Cobalt catalysts and their precursors

A cobalt catalyst precursor with cobalt oxide crystallites in titania support addresses the challenges of fixed bed Fischer-Tropsch processes by enhancing activity and selectivity, producing longer hydrocarbons efficiently.

JP7572956B2Active Publication Date: 2024-10-24JOHNSON MATTHEY DAVY TECHNOLOGIES LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021545381
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-14
Filing Date
2020-03-10
Publication Date
2024-10-24
Estimated Expiration
2040-03-10

AI Technical Summary

Technical Problem

Existing Fischer-Tropsch catalysts with small particle diameters face challenges in commercial-scale fixed bed processes due to high pressure drops and instability, necessitating improved catalysts for high activity and selectivity.

Method used

A cobalt catalyst precursor is developed with cobalt oxide crystallites within the pores of a titania support, having specific size and pore diameter ratios, prepared by impregnating spherical titania with cobalt nitrate and calcining, followed by reduction to form elemental cobalt, suitable for use in fixed bed reactors.

Benefits of technology

The catalyst exhibits high activity and selectivity for long-term use in fixed bed reactors, producing longer hydrocarbon chains with improved performance and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572956000001
    Figure 0007572956000001
Patent Text Reader

Abstract

A cobalt catalyst precursor comprising cobalt oxide crystallites disposed within pores of a titania support, the cobalt oxide crystallites having an average size determined by XRD in the range of 6 to 18 nm, the titania support being a spherical titania support having a particle size in the range of 100 to 1000 μm, and the catalyst precursor having a particle size in the range of 0.2 to 0.6 cm 3 A cobalt catalyst precursor is described, having a pore volume of 1000 s / g and an average pore diameter in the range of 30-60 nm, wherein the catalyst precursor has an average cobalt oxide crystallite size to average pore diameter ratio in the range of 0.1:1 to 0.6:1. The catalyst precursor may be reduced to provide a catalyst suitable for use in Fischer-Tropsch reactions.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cobalt catalyst precursor comprising cobalt oxide supported on titania particles, a method for producing such a precursor, and the use of such a precursor in the preparation of a fixed bed Fischer-Tropsch catalyst. [Background technology]

[0002] Fischer–Tropsch catalysts with nominal diameters less than about 1 mm offer the potential for high reaction rates and improved selectivity towards C5+ hydrocarbons, but their use in commercial scale fixed beds is usually made impractical by unacceptably high pressure drops and are therefore typically associated with use in suspension, such as in slurry bubble column reactors.

[0003] WO 2012 / 146903 A1 discloses a Fischer-Tropsch process using a fixed bed of small particle catalyst, the catalyst being arranged in a plurality of catalyst vessels placed within an externally cooled reactor tube. The catalyst particles may have a diameter of about 100 μm to about 1 mm.

[0004] Such processes offer the opportunity to produce an improved set of hydrocarbon products, but there is a need to improve the performance of small particle catalysts suitable for use in fixed-bed Fischer-Tropsch processes. Summary of the Invention [Problem to be solved by the invention]

[0005] Titania supported catalysts provide improved performance in the Fischer-Tropsch process. For example, WO 97 / 00231 discloses a catalyst for use in a process for the preparation of hydrocarbons comprising cobalt and manganese and / or vanadium supported on a carrier, the cobalt:(manganese and / or vanadium) atomic ratio being at least 12:1. In the examples, commercially available rutile titania particles of 30-80 mesh size were impregnated with a cobalt nitrate solution with or without manganese nitrate, dried at 120°C, and calcined at 400°C. U.S. Pat. No. 4,822,824 discloses catalysts useful for the preparation of higher hydrocarbons from synthesis gas, prepared by depositing cobalt and ruthenium on a refractory carrier such as titania, and oxidizing and reducing the catalytic metals to form a catalyst in which the cobalt and ruthenium are in intimate contact. However, these catalysts were tested in a laboratory scale test apparatus for a relatively short period of time. Therefore, there remains a need for small particle catalysts suitable for use in commercial-scale fixed-bed Fischer-Tropsch processes that exhibit high activity and selectivity and stable operation during long-term use.

[0006] Accordingly, the present invention provides a cobalt catalyst precursor comprising cobalt oxide crystallites disposed within the pores of a titania support, the cobalt oxide crystallites having an average size determined by XRD in the range of 6-18 nm, the titania support being a spherical titania support having a particle size in the range of 100-1000 μm, the catalyst precursor being a spherical titania support having a particle size in the range of 0.2-0.6 cm 3 / g and an average pore diameter in the range of 30 to 60 nm, the catalyst precursor having a ratio of average cobalt oxide crystallite size to average pore diameter in the range of 0.1:1 to 0.6:1.

[0007] The present invention further provides a method for preparing a catalyst precursor by impregnating a spherical titania support with cobalt nitrate, and drying and calcining the impregnated titania support, thereby forming cobalt oxide crystallites within the pores of the titania support.

[0008] The invention further provides a catalyst formed by reducing cobalt oxide crystallites in a catalyst precursor with a stream of reducing gas to form elemental cobalt crystallites. The reducing gas may be applied ex-situ prior to introducing the catalyst precursor into the Fischer-Tropsch process, in which case the catalyst may be encapsulated with wax or subjected to a passivation treatment prior to introduction into the Fischer-Tropsch process. Alternatively, the reducing gas may be applied in-situ after introducing the catalyst precursor into the Fischer-Tropsch reactor.

[0009] The present invention further provides a catalyst precursor or catalyst combination disposed within a catalyst carrier suitable for use in the reactor tubes of a Fischer-Tropsch reactor.

[0010] The present invention further provides a method of using the catalyst precursor or catalyst in a Fischer-Tropsch reactor to produce hydrocarbons from a synthesis gas comprising hydrogen and carbon monoxide.

