Image forming method and image formed product

The image forming method addresses the issue of color density loss in pigment-based inkjet textile printing by forming a protective layer thinner than the coloring material layer, enhancing color density and maintaining fabric texture.

JP7574552B2Active Publication Date: 2024-10-29KONICA MINOLTA INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020108849
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-24
Publication Date
2024-10-29
Estimated Expiration
2040-06-24

AI Technical Summary

Technical Problem

Inkjet textile printing using pigment-based inks often results in coating films with surface irregularities due to dispersible coloring materials, leading to diffuse reflection of light and a decrease in color density.

Method used

An image forming method involving the application of a dispersible coloring material to form a coloring material layer followed by a protective layer with an average thickness thinner than the coloring material layer, using a thin film forming process to reduce surface unevenness and diffuse reflection.

Benefits of technology

The method effectively suppresses the decrease in color density by minimizing surface irregularities and diffuse reflection, maintaining high color density while preserving the fabric's texture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574552000001
    Figure 0007574552000001
  • Figure 0007574552000002
    Figure 0007574552000002
  • Figure 0007574552000003
    Figure 0007574552000003
Patent Text Reader

Abstract

To provide an image formation method that can prevent reduced color density in an article with an image thereon, which is formed with ink including a dispersible colorant.SOLUTION: An image formation method includes the steps of: treating the surface of a fabric with ink including water and a dispersible colorant dispersed therein by an inkjet process to form a colorant layer; and forming, on the surface of the colorant layer, a protective layer that is thinner than the colorant layer in average thickness.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an image forming method and an image formed thereon. [Background technology]

[0002] In recent years, so-called ink-jet printing, in which an image is formed on a fabric by an ink-jet system, has become widespread as a textile printing method because it allows dyeing in a short time and has high production efficiency.

[0003] In inkjet textile printing, minute droplets of ink are ejected from an inkjet recording head and landed on a fabric to form an image. Types of coloring materials contained in inks used in such inkjet textile printing include dyes and pigments.

[0004] In inkjet printing using dye-based inks, the dye contained in the ink dissolves in or reacts with the fibers of the fabric, making it easy to obtain images with high fixability without damaging the texture of the fibers. On the other hand, a process is required to wash away the undissolved or unreacted dye.

[0005] From the viewpoint of omitting such a washing step, inkjet printing using a pigment-based ink has been studied. For example, an inkjet printing method is known in which a pigment-based ink is ejected and adhered onto a fabric by an inkjet method, and then a coating composition is further adhered thereto (for example, Patent Document 1). It is said that the abrasion fastness can be improved by making the Young's modulus of the coating film of the coating composition higher than that of the pigment-based ink. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2019-99790 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, compared to coating films obtained using dye-based inks, coating films obtained using pigment-based inks are more likely to have unevenness on the surface of the coating film due to dispersible colorant particles such as pigments, which can easily cause diffuse reflection of light and reduce color density.

[0008] As in Patent Document 1, a similar problem may occur in an image-formed product having a coating film (colorant layer) of a pigment-based ink and a coating film (protective layer) of a coating composition.

[0009] The present invention has been made in consideration of the above circumstances, and has an object to provide an image forming method and an image formed product that are capable of suppressing a decrease in color density in an image formed product obtained using an ink containing a dispersible colorant. [Means for solving the problem]

[0010] The present invention relates to the following image forming method and image formed product.

[0011] The image forming method of the present invention includes a step of applying an ink containing water and a dispersible colorant dispersed therein to a surface of a fabric by an inkjet method to form a colorant layer, and a step of forming a protective layer on the surface of the colorant layer, the protective layer having an average thickness thinner than that of the colorant layer.

[0012] The image-formed product of the present invention has a fabric, a colorant layer, and a protective layer in this order, the colorant layer containing a dispersible colorant, and the average thickness of the protective layer is thinner than the average thickness of the colorant layer. Effect of the Invention

[0013] According to the present invention, it is possible to provide an image forming method and an image formed product that are capable of suppressing a decrease in color density in an image formed product obtained by using an ink containing a dispersible colorant. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Although Patent Document 1 does not disclose any relationship between the thickness of the color material layer and the thickness of the protective layer, the thickness of the protective layer is generally made thicker than that of the color material layer. In such an image-formed product, the color density is likely to decrease due to diffuse reflection of light on the surface, as in the case where no protective layer is provided.

[0015] In particular, in a colorant layer containing a dispersible colorant such as a pigment, a polymer dispersant, and a binder resin, the smaller the content of the polymer dispersant and the binder resin and the larger the content of the dispersible colorant, the greater the likelihood of the surface irregularities of the colorant layer becoming large, which makes it even more likely that a decrease in color density due to diffuse reflection of light will occur.

