By using a water-absorbing resin solution with an alkaline agent in the manufacturing process, the method addresses the issues of residual monomers and maintains water absorption capacity, enhancing the safety and performance of water-absorbing agents.
Patent Information
- Application Number
- JP2020112707
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-30
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2040-06-30
AI Technical Summary
Existing methods for producing water-absorbing resins face challenges in reducing the amount of residual monomers and maintaining water absorption capacity under pressure and without pressure when reusing fine powder, which also leads to increased toxicity and irritation concerns, especially in applications contacting the human body.
Incorporating a water-absorbing resin solution obtained from a water-absorbing resin and an alkaline agent into the manufacturing process, allowing the resin to be reused in dissolved form, thereby reducing residual monomers and maintaining the water absorption capacity.
The method effectively suppresses the decrease in water absorption capacity under both pressure and no pressure, while reducing residual monomer amounts, thus improving the safety and performance of the water-absorbing agent.
Smart Images

Figure 0007572800000001 
Figure 0007572800000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a water-absorbing agent. [Background technology]
[0002] Super absorbent polymers (SAPs) are water-swellable, water-insoluble polymer gelling agents that are widely used in a variety of fields, including absorbent articles such as disposable diapers and sanitary napkins, agricultural and horticultural water retention agents, and industrial water-stopping agents.
[0003] The above-mentioned water-absorbent resins are made of many monomers and hydrophilic polymers as their raw materials. From the viewpoint of water-absorbing performance, the water-absorbent resins mainly composed of polymers constituted by acid group-containing unsaturated monomers are most widely produced industrially.
[0004] The water-absorbent resin is required to have various functions (higher physical properties) in accordance with the high performance of paper diapers, which are the main application of the water-absorbent resin. In particular, the water absorption capacity without load and the water absorption capacity under load are very important as basic physical properties.
[0005] Such water-absorbing resins can be in various shapes such as sheets, fibers, films, etc., but are generally used as powder or particulate water-absorbing agents.
[0006] The main manufacturing method of the powdered or particulate water absorbent includes an aqueous solution polymerization method and a reversed-phase suspension polymerization method. In particular, the aqueous solution polymerization method, which uses an aqueous monomer solution to carry out polymerization, usually requires many manufacturing steps, such as a polymerization step of polymerizing an aqueous solution of an acid group-containing unsaturated monomer, a gel crushing (fine graining) step of crushing the hydrogel polymer obtained by polymerization, a drying step of drying the crushed gel, a crushing step of crushing the dried product, a classification step of adjusting the crushed product to an appropriate particle size range, and a surface crosslinking step of treating the classified water absorbent resin powder with a surface crosslinking agent, in order to finally obtain a particulate water absorbent resin.
[0007] In such a manufacturing process, unnecessary water absorbent resin such as fine powder and non-standard products is generated. For example, the amount of fine powder generated reaches 10 to several tens of mass% (for example, 20 to 30 mass%) of the total production amount. The unnecessary water absorbent resin is removed in the manufacturing process, but since it is cost-inefficient to dispose of the removed water absorbent resin, the removed water absorbent resin is recovered and reused in a process before the classification process, particularly in a process before the drying process. Many studies have been conducted so far on the recovery and reuse of water absorbent resin.
[0008] In Patent Document 1, fine powder of a water-absorbing resin is dispersed in acrylic acid to obtain a dispersion liquid, and then the dispersion liquid is added to an aqueous monomer solution, thereby reusing the fine powder.
[0009] In addition, in Patent Document 2, fine powder of water-absorbent resin is treated with an alkaline substance, and then the treated body is added to an aqueous monomer solution, thereby reusing the fine powder. According to Patent Document 2, by carrying out this process, the absorbent resin obtained has an improved absorption capacity for retaining liquid in an unloaded state. In addition, Patent Document 2 states that the treatment with the alkaline substance is "evenly distributed on the fine powder of superabsorbent polymer by spraying or dripping," and the form of the fine powder is maintained even after the treatment.
[0010] In addition, as a method for recovering fine powder, there is a method of recovering fine powder by granulating the fine powder. If the strength of the fine powder granulated product is insufficient when granulating the fine powder, fine powder will be generated again in, for example, the drying process, the crushing process, and the classification process, and as a result, the amount of fine powder generated in the entire manufacturing process will increase. Various proposals have been made so far to improve the strength of the fine powder granulated product. For example, Patent Document 3 proposes a method of firmly binding the fine powder together by gelling the fine powder with a large amount of warm water. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Special Publication No. 5-508674 [Patent Document 2] Special Publication No. 2012-506462 [Patent Document 3] Japanese Patent Application Publication No. 11-106514 Summary of the Invention [Problem to be solved by the invention]
[0012] According to the description in Patent Document 2, the process improves the centirfuge retention capacity (CRC) of the water absorbent resin obtained compared to the case where untreated fine powder is added, but there is still room for improvement. Furthermore, suppressing the decrease in the centirfuge retention capacity under pressure, which is a basic physical property similar to the centirfuge retention capacity under pressure, is also an important issue.
[0013] On the other hand, the polymer constituting the water-absorbing resin is produced by adding an acid group-containing unsaturated monomer such as acrylic acid together with a polymerization initiator and polymerizing it by heating. In this case, there is a problem that the acid group-containing unsaturated monomer component used as the raw material remains in the polymer reaction product after the production of the polymer (problem of residual monomer). This is not preferable in terms of the productivity and performance of the polymer. In addition, particularly in applications where the polymer comes into contact with the human body, it is required to reduce the toxicity and irritation caused by the residual monomer as much as possible. However, when reusing the water-absorbing resin obtained by the conventional fine powder recovery method such as the fine powder recovery method by granulation, the amount of residual monomer in the obtained water-absorbing resin tends to increase.
[0014] An object of the present invention is to provide a method for producing a water-absorbing agent, which can suppress a decrease in the water absorption capacity under no load or the water absorption capacity under load of the obtained water-absorbing agent, even when a water-absorbing resin such as a fine powder is recovered and reused.
[0015] Another object of the present invention is to provide a method for producing a water-absorbing agent, which reduces the amount of residual monomers in the product. [Means for solving the problem]
[0016] The present invention is characterized in that a water-absorbent resin solution obtained by using a water-absorbent resin and an alkaline agent is added to a manufacturing process of a water-absorbing agent. Effect of the Invention
[0017] According to the method for producing a water absorbing agent of the present invention, even when a water absorbing resin such as a fine powder is recovered and reused, the decrease in the water absorption capacity without load of the obtained water absorbing agent is suppressed. Also, according to the method for producing a water absorbing agent of the present invention, the amount of residual monomers in the obtained water absorbing agent is reduced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The present invention will be described in detail below, but the scope of the present invention is not limited to these descriptions, and in addition to the following examples, the present invention can be implemented by making appropriate modifications within the scope of the invention. Furthermore, the present invention is not limited to the following embodiments, and various modifications are possible within the scope of the claims. Other embodiments obtained by appropriately combining the technical means disclosed in each of the embodiments are also included in the technical scope of the present invention. [1] Definitions of terms [1-1] “Water-absorbing resin” The "water-absorbent resin" in the present invention refers to a water-swellable, water-insoluble polymer gelling agent that satisfies the following physical properties: That is, the water-swellable polymer gelling agent has a CRC (centrifuge retention capacity) of 5 g / g or more as specified in NWSP 241.0.R2(15) (NWSP will be described later), and a water-insoluble polymer gelling agent has an Ext (water-soluble content) of 50 mass% or less as specified in NWSP 270.0.R2(15).
[0019] The water-absorbing resin can be designed according to its use and purpose, and is not particularly limited, but is preferably a hydrophilic cross-linked polymer obtained by cross-linking an unsaturated monomer having a carboxyl group. In addition, it is not limited to a form in which the entire amount is a cross-linked polymer, and may be a composition containing additives, etc.
[0020] The "water absorbent resin" in the present invention may be surface cross-linked (also called post-cross-linked or secondary cross-linked) or may not be surface cross-linked. In the present invention, the water absorbent resin that has been subjected to a predetermined surface cross-linking treatment may be separately referred to as a surface cross-linked water absorbent resin.
[0021] [1-2] "Poly(meth)acrylic acid (salt)" The term "poly(meth)acrylic acid (salt)" in the present invention refers to poly(meth)acrylic acid and / or a salt thereof, and means a crosslinked polymer containing (meth)acrylic acid and / or a salt thereof (hereinafter also referred to as "(meth)acrylic acid (salt)") as a main component as a repeating unit and containing a graft component as an optional component.
[0022] The above "main component" means that the amount (content) of (meth)acrylic acid (salt) used is preferably 50 mol% to 100 mol%, more preferably 70 mol% to 100 mol%, even more preferably 90 mol% to 100 mol%, and particularly preferably substantially 100 mol%, based on the total amount of monomers used in the polymerization.
[0023] Here, the poly(meth)acrylic acid (salt) may be unneutralized, but is preferably a partially or completely neutralized poly(meth)acrylic acid salt, more preferably a monovalent salt, further preferably an alkali metal salt or ammonium salt, even more particularly preferably an alkali metal salt, and particularly preferably a sodium salt.
[0024] (1-3) "Water absorbent" The "water absorbing agent" in the present invention means an absorbent gelling agent for aqueous liquids, containing a water absorbing resin as a main component. The water absorbing agent according to the present invention is suitably used as a sanitary material for absorbing aqueous liquids. The water absorbing agent of the present invention preferably contains 60 to 100 mass%, 70 to 100 mass%, 80 to 100 mass%, or 90 to 100 mass% of the water absorbing resin, and may contain various additives as other components, which will be described later. That is, a water absorbing resin composition in which these components are integrated also falls within the scope of the water absorbing agent of the present invention. The water absorbing agent of the present invention may be referred to as a water absorbing resin, a water absorbing resin powder, and a water absorbing resin particle. In particular, in the definition of the evaluation method described below, when the water absorbing agent is evaluated, the water absorbing resin is defined as a water absorbing agent.
[0025] [1-3] Definition of evaluation method "NWSP" stands for "Non-Woven Standard Procedures-Edition 2015", which was jointly issued by EDANA (European Disposables And Nonwovens Association) and INDA (Association of the Nonwoven Fabrics Industry) to standardize evaluation methods for nonwoven fabrics and their products in the United States and Europe, and indicates standard measurement methods for water-absorbent resins. Unless otherwise specified, in the present invention, the physical properties of the water-absorbent resin are measured in accordance with "Non-Woven Standard Procedures-Edition 2015". Evaluation methods not described in NWSP are measured by the methods and conditions described in the examples.
[0026] [1-3-1] “CRC” (NWSP 241.0.R2(15)) "CRC" is an abbreviation of Centrifuge Retention Capacity, and means the water absorption capacity of a water-absorbent resin under no pressure (sometimes called "water absorption capacity"). Specifically, it means the water absorption capacity (unit: g / g) after 0.2 g of a water-absorbent resin is placed in a nonwoven bag, immersed in a large excess of 0.9 mass% sodium chloride aqueous solution for 30 minutes to allow free swelling, and then drained with a centrifuge (250G) for 3 minutes. For the hydrogel after polymerization and / or gel crushing, 0.4 g of hydrogel is used, the measurement time is changed to 24 hours, and the CRC is obtained by correcting for the solid content.
[0027] [1-3-2] "PSD" (NWSP 220.0.R2(15)) "PSD" is an abbreviation of Particle Size Distribution, and means the particle size distribution of the water absorbent resin measured by sieve classification. The mass median particle diameter (D50) and the logarithmic standard deviation of the particle size distribution (σζ) are measured by a vibration classifier (power supply 60 Hz) in the same manner as described in (3) Mass median particle diameter (D50) and logarithmic standard deviation of the particle size distribution in columns 27 to 28 of U.S. Patent No. 7,638,570.
[0028] [1-3-3] "AAP" (NWSP 242.0.R2(15)) "AAP" is an abbreviation for Absorption Against Pressure, and means the water absorption capacity of a water-absorbent resin under pressure. Specifically, it means the water absorption capacity (unit: g / g) measured under the conditions described in the Examples.
[0029] [1-3-4] “ResidualMonomers” (NWSP 210.0.R2(15)) "Residual Monomers" means the ratio (unit: ppm) of the mass of monomers remaining in the water-absorbent resin (hereinafter referred to as "residual monomers") to the mass of the water-absorbent resin. Specifically, 1.0 g of the water-absorbent resin is added to 200 ml of a 0.9% by mass aqueous sodium chloride solution, and the amount of monomers eluted after stirring for 1 hour is measured using high performance liquid chromatography. The residual monomers in the water-containing gel are the ratio (unit: mass%) of the residual monomer mass obtained by measuring the residual monomer mass by the method described below after performing a polymerization termination operation such as forced cooling as necessary to the mass of the resin solid content of the water-containing gel.
[0030] [1-3-5] "Vortex" The term "vortex" in the present invention is an index representing the water absorption speed of a water absorbent resin, and means the time (unit: seconds) required for 2.0 g of a water absorbent resin to absorb 50 ml of a 0.9 mass % aqueous sodium chloride solution to a predetermined state.
[0031] [1-4] Other In this specification, the term "X to Y" indicating a range means "X or more and Y or less." In addition, unless otherwise noted, the unit of mass "t (ton)" means "metric ton," and "ppm" means "ppm by mass" or "ppm by weight." Furthermore, "mass" and "weight," "parts by mass" and "parts by weight," "% by mass" and "% by weight" are treated as synonyms, respectively. In addition, "acid (salt)" means "acid and / or its salt," and "(meth)acrylic" means "acrylic and / or methacrylic," respectively. [2] Manufacturing method of water absorbing agent The manufacturing method according to the present invention is a manufacturing method of a water-absorbing agent, which comprises obtaining a water-absorbent resin solution obtained from a water-absorbent resin and an alkaline agent, and adding the water-absorbent resin solution to a manufacturing process of a water-absorbing agent. Hereinafter, the water-absorbent resin mixed with the alkaline agent is also referred to as water-absorbent resin A.
[0032] The water absorbent obtained by such a manufacturing method can suppress the deterioration of the basic physical properties of CRC and AAP even when the recovered water absorbent resin is reused in the manufacturing process of the water absorbent. In the water absorbent resin solution, the water absorbent resin A is not in a powdery or gel form but exists as a dissolved water absorbent resin. Since the water absorbent resin is in a dissolved form, the water absorbent resin A becomes a raw material monomer and / or a soluble component derived from the raw material monomer, and by using the solution in the manufacturing process of the water absorbent, it becomes possible to be incorporated (react) into the water absorbent resin by heating in the process. Therefore, it is considered that the deterioration of the physical properties of the obtained water absorbent is suppressed.
[0033] In addition, the water absorbent obtained by conventional fine powder recovery and reuse, such as the method of granulating the recovered fine powder and reusing it, had a tendency to increase the amount of residual monomers. When the water absorbent resin is reused in the process of the water absorbent resin by a conventional method (such as fine powder granulation), the reused water absorbent resin captures monomers from the surrounding monomer aqueous solution or hydrous gel, reducing the reactivity of the monomers, which is thought to lead to an increase in the amount of residual monomers in the final product. On the other hand, when the water absorbent resin solution obtained from the water absorbent resin A and an alkali agent is reused in the process of the water absorbent resin as in the present invention, not only does it not capture the surrounding monomers, but the residual monomers originally contained in the water absorbent resin A can also react with the surrounding unreacted parts (monomers, initiators, etc.) by heating in the process, and it is thought to be effective in reducing the amount of residual monomers. As shown in the examples described later, the amount of residual monomers is reduced in the examples compared to the reference examples in which the water absorbent resin A was not added in the manufacturing process. This effect suggests that the water absorbent resin solution has a new function as an additive in the production of the water absorbent agent.
[0034] According to the above-mentioned production method, the alkaline agent in the water-absorbent resin solution can act as a neutralizing agent for the acid group in the acid group-containing unsaturated monomer or the polymer obtained by polymerizing the acid group-containing unsaturated monomer, and therefore, even if the water-absorbent resin solution is added during the production process, there is little effect on the physical properties of the water-absorbent resin.
[0035] It should be noted that the above assumption does not limit the technical scope of the present invention in any way.
[0036] The water-absorbing resin solution is added in any one of the steps of producing the water-absorbing agent, in other words, the water-absorbing resin solution is used as a part of the raw material of the water-absorbing agent.
[0037] Specifically, the water-absorbent resin solution is preferably added to any one or more of the following production steps (1) to (5). (1) Preparation of an aqueous monomer solution (form 1); (2) Polymerization step (form 2), (3) Gel crushing process (form 3) (4) Fine powder granulation process (Form 4) (5) Surface crosslinking step (Form 5).