[0011] The catalyst precursor comprises cobalt oxide crystallites. The cobalt oxide crystallites preferably consist essentially of Co3O4 with no detectable CoO or other cobalt oxides or hydroxides. The average particle size of the cobalt oxide crystallites ranges from 6 to 18 nanometers (nm), preferably 7 to 16 nm, and more preferably 8 to 12 nm. The average particle size is determined by X-ray diffraction (XRD). A particularly suitable method uses a Bruker D8 Advance XRD instrument at a CuKα wavelength of 1.5406 Å with a Lynxeye PSD detector. This detection system is useful because the operating settings can be adjusted to suppress the fluorescence generated by the presence of cobalt. Rietveld analysis and Scherrer line broadening are common methods of XRD crystallite size determination. Either method can be used, but Rietveld analysis is preferred.

[0012] The catalyst precursor comprises a spherical titania support. The term "spherical support" includes support shapes having a sphericity (ψ) of at least about 0.90, preferably at least about 0.95, and approximately spherical aggregates of titania powder. Spherical titania particles are sometimes referred to as "microspheres". The particle size of the titania support ranges from 100 to 1000 micrometers (μm), preferably from 300 to 800 μm. The volume median diameter D[v,0.5] of the titania support within this range is preferably from 300 to 500 μm, more preferably from 350 to 450 μm, most preferably from 350 to 425 μm, especially from 375 to 425 μm. The catalyst precursor has essentially the same particle size characteristics as the catalyst support. Thus, the catalyst precursor provides a highly active catalyst with acceptable pressure drop when used in commercial scale fixed beds, especially when used as a fixed bed in a catalyst carrier in a multi-tube Fischer-Tropsch reactor. The term volume median diameter D[v,0.5], sometimes referred to as D50 or D0.5, is defined by Dr Alan Rawle in the paper "Basic Principles of Particle Size Analysis" available from Malvern Instruments Ltd, Malvern, UK (www.malvern.co.uk) and is calculated from particle size analysis which may be conveniently achieved by laser diffraction, for example using a Malvern Mastersizer®.

[0013] Suitable spherical titania supports are commercially available. The spherical titania supports can be conveniently preformed from commercially available titania powders made by flame hydrolysis or flame pyrolysis of titania precursors such as titanium tetrachloride, if necessary. Commercially available titania powders typically have particle sizes less than 5 micrometers, so the spherical titania supports typically comprise agglomerates of titania powders. One or more binders, such as polymeric binders, may be present in the support to increase its strength, but this is not required. The agglomerates can be formed by any suitable forming technique that produces spheres, such as spray drying, granulation, spray granulation, drip casting, or spheronization.

[0014] The titania support is preferably low in elements that have been found to be poisons in cobalt-catalyzed Fischer-Tropsch reactions, such as sulfur and alkali metals. Thus, the sulfur content of the catalyst precursor is desirably <30 ppmw, and the alkali metal (e.g., Na or K) content of the catalyst precursor is preferably <50 ppmw. Furthermore, to avoid corrosion of catalyst production and processing equipment, the chloride content of the catalyst precursor is preferably less than 1500 ppmw, especially less than 650 ppmw. The titania can be washed to reduce the presence of these contaminants before or after shaping to achieve the desired levels.

[0015] Titania may be present in rutile or anatase crystalline forms. The catalyst precursor preferably comprises an anatase-containing support, preferably an anatase-rich support, in which the anatase form is present in an amount >50% by weight of the support. More preferably, the titania support has an anatase content of ≥70% by weight of the support, and most preferably, the titania support has an anatase content of ≥80% by weight of the support. The anatase form of titania is more porous and softer than the rutile form, and is particularly suitable for use as a Fischer-Tropsch catalyst precursor support.

[0016] Preferably, the titania carrier is 25 to 75 m 2 / g range of BET surface area.

[0017] The pore volume of the catalyst precursor is 0.20 to 0.60 cm 3 / g, preferably 0.30 to 0.50 cm 3 The catalyst precursor has an average pore diameter of preferably 30 to 60 nm, more preferably 40 to 50 nm. The catalyst precursor has a BET surface area of ​​preferably 35 to 65 m 2 / g. BET surface area and pore volume can be measured using nitrogen physisorption. Pore volume may also be determined using mercury porosimetry. Mercury porosimetry, also known as mercury intrusion porosimetry, is more suitable for use in the present invention due to the relatively large pore diameter. Pore diameter may also be determined using these techniques. Mercury intrusion porosimetry is a well-known technique that involves exposing a powder sample to mercury under pressure and measuring the change in volume. By "average pore diameter" is meant four times the pore volume divided by the surface area (4V / A). This relationship is derived from the geometry of a right circular cylinder of diameter D and height h, where the surface area (A) is given by πDh and the volume (V) is given by πD 2 It is given by h / 4.

[0018] The catalyst precursor has small cobalt oxide crystallites located within the pores of the catalyst support. The catalyst precursor has a ratio of average cobalt oxide crystallite size to average pore diameter of the catalyst precursor in the range of 0.1:1 to 0.6:1, preferably 0.2:1 to 0.4:1. This ratio is surprising because it is generally believed that the pore diameter of the support controls the metal oxide crystallite size, with pores with larger average diameters resulting in larger cobalt oxide crystallites. Applicant has surprisingly discovered that small cobalt oxide crystallites form within the relatively large pores of the titania support. Applicant has discovered that a combination of the physical properties of the titania support, the cobalt source, and the preparation conditions produces a catalyst precursor having the claimed ratio, which provides a Fischer-Tropsch catalyst with improved performance.

[0019] The preparation method that produces catalyst precursors having the claimed ratios is in contrast to prior art impregnation / deposition methods, such as those using cobalt ammine carbonate solutions, which typically can be difficult to reduce and, upon reduction, tend to rapidly sinter under FT conditions, producing very small cobalt oxide crystallites, typically <5 nm in average size, resulting in loss of activity.

