Manufacturing method for semiconductor package substrate

The method addresses short circuits and connection reliability issues in semiconductor package substrates by using a support structure with precise reference surfaces and resin layers to form aligned copper pillars, ensuring reliable connections and mechanical strength with minimal solder.

JP7574560B2Active Publication Date: 2024-10-29TOPPAN HOLDINGS INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020126198
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-27
Publication Date
2024-10-29
Estimated Expiration
2040-07-27

AI Technical Summary

Technical Problem

Existing semiconductor package substrates face issues with short circuits and connection reliability due to reduced solder amounts, leading to open defects and weakened mechanical strength, especially with finer pitches and copper pillars.

Method used

A manufacturing method involving a support structure with precise reference surfaces and resin layers to form connection terminals, ensuring consistent solder connections and mechanical strength, using a multilayer wiring board with aligned copper pillars and underfill resin.

Benefits of technology

Ensures reliable connections and mechanical strength with minimal solder, preventing open defects and enhancing the reliability of semiconductor package substrates even at narrow pitches.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574560000001
    Figure 0007574560000001
  • Figure 0007574560000002
    Figure 0007574560000002
  • Figure 0007574560000003
    Figure 0007574560000003
Patent Text Reader

Abstract

To provide a rewiring board, a manufacturing method of a semiconductor package board, and a semiconductor package board that suppress open defects due to variations in the amount of solder and ensures connection reliability and mechanical strength even with a small amount of solder.SOLUTION: A rewiring board 10 includes a support 21, a peeling layer formed on one side of the support 21 and provided with a first reference plane S1, a wiring layer formed adjacent to the peeling layer and provided with a plurality of connection terminals, and a resin layer 25 formed on the side of the other surface of the support 21 and provided with a second reference plane S2 parallel to the first reference plane S1, and the end face of the connection terminal facing the support 21 has the same distance from the second reference plane S2, and after connecting a main board 1 and the rewiring board 10, the support 21 is deleted to obtain a more compact semiconductor package board 100.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention ,half How to manufacture a conductive package substrate By law Regarding. [Background technology]

[0002] As the technology node of semiconductor chips advances year by year, there is a demand for narrower pitches between terminals of semiconductor chips, and there is also a demand for finer and narrower pitches between terminals in semiconductor package substrates on which semiconductor chips are mounted.Here, microbumps connected by solder are often used in the connection terminal structure between the semiconductor chip and the semiconductor package substrate (see Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2004-47510 A [Patent Document 2] JP 2014-203963 A Summary of the Invention [Problem to be solved by the invention]

[0004] According to the microbumps disclosed in Patent Documents 1 and 2, the solder for connecting the semiconductor chips has a drum shape, so if the terminals are arranged with a narrower pitch, there is a problem that short circuits are more likely to occur between the solder of adjacent terminals. If the amount of solder is reduced to prevent this short circuit, it will not be possible to ensure a gap between the semiconductor chip and the semiconductor package substrate, which will lead to a deterioration in the injectability of the underfill resin. For this reason, a copper pillar is used in the terminal structure to accommodate the miniaturization of semiconductor chips, ensuring a gap and preventing poor injection of the underfill resin even with a small amount of solder.

[0005] However, reducing the amount of solder narrows and reduces the solder margin relative to the copper pillar variations, which may lead to localized open defects (connection defects). In addition, when using thin copper pillars, the amount of solder placed on the top of the small-diameter copper pillar is reduced. The solder layer is generally softer than the IMC (Intermetallic Layer) that is alloyed with the solder, and therefore has the function of absorbing mechanical shocks. However, the longer the melting time at high temperatures, the thinner the solder layer tends to become, which causes the problem of weakening the mechanical strength of the connection surface.

