Polymers based on dimeric fatty acid-polyester diols containing isocyanate groups

A polymer based on diphenylmethane 4,4'-diisocyanate and dimeric fatty acid polyester diols addresses adhesion issues to residual adhesive beads in moisture-curing polyurethane adhesives, ensuring effective adhesion, cure speed, and low hazardous content, while maintaining elasticity and weatherability.

JP7572957B2Active Publication Date: 2024-10-24SIKA TECH AG
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021545417
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-05
Filing Date
2020-04-02
Publication Date
2024-10-24
Estimated Expiration
2040-04-02

AI Technical Summary

Technical Problem

Existing moisture-curing polyurethane adhesives face challenges in achieving good adhesion to difficult substrates like residual adhesive beads without compromising storage stability, cure speed, strength, extensibility, elasticity, and hazardous material classification, particularly due to the presence of diisocyanate monomers that are harmful and require special handling.

Method used

Development of a polymer containing isocyanate groups based on diphenylmethane 4,4'-diisocyanate and polyester diols derived from dimeric fatty acids, with a controlled NCO content of 1.5% to 6% and diisocyanate monomer content of 0.5% or less, ensuring low viscosity and compatibility, which can be used as an adhesion promoter in moisture-curing elastomeric polyurethane adhesives.

Benefits of technology

The polymer provides improved adhesion to residual adhesive beads with good cure speed, strength, extensibility, and elasticity, while maintaining low hazardous substance classification, allowing for easy handling and application at room temperature with enhanced weatherability and matte surface finish.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572957000001
    Figure 0007572957000001
  • Figure 0007572957000002
    Figure 0007572957000002
  • Figure 0007572957000003
    Figure 0007572957000003
Patent Text Reader

Abstract

The present invention relates to a polyesterurethane polymer containing isocyanate groups and liquid at ambient temperature, obtained by reacting at least one diisocyanate monomer in an NCO / OH ratio of at least 3 / 1 with a polyesterdiol based on a dimeric fatty acid having an OH value in the range of 28 to 120 mg KOH / g, followed by removal of most of the diisocyanate monomer by a suitable separation process. The polymer is characterized by an NCO content in the range of 1.5 to 6 wt. % and a diisocyanate monomer content of up to 0.5 wt. %. The present invention also relates to the use of this polymer as an adhesion promoter and to moisture-curing polyurethane compositions containing this polymer. The polymer according to the present invention is easy to use. The polymer according to the present invention allows the production of moisture-curing polyurethane compositions with improved properties in terms of open time, adhesion, application, and weather resistance, accompanied by good properties unchanged in terms of storage stability, cure speed, strength, ductility, elasticity, and hazardous material classification for ambient temperature applications. Compositions of this type are particularly suitable for use as elastic adhesives in replacement glass for vehicles.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to polymers containing isocyanate groups and having a low monomer content and their use in moisture-curable polyurethane compositions, in particular for use as adhesives for glass replacement in automobiles. [Background technology]

[0002] Curable compositions based on polyurethanes are often used as adhesives for elastic bonds, for example in automotive assembly, which require good properties, especially with regard to storage stability, applicability, open time, curing speed, adhesion, strength, elasticity, weather resistance and hazardous materials classification.

[0003] One-component moisture-curing systems are especially popular due to their ease of handling. In general, these systems show good adhesive properties. However, there are applications on certain substrates on which it is difficult to achieve good adhesion. An example of this is the bonding of replacement panes in automobiles, where the body flanges as substrates have both areas with exposed paint and areas with residues of the old adhesive that have stuck to the paint and have not been completely removed or left as a bonding substrate ("residual adhesive beads"). If the new adhesive does not completely adhere to the residual adhesive beads, the effects can be unwanted water ingress or wind noise, or even delamination of the pane. Moisture-curing adhesives available now without a suitable pretreatment on the residual adhesive beads often simply result in inadequate adhesion, especially when the old adhesive has aged considerably and therefore become hard or brittle. For the improvement of adhesion on the residual adhesive beads, it is possible to use known adhesion promoters, such as diisocyanate oligomers or their derivatives. However, this leads to a loss of elasticity of the adhesive after curing.

[0004] Polymers containing isocyanate groups, present as binders in one-component polyurethane adhesives and cured by reaction with moisture, are prepared by reaction of polyols with diisocyanate monomers. Such polymers typically contain residual diisocyanate monomer content ranging from 0.5% to 3% by weight due to chain extension reactions. However, diisocyanate monomers are potentially harmful to health. In particular, formulations containing diisocyanate monomers at concentrations above 0.1% by weight must be provided with hazard symbols and warning messages on labels and in data sheets, and may be subject to restrictions on sale and use in some countries.

[0005] Polyurethanes containing polyester polyols based on dimer fatty acids are known. They are usually used as constituents of the polyol component of two-component polyurethanes, for example in EP 2,144,944 to increase the hydrolysis and solvent resistance of the elastomers or in WO 2018 / 210568 to obtain high elongation coupled with high strength.

[0006] EP 1,476,485 describes a two-component polyurethane for the production of microcellular polyurethane foams, in which the isocyanate component constitutes the reaction product of a polyester polyol based on dimer fatty acid and a large excess of diphenylmethane 4,4'-diisocyanate, which is then cured with a polyol component consisting mainly of a further polyester polyol based on dimer fatty acid. The reaction products described there are not suitable for use in moisture-curing polyurethane compositions due to their high NCO content. On curing of such compositions by moisture, blisters form and the elasticity and extensibility of the products thus obtained are too low.

[0007] WO 2017 / 103070 describes a moisture-curing polyurethane adhesive with high early strength, which is heated for application and contains a polymer containing isocyanate groups, which is a reaction product prepared in several stages from a polyol mixture containing a polyol based on dimer fatty acid. This reaction product has a very high viscosity and its preparation is complicated. Due to its poor extrudability, it is not suitable for an adhesive that can be applied at room temperature, which does not allow the desired adhesion to the residual adhesive beads. Summary of the Invention [Problem to be solved by the invention]

[0008] It is an object of the present invention to provide an adhesion promoter for moisture-curing elastic polyurethane adhesives which is processable at room temperature, which improves the adhesion of the adhesive to difficult substrates, e.g. residual adhesive beads, without loss in further relevant product properties, in particular storage stability, application, cure speed, blister formation, strength, extensibility, elasticity and hazardous materials classification. [Means for solving the problem]

[0009] This object is achieved by the polymer according to claim 1. The polymer is based on a polyester diol based on diisocyanate monomers, in particular diphenylmethane 4,4'-diisocyanate, and dimer fatty acids. It has an NCO content in the range of 1.5% to 6% by weight, and a diisocyanate monomer content of 0.5% by weight or less. The polymer according to the invention is liquid at room temperature, has a narrow molecular weight distribution and a practically useful viscosity. It is eminently suitable for use as an adhesion promoter in moisture-curing elastic polyurethane adhesives, where it has surprisingly good compatibility, in particular clearly improving the adhesion to residual adhesive beads and the open time, without adversely affecting the curing speed, strength, extensibility and other relevant product properties. The positive effect on the adhesive properties and the open time is surprising here, since experience has shown that polymers containing isocyanate groups and having a low monomer content are likely to be detrimental to good adhesion. Due to the low monomer content, it can also be used in large quantities without adversely affecting the harmful substances classification of the adhesive. Moreover, it improves the weatherability of polyurethane compositions, especially adhesives filled with carbon black, so that they have a much lower tendency for the carbon black to leach out and therefore do not stain the substrate even after extended use.Furthermore, the polymers of the present invention provide a matte adhesive surface, which in the case of a visible adhesive bond is highly desirable for many users.

[0010] Surprisingly, the polymer based on dimer fatty acid of the present invention has another unexpected advantage when used in moisture-curing polyurethane adhesive.What is particularly surprising is its favorable effect on application properties.Such adhesives can be easily pressed out of containers at room temperature and at low ambient and adhesive temperatures, especially with unchanged good sag resistance and short thread formation, even in the case of low content of the polymer of the present invention.

[0011] In order to improve early strength, sag resistance and thread formation, moisture-curing polyurethane adhesives, especially for automotive assembly, often contain a meltable component, typically a room-temperature solid polyurethane polymer based on crystalline polyester polyol.However, the extrusion force for adhesives at room temperature and under low temperature conditions is increased by the meltable component, and the sag resistance is highly shear-dependent, which can lead to problems in production and application.As a result of using the polymer based on dimer fatty acid of the present invention, even polyurethane adhesives with meltable components are surprisingly clearly better extrudable at room temperature and under low temperature conditions, and their rheological properties are significantly less shear-dependent.More specifically, the polymer of the present invention allows adhesives that can use much less meltable components or can be completely omitted.

[0012] The polyester urethane polymers based on dimeric fatty acids of the invention allow moisture-curing elastic polyurethane compositions which are liquid, optionally pasty, and therefore processable at room temperature, and which, together with good properties that do not change with respect to storage stability, cure speed, blistering, strength, extensibility, elasticity and harmful substance classification, have improved adhesion properties on certain substrates, in particular residual adhesive beads, improved application properties, in particular particularly good extrudability even at low temperatures (wherein the increase in the extruding force between room temperature and 5° C. is particularly small), long open times, non-glossy surfaces and better weather resistance.

