in the above (a), (b), (c), and (d) may be appropriately adjusted depending on the physical properties of the desired copolymer.
[0075] The polymerization reaction can be carried out without a solvent, but may be carried out by stirring the mixture using an aprotic solvent or a protic solvent generally used in radical polymerization. Examples of aprotic solvents that can be used include anisole, benzene, toluene, propylene glycol monomethyl ether acetate, ethyl acetate, and tetrahydrofuran (THF). Examples of protic solvents include water, methanol, and 1-methoxy-2-propanol. The solvent may be used alone or in combination of two or more. The amount of the solvent used may be appropriately adjusted, and is preferably 0.01 ml to 50 ml per 1 g of vinyl monomer. The reaction temperature and reaction time may be appropriately adjusted depending on the molecular weight or molecular weight distribution of the resulting copolymer, but the mixture is usually stirred at 0°C to 150°C for 1 minute to 100 hours. After the polymerization reaction is completed, the solvent used and the remaining vinyl monomer are removed from the resulting reaction mixture by a conventional separation and purification means, and the target copolymer can be separated.
[0076] The growing end of the copolymer obtained by the polymerization reaction is -TeR derived from the tellurium compound. 61 (In the formula, R 61 is the same as above), and is deactivated by handling in air after the polymerization reaction is completed, but tellurium atoms may remain. Since copolymers with tellurium atoms remaining at the terminals are colored and have poor thermal stability, it is preferable to remove the tellurium atoms. Methods for removing tellurium atoms include radical reduction methods, adsorption methods using activated carbon, and adsorption of metals using ion exchange resins, and these methods can also be used in combination. The other end of the copolymer obtained by the polymerization reaction (the end opposite to the growing end) is formed of -CR derived from the tellurium compound. 62 R 63 R 64 (In the formula, R 62 , R 63 and R 64 is R in Eq. (6). 62 , R 63 and R 64 (same as above.)
[0077] (1-3. Crosslinking Agent) The crosslinking agent is a compound having two or more reactive functional groups (third reactive functional groups) in one molecule that can react with the reactive functional groups (second reactive functional groups) of the copolymer, or a compound that can crosslink the reactive functional groups (second reactive functional groups) of the copolymer. Examples of the reactive functional groups of the crosslinking agent include an isocyanate group, an epoxy group, and an aziridine group.
[0078] The crosslinking agent is not particularly limited, and examples thereof include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, aziridine-based crosslinking agents, etc. Among these, at least one selected from the group consisting of isocyanate-based crosslinking agents and epoxy-based crosslinking agents is more preferred from the viewpoints of ease of controlling the degree of progress of the crosslinking reaction and adhesion to the substrate.
[0079] The isocyanate crosslinking agent is a compound having two or more isocyanate groups (including isocyanate regenerating functional groups in which the isocyanate group is temporarily protected by a blocking agent or oligomerization) in one molecule as a reactive functional group. The isocyanate crosslinking agent may be used alone or in combination of two or more kinds. Examples of the isocyanate crosslinking agent include aromatic isocyanates such as tolylene diisocyanate and xylylene diisocyanate, alicyclic isocyanates such as isophorone diisocyanate, and aliphatic isocyanates such as hexamethylene diisocyanate. More specifically, for example, lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate and isophorone diisocyanate; aromatic diisocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate and polymethylene polyphenyl isocyanate; trimethylolpropane / tolylene diisocyanate trimer adduct, trimethylolpropane One or more selected from isocyanate adducts such as hexamethylene diisocyanate trimer adducts and isocyanurates of hexamethylene diisocyanate; trimethylolpropane adducts of xylylene diisocyanate; trimethylolpropane adducts of hexamethylene diisocyanate; polyether polyisocyanates, polyester polyisocyanates, and adducts of these with various polyols, polyisocyanates multifunctionalized with isocyanurate bonds, biuret bonds, allophanate bonds, etc. can be used. Among these, it is preferable to use aliphatic isocyanates, and isocyanurates of aliphatic isocyanates (for example, isocyanurates of hexamethylene diisocyanate) are more preferable.
[0080] The epoxy crosslinking agent refers to a compound having two or more epoxy groups in one molecule as reactive functional groups. The epoxy crosslinking agent may be used alone or in combination of two or more. Examples of the epoxy crosslinking agent include bisphenol A, epichlorohydrin type epoxy resin, ethylene glycidyl ether, N,N,N',N'-tetraglycidyl-m-xylylenediamine, diglycidylaniline, diamine glycidylamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, and the like. glycidyl ether, sorbitol polyglycidyl ether, glycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, polyglycerol polyglycidyl ether, sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, adipic acid diglycidyl ester, o-phthalic acid diglycidyl ester, triglycidyl-tris(2-hydroxyethyl)isocyanurate, resorcinol diglycidyl ether, bisphenol-S-diglycidyl ether, and the like.
[0081] The aziridine crosslinking agent is a compound having two or more aziridine groups in one molecule as reactive functional groups. The aziridine crosslinking agent may be used alone or in combination of two or more. Examples of the aziridine crosslinking agent include tris-2,4,6-(1-aziridinyl)-1,3,5-triazine, tris[1-(2-methyl)-aziridinyl]phosphine oxide, and hexa[1-(2-methyl)-aziridinyl]triphosphatriazine.