[0006] The present invention suppresses open defects caused by variations in the amount of solder, and can ensure connection reliability and mechanical strength even with a small amount of solder. Half How to manufacture a conductive package substrate Law The purpose is to provide. [Means for solving the problem]

[0008] In order to solve the above problems, one of the representative methods for manufacturing a semiconductor package substrate of the present invention is to A step of forming a first reference surface by grinding one surface of a support formed from a glass plate; The above First reference plane On top forming a release layer; On the other side of the support forming a resin layer, and grinding the resin layer based on the first reference surface, A second reference plane parallel to the first reference plane of forming a laminating the release layer to form a resin pattern layer having openings; forming a plurality of connection terminals in the openings of the resin pattern layer such that inner end surfaces of the connection terminals are in contact with the first reference surface; removing a portion of the resin pattern layer to expose the vicinity of an outer end surface of the connection terminal; a step of connecting an outer end surface of the connection terminal to a wiring terminal of a main board by soldering; filling an underfill resin around the connected connection terminal; removing the support and the release layer; and removing the remainder of the resin pattern layer. In addition, since it is difficult to directly specify the semiconductor package substrate of the present invention based on its structure or characteristics, the structure itself is specified based on the manufacturing method of the structure, and there are impossible or impractical circumstances. Effect of the Invention

[0009] According to the present invention, it is possible to suppress open defects caused by variations in the amount of solder, and to ensure connection reliability and mechanical strength even with a small amount of solder. Half How to manufacture a conductive package substrate Law can be provided. Problems, configurations and effects other than those described above will become apparent from the following description of the embodiments. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a cross-sectional view of a main board according to the present embodiment. [Diagram 2] FIG. 2 is a cross-sectional view of the rewiring substrate according to the present embodiment. [Diagram 3] 3A to 3C are cross-sectional views showing the steps of producing a rewiring substrate according to this embodiment. [Figure 4] 4A to 4C are cross-sectional views showing the steps of producing a rewiring substrate according to this embodiment. [Diagram 5] FIG. 5 is a cross-sectional view showing a process for producing a rewiring substrate according to this embodiment. [Figure 6] FIG. 6 is a cross-sectional view showing a process for producing a rewiring substrate according to this embodiment. [Figure 7] 7A to 7C are cross-sectional views showing the steps of manufacturing the rewiring substrate according to this embodiment. [Figure 8] FIG. 8 is a cross-sectional view showing a process for producing a rewiring substrate according to this embodiment. [Figure 9] FIG. 9 is a cross-sectional view showing a process for producing a rewiring substrate according to this embodiment. [Figure 10] 10A to 10C are cross-sectional views showing the steps of manufacturing the rewiring substrate according to this embodiment. [Figure 11] FIG. 11 is a cross-sectional view showing a process for producing a rewiring substrate according to this embodiment. [Figure 12] 12A to 12C are cross-sectional views showing the steps of manufacturing the rewiring substrate according to this embodiment. [Figure 13] FIG. 13 is a cross-sectional view showing a process of connecting the rewiring board and the main board according to the present embodiment. [Figure 14] FIG. 14 is a cross-sectional view showing a process of connecting the rewiring board and the main board according to the present embodiment. [Figure 15] FIG. 15 is a cross-sectional view showing a semiconductor package substrate according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] An embodiment of the present invention is described below.

[0012] In this disclosure, the term "surface" may refer not only to the surface of a plate-shaped member, but also to the interface of a layer contained in the plate-shaped member that is approximately parallel to the surface of the plate-shaped member. Additionally, the terms "upper surface" and "lower surface" refer to the surface shown at the top or bottom of a drawing of a plate-shaped member or a layer contained in the plate-shaped member. The term "side surface" refers to a surface of a plate-like member or a layer included in a plate-like member, or a portion of the thickness of a layer. Furthermore, a part of a surface and a side surface may be collectively referred to as an "end portion." In addition, "upper" refers to the vertically upward direction when a plate-like member or layer is placed horizontally. Furthermore, "upper" and its opposite, "lower", are sometimes referred to as the "Z-axis direction", and the horizontal direction is sometimes referred to as the "X-axis direction" or the "Y-axis direction". Additionally, the terms "planar shape" and "plan view" refer to the shape of a surface or layer when viewed from above. Furthermore, the terms "cross-sectional shape" and "cross-sectional view" refer to the shape of a plate-like member or layer when cut in a specific direction and viewed from the horizontal direction. Furthermore, the term "central portion" refers to the central portion other than the peripheral portion of the surface or layer, and the term "toward the center" refers to the direction from the peripheral portion of the surface or layer toward the center of the planar shape of the surface or layer.

[0013] In addition, the embodiments shown below are merely examples of devices and methods for embodying the technical idea of ​​the present invention, and the technical idea of ​​the present invention does not specify the materials, shapes, structures, arrangements, etc. of the components to those described below. The technical idea of ​​the present invention can be modified in various ways within the technical scope defined by the claims.