[0020] Without being bound by theory, improved catalytic performance may result from catalyst precursors having the claimed average pore diameter to average cobalt crystallite size ratios, since the claimed ratios facilitate diffusion of reactants and products to and from catalytically active sites located within the pore structure, thereby enhancing catalytic selectivity and providing high activity. Additionally, the use of titania supports having relatively large pores and loading these pores with relatively small cobalt oxide crystallites is advantageous in providing longer hydrocarbon chain products than previously possible, and potentially in providing high alpha values.

[0021] The cobalt content of the oxidized catalyst precursor, expressed as Co, is preferably 5-25 wt%, more preferably 8-16 wt%. Despite the relatively low cobalt content, the resulting catalyst has a surprisingly high activity per gram in the Fischer-Tropsch reaction. In an active catalyst, at least a portion of the cobalt oxide in the catalyst precursor is reduced to elemental form, and the proportion of cobalt in the active catalyst increases as oxygen atoms in the cobalt oxide are removed. Particularly effective catalysts contain 8-12 wt% cobalt with a degree of reduction of 80 mole% cobalt oxide.

[0022] The catalyst precursor may further comprise one or more additives and / or promoters to improve the catalyst performance in the Fischer-Tropsch process. The additives are typically incorporated into the catalyst precursor at a higher concentration than the promoters. Suitable additives are selected from compounds of barium (Ba), silver (Ag), copper (Cu), nickel (Ni), iron (Fe), vanadium (V), tin (Sn), gallium (Ga), manganese (Mn), zirconium (Zr), lanthanum (La), cerium (Ce), magnesium (Mg), zinc (Zn), aluminum (Al), thorium (Th), tungsten (W), or silicon (Si). Suitable promoters include rhodium (Rh), iridium (Ir), ruthenium (Ru), rhenium (Re), platinum (Pt), and palladium (Pd). It has been found that the titania supported cobalt Fischer-Tropsch catalyst preferably further comprises manganese present in the catalyst precursor as one or more manganese oxides. If desired, one or more promoters selected from Ru, Re, and Pt may be included in the catalyst precursor. The additives and / or promoters may be incorporated into the catalyst precursor by using suitable compounds such as acids, for example perrhenic acid, metal salts, for example metal nitrates and oxynitrates or metal acetates, or suitable metal organic compounds, such as metal alkoxides or metal acetylacetonates. The amount of metal additive may vary from 1 to 25 wt% in the catalyst precursor, preferably from 1 to 15 wt% in the catalyst precursor. The amount of promoter metal may vary from 0.01 to 1.00 wt% in the catalyst precursor, preferably from 0.01 to 0.50 wt% in the catalyst precursor.

[0023] The catalyst precursor is prepared by impregnating a spherical titania support with a cobalt nitrate solution and drying and calcining the impregnated titania support to form cobalt oxide crystallites within the pores of the titania support. Impregnation, drying, and / or calcination can be repeated as necessary to obtain the desired catalyst precursor.

[0024] The cobalt nitrate is preferably cobalt(II) nitrate hexahydrate, which can be dissolved in its water of hydration, for example by heating to above 50° C., to form a concentrated solution of molten cobalt nitrate. Alternatively, the cobalt nitrate can be dissolved in water or another solvent to form a more dilute solution. Water, desirably demineralized water, is the preferred solvent. Impregnation can be carried out by adding the cobalt nitrate solution to the spherical titania support in a suitable mixer, such as a Plowshare mixer. Impregnation is carried out with the cobalt nitrate solution, preferably heated at a temperature above 50° C. The volume of cobalt nitrate solution used preferably approximates the total pore volume of the titania support. Such impregnation, which may be referred to as “dry impregnation” or “incipient wetness impregnation”, advantageously improves the deposition of the cobalt compound in the pores of the support and minimizes the amount of drying required. If desired, suitable additives and / or promoter compounds may be added in suitable amounts to the cobalt nitrate solution. Alternatively, they may be combined with the catalyst precursor before or after drying and / or before the final calcination.

[0025] The impregnated support is dried to remove the solvent, typically water, present in the cobalt nitrate solution, desirably leaving partially hydrated cobalt nitrate in the pores of the support. The drying step is preferably carried out at a temperature in the range of 50-150°C. The drying step can be carried out at atmospheric pressure in air or an inert gas such as nitrogen, or under vacuum. Drying times can range from 0.5 to 16 hours as appropriate, but are more preferably carried out at 80-120°C for 1 to 5 hours.

[0026] The dried impregnated support is a free-flowing powder comprising cobalt nitrate, preferably partially hydrated cobalt nitrate. To produce the catalyst precursor, the dried material is subjected to a heat treatment, sometimes called calcination, to convert the cobalt nitrate to a crystalline cobalt oxide having the desired crystallite size range. The heat treatment can be carried out conventionally in air, or by heating the dried material under nitrogen or another non-reducing gas mixture, or by heating under vacuum. The heat treatment can be carried out in a static or moving bed oven, or preferably in a fluidized bed reactor. A fluidized bed reactor has surprisingly been found to produce catalyst precursors having small average cobalt oxide crystallite sizes, for example in the range of 6-12 nm, especially 7-8 nm. The calcination temperature in the present invention is desirably in the temperature range of 220-320°C, preferably 240-300°C, to minimize sintering of the cobalt oxide crystallites and preserve the cobalt surface area. Calcination at these temperatures also avoids the possibility of the anatase in the titania support being converted to the rutile form. The calcination time may range from 0.5 to 16 hours as required, but is preferably carried out at 240 to 300°C for 1 to 4 hours. Under fluidized bed conditions, the calcination gas hourly space velocity (GHSV) is 1000 to 5000 h at normal temperature and pressure (NTP). -1 , preferably 2000 to 4000 hours -1 It could be.

