Heat dissipation sheet and its manufacturing method
The silicone resin-alumina composite heat dissipation sheet addresses the issues of conventional sheets by providing low compressive stress and resilience, ensuring efficient heat transfer and easy installation while preventing component damage.
Patent Information
- Application Number
- JP2023136628
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-08-24
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2039-08-30
AI Technical Summary
Conventional heat dissipation sheets with unvulcanized compound layers between thin film reinforcing layers lack rubber elasticity and recovery properties, leading to gaps between heat generating components and radiators, poor workability, and high compressive stress during attachment, which can damage components and hinder efficient heat transfer.
A heat dissipation sheet made of silicone resin mixed with alumina, with specific particle size distributions and hardness properties, designed to have low compressive stress and resilience, allowing efficient heat transfer and improved workability.
The sheet effectively transfers heat without damaging components, maintains contact during thermal cycles, and facilitates easy installation by reducing the force required for attachment, ensuring efficient heat dissipation.
Smart Images

Figure 0007573703000001 
Figure 0007573703000002 
Figure 0007573703000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a heat dissipation sheet and a method for producing the same. [Background technology]
[0002] To prevent runaway or damage caused by heat generation, heat-generating components such as CPUs may have heat sinks, such as heat sink fins or fans, attached to their surfaces via heat dissipation sheets.
[0003] In order to efficiently transfer heat from the heat-generating component to the heat sink using a heat sink sheet interposed between the heat-generating component and the heat sink, it is preferable for the heat sink sheet to be in close contact with both the heat-generating component and the heat sink without any gaps. Therefore, with the heat sink sheet interposed on the surface of the heat-generating component, the heat sink is attached with clips or screws, etc., so that the heat sink is compressed between the heat-generating component and the heat sink. In this case, if the heat sink sheet is too hard, it may damage the heat-generating component and the heat sink, so it is preferable for the heat sink sheet to have a low hardness.
[0004] Conventional heat dissipation sheets have an unvulcanized compound layer sandwiched between thin-film reinforcing layers that have been hardened into a rubber-like material; when pressure is applied to the heat dissipation sheet by attaching a heat sink, the compound layer between the thin-film reinforcing layers protrudes laterally, thereby relieving stress (Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2002-33427 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, in a heat dissipation sheet in which an unvulcanized compound layer is sandwiched between thin-film reinforcing layers that have been hardened into a rubber-like material, the inner unvulcanized compound layer is unvulcanized, so it lacks rubber elasticity and has poor recovery properties. Therefore, during the cooling and heating cycles that occur depending on how the heat-generating component is used, gaps may form between the heat-generating component or the heat sink, and the heat from the heat-generating component may not be transferred efficiently to the heat sink. In addition, the pressure applied when attaching the heat sink causes the compound layer between the thin film reinforcing layers to protrude laterally, which results in poor workability when attaching the heat sink sheet. Furthermore, since the rubber layers sandwiching the thin-film reinforcing layer are made of vulcanized rubber, they have a high compressive stress, which requires a large force to attach the radiator, making the attachment process difficult.
[0007] The present invention has been made in consideration of the above-mentioned points, and an object of the present invention is to provide a heat dissipation sheet which has low hardness, low compressive stress properties and recovery properties, and which has good workability, and a method for producing the same. [Means for solving the problem]
[0008] First aspect The present invention is characterized in that, in a heat dissipation sheet made of a silicone resin mixed with alumina, the silicone resin has a penetration of 60 to 90, 150 to 300 parts by weight of the alumina is mixed into 100 parts by weight of the silicone resin, and 10 to 20 wt % of the alumina has an average particle diameter (d50) of 70 to 100 μm.
[0009] Second Aspect teeth, First aspect The alumina has an average particle size (d50) of 0.1 to 5 μm in an amount of 60 to 80 wt %.
[0010] Third aspect teeth, First aspect or Second Aspect The present invention is characterized in that a resin coating is laminated on the surface of the layer made of silicone resin mixed with alumina.
[0011] Fourth aspect teeth, First aspect from Third aspect Either one of Aspects of The heat dissipation sheet has a surface hardness of 2 to 10 degrees in Asker C hardness and a 50% compressive stress (in accordance with ASTM D575-91) of 0.1 to 0.2 MPa.
[0012] Fifth aspect The present invention relates to a method for producing a heat dissipation sheet made of silicone resin mixed with alumina, characterized in that 100 parts by weight of silicone resin having a penetration of 60 to 90 and 150 to 300 parts by weight of alumina in which 10 to 20 wt% of the alumina has an average particle size (d50) of 70 to 100 μm are mixed, the mixture is vacuum degassed, and then the mixture is formed into a sheet and heat cured.
[0013] Sixth Aspect teeth, Fifth aspect The alumina has an average particle diameter (d50) of 0.1 to 5 μm in an amount of 60 to 80 wt %.
