Method for manufacturing substrate laminate

By forming curable resin patterns on substrates and molding them to achieve precise bonding, the method addresses uniformity and reliability issues in adhesive layers, enhancing substrate laminate quality for MEMS sensors.

JP7573468B2Active Publication Date: 2024-10-25KANEKA CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021048012
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-23
Publication Date
2024-10-25
Estimated Expiration
2041-03-23

AI Technical Summary

Technical Problem

Conventional methods for applying adhesive layers in substrate laminates, such as those used in MEMS sensors, face challenges with uniformity and surface quality, leading to variations in bonding height and reliability.

Method used

A method involving forming a first pattern of curable resin on a substrate using a printing technique, followed by molding to create a second pattern, and bonding the substrates together via this pattern, ensuring precise control over height and surface roughness.

Benefits of technology

This approach results in a substrate laminate with stable bonding surfaces and reduced individual differences, suitable for manufacturing hollow structures in CMOS/CCD sensors and MEMS devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573468000002
    Figure 0007573468000002
  • Figure 0007573468000003
    Figure 0007573468000003
  • Figure 0007573468000004
    Figure 0007573468000004
Patent Text Reader

Abstract

To provide a manufacturing method for a substrate laminate having an adhesive layer with high adhesion reliability by forming a pattern of a curable resin having a good shape as an adhesive layer.SOLUTION: A manufacturing method for a substrate laminate includes the steps of forming a first pattern 1 of a curable resin on a first substrate 2 using a printing method, molding the first pattern to form a second pattern 4, and bonding the first substrate and the second substrate together with the second pattern interposed therebetween.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a substrate laminate. [Background technology]

[0002] In MEMS sensors such as image sensors, acceleration sensors, and pressure sensors, in order to adjust light transmittance and ensure the movement of mechanical parts, it is necessary to provide a hollow space by bonding the semiconductor element substrate and a sealing substrate made of glass, metal, ceramic, etc. with an adhesive placed around the semiconductor element. At this time, a method is used in which a liquid adhesive is used to form a pattern of the adhesive layer by a dispense method or a screen printing method (Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-115104 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, in the conventional dispensing method using a liquid adhesive as in Patent Document 1, it is difficult to apply the adhesive at a uniform height, and in the case of screen printing, mesh marks of the screen remain on the upper surface of the adhesive layer, making it difficult to flatten it. As a result, it was found that the distance between the substrates is difficult to keep constant when bonded, causing variations in the height of the laminate and uneven bonding surfaces, resulting in individual differences in the reliability of the obtained substrate laminate.

[0005] The present invention has been made in consideration of the above points, and aims to provide a method for manufacturing a substrate laminate having an adhesive layer with high adhesive reliability by forming a curable resin pattern having excellent height uniformity and a good shape. [Means for solving the problem]

[0006] As a result of intensive research into solving the above problems, the present inventors have found that the above problems can be solved by a method for manufacturing a substrate laminate, the method including the steps of forming a first pattern of a curable resin on a first substrate by using a printing method, forming a second pattern by molding the first pattern in a mold, and bonding the first substrate and the second substrate together via the second pattern, thereby completing the invention.

[0007] [1] A method for manufacturing a substrate laminate, comprising the steps of forming a first pattern of a curable resin on a first substrate using a printing method, molding the first pattern in a mold to form a second pattern, and bonding the first substrate and second substrate together via the second pattern.

[0008] [2] The method for producing a substrate laminate according to [1], wherein the printing method is screen printing.

[0009] [3] The method for producing a substrate laminate according to [1] or [2], wherein the surface roughness Ra2 of the mold is 5 μm or less.

[0010] [4] The method for producing a substrate laminate according to any one of [1] to [3], wherein one of the first substrate and the second substrate is a transparent substrate.

[0011] [5] The method for producing a substrate laminate according to [4], wherein the other substrate is a semiconductor element substrate.

[0012] [6] The method for producing a substrate laminate according to any one of [1] to [5], wherein the curable resin contains at least either a glycidyl group or an alicyclic epoxy group.

[0013] [7] The method for producing a substrate laminate according to any one of [1] to [6], wherein the curable resin is a polysiloxane compound.

[0014] [8] The method for producing a substrate laminate according to any one of [1] to [7], wherein the curable resin is a photosensitive resin.

[0015] [9] The method for manufacturing a substrate laminate according to [8], further comprising a step of exposing to the first pattern or the second pattern. Effect of the Invention

[0016] By using the manufacturing method of the present invention, a stabilized adhesive surface can be obtained, resulting in excellent adhesive reliability, and a substrate laminate can be obtained in which individual differences in semiconductors due to differences in the distance between the substrates are suppressed. In addition, since a substrate laminate with highly accurate pattern control can be obtained using a simple process, the method is particularly suitable for manufacturing hollow structures for CMOS / CCD sensors and hollow structures for MEMS devices. [Brief description of the drawings]

[0017] [Figure 1] FIG. 2 is a diagram showing a state in which a first pattern is formed on a first substrate according to an embodiment of the present invention. [Diagram 2] 4A to 4C are diagrams showing a process of forming a second pattern by molding a first pattern in a mold according to an embodiment of the present invention. [Diagram 3] FIG. 4 is a diagram showing a state in which a first substrate and a second substrate are bonded together via a second pattern according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] (1. Substrate Laminate) The substrate laminate of the present invention is obtained through a process of forming a first pattern of a curable resin on a first substrate by using a printing method, forming a second pattern by molding the first pattern in a mold, and bonding the first substrate and the second substrate together via the second pattern.

