Positive resist composition and resist pattern forming kit

A positive resist composition with a polymer of specified molecular weight and distribution, combined with a specific developer, addresses the challenge of forming high-resolution fine resist patterns in EUV lithography by enhancing pattern clarity and reducing defects.

JP7574566B2Active Publication Date: 2024-10-29ZEON CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020134206
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-15
Filing Date
2020-08-06
Publication Date
2024-10-29
Estimated Expiration
2040-08-06

AI Technical Summary

Technical Problem

Conventional resist compositions struggle to efficiently form fine resist patterns with high resolution using extreme ultraviolet light (EUV) due to issues such as surface roughness and missing contact holes, particularly in EUV lithography.

Method used

A positive resist composition is developed using a polymer with specific molecular weight ranges and molecular weight distribution, combined with a solvent, to enhance the resolution and clarity of resist patterns when exposed to EUV light. The polymer includes monomer units with predetermined fluorine atoms and a weight average molecular weight between 100,000 and 300,000, and a molecular weight distribution of 1.3 to 2.0, along with a developer having a solubility parameter less than 7.0 (cal/cm³)¹/² to improve contrast and efficiency.

Benefits of technology

The solution enables the formation of fine resist patterns with improved surface smoothness and reduced defects, achieving high resolution and efficient pattern formation in EUV lithography.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574566000001
    Figure 0007574566000001
  • Figure 0007574566000002
    Figure 0007574566000002
  • Figure 0007574566000003
    Figure 0007574566000003
Patent Text Reader

Abstract

To provide a resist composition and a resist pattern forming kit which are capable of efficiently forming a fine resist pattern with high resolution.SOLUTION: A positive resist composition contains: a polymer comprising a monomer unit (A) represented by formula (I) and a monomer unit represented by formula (II) and having a weight average molecular weight of 100,000 or more and 300,000 or less and a molecular weight distribution (Mw / Mn) of 1.3 or more and 2.0 or less; and a solvent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive resist composition and a resist pattern forming kit. [Background technology]

[0002] Conventionally, in the field of semiconductor manufacturing and the like, polymers whose main chains are cleaved and whose solubility in a developer is increased by irradiation with ionizing radiation such as electron beams or short-wavelength light such as ultraviolet light (hereinafter, ionizing radiation and short-wavelength light may be collectively referred to as "ionizing radiation, etc.") have been used as main-chain scission type positive resists.

[0003] Such a polymer is used, for example, as a positive resist composition containing the polymer and a solvent to form a resist pattern. Specifically, the solvent is removed from the positive resist composition supplied onto a substrate to form a resist film, and the resist film is irradiated (exposed) with ionizing radiation or the like to draw a desired pattern. Next, the exposed resist film is brought into contact with a developer (developed) to dissolve the exposed portion of the resist film, and a resist pattern consisting of unexposed portions can be formed on the substrate. In order to improve the characteristics of resist patterns, efforts have been made to improve polymers that can be used as main chain scission type positive resists.

[0004] For example, Patent Document 1 proposes a specific polymer containing an α-chloroacrylic acid fluoroester unit having an organic group with 5 to 7 fluorine atoms as a polymer that can be used as a main chain scission type positive resist. According to Patent Document 1, the polymer has excellent sensitivity when used as a positive resist, and by forming a resist pattern using a positive resist composition containing the polymer, it is possible to suppress collapse of the resist pattern while ensuring the clarity of the resulting resist pattern. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2018 / 123667 Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, EUV lithography technology using extreme ultraviolet (EUV) has been attracting attention as a technology that enables fine pattern formation with less proximity effect during exposure compared to electron beams, etc. However, the above conventional technology has room for improvement in terms of efficiently forming fine resist patterns with high resolution, for example, by using extreme ultraviolet as a light source for exposure.

[0007] SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide a positive resist composition and a resist pattern formation kit that can be used to efficiently form a fine resist pattern with high resolution. [Means for solving the problem]

[0008] The present inventors have conducted extensive research in order to achieve the above object, and have discovered that by using a polymer formed from specific monomers, which has a weight average molecular weight and a molecular weight distribution each falling within a specific range, a positive resist composition capable of efficiently forming a fine resist pattern with high resolution can be prepared, thereby completing the present invention.

[0009] That is, an object of the present invention is to solve the above-mentioned problems in an advantageous manner, and a positive resist composition of the present invention comprises a compound represented by the following general formula (I): [ka] [In the general formula (I), X is a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, or an astatine atom; R 1 is an organic group having 3 to 7 fluorine atoms.] and a monomer unit (A) represented by the following general formula (II): [ka] [In general formula (II), R 2 is a hydrogen atom, a fluorine atom, an unsubstituted alkyl group or an alkyl group substituted with a fluorine atom, and R 3 is a hydrogen atom, an unsubstituted alkyl group, or an alkyl group substituted with a fluorine atom, p and q are integers of 0 to 5, and p+q=5.], and a polymer having a weight average molecular weight of 100,000 to 300,000 and a molecular weight distribution (Mw / Mn) of 1.3 to 2.0, and a solvent. In this way, by using a positive resist composition containing a polymer that contains the monomer units (A) and (B) and has a weight average molecular weight and a molecular weight distribution each within a predetermined range, it is possible to efficiently form a fine resist pattern with high resolution, even when extreme ultraviolet light is used as a light source for exposure.

[0010] In the present invention, "high resolution" refers to suppression of surface roughness on the exposed surface after development, the occurrence of missing contact holes, etc., and good evaluation results such as CD value (CD: Critical Dimension, a value representing the critical dimension of the line width of the resist pattern), LWR value (LWR: Line Width Roughness, a value representing line width roughness), LER value (LER: Line Edge Roughness, a value representing line edge roughness), LCDU value (LCDU: Local Critical Dimension Uniformity, a value representing the uniformity of local critical dimensions), etc. In the present invention, the "weight average molecular weight" and the "molecular weight distribution" can be determined by the method described in the Examples of this specification.

[0011] In the positive resist composition of the present invention, X in the general formula (I) is preferably a chlorine atom. If X in the general formula (I) is a chlorine atom, the scission property of the main chain of the polymer when irradiated with ionizing radiation or the like can be improved. In addition, the preparation of the polymer becomes easier.

[0012] Furthermore, in the positive resist composition of the present invention, the polymer preferably has a proportion of 0.2% or less of components having a molecular weight of less than 10,000. If the proportion of components having a molecular weight of less than 10,000 in the polymer is 0.2% or less, the resolution of the obtained resist pattern can be improved. In the present invention, the "proportion of components having a molecular weight of less than 10,000" can be determined by the method described in the Examples of this specification.

[0013] The positive resist composition of the present invention is preferably a positive resist composition for extreme ultraviolet (EUV) lithography. By using the positive resist composition of the present invention, lithography using extreme ultraviolet rays can be suitably carried out.

[0014] Another object of the present invention is to advantageously solve the above problems, and the resist pattern formation kit of the present invention is characterized by comprising any one of the above-mentioned positive resist compositions and a developer. By using the resist pattern formation kit comprising the above-mentioned positive resist composition and developer, it is possible to efficiently form a fine resist pattern with high resolution.

[0015] In the resist pattern formation kit of the present invention, the solubility parameter of the developer is 7.0 (cal / cm 3 ) 1 / 2 The solubility parameter of the developer is preferably less than 7.0 (cal / cm 3 ) 1 / 2 If it is less than this, the contrast between the exposed and unexposed areas of the positive resist composition can be easily adjusted, improving the efficiency of forming a resist pattern. In the present invention, the "solubility parameter" can be determined by the method described in the examples of this specification. Effect of the Invention

[0016] According to the present invention, it is possible to provide a positive resist composition and a resist pattern formation kit that are capable of efficiently forming a fine resist pattern with high resolution. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, an embodiment of the present invention will be described in detail. Here, the positive resist composition of the present invention contains a specific polymer as a positive resist. The positive resist composition of the present invention can be suitably used when forming a resist pattern in the manufacturing process of, for example, printed circuit boards such as build-up boards, semiconductors, photomasks, and molds. Furthermore, the resist pattern forming kit of the present invention comprises the positive resist composition of the present invention and a developer, and can be suitably used when forming a resist pattern. In particular, the positive resist composition of the present invention can be suitably used when forming a resist pattern by irradiating extreme ultraviolet rays.

[0018] (Positive resist composition) The positive resist composition of the present invention contains a specific polymer and a solvent, and optionally further contains known additives that can be blended into positive resist compositions. The positive resist composition of the present invention contains the specific polymer as a positive resist. Therefore, by using a resist film obtained by applying the positive resist composition of the present invention onto a substrate and drying it, a fine resist pattern can be efficiently formed with high resolution.