[0014] Seventh aspect teeth, Fifth aspect or Sixth Aspect After the mixing and vacuum degassing, the resin coating is laminated into a sheet shape and then cured by heating. Effect of the Invention
[0015] According to the present invention, the heat dissipation sheet is made by mixing 100 parts by weight of silicone resin having a penetration of 60 to 90 with 150 to 300 parts by weight of alumina, of which 10 to 20 wt% has an average particle diameter (d50) of 70 to 100 μm, and therefore has low hardness, low compressive stress properties and recovery properties.
[0016] Furthermore, since the heat dissipation sheet of the present invention has low hardness and low compressive stress, it is possible to reduce the force required when attaching a heat sink to the surface of a heat-generating part by sandwiching the heat dissipation sheet of the present invention therebetween. Since the heat dissipation sheet of the present invention is made of silicone resin mixed with alumina, there is no problem of the unvulcanized compound layer protruding laterally due to pressure, as occurs with heat dissipation sheets in which an unvulcanized compound layer is sandwiched between rubber layers, and installation workability is improved. Furthermore, since the heat dissipation sheet of the present invention has recovery properties, it recovers in accordance with the temperature during the cooling and heating cycles that occur when the heat-generating component is in use, and no gaps are created between the heat dissipation sheet and the heat-generating component or heat sink, so that the heat from the heat-generating component can be efficiently transferred to the heat sink via the heat dissipation sheet.
[0017] Furthermore, according to the method for producing a heat-dissipating sheet of the present invention, a heat-dissipating sheet having low hardness, low compressive stress properties and recovery properties as described above, and excellent workability can be easily obtained. [Brief description of the drawings]
[0018] [Figure 1] 1 is a cross-sectional view of a first embodiment of a heat dissipation sheet according to the present invention. [Diagram 2] FIG. 4 is a cross-sectional view of a second embodiment of a heat dissipation sheet according to the present invention. [Diagram 3] 1 is a first table showing the configurations and physical properties of each example of the present invention and each comparative example. [Figure 4] 2 is a second table showing the configurations and physical properties of each example of the present invention and each comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] A heat dissipation sheet 10 according to a first embodiment of the present invention shown in Fig. 1 is made of alumina-mixed silicone resin 11. The heat dissipation sheet 10 is placed on the surface of a heat-generating component, and is intended to efficiently transfer heat from the heat-generating component to a heat sink attached to the heat-generating component with the heat dissipation sheet 10 sandwiched therebetween.
[0020] The heat dissipation sheet 10 preferably has a low surface hardness of 2 to 10 on the Asker C hardness scale and a low compressive stress of 0.1 to 0.2 MPa (based on ASTM D575-91). If at least one of the surface hardness and 50% compressive stress of the heat dissipation sheet 10 is higher than the above range, the pressure required to attach the heat sink to the heat-generating component via the heat dissipation sheet 10 may increase, making it difficult to attach the heat sink or damaging the heat-generating component.
[0021] In order to efficiently transfer heat from heat-generating components to a radiator, the heat dissipation sheet 10 preferably has a thermal conductivity (based on JIS R2616) of 1.2 W / (m·K) or more, and more preferably 1.2 to 1.9 W / (m·K).
[0022] Furthermore, in order for the heat dissipation sheet 10 to recover in response to changes in temperature during the cooling and heating cycles that occur when the heat-generating components are in use, and to prevent gaps from occurring between the heat dissipation sheet and the heat-generating components and radiator, it is preferable that the compression set (C-set, 100°C, 50% compression rate) based on JIS K6262 be 20 to 60%.
[0023] A thin heat dissipation sheet 10 is preferable in order to efficiently transfer heat from the heat generating component to the heat sink. On the other hand, a thick heat dissipation sheet 10 is preferable in order to prevent damage to the heat generating component due to pressure applied when the heat sink is attached to the heat generating component with the heat dissipation sheet 10 sandwiched therebetween, and due to pressure applied by the heat sink to keep the heat dissipation sheet 10 in close contact with the heat generating component and the heat sink. To satisfy both of these requirements, the thickness of the heat dissipation sheet 10 is preferably 0.5 to 5.0 mm.
[0024] The alumina-mixed silicone resin 11 constituting the heat dissipation sheet 10 is made by mixing 150 to 300 parts by weight of alumina into 100 parts by weight of silicone resin. The cured silicone resin preferably has a penetration (based on JIS K2220) of 60 to 90. If the penetration is lower than 60, the silicone resin (cured product) will be too hard, and conversely, if the penetration is higher than 90, the silicone resin (cured product) will be too soft. In either case, the thermal dissipation sheet 10 will not be able to provide sufficient cushioning against pressure applied during and after installation on the radiator, which may cause damage to the heat-generating components.
[0025] The silicone resin as a raw material is mainly composed of organopolysiloxane and is liquid at room temperature. There are one-liquid silicone resins and two-liquid silicone resins. The one-liquid silicone resin contains a crosslinkable silyl group-containing low molecular weight compound as a crosslinking component in the main component composed of organopolysiloxane having a silanol group at the end. The two-liquid silicone resin is composed of a base agent composed of organopolysiloxane having a silanol group at the end and a curing agent composed of aminoxyalkylsilane, and is used by mixing the base agent and the curing agent. In addition, the curing reaction of the silicone resin is classified into moisture curing and heat curing types, and a moisture curing type raw material may be used, or a heat curing type raw material may be used. In the present invention, either one-liquid type or two-liquid type may be used, but the two-liquid type is preferable because it is easy to adjust the pot life (usable time).