[0016] In response to this, the present inventors have newly discovered that the color density of the color material layer can be increased by making the thickness of the protective layer thinner than the thickness of the color material layer.

[0017] The mechanism is not clear, but is presumed to be as follows. If the thickness of the protective layer is thicker than that of the color material layer, the unevenness of the surface of the protective layer is likely to increase (as the thickness increases), and the unevenness of the surface of the protective layer is likely to increase further by being superimposed on the unevenness of the surface of the color material layer. As a result, the unevenness of the surface of the protective layer is likely to cause diffuse reflection of light, the color of the color material layer becomes whitish, and the color density is likely to decrease. In response to this, the unevenness of the surface of the protective layer can be reduced by making the thickness of the protective layer thinner than that of the color material layer. This makes it possible to suppress the decrease in color density. The configuration of the present invention will be described below.

[0018] 1. Image forming method The image forming method of the present invention includes the steps of 1) applying an ink (inkjet printing ink) containing a dispersible colorant and water to the surface of a fabric by an inkjet method to form a colorant layer, and 2) forming a protective layer on the surface of the colorant layer.

[0019] Regarding step 1) (the process of forming the color material layer) First, the fabric is prepared.

[0020] The fiber material constituting the fabric is not particularly limited, and may be natural fibers such as cotton (cellulose fiber), hemp, wool, and silk, or chemical fibers such as rayon, vinylon, nylon, acrylic, polyurethane, polyester, and acetate. The fabric may be any form of fabric made from these fibers, such as woven fabric, nonwoven fabric, knitted fabric, etc. The fabric may also be a blended woven fabric or blended nonwoven fabric of two or more types of fibers. The fabric may be pretreated (see step 3) described below).

[0021] Next, ink is applied to the surface of the fabric by an inkjet method. Specifically, ink is ejected from an inkjet recording head to apply ink droplets.

[0022] The ink is an aqueous ink containing a dispersible colorant such as a pigment and water, as described below. From the viewpoint of increasing the dispersibility of the dispersible colorant, the ink preferably further contains a polymer dispersant or contains a self-dispersible pigment as the dispersible colorant. Details of the composition of the ink will be described later.

[0023] The ink applied to the fabric is then dried and fixed to form a colorant layer.

[0024] The drying and fixing are preferably performed by heating. That is, the drying method is not particularly limited and may be a method using a heater, a hot air dryer, a heating roller, etc. Among them, it is preferable to heat and dry both sides of the fabric using a hot air dryer and a heater.

[0025] The drying temperature is not particularly limited, but from the viewpoint of sufficiently removing solvent components such as water contained in the applied ink, it is preferably 110° C. or higher, and more preferably 130 to 180° C. The drying time varies depending on the drying temperature, but can be, for example, about 0.5 to 10 minutes.

[0026] The resulting colorant layer contains a dispersible colorant and a polymer dispersant and / or a binder resin, and the composition of the colorant layer is the same as the composition of the solid content of the ink described below.

[0027] The average thickness t1 of the coloring layer is not particularly limited as long as it does not impair the texture of the fabric, but is preferably, for example, 0.3 to 1.5 μm. If the average thickness t1 of the coloring layer is 0.3 μm or more, sufficient color density is easily obtained, and if it is 1.5 μm or less, deterioration of the texture due to stiffness is easily suppressed. From the same viewpoint, the average thickness t1 of the coloring layer is more preferably 0.6 to 1 μm.

[0028] The average thickness t1 of the color material layer can be measured by cutting the entire fabric in the cross-sectional direction and observing it with an electron microscope. Specifically, since the thickness of the color material layer differs for each measurement location, samples are taken from the image-formed product at both ends and the center of the sample (for example, at three evenly spaced positions) in the main scanning direction, and at three points (total of nine points) at equal intervals (for example, 5 cm intervals) in the sub-scanning direction. Next, each sample is cut in a direction parallel to the main scanning direction, and the thickness of the colorant layer attached to the fabric at the cut surface is measured, for example, at 10 points in the electron microscope image (total of 90 points), and the average value is taken as the "average thickness t1 of the colorant layer." Note that the main scanning direction is usually the width direction of the image-formed product (or fabric). When cutting in the cross-sectional direction, the sample may be cut in a state cooled with liquid nitrogen in order to prevent the cut surface from being deformed by cutting. This allows for more accurate measurement.

[0029] Regarding step 2) (the process of forming the protective layer) Next, a protective layer is formed on the resulting color material layer.

[0030] The protective layer is preferably transparent from the viewpoint of making the color material layer visible (through the protective layer). Specifically, the transmittance of the protective layer at a wavelength of 400 to 700 nm is preferably 80% or more. The transmittance can be measured by measuring the transmittance of a protective layer of known thickness with a spectrophotometer and converting it into the transmittance of the protective layer at its actual thickness.

