Heterogeneous double-effect catalyst as well as preparation method and application thereof
By externally loading vanadium pentoxide and tungsten trioxide on hollow mesoporous titanium dioxide nano microspheres and internally loading copper oxide, the problem of low synergistic removal efficiency of NOx and VOCs in flue gas in the steel industry is solved, and the problem of low efficiency of NOx and VOCs in the steel industry is achieved. Highly efficient and low-cost catalytic performance.
Patent Information
- Application Number
- CN202410926090.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art has low efficiency in the synergistic removal of NOx and VOCs in flue gas in the steel industry, and traditional catalyst equipment is complex, large in area and high in cost.
Using an exosite dual-effect catalyst, hollow mesoporous titanium dioxide nano microspheres were prepared through step-by-step reaction, with externally loaded vanadium pentoxide and tungsten trioxide and internally loaded copper oxide to achieve coordinated removal of NOx and VOCs.
The removal efficiency of NOx and VOCs is improved, the equipment complexity and cost are reduced, and efficient coordinated removal is achieved at low temperatures.
Smart Images

Figure CN118925741A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of environmental catalysis, and in particular to an exotic dual-effect catalyst and a preparation method and application thereof. Background Art
[0002] NO and volatile organic compounds (VOCs) are widely present in the flue gas of the steel industry. Under light conditions, they undergo photochemical reactions to generate O 3 and SOA. Currently, the mainstream NO x The control method is NH 3 Selective Catalytic Reduction of NO x (NH 3 -SCR) technology, the core of which is to use NO x Catalysts with high removal effects, such as vanadium tungsten titanium (VWT) catalysts, have mature commercial applications. Volatile organic compounds are organic compounds with boiling points between 50-260°C. In industry, they often exist in the form of benzene series such as toluene or olefins and ketones. Conventional metal oxide catalysts, such as V, Cu, Ce, and Mn, have low efficiency in removing VOCs simultaneously in the SCR temperature range, and a large amount of organic by-products are generated. Therefore, a highly efficient NO x It has become a challenging task to develop a catalyst with high performance for the simultaneous removal of VOCs.
[0003] CN107970948A discloses a honeycomb catalyst for simultaneous denitration and de-VOCs of flue gas and a preparation method thereof. The catalyst of the invention uses metatitanic acid and refined palygorskite as carriers, copper oxide, manganese oxide, and vanadium oxide as active substances, and cobalt oxide as an active auxiliary agent; the catalyst of the invention can simultaneously denitrate and de-VOCs the flue gas, and the absorbent can simultaneously and efficiently purify dust, SO in the flue gas in one set of equipment. 2 、NO x and VOCs and other pollutants, but the invention has the disadvantages of complex equipment, large footprint, high investment and operating costs.
[0004] CN117225427A discloses a method for removing NO by magnetic field enhancement x An integral catalyst for removing VOCs and its preparation method and application, the preparation method of the catalyst comprising: (1) hydrothermal synthesis of catalyst powder; (2) magnetic rod modification; (3) preparation of an integral catalyst. The active component of the catalyst accounts for 7-10% of the carrier mass, and ferric oxide accounts for 10-15% of the carrier mass; and the mass ratio of cerium oxide, manganese oxide and praseodymium oxide in the active components is 3-4:2-3:2-3. However, the removal efficiency of NO and toluene using the above catalyst in the invention still needs to be further improved.
[0005] CN112774687A discloses a SCR catalyst for synergistically removing NO and VOCs and a preparation method thereof. The SCR catalyst of the invention is composed of V 2 O 5 -WO 3 / TiO 2 The catalyst is doped with iron oxide. The preparation method of the SCR catalyst of the invention includes the following steps: adding titanium dioxide, ammonium metavanadate, ammonium metatungstate and soluble iron salt into water, adding oxalic acid and stirring, then evaporating and removing water, and then calcining the obtained solid product to obtain the SCR catalyst. However, the effect of the SCR catalyst of the invention in synergistically removing NO and VOCs needs to be improved.
[0006] In view of the shortcomings of existing technologies, it is urgent to provide a method that can efficiently and synergistically remove VOCs and NO x And a catalyst with excellent catalytic performance. Summary of the invention
[0007] The purpose of the present invention is to provide a heterogeneous dual-effect catalyst and its preparation method and application, and to prepare a heterogeneous dual-effect catalyst of hollow nano-microspheres with external loading of vanadium pentoxide and tungsten trioxide and internal loading of copper oxide through step-by-step reaction, and the prepared catalyst is used for VOCs and NO x Synergistic removal, with good catalytic performance.
[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a heterogeneous dual-effect catalyst, the heterogeneous dual-effect catalyst comprising hollow mesoporous titanium dioxide nano-microspheres, the spherical shell of the hollow mesoporous titanium dioxide nano-microspheres is loaded with vanadium pentoxide and tungsten trioxide on the outside, and the spherical shell of the hollow mesoporous titanium dioxide nano-microspheres is loaded with copper oxide on the inside;
[0010] The loading amount of vanadium pentoxide on the hollow mesoporous titanium dioxide nanospheres is 1-5wt%, for example, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0011] The loading amount of tungsten trioxide on the hollow mesoporous titanium dioxide nanospheres is 5-20wt%, for example, it can be 5wt%, 5.5wt%, 10wt%, 14.7wt%, 17.6wt%, 19.6wt% or 20wt%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0012] The loading amount of the copper oxide on the hollow mesoporous titanium dioxide nanospheres is 1-3wt%, for example, it can be 1wt%, 1.4wt%, 1.8wt%, 2.2wt%, 2.6wt% or 3wt%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0013] The heterogeneous dual-effect catalyst provided by the present invention uses hollow mesoporous titanium dioxide nano-microspheres as carriers, and loads the vanadium pentoxide active component on the outside of the spherical shell of the carrier, the tungsten trioxide auxiliary agent is also loaded on the outside of the spherical shell of the carrier, and the copper oxide active component is loaded on the inside of the spherical shell of the carrier. Compared with traditional catalysts, the present invention loads different active components of the catalyst at different positions inside and outside the catalyst, so that the SCR reaction area and the VOCs removal area are separated, thereby effectively improving the removal efficiency of the catalyst for the two pollutants.
