Phosphorus removal and bacteriostasis modified zeolite filler as well as preparation method and application thereof
By combining chitosan with lanthanum hydroxide and quaternized chitosan with natural zeolites, a lanthanum-chitosan-zeolite composite material was formed, and a highly efficient phosphorus removal and antibacterial modification zeolite filler was prepared, which solved the phosphorus in water. Deep removal and matrix blockage problems have achieved efficient and low-cost phosphorus removal effect.
Patent Information
- Application Number
- CN202411284471.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-13
AI Technical Summary
The prior art is costly and cannot achieve deep removal when removing phosphorus from water bodies. Traditional substrates such as sand, gravel and natural zeolites have insufficient phosphorus removal capabilities and are prone to clogging of artificial wetland substrates, limiting their application.
Using a preparation method of phosphorus removal and antibacterial modified zeolite filler, by combining chitosan with lanthanum hydroxide and quaternized chitosan with natural zeolite, lanthanum-chitosan-zeolite composite material and with cement Mixed granulation to prepare phosphorus removal and antibacterial modified zeolite filler with high efficiency adsorption and antibacterial effects.
It achieves efficient adsorption and antibacterial effects on phosphorus, solves the problem of matrix blockage, significantly improves the phosphorus removal ability and filler service life of artificial wetlands, and is suitable for the depth removal of micro-polluted water bodies.
Smart Images

Figure CN118993356A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a filler and a preparation method and application thereof, in particular to a phosphorus-removing and bacteriostatic modified zeolite filler and a preparation method and application thereof. Background Art
[0002] Phosphorus is an important nutrient for aquatic organisms such as algae. Excessive phosphorus content in water bodies will lead to eutrophication of water bodies. Eutrophication of water bodies will cause irreversible problems such as biodiversity degradation, water quality deterioration, changes in the composition and dominance of alien species. At present, phosphorus removal methods include chemical precipitation and activated sludge. These traditional treatment technologies can effectively remove phosphorus and meet discharge standards, but deep phosphorus removal requires a large amount of chemical agents, which is costly. Therefore, there is an urgent need for a low-cost, high-efficiency, pollution-free technology to remove phosphorus from water bodies.
[0003] Constructed wetlands (CWs) are a promising ecological water treatment technology. Due to their low cost, convenient operation, and landscape potential, they have been widely used in the deep removal of phosphorus from tailwater or aquatic environments in recent years. Phosphorus removal in constructed wetlands is mainly achieved by the synergistic effect of substrates, plants, and microorganisms. Among them, the role of the substrate is dominant, but traditional substrates such as sand, gravel, and natural zeolite are used to support the growth of artificial wetland plants. They usually do not have phosphorus removal capabilities or have weak phosphorus removal capabilities. In addition, the problem of the substrate being easily blocked, resulting in a short service life of the artificial wetland, still exists, limiting the application of artificial wetlands in the treatment of micro-polluted water bodies.
[0004] The basic structure of natural zeolite is silicon-oxygen tetrahedron and aluminum-oxygen tetrahedron, in which the aluminum-oxygen tetrahedron carries a negative charge. However, the adsorption effect of natural zeolite on phosphorus is not ideal. In order to improve the treatment performance, natural zeolite is usually modified. At present, most of the research on the modification of natural zeolite and its denitrification and phosphorus removal performance is aimed at enhancing the removal capacity of ammonia nitrogen, while for the adsorption of phosphate, rare earth modification represented by lanthanum hydroxide is a modification technology that has been studied more in recent years, and it can achieve removal effect even under low phosphorus concentration. However, the antibacterial effect of natural zeolite modified with rare earth alone is not significant, and it is impossible to achieve simultaneous phosphorus removal and antibacterial inhibition, and it cannot alleviate the biological clogging of artificial wetlands. Summary of the invention
[0005] Purpose of the invention: In order to overcome the deficiencies in the prior art, the purpose of the present invention is to provide a simple and convenient method for preparing a phosphorus removal and antibacterial modified zeolite filler. Another purpose of the present invention is to provide a phosphorus removal and antibacterial modified zeolite filler with fast adsorption, large adsorption capacity and good phosphorus removal and antibacterial effect. Another purpose of the present invention is to provide a phosphorus removal and antibacterial modified zeolite filler for use in phosphorus removal, adsorption and antibacterial inhibition in artificial wetlands.