[0031] The average thickness t2 of the protective layer is smaller than the average thickness t1 of the color material layer, which reduces the unevenness of the surface of the protective layer caused by the unevenness of the surface of the color material layer, thereby suppressing a decrease in color density due to diffuse reflection of light.

[0032] Specifically, the ratio t2 / t1 of the average thickness t1 of the color material layer to the average thickness t2 of the protective layer is preferably 0.95 or less. When t2 / t1 is 0.95 or less, the surface irregularities of the protective layer can be reduced, so that the decrease in color density due to diffuse reflection of light can be further suppressed. The lower limit of t2 / t1 is not particularly limited, but is preferably 0.1 or more from the viewpoint of suppressing the protective layer from cracking due to friction and increasing the surface irregularities. From the same viewpoint, t2 / t1 is more preferably 0.7 to 0.9. The average thickness t2 of the protective layer can be measured by the same method as described above.

[0033] Such a protective layer is preferably a thin film formed by a thin film forming process (vapor phase method). The thin film may be an inorganic thin film or a resin thin film.

[0034] It is preferable that the inorganic material constituting the inorganic thin film and the resin material constituting the resin thin film have a refractive index higher than that of air (1.0) and lower than that of the dispersible colorant contained in the colorant layer. This not only reduces the unevenness of the surface of the image-formed product, but also reduces the refractive index difference between layers (the refractive index difference between the air layer and the protective layer, and between the protective layer and the colorant layer). This further reduces diffuse reflection of light on the surface of the image-formed product, and further increases color density.

[0035] Specifically, the refractive index of inorganic materials and resin materials at a wavelength of 589.3 nm is preferably 1.2 to 1.9, and more preferably 1.3 to 1.7. When the refractive index of the protective layer is within the above range, the difference in refractive index between the air layer and the protective layer, and the difference in refractive index between the protective layer and the color material layer can be reduced, so that diffuse reflection of light on the surface of the image-formed product can be further reduced and color density can be further increased.

[0036] Furthermore, when the refractive index of light with a wavelength of 589.3 nm of the dispersible colorant contained in the colorant layer is n1, and the refractive index of light with a wavelength of 589.3 nm of the inorganic material or resin material contained in the protective layer is n2, it is preferable that the difference between n1 and n2 (n1-n2) is 0.7 or less.

[0037] The refractive index of the inorganic material or resin material contained in the protective layer and the dispersible colorant contained in the colorant layer can be measured according to JIS K0062:1992.

[0038] The inorganic material may have the above-mentioned refractive index and is not particularly limited, but includes, for example, metal oxides such as silicon dioxide (silica), silicon monoxide, aluminum oxide, and magnesium oxide, and metal fluorides such as magnesium fluoride and calcium fluoride, etc. The resin material may have the above-mentioned refractive index and is not particularly limited, but includes, for example, fluororesins such as PTFE, acrylic resins such as PMMA, olefin resins such as polyethylene, and urethane resins.

[0039] The content of the inorganic material or resin material is preferably 80% by mass or more, and more preferably 90 to 100% by mass, based on the protective layer.

[0040] The protective layer may further contain other components than those described above, as long as the effects of the present invention are not impaired.

[0041] The refractive index of the protective layer or color material layer can be adjusted by the composition. For example, when the protective layer is a thin film made of an inorganic material or a resin material, the refractive index of the protective layer is the same as the refractive index of the inorganic material or the resin material.

[0042] As described above, the method for forming the protective layer is preferably a thin film formation process (gas phase method). Examples of the thin film formation method include PVD methods (physical vapor deposition methods) such as vacuum deposition and sputtering, and CVD methods (chemical vapor deposition methods) such as plasma CVD.

[0043] For example, from the viewpoint of productivity, the vacuum deposition method is preferred. The heating means of the vacuum deposition apparatus used in the vacuum deposition method may be any of an electron beam heating method, a resistance heating method, and an induction heating method. In addition, from the viewpoint of increasing the transparency of the protective layer, reactive deposition may be performed by blowing in oxygen gas during deposition.

[0044] The image forming method of the present invention may further include the step 3) of pretreating the fabric, if necessary.

[0045] Regarding step 3 (pre-processing step) The pretreatment can be carried out by applying a pretreatment agent to the fabric.

[0046] The pretreatment agent is not particularly limited as long as it contains a component that enhances the fixation of the ink to the surface of the fabric. Examples of such components include compounds having an anionic group (e.g., a carboxyl group, a phosphoric acid group, a phosphonic acid group, a sulfonic acid group, etc.) and compounds having a cationic group (e.g., an amino group, a quaternary ammonium group, etc.).