[0019] Examples of substrates that can be used include semiconductor element substrates, silicon wafers, glass substrates, transparent resin substrates, colored resin substrates, ceramic substrates, etc. In the manufacture of an image sensor described below, a semiconductor element substrate is used as the first substrate or the second substrate, and a glass substrate is used as the other substrate.

[0020] The shape of the substrate may be either round or rectangular. From the viewpoint of productivity, it is preferable to use a square substrate of 100 mm×100 mm or more, a substrate obtained by rearranging substrates that have been diced into individual pieces in an area of ​​100 mm×100 mm or more, or a round substrate of 4 to 12 inches. The first substrate and the second substrate may be the same or different in size and shape.

[0021] The curable resin patterned on the substrate of the substrate laminate of the present invention functions as an adhesive layer that bonds the first substrate and the second substrate. The width and height of the adhesive layer can be set as appropriate, and by selecting them appropriately, a substrate laminate having a hollow structure can be easily obtained. In particular, when the substrate laminate is used for a CMOS / CCD sensor, if the adhesive layer is too low, the sensor substrate may be damaged during assembly. Also, if the adhesive layer is too high, a good pattern may not be obtained. From these points, the height of the adhesive layer is 1 μm to 300 μm, preferably 50 μm to 150 μm. If the width of the adhesive layer is too thin, sufficient adhesive strength may not be obtained, and if the width of the adhesive layer is too wide, there is a risk that there will be no space to place the sensor substrate. From these points, the width of the adhesive layer is 1 μm to 1000 μm, preferably 100 μm to 300 μm.

[0022] In addition, the surface roughness Ra1 of the upper surface of the adhesive layer formed on the first substrate, i.e., the surface in contact with the second substrate, is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less. By making it 5 μm or less, it is possible to improve the bonding property and increase the adhesion reliability, and it is also effective in reducing the height variation. The surface roughness can be measured using a 3D measuring laser microscope.

[0023] (2. Method for manufacturing substrate laminate) An embodiment of the method for producing a substrate laminate of the present invention will be described in detail below.

[0024] The method for preparing the curable resin used as the adhesive layer is not particularly limited, and it can be prepared by various methods. The various components may be mixed and prepared just before use, or all the components may be mixed and prepared in advance in a single liquid state and stored at low temperature. A liquid state is preferable from the viewpoint of handleability. The viscosity of the composition containing the curable resin is preferably 1 Pa·s or more in a 25°C environment from the viewpoint of suppressing bleeding. In addition, from the viewpoint of carrying out application using a printing method, it is preferable that the viscosity is 250 Pa·s or less. The viscosity can be measured using a rheometer.

[0025] First, a printing method is used to form a plurality of first patterns of a curable resin on a first substrate (FIG. 1(a) and FIG. 1(b)). The pattern shape can be appropriately set depending on the desired application. Printing methods include the dispenser method, inkjet printing, letterpress printing, flexographic printing, offset printing, gravure printing, and screen printing, among which screen printing is preferred from the viewpoint of simplicity and good patterning properties. There are no particular limitations on the plate used for screen printing as long as it allows the curable resin to pass through. It is preferable to form the first pattern so that the curable resin does not leak outside the mold used in the step of forming the second pattern.

[0026] In order to further control the pattern shape after printing, the first pattern is formed using a screen printing method, and then the first pattern is molded. First, the first pattern and the mold are aligned (FIG. 2(a)), and then the mold is pressed against the first pattern to mold it (FIG. 2(b)), and then the mold is released to form the second pattern (FIG. 2(c)). It is preferable that the second pattern has the same height as the first pattern, or a lower height. In addition, from the viewpoint of placing the second pattern inside the mold, it is preferable that the width of the mold is wider than the first pattern. In terms of the width and height of the mold, the cross-sectional area of ​​the mold is preferably 1 to 2 times the cross-sectional area of ​​the first pattern, from the viewpoint of preventing the resin from leaking out of the mold.

[0027] The material of the mold used is not particularly limited, but may be metal such as stainless steel, inorganic material such as glass, organic material such as rubber or resin, or a combination of these. In addition, the mold surface may be treated to improve the releasability and durability of the pattern. For example, organic coating such as fluorine, silicone, PEEK, or metal coating such as cemented carbide, hard chrome, DLC, etc. may be applied, or the surface may be matte-finished.

[0028] From the viewpoint of reducing the surface roughness of the upper surface of the second pattern, i.e., the surface in contact with the second substrate, and improving adhesion and bonding, the surface roughness Ra2 of the mold is preferably 5 μm or less, more preferably 3 μm or less, and further preferably 1 μm or less. The surface roughness Ra2 of the mold can be measured, for example, using a 3D measuring laser microscope.

[0029] The mold and the substrate may be heated from before the mold is pressed against the substrate until it is released from the substrate. The heating temperature is preferably 40° C. to 300° C., and more preferably 40° C. to 150° C. from the viewpoints of removing the solvent and adjusting the physical properties of the cured product.