[0014] In a second aspect, the present invention provides a method for preparing the heterogeneous dual-effect catalyst as described in the first aspect, the preparation method comprising the following steps:
[0015] (1) mixing an alkali agent, a first solvent, ethanol and a silicon precursor, and then centrifuging and washing the mixture to obtain a silicon dioxide precipitate;
[0016] (2) dispersing the silicon dioxide precipitate obtained in step (1) in a copper nitrate solution, and then evaporating and first calcining to obtain a copper silicon template powder;
[0017] (3) dispersing the copper-silicon template powder obtained in step (2) in ethanol, and then mixing it with a surfactant and a second solvent to obtain a dispersed turbid liquid;
[0018] (4) injecting the ethanol solution of the titanium precursor into the dispersed turbid liquid obtained in step (3), and then centrifuging, washing and calcining in sequence after refluxing in a water bath to obtain a silicon-titanium precursor;
[0019] (5) dispersing the silicon-titanium precursor obtained in step (4) in a vanadium and tungsten solution, evaporating and performing a third calcination in a water bath to obtain a vanadium-titanium-copper precursor;
[0020] (6) mixing the alkaline solution with the vanadium-titanium-copper precursor obtained in step (5) and etching, and then centrifuging and washing for the third time to obtain the heterogeneous dual-effect catalyst.
[0021] The present invention comprises the following steps: impregnating a copper active component precursor on a spherical silica hard template to obtain a copper-silicon hard template; wrapping a titanium precursor on the copper-silicon hard template to generate a spherical silicon-titanium precursor; impregnating the silicon-titanium precursor with vanadium and tungsten active components to obtain a vanadium-titanium-copper precursor; etching the vanadium-titanium-copper precursor in an alkaline solution to remove the silica template to obtain an exotic dual-effect catalyst containing vanadium and tungsten on the outside and copper on the inside.
[0022] Preferably, the alkaline agent in step (1) comprises any one of sodium hydroxide, aqueous ammonia or urea, or a combination of at least two of them. Typical but non-limiting combinations include a combination of sodium hydroxide and aqueous ammonia, a combination of aqueous ammonia and urea, or a combination of sodium hydroxide, aqueous ammonia and urea.
[0023] Preferably, the concentration of the aqueous ammonia is 10-30wt%, for example, 10wt%, 14wt%, 18wt%, 22wt%, 26wt% or 30wt%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0024] Preferably, in step (1), the first solvent comprises deionized water.
[0025] Preferably, the silicon precursor in step (1) comprises any one of tetraethyl silicate, tetramethyl silicate, silicon tetrachloride or silicic acid, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of tetraethyl silicate and tetramethyl silicate, a combination of tetraethyl silicate, tetramethyl silicate and silicic acid, a combination of silicon tetrachloride and silicic acid, or a combination of tetraethyl silicate, tetramethyl silicate, silicon tetrachloride and silicic acid.
[0026] Preferably, the mass volume ratio of the alkali agent to ethanol in step (1) is (10-20) g:100 mL, for example, it can be 10:100, 12:100, 15:100, 16:100, 18:100 or 20:100, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0027] Preferably, in step (1), the mass volume ratio of the first solvent to ethanol is (2-8) g:100 mL, for example, 2:100, 3:100, 4:100, 5:100, 6:100, 7:100 or 8:100, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0028] Preferably, the mass volume ratio of the silicon precursor to ethanol in step (1) is (8-15) g:100 mL, for example, it can be 8:100, 9:100, 10:100, 11.5:100, 12:100, 13:100, 14:100 or 15:100, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0029] In the preparation method provided by the present invention, the silicon precursor in step (1) is hydrolyzed in a solution to generate a silicon dioxide spherical template.
[0030] Preferably, the concentration of the copper nitrate solution in step (2) is 0.08-0.15 g / L, for example, 0.08 g / L, 0.09 g / L, 0.1 g / L, 0.11 g / L, 0.12 g / L, 0.13 g / L, 0.14 g / L or 0.15 g / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0031] Preferably, the copper content in the copper silicon template powder in step (2) is 1-3wt%, for example, it can be 1wt%, 1.5wt%, 2wt%, 2.5wt% or 3wt%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0032] Preferably, the evaporation in step (2) comprises rotary evaporation.
[0033] The present invention has no special requirement on the time of the rotary evaporation, as long as the liquid in the mixed liquid can be evaporated to dryness.
[0034] Preferably, the temperature of the first calcination in step (2) is 400-800°C, for example, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C or 800°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0035] Preferably, the first calcination time in step (2) is 2.5-5 h, for example, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h or 5 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0036] In the preparation method provided by the present invention, the copper nitrate in the copper nitrate solution in step (2) is decomposed into copper oxide on the silicon dioxide precipitate during the calcination process and is impregnated on the surface of the copper silicon template powder.
[0037] Preferably, the mass volume ratio of the copper silicon template powder to ethanol in step (3) is 1g:(20-50)mL, for example, it can be 1g:20mL, 1g:25mL, 1g:30mL, 1g:35mL, 1g:40mL, 1g:45mL or 1g:50mL, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0038] Preferably, the surfactant in step (3) comprises hydroxypropyl cellulose and / or polyether P123.
[0039] Preferably, the mass ratio of the surfactant to the copper silicon template powder in step (3) is (8-10):100, for example, it can be 8:100, 8.5:100, 9:100, 9.5:100 or 10:100, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0040] Preferably, in step (3), the second solvent comprises deionized water.
[0041] Preferably, in step (3), the mass ratio of the second solvent to ethanol is (1-5):100, for example, 1:100, 2:100, 3:100, 4:100 or 5:100, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0042] Preferably, the titanium precursor in step (4) comprises tetrabutyl titanate and / or titanium tetrachloride.
[0043] Preferably, the mass ratio of the titanium precursor in the ethanol solution of the titanium precursor in step (4) to the copper silicon template powder in the dispersed turbid solution is (150-250):100, for example, it can be 150:100, 180:100, 200:100, 220:100, 230:100 or 250:100, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0044] Preferably, the water bath reflux temperature in step (4) is 70-78°C, for example, 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C or 78°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0045] Preferably, the water bath reflux time in step (4) is 2.5-5 h, for example, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h or 5 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0046] In the present invention, the function of water bath reflux is to hydrolyze the titanium precursor into titanium hydroxide, which is produced on the surface of the silicon dioxide template under the action of a surfactant.