[0019] <Polymer> The polymer contained in the positive resist composition of the present invention is a main chain scission type positive resist in which the main chain is scissed and the molecular weight is reduced by irradiation with ionizing radiation such as an electron beam or short wavelength light such as ultraviolet light (including EUV), and the polymer is represented by the following general formula (I): [ka] [In the general formula (I), X is a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, or an astatine atom; R1 is an organic group having 3 to 7 fluorine atoms; The following general formula (II): [ka] [In general formula (II), R 2 is a hydrogen atom, a fluorine atom, an unsubstituted alkyl group or an alkyl group substituted with a fluorine atom, and R 3 is a hydrogen atom, an unsubstituted alkyl group or an alkyl group substituted with a fluorine atom, p and q are integers of 0 to 5, and p+q=5.], and is characterized in that the polymer has a weight average molecular weight of 100,000 or more and 300,000 or less and a molecular weight distribution (Mw / Mn) of 1.3 or more and 2.0 or less.

[0020] The polymer of the present invention may contain any monomer unit other than the monomer unit (A) and the monomer unit (B). However, the proportion of the monomer unit (A) and the monomer unit (B) in all the monomer units constituting the polymer is preferably 90 mol % or more in total, more preferably substantially 100 mol %, and even more preferably 100 mol % (i.e., the polymer contains only the monomer unit (A) and the monomer unit (B)). The polymer of the present invention may be, for example, a random polymer, a block polymer, an alternating polymer (ABAB...), etc., so long as it has the monomer unit (A) and the monomer unit (B). However, it is preferable that the polymer contains 90% by mass or more (upper limit is 100% by mass) of an alternating polymer. Here, it is preferable that the alternating polymers do not form crosslinks with each other. The polymer is a polymer in which R of the monomer unit (A) is 1 Since it contains fluorine atoms, it is difficult to form a crosslinked product.

[0021] Since the polymer contains a predetermined monomer unit (A) and a monomer unit (B), when irradiated with ionizing radiation or the like (e.g., an electron beam, a KrF laser, an ArF laser, an EUV laser, etc.), the main chain is cut and the molecular weight is reduced. Furthermore, the polymer contains a predetermined monomer unit (A) and a monomer unit (B), and the weight average molecular weight and the molecular weight distribution are each within a predetermined range. Therefore, by using a positive resist composition containing the polymer, a fine resist pattern can be efficiently formed with high resolution.

[0022] [Monomer unit (A)] The monomer unit (A) has the following general formula (III): [ka] (In the general formula (III), X and R 1 is the same as in general formula (I).

[0023] The proportion of the monomer units (A) in all the monomer units constituting the polymer is not particularly limited, and can be, for example, 30 mol% or more and 70 mol% or less, preferably 40 mol% or more and 60 mol% or less, and more preferably 45 mol% or more and 55 mol% or less.

[0024] Here, X in general formula (I) and general formula (III) must be a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, or an astatine atom from the viewpoint of the absorption efficiency of ionizing radiation, etc. From the viewpoint of improving the severability of the main chain of the polymer when irradiated with ionizing radiation, etc., X in general formula (I) and general formula (III) is preferably a chlorine atom. Note that the monomer (a) in which X in general formula (III) is a chlorine atom has excellent polymerizability, and the polymer having the monomer unit (A) in which X in general formula (I) is a chlorine atom is also excellent in terms of ease of preparation.

[0025] Here, R in general formula (I) and general formula (III) 1R must be an organic group having 3 to 7 fluorine atoms. 1 If the number of fluorine atoms in R is 3 or more, the polymer main chain can be sufficiently cut when irradiated with ionizing radiation or the like. 1 When the number of fluorine atoms in R is 7 or less, the resolution of the resist pattern can be further improved. 1 is preferably an organic group having 3 or more and 5 or less fluorine atoms, and more preferably an organic group having 5 fluorine atoms.

[0026] Also, R 1 The number of carbon atoms in R is preferably 2 or more and 10 or less, more preferably 3 or more and 4 or less, and even more preferably 3. 1 If the number of carbon atoms in R is 2 or more, the solubility of the polymer in the developer after exposure can be sufficiently ensured. 1 Provided the number of carbon atoms is 10 or less, the glass transition temperature will not decrease excessively, and the resolution of the resulting resist pattern can be adequately ensured.

[0027] Specifically, R in the general formula (I) and the general formula (III) 1 is preferably a fluoroalkyl group having 3 or more and 7 or less fluorine atoms, a fluoroalkoxyalkyl group having 3 or more and 7 or less fluorine atoms, or a fluoroalkoxyalkenyl group having 3 or more and 7 or less fluorine atoms, and more preferably a fluoroalkyl group having 3 or more and 7 or less fluorine atoms.

[0028] Here, examples of the fluoroalkyl group having 3 or more and 7 or less fluorine atoms include a 2,2,2-trifluoroethyl group (having 3 fluorine atoms and 2 carbon atoms), a 2,2,3,3,3-pentafluoropropyl group (having 5 fluorine atoms and 3 carbon atoms, structural formula X below), a 3,3,4,4,4-pentafluorobutyl group (having 5 fluorine atoms and 4 carbon atoms, structural formula Y below), a 1H-1-(trifluoromethyl)trifluoroethyl group (having 6 fluorine atoms and 3 carbon atoms), a 1H,1H,3H-hexafluorobutyl group (having 6 fluorine atoms and 4 carbon atoms), a 2,2,3,3,4,4,4-heptafluorobutyl group (having 7 fluorine atoms and 4 carbon atoms), and a 1,2,2,2-tetrafluoro-1-(trifluoromethyl)ethyl group (having 7 fluorine atoms and 3 carbon atoms). Among these, a 2,2,3,3,3-pentafluoropropyl group (having 5 fluorine atoms and 3 carbon atoms, and having the following structural formula X) is preferred. Furthermore, examples of fluoroalkoxyalkyl groups having 3 to 7 fluorine atoms include a pentafluoroethoxymethyl group (having 5 fluorine atoms and 3 carbon atoms) and a pentafluoroethoxyethyl group (having 5 fluorine atoms and 4 carbon atoms). Furthermore, examples of the fluoroalkoxyalkenyl group having 3 or more and 7 or less fluorine atoms include a pentafluoroethoxyvinyl group (having 5 fluorine atoms and 4 carbon atoms). [ka] [ka]

[0029] The monomer (a) represented by the above-mentioned general formula (III) capable of forming the monomer unit (A) represented by the above-mentioned general formula (I) is not particularly limited, and examples thereof include 2,2,2-trifluoroethyl α-chloroacrylate (number of fluorine atoms: 3), 2,2,3,3,3-pentafluoropropyl α-chloroacrylate (number of fluorine atoms: 5), 3,3,4,4,4-pentafluorobutyl α-chloroacrylate (number of fluorine atoms: 5), 1H-1-(trifluoromethyl)trifluoroethyl α-chloroacrylate (number of fluorine atoms: 6), 1H,1H,3H-hexafluorobutyl α-chloroacrylate (number of fluorine atoms: 6), 1, Examples of α-chloroacrylic acid fluoroalkyl esters include 2,2,2-tetrafluoro-1-(trifluoromethyl)ethyl (number of fluorine atoms: 7) and α-chloroacrylic acid 2,2,3,3,4,4,4-heptafluorobutyl (number of fluorine atoms: 7); α-chloroacrylic acid fluoroalkoxyalkyl esters include α-chloroacrylic acid pentafluoroethoxymethyl ester (number of fluorine atoms: 5) and α-chloroacrylic acid pentafluoroethoxyethyl ester (number of fluorine atoms: 5); and α-chloroacrylic acid fluoroalkoxyalkenyl esters include α-chloroacrylic acid pentafluoroethoxyvinyl ester (number of fluorine atoms: 5).

[0030] The monomer unit (A) is preferably a structural unit derived from an α-chloroacrylic acid fluoroalkyl ester. More specifically, the monomer unit (A) is more preferably a structural unit derived from α-chloroacrylic acid 2,2,3,3,3-pentafluoropropyl ester among α-chloroacrylic acid fluoroalkyl esters. If the monomer unit (A) is a structural unit derived from α-chloroacrylic acid 2,2,3,3,3-pentafluoropropyl ester, the resolution of the resist pattern can be improved while sufficiently ensuring the scission property of the polymer main chain when irradiated with ionizing radiation or the like.

[0031] [Monomer unit (B)] The monomer unit (B) is represented by the following general formula (IV): [ka] (In general formula (IV), R 2 ~R 3 and p and q are the same as in general formula (II).

[0032] The proportion of the monomer units (B) in all the monomer units constituting the polymer is not particularly limited, and can be, for example, 30 mol% or more and 70 mol% or less, preferably 40 mol% or more and 60 mol% or less, and more preferably 45 mol% or more and 55 mol% or less.

