How to prevent inner bead peeling
The method stabilizes inner bead shape in welded steel pipes by using a high-frequency induction heating process with inert gas cooling to suppress peeling, addressing the issue of internal bead peeling and ensuring stable transportation.
Patent Information
- Application Number
- JP2021013480
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-29
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-01-29
AI Technical Summary
Internal beads in welded steel pipes can partially peel off due to variations in oxidation, causing damage and transportation issues, despite existing methods that smooth the inner bead surface.
A method involving a high-frequency induction heating process with an impeder and inert gas cooling to stabilize the inner bead shape and suppress peeling, using a multistage forming roll, squeeze roll, and inert gas shielding to prevent oxidation and maintain a stable bead form.
The method stabilizes the inner bead shape without cutting or crushing, effectively suppressing peeling and preventing damage during transportation.
Smart Images

Figure 0007573452000001 
Figure 0007573452000002 
Figure 0007573452000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing welded steel pipes in which a strip of steel is bent into a cylindrical shape, heated by high-frequency induction current, and both ends of the strip of steel are welded, and relates to a method for suppressing peeling of the inner bead that occurs inside the pipe. [Background technology]
[0002] As one method for manufacturing metal pipes, a method for manufacturing welded steel pipes is generally known, in which a metal strip is formed into a cylindrical shape to form an open pipe, and both end faces of the open pipe are welded to form a pipe shape. The welding process in this manufacturing method is performed by raising the end faces of the open pipe to a melting temperature using a high-frequency induction heating coil, and pressure welding both end faces of the open pipe with a squeeze roll. In addition, in this welding method, when both end faces of the open pipe are pressure welded, weld beads, which are raised weld marks, are generated.
[0003] For example, Patent Document 1 discloses a method of crushing a weld bead (inner surface bead) formed on the inner surface of a welded steel pipe with a jig to smooth the inner surface of the welded steel pipe. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6058410 Summary of the Invention [Problem to be solved by the invention]
[0005] The device for smoothing the inner bead of a welded steel pipe as shown in Patent Document 1 can easily and reliably smooth the inner bead of a welded steel pipe. On the other hand, in the manufacture of welded steel pipes in which the inner bead is permitted due to the product specifications, a process for crushing such an inner bead or a known process for removing the inner bead by cutting or the like has not been required.
[0006] However, the inner bead formed on the inner wall surface of the welded steel pipe may peel off partially from the inner wall surface due to variations in the degree of oxidation, etc., and such partial peeling may lead to problems such as damage to the blade when cutting the welded steel pipe. Furthermore, even after the welded steel pipe is cut, the peeled inner bead may remain inside the pipe, which may cause problems during transportation.
[0007] Therefore, the present invention has been made in consideration of the above-mentioned matters, and provides a method for suppressing peeling of the inner bead of a welded steel pipe, which can stabilize the shape of the inner bead without cutting or crushing the inner bead, and suppress partial peeling of the inner bead. [Means for solving the problem]
[0008] The present invention has been made to achieve the above object and has the following features.
[0009] The method for controlling inner bead peeling of a welded steel pipe according to the present invention includes the steps of forming a steel strip into an open pipe by a multi-stage forming roll, heating an end face weld of the open pipe by a high-frequency induction heating coil, compressing the heated end face weld with a squeeze roll, cooling an impedancer by a liquefied inert gas, generating an inert gas during cooling by the liquefied inert gas, and spraying the inert gas onto the end face weld. The impedancer includes an outer cylinder holder and is disposed inside the open tube. An annular gap is formed between the impedancer and the outer cylinder holder. The impedancer is disposed eccentrically with respect to the inner diameter of the outer cylinder holder. It is characterized by:
[0010] In the method for controlling inner bead peeling of a welded steel pipe according to the present invention, ,before One end of the outer cylinder holder is located upstream of the end face welded portion, and the other end of the outer cylinder holder is connected to a cooling nozzle for injecting the liquefied inert gas. Can It is preferable that:
[0011] In the method for controlling inner bead peeling of a welded steel pipe according to the present invention, ,before It is preferable that the annular gap is disposed so that the wider gap is located on the welded portion side.