[0006] Technical solution: The preparation method of a phosphorus removal and antibacterial modified zeolite filler of the present invention comprises the following steps:
[0007] Step 1, dissolving chitosan in acetic acid, stirring and mixing to dissolve, then adding dimethyldiallyl ammonium chloride solution, mixing evenly and heating to react, cooling to room temperature after the reaction, then adding acetone to generate precipitation, washing, drying and grinding into powder to obtain quaternized chitosan;
[0008] Step 2: firstly mix the natural zeolite with quaternized chitosan and water, stir evenly, then drip into a sodium hydroxide solution, wash and dry, then stir and mix evenly with lanthanum nitrate hexahydrate, adjust the pH to 11-14, stir, wash and dry; or firstly stir and mix the natural zeolite with lanthanum nitrate hexahydrate, adjust the pH to 11-14, stir, wash and dry, then mix with quaternized chitosan and water, stir evenly, then drip into a sodium hydroxide solution, wash and dry, to obtain a lanthanum-chitosan-zeolite composite material;
[0009] Step three, mixing the lanthanum-chitosan-zeolite composite material with cement to form granules, drying in the shade, steam curing, and drying to obtain phosphorus-removing and antibacterial modified zeolite filler.
[0010] Furthermore, in step 1, the mass ratio of chitosan, acetic acid and dimethyldiallyl ammonium chloride solution is 4:1:1-2. The volume percentage of dimethyldiallyl ammonium chloride in the dimethyldiallyl ammonium chloride solution is 20-25 vol%. The heating reaction temperature is 50-60° C., and the reaction time is 20-30 min.
[0011] Furthermore, in step 2, the mass ratio of natural zeolite to quaternized chitosan is 3:0.5 to 1. The concentration of lanthanum nitrate hexahydrate is 0.1 to 0.5 mol / L.
[0012] Preferably, in step 2, the natural zeolite is first stirred and mixed evenly with lanthanum nitrate hexahydrate, the pH is adjusted to 11-14, stirred, washed and dried, and then mixed with quaternized chitosan and water, stirred evenly, and then dripped into a sodium hydroxide solution, washed and dried, so as to obtain a lanthanum-chitosan-zeolite composite material with better antibacterial effect.
[0013] Furthermore, in step three, the mass ratio of the lanthanum-chitosan-zeolite composite material to cement is 2 to 8:1.
[0014] Furthermore, the washing and drying temperature is 50-60°C.
[0015] The phosphorus removal and antibacterial modified zeolite filler prepared by the method for preparing the phosphorus removal and antibacterial modified zeolite filler of the present invention.
[0016] The phosphorus removal and antibacterial modified zeolite filler of the present invention is used in phosphorus removal, adsorption and antibacterial in artificial wetlands.
[0017] Furthermore, the application specifically includes the following steps: adding the phosphorus-removing and antibacterial modified zeolite filler into a phosphate-containing solution, and fully saturating the solution in a 25° C. water bath shaker for adsorption.
[0018] Preparation principle: Chitosan is a biodegradable, non-toxic biopolymer material with low cost, broad-spectrum antibacterial properties, and active functional groups. The introduction of quaternary ammonium groups can not only enhance the ability of chitosan to remove phosphorus, but also enhance the antibacterial effect. Quaternary ammonium chitosan and metal ions have a chelating effect and are loaded on the surface of zeolite. Positively charged metal ions and functional groups can interact with negatively charged bacterial membranes through electrostatic interactions, thereby interfering with the normal physiological functions of bacteria and causing bacterial death.
[0019] Beneficial effects: Compared with the prior art, the present invention has the following significant features:
[0020] 1. The obtained filler has the advantages of being non-toxic, having strong adsorption performance and good stability. In particular, the filler has an antibacterial effect, which can not only alleviate the problem of short filler saturation time caused by matrix blockage, but also efficiently adsorb phosphorus in micro-pollution;
[0021] 2. An adsorption and phosphorus removal experiment was carried out under low concentration conditions. The experimental results showed that the removal efficiency of the phosphorus removal material was greater than 95% when the initial phosphorus concentration was 2 mg / L, and it can be used to remove phosphorus in slightly polluted water bodies. The preparation process of the present invention is simple, and the prepared material has fast adsorption and large adsorption capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 is the adsorption amount of 100 mg / L phosphate concentration by the materials prepared in Example 1, Comparative Example 1 and Comparative Example 2;
[0023] Figure 2 is the adsorption removal rate of the materials prepared in Example 1, Comparative Example 1 and Comparative Example 2 for a phosphate concentration of 2 mg / L;
[0024] Figure 3 The growth of bacteria on the surface of the materials prepared in Example 1 and Comparative Example 1 on the plate, wherein a) the control group of Comparative Example 1, b) the control group of Example 1, c) the treatment group of Example 1, d) the treatment group of Comparative Example 1;
[0025] Figure 4 are the breakthrough curves at different initial phosphate concentrations;
[0026] Figure 5It is a comparison of the antibacterial effects of the materials prepared in Example 2, Comparative Example 1, Comparative Example 2, and Comparative Example 3 (0: the antibacterial circle of the material prepared in Comparative Example 1, 1: the antibacterial circle of the material prepared in Example 2, 2: the antibacterial circle of the material prepared in Comparative Example 3, 3: the antibacterial circle of the material prepared in Comparative Example 2);
[0027] Figure 6 It is the adsorption graph of the materials prepared in Example 1, Example 2, Comparative Example 1, Comparative Example 2, and Comparative Example 3 to a phosphate concentration of 2 mg / L. DETAILED DESCRIPTION
[0028] Example 1
[0029] A method for preparing a phosphorus-removing and antibacterial modified zeolite filler comprises the following steps:
[0030] (1) Rinse the natural zeolite with distilled water repeatedly for 3 times, then soak it in distilled water for 24 hours, change the water every 4 hours to dissolve the impurities, and then dry it in a drying oven at 60°C for 12 hours. Crush the dried zeolite and put it into a container for later use.
