Photosensitive coloring composition, cured film, light-shielding filter, color filter, image display device, solid-state imaging device, and infrared sensor
The photosensitive coloring composition with a 9,9-bisarylfluorene structure addresses issues of external light reflection and curing-induced wrinkles by enhancing adhesion and maintaining refractive index uniformity, resulting in improved light-shielding properties for image display devices and sensors.
Patent Information
- Application Number
- JP2020192443
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-19
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-11-19
AI Technical Summary
Conventional photosensitive compositions for forming light shielding filters in image display devices and solid-state image sensors suffer from issues such as external light reflection, pattern chipping during alkaline development, poor adhesion, and surface wrinkles due to uneven curing, which affect the optical density and light-shielding properties.
A photosensitive coloring composition comprising a colorant, an alkali-soluble resin, a polymerizable compound with a 9,9-bisarylfluorene structure, and a photopolymerization initiator, which enhances adhesion and suppresses wrinkles by aligning molecules through π-π interactions and maintaining a small refractive index difference, thereby improving light-shielding properties.
The composition achieves high light-shielding properties with reduced external light reflection, improved pattern shape and adhesion, and minimizes surface wrinkles, resulting in superior performance of cured films for light shielding filters and image display devices.
Smart Images

Figure 0007574619000017 
Figure 0007574619000018 
Figure 0007574619000019
Abstract
Description
[Technical field]
[0001] The present invention relates to a photosensitive coloring composition. [Background technology]
[0002] 2. Description of the Related Art Color filters used in image display devices such as liquid crystal and organic electroluminescence devices are provided with a light-shielding filter called a black matrix for the purpose of blocking light between pixels and improving contrast. In addition, solid-state imaging elements such as C-MOS (Complement ray Metal Oxide Semiconductor) image sensors and CCD (Charge Coupled Device) image sensors used in imaging units of smartphones, tablet terminals, etc. are equipped with light-shielding filters for the purposes of preventing noise generation and improving image quality.
[0003] Compositions containing black coloring materials such as carbon black and titanium black are known as compositions for forming light-shielding filters. For example, Patent Document 1 discloses a composition for forming a light-shielding film, which is characterized by containing a black colorant having an average particle size of 40 nm or less and a resin component, capable of forming a coating film disposed on the periphery of an effective pixel region of a solid-state imaging device. Patent Document 2 discloses a photosensitive composition for forming partition walls of optical elements, which contains an alkali-soluble resin having a photocurable ethylenically unsaturated double bond, a photopolymerization initiator, a black pigment, and hollow fine particles having an average primary particle size of 20 to 100 nm. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2006-156801 A [Patent Document 2] JP 2011-48195 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, although the cured film formed from the conventional composition has excellent light-shielding properties, it has a problem of reflecting light entering an image display device (hereinafter referred to as external light reflection).Furthermore, there are problems such as chipping of the pattern after alkali development due to insufficient photocuring, adhesion problems in which the pattern peels off from the substrate, and wrinkles occurring on the pattern surface after post-baking.
[0006] An object of the present invention is to provide a photosensitive coloring composition that has high light-shielding properties, suppresses external light reflection, has good pattern shape and adhesion after development, and can suppress the occurrence of wrinkles after post-baking. [Means for solving the problem]
[0007] The present invention relates to a photosensitive coloring composition comprising a colorant (A), an alkali-soluble resin (B), a polymerizable compound (C), and a photopolymerization initiator (D), The present invention relates to a photosensitive coloring composition, wherein the polymerizable compound (C) comprises a polymerizable compound (C-1) having a 9,9-bisarylfluorene structure. Effect of the Invention
[0008] According to the present invention, it is possible to provide a cured film having high light-shielding properties, suppressing external light reflection, having good pattern shape and adhesion after development, and suppressing the occurrence of wrinkles after post-baking. The present invention also provides a cured film, a light-shielding filter, a color filter, an image display device, a solid-state imaging device, and an infrared sensor. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view of an image display device. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a solid-state imaging device. [Diagram 3] FIG. 3 is a schematic cross-sectional view of an infrared sensor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the embodiment for carrying out the photosensitive coloring composition of the present invention will be described in detail. Note that the present invention is not limited to the following embodiment, and can be modified within the scope of the problem that can be solved.
[0011] In this specification, unless otherwise specified, "(meth)acryloyl", "(meth)acrylic", "(meth)acrylic acid", "(meth)acrylate", or "(meth)acrylamide" means "acryloyl and / or methacryloyl", "acrylic and / or methacrylic", "acrylic acid and / or methacrylic acid", "acrylate and / or methacrylate", or "acrylamide and / or methacrylamide", respectively. In addition, "CI" means Color Index (CI; published by The Society of Dyers and Colourists). The polymerizable unsaturated group is an ethylenically unsaturated double bond.
[0012] <Photosensitive coloring composition> The present invention relates to a photosensitive coloring composition comprising a colorant (A), an alkali-soluble resin (B), a polymerizable compound (C), and a photopolymerization initiator (D), The photosensitive coloring composition contains a polymerizable compound (C) having a 9,9-bisarylfluorene structure (C-1).
[0013] The present inventors speculate as follows about the mechanism by which the photosensitive coloring composition of the present invention can solve the problems of the present invention.
[0014] Photosensitive coloring compositions containing colorants such as carbon black and exhibiting a black color are widely used because they can obtain high light-shielding properties over a wide wavelength range. However, for example, when a photosensitive coloring composition is pattern-exposed to ultraviolet light such as g-rays, h-rays, and i-rays, the light does not reach the inside of the photosensitive coloring composition layer (hereinafter referred to as the coating), so that poor adhesion such as chipping or peeling of the cured film occurs during alkali development, and wrinkles occur on the surface due to a difference in thermal curing shrinkage between the inside and the surface during heat treatment (hereinafter also referred to as post-bake). Therefore, there was a problem of reduced optical density and poor light-shielding properties. However, since the polymerizable compound (C-1) with a 9,9-bisarylfluorene structure has four aromatic rings in one molecule, it is thought that the molecules stack together through π-π interactions, improving the adhesion of the film. In addition, since it has a rigid structure, it is thought that shrinkage during curing is unlikely to occur, suppressing the occurrence of wrinkles. Furthermore, it is speculated that the orientation of the polymerizable compound (C-1) with a 9,9-bisarylfluorene structure on the film surface reduces the refractive index difference between the air layer and the film, achieving low reflectance while maintaining high light blocking properties.
[0015] [Colorant (A)] The photosensitive coloring composition of the present invention contains a colorant (A).
[0016] The colorant (A) may be either a pigment or a dye, but is preferably a pigment from the viewpoints of light resistance, heat resistance, and solvent resistance. In addition, it is preferable to include a colorant (A) that exhibits black color, since it is possible to obtain a photosensitive coloring composition that has a more excellent effect of the present invention. It is also preferable to use a combination of multiple colorants (A) that do not exhibit black color by themselves, and adjust the combination to produce a black color as a whole.
[0017] (Pigments) The pigment is not particularly limited, and known inorganic pigments and organic pigments can be used.
[0018] [Inorganic pigments] Examples of inorganic pigments include titanium oxide, barium sulfate, zinc oxide, lead sulfate, yellow lead, zinc yellow, red oxide (red iron (III)), cadmium red, ultramarine, Prussian blue, chromium oxide green, cobalt green, and amber. Examples of black inorganic pigments include metal oxides, metal nitrides, and metal oxynitrides containing one or more metal elements selected from the group consisting of metal elements of Group 4 such as titanium and zirconium, metal elements of Group 5 such as vanadium and niobium, cobalt, chromium, copper, manganese, ruthenium, iron, nickel, tin, and silver, and carbon black. Two or more of these inorganic pigments may be used in combination, and in order to improve the light-shielding properties, organic pigments and dyes described below may be used in combination. Among them, carbon black is more preferable because it is inexpensive and can form a film with high light-shielding properties in a small amount.
[0019] Examples of carbon black include lamp black, acetylene black, thermal black, channel black, furnace black, etc. Among these, furnace black is preferable.
[0020] The average primary particle diameter of carbon black is preferably 10 to 30 nm, more preferably 10 to 20 nm. With a suitable particle diameter, it is easy to achieve both light-shielding properties and curability. The average primary particle diameter is determined by averaging approximately 20 random particles displayed in a magnified image (approximately 1,000 to 10,000 times) of a cross section of a film formed from a photosensitive coloring composition using a scanning electron microscope. When a particle has a length in the long axis direction and a length in the short axis direction, the length in the long axis direction is used.
[0021] From the viewpoint of light blocking, the specific surface area of carbon black is set to 100 to 500 m 2 / g is preferable, and 150 to 400m 2 / g is more preferable. The specific surface area can be measured by a known method. For example, the specific surface area can be measured by adsorbing iodine, nitrogen (BET method, STSA method), cetyltrimethylammonium bromide, or the like onto the surface of the carbon black. Among these, the nitrogen BET method is preferable.
[0022] Examples of commercially available carbon black products include #30, 30L, 32, 40, 44, 45, 45L, 47, 52, 650, 850, 900, 950, 960, 980, 1000, 1000N, 2300, 2350, 2600, 2650, 3230, 3400, 4000, MCF88, MA7, 8, 11, 77, 100, 230, 600 manufactured by Mitsubishi Chemical Corporation, and BLACK PEARLS 460, 800, 880, 900, 1000, 4840, 1300, 1400, L, and REGAL 330, 400, 600 manufactured by CABOT Corporation.
[0023] From the viewpoint of light-shielding properties, the content of carbon black is preferably from 5 to 30 mass %, and more preferably from 10 to 25 mass %, in 100 mass % of the nonvolatile content of the photosensitive coloring composition.
[0024] [Organic pigments] Examples of organic pigments include compounds classified as pigments in the Color Index. Specifically, CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 12, 14, 15, 16, 17, 21, 22, 23, 31, 32, 37, 38, 41, 47, 48, 48:1, 48:2, 48:3, 48:4, 49, 49:1, 49:2, 50:1, 52:1, 52:2, 53, 53:1, 53:2, 53:3, 57, 57:1, 57:2, 58:4, 60, 63, 63: 1,63:2,64,64:1,68,69,81,81:1,81:2,81:3,81:4,83,88,90:1,101,101:1,104,108,108:1,109,112,113,114,122,123,144,146,147,149,151,166,168,169,170,172,173,174,175,176,177,178,179,18 1,184,185,187,188,190,193,194,200,202,206,207,208,209,210,214,216,220,221,224,230,231,232,233,235,236,237,238,239,242,243,245,247,249,250,251,253,254,255,256,257,258,259,26 Red organic pigments such as pigments described in JP 0,262,263,264,265,266,267,268,269,270,271,272,273,274,275,276,277,278,279,280,281,282,283,284,285,286,287,291,295,296, pigments described in JP 2014-134712 A, and pigments described in JP 6368844 A; Orange organic pigments such as CI Pigment Orange 36, 38, 43, 62, 64, 71, 73; CI Pigment Yellow 1, 2, 3, 4, 5, 6, 10, 12, 13, 14, 15, 16, 17, 18, 24, 31, 32, 34, 35, 35:1, 36, 36:1, 37, 37:1, 40, 42, 43, 53, 55, 60, 61, 62, 63, 65, 73, 74, 77, 81, 83, 93, 94, 95, 97, 98, 100, 101, 104, 106, 108, 109, 110, 113, 114, 115, 116, 117, 118, 119, 120, 123, 126, 1 Yellow organic pigments such as those described in JP 2012-226110 A and JP 2012-226110 A; Green organic pigments such as CI Pigment Green 1, 2, 4, 7, 8, 10, 13, 14, 15, 17, 18, 19, 26, 36, 37, 45, 48, 50, 51, 54, 55, 58, 59, 62, 63; Blue organic pigments such as CI Pigment Blue 1, 1:2, 9, 14, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 17, 19, 25, 27, 28, 29, 33, 35, 36, 56, 56:1, 60, 61, 61:1, 62, 63, 66, 67, 68, 71, 72, 73, 74, 75, 76, 78, 79; Purple organic pigments such as CI Pigment Violet 1, 1:1, 2, 2:2, 3, 3:1, 3:3, 5, 5:1, 14, 15, 16, 19, 23, 25, 27, 29, 31, 32, 37, 39, 42, 44, 47, 49, 50; Examples of black organic pigments include perylene compounds such as CI Pigment Black 21, 30, 31, 32, 33, and 34, bisbenzofuranone compounds described in JP-T-2010-534726, JP-T-2012-515233, and JP-T-2012-515234, and azomethine compounds described in JP-A-1-170601 and JP-A-2-34664. Among these, a combination that exhibits black color by including at least two or more organic pigments selected from red organic pigments, yellow organic pigments, blue organic pigments, and purple organic pigments is preferred.
[0025] Examples of the combination that provides a black color include the following. Contains yellow and purple organic pigments. Contains red organic pigment, yellow organic pigment, and purple organic pigment. Contains red organic pigment, yellow organic pigment, and blue organic pigment. Contains yellow organic pigment, blue organic pigment, and purple organic pigment. Contains red organic pigment, yellow organic pigment, blue organic pigment, and purple organic pigment.
[0026] A specific example of the above embodiment (1) is an embodiment containing at least one selected from CI Pigment Yellow 138, 139, 185, 231, and 233 as a yellow organic pigment, and CI Pigment Violet 23 as a purple organic pigment. A specific example of the above embodiment (2) is an embodiment containing at least one selected from CI Pigment Red 177, 254, 291, 295, and 296 as a red organic pigment, at least one selected from CI Pigment Yellow 139, 185, 231, and 233 as a yellow organic pigment, and CI Pigment Violet 23 as a purple organic pigment. A specific example of the above embodiment (3) is an embodiment containing at least one red organic pigment selected from CI Pigment Red 177, 254, 291, 295, and 296, at least one yellow organic pigment selected from CI Pigment Yellow 138, 139, 185, 231, and 233, and at least one blue organic pigment selected from CI Pigment Blue 15:3, 15:4, and 15:6. A specific example of the above embodiment (4) is an embodiment containing at least one selected from CI Pigment Yellow 138, 139, 185, 231, and 233 as a yellow organic pigment, at least one selected from CI Pigment Blue 15:3, 15:4, and 15:6 as a blue organic pigment, and CI Pigment Violet 23 as a purple organic pigment. A specific example of the above embodiment (5) is an embodiment containing at least one selected from CI Pigment Red 177, 254, 291, 295, and 296 as a red organic pigment, at least one selected from CI Pigment Yellow 138, 139, 185, 231, and 233 as a yellow organic pigment, at least one selected from CI Pigment Blue 15:3, 15:4, and 15:6 as a blue organic pigment, and CI Pigment Violet 23 as a purple organic pigment.
[0027] Among the above embodiments (1) to (5), the above embodiment (4) is preferred from the viewpoints of light blocking properties and reflectivity.
[0028] Among the above-mentioned embodiment (4), it is more preferable to contain CI Pigment Yellow 139 as the yellow organic pigment, CI Pigment Blue 15:6 as the blue organic pigment, and CI Pigment Violet 23 as the purple organic pigment.
[0029] Table 1 shows the preferred mass ratios (mass %) of each organic pigment in each embodiment.
[0030] [Table 1]
[0031] (dye) The dye is not particularly limited, and any known dye can be used.
[0032] Examples of the dye include acid dyes, direct dyes, basic dyes, salt-forming dyes, oil-soluble dyes, disperse dyes, reactive dyes, mordant dyes, vat dyes, sulfur dyes, etc. Furthermore, derivatives of these dyes and dyes in the form of lakes may also be used.
[0033] The acid dye preferably has an acid group such as sulfonic acid or carboxylic acid. The direct dye preferably forms an inorganic salt of the acid dye, or a salt-forming compound between the acid dye and a nitrogen-containing compound such as a quaternary ammonium salt compound, a tertiary amine compound, a secondary amine compound, or a primary amine compound. Also preferred are salt-forming compounds that are salts between a resin component having these functional groups and an acid dye. The salt-forming compound is also sulfonamidated to modify it into a sulfonic acid amide compound, which makes it easy to obtain a photosensitive coloring composition with excellent resistance (light resistance, solvent resistance). In addition, a salt-forming compound of an acid dye and a compound having an onium salt group is also preferable because it has excellent resistance (light resistance, solvent resistance). The compound having an onium salt group is preferably a resin having a cationic group.