[0038] More preferably, the dissolving solution is added to one or more of the production steps (1), (2) and (3), since this further enhances the effects of the present invention.
[0039] More preferably, a water-absorbing resin solution is added to the production process (1) since the water-absorbing speed of the resulting water-absorbing agent is improved.
[0040] Each step will be described in detail below.
[0041] [2-1] Water absorbent resin solution preparation process In this step, a water-absorbent resin is mixed with an alkaline agent, and if necessary, with water, to obtain a water-absorbent resin solution. The water-absorbent resin to be mixed with the alkaline agent is also referred to as water-absorbent resin A.
[0042] The dissolved liquid refers to a state in which the water absorbent resin is almost completely dissolved in the aqueous solution of the alkaline agent, and whether or not it is dissolved can be determined by visual inspection. In other words, when the liquid is visually inspected, it refers to a state in which no precipitate or suspended matter is present and the liquid is a homogeneous solution. More specifically, when the liquid is filtered using a sieve with a nominal mesh size of 850 μm conforming to JIS Z 8801-1:2019, the amount of insoluble matter remaining on the sieve is 10% by weight or less relative to the weight of the dissolved liquid.
[0043] The method for obtaining the water-absorbent resin solution is not particularly limited, and when the water-absorbent resin has a high water content (for example, a hydrous gel), an alkaline agent described below may be directly mixed with the water-absorbent resin. In a preferred embodiment, the water-absorbent resin solution can be obtained by mixing an aqueous solution of the water-absorbent resin and an alkaline agent (hereinafter referred to as an alkaline aqueous solution).
[0044] The method of mixing the water-absorbing resin with the alkaline aqueous solution is not particularly limited, and may be any method such as a method of gradually adding the water-absorbing resin while stirring the alkaline aqueous solution, a method of gradually adding the alkaline aqueous solution while stirring the water-absorbing resin, etc. Furthermore, the water-absorbing resin may be in a form swollen with a certain amount of water or an alkaline aqueous solution before being added to the alkaline aqueous solution.
[0045] The amount (solid content) of the water absorbent resin A added to the alkaline aqueous solution is not particularly limited, but considering the solubility of the water absorbent resin A in the alkaline aqueous solution and the recovery efficiency of the water absorbent resin A, the amount is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, and further more preferably 1 to 3 parts by mass, relative to 100 parts by mass of the alkaline aqueous solution.
[0046] The liquid temperature of the alkaline aqueous solution when the water absorbent resin A is added is not particularly limited, and is about 5 to 100°C. Since the higher the temperature, the more improved the solubility of the water absorbent resin, the temperature of the alkaline aqueous solution is preferably 15°C or higher, and more preferably 20°C or higher. In addition, taking into consideration the heat of neutralization, the upper limit is preferably 100°C or lower, and more preferably 80°C or lower. In order to control the temperature to the above range, the alkaline aqueous solution may be appropriately cooled or heated.
[0047] Furthermore, when the water-absorbent resin A is mixed with an alkaline aqueous solution, dissolution of the water-absorbent resin is promoted by applying UV light or ultrasonic waves. Also, dissolution of the water-absorbent resin is promoted by using an oxidizing agent such as hydrogen peroxide in combination.
[0048] The alkaline agent may be a compound that is water-soluble and shows alkalinity when made into an aqueous solution, and examples of the alkaline agent include inorganic alkaline agents such as hydroxides of alkali metals such as sodium hydroxide, ammonium hydroxide, potassium hydroxide, and lithium hydroxide, and hydroxides of alkaline earth metals such as calcium hydroxide and magnesium hydroxide; and organic alkaline agents such as monomethylamine, diethanolamine, triethanolamine, monoisopropanolamine, diisopropanolamine, DBU (1,8-diazabicyclo[5,4,0]-7-undecene), DBN (1,5-diazabicyclo[4,3,0]-5-nonene), tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, and triethylbutylammonium hydroxide. From the viewpoint of sufficiently dissolving the water-absorbing resin A, an alkaline agent that shows strong alkalinity when made into an aqueous solution is preferred, and an inorganic alkaline agent is preferred. Specifically, an alkaline agent that has a pH of 10 or more in an alkaline aqueous solution is preferred. Among these, hydroxides of alkali metals are preferred, sodium hydroxide and / or potassium hydroxide are more preferred, and sodium hydroxide is even more preferred. The above-mentioned hydroxides of alkali metals can be used as an alkaline agent to suitably use as a neutralizing agent for obtaining an acid group-containing unsaturated monomer (salt), which is the main raw material of a water absorbent resin. These alkaline agents can be used alone or in combination of two or more. In addition, from the viewpoint of the performance of the obtained water absorbent resin, it is preferred that the alkaline agent is the same as the basic substance used as a neutralizing agent for an acid group-containing unsaturated monomer and / or a polymer obtained by polymerizing the monomer, which will be described later.
[0049] The concentration of the alkaline agent in the alkaline aqueous solution is preferably 1% by mass or more, more preferably 5% by mass or more, from the viewpoint of sufficiently proceeding with the neutralization of the acid group-containing unsaturated monomer / polymer obtained by polymerization of the monomer, and is preferably 50% by mass or less, more preferably 30% by mass or less, taking into consideration the solubility of the water absorbent resin A. The concentration of the alkaline agent in the alkaline aqueous solution is preferably 1 to 50% by mass, more preferably 5 to 30% by mass. The pH of the alkaline aqueous solution is preferably 10 or more, more preferably 12 or more.
[0050] The water used in the alkaline aqueous solution may be, for example, deionized water (ion-exchanged water), pure water, ultrapure water, distilled water, or the like, with deionized water (ion-exchanged water) being preferred.
[0051] The alkaline aqueous solution may contain a small amount of a hydrophilic solvent. Examples of the hydrophilic solvent include alcohols such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, and t-butyl alcohol. The solvent used in combination is used in an amount of, for example, 0 to 10% by mass relative to water. From the viewpoint of recovery efficiency of the water absorbent resin A, the water and / or the hydrophilic solvent may be distilled off after dissolving the water absorbent resin A in the alkaline aqueous solution.
[0052] The method for obtaining the water-absorbing resin A is not particularly limited. The water-absorbing resin A may be obtained in the manufacturing process of the water-absorbing agent of the present invention, or may be obtained in another manufacturing process of a water-absorbing resin or a water-absorbing agent different from the present invention. In addition, a commercially available product or a stock water-absorbing resin may be used as the water-absorbing resin A. The water-absorbing resin A may be manufactured to have the physical properties and / or particle size described below according to a known manufacturing method (for example, a manufacturing method of a water-absorbing agent described later) and manufacturing conditions. For example, the water-absorbing resin A may be obtained by aqueous solution polymerization or reverse phase suspension polymerization. Examples of the water-absorbing resin A include fine powder formed during the manufacturing process, a final product, and an absorbent resin taken out from a commercially available diaper. The shape of the water-absorbing resin A is not particularly limited, and examples include an irregularly crushed shape, a spherical shape, a sausage shape, and granulated shapes thereof, and a broccoli shape. In addition, the water-absorbing resin A may be in a gel state after absorbing water, and includes intermediate products obtained in the manufacturing process of known water-absorbing resins, and is not limited to the definition of the water-absorbing resin in [1-1]. For example, when an apparatus to which a water-absorbing resin is attached, which is used in a manufacturing process of a water-absorbing agent, is washed with water, etc., a gelled water-absorbing resin A can be obtained. Also, when a hydrogel attached to a belt during continuous belt polymerization described later is washed with water, a gelled water-absorbing resin A can be obtained. Also, a gelled water-absorbing resin A can be obtained from used diapers.
[0053] The monomer composition used for the polymer constituting the water absorbent resin A is preferably the same as the monomer composition constituting the polymer contained in the water absorbent resin produced by the present invention. Therefore, the water absorbent resin A is preferably a water absorbent resin mainly composed of a polymer (preferably a polymer polymerized from (meth)acrylic acid (salt)) obtained by polymerizing an acid group-containing unsaturated monomer (salt). Here, the main component refers to 50 mol% or more in the water absorbent resin (upper limit 100 mol%), preferably 70 mol% to 100 mol%, more preferably 90 mol% to 100 mol%. The acid group in the acid group-containing unsaturated monomer is not particularly limited, and examples and preferred forms are the same as those of the acid group-containing unsaturated monomer described in the section on the monomer aqueous solution preparation step described later.
[0054] The polymer obtained by polymerizing the acid group-containing unsaturated monomer (salt) may be unneutralized or neutralized. A partially or completely neutralized poly(meth)acrylic acid (salt)-based polymer is preferable. A poly(meth)acrylic acid (salt)-based polymer is more preferable, more preferably, neutralized with an alkali metal salt or ammonium salt, even more preferably, with an alkali metal salt, and even more preferably, with a sodium salt. Here, the poly(meth)acrylic acid (salt)-based polymer refers to one in which the main component of the monomer mixture used during polymerization is (meth)acrylic acid. Here, the main component refers to 50 mol % or more (upper limit 100 mol %) in the monomer mixture used during polymerization, preferably 70 mol % to 100 mol %, and more preferably 90 mol % to 100 mol %.
[0055] The neutralization rate of the polymer obtained by polymerizing the acid group-containing unsaturated monomer (salt) is appropriately adjusted by a known method, but is preferably 40 mol% or more, more preferably 40 mol% to 80 mol%, even more preferably 45 mol% to 78 mol%, and particularly preferably 50 mol% to 75 mol%.
[0056] The polymer obtained by polymerizing the acid group-containing unsaturated monomer (salt) is preferably a crosslinked polymer crosslinked by an internal crosslinking agent, as described in the section on the method for producing the water absorbent below. That is, preferably, the water absorbent resin A contains a crosslinked polymer obtained by polymerizing the acid group-containing unsaturated monomer (salt). As described below, in order to improve the physical properties of the water absorbent resin, a crosslinked polymer is often formed by using an internal crosslinking agent when polymerizing the acid group-containing unsaturated monomer. Fine powders and the like generated during the production of the water absorbent resin containing the internally crosslinked crosslinked polymer may be collected. In this way, when the water absorbent resin containing the internally crosslinked crosslinked polymer is collected, the water absorption rate of the obtained water absorbent resin is improved by uniformly treating it with an alkaline agent as in the present invention. The crosslinked chain is broken by mixing the internally crosslinked polymer with an alkaline aqueous solution. By making the polymer into a chain in this way, particularly when it is contained in a monomer aqueous solution, the thickening effect of the monomer aqueous solution is exhibited as described below, and the water absorption rate of the obtained water absorbent is further improved. From the above viewpoint, the internal crosslinking agent is preferably a compound having an ester bond in its molecule or forming an ester bond by crosslinking polymerization reaction. More preferably, the internal crosslinking agent is a compound having an ester bond in its molecule, and even more preferably a (meth)acrylate compound. The type, amount, etc. of the internal crosslinking agent used in producing the crosslinked polymer, and the preferred form thereof are the same as those described in the section on the preparation process of the aqueous monomer solution of the water absorbent resin below.
[0057] In addition, the polymer obtained by polymerizing the acid group-containing unsaturated monomer (salt) may or may not be subjected to surface crosslinking as described in the section on the surface crosslinking step of the water absorbent resin below. For example, if the hydrogel-like water absorbent resin before the drying step is collected, or if the water absorbent resin powder removed during the classification step before the surface crosslinking after the drying step (such a water absorbent resin powder may be called a base polymer) is collected, the surface crosslinking is not carried out, and if the water absorbent resin powder removed during the classification step after the surface crosslinking is collected, the surface crosslinked water absorbent resin powder is surface crosslinked. The type of the surface crosslinking agent, the amount of the surface crosslinking agent used, the method of surface crosslinking, and the preferred forms thereof are the same as those described in the section on the surface crosslinking step of the water absorbent resin below. From the viewpoint of reducing the residual monomer, a so-called base polymer that is not surface crosslinked with the acid group-containing unsaturated monomer (salt) may be used as the water absorbent resin A. In addition, the base polymer may be a base polymer before the classification or sizing step, or a base polymer after the classification or sizing step.
[0058] From the viewpoint of fluidity and mixability, the solid content of the water absorbent resin A in the form of a powder is preferably 75% by mass or more, more preferably 80% by mass or more, and even more preferably 85% by mass or more. Although the upper limit is not particularly limited, the solid content is usually 99.9% by mass or less, and preferably 99.5% by mass or less. The method for measuring the solid content of the water absorbent resin will be described later in the examples.
[0059] The CRC (centrifuge retention capacity) of the water absorbent resin A is preferably 5 g / g or more, more preferably 10 g / g or more, further preferably 15 g / g or more, and particularly preferably 18 g / g or more, calculated as solid content. When the CRC is within the above range, the dissolution rate is improved and the process efficiency can be increased. The upper limit of the CRC of the water absorbent resin A is not particularly limited, but is, for example, 80 g / g or less.
[0060] The water absorbent resin A may contain water or additives described in the step of adding other additives to the water absorbent resin described later. That is, the water absorbent resin A is not limited to a form in which 100% is a polymer, and the water absorbent resin A may contain water or other minor components (e.g., inorganic fine particles, etc.) that are secondary raw materials of the water absorbent resin powder.
[0061] Preferably, the water absorbent resin A is unnecessary water absorbent resin powder (e.g., coarse particles (having a mass average particle diameter of 850 μm or more) and crushed particles thereof, fine powder having a mass average particle diameter of 150 μm or less, or water absorbent resin powder having deviated from desired physical properties (e.g., nonstandard water absorbent resin powder) classified in a classification step or a sizing step (a drying step, a classification step after a crushing step, a classification step after a surface crosslinking step (after an optional additive addition step), a sizing step, etc.) carried out in a production step of a known water absorbent resin, and more preferably is fine powder. That is, it is preferable that the fine powder removed in the classification step is collected and provided to this step as a recovered water absorbent resin powder.
[0062] The fine powder is a particulate or powdered water absorbent resin. It is known that the water absorption performance, handling property, and usability of a powdered or particulate water absorbent resin vary depending on the particle size, particle size distribution, and the like. Therefore, a powdered or particulate water absorbent resin having a properly controlled particle size and particle size distribution is required. In particular, in the application of sanitary products such as paper diapers, it is considered that a water absorbent resin powder having a small content of fine powder (for example, a particle size distribution of 850 to 150 μm) is preferable from the viewpoint of water absorption capacity under pressure and liquid permeability. For this reason, the fine powder may be removed by an operation such as classification. Since it is not preferable to discard the removed fine powder in this way from the viewpoint of cost, it is preferable to recycle the fine powder during the process, and in that case, the method of the present invention can be applied.
[0063] The fine powder applicable to the water absorbent resin A of the present invention has a mass average particle diameter (D50) determined by sieve classification of preferably less than 150 μm, more preferably 10 to 150 μm, and even more preferably 20 to 140 μm. The ratio of particles having a particle diameter of less than 150 μm contained in this fine powder (sieve permeability of JIS standard sieve with 150 μm mesh) is preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, and ideally 100 mass%.
[0064] [2-2] Manufacturing process of crosslinked polymer using acid group-containing unsaturated monomer In the process for producing the crosslinked polymer, the water-absorbent resin solution obtained in [2-1] (hereinafter, also simply referred to as solution) may be added, and this embodiment is preferable.
[0065] When a dissolving solution is added in the process for producing the present crosslinked polymer, it can be added in either or both of the step of preparing an aqueous monomer solution (Mode 1) and the polymerization step (Mode 2).
[0066] In the first and second forms, the timing of adding the dissolving solution is different. In either form, the alkaline agent in the dissolving solution also acts as a neutralizing agent for the acid group in the acid group-containing unsaturated monomer or the polymer obtained by polymerizing the acid group-containing unsaturated monomer. That is, the water-absorbent resin dissolving solution is used as a part of the raw material of the water-absorbing agent. The dissolving solution is added either before the start of the polymerization reaction, during the polymerization reaction, or after the end of the polymerization reaction. When the dissolving solution is used as a neutralizing agent in the case of multi-stage neutralization, it may be used at any timing, but it is preferable to use it as a neutralizing agent in the first neutralization.
[0067] Preferred embodiments will now be described in detail.
[0068] [2-2-1: Preparation of monomer aqueous solution] This is a process for preparing an aqueous solution containing an acid group-containing unsaturated monomer as a main component (hereinafter referred to as "aqueous monomer solution"). Note that, a slurry solution of the monomer (a dispersion solution having a monomer concentration exceeding a saturation concentration) can also be used within a range in which the water absorption performance of the obtained water absorbing agent is not deteriorated, and for the sake of convenience in this section, such a slurry solution is also included in the aqueous monomer solution.
