Circuit board manufacturing method
Patent Information
- Application Number
- JP2020188233
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-11
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-11-11
AI Technical Summary
【0012】 本発明によれば、めっき焼けを抑制しつつ、微細配線を形成することができる、新規な回路基板の製造方法を提供することができる。
Smart Images

Figure 0007574616000001 
Figure 0007574616000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a circuit board. [Background technology]
[0002] In the manufacture of circuit boards such as wafer level packages (WLPs) and panel level packages (PLPs), redistribution layers are generally formed by applying a photosensitive material onto a wafer or panel substrate using a spin coating method, hardening it to form an insulating layer, and then forming a conductor layer using a sputtering method or the like, and repeating this process to create multiple layers.
[0003] As electronic devices become more sophisticated, circuit boards are required to have finer wiring. However, photosensitive materials tend to have inferior physical properties, such as insulation and thermal expansion coefficient, compared to thermosetting materials, making it difficult to further thin the insulating layer and limiting further fine wiring (finer wiring and higher density). Therefore, it is expected that insulating layers will be formed using thermosetting materials, which have excellent physical properties, such as insulation and thermal expansion coefficient (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-016647 A Summary of the Invention [Problem to be solved by the invention]
[0005] To achieve even finer wiring, it is necessary to make the conductor layer thinner, and it is also necessary to make the plating seed layer, which serves as the base for forming the conductor layer, thinner. In addition, when forming an insulating layer using a thermosetting material, it is necessary to perform a hole drilling process using a laser or the like and a desmear process to remove the resin residue (smear) generated by the hole drilling process.
[0006] In the desmear process, the surface of the insulating layer is also roughened, but when the roughness of the insulating layer surface becomes high, the thickness of the plating seed layer formed thereon becomes non-uniform due to the unevenness of the insulating layer surface. The inventors have found that the thin portion of the plating seed layer has a high electrical resistance value, so that in the subsequent electrolytic plating process, the growth of the plating is delayed, the formation of the conductor layer becomes insufficient, and it becomes difficult to form a uniform conductor layer. This problem was first discovered when an attempt was made to form a thin plating seed layer in order to realize finer wiring.
[0007] In addition, when forming a plating seed layer by sputtering, the conductor, which is the material of the plating seed layer, adheres to the surface of the insulating layer from above, so depending on the uneven structure of the insulating layer surface, there may be some parts where it is difficult to adhere the conductor, making it difficult to form the plating seed layer in some places. This causes the problem that it becomes even more difficult to form a uniform conductor layer.
[0008] Thus, the inventors have discovered that when an insulating layer is formed using a thermosetting material and a thin conductor layer is then formed on the surface thereof in order to achieve even finer wiring, the conductor layer formed becomes uneven, a phenomenon known as plating burn.
[0009] An object of the present invention is to provide a novel method for manufacturing a circuit board, which is capable of forming fine wiring while suppressing plating burn. [Means for solving the problem]
[0010] As a result of intensive research into solving the above problems, the present inventors have found that the above problems can be solved by a method for manufacturing a circuit board having the following configuration, and have thus completed the present invention.
[0011] That is, the present invention includes the following. [1] (X) A process for forming a plating seed layer on the surface of the insulating layer Including, A method for producing a circuit board, wherein the thickness of a plating seed layer is 250 nm or less, and the arithmetic mean roughness (Ra) of an insulating layer surface is 100 nm or less. [2] The thickness of the plating seed layer is D s (nm), and Ra of the insulating layer surface is Ra i (nm), 1≦D s / Ra i The method according to claim 1, wherein [3] The method according to [1] or [2], wherein in the step (X), a plating seed layer is formed by a sputtering method. [4] The method according to any one of [1] to [3], comprising a step of forming a conductor layer on the plating seed layer by electrolytic plating. [5] The method according to [4], wherein the line / space ratio (L / S) of the conductor layer is 5 / 5 μm or less. [6] Before step (X), (1) a step of laminating a resin sheet including a support and a thermosetting resin composition layer provided on the support onto a substrate such that the thermosetting resin composition layer is bonded to the substrate; (2) a step of thermally curing the thermosetting resin composition layer to form an insulating layer; (3) drilling holes in the insulating layer; and (4) Desmearing the insulating layer The method according to any one of [1] to [5], comprising: [7] The method according to [6], wherein the thermosetting resin composition layer contains an active ester-based curing agent. [8] The method according to any one of [1] to [7], wherein the circuit board is a wafer level package or a panel level package. Effect of the Invention
[0012] According to the present invention, it is possible to provide a novel method for manufacturing a circuit board, which is capable of forming fine wiring while suppressing plating burn. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described in detail below with reference to preferred embodiments. However, the present invention is not limited to the following embodiments and examples, and can be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.
[0014] [Circuit board manufacturing method] The method for producing a circuit board of the present invention (hereinafter, also simply referred to as the "production method of the present invention") is as follows: (X) A process for forming a plating seed layer on the surface of the insulating layer Including, The plating seed layer is characterized in that the thickness is 250 nm or less, and the insulating layer surface has an arithmetic mean roughness (Ra) of 100 nm or less.
[0015] In forming a rewiring layer in a circuit board such as WLP or PLP, the thickness of a plating seed layer serving as a base for a conductor layer is generally set to about 600 nm to 1000 nm. When forming such a relatively thick plating seed layer, there was no problem of plating burn occurring when forming a conductor layer on the plating seed layer by electrolytic plating.
[0016] In order to meet the recent demand for finer wiring (finer and denser wiring), the present inventors have attempted to form an insulating layer using a thermosetting material and a thin plating seed layer on the surface of the insulating layer, and have found that the thickness of the conductor layer formed on the plating seed layer by electrolytic plating varies, resulting in the problem of plating burn. When an insulating layer is formed using a thermosetting material, the surface roughness of the insulating layer tends to be high due to desmearing performed after drilling, and when a thin plating seed layer is formed on the surface of such an insulating layer, the thickness of the plating seed layer is likely to be non-uniform due to the unevenness of the insulating layer surface. In this case, the electrical resistance value of the thin plating seed layer is higher than that of the thick plating seed layer, and when a conductor layer is formed on the thin plating seed layer by electrolytic plating, the plating growth is delayed in the thin plating seed layer and high electrical resistance value parts compared to other parts, resulting in insufficient formation of the conductor layer. It is presumed that plating burn occurs due to such non-uniformity in the thickness of the plating seed layer.
[0017] In contrast, the manufacturing method of the present invention, which includes a step of forming a plating seed layer having a thickness of 250 nm or less on the surface of an insulating layer having an arithmetic mean roughness (Ra) of 100 nm or less, makes it possible to form a thin conductor layer with a line / space ratio (L / S) of 5 / 5 μm or less while significantly suppressing plating burn, and significantly contributes to the further fine wiring that has been required in recent years.
[0018] In the manufacturing method of the present invention, even if the thickness of the plating seed layer is made thinner, it is possible to suppress plating burn and achieve the desired effect. For example, the thickness of the plating seed layer may be preferably 240 nm or less, 220 nm or less, or 200 nm or less, more preferably 180 nm or less, 160 nm or less, or 150 nm or less, and even more preferably 140 nm or less, 120 nm or less, or 100 nm or less. After forming a conductor layer in a desired pattern on the plating seed layer, unnecessary parts other than the conductor layer forming part are removed by etching or the like. At this time, the thinner the plating seed layer is, the easier it is to remove the unnecessary parts of the plating seed layer, and the erosion of the conductor pattern when removing the unnecessary parts can be minimized, which is advantageous in realizing fine wiring.
[0019] The plating seed layer includes at least a conductive seed layer. The conductive seed layer is a layer that functions as an electrode in an electrolytic plating method. The conductive material constituting the conductive seed layer is not particularly limited as long as it exhibits sufficient conductivity, and suitable examples include copper, palladium, gold, platinum, silver, aluminum, and alloys thereof. The plating seed layer may also include a diffusion barrier layer. The diffusion barrier layer is a layer that prevents the conductive material constituting the conductive seed layer from diffusing into the insulating layer and causing dielectric breakdown. In addition, the material constituting the diffusion barrier layer is not particularly limited as long as it can suppress or prevent the diffusion of the conductive material constituting the conductive seed layer, and suitable examples include titanium, tungsten, tantalum, and alloys thereof. When the plating seed layer includes a diffusion barrier layer, the "thickness of the plating seed layer" in the present invention refers to the average thickness of the entire plating seed layer including not only the conductive seed layer but also the diffusion barrier layer.
[0020] When the plating seed layer includes a diffusion barrier layer, the thickness of the diffusion barrier layer is not particularly limited as long as it can suppress or prevent the diffusion of the conductive material constituting the conductive seed layer, but from the viewpoint of contributing to fine wiring, it is preferably 20 nm or less, more preferably 15 nm or less, and even more preferably 10 nm or less. The lower limit of the thickness of the diffusion barrier layer is not particularly limited, and may be, for example, 1 nm or more, 3 nm or more, 5 nm or more, etc. In this case, the remainder of the plating seed layer is preferably a conductive seed layer, and the thickness of the conductive seed layer may be determined so that the thickness of the entire plating seed layer is in the above-mentioned preferred range in relation to the thickness of the diffusion barrier layer.
