Oil-resistant film, oil-resistant base material and oil-resistant paper

The combination of polyvinyl alcohol polymer and low-Tg polymer particles in a sea-island structure addresses oil resistance issues in conventional films, ensuring effective oil barrier performance on flat and folded surfaces without fluorine-based complications.

JP7572859B2Active Publication Date: 2024-10-24KURARAY CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2020561541
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-17
Filing Date
2019-12-20
Publication Date
2024-10-24
Estimated Expiration
2039-12-20

AI Technical Summary

Technical Problem

Conventional non-fluorine-based oil-resistant films and papers suffer from inadequate oil resistance, particularly at bends where cracking occurs, leading to oil penetration and contamination, and existing solutions like polyethylene laminates cause steam retention and recycling issues.

Method used

An oil-resistant film comprising polyvinyl alcohol polymer and polymer particles with a glass transition temperature below 40°C, forming a sea-island phase separation structure, enhances oil resistance on both flat and folded parts.

Benefits of technology

The film provides excellent oil resistance on both flat and folded parts, preventing oil penetration and contamination, while being recyclable without the need for expensive equipment and toxic fluorine compounds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572859000006
    Figure 0007572859000006
  • Figure 0007572859000007
    Figure 0007572859000007
  • Figure 0007572859000008
    Figure 0007572859000008
Patent Text Reader

Abstract

The present invention provides an oil-resistant film that provides an oil-resistant substrate with excellent oil resistance not only in the flat portion of a packaging body but also in the folded portion, and also provides an oil-resistant substrate having the oil-resistant film and an oil-resistant paper having the oil-resistant film. Specifically, the present invention provides an oil-resistant film that contains a polyvinyl alcohol-based polymer (A) and polymer particles (B) containing a polymer having a glass transition temperature of 40°C or lower, and in which the content of the polymer particles (B) is 1 part by mass or more and less than 150 parts by mass per 100 parts by mass of the polyvinyl alcohol-based polymer (A), and an oil-resistant substrate (oil-resistant paper) having the oil-resistant film on a substrate (paper).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an oil-resistant film, an oil-resistant substrate, and an oil-resistant paper. [Background technology]

[0002] Packaging materials used for serving oily foods such as French fries and fried chicken, packaging sheets for wrapping butter, and cooking paper used for baking bread or cakes are required to have a function of preventing oil from leaking out of the food. When oil contained in food permeates the packaging material and leaks out, the surface of the packaging material may be stained with oil, causing the printed area on the surface of the packaging material to bleed due to oil stains, and the OCR suitability of barcodes and QR codes (registered trademarks) may be reduced. There is also a problem that the oil may transfer to clothes or skin, causing contamination. To solve such problems, it is known to use polylaminated paper such as polyethylene laminated paper for packaging materials. However, since it has low moisture permeability and does not allow steam to pass through, there is a problem that when hot food is wrapped in the packaging material, it becomes steamy and soggy. Furthermore, in order to recycle paper, it is necessary to use equipment (such as a crusher) to remove the polyethylene film, but because the polyethylene adheres to the equipment and is difficult to remove, and because the equipment is expensive, the price of recycled paper also increases, which is an obstacle to promoting the use of recycled paper in the market. For this reason, packaging that uses a coating agent that does not need to be removed later has been considered, and for example, a method has been proposed in which a fluorine-based oil-resistant agent containing a fluorine compound (see, for example, Patent Document 1) is attached to the surface or inside of the packaging.

[0003] When a fluorine-based oil-resistant agent containing a fluorine compound is used in a package, when the package is incinerated, highly corrosive gases such as hydrogen fluoride gas and organic gases other than resins made of hydrocarbons may be generated. In addition, fluorine compounds and fluorine-containing organic compounds generated by the combustion of the fluorine compounds are generally difficult to decompose, and there are concerns about environmental loads and health damage. Furthermore, fluorine compounds are expensive to begin with. Therefore, for example, as an oil-resistant agent used in a package for food, an oil-resistant agent other than a fluorine-based oil-resistant agent, that is, a non-fluorine-based oil-resistant agent, is desired.

[0004] As an invention relating to a non-fluorinated oil-resistant agent, there has been proposed an oil-resistant, water-absorbing composition (see Patent Document 2) which contains an acrylic resin, a film-forming agent, and water-insoluble cellulose, in which the acrylic resin and the film-forming agent are contained in a weight ratio of acrylic resin / film-forming agent = 90 / 10 to 40 / 60, and the water-soluble cellulose is contained in an amount of 0.5 to 5 parts by weight per 100 parts by weight of the total of the acrylic resin and the film-forming agent. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2009-120996 A [Patent Document 2] JP 2016-124898 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the case of a package using a conventional non-fluorinated oil-proofing agent, although the oil resistance on the flat surface is good to a certain extent, it is not necessarily sufficient. Also, it has been found that cracks occur in the oil-resistant film at the folded portion, which makes it easy for oil to penetrate through the cracks, resulting in problems such as oil stains on the folded portion, which damages the appearance, and oil transfers to clothes or skin, causing staining. In particular, when the amount of oil-proofing agent applied is small, such problems tend to occur easily, so it has been even more difficult to avoid the above problems while reducing the amount of application in order to achieve excellent moisture permeability required for food packaging. On the other hand, it is possible to add a plasticizer such as glycerin to the film-forming agent to impart flexibility and make the oil-resistant film less likely to crack even at bent parts. However, this method plasticizes the oil-resistant film (reducing its elastic modulus), making it more likely for oil to penetrate the film and for the plasticizer to bleed out of the film, which can cause contamination of clothing or skin.

[0007] Therefore, the object of the present invention is to provide an oil-resistant film that can provide an oil-resistant substrate having excellent oil resistance not only in the flat portion of the packaging body but also in the folded portion, and to provide an oil-resistant substrate having said oil-resistant film and an oil-resistant paper having said oil-resistant film. [Means for solving the problem]

[0008] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by an oil-resistant film containing a predetermined amount of a polyvinyl alcohol-based polymer and a polymer particle containing a polymer having a glass transition temperature of a predetermined value or lower. Based on this finding, further research has led to the completion of the present invention. That is, the present invention is as follows.

[0009] [1] An oil-resistant film comprising: a polyvinyl alcohol-based polymer (A) and polymer particles (B) containing a polymer having a glass transition temperature of 40°C or lower, wherein the content of the polymer particles (B) is 1 part by mass or more and less than 150 parts by mass per 100 parts by mass of the polyvinyl alcohol-based polymer (A). [2] The oil-resistant film according to the above [1], wherein the polymer particles (B) have a number average molecular weight of 5,000 or more. [3] The oil-resistant film according to the above [1] or [2], wherein the average particle size of the polymer particles (B) is 10 to 500 nm. [4] The oil-resistant film according to any one of the above [1] to [3], wherein the polymer particles (B) are (meth)acrylic acid ester-based polymer particles. [5] The oil-resistant film according to any one of the above [1] to [4], wherein the polymer particles (B) are (meth)acrylic acid ester-based homopolymer particles. [6] The oil-resistant film according to any one of the above [1] to [5], wherein the polymer particles (B) contain a dispersant containing an ionic group. [7] The oil-resistant film according to the above [6], wherein the ionic group is at least one selected from the group consisting of anionic groups and salts of anionic groups. [8] The oil-resistant film according to any one of the above [1] to [3], wherein the polymer particles (B) are at least one selected from the group consisting of aromatic vinyl compound-conjugated diene compound copolymer particles and vinyl acetate polymer particles. [9] The oil-resistant film according to any one of the above [1] to [8], wherein the polyvinyl alcohol-based polymer (A) is an unmodified polyvinyl alcohol or a modified polyvinyl alcohol.

[10] The oil-resistant film according to any one of the above [1] to [9], wherein the polyvinyl alcohol-based polymer (A) is an ethylene-vinyl alcohol copolymer, and the content of ethylene units in the ethylene-vinyl alcohol copolymer is 0.5 to 19 mol % based on all structural units.

[11] The oil-resistant film according to any one of the above [1] to

[10] , wherein the oil-resistant film has a phase-separated structure of a sea-island structure, in which the polyvinyl alcohol-based polymer (A) constitutes a sea phase and the polymer particles (B) constitute an island phase.

[12] The oil-resistant film according to any one of the above [1] to

[11] , having a thickness of 0.1 to 50 μm.

[13] An oil-resistant substrate having the oil-resistant film according to any one of the above [1] to

[12] on the substrate.

[14] Grease-resistant paper having an oil-resistant film according to any one of [1] to

[12] above on the paper. Effect of the Invention

[0010] According to the present invention, it is possible to provide an oil-resistant film that provides an oil-resistant substrate having excellent oil resistance not only in the flat portion of a packaging body but also in the folded portion, and to provide an oil-resistant substrate having said oil-resistant film and an oil-resistant paper having said oil-resistant film. [Brief description of the drawings]

[0011] [Figure 1] 1 is a scanning electron microscope (SEM) photograph of a cross section of the grease-resistant paper having an oil-resistant film produced in Example 1 before the paper was folded. [Diagram 2] 1 is a scanning electron microscope (SEM) photograph of a cross section of the grease-resistant paper having an oil-resistant film produced in Example 1 after being folded and then returned to its original shape. [Diagram 3] 1 is a transmission electron microscope (TEM) photograph (direct magnification: 10,000 times) of a cast film separately prepared for observation of a phase-separated structure in Example 1. [Figure 4] 1 is a transmission electron microscope (TEM) photograph (direct magnification: 50,000 times) of a cast film separately prepared for observing a phase-separated structure in Example 1. [Diagram 5] 1 is a scanning electron microscope (SEM) photograph of a cross section of comparative grease-resistant paper having an oil-resistant film produced in Comparative Example 1 before being folded. [Figure 6] 1 is a scanning electron microscope (SEM) photograph of a cross section of comparative grease-resistant paper having an oil-resistant film produced in Comparative Example 1 after being folded and then returned to its original shape. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The oil-resistant film of the present invention contains a predetermined amount of a polyvinyl alcohol-based polymer (A) and a polymer particle (B) containing a polymer having a glass transition temperature (Tg) of 40° C. or less. By using the oil-resistant film, an oil-resistant base material having excellent oil resistance can be obtained not only in the flat part of the package but also in the folded part. In this specification, "polyvinyl alcohol" may be referred to as "PVA", and "polyvinyl alcohol-based polymer" may be referred to as "PVA-based polymer". The total content of the polyvinyl alcohol polymer (A) and the polymer particles (B) containing a polymer having a glass transition temperature of 40° C. or less in the oil-resistant film of the present invention is, from the viewpoint of the effects of the present invention, preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, and may be substantially 100% by mass. In this specification, "room temperature" refers to 25°C. Each component contained in the oil-resistant film will be described in detail below.