[0031] (2) Dissolve 1g of chitosan in 50mL of 5vol% acetic acid and stir to dissolve. Slowly add 25mL of 20vol% dimethyldiallylammonium chloride solution and mix thoroughly. Immediately place the conical flask in a 55℃ constant temperature magnetic stirrer and heat for 20min. After the reaction is completed, cool to room temperature.
[0032] (3) In a fume hood, an equal volume of acetone was added to the reaction system of step (2) to generate a large amount of white flocs. After centrifugation, the flocs were washed three times with anhydrous ethanol. Finally, the product was placed in a drying oven at 60° C. and dried for 24 h. The product was taken out and ground to obtain a slightly yellow powder of quaternized chitosan.
[0033] (4) Dissolve quaternized chitosan in water to form a 10 g / L quaternized chitosan solution, add 3 g of zeolite into 50 mL of the quaternized chitosan solution, and keep stirring on a magnetic stirrer for 4 h.
[0034] (5) The solution obtained in step (4) was dripped into a 1 mol / L NaOH solution. Then, the chitosan-zeolite composite was washed with deionized water until the pH value was constant, and dried in an oven at 60° C. to prepare a chitosan-zeolite composite material.
[0035] (6) 3 g of chitosan-zeolite composite material was added to 50 mL of 0.1 mol / L (La(NO)3)3·6H2O solution and stirred to mix evenly, the pH was adjusted to 11, and stirred at room temperature for 24 h. After the reaction, the composite modified material was rinsed with deionized water and then dried in an oven at 60 °C for 24 h to obtain a lanthanum-chitosan-zeolite composite material.
[0036] (7) The lanthanum-chitosan-zeolite composite material and cement are mixed and granulated in a mass ratio of 2:1 to form spherical particles of 4 to 5 mm, which are shade-dried for 24 hours and steam-cured for 2 hours to obtain a phosphorus-removing and antibacterial modified zeolite filler after drying.
[0037] Comparative Example 1
[0038] The natural zeolite was repeatedly rinsed with distilled water for 3 times, and then soaked in distilled water for 24 hours. The water was changed every 4 hours to dissolve the impurities, and then dried in a drying oven at 60°C for 12 hours. The dried zeolite was crushed and put into a container for later use.
[0039] Comparative Example 2
[0040] A method for preparing a chitosan-zeolite composite material comprises the following steps:
[0041] (1) Rinse the natural zeolite with distilled water repeatedly for 3 times, then soak it in distilled water for 24 hours, change the water every 4 hours to dissolve the impurities, and then dry it in a drying oven at 60°C for 12 hours. Crush the dried zeolite and put it into a container for later use.
[0042] (2) Dissolve 1g chitosan in 50mL 5% acetic acid and stir to dissolve. Slowly add 25mL 20% dimethyldiallyl ammonium chloride solution and mix thoroughly. Immediately place the conical flask in a 55℃ constant temperature magnetic stirrer and heat to react for 20min. After the reaction is completed, cool to room temperature.
[0043] (3) In a fume hood, an equal volume of acetone was added to the reaction system of step (2) to generate a large amount of white flocs. After centrifugation, the flocs were washed three times with anhydrous ethanol. Finally, the product was placed in a drying oven at 60° C. and dried for 24 h. The product was taken out and ground to obtain a slightly yellow powder of quaternized chitosan.