[0047] Preferably, the temperature of the second calcination in step (4) is 500-800°C, for example, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C or 800°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0048] Preferably, the second calcination time in step (4) is 2.5-5 h, for example, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h or 5 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0049] The second calcination of the present invention is to pyrolyze the titanium hydroxide obtained by hydrolysis into titanium dioxide, while forming a certain crystal form and voids in the catalyst and increasing the mechanical strength of the catalyst. If the calcination temperature is too high, the titanium dioxide will be transformed from the anatase phase to the rutile phase, and if the calcination temperature is too low, part of the titanium dioxide will still be titanium hydroxide, so the calcination temperature needs to be controlled within a reasonable range.
[0050] Preferably, the vanadium and tungsten solutions in step (5) include a combination of an ammonium metavanadate solution and an ammonium metatungstate solution or a combination of a vanadium hydroxide solution and a tungsten trioxide solution.
[0051] Preferably, the mass ratio of the vanadium precursor to the silicon-titanium precursor in the vanadium-tungsten solution in step (5) is (1-5):100, for example, it can be 1:100, 2:100, 3:100, 4:100 or 5:100, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0052] Preferably, the mass ratio of the tungsten precursor to the silicon-titanium precursor in the vanadium-tungsten solution in step (5) is (5-20):100, for example, it can be 5:100, 8:100, 10:100, 15:100 or 20:100, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0053] Preferably, the temperature of the water bath in step (5) is 50-80°C, for example, 50°C, 60°C, 70°C, 80°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0054] Preferably, the water bath time in step (5) is 1-3 h, for example, 1 h, 1.5 h, 2 h, 2.5 h or 3 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0055] Preferably, the temperature of the third calcination in step (5) is 500-800°C, for example, 500°C, 600°C, 700°C, 800°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0056] If the temperature of the third calcination in the present invention is too low, vanadium and copper crystals cannot be formed. If the temperature is too high, the titanium dioxide crystal phase will be transformed and vanadium and copper crystals will aggregate. Therefore, the temperature of the third calcination needs to be controlled within a reasonable range.
[0057] Preferably, the time of the third calcination in step (5) is 2.5-5 h, for example, 2.5 h, 3 h, 3.5 h, 4 h or 5 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0058] Preferably, the alkali solution in step (6) comprises sodium hydroxide solution.
[0059] Preferably, the concentration of the sodium hydroxide solution is 0.5-4 mol / L, for example, 0.5 mol / L, 1 mol / L, 2 mol / L, 3 mol / L or 4 mol / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0060] Preferably, the amount of sodium hydroxide solution added is 50-400 mL, for example, 50 mL, 100 mL, 150 mL, 200 mL, 250 mL, 300 mL, 350 mL or 400 mL, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0061] Preferably, the etching temperature in step (6) is 50-90°C, for example, it can be 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C or 90°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0062] Preferably, the etching time in step (6) is 4-24 hours, for example, it can be 4 hours, 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0063] The etching step in the present invention can remove the silicon dioxide spherical template inside the vanadium titanium copper precursor to obtain a spherical shell titanium dioxide carrier; during the etching process, copper oxide remains inside the spherical shell titanium dioxide carrier.
[0064] In the present invention, if the etching temperature is too high, the externally loaded vanadium and tungsten species will be destroyed, and if the temperature is too low, the etching will be incomplete, and the copper-silicon template will remain inside the catalyst. Therefore, the etching temperature range needs to be strictly controlled.
[0065] Preferably, the endpoint of the third washing in step (6) is to make the washing liquid neutral.
[0066] It should be noted that the preparation method provided by the present invention does not limit the amount of ethanol used, as long as it can satisfy the requirement of completely immersing the carrier; the present invention does not limit the specific process of the first washing and the second washing, as long as the material can be cleaned.
[0067] As a preferred technical solution of the preparation method of the present invention, the preparation method comprises the following steps:
[0068] (1) mixing an alkali agent, a first solvent, ethanol and a silicon precursor, and then centrifuging and washing for the first time to obtain a silicon dioxide precipitate; the mass volume ratio of the alkali agent to the ethanol is (10-20) g:100 mL; the mass volume ratio of the first solvent to the ethanol is (2-8) g:100 mL; the mass volume ratio of the silicon precursor to the ethanol is (8-15) g:100 mL;
[0069] (2) dispersing the silicon dioxide precipitate obtained in step (1) in a copper nitrate solution having a concentration of 0.08-0.15 g / L, and then performing rotary evaporation and a first calcination at 400-800° C. for 2.5-5 h to obtain a copper silicon template powder having a copper content of 1-3 wt %;
[0070] (3) dispersing the copper-silicon template powder obtained in step (2) in ethanol, and then mixing with a surfactant and a second solvent to obtain a dispersed turbid liquid; the mass volume ratio of the copper-silicon template powder to ethanol is 1 g: (20-50) mL; the mass ratio of the surfactant to the copper-silicon template powder is (8-10): 100; the mass ratio of the second solvent to ethanol is (1-5): 100;
[0071] (4) injecting the ethanol solution of the titanium precursor into the dispersed turbid liquid obtained in step (3), and then refluxing in a water bath at 70-78° C. for 2.5-5 h, centrifuging, washing for the second time, and calcining for the second time at 500-800° C. for 2.5-5 h in sequence to obtain a silicon-titanium precursor; the mass ratio of the titanium precursor in the ethanol solution of the titanium precursor to the copper-silicon template powder in the dispersed turbid liquid is (150-250):100;
[0072] (5) dispersing the silicon-titanium precursor obtained in step (4) in a vanadium and tungsten solution, and then evaporating it in a water bath at 50-80° C. for 1-3 hours and calcining it for the third time at 500-800° C. for 2.5-5 hours to obtain a vanadium-titanium-copper precursor; the mass ratio of the vanadium precursor to the silicon-titanium precursor in the vanadium and tungsten solution is (1-5):100; the mass ratio of the tungsten precursor to the silicon-titanium precursor in the vanadium and tungsten solution is (5-20):100;
[0073] (6) Mix 50-400 mL of a 0.5-4 mol / L sodium hydroxide solution with the vanadium titanium copper precursor obtained in step (5) and etch at 50-90° C. for 4-24 h, then centrifuge and wash for the third time until the washing liquid is neutral to obtain the heterogeneous dual-effect catalyst.