[0013] <Polyvinyl alcohol polymer (A)> Polyvinyl alcohol polymer (A) [hereinafter, sometimes referred to as "PVA polymer (A)"] is a polymer having a vinyl alcohol unit, and in some cases, a polymer having a vinyl alcohol unit and a vinyl alcohol derivative unit. In this specification, "having a unit" means "having a structural unit derived from". The vinyl alcohol unit is a structural unit that is linked at a vinyl group site and has a hydroxyl group as a side chain. The vinyl alcohol derivative unit is not particularly limited, and examples thereof include (1) a structural unit in which a hydroxyl group of the vinyl alcohol unit is converted to an acetoxy group, and (2) a structural unit in which two vinyl alcohol units are acetalized. Note that the vinyl alcohol derivative unit does not necessarily have to be derived from vinyl alcohol as long as the structural unit can be derived from a vinyl alcohol unit or the derivative unit can be converted to vinyl alcohol. Incidentally, the PVA polymer (A) may be an ionomer, although it is not particularly limited thereto. The term "ionomer" is defined in the same manner as in the general definition, that is, it is a polymer having an intermolecular crosslinking structure or molecular aggregation structure caused by ions. The ions are not particularly limited, but include alkali metal cations, alkaline earth metal cations, transition metal cations such as zinc, organic cations such as ammonium ions, and anions such as halide ions.

[0014] Examples of the PVA-based polymer (A) include unmodified PVA and modified PVA. Here, "unmodified PVA" refers to a PVA obtained by saponifying a homopolymer of a vinyl ester and a PVA obtained by saponifying a copolymer of two or more vinyl esters. "Modified PVA" refers to a PVA in which at least a part of the molecular terminal, main chain, and side chain of the unmodified PVA is substituted (including crosslinked) with a reactive group or the like, and a PVA obtained by saponifying a copolymer of a vinyl ester and another ethylenically unsaturated monomer, or both of these PVAs.

[0015] The modified PVA includes PVA obtained by saponifying a copolymer of vinyl ester and other ethylenically unsaturated monomer as described above, and in the case of this PVA, it is a PVA containing at least one unit of "other ethylenically unsaturated monomer" described in "Production method of PVA-based polymer (A)" described later together with vinyl alcohol unit. Among them, ethylene-modified PVA, carboxyl group or its salt-modified PVA, silicon-modified PVA, acetoacetyl group-modified PVA, diacetone group-modified PVA, maleic anhydride-modified PVA, hydroxyl group-modified PVA, etc. are preferred, and ethylene-modified PVA is more preferred. The PVA-based polymer (A) may be used alone or in combination of two or more kinds. As the PVA-based polymer (A), among the above-mentioned examples, unmodified PVA and ethylene-modified PVA are preferred from the viewpoint of oil resistance. Either unmodified PVA or ethylene-modified PVA may be used, but ethylene-modified PVA is more preferred from the viewpoint of oil resistance and water resistance.

[0016] (Ethylene modified PVA) From the viewpoints of oil resistance and water resistance, the ethylene-modified PVA is preferably an ethylene-vinyl alcohol copolymer, and from the viewpoints of oil resistance, water resistance and ease of preparation of an aqueous solution or dispersion, the content of ethylene units in the ethylene-vinyl alcohol copolymer is preferably 0.5 to 19 mol% based on the total structural units. If it is 0.5 mol% or more, the water resistance of the oil-resistant film tends to be good, and if it is 19 mol% or less, the preparation of an aqueous solution or dispersion of the ethylene-vinyl alcohol copolymer tends to be easy. From the same viewpoint, the content of ethylene units in the ethylene-vinyl alcohol copolymer is more preferably 1.5 to 15 mol %, further preferably 2.0 to 12 mol %, and particularly preferably 4.0 to 8.0 mol %, based on all structural units. Hereinafter, the explanation regarding ethylene-modified PVA can be read as the explanation regarding ethylene-vinyl alcohol copolymer.

[0017] The content of ethylene units in ethylene-modified PVA is: 1 For example, the ethylene unit-containing vinyl ester copolymer, which is a precursor or reacetylated product of ethylene-modified PVA, can be determined by H-NMR measurement. 1 The H-NMR measurement is used to determine the amount of the vinyl ester copolymer. More specifically, the vinyl ester copolymer is purified by reprecipitation in a mixture of n-hexane and acetone three or more times, and then dried under reduced pressure at 80°C for three days to obtain a vinyl ester copolymer for analysis. The vinyl ester copolymer is dissolved in DMSO-d6 and 1 The measurement is performed using a H-NMR measurement device (e.g., 500 MHz) at 80° C. The content of ethylene units is calculated using the peak (4.7 to 5.2 ppm) derived from the main chain methine of the vinyl ester and the peak (0.8 to 1.6 ppm) derived from the main chain methylene of ethylene, vinyl ester, and the third component.

[0018] The ethylene-modified PVA contains vinyl alcohol units and ethylene units, and in some cases vinyl ester units, and may or may not further contain other monomer units. Examples of compounds constituting the other monomer units include, but are not limited to, α-olefins such as propylene, 1-butene, isobutene, and 1-hexene; unsaturated acids or salts thereof, such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, maleic anhydride, and itaconic acid, or monoalkyl esters or dialkyl esters of the unsaturated acids; vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, and n-butyl vinyl ether; hydroxyl group-containing vinyl ethers such as ethylene glycol vinyl ether, 1,3-propanediol vinyl ether, and 1,4-butanediol vinyl ether; allyl ethers such as allyl acetate, propyl allyl ether, butyl allyl ether, and hexyl allyl ether; compounds having an oxyalkylene group; vinyl silyl compounds such as vinyltrimethoxysilane; isopropenyl acetate; 3-buten-1-ol, 4-penten-1-ol, and the like. hydroxyl group-containing α-olefins such as olefins, 5-hexen-1-ol, 7-octen-1-ol, 9-decen-1-ol, and 3-methyl-3-buten-1-ol; compounds having a sulfonic acid group derived from ethylene sulfonic acid, allyl sulfonic acid, methallyl sulfonic acid, 2-acrylamido-2-methylpropane sulfonic acid, or a salt thereof; and compounds having a cationic group derived from vinyloxyethyl trimethyl ammonium chloride, vinyloxybutyl trimethyl ammonium chloride, vinyloxyethyl dimethylamine, vinyloxymethyl diethylamine, N-acrylamido methyl trimethyl ammonium chloride, 3-(N-methacrylamido)propyl trimethyl ammonium chloride, N-acrylamido ethyl trimethyl ammonium chloride, N-acrylamido dimethylamine, allyl trimethyl ammonium chloride, methallyl trimethyl ammonium chloride, dimethylallylamine, allylethylamine, or the like. When the ethylene-modified PVA contains other monomer units, the content thereof is preferably 20 mol % or less, may be 5 mol % or less, may be 1 mol % or less, or may be 0.5 mol % or less.

[0019] (Viscosity average degree of polymerization) The viscosity average degree of polymerization of the PVA polymer (A) [hereinafter sometimes abbreviated as "degree of polymerization"] is preferably 200 to 18,000. The degree of polymerization of the PVA polymer (A) is more preferably 300 to 15,000, further preferably 300 to 10,000, further more preferably 300 to 5,000, particularly preferably 300 to 3,000, and most preferably 500 to 2,000. When the degree of polymerization of the PVA polymer (A) is equal to or higher than the lower limit, the strength of the oil-resistant film is prevented from decreasing and the film is easily permeated into the substrate during coating, and as a result, the oil resistance tends to improve. On the other hand, when the degree of polymerization is equal to or lower than the upper limit, the solution viscosity is prevented from increasing, and the moldability tends to improve. The degree of polymerization of the PVA polymer (A) is a value measured by the method described in "3.7 Average degree of polymerization" of JIS K6726 (1994).

[0020] (Saponification degree) The saponification degree of the PVA polymer (A) is preferably 50 mol% or more, more preferably 70 mol% or more, even more preferably 85 mol% or more, particularly preferably 95 mol% or more, and most preferably 98 mol% or more. The upper limit of the saponification degree of the PVA polymer (A) is not particularly limited, and may be 100 mol% or 99.8 mol%. If the saponification degree is 50 mol% or more, the solubility in water is good, and it tends to be easy to prepare an aqueous solution or aqueous dispersion of the PVA polymer (A). In addition, by increasing the saponification degree, the moisture permeability of the PVA polymer (A) tends to be increased. The degree of saponification is a value measured by the method described in "3.5 Degree of saponification" of JIS K6726 (1994).

[0021] (Production method of PVA polymer (A)) There is no particular limitation on the method for producing the PVA polymer (A), and a general production method can be adopted, for example, by saponifying a polyvinyl ester. Examples of the polyvinyl ester include (i) homopolymers of vinyl esters, (ii) copolymers of two or more kinds of vinyl esters, and (iii) copolymers of vinyl esters and other ethylenically unsaturated monomers. Examples of the vinyl ester include vinyl formate, vinyl acetate, vinyl propionate, vinyl versatate, vinyl pivalate, etc. Among these, vinyl acetate is preferred from the viewpoint of production costs. The other ethylenically unsaturated monomer is not particularly limited as long as it is copolymerizable with the vinyl ester, and examples thereof include ethylene, α-olefin, halogen-containing monomer, carboxylic acid-containing monomer and its anhydride or ester, (meth)acrylic acid ester, vinyl ether, sulfonic acid group-containing monomer, amide group-containing monomer, amino group-containing monomer, quaternary ammonium base-containing monomer, silyl group-containing monomer, hydroxyl group-containing monomer, acetyl group-containing monomer, etc. Among these, ethylene is preferable as the other ethylenically unsaturated monomer.

[0022] The PVA polymer (A) may be copolymerized with other monomers, or may be modified at the end of the polymer using a chain transfer agent. Examples of the chain transfer agent include aldehydes such as acetaldehyde, propionaldehyde, butylaldehyde, and benzaldehyde; ketones such as acetone, methyl ethyl ketone, hexanone, and cyclohexanone; mercaptans such as 2-hydroxyethanethiol; thiocarboxylic acids such as thioacetic acid; and halogenated hydrocarbons such as trichloroethylene and perchloroethylene. Among these, aldehydes and ketones are preferred. When a chain transfer agent is used, the amount of the chain transfer agent can be determined according to the chain transfer coefficient of the chain transfer agent used and the polymerization degree of the desired PVA polymer (A), and is not particularly limited, but is preferably 0.1 to 10 parts by mass relative to 100 parts by mass of vinyl ester.

[0023] The polymerization method for producing the polyvinyl ester may be a known method such as bulk polymerization, solution polymerization, suspension polymerization, emulsion polymerization, or dispersion polymerization. Among these, from an industrial viewpoint, solution polymerization, emulsion polymerization, or dispersion polymerization is preferred. For the polymerization operation, any of a batch method, a semi-batch method, or a continuous method may be used. The polymerization temperature is not particularly limited, but is preferably from 0 to 150°C, more preferably from 20 to 150°C, and even more preferably from 30 to 80°C. The polyvinyl ester thus obtained is saponified with a saponification catalyst such as sodium hydroxide, and if necessary, subjected to a pulverization step, a drying step, and the like, to obtain a PVA polymer (A). The PVA polymer (A) may be used in the form of a solution dissolved in water or the like, or in the form of a dispersion dispersed therein, or in a mixture of both.