[0047] Examples of the compound having a cationic group include polyvalent metal salts, resins having a cationic group (such as cationic urethane resins and cationic olefin resins), and cationic surfactants.

[0048] Examples of compounds having an anionic group include resins having an anionic group (for example, plant skins such as pectinic acid, cellulose derivatives such as carboxymethyl cellulose, modified starches such as carboxymethyl starch and carboxyethyl starch, acrylic polymers having acrylic acid as a copolymerization component such as acrylic acid-acrylic acid ester copolymers and styrene-acrylic acid copolymers), and anionic surfactants.

[0049] The pretreatment agent may further contain, as necessary, a pH adjuster, a preservative, etc. As the preservative, the same preservatives as those exemplified for the ink can be used.

[0050] The method for applying the pretreatment agent to the fabric is not particularly limited, and may be, for example, a pad method, a coating method, a spray method, or an inkjet method.

[0051] The pretreatment agent applied to the fabric may be heated and dried using hot air, a hot plate, or a heat roller.

[0052] Next, the composition of the ink used in the image forming method of the present invention will be described.

[0053] 2. Ink The ink contains a dispersible colorant and water.

[0054] 2-1. Dispersible coloring material The dispersible colorant is not particularly limited and may be a solid dye such as a disperse dye or a pigment. Among them, a pigment is preferred from the viewpoint of facilitating the formation of an image having excellent weather resistance.

[0055] (Pigments) The pigment is not particularly limited, but may be, for example, an organic or inorganic pigment having the following numbers as described in the Color Index:

[0056] Examples of red or magenta pigments include Pigment Red 3, 5, 19, 22, 31, 38, 43, 48:1, 48:2, 48:3, 48:4, 48:5, 49:1, 53:1, 57:1, 57:2, 58:4, 63:1, 81, 81:1, 81:2, 81:3, 81:4, 88, 104, 108, 112, 122, 123, 144, 146, 149, 166, 168, 169, 170, 177, 178, 179, 184, 185, 208, 216, 226, 257, Pigment Violet 3, 19, 23, 29, 30, 37, 50, 88, Pigment Orange 13, 16, 20, 36.

[0057] Examples of blue or cyan pigments include Pigment Blue 1, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 17-1, 22, 27, 28, 29, 36, 60.

[0058] Examples of green pigments include Pigment Green 7, 26, 36, and 50. Examples of yellow pigments include Pigment Yellow 1, 3, 12, 13, 14, 17, 34, 35, 37, 55, 74, 81, 83, 93, 94, 95, 97, 108, 109, 110, 137, 138, 139, 153, 154, 155, 157, 166, 167, 168, 180, 185, and 193.

[0059] Examples of black pigments include Pigment Black 7, 28, and 26.

[0060] Commercially available examples of pigments include: Chromofine Yellow 2080, 5900, 5930, AF-1300, 2700L, Chromofine Orange 3700L, 6730, Chromofine Scarlet 6750, Chromofine Magenta 6880, 6886, 6891N, 6790, 6887, Chromofine Violet RE, Chromofine Red 6820, 6830, Chromofine Blue HS-3, 5187, 5108, 5197, 5085N, SR-5020, 5026, 5050, 4920, 4927, 4937, 4824, 4933GN-EP, 4940, 4973, 5205, 5208, 5214, 5221, 5000P , Chrome Fine Green 2GN, 2GO, 2G-550D, 5310, 5370, 6830, Chrome Fine Black A-1103, Seika Fast Yellow 10GH, A-3, 2035, 2054, 2200, 2270, 2300, 2400(B), 2500, 2600, ZAY-260, 2700(B), 2770 , Seika Fast Red 8040, C405(F), CA120, LR-116, 1531B, 8060R, 1547, ZAW-262, 1537B, GY, 4R-4016, 3820, 3891, ZA-215, Seika Fast Carmine 6B1476T-7, 1483LT, 3840, 3870, Seika Fast Bordeaux 10B-430, Seika Light Rose R40, Seika Light Violet B800, 7805, Seika Fast Maroon 460N, Seika Fast Orange 900, 2900, Seika Light Blue C718, A612, Cyanine Blue 4933M, 4933GN-EP, 4940, 4973 (Dainichi Seika Chemicals); KET Yellow 401, 402, 403, 404, 405, 406, 416, 424, KET Orange 501, KET Red 301, 302, 303, 304, 305, 306, 307, 308, 309, 310, 336, 337, 338, 346, KET Blue 101, 102, 103, 104, 105, 106, 111, 118, 124, KET Green 201 (manufactured by Dainippon Ink & Chemicals);Colortex Yellow 301, 314, 315, 316, P-624, 314, U10GN, U3GN, UNN, UA-414, U263, Finecol Yellow T-13, T-05, Pigment Yellow1705, Colortex Orange 202, Colortex Red101, 103, 115, 116, D3B, P-625, 102, H-1024, 105C, UFN, UCN, UBN, U3BN, URN, UGN, UG276, U456, U457, 105C, USN, Colortex Maroon601, Colortex BrownB610N, Colortex Violet600, Pigment Red 122, Colortex Blue516, 517, 518, 519, A818, P-908, 510, Colortex Green 402, 403, Colortex Black 702, U905 (Sanyo Pigment); Lionol Yellow 1405G, Lionol Blue FG7330, FG7350, FG7400G, FG7405G, ES, ESP-S (Toyo Ink Co., Ltd.); Toner Magenta E02, Permanent Rubin F6B, Toner Yellow HG, Permanent Yellow GG-02, Hostapearm Blue B2G (Hoechst Industry); Novoperm P-HG, Hostaperm Pink E, Hostaperm Blue B2G (manufactured by Clariant); Carbon black #2600, #2400, #2350, #2200, #1000, #990, #980, #970, #960, #950, #850, MCF88, #750, #650, MA600, MA7, MA8, MA11, MA100, MA100R, MA77, #52, #50, #47, #45, #45L, #40, #33, #32, #30, #25, #20, #10, #5, #44, CF9 (manufactured by Mitsubishi Chemical).