[0013] Further aspects of the invention are the subject of further independent claims. Particularly preferred embodiments of the invention are the subject of the dependent claims. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present invention provides a room temperature liquid polyester urethane polymer containing isocyanate groups obtained by reaction of at least one diisocyanate monomer with a polyester diol based on dimeric fatty acid having an OH value in the range of 28-120 mg KOH / g in an NCO / OH ratio of at least 3 / 1, followed by removal of most of the diisocyanate monomer using a suitable separation method, characterized in that it has an NCO content in the range of 1.5% to 6% by weight and a diisocyanate monomer content of 0.5% by weight or less.

[0015] "Diisocyanate monomer" refers to an organic compound having two isocyanate groups separated from each other by a divalent hydrocarbyl group having from 4 to 15 carbon atoms.

[0016] A "polyester urethane polymer" refers to a polymer that has ester groups as repeat units and further contains urethane groups.

[0017] "Dimer fatty acid-based polyester diol" refers to a polyester diol prepared from dimer fatty acid and / or dimer fatty alcohol.

[0018] "NCO content" refers to the content of isocyanate groups in weight percent based on total polymer.

[0019] "Molecular weight" refers to the molar mass (in g / mol) of a molecule or molecular residue. "Average molecular weight" refers to the number average molecular weight (M n ), which is determined by gel permeation chromatography (GPC) against polystyrene as a standard.

[0020] A substance or composition is said to be "storage stable" or "storable" when it can be stored in a suitable container at room temperature for an extended period of time, typically at least three to six months or more, without a change in its application or use characteristics as a result of storage to an extent that would be relevant to its use.

[0021] "Room temperature" refers to a temperature of 23°C.

[0022] All industry standards mentioned herein relate to the version in effect as of the date of first filing.

[0023] Percentage by weight (wt %) refers to the proportion by mass of a component or molecule of a composition based on the entire composition or molecule, unless otherwise specified. The terms "mass" and "weight" are used synonymously herein.

[0024] The polymers of the present invention may also be referred to as polyurethane prepolymers.

[0025] The polymers of the present invention preferably have an NCO content in the range of 1.8% to 5% by weight, more preferably 2% to 4% by weight, especially 2.2% to 3.4% by weight. Such polymers allow for polyurethane compositions with an attractive combination of good extrudability, good adhesion properties and high strength.

[0026] The polymers of the present invention preferably have a diisocyanate monomer content of 0.3% by weight or less, in particular 0.2% by weight or less. Such polymers are particularly suitable for use in polyurethane compositions having less than 0.1% by weight of diisocyanate monomer. They are safe to handle without special safety precautions and can be sold in many countries without hazardous material classification.

[0027] Suitable diisocyanate monomers are commercially available aromatic, aliphatic or cycloaliphatic diisocyanates, in particular diphenylmethane 4,4'-diisocyanate (MDI), optionally with a fraction of diphenylmethane 2,4'- and / or 2,2'-diisocyanate, tolylene 2,4-diisocyanate with tolylene 2,6-diisocyanate or mixtures thereof (TDI), phenylene 1,4-diisocyanate (PDI), naphthalene 1,5-diisocyanate (NDI), hexane 1,6-diisocyanate (HDI), 2,2( 4), 4-trimethylhexamethylene 1,6-diisocyanate (TMDI), cyclohexane 1,3- or 1,4-diisocyanate, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate or IPDI), perhydro(diphenylmethane 2,4'- or 4,4'-diisocyanate) (HMDI), 1,3- or 1,4-bis(isocyanatomethyl)cyclohexane, m- or p-xylylene diisocyanate (XDI), or mixtures thereof.

[0028] The diisocyanate monomers used for the reaction are preferably diphenylmethane 4,4'-diisocyanate (4,4'-MDI), tolylene 2,4-diisocyanate with tolylene 2,6-diisocyanate or mixtures thereof (TDI), 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (IPDI) or hexane 1,6-diisocyanate (HDI). These diisocyanates are easily obtainable, inexpensive and allow good mechanical strength. It is also possible to use a combination of two or more of these diisocyanate monomers.

[0029] IPDI is particularly preferred. Such polymers are particularly suitable in moisture-curable polyurethane compositions which have particularly high light stability.

[0030] Most preferred as a diisocyanate monomer is 4,4'-MDI, especially those qualities which contain only small fractions of diphenylmethane 2,4'- and / or 2,2'-diisocyanate, which are solid at room temperature. Such polymers cure particularly quickly and allow for particularly high strength.

[0031] The polyester diols based on dimeric fatty acids used for the reaction are typically liquid at room temperature, having an OH number in the range of 28 to 120 mg KOH / g.

[0032] Such polyester diols based on dimeric fatty acids have average molecular weights M in the range of 950 to 4,000 g / mol. n These have a mostly linear structure and an average OH functionality of about 2.

[0033] The polyester diols based on dimer fatty acids are preferably amorphous.

[0034] Suitable dimer fatty acid-based polyester diols are in particular obtained from the esterification of at least one dimer fatty acid and / or at least one dimer fatty alcohol with a diol, such as ethylene glycol or butanediol, and / or a dicarboxylic acid, such as adipic acid, in such a stoichiometry that the product is amorphous, liquid at room temperature and has an OH number in the range of 28 to 120 mg KOH / g.

[0035] The polyester diols based on dimer fatty acids preferably contain a content of carbon atoms from renewable sources according to ASTM D6866, based on the total carbon content in the range of 50% to 100%, preferably 60% to 95%, in particular 70% to 90%. Such polyester diols are amorphous and hydrophobic and have particularly good compatibility in polyurethane adhesives.

[0036] The polyester diols based on dimeric fatty acids preferably have an OH number in the range of 34 to 120 mg KOH / g, in particular in the range of 52 to 60 mg KOH / g. Such polyester diols based on dimeric fatty acids have an average molecular weight M in the range of 950 to 3,300 g / mol, in particular in the range of 1,900 to 2,200 g / mol. n Such polymers allow for polyurethane compositions having a particularly attractive combination of good extrudability, good adhesion properties and high strength.

[0037] Particularly suitable are commercially available polyester diols based on amorphous dimeric fatty acids, in particular the grades available under the trade name Priplast®: Priplast® 1837, 1838, 3187, 3196, 3197, 3199 or 3238 (from Croda). Of these, Priplast® 1838 is preferred.

[0038] The polymers of the present invention result from the reaction of at least one diisocyanate monomer with a dimer fatty acid based polyester diol in an NCO / OH ratio of at least 3 / 1.

[0039] The NCO / OH ratio is preferably in the range of from 3 / 1 to 10 / 1, more preferably from 3 / 1 to 8 / 1, particularly from 4 / 1 to 7 / 1, and most preferably from 5 / 1 to 7 / 1.

[0040] The reaction is preferably carried out at a temperature ranging from 20 to 160° C., in particular from 40 to 140° C., optionally in the presence of a suitable catalyst and with the exclusion of moisture.

[0041] After the reaction, any diisocyanate monomer remaining in the reaction mixture is removed using appropriate separation methods to the residual contents described.

[0042] A preferred separation method is a distillation method, particularly thin film or short path distillation, preferably under reduced pressure.

[0043] Particularly preferred is a multi-stage process in which the diisocyanate monomer is removed in a short-path evaporator with a jacket temperature in the range of 120-200° C. and a pressure of 0.001-0.5 mbar.

[0044] In the case of 4,4'-MDI, which is preferred as diisocyanate monomer, removal by distillation is particularly demanding; for example, it must be ensured that the condensate does not solidify and block the system. It is preferred to operate at 0.001-0.5 mbar with a jacket temperature in the range of 160-200°C and to condense the removed monomer at a temperature in the range of 40-60°C.

[0045] It is preferred to react the diisocyanate monomer with the dimer fatty acid-based polyester diol followed by removal of most of the diisocyanate monomer remaining in the reaction mixture without the use of a solvent or entraining agent.

[0046] It is preferred to subsequently reuse the diisocyanate monomer removed after the reaction, ie to use it again for the preparation of a polymer containing isocyanate groups.

[0047] The polymer of the present invention preferably has a viscosity of 1,000 Pa·s or less, in particular 500 Pa·s or less, at 20° C. The viscosity at 20° C. is preferably in the range of 100 to 1,000 Pa·s, in particular 100 to 500 Pa·s. The viscosity at 30° C. is preferably in the range of 50 to 500 Pa·s, in particular 50 to 200 Pa·s. The viscosity at 40° C. is preferably in the range of 25 to 200 Pa·s, in particular 25 to 100 Pa·s. The viscosity at 60° C. is preferably in the range of 5 to 25 Pa·s, in particular 5 to 20 Pa·s. The viscosity is measured here in a cone-plate viscometer having a cone diameter of 25 mm, a cone angle of 1°, and a cone tip-plate distance of 0.5 mm, and is preferably less than 50 s. -1 The shear rate is measured.