[0074] In a third aspect, the present invention provides an application of the heterogeneous dual-effect catalyst as described in the first aspect, wherein the heterogeneous dual-effect catalyst is used to catalyze an SCR reaction and coordinate catalytic oxidation of toluene;
[0075] The temperature of the SCR reaction in coordination with the catalytic oxidation of toluene is 100-400°C, for example, 100°C, 200°C, 300°C or 400°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0076] The heterogeneous dual-effect catalyst provided by the present invention can simultaneously achieve the degradation of VOCs and NO at low temperature. x Efficient removal.
[0077] Compared with the prior art, the present invention has the following beneficial effects:
[0078] (1) The heterogeneous dual-effect catalyst provided by the present invention uses hollow mesoporous titanium dioxide nano-microspheres as carriers, and loads the vanadium pentoxide active component on the outside of the spherical shell of the carrier, the tungsten trioxide auxiliary agent is also loaded on the outside of the spherical shell of the carrier, and the copper oxide active component is loaded on the inside of the spherical shell of the carrier. Compared with the traditional catalyst, the present invention loads different active components of the catalyst at different positions inside and outside the catalyst, so that the SCR reaction area and the VOCs removal area are separated, avoiding competitive adsorption on the catalyst, thereby effectively improving the catalyst's VOCs and NO x removal efficiency;
[0079] (2) The present invention can prepare a heterogeneous dual-effect catalyst having a hollow microsphere morphology with external loading of vanadium and tungsten and internal loading of copper oxide through a multi-step reaction, and the prepared catalyst is used for VOCs and NO x Synergistic removal, with good catalytic performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0080] Figure 1 is a TEM image of the heterogeneous dual-effect catalyst provided in Example 1 of the present invention;
[0081] Figure 2 yes Figure 1 A partial enlarged view of the middle-lined area;
[0082] Figure 3 is an elemental analysis diagram of the heterogeneous dual-effect catalyst provided in Example 1 of the present invention;
[0083] Figure 4 It is the XRD diagram of the heterogeneous dual-effect catalyst provided in Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3 of the present invention;
[0084] Figure 5 NH is the heterogeneous dual-effect catalyst provided in Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3 of the present invention. 3 -TPD graph. DETAILED DESCRIPTION
[0085] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0086] Example 1
[0087] This embodiment provides a heterogeneous dual-effect catalyst, which includes hollow mesoporous titanium dioxide nano-microspheres, wherein the spherical shell of the hollow mesoporous titanium dioxide nano-microspheres is loaded with vanadium pentoxide and tungsten trioxide, and the spherical shell of the hollow mesoporous titanium dioxide nano-microspheres is loaded with copper oxide;
[0088] The loading amount of vanadium pentoxide on the hollow mesoporous titanium dioxide nano-microspheres is 3wt%; the loading amount of tungsten trioxide on the hollow mesoporous titanium dioxide nano-microspheres is 5wt%; and the loading amount of copper oxide on the hollow mesoporous titanium dioxide nano-microspheres is 1wt%.
[0089] The preparation method of the heterogeneous dual-effect catalyst comprises the following steps:
[0090] (1) mixing ammonia water, deionized water, ethanol and tetraethyl silicate with a concentration of 28 wt%, and then centrifuging and washing for the first time to obtain a silicon dioxide precipitate; the mass volume ratio of the ammonia water to the ethanol is 15 g:100 mL; the mass volume ratio of the deionized water to the ethanol is 5 g:100 mL; the mass volume ratio of the tetraethyl silicate to the ethanol is 11.5 g:100 mL;
[0091] (2) dispersing the silicon dioxide precipitate obtained in step (1) in a copper nitrate solution having a concentration of 0.1 g / L, and then performing rotary evaporation and a first calcination at 600° C. for 3.5 h to obtain a copper silicon template powder having a copper content of 2 wt%;
[0092] (3) dispersing the copper-silicon template powder obtained in step (2) in ethanol, and then mixing with hydroxypropyl cellulose and deionized water to obtain a dispersed turbid liquid; the mass volume ratio of the copper-silicon template powder to ethanol is 1 g:35 mL; the mass ratio of the hydroxypropyl cellulose to the copper-silicon template powder is 9:100; and the mass ratio of the deionized water to ethanol is 3:100;
[0093] (4) injecting the ethanol solution of tetrabutyl titanate into the dispersed turbid liquid obtained in step (3), and then refluxing in a water bath at 75° C. for 3.5 hours, centrifuging, washing for the second time, and calcining for the second time at 600° C. for 3 hours in sequence to obtain a silicon-titanium precursor; the mass ratio of tetrabutyl titanate in the ethanol solution of tetrabutyl titanate to the copper-silicon template powder in the dispersed turbid liquid is 200:100;
[0094] (5) dispersing the silicon-titanium precursor obtained in step (4) in a mixed solution of ammonium metavanadate and ammonium metatungstate, and then evaporating and calcining for the third time at 600°C for 3.5h after being in a water bath at 60°C for 2h to obtain a vanadium-titanium-copper precursor; the mass ratio of ammonium metavanadate to the silicon-titanium precursor in the mixed solution of ammonium metavanadate and ammonium metatungstate is 3:100; the mass ratio of ammonium metatungstate to the silicon-titanium precursor in the mixed solution of ammonium metavanadate and ammonium metatungstate is 10:100;
[0095] (6) Mix 100 mL of 2 mol / L sodium hydroxide solution with the vanadium titanium copper precursor obtained in step (5) and etch at 70° C. for 12 h, then centrifuge and wash for the third time until the washing liquid is neutral to obtain the heterogeneous dual-effect catalyst.