[0061] (self-dispersing pigment) The pigment may be a self-dispersing pigment. A self-dispersing pigment is a pigment particle whose surface is modified with a group having a hydrophilic group, and has pigment particles and hydrophilic groups bonded to the surface of the pigment particles.

[0062] Examples of hydrophilic groups include carboxyl groups, sulfonic acid groups, and phosphorus-containing groups. Examples of phosphorus-containing groups include phosphoric acid groups, phosphonic acid groups, phosphinic acid groups, phosphite groups, and phosphate groups.

[0063] Commercially available examples of self-dispersing pigments include Cabot's Cab-0-Jet® 200K, 250C, 260M, and 270V (sulfonic acid group-containing self-dispersing pigments), Cab-0-Jet® 300K (carboxylic acid group-containing self-dispersing pigments), and Cab-0-Jet® 400K, 450C, 465M, 470V, and 480V (phosphate group-containing self-dispersing pigments).

[0064] The content of the dispersible colorant is not particularly limited, but from the viewpoint of easily adjusting the viscosity of the ink within the above range and enabling the formation of a high-density image, it is preferably 1.5 to 15% by mass relative to the ink. If the content of the dispersible colorant is 1.5% by mass or more, a high-density image is easily formed, and if it is 15% by mass or less, the viscosity of the ink does not become too high, so that ejection stability is not easily impaired. From the same viewpoint, the content of the dispersible colorant is more preferably 5 to 15% by mass relative to the ink.

[0065] 2-2.Other ingredients The ink may further contain other components as necessary, such as a solvent other than water, a polymer dispersant, a binder resin, a preservative, and a pH adjuster.

[0066] (solvent) The solvent is not particularly limited, but is preferably a water-soluble organic solvent. The water-soluble organic solvent is not particularly limited as long as it is compatible with water, but from the viewpoint of making it easier for the ink to penetrate into the interior of the fabric and from the viewpoint of making it difficult to impair the ejection stability in the inkjet method, it is preferable that the ink does not easily thicken due to drying. Therefore, it is preferable that the ink contains a high-boiling point solvent with a boiling point of 200°C or more.

[0067] The high-boiling solvent having a boiling point of 200° C. or higher may be any water-soluble organic solvent having a boiling point of 200° C. or higher, and is preferably a polyol or a polyalkylene oxide.

[0068] Examples of polyols having a boiling point of 200°C or higher include dihydric alcohols such as 1,3-butanediol (boiling point 208°C), 1,6-hexanediol (boiling point 223°C), and polypropylene glycol; and trihydric or higher alcohols such as glycerin (boiling point 290°C) and trimethylolpropane (boiling point 295°C).

[0069] Examples of polyalkylene oxides having a boiling point of 200° C. or higher include ethers of dihydric alcohols such as diethylene glycol monoethyl ether (boiling point 202° C.), triethylene glycol monomethyl ether (boiling point 245° C.), tetraethylene glycol monomethyl ether (boiling point 305° C.), tripropylene glycol monoethyl ether (boiling point 256° C.) and polypropylene glycol, and ethers of trihydric or higher alcohols such as glycerin (boiling point 290° C.) and hexanetriol.

[0070] The solvent may further include a solvent other than the high boiling point solvent. As the other solvent, the same solvents as those exemplified as the solvents included in the pretreatment agent can be used.