[0048] In the reaction, the OH groups of the polyester diol based on dimeric fatty acid react with the isocyanate groups of the diisocyanate monomer. This also results in so-called chain extension reactions, in that there is a reaction of the OH groups and / or isocyanate groups of the reaction product between the diol and the diisocyanate monomer. The higher the selected NCO / OH ratio, the lower the level of chain extension reactions that occurs and the lower the polydispersity and therefore also the viscosity of the resulting polymer. A measure of the chain extension reactions is the average molecular weight of the polymer, or the width and distribution of the peaks in the GPC analysis. A further measure is the effective NCO content of the polymer without monomers, relative to the theoretical NCO content calculated from the reaction of all OH groups with the diisocyanate monomer.

[0049] The NCO content in the polymer of the present invention is preferably at least 75%, in particular at least 80%, of the theoretical NCO content calculated from the addition of one mole of diisocyanate monomer per mole of OH group of polyester diol based on dimer fatty acid. Such polymers are of low viscosity, allowing good application properties.

[0050] Particularly preferred polyester urethane polymers of the invention are obtained by reacting 4,4'-MDI with a polyester diol based on an amorphous dimeric fatty acid having an OH number in the range of 34 to 120 mg KOH / g, in particular 52 to 60 mg KOH / g, in an NCO / OH ratio in the range of 4 / 1 to 10 / 1, followed by removal of the 4,4'-MDI by distillation, and finally have an NCO content in the range of 2% to 5% by weight, in particular 2.2% to 4% by weight, a diisocyanate monomer content of less than or equal to 0.3% by weight, and a viscosity in the range of 100 to 1,000 Pa·s, preferably 100 to 500 Pa·s, at 20°C.

[0051] The polymers of the invention are liquid at room temperature and therefore easy to handle, have only a low, if any, hazardous materials classification due to their low monomer content and are suitable as adhesion promoters in moisture-curing elastic polyurethane adhesives, where they further improve the application properties and weather resistance.

[0052] The present invention further provides the use of the polyester urethane polymer of the present invention as an adhesion promoter in a moisture-curable polyurethane composition.

[0053] For use as an adhesion promoter, the polyester urethane polymer of the present invention is used in an amount ranging from 0.5% to 15% by weight, preferably from 1% to 10% by weight, based on the total polyurethane composition.

[0054] The use as an adhesion promoter improves the adhesive properties of moisture-curing polyurethane compositions. In particular, the adhesion to the residual adhesive bead is improved. This adhesion is particularly important in the replacement of panes in automobiles when new panes are bonded by moisture-curing polyurethane adhesives, in which case the substrate also contains residues of the old adhesive bead to which the replaced pane is bonded. Very good adhesion to the residual adhesive bead is important even when only small amounts of such residues on the substrate are present, since spots of incomplete adhesion can cause water ingress or annoying wind noise in the operation of the vehicle.

[0055] When used as adhesion promoters, the polymers of the present invention exhibit further desirable effects, such as an improvement in the extrudability of the composition coupled with good shear-independent sag resistance and short thread formation, a small increase in the extrudability under low temperature conditions, better weatherability of the composition and a non-glossy surface, without any loss in storage stability, hardening, mechanical properties or hazardous material classification.

[0056] The present invention further comprises: at least one polyether urethane polymer containing isocyanate groups, and - the polyester urethane polymers described which contain isocyanate groups The present invention provides a moisture-curable polyurethane composition suitable as an elastic adhesive and / or sealant, comprising:

[0057] The moisture-curable polyurethane composition is preferably liquid, optionally pasty, at room temperature and therefore has good room temperature processability.

[0058] The moisture-curable polyurethane composition preferably contains 0.5% to 15% by weight, preferably 1% to 10% by weight, of a polyester urethane polymer containing isocyanate groups.

[0059] Suitable polyether urethane polymers containing isocyanate groups are especially those with a majority of polyoxypropylene structural units. Such polymers are particularly suitable as the main binder for elastic adhesives and / or sealants that are processable at room temperature and have high extensibility.

[0060] The polyether segments in the polyetherurethane polymer preferably consist of at least 80% 1,2-propyleneoxy units and, optionally, further 1,2-ethyleneoxy units.

[0061] The polyether urethane polymer containing isocyanate groups preferably has an average molecular weight M in the range of 2,000 to 20,000 g / mol, preferably 3,000 to 15,000 g / mol. n has.

[0062] It is preferably a liquid at room temperature.

[0063] The polyetherurethane polymers containing isocyanate groups preferably have an NCO content in the range from 1% to 5% by weight, in particular from 1% to 3% by weight.

[0064] Suitable polyether urethane polymers containing isocyanate groups are in particular obtained by reacting at least one polyether polyol with a superstoichiometric amount of at least one diisocyanate monomer, the reaction being preferably carried out at temperatures ranging from 20 to 160° C., in particular from 40 to 140° C., optionally in the presence of a suitable catalyst, with the exclusion of moisture.

[0065] The NCO / OH ratio is preferably in the range from 1.3 / 1 to 10 / 1. The diisocyanate monomers remaining in the reaction mixture after reaction of the OH groups can in particular be removed by distillation.

[0066] If the excess diisocyanate monomer is removed by distillation, the NCO / OH ratio in the reaction mass is preferably in the range of 3 / 1 to 10 / 1, in particular 4 / 1 to 7 / 1, and the resulting polymer containing isocyanate groups contains, after distillation, preferably not more than 0.5% by weight, more preferably not more than 0.3% by weight, of diisocyanate monomer. The diisocyanate monomer is in particular removed here by short path distillation under reduced pressure.

[0067] If excess diisocyanate monomer is not removed from the polymer, the NCO / OH ratio in the reaction mass is preferably in the range of 1.3 / 1 to 2.5 / 1.Such polyether urethane polymers in particular contain not more than 3% by weight, preferably not more than 2% by weight, of diisocyanate monomer.

[0068] Preferred diisocyanate monomers are the aromatic, aliphatic or cycloaliphatic diisocyanates already mentioned, in particular MDI, TDI, HDI or IPDI, or mixtures thereof.

[0069] Most preferred is 4,4'-MDI, which provides elastic adhesives and / or sealants with particularly high strength coupled with high extensibility.

[0070] Suitable polyether polyols are the polymerization products of commercially available polyols or mixtures thereof, in particular of ethylene oxide or 1,2-propylene oxide or 1,2- or 2,3-butylene oxide or oxetane or tetrahydrofuran or mixtures thereof, in which these are polymerized with starter molecules having two or three active hydrogen atoms, in particular starter molecules such as water, ammonia or compounds having several OH or NH groups, for example ethane-1,2-diol, propane-1,2- or -1,3-diol, neopentylglycerol, ethylene oxide, 1,2-propylene ... The polyether polyols may be polymerized with the aid of ethylene glycol, diethylene glycol, triethylene glycol, the isomeric dipropylene glycols or tripropylene glycols, the isomeric butanediols, pentanediols, hexanediols, heptanediols, octanediols, nonanediols, decanediols, undecanediols, cyclohexane-1,3- or -1,4-dimethanol, bisphenol A, hydrogenated bisphenol A, 1,1,1-trimethylolethane, 1,1,1-trimethylolpropane, glycerol or aniline, or mixtures of the abovementioned compounds. Also suitable are polyether polyols having polymer particles dispersed therein, in particular those having styrene / acrylonitrile (SAN) particles or polyurea or polyhydrazodicarbonamide (PHD) particles.

[0071] Preferred polyether polyols are polyoxypropylene diols or triols, or so-called ethylene oxide-terminated (EO-capped or EO-tipped) polyoxypropylene diols or triols, the latter being polyoxyethylene / polyoxypropylene copolyols, which are obtained in particular by further alkoxylation of polyoxypropylene diols or triols with ethylene oxide, as a result of a polypropoxylation reaction, resulting in these having primary hydroxyl groups.

[0072] Polyether polyols having an OH value in the range of 6 to 280 mg KOH / g, particularly 7.5 to 112 mg KOH / g, are preferred.

[0073] Average molecular weight M in the range of 400 to 20,000 g / mol, in particular 1,000 to 15,000 g / mol n Preferred is a polyether polyol having the formula:

[0074] Polyether polyols with an average OH functionality in the range of 1.6 to 3 are preferred.

[0075] In preparing polyether urethane polymers containing isocyanate groups, it is also possible to include a proportion of di- or polyfunctional alcohols.

[0076] In a preferred embodiment of the present invention, the polyether urethane polymer containing isocyanate groups contains a slightly low content of diisocyanate monomers, preferably less than 0.5% by weight, more preferably less than 0.3% by weight, in particular less than 0.2% by weight. Such polymers allow polyurethane compositions with a particularly attractive hazard classification.

[0077] Particularly preferred are polyether urethane polymers containing isocyanate groups and having an NCO content in the range of 1% to 2.5% by weight, in particular 1.3% to 2.1% by weight, and a diisocyanate monomer content of 0.3% by weight or less, which can be obtained by reacting at least one diisocyanate monomer with a polyether triol having an average OH functionality in the range of 2.2 to 3 and an OH number in the range of 20 to 42 mg KOH / g, in an NCO / OH ratio of at least 3 / 1, followed by removal of most of the diisocyanate monomer using a suitable separation method.Preferred diisocyanate monomers are IPDI or 4,4'-MDI, in particular 4,4'-MDI.

