Preparation method of titanium dioxide / cuprous oxide heterojunction material and application of titanium dioxide / cuprous oxide heterojunction material in photocatalytic hydrogen production
By introducing Cu2O into the titanium dioxide branched structure to form an n-p-p-type ternary heterojunction, the problems of narrow photoresponse range and high electron hole recombination rate of titanium dioxide photocatalytic materials are solved, and the photocatalytic performance improvement and photocatalytic decomposition of aquatic products are achieved. Excellent effect of hydrogen.
Patent Information
- Application Number
- CN202410823155.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-11-01
AI Technical Summary
The existing titanium dioxide photocatalytic materials have a wide bandwidth, can only absorb ultraviolet light, and the probability of photogenerated electron hole recombination is high, which limits its photocatalytic performance.
In the titanium dioxide branched structure with n-p-type homojunction, the p-type semiconductor catalyst Cu2O is introduced to form an n-p-p-type ternary heterojunction, and the titanium dioxide/cubous oxide heterojunction material is prepared by hydrothermal method and sintering method to expand the photo response Range and promote charge separation and transfer.
The light utilization rate and photocatalytic performance of the material are improved, and the excellent photocatalytic decomposition of aquatic hydrogen is shown. The Cu2O particles are loaded uniformly on the TiO2 branched structure, effectively inhibiting the separation of photogenerated carriers.
Smart Images

Figure HDA0004909677990000011 
Figure HDA0004909677990000012 
Figure HDA0004909677990000021
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photocatalytic hydrogen production materials, and in particular to a preparation method and application of a titanium dioxide / cuprous oxide heterojunction material. Background Art
[0002] As the most widely used semiconductor photocatalytic material, TiO2 has the advantages of relatively stable chemical properties, strong redox ability, non-toxic and pollution-free to the environment, and low cost. At present, the photocatalytic performance of titanium dioxide is mainly restricted by two factors. One is that the band gap of TiO2 is relatively wide and can only absorb ultraviolet light. The other is that after TiO2 is excited, the probability of recombination of photogenerated electron-hole pairs is relatively high. Constructing np-type heterojunction in TiO2 material can effectively inhibit the recombination of photogenerated electrons and holes.
[0003] The photocatalytic process can be divided into five parts: light absorption, material excitation to generate electrons and holes, hole and electron separation, electron hole migration to the catalyst surface, and electron hole and adsorbate redox reaction. Therefore, improving the catalytic performance of a material depends largely on the generation, separation, transfer and utilization of photogenerated charges. Semiconductor heterojunction structure plays a significant role in improving the performance of catalysts in the field of photocatalysis. The construction of binary heterojunctions has been widely studied by researchers, including traditional II heterojunctions, Z-type heterojunctions, surface heterojunctions, and np heterojunctions.
[0004] Among these heterojunctions, the np heterojunction formed by n-type semiconductor and p-type semiconductor is a very popular photocatalytic material because the Fermi level difference between these two types of semiconductors is large, and a very strong internal electric field will be formed at the interface of the two phases before being irradiated, which can promote the effective transfer and separation of charges. According to current research, there are related patents on the preparation of titanium dioxide / cuprous oxide heterojunction materials, but the innovative points of the preparation method designed by this patent are different. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for preparing a titanium dioxide / cuprous oxide heterojunction material in view of the deficiencies of the above-mentioned prior art. The present invention introduces a p-type semiconductor catalyst Cu2O into a TiO2 dendritic structure having an np-type homojunction to form an npp-type ternary heterojunction in space, and the prepared titanium dioxide / cuprous oxide heterojunction material exhibits excellent photocatalytic water decomposition and hydrogen production performance.