[0014] The semiconductor package substrate of this embodiment is produced by producing a main substrate and a rewiring substrate in separate processes, soldering the corresponding rewiring substrate onto the main substrate, and bonding them by injecting underfill resin.

[0015] In this embodiment, the wiring scale of the rewiring substrate is L / S (wiring / space) = 0.5 μm / 0.5 μm to L / S = 10 μm / 10 μm (in other words, 0.5 μm≦L≦10 μm, 0.5 μm≦S≦10 μm), the wiring scale of the main substrate is L / S = 10 μm / 10 μm or more, and rigidity is ensured by using an insulating resin material containing glass cloth for the main substrate.

[0016] Furthermore, due to the characteristics of insulating resin materials containing glass cloth, the unevenness of the woven glass cloth fibers affects the surface of the insulating resin material, so that it is generally difficult to achieve the above-mentioned fine wiring scale of L / S=0.5 μm / 0.5 μm to L / S=10 μm / 10 μm on this insulating resin material, and insulating resins containing glass cloth cannot be used as is. Therefore, in this embodiment, in the manufacturing process of the rewiring substrate, which is manufactured separately from the main substrate, a rigid support is used to form the rewiring substrate (also called an interposer), thereby ensuring the rigidity of the rewiring substrate throughout the entire process and thereby realizing ease of manufacturing. In addition, after the main substrate and the rewiring substrate are connected, the support is removed to obtain a more compact semiconductor package substrate.

[0017] The main substrate is manufactured in the same manner as a flip-chip type semiconductor package substrate, which has a core made of a typical insulating resin material containing glass cloth.

[0018] <Main board and its manufacturing method> An example of a method for manufacturing the main substrate will now be described in detail.

[0019] (Line pattern formation) First, through holes 11a are drilled with a 150 μm diameter drill at predetermined positions in an 800 μm glass epoxy substrate (core substrate) 11, and an electroless copper plating layer 12 is formed on the exposed surface of the glass epoxy substrate 11 by electroless copper plating. The inside of the through holes 11a is then electrolytically copper plated to form an electrolytic copper plating layer 12a. Electrical connections are made between the front and back surfaces of the glass epoxy substrate 11 via the electrolytic copper plating layer 12a. If necessary, the electroless copper plating layer 12 and the electrolytic copper plating layer 12a are etched by a subtractive method to form a line pattern.

[0020] (Formation of interlayer insulating resin layer) Next, a 40 μm-thick resin (product name GX-T31) manufactured by Ajinomoto Fine-Techno Co., Ltd. is vacuum laminated onto the copper line pattern as the main board interlayer insulating resin 13. Furthermore, a UV laser device is used to align with the underlying copper line pattern and open holes 13a arranged in a matrix with an opening diameter of 70 μm and a pitch of 150 μm between adjacent holes.

[0021] (Copper wiring formation of interlayer insulating resin) Furthermore, 1 μm-thick electroless copper plating is applied onto the interlayer insulating resin 13, and then a dry film resist pattern with openings for line patterns is formed using a dry film resist (product name RY-5325) manufactured by Hitachi Chemical Co., Ltd., followed by 15 μm-thick electrolytic copper plating. The unnecessary dry film resist is peeled off with a 20% monoethanolamine aqueous solution, and the exposed 1 μm-thick electroless copper plating layer is etched with a sulfuric acid / hydrogen peroxide-based etching solution to produce independent copper wiring 14. The copper wiring 14 is then encapsulated with resin to form the wiring layer 15.

[0022] (Lamination of copper wiring and interlayer insulating resin) Furthermore, by alternately laminating wiring layers 15 and interlayer insulating resin 13, a multi-layered main substrate 1 can be obtained, but here, each is formed one layer at a time. This method is called a semi-additive method, and the minimum wiring scale in the multi-layered main substrate 1 is line / space (L / S) = 10 / 10 μm.

[0023] Finally, solder resist 16 is coated, exposed, and developed on both sides of main board 1. This makes it possible to form main board 1 with a desired opening pattern, as shown in Fig. 1. Note that the method for manufacturing main board 1 is not limited to the above.