[0027] The calcination step may be followed by a polishing step in which the calcined material is heated in a dilute hydrogen flow under conditions that do not cause the reduction of cobalt oxide to its elemental form. The polishing step may be advantageously used to reduce the residual nitrate content of the calcined material. The hydrogen flow may consist of, for example, 0.1-10% by volume hydrogen, preferably 1-5% by volume hydrogen, in an inert gas such as nitrogen. The pressure may be 1-10 bar absolute, preferably 1-3 bar absolute. The maximum temperature of the polishing step may range from 100 to 225°C, preferably 140 to 200°C. The polishing step may be suitably carried out for 0.5 to 16 hours as required, but is preferably carried out at 140 to 200°C for 1 to 3 hours. The gas hourly space velocity (GHSV) of the hydrogen / inert gas flow in the polishing step is 50 to 2000 hr -1 However, it is preferable to perform the treatment at room temperature and pressure (NTP) for 50 to 1000 hours. -1 , more preferably 100 to 500 hours -1 Under these conditions, essentially no reduction of cobalt oxide occurs. The polishing step reduces the residual nitrates in the catalyst precursor to levels below 0.1 wt. %, so that the subsequent reduction can be carried out without the need to take special steps to manage the ammonia formed during reduction. This is particularly useful when the catalyst precursor is reduced in-situ, i.e., in the reactor used for the Fischer-Tropsch process.

[0028] The catalyst precursor may be introduced into a reactor used for the Fischer-Tropsch reaction and activated to form the catalyst by in-situ reduction of at least a portion of the cobalt oxide to its elemental form. Such activation may be carried out using any suitable reducing agent, but is preferably carried out using a reducing gas stream selected from a hydrogen gas stream or a synthesis gas stream containing hydrogen and carbon monoxide. The reducing gas stream may consist of 1-100% by volume hydrogen in an inert gas such as nitrogen, or may be synthesis gas. The synthesis gas may suitably be a Fischer-Tropsch synthesis gas consisting essentially of hydrogen and carbon monoxide, with a hydrogen:carbon monoxide molar ratio in the range of 1.6-2.2. Alternatively, the reducing gas may comprise a mixture of these gases. The gas hourly space velocity (GHSV) of the reducing gas passing through the catalyst precursor may be between 4000 and 10000 hr at ambient temperature and pressure (NTP). -1 The gas hourly space velocity of the reducing gas may be varied during the reduction to control exposure of the cobalt oxide and reduced cobalt to water vapor. The maximum temperature used in the reduction step may range from 250 to 400°C, but is preferably in the range of 250 to 300°C to minimize sintering of the reduced cobalt crystallites. The reduction may be carried out at ambient or elevated pressure, i.e., the pressure of the reducing gas may be from 1 to 50 bar absolute.

[0029] Alternatively, the catalyst precursor may be pre-reduced ex-situ in a reduction vessel to provide the catalyst. Pre-reduction may be carried out using any suitable reducing agent, but is preferably carried out using a hydrogen gas stream operating in a loop that removes by-product water from the recycled reduction gas stream. The hydrogen stream may consist of 10-100% by volume hydrogen in an inert gas such as nitrogen. The concentration of hydrogen in the reduction gas may vary during the reduction. The gas hourly space velocity (GHSV) of the hydrogen / inert gas stream is between 3000 and 10000 hr at ambient temperature and pressure (NTP). -1 , preferably 4000 to 10000 hours -1The gas hourly space velocity of the reducing gas may be varied during the reduction to control exposure of the cobalt oxide and reduced cobalt to water vapor. The maximum temperature used in the reduction step may range from 250 to 400°C, but is preferably in the range of 250 to 300°C to minimize sintering of the reduced cobalt crystallites. The reduction may be carried out at ambient or elevated pressure, i.e., the pressure of the reducing gas may be from 1 to 50, preferably from 1 to 20, more preferably from 1 to 10 bar absolute.

[0030] Catalysts in the reduced state can be difficult to handle, as they may spontaneously react with oxygen in the air, leading to undesirable self-heating and loss of activity. As a result, the reduced catalyst can be protected by encapsulating the reduced catalyst with a suitable barrier coating. In the case of Fischer-Tropsch catalysts, this may suitably be a hydrocarbon wax, such as the wax produced by Fischer-Tropsch synthesis. Alternatively, the reduced catalyst may be passivated after reduction by exposure to an oxygen-containing gas, such as air or oxygen, which may be diluted with an inert gas, such as nitrogen, to form a protective outer layer of cobalt oxide on the cobalt crystallites. The encapsulating wax or the passivating outer layer of cobalt oxide can be removed from the catalyst after it has been introduced into the Fischer-Tropsch reactor by heating the catalyst under a flow of hydrogen gas or a flow of synthesis gas.

[0031] Whichever route is chosen, the cobalt catalyst provides a high metal surface area per gram of reduced metal. For example, the catalyst precursor preferably has a surface area of ​​≧5 m when reduced with hydrogen at 250° C., as measured by hydrogen chemisorption. 2 / g of cobalt surface area of ​​the catalyst.

[0032] Catalysts derived from the catalyst precursors are particularly useful for the Fischer-Tropsch synthesis of hydrocarbons. The Fischer-Tropsch synthesis of hydrocarbons using cobalt catalysts is well established. The Fischer-Tropsch synthesis converts a mixture of carbon monoxide and hydrogen into hydrocarbons, preferably those with a carbon chain length of ≥5. The mixture of carbon monoxide and hydrogen is typically synthesis gas having a hydrogen:carbon monoxide ratio in the range of 1.6-2.2:1. The reaction can be carried out in a continuous or batch process using one or more reactors such as fixed bed reactors, slurry phase reactors, bubble column reactors, loop reactors, or fluidized bed reactors. The process can be operated at pressures in the range of 0.1-10 MPa and temperatures in the range of 150-350°C. The gas hourly space velocity (GHSV) for continuous operation is between 1000-25000 hr -1 The range is.