[0026] The silicone resin is not limited to one type, and multiple types may be used. When multiple types are used, each of the cured products may have a penetration (based on JIS K2220) of 60 to 90, or at least one of the silicone resins may have a penetration (based on JIS K2220) outside the range of 60 to 90, and multiple types may be mixed together to produce a cured product with a penetration of 60 to 90.
[0027] By mixing 150 to 300 parts by weight, preferably 160 to 300 parts by weight, of alumina with 100 parts by weight of silicone resin, the heat dissipation sheet 10 can have good thermal conductivity without impairing the low compressive stress properties.
[0028] Of the 150-300 parts by weight of alumina contained in 100 parts by weight of silicone resin, 10-20 wt%, more preferably 12-17 wt%, of the total amount of alumina (100 wt%), is composed of large diameter particles (preferably 70-100 μm) with an average particle diameter (d50, median diameter) of 70 μm or more. By containing 10-20 wt% of alumina with an average particle diameter (d50) of 70-100 μm in 150-300 parts by weight of alumina, the 50% compressive stress (in accordance with ASTM D575-91) of the heat dissipation sheet 10 can be set to 0.1-0.2 MPa, and the thermal conductivity can be improved to 1.2 W / (m·K) or more. If the amount of alumina with an average particle diameter (d50) of 70-100 μm is more than 20 wt%, the 50% compressive stress becomes too high. If the alumina having an average particle size (d50) of 70 to 100 μm is less than 10 wt %, even if the total alumina content is 150 to 300 parts by weight, the 50% compressive stress will be too low and the thermal conductivity will be low.
[0029] As for 150-300 parts by weight of alumina contained in 100 parts by weight of silicone resin, 10-20wt% of alumina having a large diameter (70-100μm) with an average particle diameter (d50, median diameter) of 70μm or more and 60-80wt% of alumina having a small diameter (preferably 0.1-5μm) with an average particle diameter (d50) of less than 5μm is preferably contained as alumina with a small diameter, more preferably 60-70wt%. By setting the content of alumina having an average particle diameter (d50) of 70-100μm and alumina having an average particle diameter (d50) of 0.1-5μm within the above range, the low compressive stress property of the heat dissipation sheet 10 can be improved.
[0030] In addition, when the total content of alumina having an average particle size (d50) of 70 to 100 μm and alumina having an average particle size (d50) of 0.1 to 5 μm is less than 100 wt%, the remaining alumina contained in the total amount of alumina (100 wt%) is preferably alumina having an average particle size (d50, median size) of 5 μm to 70 μm. By making the average particle size (d50) of the remaining alumina contained in the total amount of alumina (100 wt%) in the range of 5 μm to 70 μm, it is easy to form a network structure (a structure in which powder particles contact each other), and the thermal conductivity can be improved while maintaining a low compressive stress.
[0031] Inorganic fillers such as flame retardants are appropriately mixed into the alumina-mixed silicone resin 11. Examples of the flame retardant include aluminum hydroxide and magnesium hydroxide. The amount of aluminum hydroxide mixed is preferably 10 to 50 parts by weight per 100 parts by weight of the silicone resin.
[0032] 2, a heat dissipation sheet 10A of the second embodiment has a structure in which a resin coating 21A is laminated on the surface of an alumina-mixed silicone resin layer 11A. Since the surface of the alumina-mixed silicone resin layer 11A has tackiness (stickiness), by covering the surface of the alumina-mixed silicone resin layer 11A with the resin coating 21A, the handleability of the heat dissipation sheet 10A can be improved.
[0033] The alumina-mixed silicone resin layer 11A is made of silicone resin, alumina, inorganic fillers such as flame retardants, etc., similar to the alumina-mixed silicone resin 11 that constitutes the heat dissipation sheet 10 of the first embodiment, as described in the heat dissipation sheet 10 of the first embodiment.
[0034] Examples of the resin coating 21A include an acrylic resin coating, a polyvinylidene chloride resin (PVDC) film, a polyester film, a polyamide film, etc. The thickness of the resin coating 21A is preferably less than 1 μm so as not to affect thermal conduction, or 10 μm or more so as to have an effect as a reinforcing material. The resin coating 21A is not limited to being provided on one surface of the alumina-mixed silicone resin layer 11A, but may be provided on both surfaces.
[0035] A method for manufacturing the heat dissipating sheet 10 of the first embodiment and the heat dissipating sheet 10A of the second embodiment will be described. The method for producing the heat dissipation sheet 10 of the first embodiment is to mix 100 parts by weight of silicone resin having a penetration of 60 to 90 with 150 to 300 parts by weight of alumina in which 10 to 20 wt% of the alumina has an average particle size (d50) of 70 to 100 μm, degass the mixture in a vacuum, form it into a sheet, and heat cure it to obtain the heat dissipation sheet 10. When an inorganic filler or the like is mixed into the silicone resin, the inorganic filler or the like is mixed with the silicone resin and alumina. The silicone resin, alumina, inorganic filler, and the like are as described in the heat dissipation sheet 10 of the first embodiment.