[0034] Although the basic dye can be used as it is, a salt-forming compound that forms a salt with an organic acid, perchloric acid or a metal salt thereof is preferred. The salt-forming compound of the basic dye is preferred because it has excellent resistance (light resistance, solvent resistance) and affinity with pigments. In addition, the anion component that acts as a counter ion in the salt-forming compound of the basic dye is preferably an organic sulfonic acid, an organic sulfuric acid, a fluorine group-containing phosphorus anion compound, a fluorine group-containing boron anion compound, a cyano group-containing nitrogen anion compound, an anion compound having a conjugate base of an organic acid having a halogenated hydrocarbon group, or a salt-forming compound formed with an acid dye. The resistance of the salt-forming compound is further improved when the salt-forming compound contains a polymerizable unsaturated group in the molecule.
[0035] The chemical structure of the dye may be, for example, azo dyes, disazo dyes, azomethine dyes (indoaniline dyes, indophenol dyes, etc.), dipyrromethene dyes, quinone dyes (benzoquinone dyes, naphthoquinone dyes, anthraquinone dyes, anthrapyridone dyes, etc.), carbonium dyes (diphenylmethane dyes, triphenylmethane dyes, xanthene dyes, acridine dyes, etc.), quinoneimine dyes (oxazine dyes, thiazine dyes, etc.), azine dyes, polymethy Examples of the dye structure include, but are not limited to, dyes derived from dyes selected from the group consisting of amine dyes (oxonol dyes, merocyanine dyes, arylidene dyes, styryl dyes, cyanine dyes, squarylium dyes, croconium dyes, etc.), quinophthalone dyes, phthalocyanine dyes, subphthalocyanine dyes, perinone dyes, indigo dyes, thioindigo dyes, quinoline dyes, nitro dyes, nitroso dyes, rhodamine dyes, and metal complex dyes thereof. Among these, dyes containing two or more dyes and exhibiting black color are preferred. Examples of black dyes include pyrazole azo dyes, pyrromethene dyes, anilino azo dyes, triphenylmethane dyes, anthraquinone dyes, benzylidene dyes, oxonol dyes, pyrazolotriazole azo dyes, pyridone azo dyes, cyanine dyes, and phenothiazine dyes.
[0036] Specific examples of black dyes include CI Solvent Black 27-47.
[0037] From the viewpoint of light-shielding properties, the content of the colorant (A) is preferably from 5 to 70 mass %, more preferably from 10 to 60 mass %, in 100 mass % of the nonvolatile content of the photosensitive coloring composition.
[0038] (Micronization of pigments) The pigment is preferably used in a finely divided state. The method of finely dividing is not particularly limited, and for example, any of wet grinding, dry grinding, and solution precipitation can be used. Among these, salt milling treatment by a kneader method, which is a type of wet grinding, is preferred. The average primary particle size of the finely divided pigment determined by TEM (transmission electron microscope) is preferably 5 to 90 nm. From the viewpoints of dispersibility and contrast ratio, the average primary particle size is more preferably 10 to 70 nm.
[0039] Salt milling is a process in which a mixture of a pigment, a water-soluble inorganic salt, and a water-soluble organic solvent is mechanically kneaded while being heated using a kneader, a two-roll mill, a three-roll mill, a ball mill, an attritor, a sand mill, or other kneading machine, and then the water-soluble inorganic salt and the water-soluble organic solvent are removed by washing with water. The water-soluble inorganic salt acts as a crushing aid, and the pigment is crushed during salt milling by utilizing the high hardness of the inorganic salt. By optimizing the conditions for salt milling the pigment, it is possible to obtain a pigment with a very fine primary particle size, a narrow distribution width, and a sharp particle size distribution.
[0040] Examples of the water-soluble inorganic salt include sodium chloride, potassium chloride, sodium sulfate, etc., and sodium chloride (table salt) is preferred from the viewpoint of cost. The amount of the water-soluble inorganic salt used is preferably 50 to 2,000 parts by mass, and more preferably 300 to 1,000 parts by mass, per 100 parts by mass of the pigment, from the viewpoints of both treatment efficiency and production efficiency.
[0041] The water-soluble organic solvent is not particularly limited as long as it functions to wet the pigment and the water-soluble inorganic salt, dissolves (mixes) in water, and does not substantially dissolve the inorganic salt used. However, since the temperature rises during salt milling and the solvent becomes prone to evaporate, a high boiling point solvent with a boiling point of 120°C or more is preferable from the viewpoint of safety. For example, 2-methoxyethanol, 2-butoxyethanol, 2-(isopentyloxy)ethanol, 2-(hexyloxy)ethanol, diethylene glycol, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, triethylene glycol, triethylene glycol monomethyl ether, liquid polyethylene glycol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, dipropylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, liquid polypropylene glycol, etc. are used. The amount of the water-soluble organic solvent used is preferably 5 to 1,000 parts by mass, more preferably 50 to 500 parts by mass, relative to 100 parts by mass of the pigment.
[0042] In the salt milling treatment, a resin may be added as necessary. The type of the resin is not particularly limited, and examples thereof include natural resins, modified natural resins, synthetic resins, and synthetic resins modified with natural resins. Among these, it is preferable that the resin is solid at room temperature, insoluble in water, and partially soluble in the organic solvent. The amount of the resin added is preferably 2 to 200 parts by mass relative to 100 parts by mass of the pigment.
[0043] [Dye derivative (E)] The photosensitive coloring composition of the present invention may contain a dye derivative (E) as necessary. The dye derivative (E) is adsorbed on the surface of the colorant (A), which makes the surface of the colorant (A) polar and increases the affinity with other components, thereby improving dispersibility.
[0044] Examples of the dye derivative (E) include dye derivatives having an acidic group, a basic group, a neutral group, etc. in the organic dye residue. Examples of the dye derivative (E) include compounds having an acidic substituent such as a sulfo group, a carboxy group, or a phosphate group, and amine salts thereof, compounds having a basic substituent such as a sulfonamide group or a tertiary amino group at the terminal, and compounds having a neutral substituent such as a phenyl group or a phthalimidoalkyl group. Examples of organic pigments include diketopyrrolopyrrole pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, perinone pigments, perylene pigments, thiazine indigo pigments, triazine pigments, benzimidazolone pigments, indole pigments such as benzoisoindole, isoindoline pigments, isoindolinone pigments, quinophthalone pigments, naphthol pigments, threne pigments, metal complex pigments, and azo pigments such as azo, disazo, and polyazo.
[0045] Specifically, diketopyrrolopyrrole dye derivatives are described in JP 2001-220520 A, WO 2009 / 081930 A, WO 2011 / 052617 A, WO 2012 / 102399 A, and JP 2017-156397 A, phthalocyanine dye derivatives are described in JP 2007-226161 A, WO 2016 / 163351 A, JP 2017-165820 A, and Japanese Patent No. 5753266 A, and anthraquinone dye derivatives are described in JP 63-26 4674, JP-A-09-272812, JP-A-10-245501, JP-A-10-265697, JP-A-2007-079094, WO 2009 / 025325; quinacridone dye derivatives are disclosed in JP-A-48-54128, JP-A-03-9961, and JP-A-2000-273383; dioxazine dye derivatives are disclosed in JP-A-2011-162662; thiazine indigo dye derivatives are disclosed in JP-A-2007-314785; Azine dye derivatives are disclosed in JP-A-61-246261, JP-A-11-199796, JP-A-2003-165922, JP-A-2003-168208, JP-A-2004-217842, and JP-A-2007-314681; benzoisoindole dye derivatives are disclosed in JP-A-2009-57478; quinophthalone dye derivatives are disclosed in JP-A-2003-167112, JP-A-2006-291194, JP-A-2008-31281, and JP-A-2012-2 Examples of the known dye derivatives include those described in JP-A-2002-26110, naphthol dye derivatives include those described in JP-A-2012-208329 and JP-A-2014-5439, azo dye derivatives include those described in JP-A-2001-172520 and JP-A-2012-172092, acidic substituents include those described in JP-A-2004-307854, and basic substituents include those described in JP-A-2002-201377, JP-A-2003-171594, JP-A-2005-181383, JP-A-2005-213404, and the like. In these documents, the dye derivative may be referred to as a derivative, a pigment derivative, a dispersant, a pigment dispersant, or simply as a compound, but the compound having a substituent such as an acidic group, a basic group, or a neutral group in the organic dye residue is synonymous with the dye derivative.
[0046] The dye derivative (E) can be used alone or in combination of two or more kinds.
[0047] The content of the dye derivative (E) is preferably from 1 to 20 parts by mass, and more preferably from 2 to 10 parts by mass, based on 100 parts by mass of the colorant (A).
[0048] [Dispersion resin (F)] The photosensitive coloring composition of the present invention may contain a dispersing resin (F) as required. The dispersing resin (F) has an adsorptive group that has a high affinity for the pigment, and the adsorptive group is preferably one or more of a cationic group and an anionic group.
[0049] Examples of the cationic group-containing resin include a cationic group that includes a primary amino group, a secondary amino group, a tertiary amino group, a quaternary ammonium salt group, and a group containing a nitrogen atom such as a nitrogen-containing heterocycle.
[0050] Examples of the resin having an anionic group include a carboxyl group, a phosphoric acid group, a sulfonic acid group, etc. Among these, the carboxyl group and the phosphoric acid group are preferred from the viewpoint of adsorptivity to the pigment.
[0051] Examples of the resin type of the dispersion resin (F) include urethane resins, polycarboxylates such as polyacrylates, unsaturated polyamides, polycarboxylic acids, polycarboxylate (partial) amine salts, polycarboxylate ammonium salts, polycarboxylate alkylamine salts, polysiloxanes, long-chain polyaminoamide phosphates, hydroxyl-containing polycarboxylates, and modified products thereof, amides and salts thereof formed by the reaction of poly(lower alkylene imines) with polyesters having free carboxyl groups, water-soluble resins and water-soluble polymer compounds such as (meth)acrylic acid-styrene copolymers, (meth)acrylic acid-(meth)acrylic acid ester copolymers, styrene-maleic acid copolymers, polyvinyl alcohols, and polyvinylpyrrolidone, polyesters, modified polyacrylates, ethylene oxide / propylene oxide adducts, and phosphates.
[0052] Examples of the structure of the dispersing resin (F) include a random structure, a block structure, a graft structure, a comb structure, and a star structure. Among these, from the viewpoint of dispersion stability, the block structure, the graft structure, and the comb structure are preferred.
[0053] Commercially available dispersion resins (F) include, for example, Disperbyk-101, 103, 107, 108, 110, 111, 116, 130, 140, 154, 161, 162, 163, 164, 165, 166, 167, 168, 170, 171, 174, 180, 181, 182, 183, 184, 185, 190, 2000, 2001, 2009, 2010, 2020, 2025, 2050, 2070, 2095, 2150, 2155, 2163, 2164, Anti-Terra-U203, 204, and BYK-P104, P104S, manufactured by BYK-Chemie Japan Co., Ltd. ,220S, or Lactimon, Lactimon-WS, or Bykumen, etc., SOLSPERSE-3000, 9000, 13000, 13240, 13650, 13940, 16000, 17000, 18000, 20000, 21000, 24000, 26000, 27000, 28000, 31845, 32000, 32500, 32550, 33500, 32600, 34750, 35100, 36 600, 38500, 41000, 41090, 53095, 55000, 56000, 76500, etc. EFKA-46, 47, 48, 452, 4008, 4009, 4010, 4015, 4020, 4047, 4050, 4055, 4060, 4080, 4400, 4401, 4402, 4403, 4406, 4408, 4300, 4310, 4320, 4330, 4340, 450, 451, 453, 4540, 455 manufactured by BASF Japan Examples of resins that can be used include 0, 4560, 4800, 5010, 5065, 5066, 5070, 7500, 7554, 1101, 120, 150, 1501, 1502, and 1503 manufactured by Ajinomoto Fine-Techno Co., Ltd., Ajisuper PA111, PB711, PB821, PB822, and PB824 manufactured by Ajinomoto Fine-Techno Co., Ltd., and resins described in JP-A-2008-029901, JP-A-2009-155406, JP-A-2010-185934, and JP-A-2011-157416.
[0054] The dispersing resin (F) can be used alone or in combination of two or more kinds.
[0055] From the viewpoint of dispersion stability, the content of the dispersing resin (F) is preferably from 3 to 200 parts by mass, and more preferably from 5 to 100 parts by mass, relative to 100 parts by mass of the colorant (A).
[0056] [Alkali-soluble resin (B)] The photosensitive coloring composition of the present invention contains an alkali-soluble resin (B). The alkali-soluble resin (B) is a resin that dissolves in an alkali developer, and is preferably a resin that has a transmittance of 80% or more over the entire wavelength range of 400 to 700 nm when a coating film having a thickness of 2 μm is formed, and the transmittance is preferably 95% or more. The alkali-soluble resin (B) can be classified into a non-photosensitive alkali-soluble resin and a photosensitive alkali-soluble resin. Examples of the alkali-soluble group include a carboxyl group, a phosphoric acid group, a sulfonic acid group, a hydroxyl group, and a phenolic hydroxyl group. Among these, a carboxyl group is preferable. The alkali-soluble resin (B) can also contain a thermosetting group such as an epoxy group or an oxetanyl group.
[0057] (Non-photosensitive alkali-soluble resin) Examples of the non-photosensitive alkali-soluble resin include an acrylic resin having an acidic group, an α-olefin / maleic acid (anhydride) copolymer, a styrene / styrene sulfonic acid copolymer, an ethylene / (meth)acrylic acid copolymer, an isobutylene / maleic acid (anhydride) copolymer, etc. Among these, an acrylic resin having an acidic group and a styrene / styrene sulfonic acid copolymer are preferred.
[0058] (Photosensitive alkali-soluble resin) The photosensitive alkali-soluble resin is an alkali-soluble resin having a polymerizable unsaturated group. The photosensitive alkali-soluble resin is preferably a resin synthesized by the following method (i) or (ii). When cured with active energy rays, the resin is three-dimensionally crosslinked, increasing the crosslink density and improving chemical resistance.
[0059] [Method (i)] In the method (i), for example, a polymer of an epoxy group-containing monomer and other monomers is first synthesized, and then a monocarboxyl group-containing monomer is added to the epoxy group of the polymer, and a polybasic acid anhydride is reacted with the generated hydroxyl group to obtain a photosensitive alkali-soluble resin.
[0060] Examples of the epoxy group-containing monomer include glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, 2-glycidoxyethyl (meth)acrylate, 3,4-epoxybutyl (meth)acrylate, and 3,4-epoxycyclohexyl (meth)acrylate. Among these, glycidyl (meth)acrylate is preferred from the viewpoint of reactivity.
[0061] Examples of other monomers include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxy (meth)acrylates such as diethylene glycol (meth)acrylate, methoxy polypropylene glycol (meth)acrylate, ethoxy polyethylene glycol (meth)acrylate, ethylene oxide (EO) modified cresol acrylate, n-nonylphenoxy polyethylene glycol acrylate, phenoxyethyl acrylate, ethoxylated phenyl acrylate, EO modified (meth)acrylate of phenol, EO or propylene oxide (PO) modified (meth)acrylate of paracumylphenol, EO modified (meth)acrylate of nonylphenol, PO modified (meth)acrylate of nonylphenol, etc.; (Meth)acrylamides such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, diacetone(meth)acrylamide, or acryloylmorpholine; Styrene or styrenes such as alpha-methylstyrene; vinyl ethers such as ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, or isobutyl vinyl ether; vinyl acetate or vinyl propionate or other vinyl fatty acids; Cyclohexylmaleimide, phenylmaleimide, methylmaleimide, ethylmaleimide, 1,2-bismaleimidoethane 1,6-bismaleimidohexane, 3-maleimidopropionic acid, 6,7-methylenedioxy-4-methyl-3-maleimidocoumarin, 4,4'-bismaleimidodiphenylmethane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, N,N'-1,3-phenylenedimaleimide, N,N'-1,4-phenylenedimaleimide, N-(1-pyrenyl)maleimide, N-(2,4,6-trichloro N-substituted maleimides such as N-(4-aminophenyl)maleimide, N-(4-nitrophenyl)maleimide, N-benzylmaleimide, N-bromomethyl-2,3-dichloromaleimide, N-succinimidyl-3-maleimidobenzoate, N-succinimidyl-3-maleimidopropionate, N-succinimidyl-4-maleimidobutyrate, N-succinimidyl-6-maleimidohexanoate, N-[4-(2-benzimidazolyl)phenyl]maleimide, and 9-maleimidoacridine; Examples of the monomer include phosphate group-containing monomers such as 2-(meth)acryloyloxyethyl acid phosphate and compounds in which the hydroxyl group of a hydroxyl group-containing monomer described below is reacted with a phosphate esterifying agent such as phosphorus pentoxide or polyphosphoric acid.