[0071] (Polymer dispersant) When the pigment is not a self-dispersing pigment, from the viewpoint of facilitating dispersion of the pigment, it is preferable that the ink further contains a polymer dispersant.

[0072] The type of polymer dispersant is not particularly limited, and may be any of a cationic dispersant, an anionic dispersant, and a nonionic dispersant.

[0073] Examples of the cationic group contained in the cationic dispersant include a secondary amino group (imino group), a tertiary amino group, or a quaternary ammonium group.

[0074] Such a cationic dispersant may be any that can form a pigment dispersion, and is not particularly limited. Examples of such a cationic dispersant include acrylic (co)polymers having a cationic group (a tertiary amino group or a quaternary ammonium group).

[0075] The anionic dispersant is a polymeric dispersant having a hydrophilic group selected from the group consisting of a carboxylic acid group, a phosphorus-containing group, and a sulfonic acid group.

[0076] Examples of the polymer dispersant having a carboxylic acid group include polycarboxylic acids or their salts. Examples of the polycarboxylic acids include (co)polymers of monomers selected from acrylic acid or its derivatives, maleic acid or its derivatives, itaconic acid or its derivatives, and fumaric acid or its derivatives, and salts thereof.

[0077] The polymeric dispersant having a phosphorus-containing group is a polymeric dispersant having a phosphoric acid group or a phosphonic acid group. Examples of the polymeric dispersant having a phosphoric acid group or a phosphonic acid group include alkyl phosphoric acid esters or salts thereof.

[0078] Examples of polymeric dispersants having sulfonic acid groups include formalin condensates of aromatic sulfonic acids and formalin condensates of lignin sulfonic acids, and preferably formalin condensates of aromatic sulfonic acids. Examples of formalin condensates of aromatic sulfonic acids include sodium condensed naphthalene sulfonate.

[0079] Examples of non-ionic dispersants include polyoxyalkylenes, polyoxyalkylene alkyl ethers, and the like.

[0080] The content of the polymer dispersant is preferably 10 to 50% by mass relative to the dispersible colorant. When the content of the polymer dispersant is 10% by mass or more, the dispersibility of the dispersible colorant is easily increased sufficiently, and when the content is 50% by mass or less, an excessive increase in viscosity is easily suppressed. From the same viewpoint, the content of the polymer dispersant is preferably 20 to 40% by mass relative to the dispersible colorant.

[0081] (binder resin) The binder resin can be a water-soluble resin or resin particles (water-dispersible resin).

[0082] The weight average molecular weight of the binder resin may be equal to or greater than 10,000. The weight average molecular weight can be measured by a GPC method in terms of polystyrene.

[0083] However, from the viewpoint of preventing the texture of the fabric from being damaged, it is preferable that the content ratio of the polymer dispersant and the binder resin is low. On the other hand, if the content ratio is low, the content ratio of the dispersible colorant is high, and the unevenness of the surface of the colorant layer is likely to become large. In such a case, the present invention is particularly effective.

[0084] Specifically, the ratio of the total content of the polymer dispersant and the binder resin to the content of the dispersible colorant is preferably 1.5 or less, and more preferably 1.2 or less, in mass ratio.

[0085] (Preservatives, pH adjusters) As the preservatives and pH adjusters, the same preservatives and pH adjusters as those given as specific examples of the preservatives and pH adjusters optionally contained in the pretreatment agent can be used.

[0086] 2-3.Physical properties The viscosity of the ink at 25°C is not particularly limited as long as it provides good ejection properties using an inkjet method, but is preferably 3 to 20 mPa s, and more preferably 4 to 12 mPa s. The viscosity of the ink can be measured at 25°C using an E-type viscometer.

[0087] 2-4. Preparation of ink The ink can be produced by any method, for example, by mixing the dispersible colorant, water, any dispersant, and the like.

[0088] 3. Image formation The image-formed product obtained by the image-forming method of the present invention has a fabric, a colorant layer, and a protective layer.

[0089] As described above, the average thickness t2 of the protective layer is smaller than the average thickness t1 of the color material layer. Specifically, t2 / t1 satisfies the above range. This makes it possible to reduce the unevenness of the surface of the image-formed product caused by the unevenness of the surface of the color material layer, and to suppress the decrease in color density caused by diffuse reflection of light. EXAMPLES

[0090] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these.