[0024] <Rewiring board> 2 is produced in parallel with the production of the main substrate 1. The rewiring substrate 10 has a support 21, a release layer (including an LTHC layer 23 and a seed layer 24 here) formed on one surface of the support 21 and having a first reference surface S1, a wiring layer formed adjacent to the release layer and having a plurality of connection terminals (including a first plating layer 27 and a copper pillar 32a here), and a resin layer 25 formed on the other surface of the support 21 and having a second reference surface S2 parallel to the first reference surface S1, and the end surface of the first plating layer 27 facing the support 21 is equidistant from the second reference surface S2.

[0025] After the rewiring board 10 of this embodiment is assembled to the main board 1, the support 21 is separated to form what is called a "coreless board" and to enable connection to a semiconductor element. A typical build-up multilayer wiring board (for example, the main board 1) requires a core board with high rigidity to alternately stack wiring layers and insulating layers. However, providing a core board increases the thickness of the wiring board, which is disadvantageous during mounting. Therefore, when manufacturing the rewiring board 10 of this embodiment, the support 21 is used to ensure rigidity as described below, but for example, after connection to the main board 1, the unnecessary support 21 is separated to leave only the wiring layers and insulating layers, thereby forming a thin semiconductor package board.

[0026] <Method of manufacturing rewiring substrate> A method for manufacturing the rewiring substrate 10 will now be described.

[0027] (Preparation of Support) As shown in FIG. 3, a support 21 made of a light-transmitting material is prepared. Here, soda lime glass having a thickness of 1.1 mm is used as the support 21, but generally, glass plates are often slightly distorted. Therefore, as shown in FIG. 4, the surface of the support 21 is ground with a grinding wheel 22. By grinding one side of the support 21, a first reference surface S1, which will be described later, can be formed. In addition, since a second reference surface S2 is formed on a resin layer 25 as will be described later, it is not necessary to grind the other side of the support 21, which reduces the number of manufacturing steps. The support 21 may be made of ceramic or resin.

[0028] (Formation of peeling layer) 5, a film of LTHC resin manufactured by 3M is formed on the surface of the support 21 by spin coating, forming a LTHC layer 23 with a thickness of 800 nm. Next, the edge of the LTHC layer 23 is rinsed, and a copper film with a thickness of 300 nm is sputtered on the LTHC layer 23 in a sputtering device so that the LTHC layer 23 is not exposed. The surface of the seed layer 24 is defined as a first reference plane S1. The LTHC layer 23 and the seed layer 24 form a release layer. Since the surface of the support 21 is flat, the first reference plane S1 is also flat with high accuracy.

[0029] (Formation of resin layer) Next, as shown in Fig. 6, the back surface where the support 21 is exposed is coated with a thermosetting resin of 10 µm or more, and then thermally cured to form a resin layer 25. If the resin layer 25 is too thick, the curing shrinkage of the epoxy resin will cause a large amount of warping, so it is preferable to coat the resin with a thickness of about 15 µm. Here, an inexpensive epoxy resin is used as an example, but resins other than epoxy resin may be used as long as they have a heat resistance of 200°C or more.

[0030] (Formation of the reference surface) 7, the copper sputtered surface (seed layer 24) of support 21 is adsorbed and fixed to a porous adsorption stage of a grinding device (not shown), and the resin layer 25 on the back surface is ground with grinding wheel 22 so that the parallelism is 1 μm or less, using a first reference surface (copper sputtered surface) S1 as a reference surface. This makes it possible to form a flat surface (referred to as a second reference surface S2) parallel to the first reference surface S1, as shown in FIG.

[0031] (Formation of resin pattern layer) Next, as shown in FIG. 9, a 25 μm thick photosensitive polyimide resin is spin-coated on the surface of the seed layer 24, and then exposed, developed, and cured to form a resin pattern layer (wiring layer) 26 having an opening pattern with openings corresponding to the desired copper pillars.

[0032] (Connection terminal formation) 10, power is supplied from the opening of the resin pattern layer 26, and electrolytic plating is performed in order to form the first plating layer 27 in contact with the first reference surface S1 by electrolytic solder plating of Sn-0.7%Cu, then electrolytic nickel plating is performed to form the second plating layer 28, and further electrolytic copper plating is performed to form the third plating layer 29. Note that electrolytic copper plating of the third plating layer 29 is performed until it is higher than the photosensitive polyimide resin surface. At this point, the lower end surfaces (inner end surfaces) of the first plating layer 27 constituting a part of the connection terminal are each equally distant from the second reference surface S2 of the resin layer 25. Here, "equally distant" means that the distance from the second reference surface of the resin layer 25 is within 5 μm.