[0033] Here, R in general formula (II) and general formula (IV) 2 ~R 3 The fluorine-substituted alkyl group that can constitute the above formula is not particularly limited, and examples thereof include groups having a structure in which some or all of the hydrogen atoms in an alkyl group are substituted with fluorine atoms. In addition, R in the general formula (II) and the general formula (IV) 2 ~R 3 The unsubstituted alkyl group that can constitute R is not particularly limited, and examples thereof include unsubstituted alkyl groups having 1 to 5 carbon atoms. 2 ~R 3 The unsubstituted alkyl group which may constitute the above formula is preferably a methyl group or an ethyl group.

[0034] From the viewpoint of improving the ease of preparation of the polymer, it is preferable that the number of R 2 and / or R 3 are all preferably hydrogen atoms or unsubstituted alkyl groups, more preferably hydrogen atoms or unsubstituted alkyl groups having 1 to 5 carbon atoms, and even more preferably hydrogen atoms. From the viewpoint of improving the ease of preparation of the polymer, it is preferable that p in the general formula (II) and the general formula (IV) is 5, q is 0, and there are five R 2It is preferable that all of R are hydrogen atoms or unsubstituted alkyl groups. 2 It is more preferable that all of R are hydrogen atoms or unsubstituted alkyl groups having 1 to 5 carbon atoms. 2 It is more preferable that all of are hydrogen atoms.

[0035] The monomer (b) represented by the above general formula (IV) capable of forming the monomer unit (B) represented by the above general formula (II) is not particularly limited, and examples thereof include α-methylstyrene (AMS) and its derivatives such as the following (b-1) to (b-11) (e.g., 4-fluoro-α-methylstyrene (4FAMS) according to the general formula (b-2)). [ka]

[0036] From the viewpoint of improving the ease of preparation of the polymer, it is preferable that the monomer unit (B) does not contain a fluorine atom (i.e., only the monomer unit (A) contains a fluorine atom), and it is more preferable that the monomer unit (B) is a structural unit derived from α-methylstyrene. 2 ~R 3 is p=5, q=0, and there are five R 2 It is particularly preferable that all of are hydrogen atoms.

[0037] [Weight average molecular weight] The weight average molecular weight (Mw) of the polymer must be 100,000 or more, preferably 125,000 or more, more preferably 150,000 or more, and must be 300,000 or less, preferably 200,000 or less. If the weight average molecular weight (Mw) of the polymer is 100,000 or more, the pattern formation efficiency of the resist pattern can be improved. On the other hand, if the weight average molecular weight (Mw) of the polymer is 300,000 or less, the sensitivity in the formation of the resist pattern is improved while ensuring the productivity of the polymer, so that even when extreme ultraviolet light is used as a light source for exposure, a fine resist pattern can be efficiently formed with high resolution.

[0038] [Number average molecular weight] The number average molecular weight (Mn) of the polymer is preferably 90,000 or more, more preferably 120,000 or more, and preferably 200,000 or less, and more preferably 150,000 or less. If the number average molecular weight (Mn) of the polymer is 90,000 or more, the pattern formation efficiency of the resist pattern can be further improved. On the other hand, if the number average molecular weight (Mn) of the polymer is 200,000 or less, the sensitivity in the formation of the resist pattern can be further improved.

[0039] [Molecular weight distribution] The molecular weight distribution (Mw / Mn) of the polymer must be 1.3 or more, preferably 1.35 or more, more preferably 1.39 or more, and must be 2.0 or less, preferably 1.6 or less, and more preferably 1.5 or less. If the molecular weight distribution (Mw / Mn) of the polymer is 1.3 or more, the polymer can be produced efficiently. On the other hand, if the molecular weight distribution (Mw / Mn) of the polymer is 2.0 or less, the contrast in the formation of the resist pattern can be improved, and a fine resist pattern can be efficiently formed with high resolution.

[0040] [Ratio of components with molecular weight less than 10,000] The polymer preferably has a molecular weight distribution in which the proportion of components less than 10,000 is 0.2% or less, more preferably 0.15% or less. If the proportion of components less than 10,000 in molecular weight is 0.2% or less, the resolution of the resist pattern can be further improved. There is no particular lower limit to the proportion of components less than 10,000 in molecular weight.

[0041] <Method of preparing polymer> The polymer having the above-mentioned monomer unit (A) and monomer unit (B) can be prepared, for example, by polymerizing a monomer composition containing monomer (a) and monomer (b) and then optionally purifying the obtained polymer.

[0042] The composition, molecular weight distribution, weight average molecular weight, number average molecular weight, and the ratio of each molecular weight component in the polymer can be adjusted by changing the polymerization conditions and purification conditions. Specifically, for example, the composition of the polymer can be adjusted by changing the content ratio of each monomer in the monomer composition used in the polymerization.

[0043] [Polymerization of Monomer Composition] Here, the monomer composition used for preparing the polymer can be a mixture of monomer components including monomer (a) and monomer (b), an optional solvent, a polymerization initiator, and optional additives. The polymerization of the monomer composition can be carried out using a known method. Among them, when a solvent is used, it is preferable to use cyclopentanone or the like as the solvent. Also, it is preferable to use a radical polymerization initiator such as azobisisobutyronitrile as the polymerization initiator.

[0044] The polymer obtained by polymerizing the monomer composition may be used as it is, but is not particularly limited thereto. After adding a good solvent such as tetrahydrofuran to a solution containing the polymer, the solution to which the good solvent has been added is dropped into a poor solvent such as methanol to coagulate the polymer, whereby the polymer can be recovered and purified as follows.

[0045] [Purification of polymer] The purification method used for purifying the obtained polymer to obtain a polymer having the above-mentioned properties is not particularly limited, and known purification methods such as reprecipitation and column chromatography can be used. Among them, the reprecipitation method is preferably used as the purification method. The purification of the polymer may be repeated several times.

[0046] The purification of the polymer by the reprecipitation method is preferably carried out, for example, by dissolving the obtained polymer in a good solvent such as tetrahydrofuran, and then dropping the obtained solution into a mixed solvent of a good solvent such as tetrahydrofuran and a poor solvent such as methanol to precipitate a part of the polymer. In this way, if the polymer solution is dropped into a mixed solvent of a good solvent and a poor solvent to purify the polymer, the molecular weight distribution, weight average molecular weight, number average molecular weight, and the proportion of high molecular weight components (for example, components with a molecular weight of 100,000 or more) of the obtained polymer can be easily adjusted by changing the type and mixing ratio of the good solvent and the poor solvent. Specifically, for example, the molecular weight of the polymer precipitated in the mixed solvent can be increased by increasing the proportion of the good solvent in the mixed solvent.

[0047] In addition, when purifying a polymer by the reprecipitation method, a polymer precipitated in a mixed solvent of a good solvent and a poor solvent may be used as long as it satisfies the desired properties, or a polymer that has not precipitated in the mixed solvent (i.e., a polymer dissolved in the mixed solvent) may be used. Here, the polymer that has not precipitated in the mixed solvent can be recovered from the mixed solvent by a known method such as concentration to dryness.

[0048] <Solvent> The solvent contained in the positive resist composition of the present invention is not particularly limited as long as it is a solvent that can dissolve the above-mentioned polymer, and it is possible to use known solvents such as those described in Japanese Patent No. 5938536. Among them, from the viewpoint of obtaining a positive resist composition with an appropriate viscosity and improving the coatability of the positive resist composition, the solvent is preferably an organic acid ester such as n-pentyl ester, n-hexyl ester, 2-methoxy-1-methylethyl acetate, isoamyl acetate, or a mixture thereof, more preferably 2-methoxy-1-methylethyl acetate, isoamyl acetate, or a mixture thereof, and even more preferably isoamyl acetate.

[0049] (Preparation of Positive Resist Composition) The positive resist composition of the present invention can be prepared by mixing the above-mentioned polymer, the solvent, and any known additives that may be used. In this case, the mixing method is not particularly limited, and the components may be mixed by a known method. In addition, the process may include a step of filtering the mixture after mixing the components.

[0050] 〔filtration〕 Here, the method of filtering the mixture is not particularly limited, and for example, the mixture can be filtered using a filter. The filter is not particularly limited, and examples thereof include fluorocarbon, cellulose, nylon, polyester, and hydrocarbon filtration membranes. Among them, from the viewpoint of effectively preventing impurities such as metals from being mixed into the positive resist composition from metal piping and the like that may be used during the preparation of the polymer, the material constituting the filter is preferably polyfluorocarbon such as nylon, polyethylene, polypropylene, polytetrafluoroethylene, Teflon (registered trademark), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), nylon, and a composite membrane of polyethylene and nylon. As the filter, for example, one disclosed in U.S. Pat. No. 6,103,122 may be used. In addition, the filter is commercially available as Zeta Plus (registered trademark) 40Q manufactured by CUNO Incorporated. Furthermore, the filter may contain a strong cationic or weak cationic ion exchange resin. Here, the average particle size of the ion exchange resin is not particularly limited, but is preferably 2 μm or more and 10 μm or less. Examples of cation exchange resins include sulfonated phenol-formaldehyde condensates, sulfonated phenol-benzaldehyde condensates, sulfonated styrene-divinylbenzene copolymers, sulfonated methacrylic acid-divinylbenzene copolymers, and other types of sulfonic or carboxylic acid group-containing polymers. + Counterion, NH4 + Counterion or alkali metal counterion, e.g. K + and Na + Counterions are provided. The cation exchange resin preferably has hydrogen counterions. Examples of such cation exchange resins include H + Sulfonated styrene-divinylbenzene copolymers with counterions include Microlite® PrCH from Purolite Corp. Such cation exchange resins are commercially available as AMBERLYST® from Rohm and Haas.

