Container, container manufacturing method, and drug solution container

A container with a controlled distribution of metal components and organic substances in its coating layer addresses the issue of impurity elution, maintaining the performance of stored chemical solutions by reducing impurity release.

JP7573663B2Active Publication Date: 2024-10-25FUJIFILM CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023017331
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-07-13
Filing Date
2023-02-08
Publication Date
2024-10-25
Estimated Expiration
2038-07-17

AI Technical Summary

Technical Problem

Existing containers used for storing chemical solutions, particularly those required for semiconductor manufacturing and medical purposes, fail to maintain the performance of the stored solutions over time due to the elution of impurity components, which deteriorate the chemical properties of the solutions.

Method used

A container with a specific composition and coating layer, containing polyolefin and selected metals like Ti, Al, Mg, Zr, Hf, Fe, Ni, Sn, Zn, Cr, and Mo, is designed to control the distribution of metal components and organic substances, ensuring a ratio of secondary ion intensities measured by time-of-flight secondary ion mass spectrometry is less than 1.00, thereby reducing impurity elution.

Benefits of technology

The container effectively maintains the performance of stored chemical solutions by minimizing impurity elution, ensuring the solutions remain effective for extended periods without degradation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573663000001
    Figure 0007573663000001
  • Figure 0007573663000002
    Figure 0007573663000002
  • Figure 0007573663000003
    Figure 0007573663000003
Patent Text Reader

Abstract

The present invention aims to provide a container that prevents deterioration of the performance of a liquid medicine over time even when the liquid medicine is stored for a long period of time. It also aims to provide a method for manufacturing the container and a liquid medicine container. [Solution] The container has a substrate and a coating layer having a thickness of 50 μm or more, which is disposed on at least a portion of the substrate and contains a composition containing polyolefin and at least one metal component selected from the group consisting of Ti, Al, Mg, Zr, Hf, Fe, Ni, Sn, Zn, Cr, and Mo. When the composition contains one metal component, the ratio RCAs calculated as CA1s / CA2s is less than 1.0, or when the composition contains two or more metal components, the average value of RCAs calculated for each of the two or more metal components is less than 1.0 in at least a portion of the coating layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a container, a method for manufacturing the container, and a drug solution container. [Background technology]

[0002] In the manufacture of semiconductor devices, chemicals containing solvents (typically organic solvents) are used. In recent years, there has been a demand to further reduce the impurities contained in the chemicals. In addition, the manufacture of semiconductor devices with a 10 nm node or less is being considered, and the demand is becoming even stronger.

[0003] Patent Document 1 states that "the density is 945 kg / cm 3 The document states that the container is made of a polyethylene resin composition containing a high-density polyethylene having a molecular weight of 100 or more and 50 ppm to 2000 ppm of an organic nucleating agent, and the content of hydrocarbon components having 18 and 20 carbon atoms extracted with ethanol is 100 ppm or less, and the total content of Al, Mg, Ti, Zr, and Hf is 40 ppm or less. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-249094 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present inventors produced a drug solution container by storing a drug solution in the container described in Patent Document 1, and conducted an investigation. As a result, they found that when the drug solution container is stored, the performance of the drug solution taken out of the drug solution container after storage may be reduced.

[0006] Therefore, an object of the present invention is to provide a container in which the performance of the liquid medicine is unlikely to deteriorate over time even when the liquid medicine is stored for a long period of time (hereinafter, also referred to as "having the effect of the present invention"). Another object of the present invention is to provide a method for manufacturing the container, and a liquid medicine container. [Means for solving the problem]

[0007] As a result of intensive research, the present inventors have found that the above object can be achieved by the following configuration.

[0008] [1] A container having a substrate and a coating layer having a thickness of 50 μm or more, the coating layer containing a composition containing polyolefin and at least one metal component selected from the group consisting of Ti, Al, Mg, Zr, Hf, Fe, Ni, Sn, Zn, Cr, and Mo, disposed on at least a portion of the substrate, wherein the composition contains one metal component, the surface region is defined as a region between the surface of the coating layer and a position 10 nm away from the surface in the thickness direction of the coating layer, and the internal region is defined as a region between a position 30 μm away from the surface in the thickness direction of the coating layer and a position 50 μm away from the surface in the thickness direction of the coating layer, and the surface region and the internal region are analyzed by a time-of-flight secondary ion mass spectrometer. A container in which, when measured, in at least a portion of the coating layer, the ratio RCAs calculated as CA1s / CA2s, where CA1s is the intensity ratio of the peak intensity of secondary ions derived from the metal component in the surface region to the peak intensity of secondary ions derived from the polyolefin in the surface region, and CA2s is the intensity ratio of the peak intensity of secondary ions derived from the metal component in the inner region to the peak intensity of secondary ions derived from the polyolefin in the inner region, is less than 1.00, or, when the composition contains two or more metal components, the average value of the RCAs calculated for each of the two or more metal components in at least a portion of the coating layer is less than 1.00. [2] A container made of a composition containing a polyolefin and at least one metal component selected from the group consisting of Ti, Al, Mg, Zr, Hf, Fe, Ni, Sn, Zn, Cr, and Mo, wherein when the composition contains one metal component, the surface region of the container is defined as a region between the surface of the container and a position 10 nm in the thickness direction of the container from the surface, and the internal region is defined as a region between a position 30 μm in the thickness direction of the container from the surface and a position 50 μm in the thickness direction of the container from the surface, and when the surface region and the internal region are measured with a time-of-flight secondary ion mass spectrometer, A container in which the ratio RCA, calculated by CA1 / CA2 using the intensity ratio CA1 of the peak intensity of secondary ions derived from metal components in the surface region to the peak intensity of secondary ions derived from polyolefin in the surface region, and the intensity ratio CA2 of the peak intensity of secondary ions derived from metal components in the internal region to the peak intensity of secondary ions derived from polyolefin in the internal region, is less than 1.00, or, when the composition contains two or more metal components, the average RCA value calculated for each of the two or more metal components in at least a portion of the container is less than 1.00. [3] A container having a substrate and a coating layer having a thickness of less than 50 μm, the coating layer containing a composition containing polyolefin and at least one metal component selected from the group consisting of Ti, Al, Mg, Zr, Hf, Fe, Ni, Sn, Zn, Cr, and Mo, disposed on at least a portion of the substrate, wherein when the composition contains one metal component, the surface region is defined as a region between the surface of the coating layer and a position 10 nm in the thickness direction of the coating layer from the surface as a reference, and the inner region is defined as a region between a position corresponding to 70% of the total thickness of the coating layer from the surface as a reference in the thickness direction of the coating layer and a position corresponding to 100% of the total thickness of the coating layer from the surface as a reference in the thickness direction of the coating layer, and a container in which, when a partial region is measured using a time-of-flight secondary ion mass spectrometer, in at least a portion of the coating layer, the ratio RCAt calculated from the intensity ratio CA1t of the peak intensity of secondary ions derived from metal components in the surface region to the peak intensity of secondary ions derived from polyolefin in the surface region, and the intensity ratio CA2t of the peak intensity of secondary ions derived from metal components in the inner region to the peak intensity of secondary ions derived from polyolefin in the inner region, is less than 1.00, or, when the composition contains two or more types of metal components, the average value of RCAt calculated for each of the two or more types of metal components in at least a portion of the coating layer is less than 1.00. [4] In at least a portion of the coating layer, the intensity ratio of the peak intensity of the secondary ion represented by CnH2n- to the peak intensity of the secondary ion derived from the polyolefin, measured by a time-of-flight secondary ion mass spectrometer in the surface region, to the peak intensity of the secondary ion derived from the polyolefin, p H 2p COO - The intensity ratio of the peak intensity of the secondary ions represented by C q H 2q PO 2- The average value CB1 of the peak intensity ratio of the secondary ions represented by the formula (I) is expressed as follows: n H2n - The intensity ratio of the secondary ion peak intensity, expressed as C p H 2p COO - The intensity ratio of the peak intensity of the secondary ions represented by C q H 2q PO 2- The container according to [1] or [3], wherein a ratio RCB calculated from an average value CB2 of intensity ratios of secondary ion peak intensities represented by the formula (CB1 / CB2) is less than 1.00, n is an integer of 12 to 20, p is an integer of 8 to 24, and q is an integer of 8 to 24. [5] In at least a portion of the surface, the peak intensity of secondary ions originating from polyolefin measured by a time-of-flight secondary ion mass spectrometer in the surface region is C n H 2n - The intensity ratio of the secondary ion peak intensity, expressed as C p H 2p COO - The intensity ratio of the peak intensity of the secondary ions represented by C q H 2q PO 2- The average value CB1 of the peak intensity ratio of the secondary ions represented by the formula (I) is expressed as follows: n H 2n - The intensity ratio of the secondary ion peak intensity, expressed as C p H 2p COO - The intensity ratio of the peak intensity of the secondary ions represented by C q H 2q PO 2-The container according to [2], wherein a ratio RCB calculated from an average value CB2 of the intensity ratios of secondary ion peak intensities represented by the formula (CB1 / CB2) is less than 1.00, n is an integer of 12 to 20, p is an integer of 8 to 24, and q is an integer of 8 to 24. [6] 100 ml of 40°C pure water was placed in a container so that the volume of the container was 50% of the volume of the container. After keeping the container for one day, When the pure water contains Fe, the content of Fe in the pure water is 0.01 ppt by mass to 0.3 ppb by mass with respect to the total mass of the pure water, When Cr is contained in the pure water, the Cr content is 0.01 mass ppt to 0.3 mass ppb with respect to the total mass of the pure water, The container according to any one of [1] to [5], wherein when the pure water contains Ni, the Ni content is 0.01 ppt by mass to 0.3 ppb by mass with respect to the total mass of the pure water. [7] 100 ml of pure water at 40°C is placed in a container so that the volume of the container is 50 volume % of the volume of the container, and after holding for one day, a compound selected from the group consisting of an aliphatic amide and an organic substance having a boiling point of 300°C or higher is contained in the pure water, The content of the compound is 0.1 ppb by mass to 1000 ppm by mass relative to the total mass of the pure water, The organic matter with a boiling point of 300°C or higher contains alkyl olefins, or The container according to any one of [1] to [6], wherein the aliphatic amide contains an aliphatic chain having 16 or more carbon atoms linked to a carbonyl group. [8] A method for producing a pre-cleaned coating layer by contacting a composition containing a polyolefin and at least one metal component selected from the group consisting of Ti, Al, Mg, Zr, Hf, Fe, Ni, Sn, Zn, Cr, and Mo, on a substrate; and washing the pre-washed coating layer with a cleaning liquid containing at least one selected from the group consisting of pure water, an acid, a base, and an organic solvent to obtain the container described in [1] or [3]. [9] The metal ion content in the cleaning solution is 100 mass ppt or less, and the organic impurity content in the cleaning solution is 100 mass ppm or less; The method for manufacturing a container according to [8], wherein the number of counted particles having a size of 30 nm or more as counted by a light scattering type liquid-borne particle counter is 50 or less per ml of cleaning liquid.

[10] A method for producing a container according to [2], comprising washing a substrate made of a composition containing a polyolefin and at least one metal component selected from the group consisting of Ti, Al, Mg, Zr, Hf, Fe, Ni, Sn, Zn, Cr, and Mo, with a washing liquid containing at least one selected from the group consisting of pure water, an acid, a base, and an organic solvent, to obtain the container according to [2], The content of metal ions in the cleaning solution is 100 ppt by mass or less, and the content of organic impurities in the cleaning solution is 100 ppm by mass or less; A method for manufacturing a container, in which the number of counted particles having a size of 30 nm or more, as counted by a light scattering liquid-borne particle counter, is 50 or less per ml of cleaning liquid.

[11] When the cleaning solution after cleaning contains one type of ion selected from the group consisting of Ti, Al, Mg, Zr, Hf, Fe, Ni, Sn, Zn, Cr, and Mo, the content of the one type of ion relative to the total mass of the cleaning solution after cleaning is 0.01 ppt by mass to 1.0 ppm by mass; The method for manufacturing a container according to any one of [8] to

[10] , wherein, when the cleaning liquid after cleaning contains two or more types of ions selected from the group consisting of Ti, Al, Mg, Zr, Hf, Fe, Ni, Sn, Zn, Cr, and Mo, the average content of the two or more types of ions relative to the total mass of the cleaning liquid after cleaning is 0.01 ppt by mass to 1.0 ppm by mass.

[12] The method for manufacturing a container according to any one of [8] to

[11] , wherein the cleaning liquid after cleaning contains organic impurities in an amount of 1.0 ppt to 500 ppm by mass.

[13] The method for manufacturing a container according to any one of [8] to

[12] , further comprising repeating washing until the washing liquid after washing satisfies requirements 1 and 2 described below.

[14] A drug solution container comprising the container according to any one of [1] to [7] and a drug solution contained in the container.

[15] The drug solution container according to

[14] , wherein the filling rate calculated by the formula (X) described below is 60 volume % or more.

[16] The drug solution container according to

[14] or

[15] , wherein the organic substance concentration calculated by the formula (Y) described below is 1 ppm by volume or less.

[17] A chemical solution containing water, the content of water in the chemical solution being 50 mass% or more, the chemical solution being applied to a substrate, and the change in density of particles with a particle size of 19 nm or less measured on the substrate before and after the application of the chemical solution using a particle inspection device is 0.3 particles / cm 2 The drug solution container according to any one of

[14] to

[16] , which is as follows:

[18] The chemical solution contains water, and the water content in the chemical solution is 50% by mass or less; The drug solution container according to any one of

[14] to

[17] , wherein particulate matter having a particle diameter of 30 nm or less in the drug solution is 1.0 ppb by mass or less relative to the total mass of the drug solution, as measured by a single particle inductively coupled plasma mass spectrometer.

[19] The drug solution container according to any one of

[14] to

[18] , wherein the drug solution further contains a surfactant. Effect of the Invention

[0009] According to the present invention, it is possible to provide a container in which the performance of the liquid medicine is unlikely to deteriorate over time even when the liquid medicine is stored for a long period of time (hereinafter, also referred to as "having the effect of the present invention"). Furthermore, according to the present invention, it is also possible to provide a method for manufacturing the container and a liquid medicine container. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below. The following description of the components may be based on a representative embodiment of the present invention, but the present invention is not limited to such an embodiment. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits. In this specification, the term "average" simply refers to the arithmetic mean. In addition, in the present invention, the term "preparation" includes not only synthesizing or compounding specific materials, but also procuring predetermined items by purchasing or the like. In the present invention, "ppm" stands for "parts-per-million (10 -6 ) and "ppb" stands for "parts-per-billion (10 -9 )" and "ppt" stands for "parts-per-trillion (10 -12 )" and "ppq" is "parts-per-quadrillion(10 -15 )".

[0011] [Container (first embodiment)] The container according to the first embodiment of the present invention is a container having a substrate (container body) and a coating layer having a thickness of 50 μm or more, which is disposed on at least a part of the substrate and contains a composition (hereinafter also referred to as the "specific composition") containing polyolefin and at least one metal component (hereinafter also referred to as the "specific metal") selected from the group consisting of Ti, Al, Mg, Zr, Hf, Fe, Ni, Sn, Zn, Cr, and Mo, and satisfies the requirements described below. In the above, the specific metal may be in the form of particles or ions.

[0012] High purity chemicals used in the semiconductor manufacturing process and / or high purity chemicals used for medical purposes such as sterilization or disinfection are required to have a certain level of cleanliness (reducing the amount of impurities that migrate from the container into the chemicals). In the container described in Patent Document 1, the amounts of specific hydrocarbon components and metal components extracted with ethanol are suppressed to below a certain level. However, according to the study by the present inventors, when a high-purity chemical solution, which is currently required, is stored in the container, impurity components may leach out of the container over time, causing the performance of the chemical solution to deteriorate. That is, it was found that the container of Patent Document 1 was insufficient for storing chemical solutions of a high purity level that is nowadays required.

[0013] As a result of extensive research into solving the above-mentioned problems, the inventors have discovered that the problems can be solved by controlling the distribution of specific components in the above-mentioned container between a position 10 nm in the thickness direction of the coating layer from the surface of the coating layer (the surface means the interface between the coating layer and another phase) as a reference (surface region), between a position 30 μm in the thickness direction of the container from the surface of the coating layer as a reference, and a position 50 μm in the thickness direction of the coating layer from the surface as a reference (internal region), and thus completed the present invention.

[0014] That is, in the container of this embodiment, when the composition contains one specific metal, when the surface region and the internal region are measured with a time-of-flight secondary ion mass spectrometer, in at least a part of the coating layer, the ratio RCAs calculated using the intensity ratio CA1s of the peak intensity of secondary ions derived from the specific metal in the surface region to the peak intensity of secondary ions derived from the polyolefin in the surface region, and the intensity ratio CA2s of the peak intensity of secondary ions derived from the one specific metal in the internal region to the peak intensity of secondary ions derived from the polyolefin in the internal region, is less than 1.00; or, when the composition contains two or more metal components, in at least a part of the coating layer, the average value of the RCAs calculated for each of the two or more specific metals is less than 1.00. The materials and properties of the container will be described in detail below.

[0015] The container according to this embodiment (hereinafter also referred to as "this container") is a container having a coating layer having a thickness of 50 μm or more containing a specific composition on at least a portion of a substrate, and a container having a coating layer having a thickness of 50 μm or more and made of a specific composition is preferred. The container preferably has a coating layer on at least a part of the liquid-contacting part (the part that may come into contact with the liquid when the liquid is contained in the container). That is, it is preferable that at least a part of the part on the substrate that becomes the liquid-contacting part has a coating layer, it is more preferable that the entire liquid-contacting part has a coating layer, it is even more preferable that the entire inner surface of the container has a coating layer, and it is particularly preferable that the entire surface of the container has a coating layer. In other words, in this container, it is preferable that a coating layer is disposed on the entire surface of the storage section of the container body (corresponding to the substrate) having a storage section capable of storing a medicinal solution, and it is more preferable that a coating layer is disposed on the entire surface of the container body.

[0016] [Base material] The container according to the present embodiment has a coating layer containing a specific composition on a substrate. The substrate is not particularly limited, and for example, organic materials (such as resins) and inorganic materials (such as glass and metals) can be used. The substrate is preferably a container body having a storage portion capable of storing a chemical solution.

[0017] In particular, in order to obtain a container having better effects of the present invention, it is preferable that the substrate contains a polyolefin and / or a corrosion-resistant material described below, and it is preferable that the substrate is made of a polyolefin and / or a corrosion-resistant material.

[0018] <Corrosion-resistant materials> The substrate is formed of at least one material (corrosion-resistant material) selected from the group consisting of fluororesin and electropolished metal materials, and the metal material contains at least one material selected from the group consisting of chromium and nickel, and it is preferable that the total content of chromium and nickel is more than 25 mass% based on the total mass of the metal material.