[0069] The above-mentioned "main component" means that the amount (content) of the acid group-containing unsaturated monomer used is usually 50 mol % or more, preferably 70 mol % or more, and more preferably 90 mol % or more (upper limit: 100 mol %) based on the total monomers (excluding the internal crosslinking agent) to be subjected to the polymerization reaction of the water absorbent resin.
[0070] The acid group in the acid group-containing unsaturated monomer is not particularly limited, but examples thereof include a carboxyl group, a sulfone group, and a phosphoric acid group. Examples of the acid group-containing unsaturated monomer include (meth)acrylic acid, (anhydrous) maleic acid, itaconic acid, cinnamic acid, vinyl sulfonic acid, allyl toluene sulfonic acid, vinyl toluene sulfonic acid, styrene sulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, 2-(meth)acryloyloxyethanesulfonic acid, 2-(meth)acryloyloxypropanesulfonic acid, and 2-hydroxyethyl (meth)acryloyl phosphate. From the viewpoint of water absorption performance, preferred are (meth)acrylic acid, (anhydrous) maleic acid, itaconic acid, and cinnamic acid, and more preferred is (meth)acrylic acid.
[0071] It is preferable that the acid groups contained in the acid group-containing unsaturated monomer contained in the aqueous monomer solution are partially or entirely neutralized. The salt of the acid group-containing unsaturated monomer is appropriately selected from salts with inorganic cations such as alkali metal salts, alkaline earth metal salts, and ammonium salts, and salts with basic substances such as amine-based organic compounds having amino groups or imino groups. Among them, salts with monovalent cations are more preferable, and at least one selected from alkali metal salts, ammonium salts, and amine salts are more preferable, and alkali metal salts are even more preferable. Among the alkali metal salts, at least one selected from sodium salts, lithium salts, and potassium salts is even more preferable, and sodium salts are particularly preferable.
[0072] The neutralizing agent used to neutralize the acid group-containing unsaturated monomer is not particularly limited, but may be a salt containing a cation constituting the salt of the acid group-containing insoluble monomer, and may be appropriately selected and used from inorganic salts such as sodium hydroxide, potassium hydroxide, sodium carbonate, ammonium carbonate, and basic substances such as amine-based organic compounds having amino groups or imino groups. Two or more basic substances may be used in combination as the neutralizing agent. The monomer in the present invention is a concept that includes neutralized salts, unless otherwise specified.
[0073] In the embodiment 1, by mixing the water-absorbent resin solution with the aqueous monomer solution, the solution also serves as a neutralizing agent for the acid group-containing unsaturated monomer.
[0074] From the viewpoint of water absorption performance, the number of moles of the neutralization salt relative to the total number of moles of the acid group-containing unsaturated monomer and its neutralization salt (hereinafter referred to as "neutralization rate") is adjusted to be preferably 40 mol% or more, more preferably 40 mol% to 80 mol%, even more preferably 45 mol% to 78 mol%, and particularly preferably 50 mol% to 75 mol%. The suitable range of the neutralization rate is the same in the case of post-neutralization (neutralization in the hydrous gel polymer).
[0075] The method for adjusting the neutralization rate includes a method of mixing a neutralized salt of an acid group-containing unsaturated monomer obtained by mixing an acid group-containing unsaturated monomer and a water absorbent resin solution with an acid group-containing insoluble monomer; a method of adding a water absorbent resin solution and / or a known neutralizing agent to an acid group-containing unsaturated monomer; a method of adding a water absorbent resin solution to an acid group-containing unsaturated monomer and then adding a known neutralizing agent; a method of using a partially neutralized salt of an acid group-containing unsaturated monomer (i.e., a mixture of an acid group-containing unsaturated monomer and its neutralizing salt) previously adjusted to a predetermined neutralization rate using a water absorbent resin solution as the whole or part of the neutralizing agent; etc. Also, these methods may be combined.
[0076] The neutralization rate may be adjusted before the start of the polymerization reaction of the acid group-containing unsaturated monomer (embodiment of form 1), during the polymerization reaction of the acid group-containing unsaturated monomer (embodiment of form 2), or on the hydrogel-like crosslinked polymer obtained after the completion of the polymerization reaction of the acid group-containing unsaturated monomer (post-neutralization, embodiment of form 2). The neutralization rate may be adjusted by selecting one of the stages before the start of the polymerization reaction, during the polymerization reaction, or after the completion of the polymerization reaction, or the neutralization rate may be adjusted in multiple stages. That is, the neutralizing agent may be added once or in multiple stages (for example, two-stage neutralization). Two-stage neutralization is a method in which the neutralizing agent is added in two stages. In any of the embodiments, as long as a water-absorbent resin solution is used as the whole or part of the neutralizing agent for the acid group-containing unsaturated monomer or its polymer, it is included in the scope of the present invention.
[0077] The aqueous monomer solution may contain a monomer other than the acid group-containing unsaturated monomer.
[0078] The monomer other than the acid group-containing unsaturated monomer may be any compound that can be polymerized to become a water-absorbing resin. For example, amide group-containing unsaturated monomers such as (meth)acrylamide, N-ethyl (meth)acrylamide, and N,N-dimethyl (meth)acrylamide; amino group-containing unsaturated monomers such as N,N-dimethylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylate, and N,N-dimethylaminopropyl (meth)acrylamide; mercapto group-containing unsaturated monomers; phenolic hydroxyl group-containing unsaturated monomers; lactam group-containing unsaturated monomers such as N-vinylpyrrolidone; etc.
[0079] The monomer concentration in the aqueous monomer solution (=total monomer amount / (total monomer amount+total polymerization solvent amount (usually water), where the monomer includes monomers other than the acid group-containing unsaturated monomer) is preferably 10 mass % to 90 mass %, more preferably 20 mass % to 80 mass %, further preferably 30 mass % to 70 mass %, particularly preferably 40 mass % to 60 mass %, from the viewpoint of physical properties and productivity of the water absorbent resin. Hereinafter, the monomer concentration may be referred to as "monomer concentration".
[0080] The aqueous monomer solution prepared in this step may contain a polymerization inhibitor, an internal crosslinking agent, etc. As described above, it is preferable that the aqueous monomer solution contains an internal crosslinking agent.
[0081] Polymerization inhibitor The monomer used in the polymerization preferably contains a small amount of a polymerization inhibitor from the viewpoint of polymerization stability. A preferred polymerization inhibitor is p-methoxyphenol. The amount of the polymerization inhibitor contained in the monomer (particularly acrylic acid and its salts) is usually 1 ppm to 250 ppm, preferably 10 ppm to 160 ppm, and more preferably 20 ppm to 80 ppm.
[0082] Internal crosslinking agent The internal crosslinking agent adjusts the water absorption performance and gel strength of the resulting water absorbent resin when absorbing water.
[0083] The internal crosslinking agent may have a total of two or more unsaturated bonds or reactive functional groups in one molecule. For example, examples of internal crosslinking agents having a plurality of polymerizable unsaturated groups (copolymerizable with monomers) in the molecule include N,N-methylenebis(meth)acrylamide, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, glycerin (meth)acrylate, glycerin acrylate methacrylate, ethylene oxide modified trimethylolpropane tri(meth)acrylate, pentaerythritol hexa(meth)acrylate, triallyl cyanurate, triallyl isocyanurate, triallyl phosphate, trimethylolpropane di(meth)allyl ether, poly(meth)allyl ether of polyol having 2 to 10 carbon atoms, pentaerythritol triallyl ether, and tetraallyloxyethane. Examples of internal crosslinking agents having multiple reactive functional groups (which can react with functional groups of monomers (e.g., carboxy groups)) in the molecule include triallylamine, polyallyloxyalkane, (poly)ethylene glycol diglycidyl ether, glycerol diglycidyl ether, ethylene glycol, polyethylene glycol, propylene glycol, glycerin, 1,4-butanediol, pentaerythritol, ethylenediamine, ethylene carbonate, propylene carbonate, and polyethyleneimine (note that here, cyclic carbonates such as ethylene carbonate are crosslinking agents that further generate functional groups OH by reacting with carboxyl groups). Examples of internal crosslinking agents having polymerizable unsaturated groups and reactive functional groups in the molecule include glycidyl (meth)acrylate. Two or more of these may be used in combination.
[0084] Among these internal crosslinking agents, from the viewpoint of the effects of the present invention, a compound having a plurality of polymerizable unsaturated groups in the molecule is preferable, a compound having a (poly)alkylene structural unit in the molecule is more preferable, a compound having a polyethylene glycol structural unit is even more preferable, and an acrylate compound having a polyethylene glycol structural unit is particularly preferable. In the hydrogel obtained by using these internal crosslinking agents, the effect that the water absorption capacity is easily improved by drying is obtained.
[0085] The amount of the internal crosslinking agent used is appropriately set depending on the type of monomer and the internal crosslinking agent. From the viewpoint of gel strength of the obtained water absorbent resin, the amount is preferably 0.001 mol% or more, more preferably 0.005 mol% or more, and even more preferably 0.01 mol% or more, based on the monomer. From the viewpoint of improving the water absorption performance of the water absorbent resin, the amount is preferably 5 mol% or less, more preferably 2 mol% or less. Note that, under polymerization conditions where the self-crosslinking reaction of the monomer is effective, the internal crosslinking agent may not be used.
[0086] When an internal crosslinking agent is added, the timing of adding the internal crosslinking agent to the acid group-containing monomer is not particularly limited, and the internal crosslinking agent may be added at any time before the start of polymerization. For example, in the case of polymerization form 1, the internal crosslinking agent may be added before or after the addition of the dissolving solution.
[0087] Other substances Within the scope of achieving the object of the present invention, the following substances (hereinafter referred to as "other substances") can also be added to the aqueous monomer solution.
[0088] Specific examples of other substances include chain transfer agents such as thiols, thiolic acids, secondary alcohols, amines, and hypophosphites; foaming agents such as carbonates, bicarbonates, azo compounds, and bubbles; chelating agents such as ethylenediaminetetra(methylenephosphinic acid) and metal salts thereof, ethylenediaminetetraacetic acid and metal salts thereof, and diethylenetriaminepentaacetic acid and metal salts thereof; hydrophilic polymers such as polyacrylic acid (salts) and crosslinked products thereof (for example, fine powders made of water-absorbent resins), starch, cellulose, starch-cellulose derivatives, and polyvinyl alcohol. The other substances may be used alone or in combination of two or more.
[0089] The amount of other substances used is not particularly limited, but the total concentration of other substances is preferably 10% by mass or less, more preferably 0.001% by mass to 5% by mass, and particularly preferably 0.01% by mass to 1% by mass, relative to the monomer.
[0090] (dissolved oxygen) It is also preferable to reduce the dissolved oxygen in the aqueous monomer solution before polymerization by raising the temperature or replacing it with an inert gas. For example, the dissolved oxygen is preferably reduced to 5 ppm or less, more preferably 3 ppm or less, and particularly preferably 1 ppm or less.
[0091] It is also possible to disperse bubbles (particularly the above-mentioned inert gases) in the aqueous monomer solution, in which case the polymerization reaction will result in foaming polymerization.
[0092] (Form 1) In the embodiment 1, the water absorbent resin A is added in the step of preparing the aqueous monomer solution. That is, an aqueous monomer solution containing a water absorbent resin solution and an acid group-containing unsaturated monomer is obtained, and the aqueous monomer solution is used to polymerize the acid group-containing unsaturated monomer in the next step.
[0093] In the embodiment 1, the water absorbent resin solution is added to the monomer aqueous solution, and the viscosity of the aqueous solution is increased by the polymer component derived from the water absorbent resin A contained in the solution. Due to such an increase in viscosity, air bubbles generated during polymerization are difficult to escape, and the surface area of the obtained water absorbent resin is increased. Therefore, the water absorption speed of the water absorbent resin is further improved.
[0094] In the first embodiment, the dissolving solution and the acid group-containing unsaturated monomer are mixed to form an aqueous monomer solution. Here, examples of the mixing include a form in which the acid group-containing unsaturated monomer and the dissolving solution are added together and mixed; a form in which the acid group-containing unsaturated monomer aqueous solution is formed, and then the dissolving solution is added to the aqueous acid group-containing unsaturated monomer solution; and the like. In the case of a form in which the dissolving solution is added to the aqueous acid group-containing unsaturated monomer solution after the aqueous acid group-containing unsaturated monomer solution is formed, the polymerization may be started after the entire amount of the dissolving solution is added to the aqueous acid group-containing unsaturated monomer solution, or the polymerization may be performed while the aqueous acid group-containing unsaturated monomer solution and the dissolving solution are separately and continuously supplied. Preferably, the polymerization is performed after the aqueous acid group-containing unsaturated monomer solution and the dissolving solution are separately and continuously supplied, for example, by line mixing, and then the polymerization is performed. In addition, a neutralizing agent aqueous solution may be added in advance to the acid group-containing unsaturated monomer to form an aqueous acid group-containing unsaturated monomer solution, and then the dissolving solution is added to the aqueous acid group-containing unsaturated monomer solution.
[0095] The amount of the dissolving solution added to the acid group-containing monomer is appropriately set in consideration of the degree of neutralization, the effect on the physical properties of the resulting water absorbent resin, recovery efficiency, etc., and is, for example, 1 to 400 parts by mass relative to 100 parts by mass of acrylic acid.
[0096] The temperature of the aqueous alkaline solution when the dissolving solution is added to the aqueous monomer solution is preferably 5 to 100°C, more preferably 10 to 60°C, and even more preferably 15 to 40°C.
[0097] [2-2-2: Polymerization step] This step is a step in which the aqueous monomer solution is polymerized and then, if necessary, neutralized to obtain a hydrogel polymer (hereinafter, sometimes referred to as "hydrogel").
[0098] The polymerization reaction can be carried out by adding a polymerization initiator. The monomer aqueous solution may contain a polymerization initiator. The polymerization initiator is appropriately selected depending on the polymerization form and the like, and is not particularly limited. For example, a thermally decomposable polymerization initiator, a photodecomposable polymerization initiator, or a combination of these, or a redox-based polymerization initiator combined with a reducing agent that promotes the decomposition of the polymerization initiator, etc., can be mentioned. Specifically, one or more of the polymerization initiators disclosed in U.S. Pat. No. 7,265,190 are used. In addition, from the viewpoint of the handling of the polymerization initiator and the physical properties of the water-absorbing resin, preferably a peroxide or an azo compound, more preferably a peroxide, and even more preferably a persulfate is used.
[0099] The amount of the polymerization initiator used is preferably 0.001 mol % to 1 mol %, more preferably 0.001 mol % to 0.5 mol %, based on the monomer. When redox polymerization is performed as necessary, the amount of the reducing agent used in combination with the oxidizing agent is preferably 0.0001 mol % to 0.02 mol %, based on the monomer.
[0100] In addition to the method of carrying out a polymerization reaction by adding the polymerization initiator, there is a method of irradiating with active energy rays such as radiation, electron beams, ultraviolet rays, etc. In addition, irradiation with active energy rays may be carried out in combination with the addition of a polymerization initiator.
[0101] The polymerization form is not particularly limited. From the viewpoint of water absorption performance and ease of polymerization control, etc., preferably, droplet polymerization in a gas phase, aqueous solution polymerization, reversed-phase suspension polymerization (here, droplet polymerization in a hydrophobic organic solvent is also included as an example of reversed-phase suspension), more preferably, aqueous solution polymerization, reversed-phase suspension polymerization, and even more preferably, aqueous solution polymerization can be mentioned. For details on reversed-phase suspension polymerization,
[0016] to
[0033] of Japanese Patent No. 4969778, specifically, Example 1 can be referred to. Among them, continuous aqueous solution polymerization is particularly preferable, and examples thereof include continuous belt polymerization and continuous kneader polymerization. By adopting continuous aqueous solution polymerization, the production efficiency of the water absorbent resin is improved.
[0102] In addition, preferred forms of aqueous solution polymerization include "high-temperature initiated polymerization" and "high-concentration polymerization." "High-temperature initiated polymerization" refers to a form in which polymerization is initiated at a temperature of the aqueous monomer solution of preferably 30°C or higher, more preferably 35°C or higher, even more preferably 40°C or higher, and particularly preferably 50°C or higher (upper limit is the boiling point), and "high-concentration polymerization" refers to a form in which polymerization is performed at a monomer concentration of preferably 30% by mass or higher, more preferably 35% by mass or higher, even more preferably 40% by mass or higher, and particularly preferably 45% by mass or higher (upper limit is the saturated concentration). These polymerization forms can also be used in combination.