[0036] The temperature during mixing is set lower than the temperature at which the silicone resin hardens, so that the silicone resin does not harden during mixing. The mixing is carried out using a planetary mixer or the like, and by carrying out mixing under reduced vacuum conditions, mixing and vacuum degassing can be carried out simultaneously.
[0037] Methods for making sheets include using a press mold and pouring it onto a film. The method using a press mold is a method in which the alumina-mixed silicone resin solution obtained by mixing and vacuum degassing is discharged into a press mold and pressed into a sheet shape, and the alumina-mixed silicone resin is thermally cured by heating the press mold.
[0038] The method of pouring onto a film is a method in which the alumina-mixed silicone resin solution obtained by mixing and vacuum degassing is poured onto a plastic film conveyed by a conveyer belt, rolled with rolls arranged above and below the plastic film, and passed through a hot air heating oven while being formed into a sheet of a specified thickness, whereby the silicone resin is heated and cured. Suitable plastic films onto which the alumina-mixed silicone resin solution is poured are fluorine-based such as PTFE (polytetrafluoroethylene) having mold releasability, polyester (PET) with mold release treatment, etc.
[0039] A method for producing the heat dissipating sheet 11 of the second embodiment will be described. The alumina-mixed silicone resin solution is obtained by mixing and vacuum degassing in the same manner as in the manufacturing method of the heat dissipation sheet 11 of the first embodiment. The obtained alumina-mixed silicone resin solution is formed into a sheet shape by using a press die or by pouring it onto a film, and a resin coating is laminated and heated to harden.
[0040] In the method using a press mold, when the alumina-mixed silicone resin solution obtained by mixing and vacuum degassing is ejected into the press mold, a film constituting the resin coating 21A is placed on at least one mold surface of the press mold in advance, and the rest is carried out in the same manner as in the manufacture of the heat dissipation sheet 10 of the first embodiment.
[0041] In the method of casting on a film, the film that constitutes the resin coating 21A is used as the plastic film transported by a conveyer, and the rest of the process is the same as the method of manufacturing the heat dissipation sheet 10 of the first embodiment. When providing resin coatings on both sides of the alumina-mixed silicone resin layer, a film that will form the resin coating on one side is used as the plastic film transported by the conveyor, the alumina-mixed silicone resin solution is poured onto that plastic film, and the plastic film that will form the resin coating on the other side is laminated on top of the alumina-mixed silicone resin solution, and the upper and lower plastic films are sandwiched between rolls and rolled, and the rest is the same as when providing a resin coating on one side. EXAMPLES
[0042] The following silicone resin, alumina, aluminum hydroxide, acrylic resin coating, and PVDC film were used to manufacture the heat dissipation sheets of the examples and comparative examples shown in FIG. 3 and FIG. Silicone resin 1; 2-component type, Product name: KE-1013, Shin-Etsu Chemical Co., Ltd., Penetration 60 Silicone resin 2; 2-component type, Product name; EG-3100, manufactured by Dow Corning Toray Co., Ltd., Penetration 85 Alumina 1: Average particle size (d50) 4.6 μm, Product name: AL-43KT, manufactured by Showa Denko K.K. Alumina 2: average particle size (d50) 55 μm, product name: LS-13, manufactured by Nippon Light Metal Co., Ltd. Alumina 3: Average particle size (d50) 80 μm, Product name: F180, manufactured by Nippon Light Metal Co., Ltd. Aluminum hydroxide; average particle size (d50) 27 μm; product name: SB-303; manufactured by Nippon Light Metal Co., Ltd. Polyester film with acrylic resin coating layer; acrylic layer thickness 0.6μm; Product name; Made by Hill Print Co., Ltd. PVDC film; thickness 10 μm; product name: Saran Wrap (registered trademark); manufactured by Asahi Kasei Home Products Corporation
[0043] A heat dissipation sheet having a thickness of 5 mm was manufactured by mixing silicone resin, alumina, and aluminum hydroxide in the compositions shown in each of the examples and comparative examples in Fig. 3 and Fig. 4 and pouring them onto the film (lower film, release PET film) of the conveyor belt. Mixing was performed for 15 minutes at 350 rpm using a planetary mixer (35 °C) under vacuum reduced pressure. Except for Examples 5 and 6, a release PET film was laminated on the alumina-mixed silicone resin solution as an upper film. In Example 5, a laminated film of an acrylic resin coating (thickness 0.6 μm) and a PET film was used as the upper film, and the acrylic resin coating was made to contact the silicone resin. In Example 6, the film on the upper surface was a PVDC film (thickness 10 μm). In Example 5, the film was heated in a hot air oven at 130° C. for 15 minutes, and in all other examples, the film was heated in a hot air oven at 150° C. for 15 minutes. The gap between the upper and lower metal rolls was 5 mm, so that the thickness of the heat dissipation sheet was 5 mm. After heat curing, the release PET films on the upper and lower surfaces were peeled off to produce a heat dissipation sheet. The acrylic resin coating on the upper surface of Example 5 and the PVDC film on the upper surface of Example 6 were left in their original state without being peeled off to produce a heat dissipation sheet.