[0019] (Electrolytically polished metal material (electrolytically polished metal material)) The metal material used in producing the electrolytically polished metal material is not particularly limited as long as it contains at least one selected from the group consisting of chromium and nickel, and the total content of chromium and nickel is more than 25 mass% based on the total mass of the metal material, and examples thereof include stainless steel and nickel-chromium alloys. The total content of chromium and nickel in the metal material is preferably 25 mass % or more, and more preferably 30 mass % or more, based on the total mass of the metal material. The upper limit of the total content of chromium and nickel in the metal material is not particularly limited, but is generally preferably 90 mass % or less.

[0020] The stainless steel is not particularly limited, and known stainless steels can be used. Among them, an alloy containing 8% or more by mass of nickel is preferable, and an austenitic stainless steel containing 8% or more by mass of nickel is more preferable. Examples of austenitic stainless steel include SUS (Steel Use Stainless) 304 (Ni content 8% by mass, Cr content 18% by mass), SUS304L (Ni content 9% by mass, Cr content 18% by mass), SUS316 (Ni content 10% by mass, Cr content 16% by mass), and SUS316L (Ni content 12% by mass, Cr content 16% by mass). The Ni content and Cr content in the above parentheses are the content ratios relative to the total mass of the metal material.

[0021] The nickel-chromium alloy is not particularly limited, and any known nickel-chromium alloy can be used. Among them, a nickel-chromium alloy having a nickel content of 40 to 75 mass % and a chromium content of 1 to 30 mass % relative to the total mass of the metal material is preferred. Examples of nickel-chromium alloys include Hastelloy (trade name, the same applies below), Monel (trade name, the same applies below), and Inconel (trade name, the same applies below), etc. More specifically, examples include Hastelloy C-276 (Ni content 63 mass%, Cr content 16 mass%), Hastelloy-C (Ni content 60 mass%, Cr content 17 mass%), and Hastelloy C-22 (Ni content 61 mass%, Cr content 22 mass%), etc. Furthermore, the nickel-chromium alloy may further contain boron, silicon, tungsten, molybdenum, copper, cobalt, and the like, in addition to the above-mentioned alloy, as required.

[0022] The method for electrolytically polishing the metal material is not particularly limited, and any known method can be used. For example, the methods described in paragraphs

[0011] to

[0014] of JP 2015-227501 A and paragraphs

[0036] to

[0042] of JP 2008-264929 A can be used.

[0023] It is presumed that the chromium content in the surface passive layer of a metal material becomes higher than the chromium content in the parent phase due to electrolytic polishing. The metal material may be buffed. The method of buffing is not particularly limited, and known methods can be used. The size of the polishing grains used for finishing the buffing is not particularly limited, but #400 or less is preferable because it tends to reduce the unevenness of the surface of the metal material. The buffing is preferably performed before the electrolytic polishing.

[0024] (Fluorine resin) The fluororesin is not particularly limited as long as it is a resin (polymer) containing fluorine atoms, and known fluororesins can be used. Examples of the fluororesin include polytetrafluoroethylene, polychlorotrifluoroethylene, polyvinylidene fluoride, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, tetrafluoroethylene-ethylene copolymer, chlorotrifluoroethylene-ethylene copolymer, and perfluoro(butenyl vinyl ether) cyclized polymer (CYTOP (registered trademark)).

[0025] The thickness of the substrate is not particularly limited, but is generally preferably 100 μm to 500 mm.

[0026] The container according to the present embodiment has a coating layer disposed on a substrate, and the coating layer contains a specific composition, and preferably consists of the specific composition. The thickness of the coating layer is not particularly limited as long as it is 50 μm or more, but is generally preferably 3000 μm or less, and more preferably 2000 μm or less.

[0027] [Composition] <Polyolefin> The specific composition contains a polyolefin and a specific metal. The content of the polyolefin in the specific composition is not particularly limited, but is generally preferably 95.0 mass% or more, more preferably 98.0 mass% or more, based on the total mass of the composition. The upper limit is not particularly limited, but is generally preferably 99.99999 mass% or less.

[0028] In this specification, polyolefin means a polymer synthesized using olefins as monomers. Examples of polyolefin include polyethylene and polypropylene. In addition, a copolymer of ethylene and other α-olefins can also be used as the polyolefin. The α-olefin is not particularly limited, but includes α-olefins having 3 to 20 carbon atoms, more specifically, propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, and 1-tetradecene. The polyolefin may be used alone or in combination of two or more kinds. When two or more kinds of polyolefins are used in combination, it is preferable that the total content is within the above range.

[0029] Among them, the polyolefin is preferably at least one selected from the group consisting of polyethylene and copolymers of ethylene and α-olefin, more preferably polyethylene, in that a container having the more excellent effects of the present invention can be obtained. Among them, high density polyethylene (HDPE) is even more preferable, in that a container having the more excellent effects of the present invention can be obtained.

[0030] The weight average molecular weight (Mw) of HDPE is not particularly limited, but in general, it is preferably from 1,000 to 1,000,000, and more preferably from 5,000 to 500,000. The molecular weight distribution (Mw / Mn) of HDPE is not particularly limited, but is preferably 2.0 to 6.0. If the Mw / Mn value is 2.0 or more, the high-density polyethylene has excellent fluidity and is easy to be blow molded and injection molded. On the other hand, if it is 6.0 or less, the amount of low-molecular-weight components is reduced, and not only the cleanliness is improved but also the impact resistance is improved. The Mw / Mn value of the high-density polyethylene is more preferably 2.5 to 5.5, and even more preferably 3.0 to 5.0. In this specification, the weight-average molecular weight (Mw) and the number-average molecular weight (Mn) refer to values ​​calculated in terms of polystyrene by gel permeation chromatography.

[0031] <Specific metals> The specific composition contains a specific metal. The content of the specific metal in the specific composition is not particularly limited, but is generally preferably 0.1 to 100 ppm by mass, more preferably 0.1 to 30 ppm by mass, and even more preferably 0.1 to 20 ppm by mass, relative to the total mass of the specific composition.

[0032] The specific metal may be contained in the specific composition by being intentionally mixed with the polyolefin, or may be contained in the composition unintentionally (for example, as an impurity derived from the raw materials, or as contamination during the manufacturing process, etc.). A typical example of the specific composition containing a specific metal is when the specific metal is used as a polymerization catalyst for polyolefin, i.e., when the polymerization catalyst containing the specific metal used in the polymerization process of polyolefin remains in the specific composition.

[0033] The polymerization catalyst is not particularly limited, and examples thereof include Ziegler-Natta catalysts, metallocene catalysts, Phillips catalysts, etc. These catalysts may be used alone or in combination of two or more.

[0034] ·Ziegler-Natta catalyst The Ziegler-Natta catalyst may be a catalyst consisting of a solid catalyst component containing Mg, Ti, a halogen, and an electron donor, and an organoaluminum compound. The electron donor is an organic compound containing an oxygen atom, such as ethers and esters, with esters being preferred. Specific examples of the solid catalyst component include TiCl4, TiBr4, Ti(OEt)3Cl, and Ti(OEt)2Br. 2、 and the like. The organoaluminum compound is a compound containing at least one type of Al (aluminum)-carbon bond, and examples thereof include trimethyl Al, triethyl Al, and triisobutyl Al.

[0035] Metallocene catalyst The metallocene catalyst may be a catalyst comprising a complex of a Group 4 transition metal having a group having a cyclopentadiene-type anion skeleton and an aluminoxane. Examples of groups containing a cyclopentadiene-type anion skeleton include a cyclopentadienyl group, an n-butylcyclopentadienyl group, and an indenyl group, with an n-butylcyclopentadienyl group or an indenyl group being preferred.Further examples include those crosslinked with an alkylene group or a silylene group, such as a dimethylsilylenebisindenyl group and an ethylenebisindenyl group.

[0036] Examples of the Group 4 transition metal atom include Ti, Zr, and Hf, with Zr being preferred. Examples of complexes of Group 4 transition metal atoms having a group having a cyclopentadiene-type anion skeleton include dicyclopentadienyl zirconium dichloride, di-n-butylcyclopentadienyl zirconium dichloride, dimethylsilylene bisindenyl zirconium dichloride, and ethylene bisindenyl zirconium dichloride. An aluminoxane is a compound containing the structure -(Al(R)-O)n-, where R is an alkyl group having 1 to 4 carbon atoms, and the alkyl groups may be the same or different, and n is a number from 2 to 50. Examples of the alkyl group (R) of the aluminoxane include a methyl group, an ethyl group, etc. n is preferably 10 to 30. Examples of the aluminoxane include methylaluminoxane and ethylaluminoxane.

[0037] ·Philips Catalyst The Phillips catalyst is a chromium catalyst in which a chromium compound is supported on an inorganic oxide support such as silica, silica-alumina, or silica-titania, and activated in a non-reducing atmosphere to convert at least a portion of the supported chromium element to a hexavalent chromium. Phillips catalysts include CrO3, chromocene, silyl chromate and the like, which are described in U.S. Pat. Nos. 4,124,532 and 4,302,565.

[0038] Post-metallocene catalysts As for postmetallocene catalysts (for example, "Polyethylene Technology Reader" published by Kogyo Chosakai Co., Ltd. in 2001, "Living Polymerization with Homogeneous Transition Metal Catalysts" published by IPC Co., Ltd. in 1999, "Encyclopedia of Catalyst Usage" published by Kogyo Chosakai Co., Ltd. in 2004), those whose central metal is Ti, Zr, or Hf, which is in group 4B of the periodic table, or those whose central metal is Cr, Fe, or Ni, show high activity.

[0039] Other catalysts include standard catalysts composed of a main catalyst containing molybdenum oxide and a catalyst carrier made of aluminum oxide, and nickel-based catalysts, and are described in JP-A-5-175072 and JP-A-6-122721, etc.

[0040] The polymerization catalyst may be supported on a carrier. Such a carrier is not particularly limited. Examples of the organic carrier include (co)polymers of α-olefins having 2 to 10 carbon atoms (polyethylene, polypropylene, polybutene-1, ethylene-propylene copolymer, ethylene-butene-1 copolymer, ethylene-hexene-1 copolymer, propylene-butene-1 copolymer, and propylene-divinylbenzene copolymer), aromatic unsaturated hydrocarbon polymers (polystyrene and styrene-divinylbenzene copolymer), and polar group-containing polymers (polyacrylic acid esters, polymethacrylic acid esters, polyacrylonitrile, polyvinyl chloride, polyamides, and polycarbonates).

[0041] Examples of inorganic carriers include SiO2, Al2O3, MgO, TiO2, B2O3, CaO, ZnO, BaO, ThO, SiO2-MgO, SiO2-Al2O3, SiO2-V2O5, MgCl2, AlCl3, MnCl2, Na2CO3, K2CO3, CaCO3, MgCO3, Al2(SO4)3, BaSO4, KNO3, Mg(NO3)2, Mg(OH)2, Al(OH)3, and Ca(OH)2. The particle size of the carrier is not particularly limited, but is generally preferably 1 to 3000 μm, more preferably 5 to 2000 μm, and further preferably 10 to 1000 μm.

[0042] The form in which the specific composition contains the specific metal is not limited to the above. For example, Ti, Al, Mg, Zr, Hf, Fe, Ni, Sn, Zn, Cr, and Mo migrate as impurities from liquid-contacting parts of a polyolefin production apparatus (such as a reaction tank, a storage tank, and a pipeline) to polyolefin, resulting in the composition containing the specific metal.

[0043] <Other ingredients> The specific composition may contain components other than those described above. Examples of the components other than those described above include nucleating agents (crystal nucleating agents). Examples of the nucleating agents include phosphate metal salts, carboxylate metal salts, rosin metal salts, benzylidene sorbitol, quinacridone, cyanine blue, and talc. Among them, phosphate metal salts or carboxylate metal salts are preferred because they can provide a container with the effects of the present invention. The content of the nucleating agent in the specific composition is not particularly limited, but is generally preferably 0.01 to 2.0% by mass based on the total mass of the composition. The nucleating agent may be used alone or in combination of two or more. When two or more nucleating agents are used in combination, the total content is preferably within the above range.

[0044] Examples of the phosphate metal salt include sodium-2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate, sodium-2,2'-ethylidene-bis(4,6-di-t-butylphenyl)phosphate, lithium-2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate, lithium-2,2'-ethylidene-bis(4,6-di-t-butylphenyl)phosphate, calcium-bis[2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate] phosphate], magnesium bis[2,2'-methylene bis(4,6-di-t-butylphenyl) phosphate], aluminum tris[2,2'-methylene bis(4,6-di-t-butylphenyl) phosphate], 2,2'-methylene bis(4,6-di-t-butylphenyl) phosphate basic aluminum salt, and bis(2,4,8,10-tetra-t-butyl-hydroxy-12H-dibenzo[d,g][1,3,2]dioxaphosphocin-6-oxide)aluminum hydroxide.

[0045] Examples of the metal salt of a carboxylate include metal salts of aromatic carboxylic acids or aliphatic carboxylic acids, and specific examples thereof include aluminum benzoate, aluminum pt-butylbenzoate, sodium adipate, sodium thiophenecarboxylate, and sodium pyrrolecarboxylate.

[0046] [Physical properties of container] <rcas> In the container according to the embodiment of the present invention, when the specific composition contains one specific metal, at least a part of the coating layer has a surface S0 and a position S10 nm apart from the surface S0 in the thickness direction of the container. 10 Peak intensity I of secondary ions derived from polyolefin measured by a time-of-flight secondary ion mass spectrometer in the surface region between 10 , the peak intensity M of secondary ions originating from a specific metal 10 Intensity ratio CA1s(M 10 / I 10 ) and the peak intensity I of secondary ions derived from polyolefin measured by a time-of-flight secondary ion mass spectrometer between a position 30 μm from the surface in the thickness direction of the container and a position 50 μm from the surface in the thickness direction of the container (internal region). 50k The peak intensity M of secondary ions originating from one specific metal 50k Intensity ratio of CA2s (M 50k / I 50k ) The ratio RCAs calculated by CA1s / CA2s is less than 1.00, or When the specific composition contains two or more specific metals, the container has an average RCAs determined for each of the two or more specific metals in at least a portion of the coating layer of less than 1.00.

[0047] In addition, I 10 means the average peak intensity (integrated intensity) of secondary ions derived from polyolefin measured at each measurement point in the surface region, and the number of measurement points in the surface region is 20. 10 The same applies to. In addition, I 50k means the average peak intensity (integrated intensity) of secondary ions derived from polyolefin measured at each measurement point in the inner region, and the number of measurement points in the inner region is 20. 50k The same applies to. Detailed measurement conditions are as described in the Examples.

[0048] When a container satisfies RCAs < 1.00, it means that the surface area has a relatively low content of the specific metal compared to the internal area. If the liquid-contacting part of the container satisfies the above relationship, impurities are less likely to leach out of the container even when the container contains a chemical solution and is stored for a long period of time, and the performance of the chemical solution is more likely to be maintained.

[0049] RCAs is not particularly limited as long as it is less than 1.00, but is preferably 0.90 or less, more preferably less than 0.70, even more preferably less than 0.40, and particularly preferably 0.25 or less, in order to obtain a container having a better effect of the present invention. The lower limit is not particularly limited, but is generally preferably 0.001 or more. RCAs can be measured by time-of-flight secondary ion mass spectrometry. 10 , M 10 , I 50k , and M 50k The method for preparing the measurement sample and the measurement conditions are as described in the Examples.

[0050] It is sufficient that the above relationship is satisfied in at least a portion of the coating layer. However, in order to obtain a container having a better effect of the present invention, it is preferable that the relationship is satisfied in the portion of the coating layer that becomes the liquid-contacting portion, it is more preferable that the relationship is satisfied in the entire coating layer that becomes the liquid-contacting portion, and it is even more preferable that the relationship is satisfied in the entire coating layer.

[0051] The container according to the present embodiment may further include a lid. When the container according to the present embodiment includes a lid, the lid preferably has the same material and characteristics as the container.

[0052] [Container (second embodiment)] The container according to the second embodiment of the present invention is a container made of a specific composition and satisfies the requirements described below. The container according to the above embodiment will be described below, but materials and requirements not described below are the same as those in the first embodiment.

[0053] High purity chemicals used in the semiconductor manufacturing process and / or high purity chemicals used for medical purposes such as sterilization or disinfection are required to have a certain level of cleanliness (reducing the amount of impurities that migrate from the container into the chemicals). In the container described in Patent Document 1, the amounts of specific hydrocarbon components and metal components extracted with ethanol are suppressed to below a certain level. However, according to the studies of the present inventors, when a high-purity chemical solution, which is currently required, is stored in the container, impurity components may leach out of the container over time, causing the performance of the chemical solution to deteriorate over time. That is, it was found that the container of Patent Document 1 was insufficient for storing chemical solutions of a high purity level that is nowadays required.

[0054] As a result of extensive research into solving the above problems, the inventors have discovered that the problems can be solved by controlling the distribution of a specific component in a container made of a specific composition between a position 10 nm in the thickness direction of the container from the surface of the container (surface region), and between a position 30 μm in the thickness direction of the coating layer from the surface of the container and a position 50 μm in the thickness direction of the coating layer from the surface (internal region), and thus completed the present invention.

[0055] That is, in the container according to this embodiment, when the specific composition contains one specific metal, the surface region is defined as the region between the surface of the container and a position 10 nm in the thickness direction of the container from the surface, and the internal region is defined as the region between a position 30 μm in the thickness direction of the container from the surface and a position 50 μm in the thickness direction of the container from the surface, and when the surface region and the internal region are measured with a time-of-flight secondary ion mass spectrometer, in at least a part of the container, the ratio RCA calculated by CA1 / CA2, where CA1 is the intensity ratio of the peak intensity of secondary ions derived from metal components in the surface region to the peak intensity of secondary ions derived from polyolefin in the surface region, and CA2 is the intensity ratio of the peak intensity of secondary ions derived from metal components in the internal region to the peak intensity of secondary ions derived from polyolefin in the internal region, is less than 1.00, or When the specific composition contains two or more metal components, the container has an average RCA value determined for each of the two or more metal components in at least a portion of the container that is less than 1.00.

[0056] [Physical properties of container] In the container according to the embodiment of the present invention, when the specific composition contains one specific metal, at least a part of the surface has a surface S0 and a position S10 nm away from the surface S0 in the thickness direction of the container. 10 The peak intensity of secondary ions originating from polyolefin measured by a time-of-flight secondary ion mass spectrometer in the surface region between 10 , the peak intensity M of secondary ions originating from a specific metal 10 Intensity ratio CA1(M 10 / I 10 ), and the peak intensity I of secondary ions derived from polyolefin measured by a time-of-flight secondary ion mass spectrometer between a position 30 μm from the surface in the thickness direction of the container and a position 50 μm from the surface in the thickness direction of the container (inner region). 50k The peak intensity M of secondary ions originating from one specific metal 50k Intensity ratio of CA2(M 50k / I 50k ) The ratio RCA calculated by CA1 / CA2 is less than 1.00, or When the specific composition contains two or more specific metals, the container has an average RCA value of less than 1.00 calculated for each of the two or more specific metals on at least a portion of the surface.