[0082] The content of the reactive functional group of the crosslinking agent is preferably 0.1 mmol / g or more, more preferably 0.2 mmol / g or more, even more preferably 0.4 mmol / g or more, and is preferably 20 mmol / g or less, more preferably 15 mmol / g or less, even more preferably 12 mmol / g or less. If the content of the reactive functional group of the crosslinking agent is 0.1 mmol / g or more, the crosslinking density is high and the strength of the release layer is further improved, and if it is 20 mmol / g or less, the stability such as the pot life of the crosslinking agent composition is good.
[0083] When the crosslinking agent has an N-methylol group and an N-alkoxymethylol group in the molecule, there is a risk of formaldehyde being emitted during the formation of the release layer, etc. Therefore, it is preferable that the crosslinking agent does not contain an N-methylol group and an N-alkoxymethylol group.
[0084] The content of the crosslinking agent in the release agent composition is preferably 0.01 parts by mass or more, more preferably 0.2 parts by mass or more, and even more preferably 0.5 parts by mass or more, relative to 100 parts by mass of the copolymer, and is preferably 35 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 15 parts by mass or less. If the content of the crosslinking agent is 0.01 parts by mass or more, the crosslinking density becomes high and the strength of the release layer is further improved, and if it is 35 parts by mass or less, the stability such as the pot life of the crosslinking agent composition becomes good.
[0085] In the release agent composition, the molar ratio of the third reactive functional group of the crosslinking agent to the total amount of the first reactive functional group of the polyester resin and the second reactive functional group of the copolymer (third reactive functional group / (first reactive functional group+second reactive functional group)) is preferably 0.001 or more, more preferably 0.005 or more, even more preferably 0.01 or more, particularly preferably 0.5 or more, and is preferably 1.5 or less, more preferably 1.2 or less, and even more preferably 1.0 or less.
[0086] (1-4. Crosslinking accelerator) The release agent composition may be used by blending a crosslinking accelerator as necessary. Examples of the crosslinking accelerator include an organic tin compound and a metal chelate compound. The crosslinking accelerator may be used alone or in combination of two or more kinds.
[0087] Examples of the organotin compound include dibutyltin dilaurate, dioctyltn dilaurate, and dibutyltin dioctylate. Examples of the metal chelate compounds include zirconium chelate compounds such as zirconium tetraacetylacetonate, zirconium tributoxy monoacetylacetonate, zirconium monobutoxy acetylacetonate bis(ethylacetoacetate), and zirconium dibutoxy bis(ethylacetoacetate); titanium chelate compounds such as titanium ethylacetoacetate, titanium diisopropoxy bis(acetylacetonate), titanium tetraacetylacetonate, and titanium diisopropoxy bis(ethylacetoacetate); aluminum chelate compounds such as aluminum tris(acetylacetonate), aluminum bisethylacetoacetate monoacetylacetonate, aluminum tris(ethylacetoacetate), aluminum ethylacetoacetate diisopropylate, and aluminum alkylacetoacetate diisopropylate; zinc chelate compounds such as zinc(II) bisacetylacetonate monohydrate; and barium chelate compounds such as bis(acetylacetonate)diaquabarium(II). Examples of suitable chelates include lithium chelate compounds, calcium chelate compounds such as bis(acetylacetonate)diaquacalcium(II), copper chelate compounds such as copper(II) bisacetylacetonate, strontium chelate compounds such as bis(acetylacetonate)diaquastrontium(II), chromium chelate compounds such as chromium tris(acetylacetonate), cobalt chelate compounds such as cobalt(III) tris(acetylacetonate) and bis(acetylacetonate)diaquacobalt(II), iron chelate compounds such as iron(III) tris(acetylacetonate) and bis(acetylacetonate)diaquairon(II), indium chelate compounds such as indium tris(acetylacetonate), magnesium chelate compounds such as bis(acetylacetonate)diaquamagnesium(II), manganese chelate compounds such as bis(acetylacetonate)diaquamanganese(II), and nickel chelate compounds such as nickel(II) bisacetylacetonate dihydrate. Among these, zirconium chelate compounds and titanium chelate compounds are preferred.
[0088] The content of the crosslinking accelerator in the release agent composition is preferably 0.001 part by mass or more, more preferably 0.005 part by mass or more, and even more preferably 0.01 part by mass or more, relative to 100 parts by mass of the copolymer. By setting the content of the crosslinking accelerator in the above range, which is preferably 1.5 parts by mass or less, and more preferably 1.0 part by mass or less, it is possible to obtain an excellent crosslinking promotion effect.
[0089] (1-5. Crosslinking retarder) The release agent composition may be used by blending a crosslinking retarder as necessary. The crosslinking retarder is a compound that can suppress excessive viscosity increase of a release agent composition containing, for example, an isocyanate-based crosslinking agent by blocking the isocyanate group of the crosslinking agent. The type of crosslinking retarder is not particularly limited, and examples thereof include β-diketones such as acetylacetone, hexane-2,4-dione, heptane-2,4-dione, and octane-2,4-dione; β-ketoesters such as methyl acetoacetate, ethyl acetoacetate, propyl acetoacetate, butyl acetoacetate, octyl acetoacetate, oleyl acetoacetate, lauryl acetoacetate, and stearyl acetoacetate; benzoylacetone; and alcohols such as isopropyl alcohol. The crosslinking retarder may be used alone or in combination of two or more kinds.
[0090] When the crosslinking retarder is blended, the content of the crosslinking retarder in the release agent composition is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1.0 parts by mass or more, and is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less, relative to 100 parts by mass of the copolymer. By adjusting the content of the crosslinking retarder within the above range, it is possible to suppress excessive viscosity increase and gelation of the release agent composition after blending the crosslinking agent in the release agent composition, and to extend the storage stability (pot life) of the release agent composition.