[0044] The heat dissipation sheets of each Example and Comparative Example were measured or judged for surface hardness, 50% compression stress, compression set, thermal conductivity, tackiness, and shape retention, and a comprehensive evaluation was performed. Note that the heat dissipation sheets of Examples 5 and 6 were measured with the film surface facing up. The surface hardness was measured by an Asker C hardness tester. The 50% compressive stress was measured based on ASTM D575-91, and was determined by measuring the stress when the specimen was compressed by 50% and held for 60 seconds. Compression set was calculated based on JIS K6262 by compressing the sample by 50% of the original thickness using a spacer and maintaining the state at 100°C for 22 hours, then removing the sample from the compression tool and measuring the thickness after compression using the following formula. Compression set = (original thickness - thickness after compression) / (original thickness - spacer thickness) x 100 The thermal conductivity was measured based on JIS R2616. Tackiness was evaluated as "tacky" if the surface of the heat dissipation sheet was touched with the hand and felt sticky, and "not tacky" if no stickiness was felt. Note that in Example 5, the evaluation was based on the touch feeling against the acrylic resin coating, and in Example 6, the evaluation was based on the touch feeling against the PVDC film. The shape retention was evaluated by peeling the release film off the heat dissipation sheet with the release film, attaching the heat dissipation sheet to a specified location, and observing the sheet deformability at that time. When the release film was peeled off from the heat dissipation sheet with the release film and the heat dissipation sheet was attached, if there was no deformation of the sheet shape and there were no problems with the attachment, it was rated as "◎", if there was a risk of the sheet shape being deformed, it was rated as "◯", and if the sheet shape was deformed and the attachment was difficult, it was rated as "×". The overall evaluation was rated as "X" if at least one of the items of surface hardness, compressive stress, thermal conductivity, and shape retention was outside the specified range below. If each of the items of surface hardness, compressive stress, and thermal conductivity was within the respective standard range and shape retention was ◯, the overall evaluation was ◯, and if each of the items of surface hardness, compressive stress, and thermal conductivity was within the respective standard range and shape retention was ◎, the overall evaluation was ◎. The pass criteria for each item of surface hardness, compressive stress, thermal conductivity, and shape retention are surface hardness (2 to 10 degrees), compressive stress (0.1 to 0.2 MPa), thermal conductivity (1.2 W / (m·K) or more), and shape retention (◯ or ◎).
[0045] Example 1 Example 1 is an example in which the silicone resin 1 (penetration 60) is 20 parts by weight, the silicone resin 2 (penetration 85) is 80 parts by weight, the silicone resin has a penetration of 65, the alumina 1 (average particle size (d50) 4.6 μm) is 55 parts by weight, the alumina 2 (average particle size (d50) 55 μm) is 80 parts by weight, the alumina 3 (average particle size (d50) 80 μm) is 30 parts by weight, the aluminum hydroxide is 50 parts by weight, the total amount of alumina is 165 parts by weight, the content of alumina 3 (average particle size (d50) 80 μm) is 18 wt% in the total amount of alumina 100 wt%, the content of alumina 1 (average particle size (d50) 4.6 μm) is 33 wt%, and there is no acrylic resin coating or PVDC film. The penetration value of the entire silicone resin is a value measured according to JIS K2220.
[0046] Example 1 has a surface hardness (Asker C hardness) of 4, a 50% compressive stress of 0.13 MPa, and It has a permanent set of 45%, thermal conductivity of 1.2 W / (m K), tackiness, shape retention "◎", and an overall rating of "◎". It is a heat dissipation sheet that has low hardness, low compressive stress and recovery, and is easy to install.
[0047] Example 2 Example 2 is an example in which the alumina 1 (average particle diameter (d50) 4.6 μm) in Example 1 is 140 parts by weight, the alumina 2 (average particle diameter (d50) 55 μm) is 40 parts by weight, the alumina 3 (average particle diameter (d50) 80 μm) is 25 parts by weight, the total amount of alumina is 205 parts by weight, the content of alumina 3 (average particle diameter (d50) 80 μm) is 12 wt% and the content of alumina 1 (average particle diameter (d50) 4.6 μm) is 68 wt% out of a total amount of alumina of 100 wt%, and the rest are the same as Example 1.
[0048] Example 2 has a surface hardness (Asker C hardness) of 4, a 50% compressive stress of 0.12 MPa, a compression set of 46%, a thermal conductivity of 1.3 W / (m K), tackiness, shape retention of "◎", and an overall rating of "◎". It is a heat dissipation sheet with low hardness, low compressive stress and recovery properties, and easy installation and workability.
[0049] Example 3 Example 3 is an example in which the alumina 1 (average particle diameter (d50) 4.6 μm) in Example 1 is 170 parts by weight, the alumina 2 (average particle diameter (d50) 55 μm) is 55 parts by weight, the alumina 3 (average particle diameter (d50) 80 μm) is 45 parts by weight, the total amount of alumina is 270 parts by weight, the content of alumina 3 (average particle diameter (d50) 80 μm) is 17 wt% and the content of alumina 1 (average particle diameter (d50) 4.6 μm) is 63 wt% out of the total amount of alumina 100 wt%, and the rest are the same as Example 1.