[0057] In addition, I 10 means the average peak intensity (integrated intensity) of secondary ions derived from polyolefin measured at each measurement point in the surface region, and the number of measurement points in the surface region is 20. 10 The same applies to. In addition, I 50k means the average peak intensity (integrated intensity) of secondary ions derived from polyolefin measured at each measurement point in the inner region, and the number of measurement points in the inner region is 20. 50k The same applies to.

[0058] When a container satisfies RCA<1.00, it means that the surface area has a relatively low content of the specific metal compared to the internal area. If the liquid-contacting part of the container satisfies the above relationship, impurities are less likely to leach out from the container even when the container contains a chemical solution and stores it for a long period of time, and the performance of the chemical solution is more likely to be maintained.

[0059] The RCA is not particularly limited as long as it is less than 1.00, but is preferably 0.90 or less, more preferably less than 0.70, even more preferably less than 0.40, and particularly preferably 0.25 or less, in order to obtain a container having a better effect of the present invention. The lower limit is not particularly limited, but is generally preferably 0.001 or more. The RCA is a value that can be measured by time-of-flight secondary ion mass spectrometry, and the method for preparing the measurement sample and the measurement conditions are as described in the Examples.

[0060] It is sufficient that the above relationship is satisfied in at least a portion of the container, but in order to obtain a container having a better effect of the present invention, it is preferable that only a portion of the liquid-contacting portion of the container is satisfied, it is even more preferable that all of the liquid-contacting portion of the container is satisfied, and it is particularly preferable that the entire container is satisfied.

[0061] The container according to the present embodiment may further include a lid. When the container according to the present embodiment includes a lid, the lid preferably has the same material and characteristics as the container. In addition, the thickness of the container according to this embodiment is not particularly limited, but is generally preferably greater than 50 μm, more preferably 100 μm or more, and even more preferably 200 μm or more, and is preferably 100 mm or less, more preferably 80 mm or less, and even more preferably 50 mm or less.

[0062] [Container (third embodiment)] The container according to the third embodiment of the present invention is a container having a coating layer having a thickness of less than 50 μm and containing a specific composition on a substrate, and a container having a coating layer having a thickness of less than 50 μm and consisting of a specific composition is preferred.

[0063] High purity chemicals used in the semiconductor manufacturing process and / or high purity chemicals used for medical purposes such as sterilization or disinfection are required to have a certain level of cleanliness (reducing the amount of impurities that migrate from the container into the chemicals). In the container described in Patent Document 1, the amounts of specific hydrocarbon components and metal components extracted with ethanol are suppressed to below a certain level. However, according to the studies of the present inventors, when a high-purity chemical solution, which is currently required, is stored in the container, impurity components may leach out of the container over time, causing the performance of the chemical solution to deteriorate. That is, it was found that the container of Patent Document 1 was insufficient for storing chemical solutions of a high purity level that is nowadays required.

[0064] As a result of extensive research into solving the above-mentioned problems, the inventors have discovered that the problems can be solved by controlling the distribution of specific components in the above-mentioned container between a position 10 nm in the thickness direction of the coating layer from the surface of the coating layer (surface region), and between a position corresponding to 70% of the total thickness of the coating layer in the thickness direction of the coating layer from the surface of the coating layer, and a position corresponding to 100% of the total thickness of the coating layer in the thickness direction of the coating layer from the surface of the coating layer (internal region), thereby completing the present invention.

[0065] That is, the container according to the present embodiment is a container having a substrate and a coating layer having a thickness of less than 50 μm, which contains a specific composition and is disposed on at least a portion of the substrate, and when the specific composition contains one type of specific metal, the surface region is defined as a region between the surface of the coating layer and a position of 10 nm in the thickness direction of the coating layer from the surface as a reference, and the internal region is defined as a region between a position corresponding to a thickness of 70% of the total thickness of the coating layer from the surface as a reference in the thickness direction of the coating layer and a position corresponding to a thickness of 100% of the total thickness of the coating layer from the surface as a reference in the thickness direction of the coating layer, and when the surface region and the internal region are measured with a time-of-flight secondary ion mass spectrometer, A container in which, in at least a portion of the layer, the ratio RCAt calculated using CA1t / CA2t, where CA1t is the intensity ratio of the peak intensity of secondary ions derived from the metal component in the surface region to the peak intensity of secondary ions derived from the polyolefin in the surface region, and CA2t is the intensity ratio of the peak intensity of secondary ions derived from the metal component in the internal region to the peak intensity of secondary ions derived from the polyolefin in the internal region, is less than 1.00, or, when a specific composition contains two or more metal components, the average value of RCAt calculated for each of the two or more metal components in at least a portion of the coating layer is less than 1.00.

[0066] When a container satisfies RCAt<1.00, it means that the surface area has a relatively low content of the specific metal compared to the internal area. If the liquid-contacting part of the container satisfies the above relationship, impurities are less likely to leach out from the container even when the chemical solution is stored in the container for a long period of time, and the performance of the chemical solution is more likely to be maintained.

[0067] RCAt is not particularly limited as long as it is less than 1.00, but is preferably 0.90 or less, more preferably less than 0.70, even more preferably less than 0.40, and particularly preferably 0.25 or less, in order to obtain a container having a better effect of the present invention. The lower limit is not particularly limited, but is generally preferably 0.001 or more. It should be noted that RCAt is a value that can be measured by time-of-flight secondary ion mass spectrometry, and the method for preparing the measurement sample and the measurement conditions are as described in the Examples.

[0068] It is sufficient that the above relationship is satisfied over at least a portion of the surface of the coating layer. However, in order to obtain a container having a better effect of the present invention, it is preferable that the relationship is satisfied over a portion of the liquid-contacting portion, it is even more preferable that the relationship is satisfied over the entire liquid-contacting portion, and it is particularly preferable that the relationship is satisfied over the entire surface of the coating layer.

[0069] The container according to the present embodiment may further include a lid. When the container according to the present embodiment includes a lid, the lid preferably has the same material and characteristics as the container.

[0070] The container according to the present embodiment has a coating layer disposed on a substrate, and the coating layer contains a specific composition, and preferably consists of the specific composition. The thickness of the coating layer is not particularly limited as long as it is less than 50 μm, but in general, it is preferably 20 μm or more, and more preferably 30 μm or more.

[0071] [Container physical properties (other)] [RCB] In the containers according to the embodiments of the present invention described so far, it is preferable that the RCB determined by the following method is less than 1.0 in at least a part of the container (or the coating layer if present), in order to obtain a container having better effects of the present invention. In order to obtain a container having better effects of the present invention, the above relationship is preferably satisfied in a part of the liquid-contacting part, more preferably satisfied in the entire liquid-contacting part, and even more preferably satisfied in the entire surface (or coating layer). As described later, RCB is a value reflecting the distribution of components derived from polyolefins (particularly polyolefins with a low degree of polymerization) and components derived from nucleating agents in a container, and the fact that RCB is less than 1.0 in a part of the surface means that the content of components derived from polyolefins (particularly polyolefins with a low degree of polymerization) and / or components derived from nucleating agents in the surface region is relatively low compared to the inner region. According to the study by the present inventors, it has been found that components derived from polyolefins (particularly polyolefins with a low degree of polymerization) and components derived from nucleating agents are dissolved over time into the chemical solution contained in the container, and therefore become one of the factors that deteriorate the performance of the chemical solution when stored for a long period of time. Note that the "components derived from" include the components themselves, as well as their reaction products and decomposition products. When the container according to the embodiment of the present invention satisfies RCB<1.00, components derived from polyolefins (especially polyolefins with a low degree of polymerization) and / or components derived from nucleating agents are less likely to dissolve into the chemical solution stored in the container, and as a result, the performance of the chemical solution is more likely to be maintained for a long period of time.

[0072] Below we explain how to calculate RCB.

[0073] (CB1) CB1 is the surface region measured by a time-of-flight secondary ion mass spectrometer, and is the L 10 / I 10 , A 10 / I 10 , and P 10 / I 10 It is calculated as the arithmetic mean of (A) Peak intensity of secondary ions derived from polyolefin I 10 For C n H 2n - the secondary ion peak intensity L 10 Intensity ratio (L 10 / I 10 ) (B) Peak intensity of secondary ions derived from polyolefin I 10 For C p H 2p The peak intensity of the secondary ion represented by COO- is A 10 Intensity ratio (A 10 / I 10 ) (C) Peak intensity of secondary ions derived from polyolefin I 10 For C q H 2q The secondary ion peak intensity P is represented by PO2- 10 Intensity ratio (P 10 / I 10 ) In addition, n represents an integer of 12 to 20, p represents an integer of 8 to 24, and q represents an integer of 8 to 24. In the above, (A) reflects the content of components derived from polyolefins with low degrees of polymerization in the surface region, and (B) and (C) reflect the content of components derived from the nucleating agent in the surface region.

[0074] (CB2) CB2 is the above L measured by a time-of-flight secondary ion mass spectrometer in the inner region. 50k / I 50k , A 50k / I 50k , and P 50k / I 50k It is calculated as the arithmetic mean of (a) Peak intensity of secondary ions derived from polyolefin I 50k For C n H 2n - the secondary ion peak intensity L 50k Intensity ratio (L 50k / I 50k ) (b) Peak intensity of secondary ions derived from polyolefin (I 50k ) for C p H 2p The peak intensity of the secondary ions represented by COO- (A 50k ) intensity ratio (A 50k / I 50k ) (c) Peak intensity of secondary ions derived from polyolefin (I 50k ) for C q H 2q The peak intensity of the secondary ion represented by PO2- (P 50k ) intensity ratio (P 50k / I 50k ) The definitions of n, p and q are as described above.

[0075] The RCB calculated by CB1 / CB2 is not particularly limited as long as it is less than 1.00, but is more preferably less than 0.70, and even more preferably less than 0.40, in order to obtain a container having a better effect of the present invention. The lower limit is not particularly limited, but is generally preferably 0.001 or more. RCB can be measured by time-of-flight secondary ion mass spectrometry. 10 , L 10 , A 10 , P 10 , I 50k , L 50k , A 50k , and P 50k The method for preparing the measurement sample and the measurement conditions are as described in the Examples.

[0076] [Amount of metal components and organic impurities dissolved in pure water] In order to obtain a container having better effects of the present invention, the container preferably satisfies the following requirement A and / or requirement B, and more preferably satisfies requirements A and B, in the following dissolution test.

[0077] Dissolution test: 100 ml of pure water at 40°C is placed in a container so that the volume of the container is 50% by volume, and the container is kept in this state for one day. Requirement A: The average content of metal components contained in the pure water after the elution test is 1.0 ppb by mass or less (preferably, 10 ppt by mass or less, and more preferably, 1 ppt by mass or less). Requirement B: TOC (total organic carbon) in the pure water after the elution test is 1000 ppm by mass or less (preferably 100 ppm by mass or less, and more preferably 1 ppm by mass or less).

[0078] In the elution test, the pure water after the elution test may contain any one of the metal elements Fe, Cr, and Ni. When Fe is contained in the pure water after the elution test, the content of Fe in the pure water after the elution test is preferably 0.01 mass ppt to 0.30 mass ppb. The upper limit is preferably 0.1 mass ppb or less, more preferably 0.01 mass ppb or less, and even more preferably 0.001 mass ppb or less. When Cr is contained in the pure water after the elution test, the Cr content in the pure water after the elution test is preferably 0.01 mass ppt to 0.30 mass ppb. The upper limit is preferably 0.1 mass ppb or less, more preferably 0.01 mass ppb or less, and even more preferably 0.001 mass ppb or less. When Ni is contained in the pure water after the elution test, the Ni content in the pure water after the elution test is preferably 0.01 mass ppt to 0.30 mass ppb. The upper limit is preferably 0.1 mass ppb or less, more preferably 0.01 mass ppb or less, and even more preferably 0.001 mass ppb or less. When the content of each metal element (Fe, Cr, Ni) is equal to or less than the upper limit value described above, the occurrence of defects after processing the wafer with the chemical solution contained in the container is further suppressed. Also, when the content of each metal element (Fe, Cr, Ni) is equal to or more than the lower limit value described above, the load of the cleaning process on the container can be reduced in the first place, and as a result, damage to the container caused by the cleaning process can be suppressed, and the elution of organic impurities from the container can be suppressed.

[0079] In the elution test, the pure water after the elution test may contain a compound selected from the group consisting of aliphatic amides and organic substances having a boiling point of 300°C or higher, and the organic substance having a boiling point of 300°C or higher may contain an alkyl olefin (preferably, a low-polymerization alkyl olefin). The low-polymerization alkyl olefin means an alkyl olefin having 22 or less carbon atoms. The aliphatic amide may contain an aliphatic chain having 16 or more carbon atoms linked to a carbonyl group. The aliphatic chain may have a substituent. The boiling point means a boiling point at 1 atmospheric pressure. The content of the above compound in the pure water after the elution test is preferably 0.1 ppb by mass to 1000 ppm by mass relative to the total mass of the pure water. The content of the aliphatic amide in the pure water after the elution test is preferably 0.1 ppb by mass to 1000 ppm by mass. The content of alkylolefin in the pure water after the elution test is preferably 0.1 ppb by mass to 1000 ppm by mass. When the content of the above components is equal to or less than the upper limit value described above, the occurrence of defects after processing the wafer with the chemical solution contained in the container is further suppressed. When the content of the above components (particularly, the aliphatic amide) is equal to or more than the lower limit value described above, further deterioration of defects can be suppressed when the chemical solution contained in the container is used after long-term storage. Although the mechanism of suppression is unclear, it is thought that the above components are eluted in small amounts from the container into the chemical solution, interacting with the inorganic impurities and metal ions contained in extremely small amounts in the chemical solution to stabilize the inorganic impurities and metal ions, thereby suppressing the growth of defect sources derived from them.

[0080] The metal content can be measured using ICP-MS, and TOC can be measured using a total organic carbon meter. In order to improve the detection sensitivity, the drug solution to be evaluated may be concentrated in advance and then evaluated. The concentration ratio is appropriately selected from an optimum ratio of about 2 to 100,000.

[0081] [First embodiment of container manufacturing method] The first embodiment of the method for producing a container of the present invention is a method for producing a container, comprising the steps of contacting a specific composition on a substrate to form a pre-washing coating layer, and cleaning the pre-washing coating layer with a cleaning liquid containing at least one selected from the group consisting of pure water, an acid, a base, and an organic solvent to obtain a container. Each step will be described in detail below.

[0082] <Pre-cleaning coating layer formation process> In this step, first, a substrate is prepared. The material of the substrate prepared in this step is not particularly limited, but it is preferable to use the substrate already described. The shape of the substrate is not particularly limited, but it is preferable to use a shape suitable for containing a liquid. The substrate may also be formed using a specific composition. However, in this case, the specific composition is different from the specific composition that forms the pre-cleaning coating layer. The shape of the substrate is not particularly limited, and may be any shape suitable for containing a liquid.

[0083] This step may further include a step of subjecting a part or the whole of the surface of the substrate to an easy-adhesion treatment and / or a step of forming an easy-adhesion layer on a part or the whole of the surface of the substrate. That is, the substrate may be an easy-adhesion treated substrate or a substrate with an easy-adhesion layer. The easy-adhesion treatment is not particularly limited, and examples thereof include a method of irradiating the surface of the substrate with plasma and irradiating with ionizing radiation, etc. The easy-adhesion layer can be formed by applying a known adhesive.

[0084] This step is a step of contacting the specific composition on a substrate to obtain a pre-cleaning coating layer. On the substrate means at least a part of the surface of the substrate, preferably a part of the part that forms the liquid-contacting part in the formed container, more preferably the entire part that forms the liquid-contacting part, and even more preferably the entire surface. The method for contacting the composition with the substrate is not particularly limited, and examples thereof include a method of simultaneously forming the substrate and the pre-cleaning coating layer by co-extrusion (lamination, blowing, etc.), a method of applying a specific composition to the substrate and drying and / or baking to form a coating film-like pre-cleaning coating layer, etc. Among these, the co-extrusion method is preferred because it allows a container to be obtained more easily.

[0085] A specific composition for forming the coating layer used to form the pre-cleaning coating layer will now be described. The specific composition for forming the coating layer is not particularly limited as long as it contains polyolefin and specific metal. When the container is formed by co-extrusion, the specific composition for forming the coating layer is typically prepared as pellets, which are melted and extruded. At this time, the pellets are preferably washed with the washing solution already described. Washing the pellets makes it easier to obtain a container that meets the specified requirements.

[0086] This manufacturing method has a cleaning step after the pre-cleaning coating layer forming step. The cleaning step is a step of cleaning the surface of the pre-cleaning coating layer using a cleaning liquid described below. By cleaning the surface of the pre-cleaning coating layer with a predetermined cleaning liquid, the content of the specific metal in the surface region of the obtained coating layer tends to be lower than the content of the specific metal in the internal region. In this step, the surface means a part of the coating layer, and preferably a part of the part constituting the liquid-contacting part of the coating layer, more preferably the entire part of the coating layer constituting the liquid-contacting part, even more preferably the entire coating layer, and particularly preferably the entire surface of the container.

[0087] Cleaning process The cleaning step is a step of cleaning the pre-cleaned coating layer with a cleaning liquid containing at least one selected from the group consisting of pure water, an acid, a base, and an organic solvent.

[0088] The cleaning liquid may contain at least one selected from the group consisting of pure water, an acid, a base, and an organic solvent (hereinafter also referred to as "main agent"), and may contain two or more. In particular, it is preferable that the cleaning liquid contains at least one selected from the group consisting of an acid, a base, and an organic solvent, in order to obtain a container having a more excellent effect of the present invention. The content of the base agent in the cleaning solution is not particularly limited, but is generally preferably 99.98 to 100% by mass based on the total mass of the cleaning solution. The base agent may be used alone or in combination of two or more. When two or more base agents are used in combination, the total content is preferably within the above range.

[0089] The acid as the base agent is not particularly limited, and any acid known for use in cleaning solutions can be used. Examples of the acid include hydrochloric acid, hydrofluoric acid, sulfuric acid, nitric acid, phosphoric acid (H3PO4), phosphonic acid (H3PO3), organic acids, and mixtures of these with water. As the organic acid, for example, the acids described in paragraphs 0031 and 0032 of JP2014-232872A can be used. The base as the base agent is not particularly limited, and a known base for cleaning can be used. Examples of the base include ammonium salts such as ammonium sulfate, water-soluble nitrogen-containing compounds such as triethanolamine and diethanolamine, and mixtures of ammonium sulfate and water. In addition, inorganic bases and organic bases described in paragraphs 0030 to 0068 of JP 2014-232874 A can also be used. The organic solvent as the base agent is not particularly limited, and a known organic solvent for cleaning can be used. The organic solvent can be appropriately selected from at least one organic solvent selected from the group consisting of hydrocarbon solvents, ketone solvents, ester solvents, alcohol solvents, amide solvents, and ether solvents. Specific examples include IPA (isopropyl alcohol), propylene glycol monoalkyl ether, methyl isobutyl carbinol, cyclohexane, methyl ethyl ketone, methyl isobutyl ketone, butyl acetate, isopropyl acetate, propylene glycol monomethyl ether acetate, ethyl lactate, gamma butyrolactone, and mixtures thereof, as well as mixtures of these with water.