[0033] The catalyst of the present invention is particularly suitable as a fixed bed catalyst, ie, a catalyst bed fixed within a reaction vessel through which the reactant synthesis gas is passed.

[0034] The physical properties of the catalyst precursor mean that it is suitable for use in a microchannel reactor, i.e. a Fischer-Tropsch reactor having multiple catalyst-containing channels with widths or heights in the range 2-10 mm through which synthesis gas passes, or in a catalyst carrier placed in a reaction tube in a Fischer-Tropsch reactor, such as a downflow multi-tube Fischer-Tropsch reactor.

[0035] The catalyst or catalyst precursor has been found to be particularly effective when used in combination with a catalyst carrier suitable for use in a tubular reactor. By "catalyst carrier" is meant a catalyst vessel, for example in the form of a cup or can, configured to allow gas and / or liquid to flow into or out of the carrier and through a bed of catalyst or catalyst precursor disposed within the carrier. Any suitable catalyst carrier may be used. In one configuration, the catalyst carrier is one described in WO2011 / 048361, the contents of which are incorporated herein by reference. The catalyst carrier described in WO 2011 / 048361 comprises an annular vessel for holding a catalyst in use, the vessel having a perforated inner wall defining a tube, a perforated outer wall, a top surface closing the annular vessel, and a bottom surface closing the annular vessel; a surface closing the bottom of the tube formed by the inner wall of the annular vessel; a skirt extending upwardly from the perforated outer wall of the annular vessel from a position at or near the bottom surface of the vessel to a position below the position of a seal; and a seal located at or near the top surface and extending from the vessel a distance that extends beyond the outer surface of the skirt. In one configuration, the catalyst carrier is as disclosed in WO 2016 / 050520, the contents of which are incorporated herein by reference. Thus, the catalyst carrier may comprise a vessel suitable for holding a catalyst precursor or catalyst in place, the vessel having a bottom surface closing the vessel and a top surface; a carrier outer wall extending from the bottom surface to the top surface of the vessel; and a seal extending a distance from the vessel extending beyond the carrier outer wall, the carrier outer wall having an opening disposed below the seal. In a preferred configuration, the catalyst carrier may comprise an annular vessel suitable for holding a catalyst precursor or catalyst in place, the vessel having a perforated inner vessel wall defining an inner channel, a perforated outer vessel wall, a top surface closing the annular vessel, a bottom surface closing the annular vessel, and a surface closing the bottom of the inner channel formed by the inner vessel wall of the annular vessel. The catalyst carrier is generally sized to have dimensions smaller than the internal dimensions of the reactor tube in which it is placed during use. The seal is sized to interact with the inner wall of the reactor tube when the catalyst carrier of the present invention is in place within the reactor tube.

[0036] When used in a vertical reactor with downflow, the reactants flow downward through the reactor tubes and thus first contact the upper surface of the catalyst carrier. A seal blocks the reactants from passing around the sides of the carrier so that its upper surface directs them into the inner channel defined by the inner vessel wall. The reactants then enter the annular vessel through the perforated inner vessel wall and then pass radially through the catalyst bed towards the perforated outer vessel wall. During the passage from the inner vessel wall to the outer vessel wall, the reactants contact the catalyst and the Fischer-Tropsch reaction occurs. The unreacted reactants and products then flow out of the vessel through the perforated outer vessel wall. The carrier outer wall then directs the reactants and products upward between the inner surface of the carrier outer wall and the perforated outer vessel wall of the annular vessel until they reach openings in the carrier outer wall. They are then directed through openings located in the carrier outer wall and flow downward between the outer surface of the carrier outer wall and the inner surface of the reactor tube where heat transfer takes place. If the reactor is operated so that the flow is reversed, the path is reversed.

[0037] The catalyst precursor can be loaded onto a catalyst carrier and the resulting combination loaded into the reactor tube of a Fischer-Tropsch reactor to reduce and activate the catalyst in-situ as described above. Alternatively, the combination can be subjected to ex-situ reduction in a reduction vessel, the combination can be encapsulated or subjected to a passivation treatment. The resulting combination can then be safely loaded into the reactor tube of a Fischer-Tropsch reactor.

[0038] The invention will now be further described with reference to the following examples.

[0039] In the examples, the following measurements were carried out.

[0040] Particle size: Particle size was determined according to ASTM D4464 by laser light scattering using a Malvern Mastersizer3000 laser diffraction particle size analyzer using the optical properties of TiO2 (anatase) from the Malvern MS3000 optical properties database in the instrument software (refractive index 2.51, absorptivity 0.01). Wet dispersion measurements were performed in deionized water using 0% and 85% sonication and 50% stirring speed using a Hydro MV sample dispersion unit. Sufficient sample was added to the unit until the laser beam was 0.1-20% obscured. Five measurements were taken for each aliquot of sample, with a measurement time of 5 seconds. Dry dispersion measurements were performed in an Aero dry dispersion unit equipped with a microvolume tray and standard venturi, using dispersion air pressures of 0.5 bar and 3.0 bar using on-site compressed air, with a feed rate of 20%. One measurement was taken per aliquot of sample, with the entire aliquot measured for each measurement. The measurement time is 15 seconds when the laser beam is 0.1-10% blocked. To calculate the results, the Malvern software uses Mie theory to convert the resulting diffraction pattern into a particle size distribution.

[0041] Pore ​​volume. Mercury intrusion / extrusion data were measured on a Micromeritics AutoPore 9520 mercury porosimeter according to ASTM Method D4284-03; Test Method for Determining Pore Volume Distribution of Catalysts by Mercury Intrusion Porosimetry. Intrusion curves were measured over a pressure range of 0.5-60000 psia and then extruded to atmospheric pressure. An equilibration time of 15 seconds was used for each data point on both the intrusion and extrusion curves, with a mercury contact angle of 140° and a mercury surface tension of 485 dynes / cm. Samples were dried overnight at 115°C in an oven prior to analysis. Temperature and pressure effects manifested during porosimetry measurements were accounted for by performing a blank correction with an empty hardness tube and then subtracted from the experimental data.