[0050] Example 3 has a surface hardness (Asker C hardness) of 7, a 50% compressive stress of 0.19 MPa, a compression set of 45%, a thermal conductivity of 1.62 W / (m K), tackiness, shape retention of "◎", and an overall rating of "◎". It is a heat dissipation sheet with low hardness, low compressive stress and recovery properties, and easy installation workability.
[0051] Example 4 Example 4 is an example in which silicone resin 1 (penetration 60) is 0 parts by weight, silicone resin 2 (penetration 85) is 100 parts by weight, the total penetration of the silicone resin is 85, alumina 1 (average particle diameter (d50) 4.6 μm) is 140 parts by weight, alumina 2 (average particle diameter (d50) 55 μm) is 110 parts by weight, alumina 3 (average particle diameter (d50) 80 μm) is 50 parts by weight, aluminum hydroxide is 50 parts by weight, the total amount of alumina is 300 parts by weight, the content of alumina 3 (average particle diameter (d50) 80 μm) is 17 wt% and the content of alumina 1 (average particle diameter (d50) 4.6 μm) is 47 wt% in 100 wt% of the total amount of alumina, and there is no acrylic resin coating or PVDC film.
[0052] Example 4 has a surface hardness (Asker C hardness) of 10, a 50% compressive stress of 0.2 MPa, a compression set of 44%, a thermal conductivity of 1.86 W / (m K), tackiness, shape retention of "good", and an overall rating of "good". It is a heat dissipation sheet with low hardness, low compressive stress and recovery properties, and easy installation and workability.
[0053] Comparative Example 1 Comparative Example 1 is an example in which silicone resin 1 (penetration 60) is 0 parts by weight, silicone resin 2 (penetration 85) is 100 parts by weight, the total silicone resin has a penetration of 85, alumina 1 (average particle diameter (d50) 4.6 μm) is 190 parts by weight, alumina 2 (average particle diameter (d50) 55 μm) is 90 parts by weight, alumina 3 (average particle diameter (d50) 80 μm) is 60 parts by weight, aluminum hydroxide is 50 parts by weight, the total amount of alumina is 340 parts by weight, the content of alumina 3 (average particle diameter (d50) 80 μm) is 18 wt% and the content of alumina 1 (average particle diameter (d50) 4.6 μm) is 56 wt% in 100 wt% of the total amount of alumina, and there is no acrylic resin coating or PVDC film.
[0054] Comparative Example 1 had a surface hardness (Asker C hardness) of 10 degrees, a 50% compressive stress of 0.24 MPa, a compression set of 45%, a thermal conductivity of 1.7 W / (m K), tackiness, shape retention of "good", and an overall rating of "poor". Due to the large total amount of alumina, the 50% compressive stress was high (high compressive stress).
[0055] Comparative Example 2 Comparative Example 2 is an example in which the alumina 1 (average particle diameter (d50) 4.6 μm) in Comparative Example 1 is used at 200 parts by weight, the alumina 2 (average particle diameter (d50) 55 μm) at 70 parts by weight, the alumina 3 (average particle diameter (d50) 80 μm) at 100 parts by weight, the total amount of alumina is 370 parts by weight, and the content of alumina 3 (average particle diameter (d50) 80 μm) is 27 wt% and the content of alumina 1 (average particle diameter (d50) 4.6 μm) is 54 wt% out of the total amount of alumina 100 wt%, with the rest being the same as Comparative Example 1.
[0056] Comparative Example 2 had a surface hardness (Asker C hardness) of 11 degrees, a 50% compressive stress of 0.3 MPa, a compression set of 45%, a thermal conductivity of 1.62 W / (m K), tackiness, shape retention of "good", and an overall rating of "poor". The total amount of alumina was high, and the content (wt%) of Alumina 3 (average particle size (d50) 80 μm) was also high, resulting in a high 50% compressive stress (high compressive stress).
[0057] Comparative Example 3 Comparative Example 3 is an example in which the alumina 1 (average particle diameter (d50) 4.6 μm) in Comparative Example 1 is 200 parts by weight, the alumina 2 (average particle diameter (d50) 55 μm) is 120 parts by weight, the alumina 3 (average particle diameter (d50) 80 μm) is 80 parts by weight, the total amount of alumina is 400 parts by weight, the content of alumina 3 (average particle diameter (d50) 80 μm) is 20 wt% and the content of alumina 1 (average particle diameter (d50) 4.6 μm) is 50 wt% out of a total amount of alumina of 100 wt%, and the rest are the same as in Comparative Example 1.
[0058] In Comparative Example 3, the surface hardness (Asker C hardness) was 11 degrees, the 50% compressive stress was 0.27 MPa, the compression set was 47%, the thermal conductivity was 1.86 W / (m K), there was tackiness, the shape retention was "good", and the overall evaluation was "poor". Since the total amount of alumina was high, the 50% compressive stress was high (high compressive stress).