[0078] More particularly preferred are linear polyether urethane polymers containing isocyanate groups and having an NCO content ranging from 1% to 2.5% by weight, in particular from 1.3% to 2.1% by weight, and a diisocyanate monomer content of 0.3% or less by weight, which are obtained by reacting at least one diisocyanate monomer with a polyoxypropylene diol having an OH value ranging from 13 to 38 mg KOH / g, in particular from 22 to 32 mg KOH / g, in an NCO / OH ratio of at least 3 / 1, and then removing most of the diisocyanate monomer using a suitable separation method.The preferred diisocyanate monomer is IPDI or 4,4'-MDI, in particular 4,4'-MDI.

[0079] Mixtures of these two particularly preferred polyether urethane polymers are even more particularly preferred.

[0080] The moisture-curable polyurethane composition preferably further comprises at least one additional component selected from meltable components, blocked amines, fillers, plasticizers, diisocyanate oligomers, catalysts and stabilizers.

[0081] In one embodiment of the present invention, the moisture-curable polyurethane composition preferably further comprises at least one meltable component.

[0082] Suitable meltable components are in particular the room temperature solid polyester urethane polymers containing isocyanate groups which result from the reaction of at least one diisocyanate monomer, in particular 4,4'-MDI, with at least one crystalline polyester diol or polycarbonate diol.

[0083] Suitable polyesterdiols are in particular OH-functional polyesters of adipic acid or sebacic acid or dodecanedicarboxylic acid with butane-1,4-diol or hexane-1,6-diol.

[0084] Suitable polycarbonate diols are especially the OH-functional polycarbonates of hexane-1,6-diol.

[0085] Such polymers are typically solid at room temperature and have at least partially crystalline characteristics.

[0086] Such meltable components are suitable for adhesives that are applied first in a heated state, for example at a temperature of about 60° C., and have a high initial strength very quickly after application, so that the joined parts are self-supporting and do not need to be fixed. The meltable components are now in molten form in the adhesive heated by application, and crystallize as the applied adhesive cools. Furthermore, such meltable components are suitable for adhesives that are applied at ambient temperature, where the meltable components are in crystallized form, resulting in increased sag resistance. However, meltable components are difficult to handle, and the sag resistance obtained thereby is highly shear dependent, which can lead to problems in production and application. Furthermore, the meltable components make it difficult to extrude the adhesive at room temperature and at low ambient or bonding temperatures.

[0087] The dimer fatty acid based polyester urethane polymers of the present invention have a specific ratio of meltable components and allow for adhesives with better extrudability at room temperature and under low temperature conditions.

[0088] Furthermore, the polyester urethane polymers based on dimer fatty acids of the present invention allow for adhesives with very good sag resistance, where meltable components are used in much lower amounts or are completely free of meltable components.

[0089] In a further embodiment of the present invention, the moisture-curable polyurethane composition preferably further comprises at least one blocked amine.

[0090] Suitable blocked amines preferably have at least one aldimino or oxazolidino group, which upon contact with moisture can be hydrolyzed with release of an amino group and react with available isocyanate groups, promoting rapid blister-free curing, particularly non-sticky surfaces and / or particularly good mechanical properties.

[0091] Preferred oxazolidines are mono- or bis-oxazolidines, especially those derived from isobutyraldehyde, benzaldehyde or substituted benzaldehydes, especially benzaldehydes substituted in the para position with an optionally branched alkyl group having 10 to 14 carbon atoms.

[0092] Particularly preferred are monooxazolidines derived from N-alkylethanolamines, such as Nn-butylethanolamine, or bisoxazolidines from the reaction of OH-functional monooxazolidines derived from diethanolamine with diisocyanates, in particular hexane 1,6-diisocyanate.

[0093] Suitable aldimines are in particular di- or tri-aldimines from the reaction of commercially available primary di- or triamines with non-enolizable aldehydes, which are aldehydes that do not have a hydrogen atom in the alpha position to the carbon atom of the aldehyde group.

[0094] Preferred blocked amines are aldimines of formula (I) and (II) [ka] is selected from the group consisting of n is 2 or 3; A is an n-valent hydrocarbyl group optionally containing an ether oxygen and having a molecular weight in the range of 28 to 6,000 g / mol; R 1 and R 2are each independently a monovalent hydrocarbyl group having 1 to 12 carbon atoms or together a divalent hydrocarbyl group having 4 to 12 carbon atoms which is part of an optionally substituted carbocyclic ring having 5 to 8, preferably 6, carbon atoms; R 3 is hydrogen or a linear or branched alkyl, arylalkyl or alkoxycarbonyl group having 1 to 12 carbon atoms; R 4 is hydrogen or a monovalent hydrocarbyl group having 1 to 20 carbon atoms; R 5 is an alkyl or alkoxy group having 6 to 20 carbon atoms.

[0095] A is preferably an aliphatic, cycloaliphatic or arylaliphatic radical, in particular having a molecular weight in the range of 28 to 500 g / mol, in particular 1,6-hexylene, (1,5,5-trimethylcyclohexan-1-yl)methane-1,3,4(2)-methyl-1,3-cyclohexylene, 1,3-cyclohexylenebis(methylene), 1,4-cyclohexylenebis(methylene), 1,3-phenylenebis(methylene), 1,2-cyclohexylene, 1,3-cyclohexylene, 1,4-cyclohexylene, methylenebis(2-methylcyclohexan-4-yl), (bicyclo[2.2.1]heptane-2,5(2,6)-diyl)dimethylene, (tricyclo[5.2.1.0 ... 2,6 ]Decan-3(4),8(9)-diyl)dimethylene, average molecular weight M in the range of 170-500 g / mol n and an average molecular weight M in the range of 330 to 500 g / mol. n or glycerol-initiated tris(ω-polyoxypropylene) having the formula:

[0096] Preferably, R 1 and R 2 are each methyl.

[0097] Preferably, R3 is hydrogen.

[0098] Preferably, R 4 is methyl or undecyl.

[0099] Preferably, R 5 is an optionally branched alkyl group in the para position having 10 to 14 carbon atoms.

[0100] Particularly preferred blocked amines are N,N'-bis(2,2-dimethyl-3-lauroyloxypropylidene)hexylene-1,6-diamine, N,N'-bis(2,2-dimethyl-3-acetoxypropylidene)-3-aminomethyl-3,5,5-trimethylcyclohexylamine, N,N'-bis(2,2-dimethyl-3-lauroyloxypropylidene)-3-aminomethyl-3,5,5-trimethylcyclohexylamine, N,N'-bis(4-C 10~14 -alkylbenzylidene)-3-aminomethyl-3,5,5-trimethylcyclohexylamine, with average molecular weight M in the range of 450-880 g / mol n N,N'-bis(2,2-dimethyl-3-acetoxypropylidene)polyoxypropylenediamine having an average molecular weight M in the range of 750 to 1,050 g / mol n N,N'-bis(2,2-dimethyl-3-lauroyloxypropylidene)polyoxypropylenediamine having an average molecular weight M in the range of 680 to 1,100 g / mol n N,N'-bis(4-C 10~14 -alkylbenzylidene)polyoxypropylenediamine, with average molecular weight M in the range of 730-880 g / mol n N,N',N''-tris(2,2-dimethyl-3-acetoxypropylidene)polyoxypropylenetriamine having an average molecular weight M in the range of 1,150 to 1,300 g / mol n and N,N',N''-tris(2,2-dimethyl-3-lauroyloxypropylidene)polyoxypropylenetriamine having an average molecular weight M in the range of 1,000 to 1,350 g / mol. nN,N',N''-Tris(4-C 10~14 -alkylbenzylidene)polyoxypropylenetriamines.

[0101] Suitable fillers are in particular powdered or precipitated calcium carbonate, optionally coated with fatty acids, in particular stearic acid, barite, quartz flour, quartz sand, dolomite, wollastonite, calcined kaolin, sheet silicates, for example mica or talc, zeolites, aluminium hydroxide, magnesium hydroxide, silica, including finely divided silica from pyrolysis processes, cement, gypsum, fly ash, industrially produced carbon black, graphite, metal powders, for example of aluminium, copper, iron, silver or steel, PVC powder or lightweight fillers, for example hollow glass beads or gas-filled plastic spheres (microspheres), in particular the type available under the brand name Expancel® (from Akzo Nobel).

[0102] Calcium carbonate, calcined kaolin, micronized silica or industrially produced carbon black, optionally coated with a fatty acid, in particular stearic acid, are preferred.