[0090] The cleaning solution used in the cleaning step may contain metal ions. The content of metal ions is not particularly limited, but is preferably 100 mass ppt or less, more preferably 50 mass ppt or less, and even more preferably 20 mass ppt or less. The lower limit is not particularly limited, but is preferably 0.01 mass ppt or more in terms of the lower limit of quantification. In this specification, the content of metal ions contained in the cleaning solution can be measured using an ICP-MS (inductively coupled plasma mass spectrometer). When two or more types of metal ions are contained in the cleaning solution, the above value is the arithmetic average of the content of each metal ion.

[0091] The cleaning solution used in the cleaning step may contain organic impurities. In this specification, organic impurities refer to organic compounds other than the main component in the cleaning solution. The content of organic impurities in the cleaning solution is not particularly limited, but is preferably 100 mass ppm or less, more preferably 50 mass ppm or less, and even more preferably 30 mass ppm or less. The lower limit is not particularly limited, but is preferably 1.0 mass ppt or more, more preferably 0.1 mass ppm or more, from the viewpoint of the lower limit of quantification. In this specification, the content of organic impurities contained in the cleaning solution can be measured by the method described in the Examples using a GC-MS (gas chromatograph mass spectrometer). When the cleaning solution contains two or more types of organic impurities, the above value is the arithmetic average of the contents of each organic impurity.

[0092] In addition, the number of countable particles having a size of 30 nm or more, as counted by a light scattering type liquid particle counter, is preferably 50 or less per ml of the cleaning liquid. In order to obtain a container having a better effect, the number of countable particles is preferably 100 or less, and more preferably 50 or less, per ml of the cleaning liquid. The lower limit is not particularly limited, but from the viewpoint of the lower limit of quantification, generally, 0.1 or more is preferable.

[0093] In particular, in terms of obtaining a container having a more excellent effect of the present invention, it is preferable that the cleaning liquid contains metal ions of 100 ppt by mass or less, contains organic impurities of 100 ppm by mass or less, and contains 50 or less counted particles having a size of 30 nm or more per ml of cleaning liquid as counted by a light scattering type liquid-borne particle counter.

[0094] The cleaning method for cleaning the pre-cleaning coating layer is not particularly limited, and examples of the cleaning method include immersing the pre-cleaning coating layer in a cleaning liquid (the effect can be further enhanced by irradiating the layer with ultrasonic waves during immersion and / or by heating the cleaning liquid), spraying the cleaning liquid onto the pre-cleaning coating layer, and the like. The cleaning solution may be used alone or in combination of two or more. When two or more cleaning solutions are used in combination, the cleaning solutions may be mixed and used, or the container may be washed in sequence with two or more cleaning solutions. In particular, it is preferable to wash the container in sequence with two or more cleaning solutions, since this provides a container with a more excellent effect of the present invention.

[0095] ·Confirmation process The cleaning step may further include a confirmation step of measuring the content of impurities and the like contained in the cleaning liquid after cleaning and confirming whether the value is within a predetermined numerical range. By confirming the content of impurities and the like contained in the cleaning liquid in the confirmation step, the progress of cleaning of the substrate can be grasped. In the confirmation step, examples of impurities to be confirmed include metal ions (particularly ions of a specific metal) and organic impurities contained in the cleaning liquid after cleaning.

[0096] As a confirmation step, it is preferable to repeat washing until the washing solution after washing satisfies the following requirements 1 and 2. Requirement 1: When the cleaning solution after cleaning contains one type of specific metal ion (ion of a specific metal), the content of the one type of specific metal ion is 1.0 ppt by mass or less (more preferably, 0.01 ppt by mass to 0.5 ppm by mass); or, when the cleaning solution after cleaning contains two or more types of specific metal ions, the average content of the two or more types of specific metal ions is 1.0 ppt by mass or less (more preferably, 0.01 ppt by mass to 0.5 ppm by mass). Requirement 2: When the cleaning solution after cleaning contains one type of organic impurity, the content of the organic impurity is 500 ppm by mass or less, or when the cleaning solution after cleaning contains two or more types of organic impurities, the average content of the two or more types of organic impurities is 500 ppt by mass or less (more preferably, 1.0 ppt by mass to 300 ppm by mass).

[0097] The content of specific metal ions in the cleaning solution can be measured by ICP-MS. The content of organic impurities in the cleaning solution can be measured by GC-MS.

[0098] In the case of requirements 1 and 2, when the content of each of the above components contained in the cleaning solution is equal to or less than the upper limit, the cleaning is sufficiently performed, and the above components are prevented from adhering again to the cleaning target even when the cleaning target is washed multiple times with the same cleaning solution. The lower limit is generally selected from the lower limit of quantification.

[0099] In the washing step, washing may be performed once or multiple times. In particular, in order to obtain a container having a more excellent effect of the present invention, the washing step is preferably a step of washing the substrate with a washing liquid, and then repeatedly washing the coating layer with the washing liquid until the content of specific metal ions in the washing liquid after washing is 1.0 mass ppm or less and the content of organic impurities is 500 mass ppm or less. The cleaning progress of the coating layer can be grasped by repeatedly using the cleaning solution and checking the content of impurities, etc., contained in the cleaning solution after cleaning by the method already described. According to the container manufacturing method having the above steps, a container that meets the specified requirements can be manufactured more reliably.

[0100] [Second embodiment of container manufacturing method] The second embodiment of the method for producing a container of the present invention is a method for producing a container made of a composition, and includes the following steps. Each step will be described in detail below.

[0101] <Step of Preparing the Substrate> The step of obtaining a substrate is a step of preparing a substrate molded using a composition containing a polyolefin and a specific metal. Methods for preparing a substrate include, for example, purchasing and procurement, and synthesis and molding.

[0102] The synthesis method of the polyolefin used for the substrate is not particularly limited, and a known synthesis method can be used. Examples of known synthesis methods include slurry polymerization and gas phase polymerization. The polymerization pressure is not particularly limited, but is preferably 1 to 100 atm, and more preferably 3 to 30 atm. The polymerization temperature is not particularly limited, but is preferably 20°C to 115°C, and more preferably 50 to 90°C. Among them, the slurry polymerization method is preferred in that a container having a better effect of the present invention can be obtained. In addition, examples of the solvent used in the slurry polymerization method include isobutane, isopentane, heptane, hexane, and octane.

[0103] The method for forming the substrate by molding the polyolefin synthesized above is not particularly limited, and any known method can be used. Examples of known molding methods include blow molding and injection molding, and the molding conditions are also known.

[0104] <Cleaning process> The cleaning step is a step of cleaning the prepared substrate with a cleaning liquid containing at least one selected from the group consisting of pure water, an acid, a base, and an organic solvent to obtain a container. The cleaning liquid and cleaning method are the same as those described in the first embodiment. [Drug solution container] The liquid medicine container according to the embodiment of the present invention includes the container described above and the liquid medicine contained in the container. Since the container satisfies certain requirements, the performance of the liquid medicine contained in the liquid medicine container is unlikely to deteriorate even when stored for a long period of time. In order to prevent contamination of the chemical solution by the TOC components contained in the voids and to prevent deterioration of the chemical solution due to oxygen contained in the voids, the filling rate in the container calculated by formula (X) is preferably 60% by volume or more, more preferably 70% by volume or more, and even more preferably 85% by volume or more. There is no particular upper limit, but it is often 99% by volume or less. Formula (X): Filling rate = (Volume of drug solution in container / Volume of container) x 100 In order to prevent contamination of the chemical solution with the TOC components contained in the voids, the organic concentration calculated by formula (Y) is preferably 1 ppm by volume or less. There is no particular lower limit to the organic concentration, but it is often 0.1 ppb by volume or more. Formula (Y): Organic matter concentration = (volume of organic matter contained in the space in the container that is not filled with chemical solution / volume of the space in the container that is not filled with chemical solution) x 100 However, the organic matter does not include components contained in the chemical solution. Additionally, the volume of organic matter is estimated at 1 g / 1 mL.

[0105] [Chemical solution] The chemical liquid contained in the chemical liquid container is not particularly limited, and may be water-based or organic solvent-based. In this specification, water-based means that the content of water contained in the chemical liquid exceeds 50 mass% based on the total mass of the chemical liquid, and solvent-based means that the content of organic solvent contained in the chemical liquid (the total amount when two or more organic solvents are contained) exceeds 50 mass%.

[0106] <Water system> The aqueous chemical solution contains water. The content of water in the chemical solution is not particularly limited as long as it exceeds 50% by mass based on the total mass of the chemical solution. Examples of components contained in the aqueous chemical liquid include an alkaline developer, a resist stripper, an etching liquid, a chemical mechanical polishing (CMP) slurry, and a post-CMP cleaner.

[0107] The water is not particularly limited, but is preferably ultrapure water used in semiconductor manufacturing, and more preferably water obtained by further purifying the ultrapure water to reduce the content of inorganic anions and metal ions. The purification method is not particularly limited, but purification using a filtration membrane or an ion exchange membrane, and purification by distillation are preferred. In addition, it is preferable to purify the water by the method described in JP-A-2007-254168, for example. The water preferably contains less than 0.001 ppt by weight of metals.

[0108] (First embodiment of aqueous chemical solution) A first embodiment of the aqueous chemical solution includes (1) hydrofluoric acid or a salt of hydrofluoric acid (examples of the base include organic amines such as hydroxylamines, primary, secondary or tertiary aliphatic amines, alicyclic amines, aromatic amines, heterocyclic amines, etc., ammonia water, and lower alkyl quaternary ammonium hydroxides), (2) an alkali compound (e.g., one selected from the group consisting of hydroxylamine or a salt thereof, an amine, an amidine compound, and a quaternary ammonium compound), and (3) others (water-soluble organic solvents, pH adjusters, surfactants, corrosion inhibitors, etc.) and water. The above-mentioned chemical liquid can be used as a resist stripper, an etching liquid, a cleaning liquid, and the like.

[0109] (Second embodiment of aqueous chemical solution) A second embodiment of the aqueous chemical solution includes a chemical solution containing (1) abrasive grains such as colloidal silica, (2) an oxidizing agent such as hydrogen peroxide, (3) a corrosion inhibitor such as an azole compound, and (4) other substances (amino acids, pH adjusters, surfactants, etc.), and water. The above-mentioned chemical solution can be used as a CMP slurry.

[0110] (Third embodiment of aqueous chemical solution) A third embodiment of the aqueous chemical solution is a mixture of sulfuric acid, hydrogen peroxide, and water. The above-mentioned chemical solution can be used as a stripping solution, a cleaning solution, and the like.

[0111] (Fourth embodiment of aqueous chemical solution) A fourth embodiment of the aqueous solution is a solution containing a quaternary ammonium compound and water. The solution can be used as a developer, for example.

[0112] ·Quaternary ammonium compounds The chemical solution contains a quaternary ammonium compound represented by the following general formula (N).

[0113] [ka] In general formula (N), R N1 ~R N4 each independently represents an alkyl group, a phenyl group, a benzyl group, or a cyclohexyl group, and these groups may have a substituent.

[0114] R N1 ~R N4 The alkyl group preferably has 1 to 8 carbon atoms, and more preferably has 1 to 4 carbon atoms. R N1 ~R N4 Examples of the substituent that the alkyl group, phenyl group, benzyl group or cyclohexyl group may have include a hydroxy group.

[0115] Examples of quaternary ammonium compounds include tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide (TEAH), tetrapropylammonium hydroxide, and tetrabutylammonium hydroxide (TBAH). hydroxide), tetrapentylammonium hydroxide, tetrahexylammonium hydroxide, tetraoctylammonium hydroxide, ethyltrimethylammonium hydroxide, butyltrimethylammonium hydroxide, methyltriamylammonium hydroxide, dibutyldipentylammonium hydroxide, triethylphenylammonium hydroxide, trimethylbenzylammonium hydroxide, triethylbenzylammonium hydroxide, tribenzylmethylammonium hydroxide, tetrabenzylammonium hydroxide, trimethylcyclohexylammonium hydroxide, tributylcyclohexylammonium hydroxide, monohydroxyethyltrimethylammonium hydroxide, dihydroxyethyldimethylammonium hydroxide (dimethylbis(2-hydroxyethyl)ammonium hydroxide), trihydroxyethylmonomethylammonium hydroxide, monohydroxyethyltriethylammonium hydroxide, dihydroxyethyldiethylammonium hydroxide, trihydroxyethylmonoethylammonium hydroxide, monohydroxypropyltrimethylammonium hydroxide, dihydroxypropyldimethylammonium hydroxide, trihydroxypropylmonomethylammonium hydroxide, monohydroxypropyltriethylammonium hydroxide, dihydroxypropyldiethylammonium hydroxide, and trihydroxypropylmonoethylammonium hydroxide.

[0116] Among these, the quaternary ammonium compound is preferably tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrabutylammonium hydroxide, or dimethylbis(2-hydroxyethyl)ammonium hydroxide, and more preferably tetramethylammonium hydroxide or dimethylbis(2-hydroxyethyl)ammonium hydroxide.

[0117] The content of the quaternary ammonium compound in the chemical solution is not particularly limited, but generally, it is preferably 25% by mass or less, more preferably 20% by mass or less, preferably 15% by mass or more, and more preferably 10% by mass or more, based on the total mass of the chemical solution. The quaternary ammonium compound may be used alone or in combination of two or more. When two or more quaternary ammonium compounds are used in combination, the total content is preferably within the above range.

[0118] The quaternary ammonium compound can be purified by known methods, for example, by adsorption purification using silicon carbide as described in International Publication WO12 / 043496, followed by repeated filtration.

[0119] Chelating agents The chemical solution may contain a chelating agent. The chelating agent is not particularly limited, but is preferably a compound that forms a coordinate bond with a metal atom via two or more functional groups in one molecule. The functional group is preferably a metal-adsorbing group. It is more preferable that the chelating agent contains two or more metal-adsorbing groups in one molecule.

[0120] The metal-adsorbing group is preferably an acid group or a cationic group. The acid group preferably has an acid dissociation constant (pKa) of 7 or less. Examples of the acid group include a phenolic hydroxyl group, -COOH, -SO3H, -OSO3H, -PO3H2, -OPO3H2, and COCH2COCH3. The acid group is particularly preferably -COOH.

[0121] These acid groups may also be in the form of salts of the acid groups, such as metal salts and salts of nitrogen-containing cations.

[0122] The metal salt is preferably at least one salt selected from the group consisting of Na, K, Ca, Fe, Cu, Mg, Mn, Li, Al, Cr, Ni, and Zn.

[0123] The nitrogen-containing cation is not particularly limited as long as it is a quaternary ammonium cation or a cation which is a hydrogen adduct of an amine. Examples of the quaternary ammonium cation include tetramethylammonium cation, tetraethylammonium cation, tetrapropylammonium cation, methyltributylammonium cation, tetrabutylammonium cation, and choline type cation (hydroxyethyltrimethylammonium cation). Among these, tetramethylammonium cation, tetraethylammonium cation, tetrapropylammonium cation, tetrabutylammonium cation, or choline-type cation is preferred, and tetramethylammonium cation, tetraethylammonium cation, tetrapropylammonium cation, or choline-type cation is more preferred.

[0124] The cationic polymer may also be a counter ion.

[0125] The cationic group as the metal-adsorbing group is preferably an onium group. Examples of the onium group include ammonium group, phosphonium group, arsonium group, stibonium group, oxonium group, sulfonium group, selenonium group, stannonium group, and iodonium group. The onium group is preferably an ammonium group, phosphonium group, or sulfonium group, more preferably an ammonium group or phosphonium group, and even more preferably an ammonium group.

[0126] A specific example of the chelating agent of the present invention is a compound having a carboxy group (hereinafter, also referred to as "carboxylic acid compound" as appropriate). The carboxylic acid compound has at least one carboxy group in one molecule, and more preferably has two or more carboxy groups in one molecule.

[0127] The carboxylic acid compound having one carboxy group preferably has, in addition to the carboxy group, another metal-adsorbing group or a functional group that has a weaker metal-coordinating ability than the carboxy group, such as an alcoholic hydroxyl group, a mercapto group, an amino group, or a carbonyl group. Specific examples include glycolic acid, thioglycolic acid, lactic acid, β-hydroxypropionic acid, gluconic acid, pyruvic acid, acetoacetic acid, salicylic acid, 5-sulfosalicylic acid, β-alanine, phenylalanine, and N-ethylglycine.

[0128] Specific examples of carboxylic acid compounds having two carboxy groups include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, maleic acid, phthalic acid, 3-sulfophthalic acid, 4-sulfophthalic acid, 2-sulfoterephthalic acid, 3-hydroxyphthalic acid, 4-hydroxyphthalic acid, tartaric acid, malic acid, dipicolinic acid, and citric acid.

[0129] Among these, preferred are compounds having two or more carboxy groups and one sulfo group on an aromatic ring, such as 3-sulfophthalic acid, 4-sulfophthalic acid, and 2-sulfoterephthalic acid; compounds having a hydroxyl group, a carboxy group, and a sulfo group on an aromatic ring, such as 5-sulfosalicylic acid; 4-hydroxyphthalic acid, oxalic acid, tartaric acid, malic acid, and dipicolinic acid; and more preferred are sulfophthalic acids, such as 3-sulfophthalic acid and 4-sulfophthalic acid; 5-sulfosalicylic acid; and 4-hydroxyphthalic acid.

[0130] In addition, the following low molecular weight organic compounds having three or more carboxy groups and no other functional groups containing atoms other than carbon and hydrogen atoms are also preferred as the carboxylic acid compound.

[0131] Specific examples of these include propane-1,2,3-tricarboxylic acid, butane-1,2,3-tricarboxylic acid, butane-1,2,4-tricarboxylic acid, butane-1,2,3,4-tetracarboxylic acid, 2-carboxymethylpropane-1,3-dicarboxylic acid, pentane-1,2,3-tricarboxylic acid, pentane-1,2,4-tricarboxylic acid, pentane-1,2,5-tricarboxylic acid, pentane-1,3,4-tricarboxylic acid, pentane-2,3,4-tricarboxylic acid, pentane-1,2,3,4-tetra ... Examples of suitable carboxymethylbutane-1,2,3,5-tetracarboxylic acid, 2-carboxymethylbutane-1,3-dicarboxylic acid, 2-carboxymethylbutane-1,4-dicarboxylic acid, 3-carboxymethylbutane-1,2-dicarboxylic acid, 3-carboxymethylbutane-1,2,4-tricarboxylic acid, 2,2-dicarboxymethylpropane-1,3-dicarboxylic acid, 1,2,3,4-cyclopentanetetracarboxylic acid, hemimellitic acid, trimellitic acid, pyromellitic acid, and naphthalene-1,4,5,8-tetracarboxylic acid.