[0024] <Polymer particles (B) containing a polymer having a glass transition temperature (Tg) of 40° C. or less> The oil-resistant film of the present invention contains polymer particles (B) containing a polymer having a Tg of 40° C. or less [hereinafter, may be simply referred to as "polymer particles (B)] together with the PVA polymer (A). The polymer particles (B) may be a polymer itself having a Tg of 40° C. or less. The polymer particles (B) may be used alone or in combination of two or more kinds. However, the polymer particles (B) are not the PVA polymer (A) itself. The polymer particles (B) may be single-layer type polymer particles (single particles), or may be core-shell type polymer particles consisting of a core and a shell covering at least a part of the core. In the case of core-shell particles, at least one of the core and the shell may contain a polymer having a Tg of 40° C. or less. The polymer particles (B) may be an ionomer. The ionomer is as described above. The polymer particles (B) containing a polymer having a Tg of 40° C. or less are highly flexible, and by including the polymer particles (B), the stress generated in the oil-resistant film is dispersed, the oil-resistant film is less likely to crack at the folded portion of the package, and the oil resistance is improved. In addition, by blending the polymer particles (B) with the PVA polymer (A), the breaking elongation of the obtained oil-resistant film tends to be improved. From the viewpoint of improving the oil resistance at the folded portion of the packaging body, the polymer particles (B) preferably contain a polymer having a Tg of -100 to 40°C, more preferably contain a polymer having a Tg of -100 to 35°C, even more preferably contain a polymer having a Tg of -70 to 20°C, even more preferably contain a polymer having a Tg of -70 to 0°C, even more preferably contain a polymer having a Tg of -70 to -10°C, particularly preferably contain a polymer having a Tg of -65 to -35°C, and most preferably contain a polymer having a Tg of -60 to -50°C. In the present invention, Tg is a value determined according to the method described in the Examples.

[0025] (Average particle size) The average particle size of the polymer particles (B) is not particularly limited, but from the viewpoint of the balance between polymerization stability and polymerization rate and from the viewpoint of oil resistance, it is preferably 10 to 500 nm, more preferably 50 to 400 nm, even more preferably 100 to 350 nm, and even more preferably 200 to 300 nm. The average particle size may be 10 to 150 nm, 20 to 120 nm, 50 to 100 nm, 50 to 80 nm, or 50 to 300 nm, 80 to 300 nm, 130 to 280 nm, 150 to 280 nm, 200 to 280 nm, or 200 to 250 nm. The average particle size is a median size obtained by measuring the polymer particles (B) present in the aqueous dispersion by a dynamic light scattering measuring device according to the method described in the Examples. However, since the average particle size of the polymer particles (B) present in the oil-resistant film determined by observation with a transmission electron microscope (TEM) according to the method described in the Examples also tends to be approximately the same as the average particle size measured with a dynamic light scattering measuring device, it is preferable that the average particle size in this case is also within the above-mentioned range. The average particle size refers to the primary particle size of the polymer particles (B), but when the polymer particles (B) are aggregated in the film to form secondary particles, the secondary particle size of the aggregated particles may be 20 to 15,000 nm, 40 to 10,000 nm, 100 to 8,000 nm, or 160 to 7,500 nm. However, from the viewpoint of oil resistance, it is preferable that the polymer particles (B) are not aggregated.

[0026] (Number average molecular weight (Mn)) From the viewpoint of improving the oil resistance at the folded portion of the package, the number average molecular weight of the polymer particles (B) is preferably 5,000 or more, more preferably 5,000 to 150,000, even more preferably 8,000 to 120,000, still more preferably 10,000 to 100,000, and particularly preferably 15,000 to 100,000. From the same viewpoint, the number average molecular weight may be 5,000 to 50,000, 10,000 to 50,000, 15,000 to 50,000, 15,000 to 35,000, 35,000 to 150,000, 45,000 to 120,000, or 70,000 to 100,000. Here, the number average molecular weight is a value calculated in terms of standard polystyrene as measured by gel permeation chromatography (GPC), and more specifically, is a value measured according to the measurement method described in the Examples.

[0027] The polymer particles (B) may be a homopolymer consisting of one type of monomer unit, or a copolymer consisting of multiple types of monomer units. From the viewpoint of improving the oil resistance at the folded portion of the package, the polymer particles (B) preferably contain a polymer (B1) containing an ethylenically unsaturated monomer (b1) unit, more preferably contain 50% by mass or more of a polymer (B1) containing an ethylenically unsaturated monomer (b1) unit, even more preferably contain 80% by mass or more of a polymer (B1) containing an ethylenically unsaturated monomer (b1) unit, particularly preferably contain 90% by mass or more of a polymer (B1) containing an ethylenically unsaturated monomer (b1) unit, and most preferably contain substantially 100% by mass of a polymer (B1) containing an ethylenically unsaturated monomer (b1) unit, i.e., a polymer (B1) containing substantially an ethylenically unsaturated monomer (b1) unit. The proportion of ethylenically unsaturated monomer (b1) units contained in polymer (B1) is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more.

[0028] The polymer particles (B) may contain other polymers other than the polymer (B1) as necessary. Examples of such other polymers include PVA polymers (A), and the preferred ones are the same as those described for the PVA polymer (A). When the polymer particles (B) contain other polymers, the content is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 20% by mass or less, even more preferably 10% by mass or less, and particularly preferably 5% by mass or less. In addition, it is also a preferred embodiment that the polymer particles (B) do not contain a PVA polymer.

[0029] Hereinafter, the "ethylenically unsaturated monomer (b1)" may be simply referred to as the "monomer (b1)". Also, the "polymer (B1) containing an ethylenically unsaturated monomer (b1) unit" may be simply referred to as the "polymer (B1)". In the present specification, "(meth)acryl" means one or two selected from "acryl" and "methacryl." In addition, "(N-alkyl)(meth)acrylamide" means one or more selected from "(meth)acrylamide" and "N-alkyl(meth)acrylamide." In other words, it is a general term for compounds in which the nitrogen atom of (meth)acrylamide is substituted with an alkyl group and compounds in which the alkyl group is not substituted.

[0030] <Ethylenically unsaturated monomer (b1)> Examples of the monomer (b1) include (meth)acrylic acid and salts thereof; methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, tricyclodecanyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, 3-(trimethoxysilyl)propyl (meth)acrylate, hydroxyalkyl (meth)acrylates, and N,N'-dialkylamino (meth)acrylate. (Meth)acrylic acid esters such as alkyl esters, tri(meth)acrylic acid esters [e.g., trimethylolpropane tri(meth)acrylate], and tetra(meth)acrylic acid esters [e.g., pentaerythritol tetra(meth)acrylate]; (N-alkyl)(meth)acrylamides such as (meth)acrylamide, N-methyl(meth)acrylamide, and N-ethyl(meth)acrylamide; styrene, α-methylstyrene, 1-vinylnaphthalene, 3-methylstyrene, 4-propylstyrene, 4 -Aromatic vinyl compounds such as cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, and halogenated styrenes; vinyl cyanide compounds such as acrylonitrile and methacrylonitrile; butadiene, isoprene, 2,3-dimethylbutadiene, 2-methyl-3-ethylbutadiene, 1,3-pentadiene, 3-methyl-1,3-pentadiene, 2-ethyl-1,3-pentadiene, 1,3-hexadiene, 2-methyl-1,3-hexadiene, 3,4 -Dimethyl-1,3-hexadiene, 1,3-heptadiene, 3-methyl-1,3-heptadiene, 1,3-octadiene, cyclopentadiene, chloroprene, myrcene, farnesene, and other conjugated diene compounds; aliphatic vinyl compounds such as ethylene and isobutylene; esters of unsaturated monocarboxylic acids and unsaturated alcohols such as allyl (meth)acrylate, methallyl (meth)acrylate, allyl cinnamate, methallyl cinnamate, diallyl maleate, diallyl phthalate, diallyl terephthalate, and diallyl isophthalate;Examples of the diesters include diesters of unsaturated monocarboxylic acids and glycols, such as ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, and hexanediol di(meth)acrylate; polyfunctional aromatic vinyls, such as divinylbenzene; and vinyl acetates, such as vinyl acetate. As the monomer (b1), one type may be used alone, or two or more types may be used in combination.

[0031] Among the examples of the monomer (b1), from the viewpoint of the effect of improving the oil resistance at the folded portion of the packaging body, (meth)acrylic acid esters, aromatic vinyl compounds, conjugated diene compounds, aliphatic vinyl compounds, and vinyl acetate are preferred, and methyl methacrylate, ethyl acrylate, n-butyl acrylate, t-butyl acrylate, allyl methacrylate, 2-phenoxyethyl acrylate, trimethacrylic acid esters, 3-(trimethoxysilyl)propyl methacrylate, styrene, butadiene, isoprene, farnesene, ethylene, isobutylene, and vinyl acetate are more preferred, and methyl methacrylate, ethyl acrylate, n-butyl acrylate, t-butyl acrylate, allyl methacrylate, 2-phenoxyethyl acrylate, trimethacrylic acid esters (preferably trimethylolpropane tri(meth)acrylate), 3-(trimethoxysilyl)propyl methacrylate, styrene, butadiene, ethylene, and vinyl acetate are even more preferred. As the monomer (b1), from the viewpoint of improving the oil resistance at the folded portion of the package, the embodiment (i) in which n-butyl acrylate is used alone is also preferred, the embodiment (ii) in which n-butyl acrylate, allyl methacrylate, and trimethylolpropane tri(meth)acrylate are used in combination is also preferred, the embodiment (iii) in which n-butyl acrylate, methyl methacrylate, and 3-(trimethoxysilyl)propyl methacrylate are used in combination is also preferred, the embodiment (iv) in which n-butyl acrylate and methyl methacrylate are used in combination is also preferred, and the embodiment (v) in which n-butyl acrylate and 3-(trimethoxysilyl)propyl methacrylate are used in combination is also preferred. In addition, as the monomer (b1), the embodiment (vi) in which an aromatic vinyl compound and a conjugated diene compound are used in combination is also preferred, the embodiment (vii) in which an aromatic vinyl compound and a (meth)acrylic acid ester are used in combination is also preferred, and the embodiment (viii) in which an aliphatic vinyl compound and vinyl acetate are used in combination is also preferred. Here, when the monomer (b1) is a (meth)acrylic acid ester, the polymer particles (B) are referred to as (meth)acrylic acid ester-based polymer particles, and particularly when there is one type of (meth)acrylic acid ester, the polymer particles (B) are referred to as (meth)acrylic acid ester-based homopolymer particles.