[0059] Comparative Example 4 Comparative Example 4 is an example in which the alumina 1 (average particle diameter (d50) 4.6 μm) in Example 1 is used as 100 parts by weight, the alumina 2 (average particle diameter (d50) 55 μm) as used as 40 parts by weight, the alumina 3 (average particle diameter (d50) 80 μm) as used as 10 parts by weight, the total amount of alumina is 150 parts by weight, the content of alumina 3 (average particle diameter (d50) 80 μm) is 7 wt% and the content of alumina 1 (average particle diameter (d50) 4.6 μm) is 67 wt% out of the total amount of alumina being 100 wt%, and the rest are the same as in Example 1.
[0060] In Comparative Example 4, the surface hardness (Asker C hardness) was 4, the 50% compressive stress was 0.09 MPa, the compression set was 45%, the thermal conductivity was 0.8 W / (m K), there was tackiness, the shape retention was "◎", and the overall rating was "×". Since the total amount of alumina was less than that of Example 1, and the content (wt%) of Alumina 3 (average particle size (d50) 80 μm) was also less, the 50% compressive stress and the thermal conductivity were low, and it is not preferable as a heat dissipation sheet.
[0061] Comparative Example 5 Comparative Example 5 is an example in which the alumina 1 (average particle diameter (d50) 4.6 μm) in Example 1 is 50 parts by weight, the alumina 2 (average particle diameter (d50) 55 μm) is 130 parts by weight, the alumina 3 (average particle diameter (d50) 80 μm) is 50 parts by weight, the total amount of alumina is 230 parts by weight, and the content of alumina 3 (average particle diameter (d50) 80 μm) is 22 wt% and the content of alumina 1 (average particle diameter (d50) 4.6 μm) is 22 wt% out of the total amount of alumina 100 wt%, with the rest being the same as in Example 1.
[0062] Comparative Example 5 had a surface hardness (Asker C hardness) of 11 degrees, a 50% compressive stress of 0.21 MPa, a compression set of 45%, a thermal conductivity of 1.23 W / (m K), tackiness, shape retention of "◎", and an overall rating of "×". The total amount of alumina was greater than that of Example 1, and the content (wt%) of Alumina 3 (average particle size (d50) 80 μm) was also greater, so the 50% compressive stress was high (high compressive stress).
[0063] Example 5 Example 5 is an example having 20 parts by weight of silicone resin 1 (penetration 60), 80 parts by weight of silicone resin 2 (penetration 85), a penetration of the entire silicone resin of 65, 140 parts by weight of alumina 1 (average particle diameter (d50) 4.6 μm), 40 parts by weight of alumina 2 (average particle diameter (d50) 55 μm), 30 parts by weight of alumina 3 (average particle diameter (d50) 80 μm), 50 parts by weight of aluminum hydroxide, a total amount of alumina of 210 parts by weight, alumina 3 (average particle diameter (d50) 80 μm) content of 14 wt% and alumina 1 (average particle diameter (d50) 4.6 μm) content of 67 wt% in a total amount of alumina of 100 wt%, and an acrylic resin coating.
[0064] Example 5 has a surface hardness (Asker C hardness) of 4, a 50% compressive stress of 0.12 MPa, a compression set of 45%, a thermal conductivity of 1.5 W / (m K), no tackiness, shape retention of "◎", and an overall rating of "◎". It is a heat dissipation sheet with low hardness, low compressive stress and recovery properties, and easy installation and workability.
[0065] Example 6 Example 6 is an example in which a PVDC film was laminated on the surface instead of the acrylic resin film in Example 5, and the rest of the configuration was the same as Example 5. Example 6 has a surface hardness (Asker C hardness) of 8, a 50% compressive stress of 0.15 MPa, a compression set of 45%, a thermal conductivity of 1.35 W / (m K), no tackiness, shape retention of "◎", and an overall rating of "◎". It is a heat dissipation sheet with low hardness, low compressive stress and recovery properties, and easy installation and workability.
[0066] Example 7 Example 7 is an example in which the acrylic resin coating in Example 5 was omitted, and the other parts were the same as Example 5. Example 7 has a surface hardness (Asker C hardness) of 4, a 50% compressive stress of 0.12 MPa, a compression set of 45%, a thermal conductivity of 1.5 W / (m K), no tackiness, shape retention of "◎", and an overall rating of "◎". It is a heat dissipation sheet with low hardness, low compressive stress and recovery properties, and easy installation and workability.
[0067] Example 8 Example 8 is an example in which silicone resin 1 (penetration 60) is 0 parts by weight, silicone resin 2 (penetration 85) is 100 parts by weight, the total penetration of the silicone resin is 85, alumina 1 (average particle diameter (d50) 4.6 μm) is 140 parts by weight, alumina 2 (average particle diameter (d50) 55 μm) is 40 parts by weight, alumina 3 (average particle diameter (d50) 80 μm) is 30 parts by weight, aluminum hydroxide is 50 parts by weight, the total amount of alumina is 210 parts by weight, the content of alumina 3 (average particle diameter (d50) 80 μm) is 14 wt% and the content of alumina 1 (average particle diameter (d50) 4.6 μm) is 67 wt% in 100 wt% of the total amount of alumina, and there is no acrylic resin coating or PVDC film.