[0103] Suitable plasticizers are in particular carboxyl esters, such as phthalates, in particular diisononyl phthalate (DINP), diisodecyl phthalate (DIDP) or di(2-propylheptyl)phthalate (DPHP), hydrogenated phthalates or cyclohexane-1,2-dicarboxylates, in particular hydrogenated diisononyl phthalate or diisononyl cyclohexane-1,2-dicarboxylate (DINCH), terephthalates, in particular bis(2-ethylhexyl)terephthalate (DOTP) or diisononyl terephthalate (DINT), hydrogenated terephthalates or cyclohexane-1,4-dicarboxylates, in particular hydrogenated bis(2-ethylhexyl)terephthalate or bis(2-ethyl hexyl)cyclohexane-1,4-dicarboxylate, or hydrogenated diisononyl terephthalate or diisononyl cyclohexane-1,4-dicarboxylate, isophthalates, trimellitates, adipates, in particular dioctyl adipate, azelates, sebacates, benzoates, glycol ethers, glycol esters, plasticizers having a polyether structure, in particular polypropylene oxide mono-, di- or triols having hydroxyl groups blocked in the form of acetate groups, organic phosphates or sulfonates, polybutenes, polyisobutenes, or plasticizers derived from natural fats or oils, in particular epoxidized soybean oil or linseed oil.

[0104] Preferred plasticizers are those having a phthalate or polyether structure.

[0105] Suitable diisocyanate oligomers are in particular HDI biurets, such as Desmodur® N100 or N3200 (from Covestro), Tolonate® HDB or HDB-LV (from Vencorex) or Duranate® 24A-100 (from Asahi Kasei); HDI isocyanurates, such as Desmodur® N3300, N3600 or N3790BA (all from Covestro), Tolonate® HDT, HDT-LV or HDT-LV2 (from Vencorex), Duranate® TPA-100 or THA-100 (from Asahi Kasei) or Coronate® HX (from Tosoh). Corp.); HDI uretdiones, such as Desmodur® N3400 (from Covestro); HDI iminooxadiazinediones, such as Desmodur® XP2410 (from Covestro); HDI allophanates, such as Desmodur® VP LS2102 (from Covestro); IPDI isocyanurates, either in solution, such as Desmodur® Z4470 (from Covestro), or in solid form, such as Vestanat® T1890 / 100 (from Evonik Industries); TDI oligomers, such as Desmodur® IL (from Covestro); or mixed isocyanurates based on TDI / HDI, such as Desmodur® HL (from Covestro).

[0106] Suitable catalysts are catalysts for accelerating the reaction of isocyanate groups, in particular organotin(IV) compounds, such as, in particular, dibutyltin diacetate, dibutyltin dilaurate, dibutyltin dichloride, dibutyltin diacetylacetonate, dimethyltin dilaurate, dioctyltin diacetate, dioctyltin dilaurate or dioctyltin diacetylacetonate, complexes of bismuth(III) or zirconium(IV) with ligands selected from alkoxides, carboxylates, 1,3-diketonates, oxinates, 1,3-ketoesterates and 1,3-ketoamidates, or compounds containing tertiary amino groups, such as, in particular, 2,2′-dimorpholinodiethyl ether (DMDEE).

[0107] If the moisture-curable polyurethane composition contains blocked amines, suitable catalysts are also catalysts for the hydrolysis of blocked amino groups, in particular organic acids, in particular carboxylic acids such as 2-ethylhexanoic acid, lauric acid, stearic acid, isostearic acid, oleic acid, neodecanoic acid, benzoic acid, salicylic acid or 2-nitrobenzoic acid, organic carboxylic acid anhydrides such as phthalic anhydride, hexahydrophthalic anhydride or methylhexahydrophthalic anhydride, silyl esters of carboxylic acids, organic sulfonic acids such as methanesulfonic acid, p-toluenesulfonic acid or 4-dodecylbenzenesulfonic acid, sulfonic acid esters, other organic or inorganic acids, or mixtures of the abovementioned acids and acid esters. Particular preference is given to carboxylic acids, in particular aromatic carboxylic acids such as benzoic acid, 2-nitrobenzoic acid or in particular salicylic acid.

[0108] Also particularly suitable are combinations of different catalysts.

[0109] Suitable stabilizers are in particular stabilizers against oxidation, heat, light or UV light, in particular titanium dioxide, iron oxide, zinc oxide, benzophenones, benzotriazoles, compounds which have a 2,6-di-tert-butylphenol group (for example those known under the trade name Irganox® (from BASF)), compounds which have a 2,2,6,6-tetramethylpiperidine group (referred to as HALS (hindered amine light stabilizers), for example those known under the trade name Tinuvin® (from BASF)), or phosphorus-containing compounds (for example those known under the trade name Irgafos® (from BASF)).

[0110] The moisture-curable polyurethane composition may further comprise additional additives, in particular inorganic or organic pigments, in particular titanium dioxide, chromium oxide or iron oxide; fibres, in particular glass fibres, carbon fibres, metal fibres, ceramic fibres, polymer fibres, for example polyamide fibres or polyethylene fibres, or natural fibres, for example wool, cellulose, hemp or sisal; - nanofillers, such as graphene or carbon nanotubes; - dye; - desiccant, in particular molecular sieve powder, calcium oxide, highly reactive isocyanates such as p-tosylisocyanate, monooxazolidines such as Incozol® 2 (from Incorez) or orthoformates; adhesion promoters, in particular organoalkoxysilanes, in particular epoxysilanes, such as, in particular, 3-glycidoxypropyltrimethoxysilane or 3-glycidoxypropyltriethoxysilane, (meth)acrylosilanes, anhydridosilanes, carbamatosilanes, alkylsilanes or iminosilanes, or oligomeric forms of these silanes, or titanates; - further catalysts which accelerate the reaction of isocyanate groups; rheology modifiers, in particular thickeners, in particular sheet silicates, for example bentonite, derivatives of castor oil, hydrogenated castor oil, polyamides, polyamide waxes, polyurethanes, urea compounds, fumed silica, cellulose ethers or hydrophobically modified polyoxyethylenes; solvents, in particular acetone, methyl acetate, tert-butyl acetate, 1-methoxy-2-propyl acetate, ethyl 3-ethoxypropionate, diisopropyl ether, diethylene glycol diethyl ether, ethylene glycol diethyl ether, ethylene glycol monobutyl ether, ethylene glycol mono-2-ethylhexyl ether, acetals such as propylal, butyral, 2-ethylhexylal, dioxolane, glycerol formal or 2,5,7,10-tetraoxaundecane (TOU), toluene, xylene, heptane, octane, naphtha, white spirit, petroleum ether or gasoline, in particular the Solvesso™ grades (from Exxon), and also propylene carbonate, dimethyl carbonate, butyrolactone, N-methylpyrrolidone, N-ethylpyrrolidone, p-chlorobenzotrifluoride or benzotrifluoride; natural resins, fats or oils, such as rosin, shellac, linseed oil, castor oil or soybean oil; - non-reactive polymers, in particular homo- or copolymers of unsaturated monomers from the group comprising ethylene, propylene, butylene, isobutylene, isoprene, vinyl acetate or alkyl (meth)acrylates, in particular polyethylene (PE), polypropylene (PP), polyisobutylene, ethylene / vinyl acetate copolymers (EVA) or atactic poly-α-olefins (APAO); - flame-retardant substances, in particular the aluminium hydroxide or magnesium hydroxide fillers already mentioned, and also in particular organic phosphates, such as, in particular, triethyl phosphate, tricresyl phosphate, triphenyl phosphate, diphenylcresyl phosphate, isodecyl diphenyl phosphate, tris(1,3-dichloro-2-propyl)phosphate, tris(2-chloroethyl)phosphate, tris(2-ethylhexyl)phosphate, tris(chloroisopropyl)phosphate, tris(chloropropyl)phosphate, isopropylated triphenyl phosphate, mono-, bis- or tris(isopropylphenyl)phosphates of different degrees of isopropylation, resorcinol bis(diphenyl phosphate), bisphenol A bis(diphenyl phosphate) or ammonium polyphosphate; additives, in particular wetting agents, levelling agents, defoamers, air release agents or biocides; or further substances which are customarily used in moisture-curable polyurethane compositions. may contain

[0111] It may be advisable to chemically or physically dry certain materials before incorporating them into the composition.

[0112] Preferably, the polyurethane composition of the present invention is substantially solvent-free, in particular containing less than 5% by weight, preferably less than 2.5% by weight of solvent, and most preferably, the polyurethane composition of the present invention is essentially solvent-free.

[0113] The moisture-curable polyurethane composition preferably comprises - 20% to 60% by weight of a polyether urethane polymer containing isocyanate groups, - 0.5% to 10% by weight of a polyester urethane polymer based on a dimeric fatty acid according to the invention containing isocyanate groups, - 0% to 5% by weight of meltable components; - 20% to 60% by weight of a filler, - 0% to 35% by weight of a plasticizer, and Optionally further components, in particular blocked amines, diisocyanate oligomers, catalysts or stabilizers Contains:

[0114] The moisture-curable polyurethane compositions of the present invention preferably contain less than 0.1% by weight of total diisocyanate monomers, and such compositions can be shipped and sold in many countries without hazardous material classification.

[0115] The moisture-curable polyurethane composition is in particular produced with the exclusion of moisture and stored in a moisture-tight container at ambient temperature. Suitable moisture-tight containers are in particular made of metal and / or plastic, optionally coated, in particular drums, transport boxes, hobbocks, buckets, canisters, cans, bags, tubular bags, cartridges or tubes.