[0044] (4) Add 3 g of zeolite to 50 mL of the 10 g / L quaternized chitosan solution obtained in step (3), and keep stirring on a magnetic stirrer for 4 h.
[0045] (5) The solution obtained in step (4) was dripped into a 1 mol / L NaOH solution. Then, the chitosan-zeolite composite was washed with deionized water to a constant pH, and dried in an oven at 60° C. to prepare a chitosan-zeolite composite material.
[0046] Application Example 1
[0047] Removal of phosphate from water by adsorption:
[0048] In a 150mL conical flask, 100mL of 2mg / L and 100mg / L phosphorus-containing solutions were added, the pH of the solution was adjusted to 7 with dilute hydrochloric acid (0.1mol / L) and sodium hydroxide solution (1mol / L), and 100mg of the materials prepared in Example 1, Comparative Example 1 and Comparative Example 2 were added. The mixture was sealed with plastic wrap and placed in a constant temperature oscillator to react for 24h. After the reaction was completed, the mixture was taken out and allowed to stand for 5min. A 5mL syringe was used to take the supernatant of the phosphate solution, and it was filtered using a 0.45μm water filter head. The residual phosphate concentration was determined using ammonium molybdate spectrophotometry.
[0049] The adsorption amount of phosphate by the phosphorus removal and antibacterial modified zeolite filler prepared in Example 1 and the original natural zeolite material prepared in Comparative Example 1 as adsorbents was calculated. Figure 1 As shown, by calculation, the adsorption capacity of phosphate ions by the phosphorus removal and antibacterial modified zeolite filler prepared in Example 1 reached 46.69 mg / g, the adsorption capacity of phosphate ions by the original natural zeolite material prepared in Comparative Example 1 was 2.89 mg / g, and the adsorption capacity of phosphate ions by the chitosan modified zeolite prepared in Comparative Example 2 was 14.68 mg / g. Figure 2 As shown, in the low-concentration phosphorus treatment experiment of 2 mg / L, the phosphorus removal and antibacterial modified zeolite filler prepared in Example 1 has a phosphorus removal rate of up to 93%, the removal rate of the original natural zeolite material prepared in Comparative Example 1 is only 6%, and the removal rate of the chitosan modified zeolite material prepared in Comparative Example 2 is 34%.
[0050] Application Example 2
[0051] Antibacterial potential application:
[0052] (1) Escherichia coli was cultured in 50 mL LB liquid medium for 12 h, taken out and centrifuged at 5000 rpm for 10 min, then washed several times with PBS and stored in a 4°C refrigerator for later use.
[0053] (2) A certain amount of the natural zeolite of Comparative Example 1 and the composite modified zeolite of Example 1 were added to a sterilized conical flask, respectively. 100 μL of the diluted bacterial solution was added to 100 mL of phosphorus-containing solution for microbial experiments, and the mixture was shaken at 25° C. for 8 h.
[0054] (3) The reaction system of step (2) was taken out, the supernatant was discarded, the material was washed three times with PBS buffer, and then the material was treated with a vortex oscillator to shake and desorb the microorganisms attached to the surface of the material.
[0055] (4) Take 100 μL of the bacterial suspension and dilute it four times in a 10-fold concentration gradient. Spread the bacterial suspension at each dilution multiple on LB medium, then place it in a constant temperature incubator at 37°C for 24 h and observe the bacterial growth on the medium.
[0056] The surface of the phosphorus removal and antibacterial modified zeolite filler prepared in Example 1 is loaded with quaternary ammonium chitosan and La having antibacterial function. 3+ ,like Figure 3 As shown, compared with the unmodified natural zeolite, the phosphorus removal and antibacterial modified zeolite filler prepared in Example 1 has antibacterial function and can alleviate the clogging problem of artificial wetland fillers.
[0057] Example 2
[0058] A method for preparing a phosphorus-removing and antibacterial modified zeolite filler comprises the following steps:
[0059] (1) Rinse the natural zeolite with distilled water repeatedly for 3 times, then soak it in distilled water for 24 hours, change the water every 4 hours to dissolve the impurities, and then dry it in a drying oven at 60°C for 12 hours. Crush the dried zeolite and put it into a container for later use.
[0060] (2) Dissolve 1g chitosan in 50mL 5% acetic acid and stir to dissolve. Slowly add 25mL 20% dimethyldiallyl ammonium chloride solution and mix thoroughly. Immediately place the conical flask in a 55℃ constant temperature magnetic stirrer and heat to react for 20min. After the reaction is completed, cool to room temperature.