[0062] Examples of the monocarboxyl group-containing monomer include monocarboxylic acids such as (meth)acrylic acid, crotonic acid, o-, m-, and p-vinylbenzoic acid, and (meth)acrylic acid substituted with haloalkyl, alkoxyl, halogen, nitro, or cyano at the α-position.
[0063] Examples of polybasic acid anhydrides include tetrahydrophthalic anhydride, phthalic anhydride, hexahydrophthalic anhydride, succinic anhydride, maleic anhydride, etc. If necessary, the remaining anhydride groups can be hydrolyzed using a tricarboxylic dianhydride such as trimellitic anhydride or a tetracarboxylic dianhydride such as pyromellitic anhydride.
[0064] As a method similar to method (i), for example, a polymer of a carboxyl group-containing monomer and other monomers is synthesized, and then an epoxy group-containing monomer is added to a part of the carboxyl groups of the polymer to obtain a photosensitive alkali-soluble resin.
[0065] [Method (ii)] In the method (ii), for example, a polymer of a hydroxyl group-containing monomer, a monocarboxyl group-containing monomer, and other monomers is synthesized, and then the hydroxyl group of the polymer is reacted with an isocyanate group of an isocyanate group-containing monomer.
[0066] Examples of the hydroxyl group-containing monomer include hydroxyalkyl methacrylates such as 2-hydroxyethyl (meth)acrylate, 2- or 3-hydroxypropyl (meth)acrylate, 2-, 3- or 4-hydroxybutyl (meth)acrylate, glycerol mono(meth)acrylate, and cyclohexanedimethanol mono(meth)acrylate. Other examples include polyether mono(meth)acrylate obtained by addition polymerization of ethylene oxide, propylene oxide, and / or butylene oxide to a hydroxyalkyl (meth)acrylate, and polyester mono(meth)acrylate obtained by addition of polyγ-valerolactone, polyε-caprolactone, and / or poly12-hydroxystearic acid. Among these, 2-hydroxyethyl methacrylate and glycerol mono(meth)acrylate are preferred in terms of preventing foreign matter from being generated in the coating. Glycerol mono(meth)acrylate is also preferred in terms of photosensitivity.
[0067] Examples of the isocyanate group-containing monomer include 2-(meth)acryloylethyl isocyanate, 2-(meth)acryloyloxyethyl isocyanate, and 1,1-bis[methacryloyloxy]ethyl isocyanate.
[0068] As the monocarboxyl group-containing monomer and other monomers, those mentioned above can be used.
[0069] The raw materials used in the synthesis of the alkali-soluble resin (B) can be used alone or in combination of two or more kinds.
[0070] The alkali-soluble resin (B) can be used alone or in combination of two or more kinds.
[0071] From the viewpoint of developability, the weight average molecular weight (Mw) of the alkali-soluble resin (B) is preferably 2,000 to 40,000, more preferably 3,000 to 300,000, and particularly preferably 4,000 to 20,000. The value of Mw / Mn is preferably 10 or less. An appropriate weight average molecular weight (Mw) improves adhesion to a substrate and solubility in alkaline development.
[0072] The acid value of the alkali-soluble resin (B) is preferably from 50 to 200 mgKOH / g, more preferably from 70 to 180 mgKOH / g, and even more preferably from 90 to 170 mgKOH / g. A suitable acid value improves adhesion to a substrate and solubility in alkaline development.
[0073] The content of the alkali-soluble resin (B) is preferably from 20 to 400 parts by mass, and more preferably from 50 to 250 parts by mass, based on 100 parts by mass of the colorant (A).
[0074] [Polymerizable compound (C)] (Polymerizable compound (C-1) having a 9,9-bisarylfluorene structure) The photosensitive coloring composition of the present invention contains a polymerizable compound (C) having a 9,9-bisarylfluorene structure (C-1). This makes it possible to obtain a cured film with low reflection, improved adhesion failure due to the difference in the degree of curing between the film surface and the inside during curing, and improved wrinkles during post-baking. The polymerizable compound (C) is a monomer or oligomer containing a polymerizable unsaturated group. Examples of the polymerizable unsaturated group include a vinyl group, a (meth)allyl group, a (meth)acryloyl group, and a (meth)acryloyloxy group.
[0075] Commercially available polymerizable compounds (C-1) having a 9,9-bisarylfluorene structure include OGSOL EA-0200, EA-0300, GA-5060P, and GA-2800 manufactured by Osaka Gas Chemicals Co., Ltd., and Miramer HR6060, HR6100, and HR6200 manufactured by Miwon Specialty Chemical Co., Ltd.
[0076] The glass transition temperature (hereinafter also referred to as Tg) of the polymerizable compound (C-1) having a 9,9-bisarylfluorene structure is preferably 200° C. or higher, more preferably 200 to 300° C., from the viewpoints of adhesion and wrinkle prevention. The glass transition temperature can be measured by a known method. For example, a cured film is prepared by reacting a polymerizable compound (C-1) having a 9,9-bisarylfluorene structure with a photopolymerization initiator, and the glass transition temperature can be measured by differential scanning calorimetry of the cured film. Specifically, the glass transition temperature can be measured by the method described in Example 2 of JP2009-173646A.
[0077] The polymerizable compound (C-1) having a 9,9-bisarylfluorene structure is preferably a compound represented by the following general formulas (1) to (3).
[0078] General formula (1) [ka]
[0079] (In general formula (1), R 1 , R 3 each independently represents a hydrogen atom or a methyl group; R 2 , R 4 each independently represents an alkylene group, and each of m and n independently represents an integer of 1 to 10.
[0080] General formula (2) [ka]
[0081] (In general formula (2), R 5 , R 6 each independently represents a hydrogen atom or a methyl group.
[0082] General formula (3) [ka]
[0083] (In general formula (3), R 7 , R 8 each independently represents a hydrogen atom or a methyl group.
[0084] Among these, from the viewpoint of adhesion, the compound represented by general formula (1) is more preferable, and the compound represented by the following chemical formula (4) is particularly preferable.
[0085] Chemical formula (4) [ka]
[0086] From the viewpoints of adhesion, wrinkle suppression, and reflectance, the content of the polymerizable compound (C-1) having a 9,9-bisarylfluorene structure is preferably 10 mass% or more, more preferably 20 to 80 mass%, and particularly preferably 30 to 60 mass%, based on 100 mass% of the polymerizable compound (C).
[0087] (Polymerizable compound having a urethane bond (C-2)) The photosensitive coloring composition of the present invention preferably contains a polymerizable compound (C-2) having a urethane bond, which can more effectively improve adhesion failure, pattern shape failure, and surface wrinkles caused by the difference in the degree of curing between the film surface and the inside during curing.
[0088] Examples of the polymerizable compound (C-2) having a urethane bond include urethane (meth)acrylates obtained by reacting a (meth)acrylate having a hydroxyl group with a polyfunctional isocyanate, and urethane (meth)acrylates obtained by reacting a polyhydric alcohol with a polyfunctional isocyanate and further reacting the polyhydric alcohol with a (meth)acrylate having a hydroxyl group.
[0089] Examples of the (meth)acrylate having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol tri(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol ethylene oxide modified penta(meth)acrylate, dipentaerythritol propylene oxide modified penta(meth)acrylate, dipentaerythritol caprolactone modified penta(meth)acrylate, glycerol acrylate methacrylate, glycerol dimethacrylate, 2-hydroxy-3-acryloylpropyl methacrylate, a reaction product of an epoxy group-containing compound and a carboxy(meth)acrylate, and a hydroxyl group-containing polyol polyacrylate.
[0090] Examples of the polyfunctional isocyanate include aromatic diisocyanates such as tolylene diisocyanate, diphenylmethylene diisocyanate, and xylene diisocyanate, aliphatic diisocyanates such as trimethylene diisocyanate, tetramethylene diisocyanate, and hexamethylene diisocyanate, and alicyclic diisocyanates such as isophorone diisocyanate, as well as biuret derivatives, isocyanate nurate derivatives, and trimethylolpropane adduct derivatives thereof.
[0091] The polymerizable compound (C-2) having a urethane bond may have an acid group. Examples of the acid group include a sulfonic acid group, a carboxyl group, and a phosphoric acid group. Among them, a carboxyl group is preferable. The polymerizable compound having a urethane bond and an acid group is preferably a compound represented by the following general formula (5). General formula (5)(H 2 C=C(R 1 )COO) m -X-(OCOCH(R 1 )CH 2 S(R 2 )COOH) n In general formula (5), R 1is a hydrogen atom or a methyl group, R 2 represents a hydrocarbon group having 1 to 12 carbon atoms, X represents an (m+n)-valent organic group having a urethane bond having 3 to 60 carbon atoms, m represents an integer of 2 to 18, and n represents an integer of 1 to 3.
[0092] The compound represented by the general formula (5) can be synthesized, for example, by first reacting the polyfunctional isocyanate compound with the (meth)acrylate having a hydroxyl group, and then adding a mercapto compound having a carboxyl group to the product.
[0093] Examples of the mercapto compound having a carboxyl group include mercaptoacetic acid, 2-mercaptopropionic acid, 3-mercaptopropionic acid, o-mercaptobenzoic acid, 2-mercaptonicotinic acid, and mercaptosuccinic acid.
[0094] From the viewpoint of preventing wrinkles, the polymerizable compound (C-2) having a urethane bond preferably contains an aliphatic urethane (meth)acrylate, which is a reaction product of a (meth)acrylate having a hydroxyl group and an aliphatic diisocyanate. The use of an aliphatic diisocyanate increases flexibility and reduces shrinkage during curing, thereby preventing wrinkles more effectively.
[0095] The number of polymerizable unsaturated groups in the polymerizable compound (C-2) having a urethane bond is preferably from 3 to 15, and more preferably from 6 to 12, from the viewpoints of adhesion and prevention of wrinkles.
[0096] Commercially available polymerizable compounds (C-2) having a urethane bond include AH-600, AT-600, UA-306H, UA-306T, UA-306I, UA-510H, UF-8001G, and DAUA-167 manufactured by Kyoeisha Chemical Co., Ltd., U-15HA, UA-160TM, and 1100H manufactured by Shin-Nakamura Chemical Co., Ltd., UV-4108F and UV-4117F manufactured by Osaka Organic Chemical Industry Co., Ltd., and EBECRY220, 1290, 4513, and 5129 manufactured by Daicel-Allnex Corporation.
[0097] The mass ratio of the polymerizable compound (C-1) having a 9,9-bisarylfluorene structure to the polymerizable compound (C-2) having a urethane bond is preferably 80:20 to 20:80, and more preferably 70:30 to 30:70.
[0098] The content of the polymerizable compound (C-2) having a urethane bond is preferably 40 mass% or more, more preferably 50 mass% or more, and particularly preferably 60 to 90 mass%, in 100 mass% of the polymerizable compound (C), that is, the total content of the polymerizable compound (C-1) having a 9,9-bisarylfluorene structure and the polymerizable compound (C-2) having a urethane bond.
[0099] (Polymerizable compound having an acid group (C-3)) The photosensitive coloring composition of the present invention can contain a polymerizable compound (C-3) having an acid group (excluding the above (C-2)). This can suppress development residues when forming a pattern by photolithography. Examples of the acid group of the polymerizable compound (C-3) having an acid group include a sulfonic acid group, a carboxyl group, a phosphoric acid group, etc. Among these, the carboxyl group is preferred.
[0100] Examples of the polymerizable compound (C-3) having an acid group include esters of free hydroxyl group-containing poly(meth)acrylates of polyhydric alcohols and (meth)acrylic acid with dicarboxylic acids; esters of polycarboxylic acids with monohydroxyalkyl (meth)acrylates; and the like. Examples of polyhydric alcohols include ethylene glycol, propylene glycol, polyethylene glycol, polypropylene glycol, glycerin, trimethylolpropane, ditrimethylolpropane, pentaerythritol, and dipentaerythritol. Examples of dicarboxylic acids include malonic acid, succinic acid, maleic acid, glutaric acid, phthalic acid, itaconic acid, and the like. Examples of polyvalent carboxylic acids include trimellitic acid and pyromellitic acid. Examples of monohydroxyalkyl (meth)acrylates include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, pentaerythritol triacrylate, and 2-hydroxy-3-acryloyloxypropyl methacrylate.
[0101] Commercially available products of the polymerizable compound (C-3) having an acid group include, for example, Viscoat #2500P manufactured by Osaka Organic Industries, and Aronix M-5300, M-5400, M-5700, M-510, M-520, and M-521 manufactured by Toagosei Co., Ltd.
[0102] (Other polymerizable compounds (C-4)) Examples of other polymerizable compounds (C-4) include methyl (meth)acrylate, ethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, cyclohexyl (meth)acrylate, β-carboxyethyl (meth)acrylate, polyethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, triethylene glycol di(meth)acrylate, and polypropylene glycol di(meth)acrylate. Tricyclodecane dimethanol di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, trimethylolpropane tri(meth)acrylate, phenoxytetraethylene glycol (meth)acrylate, phenoxyhexaethylene glycol (meth)acrylate, trimethylolpropane PO modified tri(meth)acrylate, trimethylolpropane EO modified tri(meth)acrylate, isocyanuric acid EO modified di(meth)acrylate, isocyanuric acid EO modified Examples of the acrylic acid esters and methacrylic acid esters include tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, 1,6-hexanediol diglycidyl ether di(meth)acrylate, bisphenol A diglycidyl ether di(meth)acrylate, neopentyl glycol diglycidyl ether di(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, tricyclodecanyl (meth)acrylate, (meth)acrylic acid esters of methylolated melamine, and epoxy (meth)acrylate, as well as various acrylic acid esters and methacrylic acid esters, styrene, vinyl acetate, hydroxyethyl vinyl ether, ethylene glycol divinyl ether, pentaerythritol trivinyl ether, (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, N-vinyl formamide, and acrylonitrile.
[0103] Other commercially available polymerizable compounds (C-4) include, for example, KAYARAD R-128H, R526, PEG400DA, MAND, NPGDA, R-167, HX-220, R-551, R712, R-604, R-684, GPO-303, TMPTA, DPHA, DPEA-12, DPHA-2C, D-310, D-330, DPCA-20, DPCA-30, DPCA-60, and DPCA-120 manufactured by Nippon Kayaku Co., Ltd., and Aronix M-303, M-305, M-306, M-309, and M-310 manufactured by Toagosei Co., Ltd. , M-321, M-325, M-350, M-360, M-313, M-315, M-400, M-402, M-403, M-404, M-405, M-406, M-450, M-452, M-408, M-211B, M-101A, NK Ester ABE-300, A-DOG, A-DCP, A-BPE-4 manufactured by Shin-Nakamura Chemical Co., Ltd., and EBECRY40, 130, 140, 145 manufactured by Daicel-Allnex Co., Ltd.
[0104] The polymerizable compound (C) can be used alone or in combination of two or more kinds.
[0105] The content of the polymerizable compound (C) is preferably from 1 to 60 mass%, more preferably from 5 to 55 mass%, particularly preferably from 10 to 50 mass%, based on 100 mass% of the nonvolatile content of the photosensitive coloring composition.
[0106] [Photopolymerization initiator (D)] The photosensitive coloring composition of the present invention contains a photopolymerization initiator (D). By containing the photopolymerization initiator (D), the photosensitive coloring composition can be cured by ultraviolet irradiation to form a cured film.
[0107] Examples of the photopolymerization initiator (D) include acetophenone-based compounds such as 4-phenoxydichloroacetophenone, 4-t-butyl-dichloroacetophenone, diethoxyacetophenone, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-(dimethylamino)-1-[4-(4-morpholino)phenyl]-2-(phenylmethyl)-1-butanone, and 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone; triazine-based compounds such as 2,4,6-trichloro-s-triazine, 2-phenyl-4,6-bis(trichloromethyl)-s-triazine, 2-(p-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(p-tolyl)-4,6-bis(trichloromethyl)-s-triazine, 2-piperonyl-4,6-bis(trichloromethyl)-s-triazine, 2,4-bis(trichloromethyl)-6-styryl-s-triazine, 2-(naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-methoxy-naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2,4-trichloromethyl-(piperonyl)-6-triazine, or 2,4-trichloromethyl-(4'-methoxystyryl)-6-triazine; Oxime ester compounds such as 1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], or ethanol, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime); Phosphine compounds such as bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide or diphenyl-2,4,6-trimethylbenzoylphosphine oxide; Examples of the compounds include quinone-based compounds such as 9,10-phenanthrenequinone, camphorquinone, and ethylanthraquinone; borate-based compounds; carbazole-based compounds; imidazole-based compounds; and titanocene-based compounds.