[0091] (1-6. Other additives) In addition to the above components, other additives may be blended into the release agent composition as necessary. Examples of other additives include antioxidants, chlorine absorbers, ultraviolet absorbers, plasticizers, flame retardants, antistatic agents, colorants, and antiblocking agents. These are appropriately selected and blended according to the application and purpose of the release agent. The other additives may be used alone or in combination of two or more.
[0092] Examples of the antioxidant include phenol-based acid antioxidants, hindered amine-based antioxidants, phosphite-based antioxidants, lactone-based antioxidants, tocopherol-based antioxidants, etc. Specific examples include 2,6-di-t-butyl-p-cresol, pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxy)benzene, tris(2,4-di-t-butylphenyl)phosphite, etc.
[0093] The chlorine absorbent may, for example, be a metal soap such as calcium stearate. Examples of the ultraviolet absorbing agent include benzotriazole, benzophenone, and hydroxybenzoate. Examples of the plasticizer include citrate esters, dibutyl phthalate, polyethylene glycols, propylene glycols, and glycerin. Examples of the flame retardant include phosphazene-based compounds, phosphate esters, condensed phosphate esters, inorganic phosphorus-based, halogen-based, and silicone-based flame retardants, metal oxide-based flame retardants, metal hydroxide-based flame retardants, organic metal salt-based flame retardants, nitrogen-based flame retardants, and boron compound-based flame retardants. Examples of the antistatic agent include glycerin monoesters (such as glycerin monostearate), and ethoxylated secondary amines. Examples of the colorant include various colored dyes, colored pigments, and fluorescent dyes.
[0094] The antiblocking agent is added to prevent blocking, and is not particularly limited as long as it does not exert an effect as a nucleating agent. Examples of the antiblocking agent include inorganic particles and organic particles. Examples of the inorganic particles include particles of silica, alumina, (synthetic) zeolite, calcium carbonate, kaolin, talc, mica, zinc oxide, magnesium oxide, quartz, magnesium carbonate, barium sulfate, titanium dioxide, and the like. Examples of the organic particles include particles of polystyrene resin, polyacrylic resin, polymethyl methacrylate (PMMA) resin, crosslinked polyethylene resin, polyester resin, polyamide resin, polycarbonate resin, polyether resin, polyethersulfone resin, polyetherimide resin, polyphenylene sulfide resin, polyetheretherketone resin, polyamideimide resin, benzoguanamine resin, furan resin, epoxy resin, phenol resin, unsaturated polyester resin, vinyl ester resin, diallyl phthalate resin, polyimide resin, fatty acid amide resin, and fatty acid glycerin ester compound, and the like. Among these, PMMA resin particles and silica particles are more preferred because they are excellent in blocking resistance and imparting slipping properties.The antiblocking agent preferably has a particle size of 0.1 μm to 10 μm.
[0095] It is preferable that the release agent composition does not substantially contain a silicone compound. By substantially not containing a silicone compound, adverse effects on electrical components, etc. caused by the silicone compound present in the release layer formed from the release agent composition can be prevented. The release agent composition substantially does not contain a silicone compound means that the amount of the silicone compound in the components excluding the solvent is 500 μg / g or less, preferably 100 μg / g or less. The silicone compound is a polymer having a main skeleton of a siloxane bond (Si-O-Si) consisting of silicon and oxygen, and an organic group is bonded to the silicon.
[0096] When the release agent composition contains a compound having an N-methylol group and / or an N-alkoxymethylol group such as a melamine resin, there is a risk of formaldehyde being emitted during the formation of the release layer. Therefore, the content of N-methylol groups and N-alkoxymethylol groups in the solid content (components other than the solvent) contained in the release agent composition is preferably 0.3 mmol / g or less, more preferably 0.03 mmol / g or less. It is preferable that the release agent composition does not contain a compound having an N-methylol group and / or an N-alkoxymethylol group. The content of N-methylol groups and N-alkoxymethylol groups in the solid content can be calculated from the amount of the compound and polymerization raw material used.
[0097] (1-7. Method for producing the release agent composition) The release agent composition can be produced by mixing a polyester resin, a (meth)acrylic copolymer, a crosslinking agent, and a crosslinking accelerator, a crosslinking retarder, and other additives that are used as necessary. The release agent composition may contain a solvent derived from the production of the copolymer, or may be a solution diluted with a suitable solvent to have a viscosity suitable for forming a release layer.
[0098] Examples of the solvent include organic solvents such as aliphatic hydrocarbons such as hexane and heptane; aromatic hydrocarbons such as toluene and xylene; halogenated hydrocarbons such as methylene chloride and ethylene chloride; ketones such as acetone, methyl ethyl ketone, 2-pentanone, isophorone, and cyclohexanone; esters such as ethyl acetate and butyl acetate; cellosolve-based solvents such as ethyl cellosolve; and glycol ether-based solvents such as propylene glycol monomethyl ether. The boiling point of the solvent is preferably 10° C. to 150° C., and more preferably 20° C. to 120° C., from the viewpoint of improving the handling property of the coating liquid and the production efficiency of the release film. These solvents may be used alone or in combination of two or more.
[0099] The concentration of components other than the solvent in the release agent composition (i.e., the concentration of solid components remaining in the surface layer of the substrate after the solvent has been removed, e.g., the total concentration of the polyester resin, the (meth)acrylic copolymer, and the crosslinking agent, as well as other additives blended as necessary) is not limited, but is preferably 0.1% by mass to 10% by mass relative to the total amount of the release agent composition, from the viewpoints of the stability and coating suitability of the release agent composition.