[0006] The technical solution adopted by the present invention to solve the above-mentioned problems is:
[0007] A titanium dioxide / cuprous oxide heterojunction material is prepared by the following method:
[0008] 1) dissolving amorphous titanium dioxide (TiO2-As) in anhydrous ethanol, uniformly dispersing by ultrasonication, then adding glycerol and stirring for 20-40 minutes, and then adding tetrabutyl titanate and stirring for 20-40 minutes;
[0009] 2) transferring the mixed solution obtained in step 1) into a polytetrafluoroethylene-lined autoclave, reacting at 170-190° C. for 10-15 hours, cooling to room temperature, separating the solid product, washing and drying;
[0010] 3) calcining the solid product obtained in step 2) at 450-500° C. for 1.5-2.5 h in an air atmosphere to obtain a titanium dioxide TiO2 dendritic structure having an np-type homojunction;
[0011] 4) dissolving cupric acetate in anhydrous ethanol, then adding polyvinyl pyrrolidone and mixing evenly to obtain a mixed solution;
[0012] 5) adding titanium dioxide TiO2 dendrite structure having np-type homojunction to the mixed solution obtained in step 4), stirring at a constant temperature of 30-50° C. for 20-40 min to obtain a precursor solution;
[0013] 6) Glucose solution is added to the precursor solution obtained in step 5), and sodium hydroxide is added after mixing evenly. After precipitation occurs, ultrasonic treatment is performed for 3-5 minutes. The precipitated product is washed alternately with ethanol and deionized water and then dried to obtain a titanium dioxide / cuprous oxide heterojunction material.
[0014] According to the above scheme, in step 1), the preparation method of amorphous titanium dioxide (TiO2-As) comprises the following steps:
[0015] (1) Add titanium dioxide P25 to deionized water at a concentration of 4-6 mg / mL and stir until a milky white solution is obtained;
[0016] (2) transferring the mixed solution obtained in step (1) into a polytetrafluoroethylene-lined autoclave, reacting at a constant temperature of 170-190° C. for 45-50 hours, cooling to room temperature, washing the product with deionized water and drying;
[0017] (3) Grind the product in step (2) and dissolve it in 0.05-0.2 mol / L HCl. Stir ultrasonically for 24 h and then filter. Dissolve the product in HCl again. Repeat the above steps 3 times. Wash the product with deionized water and dry it to obtain TiO2-As.
[0018] According to the above scheme, in step 1), the addition concentration of TiO2-As in anhydrous ethanol is 2-6 mg / mL, the volume ratio between glycerol and anhydrous ethanol is 1:(2-4), and the addition concentration of tetrabutyl titanate is 20-30 mg / mL (the addition concentration here refers to the mass concentration relative to the total volume of glycerol and anhydrous ethanol).
[0019] According to the above scheme, in step 4), the concentration of copper acetate added in anhydrous ethanol is 3-6 mg / mL, and the concentration of polyvinyl pyrrolidone added is 10-15 mg / mL.
[0020] According to the above scheme, in step 4), the mixture is stirred at a constant temperature of 30-50° C. for 5-15 minutes to achieve uniform mixing.
[0021] According to the above scheme, in step 5), the addition concentration of titanium dioxide TiO2 dendrite structure having np-type homojunction is 5-10 mg / mL.
[0022] According to the above scheme, in step 6), the concentration of the glucose solution is 0.1-0.3 mol / L; the volume ratio between the glucose solution and the precursor solution is 1:(2-4).
[0023] According to the above scheme, in step 6), the concentration of sodium hydroxide added to the mixed solution of glucose solution and precursor solution is 8-12 mg / mL.
[0024] The titanium dioxide / cuprous oxide heterojunction material prepared by the above method can be used as a photocatalyst in the field of photocatalytic hydrogen production. In the titanium dioxide / cuprous oxide heterojunction material, TiO2 is a branched structure, and Cu2O particles are loaded on the TiO2 branches; the size of the Cu2O particles is about 10 to 15 nm, the size is relatively uniform, and the dispersion is relatively uniform, and no obvious agglomeration of Cu2O particles is found; and the theoretical mass ratio of TiO2 to Cu2O is (4-6):1, preferably 5:1.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The present invention firstly adopts a hydrothermal method and a sintering method to prepare a TiO2 dendritic structure with an np-type homojunction, then introduces a p-type semiconductor catalyst Cu2O into the TiO2 dendritic structure with an np-type homojunction by a chemical precipitation method, and then constructs a pp-type heterojunction between p-TiO2 and Cu2O, thereby forming a continuous electron transfer pathway of an npp-type ternary heterojunction in space, thereby achieving the purpose of further improving the photocatalytic performance of the material. In the titanium dioxide / cuprous oxide heterojunction material prepared by the present invention, Cu2O particles are loaded on TiO2 with an np-type homojunction, so that its response range to light is widened to about 400nm, the light utilization rate of the material is improved, and the construction of the ternary heterojunction allows the charges to be effectively separated and continuously transferred, effectively suppressing the separation of photogenerated carriers, and therefore is a very promising photocatalyst, showing excellent photocatalytic water decomposition hydrogen production performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is the XRD spectrum of the amorphous titanium dioxide TiO2-As used in the example and the titanium dioxide TiO2 with np type homojunction prepared, wherein a is the amorphous titanium dioxide TiO2-As, and b is the titanium dioxide TiO2 with np type homojunction prepared in step (4) of Example 1.