[0108] Commercially available products include acetophenone compounds manufactured by IGM Resins, such as "Omnirad 907" (2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one), "Omnirad 369E" (2-(dimethylamino)-1-[4-(4-morpholino)phenyl]-2-(phenylmethyl)-1-butanone), and "Omnirad 379EG" (2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone), and phosphine compounds manufactured by IGM Resins, such as "Omnirad 819" (bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide) and "Omnirad Examples of oxime compounds include 1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)] (IRGACURE OXE-01) manufactured by BASF Japan, ethanol, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime) (IRGACURE OXE 02) and IRGACURE OXE 04 manufactured by ADEKA Corporation, N-1919, NCI-730, NCI-831 and NCI-930 manufactured by Changzhou Strong New Materials Co., Ltd., and TRONLY TR-PBG-304, TRONLY TR-PBG-305, TRONLY TR-PBG-309 and TRONLY TR-PBG-3054 manufactured by Changzhou Strong New Materials Co., Ltd. Further examples include oxime-based compounds described in JP2007-210991A, JP2009-179619A, JP2010-037223A, JP2010-215575A, JP2011-020998A, International Publication WO2015 / 036910, etc. Among these, oxime-based compounds are preferred from the viewpoint of curability.
[0109] The photopolymerization initiator (D) can be used alone or in combination of two or more kinds.
[0110] The content of the photopolymerization initiator (D) is preferably from 2 to 50 parts by mass, and more preferably from 2 to 30 parts by mass, based on 100 parts by mass of the colorant (A) from the viewpoints of photocurability and developability.
[0111] [Near infrared absorbing agent (G)] In the photosensitive coloring composition of the present invention, when the colorant (A) contains two or more organic pigments and exhibits black color, it is preferable to contain a near infrared absorbing agent (G). This makes it possible to manufacture an infrared sensor that can block light in the visible light region and control the transmission of infrared light of a specific wavelength, thereby suppressing the generation of noise derived from visible light. The near infrared absorbing agent (G) is a compound that absorbs light with a wavelength of 750 to 1,200 nm.
[0112] Examples of the near infrared absorbent (G) include cyanine compounds, phthalocyanine compounds, naphthalocyanine compounds, immonium compounds, pyrrolopyrrole compounds, squarylium compounds, croconium compounds, etc. Among these, cyanine compounds, pyrrolopyrrole compounds, and squarylium compounds are preferred.
[0113] Among the near infrared absorbers (G), cyanine compounds are disclosed in International Publication No. WO2006 / 006573, International Publication No. WO2010 / 073857, JP2013-241598A, JP2016-113501A, and JP2016-113504A; phthalocyanine compounds are disclosed in JP4-23868A, JP06-192584A, JP2000-63691A, and International Publication No. WO2014 / 208514; naphthalocyanine compounds are disclosed in JP11-152414A, JP2000-86919A, JP2009-29955A, and International Publication No. WO2018 / 186490; immonium compounds are disclosed in , JP 2005-336150 A, JP 2007-197492 A, JP 2008-88426 A; pyrrolopyrrole compounds are described in JP 2009-263614 A, JP 2010-90313 A, JP 2011-068731 A; squarylium compounds are described in JP 2011-132361 A , JP 2016-142891 A, International Publication No. WO 2017 / 135359, International Publication No. WO 2018 / 225837, JP 2019-001987 A, International Publication No. WO 2020 / 054718; croconium compounds include compounds described in International Publication No. WO 2019 / 021767, etc.
[0114] The near infrared absorbing agent (G) can be used alone or in combination of two or more kinds.
[0115] The content of the near infrared absorber (G) is preferably 10 to 200 parts by mass, more preferably 15 to 150 parts by mass, and particularly preferably 20 to 100 parts by mass, relative to 100 parts by mass of the colorant (A) from the viewpoint of suppressing the generation of noise derived from visible light.
[0116] [Sensitizer (H)] The photosensitive coloring composition of the present invention can contain a sensitizer (H).
[0117] Examples of the sensitizer (H) include polymethine dyes such as chalcone derivatives, unsaturated ketones typified by dibenzalacetone, 1,2-diketone derivatives typified by benzil and camphorquinone, benzoin derivatives, fluorene derivatives, naphthoquinone derivatives, anthraquinone derivatives, xanthene derivatives, thioxanthene derivatives, xanthone derivatives, thioxanthone derivatives, coumarin derivatives, ketocoumarin derivatives, cyanine derivatives, merocyanine derivatives, and oxonol derivatives, acridine derivatives, azine derivatives, thiazine derivatives, oxazine derivatives, indoline derivatives, azulene derivatives, azulenium derivatives, squarylium derivatives, porphyrin derivatives, tetraphenylporphyrin derivatives, triarylmethane derivatives, tetrabenzoporphyrin derivatives, and tetrapyrazinoporphyrazine derivatives. conductors, phthalocyanine derivatives, tetraazaporphyrazine derivatives, tetraquinoxaliroporphyrazine derivatives, naphthalocyanine derivatives, subphthalocyanine derivatives, pyrylium derivatives, thiopyrylium derivatives, tetraphylline derivatives, annulene derivatives, spiropyran derivatives, spirooxazine derivatives, thiospiropyran derivatives, metal arene complexes, organic ruthenium complexes, or Michler's ketone derivatives, α-acyloxy esters, acyl oxides, methylphenyl glyoxylate, benzyl, 9,10-phenanthrenequinone, camphorquinone, ethyl anthraquinone, 4,4'-diethylisophthalophenone, 3,3' or 4,4'-tetra(t-butylperoxycarbonyl)benzophenone, 4,4'-bis(diethylamino)benzophenone, and the like.
[0118] Among the sensitizers (H), thioxanthone derivatives, Michler's ketone derivatives, and carbazole derivatives are preferred.Specific examples of preferred compounds include 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-dichlorothioxanthone, 2-isopropylthioxanthone, 4-isopropylthioxanthone, 1-chloro-4-propoxythioxanthone, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, 4,4'-bis(ethylmethylamino)benzophenone, N-ethylcarbazole, 3-benzoyl-N-ethylcarbazole, and 3,6-dibenzoyl-N-ethylcarbazole.
[0119] The sensitizer (H) can be used alone or in combination of two or more kinds.
[0120] The content of the sensitizer (H) is preferably 3 to 60 parts by mass, more preferably 5 to 50 parts by mass, based on 100 parts by mass of the photopolymerization initiator (D). When an appropriate amount is contained, photocurability and developability are improved.
[0121] [Thermosetting compound (I)] The photosensitive coloring composition of the present invention can contain a thermosetting compound (I). This allows the thermosetting compound (I) to react in the heating step, increasing the crosslink density and improving the heat resistance.
[0122] The thermosetting compound (I) may be a low molecular weight compound or a high molecular weight compound such as a resin. Examples of the thermosetting compound (I) include epoxy compounds, oxetane compounds, benzoguanamine compounds, rosin-modified maleic acid compounds, rosin-modified fumaric acid compounds, melamine compounds, urea compounds, and phenol compounds. Among these, epoxy compounds and oxetane compounds are preferred.
[0123] (Epoxy compound (I-1)) Examples of the epoxy compound (I-1) include polycondensates of bisphenols (bisphenol A, bisphenol F, bisphenol S, biphenol, bisphenol AD, etc.), polycondensates of phenols (phenol, alkyl-substituted phenol, aromatic-substituted phenol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, alkyl-substituted dihydroxybenzene, dihydroxynaphthalene, etc.) and various aldehydes (formaldehyde, acetaldehyde, alkyl aldehyde, benzaldehyde, alkyl-substituted benzaldehyde, hydroxybenzaldehyde, naphthaldehyde, glutaraldehyde, phthalaldehyde, crotonaldehyde, cinnamaldehyde, etc.), polycondensates of phenols and various diene compounds (dicyclopentadiene, terpenes, vinylcyclohexene, norbornadiene, vinylnorbornene, tetrahydroindene, divinylbenzene, etc.), and polycondensates of phenols and various diene compounds (dicyclopentadiene, terpenes, vinylcyclohexene, norbornadiene, vinylnorbornene, tetrahydroindene, divinylbenzene, etc.). Examples of such epoxy resins include polymers of phenols and ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, benzophenone, etc.), polycondensates of phenols and aromatic dimethanols (benzene dimethanol, α,α,α',α'-benzene dimethanol, biphenyl dimethanol, α,α,α',α'-biphenyl dimethanol, etc.), polycondensates of phenols and aromatic dichloromethyls (α,α'-dichloroxylene, bischloromethylbiphenyl, etc.), polycondensates of bisphenols and various aldehydes, glycidyl ether epoxy resins obtained by glycidylating alcohols, alicyclic epoxy resins, heterocyclic epoxy resins, aliphatic epoxy resins, glycidyl amine epoxy resins, and glycidyl ester epoxy resins.
[0124] Commercially available products include, for example, Epicoat 807, 815, 825, 827, 828, 190P, and 191P manufactured by Yuka Shell Epoxy Co., Ltd., and TECHMORE manufactured by Mitsui Chemicals, Inc. VG3101L, EPPN-201, 501H, 502H, EOCN-102S, 103S, 104S, 1020 manufactured by Nippon Kayaku Co., Ltd., Epicoat 1004, 1256, JER1032H60, 157S65, 157S70, 152, 154 manufactured by Japan Epoxy Resins Co., Ltd., Celloxide 2021, EHPE-3150 manufactured by Daicel Chemical Industries, Ltd., Denacol EX-211, 212, 252, 313, 314, 321, 411, 421, 512, 521, 611, 612, 614, 614B, 622, 711, 721 manufactured by Nagase ChemteX Corporation, TEPIC-L, H, S manufactured by Nissan Chemical Industries, Ltd., and the like.
[0125] The content of the epoxy compound (I-1) is preferably from 0.5 to 300 parts by mass, and more preferably from 1.0 to 50 parts by mass, based on 100 parts by mass of the colorant (A) from the viewpoint of heat resistance of the cured film.
[0126] (Oxetane Compound (I-2)) The oxetane compound (I-2) is a known compound having an oxetane group. Examples of the oxetane compound include monofunctional oxetane compounds, bifunctional oxetane compounds, and trifunctional or higher oxetane compounds.
[0127] Examples of monofunctional oxetane compounds include (3-ethyloxetan-3-yl)methyl acrylate, (3-ethyloxetan-3-yl)methyl methacrylate, 3-ethyl-3-hydroxymethyloxetane, 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, 3-ethyl-3-(phenoxymethyl)oxetane, 3-ethyl-3-(2-methacryloxymethyl)oxetane, and 3-ethyl-3-{[3-(triethoxysilyl)propoxy]methyl}oxetane.
[0128] Examples of commercially available products include OXE-10,30 manufactured by Osaka Organic Chemical Industry Co., Ltd. and OXT-101,212 manufactured by Toagosei Co., Ltd.
[0129] Examples of the bifunctional oxetane compound include 4,4'-bis[(3-ethyl-3-oxetanyl)methoxymethyl]biphenyl), 1,4-bis[(3-ethyl-3-oxetanyl)methoxymethyl]benzene, 1,4-bis{[(3-ethyl-3-oxetanyl)methoxy]methyl}benzene, di[1-ethyl(3-oxetanyl)]methyl ether, di[1-ethyl(3-oxetanyl)]methyl ether 3-ethyl-3-hydroxymethyl oxetane, 3- Ethyl-3-(2-ethylhexyloxymethyl)oxetane, 3-ethyl-3-(2-phenoxymethyl)oxetane, 3,7-bis(3-oxetanyl)-5-oxa-nonane, 1,2-bis[(3-ethyl-3-oxetanylmethoxy)methyl]ethane, 1,3-bis[(3-ethyl-3-oxetanylmethoxy)methyl]propane, ethyleneglycol bis(3-ethyl-3-oxetanylmethyl)ether, dicyclopentenyl bis(3-ethyl- 3-oxetanylmethyl) ether, triethylene glycol bis(3-ethyl-3-oxetanylmethyl) ether, tetraethylene glycol bis(3-ethyl-3-oxetanylmethyl) ether, 1,4-bis(3-ethyl-3-oxetanylmethoxy)butane, 1,6-bis(3-ethyl-3-oxetanylmethoxy)hexane, polyethylene glycol bis(3-ethyl-3-oxetanylmethyl) ether, ethylene oxide (EO)-modified bisphenol A bis(3-ethyl-3-oxetanylmethyl) ether, propylene oxide (PO)-modified bisphenol A bis(3-ethyl-3-oxetanylmethyl) ether, EO-modified hydrogenated bisphenol A bis(3-ethyl-3-oxetanylmethyl) ether, PO-modified hydrogenated bisphenol A bis(3-ethyl-3-oxetanylmethyl) ether, EO-modified bisphenol F(3-ethyl-3-oxetanylmethyl) ether, and the like.
[0130] Examples of commercially available products include OXBP and OXTP manufactured by Ube Industries, and OXT-121 and 221 manufactured by Toagosei.
[0131] Examples of the trifunctional or higher oxetane compounds include pentaerythritol tris(3-ethyl-3-oxetanylmethyl)ether, pentaerythritol tetrakis(3-ethyl-3-oxetanylmethyl)ether, dipentaerythritol hexa(3-ethyl-3-oxetanylmethyl)ether, dipentaerythritol pentakis(3-ethyl-3-oxetanylmethyl)ether, dipentaerythritol tetrakis(3-ethyl-3-oxetanylmethyl)ether, and caprolactone-modified dipentaerythritol. Examples of such polymers include erythritol hexa(3-ethyl-3-oxetanylmethyl) ether, caprolactone-modified dipentaerythritol pentakis(3-ethyl-3-oxetanylmethyl) ether, ditrimethylolpropane tetrakis(3-ethyl-3-oxetanylmethyl) ether, resins containing an oxetane group (e.g., the oxetane-modified phenol novolac resin described in Japanese Patent No. 3783462), and polymers obtained by radical polymerization of (meth)acrylic monomers such as the above-mentioned OXE-30.
[0132] The content of the oxetane compound (I-2) is preferably from 0.5 to 50 mass %, and more preferably from 1 to 40 mass %, in 100 mass % of the nonvolatile content of the photosensitive coloring composition.
[0133] The melamine compound is a compound having a melamine ring structure. The melamine compound is preferably a methylol type or ether type compound, and more preferably a melamine compound having an average of 5.0 or more methylol groups and / or ether groups per melamine ring. If the compound has an appropriate number of methylol groups or ether groups, it is easy to obtain just the right amount of heat resistance.
[0134] Examples of commercially available products include Nikalac MW-30HM, MW-390, MW-100LM, MX-750LM, MW-30M, MW-30, MW-22, MS-21, MS-11, MW-24X, MS-001, MX-002, MX-730, MX-750, MX-708, MX-706, MX-042, MX-45, MX-500, MX-520, MX-43, MX-417, and MX-410 manufactured by Sanwa Chemical Co., Ltd., and Cymel 232, 235, 236, 238, 285, 300, 301, 303, 350, and 370 manufactured by Nippon Cytec Industries Co., Ltd.
[0135] Among these, Nikarak MW-30HM, MW-390, MW-100LM, MX-750LM, MW-30M, MW-30, MW-22, MS-21, MS-11, MW-24X, MX-45 (all manufactured by Sanwa Chemical Co., Ltd.), Cymel 232, 235, 236, 238, 300, 301, 303, 350 (all manufactured by Nippon Cytec Industries Co., Ltd.), and the like, which have an average of 5.0 or more methylol groups and / or ether groups per melamine ring, are preferred in terms of increasing the crosslink density.
[0136] The thermosetting compound (I) can be used alone or in combination of two or more kinds.
[0137] [Hardening agent (curing accelerator)] The photosensitive coloring composition of the present invention can be used in combination with a curing agent (curing accelerator) to aid in the curing of the thermosetting compound (I). Examples of the curing agent include amine compounds, acid anhydrides, active esters, carboxylic acid compounds, and sulfonic acid compounds. Examples of the curing agent include amine compounds (e.g., dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, 4-methyl-N,N-dimethylbenzylamine, etc.), quaternary ammonium salt compounds (e.g., triethylbenzylammonium chloride, etc.), blocked isocyanate compounds (e.g., dimethylamine, etc.), imidazole derivatives, bicyclic amidine compounds and their salts (e.g., imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole, etc.), phosphorus compounds (e.g., triphenylphosphine, etc.), S-triazine derivatives (e.g., 2,4-diamino-6-methacryloyloxyethyl-S-triazine, 2-vinyl-2,4-diamino-S-triazine, 2-vinyl-4,6-diamino-S-triazine·isocyanuric acid adduct, 2,4-diamino-6-methacryloyloxyethyl-S-triazine·isocyanuric acid adduct, etc.).