[0030] When the curable resin used as the adhesive layer is a photosensitive resin, it is preferable to further include a step of exposing the first pattern or the second pattern. The exposure may be performed after the formation of the first pattern, after the formation of the second pattern, or both, and in the case of the formation of the second pattern, it may be performed before or after the demolding. By including the exposure step, the change over time of the pattern shape can be suppressed.

[0031] As a light source for photocuring (exposure), a light source that emits light with the absorption wavelength of the polymerization initiator and sensitizer used may be used, and typically a light source having a wavelength in the range of 200 nm to 450 nm (e.g., a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a high-power metal halide lamp, a xenon lamp, a carbon arc lamp, or a light-emitting diode, etc.) can be used.

[0032] In order to remove the solvent and adjust the physical properties of the cured product, heat may be applied before or after photocuring to a degree that does not reduce the adhesiveness of the pattern resin, for pre-baking and after-baking. The temperature at this time can be appropriately set, but is preferably 40°C to 300°C, more preferably 40°C to 150°C.

[0033] Next, after forming the second pattern, the first substrate on which the multiple patterns are formed and the second substrate are pressure-bonded to obtain a substrate laminate. The pressure-bonding temperature is usually 25°C to 350°C, preferably 60°C to 300°C, and more preferably 80°C to 250°C. The pressure applied to the bonding surfaces is usually 0MPa to 50MPa, preferably 0MPa to 40MPa, and more preferably 0MPa to 30MPa during pressure-bonding. From the viewpoint of improving adhesive strength, it is preferable to cure the substrate at 80°C to 350°C after pressure-bonding. Then, each pattern is diced to obtain individual substrates (FIG. 3).

[0034] In the above description, an example of pressure bonding a first substrate on which a plurality of patterns are formed and a second substrate is described, but the present invention is not limited to this method. For example, after forming a plurality of second patterns on a first substrate, the pieces of the first substrate on which the patterns are formed by dicing may be individually bonded to a second substrate which has been previously diced, or the first substrate which has been previously diced may be rearranged to form a plurality of second patterns, and then bonded to the second substrate either collectively or individually.

[0035] (3. Curing resin) The curable resin in the present invention may be a resin that is cured by heat, light, or both heat and light. When the curable resin is a photosensitive resin that is cured by light, it is preferable because it can be brought into a B-stage (semi-cured) state by a photoreaction and can be easily used as an adhesive layer that constitutes the substrate laminate.

[0036] (cationic polymerizable) The adhesive layer of the present invention can be made of a compound having a cationic polymerizable functional group such as an epoxy group, an oxetane group, or a vinyl ether group. Specifically, novolac phenol type epoxy resin, biphenyl type epoxy resin, dicyclopentadiene type epoxy resin, cyclohexyl epoxy group-containing polyorganosiloxane (cyclic or linear), glycidyl group-containing polyorganosiloxane (cyclic or linear), bisphenol F diglycidyl ether, bisphenol A diglycidyl ether, 2,2'-bis(4-glycidyloxycyclohexyl)propane, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, vinylcyclohexene dioxide, 2-(3,4-epoxycyclohexyl)-5, Examples of such bisglycidyl esters include 5-spiro-(3,4-epoxycyclohexane)-1,3-dioxane, bis(3,4-epoxycyclohexyl)adipate, 1,2-cyclopropanedicarboxylic acid bisglycidyl ester, triglycidyl isocyanurate, monoallyl diglycidyl isocyanurate, diallyl monoglycidyl isocyanurate, 1,4-bis{(3-ethyl-3-oxetanyl)methoxy}methyl}benzene, bis{1-ethyl(3-oxetanyl)}methyl ether, 3-ethyl-3-(phenoxymethyl)oxetane, and 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane.

[0037] From the viewpoint of stability, it is preferable to have an epoxy group, and among the epoxy groups, it is more preferable to have at least one of a glycidyl group or an alicyclic epoxy group, and it is even more preferable to have an alicyclic epoxy group in terms of excellent cationic polymerizability by light and heat. In addition, it is sufficient to have at least one cationic polymerizable functional group in one molecule, but it is preferable to have two or more, and more preferable to have three or more. If there are three or more cationic polymerizable functional groups, a cured product with a high crosslink density can be obtained, and the cured product has the advantage of excellent heat resistance. Each cationic polymerizable functional group may be the same, or may be two or more different functional groups. The cationic polymerizable group in the curable resin is preferably 1 to 99 parts by weight of the curable resin excluding the solvent, and more preferably 5 to 90 parts by weight.

[0038] (Polysiloxane compounds) The curable resin in the present invention is preferably a polysiloxane compound from the viewpoints of heat resistance during reflow and reducing outgassing. In the present invention, the polysiloxane compound is not particularly limited as long as it is a compound having a siloxane unit Si-O-Si. Among the siloxane units in the polysiloxane compound, T units (XSiO 3 / 2 ) or Q units (SiO 4 / 2 The higher the content of XSiO, the harder the resulting cured product will be and the more heat-resistant and reliable it will be. 1 / 2 ) or D units (XSiO 2 / 2 The higher the content of ), the softer and less stressful the resulting cured product is. From the viewpoint of compatibility with other components, it is preferable that the polysiloxane compound in the curable resin has a cationically polymerizable group in the molecule.