[0021] From the viewpoint of suppressing plating burn and realizing further fine wiring, the thickness of the plating seed layer is set to D s (nm), and Ra of the insulating layer surface is Ra i (nm), 1≦D s / Ra i When such conditions are satisfied, even if the thickness of the plating seed layer is as small as 90 nm or less, 80 nm or less, 70 nm or less, 60 nm or less, or 50 nm or less, it is possible to form a thin conductor layer with a small L / S while suppressing plating burn, which is preferable. s / Ra i The upper limit of the ratio is preferably 8 or less, more preferably 6 or less, and further preferably 5 or less, 4 or less, 3.5 or less, or 3 or less, from the viewpoint of realizing fine wiring with good adhesion strength.
[0022] In the manufacturing method of the present invention, the step (X) is not particularly limited as long as the above-mentioned thickness of the plating seed layer and Ra of the insulating layer surface can be achieved.
[0023] For example, in step (X), the plating seed layer may be formed by dry plating or wet plating. Examples of dry plating include physical vapor deposition (PVD) methods such as sputtering, ion plating, and vacuum deposition, and chemical vapor deposition (CVD) methods such as thermal CVD and plasma CVD. Examples of wet plating include electroless plating. Dry plating is preferred from the viewpoint of forming a thin plating seed layer with a more uniform thickness, and sputtering is particularly preferred from the viewpoint of realizing fine wiring with excellent adhesion strength. Therefore, in a preferred embodiment, the plating seed layer is formed by sputtering in step (X).
[0024] The manufacturing method of the present invention includes, after step (X), a step of forming a conductive layer on the plating seed layer by electrolytic plating.
[0025] In the manufacturing method of the present invention, a thin plating seed layer with a uniform thickness can be formed in step (X), and plating burns can be significantly reduced when a conductor layer is formed on the plating seed layer by electrolytic plating. As a result, the manufacturing method of the present invention can form fine wiring while suppressing plating burns.
[0026] The conductor layer may be formed by a so-called semi-additive method. That is, a plating resist is formed on the plating seed layer formed in step (X) to expose a part of the plating seed layer corresponding to the desired wiring pattern. Next, a conductor layer is formed on the exposed plating seed layer by electrolytic plating, and then the plating resist is removed. Thereafter, unnecessary plating seed layer other than the conductor layer forming portion is removed by etching or the like, and a conductor layer having a desired wiring pattern (hereinafter also referred to as a "conductor pattern") can be formed.
[0027] According to the manufacturing method of the present invention, which can form a thin plating seed layer with a uniform thickness, it is possible to form a thin conductor pattern with a small L / S while suppressing plating burns.
[0028] According to the manufacturing method of the present invention, a conductor pattern having an L / S of preferably 5 / 5 μm or less, more preferably 4 / 4 μm or less, and even more preferably 3 / 3 μm or less or 2 / 2 μm or less can be formed while suppressing plating burns, and even a conductor pattern having an L / S of 1 / 1 μm can be formed without plating burns. According to the manufacturing method of the present invention, such a conductor pattern having a small L / S can be formed with a thickness of preferably 2 μm or less, 1.5 μm or less, or 1 μm or less. The lower limit of the thickness of the conductor pattern can be, for example, 0.5 μm or more, 0.6 μm or more, etc.
[0029] The manufacturing method of the present invention makes it possible to obtain excellent effects inherent in forming an insulating layer using a thermosetting material (i.e., the ability to form a thin insulating layer with excellent properties), while forming fine wiring without the problem of plating burn, and therefore significantly contributes to the fine wiring of circuit boards.
[0030] The manufacturing method of the present invention will be described below with reference to a particularly preferred embodiment in which an insulating layer is formed using a thermosetting material.
[0031] In a preferred embodiment, the production method of the present invention further comprises the steps of: (1) a step of laminating a resin sheet including a support and a thermosetting resin composition layer provided on the support onto a substrate such that the thermosetting resin composition layer is bonded to the substrate; (2) a step of thermally curing the thermosetting resin composition layer to form an insulating layer; (3) drilling holes in the insulating layer; and (4) Desmearing the insulating layer Includes.
[0032] <Resin sheet> Before describing each step, a resin sheet that is preferably used in the manufacturing method of the present invention will be described.
[0033] In a preferred embodiment, the resin sheet includes a support and a thermosetting resin composition layer provided on the support.
[0034] Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.
[0035] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polycarbonate (PC), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.
[0036] When a metal foil is used as the support, examples of the metal foil include copper foil, aluminum foil, etc., and copper foil is preferred. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.
[0037] The support may be subjected to a matte treatment or a corona treatment on the surface on the side to be bonded to the thermosetting resin composition layer. In addition, the support may be a support with a release layer having a release layer on the surface on the side to be bonded to the thermosetting resin composition layer. Examples of the release agent used in the release layer of the support with a release layer include one or more release agents selected from the group consisting of alkyd resins, olefin resins, urethane resins, and silicone resins. Examples of commercially available release agents include alkyd resin-based release agents such as "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation.
[0038] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When the support is a support with a release layer, the total thickness of the support with a release layer is preferably in the above range.
[0039] In the resin sheet, the thermosetting resin composition layer (hereinafter, simply referred to as "resin composition layer") contains a thermosetting resin as a resin. As the thermosetting resin, a conventionally known thermosetting resin used in forming a circuit board can be used, and among them, it is preferable that the thermosetting resin contains an epoxy resin from the viewpoint of easily forming an insulating layer with a small surface roughness after a desmear treatment.
[0040] -Epoxy resin- The epoxy resin means a curable resin having an epoxy group. The epoxy resin may be used alone or in combination of two or more kinds.
[0041] Examples of epoxy resins include bixylenol type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AF type epoxy resins, hydrogenated bisphenol A type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol novolac type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, naphthalene type epoxy resins, naphthol type epoxy resins, anthracene type epoxy resins, glycidylamine type epoxy resins, glycidyl esters, and the like. Examples of epoxy resins that can be used include aryl epoxy resins, cresol novolac epoxy resins, phenol aralkyl epoxy resins, biphenyl epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane epoxy resins, cyclohexane dimethanol epoxy resins, naphthylene ether epoxy resins, trimethylol epoxy resins, tetraphenylethane epoxy resins, isocyanurate epoxy resins, phenolphthalimidine epoxy resins, and phenolphthalein epoxy resins.
[0042] The resin composition layer preferably contains, as an epoxy resin, an epoxy resin having two or more epoxy groups in one molecule. The proportion of the epoxy resin having two or more epoxy groups in one molecule relative to 100% by mass of the non-volatile components of the epoxy resin is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more.
[0043] Epoxy resins include epoxy resins that are solid at a temperature of 25° C. (hereinafter also referred to as "solid epoxy resins") and epoxy resins that are liquid at a temperature of 25° C. (hereinafter also referred to as "liquid epoxy resins"). In the resin sheet, the resin composition layer may contain only a solid epoxy resin as the epoxy resin, or may contain only a liquid epoxy resin, or may contain a combination of a solid epoxy resin and a liquid epoxy resin.
[0044] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferable.
[0045] Preferred solid epoxy resins include bixylenol type epoxy resins, naphthalene type epoxy resins, naphthalene type tetrafunctional epoxy resins, naphthol novolac type epoxy resins, cresol novolac type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol type epoxy resins, biphenyl type epoxy resins, naphthylene ether type epoxy resins, anthracene type epoxy resins, bisphenol A type epoxy resins, bisphenol AF type epoxy resins, phenol aralkyl type epoxy resins, tetraphenylethane type epoxy resins, phenolphthalimidine type epoxy resins, and phenolphthalein type epoxy resins.
[0046] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins) manufactured by DIC Corporation; "N-690" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "HP-7200", "HP-7200HH", "HP-7200H", and "HP-7200L" (dicyclopentadiene type epoxy resins) manufactured by DIC Corporation; and "EXA-7311" manufactured by DIC Corporation. "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", "HP6000", "HP6000L" (naphthylene ether type epoxy resin); "EPPN-502H" (trisphenol type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC7000L" (naphthol novolac type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC3000H", "NC3000", "NC3000L", "NC3000FH", "NC3100" (biphenyl type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN 475V" (naphthalene type epoxy resin); "ESN485" (naphthol type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN375" (dihydroxynaphthalene type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YX4000H", "YX4000", "YX4000HK", "YL7890" (bixylenol type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YL6121" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX8800" (anthracene type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "Y Examples of epoxy resins include "X7700" (phenol aralkyl type epoxy resin); "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals; "YX7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical; "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical; "jER1010" (bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical; "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical; and "WHR991S" (phenolphthalimidine type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.These may be used alone or in combination of two or more.
[0047] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.
[0048] Preferred liquid epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AF type epoxy resins, hydrogenated bisphenol A type epoxy resins, naphthalene type epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, phenol novolac type epoxy resins, alicyclic epoxy resins having an ester skeleton, cyclohexane type epoxy resins, cyclohexane dimethanol type epoxy resins, and epoxy resins having a butadiene structure.
[0049] Specific examples of liquid epoxy resins include "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "828EL", "jER828EL", and "825" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630", "630LSD", and "604" (glycidylamine type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "ED-523T" (glycilol type epoxy resin) manufactured by ADEKA Corporation; "EP-3950L" and "EP-3980S" (glycidylamine type epoxy resins) manufactured by ADEKA Corporation; and "EP-4088S" (glycidylamine type epoxy resins) manufactured by ADEKA Corporation. Examples of such epoxy resins include: "ZX1059" manufactured by Nippon Steel Chemical & Material Co., Ltd. (a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin); "EX-721" manufactured by Nagase Chemtex Corporation (glycidyl ester type epoxy resin); "Celloxide 2021P" manufactured by Daicel Corporation (alicyclic epoxy resin having an ester skeleton); "PB-3600" manufactured by Daicel Corporation, "JP-100" and "JP-200" manufactured by Nippon Soda Co., Ltd. (epoxy resin having a butadiene structure); "ZX1658" and "ZX1658GS" manufactured by Nippon Steel Chemical & Material Co., Ltd. (1,4-glycidylcyclohexane type epoxy resin), "YX8000" manufactured by Mitsubishi Chemical Corporation (hydrogenated bisphenol A type epoxy resin), and "KF-101" manufactured by Shin-Etsu Chemical Co., Ltd. (epoxy modified silicone resin). These may be used alone or in combination of two or more types.