[0028] Figure 2 is a SEM image of the titanium dioxide / cuprous oxide heterojunction material prepared in Example 1;
[0029] Figure 3 is the XRD pattern of the titanium dioxide / cuprous oxide heterojunction material prepared in Example 1;
[0030] Figure 4 This is a graph of the rate of hydrogen production from photolysis of water by the titanium dioxide / cuprous oxide heterojunction material prepared in Example 1 and titanium dioxide TiO2 in Comparative Example 1. DETAILED DESCRIPTION
[0031] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with embodiments, but the present invention is not limited to the following embodiments.
[0032] In the following examples, the amorphous titanium dioxide TiO2-As used is prepared by the following steps:
[0033] (1) Add 0.3 g of titanium dioxide P25 to 60 ml of deionized water and stir until a milky white solution is obtained;
[0034] (2) transferring the mixed solution obtained in step (1) into a polytetrafluoroethylene-lined autoclave, reacting at 180° C. for 48 h, cooling to room temperature, washing the product with deionized water and drying;
[0035] (3) Grind the product in step (2) and dissolve it in 0.1 mol / L HCl. Stir it ultrasonically for 24 h and then filter it. Dissolve the product in 0.1 mol / L HCl again. Repeat the above steps 3 times. Wash the product with deionized water and dry it to obtain TiO2-As.
[0036] Example 1
[0037] A titanium dioxide / cuprous oxide heterojunction material is prepared by the following method:
[0038] (1) Dissolve 0.1 g TiO2-As in 26 ml anhydrous ethanol, disperse by ultrasonication and stir for 10 min;
[0039] (2) Add 8.6 ml of glycerol to the mixed solution obtained in step (1), stir for 30 min, then add 0.86 g of tetrabutyl titanate, and stir for 30 min;
[0040] (3) transferring the mixed solution obtained in step (2) into a polytetrafluoroethylene-lined autoclave, reacting at 180° C. for 12 h, cooling to room temperature, separating the solid product, washing with ethanol, and drying;
[0041] (4) calcining the solid product of step (3) at 470° C. in air for 2 h to obtain a titanium dioxide TiO2 dendritic structure having an np-type homojunction;
[0042] (5) 30 mL of anhydrous ethanol was added to a container, 0.14 g of copper acetate monohydrate was added, and ultrasonic dissolution was performed. Then 0.4 g of polyvinyl pyrrolidone (K30) was added, and ultrasonic dissolution was performed. The mixture was stirred at a constant temperature of 40° C. for 10 min to obtain a mixed solution.
[0043] (6) adding 0.25 g of titanium dioxide TiO2 having an np-type homojunction to the mixed solution obtained in step (5), stirring at a constant temperature of 40° C. for 30 min, to obtain a precursor solution;
[0044] (7) Add 10 mL of 0.2 mol / L glucose solution to the precursor solution obtained in step (6), and add 0.4 g of sodium hydroxide 1 min later. After precipitation, ultrasonic treatment is performed for 4 min. The solid product is washed alternately with ethanol and deionized water and dried at 60 ° C for 2 h to obtain a titanium dioxide / cuprous oxide heterojunction material TiO2 / Cu2O. The theoretical mass ratio of TiO2 to Cu2O in the sample is 5:1.