[0096] The TEM image of the heterogeneous dual-effect catalyst is as follows: Figure 1 As shown, Figure 1 The enlarged view of the area underlined in the figure is as follows: Figure 2 The elemental analysis of the heterogeneous dual-effect catalyst is shown in Figure 3 As shown in the figure, it can be seen that the supported components are highly dispersed on the catalyst without forming clusters or other structures; the XRD pattern of the heterogeneous dual-effect catalyst is shown in Figure 4 As shown in the figure, it can be seen that the crystal phase of the titanium dioxide carrier is anatase phase, and the crystallinity of the (1 0 1) and (2 0 0) crystal planes is relatively high; 3 -TPD picture Figure 5 As shown in the figure, it can be seen that the heterogeneous dual-effect catalyst provided in this embodiment has a wide NH 3 Desorption peak, which means it has more acidic sites.
[0097] Example 2
[0098] This embodiment provides a heterogeneous dual-effect catalyst, which includes hollow mesoporous titanium dioxide nano-microspheres, wherein the spherical shell of the hollow mesoporous titanium dioxide nano-microspheres is loaded with vanadium pentoxide and tungsten trioxide, and the spherical shell of the hollow mesoporous titanium dioxide nano-microspheres is loaded with copper oxide;
[0099] The loading amount of vanadium pentoxide on the hollow mesoporous titanium dioxide nano-microspheres is 1wt%; the loading amount of tungsten trioxide on the hollow mesoporous titanium dioxide nano-microspheres is 5wt%; and the loading amount of copper oxide on the hollow mesoporous titanium dioxide nano-microspheres is 1wt%.
[0100] The preparation method of the heterogeneous dual-effect catalyst comprises the following steps:
[0101] (1) mixing ammonia water, deionized water, ethanol and tetramethyl silicate with a concentration of 10 wt%, and then centrifuging and washing for the first time to obtain a silicon dioxide precipitate; the mass volume ratio of the ammonia water to the ethanol is 10 g:100 mL; the mass volume ratio of the deionized water to the ethanol is 2 g:100 mL; the mass volume ratio of the tetramethyl silicate to the ethanol is 8 g:100 mL;
[0102] (2) dispersing the silicon dioxide precipitate obtained in step (1) in a copper nitrate solution having a concentration of 0.08 g / L, and then performing rotary evaporation and a first calcination at 400° C. for 5 h to obtain a copper silicon template powder having a copper content of 1 wt%;
[0103] (3) dispersing the copper-silicon template powder obtained in step (2) in ethanol, and then mixing with polyether P123 and deionized water to obtain a dispersed turbid liquid; the mass volume ratio of the copper-silicon template powder to ethanol is 1 g:20 mL; the mass ratio of the polyether P123 to the copper-silicon template powder is 8:100; the mass ratio of the deionized water to ethanol is 1:100;
[0104] (4) injecting the ethanol solution of tetrabutyl titanate into the dispersed turbid liquid obtained in step (3), and then centrifuging, washing for the second time, and calcining for the second time at 500° C. for 5 hours after refluxing in a water bath at 70° C., to obtain a silicon-titanium precursor; the mass ratio of tetrabutyl titanate in the ethanol solution of tetrabutyl titanate to the copper-silicon template powder in the dispersed turbid liquid is 150:100;
[0105] (5) dispersing the silicon-titanium precursor obtained in step (4) in a mixed solution of ammonium metavanadate and ammonium metatungstate, and then evaporating and calcining for the third time at 500°C for 5h after being in a water bath at 50°C for 3h to obtain a vanadium-titanium-copper precursor; the mass ratio of ammonium metavanadate to the silicon-titanium precursor in the mixed solution of ammonium metavanadate and ammonium metatungstate is 1:100; the mass ratio of ammonium metatungstate to the silicon-titanium precursor in the mixed solution of ammonium metavanadate and ammonium metatungstate is 5:100;
[0106] (6) Mix 50 mL of 4 mol / L sodium hydroxide solution with the vanadium titanium copper precursor obtained in step (5) and etch at 50° C. for 24 h, then centrifuge and wash for the third time until the washing liquid is neutral to obtain the heterogeneous dual-effect catalyst.
[0107] Example 3
[0108] This embodiment provides a heterogeneous dual-effect catalyst, which includes hollow mesoporous titanium dioxide nano-microspheres, wherein the spherical shell of the hollow mesoporous titanium dioxide nano-microspheres is loaded with vanadium pentoxide and tungsten trioxide, and the spherical shell of the hollow mesoporous titanium dioxide nano-microspheres is loaded with copper oxide;
[0109] The loading amount of vanadium pentoxide on the hollow mesoporous titanium dioxide nano-microspheres is 5wt%; the loading amount of tungsten trioxide on the hollow mesoporous titanium dioxide nano-microspheres is 20wt%; and the loading amount of copper oxide on the hollow mesoporous titanium dioxide nano-microspheres is 3wt%.
[0110] The preparation method of the heterogeneous dual-effect catalyst comprises the following steps:
[0111] (1) mixing ammonia water, deionized water, ethanol and tetraethyl silicate with a concentration of 30 wt%, and then centrifuging and washing for the first time to obtain a silicon dioxide precipitate; the mass volume ratio of the ammonia water to the ethanol is 20 g:100 mL; the mass volume ratio of the deionized water to the ethanol is 8 g:100 mL; the mass volume ratio of the tetraethyl silicate to the ethanol is 15 g:100 mL;
[0112] (2) dispersing the silicon dioxide precipitate obtained in step (1) in a copper nitrate solution having a concentration of 0.15 g / L, and then performing rotary evaporation and a first calcination at 800° C. for 2.5 h to obtain a copper silicon template powder having a copper content of 3 wt%;
[0113] (3) dispersing the copper-silicon template powder obtained in step (2) in ethanol, and then mixing with hydroxypropyl cellulose and deionized water to obtain a dispersed turbid liquid; the mass volume ratio of the copper-silicon template powder to ethanol is 1 g:50 mL; the mass ratio of the hydroxypropyl cellulose to the copper-silicon template powder is 10:100; the mass ratio of the deionized water to ethanol is 5:100;
[0114] (4) injecting the ethanol solution of tetrabutyl titanate into the dispersed turbid liquid obtained in step (3), and then centrifuging, washing for the second time, and calcining for the second time at 800° C. for 2.5 hours after refluxing in a water bath at 78° C., to obtain a silicon-titanium precursor; the mass ratio of tetrabutyl titanate in the ethanol solution of tetrabutyl titanate to the copper-silicon template powder in the dispersed turbid liquid is 250:100;
[0115] (5) dispersing the silicon-titanium precursor obtained in step (4) in a mixed solution of vanadium hydroxide and tungsten trioxide, and then evaporating the mixture in a water bath at 80° C. for 1 hour and calcining the mixture at 800° C. for a third time for 2.5 hours to obtain a vanadium-titanium-copper precursor; the mass ratio of vanadium hydroxide to the silicon-titanium precursor in the mixed solution of vanadium hydroxide and tungsten trioxide is 5:100; the mass ratio of tungsten trioxide to the silicon-titanium precursor in the mixed solution of vanadium hydroxide and tungsten trioxide is 20:100;
[0116] (6) Mix 400 mL of 0.5 mol / L sodium hydroxide solution with the vanadium titanium copper precursor obtained in step (5) and etch at 90° C. for 4 h, then centrifuge and wash for the third time until the washing liquid is neutral to obtain the heterogeneous dual-effect catalyst.