[0050] The epoxy resin may be any one of a solid epoxy resin, a liquid epoxy resin, or a combination thereof. From the viewpoint of easily realizing an insulating layer with a small surface roughness after a desmear treatment, it is preferable to contain a solid epoxy resin alone or a solid epoxy resin and a liquid epoxy resin in combination.
[0051] When a solid epoxy resin and a liquid epoxy resin are used in combination as the epoxy resin, the mass ratio thereof (solid epoxy resin:liquid epoxy resin) is preferably 40:1 to 1:10, more preferably 30:1 to 1:5, and particularly preferably 20:1 to 1:1.
[0052] The epoxy equivalent of the epoxy resin is preferably 50 g / eq. to 5,000 g / eq., more preferably 60 g / eq. to 1,000 g / eq., even more preferably 80 g / eq. to 500 g / eq., and even more preferably 100 g / eq. to 300 g / eq. The epoxy equivalent is the mass of the resin per equivalent of epoxy group. This epoxy equivalent can be measured according to JIS K7236.
[0053] The weight average molecular weight (Mw) of the epoxy resin is preferably from 100 to 5,000, more preferably from 250 to 3,000, and further preferably from 400 to 1500. The weight average molecular weight of the resin can be measured by gel permeation chromatography (GPC) as a polystyrene-equivalent value.
[0054] When the resin component in the resin composition is 100% by mass, the content of the epoxy resin is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more, and is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less. In the present invention, the "resin component" refers to the non-volatile components constituting the resin composition layer, excluding the inorganic filler described below.
[0055] In the resin sheet, the resin composition layer may further contain other components. Examples of such other components include a curing agent, an inorganic filler, a thermoplastic resin, a curing accelerator, and other additives. Each component will be described in detail below.
[0056] - Hardener - The resin composition layer may contain a curing agent. The curing agent has a function of reacting with the epoxy resin to cure the resin composition. The curing agent may be used alone or in combination of two or more kinds.
[0057] The curing agent is not particularly limited, but examples thereof include active ester curing agents, phenol curing agents, naphthol curing agents, carbodiimide curing agents, acid anhydride curing agents, amine curing agents, benzoxazine curing agents, cyanate ester curing agents, and thiol curing agents. From the viewpoint of easily realizing an insulating layer with a small surface roughness after desmearing, it is preferable that the curing agent contains an active ester curing agent. Therefore, in a preferred embodiment, the thermosetting resin composition layer in the resin sheet contains an active ester curing agent.
[0058] As the active ester curing agent, a compound having one or more active ester groups in one molecule can be used. Among them, as the active ester curing agent, a compound having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, is preferred. The active ester curing agent is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester curing agent obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester curing agent obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound is more preferred.
[0059] Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid.
[0060] Examples of phenol compounds or naphthol compounds include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, the term "dicyclopentadiene-type diphenol compounds" refers to diphenol compounds obtained by condensing one molecule of dicyclopentadiene with two molecules of phenol.
[0061] Preferred specific examples of the active ester curing agent include an active ester curing agent containing a dicyclopentadiene-type diphenol structure, an active ester curing agent containing a naphthalene structure, an active ester curing agent containing an acetylated product of phenol novolac, and an active ester curing agent containing a benzoylated product of phenol novolac. Among them, an active ester curing agent containing a naphthalene structure and an active ester curing agent containing a dicyclopentadiene-type diphenol structure are more preferred. The "dicyclopentadiene-type diphenol structure" refers to a divalent structural unit consisting of phenylene-dicyclopentylene-phenylene.
[0062] Commercially available active ester compounds include "EXB9451", "EXB9460", "EXB9460S", "EXB-8000L", "EXB-8000L-65M", "EXB-8000L-65TM", "HPC-8000L-65TM", "HPC-8000", "HPC-8000-65T", "HPC-8000H", and "HPC-8000H-65TM" (manufactured by DIC Corporation) as active ester compounds containing a dicyclopentadiene-type diphenol structure; and "EXB-8100L-65T", "EXB-8150-60T", and "EXB-8150-62T" as active ester compounds containing a naphthalene structure. , "EXB-9416-70BK", "HPC-8150-60T", and "HPC-8150-62T" (manufactured by DIC Corporation); an active ester compound containing phosphorus, "EXB9401" (manufactured by DIC Corporation), an active ester compound which is an acetylated product of phenol novolac, "DC808" (manufactured by Mitsubishi Chemical Corporation), active ester compounds which are benzoylated products of phenol novolac, "YLH1026", "YLH1030", and "YLH1048" (manufactured by Mitsubishi Chemical Corporation), and an active ester compound containing a styryl group and a naphthalene structure, "PC1300-02-65MA" (manufactured by Air Water Inc.), etc.
[0063] As the phenol-based curing agent and naphthol-based curing agent, those having a novolac structure are preferred from the viewpoint of heat resistance and water resistance. Also, from the viewpoint of adhesion to the conductor layer, nitrogen-containing phenol-based curing agents and nitrogen-containing naphthol-based curing agents are preferred, and triazine skeleton-containing phenol-based curing agents and triazine skeleton-containing naphthol-based curing agents are more preferred.
[0064] Specific examples of phenol-based curing agents and naphthol-based curing agents include, for example, "MEH-7700", "MEH-7810", "MEH-7851", and "MEH-8000H" manufactured by Meiwa Chemical Industry Co., Ltd.; "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd.; and "SN-170", "SN-180", "SN-190", "SN-475", "SN-485", "SN-495", "SN-495V", and "SN-37" manufactured by Nippon Steel Chemical & Material Co., Ltd. 5" and "SN-395" manufactured by DIC Corporation; "TD-2090", "TD-2090-60M", "LA-7052", "LA-7054", "LA-1356", "LA-3018", "LA-3018-50P", "EXB-9500", "HPC-9500", "KA-1160", "KA-1163", and "KA-1165" manufactured by Gun-ei Chemical Co., Ltd.; and the like.
[0065] The carbodiimide-based curing agent is a curing agent having two or more carbodiimide structures in one molecule, and examples of the curing agent include aliphatic biscarbodiimides such as tetramethylene-bis(t-butylcarbodiimide) and cyclohexane bis(methylene-t-butylcarbodiimide); aromatic biscarbodiimides such as phenylene-bis(xylylcarbodiimide); aliphatic polycarbodiimides such as polyhexamethylenecarbodiimide, polytrimethylhexamethylenecarbodiimide, polycyclohexylenecarbodiimide, poly(methylenebiscyclohexylenecarbodiimide), and poly(isophoronecarbodiimide); Examples of polycarbodiimides include aromatic polycarbodiimides such as poly(methylenediphenylenecarbodiimide), poly(naphthylenecarbodiimide), poly(tolylenecarbodiimide), poly(methyldiisopropylphenylenecarbodiimide), poly(triethylphenylenecarbodiimide), poly(diethylphenylenecarbodiimide), poly(triisopropylphenylenecarbodiimide), poly(diisopropylphenylenecarbodiimide), poly(xylylenecarbodiimide), poly(tetramethylxylylenecarbodiimide), poly(methylenediphenylenecarbodiimide), and poly[methylenebis(methylphenylene)carbodiimide].
[0066] Commercially available carbodiimide curing agents include, for example, "Carbodilite V-02B", "Carbodilite V-03", "Carbodilite V-04K", "Carbodilite V-07", and "Carbodilite V-09" manufactured by Nisshinbo Chemical Inc.; and "Stavaxol P", "Stavaxol P400", and "Hi-Kasil 510" manufactured by Rhein Chemie.
[0067] The acid anhydride curing agent is a curing agent having one or more carboxylic acid anhydride groups (-CO-O-CO-) in one molecule, and examples thereof include phthalic anhydride, pyromellitic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-diphenylethertetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, methylene-4,4' aromatic acid anhydride-based hardeners such as tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenylsuccinic anhydride, cyclopentanetetracarboxylic dianhydride, cyclohexane-1,2,4,5-tetracarboxylic dianhydride, and the like; and polymeric anhydride-based hardeners such as styrene / maleic anhydride copolymer, and alkyl (meth)acrylate / styrene / maleic anhydride copolymer. Commercially available acid anhydride curing agents include "HNA-100", "MH-700", "MTA-15", "DDSA", and "OSA" manufactured by New Japan Chemical Co., Ltd., "YH-306" and "YH-307" manufactured by Mitsubishi Chemical Corporation, and "HN-2200" and "HN-5500" manufactured by Hitachi Chemical Co., Ltd.