[0138] The curing agents can be used alone or in combination of two or more kinds.
[0139] The content of the curing agent is preferably 0.01 to 15 parts by mass based on 100 parts by mass of the thermosetting compound (I).
[0140] [Thiol-based chain transfer agents (J)] The photosensitive coloring composition of the present invention can contain a thiol chain transfer agent (J). When the thiol chain transfer agent (J) is used in combination with the photopolymerization initiator (D), a thiyl radical that is not easily inhibited by oxygen during radical polymerization after irradiation with light is generated, improving the photosensitivity of the photosensitive coloring composition.
[0141] The thiol chain transfer agent (J) is preferably a polyfunctional thiol having two or more thiol groups (SH groups). It is more preferable that the thiol chain transfer agent has four or more SH groups. As the number of functional groups increases, the film becomes easier to photocure from the surface to the deepest part.
[0142] Examples of polyfunctional thiols include hexanedithiol, decanedithiol, 1,4-butanediol bisthiopropionate, 1,4-butanediol bisthioglycolate, ethylene glycol bisthioglycolate, ethylene glycol bisthiopropionate, trimethylolpropane tristhioglycolate, trimethylolpropane tristhiopropionate, trimethylolpropane tris(3-mercaptobutyrate), pentaerythritol tetrakisthioglycolate, pentaerythritol tetrakisthioglycolate, Examples of the thiopropionate include erythritol tetrakisthiopropionate, trimercaptopropionic acid tris(2-hydroxyethyl)isocyanurate, 1,4-dimethylmercaptobenzene, 2,4,6-trimercapto-s-triazine, 2-(N,N-dibutylamino)-4,6-dimercapto-s-triazine, and the like. Preferred examples include ethylene glycol bisthiopropionate, trimethylolpropane tristhiopropionate, and pentaerythritol tetrakisthiopropionate.
[0143] The thiol chain transfer agent (J) can be used alone or in combination of two or more kinds.
[0144] The content of the thiol chain transfer agent (J) is preferably 1 to 10 parts by mass, more preferably 2 to 8 parts by mass, based on 100 parts by mass of the nonvolatile content of the photosensitive coloring composition. When an appropriate amount is contained, the photosensitivity is improved and wrinkles are less likely to occur on the surface of the cured film.
[0145] [Polymerization inhibitor (K)] The photosensitive coloring composition of the present invention may contain a polymerization inhibitor (K). Examples of the polymerization inhibitor (K) include alkyl catechol compounds such as catechol, resorcinol, 1,4-hydroquinone, 2-methyl catechol, 3-methyl catechol, 4-methyl catechol, 2-ethyl catechol, 3-ethyl catechol, 4-ethyl catechol, 2-propyl catechol, 3-propyl catechol, 4-propyl catechol, 2-n-butyl catechol, 3-n-butyl catechol, 4-n-butyl catechol, 2-t-butyl catechol, 3-t-butyl catechol, 4-t-butyl catechol, and 3,5-di-t-butyl catechol; 2-methyl resorcinol, 4-methyl resorcinol, 2-ethyl resorcinol, 4-ethyl resorcinol, 2-propyl resorcinol, 4-propyl resorcinol, and 2-n-butyl catechol; Examples of the alkyl resorcinol compounds include ethylresorcinol, 4-n-butylresorcinol, 2-t-butylresorcinol, and 4-t-butylresorcinol; alkylhydroquinone compounds such as methylhydroquinone, ethylhydroquinone, propylhydroquinone, t-butylhydroquinone, and 2,5-di-t-butylhydroquinone; phosphine compounds such as tributylphosphine, trioctylphosphine, tricyclohexylphosphine, triphenylphosphine, and tribenzylphosphine; phosphine oxide compounds such as trioctylphosphine oxide and triphenylphosphine oxide; phosphite compounds such as triphenylphosphite and trisnonylphenylphosphite; pyrogallol; and phloroglucine.
[0146] The content of the polymerization inhibitor (K) is preferably 0.01 to 0.4 mass % in 100 mass % of the nonvolatile content of the photosensitive coloring composition.
[0147] [Ultraviolet absorber (L)] The photosensitive coloring composition of the present invention may contain an ultraviolet absorber (L). The ultraviolet absorber (L) is an organic compound having an ultraviolet absorbing function, and examples thereof include benzotriazole-based organic compounds, triazine-based organic compounds, benzophenone-based organic compounds, salicylic acid ester-based organic compounds, cyanoacrylate-based organic compounds, and salicylate-based organic compounds.
[0148] Benzotriazole compounds include, for example, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-(2-hydroxy-5-t-butylphenyl)-2H-benzotriazole, 2-[2-hydroxy-3,5-bis(α, α-Dimethylbenzyl)phenyl]-2H-benzotriazole, 2-(3-t-butyl-5-methyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, 5% 2-methoxy-1-methylethyl acetate and 95% benzenepropanoic acid, 3-(2H-benzotriazol-2-yl)-(1,1-dimethylethyl)-4-hydroxy, C7-9 side and linear alkyl ester mixture, 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol, 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol, methyl 3-(3-(2H-benzotriazol-2-yl)-5-t-butyl-4-hydroxyphenyl)propionate / polyethylene glycol 300 reaction products, 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol, 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol], 2-(2H-benzotriazol-2-yl)-p-cresol, 2-(5-chloro-2H-benzotriazol-2-yl)-6-t-butyl Examples of the hydroxyphenyl esters include 2-(3,5-di-t-amyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-5-[2-(methacryloyloxy)ethyl]phenyl]-2H-benzotriazole, octyl-3-[3-tert-butyl-4-hydroxy-5-(5-chloro-2H-benzotriazol-2-yl)phenyl]propionate, and 2-ethylhexyl-3-[3-tert-butyl-4-hydroxy-5-(5-chloro-2H-benzotriazol-2-yl)phenyl]propionate.
[0149] Examples of commercially available products include TINUVIN P, PS, 234, 326, 329, 384-2, 900, 928, 99-2, and 1130 manufactured by BASF Japan Ltd., ADK STAB LA-29, LA-31RG, LA-32, and LA-36 manufactured by ADEKA CORPORATION, KEMISORB71, 73, 74, 79, and 279 manufactured by Chemipro Chemical Co., Ltd., and RUVA-93 manufactured by Otsuka Chemical Co., Ltd.
[0150] Examples of triazine compounds include 2,4-bis(2,4-dimethylphenyl)-6-(2-hydroxy-4-n-octyloxyphenyl)-1,3,5-triazine, 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl]-5-[3-(dodecyloxy)-2-hydroxypropoxy]phenol, and the reaction product of 2-(2,4-dihydroxyphenyl)-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine with (2-ethylhexyl)-glycidic acid ester. Examples of the compound include 2,4-bis[2-hydroxy-4-butoxyphenyl]-6-(2,4-dibutoxyphenyl)-1,3,5-triazine, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-(hexyloxy)phenol, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]phenol, and 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine.
[0151] Examples of commercially available products include KEMISORB 102 manufactured by Chemipro Chemicals, TINUVIN 400, 405, 460, 477, 479, and 1577ED manufactured by BASF Japan, Adeka STAB LA-46 and LA-F70 manufactured by ADEKA, and CYASORB UV-1164 manufactured by Sun Chemical.
[0152] Examples of benzophenone compounds include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone 5-sulfonic acid-3-water, 2-hydroxy-4-n-octoxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 4-dodecyloxy-2-hydroxybenzophenone, 2-hydroxy-4-octadecyloxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, and 2-hydroxy-4-methoxy-2'-carboxybenzophenone.
[0153] Examples of commercially available products include KEMISORB 10, 11, 11S, 12, and 111 manufactured by Chemipro Chemicals, SEESORB 101 and 107 manufactured by Shipro Chemicals, Adeka STAB 1413 manufactured by ADEKA, and UV-12 manufactured by Sun Chemical.
[0154] Examples of the salicylate ester compounds include phenyl salicylate, p-octylphenyl salicylate, and p-tert-butylphenyl salicylate.
[0155] The content of the ultraviolet absorber (L) is preferably from 5 to 70% by mass in 100% by mass of the total of the photopolymerization initiator (D) and the ultraviolet absorber (L).
[0156] [Antioxidants (M)] The photosensitive coloring composition of the present invention can contain an antioxidant (M). The antioxidant (M) prevents the photopolymerization initiator (D) and the thermosetting compound (I) in the photosensitive coloring composition from yellowing due to oxidation caused by the thermal process during thermal curing or ITO annealing. In particular, when the concentration of the colorant (A) in the photosensitive coloring composition is high, the content of the polymerizable compound (C) is relatively reduced, so that the cured film is likely to yellow if the amount of the photopolymerization initiator (D) is increased or a thermosetting compound is added. Therefore, by including an antioxidant, the yellowing of the cured film due to oxidation during the heating process is prevented. In this specification, the antioxidant is preferably a compound that does not contain a halogen atom.
[0157] Examples of the antioxidant (M) include hindered phenol-based, hindered amine-based, phosphorus-based, sulfur-based, and hydroxylamine-based compounds, etc. Among these, hindered phenol-based antioxidants, hindered amine-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants are preferred.
[0158] Examples of the hindered phenol antioxidant include 1,3,5-tris(3,5-di-t-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 1,1,3-tris-(2'-methyl-4'-hydroxy-5'-t-butylphenyl)-butane, 4,4'-butylidene-bis-(2-t-butyl-5-methylphenol), 3-(3,5-di-t-butyl-4-hydroxyphenyl)stearyl propionate, pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 3,9-bis[2-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]Undecane, 1,3,5-tris(3,5-di-t-butyl-4-hydroxyphenylmethyl)-2,4,6-trimethylbenzene, 1,3,5-tris(3-hydroxy-4-t-butyl-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,2'-methylenebis(6-t-butyl-4-ethylphenol), 2,2'-thiodiethylbis-(3,5-di- t-Butyl-4-hydroxyphenyl)-propionate, N,N-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), i-octyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 4,6-bis(dodecylthiomethyl)-o-cresol, calcium salt of 3,5-di-t-butyl-4-hydroxybenzylphosphonic acid monoethyl ester, 4, 6-Bis(octylthiomethyl)-o-cresol, bis[3-(3-methyl-4-hydroxy-5-t-butylphenyl)propionic acid]ethylene bisoxybisethylene, 1,6-hexanediol bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,4-bis-(n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, 2 , 2'-thio-bis-(6-t-butyl-4-methylphenol), 2,5-di-t-amyl-hydroquinone, 2,6-di-t-butyl-4-nonylphenol, 2,2'-isobutylidene-bis-(4,6-dimethyl-phenol), 2,2'-methylene-bis-(6-(1-methyl-cyclohexyl)-p-cresol), 2,4-dimethyl-6-(1-methyl-cyclohexyl)-phenol, etc.
[0159] Examples of commercially available products include ADK STAB AO-20, AO-30, AO-40, AO-50, AO-60, AO-80, and AO-330 manufactured by ADEKA CORPORATION, KEMINOX 101, 179, 76, and 9425 manufactured by Chemipro Corporation, IRGANOX 1010, 1035, 1076, 1098, 1135, 1330, 1726, 1425WL, 1520L, 245, 259, 3114, 5057, and 565 manufactured by BASF Japan Ltd., and Cyanox CY-1790 and CY-2777 manufactured by Sun Chemical Company.
[0160] Examples of the hindered amine antioxidant include tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)-1,2,3,4-butane tetracarboxylate, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)1,2,3,4-butane tetracarboxylate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1-undecanoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate, 1,2,2,6,6-pentamethyl-4-piperidyl tetramethyl-4-piperidyl methacrylate, 2,2,6,6-tetramethyl-4-piperidyl methacrylate, polycondensation product of dimethyl succinate and 1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine, poly[[6-[(1,1,3,3-tetramethylbutyl)amino]-s-triazine-2,4-diyl]-[(2,2,6,6-tetramethyl-4-piperidyl)imino]-hexamethylene-[(2,2,6,6-tetramethyl-4-piperidyl)imino]], 4-hydroxy-2,2,6,6-tetramethyl-1- Ester of piperidineethanol with 3,5,5-trimethylhexanoic acid, N,N'-4,7-tetrakis[4,6-bis{N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino}-1,3,5-triazin-2-yl]-4,7-diazadecane-1,10-diamine, decanedioic acid bis(2,2,6,6-tetramethyl-1-(octyloxy)-4-piperidinyl)ester, reaction products of 1,1-dimethylethyl hydroperoxide with octane, bis(1,2,2,6,6-pentamethyl-4-pyridyl)[[3,5-bi 1,2,2,6,6-pentamethyl-4-pyridyl sebacate, poly[[6-morpholino-s-triazine-2,4-diyl]-[(2,2,6,6-tetramethyl-4-piperidyl)imino]-hexamethylene-[(2,2,6,6-tetramethyl-4-piperidyl)imino]], 2,2,6,6-tetramethyl-4-piperidyl-C12-21 and C18 unsaturated fatty acid esters, N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl)-1,6-Hexamethylenediamine, 2-methyl-2-(2,2,6,6-tetramethyl-4-piperidyl)amino-N-(2,2,6,6-tetramethyl-4-piperidyl)propionamide, etc.
[0161] Examples of commercially available products include ADK STAB LA-52, LA-57, LA-63P, LA-68, LA-72, LA-77Y, LA-77G, LA-81, LA-82, LA-87, LA-402F, and LA-502XP manufactured by ADEKA CORPORATION, KAMISTAB 29, 62, 77, and 94 manufactured by Chemipro Chemicals Co., Ltd., Tinuvin 111FDL, 123, 144, 249, 292, and 5100 manufactured by BASF Japan Ltd., and Cyasorb UV-3346, UV-3529, and UV-3853 manufactured by Sun Chemical Co., Ltd.
[0162] Examples of phosphorus-based antioxidants include di(2,6-di-t-butyl-4-methylphenyl)pentaerythritol diphosphite, distearyl pentaerythritol diphosphite, 2,2'-methylenebis(4,6-di-t-butylphenyl)2-ethylhexyl phosphite, tris(2,4-di-t-butylphenyl)phosphite, tris(nonylphenyl)phosphite, tetra(C12-C15 alkyl)-4,4'-isopropylidene diphenyl diphosphite, diphenyl mono (2-ethylhexyl)phosphite, diphenyl isodecyl phosphite, tris(isodecyl)phosphite, triphenyl phosphite, tetrakis(2,4-di-t-butylphenyl)-4,4-biphenyl diphosphonite, tris(tridecyl)phosphite, phenyl isooctyl phosphite, phenyl isodecyl phosphite, phenyl di(tridecyl)phosphite, diphenyl isooctyl phosphite, diphenyl tridecyl phosphite, 4,4'-isopropylide diphenol alkyl phosphite, trisnonylphenyl phosphite, trisdinonylphenyl phosphite, tris(biphenyl) phosphite, di(2,4-di-t-butylphenyl)pentaerythritol diphosphite, di(nonylphenyl)pentaerythritol diphosphite, phenyl bisphenol A pentaerythritol diphosphite, tetratridecyl 4,4'-butylidenebis(3-methyl-6-t-butylphenol) diphosphite, hexatridecyl Examples of such phosphite include 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane triphosphite, 3,5-di-t-butyl-4-hydroxybenzyl phosphite diethyl ester, sodium bis(4-t-butylphenyl)phosphite, sodium-2,2-methylene-bis(4,6-di-t-butylphenyl)-phosphite, 1,3-bis(diphenoxyphosphonyloxy)-benzene, and ethyl bis(2,4-di-t-butyl-6-methylphenyl)phosphite.
[0163] Examples of commercially available products include Adeka STAB PEP-36, PEP-8, HP-10, 2112, 1178, 1500, C, 135A, 3010, and TPP manufactured by ADEKA CORPORATION, IRGAFOS168 manufactured by BASF Japan Ltd., and HostanoxP-EPQ manufactured by Clariant Chemicals.