[0039] (4. Other Additives) (Crosslinking agent) In order to adjust the workability, reactivity, adhesiveness and strength of the cured product, a crosslinking agent having two or more photopolymerizable functional groups other than cationic polymerizable functional groups in one molecule can be added to the curable resin. The crosslinking agent is not particularly limited as long as it is selected according to the curing reaction type, and includes alkoxysilane compounds and (meth)acrylate compounds.

[0040] (Photoacid generator) The above-mentioned curable resin preferably contains a photoacid generator.The photoacid generator is not particularly limited as long as it is a compound that can release an acidic active substance that can crosslink the photopolymerizable functional group of the curable resin by being irradiated with active energy rays.The pKa of the acid generated by the photoacid generator is not limited, but is preferably less than 3, more preferably less than 1.

[0041] As the photoacid generator, known photoacid generators can be used.For example, as the photoacid generator, various compounds that are considered to be suitable in JP-A-2000-1648, JP-T-2001-515533 and WO-A-2002 / 83764 can be listed, but are not limited thereto.The photoacid generator is preferably sulfonate esters, carboxylate esters or onium salts, more preferably onium salts.

[0042] As the sulfonate esters, various sulfonic acid derivatives can be used, for example, disulfones, disulfonyldiazomethanes, disulfonylmethanes, sulfonylbenzoylmethanes, imide sulfonates such as trifluoromethylsulfonate derivatives, benzoin sulfonates, sulfonates of 1-oxy-2-hydroxy-3-propyl alcohol, pyrogallol trisulfonates, and benzylsulfonates.

[0043] Specific examples of the sulfonate esters include diphenyl disulfone, ditosyl disulfone, bis(phenylsulfonyl)diazomethane, bis(chlorophenylsulfonyl)diazomethane, bis(xylylsulfonyl)diazomethane, phenylsulfonylbenzoyldiazomethane, bis(cyclohexylsulfonyl)methane, 1,8-naphthalenedicarboxylic acid imide methyl sulfonate, 1,8-naphthalenedicarboxylic acid imide tosyl sulfonate, 1,8-naphthalenedicarboxylic acid imide trifluoromethyl sulfonate, 1,8-naphthalenedicarboxylic acid imide camphorsulfonate, succinic acid imide phenyl sulfonate, succinic acid imide dotosylsulfonate, succinimide trifluoromethylsulfonate, succinimide camphorsulfonate, phthalimide trifluorosulfonate, cis-5-norbornene-endo-2,3-dicarboxylic acid imide trifluoromethylsulfonate, benzoin tosylate, 1,2-diphenyl-2-hydroxypropyl tosylate, 1,2-di(4-methylmercaptophenyl)-2-hydroxypropyl tosylate, pyrogallol methylsulfonate, pyrogallol ethylsulfonate, 2,6-dinitrophenyl methyl tosylate, ortho-nitrophenyl methyl tosylate, and para-nitrophenyl tosylate.

[0044] These may be used alone or in combination of two or more. In the present invention, carboxylic acid esters may also be used as photoacid generators.

[0045] In general, sulfonate esters and carboxylate esters may require a heating step (50° C.-100° C.) to liberate the acid.

[0046] The onium salt is tetrafluoroborate (BF4 - ), hexafluorophosphate (PF6 - ), hexafluoroantimonate (SbF6 - ), hexafluoroarsenate (AsF6 -), hexachloroantimonate (SbCl6 - ), tetraphenylborate, tetrakis(trifluoromethylphenyl)borate, tetrakis(pentafluoromethylphenyl)borate, fluoroalkyl fluorophosphate, perchlorate ion (ClO4 - ), trifluoromethanesulfonate ion (CF3SO3 - ), fluorosulfonate ion (FSO3 - ), sulfonium salts and iodonium salts having anions such as toluenesulfonate ion, trinitrobenzenesulfonate anion, and trinitrotoluenesulfonate anion. From the viewpoint of absorption wavelength, the photoacid generator is preferably an aromatic sulfonium salt.

[0047] The anions in photoacid generators are listed in order of acid strength from strongest to weakest: SbF6 - , B(C6F5)4 - , PF6 - , CF3SO3 - , HSO4 - The stronger the acid strength of the anion of the photoacid generator, the higher the film remaining rate tends to be.

[0048] The content of the photoacid generator in the curable resin is not particularly limited. From the viewpoint of the balance between the curing speed and the physical properties of the cured product, the content of the photoacid generator is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the compound (A).

[0049] If the amount of photoacid generator is small, it may take a long time to cure or may not be possible to obtain a sufficiently cured product, whereas if the amount of photoacid generator is large, it may be undesirable because color may remain in the cured product or the coloring or heat resistance or light resistance may be impaired due to rapid curing.

[0050] (Basic compounds) The curable resin may contain a basic compound from the viewpoint of controlling the curing rate and improving storage stability.

[0051] The amount of the basic compound is preferably 0.001 to 2.0 parts by weight, more preferably 0.01 to 1.0 parts by weight, based on 100 parts by weight of the compound having a cationic polymerizable functional group. If the amount of the basic compound is 0.001 parts by weight or more, the effect can be sufficiently exhibited. If the amount of the basic compound is 2.0 parts by weight or less, the sensitivity can be improved.

[0052] The weight ratio ((B) / (A)) of the basic compound (B) to the photoacid generator (A) is 0.001 to 0.2, and preferably 0.01 to 0.15. When the weight ratio is 0.001 or more, the effect of the basic compound can be sufficiently exhibited. When the weight ratio is 0.2 or less, crosslinking can be sufficiently performed.