[0051] Furthermore, the pore size of the filter is preferably from 0.005 μm to 1 μm. If the pore size of the filter is within the above range, it is possible to sufficiently prevent impurities such as metals from being mixed into the positive resist composition.

[0052] The positive resist composition of the present invention is not particularly limited, but is preferably a positive resist composition for extreme ultraviolet lithography. By using the positive resist composition of the present invention, extreme ultraviolet lithography, which forms a resist pattern by irradiating extreme ultraviolet rays, can be suitably carried out. The method of irradiating extreme ultraviolet rays is not particularly limited, and can be carried out, for example, using a known extreme ultraviolet ray drawing device.

[0053] (Resist pattern formation kit) The resist pattern forming kit of the present invention comprises the above-mentioned positive resist composition and a developer, and can be used when forming a resist pattern. Since the resist pattern forming kit of the present invention contains the above-mentioned positive resist composition of the present invention, by using the resist pattern forming kit of the present invention, a fine resist pattern can be efficiently formed with high resolution. In particular, the resist pattern forming kit of the present invention can be suitably used when forming a resist pattern by irradiating extreme ultraviolet rays.

[0054] <Developer> There are no particular limitations on the developer used in the resist pattern formation kit of the present invention, and any solvent that is capable of dissolving the main chain scission portion of the polymer contained in the positive resist composition can be used.

[0055] [Solubility parameters] Among them, the solubility parameter of the developer (hereinafter referred to as "SP value") is 7.0 (cal / cm 3 ) 1 / 2 The SP value of the developer is preferably less than 7.0 (cal / cm 3 ) 1 / 2When the content is less than 100%, the contrast between the exposed and unexposed areas of the positive resist composition can be easily adjusted, improving the efficiency of resist pattern formation, and preventing an increase in the viscosity and surface tension of the developer, thereby improving the resolution of the resist pattern. In addition, when the developer is a mixed developer consisting of multiple types of developers, the SP value of the entire mixture must be 7.0 (cal / cm 3 ) 1 / 2 It may be less than 6.8 (cal / cm2) depending on the shape and definition of the target resist pattern. 3 ) 1 / 2 It may be less than. The SP value of the developer can be controlled by adjusting the type of developer employed, and when a mixture of multiple developers is used, by adjusting the mixing ratio thereof. The SP value of the developer is, for example, 6.0 (cal / cm 3 ) 1 / 2 It could be more than that.

[0056] 〔surface tension〕 The surface tension of the developer is preferably 17.0 mN / m or less, more preferably 15.0 mN / m or less. If the surface tension of the developer is 17.0 mN / m or less, even if the resist pattern to be developed is fine, the developer can easily enter fine gaps, so that the resist pattern can be efficiently formed. The surface tension of the developer can be, for example, 10.0 mN / m or more. The surface tension of the developer can be controlled by adjusting the type of solvent used and, when a mixture of a plurality of solvents is used, by adjusting the mixing ratio thereof.

[0057] Furthermore, when the resist pattern formation kit of the present invention is used when forming a resist pattern by irradiating with extreme ultraviolet rays, the developer is preferably a fluorine-based solvent, and particularly, the developer preferably contains a hydrofluorocarbon.

[0058] -Hydrofluorocarbon- The hydrofluorocarbon is not particularly limited, and examples thereof include 1,1,1,2,3,4,4,5,5,5-decafluoropentane, 1,1,1,2,2,3,3,4,4,5,5,6,6-tridecafluorohexane, 1,1,1,2,2,3,4,5,5,5-decafluoropentane, 1,1,1,3,3-pentafluorobutane, 1,1,1,2,2,3,3,4,4-nonafluorohexane, etc. Among them, from the viewpoint of further improving the resolution of the obtained resist pattern, the hydrofluorocarbon is preferably a hydrofluorocarbon having 5 to 6 carbon atoms, and more preferably 1,1,1,2,3,4,4,5,5,5-decafluoropentane (CF3CFHCFHCF2CF3, SP value: 6.8 (cal / cm 3 ) 1 / 2 , surface tension: 14.1 (mN / m)) is more preferable. The above-mentioned hydrofluorocarbons are commercially available, for example, as Vertrel XF (registered trademark) manufactured by Mitsui-DuPont Fluorochemicals Co., Ltd.

[0059] Moreover, the boiling point of the hydrofluorocarbon at 1 atm is preferably 40° C. or higher, more preferably 50° C. or higher, and preferably 70° C. or lower, more preferably 60° C. or lower. If the boiling point is within the above range, the resolution of the obtained resist pattern can be further improved. If the boiling point is equal to or higher than the above lower limit, the developer can be easily handled.

[0060] -Fluorine-based solvents other than hydrofluorocarbons- The fluorine-based solvent other than hydrofluorocarbon (hereinafter referred to as "other fluorine-based solvent") is not particularly limited, and for example, any fluorine-based solvent having a boiling point difference from hydrofluorocarbon of 25° C. or less in absolute value can be used. Among them, from the viewpoint of further improving the resolution of the obtained resist pattern, it is preferable to use at least one selected from the group consisting of hydrochlorofluorocarbons, hydrofluoroethers, and perfluorocarbons as the other fluorine-based solvent, and it is more preferable to use hydrofluoroethers.

[0061] Here, the hydrochlorofluorocarbon is not particularly limited, and examples thereof include 2,2-dichloro-1,1,1-trifluoroethane, 1,1-dichloro-1-fluoroethane, 1,1-dichloro-2,2,3,3,3-pentafluoropropane, 1,3-dichloro-1,1,2,2,3-pentafluoropropane, and the like. Among them, from the viewpoint of further improving the resolution of the obtained resist pattern, the hydrochlorofluorocarbon is preferably a hydrochlorofluorocarbon having 3 or less carbon atoms, and more preferably 1,1-dichloro-2,2,3,3,3-pentafluoropropane (CF3CF2CHCl2, SP value: 6.9 (cal / cm 3 ) 1 / 2 , surface tension: 16.2 mN / m) and 1,3-dichloro-1,1,2,2,3-pentafluoropropane (CClF2CF2CHClF, surface tension: 16.2 mN / m) are more preferred. The above-mentioned hydrochlorofluorocarbons are commercially available, for example, as Asahiklin AK-225 manufactured by AGC Corporation.

[0062] Furthermore, the hydrofluoroether is not particularly limited, and examples thereof include methyl nonafluorobutyl ether, methyl nonafluoroisobutyl ether, ethyl nonafluorobutyl ether, ethyl nonafluoroisobutyl ether, etc. Among these, from the viewpoint of further improving the resolution and clarity of the obtained resist pattern, the hydrofluoroether is preferably methyl nonafluorobutyl ether (CF3CF2CF2CF2OCH3, SP value: 6.5 (cal / cm 3 ) 1 / 2 , surface tension: 13.6 (mN / m)), ethyl nonafluorobutyl ether (CF3CF2CF2CF2OC2H5, SP value: 6.3 (cal / cm 3 ) 1 / 2 , surface tension: 13.6 (mN / m)), 1,1,1,2,2,3,4,5,5,5-decafluoro-3-methoxy-4-(trifluoromethyl)pentane (SP value: 6.2 (cal / cm 3 ) 1 / 2 , surface tension: 15 (mN / m)) is preferred, and methyl nonafluorobutyl ether (CF3CF2CF2CF2OCH3) is more preferred. The above-mentioned hydrofluoroethers are commercially available, for example, as Novec (registered trademark) 7100, Novec (registered trademark) 7200, Novec (registered trademark) 7300, etc. manufactured by 3M.

[0063] Furthermore, the perfluorocarbon is not particularly limited, and examples thereof include CF4, C2F6, C3F8, C4F8, and C4F 10 , C5F 12 , C6F 12 , C6F 14 , C7F 14 , C7F 16 , C8F 18 , C9F 20 Among these, from the viewpoint of further improving the resolution of the obtained resist pattern, the perfluorocarbon is preferably a perfluorocarbon having 6 to 10 carbon atoms, and more preferably C8F 18 is more preferred. The above-mentioned perfluorocarbon is commercially available, for example, as PF-5052 manufactured by 3M.

[0064] The fluorine-based solvent preferably has a boiling point at 1 atm of 40° C. or higher, more preferably 50° C. or higher, and even more preferably 60° C. or higher, and preferably 90° C. or lower, more preferably 80° C. or lower, and even more preferably 70° C. or lower. If the boiling point is within the above range, the resolution of the resulting resist pattern can be further improved. If the boiling point is equal to or higher than the above lower limit, the developer can be easily handled.