[0061] (3) In a fume hood, an equal volume of acetone was added to the reaction system of step (2) to generate a large amount of white flocs. After centrifugation, the flocs were washed three times with anhydrous ethanol. Finally, the product was placed in a drying oven at 60° C. and dried for 24 h. The product was taken out and ground to obtain a slightly yellow powder of quaternized chitosan.
[0062] (4) 3 g of the zeolite in step (1) was added to 50 mL of 0.1 mol / L (La(NO)3)3·6H2O solution and stirred to mix evenly, the pH was adjusted to 11, and stirred at room temperature for 24 h. After the reaction, the composite modified material was rinsed with deionized water, and then dried in an oven at 60° C. for 24 h to obtain a lanthanum-modified zeolite material.
[0063] (5) 3 g of the lanthanum-modified zeolite described in step (4) was added to 100 mL of the quaternized chitosan solution obtained in step (3) at a concentration of 10 g / L, and the mixture was stirred on a magnetic stirrer for 4 h.
[0064] (6) The solution obtained in step (5) was dripped into a 1 mol / L NaOH solution. Then, the lanthanum-chitosan-zeolite composite was washed with deionized water to a constant pH, then soaked in 5% glutaraldehyde overnight, and finally dried in an oven at 60° C., thereby preparing a lanthanum and chitosan composite modified zeolite material.
[0065] Application Example 3
[0066] The phosphorus removal and antibacterial modified zeolite filler prepared in Example 1 was loaded into a column, the cross-sectional diameter of the column was 1 cm, the filler height was 2 cm, and the water flow rate was controlled to be 5 mL / min; the phosphorus removal and antibacterial modified zeolite filler column was used to adsorb and remove phosphorus-containing wastewater, and the initial phosphorus concentration of the phosphorus-containing wastewater was 5 mg / L, 10 mg / L, and 20 mg / L. Figure 4 As shown, under the condition of 25℃, after the phosphorus-containing wastewater was treated by the packed columns, the phosphorus removal rate of the three columns reached 95% in the first 2 hours.
[0067] Comparative Example 3
[0068] A method for preparing a lanthanum-modified zeolite material comprises the following steps:
[0069] (1) Rinse the natural zeolite with distilled water repeatedly for 3 times, then soak it in distilled water for 24 hours, change the water every 4 hours to dissolve the impurities, and then dry it in a drying oven at 60°C for 12 hours. Crush the dried zeolite and put it into a container for later use.
[0070] (2) 3 g of the zeolite in step (1) was added to 50 mL of 0.1 mol / L (La(NO)3)3·6H2O solution and stirred to mix evenly, the pH was adjusted to 11, and stirred at room temperature for 24 h. After the reaction, the composite modified material was rinsed with deionized water and then dried in an oven at 60° C. for 24 hours to obtain a lanthanum-modified zeolite material.
[0071] Antibacterial potential test:
[0072] Take 100 μL of 10 7 CFU / mL of Escherichia coli suspension to the surface of the solid culture medium, and use a coating rod to repeatedly push the bacterial suspension until it is evenly distributed on the surface of the culture medium. Prepare 0.2g / mL of the material suspension obtained in Example 2, Comparative Example 1, Comparative Example 2, and Comparative Example 3, and immerse the filter paper in the suspension. Use tweezers to place the filter paper adsorbed with the antibacterial material in the center of the above-treated solid culture medium, culture it in a 37°C incubator for 24 hours, and observe whether the plate produces a transparent inhibition zone.
[0073] The results are as follows Figure 5As shown, an obvious transparent antibacterial zone appears around the modified zeolite material for long-term phosphorus removal artificial wetland prepared in Example 2, which proves that the modified zeolite material for long-term phosphorus removal artificial wetland has an antibacterial effect and can be used in artificial wetlands to alleviate the problem of biological clogging of the matrix.
[0074] Example 3
[0075] A method for preparing a phosphorus-removing and antibacterial modified zeolite filler comprises the following steps:
[0076] (1) Rinse the natural zeolite with distilled water repeatedly for 3 times, then soak it in distilled water for 24 hours, change the water every 4 hours to dissolve the impurities, and then dry it in a drying oven at 60°C for 12 hours. Crush the dried zeolite and put it into a container for later use.
[0077] (2) Dissolve 1g chitosan in 50mL 5% acetic acid and stir to dissolve. Slowly add 50mL 25vol% dimethyldiallylammonium chloride solution and mix thoroughly. Immediately place the conical flask in a 50℃ constant temperature magnetic stirrer and heat to react for 30min. After the reaction is completed, cool to room temperature.