[0068] The amine-based curing agent is a curing agent having two or more amino groups, and examples thereof include aliphatic amines, polyether amines, alicyclic amines, and aromatic amines. Among them, aromatic amines are preferred from the viewpoint of achieving the desired effects of the present invention. The amine-based curing agent is preferably a primary amine or a secondary amine, and more preferably a primary amine. Specific examples of the amine-based curing agent include 4,4'-methylenebis(2,6-dimethylaniline), 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, m-phenylenediamine, m-xylylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenylether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, 2,2-bis(3-amino-4-hydroxyphenyl)propane, and the like. propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, bis(4-(3-aminophenoxy)phenyl)sulfone, and the like. As the amine-based curing agent, commercially available products may be used, and examples thereof include "SEIKACURE-S" manufactured by Seika Corporation, "KAYABOND C-200S", "KAYABOND C-100", "KAYAHARD AA", "KAYAHARD AB", and "KAYAHARD AS" manufactured by Nippon Kayaku Co., Ltd., and "Epicure W" manufactured by Mitsubishi Chemical Corporation.
[0069] Specific examples of benzoxazine-based curing agents include "JBZ-OP100D" and "ODA-BOZ" manufactured by JFE Chemical Corporation; "HFB2006M" manufactured by Showa Polymer Co., Ltd.; and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.
[0070] Examples of the cyanate ester curing agent include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate (oligo(3-methylene-1,5-phenylene cyanate)), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester-based curing agents include "PT30" and "PT60" (both of which are phenol novolac-type multifunctional cyanate ester resins), "BA230" and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been converted to triazine to form a trimer), all of which are manufactured by Lonza Japan.
[0071] The thiol-based curing agent is a curing agent having two or more mercapto groups, and examples thereof include trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), and tris(3-mercaptopropyl)isocyanurate.
[0072] The reactive group equivalent of the curing agent is preferably 50 g / eq. to 3000 g / eq., more preferably 100 g / eq. to 1000 g / eq., further preferably 100 g / eq. to 500 g / eq., and particularly preferably 100 g / eq. to 300 g / eq. The reactive group equivalent is the mass of the curing agent per equivalent of reactive group. For example, the reactive group is an active ester group in the case of an active ester curing agent, and a phenolic hydroxyl group in the case of a phenol curing agent. In the case of an acid anhydride curing agent, one equivalent of a carboxylic anhydride group (-CO-O-CO-) corresponds to two equivalents of reactive group.
[0073] When the resin component in the resin composition is 100% by mass, the content of the curing agent is preferably 3% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, and is preferably 40% by mass or less, more preferably 30% by mass or less, even more preferably 25% by mass or less or 20% by mass or less.
[0074] -Inorganic filler- In the resin sheet, the resin composition layer may contain an inorganic filler. By containing an inorganic filler, an insulating layer having good thermal properties can be realized.
[0075] Examples of inorganic filler materials include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium titanate zirconate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica is particularly suitable. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. In addition, spherical silica is preferred as the silica. The inorganic filler may be used alone or in combination of two or more.
[0076] Commercially available inorganic fillers include, for example, "UFP-30" manufactured by Denka Chemical Industry Co., Ltd.; "SP60-05" and "SP507-05" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", and "YA010C" manufactured by Admatechs; "UFP-30" manufactured by Denka Company; "Silfill NSS-3N", "Silfill NSS-4N", and "Silfill NSS-5N" manufactured by Tokuyama Corporation; "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs; and "DAW-03" and "FB-105FD" manufactured by Denka Company.
[0077] From the viewpoint of easily realizing an insulating layer with a small surface roughness after desmearing, the average particle size of the inorganic filler is preferably 3 μm or less, more preferably 2 μm or less, and even more preferably 1 μm or less, 0.8 μm or less, 0.6 μm or less, 0.5 μm or less, 0.4 μm or less, or 0.3 μm or less. The lower limit of the average particle size is not particularly limited, but is preferably 0.01 μm or more, more preferably 0.05 μm or more, and even more preferably 0.07 μm or more, 0.1 μm or more, or 0.2 μm or more. The average particle size of the inorganic filler can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, the particle size distribution of the inorganic filler is created on a volume basis using a laser diffraction / scattering type particle size distribution measuring device, and the median diameter is used as the average particle size. The measurement sample can be prepared by weighing 100 mg of the inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing it by ultrasonic waves for 10 minutes. The measurement sample was measured using a laser diffraction type particle size distribution measuring device with blue and red light source wavelengths, and the particle size distribution of the inorganic filler on a volume basis was measured using a flow cell method, and the average particle size was calculated as the median diameter from the particle size distribution obtained. An example of a laser diffraction type particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.
[0078] The specific surface area of the inorganic filler is not particularly limited, but is preferably 0.1 m 2 / g or more, more preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, 3m 2 / g or more or 5m 2 The upper limit of the specific surface area is not particularly limited, but is preferably 100 m 2 / g or less, more preferably 80m 2 / g or less, more preferably 60m 2 / g or less, 50m 2 / g or less or 40m 2The specific surface area of the inorganic filler is obtained by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountech Co., Ltd.) according to the BET method, and calculating the specific surface area using the BET multipoint method.
[0079] The inorganic filler is preferably surface-treated with a suitable surface treatment agent. By performing the surface treatment, the moisture resistance and dispersibility of the inorganic filler can be improved. Examples of the surface treatment agent include silane coupling agents such as vinyl silane coupling agents, epoxy silane coupling agents, styryl silane coupling agents, (meth)acrylic silane coupling agents, amino silane coupling agents, isocyanurate silane coupling agents, ureido silane coupling agents, mercapto silane coupling agents, isocyanate silane coupling agents, and acid anhydride silane coupling agents; non-silane coupling-alkoxysilane compounds such as methyltrimethoxysilane and phenyltrimethoxysilane; and silazane compounds. The surface treatment agent may be used alone or in combination of two or more.
[0080] Examples of commercially available surface treatment agents include Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), and Shin-Etsu Chemical Co., Ltd.'s "SZ-31" (hexamethyldisilazane).
[0081] The degree of surface treatment with the surface treatment agent is preferably within a predetermined range from the viewpoint of improving the dispersibility of the inorganic filler. Specifically, it is preferable that 100% by mass of the inorganic filler is surface-treated with 0.2 to 5% by mass of the surface treatment agent.
[0082] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of the inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of preventing an increase in the melt viscosity of the resin composition layer or the melt viscosity in the form of a sheet, it is more preferable that the melt viscosity is 1.0 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is more preferable. The amount of carbon per unit surface area of the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the amount of carbon per unit surface area of the inorganic filler can be measured using a carbon analyzer. As the carbon analyzer, an "EMIA-320V" manufactured by Horiba, Ltd., or the like can be used.
[0083] When the resin composition layer contains an inorganic filler, the content of the inorganic filler in the resin composition layer is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 45% by mass or more, 50% by mass or more, 55% by mass or more, 60% by mass or more, or 65% by mass or more, when the non-volatile components in the resin composition layer are taken as 100% by mass, from the viewpoint of realizing an insulating layer with good thermal properties such as a low linear thermal expansion coefficient. The upper limit of the content of the inorganic filler is not particularly limited, but is preferably 85% by mass or less, more preferably 80% by mass or less, or 75% by mass or less.
[0084] -Thermoplastic resin- In the resin sheet, the resin composition layer may contain a thermoplastic resin. The thermoplastic resin may be used alone or in combination of two or more kinds.
[0085] Examples of thermoplastic resins include phenoxy resins, polyvinyl acetal resins, acrylic resins, polyolefin resins, polybutadiene resins, polyimide resins, polyamideimide resins, polysulfone resins, polyethersulfone resins, polyphenylene ether resins, polyetherimide resins, polycarbonate resins, polyetheretherketone resins, and polyester resins. Of these, resins selected from phenoxy resins, acrylic resins, and polyphenylene ether resins are preferred.
[0086] Examples of the phenoxy resin include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenolacetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group. The phenoxy resin may be used alone or in combination of two or more. Specific examples of phenoxy resins include "1256" and "4250" (both of which are phenoxy resins containing a bisphenol A skeleton), "YX8100" (phenoxy resin containing a bisphenol S skeleton), and "YX6954" (phenoxy resin containing a bisphenol acetophenone skeleton) manufactured by Mitsubishi Chemical Corporation, "FX280" and "FX293" manufactured by Nippon Steel Chemical & Material Co., Ltd., and "YX7200B35", "YX7500BH30", "YX6954BH30", "YX7553", "YX7553BH30", "YL7769BH30", "YL6794", "YL7213", "YL7290", and "YL7482" manufactured by Mitsubishi Chemical Corporation.
[0087] Examples of polyvinyl acetal resin include polyvinyl formal resin and polyvinyl butyral resin, and polyvinyl butyral resin is preferred.Specific examples of polyvinyl acetal resin include "Denka Butyral 4000-2", "Denka Butyral 5000-A", "Denka Butyral 6000-C", and "Denka Butyral 6000-EP" manufactured by Denki Kagaku Kogyo Co., Ltd., and S-LEC BH series, BX series (e.g. BX-5Z), KS series (e.g. KS-1), BL series, and BM series manufactured by Sekisui Chemical Co., Ltd.
[0088] The acrylic resin refers to a polymer obtained by polymerizing a monomer component including a (meth)acrylic acid ester monomer. The monomer components constituting the acrylic resin may contain, in addition to the (meth)acrylic acid ester monomer, a (meth)acrylamide monomer, a styrene monomer, a functional group-containing monomer, or the like as copolymerization components. Specific examples of acrylic resins include "ARUFON UP-1000", "ARUFON UP-1010", "ARUFON UP-1020", "ARUFON UP-1021", "ARUFON UP-1061", "ARUFON UP-1080", "ARUFON UP-1110", "ARUFON UP-1170", "ARUFON UP-1190", "ARUFON UP-1500", "ARUFON UH-2000", "ARUFON UH-2041", "ARUFON UH-2190", "ARUFON UHE-2012", "ARUFON UC-3510", "ARUFON UG-4010", "ARUFON US-6100", and "ARUFON US-6170", all manufactured by Toagosei Co., Ltd. These may be used alone or in combination of two or more.