[0065] The absolute value of the difference between the boiling point α of the hydrofluorocarbon and the boiling point β of the other fluorinated solvent (=|α-β|) is preferably from 0° C. to 25° C., more preferably from 3° C. or more, even more preferably from 5° C. or more, preferably from 15° C. or less, and more preferably from 10° C. or less. If |α-β| is within the above range, the resolution of the obtained resist pattern can be sufficiently improved. From the standpoint of further improving the resolution of the obtained resist pattern, it is preferable that the boiling point β of the other fluorine-based solvent is higher than the boiling point α of the hydrofluorocarbon.

[0066] -Content ratio- In addition, when the developer is a mixed developer of hydrofluorocarbon and other fluorine-based solvent, the content ratio of hydrofluorocarbon to other fluorine-based solvent (hydrofluorocarbon:other fluorine-based solvent) is not particularly limited, and can be, for example, 10:90 to 90:10, preferably 20:80 to 80:20, more preferably 40:60 to 60:40, based on mass. If the content ratio of hydrofluorocarbon to other fluorine-based solvent is within the above range, a clearer pattern can be efficiently formed.

[0067] <Method of forming a resist pattern using a resist pattern forming kit> The method for forming a resist pattern using the resist pattern forming kit of the present invention is not particularly limited, and may be, for example, a method including the steps shown below.

[0068] [Method of forming a resist pattern] A resist pattern forming method using the resist pattern formation kit of the present invention may include, for example, an optional step of forming an underlayer film on a substrate (underlayer film forming step), a step of forming a resist film on the substrate or the underlayer film using a positive resist composition included in the resist pattern formation kit (resist film forming step), a step of exposing the resist film to light (exposure step), a step of developing the exposed resist film using a developer included in the resist pattern formation kit (developing step), a step of rinsing the developed resist film (rinsing step), and a step of etching the underlayer film and / or the substrate (etching step).

[0069] -substrate- Here, the substrate used in the resist pattern formation method is not particularly limited, and examples of substrates that can be used include substrates having an insulating layer and a copper foil provided on the insulating layer, which are used in the manufacture of printed circuit boards, and mask blanks in which a light-shielding layer is formed on a substrate.

[0070] Examples of the substrate material include inorganic materials such as metals (silicon, copper, chromium, iron, aluminum, etc.), glass, titanium oxide, silicon dioxide (SiO2), silica, and mica; nitrides such as SiN; oxynitrides such as SiON; and organic materials such as acrylic, polystyrene, cellulose, cellulose acetate, and phenolic resin. Among these, metals are preferred as the substrate material. By using, for example, a silicon substrate, a silicon dioxide substrate, or a copper substrate, preferably a silicon substrate or a silicon dioxide substrate, as the substrate, a cylindrical structure can be formed.

[0071] The size and shape of the substrate are not particularly limited. The surface of the substrate may be smooth, may have a curved surface or an uneven surface, or may be a thin plate-shaped substrate.

[0072] Furthermore, the surface of the substrate may be subjected to a surface treatment as necessary. For example, in the case of a substrate having a hydroxyl group on the surface layer of the substrate, the surface of the substrate can be treated with a silane coupling agent capable of reacting with the hydroxyl group. This changes the surface layer of the substrate from hydrophilic to hydrophobic, thereby improving the adhesion between the substrate and the underlayer film or between the substrate and the resist layer. In this case, the silane coupling agent is not particularly limited, but hexamethyldisilazane is preferred.

[0073] -Lower film formation process- In the underlayer film forming step, an underlayer film is formed on a substrate. By providing the underlayer film on the substrate, the surface of the substrate is made hydrophobic. This increases the affinity between the substrate and the resist film, and increases the adhesion between the substrate and the resist film. The underlayer film may be an inorganic underlayer film or an organic underlayer film.

[0074] The inorganic underlayer film can be formed by applying an inorganic material onto a substrate and baking it, etc. Examples of the inorganic material include silicon-based materials.

[0075] The organic underlayer film can be formed by applying an organic material onto a substrate to form a coating film and drying it. The organic material is not limited to those having sensitivity to light or electron beams, and can be, for example, a resist material or a resin material commonly used in the semiconductor field and liquid crystal field. Among them, the organic material is preferably a material capable of forming an organic underlayer film capable of etching, particularly dry etching. With such an organic material, the pattern formed by processing the resist film can be used to etch the organic underlayer film, thereby transferring the pattern to the underlayer film to form a pattern of the underlayer film. Among them, the organic material is preferably a material capable of forming an organic underlayer film capable of etching, such as oxygen plasma etching. Examples of organic materials used for forming the organic underlayer film include AL412 from Brewer Science.

[0076] The organic material can be applied by a conventional method using spin coating or a spinner. The method for drying the coating film may be any method capable of volatilizing the solvent contained in the organic material, such as a baking method. The baking conditions are not particularly limited, but the baking temperature is preferably 80°C or more and 300°C or less, and more preferably 200°C or less and 300°C or less. The baking time is preferably 30 seconds or more, more preferably 60 seconds or more, preferably 500 seconds or less, more preferably 400 seconds or less, even more preferably 300 seconds or less, and particularly preferably 180 seconds or less. The thickness of the underlayer film after drying the coating film is not particularly limited, but is preferably 10 nm or more and 100 nm or less.

[0077] -Resist film formation process- In the resist film forming step, a positive resist composition contained in the resist pattern formation kit of the present invention is used.

[0078] In the resist film forming step, a positive resist composition is applied onto an underlayer film or a substrate, and the applied positive resist composition is dried to form a resist film. Furthermore, the method for applying and drying the positive resist composition is not particularly limited, and any method commonly used for forming a resist film can be used.

[0079] -Exposure process- In the exposure step, the resist film formed in the resist film forming step is irradiated with ionizing radiation or the like to draw a desired pattern. For the irradiation of ionizing radiation or the like, known drawing devices such as an electron beam drawing device, a laser drawing device, or an extreme ultraviolet drawing device can be used.

[0080] -Developing process- In the developing step, the resist film exposed in the exposing step is brought into contact with the developer contained in the resist pattern formation kit of the present invention to develop the resist film, thereby forming a resist pattern on the underlayer film or substrate. Here, the method of contacting the resist film with the developer is not particularly limited, and known methods such as immersing the resist film in the developer or applying the developer to the resist film can be used. The temperature of the developer during development is not particularly limited, but can be, for example, 21° C. or higher and 25° C. or lower. The development time can be, for example, 30 seconds or higher and 4 minutes or lower. By using the developer contained in the resist pattern formation kit of the present invention for development, a fine resist pattern can be efficiently formed with high resolution.

[0081] -Rinse process- In the rinsing step, the resist film developed in the developing step is brought into contact with a rinsing liquid to rinse the developed resist film, thereby forming a resist pattern on the underlayer film or the substrate. If the rinsing step is carried out after the developing step, the resist residue attached to the developed resist film can be effectively removed. Here, the method for bringing the developed resist film into contact with the rinse liquid is not particularly limited, and known methods such as immersing the resist film in the rinse liquid or applying the rinse liquid to the resist film can be used.

[0082] The rinse liquid is not particularly limited as long as it can remove resist residue adhering to the developed resist film, and any rinse liquid can be used.

[0083] The temperature of the rinse liquid during rinsing is not particularly limited, but may be, for example, 21° C. to 25° C. The rinsing time may be, for example, 5 seconds to 3 minutes.

[0084] The developer used in the developing step and the rinse solution used in the rinse step may each be filtered before use. Examples of the filtration method include the filtration method using a filter described in the above section "Preparation of a positive resist composition".

[0085] -Etching process- In the etching step, the underlayer film and / or the substrate are etched using the above-mentioned resist pattern as a mask to form a pattern in the underlayer film and / or the substrate.

[0086] In this case, the number of etching steps is not particularly limited, and may be one or more. The etching may be dry etching or wet etching, but dry etching is preferred. Dry etching can be performed using a known dry etching device. The etching gas used in dry etching can be appropriately selected depending on the elemental composition of the underlayer film and the substrate to be etched. Examples of the etching gas include fluorine-based gases such as CHF3, CF4, C2F6, C3F8, and SF6; chlorine-based gases such as Cl2 and BCl3; oxygen-based gases such as O2, O3, and H2O; reducing gases such as H2, NH3, CO, CO2, CH4, C2H2, C2H4, C2H6, C3H4, C3H6, C3H8, HF, HI, HBr, HCl, NO, NH3, and BCl3; and inert gases such as He, N2, and Ar. These gases may be used alone or in combination of two or more. For dry etching of inorganic underlayer films, oxygen-based gases are usually used. Furthermore, for dry etching of a substrate, a fluorine-based gas is usually used, and a mixture of a fluorine-based gas and an inert gas is preferably used.