[0032] From the viewpoint of improving the oil resistance of the flat surface of the package and the folded portion, particularly from the viewpoint of improving the oil resistance of the folded portion of the package, the polymer particles (B) are preferably (meth)acrylic acid ester-based polymer particles [including aromatic vinyl compound-(meth)acrylic acid ester copolymer particles], and are also preferably (meth)acrylic acid ester-based homopolymer particles. From the viewpoint of improving the oil resistance of the flat surface of the package and the folded portion, the polymer particles (B) are preferably at least one selected from the group consisting of aromatic vinyl compound-conjugated diene compound copolymer particles and vinyl acetate polymer particles (more preferably aliphatic vinyl compound-vinyl acetate copolymer particles).

[0033] From the viewpoint of improving the oil resistance at the folded part of the package, the polymer particles (B) are preferably single-layer polymer particles. The polymer particles (B) may contain a dispersant used during production, and more specifically, the polymer particles (B) may be at least partially or entirely coated with the dispersant. In addition, when the polymer particles (B) are single-layer, they are considered to be single-layer even if they contain a dispersant as described above. As the dispersant, as described later, from the viewpoint of oil resistance, particularly from the viewpoint of the effect of improving oil resistance at the folded portion of the package and from the viewpoint of emulsion dispersibility, it is preferable that the dispersant contains an ionic group, and the ionic group is preferably at least one selected from the group consisting of anionic groups and groups consisting of salts of anionic groups, and therefore the dispersant is more preferably an anionic surfactant. Examples of the anionic group include a sulfonic acid group and a carboxyl group. Examples of the salt include a sodium salt. In particular, when the PVA-based polymer (A) is an ethylene-modified PVA, if the dispersant contains an ionic group, an oil-resistant film in which aggregation of the polymer particles (B) is effectively suppressed can be formed, which tends to lead to improved oil resistance, particularly in the folded portions of the package.

[0034] (Content of polymer particles (B)) The content of the polymer particles (B) is 1 part by mass or more and less than 150 parts by mass per 100 parts by mass of the PVA polymer (A) from the viewpoint of improving the oil resistance at the folded part of the package. From the same viewpoint, the content of the polymer particles (B) is preferably 1 part by mass or more and less than 100 parts by mass per 100 parts by mass of the PVA polymer (A), more preferably 1 to 50 parts by mass, further preferably 2 to 50 parts by mass, particularly preferably 3 to 40 parts by mass, and most preferably 20 to 35 parts by mass.

[0035] (phase separation structure) The oil-resistant film of the present invention tends to have a phase-separated structure of a sea-island structure. Specifically, the PVA polymer (A) constitutes the sea phase, and the polymer particles (B) constitute the island phase. It is presumed that the phase-separated structure is one of the factors that improve the oil resistance of the flat part of the package and further the oil resistance of the folded part.

[0036] <Method for producing polymer particles (B)> The polymer particles (B) may be commercially available or may be prepared by production. The method for producing the polymer particles (B) is not particularly limited, and for example, they can be produced by utilizing an emulsion polymerization method. Examples of the monomer to be subjected to the polymerization reaction include the above-mentioned ethylenically unsaturated monomer (b1). The emulsion polymerization method can be carried out, for example, by heating water containing a dispersant with stirring, and adding a polymerization initiator and a monomer.

[0037] (Dispersant) The dispersant is not particularly limited, but examples thereof include anionic surfactants such as sodium alkylbenzene sulfonate, sodium lauryl sulfate, polyoxyethylene lauryl ether acetate, sodium polyoxyethylene lauryl ether acetate, sodium polyoxyethylene lauryl ether sulfate, sodium polyoxyalkylene lauryl ether sulfate, sodium di-2-ethylhexyl sulfosuccinate, sodium higher fatty acid, and rosin-based soap; nonionic surfactants such as polyoxyethylene alkyl ether and nonylphenol ethoxylate; cationic surfactants such as distearyl dimethylammonium chloride and benzalkonium chloride; and amphoteric surfactants such as cocamidopropyl betaine and cocamidopropyl hydroxysultaine. It is also possible to use polymer surfactants such as PVA polymers, acid-modified polyolefins, β-naphthalenesulfonic acid formalin condensate salts, and (meth)ethyl acrylate copolymers as dispersants. As the PVA polymer, the PVA polymer (A) can be used, and from the viewpoints of polymerization stability and production costs, unmodified PVA is particularly preferably used. In the present invention, from the viewpoint of improving oil resistance, particularly oil resistance at the folded portion of the package, the dispersant is preferably a dispersant containing an ionic group, and the ionic group is preferably an anionic group or a group consisting of a salt thereof, and representative examples thereof include the anionic surfactants mentioned above. The dispersants may be used alone or in combination of two or more. The amount of the dispersant used is preferably from 0.01 to 40% by mass, more preferably from 0.05 to 30% by mass, based on the dispersion medium.

[0038] (Polymerization initiator) In the emulsion polymerization method, it is preferable to use a radical polymerization initiator as the polymerization initiator. Examples of the radical polymerization initiator include persulfate-based polymerization initiators, peroxide-based polymerization initiators, water-soluble azo-based polymerization initiators, and oil-soluble azo-based polymerization initiators. Redox-based polymerization initiators may also be used as the radical polymerization initiator. Among these, persulfate-based polymerization initiators and peroxide-based polymerization initiators are preferred. Examples of the persulfate-based polymerization initiators include potassium persulfate, sodium persulfate, and ammonium persulfate. Examples of the peroxide-based polymerization initiators include hydrogen peroxide, t-butyl peroxide, and methyl ethyl ketone peroxide. The polymerization initiator may be used alone or in combination of two or more kinds. When a water-soluble polymerization initiator is used, it may be added as an aqueous solution, but when a poorly water-soluble polymerization initiator is used, it is preferable to prepare a dispersion of the radical polymerization initiator in advance using water and a dispersant and add this. In this case, the dispersant used may be the same as or different from that used in the emulsion polymerization. The amount of the polymerization initiator used is preferably from 0.0001 to 1% by mass, more preferably from 0.001 to 0.5% by mass, and even more preferably from 0.001 to 0.1% by mass, based on the dispersion medium.

[0039] In the emulsion polymerization method, a redox polymerization initiator may be used from the viewpoint of productivity. As the redox polymerization initiator, a combination of an organic peroxide and a transition metal salt is preferably used. Examples of the organic peroxide include benzoyl peroxide, n-propyl peroxycarbonate, t-butyl peroxide, and methyl ethyl ketone peroxide. Examples of the transition metal salt to be used in combination with the organic peroxide include iron compounds such as iron sulfate(II), iron thiosulfate(II), iron carbonate(II), iron chloride(II), iron bromide(II), iron iodide(II), iron hydroxide(II), and iron oxide(II); copper compounds such as copper sulfate(I), copper thiosulfate(I), copper carbonate(I), copper chloride(I), copper bromide(I), copper iodide(I), copper hydroxide(I), and copper oxide(I), and hydrates thereof.

[0040] (reducing agent) A reducing agent may be used together with the radical polymerization initiator. Examples of such reducing agents include iron compounds such as ferrous chloride and ferrous sulfate; sodium salts such as sodium hydrogen sulfate, sodium bisulfite, sodium sulfite, sodium hydrogen sulfite, and sodium hydrogen carbonate; and organic reducing agents such as ascorbic acid, Rongalite, sodium diotinite, triethanolamine, glucose, fructose, glyceraldehyde, lactose, arabinose, and maltose. Of these, an iron compound and an organic reducing agent may be used in combination. The amount of the reducing agent used is preferably 0.0001 to 1% by mass, more preferably 0.001 to 0.5% by mass, and even more preferably 0.005 to 0.1% by mass, based on the dispersion medium.

[0041] (Crosslinking agent) In the emulsion polymerization method, a crosslinking agent may be added as necessary. The monomer (b1) may also be referred to as a crosslinking agent if it has a crosslinking ability. As the crosslinking agent, a bifunctional monomer having two polymerizable groups is preferably used, but it is also possible to use a polyfunctional monomer having three or more functional groups to increase the range of the crosslink density in the polymer and adjust the mechanical properties, etc. When a conjugated diene compound such as butadiene or isoprene is used as all or part of the monomer (b1), an unsaturated double bond remains after polymerization, and this can be used as a crosslinking portion. Examples of the crosslinking agent include allyl acrylate, allyl methacrylate, ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, bisphenol A diglycidyl ether with both ends having (meth)acrylic acid adduct, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, polyester di(meth)acrylate, tris(2-hydroxyethyl)ether, tert-butyl ... tris(2-(2,3-dihydroxypropoxy)ethyl)isocyanurate tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, diol di(meth)acrylate which is an adduct of bisphenol A with ethylene oxide or propylene oxide, diol di(meth)acrylate which is an adduct of hydrogenated bisphenol A with ethylene oxide or propylene oxide, trimethylolpropane tri(meth)acrylate, trimethylolpropane trioxyethyl (meth)acrylate, etc. Among these, allyl methacrylate and trimethylolpropane trimethacrylate are preferred. The crosslinking agent may be used alone or in combination of two or more kinds.

[0042] (Grafting Agent) In the emulsion polymerization method, a grafting agent may be added as necessary. The monomer (b1) may also be called a grafting agent if it has a grafting ability. Examples of the grafting agent include maleic acid, maleic anhydride, metal salts of maleic acid monoethyl ester, fumaric acid, metal salts of fumaric acid monoethyl ester, itaconic acid, vinylbenzoic acid, vinylphthalic acid, methacrylic acid, 3-(trimethoxysilyl)propyl methacrylate; monoesters or diesters of maleic acid, fumaric acid or itaconic acid, and the like. Examples of the monoesters and diesters include methyl monoesters, methyl diesters, propyl monoesters, propyl diesters, isopropyl monoesters, isopropyl diesters, butyl monoesters, butyl diesters, isobutyl monoesters, isobutyl diesters, hexyl monoesters, hexyl diesters, cyclohexyl monoesters, cyclohexyl diesters, octyl monoesters, octyl diesters, 2-ethylhexyl monoesters, 2-ethylhexyl diesters, decyl monoesters, decyl diesters, stearyl monoesters, stearyl diesters, methoxyethyl monoesters, methoxyethyl diesters, ethoxyethyl monoesters, ethoxyethyl diesters, hydroxy monoesters, hydroxy diesters, ethyl monoesters, and ethyl diesters. Of the above, the grafting agent is preferably 3-(trimethoxysilyl)propyl methacrylate.

[0043] (Metal ion chelating agent) In the emulsion polymerization method, a metal ion chelating agent may be added as necessary, specifically, disodium dihydrogen ethylenediaminetetraacetate and the like.

[0044] (Thickening inhibitor) In the emulsion polymerization method, an electrolyte may be added as a thickening inhibitor to the emulsion polymerization system, if necessary. Specific examples of the electrolyte include sodium chloride, sodium sulfate, and trisodium phosphate.