[0078] (3) In a fume hood, an equal volume of acetone was added to the reaction system of step (2) to generate a large amount of white flocs. After centrifugation, the flocs were washed three times with anhydrous ethanol. Finally, the product was placed in a drying oven at 50° C. and dried for 24 h. The product was taken out and ground to obtain a quaternized chitosan in the form of a slightly yellow powder.
[0079] (4) Dissolve quaternary ammonium chitosan in water to form a 10 g / L quaternary ammonium chitosan solution, add 3 g of zeolite into 100 mL of the quaternary ammonium chitosan solution, and keep stirring on a magnetic stirrer for 4 h.
[0080] (5) The solution obtained in step (4) was dripped into a 1 mol / L NaOH solution. Then, the chitosan-zeolite composite was washed with deionized water until the pH value was constant, and dried in an oven at 50° C. to prepare a chitosan-zeolite composite material.
[0081] (6) 3 g of chitosan-zeolite composite material was added to 50 mL of 0.5 mol / L (La(NO)3)3·6H2O solution and stirred to mix evenly, the pH was adjusted to 14, and stirred at room temperature for 24 h. After the reaction, the composite modified material was rinsed with deionized water and then dried in an oven at 60 ° C for 24 h to obtain a lanthanum-chitosan-zeolite composite material.
[0082] (7) The lanthanum-chitosan-zeolite composite material and cement are mixed and granulated in a mass ratio of 4:1 to form spherical particles of 4 to 5 mm, which are shade-dried for 24 hours and steam-cured for 2 hours to obtain a phosphorus-removing and antibacterial modified zeolite filler after drying.
[0083] Example 4
[0084] A method for preparing a phosphorus-removing and antibacterial modified zeolite filler comprises the following steps:
[0085] (1) Rinse the natural zeolite with distilled water repeatedly for 3 times, then soak it in distilled water for 24 hours, change the water every 4 hours to dissolve the impurities, and then dry it in a drying oven at 60°C for 12 hours. Crush the dried zeolite and put it into a container for later use.
[0086] (2) Dissolve 1g chitosan in 50mL 5% acetic acid and stir to dissolve. Slowly add 30mL 21vol% dimethyldiallylammonium chloride solution and mix thoroughly. Immediately place the conical flask in a 60℃ constant temperature magnetic stirrer and heat to react for 25min. After the reaction is completed, cool to room temperature.
[0087] (3) In a fume hood, an equal volume of acetone was added to the reaction system of step (2) to generate a large amount of white flocs. After centrifugation, the flocs were washed three times with anhydrous ethanol. Finally, the product was placed in a drying oven at 55° C. and dried for 24 h. The product was taken out and ground to obtain a slightly yellow powder of quaternized chitosan.
[0088] (4) Dissolve quaternized chitosan in water to form a 10 g / L quaternized chitosan solution, add 3 g of zeolite into 80 mL of the quaternized chitosan solution, and keep stirring on a magnetic stirrer for 4 h.
[0089] (5) The solution obtained in step (4) was dripped into a 1 mol / L NaOH solution. Then, the chitosan-zeolite composite was washed with deionized water until the pH value was constant, and dried in an oven at 55° C. to prepare a chitosan-zeolite composite material.
[0090] (6) 3 g of chitosan-zeolite composite material was added to 50 mL of 0.3 mol / L (La(NO)3)3·6H2O solution and stirred to mix evenly, the pH was adjusted to 12, and stirred at room temperature for 24 h. After the reaction, the composite modified material was rinsed with deionized water and then dried in an oven at 60 °C for 24 h to obtain a lanthanum-chitosan-zeolite composite material.
[0091] (7) The lanthanum-chitosan-zeolite composite material and cement are mixed and granulated in a mass ratio of 8:1 to form spherical particles of 4 to 5 mm, which are shade-dried for 24 hours and steam-cured for 2 hours to obtain a phosphorus-removing and antibacterial modified zeolite filler after drying.
[0092] Example 5
[0093] A method for preparing a phosphorus-removing and antibacterial modified zeolite filler comprises the following steps:
[0094] (1) Rinse the natural zeolite with distilled water repeatedly for 3 times, then soak it in distilled water for 24 hours, change the water every 4 hours to dissolve the impurities, and then dry it in a drying oven at 60°C for 12 hours. Crush the dried zeolite and put it into a container for later use.
[0095] (2) Dissolve 1g chitosan in 50mL 5% acetic acid and stir to dissolve. Slowly add 40mL 22vol% dimethyldiallylammonium chloride solution and mix thoroughly. Immediately place the conical flask in a 52℃ constant temperature magnetic stirrer and heat for 22min. After the reaction is completed, cool to room temperature.