[0087] Furthermore, if necessary, the underlayer film remaining on the substrate may be removed before or after etching the substrate. When the underlayer film is removed before etching the substrate, the underlayer film may be a patterned underlayer film or an unpatterned underlayer film.

[0088] Here, the method of removing the underlayer film includes, for example, the above-mentioned dry etching. In addition, in the case of an inorganic underlayer film, a liquid such as a basic liquid or an acid liquid, preferably a basic liquid, may be brought into contact with the underlayer film to remove the underlayer film. Here, the basic liquid is not particularly limited, and examples thereof include alkaline hydrogen peroxide and the like. The method of removing the underlayer film by wet stripping using alkaline hydrogen peroxide is not particularly limited as long as the underlayer film and alkaline hydrogen peroxide can be brought into contact with each other for a certain period of time under heating conditions, and examples thereof include a method of immersing the underlayer film in heated alkaline hydrogen peroxide, a method of spraying alkaline hydrogen peroxide on the underlayer film in a heated environment, and a method of coating the underlayer film with heated alkaline hydrogen peroxide. After performing any of these methods, the substrate is washed with water and dried to obtain a substrate from which the underlayer film has been removed.

[0089] Two examples of the resist pattern forming method using the resist pattern forming kit of the present invention will be described below. However, since the substrate and the conditions in each step used in the following examples are the same as the substrate and the conditions in each step described above, the explanation will be omitted below. Note that the resist pattern forming method using the resist pattern forming kit of the present invention is not limited to the method shown in the following examples.

[0090] <<First example>> The first example is a method of forming a resist pattern using EUV, which includes the above-mentioned underlayer film forming step, resist film forming step, exposure step, development step, rinsing step, and etching step.

[0091] Specifically, in the underlayer film forming step, an inorganic material is applied onto a substrate and then baked to form an inorganic underlayer film.

[0092] Next, in the resist film forming step, the resist composition contained in the resist pattern forming kit of the present invention is applied onto the inorganic underlayer film formed in the underlayer film forming step, and then dried to form a resist film.

[0093] Then, in the exposure process, the resist film formed in the resist film formation process is irradiated with EUV light to draw the desired pattern.

[0094] Furthermore, in the developing step, the resist film exposed in the exposing step is brought into contact with the developer contained in the resist pattern formation kit of the present invention to develop the resist film, thereby forming a resist pattern on the underlayer film.

[0095] Then, in the rinsing step, the resist film developed in the developing step is brought into contact with a rinsing liquid to rinse the developed resist film.

[0096] Then, in an etching process, the underlying film is etched using the resist pattern as a mask to form a pattern in the underlying film.

[0097] Next, the substrate is etched using the underlying film on which the pattern is formed as a mask to form a pattern on the substrate.

[0098] <<Second Example>> The second example is a method of forming a resist pattern using EB, and includes the above-mentioned resist film forming step, exposure step, development step, rinsing step, and etching step.

[0099] Specifically, in the resist film forming step, the resist composition contained in the resist pattern formation kit of the present invention is applied onto a substrate, and then dried to form a resist film.

[0100] Next, in the exposure step, the resist film formed in the resist film formation step is irradiated with EB to depict a desired pattern.

[0101] Furthermore, in the developing step, the resist film exposed in the exposing step is brought into contact with the developer contained in the resist pattern formation kit of the present invention to develop the resist film, thereby forming a resist pattern on the substrate.

[0102] Then, in the rinsing step, the resist film developed in the developing step is brought into contact with a rinsing liquid to rinse the developed resist film.

[0103] Then, in an etching process, the substrate is etched using the resist pattern as a mask to form a pattern on the substrate. EXAMPLES

[0104] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following description, "%" representing an amount is based on mass unless otherwise specified. In the examples and comparative examples, the weight average molecular weight, number average molecular weight, and molecular weight distribution of the polymer, the proportion of each molecular weight component in the polymer, SP value, surface tension, optimum exposure dose, CD value, LWR value, LER value, and LCDU value were measured by the following methods.

[0105] <Weight average molecular weight, number average molecular weight and molecular weight distribution> The weight average molecular weight (Mw) and number average molecular weight (Mn) of the polymers obtained in the examples and comparative examples were measured using gel permeation chromatography, and the molecular weight distribution (Mw / Mn) was calculated. Specifically, a gel permeation chromatograph (Tosoh Corporation, HLC-8220) was used, and tetrahydrofuran was used as a developing solvent to determine the weight average molecular weight (Mw) and number average molecular weight (Mn) of the polymer in terms of standard polystyrene. Then, the molecular weight distribution (Mw / Mn) was calculated.

[0106] <Proportion of each molecular weight component in the polymer> Gel permeation chromatography (manufactured by Tosoh Corporation, HLC-8220) was used, and tetrahydrofuran was used as the developing solvent to obtain a chromatogram of the polymer. Then, from the obtained chromatogram, the total peak area (A), the total peak area of components with a molecular weight less than 6,000 (B), the total peak area of components with a molecular weight less than 10,000 (C), the total peak area of components with a molecular weight greater than 20,000 (D), the total peak area of components with a molecular weight greater than 30,000 (E), the total peak area of components with a molecular weight greater than 40,000 (F), the total peak area of components with a molecular weight greater than 50,000 (G), the total peak area of components with a molecular weight greater than 60,000 (H), the total peak area of components with a molecular weight greater than 80,000 (I), and the total peak area of peaks with a molecular weight greater than 100,000 (J) were determined. Then, the ratio of components of each molecular weight was calculated using the following formula. Ratio (%) of components with a molecular weight less than 6,000 = (B / A) × 100 Ratio (%) of components with a molecular weight less than 10,000 = (C / A) × 100 Ratio (%) of components with a molecular weight greater than 20,000 = (D / A) × 100 Ratio (%) of components with a molecular weight greater than 30,000 = (E / A) × 100 Ratio (%) of components with a molecular weight greater than 40,000 = (F / A) × 100 Ratio (%) of components with a molecular weight greater than 50,000 = (G / A) × 100 Ratio (%) of components with a molecular weight greater than 60,000 = (H / A) × 100 Ratio (%) of components with a molecular weight greater than 80,000 = (I / A) × 100 Ratio (%) of components with a molecular weight greater than 100,000 = (J / A) × 100

[0107] <SP value> The SP values of the developer and the rinse solution used in the examples and comparative examples were calculated using Hoy's group contribution method. When the developer is a mixed developer composed of two types of developers, developer (I) with an SP value of α and developer (II) with an SP value of β (the mass ratio of developer (I) to developer (II) ((I):(II)=x:y)), the SP value was measured by the following method. SP value of the mixed developer = α×(x / x + y) + β×(y / x + y)

[0108] <Surface tension> The surface tensions of the developers and rinse liquids used in the examples and comparative examples were measured at 25°C using the ring method.

[0109] <Optimal exposure amount (E op )> The optimal exposure amount (Eop) was determined as the most excellent point from the CD value, LER value, and LWR value by varying the exposure amount and focus.

[0110] <CD value, LWR value, LER value, LCDU value> The CD value, LWR value, LER value, and LCDU value of the resist patterns formed in the examples and comparative examples were measured and calculated using a high-resolution FEB length measurement device (CG5000, manufactured by Hitachi High-Technologies Corporation) and analysis software (Design Metrology System, manufactured by Hitachi High-Technologies Corporation). The fact that the CD value is within the range of half pitch (hp) or contact hole ±5 nm and the lower the LWR, LER values, and LCDU value, the higher the resolution of the resist pattern is indicated.

[0111] <Preparation of polymer A (crude)> [Polymerization of the monomer composition] A monomer composition containing 3.0 g of α-chloroacrylic acid 2,2,3,3,3-pentafluoropropyl (ACAPFP) as monomer (a) and 3.4680 g of α-methylstyrene (AMS) as monomer (b), 0.0014 g of azobisisobutyronitrile (AIBN) as a polymerization initiator, and 6.4666 g of cyclopentanone (CPN) as a solvent was placed in a glass container, the glass container was sealed and replaced with nitrogen, and the mixture was stirred in a constant temperature bath at 40°C under a nitrogen atmosphere for 50 hours. After that, the temperature was returned to room temperature, the glass container was opened to the atmosphere, and 10 g of tetrahydrofuran (THF) was added to the obtained solution. Then, the solution to which THF was added was dropped into 100 g of methanol to precipitate a polymer. Then, the solution containing the precipitated polymer was filtered using a Kiriyama funnel to obtain a white coagulated product (polymer A; crude). The obtained polymer A (crude) contained 50 mol % each of 2,2,3,3,3-pentafluoropropyl α-chloroacrylate units and α-methylstyrene units. [Purification of Polymer A (crude)] Next, the obtained polymer A (crude) was dissolved in 100 g of THF, and the obtained solution was dropped into 1000 g of a mixed solvent of THF and methanol (the mixing ratio of THF and methanol was THF:methanol=25.5:74.5 by mass ratio), and a white coagulated material (polymer A containing α-chloroacrylic acid 2,2,3,3,3-pentafluoropropyl unit and α-methylstyrene unit) was precipitated. Then, the solution containing the precipitated polymer A was filtered using a Kiriyama funnel to obtain a white polymer A. Then, the weight average molecular weight, number average molecular weight, and molecular weight distribution of the obtained polymer A, as well as the proportion of each molecular weight component in polymer A, were measured. The results are shown in Table 1.