[0103] In the droplet polymerization in the gas phase, the polymerization can be carried out under an air atmosphere, but from the viewpoint of the color tone of the obtained water absorbent resin, it is preferable to carry out the polymerization under an inert gas atmosphere such as nitrogen or argon. In this case, for example, it is preferable to control the oxygen concentration in the gas phase to 1 volume % or less.
[0104] By polymerization of the acid group-containing unsaturated monomer, a hydrogel-like polymer (hereinafter, also simply referred to as hydrogel) is obtained.
[0105] (Form 2) In the second embodiment, the solution is added in the polymerization step. Here, the timing of adding the solution is not particularly limited, but it is preferable to add the water-absorbent resin solution to the hydrogel (i.e., before the drying treatment step). Specifically, the water-absorbent resin solution is added during polymerization of a monomer aqueous solution containing an acid group-containing unsaturated monomer (specifically, for example, in the case where polymerization and gel crushing are performed simultaneously as in continuous kneader polymerization, the water-absorbent resin solution is added in the gel crushing step during the polymerization step); the water-absorbent resin solution is added to a polymer obtained by polymerizing a monomer aqueous solution containing an acid group-containing unsaturated monomer; and the like. The amount of the water-absorbent resin solution added to the hydrogel polymer is appropriately set in consideration of the degree of neutralization, the effect on the physical properties of the obtained water-absorbent resin, the recovery efficiency, and the like, and is, for example, 1 to 100 parts by mass with respect to 100 parts by mass of the hydrogel polymer.
[0106] [2-3] Gel crushing process This step is a step of crushing the hydrogel polymer obtained in the polymerization step simultaneously with and / or after polymerization to obtain a particulate hydrogel crosslinked polymer (hereinafter, "particulate hydrogel"). This step may be performed two or more times to obtain a particulate hydrogel of a predetermined particle size. In addition, this step may not be performed when a particulate hydrogel of a desired particle size is obtained in the polymerization step, such as in reverse phase suspension polymerization or gas phase polymerization. In addition, if necessary, a shredding step may be performed after the polymerization step and before the gel crushing step, in which the hydrogel crosslinked polymer is cut or roughly crushed into a size that can be put into a gel crushing device using a roller cutter, a guillotine cutter, or the like. In particular, when the polymerization step is belt polymerization and a sheet-like or block-like hydrogel is obtained, it is preferable to perform the shredding step.
[0107] (Form 3) The addition of the water-absorbent resin solution of the present invention may be carried out simultaneously with the present gel crushing step (form 3). The water-absorbent resin solution may be added in a shredding step in which the water-absorbent resin is cut or roughly crushed to a size that can be put into a gel crushing device described later before the gel crushing step. When the water-absorbent resin solution is added in the gel crushing step, it is preferable that the water-absorbent resin solution is added before the gel crushing step and / or during the gel crushing step and is thoroughly mixed during gel crushing. The amount of the water-absorbent resin solution added to the hydrogel polymer is appropriately set in consideration of the degree of neutralization, the effect on the physical properties of the obtained water-absorbent resin, the recovery efficiency, etc., and is, for example, 1 to 100 parts by mass with respect to 100 parts by mass of the hydrogel polymer. In addition, when only a part of the acid group-containing unsaturated monomer is neutralized in the monomer aqueous solution preparation step (2-2-1) or polymerization is carried out in (2-2-2) without neutralization, neutralization can be carried out in the present gel crushing step. Preferably, the water-absorbent resin solution of the present invention can be used in part or in whole as a neutralizing agent. In addition, a mixture and / or granules obtained by adding an aqueous liquid (solvent) to the coarse particles removed in the sizing step described below or the fine powder obtained in the fine powder granulation step may be added to the gel crushing step.
[0108] In the production method of the present invention, the type of gel grinding device is not particularly limited as long as a particulate hydrogel of a predetermined particle size can be obtained without impairing the water absorption performance. For example, a gel grinder equipped with multiple rotating agitating blades such as a batch or continuous double-arm kneader, a single-screw extruder, a twin-screw extruder, a meat chopper, etc. can be mentioned.
[0109] A gel fluidizer may be added before and / or during the gel crushing step. The addition of the gel fluidizer suppresses adhesion between hydrogel particles in the drying step described below, and improves the water absorption rate of the resulting water absorbent resin. In addition, the load in the crushing step after drying described below is reduced, and the amount of fine powder generated is reduced. Note that, even in an embodiment that does not require a gel crushing step, the above effect can be obtained by adding a gel fluidizer to the particulate hydrogel before the drying step.
[0110] Examples of the gel fluidizing agent include anionic, cationic, nonionic and amphoteric surfactants, their low molecular weight and polymeric surfactants, and polymeric lubricants. Polymeric lubricants are another name for specific nonionic surfactants, and examples thereof include polyalkylene oxides and their maleic anhydride modified products. A surfactant (particularly a non-polymeric surfactant) and a polymeric lubricant may be used in combination.
[0111] The type and amount of the gel fluidizing agent are appropriately adjusted in consideration of the fluidity of the particulate hydrogel in the gel crushing step and the drying step. In addition, as form 3, when the water-absorbent resin dissolving liquid is added to the hydrogel in this step, it may be mixed with the gel fluidizing agent and added, or may be added separately to the hydrogel. As described above, the hydrogel may be crushed simultaneously with the polymerization, in which case forms 2 and 3 are carried out in parallel.
[0112] The polymerization rate of the particulate hydrogel is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 98% by mass or more, from the viewpoint of suppressing aggregation during drying of the particulate hydrogel-like crosslinked polymer and reducing the residual monomer in the obtained water-absorbent resin. When a drying step is carried out using a hydrogel having a low polymerization rate containing a large amount of unreacted monomer, a polymerization reaction may proceed during drying, and large-sized gel particles may be regenerated or by-produced from small-sized gel particles. The large-sized gel particles cause problems such as a decrease in the water absorption rate of the obtained water-absorbent resin, large particles of the dried product, and fine powder generation due to re-crushing to the target product particle size. In order to avoid this problem, it is preferable to set the polymerization rate of the hydrogel to the above range.
[0113] The upper limit of the polymerization rate of the particulate hydrogel is not particularly limited, and 100% by mass is ideal, but a long polymerization time and strict polymerization conditions are required for a high polymerization rate, which may lead to a decrease in productivity and physical properties, so the upper limit is 99.95% by mass, further 99.9% by mass, and usually about 99.8% by mass. Typically, it is 98 to 99.99% by mass.
[0114] The CRC (centrifuge retention volume) of the polymer of the particulate hydrogel is preferably 5 g / g to 80 g / g, more preferably 10 g / g to 50 g / g, further preferably 15 g / g to 45 g / g, and particularly preferably 20 g / g to 40 g / g, calculated as solid content. Note that the term "solid content conversion" refers to physical properties converted into physical properties per solid content of the water-absorbent resin in the hydrogel after measuring various physical properties such as CRC in the hydrogel (for example, for a hydrogel with a water content of 50% (solid content of 50%), the physical properties are converted into twice the measured values of the physical properties in the hydrogel).
[0115] The solid content of the particulate hydrogel (hereinafter, gel solid content) is preferably 25% by mass or more. From the viewpoints of suppressing aggregation of hydrogel particles after gel crushing, energy required for crushing, drying efficiency, and absorption performance, the gel solid content is more preferably 25% by mass to 75% by mass, even more preferably 30% by mass to 70% by mass, even more preferably 35% by mass to 65% by mass, and particularly preferably 40% by mass to 60% by mass. The gel solid content is measured by the method described in the examples below.
[0116] [2-4] Drying process This step is a step of drying the particulate hydrogel obtained in the above polymerization step and / or gel crushing step to a desired resin solid content to obtain a dry polymer. The resin solid content is determined from the loss on drying (the change in mass when 1 g of the water-absorbent resin is heated at 180°C for 3 hours), and is preferably 80 mass% or more, more preferably 85 to 99 mass%, further preferably 90 to 98 mass%, and particularly preferably 92 to 97 mass%.
[0117] The method for drying the particulate hydrogel is not particularly limited, and examples thereof include heat drying, hot air drying, reduced pressure drying, fluidized bed drying, infrared drying, microwave drying, drum dryer drying, drying by azeotropic dehydration with a hydrophobic organic solvent, high humidity drying using high-temperature water vapor, etc. Among these, hot air drying is preferred from the viewpoint of drying efficiency.
[0118] Hot air drying methods include a method of drying in a stationary state, a method of drying in an agitated state, a method of drying in a vibrated state, a method of drying in a fluidized state, a method of drying with an air current, etc. Among these, from the viewpoint of efficiency, stationary drying is preferred, ventilation band drying is more preferred, and hot air drying using continuous stationary drying (continuous ventilation band drying) is particularly preferred.
[0119] The drying temperature (hot air temperature) in the hot air drying is preferably 120 to 250° C., more preferably 150 to 200° C., from the viewpoint of the color tone and drying efficiency of the water-absorbent resin. The drying conditions other than the drying temperature, such as the hot air speed and drying time, may be appropriately set according to the water content and total weight of the particulate hydrogel to be dried and the target resin solid content, and when band drying is performed, the conditions described in WO 2006 / 100300, WO 2011 / 025012, WO 2011 / 025013, WO 2011 / 111657, etc. are appropriately applied.
[0120] [2-5] Grinding process, classification process This step is a step of pulverizing the dried polymer obtained in the above drying step (pulverizing step) and adjusting the particle size to a predetermined range (classifying step) to obtain a water absorbent resin powder (a powdered water absorbent resin before surface crosslinking is conveniently referred to as a "water absorbent resin powder").
[0121] Examples of equipment that can be used in the grinding step of the present invention include high-speed rotary grinders such as roll mills, hammer mills, screw mills and pin mills, vibration mills, knuckle-type grinders and cylindrical mixers, which can be used in combination as necessary.
[0122] Further, the particle size adjustment method in the classification step of the present invention is not particularly limited, but examples thereof include sieve classification using a JIS standard sieve (JIS Z8801-1 (2000)) and air flow classification. The particle size adjustment of the water absorbent resin is not limited to the above-mentioned pulverization step and classification step, and can be appropriately performed in a polymerization step (particularly, reversed-phase suspension polymerization or spray droplet polymerization) or other steps. Further, it is also possible to remove non-standard products (for example, fine powder) classified in the classification step, and the removed water absorbent resin powder may be used as the water absorbent resin powder to be recovered.
[0123] The water absorbent resin powder (water absorbent resin powder before the surface cross-linking step, so-called base polymer) obtained in the above step has a mass average particle diameter (D50) of preferably 200 to 600 μm, more preferably 200 to 550 μm, and even more preferably 250 to 500 μm. The ratio of particles having a particle diameter of less than 150 μm is preferably 10 mass% or less, more preferably 5 mass% or less, and even more preferably 1 mass% or less, and the ratio of particles having a particle diameter of 850 μm or more is preferably 5 mass% or less, more preferably 3 mass% or less, and even more preferably 1 mass% or less. In any case, the lower limit of the ratio of these particles is preferably as small as possible, and 0 mass% is desirable, but it may be about 0.1 mass%. Furthermore, the logarithmic standard deviation (σζ) of the particle size distribution is preferably 0.20 to 0.50, more preferably 0.25 to 0.40, and even more preferably 0.27 to 0.35. The particle sizes are measured using standard sieves in accordance with the measurement methods disclosed in U.S. Pat. No. 7,638,570 and NWSP 220.0.R2(15).
[0124] The above-mentioned particle size is applied not only to the water absorbent resin after surface cross-linking (hereinafter, for convenience, may be referred to as "water absorbent resin particles") but also to the water absorbing agent as a final product. Therefore, in the water absorbent resin particles, it is preferable to carry out a surface cross-linking treatment (surface cross-linking step) so as to maintain the particle size in the above range, and the particle size may be adjusted by providing a sizing step (pulverization, classification step) after the surface cross-linking step.
[0125] [2-6] Fine powder granulation process This step is a step of granulating the fine powder classified in 2-5 or the fine powder obtained in the sizing step after the surface crosslinking step 2-8 described later. The granulated material obtained in this step is preferably recycled during the manufacturing process.
[0126] Granulation is the process of forming particles larger than the original particles by adhering them to each other using physical or chemical techniques.
[0127] The granulation is preferably performed by granulation using a solvent such as water or a hydrophilic solvent. Examples of the solvent include water; alcohols such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, and t-butyl alcohol; and combinations thereof. The solvent is preferably water. In granulation, the solvent is preferably sprayed or dropped onto the fine powder, more preferably sprayed. The amount of the solvent depends on the moisture content of the fine powder used, but is usually in the range of 25 to 250 parts by mass, preferably 25 to 200 parts by mass, per 100 parts by mass of the solid content of the water absorbent resin.
[0128] The device used when mixing the solvent and the fine powder is not particularly limited. For example, if the container is a fixed type mixer, a mechanical stirring type mixer is preferable. Specific examples include Turbulizer (manufactured by Hosokawa Micron Corporation), Loedige Mixer (manufactured by Loedige Corporation), and Mortar Mixer (manufactured by Nishinippon Shikenki Co., Ltd.). In addition, either a batch type mixer or a continuous type mixer may be used for mixing.
[0129] The heating temperature of the inside of the mixer, preferably the inner wall surface of the mixer, and / or the stirring means during the above mixing is preferably 60°C or higher, more preferably 65°C or higher, even more preferably 70°C or higher, and preferably 120°C or lower, more preferably 100°C or lower, even more preferably 90°C or lower. By heating the mixer (preferably either the inner wall surface or the stirring means, more preferably both), the fine powder can be uniformly granulated in a short time, improving productivity. The temperature inside the mixer can be appropriately adjusted, for example, by supplying heated gas or by conductive heating.
[0130] In this step, a water-absorbent resin solution can be added (Mode 4). In this case, it is preferable to use the above-mentioned solvent and the water-absorbent resin solution in combination, in that the granulation strength and physical properties of the granulated material can be adjusted. When using them in combination, the above-mentioned solvent and the water-absorbent resin solution may be mixed, or may be dropped or sprayed in a line separate from the solvent.
[0131] When mixing the solvent and water-absorbent resin solution with the fine powder to granulate, it is preferable to use a solvent and water-absorbent resin solution that have been heated in advance. By using a heated solvent and water-absorbent resin solution, the fine powder can be granulated uniformly in a short time, improving productivity. The temperature of the solvent and / or water-absorbent resin solution is preferably 40°C or higher, more preferably 50°C or higher, even more preferably 60°C or higher, and particularly preferably 70°C or higher, and is preferably the boiling point of the solvent or lower, more preferably 100°C or lower. The boiling point can be adjusted by adding salts or solvents, applying pressure (reduced pressure or increased pressure), or the like.
[0132] The amount of the water-absorbent resin solution added to the fine powder is appropriately set in consideration of the effect on the physical properties of the resulting water-absorbent resin, recovery efficiency, etc., and is, for example, 0.1 to 100 parts by mass per 100 parts by mass of the fine powder.
[0133] [2-7] Surface crosslinking process This step is a step of providing a portion with a higher crosslink density on a surface layer (a portion several tens of μm from the surface of the water absorbent resin powder) of the water absorbent resin powder obtained through the above-mentioned steps, and is composed of a mixing step, a heat treatment step, and a cooling step (optional).
[0134] In the surface cross-linking step, a surface-cross-linked water-absorbent resin (water-absorbent resin particles) is obtained by radical cross-linking or surface polymerization on the surface of the water-absorbent resin powder, a cross-linking reaction with a surface cross-linking agent, or the like.
[0135] In this step, a water absorbent resin solution can be added (Mode 5). In this case, the following surface crosslinking agent solution and solution may be mixed, and then the mixture may be mixed with the water absorbent resin powder and added, or the following surface crosslinking agent solution and water absorbent resin solution may be mixed in a separate line.
[0136] The amount of the water absorbent resin solution added to the water absorbent resin is appropriately set in consideration of the effect on the physical properties of the resulting water absorbent resin, recovery efficiency, etc., and is, for example, 0.1 to 100 parts by mass relative to 100 parts by mass of the water absorbent resin.
[0137] [2-7-1: Mixing process] This step is a step of mixing a water absorbent resin powder and a surface crosslinking agent. A method of mixing the surface crosslinking agent is not particularly limited, but includes a method of preparing a surface crosslinking agent solution in advance, and mixing the liquid by preferably spraying or dropping, more preferably spraying, to the water absorbent resin powder.
[0138] The device for carrying out the mixing is not particularly limited, but is preferably a high-speed stirring type mixer, more preferably a high-speed stirring type continuous mixer.