[0100] <2. Release film> The release film of the present invention has a base film and a release layer formed on at least one surface of the base film. The release layer is formed from the release agent composition. In the release layer formed from the release agent composition, components derived from the copolymer are segregated near the surface (release surface) of the release layer, and the alkyl chains of the copolymer (R 11 It is believed that the group represented by the formula (I) is oriented toward the air surface. Therefore, due to the above-mentioned segregation of the copolymer, the release film has a small peeling force and good releasability, and has good appearance and strength (abrasion resistance). In addition, since it is not necessary to use a silicone compound, the components of the release agent are unlikely to migrate to the article.
[0101] Generally, a "sheet" is defined in JIS as a thin, flat product whose thickness is generally small relative to its length and width, and a "film" is generally a thin, flat product whose thickness is extremely small compared to its length and width, and whose maximum thickness is arbitrarily limited, and which is usually supplied in the form of a roll (Japanese Industrial Standard JIS K6900). For example, in terms of thickness, in the narrow sense, a product with a thickness of 100 μm or more is called a sheet, and a product with a thickness of less than 100 μm is sometimes called a film. However, the boundary between a sheet and a film is unclear, and since there is no need to distinguish between the two in the present invention, in this specification, the term "sheet" is intended to include "film", and the term "film" is intended to include "sheet".
[0102] (2-1. Base film) The substrate film can be any substrate that is commonly used, without any particular limitation. For example, in addition to films containing resins such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polybutylene terephthalate (PBT), polyester resins such as polypropylene, polyethylene, polycycloolefin, and cycloolefin copolymer, acetylcellulose resins such as triacetyl cellulose (TAC), acrylic resins such as polymethyl methacrylate (PMMA), polystyrene resins, polyamide resins, polycarbonate resins, polyvinyl chloride resins, polyphenylene sulfide resins, polyimide resins, polyetherimide resins, polyether ketone resins, polyether ether ketone resins, polynorbornene resins, polyacrylonitrile resins, and polyvinyl alcohol resins, thin sheets of paper such as fine paper, dust-free paper, glassine paper, clay-coated paper, resin-coated paper, and laminated paper (polyethylene-laminated paper, polypropylene-laminated paper, etc.), nonwoven fabric, and metal foil can also be used.
[0103] When the base film is a film containing a resin, it may contain only one type of the resin, or may contain two or more types in combination. From the viewpoint of heat resistance and strength of the release layer, the film containing the resin is preferably a film containing at least one selected from the group consisting of polyester resins, olefin resins, and polyimide resins as a main component. From the viewpoint of adhesion with the release layer, it is more preferable that the film is a layer containing at least one selected from the group consisting of polyester resins, olefin resins, and polyimide resins as a main component.
[0104] In this specification, the term "main component" means a component that is contained in an amount of 50% by mass or more, and the proportion of the main component is preferably 70% by mass or more, more preferably 80% by mass or more, further preferably 90% by mass or more, and particularly preferably 95% by mass or more. The proportion of the main component may be 100% by mass.
[0105] The base film may contain additives. The types and components of the additives may be the same as those described above in the section on the release agent composition.
[0106] The base film may be a film constituted by any one of a non-stretched film, a uniaxially stretched film, and a biaxially stretched film. From the viewpoints of processability, transparency, and dimensional stability, the base film is preferably a layer constituted by a biaxially stretched film.
[0107] The thickness of the substrate film varies depending on the application and substrate, but is preferably 2 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more from the viewpoint of processability. The thickness of the substrate layer is preferably 500 μm or less, more preferably 200 μm or less, and even more preferably 100 μm or less from the viewpoint of handling properties during product use.
[0108] The substrate film may be subjected to a surface treatment by an oxidation method, a roughening method, or the like on one or both sides as desired, for the purpose of improving adhesion to a layer provided on the surface. Examples of the oxidation method include corona discharge treatment, plasma treatment, chromic acid treatment (wet), flame treatment, hot air treatment, ozone / ultraviolet light irradiation treatment, and the like. Examples of the roughening method include sandblasting and solvent treatment. These surface treatment methods are appropriately selected depending on the type of substrate film, but generally, corona discharge treatment is preferably used in terms of effectiveness and operability.
[0109] (2-2. Peeling layer) The release layer is formed from the release agent composition. The release layer is a layer for imparting releasability to the release film. The thickness of the release layer is preferably 0.01 μm or more, more preferably 0.05 μm or more, and even more preferably 0.1 μm or more, from the viewpoint of easy enhancement of releasability. From the viewpoint of curing property of the release agent composition, the thickness is preferably 3 μm or less, more preferably 2 μm or less, and even more preferably 1 μm or less.
[0110] The release layer is formed on at least one surface of the base film. The release layer may be a single layer or may have a multi-layer structure. The release layer may be formed between the base film surface and each layer such as a primer layer, but it is preferable that the release layer is formed directly on the base film surface.
[0111] (2-2-1. Method for forming release layer) The method for forming the release layer is not particularly limited, and examples thereof include a method in which the release agent composition is applied to one or both sides of a base film using various coating devices, the solvent in the coating layer is removed, and curing is performed as necessary.
[0112] Examples of the coating device include a reverse roll coater, a gravure coater, a forward roll coater, a knife coater, a wire bar coater, a doctor blade coater, a slot die coater, a curtain coater, and a dip coater.
[0113] The method for removing the solvent from the coating layer is not particularly limited as long as the solvent can be volatilized. Note that removing the solvent does not mean completely removing the solvent, but also includes removing the solvent to the extent that a layer is formed. Examples of the method for removing the solvent include a method of drying the coating layer by blowing air on it, and a method of drying the coating layer by heating it with electromagnetic waves such as infrared rays.