[0012] Inner bead peeling of the welded steel pipe according to the present invention restraint In the method, the welded steel pipe to be formed into the open pipe is preferably a stainless steel pipe.
[0013] The above summary of the invention does not list all of the features necessary for the present invention, and any subcombination of these features may also constitute an invention. Effect of the Invention
[0014] According to the present invention, the shape of the inner bead can be stabilized without cutting or crushing the inner bead, and partial peeling of the inner bead can be suppressed. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a flow chart showing a manufacturing process for a welded steel pipe according to the present embodiment. [Diagram 2] FIG. 1 is a perspective view showing a welding process according to an embodiment of the present invention; [Diagram 3] FIG. 13 is a perspective view showing an example of peeling of an inner bead [Figure 4] Cross section AA of Figure 3 [Diagram 5] Cross section B-B of Figure 3 [Figure 6] FIG. 1 is a perspective view showing an example of a welded steel pipe in which the inner bead peels off and cutting is poor. [Figure 7] 1 is a cross-sectional view showing a welding process according to the embodiment; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Preferred embodiments for carrying out the present invention will be described below with reference to the drawings. Note that the following embodiments do not limit the inventions according to the claims, and all of the combinations of features described in the embodiments are not necessarily essential to the solution of the invention.
[0017] FIG. 1 is a flow diagram showing the manufacturing process of a welded steel pipe according to this embodiment, FIG. 2 is an oblique view showing the welding process according to this embodiment, FIG. 3 is an oblique view showing an example of peeling of an inner bead, FIG. 4 is a cross-sectional view taken along line AA of FIG. 3, FIG. 5 is a cross-sectional view taken along line BB of FIG. 3, FIG. 6 is an oblique view showing an example of a welded steel pipe that has a cutting defect due to peeling of an inner bead, and FIG. 7 is a cross-sectional view showing the welding process according to this embodiment.
[0018] The method for suppressing peeling of an inner bead according to this embodiment is performed by the steps shown in Fig. 1 and is included in a part of a method for manufacturing a welded steel pipe. The welded steel pipe according to this embodiment includes a stainless steel pipe, a carbon steel pipe, an alloy steel pipe, etc.
[0019] First, an outline of the manufacturing method of the welded steel pipe in this embodiment will be described. In the following description, the terms "upstream" and "downstream" refer to the upstream and downstream directions of the steel material in the forming machine in the manufacturing process of the welded steel pipe.
[0020] In the manufacturing method of the welded steel pipe in this embodiment, first, as shown in FIG. 1, a steel plate is cut to a predetermined width according to the outer diameter of the pipe to be manufactured, to prepare a steel strip as a material for the welded steel pipe. Then, if necessary, the longitudinal end of the cut steel strip is welded to the end portion already loaded in the forming machine, to prepare a steel strip of a length that can continuously manufacture the welded steel pipe. Next, the flat steel strip is loaded into the forming machine and gradually formed into a cylindrical shape by multi-stage forming rolls. The steel strip formed into a cylindrical shape is formed into an open pipe 1 with a part open as shown in FIG. 2, with both ends in the width direction facing each other. As shown in FIG. 2, the open pipe 1 with a part open is pressed at both end faces 1a, 1b by the squeeze roll 3 to form a contact point 1c.
[0021] As shown in Figure 2, a high-frequency induction heating coil 2 is installed upstream of the squeeze roll 3 so as to surround the outer circumference of the open tube 1, and a high-frequency current flows through the high-frequency induction heating coil 2. As a result, a high-frequency magnetic field is generated from the high-frequency induction heating coil 2, and an eddy current flows through the open tube 1 along the contact point 1c. The contact point 1c is rapidly heated by the Joule heat of the eddy current generated at this time, and reaches its melting temperature. The contact point 1c, which is heated and melted by the high-frequency induction heating coil 2, is crimped and joined as it passes through the squeeze roll 3, completing the welding of both end faces 1a, 1b. The welded steel pipe 1d then undergoes cutting, straightening, and, if necessary, heat treatment, and various inspections to complete the process.