[0139] The surface cross-linking agent used in the present invention is not particularly limited, but may be an organic or inorganic surface cross-linking agent. Among them, from the viewpoint of the physical properties of the water-absorbent resin and the handling of the surface cross-linking agent, an organic surface cross-linking agent that reacts with a carboxyl group is preferred. For example, one or more surface cross-linking agents disclosed in U.S. Patent No. 7,183,456 may be mentioned. More specifically, polyhydric alcohol compounds, epoxy compounds, haloepoxy compounds, polyamine compounds or their condensates with haloepoxy compounds, oxazoline compounds, oxazolidinone compounds, polyvalent metal salts, alkylene carbonate compounds, cyclic urea compounds, etc. may be mentioned.
[0140] Specific examples of the organic surface crosslinking agent include polyalcohol compounds such as (di, tri, tetra, poly)ethylene glycol, (di, poly)propylene glycol, 1,3-propanediol, 2,2,4-trimethyl-1,3-pentanediol, (poly)glycerin, 2-butene-1,4-diol, 1,4-butanediol, 1,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, trimethylolpropane, di- or triethanolamine, pentaerythritol, and sorbitol; Epoxy compounds such as ethylene glycol diglycidyl ether, (di, poly)glycerol polyglycidyl ether, and glycidol; oxazoline compounds such as 2-oxazolidone, N-hydroxyethyl-2-oxazolidone, and 1,2-ethylenebisoxazoline; 1,3-dioxolan-2-one (ethylene carbonate), 4-methyl-1,3-dioxolan-2-one, 4,5-dimethyl-1,3-dioxolan-2-one, 4,4-dimethyl-1,3-dioxolan-2-one, and 4-ethyl-1,3-dioxo alkylene carbonate compounds such as 1,3-lane-2-one, 4-hydroxymethyl-1,3-dioxolan-2-one, 1,3-dioxan-2-one, 4-methyl-1,3-dioxan-2-one, 4,6-dimethyl-1,3-dioxan-2-one, and 1,3-dioxopan-2-one; haloepoxy compounds such as epichlorohydrin, epibromohydrin, and α-methylepichlorohydrin, and polyamine adducts thereof (e.g., Hercules Kaimen; registered trademark); γ-glycidoxypropyltrimethoxysilane, Examples of the compound include silane coupling agents such as γ-aminopropyltriethoxysilane; oxetane compounds such as 3-methyl-3-oxetanemethanol, 3-ethyl-3-oxetanemethanol, 3-butyl-3-oxetanemethanol, 3-methyl-3-oxetaneethanol, 3-ethyl-3-oxetaneethanol, 3-butyl-3-oxetaneethanol, 3-chloromethyl-3-methyloxetane, 3-chloromethyl-3-ethyloxetane, and polyvalent oxetane compounds; and cyclic urea compounds such as 2-imidazolidinone.
[0141] The polyhydric alcohol is preferably a polyhydric alcohol having 2 to 8 carbon atoms, more preferably a polyhydric alcohol having 3 to 6 carbon atoms, and even more preferably a polyhydric alcohol having 3 or 4 carbon atoms. Furthermore, diols are preferred, and examples thereof include ethylene glycol, propylene glycol, 1,3-propanediol, and 1,4-butanediol, with polyhydric alcohols selected from propylene glycol (1,2-propanediol), 1,3-propanediol, and 1,4-butanediol being preferred.
[0142] As the epoxy compound, a polyglycidyl compound is preferred, and ethylene glycol diglycidyl ether is preferably used.
[0143] In addition to the organic surface crosslinking agent, a polyvalent cationic polymer such as a polyamine polymer or a water-soluble polyvalent metal cation-containing compound may be used in combination as an ion-binding surface crosslinking agent. Examples of the water-soluble polyvalent metal cation-containing compound include inorganic salts of polyvalent metals such as aluminum sulfate, aluminum chloride, zirconium oxide chloride, ammonium zirconium carbonate, potassium zirconium carbonate, potassium zirconium carbonate, zirconium sulfate, zirconium acetate, and zirconium nitrate, and polyvalent metal compounds such as organic salts of polyvalent metals such as aluminum acetate, aluminum lactate, hydroxyzirconium chloride, titanium triethanolamine, and titanium lactate. Among them, a compound containing an aluminum ion as a polyvalent metal cation is preferable.
[0144] The amount of the surface crosslinking agent used (when a plurality of agents are used, the total amount used) is preferably 0.01 to 10 parts by mass, more preferably 0.01 to 5 parts by mass, relative to 100 parts by mass of the water absorbent resin powder. The surface crosslinking agent is preferably added as an aqueous solution, and in this case, the amount of water used is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 10 parts by mass, relative to 100 parts by mass of the water absorbent resin powder. Furthermore, when a hydrophilic organic solvent is used as necessary, the amount used is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, relative to 100 parts by mass of the water absorbent resin powder.
[0145] As described above, in the surface cross-linking step, a water-soluble polyvalent metal cation-containing compound may be added.
[0146] [2-7-2: Heat treatment process] This step is a step in which heat is applied to the mixture discharged from the above mixing step to cause a crosslinking reaction on the surface of the water absorbent resin powder.
[0147] The device for carrying out the crosslinking reaction is not particularly limited, but preferably includes a paddle dryer. The reaction temperature in the crosslinking reaction is appropriately set depending on the type of the surface crosslinking agent used, but is preferably 50 to 300°C, more preferably 100 to 200°C.
[0148] [2-7-3: Cooling process] This step is an optional step which is performed as necessary after the heat treatment step.
[0149] The cooling device is not particularly limited, but is preferably a device having the same specifications as the device used in the heat treatment step, and more preferably a paddle dryer. This is because it can be used as a cooling device by changing the heat medium to a refrigerant. The water-absorbent resin particles obtained in the heat treatment step are forcibly cooled, if necessary, to preferably 40 to 80°C, more preferably 50 to 70°C in the cooling step.
[0150] [2-8] Sizing process This step is a step of adjusting the particle size of the dried polymer or the surface-crosslinked (particulate) dried polymer. By carrying out the particle size regulation step after the surface crosslinking step, a water absorbent resin powder having a highly controlled particle size or particle size distribution can be obtained.
[0151] Preferably, the sizing process includes a grinding step and / or a classification step.
[0152] The pulverization step is a step in which a lump-shaped dry polymer or a strongly aggregated particulate dry polymer obtained when static drying is performed in the drying step or the heat treatment step is pulverized with a pulverizer to adjust the particle size. Note that this pulverization step differs from the above-mentioned gel pulverization step in that the dried polymer to be pulverized has been subjected to a drying step.
[0153] Examples of the pulverizer used in the pulverization step include high-speed rotary pulverizers such as roll mills, hammer mills, screw mills, and pin mills, vibration mills, knuckle-type pulverizers, cylindrical mixers, etc. Among these, the preferred pulverizer is the roll mill, from the viewpoint of easy control of particle size distribution.
[0154] The classification step is a process of removing coarse particles and fine powder from the (particulate) dried polymer, the surface-crosslinked (particulate) dried polymer, or a pulverized or crushed product thereof using a classifier. As the classifier used in the classification step, a vibrating or rocking sieve classifier using a sieve mesh is used. The coarse particles and fine powder removed in the classification step may be used as the water absorbent resin A of the present invention. Crushed products of the coarse particles can be used as the water absorbent resin A.
[0155] From the viewpoint of water absorption performance, the mass median particle diameter (D50) of the water absorbent resin powder obtained through the granulation step is preferably 200 μm or more, more preferably 200 to 600 μm, further preferably 250 to 550 μm, and particularly preferably 300 to 500 μm.
[0156] [2-9] Addition process of other additives This step is an optional step carried out for the purpose of imparting various additional functions to the water absorbent resin and improving the water absorption performance, and is a step of adding an additive in any of the steps. From the viewpoint of the effect of addition, it is preferable that the following additive is present on the surface of each particle of the water absorbent resin powder. Therefore, this step is preferably carried out simultaneously with or separately from the surface cross-linking step, and more preferably after the surface cross-linking step.
[0157] Examples of other additives include chelating agents, organic reducing agents, inorganic reducing agents, oxidizing agents, hydroxycarboxylic acid compounds, surfactants, compounds having phosphorus atoms, organic powders such as metal soaps, deodorants, antibacterial agents, pulp, thermoplastic fibers, etc. Liquid permeability is one example of the water absorption performance imparted to the water absorbent resin, and additives for improving the liquid permeability include the following polyvalent metal salts, cationic polymers, and inorganic fine particles, and it is preferable to use at least one of these.
[0158] Polyvalent metal salts Preferred examples of the polyvalent metal of the polyvalent metal salt include aluminum, zirconium, etc. Preferred examples of the polyvalent metal salt that can be used include aluminum lactate and aluminum sulfate, and more preferably aluminum sulfate.
[0159] The amount of the polyvalent metal salt to be added is preferably 3.6×10 metal cations per 1 g of water absorbent resin powder. -5 less than 2.8×10 -5 mol, more preferably less than 2.0×10 -5 Less than a mole.
[0160] Cationic polymers As the cationic polymer, preferably, the compound exemplified in U.S. Patent No. 7,098,284 can be mentioned. Among them, vinylamine polymer is preferable. The amount of the cationic polymer added is preferably less than 2.5 parts by mass, more preferably less than 2.0 parts by mass, and further preferably less than 1.0 parts by mass, relative to 100 parts by mass of the water absorbent resin powder.
[0161] ·Inorganic fine particles Specific examples of inorganic fine particles include minerals such as talc, kaolin, fuller's earth, hydrotalcite, bentonite, activated clay, barite, natural asphalt, strontium ore, ilmenite, and perlite; aluminum compounds such as aluminum sulfate 14-18 hydrate (or its anhydride), potassium aluminum sulfate 12 hydrate, sodium aluminum sulfate 12 hydrate, ammonium aluminum sulfate 12 hydrate, aluminum chloride, polyaluminum chloride, and aluminum oxide; other polyvalent metal salts such as calcium phosphate, polyvalent metal oxides, and polyvalent metal hydroxides; hydrophilic amorphous silicas; oxide complexes such as silicon oxide-aluminum oxide-magnesium oxide complexes, silicon oxide-aluminum oxide complexes, and silicon oxide-magnesium oxide complexes; and the like. Among these, two or more kinds may be used in combination. The amount of the inorganic fine particles to be added is preferably less than 2.0 parts by mass, more preferably less than 1.5 parts by mass, and even more preferably less than 1.0 part by mass, relative to 100 parts by mass of the water absorbent resin powder.
[0162] [2-10] Other processes The production method according to the present invention may further include, as necessary, a cooling step, a rewetting step, a pulverizing step, a classifying step, a transporting step, a storing step, a packaging step, a storage step, etc. In addition, the production method of the water absorbing agent according to the present embodiment may be used in combination with a conventional recovery and reuse of a water absorbent resin powder (for example, recovery and reuse using granulation of fine powder).
[0163] 3. Properties of the obtained water-absorbing agent The present invention also provides a water absorbing agent obtained by the manufacturing method of the above embodiment. The physical properties of the water absorbing agent are preferably as follows. The preferred ranges of the physical properties of the water absorbing resin are also the same as the preferred ranges of the physical properties (CRC, etc.) of the water absorbing agent described below.
[0164] [3-1] CRC (centrifuge holding capacity) The CRC (centrifuge retention capacity) of the water absorbing agent is usually 5 g / g or more, preferably 15 g / g or more, more preferably 25 g / g or more. The upper limit is not particularly limited, and a higher CRC is preferable, but from the viewpoint of the balance with other physical properties, it is preferably 70 g / g or less, more preferably 50 g / g or less, and further preferably 40 g / g or less.
[0165] If the CRC is less than 5 g / g, the absorption amount is small and the material is not suitable for use as an absorbent for absorbent articles such as paper diapers. If the CRC is more than 70 g / g, the speed at which the material absorbs body fluids such as urine and blood decreases, making the material unsuitable for use in paper diapers with high water absorption rates. The CRC can be controlled by changing the type and amount of the internal crosslinking agent or surface crosslinking agent.
[0166] [3-2] Particle size When the water absorbing agent is a powder, the mass median particle diameter d3 (D50) of the water absorbent resin is preferably 200 μm or more, more preferably 200 to 600 μm, even more preferably 250 to 550 μm, and particularly preferably 300 to 500 μm. The ratio of particles having a particle diameter of less than 150 μm is usually 15 mass% or less, preferably 10 mass% or less, more preferably 8 mass% or less, and even more preferably 6 mass% or less. The ratio of particles having a particle diameter of more than 850 μm is preferably 5 mass% or less, more preferably 3 mass% or less, and even more preferably 1 mass% or less. The water absorbent resin contains particles having a particle diameter of 150 to 850 μm, preferably 90 mass% or more, more preferably 95 mass% or more, even more preferably 97 mass% or more, and especially preferably 99 mass% or more. Ideally, it is 100 mass%. The logarithmic standard deviation (σζ) of the particle size distribution is preferably 0.20 to 0.50, more preferably 0.25 to 0.40, and further preferably 0.27 to 0.35.
[0167] [3-3] AAP (absorption capacity under pressure) The AAP (absorption capacity against pressure) of the water absorbing agent is preferably 15 g / g or more, more preferably 20 g / g or more, further preferably 23 g / g or more, particularly preferably 24 g / g or more, and most preferably 25 g / g or more. The upper limit is not particularly limited, but is preferably 40 g / g or less.
[0168] If the AAP is less than 15 g / g, the amount of liquid returning when pressure is applied to the absorbent (sometimes called "Re-Wet") increases, making it unsuitable for use as an absorbent in absorbent articles such as disposable diapers. The AAP can be controlled by adjusting the particle size, changing the surface cross-linking agent, etc.
[0169] [3-4] Vortex (water absorption speed) The Vortex (water absorption speed) of the water absorbing agent is preferably 60 seconds or less, more preferably 50 seconds or less, further preferably 40 seconds or less, and particularly preferably 30 seconds or less. There is no particular restriction on the lower limit, but it is preferably 5 seconds or more, more preferably 10 seconds or more.
[0170] By setting the Vortex within the above range, it becomes possible to absorb a given amount of liquid in a short time. When used in the absorbent body of an absorbent article such as a disposable diaper, the time that the user feels the skin is wet is shortened, which reduces discomfort and reduces the amount of leakage.
[0171] [3-5] Residual monomer amount The amount of residual monomer in the water absorbing agent is preferably 500 ppm or less, more preferably 450 ppm or less, and further preferably 400 ppm or less. From the viewpoint of safety, the smaller the amount of residual monomer, the better.
[0172] [4] Uses of water absorbents The use of the water-absorbing agent is not particularly limited, but preferably includes use as an absorbent for absorbent articles such as paper diapers, sanitary napkins, incontinence pads, etc. In particular, it can be used as an absorbent for high-concentration paper diapers.
[0173] In addition, as the raw material of the absorbent body, an absorbent material such as pulp fiber can be used together with the water absorbing agent. In this case, the content (core concentration) of the water absorbent resin in the absorbent body is preferably 30% by mass to 100% by mass, more preferably 40% by mass to 100% by mass, even more preferably 50% by mass to 100% by mass, even more preferably 60% by mass to 100% by mass, particularly preferably 70% by mass to 100% by mass, and most preferably 75% by mass to 95% by mass.
[0174] By setting the core concentration within the above range, when the absorbent is used in the upper layer of an absorbent article, the absorbent article can be maintained in a clean white state. Furthermore, since the absorbent has excellent diffusibility of body fluids such as urine and blood, efficient liquid distribution is achieved, and an improvement in the absorption amount can be expected. EXAMPLES
[0175] The present invention will be described in more detail with reference to the following experimental examples. However, the present invention is not limited to these explanations, and experimental examples obtained by appropriately combining the technical means disclosed in each experimental example are also included in the scope of the present invention.
[0176] In addition, the term "water-absorbent resin" described below means a granular dried material that has been subjected to a drying process, a surface-crosslinked granular dried material or a water-absorbent resin powder, and a surface-crosslinked water-absorbent resin powder, and the term "water-containing gel" means a water-containing gel-like crosslinked polymer or a particulate water-containing gel-like crosslinked polymer that has not been subjected to a drying process.
[0177] In addition, unless otherwise noted, electric devices (including devices for measuring the physical properties of the water-absorbent resin) used in the experimental examples were powered by a 60 Hz, 200 V or 100 V power source. In addition, unless otherwise noted, the various physical properties of the water-absorbent resin and the hydrous gel described below were measured under the conditions of room temperature (20°C to 25°C) and a relative humidity of 50% RH ± 10%.
[0178] For convenience, "liter" may be expressed as "l" or "L", and "mass%" or "weight%" as "wt%". When measuring trace components, amounts below the detection limit may be expressed as ND (Non Detected).