[0042] Surface areas were measured using a Micromeritics 2420 ASAP physisorption analyzer applying the BET method according to ASTM Method D 3663-03; Standard Test for Surface Area. Nitrogen was used as the adsorbate and measurements were performed at liquid nitrogen temperature (77 K). The cross-sectional area of ​​the nitrogen molecule was taken as 16.2 Å. Prior to analysis, samples were degassed by purging with dry nitrogen gas at 140 °C for a minimum of 1 h. Five relative pressure / volume data pairs were acquired over the relative pressure range of 0.05 to 0.20 P / Po. The equilibration time for each point was 10 s. Surface areas are reported based on the weight of the sample after degassing.

[0043] Average pore diameter. Average pore diameter was calculated from measurements of pore volume and surface area. The average pore diameter is four times the corrected pore volume divided by the calculated surface area (4V / A). This relationship is derived from the geometry of a right circular cylinder of diameter D and height h, where the surface area (A) is given by πDh and the volume (V) is given by πD 2 It is given by h / 4.

[0044] Median Pore Diameter. Median pore diameter was derived from pore volume measurements. "Median pore diameter" means the pore diameter that represents the midpoint of the cumulative mercury intrusion curve, corrected for interparticle void filling.

[0045] Cobalt content, as determined by ICPAES (inductively coupled plasma atomic emission spectroscopy) or ICPMS (inductively coupled plasma mass spectroscopy) of the calcined catalyst precursor and expressed as weight percent of cobalt on a loss-free basis.

[0046] Cobalt oxide crystallite size. Cobalt oxide crystallite size was determined by XRD using a Bruker D8 Advance X-ray diffractometer. Powdered catalyst precursor samples were pressed into a sample holder and loaded into the instrument. Parallel beam (Gobel mirror) optics. Software; Bruker EVA for phase identification; Topas for patterning. Diffractometer conditions were: X-ray Lynxeye PSD detector detects Cu Ka wavelength of 1.5406A. Start 2 Theta 10, End 2 Theta 130 Step 0.022 Step time, seconds 4 X-ray current, mA 40 X-ray voltage, kV 40 Cobalt oxide crystallite size was determined using Rietveld analysis (Bruker Topas v4.2). The Rietveld analysis of powder XRD data begins with a calculated diffraction pattern based on symmetry information and an approximate structure. The Rietveld analysis then uses least squares minimization to compare all observed points to the calculated plot and refine the calculated structure to minimize the differences.

[0047] Cobalt surface area. The surface area of ​​cobalt metal was measured on a Micromeritics 2480 HTP 6 Station Chemisorption Analyser. Samples were reduced with 100% hydrogen by volume for 120 minutes at 250°C with a hydrogen flow rate of 200 SCCM. After the reduction step was completed, the samples were purged with helium for 15 minutes and then cooled under vacuum to the analysis temperature of 35°C. After a vacuum of <10 μmHg was reached, evacuation was continued for 45 minutes. The samples were then loaded with 100% hydrogen by volume over a pressure range of 100-760 mmHg. At each pressure, the chemisorbed hydrogen was allowed to equilibrate and the volume of hydrogen uptake was measured and automatically recorded. The pressure / uptake pairs were plotted to obtain an isotherm that exhibited a well-defined plateau region. Data points were selected within this region to achieve a best linear fit, which was then extrapolated back to zero pressure. The intercept value was used to calculate the cobalt surface area using a stoichiometry of 1.0 for H2 / Co, and the cobalt surface area was reported based on the mass of reduced catalyst.

[0048] Example 1.3 Catalyst precursor preparation on 12 μm titania spheres a) 20 wt / wt% Co, 0.2 wt / wt% Ru. (i) 346.4 g of cobalt nitrate hexahydrate crystals (19.80 wt / wt% Co) and 5.4 g of ruthenium nitrosyl nitrate solution (12.54 wt / wt% Ru) were placed in a glass beaker and heated to 80° C. on a hot plate. The hot solution was added to 500.05 g of 312 μm D50 titania spheres (>85 wt / wt% anatase by XRD) in a preheated Z-blade mixer. The temperature of the titania before the addition of the solution was 65° C. and the mixer walls were at 69° C. The solution was poured onto the mixed titania spheres over a period of approximately 4 minutes. Mixing was continued for 2 minutes after the solution addition. 842.0 g of impregnated material was discharged and placed into seven stainless steel trays. This material was then dried at 110° C. for 3 hours and calcined at 280° C. for 2 hours. This produced 599.9 g of calcined material. (ii) 594.3 g of calcined material from step (i) was placed in a preheated Z-blade mixer. 286.7 g of cobalt nitrate hexahydrate crystals and 4.6 g of ruthenium nitrosyl nitrate solution were placed in a glass beaker and heated to 80° C. on a hot plate. The temperature of the material before the addition of the solution was 64° C. and the mixer walls were 68° C. The solution was poured into the mixed material over a period of approximately 3 minutes. Mixing was continued for 2 minutes after the addition of the solution. 876.2 g of impregnated material was discharged and placed into seven stainless steel trays. The material was then dried at 110° C. for 3 hours and calcined at 280° C. for 2 hours. This produced 671.8 g of calcined material.