[0045] When a dispersant and a thickening inhibitor are used in combination, the amount of the thickening inhibitor used is not particularly limited, but from the viewpoint of the stability of micelles in the dispersion, it is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less relative to the dispersant. When the reducing agent, metal ion chelating agent and electrolyte are used, they may be added during the polymerization reaction, but it is preferable to add them to water from the beginning of the emulsion polymerization.

[0046] (Chain transfer agent) In the emulsion polymerization method, a chain transfer agent may be added as necessary. In particular, in the present invention, the degree of polymerization can be adjusted by adding a chain transfer agent. Examples of the chain transfer agent include hydrocarbon mercaptans such as n-octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, hexadecyl mercaptan, and n-octadecyl mercaptan; thiols such as mercaptoacetic acid, 2-ethylhexyl mercaptoacetate, 3-methoxybutyl mercaptoacetate, β-mercaptopropionic acid, methyl β-mercaptopropionate, 2-ethylhexyl β-mercaptopropionate, 3-methoxybutyl β-mercaptopropionate, 2-mercaptoethanol, and 3-mercapto-1,2-propanediol (excluding the above-mentioned hydrocarbon mercaptans); and hydrocarbon compounds with a large chain transfer constant such as α-methylstyrene dimer. Among these, hydrocarbon mercaptans are preferred, and n-dodecyl mercaptan and t-dodecyl mercaptan are more preferred. The chain transfer agent may be used alone or in combination of two or more kinds. When a chain transfer agent is used, its amount is not particularly limited, but is preferably 0.01 to 10 mass %, more preferably 0.1 to 2 mass %, based on the amount of the monomer (b1) used in producing the polymer particles (B).

[0047] (dispersion medium) The dispersion medium is preferably an aqueous medium mainly composed of water. The aqueous medium mainly composed of water may contain a water-soluble organic solvent (alcohols, ketones, etc.) that is soluble in water at any ratio. Here, "aqueous medium mainly composed of water" refers to a dispersion medium containing 50% by mass or more of water. From the viewpoint of production cost and environmental load, the dispersion medium is preferably an aqueous medium containing 90% by mass or more of water, and more preferably water. From the viewpoint of the viscosity and stability of the emulsion, the amount of the dispersion medium used in the emulsion polymerization method is preferably 50 to 2,000 parts by mass, more preferably 80 to 1,500 parts by mass, and even more preferably 100 to 1,200 parts by mass, relative to 100 parts by mass of the total amount of the monomer (b1) used in the production of the polymer particles (B).

[0048] (Anti-aging agent) In the present invention, from the viewpoint of suppressing deterioration of the polymer particles (B), an antioxidant may be added to the dispersion after emulsion polymerization, or to the polymer particles (B) after recovery or purification. From the viewpoint of suppressing deterioration in the recovery or purification of the polymer particles (B) after the polymerization reaction, the antioxidant may be added to the dispersion after emulsion polymerization, and then the polymer particles (B) may be subjected to recovery or purification.

[0049] As the antioxidant, a commonly used material can be used. Specific examples of the anti-aging agent include phenolic compounds such as hydroquinone, hydroquinone monomethyl ether, 2,5-di-t-butylphenol, 2,6-di(t-butyl)-4-methylphenol, mono(or di, or tri)(α-methylbenzyl)phenol; bisphenolic compounds such as 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 4,4'-butylidenebis(3-methyl-6-t-butylphenol), 4,4'-thiobis(3-methyl-6-t-butylphenol); benzimidazole compounds such as 2-mercaptobenzimidazole, 2-mercaptomethylbenzimidazole; amine-ketone compounds such as 6-ethoxy-1,2-dihydro-2,2,4-trimethylquinoline, the reaction product of diphenylamine and acetone, 2,2,4-trimethyl-1,2-dihydroquinoline polymer; aromatic secondary amine compounds such as N-phenyl-1-naphthylamine, alkylated diphenylamine, octylated diphenylamine, 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, p-(p-toluenesulfonylamide)diphenylamine, N,N'-diphenyl-p-phenylenediamine; thiourea compounds such as 1,3-bis(dimethylaminopropyl)-2-thiourea, tributylthiourea, etc. can be used. The anti-aging agent may be used alone or in combination of two or more.

[0050] (Polymerization temperature) The polymerization temperature is usually preferably 0 to 110 °C, more preferably 20 to 100 °C, and even more preferably 60 to 100 °C from the viewpoint of increasing the polymerization rate.

[0051] <Other components other than the PVA-based polymer (A) and the polymer particles (B)> The oil-resistant film of the present invention may contain other components other than the PVA-based polymer (A) and the polymer particles (B) as long as the effects of the present invention are not impaired. Examples of other components include a polymer (C) not applicable to the PVA-based polymer (A) and the polymer particles (B), and an additive (D), etc. Examples of the polymer (C) include thermoplastic resins and thermoplastic elastomers, and more specifically, examples thereof include ionomers, polyester resins, polystyrene resins, polyamide resins, polyolefin resins, polyvinyl chloride resins, polycarbonate resins, acrylic resins, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, ethylene-methacrylic acid copolymers, ethylene-methacrylic acid ester copolymers, ethylene-vinyl acetate copolymers, polyvinylidene chloride, vinyl ester resins, polyester elastomers, polyurethane elastomers, chlorinated polyolefins, etc. However, all of these are limited to those that do not fall under the PVA polymer (A) and the polymer particles (B). Examples of the additive (D) include a plasticizer, an oxygen absorber, a heat stabilizer, a light stabilizer, an ultraviolet absorber, a colorant, an antistatic agent, a surfactant, an antibacterial agent, an antiblocking agent, a filler, an antiseptic, etc. The additive (D) may be added separately from the PVA polymer (A) and the polymer particles (B) and thereby contained in the oil-resistant film, or may be used during the production of the PVA polymer (A) or the polymer particles (B) and thus contained in the oil-resistant film. When the oil-resistant film of the present invention contains the other components, it is preferable not to impair the effects of the present invention, and the content (here, excluding the content of additives used in producing the PVA polymer (A) or the polymer particles (B)) is preferably 50 mass% or less, more preferably 30 mass% or less, further preferably 10 mass% or less, and particularly preferably 5 mass% or less. There is no particular restriction on the lower limit of the content, but it may be, for example, 1 mass% or 3 mass%.

[0052] (Method for preparing emulsion containing PVA polymer (A) and polymer particles (B) containing a polymer having a Tg of 40° C. or less) An emulsion is obtained by dispersing a dispersion containing the polymer particles (B) in an aqueous solution of the PVA polymer (A). At this time, the other components may be mixed together in a dispersion state as necessary to prepare the emulsion. The solid content in the emulsion is preferably 1 to 60 mass%, more preferably 2 to 30 mass%, and further preferably 3 to 15 mass%, where "solid content" in the emulsion means the total mass of the components constituting the emulsion, excluding the dispersion medium.

[0053] <Method of manufacturing oil-resistant film and oil-resistant substrate> The method for producing the oil-resistant film of the present invention is not particularly limited, but an emulsion obtained by dispersing a dispersion containing polymer particles (B) in an aqueous solution of a PVA polymer (A) can be applied to a substrate using a coater or the like as necessary, and dried to form an oil-resistant film on the substrate, thereby producing an oil-resistant substrate [coating method]. Alternatively, an oil-resistant substrate having an oil-resistant film can be produced by applying the emulsion to a support and drying it to form an oil-resistant film, which is then laminated on the substrate [lamination method]. The oil-resistant film of the present invention may be unstretched, uniaxially stretched, or biaxially stretched, but from the viewpoint of oil resistance in the planar portion and folded portion of the packaging body, it is preferable that it is unstretched. The oil-resistant film may be provided only where necessary, that is, where oil resistance is to be imparted, and does not necessarily have to be provided on the entire surface of the substrate. For example, the substrate may have or may not have an oil-resistant film on a portion that does not come into contact with the contents such as food (e.g., the outer surface of the package and a part of the inner surface that does not come into contact with the contents).

[0054] The drying conditions in the coating method and lamination method are not particularly limited, but drying is preferably performed for 1 to 10 minutes at 60 to 140° C. using hot air, infrared rays, a heating cylinder, or a combination of these, and more preferably for 3 to 8 minutes at 80 to 120° C. The coating machine is not particularly limited, but examples thereof include devices such as a size press, a shim sizer, a gate roll coater, a bar coater, and a curtain coater. The oil-resistant substrate after drying can be further improved in oil resistance and water resistance by conditioning the moisture and performing a calendar treatment. The calendar treatment conditions are not particularly limited, but the roll temperature can be from room temperature (25° C.) to 100° C., and the roll linear pressure can be from 20 to 300 kg / cm.

[0055] In the above coating method, the coating amount of the oil-resistant film after drying is not particularly limited, and is preferably 0.1 to 50 g / m 2 and may be 0.5 to 30 g / m 2 and may be 1.0 to 15 g / m 2 The thickness may be 0.1 to 15 g / m 2 It is preferable that the thickness is 0.5 to 10 g / m 2 More preferably, the thickness is 1.0 to 8.0 g / m 2 More preferably, the thickness is 2.0 to 8.0 g / m 2 More preferably, the thickness is 2.5 to 6.5 g / m 2 It is particularly preferable that the thickness is 3.5 to 6.0 g / m 2 Most preferably, it is 0.1 g / m 2 If the coating amount of the oil-resistant film is 50 g / m or more, the oil resistance of the flat surface of the package is excellent, and the oil resistance of the folded portion of the package also tends to be improved. 2 If the thickness is less than 50 g / m, the moisture permeability required for food packaging tends to be excellent. 2 Even if the above is the case, the package is extremely useful industrially in that the flat surface and folded portions of the package have excellent oil resistance.

[0056] In the lamination method, the thickness of the oil-resistant film is not particularly limited, and may be 0.1 to 50 μm, 0.5 to 30 μm, 1.0 to 15 μm, or 5.5 to 7.5 μm. In addition, 0.1 to 15 μm is preferable, 0.5 to 10 μm is more preferable, 1.0 to 8.0 μm is even more preferable, 3.5 to 8.0 μm is particularly preferable, and 4.5 to 5.5 μm is most preferable. If the thickness of the oil-resistant film is 0.1 μm or more, the oil resistance of the flat surface of the package is excellent, and the oil resistance of the folded part of the package also tends to be improved. Even if the thickness of the oil-resistant film is 50 μm or less, it is industrially very useful in that the oil resistance of the flat surface and folded part of the package is excellent. The above thickness can be considered as the thickness of the oil-resistant film of the present invention. That is, the thickness of the oil-resistant film of the present invention may be 0.1 to 50 μm, 0.5 to 30 μm, 1.0 to 15 μm, 3.5 to 8 μm, or 4.5 to 5.5 μm, and is preferably within any of these ranges. However, a part of the oil-resistant film may penetrate into the substrate, and in that case, the thickness of the oil-resistant film remaining on the substrate may be thinner than the above thickness.