[0117] Example 4
[0118] This embodiment provides a heterogeneous dual-effect catalyst. The difference between the preparation method of the heterogeneous dual-effect catalyst and that of Embodiment 1 is that, except that the temperature of the third calcination in step (5) is adjusted to 450° C., the rest is the same as that of Embodiment 1.
[0119] Example 5
[0120] This embodiment provides a heterogeneous dual-effect catalyst. The difference between the preparation method of the heterogeneous dual-effect catalyst and that of Embodiment 1 is that, except that the temperature of the third calcination in step (5) is adjusted to 850° C., the rest is the same as that of Embodiment 1.
[0121] Example 6
[0122] This embodiment provides a heterogeneous dual-effect catalyst. The difference between the preparation method of the heterogeneous dual-effect catalyst and that of Embodiment 1 is that, except that the etching temperature in step (6) is adjusted to 40° C., the rest is the same as that of Embodiment 1.
[0123] Example 7
[0124] This embodiment provides a heterogeneous dual-effect catalyst. The difference between the preparation method of the heterogeneous dual-effect catalyst and that of Embodiment 1 is that, except that the etching temperature in step (6) is adjusted to 100° C., the rest is the same as that of Embodiment 1.
[0125] Comparative Example 1
[0126] This comparative example provides a heterogeneous dual-effect catalyst, which is different from Example 1 in that the outer shell of the hollow mesoporous titanium dioxide nanospheres is not loaded with tungsten trioxide, and ammonium metatungstate is not added in step (5) of the preparation method of the heterogeneous dual-effect catalyst. The rest is the same as Example 1.
[0127] The XRD pattern of the heterogeneous dual-effect catalyst is shown in Figure 4As shown in the figure, it can be seen that the heterogeneous dual-effect catalyst provided in this comparative example also presents the spectrum peak of anatase titanium dioxide; NH 3 -TPD picture Figure 5 As shown in the figure, it can be seen that the high temperature section NH 3 The desorption amount is reduced and the medium and strong acid sites are greatly reduced.
[0128] Comparative Example 2
[0129] This comparative example provides a heterogeneous dual-effect catalyst, which is different from Example 1 in that the outer shell of the hollow mesoporous titanium dioxide nanospheres is not loaded with vanadium pentoxide, and ammonium metavanadate is not added in step (5) of the preparation method of the heterogeneous dual-effect catalyst. The rest is the same as Example 1.
[0130] The XRD pattern of the heterogeneous dual-effect catalyst is shown in Figure 4 As shown in the figure, it can be seen that the heterogeneous dual-effect catalyst provided in this comparative example also presents the spectrum peak of anatase titanium dioxide; NH 3 -TPD picture Figure 5 As shown in the figure, it can be seen that the heterogeneous dual-effect catalyst NH 3 The amount of analysis was slightly reduced, and the reduction in acidic sites was not significant.
[0131] Comparative Example 3
[0132] This comparative example provides a catalyst, which is different from Example 1 in that copper oxide is not loaded inside the shell of the hollow mesoporous titanium dioxide nanospheres, and step (2) in the preparation method is adaptively deleted. The rest is the same as Example 1.
[0133] The XRD pattern of the heterogeneous dual-effect catalyst is shown in Figure 4 As shown in the figure, it can be seen that the heterogeneous dual-effect catalyst provided in this comparative example also presents the spectrum peak of anatase titanium dioxide, but the crystallinity is less than that of Example 1, Comparative Examples 1 and 2; NH 3 -TPD picture Figure 5 As shown in the figure, it can be seen that the heterogeneous dual-effect catalyst NH 3 The amount of analysis was slightly reduced, and the reduction in acidic sites was not significant.
[0134] Comparative Example 4
[0135] This comparative example provides a catalyst, which is different from Example 1 in that the outer shell of the hollow mesoporous titanium dioxide nanospheres is not loaded with vanadium pentoxide and tungsten trioxide, and step (5) in the preparation method is adaptively deleted. The rest is the same as Example 1.
[0136] Comparative Example 5
[0137] This comparative example provides a catalyst, which differs from Example 1 in that the outer shell of the hollow mesoporous titanium dioxide nanospheres is loaded with copper oxide, step (2) in the preparation method is deleted, and step (5) is adjusted as follows: the silicon titanium precursor obtained in step (4) is dispersed in a mixed solution of ammonium metavanadate, ammonium metatungstate and copper nitrate, and then evaporated in a 60°C water bath for 2 hours and calcined for the third time at 600°C for 3.5 hours to obtain a vanadium titanium copper precursor; the mass ratio of the ammonium metavanadate to the silicon titanium precursor is 3:100; the mass ratio of the ammonium metatungstate to the silicon titanium precursor is 10:100; the mass ratio of the copper nitrate to the silicon titanium precursor is 2:100, and the rest is the same as Example 1.