[0049] FT catalyst precursor properties D50=311μm BET SA=39m 2 / g Co SA=8m 2 / g Hg intrusion volume = 0.23 cm 3 / g Hg average pore diameter = 36 nm Hg median pore diameter = 42 nm Co3O4 crystallite size (XRD) = 13.5 nm Co content (ICP)=18.4w / w% Ru content (ICP)=0.15w / w% Ratio of average cobalt oxide particle size to average pore diameter of catalyst precursor = 13.5:36 = 0.38:1

[0050] b) 11% w / w Co, 1% w / w Mn. 320.6 g of cobalt nitrate hexahydrate crystals (19.80 wt / wt% Co) and 12.0 g of demineralized water were placed in a glass beaker and heated on a hot plate. 39.14 g of manganese nitrate solution (15.4 wt / wt% Mn) was added at 60°C and the mixture was further heated until it reached 70°C. The hot solution was added to 500.05 g of 312 μm D50 titania spheres (>85 wt / wt% anatase by XRD) in a preheated Z-blade mixer. The temperature of the titania before the addition of the solution was 64°C and the mixer walls were 68°C. The solution was poured onto the mixed titania spheres over a period of approximately 3 minutes. Mixing was continued for 2 minutes after the addition of the solution. 852.2 g of the impregnated material was discharged and placed into 7 stainless steel trays. The material was then dried at 100°C for 3 hours and calcined at 250°C for 2 hours. Yield 596.7g of calcined material.

[0051] FT catalyst precursor properties D50=310μm BET SA=44m 2 / g Co SA=6m 2 / g Hg intrusion volume = 0.28 cm 3 / g Hg average pore diameter = 37 nm Hg median pore diameter = 45 nm Co3O4 crystallite size (XRD) = 13.0 nm Co content (ICP) = 10.4 wt / wt% (oxide) Mn content (ICP) = 0.96 wt / wt% (oxide) The ratio of the average cobalt oxide particle size to the average pore diameter of the catalyst precursor=13:37=0.35:1.

[0052] Example 2.4 Catalyst precursor preparation on 13 μm titania spheres a) 11% w / w Co, 1% w / w Mn. The method of Example 1(b) was repeated using 413 μm D50 titania spheres.

[0053] FT catalyst precursor properties D50=412μm BET SA=43m 2 / g Co SA=5m 2 / g Hg intrusion volume = 0.29 cm 3 / g Hg average pore diameter = 43 nm Hg median pore diameter = 43 nm Co3O4 crystallite size (XRD) = 14.8 nm Co content (ICP) = 10.6 wt / wt% (oxide) Mn content (ICP) = 1.03 wt / wt% (oxide) The ratio of the average cobalt oxide particle size to the average pore diameter of the catalyst precursor=14.8:43=0.34:1.

[0054] Example 3: Comparative Example: Catalyst preparation on 309 μm alumina spheres a) 20 wt / wt% Co, 0.2 wt / wt% Ru. 12.5 Kg of alumina balls (γ-Al2O3) were placed in a RT80 mixer and the water bath was at 80°C. This was left to heat overnight. 15.9 Kg of cobalt nitrate hexahydrate crystals (19.80 wt / wt% Co), 240 g of ruthenium nitrosyl nitrate (13.0 wt / wt% Ru) and 1210.0 g of demineralized water were heated in a stainless steel beaker on a hot plate until the cobalt nitrate crystals melted. The solution was then transferred to a preheated spray pot. The hot solution was sprayed onto the alumina balls at 54°C. The solution was then sprayed over a period of 20 minutes. Mixing was continued for 1 minute 30 seconds after the addition of the solution before discharging the material into a drum. 28.865 Kg of material was discharged. This was placed in a stainless steel tray and dried in an oven at 110°C for 3 hours. The dried material was divided into 4 batches. Each of the four batches was redried at 110° C. for 30 minutes and then calcined at 280° C. for 2 hours.

[0055] Comparative FT catalyst precursor properties D50=305μm BET SA=153m 2 / g Co SA=12m 2 / g(425℃ decrease) Hg intrusion volume = 0.45 cm 3 / g Hg average pore diameter = 14 nm Hg median pore diameter = 13 nm Co3O4 crystallite size (XRD) = 15.5 nm Co content (ICP) = 18.4 wt / wt% (oxide) Ru content (ICP) = 0.13 wt / wt% (oxide) The ratio of the average cobalt oxide particle size to the average pore diameter of the catalyst precursor=15.5:14=1.11:1.

[0056] Example 4: Catalysis Test Tests were carried out using 0.5 g of catalyst precursor diluted with 2.00 g of SiC placed in a 4 mm inner diameter laboratory reactor tube. After in situ reduction at 300° C. (1° C. / min ramp) in pure hydrogen for 7 hours using a flow rate of 60 mL / min, the temperature was then reduced to 150° C., the gas was switched to syngas (H2:CO=2:1), and the reactor was pressurized to 20 barg using a flow rate of 110 mL / min. After 6 hours, the temperature was increased (1° C. / min) to 210° C. and left overnight for about 16 hours. The flow rate was then reduced first to 50 mL / min and then to the flow rate required to achieve 50% syngas conversion, and data collection was continued for the duration of the test (about 160 hours). Inlet gas was metered into the reactor using a mass flow controller. Gaseous, liquid, and solid hydrocarbon products as well as the water phase were analyzed by gas chromatography to achieve mass balance for calculating CO conversion and selectivity. Alpha is calculated from the slope of a plot of log(Wn / n) as a function of n, where the slope is log(α), where Wn is the weight fraction of hydrocarbons of carbon number n, and α is the chain growth probability. This formula is derived from the Anderson-Schultz-Flory distribution, Wn=nα n-1 (1-α) 2Typically, C 20 ~C 40 was the range of carbon numbers used in the calculation of alpha. The results were as follows:

[0057] [Table 1]

[0058] Comparing Example 1(a) and Example 3(a), the results show that the titania sphere supported catalyst precursor according to the invention produced catalysts with improved activity and selectivity to higher hydrocarbons compared to the same metal and promoter levels on the corresponding spherical alumina supports. Example 2(a) shows the improved performance of the Mn-promoted cobalt catalyst on a titania sphere support compared to Example 1(a).