[0053] The basic compound is not particularly limited, and examples thereof include primary, secondary and tertiary aliphatic amines, mixed amines, aromatic amines, heterocyclic amines, amide derivatives and imide derivatives, etc. Among these, aromatic amines and heterocyclic amines are preferably used as the basic compound.

[0054] Examples of the aromatic amines and the heterocyclic amines include aniline, pyrrole, oxazole, thiazole, imidazole, pyrazole, furazan, pyrroline, pyrrolidine, imidazoline, imidazolidine, pyridine, pyridazine, pyrimidine, pyrazine, pyrazoline, pyrazolidine, piperidine, piperazine, morpholine, indole, isoindole, 1H-indazole, indoline, quinoline, cinnoline, quinazoline, quinoxaline, phthalazine, purine, pteridine, carbazole, phenanthridine, acridine, phenazine, 1,10-phenanthroline, adenine, adenosine, guanine, guanosine, uracil and uridine, and derivatives thereof.In addition, examples of the heterocyclic amines include 2,6-lutidine.

[0055] Among them, morpholine derivatives can be preferably used as the basic compound. Specific examples of the morpholine derivatives include bis(2-morpholinoethyl)ether, 4,4'-carbonyldimorpholine, 4-[2-(ethoxycarbonyl)ethyl]morpholine, and 4-(p-tolyl)morpholine.

[0056] The basic compound may be used alone or in combination of two or more kinds.

[0057] (sensitizer) The curable resin may contain a sensitizer. The sensitizer can improve the sensitivity of the curable resin to visible light and can also impart sensitivity to high wavelength light such as g-line (436 nm), h-line (405 nm) and i-line (365 nm). The curability of the curable resin can be adjusted by using these sensitizers in combination with the photoacid generator.

[0058] Examples of the sensitizer include anthracene-based compounds and thioxanthone-based compounds.

[0059] Specific examples of the anthracene-based compound include anthracene, 2-ethyl-9,10-dimethoxyanthracene, 9,10-dimethylanthracene, 9,10-dibutoxyanthracene, 9,10-dipropoxyanthracene, 9,10-diethoxyanthracene, 1,4-dimethoxyanthracene, 9-methylanthracene, 2-ethylanthracene, 2-tert-butylanthracene, 2,6-di-tert-butylanthracene, 9,10-diphenyl-2,6-di-tert-butylanthracene, etc. In particular, from the viewpoint of easy availability, anthracene, 9,10-dimethylanthracene, 9,10-dibutoxyanthracene, 9,10-dipropoxyanthracene, 9,10-diethoxyanthracene, etc. are preferred as the anthracene-based compound.

[0060] As the anthracene-based compound, anthracene is preferred from the viewpoint of excellent transparency of the cured product, and 9,10-dibutoxyanthracene, 9,10-dipropoxyanthracene, 9,10-diethoxyanthracene, and the like are preferred from the viewpoint of excellent compatibility with the curable resin.

[0061] Specific examples of the thioxanthone compounds include thioxanthone, 2-chlorothioxanthone, and 2,5-diethyldioxanthone.

[0062] These sensitizers may be used alone or in combination of two or more.

[0063] The content of the sensitizer is not particularly limited as long as it is an amount that can exert a sensitizing effect, but is preferably 0.01 to 300 mol, more preferably 0.01 to 100 mol, relative to 1 mol of the added photoacid generator. If the amount of the sensitizer is small, the sensitizing effect cannot be obtained, and curing may take a long time or may have an undesirable effect on the developability. On the other hand, if the amount of the sensitizer is large, color may remain in the cured product, coloring may occur due to rapid curing, or heat resistance or light resistance may be impaired.

[0064] (Adhesion improver) The curable resin may contain an adhesion improver. Examples of the adhesion improver include, in addition to commonly used adhesives, various coupling agents, epoxy compounds, oxetane compounds, phenolic resins, coumarone-indene resins, rosin ester resins, terpene-phenolic resins, α-methylstyrene-vinyltoluene copolymers, polyethylmethylstyrene, and aromatic polyisocyanates.

[0065] An example of the coupling agent is a silane coupling agent. The silane coupling agent is not particularly limited as long as it is a compound having at least one functional group reactive with an organic group and at least one hydrolyzable silicon group in the molecule. As the group reactive with an organic group, from the viewpoint of handling, at least one functional group selected from an epoxy group, a methacryl group, an acrylic group, an isocyanate group, an isocyanurate group, a vinyl group, and a carbamate group is preferable, and from the viewpoint of curing property and adhesiveness, an epoxy group, a methacryl group, or an acrylic group is particularly preferable. As the hydrolyzable silicon group, from the viewpoint of handling, an alkoxysilyl group is preferable, and from the viewpoint of reactivity, a methoxysilyl group or an ethoxysilyl group is particularly preferable.

[0066] Examples of preferred silane coupling agents include alkoxysilanes having an epoxy functional group, such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane; alkoxysilanes having a methacryl group or an acryl group, such as 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, methacryloxymethyltrimethoxysilane, methacryloxymethyltriethoxysilane, acryloxymethyltrimethoxysilane, and acryloxymethyltriethoxysilane; tris[3-(trimethoxysilylpropyl)]isocyanurate; and γ-isocyanatepropyltrimethoxysilane.