[0132] Among these, alkyl groups having 5 or less carbon atoms substituted with 3 or more carboxy groups are preferred, and propane-1,2,3-tricarboxylic acid is more preferred.

[0133] In addition, compounds having three or more carboxy groups, such as 2-phosphonobutane-1,2,3-tricarboxylic acid, and having other functional groups containing heteroatoms are also preferred.

[0134] The chelating agent is preferably a compound represented by the following general formula (K1) or (K2).

[0135] [ka]

[0136] In general formula (K1), R K1 and R K2 each independently represents a single bond or an alkylene group. R K3 represents a divalent organic group. X1 represents a CH group or a nitrogen atom. Y K1 and Y K2 each independently represents a metal-adsorbing group. A1 represents a hydrogen atom or a hydrophilic group.

[0137] In general formula (K2), R K4 , R K5 , R K6 and R K7 each independently represents a single bond or an alkylene group. R K8 represents a trivalent organic group. X2 and X3 each represent a CH group or a nitrogen atom. Y K3 , Y K4 , Y K5 and Y K6 each independently represents a metal-adsorbing group. A2 represents a hydrogen atom or a hydrophilic group.

[0138] General formula (K1) will be described below. R K1 and R K2 each independently represents a single bond or an alkylene group. R K1 and R K2 The alkylene group preferably has 1 to 6 carbon atoms, and more preferably has 1 to 3 carbon atoms, for example. R K1 and R K2 The alkylene group may be linear or branched, and is preferably linear. R K1 and R K2 Specifically, the alkylene group is more preferably a methylene group.

[0139] R K3 represents a divalent organic group. The organic group refers to a group having at least one carbon atom. R K3 Examples of the divalent organic group include an alkylene group and an arylene group. R K3 The alkylene group may be linear or branched, and is preferably linear. R K3 The alkylene group and arylene group preferably have 1 to 10 carbon atoms, more preferably have 1 to 8 carbon atoms, and further preferably have 1 to 6 carbon atoms. R K3 The divalent organic group is preferably a methylene group, an ethylene group, or a phenyl group.

[0140] X1 represents a CH group or a nitrogen atom, and is preferably a nitrogen atom.

[0141] Y K1 and Y K2 each independently represents a metal-adsorbing group. The metal-adsorbing group is preferably an acid group or a cationic group. Specific examples thereof include the same as those of the acid group or cationic group described above for the metal-adsorbing group of the carboxylic acid compound. The cationic group may be a counter ion.

[0142] A1 represents a hydrogen atom or a hydrophilic group. Examples of the hydrophilic group of A1 include a hydroxyl group, a carboxy group, a carboxylate group, a hydroxyethyl group, a polyoxyethyl group, a hydroxypropyl group, a polyoxypropyl group, an amino group, an aminoethyl group, an aminopropyl group, an ammonium group, an amido group, a carboxymethyl group, a sulfo group, and a phosphate group. The hydrophilic group of A1 is preferably a hydroxyl group.

[0143] General formula (K2) will be described below. R K4 , R K5 , R K6 and R K7 each independently represents a single bond or an alkylene group. R K4 , R K5 , R K6 and R K7 The alkylene group is R in the general formula (K1). K1 and R K2 Synonymous with R. K4 , R K5 , R K6 and R K7 A preferred embodiment of the present invention is R K1 and R K2 This is the same as the preferred embodiment of

[0144] R K8 represents a trivalent organic group. The organic group refers to a group having at least one carbon atom. R K8 The trivalent organic group preferably has 1 to 10 carbon atoms, more preferably 1 to 8 carbon atoms, and even more preferably 1 to 6 carbon atoms. The trivalent organic group may have a substituent, the substituents may be bonded to each other to form a cyclic structure, and may have a heteroatom in the organic chain. The cyclic structure formed by bonding the substituents to each other is preferably a cycloalkyl group. The heteroatom that may be present in the main chain of the organic group is preferably an oxygen atom or a nitrogen atom.

[0145] X2 and X3 each represent a CH group or a nitrogen atom. X2 is preferably a nitrogen atom. X3 is preferably a nitrogen atom. Y K3 , Y K4 , Y K5 and Y K6 each independently represents a metal-adsorbing group. Y K3 , Y K4 , Y K5 and Y K6 The metal-adsorbing group is represented by Y in the general formula (K1). K1 and Y K2 It is synonymous with the metal adsorptive group Y. K3 , Y K4 , Y K5 and Y K6 A preferred embodiment of the metal adsorbing group is Y in the general formula (K1). K1 and Y K2 This is the same as the preferred embodiment of the metal adsorptive group of the above.

[0146] A2 represents a hydrogen atom or a hydrophilic group. The hydrophilic group of A2 has the same meaning as that of A1 in the general formula (K1). A preferred embodiment of A2 is the same as that of A1 in the general formula (K1). Specific examples of the chelating agent represented by formula (K1) and the chelating agent represented by formula (K2) are shown below.

[0147] [ka]

[0148] When the processing solution for semiconductor production of the present invention is used as a developer, the chelating agent is preferably a chelating agent for divalent metals.

[0149] Chelating agents for divalent metals include, for example, polyphosphates such as Na2P2O7, Na5P3O3, Na3P3O9, Na2O4P(NaO3P)PO3Na2, and Calgon (sodium polymetaphosphate); for example, ethylenediaminetetraacetic acid, its potassium salt, its sodium salt, and its amine salt; diethylenetriaminepentaacetic acid, its potassium salt, and its sodium salt; triethylenetetraminehexaacetic acid, its potassium salt, and its sodium salt; hydroxyethylethylenediaminetriacetic acid, its potassium salt, and its sodium salt; nitrilotriacetic acid, its potassium salt, and its sodium salt; 1,2-diaminocyclohexanetetraacetic acid, its potassium salt, and its sodium salt; Examples of the aminopolycarboxylic acids include potassium salts and sodium salts thereof; 1,3-diamino-2-propanol tetraacetic acid, its potassium salt and its sodium salt, and the like; as well as organic phosphonic acids include 2-phosphonobutanetricarboxylic acid-1,2,4, its potassium salt and its sodium salt; 2-phosphonobutanonetricarboxylic acid-2,3,4, its potassium salt and its sodium salt; 1-phosphonoethanetricarboxylic acid-1,2,2, its potassium salt and its sodium salt; 1-hydroxyethane-1,1-diphosphonic acid, its potassium salt and its sodium salt; and aminotri(methylenephosphonic acid), its potassium salt and its sodium salt, and the like.

[0150] Among these, ethylenediaminetetraacetic acid, its potassium salt, its sodium salt, and its amine salt; ethylenediaminetetra(methylenephosphonic acid), its ammonium salt, and its potassium salt; and hexamethylenediaminetetra(methylenephosphonic acid), its ammonium salt, and its potassium salt are preferred.

[0151] In general, when the chemical solution is used as a developer, the optimum amount of the chelating agent for such a divalent metal is preferably 0.01 to 5 mass %, more preferably 0.01 to 0.5 mass %, based on the total mass of the chemical solution.

[0152] <Organic solvent-based> The organic solvent-based chemical solution contains an organic solvent. The content of the organic solvent in the chemical solution is not particularly limited as long as it exceeds 50% by mass relative to the total mass of the chemical solution, but is generally preferably 97.0 to 99.999% by mass, more preferably 99.9 to 99.9% by mass, relative to the total mass of the chemical solution. The organic solvent may be used alone or in combination of two or more kinds. When two or more kinds of organic solvents are used in combination, it is preferable that the total content is within the above range. In this specification, the organic solvent refers to a liquid organic compound contained in an amount exceeding 10,000 ppm by mass per component relative to the total mass of the chemical solution. In other words, in this specification, a liquid organic compound contained in an amount exceeding 10,000 ppm by mass relative to the total mass of the chemical solution corresponds to an organic solvent. In this specification, the term "liquid" refers to a state in which the substance is liquid at 25° C. and atmospheric pressure.

[0153] (Organic solvent) The type of organic solvent is not particularly limited, and known organic solvents can be used. Examples of the organic solvent include alkylene glycol monoalkyl ether carboxylate, alkylene glycol monoalkyl ether, alkyl lactate, alkyl alkoxypropionate, cyclic lactone (preferably having 4 to 10 carbon atoms), monoketone compound which may have a ring (preferably having 4 to 10 carbon atoms), alkylene carbonate, alkyl alkoxyacetate, and alkyl pyruvate. In addition, as the organic solvent, for example, those described in JP-A-2016-57614, JP-A-2014-219664, JP-A-2016-138219, and JP-A-2015-135379 may be used.

[0154] Among these, the organic solvent is preferably at least one selected from the group consisting of propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monomethyl ether acetate, ethyl lactate, methyl methoxypropionate, cyclopentanone, cyclohexanone, γ-butyrolactone, diisoamyl ether, butyl acetate, isoamyl acetate, isopropanol, 4-methyl-2-pentanol, dimethyl sulfoxide, n-methyl-2-pyrrolidone, diethylene glycol, ethylene glycol, dipropylene glycol, propylene glycol, ethylene carbonate, propylene carbonate, sulfolane, cycloheptanone, and 2-heptanone.

[0155] Examples of organic solvent-based chemicals include solvent-based developers and pre-wet liquids.

[0156] <Other ingredients> The chemical solution may contain other components in addition to those described above, such as surfactants, specific metal ions, and other impurities.

[0157] (Surfactant) The chemical solution preferably contains a surfactant. The content of the surfactant in the chemical solution is not particularly limited, but in general, the content is preferably 0.0001 to 2.0 mass %, more preferably 0.0005 to 1.0 mass %, based on the total mass of the surfactant. The surfactant may be used alone or in combination of two or more. When two or more surfactants are used in combination, the total content is preferably within the above range.

[0158] The surfactant contained in the chemical solution is not particularly limited, and a known surfactant can be used. As the surfactant, a fluorine-based surfactant and / or a silicon-based surfactant may be used, or other surfactants may be used. As the other surfactant, an anionic surfactant, a nonionic surfactant, or a cationic surfactant, which does not contain either fluorine or silicon, as described below, may be used as appropriate. Examples of the fluorosurfactant and / or silicone surfactant include the surfactants described in paragraph 0276 of US Patent Application Publication No. 2008 / 0248425. As surfactants other than fluorine-based surfactants and silicon-based surfactants, for example, surfactants described in U.S. Patent Application Publication No. 2008 / 0248425, paragraph 0280 can be used. In addition, surfactants described in JP-A-2010-256842, paragraphs 0313 to 0316 can also be used. The surfactant may be used alone or in combination of two or more. When two or more surfactants are used in combination, the total content is preferably within the above range.

[0159] When the composition of the present invention contains a surfactant, the amount of the surfactant used is preferably from 0.0001 to 2 mass %, more preferably from 0.0005 to 1 mass %, based on the total solid content of the composition.

[0160] As surfactants other than those mentioned above, anionic surfactants, nonionic surfactants, and cationic surfactants can also be used. Examples of the anionic surfactant include alkyl sulfate, alkyl sulfonic acid, alkyl benzene sulfonic acid, alkyl naphthalene sulfonic acid, alkyl diphenyl ether sulfonic acid, polyoxyethylene alkyl ether carboxylic acid, polyoxyethylene alkyl ether acetic acid, polyoxyethylene alkyl ether propionic acid, polyoxyethylene alkyl ether sulfuric acid, polyoxyethylene aryl ether acetic acid, polyoxyethylene aryl ether propionic acid, polyoxyethylene aryl ether sulfuric acid, and salts thereof. Among these, alkyl sulfate ester, polyoxyethylene aryl ether sulfate, or polyoxyethylene alkyl ether sulfate is preferred, and polyoxyethylene aryl ether sulfate is more preferred.

[0161] Examples of nonionic surfactants include polyalkylene oxide alkyl phenyl ether surfactants, polyalkylene oxide alkyl ether surfactants, block polymer surfactants consisting of polyethylene oxide and polypropylene oxide, polyoxyalkylene distyrene-type phenyl ether surfactants, polyalkylene tribenzyl phenyl ether surfactants, and acetylene polyalkylene oxide surfactants.

[0162] The nonionic surfactant is preferably a compound represented by the following general formula (A1).

[0163] [ka]

[0164] In general formula (A1), R a1 , R a2 , R a3 and R a4 each independently represents an alkyl group. L a1 and L a2 each independently represents a single bond or a divalent linking group.

[0165] General formula (A1) will be described below. R a1 , R a2 , R a3 and R a4 each independently represents an alkyl group. R a1 , R a2 , R a3 and R a4 The alkyl group may be linear or branched, and may have a substituent. R a1 , R a2 , R a3 and R a4 The alkyl group preferably has a carbon number of 1 to 5. Examples of the alkyl group having a carbon number of 1 to 5 include a methyl group, an ethyl group, an isopropyl group, and a butyl group.

[0166] L a1 and L a2 each independently represents a single bond or a divalent organic group. L a1 and L a2 The divalent linking group is an alkylene group, -OR a5 R - groups and combinations thereof are preferred. a5 represents an alkylene group.

[0167] Examples of nonionic surfactants include 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 3,6-dimethyl-4-octyne-3,6-diol, and 3,5-dimethyl-1-hexyne-3-ol.

[0168] Examples of the compound represented by general formula (A2) include compounds represented by the following general formula (A2).

[0169] [ka]

[0170] In general formula (A2), R a1 , R a2 , R a3 and R a4 each independently represents an alkyl group. m and n each independently represent a positive number of 0.5 to 80, and satisfy m+n≧1.

[0171] General formula (A2) will be described below. R a1 , R a2 , R a3 and R a4 each independently represents an alkyl group. R a1 , R a2 , R a3 and R a4 The alkyl group represented by R a1 , R a2 , R a3 and R a4 The alkyl groups are the same as those in the above.

[0172] m and n represent the number of moles of ethylene oxide added, each independently represents a positive number of 0.5 to 80, and satisfies m+n≧1. Any value can be selected within the range that satisfies m+n≧1. m and n preferably satisfy 1≦m+n≦100, and more preferably satisfy 3≦m+n≦80.

[0173] Examples of the compound represented by general formula (A2) include 2,5,8,11-tetramethyl-6-dodecyne-5,8-diol, 5,8-dimethyl-6-dodecyne-5,8-diol, 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 4,7-dimethyl-5-decyne-4,7-diol, 8-hexadecyne-7,10-diol, 7-tetradecyne-6,9-diol, 2,3,6,7-tetramethyl-4-octyne-3,6-diol, 3,6-diethyl-4-octyne-3,6-diol, 3,6-dimethyl-4-octyne-3,6-diol, and 2,5-dimethyl-3-hexyne-2,5-diol.

[0174] In addition, commercially available nonionic surfactants can be used, such as SURFYNOL 82, 465, 485, DYNOL 604, 607 manufactured by Air Products & Chemicals, and Olfine STG and Olfine E1010 manufactured by Nissin Chemical Industry Co., Ltd.

[0175] The HLB (Hydrophilic-Lipophilic Balance) value of the nonionic surfactant is preferably 8 or more, more preferably 10 or more. The HLB value of the nonionic surfactant is preferably 16 or less, more preferably 14 or less. Here, the HLB value is defined as a value calculated by the Griffin formula (20Mw / M; Mw=molecular weight of the hydrophilic portion, M=molecular weight of the nonionic surfactant), and in some cases, a catalog value or a value calculated by another method may be used.

[0176] Two or more kinds of nonionic surfactants may be used in combination. Of the two or more kinds of nonionic surfactants, at least two of the nonionic surfactants are preferably compounds represented by general formula (A1).

[0177] The two or more nonionic surfactants preferably include at least one nonionic surfactant having an HLB value of 12 or more and at least one nonionic surfactant having an HLB value of 10 or less. With the above combination, a pattern with excellent rectangularity can be obtained when the chemical solution is used as a developer.

[0178] The total mass of the nonionic surfactants having an HLB of 12 or more is preferably 0.5 to 4, more preferably 0.7 to 3.5, and even more preferably 1.0 to 3.0, relative to the total mass of the nonionic surfactants having an HLB of 10 or less. The present inventors have found that by having the total mass of the nonionic surfactants having an HLB of 12 or more greater than the total mass of the nonionic surfactants having an HLB of 10 or less, a pattern with excellent rectangularity can be obtained when the chemical solution is used as a developer.

[0179] Examples of cationic surfactants include quaternary ammonium salt surfactants and alkylpyridinium surfactants.

[0180] Examples of the quaternary ammonium salt surfactant include tetramethylammonium chloride, tetrabutylammonium chloride, dodecyldimethylbenzylammonium chloride, alkyltrimethylammonium chloride, octyltrimethylammonium chloride, decyltrimethylammonium chloride, dodecyltrimethylammonium chloride, tetradecyltrimethylammonium chloride, cetyltrimethylammonium chloride, and stearyltrimethylammonium chloride. The quaternary ammonium salt surfactant is not particularly limited, but dodecyldimethylbenzylammonium chloride is preferred.

[0181] Examples of alkylpyridinium surfactants include butylpyridinium chloride, dodecylpyridinium chloride, cetylpyridinium chloride, etc. Although the alkylpyridinium surfactant is not particularly limited, butylpyridinium chloride is preferred.

[0182] Cationic surfactants can be obtained, for example, by first acylating triethanolamine, methyldiethanolamine, 3-(N,N-dimethylamino)-1,2-propylene glycol, or the like with a long-chain fatty acid or fatty acid methyl group to synthesize an intermediate alkanolamine ester, which is then converted to a cationic compound using a quaternizing agent such as methyl chloride, dimethyl sulfate, or diethyl sulfate.

[0183] [Physical properties of chemical solutions] <Condition 1> It is preferable that the liquid medicine contained in the liquid medicine container satisfies the following condition 1 in terms of making it easier to maintain its performance for a long period of time. Condition 1: A chemical solution is applied to a substrate, and the change in density of particles with a particle size of 19 nm or less on the substrate before and after application of the chemical solution is measured using a particle inspection device. The change is 0.3 particles / cm 2 The following is the result. Furthermore, the performance of the chemical solution is more likely to be maintained over a long period of time if the change in particle density is less than 0.2 particles / cm 2 More preferably, it is 0.1 particles / cm or less. 2 It is even more preferable that:

[0184] A method for checking whether the chemical solution taken out of the container satisfies condition 1 will be described. First, the chemical solution is applied onto a substrate. The substrate to be used is not particularly limited, but a silicon wafer is preferable because it allows for easier measurement of changes in particle density. Rotational coating is preferable as a coating method.