[0057] [Oil-resistant base material and oil-resistant paper] As described above, the emulsion is applied to a substrate and dried to obtain an oil-resistant substrate having an oil-resistant film on the substrate. Examples of the substrate include paper, rubber, and nonwoven fabric. Examples of the paper that can be used include fine paper, medium-quality paper, lightly coated paper, coated paper, one-sided glossy paper, bleached or unbleached kraft paper (acidic paper or neutral paper), or paperboard or white paperboard used for applications such as corrugated board, building materials, white board, and chipboard. There is no particular restriction on the basis weight of the substrate, but in the case of wrapping paper, it is preferably 20 to 150 g / m 2 , more preferably 30 to 90 g / m 2 and more preferably 55 to 75 g / m 2 In the case of a molded container such as a box, the thickness is preferably 150 to 500 g / m 2 It is. In terms of performance, the performance of the folded portion can be improved not only in terms of oil resistance, but also in terms of solvent resistance, chemical resistance, and gas barrier properties such as oxygen barrier property and water vapor barrier property. An example of a case where the base material is rubber is a rubber glove. In rubber gloves, if oil or the like used during work penetrates into the inside of the rubber glove, the hands may be contaminated or roughened, and the oil-resistant film of the present invention can solve the above problems of rubber gloves. In the case of food packaging, the substrate is often paper, in which case grease-resistant paper having an oil-resistant film on the paper is obtained. EXAMPLES

[0058] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these. The ion-exchanged water used in each example had an electrical conductivity of 0.08×10 -4 The ion-exchanged water has a purity of less than S / m.

[0059] The analytical conditions and evaluation methods in each example are shown below. (1. Glass transition temperature (Tg)) The glass transition temperature (hereinafter sometimes abbreviated as Tg) of the polymer contained in the polymer particles was determined based on the value of each polymer component described in Polymer Handbook (John Wiley & Sons Inc.). In addition, when the polymer contained in the polymer particles is a multicomponent copolymer, or when a polymer component not described in Polymer Handbook (John Wiley & Sons Inc.) is used, the solid content is removed from the solution containing the obtained polymer particles and thoroughly dried, and then the Tg is determined by a differential scanning calorimeter according to the method described in JIS K6240 (2011). Equipment: Differential scanning calorimeter "DSC822" (Mettler Toledo Co., Ltd.) Measurement conditions: heating rate 10℃ / min

[0060] (2. Number Average Molecular Weight of Polymer Particles) The dispersion of polymer particles obtained in each example was dried up, and then the obtained solid content was dissolved in tetrahydrofuran (THF) to a solid content of 10 mg / mL. The insoluble matter was then filtered through a membrane filter (13JP020AN, manufactured by Toyo Roshi Kaisha, Ltd.). The solution was measured by gel permeation chromatography (GPC) under the following conditions, and the number average molecular weight was calculated in terms of standard polystyrene. Equipment: CO-8020, manufactured by Tosoh Corporation Eluent:THF Column: TSKguardcolumn H HR -H (46mmI.D.×4cm), 1 piece made by Tosoh Corporation, TSKgel GMH HR -M (7.8mmI.D.×30cm), 2 pieces of Tosoh Corporation, TSKgel G2000H HR (7.8mmI.D.×30cm), 1 Tosoh Corporation product, total of 4 connected in series Column temperature: 40℃ Detector: RI Flow rate: 1.0mL / min

[0061] (3. Average particle size of polymer particles) A mixture of 0.1 mL of the dispersion obtained in each example and 10 mL of ion-exchanged water was used to measure the particle size distribution of the particles on a volume basis using a dynamic light scattering measuring device (device name: SZ-100, manufactured by HORIBA, Ltd.), and the obtained median diameter was taken as the average particle size of the polymer particles.

[0062] (4.Dispersibility) In the examples and comparative examples, the emulsions obtained by mixing using a shaker were visually observed after standing at room temperature for 2 hours and evaluated according to the following evaluation criteria. A: No precipitation occurs and it has excellent dispersibility. B: Precipitation has occurred and dispersibility is poor.

[0063] (5. Oil resistance of flat surfaces) For the grease-resistant papers produced in the Examples and Comparative Examples, the coated surfaces were measured by the TAPPI UM-557 method (kit method), and the lowest value was taken as the oil resistance (KIT value) and was used as an index of oil resistance. In addition, since the oil resistance (KIT value) of most of the oil-resistant papers made of fluororesin currently available on the market is grade 5 or higher, and since grade 5 or higher is the oil resistance level that does not cause problems in general use, grade 5 or higher is preferable, and grade 7 or higher is preferable for applications requiring even higher oil resistance.

[0064] (6. Oil resistance of bent parts) For the grease-resistant paper produced in the examples or comparative examples, the evaluation sample was folded in half with the coated side facing inward, and a rubber roller (roll width 45 mm, roll diameter 92 mm, roll mass 2 kg, rubber hardness 80 Hs) was rolled back and forth once on the folded part to create a crease. The fold was then unfolded and returned to its original state, and the oil resistance (KIT value) of the fold was measured by the TAPPI UM-557 method (KIT method). Since the oil resistance that does not cause problems even in the folded part is grade 5 or higher, grade 5 or higher is preferable, and for applications requiring a higher oil resistance, grade 7 or higher is preferable, grade 8 or higher is more preferable, grade 10 or higher is even more preferable, and grade 11 or higher is particularly preferable.

[0065] [Production Example 1] (Production of ethylene-modified PVA-1; ethylene-vinyl alcohol copolymer) A pressurized reactor equipped with a stirrer, a nitrogen inlet, an ethylene inlet, and an initiator addition inlet was charged with 110.5 g of vinyl acetate and 39.1 g of methanol, and the temperature was raised to 60°C, after which the system was substituted with nitrogen by nitrogen bubbling for 30 minutes. Ethylene was then introduced so that the reactor pressure was 0.14 MPa. As a polymerization initiator, 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) [hereinafter sometimes referred to as "AMV"] was dissolved in methanol to prepare a 0.33 g / L solution, and nitrogen was substituted by bubbling with nitrogen gas. After adjusting the temperature inside the reactor to 60°C, 635.7 mL of the initiator solution was injected to start polymerization. During the polymerization, ethylene was introduced to maintain the reactor pressure at 0.61 MPa, and the polymerization temperature at 60° C. The polymerization was carried out by continuously adding AMV at 2.0 L / hr using the above initiator solution. After 5 hours, when the polymerization rate reached 35%, 2.22 g of sorbic acid was added and the polymerization was stopped by cooling. After opening the reaction vessel to remove ethylene, nitrogen gas was bubbled through. Next, unreacted vinyl acetate monomer was removed under reduced pressure to obtain a methanol solution of ethylene-modified polyvinyl acetate [hereinafter, polyvinyl acetate may be referred to as "PVAc".]. Methanol was further added to the obtained methanol solution of ethylene-modified PVAc, and 400 g of the methanol solution of ethylene-modified PVAc adjusted to a concentration of 25% by mass (100 g of ethylene-modified PVAc in the solution) was added with 93.0 g of an alkali solution (methanol solution containing 10% by mass of sodium hydroxide; molar ratio to vinyl acetate unit in ethylene-modified PVAc of 0.20) to perform a saponification reaction at 60 ° C. After the addition of the alkali, the gelled material was crushed in a crusher and the saponification reaction was performed for a total of 1 hour, after which 1,000 g of methyl acetate was added to neutralize the remaining alkali. After the completion of neutralization was confirmed using a phenolphthalein indicator, 1,000 g of methanol was added to the white solid ethylene-modified PVA obtained by filtration and left to stand at room temperature for 3 hours for washing. The above washing procedure was repeated three times, and the ethylene-modified PVA obtained by centrifugal deliquor was then left to dry in a dryer at 70°C for two days to obtain an ethylene-vinyl alcohol copolymer (referred to as ethylene-modified PVA-1) having an ethylene unit content of 6 mol%, a polymerization degree of 1,000, a saponification degree of 99.0 to 99.4 mol%, and a Tg of 70°C, as determined by the following measurement method. The degree of polymerization was measured by the method described in "3.7 Average degree of polymerization" of JIS K6726 (1994).

[0066] (Method of measuring ethylene unit content) Ethylene-modified PVAc, the precursor of ethylene-modified PVA-1 1More specifically, the ethylene-modified PVAc was purified by reprecipitation with a mixture of n-hexane and acetone three or more times, and then dried at 80°C for three days under reduced pressure to obtain ethylene-modified PVAc for analysis. 1 Measurement was performed using a H-NMR measurement device (500 MHz) at 80° C. The content of ethylene units was determined using the peak (4.7 to 5.2 ppm) derived from the main chain methine of the vinyl ester and the peak (0.8 to 1.6 ppm) derived from the main chain methylene of ethylene, vinyl ester, and the third component.

[0067] [Production Example 2] (Production of PVA-2; Unmodified PVA) A reaction vessel equipped with a stirrer, a nitrogen inlet, and an initiator addition port was charged with 0.59 kg of vinyl acetate and 1.0 kg of methanol, and the temperature was raised to 60°C, after which the system was purged with nitrogen by nitrogen bubbling for 30 minutes. Next, a 10% by mass solution of 2,2'-azobis(isobutyronitrile) (AIBN) was prepared as a polymerization initiator in methanol, and nitrogen was purged by bubbling with nitrogen gas. After adjusting the temperature inside the reaction vessel to 60°C, 10 mL of the initiator solution was poured in to start polymerization. After 3 hours, when the polymerization rate reached 50%, 0.1 g of 2,4-diphenyl-4-methyl-1-pentene was added, and the mixture was cooled to terminate the polymerization. Unreacted vinyl acetate monomer was removed to obtain a methanol solution of PVAc. Methanol was further added to the obtained methanol solution of PVAc, and 7.44 g of an alkali solution (methanol solution containing 10% by mass of sodium hydroxide; molar ratio to vinyl acetate units in PVAc of 0.01) was added to 400 g of the methanol solution of PVAc adjusted to a concentration of 40% by mass (160 g of PVAc in the solution), and a saponification reaction was carried out at 40°C. After the addition of the alkali, the gelled material was crushed in a crusher, and the saponification reaction was carried out for a total of 1 hour, after which 1,000 g of methyl acetate was added to neutralize the remaining alkali. After confirming the completion of neutralization using a phenolphthalein indicator, 1,000 g of methanol was added to the white solid PVA obtained by filtration, and the mixture was left to stand at room temperature for 3 hours for washing. The above washing procedure was repeated three times, and the PVA obtained by centrifugal deliquor was then left to dry in a dryer at 70°C for two days to obtain an unmodified PVA (referred to as PVA-2) with a degree of polymerization of 1,750 and a degree of saponification of 88.4 mol%.