[0116] The moisture-curable polyurethane composition may be in the form of a one-component composition or in the form of a multi-component, in particular a two-component, composition.

[0117] A composition that is referred to as a "one-component" composition is one in which all components of the composition are in the same container and are themselves storage stable.

[0118] A composition referred to as a "two-component" composition is one in which the components of the composition are in two different components that are stored in separate containers and are not mixed with each other until just before or during application of the composition.

[0119] The moisture-curable polyurethane composition is preferably a one-component composition, which, given proper packaging and storage, is typically shelf stable for several months, up to a year or more.

[0120] Application of the moisture-curable polyurethane composition initiates the curing process, which results in a cured composition.

[0121] In the case of a one-component composition, it is applied as such and then begins to harden under the influence of moisture or water. To accelerate the hardening, an accelerator component containing water and optionally a catalyst and / or a hardener can be mixed into the composition upon application, or the composition can be contacted with such an accelerator component after its application.

[0122] During the curing process, the isocyanate groups react with each other under the influence of moisture. If the moisture-curable polyurethane composition contains blocked amines, the isocyanate groups react further with the blocked amino groups as they are hydrolyzed. The overall reaction of the isocyanate groups that results in the curing of the composition is also referred to as crosslinking.

[0123] The moisture required for the curing of the moisture-curable polyurethane composition preferably enters the composition by diffusion from the air (atmospheric moisture). In this process, a solid layer of the cured composition ("skin") is formed on the surface of the composition, which is in contact with the air. The curing continues from the outside inwards in the direction of diffusion, and the skin becomes thicker and thicker, eventually surrounding the entire applied composition. Moisture can also enter the composition additionally or entirely from the substrate or substrates to which the composition is applied, and / or originate from accelerator components that are mixed into the composition during application or that come into contact with the composition after application, for example by painting or spraying.

[0124] The moisture-curable polyurethane composition is preferably applied at ambient temperatures in the range of about -10 to 50°C, preferably in the range of -5 to 45°C, in particular in the range of 0 to 40°C.

[0125] If desired, the moisture-curable polyurethane composition can also be applied in a heated state, for example at a temperature of about 60°C.

[0126] The moisture curable polyurethane composition preferably cures at ambient temperature.

[0127] Moisture curable polyurethane compositions have long processing times (open times) and rapid cure.

[0128] "Open time" refers to the period during which the composition can be worked or reworked after application without losing its ability to function. If the composition is used as an adhesive, the open time also refers in particular to the period within which bonding must be performed after its application in order for sufficient adhesion to develop. In the case of one-component compositions, the open time is exceeded at the latest when a skin is formed or when there is no longer sufficient adhesion to the substrate.

[0129] The moisture-curable polyurethane compositions are preferably used as elastic adhesives and / or sealants, in particular for bonding or sealing applications in the construction and manufacturing industries or in automotive assembly, in particular for parquet bonding, assembly, bonding of installable components, module bonding, pane bonding, joint sealing, body sealing, seam sealing or cavity sealing.

[0130] Elastic bonding in automotive assembly is, for example, the bonding attachment of parts, such as plastic covers, trim strips, flanges, fenders, cabs or other installable components to the painted body of an automobile or the bonding of panes to a vehicle body, said automobile being in particular a car, truck, bus, rail vehicle or ship. The use as an adhesive for glass replacement in automobiles is particularly preferred.

[0131] The moisture-curable polyurethane composition is preferably formulated to have a paste-like consistency with structurally viscous properties. This type of composition is applied using suitable equipment, for example from commercially available cartridges or drums or hobbies, in particular in the form of beads which may have an essentially circular or triangular cross-sectional area.

[0132] Suitable substrates which can be bonded and / or sealed with the moisture-curable polyurethane composition are in particular: - glass, glass-ceramic or screen-printed ceramic-coated glass or polycarbonate; - surface-finished metals or alloys, for example galvanized or chrome-plated metals, for example aluminium, copper, iron, steel, non-ferrous metals; - coated or painted substrates, in particular powder-coated metals or alloys or painted metal sheets; - paints or varnishes, in particular automotive topcoats; - cured adhesives, in particular based on polyurethanes, silane-modified polymers or polysulfides, in particular aged adhesives (residual adhesive beads) or body flanges with residual adhesive beads throughout or in places; - plastics, such as rigid or flexible PVC, polycarbonate, polystyrene, polyester, polyamide, PMMA, ABS, SAN, epoxy resins, phenolic resins, PUR, POM, TPO, PE, PP, EPM or EPDM, in each case untreated or surface-treated, for example by means of plasma, corona or flame; - fibre reinforced plastics, such as carbon fibre reinforced plastics (CFP), glass fibre reinforced plastics (GFP) and sheet moulding compounds (SMC); - repair or levelling compounds based on PCC (polymer modified cement mortar) or ECC (epoxy resin modified cement mortar); - insulating foams, in particular made of EPS, XPS, PUR, PIR, rock wool, mineral wool or expanded glass; - concrete, mortar, cement screed, fibre cement, in particular fibre cement boards, bricks, tiles, gypsum, in particular gypsum boards or anhydrous screeds, or natural stone, for example granite or marble, painted tiles or painted concrete, asphalt or bitumen; Leather, textiles, paper, wood, resins, e.g. wood materials bonded with phenolic, melamine or epoxy resins, resin / textile composites or further materials referred to as polymer composites. It is.

[0133] If necessary, the substrate can be pre-treated prior to application, especially by physical and / or chemical cleaning methods or by application of an activator or primer.

[0134] It is possible to bond and / or seal two identical or two different substrates.

[0135] The present invention further provides a method of bonding or sealing comprising: (i) a moisture-curable polyurethane composition as described above, - applying to a first substrate and contacting the composition with the second substrate within the open time of the composition; or - applied to a first and a second substrate and bonding the two substrates within the open time of the composition; or - application between two substrates, (ii) curing the composition by contact with moisture.

[0136] At least one of the substrates is preferably selected from the group consisting of glass, glass ceramic, screen printed and ceramic coated glass or polycarbonate, metals, alloys, powder coated metals or alloys, paints and varnishes and cured adhesives, in particular residual adhesive beads, and / or metal sheets painted with automotive topcoats.

[0137] The application and curing of the moisture-curing polyurethane composition, or the method of bonding or sealing, results in an article bonded or sealed with the composition, which may be an erected structure or part thereof, in particular an erected structure above or below ground level in civil engineering, a bridge, a roof, a staircase or a facade, or it may be an industrial or consumer item, in particular a window, a pipe, a rotor blade of a wind turbine, a domestic appliance or a means of transport, such as in particular a car, a bus, a truck, a rail car, a ship, an airplane or a helicopter, or an installable component thereof.

[0138] Thus, the present invention further provides articles resulting from the described methods of bonding or sealing.

[0139] It is particularly preferred to use this method of connection for the elastic joining of panes to motor vehicles, in particular for glass replacement.

[0140] The moisture-curing polyurethane composition has advantageous properties: particularly good bonding properties coupled with a long open time, particularly good application properties coupled with high sag resistance and short thread formation, particularly when the adhesive bead remains, particularly good extrudability, a non-glossy surface after curing coupled with good cure, strength, extensibility, elasticity and hazardous materials classification that do not change, and particularly good weatherability. Thus, the composition is particularly suitable as an elastic adhesive in automobile assembly, particularly for the replacement of defective elastically bonded windshields of automobiles. EXAMPLES

[0141] Examples intended to clarify the invention as described are presented herein below, the invention being of course not limited to these described examples.

[0142] "Standard Climatic Conditions" ("SCC") refers to a temperature of 23±1°C and a relative air humidity of 50±5%.

[0143] Unless otherwise stated, chemicals used were from Sigma-Aldrich Chemie GmbH.

[0144] Polyols used: Priplast® 1837: amorphous polyester diol based on dimeric fatty acids, OH value 110 mg KOH / g, liquid at room temperature (from Croda) Priplast® 1838: amorphous polyester diol based on dimeric fatty acids, OH value 56 mg KOH / g, liquid at room temperature (from Croda) Priplast® 3196: amorphous polyester diol based on dimeric fatty acids, OH value 37 mg KOH / g, liquid at room temperature (from Croda) Priplast® 3197: amorphous polyester diol based on dimeric fatty acids, OH value 56 mg KOH / g, liquid at room temperature (from Croda) Desmophen® 5031 BT: glycerol initiated ethylene oxide terminated polyoxypropylene triol, OH value 28 mg KOH / g (from Covestro) Acclaim® 4200: Polyoxypropylene diol, OH value 28 mg KOH / g (from Covestro) Dynacoll® 7360 room temperature solid semi-crystalline polyester diol, OH value 34 mg KOH / g (from Evonik)

[0145] Preparation of polymers containing isocyanate groups: Viscosity was measured with a thermostated Rheotec RC30 cone-plate viscometer (cone diameter 25 mm, cone angle 1°, cone tip-plate distance 0.5 mm, shear rate 50 s -1 ).

[0146] The diisocyanate monomer content was determined using HPLC (photodiode array detection; 0.04 M sodium acetate / acetonitrile as mobile phase) after prior derivatization with N-propyl-4-nitrobenzylamine.