[0185] Next, the change in particle density on the substrate before and after application was measured, and the change was 0.3 particles / cm 2 Verify that the following is true: The change in particle density on the substrate before and after application of the chemical liquid can be calculated by measuring the particle density on the substrate before application of the chemical liquid and the particle density on the substrate after application of the cleaning liquid, and calculating the difference between them. In this case, the particle density on the substrate before and after application can be measured using a particle inspection device, for example, SP-5 manufactured by KLA-Tencor.

[0186] <Condition 2> It is preferable that the liquid medicine contained in the liquid medicine container satisfies the following condition 2 in terms of making it easier to maintain its performance for a long period of time. Condition 2: The chemical solution contains water, the water content in the chemical solution is 50 mass% or less, and the amount of particulate matter having a particle diameter of 30 nm or less in the chemical solution, as measured by a single particle inductively coupled plasma mass spectrometer (SP-ICP-MS), is 1.0 mass ppb or less (preferably 0.5 mass ppb or less, and more preferably 0.2 mass ppb or less) relative to the total mass of the chemical solution.

[0187] Here, the device used in SP-ICP-MS is the same as that used in normal ICP-MS (inductively coupled plasma mass spectrometry) (hereinafter, also simply referred to as "ICP-MS"), and only the data analysis is different. Data analysis as SPICP-MS can be performed by commercially available software. In ICP-MS, the amount of a target component is measured regardless of the form it is in. Therefore, the target component is quantified as the total mass of the particulate matter and ions.

[0188] On the other hand, in SP-ICP-MS, the particulate content of the components to be measured is measured individually.

[0189] For example, an apparatus for the SP-ICP-MS method may be Agilent 8800 triple quadrupole ICP-MS (inductively coupled plasma mass spectrometry, for semiconductor analysis, option #200) manufactured by Agilent Technologies, Inc., and may be used for measurement according to the method described in the Examples. In addition to the above, PerkinElmer's NexION350S and Agilent Technologies' Agilent 8900 may also be used.

[0190] <Metal component amount> The amount of metal components in the chemical solution is not particularly limited, but is preferably 1 ppb by mass or less. The metal components include metal ions and metal particles.

[0191] <Content of compounds with boiling points of 300°C or higher> The content of the compound having a boiling point of 300° C. or higher in the chemical solution is not particularly limited, but is preferably 1 ppm by mass or less. Examples of the compound having a boiling point of 300° C. or higher include organic compounds selected from the group consisting of an ester structure, a sulfonamide structure, an amide structure, a urethane structure, a urea structure, and a carbonate structure.

[0192] <Specific metal ions> When the chemical solution contains ions of one specific metal, the content of the one specific metal ion is preferably 1000 mass ppt or less, more preferably 500 mass ppt or less, and even more preferably 100 mass ppt or less. There is no particular lower limit, but in relation to the lower limit of quantification, it is generally preferably 0.01 mass ppt or more. Furthermore, by concentrating the chemical solution before measurement during evaluation, the content can be measured with higher accuracy. When the chemical solution contains ions of two or more specific metals, it is preferable that the arithmetic mean of the contents of the ions of the two or more specific metals falls within the above range.

[0193] <Counted entity> The number of counted particles having a size of 30 nm or more, as counted by a light scattering type liquid particle counter, per 1 ml of the drug solution is preferably 100 or less, more preferably 70 or less, and even more preferably 30 or less. The lower limit is not particularly limited, but from the viewpoint of the lower limit of quantification, generally, 0.1 or more is preferable.

[0194] <Other impurities (inorganic salts)> When the chemical solution contains an anionic surfactant or a cationic surfactant, the chemical solution may contain inorganic salts as impurities, such as sulfates, nitrates, acetates, and phosphates.

[0195] The content of the inorganic salt in the chemical solution is preferably 1.0 ppq to 1000 ppt by mass, more preferably 5.0 ppq to 500 ppt by mass, further preferably 10 ppq to 500 ppt by mass, and particularly preferably 100 ppq to 100 ppt by mass, relative to the total mass of the chemical solution. The inorganic salt reacts with the metal atoms in the chemical solution to precipitate the metal salt, which causes defects. Therefore, the content of the inorganic salt in the chemical solution is preferably within the above range.

[0196] <Other impurities (peroxides)> When the chemical solution contains a nonionic surfactant, the chemical solution may contain peroxides as impurities. Examples of peroxides include calcium peroxide, magnesium peroxide, potassium peroxide, and sodium peroxide.

[0197] The content of the peroxide in the chemical solution is preferably 1.0 mass ppq to 1000 mass ppt, more preferably 5.0 mass ppq to 500 mass ppt, further preferably 10 mass ppq to 500 mass ppt, and particularly preferably 100 mass ppq to 100 mass ppt, based on the total mass of the chemical solution. Peroxides cause deterioration of the electrical properties of electronic devices and cause pattern defects. Therefore, the content of the peroxide in the chemical solution is preferably within the above range.

[0198] <Other impurities (ester compounds)> When the chemical solution contains a nonionic surfactant, the chemical solution may contain an ester compound as an impurity. Examples of the ester compound include methyl stearate, octyl stearate, butyl oleate, oleyl laurate, stearyl palmitate, stearyl behenate, myristyl myristate, hexyl acrylate, octyl methacrylate, vinyl caproate, and oleyl acetate.

[0199] The content of the ester compound in the chemical solution is preferably 1.0 mass ppq to 1000 mass ppt, more preferably 5.0 mass ppq to 500 mass ppt, further preferably 10 mass ppq to 500 mass ppt, and particularly preferably 100 mass ppq to 100 mass ppt, relative to the chemical solution. The ester compound is adsorbed to metal atoms and aggregates. The aggregated ester compound is adsorbed on the substrate and remains there. This causes defects. Therefore, the content of the ester compound is preferably within the above range relative to the chemical solution.

[0200] <Other impurities (amine compounds)> When the chemical solution contains a nonionic surfactant, the chemical solution may contain an amine compound as an impurity. Examples of the amine compound include monomethylamine, dimethylamine, trimethylamine, monoethylamine, diethylamine, and triethylamine.

[0201] The content of the amine compound in the chemical solution is preferably 1.0 mass ppq to 1000 mass ppt, more preferably 5.0 mass ppq to 500 mass ppt, further preferably 10 mass ppq to 500 mass ppt, and particularly preferably 100 mass ppq to 100 mass ppt, based on the total mass of the chemical solution. The amine compound is adsorbed to metal atoms and aggregates. The aggregated amine compound is adsorbed on the substrate and remains there, causing defects. Therefore, the content of the inorganic salt is preferably within the above range based on the chemical solution.

[0202] <Other impurities (chelate complexes)> When the chemical solution contains a chelating agent, the chemical solution may contain a chelate complex as an impurity. The chelate complex is formed by combining not all of the chelating agent but a part of the chelating agent with a metal atom such as a specific metal ion contained in the chemical solution. Examples of the chelate complex include monocalcium ethylenediaminetetraacetate and copper(II) ethylenediaminetetraacetate.

[0203] The content of the chelate complex in the chemical solution is preferably 1.0 mass ppq to 1000 mass ppt, more preferably 5.0 mass ppq to 500 mass ppt, even more preferably 10 mass ppq to 500 mass ppt, and even more preferably 100 mass ppq to 100 mass ppt, based on the total mass of the chemical solution. The chelate complex adheres to and accumulates on the wafer. This increases the load caused by development and cleaning such as rinsing. Furthermore, the chelate complex that cannot be removed by development and cleaning such as rinsing becomes a defect. Therefore, the content of the chelate complex is preferably within the above range based on the chemical solution. EXAMPLES

[0204] The present invention will be described in more detail below based on examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the following examples.

[0205] [Preparation of container] <Container Manufacturing Example 1: Examples 3 to 9, 11 to 12, Comparative Examples 1 and 2> A commercially available polyethylene canister (manufactured by Aicello, described as "commercial PE canister" in Table 1) was prepared as a substrate. It was confirmed that this polyethylene canister contained a specific metal. Next, this substrate was washed in sequence by the methods described in Table 1 to obtain a container. The washing order was as described in Table 1 as (1) to (11), and all washing processes were performed in a class 100 clean room environment. Table 1 describes the type of washing solution used, the washing method, the washing temperature, and the washing time. In Comparative Example 1, a commercially available polyethylene canister was used without washing. In Table 1, the cleaning with ultrapure water in Example 2 (1) is described as "room temperature, 5 minutes, running water", which indicates that the cleaning temperature is "room temperature", the cleaning time is "5 minutes", and the cleaning method is "running water". Also, the cleaning with ultrapure water in Example 4 (1) is described as "ultrasonic, 90°C / 1h", which indicates that the cleaning method is "ultrasonic", the cleaning temperature is "90°C", and the cleaning time is "1h (i.e., 1 hour)". In Comparative Example 2 (1), tap water filtered through a simple filter with a pore size of 1 μm was used instead of cleaning with ultrapure water. As for (2) washing with acid, for example, "hydrochloric acid (1N, 40°C / 1h)" in Example 4 means washing was performed with 1N hydrochloric acid at 40°C for 1 hour. Meanwhile, "hydrochloric acid (1N, 80°C / 12h) this treatment was performed three cycles" in Example 12 means washing was performed with 1N hydrochloric acid at 60°C for 12 hours three cycles. Regarding (3) cleaning with ultrapure water, for example, in Example 4, “ultrasonic, 90°C / 1 h” indicates that the cleaning temperature was “90°C” and ultrasonic treatment was performed for “1 h.” Regarding (4) cleaning with acid, for example, “dilute hydrofluoric acid (0.8% by mass, 40°C / 1 h)” in Example 5 indicates that 0.8% by mass dilute hydrofluoric acid was used, the cleaning temperature was “40°C”, and the cleaning time was “1 h”. Regarding washing with a base in (6), for example, "Ammonium sulfate (1.0 mass %, 60°C / 1 h)" in Example 4 indicates that a 1.0 mass % aqueous ammonium sulfate solution was used, the washing temperature was "60°C," and the washing time was "1 h." In addition, with regard to cleaning with the mixture (8), for example, "Mixture B: TMAH (0.5%) / EDTA (0.3%) / ethylenediamine (0.1%) / diethylenetriamine (0.1%) / ethyleneglycolbutylether (10%)-containing water (ultrasonic, 120°C / 1 h)" in Example 5 indicates that mixture B was used, the cleaning temperature was "120°C," and the cleaning time was "1 h." Regarding the cleaning with an organic solvent in (10), "IPA (room temperature, 5 minutes, flushing)" indicates that IPA (isopropanol) was used, the cleaning temperature was "room temperature", the cleaning time was "5 minutes", and the cleaning method was "flushing". In addition, "IPA (ultrasonic, 40°C / 1h)" in Example 11 indicates that IPA was used, the cleaning temperature was "40°C", and ultrasonic treatment was performed for "1 hour". In addition, "PGMEA / PGME / butyl acetate (ultrasonic, 40°C / 1h)" in Example 12 indicates that PGMEA (30%) / PGME (40%) / butyl acetate (30%) was used, the cleaning temperature was "40°C", and ultrasonic treatment was performed for "1 hour". In addition, in the case of (11) ultrapure water cleaning, "ultrasonic, heat (90°C / 1h)" indicates a cleaning method in which ultrasonic treatment is carried out for 1 hour in an ultrasonic treatment tank heated to 90°C. In the table, "-" indicates that the cleaning solution was not used. In the table, "RCA" and "RCB" should be read as RCAs and RCBs for Examples 1, 2, and 10.

[0206] <Container Manufacturing Example 2: Example 1> A container was obtained by forming a coating layer 1 on a polyethylene substrate, the coating layer 1 being made of a coating layer-forming composition 1 prepared by the following procedure, by injection blow molding on the liquid-contacting portion of the substrate. The thickness of the coating layer 1 was 250 μm. In Table 1, (coating layer 1 / PE) in the "substrate" column indicates that the container has coating layer 1 on PE, which is the substrate.

[0207] (Preparation of coating layer forming composition 1) First, HDPE was synthesized by the following method: First, HDPE was synthesized in a tubular polymerization reactor using a Ti / Mg catalyst and triethylaluminum as a co-catalyst in hexane at a temperature of 80°C under a pressure of 260 MPa for a residence time of 2 hours. Next, the synthesized HDPE was further dissolved in decahydroxynaphthalene at a temperature of 90°C, and then subjected to a liquid separation and purification process using 0.1N HCl water at 90°C. Then, a liquid separation and purification process was performed using pure water, and the mixture was further precipitated using high-purity cyclohexanone to obtain a coating layer forming composition 1.

[0208] <Container Manufacturing Example 3: Example 2> The container obtained in the same manner as in Example 1 was further washed under the conditions shown in Table 1. The thickness of the coating layer 1 was 250 μm.

[0209] <Container Manufacturing Example 4: Example 10> Using polyethylene as a base material, a coating layer was formed on the portion of the base material that was to come into contact with liquid by the following procedure. The coating layer 2 made of the coating layer forming composition 2 was disposed by injection blow molding so that the obtained coating layer forming composition 2 was the liquid contacting part, to obtain a container. The coating layer 2 had a thickness of 250 μm. In Table 1, (coating layer 2 / PE) in the column "base" indicates that the container has coating layer 2 on PE, which is the base material.

[0210] (Preparation of coating layer forming composition 2) First, HDPE was synthesized by the following method: HDPE was synthesized in a tubular polymerization reactor using a Ti / Mg catalyst and triethylaluminum as a co-catalyst in hexane at a temperature of 80°C under a pressure of 260 MPa for a residence time of 2 hours. Next, the synthesized HDPE was further dissolved in decahydroxynaphthalene at a temperature of 90°C, and then subjected to a liquid separation and purification treatment using distilled water at 90°C, and then subjected to a liquid separation and purification treatment using pure water to obtain a coating layer forming composition 2.

[0211] [Preparation of cleaning solution] The cleaning solutions used in each step were prepared by the following methods, and then all were filtered using a filter having a nylon filter material (pore size 20 nm, hydrophilized, manufactured by Pall).

[0212] (1) Ultrapure water: Using an ultrapure water generator (manufactured by Kurita Water Industries, Ltd.), ultrapure water with a total atomic content of 100 mass ppt or less was obtained and used as a cleaning solution. This was also used for preparing the following cleaning solutions. (2) Hydrochloric acid: A hydrogen chloride aqueous solution (TAMAPURE-AA-10 grade) manufactured by Tama Chemical Industry Co., Ltd. was used and mixed with the above ultrapure water to prepare 1N hydrochloric acid. (3) Dilute hydrofluoric acid: A 0.8 wt. % HF aqueous solution was prepared by mixing a dilute hydrofluoric acid aqueous solution (TAMAPURE-AA-10 grade) manufactured by Tama Chemical Industries Co., Ltd. with the ultrapure water described above. (4) Ammonium sulfate: manufactured by Tama Chemical Industry Co., Ltd. A 1% aqueous solution of ammonium sulfate was prepared from sulfuric acid (TAMAPURE-AA100 grade), aqueous ammonia (TAMAPURE-AA-100 grade), and the above ultrapure water. (5) IPA (isopropyl alcohol): IPA manufactured by Fujifilm Ultra Pure Co., Ltd. was used. (6) Mixture A: Using the same ammonia water as in (4) above and a 40% aqueous solution of 20% ammonium EDTA (manufactured by Toyama Pharmaceutical Co., Ltd.), an aqueous solution containing 20% ​​aqueous ammonia (5.0%), EDTA (0.3%), ethylenediamine (0.1%), diethylenetriamine (0.1%), and ethylene glycol butyl ether (10%) was prepared. EDTA is an abbreviation for ethylenediaminetetraacetic acid. Ethylene glycol butyl ether (manufactured by KH Neochem Co., Ltd.), ethylenediamine (manufactured by Hayashi Pure Chemical Industries, Ltd.), and diethylenetriamine (manufactured by Hayashi Pure Chemical Industries, Ltd.) were also used. (7) Mixture B: Using the same TMAH as in (2) above and a 40% aqueous solution of diammonium EDTA (manufactured by Toyama Pharmaceutical Co., Ltd.), an aqueous solution containing TMAH (0.5%), EDTA (0.3%), ethylenediamine (0.1%), diethylenetriamine (0.1%) and ethylene glycol butyl ether (10%) was prepared. Ethylene glycol butyl ether (manufactured by KH Neochem Co., Ltd.), ethylenediamine (manufactured by Hayashi Pure Chemical Industries, Ltd.), and diethylenetriamine (manufactured by Hayashi Pure Chemical Industries, Ltd.) were also used. (13) Butyl acetate (50%) / PGMEA (50%): FN-DP001 manufactured by Fujifilm Electronic Materials Taiwan Co., Ltd. was used as butyl acetate, and PGMEA (manufactured by KH Neochem Co., Ltd.) was used to prepare a mixed solution consisting of butyl acetate (50%) / PGMEA (50%).

[0213] It was confirmed that the metal ion content in each cleaning solution was 100 ppt by mass or less, the organic impurity content was 100 ppm by mass or less, and the number of counted particles having a size of 30 nm or more, as counted by a light scattering type liquid-borne particle counter, was 50 or less per ml of cleaning solution.

[0214] In addition, the average content of specific metal ions contained in each cleaning solution after cleaning was within the range of 0.01 ppt by mass to 1.0 ppm by mass, and the content of organic impurities was within the range of 1.0 ppt by mass to 500 ppm by mass.

[0215] [Preparation of drug solution] The chemical solutions used in the evaluation were each prepared by the following method, and then all were filtered using a filter having a nylon filter material (pore size 20 nm, hydrophilized, manufactured by Pall). (8) TMAH developer: A 2.38% by mass aqueous solution was prepared using TMAH (manufactured by Tama Chemicals) and ultrapure water (TMAH is an abbreviation for tetramethylammonium hydroxide). After thoroughly stirring to confirm dissolution, the solution was filtered (the filter used was a filter made by Entegris with a UPE (ultra-high molecular weight polyethylene) filter material, pore size 20 nm) to obtain a chemical solution. (9) Resist used in evaluation: Positive resist composition A positive resist composition was prepared as described in Example 1 of JP 2010-256842 A. That is, the following resin A, acid generator, basic compound, surfactant, hydrophobic resin, and solvent were mixed and stirred for 12 hours, and then filtered through a 3 nm UPE filter (capsule filter manufactured by Entegris, UPE is an abbreviation for ultra-high molecular weight polyethylene).