[0089] Examples of polyolefin resins include ethylene-based copolymer resins such as low-density polyethylene, very low-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-methyl acrylate copolymer; and polyolefin-based elastomers such as polypropylene and ethylene-propylene block copolymer.
[0090] Examples of polybutadiene resins include hydrogenated polybutadiene skeleton-containing resins, hydroxy group-containing polybutadiene resins, phenolic hydroxy group-containing polybutadiene resins, carboxy group-containing polybutadiene resins, acid anhydride group-containing polybutadiene resins, epoxy group-containing polybutadiene resins, isocyanate group-containing polybutadiene resins, urethane group-containing polybutadiene resins, polyphenylene ether-polybutadiene resins, and the like.
[0091] Specific examples of polyimide resins include "Rikacoat SN20" and "Rikacoat PN20" manufactured by New Japan Chemical Co., Ltd. Specific examples of polyimide resins also include modified polyimides such as linear polyimides obtained by reacting bifunctional hydroxyl-terminated polybutadiene, a diisocyanate compound, and a tetrabasic acid anhydride (polyimides described in JP-A-2006-37083), and polysiloxane skeleton-containing polyimides (polyimides described in JP-A-2002-12667 and JP-A-2000-319386, etc.).
[0092] Specific examples of polyamide-imide resins include "Viromax HR11NN" and "Viromax HR16NN" manufactured by Toyobo Co., Ltd. Specific examples of polyamide-imide resins also include modified polyamide-imides such as "KS9100" and "KS9300" (polysiloxane skeleton-containing polyamide-imide) manufactured by Hitachi Chemical Co., Ltd.
[0093] A specific example of the polyethersulfone resin is "PES5003P" manufactured by Sumitomo Chemical Co., Ltd.
[0094] Specific examples of polysulfone resins include polysulfones "P1700" and "P3500" manufactured by Solvay Advanced Polymers.
[0095] Specific examples of polyphenylene ether resins include oligophenylene ether-styrene resins "OPE-2St1200" and "OPE-2St2200" manufactured by Mitsubishi Gas Chemical Company, Inc., and "Noryl (registered trademark) SA90" manufactured by SABIC, etc. Specific examples of polyetherimide resins include "Ultem" manufactured by GE, etc.
[0096] Examples of polycarbonate resins include hydroxyl group-containing carbonate resins, phenolic hydroxyl group-containing carbonate resins, carboxyl group-containing carbonate resins, acid anhydride group-containing carbonate resins, isocyanate group-containing carbonate resins, and urethane group-containing carbonate resins. Specific examples of polycarbonate resins include "FPC0220" manufactured by Mitsubishi Gas Chemical Co., Ltd., "T6002" and "T6001" (polycarbonate diol) manufactured by Asahi Kasei Chemicals Corporation, and "C-1090", "C-2090", and "C-3090" (polycarbonate diol) manufactured by Kuraray Co., Ltd. Specific examples of polyether ether ketone resins include "Sumiploy K" manufactured by Sumitomo Chemical Co., Ltd. Examples of polyester resins include polyethylene terephthalate resins.
[0097] The weight average molecular weight of the thermoplastic resin is preferably 8,000 or more, more preferably 10,000 or more, and even more preferably 20,000 or more, and is preferably 100,000 or less, more preferably 70,000 or less, and even more preferably 60,000 or less. The weight average molecular weight of the resin can be measured as a polystyrene-equivalent value by gel permeation chromatography (GPC).
[0098] When the resin composition layer contains a thermoplastic resin, the content of the thermoplastic resin in the resin composition layer, when the resin component in the resin composition layer is 100 mass%, is preferably 50 mass% or less, more preferably 40 mass% or less, even more preferably 30 mass% or less, 20 mass% or less, or 10 mass% or less, and is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, and even more preferably 1 mass% or more.
[0099] -Curing accelerator- In the resin sheet, the resin composition layer may contain a curing accelerator.
[0100] Examples of the curing accelerator include phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, guanidine-based curing accelerators, metal-based curing accelerators, peroxide-based curing accelerators, etc. The curing accelerators may be used alone or in combination of two or more.
[0101] When the resin composition layer contains a curing accelerator, the content of the curing accelerator in the resin composition layer is preferably 0.001 mass% or more, more preferably 0.005 mass% or more, and even more preferably 0.01 mass% or more, when the resin component in the resin composition is 100 mass%, and is preferably 1 mass% or less, more preferably 0.8 mass% or less, 0.6 mass% or less, or 0.4 mass% or less.
[0102] -Other additives- In the resin sheet, the resin composition layer may further contain other additives. Examples of such other additives include organometallic compounds such as organic copper compounds, organic zinc compounds, and organic cobalt compounds; organic fillers such as rubber particles; colorants such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, and carbon black; polymerization inhibitors such as hydroquinone, catechol, pyrogallol, and phenothiazine; leveling agents such as silicone-based leveling agents and acrylic polymer-based leveling agents; thickeners such as bentone and montmorillonite; defoamers such as silicone-based defoamers, acrylic-based defoamers, fluorine-based defoamers, and vinyl resin-based defoamers; ultraviolet absorbers such as benzotriazole-based ultraviolet absorbers; adhesion improvers such as urea silane; triazole-based adhesion imparting agents, tetrazole-based adhesion imparting agents, and triazine-based adhesion imparting agents. Adhesion imparting agents such as adhesion imparting agents; antioxidants such as hindered phenol antioxidants and hindered amine antioxidants; fluorescent brighteners such as stilbene derivatives; surfactants such as fluorine-based surfactants and silicone-based surfactants; flame retardants such as phosphorus-based flame retardants (e.g., phosphate ester compounds, phosphazene compounds, phosphinic acid compounds, red phosphorus), nitrogen-based flame retardants (e.g., melamine sulfate), halogen-based flame retardants, and inorganic flame retardants (e.g., antimony trioxide); dispersants such as phosphate ester dispersants, polyoxyalkylene dispersants, acetylene dispersants, silicone-based dispersants, anionic dispersants, and cationic dispersants; stabilizers such as borate stabilizers, titanate stabilizers, aluminate stabilizers, zirconate stabilizers, isocyanate stabilizers, carboxylic acid stabilizers, and carboxylic anhydride stabilizers. Other additives may be used alone or in combination of two or more. The content of each can be appropriately set by those skilled in the art.
[0103] The resin sheet can be produced, for example, by preparing a liquid resin composition as is or a resin varnish by dissolving the resin composition in an organic solvent, applying this onto a support using a die coater or the like, and then drying to form a resin composition layer.
[0104] As the organic solvent, a known one can be appropriately used, and the type is not particularly limited. Examples of the organic solvent include ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, and γ-butyrolactone; ether-based solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, and diphenyl ether; alcohol-based solvents such as methanol, ethanol, propanol, butanol, and ethylene glycol; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, γ-butyrolactone, and methyl methoxypropionate. Examples of the organic solvent include ether ester solvents such as methyl lactate, ethyl lactate, and methyl 2-hydroxyisobutyrate; ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, and diethylene glycol monobutyl ether (butyl carbitol); amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone; sulfoxide solvents such as dimethyl sulfoxide; nitrile solvents such as acetonitrile and propionitrile; aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane; and aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. The organic solvent may be used alone or in combination of two or more in any ratio.
[0105] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is performed so that the content of the organic solvent in the resin composition layer becomes 10 mass % or less, preferably 5 mass % or less. Although it varies depending on the boiling point of the organic solvent in the resin composition (resin varnish), for example, when a resin composition (resin varnish) containing 30 mass % to 60 mass % of the organic solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 2 minutes to 10 minutes.
[0106] In one embodiment, the resin sheet may further include other layers as necessary. Examples of such other layers include a protective film equivalent to the support provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is not particularly limited, but is, for example, 1 to 40 μm. By laminating the protective film, adhesion of dirt and the like to the surface of the resin composition layer and scratches can be suppressed. When the resin sheet has a protective film, it can be used by peeling off the protective film.
[0107] Each step will be described below.
[0108] -Process (1)- In step (1), a resin sheet including a support and a thermosetting resin composition layer provided on the support is laminated onto a substrate such that the thermosetting resin composition layer is bonded to the substrate.
[0109] The resin sheet is as explained in the <Resin Sheet> section above.
[0110] The "substrate" used in step (1) is a circuit board that is stIn the case of manufacturing by the 1st chip method, a semiconductor wafer having a circuit element having a predetermined function and a plurality of electrode pads electrically connected to the circuit element may be used. The semiconductor wafer is preferably a silicon (Si)-based wafer, but is not limited thereto. For example, a wafer such as a gallium arsenide (GaAs)-based, an indium phosphide (InP)-based, a gallium phosphide (GaP)-based, a gallium nitride (GaN)-based, a gallium telluride (GaTe)-based, a zinc selenium (ZnSe)-based, or a silicon carbide (SiC)-based wafer may be used. The chip 1st method is a method in which a semiconductor chip is first provided and a rewiring layer is formed on the electrode pad surface (for example, JP 2002-289731 A, JP 2006-173345 A, etc.). In such a chip 1st method, particularly when manufacturing a package with a fan-out structure, a semiconductor wafer is first divided into individual pieces, and each semiconductor chip is arranged on a carrier (glass substrate, metal substrate, plastic substrate, etc.) at a distance from each other, and then sealed with resin, and a rewiring layer is formed on the exposed electrode pad surface and the sealing resin layer around it (for example, JP 2012-15191 A, JP 2015-126123 A, etc.). In such an embodiment, the "substrate" in step (1) may be a substrate in which the periphery of the divided semiconductor chip is sealed with sealing resin so that the electrode pad surface is exposed.