[0179] [Physical property measurement method] (a) Centrifuge Retention Capacity (CRC) of water-absorbent resins, water-absorbent agents, and hydrous gels The CRC (centrifuge retention capacity) of the water-absorbent resin was measured in accordance with NWSP 241.0.R2(15). The CRC (centrifuge retention capacity) of the hydrogel was measured in the same manner as NWSP 241.0.R2(15), except that the mass of the sample was changed to 0.4 g as the hydrogel and the free swelling time was changed to 24 hours. Furthermore, the solid content α of the hydrogel was measured separately according to the following (f), and the CRC of the hydrogel (hereinafter also referred to as gel CRC) was calculated according to the following (Equation 1).
[0180] CRC of hydrous gel (g / g) = {(mwi-mb)-msi×(α / 100)} / {msi×(α / 100)} (Equation 1) Here, msi is the mass of the hydrogel before measurement (unit: g), mb is the mass of the blank (nonwoven fabric only) after free swelling and dehydration (unit: g), mwi is the mass of the hydrogel (including nonwoven fabric) after free swelling and dehydration (unit: g), and α is the solid content of the hydrogel before measurement (unit: mass%).
[0181] (b) Water content and solid content of water-absorbent resin and water-absorbent agent The moisture content of the water-absorbent resin was measured in accordance with NWSP 230.0.R2(15). In the measurement, the mass of the sample was changed to 1.0 g, the drying temperature was changed to 180°C, and the moisture content and solid content of the water-absorbent resin were calculated from the loss on drying after drying for 3 hours.
[0182] (c) Particle size of water-absorbing resin and water-absorbing agent The particle size (particle size distribution, mass average particle size (D50) and logarithmic standard deviation of particle size distribution (σζ)) of the water-absorbent resin was measured in accordance with the method described in columns 27 and 28 of US Pat. No. 7,638,570.
[0183] (d) 150 pass rate: sieve passing rate of 150 μm mesh A classification operation similar to that for measuring the mass average particle diameter (D50) was performed, and the ratio (mass%) of particles passing through a sieve with 150 μm openings was taken as the 150 pass rate (150 μm opening sieve passing rate).
[0184] (e) Conversion rate and residual monomer content of hydrogel After sampling the hydrogel, 1.00 g of the hydrogel was immediately put into 1000 g of ion-exchanged water at room temperature (the polymerization reaction was substantially stopped at this point), and the mixture was stirred at 300 rpm for 2 hours, followed by filtration to remove insoluble matter. The amount of monomer extracted in the filtrate obtained by the above operation was measured using a liquid chromatograph. When the amount of the monomer was taken as the residual monomer amount m (g), the polymerization rate C (mass%) of the hydrogel was calculated according to the following (Equation 2), and the residual monomer amount R (mass%) of the hydrogel was calculated according to the following (Equation 3). It is preferable to measure the polymerization rate immediately after sampling the hydrogel, but if it takes time from sampling to measurement, it is necessary to perform a polymerization termination operation by forced cooling (contact with dry ice, liquid nitrogen, ice water, etc.).
[0185] C (mass%)=100×{1-m / (α×M / 100)} (Formula 2) R (mass%)=100-C (Formula 3) In the formula 2, M is the mass (g) of the hydrogel, and α is the solid content (mass%) of the hydrogel. In the formula 3, C is the polymerization rate (mass%) of the hydrogel. The solid content α of the hydrogel is measured according to the following (f).
[0186] (f) Water content and solid content of hydrogel The water content of the hydrous gel was measured in accordance with NWSP 230.0.R2(15). In the measurement, the mass of the sample was changed to 2.0 g, the drying temperature to 180 ° C, and the drying time to 24 hours. Specifically, 2.0 g of the hydrous gel was placed in an aluminum cup with a bottom diameter of 50 mm, and then the total mass W1 (g) of the sample (hydrous gel and aluminum cup) was accurately weighed. Next, the sample was placed in an oven with an atmospheric temperature set to 180 ° C. After 24 hours, the sample was removed from the oven and the total mass W2 (g) was accurately weighed. When the mass of the hydrous gel used in this measurement was M (g), the water content (100-α) (mass%) of the hydrous gel was calculated according to the following (Equation 4). α is the solid content (mass%) of the hydrous gel.
[0187] (100-α)(mass%)={(W1-W2) / M}×100 (Formula 4) (g) Vortex (absorption time) of water-absorbent resin and water-absorbent The Vortex (water absorption time) of the water-absorbent resin was measured according to the following procedure: First, 0.02 parts by mass of edible blue No. 1 (brilliant blue), a food additive, was added to 1,000 parts by mass of previously prepared physiological saline (0.9% by mass aqueous sodium chloride solution), and the liquid temperature was adjusted to 30°C.
[0188] Next, 50 ml of the physiological saline solution was weighed out into a 100 ml beaker, and 2.0 g of the water-absorbent resin was poured into the beaker while stirring at 600 rpm using a stirrer tip with a length of 40 mm and a diameter of 8 mm. The time from the time the water-absorbent resin was poured in until the water-absorbent resin absorbed the physiological saline and covered the stirrer tip was measured as a Vortex (absorption time) (unit: seconds).
[0189] (h) Residual monomer amount of water absorbent resin or water absorbent The residual monomer amount of the water absorbent resin was measured in accordance with NWSP 210.0.R2(15). Specifically, 1.0 g of the water absorbent resin was added to 200 ml of 0.9 mass% sodium chloride aqueous solution, stirred at 500 rpm for 1 hour using a 35 mm long stirrer tip, filtered, and the amount of monomer eluted in the filtrate was measured by high performance liquid chromatography. The residual monomer amount is expressed as a mass ratio to the water absorbent resin (unit: ppm).
[0190] (i) AAP (absorbency under pressure) of water-absorbent resins and water-absorbent agents The AAP (absorption capacity under pressure) of the water-absorbent resin was measured in accordance with NWSP 242.0.R2(15). That is, 0.900 g (mass W3(g)) of the water-absorbent resin was placed in the measuring device, and the mass (W4(g)) of the measuring device was measured. Next, a 0.90 mass% sodium chloride aqueous solution adjusted to 23±2°C was placed in the measuring device at 2.06 kPa (0.3 psi, 21 g / cm 2 After one hour had passed, the mass (W5(g)) of the measurement device was measured, and the absorbency against pressure (AAP) was calculated from the obtained W3(g), W4(g), and W5(g) according to the following formula 5.
[0191] AAP(g / g)=(W5-W4) / W3 (Formula 5) [Reference example 1] (Polymerization process) A monomer solution was prepared consisting of 422g of acrylic acid, 106g of 48.5% by mass sodium hydroxide aqueous solution, 0.92g of polyethylene glycol diacrylate (weight average molecular weight 523), 25.8g of 0.1% by mass trisodium diethylenetriamine pentaacetate aqueous solution, and 374g of deionized water. Next, 246g of 48.5% by mass sodium hydroxide aqueous solution was added while stirring the monomer solution adjusted to a temperature of 42.5°C. The neutralization rate of acrylic acid was 73 mol%. Note that the final neutralization rate of acrylic acid is the same for the following examples and comparative examples. The temperature rose to 92°C due to the heat of neutralization at this time. When the temperature of the monomer aqueous solution reached 90°C, 16.7g of a 4.5% by mass aqueous solution of sodium persulfate was added, and then the mixture was poured onto a Teflon (registered trademark) sheet (a 30cm x 30cm reaction vessel surrounded by a dam with a height of 1.5cm on all four sides) whose bottom had been preheated to 50°C in an atmosphere at 60°C, and polymerization was carried out. 15 seconds after the addition of the aqueous sodium persulfate solution, the polymerization system reached a maximum temperature of 105°C. After a further 3 minutes, the obtained polymer was taken out to obtain a hydrogel-like crosslinked polymer (G2).
[0192] (Gel crushing process) The obtained hydrogel-like crosslinked polymer (G2) was cut into 60 g portions. The hydrogel-like crosslinked polymer (G2) was fed into a meat chopper (manufactured by Remacom Co., Ltd., model: HL-G22SN) equipped with a 9.5 mm die aperture plate at a rate of 360 g / min, and at the same time, 22 g / min of hot water heated to 90°C was added and passed through once to obtain hydrogel-like crosslinked polymer pulverized material (MG2). The gel solid content of the hydrogel-like crosslinked polymer pulverized material (MG2) was 50.5 mass%, the gel CRC was 37.0 g / g, and the polymerization rate was 98.3%.
[0193] (Drying, crushing, classification process) 500 g of the obtained hydrogel crosslinked polymer pulverized product (MG2) was dried at 190°C for 30 minutes in a hot air dryer (Satake Chemical Industry, ventilation band type dryer) to obtain a dried product. Then, the product was pulverized in a roll mill (Inokuchi Giken Co., Ltd.) to obtain a water-absorbent resin powder (F2-1). After sieving with sieves having openings of 850 μm, 600 μm, 500 μm, 300 μm, and 150 μm, particles that passed through the 850 μm sieve and did not pass through the 150 sieve were collected to obtain a water-absorbent resin powder (F2-2). The particle rate that passed through the 150 μm sieve (150 pass rate) was 13.9 mass%. The physical properties of the water-absorbent resin powder (F2-2) are shown in Table 1.
[0194] The water absorbent resin powder (F2-2) was sieved with sieves having mesh sizes of 850 μm, 600 μm, 500 μm, 300 μm, and 150 μm, and then the particles passing through 850 μm and not passing through 600 μm were mixed at 3 mass %, the particles passing through 600 μm and not passing through 500 μm were mixed at 10 mass %, the particles passing through 500 μm and not passing through 300 μm, 54 mass %, the particles passing through 300 μm and not passing through 150 μm, and 2 mass % of the particles passing through 150 μm and not passing through 45 μm, to obtain a water absorbent resin powder (F2-3).
[0195] (Surface crosslinking process) 100 parts by mass of the particle size-adjusted water absorbent resin powder (F2-3) was mixed with a surface crosslinking agent solution consisting of 0.025 parts by mass of ethylene glycol diglycidyl ether, 0.3 parts by mass of ethylene carbonate, 0.5 parts by mass of propylene glycol, and 2.0 parts by mass of deionized water. The mixture was heat-treated at 200°C for 35 minutes to obtain surface-crosslinked water absorbent resin particles (R2). The physical properties of the water absorbent resin particles (R2) are shown in Table 2.
[0196] [Production Example 1] (Water absorbent resin A) A monomer aqueous solution was prepared consisting of 422 parts by mass of acrylic acid, 173.9 parts by mass of 48% by mass sodium hydroxide aqueous solution, 0.86 parts by mass of polyethylene glycol diacrylate (weight average molecular weight 523), 25.8 parts by mass of 0.1% by mass of diethylenetriaminepentaacetate trisodium aqueous solution, and 372 parts by mass of deionized water. Next, the monomer aqueous solution (T1-1) adjusted to 38°C was continuously fed by a metering pump, and then 178.7 parts by mass of 48% by mass sodium hydroxide aqueous solution was continuously line mixed. At this time, the liquid temperature of the monomer aqueous solution (T1-2) rose to 82°C due to the heat of neutralization.
[0197] Furthermore, 16.9 parts by mass of 4% by mass sodium persulfate aqueous solution was continuously line mixed, and then continuously fed to a continuous polymerization machine having a flat polymerization belt with a weir at both ends so that the thickness was 10 mm. Then, polymerization (polymerization time 3 minutes) was continuously performed to obtain a belt-shaped hydrogel crosslinked polymer (G1-1). The obtained belt-shaped hydrogel (G1-1) was cut continuously at equal intervals in the width direction with respect to the traveling direction of the polymerization belt so that the cut length was 300 mm, thereby obtaining a strip-shaped hydrogel crosslinked polymer (G1-2).
[0198] The obtained hydrogel crosslinked polymer (G1-2) and a 3.1% by mass aqueous solution of lauryl dimethyl amino acetic acid betaine were simultaneously fed to a screw extruder, while gel pulverization was performed. The amount of the aqueous solution of lauryl dimethyl amino acetic acid betaine fed was 0.15% by mass relative to the solid content of the hydrogel crosslinked polymer (G1-2). As the screw extruder, a meat chopper having an outer diameter of a screw shaft of 86 mm and a perforated plate having a diameter of 100 mm, a hole diameter of 12.5 mm, and a thickness of 10 mm was used, and gel pulverization was performed while feeding water and steam simultaneously with the hydrogel crosslinked polymer (G1-2). The obtained hydrogel crosslinked polymer pulverized product (MG1) had a solid content of 44% by mass (water content of 56% by mass) and a polymerization rate of 98.6%.
[0199] The obtained hydrogel-like crosslinked polymer pulverized material (MG1) was dried using a continuous ventilation band type dryer. First, the hydrogel-like crosslinked polymer pulverized material (MG1) was spread on the ventilation plate (punched metal) of this dryer to a thickness of about 10 cm, and dried with hot air at 185°C for 35 minutes. The dried material obtained at the outlet of the dryer was integrated and solidified into a single block (the width was almost equivalent to the width of the drying belt, the length was endless, and the thickness was several cm).
[0200] The integrated dried product was air-cooled and roughly crushed with a crusher (first crusher) equipped with a rotary shaft having multiple blades, and then the crushed product was fed to a three-stage roll mill (second crusher) and further crushed to obtain a water absorbent resin powder (A). The obtained water absorbent resin powder had a mass average particle diameter (d1) of 348 μm, a ratio of particles having a particle diameter of less than 150 μm of 9.8 mass%, and a solid content rate of 97.6 mass%.
[0201] Subsequently, the water absorbent resin powder (A) was classified using JIS standard sieves with 850 μm and 180 μm openings. As a passing material classified using the 180 μm opening sieve, fine powder (FP1) was obtained, which is the water absorbent resin A having a solid content of 95.2 mass%. The fine powder (FP1) had a mass average particle diameter (d2) of 102 μm, a passing rate through a 150 μm opening sieve of 93.9 mass%, and a CRC of 37.2 g / g.
[0202] [Example 1] (Dissolution solution preparation process) 106 g of 48.5 mass% sodium hydroxide aqueous solution was added to 374 g of deionized water to prepare a 10.7 mass% sodium hydroxide aqueous solution, and 7.7 g of fine powder (FP1) was added while stirring so as not to form a powder, and the mixture was stirred for 20 minutes to obtain a colorless and transparent water absorbent resin solution (A1). The temperature of the alkaline aqueous solution when the fine powder (FP1) was added to the alkaline aqueous solution was 30°C.
[0203] (Preparation of Monomer Aqueous Solution) A mixed solution of 422 g of acrylic acid, 0.92 g of polyethylene glycol diacrylate (weight average molecular weight 523), and 25.8 g of 0.1 mass % aqueous solution of trisodium diethylenetriaminepentaacetate was stirred while adding the entire amount of the water absorbent resin fine powder solution (A1) to obtain an aqueous solution.
[0204] (Polymerization process) Next, 246 g of 48.5% by mass aqueous sodium hydroxide solution was added while stirring the aqueous solution adjusted to 42.5°C, to obtain an aqueous monomer solution. The temperature rose to 92°C due to the heat of neutralization at this time. When the temperature of the aqueous monomer solution reached 90°C, 16.7 g of 4.5% by mass aqueous sodium persulfate solution was added, and then the mixture was poured onto a Teflon (registered trademark) sheet (a 30 cm x 30 cm reaction vessel surrounded by a dam with a height of 1.5 cm on all four sides) whose bottom had been preheated to 50°C in an atmosphere temperature of 60°C, and polymerization was carried out. 16 seconds after the addition of the aqueous sodium persulfate solution, the polymerization system reached a maximum temperature of 106°C. After a further 3 minutes had passed, the obtained polymer was taken out to obtain a hydrogel-like crosslinked polymer (G3).
[0205] (Gel crushing process) The same procedure as in the gel crushing step of Reference Example 1 was carried out to obtain a crushed product of a hydrogel-like crosslinked polymer (MG3).
[0206] The pulverized hydrogel crosslinked polymer (MG3) had a gel solid content of 50.8% by mass, a gel CRC of 36.1 g / g, and a polymerization rate of 98.4%.
[0207] (Drying, crushing, classification process) The same operations as those of the drying, pulverization, and classification steps of Reference Example 1 were carried out to obtain water absorbent resin powders (F3-1) and (F3-2). The particle rate (150 pass rate) of (F3-1) that passed through a 150 μm sieve was 12.1 mass%. The physical properties of the water absorbent resin powder (F3-2) are shown in Table 1.
[0208] (Surface crosslinking process) Surface-crosslinked water-absorbent resin particles (water-absorbing agent) (R3) were obtained by carrying out the same operation as in the surface-crosslinking step of Reference Example 1. The physical properties of the water-absorbing agent (R3) are shown in Table 2.