[0114] From the viewpoint of easily achieving both solvent removal and promotion of the crosslinking reaction, the air drying temperature or heating temperature is preferably 40°C to 200°C, more preferably 90°C to 150°C. The drying time or heating time is preferably 10 seconds to 300 seconds, more preferably 15 seconds to 90 seconds, and even more preferably 20 seconds to 50 seconds. The curing conditions include, for example, about 3 days to 7 days at 40°C. The crosslinking reaction (reaction between the reactive functional group of the copolymer and the crosslinking agent) is completed by the solvent removal and curing, and a release layer is formed.
[0115] The release film may be a base film and a release layer formed on only one side of the base film; or a base film and a release layer formed on both sides of the base film. The release film may be provided with fine surface roughness on the surface to improve winding suitability within a range that does not interfere with lamination when used as a release film. As a method for providing fine irregularities on the surface of the release film, an embossing method, an etching method, and each of the known surface roughening methods can be adopted.
[0116] The release film is composed of a non-silicone compound, so that the use of the release film in electrical component applications will not adversely affect the electrical components. In addition, the release layer is substantially free of N-methylol groups and N-alkoxymethylol groups, so that the release film can also be used in the medical field. For example, the release film is suitable for use as a surface protection film, a release film for adhesive tape, a release liner or separator film, a separator film for process tapes (dicing, die bonding, back grinding) used in the manufacture of semiconductor products, a carrier for forming unfired sheets in the manufacture of ceramic capacitors, a carrier in the manufacture of composite materials, a separator film for protective materials, etc.
[0117] <3. Adhesive body> The adhesive body in one embodiment of the present invention comprises the release film and an adhesive layer formed on the release layer of the release film.
[0118] It is preferable that the adhesive layer does not substantially contain a silicone compound. When the adhesive layer does not substantially contain a silicone compound, adverse effects on electrical components and the like can be more effectively prevented. Note that, "substantially not containing a silicone compound" means that the amount of the silicone compound in the adhesive layer is 500 μg / m 2 It is preferable that the concentration is 100 μg / m or less. 2 This refers to the following:
[0119] The adhesive constituting the adhesive layer can be any non-silicone adhesive that does not substantially contain a silicone compound, and can be, for example, a (meth)acrylic adhesive. The adhesive layer can be formed by applying an adhesive onto a release layer and then drying by heating. The thickness of the adhesive layer is not particularly limited and can be appropriately adjusted according to the application.
[0120] The pressure-sensitive adhesive body may further include a support that is provided on the pressure-sensitive adhesive layer and supports the pressure-sensitive adhesive layer. The support is not particularly limited, and may be any of the support exemplified as the base film of the release film of the present invention. After the pressure-sensitive adhesive body is produced, it is wound into a roll and stored. EXAMPLES
[0121] The present invention will be described in more detail below based on specific examples. The present invention is not limited to the following examples, and can be modified as appropriate within the scope of the present invention. The polymerization rate, weight average molecular weight (Mw), and molecular weight distribution (PDI) of the copolymer, as well as the peel strength, residual adhesion rate, abrasion resistance, and appearance of the release layer were evaluated according to the following methods.
[0122] The meanings of the abbreviations are as follows: BTEE: Ethyl 2-methyl-2-n-butyltellanyl-propionate AIBN: 2,2'-azobis(isobutyronitrile) SA: Stearyl acrylate 4-HBA: 4-hydroxybutyl acrylate LA: Lauryl acrylate AcOEt: ethyl acetate MeOH: Methanol MEK: Methyl ethyl ketone
[0123] (Polymerization rate) Using a nuclear magnetic resonance (NMR) measuring device (Bruker Biospin, model: AVANCE500 (frequency 500 MHz)), 1H-NMR was measured (solvent: CDCl3, internal standard: trimethylsilane). For the obtained NMR spectrum, the integral ratio of the peaks of the vinyl group derived from the monomer and the ester side chain derived from the polymer was obtained, and the polymerization rate of the monomer was calculated.
[0124] (Weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight distribution (PDI)) The molecular weight was determined by gel permeation chromatography (GPC) using a high performance liquid chromatograph (Tosoh, model HLC-8320GPC). Two TSKgel Super Multipore HZ-H (Tosoh) columns were used, a tetrahydrofuran solution was used as the mobile phase, and a differential refractometer was used as the detector. The measurement conditions were a column temperature of 40°C, a sample concentration of 10mg / mL, a sample injection volume of 10μm, and a flow rate of 0.2mL / min. A calibration curve was created using polystyrene (molecular weights 109,000, 775,000, 427,000, 289,000, 190,000, 96,400, 37,900, 10,200, 2,630, and 440) as a standard substance, and the weight average molecular weight (Mw) and number average molecular weight (Mn) were measured. The molecular weight distribution (PDI=Mw / Mn) was calculated from the measured values.
[0125] (peel strength, residual adhesion rate) A 25 mm wide polyester adhesive tape (Nitto Denko Corporation, polyester adhesive tape No. 31B) was attached to the release layer of the release film, and a 2 kg roller was rolled back and forth twice to press the tape, producing a test piece for measuring the peel strength. A 180 degree peel test was performed on this test piece to measure the peel strength.