[0112] <Preparation of Polymer B (crude)> [Polymerization of Monomer Composition] A monomer composition containing 3.0 g of α-chloroacrylic acid 2,2,3,3,3-pentafluoropropyl (ACAPFP) as monomer (a) and 3.4680 g of α-methylstyrene (AMS) as monomer (b), 0.0021 g of azobisisobutyronitrile (AIBN) as a polymerization initiator, and 6.4659 g of cyclopentanone (CPN) as a solvent was placed in a glass container, the glass container was sealed and replaced with nitrogen, and the mixture was stirred in a constant temperature bath at 53°C under a nitrogen atmosphere for 50 hours. After that, the temperature was returned to room temperature, the glass container was opened to the atmosphere, and 10 g of tetrahydrofuran (THF) was added to the obtained solution. Then, the solution to which THF was added was dropped into 100 g of methanol to precipitate a polymer. Then, the solution containing the precipitated polymer was filtered using a Kiriyama funnel to obtain a white coagulated product (polymer B; crude). The obtained polymer B (crude) contained 50 mol % each of 2,2,3,3,3-pentafluoropropyl α-chloroacrylate units and α-methylstyrene units.

[0113] [Purification of Polymer B (crude)] Next, the obtained polymer B was dissolved in 100 g of THF, and the obtained solution was dropped into 1000 g of a mixed solvent of THF and methanol (the mixing ratio of THF and methanol was THF:methanol=24:76 by mass ratio), and a white coagulated material (polymer B containing α-chloroacrylic acid 2,2,3,3,3-pentafluoropropyl unit and α-methylstyrene unit) was precipitated. Then, the solution containing the precipitated polymer B was filtered using a Kiriyama funnel to obtain a white polymer B. Then, the weight average molecular weight, number average molecular weight, and molecular weight distribution of the obtained polymer B, as well as the proportion of each molecular weight component in polymer B, were measured. The results are shown in Table 1.

[0114] <Preparation of Polymer C (crude)> [Polymerization of Monomer Composition] A monomer composition containing 3.0 g of α-chloroacrylic acid 2,2,3,3,3-pentafluoropropyl (ACAPFP) as monomer (a) and 3.4764 g of α-methylstyrene (AMS) as monomer (b), 0.0055 g of azobisisobutyronitrile (AIBN) as a polymerization initiator, and 1.6205 g of cyclopentanone (CPN) as a solvent was placed in a glass container, the glass container was sealed and replaced with nitrogen, and the mixture was stirred in a constant temperature bath at 78°C under a nitrogen atmosphere for 6 hours. After that, the temperature was returned to room temperature, the glass container was opened to the atmosphere, and 10 g of tetrahydrofuran (THF) was added to the obtained solution. Then, the solution to which THF was added was dropped into 100 g of methanol to precipitate a polymer. Then, the solution containing the precipitated polymer was filtered using a Kiriyama funnel to obtain a white coagulated product (polymer C; crude). The obtained polymer C (crude) contained 50 mol % each of 2,2,3,3,3-pentafluoropropyl α-chloroacrylate units and α-methylstyrene units.

[0115] [Purification of Polymer C (crude)] Next, the obtained polymer C (crude) was dissolved in 100 g of THF, and the obtained solution was dropped into 1000 g of a mixed solvent of THF and methanol (the mixing ratio of THF and methanol was THF:methanol=15:85 by mass ratio), and a white coagulated material (polymer C containing α-chloroacrylic acid 2,2,3,3,3-pentafluoropropyl unit and α-methylstyrene unit) was precipitated. Then, the solution containing the precipitated polymer C was filtered with a Kiriyama funnel to obtain a white polymer C. Then, the weight average molecular weight, number average molecular weight, and molecular weight distribution of the obtained polymer C, as well as the proportion of each molecular weight component in the polymer C, were measured. The results are shown in Table 1.

[0116] <Preparation of Polymer D (crude)> [Polymerization of Monomer Composition] A monomer composition containing 3.0 g of α-chloroacrylic acid 2,2,3,3,3-pentafluoropropyl (ACAPFP) as monomer (a) and 3.2832 g of α-methylstyrene (AMS) as monomer (b), 0.0005 g of azobisisobutyronitrile (AIBN) as a polymerization initiator, and 1.5709 g of cyclopentanone (CPN) as a solvent was placed in a glass container, the glass container was sealed and replaced with nitrogen, and the mixture was stirred in a constant temperature bath at 78°C under a nitrogen atmosphere for 2 hours. After that, the temperature was returned to room temperature, the glass container was opened to the atmosphere, and 10 g of tetrahydrofuran (THF) was added to the obtained solution. Then, the solution to which THF was added was dropped into 100 g of methanol to precipitate polymer D. Then, the solution containing the precipitated polymer D was filtered using a Kiriyama funnel to obtain a white coagulated product (polymer D; crude). The obtained polymer D (crude) contained 50 mol % each of 2,2,3,3,3-pentafluoropropyl α-chloroacrylate units and α-methylstyrene units.

[0117] [Purification of polymer D (crude)] Next, the obtained polymer D (crude) was dissolved in 100 g of THF, and the obtained solution was dropped into 1000 g of a mixed solvent of THF and methanol (the mixing ratio of THF and methanol was THF:methanol=21:79 by mass ratio), and a white coagulated material (polymer D containing α-chloroacrylic acid 2,2,3,3,3-pentafluoropropyl unit and α-methylstyrene unit) was precipitated. Then, the solution containing the precipitated polymer D was filtered using a Kiriyama funnel to obtain a white polymer D. Then, the weight average molecular weight, number average molecular weight, and molecular weight distribution of the obtained polymer D, as well as the proportion of each molecular weight component in the polymer D, were measured. The results are shown in Table 1.

[0118] Example 1 <Preparation of Positive Resist Composition> Polymer A was dissolved in isoamyl acetate as a solvent to prepare a positive resist composition A with a polymer concentration of 1.75%.

[0119] <Formation of Resist Pattern> Using a spin coater (MS-A150, manufactured by Mikasa), the positive resist composition A was applied onto a silicon wafer having a diameter of 4 inches. The applied positive resist composition A was then heated on a hot plate at a temperature of 150° C. for 3 minutes to form a resist film having a thickness of 50 nm on the silicon wafer. The resist film was then exposed to an optimal exposure dose (E op )57mJ / cm 2 The pattern was then written using a developer containing hydrofluorocarbon (manufactured by Mitsui DuPont Fluorochemicals Co., Ltd., Vertrel XF (CF3CFHCFHCF2CF3) as a fluorine-based solvent, SP value: 6.8 (cal / cm 3 ) 1 / 2 , surface tension: 14.1 (mN / m), boiling point: 53.6°C), and hydrofluoroether (3M, Novec (registered trademark) 7100 (C4F9OCH3), SP value: 6.5 (cal / cm) as another fluorine-based solvent. 3 ) 1 / 2 , surface tension: 13.6 (mN / m)) mixed developer (the content ratio (mass ratio) of hydrofluorocarbon to hydrofluoroether is hydrofluorocarbon:hydrofluoroether=25:75, SP value of mixed developer: 6.575 (cal / cm 3 ) 1 / 2 The developing process was carried out at a temperature of 23° C. for 30 seconds using a mixed developer (surface tension: 13.725 (mN / m)). Then, a fluorine-based solvent (3M, Novec (registered trademark) 7100 (C4F9OCH3, SP value: 6.3 (cal / cm 3 ) 1 / 2 A resist pattern was formed by rinsing for 10 seconds at a temperature of 23° C. using a rinsing solution of 1000 mL of ethyl acetate (pH 7.0, surface tension: 13.6 mN / m, boiling point: 61° C.) with ethyl acetate. The resist pattern had lines (unexposed areas) and spaces (exposed areas) of 16 nm (i.e., a half pitch (hp) of 16 nm). The CD value, LWR value, and LER value were measured using the obtained resist pattern. The results are shown in Table 2.