[0068] Example 8 has a surface hardness (Asker C hardness) of 5, a 50% compressive stress of 0.17 MPa, a compression set of 45%, a thermal conductivity of 1.5 W / (m K), tackiness, shape retention of "good", and an overall rating of "good". It is a heat dissipation sheet with low hardness, low compressive stress and recovery properties, and easy installation and workability.
[0069] Comparative Example 6 Comparative Example 6 is an example in which silicone resin 1 (penetration 60) is 0 parts by weight, silicone resin 2 (penetration 85) is 100 parts by weight, the total silicone resin has a penetration of 85, alumina 1 (average particle diameter (d50) 4.6 μm) is 40 parts by weight, alumina 2 (average particle diameter (d50) 55 μm) is 40 parts by weight, alumina 3 (average particle diameter (d50) 80 μm) is 140 parts by weight, aluminum hydroxide is 50 parts by weight, the total amount of alumina is 220 parts by weight, the content of alumina 3 (average particle diameter (d50) 80 μm) is 64 wt% and the content of alumina 1 (average particle diameter (d50) 4.6 μm) is 18 wt% in 100 wt% of the total amount of alumina, and there is no acrylic resin coating or PVDC film.
[0070] Comparative Example 6 had a surface hardness (Asker C hardness) of 9, a 50% compressive stress of 0.23 MPa, a compression set of 46%, a thermal conductivity of 1.6 W / (m K), tackiness, shape retention of "good", and an overall rating of "poor". Since the content (wt%) of Alumina 3 (average particle size (d50) 80 μm) in the total amount of alumina was high, the 50% compressive stress was high (high compressive stress).
[0071] Comparative Example 7 Comparative Example 7 is an example in which the alumina 1 (average particle diameter (d50) 4.6 μm) in Comparative Example 6 is 40 parts by weight, the alumina 2 (average particle diameter (d50) 55 μm) is 130 parts by weight, the alumina 3 (average particle diameter (d50) 80 μm) is 50 parts by weight, the total amount of alumina is 220 parts by weight, and the content of alumina 3 (average particle diameter (d50) 80 μm) is 23 wt% and the content of alumina 1 (average particle diameter (d50) 4.6 μm) is 18 wt% out of a total amount of alumina of 100 wt%, with the rest being the same as in Comparative Example 6.
[0072] Comparative Example 7 had a surface hardness (Asker C hardness) of 7, a 50% compressive stress of 0.22 MPa, a compression set of 45%, a thermal conductivity of 1.5 W / (m K), tackiness, shape retention of "good", and an overall rating of "poor". Since the content (wt%) of alumina 1 (average particle size (d50) 0.5 to 5 μm) in the total amount of alumina was low, the 50% compressive stress was high (high compressive stress).
[0073] Comparative Example 8 Comparative Example 8 is an example in which the alumina 1 (average particle diameter (d50) 4.6 μm) in Comparative Example 6 is used at 80 parts by weight, the alumina 2 (average particle diameter (d50) 55 μm) at 70 parts by weight, the alumina 3 (average particle diameter (d50) 80 μm) at 70 parts by weight, the total amount of alumina is 220 parts by weight, and the content of alumina 3 (average particle diameter (d50) 80 μm) is 32 wt% and the content of alumina 1 (average particle diameter (d50) 4.6 μm) is 36 wt% out of a total amount of alumina of 100 wt%, with the rest being the same as in Comparative Example 6.
[0074] Comparative Example 8 had a surface hardness (Asker C hardness) of 6, a 50% compressive stress of 0.21 MPa, a compression set of 44%, a thermal conductivity of 1.4 W / (m K), tackiness, shape retention of "x", and an overall rating of "x". Since the content (%) of Alumina 3 (average particle size (d50) 80 μm) in the total amount of alumina was high, the 50% compressive stress was high (high compressive stress).
[0075] Thus, according to the present invention, a heat dissipation sheet having low hardness, low compressive stress and recovery properties, and excellent workability can be obtained. [Explanation of symbols]
[0076] 10.10A heat dissipation sheet 11 Alumina-mixed silicone resin 11A Alumina-mixed silicone resin layer 21A Resin coating
Claims
[Claim 1] Alumina and A heat dissipation sheet comprising a silicone resin, 150 to 300 parts by weight of the alumina is mixed into 100 parts by weight of the silicone resin, The surface hardness of the heat dissipation sheet is 2 to 10 degrees on the Asker C hardness scale; 50% compressive stress (based on ASTM D575-91) is 0.1 to 0.2 MPa, The compression set (C-set, 100°C, 50% compression rate) based on JIS K6262 is 20 to 60%. Heat dissipation sheet.
Citation Information
Patent Citations
Cooling spacer
JP1999087958A
Heat dissipating spacer
JP1999145351A
Low-hardness radiator sheet
JP2002033427A
Thermally conductive silicone composition and thermally conductive silicone molding using the same
JP2011016923A
Silicone elastomer composition
JP2011132376A