[0091] 1. Ink materials (1) Dispersible colorants (pigments) Pigment Red 122 (Refractive index of light with a wavelength of 589.3 nm: 2.0)

[0092] (2) Polymer dispersants Styrene-acrylic copolymer (anionic dispersant, weight average molecular weight 16000)

[0093] (3) Solvent Ethylene glycol (boiling point 197.6℃) Glycerin (boiling point 290℃) Propylene glycol (boiling point 188.2℃)

[0094] <Preparation of Inks 1 to 4> The components shown in Table 1 were mixed to obtain the compositions shown in Table 1, thereby obtaining inks 1 to 4. [Table 1]

[0095] 2. Imaging and Evaluation <Tests 1-20, 23-29> (1) Pretreatment The following fabrics 1 to 3 were prepared. Fabric 1: 100% polyester fabric Fabric 2: 100% cotton fabric Fabric 3: 50% cotton and 50% polyester blend

[0096] Next, a pretreatment agent containing 3 parts by mass of styrene-acrylic acid copolymer (anionic pretreatment agent) and 97 parts by mass of water was applied to the surface of the fabric by immersion, and then the fabric was squeezed and dried for pretreatment.

[0097] (2) Formation of colorant layer Next, an inkjet printer having an inkjet head (Konica Minolta head KM1024iMAE) was prepared as an image forming apparatus. Then, the inks shown in Table 2 or 3 were ejected from the nozzles of the inkjet head to form a solid image on the pretreated fabric so that the average thickness of the resulting color material layer was the value shown in Table 2. Specifically, a solid image (200 mm x 200 mm) was formed at 540 dpi in the main scan direction and 720 dpi in the sub-scan direction. dpi refers to the number of ink droplets (dots) per 2.54 cm. The ejection frequency was 22.4 kHz.

[0098] Thereafter, the fabric on which the solid image was formed was dried for 3 minutes at 150° C. in a belt conveying dryer, thereby obtaining a colorant layer having an average thickness shown in Table 2 or 3.

[0099] (3) Formation of a protective layer The fabric on which the colorant layer was formed was set in a vacuum deposition apparatus OTFC-1300 (manufactured by Optran Co., Ltd.), and a protective layer was formed by vacuum deposition of the materials shown in Table 2 or 3 so that the average thickness of the resulting protective layer would be the value shown in Table 2 or 3. In this way, an image-formed product having (pretreated) fabric / colorant layer / protective layer was obtained.

[0100] <Test 21> An image-formed product was obtained in the same manner as in Test 1, except that the protective layer was formed by sputtering using a sputtering apparatus NSC-15 (manufactured by Optolan Co., Ltd.).

[0101] <Test 22> An image-formed product was obtained in the same manner as in Test 1, except that the protective layer was formed by a plasma CVD method using a plasma CVD apparatus CME-200E (manufactured by ULVAC, Inc.).

[0102] <Tests 30 and 31> First, the following components were mixed to prepare a composition for a protective layer. (composition) Urethane resin: 5 parts by weight Ethylene glycol: 30 parts by weight Ion-exchanged water: 65 parts by weight Next, the obtained composition was applied onto the colorant layer by the method shown in Table 2, and then dried at 150° C. in the same manner as in Test 1 to obtain an image-formed product.

[0103] <Test 32> An image formed was obtained in the same manner as in Test 1, except that no protective layer was formed.

[0104] <Thickness measurement> The average thickness t1 of the color material layer of the image-formed products obtained in Tests 1 to 32 was measured by the following method. Specifically, the obtained image-formed product was sampled at both ends and the center (three evenly spaced positions) in the main scanning direction, and at three points (total of nine points) at equal intervals (5 cm intervals) in the sub-scanning direction. Then, each sample was cut in a direction parallel to the main scanning direction, and the thickness of the colorant layer attached to the fabric on the cut surface was measured at 10 points from the electron microscope image (total of 90 points), and the average value was taken as the "average thickness t1 of the colorant layer." The main scanning direction was the width direction of the image-formed product. The average thickness t2 of the protective layer was also measured in the same manner.

[0105] <Evaluation> The image-formed products obtained in Tests 1 to 32 were evaluated for color density and texture of the images by the following methods.

[0106] (color density) The color density of the image formed was evaluated sensorily by observing the change in density before and after providing the protective layer, and was evaluated based on the following evaluation criteria. ◎: A clear improvement in density was observed before and after the protective layer was installed ○: Concentration improvement can be confirmed ×: No improvement in concentration was observed or the concentration decreased If it was ○ or above, it was judged to be good.

[0107] (Texture) The texture of the image-formed product and the fabric obtained was evaluated sensorily by touching with the fingers, based on the following criteria. ◎: Maintains the original softness of the fabric ○: The original softness of the fabric has been lost and it has become a little stiff, but the texture of the fabric is not lost. ×: The fabric is harder than it should be, and the texture of the fabric is lost. If it was equal to or greater than ○, it was considered to be within the acceptable range.

[0108] The evaluation results of tests 1 to 20 are shown in Table 2, and the evaluation results of tests 21 to 32 are shown in Table 3. The refractive index of each material was measured according to JIS K0062: 1992. The light transmittance of the protective layer at wavelengths of 400 to 700 nm was measured using a spectrophotometer V-550 (manufactured by JASCO Corporation) and was 80% or more in all cases.