[0096] (3) In a fume hood, an equal volume of acetone was added to the reaction system of step (2) to generate a large amount of white flocs. After centrifugation, the flocs were washed three times with anhydrous ethanol. Finally, the product was placed in a drying oven at 52° C. and dried for 24 h. The product was taken out and ground to obtain a quaternized chitosan in the form of a slightly yellow powder.
[0097] (4) Dissolve quaternary ammonium chitosan in water to form a 10 g / L quaternary ammonium chitosan solution, add 3 g of zeolite into 70 mL of the quaternary ammonium chitosan solution, and keep stirring on a magnetic stirrer for 4 h.
[0098] (5) The solution obtained in step (4) was dripped into a 1 mol / L NaOH solution. Then, the chitosan-zeolite composite was washed with deionized water until the pH value was constant, and dried in an oven at 52° C. to prepare a chitosan-zeolite composite material.
[0099] (6) 3 g of chitosan-zeolite composite material was added to 50 mL of 0.2 mol / L (La(NO)3)3·6H2O solution and stirred to mix evenly, the pH was adjusted to 13, and stirred at room temperature for 24 h. After the reaction, the composite modified material was rinsed with deionized water and then dried in an oven at 60 °C for 24 h to obtain a lanthanum-chitosan-zeolite composite material.
[0100] (7) The lanthanum-chitosan-zeolite composite material and cement are mixed and granulated in a mass ratio of 2:1 to form spherical particles of 4 to 5 mm, which are shade-dried for 24 hours and steam-cured for 2 hours to obtain a phosphorus-removing and antibacterial modified zeolite filler after drying.
[0101] Example 6
[0102] A method for preparing a phosphorus-removing and antibacterial modified zeolite filler comprises the following steps:
[0103] (1) Rinse the natural zeolite with distilled water repeatedly for 3 times, then soak it in distilled water for 24 hours, change the water every 4 hours to dissolve the impurities, and then dry it in a drying oven at 60°C for 12 hours. Crush the dried zeolite and put it into a container for later use.
[0104] (2) Dissolve 1 g of chitosan in 50 mL of 5% acetic acid and stir to dissolve. Slowly add 35 mL of 24 vol% dimethyldiallyl ammonium chloride solution and mix thoroughly. Immediately place the conical flask in a 58°C constant temperature magnetic stirrer and heat to react for 27 min. After the reaction is completed, cool to room temperature.
[0105] (3) In a fume hood, an equal volume of acetone was added to the reaction system of step (2) to generate a large amount of white flocs. After centrifugation, the flocs were washed three times with anhydrous ethanol. Finally, the product was placed in a drying oven at 58° C. and dried for 24 h. The product was taken out and ground to obtain a slightly yellow powder of quaternized chitosan.
[0106] (4) Dissolve quaternary ammonium chitosan in water to form a 10 g / L quaternary ammonium chitosan solution, add 3 g of zeolite into 60 mL of the quaternary ammonium chitosan solution, and keep stirring on a magnetic stirrer for 4 h.
[0107] (5) The solution obtained in step (4) was dripped into a 1 mol / L NaOH solution. Then, the chitosan-zeolite composite was washed with deionized water until the pH value was constant, and dried in an oven at 58° C. to prepare a chitosan-zeolite composite material.
[0108] (6) 3 g of chitosan-zeolite composite material was added to 50 mL of 0.4 mol / L (La(NO)3)3·6H2O solution and stirred to mix evenly, the pH was adjusted to 11, and stirred at room temperature for 24 h. After the reaction, the composite modified material was rinsed with deionized water and then dried in an oven at 60 °C for 24 h to obtain a lanthanum-chitosan-zeolite composite material.
[0109] (7) The lanthanum-chitosan-zeolite composite material and cement are mixed and granulated in a mass ratio of 4:1 to form spherical particles of 4 to 5 mm, which are shade-dried for 24 hours and steam-cured for 2 hours to obtain a phosphorus-removing and antibacterial modified zeolite filler after drying.
[0110] Example 7
[0111] 100 mg of the obtained products of Comparative Examples 1 to 3 and Examples 1 to 2 were added to 100 mL of a 2 mg / L phosphorus-containing solution, sealed with plastic wrap, and placed in a constant temperature oscillator for reaction for 24 h. After the reaction was completed, the solution was taken out and allowed to stand for 5 min. The supernatant of the phosphate solution was taken with a 5 mL syringe and filtered with a 0.45 μm water filter. The residual phosphate concentration was determined by ammonium molybdate spectrophotometry. The results are shown in Table 1. Figure 6 The phosphate removal rate of comparative example 1 is 5.64%, the phosphate removal rate of comparative example 2 is 34.16%, the phosphate removal rate of comparative example 3 is 90.57%, the phosphate removal rate of embodiment 1 is 93.83%, and the phosphate removal rate of embodiment 2 is 96.97%.