[0111] In addition, the circuit board is re-distributed to the first wiring layer (RDL-1 st In the case of manufacturing the semiconductor device by the 1st redistribution layer method, the "substrate" used in step (1) may be a substrate with a release layer (such as a glass substrate with a release layer, a metal substrate with a release layer, or a plastic substrate with a release layer). The 1st redistribution layer method is a method in which a redistribution layer is first provided, and a semiconductor chip is provided on the redistribution layer in such a state that the electrode pad surface of the semiconductor chip can be electrically connected to the redistribution layer (for example, JP 2015-35551 A, JP 2015-170767 A, etc.). In the 1st redistribution layer method, after providing the semiconductor chip on the redistribution layer, the substrate with the release layer is peeled off to expose the redistribution layer. Such a 1st redistribution layer method is particularly suitable for manufacturing a package with a fan-out structure.
[0112] The substrate and the resin sheet can be laminated, for example, by thermocompression bonding the resin sheet to the substrate from the support side. Examples of the member for thermocompression bonding the resin sheet to the substrate (hereinafter also referred to as "thermocompression bonding member") include a heated metal plate (such as a SUS plate) or a metal roll (SUS roll). It is preferable to press the thermocompression bonding member not directly onto the resin sheet, but via an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the substrate.
[0113] The lamination of the substrate and the resin sheet may be performed by a vacuum lamination method. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the thermocompression pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination is preferably performed under reduced pressure conditions of 26.7hPa or less.
[0114] The lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch type vacuum pressure laminator.
[0115] After lamination, the laminated resin sheet may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the support side. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. The lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.
[0116] -Process (2)- In step (2), the thermosetting resin composition layer is thermally cured to form an insulating layer.
[0117] The curing conditions for the resin composition layer are not particularly limited, and conditions that are usually adopted when forming an insulating layer for a circuit board may be used.
[0118] For example, the thermal curing conditions for the resin composition layer vary depending on the type of resin composition, etc., but in one embodiment, the curing temperature is preferably 120° C. to 250° C., more preferably 150° C. to 240° C., and even more preferably 180° C. to 230° C. The curing time can be preferably 5 minutes to 240 minutes, more preferably 10 minutes to 150 minutes, and even more preferably 15 minutes to 120 minutes.
[0119] Before the resin composition layer is thermally cured, the resin composition layer may be preheated at a temperature lower than the curing temperature. For example, prior to thermally curing the resin composition layer, the resin composition layer may be preheated for 5 minutes or more, preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and even more preferably 15 minutes to 100 minutes at a temperature of 50°C to 120°C, preferably 60°C to 115°C, and more preferably 70°C to 110°C. Preheating is advantageous because it is easy to realize an insulating layer with low surface roughness after desmearing.
[0120] -Process (3)- In step (3), holes are drilled in the insulating layer.
[0121] This allows the formation of via holes in the insulating layer. Step (3) may be performed using, for example, a drill, a laser, plasma, or the like, depending on the composition of the resin composition used to form the insulating layer. The dimensions and shape of the holes may be appropriately determined depending on the design of the circuit board.
[0122] -Process (4)- In step (4), the insulating layer is subjected to a desmear treatment.
[0123] This makes it possible to remove smears that have occurred in the via holes due to the drilling process. The desmearing process is not particularly limited and can be performed by various known methods. In one embodiment, the desmearing process can be a dry desmearing process, a wet desmearing process, or a combination thereof.
[0124] Examples of the dry desmear treatment include desmear treatment using plasma. In the desmear treatment using plasma, a gas is introduced into a plasma generating device to generate plasma and the plasma is used to treat the insulating layer, thereby removing smears generated in the via hole. There is no particular limitation on the method of generating plasma, and examples thereof include microwave plasma that generates plasma using microwaves, high frequency plasma that uses high frequency, atmospheric pressure plasma that is generated under atmospheric pressure, and vacuum plasma that is generated under vacuum, and vacuum plasma that is generated under vacuum is preferred. In addition, the plasma used in the desmear treatment is preferably RF plasma excited by high frequency.
[0125] The gas to be converted into plasma is not particularly limited as long as it can remove smears in the via holes, and for example, a gas containing SF6 may be used. In this case, the gas to be converted into plasma may contain other gases such as Ar and O2 in addition to SF6. Among them, from the viewpoint of easily realizing an insulating layer with a small surface roughness after the desmear process, the gas to be converted into plasma is preferably a mixed gas containing SF6 and at least one of Ar and O2, and more preferably a mixed gas containing SF6, Ar and O2.
[0126] When a mixed gas of SF6 and other gases is used, the mixing ratio (SF6 / other gases: unit: sccm) is preferably 1 / 0.01 to 1 / 1, more preferably 1 / 0.05 to 1 / 1, and further preferably 1 / 0.1 to 1 / 1, from the viewpoint of easily realizing an insulating layer with small surface roughness after desmearing.
[0127] The time for the desmear treatment using plasma is not particularly limited, but is preferably 30 seconds or more, more preferably 60 seconds or more, 90 seconds or more, or 120 seconds or more. The upper limit of the desmear treatment time is preferably 10 minutes or less, more preferably 5 minutes or less, from the viewpoint of easily realizing an insulating layer with a small surface roughness after the desmear treatment.
[0128] The desmear treatment using plasma can be carried out using a commercially available plasma desmear treatment device. Among commercially available plasma desmear treatment devices, examples suitable for the manufacture of circuit boards include a plasma dry etching device manufactured by Oxford Instruments, a microwave plasma device manufactured by Nissin, and an atmospheric pressure plasma etching device manufactured by Sekisui Chemical Co., Ltd.
[0129] The dry desmearing process may also be a dry sandblasting process in which an abrasive is sprayed from a nozzle to polish the object to be treated. The dry sandblasting process may be carried out using a commercially available dry sandblasting device. When a water-soluble abrasive is used as the abrasive, washing with water after the dry sandblasting process prevents the abrasive from remaining inside the via hole, and effectively removes the smear.
[0130] From the viewpoint of easily realizing an insulating layer with small surface roughness regardless of the composition of the resin composition layer, the desmear treatment is preferably a dry desmear treatment, and among them, a desmear treatment using plasma is more preferable. Therefore, in a preferred embodiment, the insulating layer is subjected to a dry desmear treatment, and particularly preferably to a desmear treatment using plasma.
[0131] The wet desmear treatment may be, for example, a desmear treatment using an oxidizing agent solution. When the desmear treatment is performed using an oxidizing agent solution, it is preferable to perform a swelling treatment using a swelling liquid, an oxidation treatment using an oxidizing agent solution, and a neutralization treatment using a neutralizing liquid in this order. Examples of the swelling liquid include "Swelling Dip Securiganth P" and "Swelling Dip Securiganth SBU" manufactured by Atotech Japan Co., Ltd. The swelling treatment is preferably performed by immersing the substrate on which the via holes are formed in a swelling liquid heated to 60°C to 80°C for 5 to 10 minutes. The oxidizing agent solution is preferably an alkaline permanganate solution, and examples of the solution include a solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide. The oxidation treatment using an oxidizing agent solution is preferably carried out by immersing the substrate after the swelling treatment in an oxidizing agent solution heated to 60°C to 80°C for 10 to 30 minutes. Commercially available alkaline permanganate aqueous solutions include, for example, "Concentrate Compact P", "Concentrate Compact CP", and "Dosing Solution Securigans P" manufactured by Atotech Japan Co., Ltd. The neutralization treatment using a neutralizing solution is preferably carried out by immersing the substrate after the oxidation treatment in a neutralizing solution at 30°C to 50°C for 3 to 10 minutes. The neutralizing solution is preferably an acidic aqueous solution, and a commercially available product thereof includes, for example, "Reduction Solution Securigans P" manufactured by Atotech Japan Co., Ltd.
[0132] The wet desmear treatment may also be a wet sandblasting treatment in which an abrasive and a dispersion medium are sprayed from a nozzle to polish the treatment target. The wet sandblasting treatment can be carried out using a commercially available wet sandblasting treatment device.
[0133] In one preferred embodiment, the insulating layer is subjected to a wet desmear treatment, and in a particularly preferred embodiment, the insulating layer is desmeared using an oxidizing agent solution.
[0134] When the dry desmear treatment and the wet desmear treatment are performed in combination, the dry desmear treatment may be performed first, or the wet desmear treatment may be performed first.
[0135] The support of the resin sheet may be removed between step (1) and step (2), between step (2) and step (3), between step (3) and step (4), or after step (4). From the viewpoint of easily realizing an insulating layer with a small surface roughness after the desmear treatment, the support is preferably removed after step (2), and more preferably removed after step (4).
[0136] In the manufacturing method of the present invention, after carrying out these steps (1) to (4), the above-mentioned step (X) and the conductor layer forming step are carried out, thereby making it possible to form a thin conductor pattern with a small L / S while suppressing plating burn. These steps can be collectively called a rewiring forming step, and the manufacturing method of the present invention is characterized in that the rewiring forming step includes a step of forming a plating seed layer with a thickness of 250 nm or less on the surface of an insulating layer with Ra of 100 nm or less.