[0126] Next, the polyester base adhesive tape used in the peel strength evaluation (which was attached to a release film and then peeled off) was attached to an uncoated polyethylene terephthalate (PET) film (Toyobo Co., Ltd., E5100, thickness 50 μm), and pressed against the film by rolling a 2 kg roller back and forth twice to prepare a test specimen. A 180-degree peel test was then performed on this test specimen to determine the adhesive strength. Furthermore, an unused adhesive tape identical to the polyester-based adhesive tape used in the peel strength evaluation was attached to an uncoated PET film (Toyobo Co., Ltd., E5100, thickness 50 μm) and pressed against the film by rolling it back and forth twice with a 2 kg roller to prepare a test specimen. A 180-degree peel strength test was then performed on this test specimen to measure the initial adhesive strength. From the measured adhesive strength and initial adhesive strength, the residual adhesion rate was calculated using the following formula. Residual adhesion rate (%) = (adhesive strength / initial adhesive strength) × 100
[0127] The 180-degree peel test was carried out according to the following procedure. Before the test, the test piece was left to stand for 24 hours in an environment of 23°C and 50% RH. The test was carried out at room temperature (23°C), with a gripping movement speed of 300 mm / min, and continued until the length of the peeled portion reached 125 mm or more. From the test results, a force-grip movement distance curve was created, and the average value was calculated for a peel length of at least 100 mm excluding the first 25 mm, and this was taken as the peel force, adhesive force, or initial adhesive force.
[0128] (Abrasion resistance) The release layer of the release film was rubbed with a finger, and the changes were visually observed and rated on a three-level scale. 3: There was no change in the peel layer. 2: There was some change in the peeling layer. 1: The coating becomes cloudy
[0129] (exterior) The release layer (coated surface) of the release film was visually observed and rated on a three-level scale. 3: The coating is uniform and without unevenness. 2: The coating is not uniform in some areas. 1: The coating is uneven overall.
[0130] <Production of block copolymer> (Synthesis Example 1: Block Copolymer No. 1) SA (19.6 g), AIBN (13.1 mg), and AcOEt (13.1 g) were charged into a test tube equipped with a stirrer, and after replacing with argon, BTEE (120.0 mg) was added and reacted at 60°C for 26 hours to polymerize the A block. The polymerization rate was 87%. A mixture of 4-HBA (0.6 g), AIBN (6.6 mg), and AcOEt (0.3 g), which had been replaced with argon, was added to the reaction solution, and the mixture was reacted at 60° C. for 24 hours to polymerize the B block. The polymerization rate was 85%.
[0131] After the reaction was completed, the mixture was poured into stirred MeOH. The precipitated polymer was filtered by suction and dried to obtain block copolymer No. 1. The obtained block copolymer No. 1 had an Mw of 49,090 and a PDI of 1.44. The content of each structural unit in the copolymer was calculated from the charge ratio of the monomers used in the polymerization reaction and the polymerization rate.
[0132] (Synthesis Example 2: Block Copolymer No. 2) SA (14.7g), AIBN (9.9mg), and toluene (12.5g) were charged into a test tube equipped with a stirrer, and after replacing with argon, BTEE (90.0mg) was added and reacted at 60℃ for 16 hours to polymerize the A block. The polymerization rate was 87%. A mixture of 4-HBA (0.3 g), AIBN (4.9 mg), and toluene (0.3 g), which had been replaced with argon, was added to the reaction solution, and the mixture was reacted at 60° C. for 16 hours to polymerize the B block. The polymerization rate was 84%.
[0133] After the reaction was completed, the mixture was poured into stirred MeOH. The supernatant was then removed and the mixture was dried to obtain block copolymer No. 2. The obtained block copolymer No. 2 had an Mw of 43,780 and a PDI of 1.47. The content of each structural unit in the copolymer was calculated from the charge ratio of the monomers used in the polymerization reaction and the polymerization rate.
[0134] (Synthesis Example 3: Block Copolymer No. 3) SA (19.6 g), AIBN (6.6 mg), and AcOEt (13.1 g) were charged into a test tube equipped with a stirrer, and after replacing with argon, BTEE (60.0 mg) was added and reacted at 60°C for 20 hours to polymerize the A block. The polymerization rate was 90%. A mixture of 4-HBA (0.4 g), AIBN (3.3 mg), and AcOEt (0.3 g) that had been replaced with argon was added to the reaction solution, and the mixture was reacted at 60° C. for 16 hours to polymerize the B block. The polymerization rate was 74%.
[0135] After the reaction was completed, the mixture was poured into stirred MeOH. The precipitated polymer was filtered by suction and dried to obtain block copolymer No. 3. The obtained block copolymer No. 3 had an Mw of 82,070 and a PDI of 1.48. The content of each structural unit in the copolymer was calculated from the charge ratio of the monomers used in the polymerization reaction and the polymerization rate.
[0136] (Synthesis Example 4: Block Copolymer No. 4) In a test tube equipped with a stirrer, LA (19.6 g), AIBN (13.1 mg), and AcOEt (13.1 g) were charged, and after replacing with argon, BTEE (120.0 mg) was added and reacted at 60°C for 24 hours to polymerize the A block. The polymerization rate was 90%. A mixture of 4-HBA (0.4 g), AIBN (6.6 mg), and AcOEt (0.3 g), which had been replaced with argon, was added to the reaction solution, and the mixture was reacted at 60° C. for 24 hours to polymerize the B block. The polymerization rate was 79%. After the reaction was completed, the mixture was poured into stirred MeOH. The supernatant was then removed and the mixture was dried to obtain block copolymer No. 4. The resulting block copolymer No. 4 had an Mw of 59,690 and a PDI of 1.33. The content of each structural unit in the copolymer was calculated from the charge ratio of the monomers used in the polymerization reaction and the polymerization rate.