[0138] The catalytic performance of the heterogeneous dual-effect catalysts provided in Examples 1-7, Comparative Examples 1 and 2, and the catalysts provided in Comparative Examples 3-5 was tested. The test conditions included: flue gas composition: [NO] = 500 ppm, [NH 3 ]=500ppm,[C 7 H 8 ]=100ppm,[O 2 ]=16vol%N 2 The catalyst dosage is 100 mg, the reactor temperature is 100-400°C, the flue gas flow rate is 200 mL / min, the maximum NO conversion rate of the catalytic SCR reaction and the reaction temperature at which the maximum conversion rate is reached are shown in Table 1, and the maximum toluene conversion rate of the catalytic toluene oxidation and the reaction temperature at which the maximum conversion rate is reached are shown in Table 2.
[0139] Table 1
[0140]
[0141]
[0142] Table 2
[0143] Maximum conversion rate of toluene / % Reaction temperature to achieve maximum conversion rate / ℃ Example 1 100 225 Example 2 100 250 Example 3 100 300 Example 4 79 400 Example 5 100 375 Example 6 55 400 Example 7 100 225 Comparative Example 1 100 250 Comparative Example 2 100 225 Comparative Example 3 100 400 Comparative Example 4 97 250 Comparative Example 5 100 250
[0144] It can be seen from Table 1 and Table 2 that the heterogeneous dual-effect catalyst provided by the present invention has excellent SCR reaction synergistic toluene catalytic oxidation activity, and can achieve efficient synergistic removal of two pollutants, NO and toluene, at 225°C;
[0145] By comparing Example 1 with Examples 4 and 5, it can be seen that if the temperature of the third calcination is too low, the active components cannot be generated, and if it is too high, the titanium dioxide will be transformed from the anatase phase to the rutile phase, thereby reducing the catalytic activity; by comparing Example 1 with Examples 6 and 7, it can be seen that if the etching temperature is too high, the externally loaded vanadium and tungsten species will be destroyed, and if the temperature is too low, the etching will be incomplete, so that the copper silicon template agent will remain inside the catalyst, thereby reducing the catalytic activity;
[0146] By comparing Example 1 with Comparative Examples 1-4, it can be seen that the outside of the spherical shell of the hollow mesoporous titanium dioxide nanospheres is not loaded with at least one of vanadium pentoxide, tungsten trioxide or copper oxide, which will significantly increase the reaction temperature for reaching the maximum conversion rate; by comparing Example 1 with Comparative Example 5, it can be seen that the activity of the heterogeneous dual-effect catalyst after separation of the active reaction areas is higher than that of the catalyst without separation of the reaction areas.
[0147] In summary, the heterogeneous dual-effect catalyst provided by the present invention uses hollow mesoporous titanium dioxide nano-microspheres as carriers, and loads the vanadium pentoxide active component on the outside of the spherical shell of the carrier, the tungsten trioxide auxiliary agent is also loaded on the outside of the spherical shell of the carrier, and the copper oxide active component is loaded on the inside of the spherical shell of the carrier. Compared with the traditional catalyst, the present invention loads different active components of the catalyst at different positions inside and outside the catalyst, so that the SCR reaction area and the VOCs removal area are separated, avoiding competitive adsorption on the catalyst, thereby effectively improving the catalyst's VOCs and NO x removal efficiency;
[0148] The present invention can prepare a heterogeneous dual-effect catalyst with a hollow microsphere morphology, which is externally loaded with vanadium and tungsten and internally loaded with copper oxide, through a multi-step reaction, and the prepared catalyst is used for VOCs and NO x Synergistic removal, with good catalytic performance.
[0149] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A heterogeneous dual-effect catalyst, It is characterized in that The heterogeneous dual-effect catalyst comprises hollow mesoporous titanium dioxide nano-microspheres, wherein the outer shell of the hollow mesoporous titanium dioxide nano-microspheres is loaded with vanadium pentoxide and tungsten trioxide, and the inner shell of the hollow mesoporous titanium dioxide nano-microspheres is loaded with copper oxide; The loading amount of vanadium pentoxide on the hollow mesoporous titanium dioxide nano-microspheres is 1-5wt%; the loading amount of tungsten trioxide on the hollow mesoporous titanium dioxide nano-microspheres is 5-20wt%; and the loading amount of copper oxide on the hollow mesoporous titanium dioxide nano-microspheres is 1-3wt%.
2. A method for preparing the heterogeneous dual-effect catalyst as claimed in claim 1, It is characterized in that The preparation method comprises the following steps: (1) mixing an alkali agent, a first solvent, ethanol and a silicon precursor, and then centrifuging and washing the mixture to obtain a silicon dioxide precipitate; (2) dispersing the silicon dioxide precipitate obtained in step (1) in a copper nitrate solution, and then evaporating and first calcining to obtain a copper silicon template powder; (3) dispersing the copper-silicon template powder obtained in step (2) in ethanol, and then mixing it with a surfactant and a second solvent to obtain a dispersed turbid liquid; (4) injecting the ethanol solution of the titanium precursor into the dispersed turbid liquid obtained in step (3), and then centrifuging, washing and calcining in sequence after refluxing in a water bath to obtain a silicon-titanium precursor; (5) dispersing the silicon-titanium precursor obtained in step (4) in a vanadium and tungsten solution, evaporating and performing a third calcination in a water bath to obtain a vanadium-titanium-copper precursor; (6) mixing the alkaline solution with the vanadium-titanium-copper precursor obtained in step (5) and etching, and then centrifuging and washing for the third time to obtain the heterogeneous dual-effect catalyst.
3. The preparation method according to claim 2, It is characterized in that The alkaline agent in step (1) includes any one of sodium hydroxide, ammonia water or urea, or a combination of at least two thereof; Preferably, in step (1), the first solvent comprises deionized water; Preferably, the silicon precursor in step (1) comprises any one of tetraethyl silicate, tetramethyl silicate, silicon tetrachloride or silicic acid, or a combination of at least two thereof; Preferably, the mass volume ratio of the alkaline agent to ethanol in step (1) is (10-20) g:100 mL; Preferably, in step (1), the mass volume ratio of the first solvent to ethanol is (2-8) g:100 mL; Preferably, the mass volume ratio of the silicon precursor to ethanol in step (1) is (8-15) g:100 mL.