[0216] ·Resin A: (87.01 parts by mass) Polymer with composition ratio 40 / 10 / 50, Mw 8200, and dispersity 1.53 [ka]

[0217] Acid generator: (10.9 parts by mass) (b36) [ka]

[0218] Basic compound: (0.71 parts by mass) (N-1) 2,6-diisopropylaniline Surfactant: (0.50 parts by weight) PF6320

[0219] Hydrophobic resin: (0.879 parts by weight) [ka] Hydrophobic resin: composition ratio = 40 / 56 / 2 / 2 (from left)

[0220] Solvent: propylene glycol monomethyl ether acetate (1540 parts by mass), propylene glycol monomethyl ether (360 parts by mass)

[0221] (10) Ultra-high purity buffered hydrofluoric acid: BHL manufactured by Stella Chemifa Corporation was used. (11) Clean 100 (Wako Pure Chemical Industries, Ltd.) Post-CMP Cleaner (12) CMP slurry: A CMP slurry was prepared using the CMP slurry described in “8071+150 ppm methanol” in Table 2 of paragraph 0058 of JP-A-2009-510224, except that PGMEA (manufactured by KH Neochem Co., Ltd.) was used instead of methanol.

[0222] [Measurement method 1] In this paragraph, "in liquid" means in a cleaning liquid and in a chemical liquid. In this example, the content of metal ions in the liquid was evaluated using ICP-MS (manufactured by Agilent). In this example, the number of counted objects having a size of 30 nm or more in the liquid was determined using KS-19X (manufactured by Rion). In this embodiment, the content of organic impurities in the liquid was measured by directly injecting the liquid to be measured using a gas chromatograph mass spectrometer (GC / MS). Of the detected components, the content of components with a molecular weight of 500 or less was calculated and defined as the content of organic impurities.

[0223] [Measurement method 2] In this embodiment, the measurement method for the container is as follows. (Sample Preparation) A plurality of slices were obtained by cutting out a portion of the liquid-contacting portion (inner wall) from the container prepared by the method described in Table 1 and the comparative container. From the slices, samples for evaluating the surface region and samples for evaluating the inner region were prepared by the following method.

[0224] Surface area evaluation sample The section of the liquid-contacting part of the container was cut obliquely from the surface of the liquid-contacting part in the thickness direction. At this time, the cross section (cut surface) obtained by cutting was inclined so that the cutting length for an area of ​​1 μm in the thickness direction from the surface of the liquid-contacting part was 5 mm. A region of the obtained cut surface with a cutting length of 50 μm, which corresponds to a surface region of 10 nm in the thickness direction from the surface of the liquid contact part, was used as a sample for surface region evaluation. Note that the "cut length" here means the length from the cutting start point of the cut surface in the cutting direction when the cut surface is observed from above.

[0225] -Sample for evaluating inner area The sections of the liquid-contacting parts of the containers were cut obliquely from the surface of the liquid-contacting parts in the thickness direction. The cut surface was inclined so that the cutting length was 10 mm for an area 50 μm in the thickness direction from the surface of the liquid-contacting parts. Of the obtained cut surfaces, a region with a cutting length of 4 mm, which corresponds to an inner region of 30 to 50 μm in the thickness direction from the surface of the liquid-contacting portion, was used as a sample for evaluating the inner region.

[0226] (Measurement of peak intensity due to each metal component) The cut surface of the surface region evaluation sample prepared above was used as the observation surface, and the peak intensity of secondary ions derived from each metal component was measured at 20 equally spaced points along the cutting direction. In addition, the position of each measurement point in the width of the cut surface was converted to the position in the thickness direction of the coating layer (or container) to which each measurement point corresponds. From the above, it was confirmed that each measurement result was data reflecting the metal component content in the desired surface region. Next, the peak intensities of the secondary ions originating from each metal component at the 20 measurement points were divided by the intensity of all ions detected at each measurement point to obtain the relative peak intensities of the secondary ions originating from each metal component, and the average values ​​obtained for each metal component were used as the relative peak intensities of the secondary ions originating from each metal component in the surface region. For the outermost surface, the average value of measurements taken at five non-cut locations was used as the measured value for the outermost surface.

[0227] Next, the cut surface of the inner region evaluation sample was used as the observation surface, and the peak intensity of secondary ions originating from each metal component was measured at 20 equally spaced points along the cutting direction. Next, the average value of the relative peak intensity of secondary ions originating from each metal component in the inner region was obtained using the same measurement and calculation procedures as those for the surface region. The above measurements were carried out using a time-of-flight secondary ion mass spectrometer: TOF-SIMS V manufactured by ION-TOF.

[0228] (Measurement of peaks derived from polyolefins) The cut surface of the surface region evaluation sample prepared above was used as the observation surface, and the C n H 2n - The intensity of the fragments of each component (n = 2-20) was divided by the intensity of all ions detected, and the sum of these values ​​was calculated. The measurement results for each measurement point were then averaged to obtain the relative intensity of the secondary ion peaks derived from polyolefin in the surface region. In addition, the relative peak intensities of secondary ions originating from polyolefin in the internal region were obtained in the same manner as above.

[0229] (RCA calculation) The ratio of the relative intensity of the secondary ion peak derived from each metal component to the relative intensity of the secondary ion peak derived from the polyolefin calculated above was determined. This was calculated separately for the surface region and the internal region, and designated as CA1 (corresponding to the surface region, data for each metal component) and CA2 (corresponding to the internal region, data for each metal component). Next, RCA=CA1 / CA2 was calculated. The RCA value (or RCAs) was calculated for each of the metal components Ti, Mg, Al, Cr, Hf, Zr, Fe, Sn, Ni, and Mo, and the arithmetic mean value of the RCA values ​​of the metal components was used as the RCA value of the sample. The results are shown in Table 1.

[0230] (RCB calculation) C n H 2n - the peak intensity of the fragment ion, represented by C p H 2p The peak intensity of the secondary ion represented by COO- and C q H 2q The intensity ratio of the peak intensities of the secondary ions represented by PO2- was calculated. This intensity ratio corresponds to the relative intensity of each component, and these were averaged for each component at each measurement point, and the average values ​​obtained for each component were then averaged again. This final average value corresponds to CB1 for the surface region and CB2 for the internal region. From this, the RCB value (RCB=CB1 / CB2) was calculated. The results are shown in Table 1. Here, n is an integer from 12 to 20, p is an integer from 8 to 24, and q is an integer from 8 to 24.

[0231] [Measurement method 3] The elution test was carried out by the following method. Each container of the examples and comparative examples was filled with 100 ml of pure water (corresponding to 50% by volume of the container volume). In this state, it was maintained at 40°C for one day. Thereafter, the pure water was collected, and the content of metal components contained in the pure water (indicated as "metal" in the table) was measured by the ICP-MS described above, and TOC was measured using a total carbon concentration meter (TOC-Vw manufactured by SHIMADZU).

[0232] [evaluation] [TMAH developer performance stability over time] The 2.38 mass % TMAH developer prepared in (8) above was placed in each of the containers shown in Table 1 to prepare chemical solution containers. Each of the liquid containers was stored at 45° C. for one month. After storage, the developer was taken out of the liquid container, and the lithography performance was evaluated. The lithography performance was evaluated as follows.

[0233] On a silicon wafer, an organic anti-reflective film forming composition ARC29A (manufactured by Nissan Chemical Industries, Ltd.) was applied, and baked at 205°C for 60 seconds to form an anti-reflective film with a thickness of 86 nm. Next, the above-mentioned positive resist composition was applied on the anti-reflective film, and baked at 100°C for 60 seconds to form a resist film with a thickness of 100 nm, to obtain a wafer with a resist film. Next, the wafer with the resist film was exposed using an ArF excimer laser immersion scanner (XT1700i, NA1.20, C-Quad, outer sigma 0.981, inner sigma 0.895, XY deflection) through a 6% halftone mask capable of forming a half-pitch 40 nm 1:1 line and space pattern. Ultrapure water was used as the immersion liquid. Next, the resist film after exposure was heated at 100°C for 60 seconds, developed with the above-mentioned developer for 30 seconds, rinsed with pure water, and then spin-dried to obtain a resist pattern. The line edge roughness (LWR) of the prepared resist pattern was measured at 100 positions using a critical dimension SEM (CG4500, manufactured by Hitachi High-Technologies Corporation), and the difference (variation) between the maximum and minimum LWR values ​​in the obtained data was calculated and used as an index of pattern quality. The results were evaluated according to the following criteria and are shown in Table 1 (listed in the "Lithography Performance" column).

[0234] A: The LWR variation was less than 0.3 nm. B: The LWR variation was greater than 0.3 nm and less than 0.5 nm. C: The LWR variation was greater than 0.5 nm and less than 0.8 nm. D: The LWR variation was greater than 0.8 nm and less than 1.2 nm. E: The LWR variation was greater than 1.2 nm.

[0235] <Number of objects to be counted in liquid> The developing solution was removed from the liquid container after storage, and the number of countable particles of 30 nm or more was determined using a light scattering type liquid particle counter: KS-19X manufactured by Rion Co., Ltd. The results were evaluated according to the following criteria and shown in Table 1 ("Number of countable particles in liquid" column). In this embodiment, when the countable particles in the liquid were measured, the same method as above was used. A: It was less than 30 cells / ml. B: More than 30 cells / ml and less than 70 cells / ml. C: More than 70 cells / ml and less than 100 cells / ml. D: More than 100 cells / ml but less than 200 cells / ml. E: Exceeded 200 cells / ml.

[0236] <Changes in particle density on the substrate> Using a Lithius-PRO coating coater, the developer removed from the liquid container after storage was coated onto a silicon wafer. At this time, the change in particle density on the silicon wafer before and after coating was measured using an SP5 (KLA Tencor). The number of particles with a particle diameter of 19 nm or more was counted. The results were evaluated according to the following criteria and shown in Table 1 (column "Coated Particles"). In this example, the particle density on the substrate was measured using the same method as above. A:0.06 pieces / cm 2 It was as follows. B:0.06 pieces / cm 2 Exceeds 0.1pc / cm 2 It was as follows. C:0.1 pieces / cm 2 More than 0.2 pieces / cm 2 It was as follows. D:0.2 pieces / cm 2 More than 0.3 pieces / cm 2 It was as follows. E:0.3 pieces / cm 2 It went beyond that.

[0237] <Evaluation of particulate matter in liquid> Evaluation equipment: Agilent 8900 Using the above-mentioned SP-ICP-MS, the particulate matter content of the liquid medicine taken out from the liquid medicine container after aging was evaluated. The results were evaluated according to the following criteria and are shown in the "Particulate matter evaluation" column of Table 1. A: It was less than 0.05 ppb by mass. B: More than 0.05 ppb by mass and less than 0.2 ppb by mass. C: More than 0.2 ppb by mass and 0.5 ppb by mass or less. D: More than 0.5 ppb by mass and 1.0 ppb by mass or less. E: Exceeded 1.0 ppb by mass.

[0238] [H2O2 / sulfuric acid stripping solution performance stability over time] A hydrogen peroxide composition (30% by mass) and sulfuric acid water (98% by mass) were mixed at a mixing ratio (mass ratio) of 1 / 1 and stirred for 2 hours. After stirring, the mixture was filtered using a 5 nm nylon filter to prepare a hydrogen peroxide solution for evaluation. This hydrogen peroxide solution was placed in each container to obtain a drug solution container. Each drug solution container was stored at 30°C and 5°C for 2 weeks. The hydrogen peroxide solution was taken out from the chemical solution container after storage. The performance stability over time was evaluated based on the resist stripping performance. The test method was as follows. In this evaluation, the sulfuric acid solution was heated to 60° C. before mixing with the hydrogen peroxide solution. In each example, after the hydrogen peroxide solution and the sulfuric acid solution were mixed, the mixture was further heated to the "treatment temperature" before being used in the resist stripping test. (Resist stripping test) Test wafer: The surface of a silicon wafer was treated with HMDS (hexamethyldisilazane), after which a 4 μm OFPR800 (positive resist manufactured by TOK) film was formed, and the stripping ability of this resist layer was evaluated under the following conditions. Volume of solution: 600ml Wafer size: 12 inch Si wafer Processing method: Single-wafer cleaning processing equipment Processing conditions: 120rpm / 1min. + 1500rpm / 30s ·Flow rate: 10ml. / min. / liquid temperature 90℃

[0239] Regarding resist strippability, the film thickness distribution was obtained for the processed wafer using VM-3110 (manufactured by Dainippon Screen Co., Ltd.), and the area of ​​the wafer with the residue was evaluated, and the removal rate was evaluated in terms of area. A time-dependent evaluation was performed for each container sample at a frequency of n=20, and the removal rate was evaluated as the ratio of the standard deviation of the removal rate when the chemical solution stored at 30°C was used to the standard deviation of the removal rate when the chemical solution stored at 5°C was used. Ratio = Standard deviation when using chemical solution stored at 30℃ / Standard deviation when using chemical solution stored at 5℃

[0240] A: The standard deviation ratio was less than 1.1. B: The ratio of standard deviations was greater than 1.1 and less than or equal to 1.3. C: The ratio of standard deviations was greater than 1.3 and less than or equal to 1.5. D: The ratio of standard deviations was greater than 1.5 and less than 2.0. E: The ratio of standard deviations exceeded 2.0.

[0241] The number of objects to be counted in the liquid, the coated particles, and the granular matter evaluations were the same as those described above.

[0242] [Temperature stability of buffered hydrofluoric acid etching solution] First, an aqueous solution (20% by mass) containing a hydroxylamine compound was prepared. Next, 14.9 g of 48% by mass potassium hydroxide (KOH) aqueous solution (containing 0.13 mol of KOH), 13.3 g of potassium carbonate (K2CO3) powder (containing 0.096 mol of K2CO3), 500.0 g of 20% by weight hydroxylamine (HA) aqueous solution, and 471.8 g of water were mixed to prepare 1000 g of etching solution. The potassium ion concentration in this etching solution was calculated to be 0.32 mol / kg, the carbonate ion concentration was calculated to be 0.096 mol / kg, and the molar ratio of the carbonate ion concentration to the potassium ion concentration was 0.30. The HA concentration in this etching solution was 10% by mass, and the pH of this etching solution was 13 or higher.

[0243] <Storage test over time> The etching solution was placed in the container to prepare a chemical solution container. The prepared chemical solution container was stored for one month under an environment of 4° C. and 40° C. After storage, the chemical solution was taken out of the chemical solution container, and the number of counted objects in the liquid, the change in particle density on the substrate, and the granular matter in the liquid were measured using the same method as above. The results are shown in Table 1.

[0244] <Evaluation of Etching Rate> A 300 mm diameter wafer with an oxide film was prepared, with an oxide film of 200 nm laminated on the wafer. Next, the wafer with the oxide film was treated at 60° C. for 30 seconds by immersion using the chemical solution (etching solution) taken out of the chemical solution container after storage. Next, the immersed wafer was rinsed with pure water multiple times and then spin-dried to prepare a treated wafer. The thickness of the oxide film on the wafer before and after the treatment was evaluated, and the etching rate was calculated from the difference in thickness of the oxide film before and after the treatment. Specifically, the average etching rate 1 of the etching liquid taken out of the chemical solution container stored for one month in an environment at 4°C and the average etching rate 2 of the etching liquid taken out of the chemical solution container stored for one month in an environment at 45°C were calculated, and the reduction rate represented by the following formula was calculated. The results were evaluated according to the following criteria and shown in Table 1. The above average etching rate 1 is obtained by preparing 50 samples of chemical solution containers stored for one month in an environment at 4° C., calculating the etching rate of the etching solution for each sample, and taking the arithmetic average of the calculated etching rates. The above average etching rate 2 is obtained by preparing 50 samples of chemical solution containers stored for one month in an environment at 40° C., calculating the etching rate of the etching solution for each sample, and taking the arithmetic average of the calculated etching rates. Formula: Reduction rate (%) = {(average etching rate 1 - average etching rate 2) / average etching rate 1} x 100

[0245] A: The rate of decrease was less than 0.5%. B: The rate of decrease was more than 0.5% but less than 1.0%. C: The rate of decrease was more than 1.0% but less than 3.0%. D: The rate of decrease was more than 3.0% but less than 5.0%. E: The rate of decrease exceeded 5.0%.

[0246] [Temperature stability of CMP (chemical mechanical polishing) slurries] A solution of CSL9044C (manufactured by FFPS (FUJIFILM Ultra Pure Solutions)) diluted 10 times was used as a CMP slurry (chemical liquid) and contained in the above container to prepare a chemical liquid container. Next, the above chemical liquid container was stored at 4°C and 40°C for one month. After storage, the chemical liquid was removed from the chemical liquid container, and the number of objects to be counted in the liquid, the change in particle density on the substrate, and particulate matter in the liquid were measured using the same methods as above, and the results are shown in Table 1.

[0247] <Evaluation of polishing speed> A 300 mm wafer with an oxide film was prepared, on which an oxide film of 200 nm was laminated. According to the following evaluation method, polished wafers were prepared, and the thicknesses of the oxide films on the wafers before and after the polishing treatment were evaluated, and the removal rate was calculated from the difference in film thickness before and after the treatment. <Evaluation method> The polishing apparatus used was a Lapmaster LGP-612, and each of the wafer films shown below was polished while supplying a slurry (polishing liquid) under the following conditions. Table rotation speed: 90 rpm Head rotation speed: 85 rpm Grinding pressure: 13.79kPa Polishing pad: Rodel Nitta Co., Ltd. Polotexpad ·Polishing liquid supply rate: 200ml / min

[0248] In the evaluation, the average value 1 of the polishing speed of the CMP slurry taken out of the chemical solution container stored for one month in an environment at 4°C and the average value 2 of the polishing speed of the CMP slurry taken out of the chemical solution container after being stored for one month in an environment at 40°C were calculated, and the reduction rate (%) of the polishing speed was calculated according to the following formula and evaluated according to the following criteria. The above average polishing rate 1 is the arithmetic mean of 50 samples of chemical solution containers stored for one month in an environment at 4° C., the polishing rate of the CMP slurry for each sample calculated, and the average polishing rate 2 is the arithmetic mean of 50 samples of chemical solution containers stored for one month in an environment at 40° C., the polishing rate of the CMP slurry for each sample calculated, and the average polishing rate 2 is the arithmetic mean of 50 samples of chemical solution containers stored for one month in an environment at 40° C. Formula: Reduction rate (%) = {(average polishing speed 1 - average polishing speed 2) / average polishing speed 1} x 100

[0249] A: The rate of decrease (%) was less than 1.0%. B: The rate of decrease (%) was more than 1.0% and less than 1.5%. C: The rate of decrease (%) was more than 1.5% and less than 2.0%. D: The rate of decrease (%) was more than 2.0% and less than 3.0%. E: The rate of decrease (%) exceeded 3.0%.

[0250] [Evaluation of stability over time of pCMP cleaner] Clean-100 (manufactured by Wako Pure Chemical Industries, Ltd.) was used as the post-CMP cleaner (referred to as "pCMP cleaner" in the table). Clean-100 was placed in the above-mentioned container to prepare a chemical solution container. Next, the above-mentioned chemical solution container was stored for one month in an environment of 4°C and 40°C. The chemical solution (pCMP cleaner) was removed from the chemical solution container after storage, and the number of objects to be counted in the liquid, the change in particle density on the substrate, and the amount of particulate matter in the liquid were measured using the same methods as above. The results are shown in Table 1.