[0045] Figure 23 is the SEM of the titanium dioxide / cuprous oxide heterojunction material prepared in Example 1. It can be seen from the figure that after TiO2 is compounded with Cu2O, the original morphology and structure of TiO2 are not destroyed, and the original branched structure is still maintained. In addition, some nanoparticles with a size of about 10 to 15 nm are grown on the TiO2 branches. The size is relatively uniform and the dispersion is relatively even. No obvious agglomeration of Cu2O particles is found, which shows that the Cu2O particles have been successfully loaded on TiO2 with an np-type homojunction, that is, the TiO2 / Cu2O ternary heterojunction is successfully constructed.
[0046] Figure 3 : This is the XRD diagram of the titanium dioxide / cuprous oxide heterojunction material prepared in Example 1. The black triangle in the figure indicates the characteristic peak of anatase TiO2 (JCPDS no.89-4921), and the black square indicates the characteristic peak of cubic crystal Cu2O (JCPDS no.78-2076). It can be seen from the figure that after compounding with Cu2O, obvious characteristic peaks appear at 2theta=36.4° and 2theta=42.3°. These two diffraction peaks belong to the (111) and (200) crystal planes of cubic Cu2O, respectively, while the original characteristic diffraction peaks of anatase TiO2 do not change significantly, which indicates that TiO2 and Cu2O are successfully compounded.
[0047] The titanium dioxide / cuprous oxide heterojunction material prepared in Example 1 was subjected to a photolysis water hydrogen production experiment. The specific steps are as follows: 20 mg of the titanium dioxide / cuprous oxide heterojunction material prepared in Example 1 was added to a mixed solution of 90 mL H2O and 10 mL methanol, and transferred to a glass reaction container after ultrasonic dispersion. Before the reaction started, the system was evacuated to a vacuum. During the entire test process, the reaction liquid needed to be continuously stirred, and the condensed water was continuously circulated in the hydrogen production device. The generated H2 was detected and analyzed by an Agilent 7890A gas chromatograph (GC) with a thermal conductivity detector (TCD).
[0048] Figure 4 This is a graph of the rate of hydrogen production from photolysis of titanium dioxide / cuprous oxide heterojunction material prepared in Example 1. It can be seen that TiO2 / Cu2O has excellent performance, with a hydrogen production rate of 5.02 mmol g -1 h -1 This is because the introduction of Cu2O enhances the light absorption performance of the catalyst, and the existence of the np homojunction promotes the photocatalytic performance. The catalyst synthesized by the in situ growth method forms a certain chemical bond between TiO2 and Cu2O, that is, a heterojunction structure is formed between p-TiO2 and Cu2O. The existence of this structure is conducive to the separation of electrons at the interface between p-TiO2 and Cu2O.
[0049] Comparative Example 1
[0050] The difference between Comparative Example 1 and Example 1 is that steps (5) to (8) are not performed, and titanium dioxide TiO2 with an np-type homojunction is directly obtained as Comparative Example 1.
[0051] The photolysis of water to produce hydrogen experiment in Comparative Example 1 was carried out with reference to Example 1, except that the titanium dioxide / cuprous oxide heterojunction material prepared in Example 1 was replaced by titanium dioxide TiO2 having an np-type homojunction.
[0052] Example 2
[0053] A titanium dioxide / cuprous oxide heterojunction material is prepared by the following method:
[0054] (1) Dissolve 0.1 g TiO2-As in 26 ml anhydrous ethanol, disperse by ultrasonication and stir for 10 min;
[0055] (2) Add 8.6 ml of glycerol to the mixed solution obtained in step (1), stir for 30 min, then add 0.86 g of tetrabutyl titanate, and stir for 30 min;
[0056] (3) transferring the mixed solution obtained in step (2) into a polytetrafluoroethylene-lined autoclave and reacting at 180° C. for 12 h;
[0057] (4) After cooling to room temperature, the product was washed with ethanol and dried, and then calcined in air at 470°C for 2 h to obtain titanium dioxide TiO2 with an np-type homojunction;
[0058] (5) 30 mL of anhydrous ethanol was added to a container, 0.14 g of copper acetate was added, and ultrasonic dissolution was performed. Then 0.4 g of polyvinyl pyrrolidone (K30) was added, and ultrasonic dissolution was performed. The mixture was stirred at a constant temperature of 40° C. for 10 min to obtain a mixed solution.