[0137] (Synthesis Example 5: Block Copolymer No. 5) In a test tube equipped with a stirrer, LA (19.6 g), AIBN (6.6 mg), and AcOEt (13.1 g) were charged, and after replacing with argon, BTEE (60.0 mg) was added and reacted at 60°C for 20 hours to polymerize the A block. The polymerization rate was 87%.
[0138] A mixture of 4-HBA (0.4 g), AIBN (3.3 mg), and AcOEt (0.3 g) that had been replaced with argon was added to the reaction solution, and the mixture was reacted at 60° C. for 16 hours to polymerize the B block. The polymerization rate was 82%.
[0139] After the reaction was completed, the mixture was poured into stirred MeOH. The supernatant was then removed and the mixture was dried to obtain block copolymer No. 5. The resulting block copolymer No. 5 had an Mw of 91,230 and a PDI of 1.56. The content of each structural unit in the copolymer was calculated from the charge ratio of the monomers used in the polymerization reaction and the polymerization rate.
[0140] [Table 1]
[0141] (Synthesis Example 6: Random Copolymer No. 1) SA (9.8 g), 4-HBA (0.2 g), AIBN (0.2 g), and toluene (20.0 g) were charged into a test tube equipped with a stirrer, and after replacing with argon, the mixture was reacted at 85°C for 8 hours to obtain random copolymer No. 1 through polymerization. The polymerization rate was 98%. The random copolymer No. 1 obtained had an Mw of 50,750 and a PDI of 4.34. The content of each structural unit in the copolymer was calculated from the charge ratio of the monomers used in the polymerization reaction.
[0142] (Synthesis Example 7: Random Copolymer No. 2) SA (9.8 g), 4-HBA (0.2 g), AIBN (0.2 g), and toluene (10.0 g) were charged into a test tube equipped with a stirrer, and after replacing with argon, the mixture was reacted at 85°C for 8 hours to obtain random copolymer No. 2. The polymerization rate was 99%. The random copolymer No. 2 obtained had an Mw of 125,470 and a PDI of 6.33. The content of each structural unit in the copolymer was calculated from the charge ratio of the monomers used in the polymerization reaction.
[0143] (Synthesis Example 8: Random Copolymer No. 3) In a test tube equipped with a stirrer, LA (9.8 g), 4-HBA (0.2 g), AIBN (0.2 g), and toluene (20.0 g) were charged, and after argon replacement, the mixture was reacted at 85°C for 8 hours to obtain random copolymer No. 3. The polymerization rate was 98%. The random copolymer No. 3 obtained had an Mw of 67,900 and a PDI of 7.01. The content of each structural unit in the copolymer was calculated from the charge ratio of the monomers used in the polymerization reaction.
[0144] (Synthesis Example 9: Random Copolymer No. 4) In a test tube equipped with a stirrer, LA (9.8 g), 4-HBA (0.2 g), AIBN (0.2 g), and toluene (5.0 g) were charged, and after argon replacement, the mixture was reacted at 85°C for 8 hours to obtain random copolymer No. 4. The polymerization rate was 99%. The random copolymer No. 4 obtained had an Mw of 150,500 and a PDI of 12.44. The content of each structural unit in the copolymer was calculated from the charging ratio of the monomers used in the polymerization reaction.
[0145] (Synthesis Example 10: Random Copolymer No. 5) SA (14.7 g), 4-HBA (0.3 g), AIBN (9.9 mg), and toluene (12.8 g) were charged into a test tube equipped with a stirrer, and after argon replacement, BTEE (90.0 mg) was added and reacted at 60°C for 16 hours to polymerize. The polymerization rate was 76%. After the reaction was completed, the mixture was poured into stirred MeOH. The precipitated polymer was suction filtered and dried to obtain random copolymer No. 5. The obtained random copolymer No. 5 had an Mw of 39,470 and a PDI of 1.33. The content of each structural unit in the copolymer was calculated from the charge ratio of the monomers used in the polymerization reaction.
[0146] (Synthesis Example 11: SA Polymer) SA (19.6 g), AIBN (13.1 mg), and AcOEt (13.1 g) were charged into a test tube equipped with a stirrer, and after replacing with argon, BTEE (120.0 mg) was added and reacted at 60°C for 26 hours to polymerize. The polymerization rate was 66%. After the reaction was completed, the mixture was poured into stirred MeOH. The precipitated polymer was suction filtered and dried to obtain an SA polymer. The obtained SA polymer had an Mw of 41,890 and a PDI of 1.30.
[0147] [Table 2]
[0148] <Preparation of release agent composition and release film> (Production Example 1: Stripping Agent Composition No. 1) To 100 parts by mass of the copolymer obtained in Synthesis Example 1, 2.52 parts by mass of a crosslinking agent in terms of solid content, 0.76 parts by mass of a crosslinking accelerator in terms of solid content, 100 parts by mass of a polyester resin, 7670 parts by mass of methyl ethyl ketone (MEK) as a solvent, and 2291 parts by mass of toluene were added and stirred to obtain release agent composition No. 1.
[0149] The obtained release agent composition No. 1 was applied onto a 50 μm PET film (manufactured by Toyobo Co., Ltd., E5100) using a bar coater #3 (thickness after drying: 140 nm), and dried at 120° C. for 30 seconds to prepare a release film. The prepared release film was left to stand at 40° C. for 3 days, and then various tests were performed.
[0150] (Examples 2 to 18) Release agent compositions Nos. 2 to 18 were prepared in the same manner as in Production Example 1. Table 3 shows the amounts of the copolymer, SA polymer, and each raw material used. Moreover, release films were prepared in the same manner as in Production Example 1 above, using the obtained release agent compositions Nos. 2 to 18.