[0068] [Production Example 3] (Production of Dispersant I) 3.73 parts by mass of "KAO AKIPO (Akipo is a registered trademark) RLM100" (main ingredient: polyoxyethylene lauryl ether acetate, manufactured by Kao Corporation) and 41.7 parts by mass of ion-exchanged water were placed in a container, and 0.44 parts by mass of sodium carbonate was added while stirring. The mixture was thoroughly stirred at room temperature to obtain Dispersant I.

[0069] [Production Example 4] (Production of Dispersant II) Dispersant II was obtained by carrying out the same operations as in Production Example 3, except that the amount of "KAO AKIPO (Akipo is a registered trademark) RLM100" was changed to 50 parts by mass, the amount of ion-exchanged water was changed to 100 parts by mass, and sodium carbonate was changed to sodium hydroxide in an amount of 5.5 parts by mass.

[0070] [Production Example 5] (Production of Dispersion 1 Containing Polymer Particles 1) Dispersant I obtained in Production Example 3 was placed in a reaction vessel equipped with a reflux condenser, and then 255 parts by mass of ion-exchanged water was added, and the contents were deoxidized by bubbling nitrogen gas at room temperature for 30 minutes, and then the temperature was raised to 70° C. Thereafter, 3.01 parts by mass of an aqueous potassium persulfate solution that had been previously prepared in a separate vessel by dissolving 0.1 part by mass of potassium persulfate (polymerization initiator) in 30 parts by mass of ion-exchanged water and deoxidized in the same manner as above was added. Next, a solution (deoxygenated) of n-butyl acrylate (monomer (b1)) and t-dodecyl mercaptan (chain transfer agent) was continuously added over 85 minutes using a feed pump. After the addition was completed, the mixture was held for 1 hour, and then heated to 90°C for 2 hours to obtain dispersion liquid 1 containing polymer particles 1. The amounts of each reagent used are summarized in Table 1. Furthermore, the number average molecular weight, average particle size and Tg of the polymer particles 1 were determined according to the above-mentioned methods. The results are shown in Table 1.

[0071] [Production Examples 6 to 14] (Production of Dispersions 2 to 10 Containing Polymer Particles 2 to 10) The same procedure as in Production Example 5 was carried out except that the types and amounts of each component were changed as shown in Table 1, to obtain dispersions 2 to 10 containing polymer particles 2 to 10, respectively. The number average molecular weight, average particle size and Tg of the obtained polymer particles 2 to 10 are shown in Table 1.

[0072] [Production Example 15] (Production of Dispersion 11 Containing Polymer Particles 11) 0.1714 parts by mass of Pelex OT-P (ingredient; sodium di-2-ethylhexyl sulfosuccinate, manufactured by Kao Corporation) was placed in a reaction vessel equipped with a reflux condenser, after which 174 parts by mass of ion-exchanged water was added, and the contents were deoxidized by bubbling nitrogen gas at room temperature for 30 minutes, and then heated to 70° C. Thereafter, 0.303 parts by mass of an aqueous potassium persulfate solution (deoxidized) that had been previously prepared in a separate vessel by dissolving 0.1 parts by mass of potassium persulfate (polymerization initiator) in 10 parts by mass of ion-exchanged water was added thereto. Next, 6.126 parts by mass of a solution (deoxygenated) obtained by mixing 120 parts by mass of n-butyl acrylate (monomer (b1)), 0.8 parts by mass of n-dodecyl mercaptan (chain transfer agent), and 1.715 parts by mass of Pelex OT-P that had been subjected to the above treatment was added continuously over 30 minutes using a feed pump, and the mixture was held for 30 minutes after the addition was completed. 5.76 parts by mass of the aqueous potassium persulfate solution prepared above was added thereto, and further, 116.389 parts by mass of a mixed solution (deoxygenated) of n-butyl acrylate and n-dodecyl mercaptan was added continuously over 4 hours using a feed pump, and the mixture was held for 1 hour after the addition was completed. The mixture was further heated to 90° C. and heated for 2 hours to obtain a dispersion 11 containing polymer particles 11. Table 1 shows the amount of each reagent used, and the number average molecular weight, average particle size and Tg of the resulting polymer particles 11.

[0073] [Production Example 16] (Production of Dispersion 12 Containing Polymer Particles 12) (Process 1) 395 parts by mass of ion-exchanged water and 30 parts by mass of PVA205 (product name, manufactured by Kuraray Co., Ltd., polyvinyl alcohol-based polymer, dispersant) were added to a reaction vessel equipped with a reflux tube, and the contents were deoxidized by bubbling nitrogen gas for 30 minutes while stirring. The contents were heated to 70°C to dissolve the PVA-based resin, thereby obtaining an aqueous solution of the PVA-based resin. An aqueous solution in which 0.05 parts by mass of potassium persulfate (polymerization initiator) was dissolved in 5 parts by mass of ion-exchanged water and 10 parts by mass of methyl methacrylate (monomer (b1)) were added to the aqueous solution all at once. (Process 2) Once it was confirmed that the conversion rate of the monomer (b1) added in the step 1 exceeded 99% by mass, a monomer mixture (deoxygenated) consisting of 30 parts by mass of n-butyl acrylate (monomer (b1)) and 0.3 parts by mass of 3-(trimethoxysilyl)propyl methacrylate (monomer (b1); grafting agent) was continuously added over 17 minutes to the dispersion obtained in the step 1. Once it was confirmed that the total monomer conversion rate exceeded 99% by mass, the polymerization tank was cooled to 25° C. to obtain a dispersion 12 containing core-shell type polymer particles 12. The number average molecular weight, average particle size and Tg of the obtained polymer particles 12 are shown in Table 1.

[0074] [Production Example 17] (Production of Dispersion 13 Containing Polymer Particles 13) A dispersion 13 containing core-shell type polymer particles 13 was obtained by carrying out the same operations as in Production Example 16, except that the methyl methacrylate (monomer (b1)) used in step 1 was changed to n-butyl acrylate (monomer (b1)). Table 1 shows the amount of each reagent used, and the number average molecular weight, average particle size and Tg of the resulting polymer particles 13.

[0075] [Production Example 18] (Production of Dispersion 14 Containing Polymer Particles 14) Dispersant II obtained in Production Example 4 was placed in a reaction vessel equipped with a reflux condenser, and then 192 parts by mass of ion-exchanged water was added, and the contents were deoxidized by bubbling nitrogen gas at room temperature for 30 minutes, and then heated to 70° C. Thereafter, 2.1 parts by mass of an aqueous potassium persulfate solution (deoxidized) that had been prepared in advance in a separate vessel by dissolving 0.1 part by mass of potassium persulfate (polymerization initiator) in 30 parts by mass of ion-exchanged water was added. A solution (deoxygenated) of 50 parts by mass of n-butyl acrylate (monomer (b1)) and 0.33 parts by mass of n-dodecyl mercaptan (chain transfer agent) was continuously added thereto using a feed pump over a period of 42 minutes, and the mixture was held for 1 hour after the addition was completed. Next, 50 parts by mass of methyl methacrylate (monomer (b1)) (deoxygenated) was continuously added using a feed pump over a period of 80 minutes, and the mixture was held for 2 hours after the addition was completed. The mixture was further heated to 90°C and heated for 2 hours to obtain a dispersion 14 containing polymer particles 14. Table 1 shows the amount of each reagent used, the number average molecular weight, average particle size and Tg of the resulting polymer particles 14.

[0076] [Production Example 19] (Production of Dispersion 15 Containing Polymer Particles 15) Dispersion 15 containing polymer particles 15 was obtained in the same manner as in Production Example 15, except that n-dodecyl mercaptan (chain transfer agent) was not used. The number average molecular weight, average particle size and Tg of the obtained polymer particles 15 are shown in Table 1.

[0077] [Production Example 20] (Production of Dispersion 16 Containing Polymer Particles 16) The same procedure as in Production Example 5 was carried out except that the components and amounts used were changed as shown in Table 1, to obtain a dispersion 16 containing polymer particles 16. The number average molecular weight, average particle size and Tg of the obtained polymer particles 16 are shown in Table 1.

[0078] [Table 1]

[0079] Here, each component listed in Table 1 will be explained below. (Dispersant) Dispersant I: Dispersant I prepared in Production Example 3, solid content 8.1% by mass Dispersant II: Dispersant II prepared in Production Example 4, solid content 32.2% by mass RLM100NV: "Kao Akipo (Akipo is a registered trademark) RLM100NV" (product name, manufactured by Kao Corporation), sodium polyoxyethylene lauryl ether acetate, solid content 24% by mass EMAL (registered trademark) 2FG: Trade name, manufactured by Kao Corporation, sodium lauryl sulfate LATEMURU (registered trademark) E-108MB: Trade name, manufactured by Kao Corporation, sodium polyoxyethylene polyoxypropylene lauryl ether sulfate, solid content 22% by mass Pelex (registered trademark) OT-P: Trade name, manufactured by Kao Corporation, sodium di-2-ethylhexyl sulfosuccinate, solid content 70% by mass PVA205: Kuraray Poval (registered trademark) PVA205, manufactured by Kuraray Co., Ltd., polymerization degree 500, saponification degree 88.2 mol% (Chain transfer agent) t-Dodecyl mercaptan: manufactured by Tokyo Chemical Industry Co., Ltd. n-Dodecyl mercaptan: manufactured by Tokyo Chemical Industry Co., Ltd. (Monomer (b1)) -n-Butyl acrylate: Nippon Shokubai Co., Ltd. Ethyl acrylate: Nippon Shokubai Co., Ltd. Allyl methacrylate: Tokyo Chemical Industry Co., Ltd. Methyl methacrylate: Kuraray Co., Ltd. 3-(Trimethoxysilyl)propyl methacrylate: Grafting agent, manufactured by Tokyo Chemical Industry Co., Ltd. Trimethylolpropane trimethacrylate: crosslinking agent, manufactured by Tokyo Chemical Industry Co., Ltd. (Polymerization initiator) Potassium persulfate: Wako Pure Chemical Industries, Ltd., radical polymerization initiator (dispersion medium) Ion-exchanged water: Electrical conductivity 0.08×10 -4 Ion-exchanged water below S / m

[0080] [Production Example 21] (Production of Ethylene-modified PVA Aqueous Solution 1) 604.5 parts by mass of ion-exchanged water was placed in a vessel equipped with a reflux condenser, and the temperature was raised to 90° C. while stirring at a rotation speed of 400 rpm using a stirrer. Next, 45.5 parts by mass of ethylene-modified PVA-1 obtained in Production Example 1 was added, and the mixture was stirred for 120 minutes, and then allowed to cool to room temperature, thereby obtaining an aqueous solution of ethylene-modified PVA 1.

[0081] [Production Example 22] (Production of PVA aqueous solution 2) A PVA aqueous solution 2 was obtained in the same manner as in Production Example 21, except that the ethylene-modified PVA-1 was changed to PVA-2.