[0109] [Table 2]

[0110] [Table 3]

[0111] As shown in Tables 2 and 3, the image formation products (invention) of Tests 1 to 25, in which the average thickness of the protective layer was thinner than the average thickness of the colorant layer, all showed less diffuse reflection of light on the surface of the colorant layer and higher color density.

[0112] In contrast, as shown in Table 3, the image formation products (comparison examples) of Tests 26 to 31, in which the average thickness of the protective layer was made thicker than the average thickness of the color material layer, and the image formation product of Test 32, in which no protective layer was provided, all showed significant diffuse reflection of light on the surface of the color material layer and low color density.

[0113] According to the present invention, it is possible to provide an image forming method and an image formed product that are capable of suppressing a decrease in color density in an image formed product obtained by using an ink containing a dispersible colorant.

Claims

1. A step of applying an ink containing water and a dispersible colorant dispersed therein to a surface of a fabric by an inkjet method to form a colorant layer; forming a protective layer on the surface of the color material layer, the protective layer having an average thickness smaller than that of the color material layer; Including, The thickness of the color material layer is 0.3 to 1 μm, the protective layer includes an inorganic material or a resin material, When the average thickness of the color material layer is t1 and the average thickness of the protective layer is t2, t2 / t1 is 0.8 or less; Image forming method.

2. The protective layer has a transmittance of 80% or more for light having a wavelength of 400 to 700 nm. The image forming method according to claim 1 .

3. t2 / t1 is 0.7 to 0.8; The image forming method according to claim 1 or 2.

4. the refractive index of the inorganic material or resin material for light having a wavelength of 589.3 nm is higher than the refractive index of air for light having a wavelength of 589.3 nm, and is lower than the refractive index of the dispersible colorant for light having a wavelength of 589.3 nm; The image forming method according to any one of claims 1 to 3.

5. The refractive index of the inorganic material or the resin material at a wavelength of 589.3 nm is 1.7 or less. The image forming method according to claim 4.

6. The ink further includes at least one of a polymer dispersant and a binder resin, The total content of the polymer dispersant and the binder resin is 1.5 or less in terms of mass ratio to the content of the dispersible colorant. The image forming method according to any one of claims 1 to 5.

7. The protective layer includes the inorganic material. The image forming method according to any one of claims 1 to 6.

8. A method for producing a colorant layer by applying an ink containing water and a dispersible colorant dispersed therein to a surface of a fabric by an inkjet method; forming a protective layer on the surface of the color material layer, the protective layer having an average thickness smaller than that of the color material layer; Including, the protective layer includes an inorganic material or a resin material, The protective layer is formed by a thin film formation process using a vapor phase method, When the average thickness of the color material layer is t1 and the average thickness of the protective layer is t2, t2 / t1 is 0.8 or less; Image forming method.

9. A step of applying an ink containing water and a dispersible colorant dispersed therein to a surface of a fabric by an inkjet method to form a colorant layer; forming a protective layer having an average thickness smaller than that of the color material layer on a surface of the color material layer by a vacuum deposition method; Including, Image forming method.

10. An image-formed product having a fabric, a color material layer, and a protective layer in this order, The color material layer contains a dispersible color material, The thickness of the color material layer is 0.3 to 1 μm, the average thickness of the protective layer is smaller than the average thickness of the color material layer, the protective layer includes an inorganic material or a resin material, When the average thickness of the color material layer is t1 and the average thickness of the protective layer is t2, t2 / t1 is 0.8 or less; Image formation.

11. The protective layer has a transmittance of 80% or more for light having a wavelength of 400 to 700 nm. The image-formed product according to claim 10.

12. t2 / t1 is 0.7 to 0.8; The image-formed product according to claim 10 or 11.

13. the refractive index of the inorganic material or resin material for light having a wavelength of 589.3 nm is higher than the refractive index of air for light having a wavelength of 589.3 nm, and is lower than the refractive index of the dispersible colorant for light having a wavelength of 589.3 nm; The image-formed product according to any one of claims 10 to 12.

14. the color material layer further contains at least one of a polymer dispersant and a binder resin; The total content of the polymer dispersant and the binder resin is 1.5 or less in terms of mass ratio to the content of the dispersible colorant. The image-formed product according to any one of claims 10 to 13.

Citation Information

Patent Citations

  • Leather-like sheet

    EP0904950A1

  • Leather-like sheet

    JP1999158782A

  • Ink set for inkjet printing

    JP2010150453A

  • Ink set for inkjet printing

    JP2010150454A

  • Coating liquid for inkjet printing

    JP2011183770A