[0137] By repeating the rewiring formation process, a rewiring layer with a multi-layer structure can be formed. According to the manufacturing method of the present invention, a thin insulating layer with excellent properties can be formed using a thermosetting material, and a thin conductor pattern with small L / S can be formed without plating burn using a thin plating seed layer, so that extremely fine and high-density wiring can be provided.
[0138] According to the manufacturing method of the present invention, it is possible to realize a circuit board such as a WLP or PLP having a thin conductor pattern with a small L / S.
[0139] The manufacturing method of circuit boards such as WLP and PLP is as described above with reference to patent documents. For example, when manufacturing a WLP with a fan-in structure, a semiconductor wafer on which a circuit element having a predetermined function and a plurality of electrode pads electrically connected to the circuit element are formed is used as a "substrate", and step (1) is carried out so that the electrode pad surface and the thermosetting resin composition layer are bonded. Then, steps (2), (3), (4), (X), and a conductor layer forming step are carried out in order to form a rewiring layer on the electrode pad surface of the semiconductor wafer. By repeatedly carrying out these steps, it is also possible to form a multi-layered rewiring layer. Then, a board connection terminal such as a bump is formed on the surface of the rewiring layer opposite to the semiconductor wafer, and the rewiring layer is divided into individual pieces, thereby manufacturing a WLP with a fan-in structure.
[0140] For example, when manufacturing a WLP with a fan-out structure, a semiconductor wafer on which a circuit element having a predetermined function and a plurality of electrode pads electrically connected to the circuit element are formed is first diced. Then, each semiconductor chip is arranged on a carrier (glass substrate, metal substrate, plastic substrate, etc.) at a distance from each other, and then resin-sealed to obtain a substrate in which the diced semiconductor chips are encapsulated with a sealing resin so that their electrode pad surfaces are exposed. Such a substrate is used as a "base material", and step (1) is carried out so that the surface of the substrate on the side on which the electrode pad surface is exposed is bonded to the thermosetting resin composition layer. Then, steps (2), (3), (4), (X), and a conductor layer forming step are carried out in order, and a rewiring layer can be formed on the exposed electrode pad surface and the sealing resin layer around it. By repeatedly carrying out these steps, it is also possible to form a multi-layer rewiring layer. Then, board connection terminals such as bumps are formed on the surface of the rewiring layer opposite to the substrate, and the substrate is diced again to manufacture a WLP with a fan-out structure.
[0141] In particular, the fan-out WLP or PLP obtained by the manufacturing method of the present invention is advantageous because it allows extremely fine and high-density wiring to be formed over a large area, coupled with the inherent feature of the fan-out structure that the redistribution layer can be formed over a large area. Therefore, in a preferred embodiment, the manufacturing method of the present invention manufactures a fan-out WLP or PLP.
[0142] The present invention can be widely applied to the manufacture of circuit boards including a process of forming a plating seed layer on the surface of an insulating layer. Manufacturing methods of circuit boards such as WLP and PLP have undergone a wide variety of developments, including the above-mentioned chip 1st method and rewiring layer 1st method, as well as the chip mounting direction (face-down type, face-up type), but the present invention relates to a technology that can be widely applied to the manufacture of circuit boards including a process of forming a plating seed layer on the surface of an insulating layer during the manufacturing process, and is extremely versatile. EXAMPLES
[0143] The present invention will be specifically described below with reference to examples. The present invention is not limited to these examples. In the following, "parts" and "%" representing amounts mean "parts by mass" and "% by mass", respectively, unless otherwise specified. Unless otherwise specified, the temperature and pressure conditions are room temperature (25°C) and atmospheric pressure (1 atm).
[0144] <Inorganic fillers used> Inorganic filler 1: Spherical silica (Denki Kagaku Kogyo Co., Ltd. "UFP-30", average particle size 0.3 μm, specific surface area 30.7 m 2 The surface was treated with 2 parts of N-phenyl-3-aminopropyltrimethoxysilane ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd.) per 100 parts of silica gel (g). Inorganic filler 2: Spherical silica (Admatechs "SO-C2", average particle size 0.5 μm, specific surface area 5.8 m 2 The surface was treated with 1 part of N-phenyl-3-aminopropyltrimethoxysilane (KBM573, manufactured by Shin-Etsu Chemical Co., Ltd.) per 100 parts of silica gel (g). Inorganic filler 3: Spherical silica (Admatechs "SO-C4", average particle size 1.1 μm, specific surface area 4.5 m 2 The surface was treated with 1 part of N-phenyl-3-aminopropyltrimethoxysilane ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd.) per 100 parts of silica gel (g).
[0145] <Preparation Example 1> (Preparation of Resin Composition 1) Bixylenol type epoxy resin (Mitsubishi Chemical Corporation "YX4000HK", epoxy equivalent approx. 185) 6 parts, naphthalene type epoxy resin (Nippon Steel Chemical & Material Corporation "ESN475V", epoxy equivalent approx. 332) 5 parts, bisphenol AF type epoxy resin (Mitsubishi Chemical Corporation "YX7760", epoxy equivalent approx. 238) 15 parts, naphthylene ether type epoxy resin (DIC Corporation "HP6000L", epoxy equivalent approx. 238) 15 parts 2 parts of cyclohexane-type epoxy resin ("ZX1658GS" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent of about 135), and 2 parts of phenoxy resin ("YX7500BH30" manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of cyclohexanone:methyl ethyl ketone (MEK) with a solid content of 30 mass%, Mw=44000) were dissolved by heating with stirring in a mixed solvent of 20 parts of solvent naphtha and 10 parts of cyclohexanone. After cooling to room temperature, 4 parts of a triazine skeleton-containing cresol novolac-based curing agent (DIC Corporation's "LA-3018-50P", hydroxyl group equivalent of about 151, 2-methoxypropanol solution with solid content of 50%), 6 parts of an active ester-based curing agent (DIC Corporation's "EXB-8000L-65TM", active group equivalent of about 220, toluene solution with non-volatile components of 65% by mass), 60 parts of inorganic filler 1, and 0.05 parts of an amine-based curing accelerator (4-dimethylaminopyridine (DMAP)) were mixed therein and uniformly dispersed using a high-speed rotating mixer, followed by filtration using a cartridge filter (ROKITECHNO Corporation's "SHP020") to prepare resin composition 1.
[0146] <Preparation Example 2> (Preparation of Resin Composition 2) Resin composition 2 was prepared in the same manner as in Preparation Example 1, except that (1) the amount of active ester curing agent (DIC Corporation's "EXB-8000L-65TM", active group equivalent of about 220, toluene solution with 65% by mass of non-volatile components) was changed from 6 parts to 12 parts, (2) 90 parts of inorganic filler 2 was used instead of 60 parts of inorganic filler 1, and (3) phenoxy resin (Mitsubishi Chemical Corporation's "YX7500BH30", 1:1 solution of cyclohexanone:methyl ethyl ketone (MEK) with a solid content of 30% by mass, Mw = 44000) was used instead of phenoxy resin (Mitsubishi Chemical Corporation's "YX7553BH30", 1:1 solution of cyclohexanone:methyl ethyl ketone (MEK) with a solid content of 30% by mass, Mw = 35000).
[0147] <Preparation Example 3> (Preparation of Resin Composition 3) Resin composition 3 was prepared in the same manner as in Preparation Example 1, except that (1) the amount of active ester curing agent (DIC Corporation's "EXB-8000L-65TM", active group equivalent of about 220, toluene solution with 65% by mass of non-volatile components) was changed from 6 parts to 12 parts, (2) 90 parts of inorganic filler 3 was used instead of 60 parts of inorganic filler 1, and (3) phenoxy resin (Mitsubishi Chemical Corporation's "YX7500BH30", 1:1 solution of cyclohexanone:methyl ethyl ketone (MEK) with a solid content of 30% by mass, Mw = 44000) was used instead of phenoxy resin (Mitsubishi Chemical Corporation's "YX7553BH30", 1:1 solution of cyclohexanone:methyl ethyl ketone (MEK) with a solid content of 30% by mass, Mw = 35000).
[0148] The components used in the preparation of resin compositions 1 to 3 and their amounts are shown in Table 1 below.
[0149] [Table 1]
[0150] [Example 1] (1) Preparation of resin sheet As a support, a PET film (Toray Industries, Inc., "Lumirror R80", thickness 38 μm, softening point 130° C., "release PET") that had been subjected to release treatment with an alkyd resin-based release agent (Lintec Corporation, "AL-5") was prepared. Resin composition 1 was uniformly applied to the release agent of the support with a die coater so that the thickness of the resin composition layer after drying was 20 μm, and the resin composition layer was provided on the release PET by drying at 70° C. to 95° C. for 2 minutes. Next, a rough surface of a polypropylene film (Oji F-Tex Co., Ltd., "Alphan MA-411", thickness 15 μm) was laminated as a protective film on the surface of the resin composition layer that was not bonded to the support so as to be bonded to the resin composition layer. This resulted in a resin sheet having a layer structure of release PET (support)\resin composition layer\protective film.
[0151] (2) Manufacturing of evaluation circuit boards A circuit board for evaluation was manufactured according to the following procedure.
[0152] (2-1) Preparation of the substrate A silicon wafer with a copper layer laminated on one side (copper layer thickness 1 μm, wafer thickness 0.8 mm, 8 inch size) was prepared as a substrate, and placed in an oven at 130° C. for 30 minutes to dry.