[0067] The amount of the silane coupling agent added can be appropriately set, but is preferably 0.1 to 20 parts by weight, more preferably 0.3 to 10 parts by weight, and even more preferably 0.5 to 5 parts by weight, relative to 100 parts by weight of the compound having a cationic polymerizable functional group. If the amount added is small, the adhesiveness improving effect is not achieved, and if the amount added is large, it may have an adverse effect on the curability and physical properties of the cured product.

[0068] Furthermore, these coupling agents, silane coupling agents, epoxy compounds, etc. may be used alone or in combination of two or more.

[0069] (thermoplastic resin) For the purpose of improving the properties of the curable resin, it is also possible to add various thermoplastic resins to the curable resin. Examples of the thermoplastic resin include acrylic resins such as polymethyl methacrylate-based resins (e.g., Optretz manufactured by Hitachi Chemical Co., Ltd.) which are homopolymers of methyl methacrylate or random, block, or graft polymers of methyl methacrylate and other monomers, and polybutyl acrylate-based resins (e.g., homopolymers of butyl acrylate or random, block, or graft polymers of butyl acrylate and other monomers), polycarbonate-based resins such as polycarbonate resins containing bisphenol A, 3,3,5-trimethylcyclohexylidene bisphenol, or the like as monomer structures (e.g., APEC manufactured by Teijin Co., Ltd.), norbornene derivatives, vinyl monomers, or the like homopolymerized or copolymerized resins, norbornene derivatives, or hydrogenated cycloolefin resins (e.g., cycloolefin resins such as hydrogenated norbornene derivatives, vinyl monomers, or the like homopolymerized or copolymerized resins, norbornene derivatives, or hydrogenated norbornene derivatives, etc. Examples of such resins include, but are not limited to, APEL (manufactured by Mitsui Chemicals, Inc.), ZEONOR and ZEONEX (manufactured by Nippon Zeon Co., Ltd.), olefin-maleimide resins such as copolymers of ethylene and maleimide (e.g., TI-PAS (manufactured by Tosoh Corporation)), polyester resins such as polyesters obtained by polycondensation of bisphenols (bisphenol A and bis(4-(2-hydroxyethoxy)phenyl)fluorene, etc.) or diols (diethylene glycol, etc.) with phthalic acids (terephthalic acid and isophthalic acid, etc.) or aliphatic dicarboxylic acids (e.g., O-PET (manufactured by Kanebo Co., Ltd.)), polyethersulfone resins, polyarylate resins, polyvinyl acetal resins, polyethylene resins, polypropylene resins, polystyrene resins, polyamide resins, silicone resins, fluororesins, and rubber-like resins such as natural rubber and EPDM. These thermoplastic resins may be used alone or in combination.

[0070] The thermoplastic resin may have a crosslinkable group. Examples of the crosslinkable group include an epoxy group, an amino group, a radically polymerizable unsaturated group, a carboxyl group, an isocyanate group, a hydroxyl group, and an alkoxysilyl group. From the viewpoint that the heat resistance of the obtained cured product is likely to be high, the thermoplastic resin preferably has one or more crosslinkable groups on average per molecule.

[0071] The molecular weight of the thermoplastic resin is not particularly limited, but from the viewpoint of easily improving compatibility with polysiloxane-based compounds, the number average molecular weight is preferably 10,000 or less, more preferably 5,000 or less. On the other hand, from the viewpoint of easily improving toughness of the obtained cured product, the number average molecular weight is preferably 10,000 or more, more preferably 100,000 or more. There is also no particular limitation on the molecular weight distribution, but from the viewpoint of easily improving moldability by reducing the viscosity of the mixture, the molecular weight distribution is preferably 3 or less, more preferably 2 or less, and even more preferably 1.5 or less.

[0072] The amount of the thermoplastic resin is not particularly limited, but is preferably 5 to 50% by weight, more preferably 10 to 30% by weight, based on the total amount of the curable resin. If the amount of the thermoplastic resin is small, the cured product may become brittle. If the amount of the thermoplastic resin is large, the heat resistance (elastic modulus at high temperatures) is likely to be low.

[0073] The thermoplastic resin may be dissolved in the curable resin and mixed in a uniform state, or may be pulverized and mixed in a particulate state, or may be dissolved in a solvent and mixed to form a dispersed state. In terms of the fact that the obtained cured product is more likely to be transparent, it is preferable to dissolve the thermoplastic resin in the curable resin and mix it in a uniform state. In this case, too, the thermoplastic resin may be directly dissolved in the curable resin, or may be mixed uniformly using a solvent or the like, or the solvent may be removed thereafter to form a uniform dispersed or mixed state.

[0074] When the thermoplastic resin is dispersed, the average particle size of the thermoplastic resin may be appropriately set, but the lower limit of the average particle size is preferably 10 nm, and the upper limit of the average particle size is preferably 10 μm. The particle system may have a distribution, and may be a single dispersion or may have multiple peak particle sizes, but from the viewpoint of low viscosity of the curable composition and good moldability, the coefficient of variation of the particle size is preferably 10% or less.