[0209] [Comparative Example 1] (Preparation of monomer aqueous solution, polymerization process) A monomer solution (T4-1) consisting of 422g of acrylic acid, 106g of 48.5% by mass sodium hydroxide aqueous solution, 0.92g of polyethylene glycol diacrylate (weight average molecular weight 523), 25.8g of 0.1% by mass trisodium diethylenetriamine pentaacetate aqueous solution, and 374g of deionized water was prepared. Next, 246g of 48.5% by mass sodium hydroxide aqueous solution was added while stirring the monomer solution (T4-1) adjusted to a temperature of 42.5°C. The temperature rose to 92°C due to the heat of neutralization at this time. 7.7g of fine powder (FP1) was added thereto and stirred for 60 seconds to obtain a monomer aqueous solution (T4-2). When the temperature of the monomer aqueous solution (T4-2) reached 90°C, 16.7g of 4.5% by mass sodium persulfate aqueous solution was added while the suspended matter derived from the fine powder added to the monomer aqueous solution was still visible, and then the mixture was poured onto a Teflon (registered trademark) sheet (a 30cm x 30cm reaction vessel surrounded by a dam with a height of 1.5cm on all four sides) whose bottom had been preheated to 50°C in an atmosphere temperature of 60°C, and polymerization was carried out. 15 seconds after the addition of the sodium persulfate aqueous solution, the polymerization system reached a maximum temperature of 105°C. After a further 3 minutes, the obtained polymer was taken out to obtain a hydrogel-like crosslinked polymer (G4).
[0210] (Gel crushing process) A pulverized hydrogel crosslinked polymer (MG4) was obtained by carrying out the same operation as in the gel pulverization step of Reference Example 1. The gel solid content of the pulverized hydrogel crosslinked polymer (MG4) was 51.1 mass%, the gel CRC was 35.2 g / g, and the polymerization rate was 98.3%.
[0211] (Drying, crushing, classification process) Water absorbent resin powders (F4-1) and (F4-2) were obtained by carrying out the same operations as the drying, pulverization, and classification steps of Reference Example 1. The particle rate (150 pass rate) of (F4-1) that passed through a 150 μm sieve was 13.1 mass%, which was higher than the particle rate (150 pass rate) of the water absorbent resin powder (F3-1) obtained in Example 1 that passed through a 150 μm sieve, 12.1 mass%. The physical property values of the water absorbent resin powder (F4-2) are shown in Table 1.
[0212] (Surface crosslinking process) Surface-crosslinked water-absorbent resin particles (water-absorbing agent) (R4) were obtained by carrying out the same operation as in the surface-crosslinking step of Reference Example 1. The physical properties of the water-absorbing agent (R4) are shown in Table 2.
[0213] [Production Example 2] (Water absorbent resin A) The water absorbent resin powder (A) obtained in Production Example 1 was sieved with sieves having openings of 850 μm, 600 μm, 500 μm, 300 μm, and 150 μm, and then the particles passing through 850 μm and not passing through 600 μm were mixed at 3 mass %, the particles passing through 600 μm and not passing through 500 μm were mixed at 10 mass %, the particles passing through 500 μm and not passing through 300 μm, 54 mass %, the particles passing through 300 μm and not passing through 150 μm, and 2 mass % of the particles passing through 150 μm and not passing through 45 μm, to obtain a water absorbent resin powder (B).
[0214] The water absorbent resin powder (B) had a mass median particle size (d3) of 346 μm and a CRC of 46.6 g / g.
[0215] 100 parts by mass of the water absorbent resin powder (B) obtained by adjusting the particle size was mixed with a surface crosslinking agent solution consisting of 0.025 parts by mass of ethylene glycol diglycidyl ether, 0.3 parts by mass of ethylene carbonate, 0.5 parts by mass of propylene glycol, and 2.0 parts by mass of deionized water. The mixture was heat-treated at 200°C for 30 minutes to obtain surface crosslinked water absorbent resin particles (R1-1).
[0216] To 100 parts by mass of surface-crosslinked water-absorbent resin particles (R1-1), 8 parts by mass of deionized water was added while stirring and mixed for 1 minute. Then, the mixture was left in a hot air dryer at 60°C for 30 minutes, passed through a wire mesh with an opening of 850 μm, and mixed with 0.6 parts by mass of hydrotalcite (DHT-6, Kyowa Chemical Industry Co., Ltd.). The mixing of hydrotalcite was performed by adding 30 g of surface-crosslinked water-absorbent resin particles (R1-2) to which deionized water had been added, and putting the hydrotalcite into a mayonnaise bottle with a capacity of 225 ml, and shaking the mixture for 3 minutes using a paint shaker to obtain a particulate water-absorbing agent (S1).
[0217] The obtained water absorbing agent (S1) was classified using JIS standard sieves with 850 μm and 180 μm openings. As a passing material classified using the 180 μm opening sieve, fine powder (FP2) was obtained, which is water absorbent resin A with a solid content of 88.9 mass%. The fine powder (FP2) had a mass average particle diameter (d4) of 114 μm, a passing rate through a 150 μm opening sieve of 87.2 mass%, and a CRC of 24.9 g / g.
[0218] [Example 2] (Dissolution solution preparation process) 106 g of 48.5 mass% sodium hydroxide aqueous solution was added to 374 g of deionized water to prepare a 10.7 mass% sodium hydroxide aqueous solution, and 7.7 g of fine powder (FP2) was added while stirring so as not to form a powder, and the mixture was stirred for 20 minutes to obtain a colorless and transparent water absorbent resin solution (A2). The temperature of the alkaline aqueous solution when the water absorbent resin fine powder was added to the alkaline aqueous solution was 30°C.
[0219] (Preparation of monomer aqueous solution, polymerization process) A total amount of the water-absorbent resin solution (A2) was added to a mixed solution of 422 g of acrylic acid, 0.92 g of polyethylene glycol diacrylate (weight average molecular weight 523), and 25.8 g of 0.1 mass% aqueous solution of trisodium diethylenetriamine pentaacetate while stirring to obtain an aqueous solution. Next, 246 g of 48.5 mass% aqueous solution of sodium hydroxide was added while stirring the aqueous solution adjusted to 42.5 ° C to obtain an aqueous monomer solution. The temperature rose to 92 ° C due to the heat of neutralization at this time. When the temperature of the aqueous monomer solution reached 90 ° C, 16.7 g of an aqueous solution of 4.5 mass% sodium persulfate was added, and then the mixture was poured onto a Teflon (registered trademark) sheet (a 30 cm × 30 cm reaction vessel surrounded by a dam with a height of 1.5 cm on all sides) whose bottom had been heated to 50 ° C in advance in an atmosphere temperature of 60 ° C., and polymerization was performed. 14 seconds after the addition of the aqueous solution of sodium persulfate, the polymerization system reached a maximum temperature of 105 ° C. After a further 3 minutes had elapsed, the resulting polymer was taken out to obtain a hydrogel-like crosslinked polymer (G5).
[0220] (Gel crushing process) In the same manner as in Reference Example 1, a pulverized hydrogel crosslinked polymer (MG5) was obtained.
[0221] The pulverized hydrogel crosslinked polymer (MG5) had a gel solid content of 51.0 mass %, a gel CRC of 35.5 g / g, and a polymerization rate of 98.3%.
[0222] (Drying, crushing, classification process) Water absorbent resin powders (F5-1) and (F5-2) were obtained in the same manner as in Reference Example 1. The particle rate (150 pass rate) of (F5-1) that passed through a 150 μm sieve was 14.3 mass%. The physical properties of the water absorbent resin powder (F5-2) are shown in Table 1.
[0223] (Surface crosslinking process) Surface-crosslinked water-absorbent resin particles (water-absorbing agent) (R5) were obtained in the same manner as in Reference Example 1. The physical properties of the water-absorbing agent (R5) are shown in Table 2.
[0224] [Comparative Example 2] (Preparation of monomer aqueous solution, polymerization process) A monomer solution (T6-1) consisting of 422 g of acrylic acid, 106 g of 48.5% by mass sodium hydroxide aqueous solution, 0.92 g of polyethylene glycol diacrylate (weight average molecular weight 523), 25.8 g of 0.1% by mass trisodium diethylenetriamine pentaacetate aqueous solution, and 374 g of deionized water was prepared. Next, 246 g of 48.5% by mass sodium hydroxide aqueous solution was added to the monomer solution (T6-1) adjusted to a temperature of 42.5°C while stirring. The temperature rose to 92°C due to the heat of neutralization at this time. 7.7g of fine powder (FP2) was added here and stirred for 60 seconds. When the temperature of the monomer aqueous solution (T6-2) reached 90°C, 16.7g of 4.5% by mass sodium persulfate aqueous solution was added while the suspended matter derived from the fine powder added to the monomer aqueous solution was still visible. Then, in an atmosphere at 60°C, the mixture was poured onto a Teflon (registered trademark) sheet (a 30cm x 30cm reaction vessel surrounded by a dam with a height of 1.5cm on all four sides) whose bottom had been preheated to 50°C, and polymerization was carried out. 15 seconds after the addition of the sodium persulfate aqueous solution, the polymerization system showed a maximum temperature of 105°C. After another 3 minutes, the polymerized product obtained was taken out to obtain a hydrogel-like crosslinked polymer (G6).
[0225] (Gel crushing process) In the same manner as in Reference Example 1, a pulverized hydrogel crosslinked polymer (MG6) was obtained.
[0226] The pulverized hydrogel crosslinked polymer (MG6) had a gel solid content of 51.5 mass %, a gel CRC of 34.6 g / g, and a polymerization rate of 98.4%.
[0227] (Drying, crushing, classification process) Water absorbent resin powders (F6-1) and (F6-2) were obtained in the same manner as in Reference Example 1. The particle rate (150 pass rate) of (F6-1) that passed through a 150 μm sieve was 14.3 mass%. The physical properties of the water absorbent resin powder (F6-2) are shown in Table 1.
[0228] (Surface crosslinking process) Surface-crosslinked water-absorbent resin particles (water-absorbing agent) (R6) were obtained in the same manner as in Reference Example 1. The physical properties of the water-absorbing agent (R6) are shown in Table 2.
[0229] [Example 3] (Dissolution solution preparation process) 172 g of 48.5 mass% sodium hydroxide aqueous solution was added to 374 g of deionized water to prepare a 15.3 mass% sodium hydroxide aqueous solution, and 4.0 g of water absorbent resin A fine powder (FP1) was added while stirring so as not to form a powder, and stirred for 20 minutes to obtain a colorless and transparent water absorbent resin solution (A3). The temperature of the alkaline aqueous solution when the water absorbent resin A fine powder (FP1) was added to the alkaline aqueous solution was 30°C.
[0230] (Preparation of monomer aqueous solution, polymerization process) 200g of acrylic acid, 0.73g of N,N'-methylenebisacrylamide and 587g of deionized water were charged into a 1L reaction vessel, and the temperature of the contents was maintained at 20°C while stirring to prepare an aqueous monomer solution (T7). Nitrogen gas was then introduced until the dissolved oxygen concentration in the aqueous monomer solution (T7) was less than 0.02%, and then 2.44g of 1% by mass hydrogen peroxide solution, 2.92g of 0.2% by mass ascorbic acid solution and 6.82g of 2% by mass 2,2-azobisaminodipropane dihydrochloride solution were added to the aqueous monomer solution (T7) under sealing to initiate the polymerization reaction. After the temperature of the aqueous monomer solution (1) in the reaction vessel reached about 85°C, it was heated at 60°C for 3 hours to obtain a hydrogel-like crosslinked polymer (G7).
[0231] (Gel crushing process) The obtained hydrogel cross-linked polymer (G7) was chopped into blocks of 3 to 5 cm square. Next, 800 g (solid content 25.3 mass%) of the block-shaped hydrogel cross-linked polymer (G7) and 553.7 g of the water-absorbent resin solution (A3) (corresponding to an amount that neutralizes 75 mol% of the carboxyl groups in the hydrogel cross-linked polymer (G7)) were charged into the feed port of a meat chopper equipped with a rotary blade and a perforated plate (diameter 70 mm, hole size 5 mm, number of holes 50, thickness 8 mm, made of SUS) at the tip and a screw shaft of 120 mm in length, and mixed while chopping to obtain a hydrogel cross-linked polymer pulverized product (MG7-1). The time from the input of the hydrogel cross-linked polymer (G7) to the discharge of the hydrogel cross-linked polymer pulverized product (MG7-1) was about 30 seconds.
[0232] Subsequently, the obtained hydrogel-like crosslinked polymer pulverized product (MG7-1) was fed again to the meat chopper of the same type as above and gel-pulverized to obtain hydrogel-like crosslinked polymer pulverized product (MG7-2). The solid content of the hydrogel-like crosslinked polymer pulverized product (MG7-2) discharged from the meat chopper was 18.9% by mass.
[0233] (Drying, crushing, classification process) Next, the same operations as those in the drying, pulverization, and classification steps of Reference Example 1 were carried out except that the drying time of the obtained hydrogel-like crosslinked polymer pulverized product (MG7-2) was extended to 35 minutes, to obtain water-absorbent resin powders (F7-1) and (F7-2). The particle rate (150 pass rate) of (F7-1) that passed through a 150 μm sieve was 13.2 mass%. The physical properties of the water-absorbent resin powder (F7-2) are shown in Table 1.
[0234] (Surface crosslinking process) Surface-crosslinked water-absorbent resin particles (water-absorbing agent) (R7) were obtained in the same manner as in Reference Example 1. The physical properties of the water-absorbing agent (R7) are shown in Table 2.
[0235] [Comparative Example 3] (Preparation of monomer aqueous solution, polymerization process) 200g of acrylic acid, 0.73g of N,N'-methylenebisacrylamide and 587g of deionized water were charged into a 1L reaction vessel, and the temperature of the contents was maintained at 20°C while stirring to prepare an aqueous monomer solution (T8). Nitrogen gas was then introduced until the dissolved oxygen concentration in the aqueous monomer solution (T8) was less than 0.02%, and then 2.44g of 1% by mass hydrogen peroxide solution, 2.92g of 0.2% by mass ascorbic acid solution and 6.82g of 2% by mass 2,2-azobisaminodipropane dihydrochloride solution were added to the aqueous monomer solution (T8) under a sealed condition to initiate a polymerization reaction. After the temperature of the aqueous monomer solution (1) in the reaction vessel reached about 85°C, it was heated at 60°C for 3 hours to obtain a hydrogel-like crosslinked polymer (G8).
[0236] (Gel crushing process) The obtained hydrogel cross-linked polymer (G8) was chopped into blocks of 3 to 5 cm square. Next, 800 g of the block-shaped hydrogel cross-linked polymer (G8) and 4.0 g of fine powder (FP1) which is water-absorbent resin A were mixed thoroughly in a PE bag, and 546 g of sodium hydroxide solution adjusted to 15.3 mass % (corresponding to the amount to neutralize 75 mol % of the carboxyl groups in the hydrogel cross-linked polymer (G8)) were added to the feed port of a meat chopper equipped with a rotary blade and a perforated plate (diameter 70 mm, hole diameter 5 mm, number of holes 50, thickness 8 mm, made of SUS) at the tip and having a screw shaft of 120 mm in length, and the mixture was mixed while chopping to obtain a hydrogel cross-linked polymer pulverized product (MG8-1). The time from the introduction of the hydrogel cross-linked polymer (G8) to the discharge of the hydrogel cross-linked polymer pulverized product (MG8-1) was about 30 seconds.
[0237] Subsequently, the obtained hydrogel-like crosslinked polymer pulverized product (MG8-1) was fed again to the meat chopper of the same type as above and gel-pulverized to obtain hydrogel-like crosslinked polymer pulverized product (MG8-2). The solid content of the hydrogel-like crosslinked polymer pulverized product (MG8-2) discharged from the meat chopper was 18.8% by mass.
[0238] (Drying, crushing, classification process) Next, the same operations as those in the drying, pulverization, and classification steps of Reference Example 1 were carried out except that the drying time of the obtained hydrogel-like crosslinked polymer pulverized material (MG8-2) was extended to 35 minutes, thereby obtaining water-absorbent resin powders (F8-1) and (F8-2). The particle rate (150 pass rate) of (F8-1) that passed through a 150 μm sieve was 13.6 mass%. The physical properties of the water-absorbent resin powder (F8-2) are shown in Table 1.
[0239] (Surface crosslinking process) Surface-crosslinked water-absorbent resin particles (water-absorbing agent) (R8) were obtained in the same manner as in Reference Example 1. Table 2 shows the physical property values of the water-absorbent resin particles (water-absorbing agent) (R8).