[0153] (2-2) Lamination of resin sheets The protective film was peeled off from the resin sheet to expose the resin composition layer. Then, using a batch-type vacuum pressure laminator (Nikko Materials Co., Ltd. 2-stage build-up laminator "CVP700"), the resin composition layer was laminated on one side of the substrate so that it was in contact with the copper layer of the substrate. This lamination was performed by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing at 130°C and a pressure of 0.74 MPa for 45 seconds. Next, the substrate was heat-pressed at 120°C and a pressure of 0.5 MPa for 75 seconds to smooth it.
[0154] (2-3) Thermal curing of the resin composition layer After laminating the resin sheet, the laminate was placed in an oven at 100°C and heated for 30 minutes, then transferred to an oven at 180°C and heated for 30 minutes to thermally cure the resin composition layer. The support was then peeled off. Thus, a substrate A was obtained in which a cured product of the resin composition layer (insulating layer; thickness 20 μm) was provided on the base material.
[0155] (2-4) Desmearing Wet desmear treatment was performed on substrate A. In detail, substrate A was immersed in a swelling solution (Atotech Japan's "Swelling Dip Securigance P", an aqueous solution of diethylene glycol monobutyl ether and sodium hydroxide) at 60°C for 5 minutes, then in a roughening solution (Atotech Japan's "Concentrate Compact P", an aqueous solution of KMnO4: 60g / L, NaOH: 40g / L) at 80°C for 15 minutes, and finally in a neutralizing solution (Atotech Japan's "Reduction Solution Securigance P", an aqueous solution of sulfuric acid) at 40°C for 5 minutes, and then dried at 80°C for 30 minutes. The obtained substrate is called substrate B.
[0156] (2-5) Formation of plating seed layer A plating seed layer was formed on the surface of the insulating layer of the substrate B. In detail, a diffusion barrier layer (Ti layer) having a thickness of 10 nm was formed on the surface of the insulating layer of the substrate B using a sputtering device ("E-400S" manufactured by Canon Anelva Corporation), and then a conductive seed layer (Cu layer) having a thickness of 50 nm was formed, thereby forming a plating seed layer having a thickness of 60 nm.
[0157] (2-6) Formation of conductor layer The obtained substrate was heated at 150°C for 30 minutes for annealing. Next, a plating resist was formed according to the semi-additive method, and a comb-tooth pattern with L / S=2 / 2μm (line width 1mm) was formed by exposure and development, followed by copper sulfate electrolytic plating to form a conductor layer (conductor pattern) with a thickness of 2μm. After the conductor pattern was formed, the substrate was heated at 200°C for 60 minutes for annealing. The obtained substrate is referred to as Substrate C.
[0158] [Example 2] Resin sheets were prepared and substrates A and B were manufactured in the same manner as in Example 1. Substrate C was formed in the same manner as in Example 1, except that in the formation of the plating seed layer, the thickness of the conductive seed layer (Cu layer) was changed from 50 nm to 100 nm to form a plating seed layer with a thickness of 110 nm.
[0159] [Example 3] Resin sheets were prepared and substrates A and B were manufactured in the same manner as in Example 1. Substrate C was formed in the same manner as in Example 1, except that in the formation of the seed layer, the thickness of the conductive seed layer (Cu layer) was changed from 50 nm to 150 nm to form a plating seed layer with a thickness of 160 nm.
[0160] [Example 4] A resin sheet was produced in the same manner as in Example 1, except that Resin Composition 2 was used instead of Resin Composition 1. Substrate A was produced in the same manner as in Example 1 using the obtained resin sheet.
[0161] In Example 4, a dry desmear process was performed on the substrate A. In detail, the substrate A was processed for 2 minutes using a plasma dry etching device ("PlasmaPro100" manufactured by Oxford Instruments) under the conditions of a mixture ratio of Ar / SF6 / O2 of 10:40:8 (sccm), a degree of vacuum of 50 mTorr, an RF power of 120 W, and an ICP power of 0 W, to obtain the substrate B.
[0162] Then, in the formation of the plating seed layer, the thickness of the conductive seed layer (Cu layer) was changed from 50 nm to 100 nm, and a plating seed layer with a thickness of 110 nm was formed, in the same manner as in Example 1, except that a substrate C was formed.
[0163] [Comparative Example 1] Except for using resin composition 2 instead of resin composition 1, resin sheets were prepared in the same manner as in Example 1, and substrates A and B were manufactured. Then, in forming the plating seed layer, the thickness of the conductive seed layer (Cu layer) was changed from 50 nm to 100 nm, and a plating seed layer with a thickness of 110 nm was formed, except that substrate C was formed in the same manner as in Example 1.
[0164] [Comparative Example 2] Except for using resin composition 3 instead of resin composition 1, resin sheets were prepared and substrates A and B were manufactured in the same manner as in Example 1. Then, in forming the plating seed layer, the thickness of the conductive seed layer (Cu layer) was changed from 50 nm to 200 nm to form a plating seed layer with a thickness of 210 nm, and substrate C was formed in the same manner as in Example 1.
[0165] [Reference example 1] Except for using resin composition 2 instead of resin composition 1, resin sheets were prepared in the same manner as in Example 1, and substrates A and B were manufactured. Then, in forming the plating seed layer, the thickness of the conductive seed layer (Cu layer) was changed from 50 nm to 300 nm, and a plating seed layer with a thickness of 310 nm was formed, except that substrate C was formed in the same manner as in Example 1.
[0166] Various measurement and evaluation methods will be explained.
[0167] <Thickness measurement> The thickness of the resin composition layer etc. was measured using a contact type film thickness meter ("MCD-25MJ" manufactured by Mitutoyo Corporation).
[0168] <Measurement of the roughness of the insulating layer surface> The arithmetic mean roughness (Ra) of the insulating layer surface was measured for the substrates B produced in the examples, comparative examples, and reference examples. A non-contact three-dimensional surface profile roughness measurement system ("Wyko GT-X3" manufactured by Bruker A-X) was used for the measurement.
[0169] <Evaluation of wiring shape (plating burn)> The conductor patterns formed on the substrates C produced in the examples, comparative examples, and reference examples were observed with an optical microscope (Hirox Corporation's "KH8700"). In detail, the conductor patterns were enlarged using an optical microscope (CCD) to confirm the shape. For a comb-tooth pattern with L / S=2 / 2 μm, 20 wirings with a height of 2 μm and a length of 1 mm were randomly observed. The number of abnormal deposition parts in the 20 wirings was counted, and when 50 or more abnormal deposition parts were observed, it was rated as "x" (bad), and when there were fewer than 50 abnormal deposition parts, it was rated as "◯" (good).
[0170] The measurement results and evaluation results of the Examples, Comparative Examples, and Reference Examples are shown in Table 2 below.
[0171] [Table 2]
[0172] In Reference Example 1, in which a plating seed layer having a thickness of more than 250 nm is formed, the contribution to fine wiring is limited due to the thickness of the plating seed layer itself, etc. When a relatively thick plating seed layer is formed as in Reference Example 1, plating burn does not occur significantly even when a conductor pattern is formed on the surface of an insulating layer having an arithmetic mean roughness (Ra) of more than 100 nm (this is evidence that the problem to be solved by the present invention was not found in the prior art). In order to realize finer wiring, when a thin plating seed layer of 250 nm or less is formed, it has been confirmed that if the Ra of the insulating layer surface exceeds 100 nm, plating burn occurs significantly (Comparative Examples 1 and 2). In contrast, in Examples 1 to 4, which include a process of forming a plating seed layer with a thickness of 250 nm or less on the surface of an insulating layer with Ra of 100 nm or less, it was confirmed that a thin conductor pattern with L / S = 2 / 2 μm could be formed while significantly suppressing plating burn, demonstrating that this method significantly contributes to the fine wiring of circuit boards.
Claims
1. (1) A step of laminating a resin sheet including a support and a thermosetting resin composition layer provided on the support onto a substrate such that the thermosetting resin composition layer is bonded to the substrate; (2) A step of thermally curing the thermosetting resin composition layer to form an insulating layer; (3) Drilling the insulating layer (4) a step of desmearing the insulating layer; (X) forming a plating seed layer on the surface of the insulating layer; and forming a conductor layer on the plating seed layer by electrolytic plating; A method for manufacturing a circuit board, comprising: The conductor layer includes a conductor pattern having a thickness of 2 μm or less and a line / space ratio (L / S) of 5 / 5 μm or less, step (4) includes a wet desmear treatment for roughening the surface of the insulating layer; the thermosetting resin composition layer contains an epoxy resin and a curing agent; The content of the curing agent is 3% by mass or more and 20% by mass or less, when the resin component in the resin composition is 100% by mass, A method for manufacturing a circuit board, wherein the thickness of the plating seed layer is 250 nm or less, and the arithmetic mean roughness (Ra) of the insulating layer surface is 100 nm or less.
2. The thickness of the plating seed layer is D s (nm), and the Ra of the insulating layer surface is Ra i (nm), 1≦D s / Ra i The method of claim 1 , wherein
3. The method according to claim 1 or 2, wherein in the step (X), the plating seed layer is formed by a sputtering method.
4. The method according to any one of claims 1 to 3, wherein the thermosetting resin composition layer contains an active ester-based curing agent.
5. The method according to any one of claims 1 to 4, wherein the circuit board is a wafer level package or a panel level package.
Citation Information
Patent Citations
Manufacturing method of printed wiring board
JP2007273615A
Method for manufacturing printed-wiring board
JP2014093355A
Temporary fixing method of fan-out wafer level package
JP2019016647A
Manufacturing method of print circuit board
JP2020136542A