[0164] Examples of sulfur-based antioxidants include 2,2-bis{[3-(dodecylthio)-1-oxopropoxy]methyl}propane-1,3-diylbis[3-(dodecylthio)propionate], ditridecyl 3,3'-thiobispropionate, 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,4-bis[(octylthio)methyl]-o-cresol, and 2,4-bis[(laurylthio)methyl]-o-cresol.
[0165] Examples of commercially available products include Adeka STAB AO-412S and AO-503 manufactured by ADEKA CORPORATION, and KEMINOXPLS manufactured by Chemipro Chemicals.
[0166] The antioxidants (M) can be used alone or in combination of two or more kinds.
[0167] The content of the antioxidant (M) is preferably 0.5 to 5.0% by mass based on 100% by mass of the nonvolatile content of the photosensitive coloring composition. When an appropriate amount is contained, the transmittance, spectral characteristics, and sensitivity are improved.
[0168] [Leveling agent (N)] The photosensitive coloring composition of the present invention can contain a leveling agent (N). This improves the wettability and drying property of the composition when applied to a substrate. Examples of the leveling agent (N) include silicone surfactants, fluorine surfactants, nonionic surfactants, cationic surfactants, anionic surfactants, and amphoteric surfactants.
[0169] Examples of silicone surfactants include linear polymers consisting of siloxane bonds and modified siloxane polymers in which organic groups have been introduced into the side chains or ends.
[0170] Commercially available products include, for example, BYK-300, 306, 310, 313, 315N, 320, 322, 323, 330, 331, 333, 342, 345, 346, 347, 348, 349, 370, 377, 378, 3455, UV3510, and 3570 manufactured by BYK-Chemie Co., Ltd., and FZ-7002 and 211 manufactured by Dow Corning Toray Co., Ltd. 0, 2122, 2123, 2191, 5609, and Shin-Etsu Chemical Co., Ltd.'s X-22-4952, X-22-4272, X-22-6266, KF-351A, KF-354L, KF-355A, KF-945, KF-640, KF-642, KF-643, X-22-4515, KF-6004, and KP-341.
[0171] The fluorosurfactant may be, for example, a surfactant or a leveling agent having a fluorocarbon chain.
[0172] Examples of commercially available products include Surflon S-242, 243, 420, 611, 651, and 386 manufactured by AGC Seimi Chemical Co., Ltd., Megafac F-253, 477, 551, 552, 555, 558, 560, 570, 575, and 576, R-40-LM, R-41, RS-72-K, and DS-21 manufactured by DIC Corporation, FC-4430 and 4432 manufactured by Sumitomo 3M Limited, EF-PP31N09, EF-PP33G1, and EF-PP32C1 manufactured by Mitsubishi Materials Electronic Chemicals Co., Ltd., and Futergent 602A manufactured by Neos Corporation.
[0173] Examples of nonionic surfactants include polyoxyethylene lauryl ether, polyoxyethylene cetyl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, polyoxyethylene alkyl ether, polyoxyethylene myristyl ether, polyoxyethylene octyldodecyl ether, polyoxyalkylene alkyl ether, polyoxyphenylenedistyrenated phenyl ether, polyoxyethylene tribenzyl phenyl ether, polyoxyethylene polyoxypropylene glycol, polyoxyalkylene alkenyl ether, polyoxyethylene nonyl phenyl ether, polyoxyethylene alkyl ether phosphate ester, sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan distearate, and sorbitan tristearate. sorbitan monooleate, sorbitan trioleate, sorbitan sesquioleate, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan tristearate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan triisostearate, polyoxyethylene sorbitan tetraoleate, glycerol monostearate, glycerol monooleate, polyethylene glycol monolaurate, polyethylene glycol monostearate, polyethylene glycol distearate, polyethylene glycol monooleate, polyoxyethylene hydrogenated castor oil, polyoxyethylene alkylamines, alkyl alkanolamides, alkyl imidazolines, and the like.
[0174] Commercially available products include, for example, Emulgen 103, 104P, 106, 108, 109P, 120, 123P, 130K, 147, 150, 210P, 220, 306P, 320P, 350, 404, 408, 409PV, 420, 430, 705, 707, 709, 1108, 1118S-70, 1135S-70, 1150S-60, 2020G-HA, 2025G, LS-106, and L manufactured by Kao Corporation. S-110, LS-114, MS-110, A-60, A-90, B-66, PP-290, LATEMURU PD-420, PD-430, PD-430S, PD-450, Leodor SP-L10, SP-P10, SP-S10V, SP-S20, SP-S30V, SP-O10V, SP-O30V, Super SP-L10, AS-10V, AO-10V, AO-15V, TW-L120, TW- L106, TW-P120, TW-S120V, TW-S320V, TW-O120V, TW-O106V, TW-IS399C, Super TW-L120, 430V, 440V, 460V, MS-50, MS-60, MO-60, MS-165V, Emanon 1112, 3199V, 3299V, 3299RV, 4110, CH-25, CH-40, CH-60(K), Ami-to 102, Examples of such polymers include 105, 105A, 302, 320, Aminone PK-02S, L-02, Homogenol L-95, ADEKA Pluronic (registered trademark) L-23, 31, 44, 61, 62, 64, 71, 72, 101, 121, TR-701, 702, 704, 913R manufactured by ADEKA Corporation, and (meth)acrylic acid-based (co)polymer Polyfluor No. 75, No. 90, No. 95 manufactured by Kyoeisha Chemical Co., Ltd.
[0175] Examples of the cationic surfactant include alkylamine salts, alkyl quaternary ammonium salts such as lauryltrimethylammonium chloride, stearyltrimethylammonium chloride, and cetyltrimethylammonium chloride, and ethylene oxide adducts thereof.
[0176] Commercially available products include, for example, Acetamine 24, Cortamine 24P, 60W, and 86P Concentrate manufactured by Kao Corporation.
[0177] Examples of the anionic surfactant include polyoxyethylene alkyl ether sulfate, sodium dodecylbenzenesulfonate, alkali salts of styrene-acrylic acid copolymers, sodium alkylnaphthalenesulfonate, sodium alkyldiphenyletherdisulfonate, monoethanolamine lauryl sulfate, triethanolamine lauryl sulfate, ammonium lauryl sulfate, monoethanolamine stearate, sodium stearate, sodium lauryl sulfate, monoethanolamine styrene-acrylic acid copolymers, and polyoxyethylene alkyl ether phosphates.
[0178] Examples of commercially available products include Futergent 100 and 150 manufactured by Neos Corporation, and Adeka Hope YES-25, Adeka Col TS-230E, PS-440E, and EC-8600 manufactured by ADEKA Corporation.
[0179] Examples of amphoteric surfactants include alkyl betaines such as lauric acid amidopropyl betaine, lauryl betaine, cocamidopropyl betaine, stearyl betaine, and alkyl dimethyl amino acetate betaine; and alkyl amine oxides such as lauryl dimethyl amine oxide.
[0180] Commercially available products include Anhythol 20AB, 20BS, 24B, 55AB, 86B, 20Y-B, and 20N manufactured by Kao Corporation.
[0181] The leveling agents (N) can be used alone or in combination of two or more kinds.
[0182] The content of the leveling agent (N) is preferably 0.001 to 2.0 mass%, more preferably 0.005 to 1.0 mass%, based on 100 mass% of the nonvolatile content of the photosensitive coloring composition. When an appropriate amount is contained, the balance between the coatability and adhesion of the photosensitive coloring composition is further improved.
[0183] [Storage stabilizer (O)] The photosensitive coloring composition of the present invention can contain a storage stabilizer (O). This stabilizes the viscosity of the photosensitive coloring composition over time. Examples of the storage stabilizer (O) include quaternary ammonium chlorides such as benzyl trimethyl chloride and diethylhydroxyamine, organic acids such as lactic acid and oxalic acid and their methyl ethers, organic phosphines such as t-butyl pyrocatechol, tetraethylphosphine, and tetraphenyl, and phosphites.
[0184] The content of the storage stabilizer (O) is preferably 0.1 to 10 parts by mass based on 100 parts by mass of the colorant (A).
[0185] [Adhesion improver (P)] The photosensitive coloring composition of the present invention can contain an adhesion improver (P). This improves the adhesion between the cured film and the substrate. In addition, it becomes easier to form a narrow pattern by photolithography.
[0186] Examples of the adhesion improver (P) include silane coupling agents. Examples of the silane coupling agent include vinyl silanes such as vinyl trimethoxysilane and vinyl triethoxysilane, (meth)acrylic silanes such as 3-methacryloxypropyl methyl dimethoxysilane, 3-methacryloxypropyl trimethoxysilane, 3-methacryloxypropyl methyl diethoxysilane, 3-methacryloxypropyl triethoxysilane, and 3-acryloxypropyl trimethoxysilane, epoxy silanes such as 2-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, 3-glycidoxypropyl methyl dimethoxysilane, 3-glycidoxypropyl trimethoxysilane, 3-glycidoxypropyl methyl diethoxysilane, and 3-glycidoxypropyl triethoxysilane, N-2-(aminoethyl)-3-aminopropyl methyl dimethoxysilane, N-2-(aminoethyl) silane coupling agents such as aminosilanes such as 3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, and N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane hydrochloride; mercaptos such as 3-mercaptopropylmethyldimethoxysilane and 3-mercaptopropyltrimethoxysilane; styryls such as p-styryltrimethoxysilane; ureidos such as 3-ureidopropyltriethoxysilane; sulfides such as bis(triethoxysilylpropyl)tetrasulfide; and isocyanates such as 3-isocyanatepropyltriethoxysilane.
[0187] The adhesion improver (P) can be used alone or in combination of two or more kinds.
[0188] The content of the adhesion improver (P) is preferably from 0.01 to 10 parts by mass, and more preferably from 0.05 to 5 parts by mass, based on 100 parts by mass of the colorant (A).
[0189] [Organic solvent (Q)] The photosensitive composition of the present invention may contain an organic solvent (Q). The organic solvent (Q) may be, for example, 1,2,3-trichloropropane, 1-methoxy-2-propanol, ethyl lactate, 1,3-butanediol, 1,3-butylene glycol, 1,3-butylene glycol diacetate, 1,4-dioxane, 2-heptanone, 2-methyl-1,3-propanediol, 3,5,5-trimethyl-2-cyclohexen-1-one, 3,3,5-trimethylcyclohexanone, 3-ethoxyethyl propionate, 3-methyl-1,3-butanediol, 3-methoxy-3-methyl-1-butanol, 3-methoxy- 3-Methylbutyl acetate, 3-methoxybutanol, 3-methoxybutyl acetate, 4-heptanone, m-xylene, m-diethylbenzene, m-dichlorobenzene, N,N-dimethylacetamide, N,N-dimethylformamide, n-butyl alcohol, n-butylbenzene, n-propyl acetate, N-methylpyrrolidone, o-xylene, o-chlorotoluene, o-diethylbenzene, o-dichlorobenzene, p-chlorotoluene, p-diethylbenzene, sec-butylbenzene, tert-butylbenzene, γ-butyro lactone, isobutyl alcohol, isophorone, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, ethylene glycol monoisopropyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether acetate, ethylene glycol monotertiary butyl ether, ethylene glycol monobutyl ether, ethylene glycol monobutyl ether acetate, ethylene glycol monopropyl ether, ethylene glycol monohexyl ether, ethylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, diisobutyl ketone, diethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether, diethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether, cyclohexanol, cyclohexanol acetate, cyclohexanone, dipropylene glycol dimethyl ether,Examples of the dipropylene glycol methyl ether acetate include dipropylene glycol monoethyl ether, dipropylene glycol monobutyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monomethyl ether, diacetone alcohol, triacetin, tripropylene glycol monobutyl ether, tripropylene glycol monomethyl ether, propylene glycol diacetate, propylene glycol phenyl ether, propylene glycol monoethyl ether, propylene glycol monoethyl ether acetate, propylene glycol monobutyl ether, propylene glycol monopropyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether propionate, benzyl alcohol, methyl isobutyl ketone, methylcyclohexanol, n-amyl acetate, n-butyl acetate, isoamyl acetate, isobutyl acetate, propyl acetate, and dibasic acid esters. Among these, from the viewpoints of pigment dispersibility and alkali-soluble resin solubility, preferred are glycol acetates such as ethyl lactate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethylene glycol monomethyl ether acetate, and ethylene glycol monoethyl ether acetate, alcohols such as benzyl alcohol and diacetone alcohol, and ketones such as cyclohexanone.
[0190] The organic solvent (Q) can be used alone or in combination of two or more kinds.
[0191] [Method of producing photosensitive coloring composition] The photosensitive coloring composition of the present invention is produced by, for example, adding a colorant (A), an alkali-soluble resin (B), and, if necessary, a dye derivative (E), a dispersing resin (F), an organic solvent (Q), etc., and carrying out a dispersion treatment. Then, the dispersion is mixed with a polymerizable compound (C) and a photopolymerization initiator (D), and the composition can be produced. The timing of mixing each material is arbitrary. The dispersion process can also be carried out multiple times.
[0192] Examples of dispersing machines for carrying out the dispersion treatment include a two-roll mill, a three-roll mill, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, and an attritor.
[0193] The average dispersed particle size (secondary particle size) of the colorant (A) in the dispersion is preferably 30 to 200 nm, more preferably 40 to 200 nm. If the colorant (A) has an appropriate particle size, a photosensitive coloring composition having high dispersion stability is easily obtained.
[0194] The average dispersed particle size (secondary particle size) is measured, for example, using Nikkiso Microtrack UPA-EX150, which employs dynamic light scattering (FFT power spectrum method), with particle permeability set to absorption mode, particle shape set to non-spherical, and D50 particle size set to average size. The dilution solvent used for measurement is the organic solvent used for dispersion, and it is preferable to measure samples treated with ultrasonic waves immediately after sample preparation, as this tends to provide results with less variation.
[0195] The photosensitive coloring composition is preferably subjected to removal of coarse particles of 5 μm or more, preferably coarse particles of 1 μm or more, more preferably coarse particles of 0.5 μm or more, and mixed dust by means of centrifugation, filtration with a sintered filter or membrane filter, etc. The photosensitive coloring composition of the present invention preferably does not substantially contain particles of 0.5 μm or more, and more preferably does not contain particles of 0.3 μm or less.
[0196] <Cured film> The cured film of the present invention can be obtained by curing a film formed using the photosensitive coloring composition of the present invention. The cured film also includes a patterned cured film.
[0197] [Method of manufacturing the cured film] The method for producing the cured film is not particularly limited, and the cured film can be produced by carrying out, for example, a step (1) of applying a photosensitive coloring composition onto a substrate to form a layer of the composition, a step (2) of exposing the layer to light through a mask in a pattern, a step (3) of developing the unexposed parts with an alkali to form a patterned cured film, and a step (4) of heat-treating (post-baking) the pattern.
[0198] The method for producing the cured film will now be described in detail. (Process (1)) In the step (1) of forming a composition layer, the photosensitive coloring composition is applied onto a substrate by, for example, rotary coating, roll coating, slit coating, casting coating, inkjet coating, or the like, and dried (prebaked) at a temperature of 50 to 120°C for 10 to 120 seconds using an oven, a hot plate, or the like as necessary. Examples of the substrate include a glass substrate and a silicon substrate. The silicon substrate may have an image sensor such as a CCD or a CMOS formed on the surface. If necessary, an undercoat layer may be provided on the substrate to improve adhesion with an upper layer, prevent diffusion of substances, and flatten the substrate surface. The coating is preferably performed so that the layer thickness after drying is 0.05 to 10.0 μm, and more preferably 0.3 to 5 μm.
[0199] (Process (2)) In the exposure step, the layer obtained in step (1) is exposed to light in a specific pattern through a mask using an exposure device such as a stepper, thereby obtaining a cured film. Examples of radiation used for exposure include ultraviolet rays such as g-rays, h-rays, and i-rays.
[0200] (Step (3)) The cured film obtained in step (2) is subjected to an alkali development treatment, whereby the composition layer in the unexposed areas is dissolved in an aqueous alkali solution, leaving only the cured areas to obtain a patterned cured film. Examples of the developing solution include alkaline compounds such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, aqueous ammonia, ethylamine, diethylamine, dimethylethanolamine, tetramethylammonium hydroxide, tetraethylammonium hydroxide, choline, pyrrole, piperidine, and 1,8-diazabicyclo-[5.4.0]-7-undecene. The concentration of the developer is preferably from 0.001 to 10% by mass, and more preferably from 0.01 to 1% by mass. The pH of the alkaline developer is preferably 11 to 13, more preferably 11.5 to 12.5. When used at an appropriate pH, it suppresses roughening and peeling of the pattern and improves the remaining film rate after development.