[0240] [Example 4] (Dissolution solution preparation process) 106 g of 48.5 mass% sodium hydroxide aqueous solution was added to 374 g of deionized water to prepare a 10.7 mass% sodium hydroxide aqueous solution, and 7.7 g of the water absorbent resin powder (F2-1) obtained in Reference Example 1, which is the water absorbent resin A, was added while stirring so as not to form a powder, and the mixture was stirred for 10 minutes in an ultrasonic cleaner (manufactured by Kyowa Irika Co., Ltd., KS-190N) to obtain a colorless and transparent water absorbent resin solution (A4). The temperature of the alkaline aqueous solution was 30°C when the water absorbent resin powder (F2-1), which is the water absorbent resin A, was added to the sodium hydroxide aqueous solution.
[0241] (Monomer aqueous solution preparation process, polymerization process) To a mixed solution of 422 g of acrylic acid, 0.92 g of polyethylene glycol diacrylate (weight average molecular weight 523), and 25.8 g of 0.1 mass % aqueous solution of trisodium diethylenetriaminepentaacetate, the entire amount of the aqueous alkali solution (A4) which is a water absorbent resin dissolving solution was added with stirring to obtain an aqueous solution.
[0242] Next, 246 g of 48.5% by mass aqueous sodium hydroxide solution was added while stirring the aqueous solution adjusted to 42.5°C, to obtain an aqueous monomer solution. The temperature rose to 92°C due to the heat of neutralization at this time. When the temperature of the aqueous monomer solution reached 90°C, 16.7 g of 4.5% by mass aqueous sodium persulfate solution was added, and then the mixture was poured onto a Teflon (registered trademark) sheet (a 30 cm x 30 cm reaction vessel surrounded by a dam with a height of 1.5 cm on all four sides) whose bottom had been heated to 50°C in advance in an atmosphere temperature of 60°C, and polymerization was carried out. 13 seconds after the addition of the aqueous sodium persulfate solution, the polymerization system reached a maximum temperature of 105°C. After a further 3 minutes had passed, the obtained polymer was taken out to obtain a hydrogel-like crosslinked polymer (G9).
[0243] (Gel crushing process) In the same manner as in Reference Example 1, a pulverized hydrogel crosslinked polymer (MG9) was obtained.
[0244] The pulverized hydrogel crosslinked polymer (MG9) had a gel solid content of 51.7% by mass, a gel CRC of 35.1 g / g, and a polymerization rate of 98.3%.
[0245] (Drying, crushing, classification process) Water-absorbent resin powders (F9-1) and (F9-2) were obtained in the same manner as in Reference Example 1. The physical properties of the water-absorbent resin powder (F9-2) are shown in Table 1.
[0246] (Surface crosslinking process) Surface-crosslinked water-absorbent resin particles (water-absorbing agent) (R9) were obtained in the same manner as in Reference Example 1. The physical properties of the water-absorbing agent (R9) are shown in Table 2.
[0247] [Comparative Example 4] (Preparation of monomer aqueous solution, polymerization process) A monomer solution (T10-1) consisting of 422 g of acrylic acid, 106 g of 48.5 mass% sodium hydroxide aqueous solution, 0.92 g of polyethylene glycol diacrylate (weight average molecular weight 523), 25.8 g of 0.1 mass% diethylenetriaminepentaacetate trisodium aqueous solution, and 374 g of deionized water is prepared.
[0248] Next, 246 g of 48.5 mass% aqueous sodium hydroxide solution was added while stirring the monomer solution (T10-1) adjusted to 42.5 ° C. The temperature rose to 92 ° C. due to the heat of neutralization at this time. 7.7 g of water absorbent resin powder (F2-1) which is water absorbent resin A was added thereto and stirred for 60 seconds. When the temperature of the monomer aqueous solution (T10-2) reached 90 ° C., 16.7 g of 4.5 mass% aqueous sodium persulfate solution was added while the floating matter derived from the water absorbent resin powder (F2-1) added to the monomer aqueous solution was confirmed, and then the mixture was poured onto a Teflon (registered trademark) sheet (a 30 cm × 30 cm reaction vessel surrounded by a dam with a height of 1.5 cm on all sides) whose bottom had been heated to 50 ° C. in an atmosphere temperature of 60 ° C., and polymerization was performed. 15 seconds after the addition of the aqueous sodium persulfate solution, the polymerization system reached a maximum temperature of 105 ° C. After a further 3 minutes had elapsed, the resulting polymer was taken out to obtain a hydrogel-like crosslinked polymer (G10).
[0249] (Gel crushing process) In the same manner as in Reference Example 1, a pulverized hydrogel crosslinked polymer (MG10) was obtained.
[0250] The pulverized hydrogel crosslinked polymer (MG10) had a gel solid content of 51.2 mass %, a gel CRC of 35.6 g / g, and a polymerization rate of 98.2%.
[0251] (Drying, crushing, classification process) Water-absorbent resin powders (F10-1) and (F10-2) were obtained in the same manner as in Reference Example 1. The physical properties of the water-absorbent resin powder (F10-2) are shown in Table 1.
[0252] (Surface crosslinking process) Surface-crosslinked water-absorbent resin particles (water-absorbing agent) (R10) were obtained in the same manner as in Reference Example 1. Table 2 shows the physical property values of the water-absorbent resin particles (water-absorbing agent) (R10).
[0253] [Reference example 2] Reference Example 2 was carried out according to the procedure of Example 1 of Japanese Patent No. 4969778.
[0254] Into a 2000 mL five-neck cylindrical round-bottom flask equipped with a stirrer, a reflux condenser, a dropping funnel, a thermometer, and a nitrogen gas inlet tube, 340 g of n-heptane and 0.92 g of a sucrose fatty acid ester with an HLB of 3.0 (product name: S-370, manufactured by Mitsubishi Chemical Corporation) were added, dispersed, heated to dissolve, and then cooled to 55°C.
[0255] Separately, 73.6 g of acrylic acid was charged into a 1000 mL Pack Ace, and while cooling it from the outside, 153.1 g of 20 mass % aqueous sodium hydroxide solution was added dropwise to neutralize 75 mol % of the acrylic acid. Furthermore, 3.9 g of deionized water, 0.11 g of 2,2'-azobis(2-amidinopropane) dihydrochloride, a water-soluble azo polymerization initiator, and 8.3 mg of ethylene glycol diglycidyl ether, an internal crosslinking agent, were added to prepare an aqueous monomer solution for the first stage polymerization.
[0256] The entire amount of this aqueous monomer solution for the first-stage polymerization was added to the five-neck cylindrical round-bottom flask under stirring to disperse the monomers. The atmosphere in the system was thoroughly replaced with nitrogen, and then the temperature was raised. The bath temperature was maintained at 70° C. and the polymerization reaction was carried out for 1 hour. The polymerization slurry was then cooled to room temperature.
[0257] Into another 1000 mL Pack Ace, 95.3 g of acrylic acid was charged, and while cooling, 156.0 g of a 25 mass % aqueous sodium hydroxide solution was added dropwise to neutralize 75 mol % of the acrylic acid. Further, 3.3 g of water, 0.14 g of 2,2'-azobis(2-amidinopropane) dihydrochloride, and 10.7 mg of ethylene glycol diglycidyl ether were added to prepare an aqueous monomer solution for the second-stage polymerization, which was then cooled using an ice-water bath.
[0258] After adding the entire amount of this monomer aqueous solution for the second stage polymerization to the polymerization slurry liquid, the system was again fully replaced with nitrogen, and then the temperature was raised, and the bath temperature was maintained at 70°C to carry out the second stage polymerization reaction for 2 hours. After the polymerization was completed, the mixture was heated in an oil bath at 120°C, and only water was removed from the system by azeotropic distillation to obtain a gel-like material. Next, 7.81 g of a 2 mass% ethylene glycol diglycidyl ether aqueous solution was added as a post-crosslinking agent, mixed, and a post-crosslinking reaction was carried out, and further water and n-heptane were removed by distillation and dried to obtain surface-crosslinked water absorbent resin particles (R11) with a mass average particle diameter (D50) of 376 μm.
[0259] [Example 5] (Dissolution solution preparation process) 4.7 g of water absorbent resin particles (R11) which are water absorbent resin A obtained in Reference Example 2 were added to 153.1 g of 20 mass% sodium hydroxide aqueous solution while stirring so as not to form powder, and stirred for 10 minutes while immersed in an ultrasonic cleaner (manufactured by Kyowa Irika Co., Ltd., KS-190N) to obtain an alkaline aqueous solution (A5) which is a colorless and transparent water absorbent resin solution. The temperature of the alkaline aqueous solution was 30°C when the water absorbent resin particles (R11) which are water absorbent resin A were added to the alkaline aqueous solution.
[0260] (Monomer aqueous solution preparation process, polymerization process) Into a 2000 mL five-neck cylindrical round-bottom flask equipped with a stirrer, a reflux condenser, a dropping funnel, a thermometer, and a nitrogen gas inlet tube, 340 g of n-heptane and 0.92 g of a sucrose fatty acid ester with an HLB of 3.0 (product name: S-370, manufactured by Mitsubishi Chemical Corporation) were added, dispersed, heated to dissolve, and then cooled to 55°C.
[0261] Separately, 73.6 g of acrylic acid was charged into a 1000 mL Pack Ace, and while cooling it from the outside, 157.8 g of the total amount of the aqueous alkali solution (A5) which is a water-absorbing resin solution was dropped to neutralize 75 mol % of the acrylic acid. Furthermore, 3.9 g of deionized water, 0.11 g of 2,2'-azobis(2-amidinopropane) dihydrochloride which is a water-soluble azo-based polymerization initiator, and 8.3 mg of ethylene glycol diglycidyl ether which is an internal crosslinking agent were added to prepare an aqueous monomer solution for the first stage polymerization.
[0262] The entire amount of this aqueous monomer solution for the first-stage polymerization was added to the five-neck cylindrical round-bottom flask under stirring to disperse the monomers. The atmosphere in the system was thoroughly replaced with nitrogen, and then the temperature was raised. The bath temperature was maintained at 70° C. and the polymerization reaction was carried out for 1 hour. The polymerization slurry was then cooled to room temperature.
[0263] Into another 1000 mL Pack Ace, 95.3 g of acrylic acid was charged, and while cooling, 156.0 g of a 25 mass % aqueous sodium hydroxide solution was added dropwise to neutralize 75 mol % of the acrylic acid. Further, 3.3 g of water, 0.14 g of 2,2'-azobis(2-amidinopropane) dihydrochloride, and 10.7 mg of ethylene glycol diglycidyl ether were added to prepare an aqueous monomer solution for the second-stage polymerization, which was then cooled using an ice-water bath.
[0264] After the entire amount of this monomer aqueous solution for the second stage polymerization was added to the polymerization slurry liquid, the system was again fully replaced with nitrogen, and then the temperature was raised, and the bath temperature was maintained at 70°C to carry out the second stage polymerization reaction for 2 hours. After the polymerization was completed, the mixture was heated in an oil bath at 120°C, and only water was removed from the system by azeotropic distillation to obtain a gel-like material. Next, 7.81 g of a 2 mass% ethylene glycol diglycidyl ether aqueous solution was added as a post-crosslinking agent, mixed, and a post-crosslinking reaction was carried out, and further water and n-heptane were removed by distillation and dried to obtain surface-crosslinked water-absorbent resin particles (water absorbent) (R12) with a mass average particle diameter (D50) of 435 μm. The physical properties of the water absorbent (R12) are shown in Table 2.
[0265] [Comparative Example 5] Into a 2000 mL five-neck cylindrical round-bottom flask equipped with a stirrer, a reflux condenser, a dropping funnel, a thermometer, and a nitrogen gas inlet tube, 340 g of n-heptane and 0.92 g of a sucrose fatty acid ester with an HLB of 3.0 (product name: S-370, manufactured by Mitsubishi Chemical Corporation) were added, dispersed, heated to dissolve, and then cooled to 55°C.
[0266] Separately, 73.6 g of acrylic acid was charged into a 1000 mL Pack Ace, and while cooling it from the outside, 153.1 g of a 20 mass% aqueous sodium hydroxide solution was dropped to neutralize 75 mol% of the acrylic acid. Furthermore, 4.7 g of water absorbent resin particles (R11) which is water absorbent resin A, 3.9 g of deionized water, 0.11 g of 2,2'-azobis(2-amidinopropane) dihydrochloride which is a water-soluble azo-based polymerization initiator, and 8.3 mg of ethylene glycol diglycidyl ether which is an internal crosslinking agent were added to prepare an aqueous monomer solution for the first stage polymerization.
[0267] The entire amount of this aqueous monomer solution for the first-stage polymerization was added to the five-neck cylindrical round-bottom flask under stirring to disperse the monomers. The system was thoroughly purged with nitrogen, and then the temperature was raised. The bath temperature was maintained at 70°C and the polymerization reaction was carried out for 1 hour. The polymerization slurry was then cooled to room temperature. However, unlike in Example 5, precipitation of coarse particles was observed at the bottom of the flask, and the second-stage polymerization reaction was therefore discontinued.
[0268] [Table 1]
[0269] [Table 2]
[0270] From the above results, the water absorbing agent obtained by the manufacturing method of the present invention suppressed the deterioration of the basic physical properties of CRC and AAP (0.3 psi). In addition, the water absorbing agent obtained by the manufacturing method of the present invention had a faster water absorption speed and a reduced amount of residual monomer than the corresponding comparative examples. In addition, in Comparative Example 5, the physical properties were not measured because the second-stage polymerization could not be performed.
Claims
1. A method for producing a water-absorbing agent, comprising adding a water-absorbing resin solution obtained by using a water-absorbing resin and an alkaline agent to a production process of the water-absorbing agent, The water-absorbent resin solution is obtained by mixing an aqueous solution of the alkaline agent and the water-absorbent resin, and a concentration of the alkaline agent in the aqueous solution of the alkaline agent is 5 to 30 mass %, The water-absorbent resin contains a crosslinked polymer obtained by polymerizing an acid group-containing unsaturated monomer (salt), The method for producing a water-absorbing agent, wherein the alkaline agent is a hydroxide of an alkali metal.
2. The method for producing a water-absorbing agent according to claim 1, wherein the water-absorbing resin solution is added to any one or more of the following production steps (1) to (5): (1) Preparation of an aqueous monomer solution (2) Polymerization process (3) Gel crushing process (4) Fine powder granulation process (5) Surface crosslinking step.
3. The method for producing a water-absorbing agent according to claim 2, wherein the water-absorbing resin solution is added to any one or more of the production steps (1), (2) and (3).
4. The method for producing a water-absorbing agent according to claim 3, wherein the water-absorbing resin solution is added to the production step (1).
5. 5. The method for producing a water-absorbing agent according to claim 3 or 4, wherein the water-absorbing agent contains an acid group-containing unsaturated monomer as a main component as a raw material monomer of the water-absorbing agent, and the water-absorbing resin solution is used as a whole or a part of a neutralizer for the acid group-containing unsaturated monomer as the raw material monomer of the water-absorbing agent or a polymer thereof.
6. A method for producing a water absorbent according to claim 5, wherein the water absorbent resin solution is used as a part of a neutralizer for an acid group-containing unsaturated monomer or its polymer as a raw material monomer for the water absorbent.
7. The method for producing a water absorbent according to claim 6, wherein the water absorbent resin solution is used as a part of a neutralizing agent for an acid group-containing unsaturated monomer as a raw material monomer of the water absorbent.
8. The method for producing a water absorbent according to claim 1, wherein the alkaline agent is sodium hydroxide and / or potassium hydroxide.
9. The method for producing a water absorbent according to any one of claims 1 to 8, wherein the water absorbent resin is a poly(meth)acrylic acid (salt)-based polymer.
10. The method for producing a water absorbing agent according to any one of claims 1 to 9, wherein the water absorbing resin has a solid content of 85 mass % or more.
11. The method for producing a water-absorbing agent according to any one of claims 1 to 10, wherein the water-absorbing resin has a CRC of 18 g / g or more.
12. The method for producing a water absorbing agent according to any one of claims 1 to 11, wherein a Vortex (water absorption speed) of the water absorbing agent is 50 seconds or less.
13. The method for producing a water absorbing agent according to any one of claims 1 to 12, wherein the amount of residual monomers in the water absorbing agent is 500 ppm or less.
Citation Information
Patent Citations
Method for manufacturing water-swellable products using ultrafine water-swellable polymer powder
JP1993508674A
Method for recycling aqueous fluid absorbent fines to polymerizer
JP1994510551A
Production of granulated water-absorbing resin
JP1999106514A
Process for the production of highly absorbent polymer gels using highly absorbent polymer fine powders
JP2012506462A
Transparent aqueous solution containing polyacrylic acid salt and potassium hydroxide
JP2016108400A