[0147] Polymer DP-1: 597.5 g of Priplast® 1838 and 402.5 g of diphenylmethane 4,4′-diisocyanate (Desmodur® 44MC L, from Covestro) were reacted at 80° C. to give a polyester urethane polymer with an NCO content of 11.0 wt. %, a viscosity of 36 Pa·s at 20° C., and a diphenylmethane 4,4′-diisocyanate content of about 26 wt. %.

[0148] Subsequently, most of the volatile constituents, especially diphenylmethane 4,4'-diisocyanate, were removed by distillation in a short-path evaporator (jacket temperature 180°C, pressure 0.1-0.005 mbar, condensation temperature 47°C). The polyester urethane polymer thus obtained was slightly turbid and of liquid, viscous consistency at room temperature. It had an NCO content of 2.8% by weight, a viscosity of 312 Pa·s at 20°C, 119 Pa·s at 30°C, 48 Pa·s at 40°C and 11.5 Pa·s at 60°C, and a diphenylmethane 4,4'-diisocyanate content of 0.09% by weight.

[0149] Polymer DP-2: 445.0 g of Priplast® 1837 and 555.0 g of diphenylmethane 4,4′-diisocyanate (Desmodur® 44MC L, from Covestro) were reacted at 80° C. to give a polyester urethane polymer with an NCO content of 14.8 wt. %, a viscosity of 6.5 Pa·s at 20° C., and a diphenylmethane 4,4′-diisocyanate content of about 35 wt. %.

[0150] Subsequently, most of the volatile constituents, especially the diphenylmethane 4,4'-diisocyanate, were removed as described for polymer DP-1. The polyester urethane polymer thus obtained was slightly turbid and of liquid, viscous consistency at room temperature. It had an NCO content of 4.8% by weight, a viscosity of 11 Pa·s at 60°C, and a diphenylmethane 4,4'-diisocyanate content of 0.06% by weight.

[0151] Polymer DP-3: 663.0 g of Priplast® 3196 and 337.0 g of diphenylmethane 4,4′-diisocyanate (Desmodur® 44MC L, from Covestro) were reacted at 80° C. to give a polyester urethane polymer with an NCO content of 9.4 wt. %, a viscosity of 57 Pa·s at 20° C., and a diphenylmethane 4,4′-diisocyanate content of about 23 wt. %.

[0152] Subsequently, most of the volatile constituents, especially the diphenylmethane 4,4'-diisocyanate, were removed as described for polymer DP-1. The polyester urethane polymer thus obtained was slightly turbid and of liquid, viscous consistency at room temperature. It had an NCO content of 2.2% by weight, a viscosity of 17 Pa·s at 60°C, and a diphenylmethane 4,4'-diisocyanate content of 0.06% by weight.

[0153] Polymer DP-4: 600.0 g of Priplast® 3197 and 400.0 g of diphenylmethane 4,4′-diisocyanate (Desmodur® 44MC L, from Covestro) were reacted at 80° C. to give a polyester urethane polymer with an NCO content of 10.7 wt. %, a viscosity of 28 Pa·s at 20° C., and a diphenylmethane 4,4′-diisocyanate content of about 25 wt. %.

[0154] Subsequently, most of the volatile constituents, especially the diphenylmethane 4,4'-diisocyanate, were removed as described for polymer DP-1. The polyester urethane polymer thus obtained was slightly turbid and of liquid, viscous consistency at room temperature. It had an NCO content of 2.8% by weight, a viscosity of 16 Pa·s at 60°C, and a diphenylmethane 4,4'-diisocyanate content of 0.08% by weight.

[0155] Polymer DP-5: 620.0 g of Priplast® 1838 and 379.9 g of 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (Vestanat® IPDI, from Evonik) were reacted at 80° C. in the presence of 0.01 g of dibutyltin dilaurate to give a polyester urethane polymer with an NCO content of 11.8 wt. %, a viscosity of 17 Pa·s at 20° C., and a 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane content of about 20 wt. %.

[0156] Subsequently, most of the volatile constituents, especially 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane, were removed by distillation in a short-path evaporator (jacket temperature 160°C, pressure 0.1-0.005 mbar). The polyester urethane polymer thus obtained was slightly turbid and of liquid, viscous consistency at room temperature. It had an NCO content of 3.1% by weight, a viscosity of 153 Pa·s at 20°C, and a 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane content of 0.23% by weight.

[0157] Polymer PP-1: 725.0 g of Desmophen® 5031BT and 275.0 g of diphenylmethane 4,4′-diisocyanate (Desmodur® 44MC L, from Covestro) were reacted by known methods to give a polyether urethane polymer with an NCO content of 7.6 wt. %, a viscosity of 6.5 Pa·s at 20° C., and a diphenylmethane 4,4′-diisocyanate content of about 20 wt. %.

[0158] Subsequently, most of the volatile constituents, especially the diphenylmethane 4,4'-diisocyanate, were removed as described for polymer DP-1. The polyetherurethane polymer thus obtained had an NCO content of 1.7% by weight, a viscosity of 19 Pa s at 20°C, and a diphenylmethane 4,4'-diisocyanate content of 0.04% by weight.

[0159] Polymer PP-2: 727.0 g of Acclaim® 4200 and 273.0 g of diphenylmethane 4,4′-diisocyanate (Desmodur® 44MC L, from Covestro) were reacted by known methods to give a polyether urethane polymer having an NCO content of 7.6 wt. %, a viscosity of 5.2 Pa·s at 20° C., and a diphenylmethane 4,4′-diisocyanate content of about 18 wt. %.

[0160] Subsequently, most of the volatile constituents, especially the diphenylmethane 4,4'-diisocyanate, were removed as described for polymer DP-1. The polyetherurethane polymer thus obtained had an NCO content of 1.8% by weight, a viscosity of 15.2 Pa s at 20°C, and a diphenylmethane 4,4'-diisocyanate content of 0.08% by weight.

[0161] Polymer M: 1000 g of Dynacoll® 7360 and 142 g of diphenylmethane 4,4′-diisocyanate (Desmodur® 44MC L, from Covestro) were reacted at 80° C. to give a room temperature solid polymer with an NCO content of 2.0 wt. % and a diphenylmethane 4,4′-diisocyanate content of 2.3 wt. %.

[0162] Polymers DP-1 to DP-5 are polyester urethane polymers based on dimer fatty acids. Polymers PP-1 and PP-2 are polyether urethane polymers. Polymer M is a room temperature solid polymer used as the meltable component.

[0163] Moisture-curable polyurethane compositions: Compositions Z1~Z5: For each composition, the specific ingredients in Table 1 were thoroughly mixed in the specific amounts (in parts by weight) using a planetary mixer under reduced pressure with the exclusion of moisture, and the compositions were dispensed into tubular bags with airtight seals and stored at room temperature.

[0164] For rapid hardening, a water-containing accelerator component was added to the composition at the time of application. For this purpose, the composition was applied from a PowerCure dispenser (available from Sika Schweiz AG) with the metered addition of 2% by weight of water-containing paste into the composition by squeezing and mixing with a dynamic mixer.

[0165] The adhesion to the residual adhesive bead was determined on the cured and aged adhesive layer. For this purpose, a commercial polyurethane adhesive for bonding panes (Sikaflex®-250SV-3, from Sika Automotive Hamburg GmbH) was applied to the glass body in the form of a triangular bead with a width of about 8 mm and a height of about 10 mm, covered with a silicone-coated release paper, pressed to a layer thickness of about 5 mm, cured under standard climatic conditions for 7 days, the release paper was removed and the compressed adhesive bead was aged at 80° C. for 14 days. Subsequently, the cured and aged adhesive bead was cut from the glass body to a layer thickness of about 1 mm.

[0166] The accelerated composition was then applied under standard climatic conditions from a PowerCure dispenser in the form of a triangular bead about 8 mm wide and about 10 mm high to a strip of silicone-coated release paper. In each case, after the waiting time specified in Table 1, the triangular bead applied to the release paper was turned over and placed on the residual adhesive bead remaining on the glass body with the release paper on top and the composition in contact with the residual adhesive bead. The composition was subsequently pressed to a layer thickness of about 5 mm and cured under standard climatic conditions for 7 days, then the release paper was removed and the adhesion of the cured composition on the residual adhesive bead was tested by making an incision in the cured composition at the narrow end directly above the bonding surface, holding the incised end of the composition with rounded tweezers and trying to pull the composition away from the substrate (=residual adhesive bead). The composition was then cut again to the substrate, the cut-out part was rolled up with rounded tweezers and an attempt was made to pull the composition away from the substrate again. In this way, the composition was cut away from the substrate by pulling it away. The bonds were then assessed for failure profile using the following scale: "Very good" represents greater than 95% cohesive failure; "Good" represents 75% to 95% cohesive failure; "Moderate" represents 50%-75% cohesive failure; "Poor" refers to less than 50% cohesive failure; "No adhesion" represents 0% cohesive failure or 100% adhesive failure.

[0167] The results are reported in Table 1.

[0168] The composition labeled "(Reference)" is a comparative example.