[0059] (6) adding 0.2 g of titanium dioxide TiO2 having an np-type homojunction to the mixed solution obtained in step (5), stirring at a constant temperature of 40° C. for 30 min to obtain a precursor solution;
[0060] (7) Add 10 mL of 0.2 mol / L glucose solution to the precursor solution obtained in step (6), and add 0.4 g of sodium hydroxide after 1 min. After precipitation, ultrasonic treatment is performed for 4 min, and the mixture is washed alternately with ethanol and deionized water and dried at 60° C. for 2 h to obtain a titanium dioxide / cuprous oxide heterojunction material TiO2 / Cu2O. The theoretical mass ratio of TiO2 to Cu2O in the sample is 4:1.
[0061] Example 3
[0062] A titanium dioxide / cuprous oxide heterojunction material is prepared by the following method:
[0063] (1) Dissolve 0.1 g TiO2-As in 26 ml anhydrous ethanol, disperse by ultrasonication and stir for 10 min;
[0064] (2) Add 8.6 ml of glycerol to the mixed solution obtained in step (1), stir for 30 min, then add 0.86 g of tetrabutyl titanate, and stir for 30 min;
[0065] (3) transferring the mixed solution obtained in step (2) into a polytetrafluoroethylene-lined autoclave and reacting at 180° C. for 12 h;
[0066] (4) After cooling to room temperature, the product was washed with ethanol and dried, and then calcined in air at 470°C for 2 h to obtain titanium dioxide TiO2 with an np-type homojunction;
[0067] (5) 30 mL of anhydrous ethanol was added to a container, 0.14 g of copper acetate was added, and ultrasonic dissolution was performed. Then 0.4 g of polyvinyl pyrrolidone (K30) was added, and ultrasonic dissolution was performed. The mixture was stirred at a constant temperature of 40° C. for 10 min to obtain a mixed solution.
[0068] (6) adding 0.30 g of titanium dioxide TiO2 having an np-type homojunction to the mixed solution obtained in step (5), stirring at a constant temperature of 40° C. for 30 min, to obtain a precursor solution;
[0069] (7) Add 10 mL of 0.2 mol / L glucose solution to the precursor solution obtained in step (6), and add 0.4 g of sodium hydroxide 1 min later. After precipitation, ultrasonic treatment is performed for 4 min. The solid product is washed alternately with ethanol and deionized water and then dried at 60° C. for 2 h to obtain a titanium dioxide / cuprous oxide heterojunction material TiO2 / Cu2O. The theoretical mass ratio of TiO2 to Cu2O in the sample is 6:1.
[0070] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and changes without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for preparing a titanium dioxide / cuprous oxide heterojunction material, It is characterized in that The following steps are involved: 1) dissolving amorphous titanium dioxide in anhydrous ethanol, dispersing it uniformly by ultrasonication, then adding glycerol and stirring it uniformly, and then adding tetrabutyl titanate and stirring it thoroughly and dispersing it uniformly; 2) transferring the mixed solution obtained in step 1) into a reaction kettle, sealing and reacting at 170-190° C. for 10-15 h, cooling to room temperature, separating the solid product, washing and drying; 3) The solid product obtained in step 2) is calcined in air at 450-500°C for 1.5-2.5h to obtain titanium dioxide TiO with np-type homojunction. 2 Branched structure; 4) dissolving cupric acetate in anhydrous ethanol, then adding polyvinyl pyrrolidone and mixing evenly to obtain a mixed solution; 5) Add titanium dioxide TiO2 having an np-type homojunction to the mixed solution obtained in step 4) 2 The branched structure is stirred evenly at a constant temperature of 30-50°C to obtain a precursor solution; 6) Glucose solution is added to the precursor solution obtained in step 5), and sodium hydroxide is added after mixing evenly to produce precipitation, followed by ultrasonic treatment, and then washed alternately with alcohol and water and dried to obtain a titanium dioxide / cuprous oxide heterojunction material.