[0151] The prepared release films were evaluated for peel strength, residual adhesion rate, abrasion resistance, and appearance. The results are shown in Table 3.
[0152] [Table 3] Polyester resin: Toyobo Co., Ltd., trade name "Vylon (registered trademark) 220" (number average molecular weight 3000, hydroxyl value 50 mg KOH / g, acid value less than 2 mg KOH / g, glass transition temperature 53°C, linear) Crosslinking agent: Asahi Kasei Corporation, trade name "Duranate (registered trademark) TPA-100" (isocyanurate of hexamethylene diisocyanate, NCO%; 23.1% by mass) Crosslinking accelerator: Nitto Kasei, product name "Neostan (registered trademark) U-810" (dioctyl tin)
[0153] In the release films No. 1 to 8, the release layer is formed from a release agent composition containing a (meth)acrylic acid ester block copolymer having an alkyl group with 17 to 28 carbon atoms in the A block and a crosslinkable functional group in the B block, a polyester resin, and an isocyanate crosslinking agent. These release films No. 1 to 8 had a small peel force, a high residual adhesion rate, and excellent strength and appearance of the release layer. In addition, in the release films No. 1 to 8, the release layer does not contain a silicone compound, so that the silicone compound does not migrate to the adhesive layer of the adhesive tape. Furthermore, the release agent composition forming the release layer does not contain an N-methylol group and / or an N-alkoxymethylol group, so that formaldehyde is not generated when heated.
[0154] The release films No. 9 and No. 16 are cases where the release layer does not contain polyester resin. These release films No. 9 and No. 16 have poor abrasion resistance of the release layer. Release films No. 10 and 11 are cases where the copolymer contained in the release agent composition does not have an alkyl group having 17 to 28 carbon atoms in the A block, but has an alkyl group having less than 17 carbon atoms. These release films No. 10 and 11 have low residual adhesion rates and poor abrasion resistance of the release layer. The copolymer contained in the release agent composition is a random copolymer in the release films Nos. 12 to 15 and 17. These release films have a high peel strength of the release layer and a low residual adhesion rate. Release film No. 18 is a case where the release agent composition contains an SA polymer. This release film has a high release strength of the release layer and a low residual adhesion rate.
Claims
1. The composition contains a polyester resin, a (meth)acrylic copolymer, and a crosslinking agent, The (meth)acrylic copolymer is a block copolymer having an A block having a structural unit (a-1) represented by general formula (1) and a B block having a structural unit (b-1) derived from a vinyl monomer having a reactive functional group, the reactive functional group is a hydroxy group and / or an acidic group, The (meth)acrylic copolymer has a molecular weight distribution of 3.0 or less. 【Chemistry 1】 [In formula (1), R 11 R represents an alkyl group having 17 to 28 carbon atoms. 12 represents a hydrogen atom or a methyl group.
2. 2. The stripping composition according to claim 1, wherein the crosslinking agent is at least one selected from the group consisting of an isocyanate-based crosslinking agent and an epoxy-based crosslinking agent.
3. The release agent composition according to claim 1 or 2, wherein a content of the structural unit (a-1) in the (meth)acrylic copolymer is 80% by mass to 99.99% by mass in 100% by mass of the (meth)acrylic copolymer.
4. The stripping composition according to any one of claims 1 to 3, wherein the (meth)acrylic copolymer has a weight average molecular weight of 5,000 to 2,000,000.
5. The release agent composition according to any one of claims 1 to 4, wherein the content of the B block is 0.1% by mass to 30% by mass in 100% by mass of the entire (meth)acrylic copolymer.
6. The release agent composition according to claim 1 or 2, wherein a total content of the structural unit (a-1) and the structural unit (b-1) in the (meth)acrylic copolymer is 80 mass% or more in 100 mass% of the (meth)acrylic copolymer.
7. The release agent composition according to any one of claims 1 to 6, wherein a mass ratio of the A block to the B block (A block / B block) in the (meth)acrylic copolymer is 70 / 30 to 99.9 / 0.
1.
8. The release agent composition according to any one of claims 1 to 7, wherein the polyester resin has a hydroxy group.
9. The release agent composition according to any one of claims 1 to 8, wherein the polyester resin has a number average molecular weight of 500 to 30,000.
10. The release agent composition according to any one of claims 1 to 9, wherein a mass ratio of the polyester resin to the (meth)acrylic copolymer (polyester resin / (meth)acrylic copolymer) is 5 / 95 to 95 / 5.
11. The release agent composition according to any one of claims 1 to 10, wherein a molar ratio of the reactive functional groups of the crosslinking agent to the total amount of the reactive functional groups of the polyester resin and the reactive functional groups of the copolymer (reactive functional groups of the crosslinking agent / reactive functional groups of the polyester resin and the reactive functional groups of the copolymer) is 0.001 to 1.
5.
12. A substrate film and a release layer formed on at least one surface of the substrate film, A release film, wherein the release layer is formed from the release agent composition according to any one of claims 1 to 11.
13. A release film according to claim 12, and an adhesive layer provided on the release layer of the release film, The adhesive layer is substantially free of silicone compounds.
Citation Information
Patent Citations
Long-chain-alkyl-pendant release treatment agent and release treatment method
JP2003147327A
Long-chain alkyl pendant type release agent and releasing method
JP2003183619A
Release treatment agent
JP2005023255A
Releasable film
JP2019209528A
Peeling agent composition, peeling sheet, and adhesive body
WO2012020673A1