[0112] Comparative Example 4
[0113] The remaining steps of this comparative example are the same as those of Example 2, except that the (La(NO)3)3·6H2O solution in step (4) is replaced by (Nd(NO)3)3·6H2O. Phosphorus removal and antibacterial experiments were conducted, and the results showed that the phosphorus removal and antibacterial effects were reduced compared with those of Example 2.
Claims
1. A method for preparing a phosphorus removal and antibacterial modified zeolite filler, characterized in that: The following steps are involved: Step 1, dissolving chitosan in acetic acid, stirring and mixing to dissolve, then adding dimethyldiallyl ammonium chloride solution, mixing evenly and heating to react, cooling to room temperature after the reaction, then adding acetone to generate precipitation, washing, drying and grinding into powder to obtain quaternized chitosan; Step 2: firstly mix the natural zeolite with quaternary ammonium chitosan and water, stir evenly, then drip into a sodium hydroxide solution, wash and dry, then stir and mix evenly with lanthanum nitrate hexahydrate, adjust the pH to 11-14, stir, wash and dry; or firstly stir and mix the natural zeolite with lanthanum nitrate hexahydrate, adjust the pH to 11-14, stir, wash and dry, then mix with quaternary ammonium chitosan and water, stir evenly, then drip into a sodium hydroxide solution, wash and dry, to obtain a lanthanum-chitosan-zeolite composite material; Step three, mixing the lanthanum-chitosan-zeolite composite material with cement to form granules, drying in the shade, steam curing, and drying to obtain phosphorus-removing and antibacterial modified zeolite filler.
2. The method for preparing a phosphorus removal and antibacterial modified zeolite filler according to claim 1, characterized in that: In the step 1, the mass ratio of chitosan, acetic acid and dimethyldiallylammonium chloride solution is 4:1:1-2.
3. The method for preparing a phosphorus removal and antibacterial modified zeolite filler according to claim 1, characterized in that: In the step 1, the volume percentage of dimethyldiallylammonium chloride in the dimethyldiallylammonium chloride solution is 20-25 vol%.
4. The method for preparing a phosphorus removal and antibacterial modified zeolite filler according to claim 1, characterized in that: In the step 1, the heating reaction temperature is 50-60° C., and the reaction time is 20-30 min.
5. The method for preparing a phosphorus removal and antibacterial modified zeolite filler according to claim 1, characterized in that: In the step 2, the mass ratio of natural zeolite to quaternized chitosan is 3:0.5-1.
6. The method for preparing a phosphorus removal and antibacterial modified zeolite filler according to claim 1, characterized in that: In the step 2, the concentration of lanthanum nitrate hexahydrate is 0.1-0.5 mol / L.
7. The method for preparing a phosphorus removal and antibacterial modified zeolite filler according to claim 1, characterized in that: In the step 3, the mass ratio of the lanthanum-chitosan-zeolite composite material to cement is 2 to 8:
1.
8. The method for preparing a phosphorus removal and antibacterial modified zeolite filler according to claim 1, characterized in that: The washing and drying temperature is 50-60°C.
9. The phosphorus-removing and antibacterial-inhibiting modified zeolite filler obtained by the preparation method of the phosphorus-removing and antibacterial-inhibiting modified zeolite filler according to any one of claims 1 to 8.
10. Use of the phosphorus removal and antibacterial modified zeolite filler according to claim 9 in phosphorus removal, adsorption and antibacterial in artificial wetlands.
Citation Information
Patent Citations
Preparation method of quaternized chitosan and application thereof
CN109293796A
Lanthanum-iron modified zeolite phosphorus removal adsorbent and preparation method and application thereof
CN109847691A
Sewage processing agent, and preparation method thereof
CN110054247A
Modified chitosan cross-linked zeolite porous adsorbent and application thereof
CN110665474A
Autoclaved porous zeolite filter material having composite manganese and phosphorus removal effect and preparation method thereof
CN112479647A
Cited By
Method for promoting bright color of flowers by lincomycin finished product liquid fertilizer
CN119431059A
Shield expansion mud for preventing ground surface settlement
CN119954448A
Anti-pollution and rhizosphere activation coupled wetland long-acting phosphorus removal method
CN122301378A