2. A method for preparing a titanium dioxide / cuprous oxide heterojunction material according to claim 1, It is characterized in that In step 1), TiO 2 The addition concentration of -As is 2-6 mg / mL, the volume ratio between glycerol and anhydrous ethanol is 1:(2-4), and the addition concentration of tetrabutyl titanate is 20-30 mg / mL.
3. A method for preparing a titanium dioxide / cuprous oxide heterojunction material according to claim 1, It is characterized in that In step 4), the concentration of copper acetate added in anhydrous ethanol is 3-6 mg / mL, and the concentration of polyvinyl pyrrolidone added is 10-15 mg / mL.
4. The method for preparing a titanium dioxide / cuprous oxide heterojunction material according to claim 1, It is characterized in that Step 4) Stirring at a constant temperature of 30-50°C for 5-15 minutes to achieve uniform mixing.
5. The method for preparing a titanium dioxide / cuprous oxide heterojunction material according to claim 1, It is characterized in that In step 5), titanium dioxide TiO having an np-type homojunction 2 The addition concentration of the dendritic structure is 5-10 mg / mL.
6. The method for preparing a titanium dioxide / cuprous oxide heterojunction material according to claim 1, It is characterized in that In step 6), the concentration of the glucose solution is 0.1-0.3 mol / L; the volume ratio between the glucose solution and the precursor solution is 1:(2-4).
7. The method for preparing a titanium dioxide / cuprous oxide heterojunction material according to claim 1, It is characterized in that In step 6), the concentration of sodium hydroxide added to the mixed solution of the glucose solution and the precursor solution is 8-12 mg / mL.
8. The method for preparing a titanium dioxide / cuprous oxide heterojunction material according to claim 1, It is characterized in that The preparation method of amorphous titanium dioxide comprises the following steps: (1) Add titanium dioxide P25 to deionized water at a concentration of 4-6 mg / mL and stir until a milky white solution is obtained; (2) transferring the mixed solution obtained in step (1) into a reaction kettle, placing it at 170-190° C. and sealing it for reaction for 45-50 hours. After cooling to room temperature, the obtained solid product was washed with deionized water and then dried; (3) Grinding the solid product obtained in step (2) and dissolving it in dilute hydrochloric acid, ultrasonically stirring for 20-30 hours and then filtering, dissolving the product in dilute hydrochloric acid again, repeating ultrasonic stirring and filtering, and finally washing with deionized water and drying to obtain amorphous titanium dioxide TiO 2 -As; wherein the concentration of dilute hydrochloric acid is 0.05-0.2 mol / L.
9. Titanium dioxide / cuprous oxide heterojunction material prepared by the method of any one of claims 1 to 8, It is characterized in that TiO with np-type homojunction 2 The dendrite structure is used as a carrier to introduce p-type semiconductor catalyst Cu 2 O nanoparticles, forming an npp-type ternary heterojunction material in space; among them, TiO 2 With Cu 2 The theoretical mass ratio of O is (4-6):
1.
10. Use of the titanium dioxide / cuprous oxide heterojunction material according to claim 9 as a photocatalyst in the field of photocatalytic hydrogen production.
Citation Information
Patent Citations
Preparation method of graphene / titanium dioxide composite photocatalyst
CN101890344A
Preparation method of cubic cuprous oxide / graphene nanocomposite
CN105664943A
Oxygen vacancy promoted direct Z mechanism mesoporous Cu2O / TiO2 photocatalyst and preparation method thereof
CN112958061A
Copper-titanium heterojunction photocatalyst as well as preparation method and application thereof
CN113198469A
Porous titanium dioxide-cuprous oxide composite material as well as preparation method and application thereof
CN113694925A
Cited By
Same-metal double-oxide loaded noble metal catalyst as well as preparation method and application thereof
CN119800435A
A metal double oxide supported noble metal catalyst and its preparation method and application
CN119800435B
TiO2 / CNQDs / fluorescein composite photocatalyst as well as preparation method and application thereof
CN122057578A
TiO2 / CNQDs / fluorescein composite photocatalyst and preparation method and application thereof
CN122057578B