[0251] <Evaluation of defect suppression performance> An oxide film was formed on a silicon wafer to a thickness of 100 nm to obtain a silicon wafer with an oxide film. Next, a resist film-forming composition film was formed on the oxide film, and pattern exposure was performed using a LS pattern with a line width of 40 nm, followed by development to form a patterned resist film.

[0252] Using the obtained patterned resist film as a mask, the insulating film (oxide film) was etched to form openings on the insulating film. The etching was performed by a plasma etching method using an etching gas containing nitrogen gas and halogen gas. Next, the patterned resist film was removed by oxygen ashing or a general-purpose resist stripper (MS6800, manufactured by FFEM (FUJIFILM Electronic Materials)), and further, the substrate was washed with a treatment solution containing a hydroxylamine compound to remove unnecessary residues resulting from the etching process.

[0253] Next, a metal film containing a film made of Ti (corresponding to a barrier film) and a film made of Co was formed in order by chemical vapor deposition on the insulating film with the opening formed therein, and the opening was filled. The unnecessary part of the metal film was removed from the base material having the obtained metal film by chemical mechanical polishing, and a planarization process was performed to form an insulating film with embedded metal wiring. At this time, chemical mechanical polishing was performed stepwise using two types of polishing liquid. Specifically, polishing was performed using a solution obtained by diluting CSL9044C (manufactured by FFPS) by 10 times as the polishing liquid until the film made of Ti was exposed, and then polishing was performed using a solution obtained by diluting BSL8178C (manufactured by FFPS) by 2 times as the polishing liquid until planarization was completed.

[0254] After polishing, the insulating film with the metal wiring embedded therein was washed with the chemical solution taken out from the stored chemical solution container, and then washed with water and isopropanol in that order. The defect suppression performance was evaluated by observing the pattern after washing using UVsion5 to determine the number of defects, and the increase in the number of defects was determined using the following method. Specifically, in the evaluation, the average number of defects 1 when processing using a chemical solution taken out of a chemical solution container stored for one month in an environment of 4°C and the average number of defects 2 when processing using a chemical solution taken out of a chemical solution container after storage for one month in an environment of 40°C were calculated, and the increase rate (%) of the number of defects was calculated according to the following formula and evaluated according to the following criteria. The average number of defects 1 is the arithmetic mean of 50 samples of drug solution containers stored for one month in an environment of 4° C., the number of defects when each sample's drug solution is used, and the average number of defects 2 is the arithmetic mean of 50 samples of drug solution containers stored for one month in an environment of 40 .... Formula: Increase rate (%) = {(average number of defects 2 - average number of defects 1) / average number of defects 1} x 100

[0255] A: The rate of increase was less than 1.0%. B: The rate of increase was more than 1.0% but less than 2.0%. C: The rate of increase was more than 2.0% but less than 3.0%. D: The increase rate was more than 3.0% but less than 5.0%. E: The increase rate exceeded 5.0%.

[0256] [Evaluation of temporal stability of pre-wetting liquid] Cyclohexanone, PGMEA (propylene glycol 1-monomethyl ether 2-acetate), ethyl lactate (EL), and PGMEA / PC (propylene carbonate) were each placed in the above-mentioned container to prepare a drug solution container. The liquid medicine container prepared above was stored for one month under environments at 4° C. and 40° C. After storage, the liquid medicine (pre-wet liquid) was taken out of the liquid medicine container, and the number of objects to be counted in the liquid, the change in particle density on the substrate, and the granular matter in the liquid were measured by the same method as above. The results are shown in Table 1.

[0257] Furthermore, for the PGMEA / PC-containing chemical solution container, a cyclic aging test was carried out in which the chemical solution was stored in the container under two conditions, (1) storage at -20°C for 2 days and (2) storage at 60°C for 5 days, was alternately carried out for 10 cycles, and the chemical solution stored in the container after the cyclic aging was evaluated in the same manner as in <Change in particle density on substrate> to evaluate the durability of the container. The evaluation results are shown in Table 1 as <Cycle evaluation>.

[0258] <Evaluation of lithography performance> A 10 cm layer of pre-wetting liquid was applied to a 300 mm diameter silicon wafer with a lower anti-reflective coating layer. 3 After spreading the composition at 500 rpm for 5 seconds, 1 cm 3 The solution was discharged and spread at 1500 rpm for 30 seconds, and then dried at 100° C. for 60 seconds to form a resist film. The lithography performance of the resist film thus obtained was evaluated in the same manner as that for the TMAH developer.

[0259] [Stability of butyl acetate developer over time] In the case where a butyl acetate developer was used instead of the TMAH developer used in the above [Temperature performance stability of TMAH developer], various evaluations were carried out in the same manner. Further, the cycle evaluation described in the above [Evaluation of temporal stability of pre-wetting liquid] was carried out. The resist composition used was a resist composition for negative development, and the evaluation was performed under changed conditions in which rinsing treatment was not performed. As a resist composition for negative development, a composition in which Resin A2 (87.01 parts by mass) was used instead of Resin A in the positive resist composition was used. Resin A2: Polymer with composition ratio of 30 / 10 / 60, Mw 8200, and dispersity of 1.53

[0260] [ka]

[0261] In Table 1, the manufacturing method of the container for each Example and Comparative Example, the physical properties of the container, and the performance of the liquid medicine stored in the container are listed in each column. For example, for the container of Example 1, the results are listed in Table 1[1]<part 1> and Table 1[2]<part 1>. That is, the container of Example 1 is a container having a coating layer on a substrate, and the results of the elution test were metal 0.9 mass ppb, TOC 200 mass ppm, RCA 0.92, and RCB 0.94. Furthermore, the performance of each liquid medicine stored in the container is as follows: The lithography performance of the TMAH developer was D, the number of countable objects in the solution was C, the coated particles were C, and the particulate matter rating was C; the stripping performance of the H2O2 / sulfuric acid stripper was D, the number of countable objects in the solution was C, the coated particles were C, and the particulate matter rating was C; the etching rate of the buffered hydrofluoric acid etchant was D, the number of countable objects in the solution was C, the coated particles were C, and the particulate matter rating was C; the polishing rate of the CMP slurry was D, the number of countable objects in the solution was C, the coated particles were C, and the particulate matter rating was C; p The CMP cleaner's defect suppression performance was rated D, the number of entities counted in the liquid was rated C, the coated particles were rated C, and the particulate matter rating was C; the cyclohexanone pre-wet liquid's lithography performance was rated D, the number of entities counted in the liquid was rated C, the coated particles were rated C, and the particulate matter rating was C; the PGMEA pre-wet liquid's lithography performance was rated D, the number of entities counted in the liquid was rated C, the coated particles were rated C, and the particulate matter rating was C; the EL pre-wet liquid's lithography performance was rated D, the number of entities counted in the liquid was rated C, the coated particles were rated C, and the particulate matter rating was C. Similarly, for the other examples and comparative examples, Example 2 is listed in Table 1[1]<Part 2> and Table 1[2]<Part 2>, Example 4 is listed in Table 1[1]<Part 3> and Table 1[2]<Part 3>, Example 6 is listed in Table 1[1]<Part 4> and Table [2]<Part 4>, Example 8 is listed in Table 1[1]<Part 5> and Table 2[2]<Part 5>, Example 10 is listed in Table 1[1]<Part 6> and Table 1[2]<Part 6>, and Example 11 is listed in Table 1[1]<Part 7> and Table 1[2]<Part 7>.

[0262] In the table, the columns "Fe", "Ni", and "Cr" represent the contents (ppb by mass) of Fe element, Ni element, and Cr element, respectively. The columns "Oleic acid amide" and "Polyethylene" show the content (ppm by mass) of oleic acid amide and polyethylene, respectively. Note that polyethylene is a low-polymerization polyethylene (polyethylene with 22 or less carbon atoms) and is classified as an organic substance with a boiling point of 300°C or higher.

[0263] [Table 1]

[0264] [Table 2]

[0265] [Table 3]

[0266] [Table 4]

[0267] [Table 5]

[0268] [Table 6]

[0269] [Table 7]

[0270] [Table 8]

[0271] [Table 9]

[0272] [Table 10]

[0273] [Table 11]

[0274] [Table 12]

[0275] [Table 13]

[0276] [Table 14]

[0277] The metal content of each chemical solution contained in each container was measured, and it was confirmed using ICP-MS (Agilent 8900) that the content of each metal species (Ti, Al, Zr, Hf, Fe, Ni, Sn, Zn, Cr, Mo, Fe, Ni, Sn) was 10 ppt by mass or less. In addition, organic impurities in each chemical solution were measured, and it was confirmed that the content of organic impurities including oleic acid amide and low-polymerization alkyl olefins (alkyl olefins having 22 or less carbon atoms) was 1 ppm by mass or less. As described above, by reducing the content of contaminating components in the stored chemical solution, damage to the container caused by impurities can be reduced, and in particular, the amount of elution over time due to low-temperature / high-temperature cycles can be suppressed.

[0278] From the results shown in Table 1, it was found that the performance of the liquid medicine contained in the container of each Example was not easily deteriorated over time. On the other hand, the performance of the liquid medicine contained in the container of each Comparative Example deteriorated over time. The container of Example 2 having a coating layer of a specific composition on a substrate had a lower RCA(s) compared to the container of Example 3 made of a specific composition, and as a result, the performance of the contained medicinal solution was less likely to deteriorate over time. The container of Example 2, which had a coating layer made of a specific composition on a substrate and was further produced by cleaning the coating layer by the method described in Table 1, had lower RCAs and RCBs than the chemical solution of Example 1, which did not undergo a cleaning process, and as a result, the performance of the stored chemical solution was less likely to deteriorate over time. In the cleaning process, the container of Example 8, in which the temperature of the cleaning liquid used was higher and the cleaning method was ultrasonic cleaning, had lower RCA and RCB than the container of Example 3, and as a result, the performance of the contained chemical liquid was less likely to deteriorate over time. The container of Example 7, which used an acid and an organic solvent as the cleaning solution in the cleaning process, had a lower RCB and a smaller amount of TOC eluted in the elution test than the container of Example 9. As a result, the performance was less likely to deteriorate over time in chemical solutions (other than the H2O2 / sulfuric acid stripping solution and the buffered hydrofluoric acid etching solution) that are more affected by organic impurities. In the cleaning process, the container of Example 8, which was cleaned with ultrapure water for 1 hour, showed less deterioration in performance over time in the TMAH developer and CMP slurry, which are more susceptible to the effects of water-soluble impurities (salts, etc.), compared to the container of Example 2, which was cleaned with ultrapure water for 5 minutes. The container of Example 5 had fewer coated particles, especially in the case of an organic solvent-based chemical solution, as a result, compared to the containers of Example 4 and Example 6. The evaluation criteria for coated particles are strict, and the influence of very small amounts of components remains, but the difference is particularly noticeable at higher evaluation ranks. When the chemical solution is an organic solvent-based solution, the coated particles are easily eluted, resulting in a worse evaluation, but the container of Example 5 had a better effect of the present invention.

[0279] In addition, for the containers of Examples 1 to 12, before storing each liquid medicine, the container was washed with the liquid medicine to be stored, and then the liquid medicine was stored. When the obtained liquid medicine storage bodies were used, the same results as above were obtained. In addition, for the containers of Examples 1 to 12, the containers were immersed in the medicinal liquid to be contained for one week before containing each medicinal liquid, and then the medicinal liquid was contained. When the obtained medicinal liquid containers were used, the same results as above were obtained.

[0280] The prepared chemical was used to clean the 2t tank for supplying chemicals connected to the solvent line of the Lithius-ProZ coater / developer for litho process, and the process unit connected to the piping to the litho device. A SUS tank / line was used as the chemical line up to the device connection. The cleaning conditions were as follows: the prepared chemical was filled into the supply tank, and the piping was flushed so that the amount of chemical flowed was 10 times the total chemical volume of the tank and piping. After the above flushing was performed for three more cycles, the chemical for production was added, the chemical was produced, and then the container described in Examples 1 to 12 was filled with the chemical. The chemical liquid in the prepared chemical liquid container was subjected to the above-mentioned lithography performance, number of objects counted in the liquid, coated particles, and granular matter evaluations, and the same results as those of the above-mentioned examples were obtained. The POU filter loaded in the coater / developer was immersed in the chemical solution to be used for one week before loading, and then connected and used before flushing.

[0281] Furthermore, a semiconductor chemical production line was used, which was equipped with a 2 ton PTFE (polytetrafluoroethylene) lined SUS kettle, PTFE lined SUS piping, and a PTFE lined SUS filter unit (pressure resistant container), and similar evaluations were carried out on the lithography performance, number of counted objects in the liquid, coated particles, and granular matter, with the same results as above being obtained.

[0282] In addition, containers were produced by carrying out the same treatment as in the Examples for the following containers: an 18 L canister-sized container, a 200 L drum-sized container, a 1 ton tote-sized container, and a 10 ton container-sized container. Various evaluations were carried out using the produced containers in the same manner as above, and similar results were obtained.

[0283] Samples were prepared in the same manner as in Examples 1 to 12, except that the operation of placing the chemical solution in the container was carried out in a class 1000 clean room, and the same evaluations were carried out. The same results as in Examples 1 to 12 were obtained. In addition, samples were prepared in the same manner as in Examples 1 to 12, except that the operation of placing the chemical liquid in the container was carried out in a class 100 clean room, and the same evaluations were carried out. The same results as in Examples 1 to 12 were obtained. In addition, samples were prepared in the same manner as in Examples 1 to 12, except that the operation of placing the chemical liquid in the actual container was carried out in a class 10 clean room, and the same evaluations were carried out. The same results as in Examples 1 to 12 were obtained.

[0284] The above-mentioned embodiments of Examples 4 and 5 correspond to an embodiment in which the filling rate, as expressed by the following formula, is 80 volume %. Formula (X): Filling rate = (Volume of drug solution in container / Container volume of container) The results of the above-mentioned evaluations of the above-mentioned embodiments of Examples 4 and 5 are shown below, with the packing rate and organic concentration adjusted as shown in Table 2. Note that Example 4-1 corresponds to an embodiment of Example 4 in which the packing rate and organic concentration are changed, and Example 5-1 corresponds to an embodiment of Example 5 in which the packing rate and organic concentration are changed. Formula (Y): Organic matter concentration = (volume of organic matter contained in the space in the container that is not filled with chemical solution / volume of the space in the container that is not filled with chemical solution) x 100

[0285] [Table 15] < / rcas>

Claims

1. A drug solution container having a container and a drug solution contained in the container, The container has a substrate, and a coating layer having a thickness of 50 μm or more, the coating layer being disposed on all of the liquid-contacting portions of the substrate and containing a composition containing a polyolefin and at least one metal component selected from the group consisting of Ti, Al, Mg, Zr, Hf, Fe, Ni, Sn, Zn, Cr, and Mo; When the composition contains one of the metal components, A surface region is defined as a region between the surface of the coating layer and a position 10 nm from the surface in the thickness direction of the coating layer, and an internal region is defined as a region between a position 30 μm from the surface in the thickness direction of the coating layer and a position 50 μm from the surface in the thickness direction of the coating layer, and when the surface region and the internal region are measured with a time-of-flight secondary ion mass spectrometer, In at least a part of the coating layer, a ratio RCAs calculated by CA1s / CA2s, where CA1s is an intensity ratio of a peak intensity of secondary ions derived from the metal component in the surface region to a peak intensity of secondary ions derived from the polyolefin in the surface region, and CA2s is an intensity ratio of a peak intensity of secondary ions derived from the metal component in the inner region to a peak intensity of secondary ions derived from the polyolefin in the inner region, is less than 1.00, When the composition contains two or more of the metal components, In at least a portion of the coating layer, an average value of the ratios RCAs calculated for each of the two or more metal components is less than 1.00; The chemical liquid container, wherein the chemical liquid is at least one selected from the group consisting of an alkaline developer, a resist stripper, an etching liquid, a slurry for chemical mechanical polishing, and a post-CMP cleaner.

2. A drug solution container having a container and a drug solution contained in the container, The container is made of a composition containing a polyolefin and at least one metal component selected from the group consisting of Ti, Al, Mg, Zr, Hf, Fe, Ni, Sn, Zn, Cr, and Mo; When the composition contains one of the metal components, A surface region is defined as a region between the surface of the container and a position 10 nm from the surface in the thickness direction of the container, and an internal region is defined as a region between a position 30 μm from the surface in the thickness direction of the container and a position 50 μm from the surface in the thickness direction of the container, and when the surface region and the internal region are measured with a time-of-flight secondary ion mass spectrometer, In at least a part of the container, a ratio RCA calculated by CA1 / CA2, where CA1 is an intensity ratio of a peak intensity of secondary ions derived from the metal component in the surface region to a peak intensity of secondary ions derived from the polyolefin in the surface region, and CA2 is an intensity ratio of a peak intensity of secondary ions derived from the metal component in the internal region to a peak intensity of secondary ions derived from the polyolefin in the internal region, is less than 1.00; When the composition contains two or more of the metal components, In at least a portion of the container, an average value of the ratio RCA calculated for each of two or more metal components is less than 1.00; The chemical liquid container, wherein the chemical liquid is at least one selected from the group consisting of an alkaline developer, a resist stripper, an etching liquid, a slurry for chemical mechanical polishing, and a post-CMP cleaner.

3. The drug solution container according to claim 1 , wherein the drug solution contains water.

4. The drug solution container according to any one of claims 1 to 3, wherein the filling rate calculated by formula (X) is 60 volume % or more. Formula (X): Filling rate = (Volume of drug solution in container / Volume of container) x 100

5. 5. The drug solution container according to claim 1, wherein the organic substance concentration calculated by formula (Y) is 1 ppm by volume or less. Formula (Y): Organic substance concentration=(Volume of organic substances contained in the space in the container that is not filled with the chemical solution / Volume of the space in the container that is not filled with the chemical solution)×100 However, the organic matter does not include components contained in the chemical solution.

6. 6. The drug solution container according to claim 1, wherein the drug solution contains water, and the content of water in the drug solution is 50% by mass or more.

7. The chemical solution was applied onto a substrate, and the change in density of particles having a particle diameter of 19 nm or less on the substrate was measured before and after application of the chemical solution using a particle inspection device, and the change was 0.3 particles / cm 2 The drug solution container according to any one of claims 1 to 6, wherein:

8. The drug solution container according to any one of claims 1 to 7, wherein particulate matter having a particle diameter of 30 nm or less in the drug solution is 1.0 mass ppb or less relative to the total mass of the drug solution, as measured by a single particle inductively coupled plasma mass spectrometer.

9. The drug solution container according to any one of claims 1 to 8, wherein the drug solution further contains a surfactant.

Citation Information

Patent Citations

  • Method for washing container

    JP1998000436A

  • Polyethylene-made container excellent in cleanness

    JP1999246714A

  • Treatment method of container

    JP2001284309A

  • Multilayer hollow container

    JP2007152712A

  • Container for fluid, and container with fluid using the same

    JP2008007153A