[0120] (Examples 2 to 6) <Preparation of Positive Resist Composition> In the same manner as in Example 1, a positive resist composition A was prepared. <Formation of Resist Pattern> A resist film was formed in the same manner as in Example 1. The optimum exposure dose (E op ), and the developer used was a hydrofluorocarbon as a fluorine-based solvent exhibiting the SP value and surface tension shown in Table 2 (Example 2), or a mixed developer of a hydrofluorocarbon as a fluorine-based solvent and a hydrofluoroether as another fluorine-based solvent exhibiting the content ratio (mass ratio), SP value, and surface tension shown in Table 2 (Examples 3 to 6). Otherwise, the "preparation of a positive resist composition" and "formation of a resist pattern" were performed in the same manner as in Example 1, and measurements were performed in the same manner as in Example 1. The results are shown in Table 2. The hydrofluorocarbons and hydrofluoroethers used in Examples 2 to 6 were the same as those used in Example 1.

[0121] Comparative Example 1 <Preparation of Positive Resist Composition> A positive resist composition C was prepared in the same manner as in Example 1, except that Polymer C was used in place of Polymer A. <Formation of Resist Pattern> A resist film was formed in the same manner as in Example 1, except that the positive resist composition C was used instead of the positive resist composition A. The optimum exposure dose (E op ) and the developer used was the same hydrofluorocarbon as in Example 1. Other than that, the "preparation of a positive resist composition" and "formation of a resist pattern" were carried out in the same manner as in Example 1, and measurements were carried out in the same manner as in Example 1. The results are shown in Table 2.

[0122] Comparative Example 2 <Preparation of Positive Resist Composition> A positive resist composition D was prepared in the same manner as in Example 1, except that polymer D was used instead of polymer A. <Formation of Resist Pattern> A resist film was formed in the same manner as in Example 1, except that the positive resist composition D was used instead of the positive resist composition A. The optimum exposure dose (E op ) and the developer used was the same hydrofluorocarbon as in Example 1. Other than that, the "preparation of a positive resist composition" and "formation of a resist pattern" were carried out in the same manner as in Example 1, and measurements were carried out in the same manner as in Example 1. The results are shown in Table 2.

[0123] (Examples 7 to 11) <Preparation of Positive Resist Composition> A positive resist composition B was prepared in the same manner as in Example 1, except that polymer B was used in place of polymer A. <Formation of Resist Pattern> A resist film was formed in the same manner as in Example 1, except that the positive resist composition B was used instead of the positive resist composition A. Then, the optimal exposure dose (E op ), and the developer used was a hydrofluorocarbon as a fluorine-based solvent (Example 7), or a mixed developer of a hydrofluorocarbon as a fluorine-based solvent and a hydrofluoroether as another fluorine-based solvent, which exhibits the content ratio (mass ratio), SP value, and surface tension shown in Table 3 (Examples 8 to 11). Otherwise, "Preparation of a positive resist composition" and "Formation of a resist pattern" were performed in the same manner as in Example 1, and measurements were performed in the same manner as in Example 1. The results are shown in Table 3. The hydrofluorocarbons and hydrofluoroethers used in Examples 7 to 11 were the same as those used in Example 1.

[0124] (Examples 12 to 14) <Preparation of Positive Resist Composition> In the same manner as in Example 1, a positive resist composition A was prepared. <Formation of Resist Pattern> A resist film was formed in the same manner as in Example 1. The optimum exposure dose (E op), and the developer used was a hydrofluorocarbon as a fluorine-based solvent (Example 12), or a mixed developer of a hydrofluorocarbon as a fluorine-based solvent and a hydrofluoroether as another fluorine-based solvent (Examples 13 and 14) showing the content ratio (mass ratio), SP value, and surface tension shown in Table 4. Furthermore, instead of a line and space with a half pitch of 16 nm, the resist pattern was a line and space with a line (unexposed area) and a space (exposed area) of 21 nm (i.e., half pitch of 21 nm). Other than that, the "preparation of a positive resist composition" and "formation of a resist pattern" were performed in the same manner as in Example 1, and measurements were performed in the same manner as in Example 1. The results are shown in Table 4. The hydrofluorocarbons and hydrofluoroethers used in Examples 12 to 14 were the same as those used in Example 1.

[0125] (Examples 15 to 18) <Preparation of Positive Resist Composition> In the same manner as in Example 1, a positive resist composition A was prepared. <Formation of Resist Pattern> A resist film was formed in the same manner as in Example 1. The optimum exposure dose (E op ), and the developer used was a mixed developer of hydrofluorocarbon as a fluorine-based solvent and hydrofluoroether as another fluorine-based solvent (Examples 15, 17, and 18), or hydrofluorocarbon as a fluorine-based solvent (Example 16), which exhibited the content ratio (mass ratio), SP value, and surface tension shown in Table 5. Furthermore, the resist pattern was changed to a 22 nm contact hole instead of a 16 nm half-pitch line and space. Other than that, the "preparation of a positive resist composition" and "formation of a resist pattern" were performed in the same manner as in Example 1, and measurements were performed in the same manner as in Example 1. The results are shown in Table 5. The hydrofluorocarbon and hydrofluoroether used in Examples 15 to 18 were the same as those used in Example 1.

[0126] Comparative Example 3 <Preparation of Positive Resist Composition> In the same manner as in Comparative Example 1, a positive resist composition C was prepared. <Formation of Resist Pattern> A resist film was formed in the same manner as in Comparative Example 1. The optimum exposure dose (E op ), and the same hydrofluorocarbon as used in Example 1 was used as the developer. Furthermore, the resist pattern was changed to 22 nm contact holes instead of 16 nm half-pitch lines and spaces. Other than that, "Preparation of positive resist composition" and "Formation of resist pattern" were performed in the same manner as in Comparative Example 1, and measurements were performed in the same manner as in Example 1. The results are shown in Table 5.

[0127] [Table 1]

[0128] [Table 2]

[0129] [Table 3]

[0130] [Table 4]

[0131] [Table 5]

[0132] It can be seen from Tables 1 to 5 that in Examples 1 to 18, which used positive resist compositions containing a polymer that contains the specified monomer unit (A) and monomer unit (B), has a weight average molecular weight of 100,000 or more and 300,000 or less, and a molecular weight distribution (Mw / Mn) of 1.3 or more and 2.0 or less, fine resist patterns could be formed with high resolution. In particular, for a half pitch of 16 nm, the optimal exposure dose (E op ) to 57 (mJ / cm 2 ) and a mixed developer containing hydrofluorocarbon and hydrofluoroether in a content ratio of 25:75 was used as the developer in Example 1, whereby a resist pattern with excellent resolution was obtained. In addition, in the case of a half pitch of 21 nm, the optimal exposure dose (E op ) to 38 (mJ / cm 2 ) and a hydrofluorocarbon was used as the developer in Example 12, whereby a resist pattern with excellent resolution was obtained. Furthermore, in the case of a contact hole of 22 nm, the optimal exposure dose (E op ) to 50.4 (mJ / cm 2 ) and a mixed developer containing hydrofluorocarbon and hydrofluoroether in a content ratio of 50:50 was used as the developer in Example 15, whereby a resist pattern with excellent resolution was obtained. On the other hand, it is seen from Comparative Examples 1 to 3 that, although containing the specified monomer unit (A) and monomer unit (B), the weight average molecular weight of Comparative Examples 1 to 3 is less than 100,000, and therefore it is not possible to form a fine resist pattern with high resolution. [Industrial Applicability]

[0133] According to the present invention, it is possible to provide a positive resist composition and a resist pattern forming kit that are capable of efficiently forming a fine resist pattern with high resolution.

Claims

1. The following general formula (I): [Formula 1] [In the general formula (I), X is a chlorine atom, and R 1 is an organic group having 3 to 7 fluorine atoms. A monomer unit (A) represented by the formula: The following general formula (II): [chemical 2] [In general formula (II), R 2 is a hydrogen atom, a fluorine atom, an unsubstituted alkyl group or an alkyl group substituted with a fluorine atom, R 3 represents a hydrogen atom, an unsubstituted alkyl group or an alkyl group substituted with a fluorine atom, p and q each represent an integer of 0 to 5, and p+q=5. and a monomer unit (B) represented by The weight average molecular weight is 125,000 or more and 300,000 or less, and a polymer having a molecular weight distribution (Mw / Mn) of 1.3 or more and 2.0 or less; A positive resist composition comprising:

2. 2. The positive resist composition according to claim 1, wherein the polymer contains 0.2% or less of components having a molecular weight of less than 10,000.

3. 3. The positive resist composition according to claim 1, which is a positive resist composition for extreme ultraviolet lithography.

4. A kit for forming a resist pattern, comprising the positive resist composition according to any one of claims 1 to 3 and a developer.

5. The solubility parameter of the developer is 7.0 (cal / cm 3 ) 1/2 The resist pattern forming kit according to claim 4 , wherein the total amount of the resist pattern forming kit is less than 100 μm.

Citation Information

Patent Citations

  • Polymer and positive resist composition

    JP2017132965A

  • Polymer, positive resist composition, and resist pattern forming method

    WO2017130870A1

  • Resist pattern forming method

    WO2017130872A1

  • Polymer, positive resist composition, and resist pattern formation method

    WO2018123667A1

  • Method for forming resist pattern

    WO2019151021A1