[0169] [Table 1]

[0170] Compositions Z6 and Z7: Each composition was prepared as described for composition Z1 using the components identified in Table 2 in the amounts (in parts by weight) identified, dispensed into aluminum cartridges with airtight seals, and stored at room temperature.

[0171] Each composition was applied between two silicone-coated release papers, pressed into a 2 mm thick film, and stored under standard climatic conditions for 14 days.After removing the release papers, square test specimens (75×150 mm) were cut from the cured film and tested in a QUV weathering device for the time specified in Table 2, and then the weathered surface was tested for carbon black staining by first manually pressing a transparent adhesive tape onto the surface, and then attaching it to white printer paper.Carbon black staining was rated as "no" if a light gray stain was visible, rated as "moderate" if the carbon black stain was a dark gray stain, and rated as "severe" if the carbon black stain was a black stain.

[0172] The results are reported in Table 2.

[0173] The composition labeled "(Reference)" is a comparative example.

[0174] [Table 2]

[0175] Compositions Z8~Z16: Each composition was prepared as described for composition Z1 using the components specified in Tables 3 and 4 in the amounts specified (in parts by weight), dispensed into aluminum cartridges with airtight seals, and stored at room temperature.

[0176] Each composition was tested as follows: The measures determined for the processability or applicability of the composition are compression force, sag resistance and thread formation. Low compression force, high sag resistance and short thread formation are representative of good processability or applicability.

[0177] The compression force was determined at 23° C. and 5° C. The first closed cartridge was stored for 7 days at 23° C., the second for 6 days at 23° C. and then for 24 hours at 5° C. The compression force was then measured in each case using an extrusion device (Zwick / Roell Z005) by screwing a nozzle with an internal diameter of 5 mm onto the cartridge and then measuring the force required to extrude the composition through the nozzle at an extrusion speed of 60 mm / min. The reported value is the average of the forces measured after compression distances of 22 mm, 24 mm, 26 mm and 28 mm.

[0178] The sag resistance of each composition was determined by applying triangular beads approximately 8 mm wide and 20 mm high to a vertical corrugated cardboard surface under standard climatic conditions in such a way that the triangular beads were arranged as a horizontal strip 8 mm wide with a protruding height (=tip) of 20 mm. After curing under standard climatic conditions, an assessment was made as to whether and how the position of the applied beads changed. More specifically, the extent to which the tip, measured from a horizontal position, sagged downwards was determined. A sag of less than 1 mm was rated as "very good", 1-3 mm as "good", 4-7 mm as "average" and 8 mm or more as "poor". A "liquid" composition is defined as one in which the applied material moves downwards, i.e. sags downwards, not only at the tip of the applied triangular bead, but also at the base.

[0179] Thread formation was determined for several compositions by measuring the length of the thread formed by moving the application cartridge away from the triangular bead that was applied for sag resistance determination.

[0180] The measure determined for the processing time (open time) was the skin time. For this purpose, a few grams of the composition were applied under standard climatic conditions to a cardboard sheet in a layer thickness of about 2 mm, and the first period was determined during which no residues were left on an LDPE pipette that was then used to gently tap the surface of the composition.

[0181] For the determination of the mechanical properties, each composition was pressed between two silicone-coated release papers to obtain a film 2 mm thick and stored under standard climatic conditions for 14 days. After removing the release papers, several test specimens were punched out and tested as described below.

[0182] For the determination of tensile strength ("TS"), elongation at break (EaB) and modulus at 0.5-5% elongation, the films were die-cut into dumbbells having a length of 75 mm with a bar length of 30 mm and a bar width of 4 mm, which were tested according to DIN EN53504 at a strain rate of 200 mm / min.

[0183] Some test specimens were also punched out for the determination of the tear resistance and tested according to DIN ISO 34 at a strain rate of 500 mm / min.

[0184] Appearance and gloss were determined visually to determine the mechanical properties of the resulting films. "Satisfactory" was used to describe a non-tacky flat film with no blistering.

[0185] To determine the strength of the adhesive bond, the overlap shear strength (LSS) for some compositions was determined on glass. For this purpose, composite specimens were produced by bonding two glass plates, degreased with isopropanol and pretreated with Sika® Aktivator 100 (from Sika Schweiz), in such a way that the overlapping adhesive bond had dimensions of 12×25 mm and a thickness of 4 mm, with the glass plates protruding at the tips. After storing the composite specimens under standard climatic conditions for 14 days, the overlap shear strength was tested according to DIN EN 1465 at a strain rate of 20 mm / min. As a measure of the thermal and hydrolytic stability of the bond, further test specimens were further stored in an air-circulating oven at 100° C. for 7 days or at 70° C. / 100% relative humidity for 7 days, cooled under standard climatic conditions and tested in the same way. The results are indicated with the addition "14d SCC" or "7d 100° C." or "7d 70 / 100".

[0186] The results are reported in Tables 3 and 4.

[0187] The composition labeled "(Reference)" is a comparative example.

[0188] [Table 3]

[0189]

Table 4

Claims

1. A method for producing a polyester urethane polymer that contains isocyanate groups and is liquid at room temperature, comprising the steps of: reacting at least one diisocyanate monomer with a polyester diol based on dimeric fatty acid having an OH number in the range of 28 to 120 mg KOH / g in an NCO / OH ratio of at least 4 / 1, and subsequently removing most of the diisocyanate monomer by a separation process which is a distillation process; Including, the polyester urethane polymer having an NCO content ranging from 1.5% to 6% by weight and a diisocyanate monomer content of 0.5% by weight or less; A method for producing a polyester urethane polymer.

2. The method of claim 1, wherein the polyester urethane polymer is produced without the use of any polyol other than the polyester diol based on the dimer fatty acid.

3. 3. The method for producing a polyester urethane polymer according to claim 1, wherein the diisocyanate monomer is diphenylmethane 4,4'-diisocyanate.

4. A process for the preparation of polyester urethane polymers according to any one of claims 1 to 3, characterized in that the polyester diol based on dimer fatty acid is amorphous.

5. The method for producing a polyester urethane polymer according to any one of claims 1 to 4, characterized in that the NCO / OH ratio is in the range of from 4 / 1 to 10 / 1.

6. A cone-plate viscometer having a cone diameter of 25 mm, a cone angle of 1°, and a cone tip-plate distance of 0.5 mm was used for 50 s -1 6. A method for producing a polyester urethane polymer according to claim 1, characterized in that the polyester urethane polymer has a viscosity in the range of 100 to 1,000 Pa·s at 20° C., measured at a shear rate of 100 to 1,000 Pa·s.

7. Use of a polyester urethane polymer produced by the process according to any one of claims 1 to 6 as an adhesion promoter in a moisture curable polyurethane composition.

8. The use according to claim 7, characterized in that the polyester urethane polymer is used in an amount ranging from 0.5% to 15% by weight, based on the total polyurethane composition.

9. A method for producing a moisture-curable polyurethane composition suitable as an elastic adhesive and / or sealant, comprising: at least one polyether urethane polymer containing isocyanate groups, and - a polyester urethane polymer containing isocyanate groups, produced by the process according to any one of claims 1 to 6 mixing the The moisture-curable polyurethane composition is liquid, optionally pasty, at a temperature of 23° C., thereby having good room temperature processability. method.

10. A method for producing a moisture-curable polyurethane composition according to claim 9, characterized in that the polyether segments in the polyether urethane polymer consist of at least 80% 1,2-propyleneoxy units and optionally further 1,2-ethyleneoxy units.

11. A method for producing a moisture-curable polyurethane composition according to claim 9 or 10, characterized in that the polyether urethane polymer has an NCO content in the range of 1% to 5% by weight.

12. 12. A method for producing a moisture-curable polyurethane composition according to any one of claims 9 to 11, characterized in that at least one further component selected from meltable components, blocked amines, fillers, plasticizers, diisocyanate oligomers, catalysts and stabilizers is present in the composition.

13. A method for producing the moisture-curable polyurethane composition of any one of claims 9 to 12, comprising: The composition, - from 20% to 60% by weight of a polyether urethane polymer containing isocyanate groups, - 0.5% to 10% by weight of said polyester urethane polymer based on dimeric fatty acids containing isocyanate groups, - 0% to 5% by weight of meltable components, - 20% to 60% by weight of a filler, and - 0% to 35% by weight of plasticizer The method of claim 1, further comprising:

14. A method for producing a moisture-curable polyurethane composition described in any one of claims 9 to 13, characterized in that the composition contains less than 0.1 weight percent diisocyanate monomer in total.

15. A method of bonding or sealing comprising the steps of: (i) a polyurethane composition produced by the method according to any one of claims 9 to 14, - applying to a first substrate and contacting said composition with a second substrate within the open time of said composition; or - applied to a first and a second substrate and bonding the two substrates together within the open time of the composition; or - application between two substrates; (ii) curing said composition by contact with moisture.

Citation Information

Patent Citations

  • Method for producing isocyanate-terminated prepolymer, one-component moisture-curing urethane composition, two-component curing urethane composition, and method for producing polyurethane

    JP2007332241A

  • One-part polyurethane adhesive with high green strength

    US20180305597A1

  • Thermoplastic moisture cure polyurethanes

    US6355317B1