[0022] Next, the welding process in this embodiment will be described in detail.
[0023] As shown in FIG. 2, an impedancer 4 is inserted inside the open tube 1. As shown in FIG. 7, the impedancer 4 passes inside the high-frequency induction heating coil 2, and the downstream end of the impedancer 4 is located slightly upstream of the contact point 1c. The downstream end of the impedancer 4 can have any shape, and may have an inclined shape as shown in FIG. 7. The impedancer 4 is made of a ferromagnetic material such as ferrite or electromagnetic steel sheet, and collects the magnetic flux generated by the high-frequency induction heating coil 2 to efficiently heat the contact point 1c. Note that the impedancer 4 itself heats up to a high temperature due to the generation of eddy currents, so it is necessary to cool the impedancer 4 as described below.
[0024] When the steel pipe 1d welded by the above-mentioned procedure is pressed by the squeeze rolls 3, a linear inner bead 10 is generated at the joint between both end faces 1a, 1b on the inner surface of the steel pipe 1d, as shown in FIG. 3. The inner bead 10 generated on the cross section of the welded steel pipe 1d is usually formed at a substantially constant height h from the inner surface of the welded steel pipe 1d, as shown in FIG. 4. Depending on the application of the completed welded steel pipe, the presence of such an inner bead 10 may not be a problem, and in such a case, the process of removing the inner bead 10 by cutting or crushing can be omitted. In this embodiment, the height h of the inner bead 10 is, for example, 1.2 mm, regardless of the outer and inner diameters of the welded steel pipe 1d.
[0025] On the other hand, as shown in FIG. 5, peeling g may occur in a part of the inner bead 10 formed in a line shape. It is speculated that the cause of such partial peeling g is the variation in the degree of oxidation of the inner bead 10. If such partial peeling g occurs, as shown in FIG. 6, when cutting the welded steel pipe 1d, the blade 20 such as a pipe cutter may not come into contact with the inner bead 10, and the inner bead 10 may not be cut. In this way, if the welded steel pipe 1d is not completely separated even after the cutting process, there is a risk of damage to the blade 20 or trouble such as failure of the manufacturing equipment in the subsequent process. Therefore, as described later, if the inner bead 10 is not removed, it is necessary to suppress the oxidation of the inner bead 10 and the peeling g.
[0026] Next, a method for cooling the impedance 4 that has become heated to a high temperature will be described.
[0027] As shown in FIG. 2, a cylindrical outer tube holder 5 is installed on the outside of the impeder 4, and an annular gap 6 is formed between the impeder 4 and the outer tube holder 5. The impeder 4 is installed eccentrically with respect to the inner diameter of the outer tube holder 5, and the annular gap 6 also has a gap 6a that is widely open in a part of the radial direction. As shown in FIGS. 2 and 7, the gap 6a is located at approximately the same angle as the angle at which the contact point 1c of the open tube 1 is located. In addition, the downstream end of the outer tube holder 5 is located downstream of the end face of the impeder 4 and slightly upstream of the contact point 1c. The downstream end of the outer tube holder 5 may have any shape, and may have an inclined shape as shown in FIG. 7.
[0028] A cooling nozzle 7 is installed on the upstream side of the outer cylinder holder 5, and the cooling nozzle 7 is connected to a liquid nitrogen supply source (not shown). Liquid nitrogen supplied from the liquid nitrogen supply source is sprayed onto the impeder 4 through the cooling nozzle 7 to cool the impeder 4. The liquid nitrogen sprayed onto the impeder 4 is vaporized into an inert gas, which is supplied to the annular gap 6 to cool the entire impeder 4. The inert gas that has cooled the impeder 4 is then discharged into the open pipe 1 from the downstream side of the outer cylinder holder 5. Note that although the connection between the cooling nozzle 7 and the outer cylinder holder 5 is not shown, it is connected to block the upstream end face of the outer cylinder holder 5 so that the inert gas does not flow to the upstream side. In this embodiment, the liquefied inert gas used for cooling has been described as liquid nitrogen, but this is not limited thereto, and a liquefied inert gas such as liquefied helium may be used.