[0033] Next, the third plating layer 29 protruding from the surface of the resin pattern layer 26 is polished using a CMP device (not shown) to make the height of the copper pillar portion 29a and the surface of the resin pattern layer 26 even.

[0034] (Wiring formation) Next, as shown in Fig. 11, a photosensitive insulating resin 30, which is a product name AH-3000 manufactured by Hitachi Chemical Co., Ltd., is coated to a thickness of 5 µm by spin coating. Next, a via pattern corresponding to the pattern of the underlying copper pillar portion 29a is exposed and developed to form a via hole 30a. Here, the photosensitive insulating resin 30 may be formed by vacuum laminating a dry film type, or may be formed by spin coating or slit coating a liquid photosensitive insulating resin.

[0035] Onto the photosensitive insulating resin 30 with the via hole 30a formed therein, a photosensitive insulating resin 31 is further coated to a thickness of 7 μm by spin coating, aligned with the via hole 30a, and exposed and developed to form a line pattern 31a. Here again, the photosensitive insulating resin 31 may be formed by vacuum laminating a dry film type, or may be formed by spin coating or slit coating a liquid photosensitive insulating resin.

[0036] 12, a seed layer of copper is formed to a thickness of 300 nm on the surface of the photosensitive insulating resin 31 on which the line pattern 31a is formed overlapping the via hole 30a by sputtering, followed by via-fill electrolytic copper plating to fill the line pattern of the photosensitive insulating resin 31 with copper plating 32. Next, the substrate is fixed to the porous adsorption stage of a grinding device, and the electrolytic copper plating on the surface is ground until the height of the photosensitive insulating resin 31 from the second reference surface S2 of the resin layer 25 becomes 10 μm, forming an independent copper line pattern.

[0037] Thereafter, the above-mentioned photosensitive insulating resin and copper plating may be repeatedly used to form wiring layers, forming a multi-layer wiring layer. A solder resist 33 is coated on the photosensitive insulating resin 31, exposed to light, and developed to form a desired opening pattern.

[0038] Finally, a dry film resist manufactured by Hitachi Chemical Co., Ltd. (product name RY-5325) is laminated on the solder resist 33, and after exposure and development into a hole pattern with adjacent φ70 μm openings in a matrix shape with a pitch of 150 μm, a 300 nm thick copper seed layer is sputtered and then electrolytic copper plating is applied to fill the hole pattern.

[0039] (Exposed connection terminals) Furthermore, after cutting this surface, the dry film resist is stripped off with an amine-based stripping solution to expose the independent copper pillars 32a, which are then diced into pieces. This completes the rewiring substrate 10 as shown in FIG.

[0040] <Semiconductor package substrate and its manufacturing method> A method for manufacturing a semiconductor package substrate will now be described.

[0041] (Connection between rewiring board and main board) First, cream solder 34 of SAC305 is screen-printed on wiring terminals 17 of main board 1, which was fabricated in a separate process. Next, as shown in Fig. 13, the end faces (outer end faces) of copper pillars 32a protruding from pieced rewiring board 10 are mounted on main board 1 while being aligned with solder 34, and solder connection is performed using a reflow device (not shown).

[0042] (Filling with underfill resin) Next, as shown in FIG. 14, after flux cleaning, underfill resin 35 is injected into the gap between main substrate 1 and rewiring substrate 10 connected via copper pillar 32a and solder 34, and is then solidified.

[0043] (Removal of the support and resin pattern layer) Furthermore, a laser beam is externally irradiated onto the LTHC layer 23 through the resin layer 25 and support 21 on the rewiring substrate 10 side, and the support 21 is peeled off from the interface with the LTHC layer 23. Furthermore, the resin pattern layer 26 is dissolved and peeled off with an alkaline peeling liquid. Through the above steps, the semiconductor package substrate 100 shown in Fig. 15 is completed. Here, the structure obtained by removing the support 21 and peeling layer from the rewiring substrate 10 is referred to as a rewiring unit.