[0201] Examples of the developing method include a dipping method, a spraying method, a paddle method, etc. The developing temperature is preferably 15 to 40° C. After the alkaline development, it is preferable to wash with pure water.
[0202] (Step (4)) In the heat treatment (post-baking), the patterned cured film obtained in step (3) is sufficiently cured by heating. The heating temperature in the post-baking is preferably 100 to 300° C., and more preferably 150 to 250° C. The heating time is preferably about 2 minutes to 1 hour, and more preferably about 3 minutes to 30 minutes.
[0203] [Properties of the cured film] The optical density (hereinafter also referred to as OD value) of the cured film obtained by curing the photosensitive coloring composition of the present invention at a film thickness of 2.0 μm is preferably 1.8 or more, more preferably 1.9 or more, and particularly preferably 2.0 or more. The upper limit is not particularly limited, but is preferably 10.0 or less.
[0204] The thickness and optical density of the cured film were measured as follows.
[0205] (Film thickness measurement) The photosensitive coloring composition of the present invention is applied onto a glass substrate by spin coating so that the film thickness after drying is 2.0 μm, and then dried on a hot plate at 70° C. for 1 minute. After that, the composition is heated at 250 mJ / cm 2 using an ultra-high pressure mercury lamp. 2 The entire surface was exposed to light at 600° C. Then, the substrate was spray-developed using a 0.04% by mass aqueous solution of tetramethylammonium hydroxide at 23° C., washed with ion-exchanged water, air-dried, and heated (post-baked) in a clean oven at 230° C. for 30 minutes to obtain a cured film. The obtained cured film was measured at five random locations using Dektak 3030 (manufactured by Japan Vacuum Engineering Co., Ltd.), and the average value was taken as the film thickness. The thickness of 2.0 μm includes the range of error permitted in the technical field to which the present invention pertains, specifically, the thickness is within the range of 2.0 μm±0.2 μm.
[0206] (Optical density measurement) The cured film whose thickness had been measured was subjected to measurement at five randomly selected points using a Macbeth densitometer (GretagMacbeth D200-II), and the average value was taken as the optical density.
[0207] <Light-shielding filter> The cured film of the present invention can be used for a light-shielding filter. As described above, the cured film of the present invention has excellent light-shielding properties and low reflectance. The light-shielding filter can be produced by the same method as that for the cured film.
[0208] <Color filters> The cured film of the present invention can be used for a color filter. The form of the color filter in which it is used is not particularly limited, but a black matrix is preferred. Examples of the black matrix include black edges provided on the periphery of image display devices such as solid-state imaging devices and liquid crystal display devices, lattice-like and / or stripe-like black portions between red, blue and green pixels, and dot-like and / or line-like black patterns for TFT light shielding.
[0209] The color filter can be produced, for example, by the following method. First, a patterned black matrix is formed on a substrate in the same manner as in the case of the above-mentioned cured film. Then, coating films of red, green, and blue photosensitive coloring compositions are sequentially formed on the substrate on which the black matrix is formed, thereby producing a color filter. The substrate may be a transparent substrate or a reflective substrate. The transparent substrate may be a glass substrate. The reflective substrate may be a substrate using an aluminum electrode or a metal thin film as a reflective surface.
[0210] <Image display device> The cured film of the present invention can be used in an image display device. Examples of the form of the image display device in which the cured film is used include a color filter having the black matrix.
[0211] As an example of the image display device of the present invention, a liquid crystal display device will be described. The liquid crystal display device comprises the color filter of the present invention and a light source. Examples of the light source include a cold cathode fluorescent lamp (CCFL) and a white LED, but in the present invention, it is preferable to use a white LED because it widens the red reproduction range. Fig. 1 is a schematic cross-sectional view of a liquid crystal display device 10 equipped with the color filter of the present invention. The device 10 shown in Fig. 1 comprises a pair of transparent substrates 11 and 21 arranged to face each other with a space therebetween, and a liquid crystal LC is sealed between them.
[0212] A TFT (thin film transistor) array 12 is formed on the inner surface of the first transparent substrate 11, and a transparent electrode layer 13 made of, for example, ITO is formed thereon. An alignment layer 14 is provided on the transparent electrode layer 13. In addition, a polarizing plate 15 is formed on the outer surface of the transparent substrate 11.
[0213] On the other hand, a color filter 22 of the present invention is formed on the inner surface of the second transparent substrate 21. Red, green and blue filter segments constituting the color filter 22 are separated by a black matrix (not shown).
[0214] A transparent protective film (not shown) is formed as necessary to cover the color filter 22, and a transparent electrode layer 23 made of, for example, ITO is formed on top of the transparent protective film. An alignment layer 24 is provided to cover the transparent electrode layer 23.
[0215] In addition, a polarizing plate 25 is formed on the outer surface of the transparent substrate 21. Below the polarizing plate 25, a backlight unit 30 is provided.
[0216] The liquid crystal LC is aligned according to a driving mode such as TN (Twisted Nematic), STN (Super Twisted Nematic), IPS (In-Plane Switching), VA (Vertical Alignment), OCB (Optically Compensated Birefringence), etc. A TFT (Thin Film Transistor) array 12 is formed on the inner surface of the first transparent substrate 11, and a transparent electrode layer 13 made of, for example, ITO is formed thereon. An alignment layer 14 is provided on the transparent electrode layer 13. In addition, a polarizing plate 15 is formed on the outer surface of the transparent substrate 11.
[0217] On the other hand, a color filter 22 of the present invention is formed on the inner surface of the second transparent substrate 21. Red, green and blue filter segments constituting the color filter 22 are separated by a black matrix (not shown).
[0218] A transparent protective film (not shown) is formed as necessary to cover the color filter 22, and a transparent electrode layer 23 made of, for example, ITO is formed on top of the transparent protective film. An alignment layer 24 is provided to cover the transparent electrode layer 23.
[0219] In addition, a polarizing plate 25 is formed on the outer surface of the transparent substrate 21. Below the polarizing plate 25, a backlight unit 30 is provided.
[0220] The white LED light source may have a fluorescent filter formed on the surface of a blue LED, or a blue LED containing a phosphor in its resin package, and has a wavelength (λ3) in the range of 430 nm to 485 nm at which the emission intensity is maximized, a wavelength (λ4) in the range of 530 nm to 580 nm at which the emission intensity is maximized, and a wavelength (λ5) in the range of 600 nm to 650 nm at which the emission intensity is maximized, and the ratio (I4 / I3) of the emission intensity I3 at wavelength λ3 to the emission intensity I4 at wavelength λ4 is 0.2 or more and 0.4 or less, Preferred is a white LED light source (LED1) having spectral characteristics in which the ratio (I5 / I3) of the emission intensity I3 at wavelength λ3 to the emission intensity I5 at wavelength λ5 is 0.1 or more and 1.3 or less, or a white LED light source (LED2) having a wavelength (λ1) at which the emission intensity is maximum within the range of 430 nm to 485 nm, a peak wavelength (λ2) of the second emission intensity within the range of 530 nm to 580 nm, and a ratio (I2 / I1) of the emission intensity I1 at wavelength λ1 to the emission intensity I2 at wavelength λ2 is 0.2 or more and 0.7 or less.
[0221] Specific examples of the LED 1 include NSSW306D-HG-V1 (manufactured by Nichia Chemical Industries, Ltd.) and NSSW304D-HG-V1 (manufactured by Nichia Chemical Industries, Ltd.).
[0222] Specific examples of the LED 2 include NSSW440 (manufactured by Nichia Chemical Industries, Ltd.) and NSSW304D (manufactured by Nichia Chemical Industries, Ltd.).
[0223] <Solid-state imaging element> The cured film of the present invention can be used for a solid-state imaging device. For example, the solid-state imaging device may have a plurality of photodiodes constituting a light receiving area of a solid-state imaging device (such as a CCD image sensor, a CMOS image sensor, or an organic CMOS image sensor) and a light receiving element made of polysilicon or the like on a substrate, and the cured film of the present invention is provided on the light receiving element forming surface side or the opposite side to the forming surface. Fig. 2 is a schematic cross-sectional view showing an example of the configuration of a solid-state imaging device provided with the cured film of the present invention.
[0224] As shown in FIG. 2, the solid-state imaging device 200 includes a rectangular solid-state imaging element 201 and a transparent cover glass 203 that is held above the solid-state imaging element 201 and seals the solid-state imaging element 201. Furthermore, a lens layer 211 is provided on the cover glass 203 via a spacer 104. The lens layer 211 is composed of a support 213 and a lens material 212. When stray light enters the peripheral region of the lens layer 211, the light diffusion weakens the light collecting effect of the lens material 212, and the amount of light that reaches the imaging unit 202 is reduced. In addition, noise is generated due to the stray light. Therefore, the peripheral region of the lens layer 211 is provided with a hardened film (light shielding) 214 of the present invention to shield the light.
[0225] The solid-state imaging element 201 photoelectrically converts an optical image formed on the imaging section 202, which is its light receiving surface, and outputs it as an image signal. The solid-state imaging element 201 includes a laminated substrate 205 in which two substrates are laminated. The laminated substrate 205 is made up of a rectangular chip substrate 206 and a circuit substrate 207 of the same size, and the circuit substrate 207 is laminated on the back surface of the chip substrate 206.
[0226] An imaging section 202 is provided in the center of the surface of the chip substrate 206. In addition, when stray light is incident on the peripheral region of the imaging section 202, a dark current (noise) is generated from the circuit in this peripheral region, so that this peripheral region is provided with the hardened film (light shielding) 215 of the present invention to shield the light.
[0227] A plurality of electrode pads 208 are provided on the edge of the surface of the chip substrate 206. The electrode pads 208 are electrically connected to the imaging unit 202 via signal lines (not shown) provided on the surface of the chip substrate 206.
[0228] External connection terminals 209 are provided on the rear surface of the circuit board 207 at positions approximately below the electrode pads 208. Each external connection terminal 209 is connected to each electrode pad 208 via a through electrode 210 that vertically penetrates the laminated substrate 205. Each external connection terminal 209 is also connected to a control circuit that controls the driving of the solid-state imaging element 201, an image processing circuit that performs image processing on an imaging signal output from the solid-state imaging element 201, and the like, via wiring (not shown).
[0229] <Infrared sensor> The cured film of the present invention can be used for an infrared sensor. Fig. 3 is a schematic cross-sectional view showing an example of the configuration of an infrared sensor provided with the cured film of the present invention. The infrared sensor 300 shown in Fig. 3 includes a solid-state imaging element 310.
[0230] The imaging area provided on the solid-state imaging element 310 is configured by combining an infrared absorbing filter 311 and a color filter 312 . The infrared absorbing filter 311 transmits light in the visible light region (for example, light with a wavelength of 400 to 700 nm) and blocks light in the infrared region (for example, light with a wavelength of 800 to 1300 nm). The color filter 312 is a color filter having pixels formed therein that transmit and absorb light of specific wavelengths in the visible light region, and for example, a color filter having red (R), green (G), and blue (B) pixels formed therein is used.
[0231] Between the infrared transmission filter 313 and the solid-state imaging element 310, a resin film 314 that is capable of transmitting light of a wavelength that has passed through the infrared transmission filter 313 is disposed. The infrared transmission filter 313 is a filter that has a visible light shielding property and transmits infrared rays of a specific wavelength, and the cured film of the present invention containing the above-mentioned near infrared absorber (G) can be used. The infrared transmission filter 113 preferably shields light with a wavelength of 400 to 830 nm and transmits light with a wavelength of 900 to 1300 nm, for example.
[0232] A microlens 315 is disposed on the incident light side of the color filter 312 and the infrared transmission filter 313. A planarization film 316 is formed so as to cover the microlens 315.
[0233] In the embodiment shown in FIG. 3, the resin film 314 is disposed, but instead of the resin film 314, an infrared transmission filter 313 may be formed.
[0234] The cured film of the present invention can be used as a light-shielding film for the end and / or side surface of the infrared absorbing filter 311, and when used on the inner wall of an infrared sensor, it can prevent internal reflection and / or incidence of unwanted light into the light receiving section, thereby improving sensitivity.
[0235] This infrared sensor can simultaneously capture image information, making it possible to perform motion sensing that recognizes the object whose movement is to be detected. In addition, this infrared sensor can obtain distance information, making it possible to capture images that include 3D information. Furthermore, this infrared sensor can also be used as a biometric authentication sensor.
[0236] The cured film of the present invention can also be used as a colored spacer. For example, when the spacer is used in a TFT-type LCD, the TFT may malfunction as a switching element due to light incident on the TFT, and the colored spacer is used to prevent this. The colored spacer can be formed in the same manner as the black matrix described above, except that a mask for the colored spacer is used.
[0237] In addition, the cured film of the present invention can also be used for applications such as micro LEDs (Light Emitting Diodes) and micro OLEDs (Organic Light Emitting Diodes). Although not particularly limited, it is suitable for use in optical filters and optical films used in micro LEDs and micro OLEDs, as well as members that impart light-shielding and anti-reflection properties. Examples of micro LEDs and micro OLEDs include those described in JP-A-2015-500562 and JP-A-2014-533890.
[0238] The cured film of the present invention can also be used for applications such as quantum dot displays. Although not particularly limited, it can be suitably used for optical filters and optical films used in quantum dot displays, as well as members that impart light-shielding and anti-reflection properties. EXAMPLES
[0239] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to these. In addition, "parts" means "parts by mass" and "%" means "% by mass".
[0240] Before describing the examples, each measurement method will be described. The weight average molecular weight (Mw), number average molecular weight (Mn), and acid value (mgKOH / g) of the resin are as follows.
[0241] (Average molecular weight of alkali-soluble resin and dispersing resin) The number average molecular weight (Mn) and weight average molecular weight (Mw) of the alkali-soluble resin and the dispersed resin were measured by gel permeation chromatography (GPC) equipped with an RI detector. The instrument used was an HLC-8220GPC (manufactured by Tosoh Corporation), with two separation columns connected in series, and both packings were "TSK-GEL SUPER HZM-N" connected in series. The oven temperature was 40°C, a tetrahydrofuran (THF) solution was used as the eluent, and the flow rate was 0.35 ml / min. The sample was dissolved in a solvent consisting of 1 wt% of the above eluent, and 20 microliters were injected. The molecular weight is a polystyrene equivalent value.
[0242] (Acid value of alkali-soluble resin and dispersing resin) 80 ml of acetone and 10 ml of water were added to 0.5 to 1 g of the alkali-soluble resin and the dispersed resin solution, and the solution was stirred to dissolve uniformly. The solution was titrated with an automatic titrator ("COM-555" manufactured by Hiranuma Sangyo Co., Ltd.) using a 0.1 mol / L KOH aqueous solution as the titrant to measure the acid value (mgKOH / g). The acid value per unit of non-volatile content of the resin was calculated from the acid value of the resin solution and the concentration of the non-volatile content of the resin solution.
[0243] (Amine value of dispersion resin) The amine value of the dispersing resin is the total amine value (mgKOH / g) measured in accordance with the method of ASTM D 2074 and converted into solid content.
[0244] <Production of Colorant (A)> (Finely divided blue organic pigment (A-1)) 100 parts of CI Pigment Blue 15:6 ("Lionol Blue ES" manufactured by Toyo Color Co., Ltd.), 800 parts of ground sodium chloride, and 100 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded for 12 hours at 70° C. This mixture was poured into 3,000 parts of warm water, and stirred for about 1 hour with a high-speed mixer while heating to about 70° C. to form a slurry. After repeatedly filtering and washing with water to remove the sodium chloride and diethylene glycol, the mixture was dried at 80° C. overnight to obtain a finely divided blue organic pigment (A-1).
[0245] (Fine yellow organic pigment (A-2)) 100 parts of CI Pigment Yellow 139 ("Novoperm Yellow P-M3R" manufactured by Clariant), 800 parts of ground sodium chloride, and 100 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho) and kneaded for 12 hours at 70° C. This mixture was poured into 3,000 parts of warm water, heated to about 70° C. and stirred with a high-speed mixer for about 1 hour to form a slurry, which was then filtered and repeatedly washed with water to remove the sodium chloride and diethylene glycol, and then dried at 80° C. overnight to obtain a finely divided yellow organic pigment (A-2).