Claims

1. 1. A cobalt catalyst precursor for a Fischer-Tropsch reaction comprising cobalt oxide crystallites disposed within the pores of a titania support, the cobalt oxide crystallites having an average size determined by XRD in the range of 6 to 18 nm, the titania support being a spherical titania support having a particle size in the range of 100 to 1000 μm, the catalyst precursor having a diameter of 0.2 to 0.6 cm 3 / g and an average pore diameter in the range of 30 to 60 nm, said catalyst precursor having a ratio of said average cobalt oxide crystallite size to said average pore diameter in the range of 0.1:1 to 0.6:

1.

2. 2. The cobalt catalyst precursor of claim 1, wherein the cobalt oxide crystallites have an average size in the range of 7 to 16 nm.

3. 3. The cobalt catalyst precursor of claim 1 or 2, wherein the particle size of the catalyst precursor is in the range of 300 to 800 μm.

4. 4. The cobalt catalyst precursor of claim 1, wherein the catalyst precursor has a volume median diameter D[v,0.5] in the range of 300 to 500 μm.

5. 5. The cobalt catalyst precursor of any one of claims 1 to 4, wherein the sulfur content of the catalyst precursor is <30 ppmw, the alkali metal content of the catalyst precursor is <50 ppmw, and the chloride content of the catalyst precursor is <1500 ppmw.

6. A cobalt catalyst precursor according to any one of claims 1 to 5, wherein the titania support used is an anatase containing support, the anatase being present in an amount of >50% by weight of the support.

7. The pore volume of the catalyst precursor is 0.2 to 0.6 cm 3 / g and the average pore diameter is in the range of 30 to 60 nm.

8. 8. The cobalt catalyst precursor of any one of claims 1 to 7, wherein the cobalt content of the catalyst precursor, expressed as Co, is in the range of 5 to 25 wt.%.

9. 9. The cobalt catalyst precursor of any one of claims 1 to 8, further comprising one or more additives selected from compounds of molybdenum (Mo), barium (Ba), silver (Ag), copper (Cu), nickel (Ni), iron (Fe), vanadium (V), tin (Sn), gallium (Ga), manganese (Mn), zirconium (Zr), lanthanum (La), cerium (Ce), chromium (Cr), magnesium (Mg), zinc (Zn), aluminum (Al), thorium (Th), tungsten (W), or silicon (Si), wherein the amount of metal additive is 1 to 25 wt% on said catalyst precursor.

10. 10. The cobalt catalyst precursor of any one of claims 1 to 9, further comprising one or more promoters selected from rhodium (Rh), iridium (Ir), ruthenium (Ru), rhenium (Re), platinum (Pt), and palladium (Pd), wherein the amount of promoter metal is 0.01 to 1.00 wt% on the catalyst precursor.

11. 11. The method for preparing a catalyst precursor according to any one of claims 1 to 10, comprising impregnating a spherical titania support having a particle size in the range of 100 to 1000 μm with a cobalt nitrate solution, and drying and calcining the impregnated titania support, thereby forming cobalt oxide crystallites in the pores of the titania support.

12. 12. The method of claim 11, wherein the impregnation is carried out with a cobalt nitrate solution heated at a temperature above 50°C.

13. 13. The method according to claim 11 or 12, wherein the volume of the cobalt nitrate solution used is less than or equal to the total pore volume of the titania support.

14. A method according to any one of claims 11 to 13, wherein the impregnated support is dried at a temperature in the range of from 50 to 150°C.

15. A method according to any one of claims 11 to 14, wherein the calcination is carried out at a temperature in the range of from 200 to 350°C.

16. The method according to any one of claims 11 to 15, wherein the calcination is carried out in a fluidized bed reactor.

17. A method for forming a catalyst comprising free-standing cobalt crystallites, the method comprising reducing the cobalt oxide crystallites in a catalyst precursor according to any one of claims 1 to 10 with a reducing gas stream.

18. 18. The method of claim 17, wherein the catalyst is subjected to a passivation treatment or encapsulated in a hydrocarbon wax.

19. A combination of catalyst precursors according to any one of claims 1 to 10 disposed within a catalyst carrier suitable for use in the reactor tubes of a Fischer-Tropsch reactor.

20. 20. The combination of claim 19, wherein the catalyst carrier comprises an annular vessel suitable for holding the catalyst precursor or catalyst in place, the vessel having a perforated inner vessel wall defining an inner channel, a perforated outer vessel wall, a top surface closing the annular vessel, a bottom surface closing the annular vessel, and a surface closing the bottom of the inner channel formed by the inner vessel wall of the annular vessel.

21. Use of a catalyst precursor according to any one of claims 1 to 10 in a process for producing hydrocarbons from a synthesis gas comprising hydrogen and carbon monoxide in a Fischer-Tropsch reactor.

22. 22. The use according to claim 21 , wherein the Fischer-Tropsch reactor is a microchannel reactor, a multi-tube Fischer-Tropsch reactor, a slurry phase reactor, a slurry bubble column reactor, a loop reactor, or a fluidized bed reactor.

23. 22. The use according to claim 21 , wherein the catalyst precursor or catalyst comprises the combination according to claim 19 or 20 and the Fischer-Tropsch reactor is a multi-tube Fischer-Tropsch reactor.

24. A method for forming a combination comprising placing a catalyst obtained by the method of claim 17 or 18 in a catalyst carrier suitable for use in a reactor tube of a Fischer-Tropsch reactor.

Citation Information

Patent Citations

  • Activation of Fischer-Tropsch supported catalysts

    JP2005516769A

  • Metal nitrate conversion method

    JP2009520674A

  • Process for preparation of catalyst using at least one rapid drying stage and at least one fluidised bed drying stage and use thereof for fischer-tropsch synthesis

    JP2013248609A

  • catalyst

    JP2014514151A

  • Fischer-Tropsch process in a radial reactor

    JP2014518905A