[0075] (filling material) The above-mentioned curable resin may contain a filler as required.Various fillers are used as the filler, and examples of such fillers include inorganic fillers such as silica-based fillers (quartz, fume silica, precipitated silica, silicic anhydride, fused silica, crystalline silica, and ultrafine amorphous silica), silicon nitride, silver powder, alumina, aluminum hydroxide, titanium oxide, glass fiber, carbon fiber, mica, carbon black, graphite, diatomaceous earth, clay, clay, talc, calcium carbonate, magnesium carbonate, barium sulfate, and inorganic balloon, as well as fillers that are generally used or proposed as fillers for conventional sealing materials, such as epoxy-based fillers.

[0076] (Anti-aging agent) An antioxidant may be added to the curable resin. Examples of the antioxidant include commonly used antioxidants such as hindered phenol-based antioxidants, as well as citric acid, phosphoric acid, and sulfur-based antioxidants.

[0077] As the hindered phenol-based antioxidant, various types can be used, including Irganox 1010 available from BASF.

[0078] Examples of the sulfur-based antiaging agents include mercaptans, mercaptan salts, sulfides (sulfide carboxylates, hindered phenol-based sulfides, etc.), polysulfides, dithiocarboxylates, thioureas, thiophosphates, sulfonium compounds, thioaldehydes, thioketones, mercaptals, mercaptols, monothioacids, polythioacids, thioamides, and sulfoxides. These antiaging agents may be used alone or in combination of two or more.

[0079] (Radical inhibitor) A radical inhibitor may be added to the curable resin. Examples of the radical inhibitor include phenol radical inhibitors such as 2,6-di-t-butyl-3-methylphenol (BHT), 2,2'-methylene-bis(4-methyl-6-t-butylphenol) and tetrakis(methylene-3(3,5-di-t-butyl-4-hydroxyphenyl)propionate)methane, and amine radical inhibitors such as phenyl-β-naphthylamine, α-naphthylamine, N,N'-sec-butyl-p-phenylenediamine, phenothiazine and N,N'-diphenyl-p-phenylenediamine. These radical inhibitors may be used alone or in combination of two or more.

[0080] (solvent) When the curable resin has a high viscosity, it can be dissolved in a solvent before use. The solvent is not particularly limited, and specifically includes hydrocarbon solvents such as benzene, toluene, hexane, and heptane; ether solvents such as tetrahydrofuran, 1,4-dioxane, 1,3-dioxolane, and diethyl ether; ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; glycol solvents such as propylene glycol-1-monomethyl ether-2-acetate (PGMEA), ethylene glycol diethyl ether, and diethylene glycol diethyl ether; halogen-based solvents such as chloroform, methylene chloride, and 1,2-dichloroethane; ester solvents such as butyl acetate and isobutyl isobutyrate; and lactone solvents such as γ-butyrolactone, ε-caprolactone, and δ-valerolactone. These solvents may be used alone or in the form of a mixed solvent of two or more.

[0081] The amount of the solvent used can be appropriately set, but the lower limit of the amount used is preferably 0.001 mL and the upper limit of the amount used is preferably 10 mL per gram of the curable resin used.

[0082] (others) To the curable resin, colorants, release agents, flame retardants, flame retardant assistants, surfactants, defoamers, emulsifiers, leveling agents, anti-repellents, ion trapping agents (antimony-bismuth, etc.), thixotropy imparting agents, tackifiers, storage stability improvers, ozone degradation inhibitors, light stabilizers, thickeners, plasticizers, reactive diluents, antioxidants, heat stabilizers, conductivity imparting agents, antistatic agents, radiation shielding agents, nucleating agents, phosphorus-based peroxide decomposers, lubricants, pigments, metal deactivators, thermal conductivity imparting agents, physical property adjusters, and the like can be added within a range that does not impair the objects and effects of the present invention.

[0083] (Application) The substrate laminate according to the present invention can be used in various applications. It can be applied to various applications in which a substrate laminate produced using conventional acrylic resin and epoxy resin adhesives is used.

[0084] As for the above-mentioned applications, if the substrate laminate manufactured by the present invention is applied to hollow structures for CMOS / CCD sensors and hollow structures for MEMS devices, the adhesion stability of the wall materials can be ensured and defects in the structures can be reduced, which is preferable.

[0085] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention. EXAMPLES

[0086] The present invention will be described in more detail below based on examples, but the present invention is not limited to the following examples.

[0087] (Pattern surface properties) The pattern shape of the produced pattern was observed using a 3D measuring laser microscope (LEXT OLS4000, manufactured by Olympus Corporation), and the surface roughness Ra1 of the pattern surface was evaluated according to the following criteria. <Evaluation criteria> ○: Very good level (Ra1 is 5 μm or less) ×: Not suitable for practical use (Ra1 exceeds 5 μm)

[0088] (Pattern height) The height of the pattern produced was measured at 10 or more points using a 3D measuring laser microscope (LEXT OLS4000, manufactured by Olympus Corporation), the difference between the maximum and minimum heights of the measured pattern was calculated, and the height variation was evaluated according to the following criteria. <Evaluation criteria> ○: Very good level (difference between maximum and minimum pattern heights is less than 6 μm) ×: Not suitable for practical use (difference between maximum and minimum pattern height is 6 μm or more)

[0089] (Pattern Adhesion) Using a 3D measuring laser microscope (LEXT OLS4000, manufactured by Olympus Corporation), the adhesive state between the second substrate and the adhesive layer was observed from the transparent substrate side and evaluated according to the following criteria. The contrast between the adhered and unadhered areas is clearly different, making it possible to judge by observation. <Evaluation criteria> ○: Very good level (adhered) ×: Not suitable for practical use (some areas are not glued)