[0029] Next, a method for suppressing oxidation and peeling of the inner bead 10 will be described.
[0030] It is generally known that when steel is welded, nitrogen or oxygen in the air dissolves in the molten metal, causing welding defects such as porosity. For this reason, a method is known in which a shielding gas that does not react with the molten metal is filled around the welded area to prevent contact between the molten metal and the air. As described above, the inert gas generated when the impedancer 4 is cooled is released into the open pipe 1 from the downstream side of the outer cylinder holder 5, and can become a shielding gas that covers the molten area.
[0031] As described above, the downstream end of the outer cylinder holder 5 is located slightly upstream of the contact point 1c, which is the melting point, and the wide gap 6a of the annular gap 6 is at the same angle as the side where the contact point 1c is located, so that the inert gas can be discharged from the vicinity of the contact point 1c, and the melting point can be covered with the inert gas efficiently. Generally, the fluid flowing through the annular gap flows at a higher rate in an eccentric annular gap than in a concentric annular gap, so that the inert gas can be sufficiently sent into the open pipe 1. In addition, the inert gas ejected from the gap 6a is subjected to vaporization pressure, so that the ejected inert gas presses the inner bead 10, forming the inner bead 10 having a linear and stable shape.
[0032] As described above, in this embodiment, the inert gas generated by cooling the impedancer 4 is utilized to block air from the molten metal and prevent welding defects, and the vaporization pressure of the inert gas is used to form an inner bead 10 with a stable shape and suppress peeling g of the inner bead 10.
[0033] In the above description, the downstream end surface of the outer cylinder holder 5 is a cut surface of a cylinder, but the shape of the downstream end surface of the outer cylinder holder 5 is not limited to this, and it may be in the form of a nozzle that actively sprays inert gas toward the contact point 1c. It is clear from the claims that such modified or improved forms are also included in the technical scope of the present invention. [Explanation of symbols]
[0034] 1 Open tube 1a, 1b end face 1c contact point 1d Welded Steel Pipe 2 High frequency induction heating coil 3 Squeeze Roll 4 Impeder 5 External cylinder holder 6 Annular gap 6a Wide Open Gap 7 Cooling nozzle 10 Inner bead 20 Knives h (height of inner bead) g Peeling off (of the inner bead)
Claims
1. forming the strip steel into an open tube by multiple forming rolls; Heating the end face weld of the open pipe by a high frequency induction heating coil; a step of pressing the heated end face welded portion with a squeeze roll; cooling the impeller with a liquefied inert gas; generating an inert gas during cooling with the liquefied inert gas; spraying the inert gas onto the end face weld; The impedancer includes an outer cylinder holder and is disposed inside the open tube. An annular gap is formed between the impedancer and the outer cylinder holder, The impedancer is disposed eccentrically with respect to the inner diameter of the outer cylinder holder. A method for suppressing peeling of an inner bead of a welded steel pipe, comprising:
2. The method for suppressing peeling of an inner bead of a welded steel pipe according to claim 1, one end of the outer cylinder holder is located upstream of the end face welded portion, A cooling nozzle for injecting the liquefied inert gas is connected to the other end of the outer cylinder holder. A method for suppressing peeling of an inner bead of a welded steel pipe, comprising:
3. The method for suppressing peeling of an inner bead of a welded steel pipe according to claim 2, The wide gap of the annular gap is positioned on the end face weld side. A method for suppressing peeling of an inner bead of a welded steel pipe, comprising:
4. The method for suppressing peeling of an inner bead of a welded steel pipe according to any one of claims 1 to 3, The welded steel pipe to be formed into the open pipe is a stainless steel pipe. A method for suppressing peeling of an inner bead of a welded steel pipe, comprising:
Citation Information
Patent Citations
Olefin polymer composition
JP1985058410A
Impeder case for electric welded steel pipe manufacturing device
JP1989178380A
Gas shield welding equipment for electric resistance welded tube
JP1998249547A
Inner surface bead smoothing method and device of welding steel pipe
JP2014147939A
Welding method for electroseamed steel pipe using seal box
JP2014188569A