[0082] [Example 1] Preparation of emulsion and production of oil-resistant film and oil-resistant paper (Preparation of Emulsion) The ethylene-modified PVA aqueous solution 1 prepared in Production Example 21 and the dispersion 1 prepared in Production Example 5 were placed in a container in the amounts shown in Table 2, and mixed at room temperature for 15 minutes at a rotation speed of 200 rpm using a shaker, and then degassed for 8 minutes using a planetary centrifugal mixer to obtain an emulsion. (Preparation of oil-resistant film and oil-resistant paper) A PET film was placed on a coating machine "K Control Coater" (manufactured by Matsuo Sangyo Co., Ltd.), and an A4 size paper was placed on top of it. On top of that, a sheet of OK Prince wood-free paper (manufactured by Oji Paper Co., Ltd., basis weight: 64 g / m2) was cut to a size of 15 cm x 29.7 cm and the mass was measured. 2 ) was then placed over the OK Prince wood-free paper. A cover PET film was then placed over the top 8 cm of the long side of the OK Prince wood-free paper and secured in place with a clip. A wire bar No. 30 was then set in the coating machine, and the emulsion prepared by the above method was poured onto the cover PET film. The wire bar was then moved at a speed of 1 m / min to coat the emulsion onto the OK Prince wood-free paper, and the mass of the coated OK Prince wood-free paper was measured and the amount of coating after drying was calculated. The results are shown in Table 2. 1.5 minutes after coating was completed, the coated OK Prince wood-free paper was placed in a hot air dryer and dried at 100°C for 5 minutes to obtain Grease-resistant Paper 1 having an oil-resistant film. The oil resistance of the obtained greaseproof paper 1 was evaluated according to the above-mentioned method. The results are shown in Table 2. A scanning electron microscope (SEM) photograph of the cross section of the greaseproof paper 1 before folding is shown in Fig. 1, and a scanning electron microscope (SEM) photograph of the cross section of the greaseproof paper 1 after folding and then returning to its original state is shown in Fig. 2. In order to confirm the phase separation structure of the oil-resistant film of the oil-resistant paper 1, the solid content of the emulsion was adjusted to 4% by weight by adding water as necessary, and then a cast film was prepared and observed with a transmission electron microscope (TEM). The transmission electron microscope (TEM) photographs are shown in Figures 3 and 4. It was observed that the PVA-based polymer (A) was in the sea phase and the polymer particles (B) were in the island phase. From the TEM photograph, the particle size of the polymer particles (B) in the oil-resistant film can be measured, and the average particle size can be obtained by calculating the average value of the particle sizes of multiple particles (for example, any 20 particles) as necessary.

[0083] [Examples 2 to 28] Preparation of emulsions and production of oil-resistant films and oil-resistant paper Except for changing the PVA aqueous solution and dispersion used and their amounts, as well as the type and coating amount of the wire bar, as shown in Tables 2 to 4, the same operations as in Example 1 were carried out to prepare emulsions and produce oil-resistant papers 2 to 28 having oil-resistant films. The oil resistance of the obtained grease-resistant papers 2 to 28 was evaluated according to the above-mentioned method. The results are shown in Tables 2 to 4.

[0084] [Comparative Examples 1 to 4] Preparation of emulsions and production of oil-resistant films and oil-resistant paper Except for changing the PVA aqueous solution and dispersion used and their amounts, as well as the type and coating amount of the wire bar, as shown in Table 5, the same operations as in Example 1 were carried out to prepare emulsions and produce comparative oil-resistant papers 1 to 4 having oil-resistant films. The oil resistance of the obtained comparative greaseproof papers 1 to 4 was evaluated according to the above-mentioned method. The results are shown in Table 5. Moreover, a scanning electron microscope (SEM) image of the cross section of comparative greaseproof paper 1 before folding is shown in Fig. 5, and a scanning electron microscope (SEM) image of the cross section of comparative greaseproof paper 1 after folding and then returning to its original state is shown in Fig. 6.

[0085] [Comparative Example 5] Preparation of oil-resistant film and oil-resistant paper Except for changing the emulsion to AG-E060 (a fluorine-based oil-resistant processing agent manufactured by AGC Corporation) and changing the type of wire bar and the amount of coating as shown in Table 5, the same operations as in Example 1 were carried out to obtain comparative oil-resistant paper 5 having an oil-resistant film. The oil resistance of the obtained comparative greaseproof paper 5 was evaluated according to the above-mentioned method. The results are shown in Table 5.

[0086] [Table 2]

[0087] [Table 3]

[0088] [Table 4]

[0089] [Table 5]

[0090] Here, each component shown in Tables 2 to 5 will be explained below. (PVA aqueous solution) Ethylene-modified PVA aqueous solution 1: Ethylene-modified PVA aqueous solution 1 prepared in Production Example 21 PVA aqueous solution 2: PVA aqueous solution 2 prepared in Example 22 (dispersion) Dispersions 1 to 16: Dispersions 1 to 16 prepared in Production Examples 5 to 20, respectively A6160 aqueous dispersion: styrene-butadiene copolymer particles (Tg: 33°C), manufactured by Asahi Kasei Corporation, used as a 48.3 mass% aqueous dispersion. A7141 aqueous dispersion: styrene-butadiene copolymer particles (Tg: -61°C), manufactured by Asahi Kasei Corporation, used as a 50.2 mass% aqueous dispersion. Harvil (registered trademark) C-3: styrene-acrylic acid ester copolymer particles (Tg: -9°C, 19°C), manufactured by Daiichi Paint Manufacturing Co., Ltd., 56.0 mass% aqueous dispersion. Harvil (registered trademark) B-7: (meth)acrylic acid ester polymer particles (Tg: -6°C, 16°C), manufactured by Daiichi Paint Manufacturing Co., Ltd., 42.0 mass% aqueous dispersion. OM-4200NT: Ethylene-vinyl acetate copolymer particles (Tg: 5°C), manufactured by Kuraray Co., Ltd., 55% by mass aqueous dispersion. AG-E060: Fluorine-based oil-resistant processing agent, manufactured by AGC Corporation, used as an 8.6% by mass aqueous dispersion.

[0091] From Tables 2 to 5, it can be seen that the grease-resistant paper produced in the examples has excellent oil resistance not only in the flat part but also in the folded part, compared to the grease-resistant paper produced in the comparative example. As shown in Figures 1 and 2, the folded part of the grease-resistant film of the grease-resistant paper produced in the examples is in good condition even after folding, and there are no cracks, so it is presumed that the folded part has excellent oil resistance. In addition, in the grease-resistant paper produced in the examples, the folded part may have better oil resistance than the flat part, but this is presumed to be because the oil-resistant film does not crack even when folded, so that the oil-resistant film shrinks and becomes thicker when the folded part is returned to the flat surface. On the other hand, from Table 5, the grease-resistant papers of Comparative Examples 1 and 2, which did not use polymer particles, the grease-resistant papers of Comparative Example 3, which used an emulsion containing polymer particles not containing a polymer with a Tg of 40° C. or less, and the grease-resistant papers of Comparative Example 5, which used a fluorine-based resin, had good oil resistance in the flat part, but poor oil resistance in the folded part. This is presumably because, as shown in FIG. 5 and FIG. 6, the grease-resistant papers produced in Comparative Examples 1 to 3 and 5 had cracks in the folded parts of the oil-resistant film after folding, which made it easier for oil to penetrate through them. In addition, the grease-resistant paper of Comparative Example 4, in which the content of polymer particles is 150 parts by mass or more relative to 100 parts by mass of the polyvinyl alcohol-based polymer (A), has low oil resistance in both the flat part and the folded part. This is presumably because the grease-resistant paper produced in Comparative Example 4 contains a large amount of polymer particles in the oil-resistant film, which has a higher affinity for oil than the polyvinyl alcohol-based polymer (A), making it easier for oil to penetrate the oil-resistant film. [Industrial Applicability]

[0092] The oil-resistant film of the present invention exhibits excellent oil resistance not only on the flat surface of the package but also on the folded portion, and is therefore useful in a wide range of applications, such as packages used for serving oily foods such as french fries and fried chicken, packaging sheets for wrapping butter, and packages such as cooking paper used for baking bread or cake, as well as rubber gloves.

Claims

1. An oil-resistant film comprising: a polyvinyl alcohol-based polymer (A) and polymer particles (B) containing a polymer having a glass transition temperature of -65 to -35°C, the polymer particles (B) being (meth)acrylic acid ester-based polymer particles or aromatic vinyl compound-conjugated diene compound copolymer particles, the polymer particles (B) containing a dispersant containing an ionic group, the ionic group being at least one type selected from the group consisting of anionic groups and groups consisting of salts of anionic groups, the content of the polymer particles (B) being 1 part by mass or more and less than 100 parts by mass per 100 parts by mass of the polyvinyl alcohol-based polymer (A), and the film does not contain a polymer having a polyalkylene ether unit.

2. 2. The oil-resistant film according to claim 1, wherein the polymer particles (B) have a number average molecular weight of 5,000 or more.

3. 3. The oil-resistant film according to claim 1, wherein the polymer particles (B) have an average particle size of 10 to 500 nm.

4. The oil-resistant film according to any one of claims 1 to 3, wherein the polymer particles (B) are (meth)acrylic acid ester-based polymer particles.

5. The oil-resistant film according to any one of claims 1 to 4, wherein the polymer particles (B) are (meth)acrylic acid ester-based homopolymer particles.

6. The oil-resistant film according to any one of claims 1 to 3, wherein the polymer particles (B) are aromatic vinyl compound-conjugated diene compound copolymer particles.

7. The oil-resistant film according to any one of claims 1 to 6, wherein the polyvinyl alcohol-based polymer (A) is an unmodified polyvinyl alcohol or a modified polyvinyl alcohol.

8. The oil-resistant film according to any one of claims 1 to 7, wherein the polyvinyl alcohol-based polymer (A) is an ethylene-vinyl alcohol copolymer, and the content of ethylene units in the ethylene-vinyl alcohol copolymer is 0.5 to 19 mol% based on all structural units.

9. The oil-resistant film according to any one of claims 1 to 8, wherein the oil-resistant film has a phase-separated structure of a sea-island structure, in which the polyvinyl alcohol-based polymer (A) constitutes a sea phase, and the polymer particles (B) constitute an island phase.

10. The oil-resistant film according to any one of claims 1 to 9, having a thickness of 0.1 to 50 µm.

11. An oil-resistant substrate having an oil-resistant film according to any one of claims 1 to 10 on the substrate.

12. Grease-resistant paper having an oil-resistant film according to any one of claims 1 to 10 on the paper.

Citation Information

Patent Citations

  • Rubber enhancing polyvinylalcohol film composition

    JP1985248763A

  • Polyvinyl alcohol molding

    JP1997328581A

  • Agent and process for separating oil

    JP2000328048A

  • Oil adsorbent filter

    JP2004066054A

  • Oil-resistant paper

    JP2006183221A