[0090] (Synthesis Example 1) 50g of diallyl monomethyl isocyanuric acid was dissolved in 100g of toluene, and 87mg of a xylene solution of platinum vinyl siloxane complex (containing 3wt% platinum) was added. The solution thus obtained was added dropwise over 3 hours to a solution of 94g of 1,3,5,7-tetrahydrogen-1,3,5,7-tetramethylcyclotetrasiloxane and 186g of toluene heated to 105°C in a nitrogen atmosphere containing 3% oxygen. 30 minutes after the end of the addition, 1 After confirming that the reaction rate of the alkenyl groups (the rate at which the alkenyl groups had decreased) was 95% or more by H-NMR, a solution of 55 g of 1-vinyl-3,4-epoxycyclohexane and 55 g of toluene was added dropwise over 1 hour. 30 minutes after the end of the addition, 1 After confirming by H-NMR that the reaction rate of the alkenyl groups was 95% or more, the reaction was terminated by cooling. The solvents toluene and dioxane were distilled off under reduced pressure to obtain "curable resin A".

[0091] (Production Example 1) A composition was obtained by mixing 100 parts by weight of the above curable resin A with 7 parts by weight of CEL2021P (alicyclic epoxy compound manufactured by Daicel Organic Synthesis Company), 2 parts by weight of CPI-210S (photoacid generator manufactured by San-Apro Co., Ltd.), and 0.5 parts by weight of IRGANOX1010 (antioxidant manufactured by BASF) in a ratio of 100 parts by weight of the above curable resin A.

[0092] Example 1 The composition containing the curable resin A obtained in Production Example 1 was screen-printed on a 100 mm x 100 mm glass substrate (D263 Teco SCHOTT) using a screen printing device (DP-320 Newlong Precision Industry Co., Ltd.) to form a first pattern with a width of 250 μm and a height of 50 μm. The screen plate used had a mesh number of 250 (lines / inch), a line diameter of 30 μm, and an emulsion thickness of 30 μm. A glass mold with a width of 280 μm, a height of 45 μm, and a surface roughness Ra2 of 5 μm or less was pressed against the substrate on which the first pattern had been formed after screen printing to form a second pattern. After the second pattern was formed, an accumulated light amount of 300 mJ / cm was applied. 2 After the exposure, the pattern surface property and the pattern height were observed by the above-mentioned method. After that, each pattern was cut into pieces, and a silicon substrate was laminated via the second pattern on the glass substrate, and a pressure of 5 MPa was applied on a hot plate at 120°C for 30 seconds to perform heat compression bonding, thereby obtaining a substrate laminate. The pattern adhesion of the obtained substrate laminate was evaluated by the above-mentioned method.

[0093] Comparative Example 1 After the first pattern was formed, the same procedure as in Example 1 was carried out except that the pattern was not molded using a mold, and the pattern surface properties and pattern adhesiveness were evaluated.

[0094] [Table 1]

[0095] As in Example 1, by forming the first pattern and then molding it in a mold, an adhesive layer with a good shape was obtained, and a substrate laminate with good height variation and adhesiveness was obtained. In Comparative Example 1, where molding was not performed in a mold, the surface properties, height variation, and adhesiveness were all insufficient. [Explanation of symbols]

[0096] 1. Hardening resin (first pattern) 2. First board 3. Mold 4. Hardening resin (second pattern) 5. Second board

Claims

1. A method for manufacturing a substrate laminate, comprising the steps of: forming a first pattern of a curable resin on a first substrate by using a printing method; molding the first pattern in a mold to form a second pattern; and bonding the first substrate and the second substrate together via the second pattern.

2. The method for manufacturing a substrate laminate according to claim 1 , wherein the printing method is screen printing.

3. Surface roughness Ra of the mold 2 The method for producing a substrate laminate according to claim 1 or 2, wherein the thickness is 5 μm or less.

4. The method for manufacturing a substrate laminate according to any one of claims 1 to 3, wherein one of the first substrate and the second substrate is a transparent substrate.

5. The method for manufacturing a substrate laminate according to claim 4 , wherein the other substrate is a semiconductor device substrate.

6. The method for producing a substrate laminate according to any one of claims 1 to 5, wherein the curable resin contains at least either a glycidyl group or an alicyclic epoxy group.

7. The method for producing a substrate laminate according to any one of claims 1 to 6, wherein the curable resin is a polysiloxane compound.

8. The method for producing a substrate laminate according to any one of claims 1 to 7, wherein the curable resin is a photosensitive resin.

9. The method for manufacturing a substrate laminate according to any one of claims 1 to 8, further comprising a step of exposing to the first pattern or the second pattern.

Citation Information

Patent Citations

  • Semiconductor imaging apparatus and manufacturing method thereof

    JP2006295481A

  • Semiconductor device and manufacturing method thereof

    JP2009188191A

  • Wafer sealing method for CMOS image sensor

    JP2013115104A

  • Method of manufacturing board having minute uneven pattern, and board having minute uneven pattern obtained by the method

    JP2016051808A

  • Replica mold-forming resin composition, replica mold, and patterning method using the replica mold

    JP2018080309A