[0044] In the completed semiconductor package substrate 100, connection terminals having first plating layers 27 of uniform height and connected to wiring terminals of the main substrate 1 are arranged at a pitch shorter than the pitch of the copper pillars 32a, facilitating connection to semiconductor chips and other electronic components via the first plating layers 27. According to this embodiment, open defects due to variations in the amount of solder are suppressed, and the growth of the IMC layer is suppressed, so that connection reliability and mechanical strength can be ensured even with a small amount of solder.

[0045] <Modification of the method for manufacturing a rewiring substrate> First, a support is coated with LTHC resin (product name) manufactured by 3M as a temporary release layer, and then the surface layer of the LTHC resin is ground. A 300 nm thick copper film is sputtered on top of the LTHC resin as a seed layer to form a reference flat surface.

[0046] Next, in order to form the desired multiple wiring layers consisting of via patterns and line patterns, the above process is repeated while aligning the lower layer line pattern, the via position of the insulating resin, and the upper layer line pattern, to construct a multilayer wiring structure.

[0047] Next, a 25μm-thick photosensitive dry film is applied onto the final wiring layer, and the film is exposed and developed in alignment with the opening pattern on the lands of the final wiring layer. Electricity is supplied to the opening pattern to perform electrolytic copper plating, electrolytic nickel plating, and electrolytic solder plating, and the photosensitive dry film resist is peeled off to form copper pillars.

[0048] Next, the substrate is cut into individual pieces together with the support to complete the rewiring substrate.

[0049] The main board including the glass cloth layer, the explanation of which is omitted, was prepared in a separate process, and the copper pillars of the rewiring board were aligned and mounted on the main board, and the main board and the rewiring board were soldered and connected using a reflow device. The flux used in the solder connection was washed away, and underfill resin was injected between the rewiring board and the main board to integrate them.

[0050] Next, a laser beam was irradiated from the outside onto the LTHC resin of the temporary release layer through the support, and the support was peeled off.Furthermore, the copper of the seed layer was etched out with an alkaline copper etching solution, and then the photosensitive polyimide film was dissolved and peeled off with an amine-based stripping solution, exposing the semiconductor chip connection terminals composed of the solder layer, barrier layer, and copper layer from the top, completing the semiconductor package substrate.

[0051] Furthermore, a semiconductor device is completed by mounting a plurality of semiconductor chips and passive electronic components on a semiconductor package substrate.

[0052] According to this embodiment, in a high density wiring board with a narrow terminal pitch, by aligning the in-plane height of the copper pillars, stable connection can be achieved even with a small amount of solder. [Explanation of symbols]

[0053] 1 Main Board 10 Rewiring board 21 Support 23 LTHC layer 24 Seed layer 25 Resin layer 32a Copper pillar 100 Semiconductor package substrate S1 1st reference plane S2 2nd reference plane

Claims

1. A method for manufacturing a substrate, comprising: forming a first reference surface by grinding one surface of a support formed from a glass plate; forming a release layer on the first reference surface; forming a resin layer on the other surface side of the support body, and grinding the resin layer based on the first reference surface to form a second reference surface parallel to the first reference surface; laminating the release layer to form a resin pattern layer having openings; forming a plurality of connection terminals in the openings of the resin pattern layer such that inner end surfaces of the connection terminals are in contact with the first reference surface; removing a portion of the resin pattern layer to expose a vicinity of an outer end surface of the connection terminal; a step of connecting an outer end surface of the connection terminal to a wiring terminal of a main board by soldering; filling an underfill resin around the connected connection terminal; removing the support and the release layer; and removing a remainder of the resin pattern layer.

2. 2. The method for manufacturing a semiconductor package substrate according to claim 1, wherein the support is made of a light-transmitting material, and the release layer is peeled off by irradiating laser light from outside through the support.

3. 3. The method for manufacturing a semiconductor package substrate according to claim 1, further comprising the steps of: grinding a surface of the resin pattern layer and the outer end face using the second reference plane as a reference before the step of exposing the vicinity of the outer end face of the connection terminal.

Citation Information

Patent Citations

  • Electrode structure and its forming method

    JP2004047510A

  • Manufacturing method of semiconductor device

    JP2012069734A

  • Semiconductor device, electronic component built-in substrate and manufacturing methods of those

    JP2013201301A

  • Method of manufacturing substrate having bump with pillar and surface treatment solution for bump with pillar

    JP2014203963A

  • Support glass substrate and laminate comprising the same

    JP2016117641A