4. The preparation method according to claim 2 or 3, It is characterized in that The concentration of the copper nitrate solution in step (2) is 0.08-0.15 g / L; Preferably, the copper content in the copper-silicon template powder in step (2) is 1-3wt%; Preferably, the evaporation in step (2) comprises rotary evaporation; Preferably, the temperature of the first calcination in step (2) is 400-800°C; Preferably, the first calcination time in step (2) is 2.5-5 hours.
5. The preparation method according to any one of claims 2 to 4, It is characterized in that The mass volume ratio of the copper-silicon template powder to ethanol in step (3) is 1 g: (20-50) mL; Preferably, the surfactant in step (3) comprises hydroxypropyl cellulose and / or polyether P123; Preferably, the mass ratio of the surfactant to the copper silicon template powder in step (3) is (8-10):100; Preferably, the second solvent in step (3) comprises deionized water; Preferably, in step (3), the mass ratio of the second solvent to ethanol is (1-5):
100.
6. The preparation method according to any one of claims 2 to 5, It is characterized in that The titanium precursor in step (4) includes tetrabutyl titanate and / or titanium tetrachloride; Preferably, the mass ratio of the titanium precursor in the ethanol solution of the titanium precursor in step (4) to the copper-silicon template powder in the dispersed turbid solution is (150-250):100; Preferably, the water bath reflux temperature in step (4) is 70-78°C; Preferably, the water bath reflux time in step (4) is 2.5-5h; Preferably, the temperature of the second calcination in step (4) is 500-800°C; Preferably, the second calcination time in step (4) is 2.5-5 hours.
7. The preparation method according to any one of claims 2 to 6, It is characterized in that The vanadium and tungsten solutions in step (5) include a combination of an ammonium metavanadate solution and an ammonium metatungstate solution or a combination of a vanadium hydroxide solution and a tungsten trioxide solution; Preferably, the mass ratio of the vanadium precursor to the silicon-titanium precursor in the vanadium-tungsten solution in step (5) is (1-5):100; Preferably, the mass ratio of the tungsten precursor to the silicon-titanium precursor in the vanadium-tungsten solution in step (5) is (5-20):100; Preferably, the temperature of the water bath in step (5) is 50-80°C; Preferably, the water bath time in step (5) is 1-3 hours; Preferably, the temperature of the third calcination in step (5) is 500-800°C; Preferably, the third calcination time in step (5) is 2.5-5 hours.
8. The preparation method according to any one of claims 2 to 7, It is characterized in that The alkali solution in step (6) comprises sodium hydroxide solution; Preferably, the concentration of the sodium hydroxide solution is 0.5-4 mol / L; Preferably, the amount of sodium hydroxide solution added is 50-400 mL; Preferably, the etching temperature in step (6) is 50-90° C.; Preferably, the etching time in step (6) is 4-24 hours; Preferably, the endpoint of the third washing in step (6) is to make the washing liquid neutral.
9. The preparation method according to any one of claims 2 to 8, It is characterized in that The preparation method comprises the following steps: (1) mixing an alkali agent, a first solvent, ethanol and a silicon precursor, and then centrifuging and washing for the first time to obtain a silicon dioxide precipitate; the mass volume ratio of the alkali agent to the ethanol is (10-20) g:100 mL; the mass volume ratio of the first solvent to the ethanol is (2-8) g:100 mL; the mass volume ratio of the silicon precursor to the ethanol is (8-15) g:100 mL; (2) dispersing the silicon dioxide precipitate obtained in step (1) in a copper nitrate solution having a concentration of 0.08-0.15 g / L, and then performing rotary evaporation and a first calcination at 400-800° C. for 2.5-5 h to obtain a copper silicon template powder having a copper content of 1-3 wt %; (3) dispersing the copper-silicon template powder obtained in step (2) in ethanol, and then mixing with a surfactant and a second solvent to obtain a dispersed turbid liquid; the mass volume ratio of the copper-silicon template powder to ethanol is 1 g: (20-50) mL; the mass ratio of the surfactant to the copper-silicon template powder is (8-10): 100; the mass ratio of the second solvent to ethanol is (1-5): 100; (4) injecting the ethanol solution of the titanium precursor into the dispersed turbid liquid obtained in step (3), and then refluxing in a water bath at 70-78° C. for 2.5-5 h, centrifuging, washing for the second time, and calcining for the second time at 500-800° C. for 2.5-5 h in sequence to obtain a silicon-titanium precursor; the mass ratio of the titanium precursor in the ethanol solution of the titanium precursor to the copper-silicon template powder in the dispersed turbid liquid is (150-250):100; (5) dispersing the silicon-titanium precursor obtained in step (4) in a vanadium and tungsten solution, and then evaporating it in a water bath at 50-80° C. for 1-3 hours and calcining it for the third time at 500-800° C. for 2.5-5 hours to obtain a vanadium-titanium-copper precursor; the mass ratio of the vanadium precursor to the silicon-titanium precursor in the vanadium and tungsten solution is (1-5):100; the mass ratio of the tungsten precursor to the silicon-titanium precursor in the vanadium and tungsten solution is (5-20):100; (6) Mix 50-400 mL of a 0.5-4 mol / L sodium hydroxide solution with the vanadium titanium copper precursor obtained in step (5) and etch at 50-90° C. for 4-24 h, then centrifuge and wash for the third time until the washing liquid is neutral to obtain the heterogeneous dual-effect catalyst.
10. A use of the heterogeneous dual-effect catalyst as claimed in claim 1, It is characterized in that The heterogeneous dual-effect catalyst is used to catalyze the SCR reaction and coordinate the catalytic oxidation of toluene; The temperature of the SCR reaction in coordination with the catalytic oxidation of toluene is 100-400°C.
Citation Information
Cited By
Catalyst for ammonia production through catalytic degradation of N-VOCs in cooperation with SCR denitration and preparation method and application of catalyst
CN122098567A
A catalyst for catalytic degradation of N-VOCs to produce ammonia and SCR denitration, and a preparation method and application thereof
CN122098567B
Hollow-structure catalyst for removing nitrogen oxides and chlorinated organics in reaction subareas as well as preparation method and application of hollow-structure catalyst
CN122230712A
A hollow structure catalyst for removing nitrogen oxides and chlorinated organic compounds in a reaction zone, and a preparation method and application thereof
CN122230712B