[0246] (Finely divided purple organic pigment (A-3)) 100 parts of CI Pigment Violet 23 ("LIONOGEN VIOLET FG-6140" manufactured by Toyo Color Co., Ltd.), 800 parts of ground sodium chloride, and 100 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded for 12 hours at 70° C. This mixture was poured into 3,000 parts of warm water, heated to about 70° C. and stirred with a high-speed mixer for about 1 hour to form a slurry, which was then filtered and repeatedly washed with water to remove the sodium chloride and diethylene glycol, and then dried at 80° C. overnight to obtain a finely divided purple organic pigment (A-3).
[0247] <Production of alkali-soluble resin (B)> (Alkali-soluble resin (B-1) solution) A separable 4-neck flask was fitted with a thermometer, a cooling tube, a nitrogen gas inlet tube, a dropping tube and a stirrer. 196 parts of cyclohexanone was charged into the reaction vessel, which was then heated to 80°C and substituted with nitrogen in the reaction vessel. From the dropping tube, a mixture of 37.2 parts of n-butyl methacrylate, 12.9 parts of 2-hydroxyethyl methacrylate, 12.0 parts of methacrylic acid, 20.7 parts of paracumylphenol ethylene oxide modified acrylate ("Aronix M110" manufactured by Toagosei Co., Ltd.), and 1.1 parts of 2,2'-azobisisobutyronitrile was added dropwise over 2 hours. After the dropwise addition was completed, the reaction was continued for another 3 hours to obtain an acrylic resin solution. After cooling to room temperature, approximately 2 parts of the resin solution was sampled and dried at 180°C for 20 minutes to measure the non-volatile content, and propylene glycol monomethyl ether acetate (PGMAc) was added to the previously synthesized resin solution so that the non-volatile content was 20%, to prepare an alkali-soluble resin (B-1) solution. The weight average molecular weight (Mw) was 26,000.
[0248] (Alkali-soluble resin (B-2) solution) A separable 4-neck flask was fitted with a thermometer, a cooling tube, a nitrogen gas inlet tube, a dropping tube and a stirrer. 207 parts of cyclohexanone was charged into the reaction vessel, which was then heated to 80°C and substituted with nitrogen in the reaction vessel. From the dropping tube, a mixture of 20 parts of methacrylic acid, 20 parts of paracumylphenol ethylene oxide modified acrylate (Aronix M110 manufactured by Toagosei Co., Ltd.), 45 parts of methyl methacrylate, 8.5 parts of 2-hydroxyethyl methacrylate and 1.33 parts of 2,2'-azobisisobutyronitrile was added dropwise over 2 hours. After the dropping was completed, the reaction was continued for another 3 hours to obtain a resin solution. Next, the obtained resin solution was stirred while stopping the nitrogen gas and injecting dry air for 1 hour, and then cooled to room temperature, and a mixture of 6.5 parts of 2-methacryloyloxyethyl isocyanate (Karens MOI manufactured by Showa Denko K.K.), 0.08 parts of dibutyltin laurate, and 26 parts of cyclohexanone was added dropwise at 70 ° C. for 3 hours. After the dropwise addition was completed, the reaction was continued for another hour to obtain an acrylic resin solution. After cooling to room temperature, about 2 parts of the resin solution was sampled and dried by heating at 180 ° C. for 20 minutes to measure the non-volatile content, and cyclohexanone was added to the resin solution synthesized earlier so that the non-volatile content was 20% to prepare an alkali-soluble resin (B-2) solution. The weight average molecular weight (Mw) was 18,000.
[0249] (Alkali-soluble resin (B-3) solution) A separable 4-neck flask equipped with a thermometer, a cooling tube, a nitrogen gas inlet tube, a dropping tube and a stirrer was charged with 370 parts of cyclohexanone, heated to 80°C, and the flask was replaced with nitrogen. From the dropping tube, a mixture of 18 parts of paracumylphenol ethylene oxide modified acrylate (Aronix M110 manufactured by Toagosei Co., Ltd.), 10 parts of benzyl methacrylate, 18.2 parts of glycidyl methacrylate, 25 parts of methyl methacrylate and 2.0 parts of 2,2'-azobisisobutyronitrile was dropped over 2 hours. After the dropping, the mixture was further reacted at 100°C for 3 hours, and then a solution of 1.0 part of azobisisobutyronitrile dissolved in 50 parts of cyclohexanone was added, and the reaction was continued at 100°C for 1 hour. Next, the inside of the container was replaced with air, and 9.3 parts of acrylic acid (100% of glycidyl groups) was added to 0.5 parts of trisdimethylaminophenol and 0.1 parts of hydroquinone. The reaction was continued for 6 hours at 120 ° C., and the reaction was terminated when the non-volatile acid value reached 0.5, to obtain an acrylic resin solution. Furthermore, 19.5 parts of tetrahydrophthalic anhydride (100% of the generated hydroxyl groups) and 0.5 parts of triethylamine were added and reacted at 120 ° C. for 3.5 hours to obtain an acrylic resin solution. After cooling to room temperature, about 2 g of the resin solution was sampled and dried by heating at 180 ° C. for 20 minutes to measure the non-volatile content, and PGMAc was added to the resin solution synthesized earlier so that the non-volatile content was 20 mass% to prepare an alkali-soluble resin (B-3) solution. The weight average molecular weight (Mw) was 19,000.
[0250] (Alkali-soluble resin (B-4) solution) A separable flask equipped with a cooling tube was prepared as a reaction vessel. Meanwhile, a thoroughly stirred mixture of 40 parts of dimethyl-2,2'-[oxybis(methylene)]bis-2-propenoate, 40 parts of methacrylic acid, 120 parts of methyl methacrylate, 4 parts of t-butylperoxy 2-ethylhexanoate ("Perbutyl O" manufactured by Nippon Oil & Fats), and 40 parts of PGMAc was prepared as a monomer dropping vessel. A thoroughly stirred mixture of 8 parts of n-dodecanethiol and 32 parts of PGMAc was prepared as a chain transfer agent dropping vessel. 395 parts of PGMAc was charged into the reaction vessel, and after replacing with nitrogen, the temperature of the reaction vessel was raised to 90°C by heating in an oil bath while stirring. After the temperature of the reaction vessel was stabilized at 90°C, dropping was started from the monomer dropping vessel and the chain transfer agent dropping vessel. Dropping was carried out over 135 minutes while maintaining the temperature at 90°C. 60 minutes after the end of dropping, the temperature was raised to 110°C. After maintaining 110°C for 3 hours, a gas inlet tube was attached to the separable flask, and bubbling of a mixed gas of oxygen / nitrogen = 5 / 95 (volume ratio) was started. Next, 70 parts of glycidyl methacrylate, 0.4 parts of 2,2'-methylenebis(4-methyl-6-t-butylphenol), and 0.8 parts of triethylamine were charged into the reaction vessel, and the reaction was carried out at 110°C for 12 hours. After that, 150 parts of PGMAc was added and cooled to room temperature, and about 2 g of the resin solution was sampled and dried at 180°C for 20 minutes to measure the non-volatile content, and PGMAc was added to the previously synthesized resin solution so that the non-volatile content was 20 mass%, to obtain an alkali-soluble resin (B-4) solution. The weight-average molecular weight of the resin was 18,000, and the acid value per non-volatile content was 2 mgKOH / g.
[0251] (Alkali-soluble resin (B-5) solution) A flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel, and a nitrogen inlet tube was charged with 333 parts of PGMAc, and the atmosphere in the flask was changed from air to nitrogen. After that, the temperature was raised to 100°C, and a solution of 70.5 parts (0.40 mol) of benzyl methacrylate, 71.1 parts (0.50 mol) of glycidyl methacrylate, 22.0 parts (0.10 mol) of tricyclodecane-skeleton monomethacrylate (FA-513M manufactured by Hitachi Chemical Co., Ltd.) and 3.6 parts of azobisisobutyronitrile added to a mixture of 164 parts of PGMAc was dropped into the flask from the dropping funnel over 2 hours, and stirring was continued at 100°C for a further 5 hours. Next, the atmosphere in the flask was changed from nitrogen to air, and 43.0 parts of methacrylic acid [0.5 moles, (100 mol% relative to the glycidyl group of the glycidyl methacrylate used in this reaction)], 0.9 parts of trisdimethylaminomethylphenol, and 0.145 parts of hydroquinone were added to the flask, and the reaction was continued for 6 hours at 110 ° C., and the reaction was terminated when the non-volatile acid value became 1 mg KOH / g. Next, 60.9 parts (0.40 moles) of tetrahydrophthalic anhydride and 0.8 parts of triethylamine were added, and the reaction was carried out at 120 ° C. for 3.5 hours to obtain a photosensitive transparent resin solution with an acid value of 80 mg KOH / g. After cooling to room temperature, about 2 parts of the photosensitive transparent resin solution were sampled and dried by heating at 180 ° C. for 20 minutes to measure the non-volatile content, and PGMAc was added to the photosensitive transparent resin solution synthesized earlier so that the non-volatile content was 20 mass % to prepare an alkali-soluble resin (B-5) solution. The mass average molecular weight (Mw) was 12,000.
[0252] (Alkali-soluble resin (B-6) solution) Into a flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel, and a nitrogen inlet tube, 182 parts of PGMAc were introduced, and the atmosphere in the flask was changed from air to nitrogen. After that, the temperature was raised to 100°C, and then a solution of 70.5 parts (0.40 mol) of benzyl methacrylate, 43.0 parts (0.5 mol) of methacrylic acid, 22.0 parts (0.10 mol) of tricyclodecane-skeleton monomethacrylate (FA-513M manufactured by Hitachi Chemical Co., Ltd.) and 136 parts of PGMAc, to which 3.6 parts of azobisisobutyronitrile had been added, was dropped from the dropping funnel into the flask over 2 hours, and stirring was continued at 100°C for a further 5 hours. Next, the atmosphere in the flask was changed from nitrogen to air, and 35.5 parts of glycidyl methacrylate [0.25 moles, (50 mol% relative to the carboxyl group of the methacrylic acid used in this reaction)], 0.9 parts of trisdimethylaminomethylphenol, and 0.145 parts of hydroquinone were added to the flask, and the reaction was continued for 6 hours at 110 ° C. to obtain a photosensitive transparent resin solution with an acid value of 79 mg KOH / g. After cooling to room temperature, about 2 parts of the photosensitive transparent resin solution were sampled and dried by heating at 180 ° C. for 20 minutes to measure the non-volatile content, and PGMAc was added to the photosensitive transparent resin solution synthesized earlier so that the non-volatile content was 20 mass% to prepare an alkali-soluble resin (B-6) solution. The mass average molecular weight (Mw) was 13,000.
[0253] <Production of polymerizable compound (C-2) having urethane bond> (Polymerizable compound having a urethane bond (C-2-1)) In a five-neck flask equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, a thermometer, and a dropping tube, 400 parts of dipentaerythritol pentaacrylate, 100 parts of PGMAc, and 0.5 parts of N,N-dimethylbenzylamine were charged, and the temperature was raised to 70°C. A mixture of 64 parts of hexamethylene diisocyanate and 64 parts of PGMAc was dropped from the dropping tube over 2 hours. After the dropwise addition, the mixture was reacted at a temperature of 50 to 70°C for 8 hours, and the IR was measured at 2180 cm. -1 The disappearance of the isocyanate absorption was confirmed. PGMAc was added so that the non-volatile content was 50 mass %, and an aliphatic urethane acrylate solution having 10 polymerizable unsaturated groups was obtained.
[0254] (Polymerizable compound having a urethane bond (C-2-2)) A four-neck flask equipped with a stirrer, reflux condenser, nitrogen inlet tube, and thermometer was charged with 5.0 parts of trimethylolpropane, 18.8 parts of hexamethylene diisocyanate, 51.3 parts of pentaerythritol triacrylate, 75.1 parts of PGMAc, 0.02 parts of p-methoxyphenol, and then 0.12 parts of dioctyltin as a catalyst, and the temperature was raised to 100°C. The reaction was carried out at 100°C for 3 hours, and the IR reading was 2180 cm. -1 The disappearance of the isocyanate absorption was confirmed. PGMAc was added so that the non-volatile content was 50 mass %, and an aliphatic urethane acrylate solution having 9 polymerizable unsaturated groups was obtained.
[0255] (Polymerizable compound having a urethane bond (C-2-3)) In a five-neck flask equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, a thermometer, and a dropping tube, 400 parts of dipentaerythritol pentaacrylate, 100 parts of PGMAc, and 0.5 parts of N,N-dimethylbenzylamine were charged, and the temperature was raised to 70°C. A mixture of 64 parts of hexamethylene diisocyanate and 64 parts of PGMAc was dropped from the dropping tube over 2 hours. After the dropwise addition, the mixture was reacted at a temperature of 50 to 70°C for 8 hours, and the IR was measured at 2180 cm. -1 The disappearance of the isocyanate absorption was confirmed. Next, 21 parts of mercaptopropionic acid and 0.6 parts of 4-methoxyphenol were charged and reacted for 6 hours at a temperature of 50 to 60°C. PGMAc was added so that the non-volatile content became 50 mass%, and an aliphatic urethane acrylate solution having 9 polymerizable unsaturated groups and an acid group was obtained.
[0256] (Polymerizable compound having a urethane bond (C-2-4)) In a five-neck flask equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, a thermometer, and a dropping tube, 400 parts of pentaerythritol triacrylate, 100 parts of PGMAc, and 0.5 parts of N,N-dimethylbenzylamine were charged, and the temperature was raised to 70°C. A mixture of 109 parts of hexamethylene diisocyanate and 109 parts of PGMAc was dropped from the dropping tube over 2 hours. After the dropwise addition, the mixture was reacted at a temperature of 50 to 70°C for 8 hours, and the IR was measured at 2180 cm. -1The disappearance of the isocyanate absorption was confirmed. PGMAc was added so that the non-volatile content was 50 mass %, and an aliphatic urethane acrylate solution having 6 polymerizable unsaturated groups was obtained.
[0257] <Production of Dispersion Resin (F)> (Dispersion resin (F-1) solution) A reaction vessel equipped with a gas inlet tube, a temperature controller, a condenser, and a stirrer was charged with 10 parts of methacrylic acid, 100 parts of methyl methacrylate, 70 parts of i-butyl methacrylate, 20 parts of benzyl methacrylate, and 50 parts of PGMAc, and substituted with nitrogen gas. The reaction vessel was heated to 50°C and stirred, and 12 parts of 3-mercapto-1,2-propanediol was added. The temperature was raised to 90°C, and a solution of 0.1 parts of 2,2'-azobisisobutyronitrile and 90 parts of PGMAc was added and reacted for 7 hours. It was confirmed that 95% had reacted by measuring the non-volatile content. 19 parts of pyromellitic anhydride, 50 parts of PGMAc, 50 parts of cyclohexanone, and 0.4 parts of 1,8-diazabicyclo-[5.4.0]-7-undecene as a catalyst were added, and the reaction was carried out at 100°C for 7 hours. The reaction was terminated after confirming by measuring the acid value that 98% or more of the acid anhydride had been half-esterified. PGMAc was then added to dilute the solution so that the non-volatile content was 30%, yielding a dispersion resin (F-1) solution with an acid value of 70 mgKOH / g and a weight average molecular weight of 8,500.
[0258] (Dispersion resin (F-2) solution) In a 500 mL round-bottomed 4-neck separable flask equipped with a cooling tube, a dropping funnel, a nitrogen inlet, a mechanical stirrer, and a digital thermometer, 250 parts by mass of tetrahydrofuran (THF) and 5.81 parts by mass of dimethylketene methyl trimethylsilyl acetal as an initiator were added through the dropping funnel, and sufficient nitrogen replacement was performed. 0.5 parts by mass of a 1 mol / L acetonitrile solution of tetrabutylammonium m-chlorobenzoate as a catalyst was injected using a syringe, and 19.7 parts by mass of 2-hydroxyethyl methacrylate, 7.5 parts by mass of 2-ethylhexyl methacrylate, 12.9 parts by mass of n-butyl methacrylate, 10.7 parts by mass of benzyl methacrylate, and 30.9 parts by mass of methyl methacrylate as solvent-philic blocking monomers were dropped using the dropping funnel over 60 minutes. The temperature was kept below 40°C by cooling the reaction flask in an ice bath. After 1 hour, 18.3 parts by mass of dimethylaminopropyl methacrylamide, a monomer for colorant adsorption functional blocks, was added dropwise over 20 minutes. After reacting for 1 hour, 1 part by mass of methanol was added to stop the reaction. The resulting block copolymer THF solution was reprecipitated in hexane, filtered, and purified by vacuum drying. Next, 15.0 parts by mass of the obtained block copolymer were dissolved in 35 parts by mass of PGMAc in a 100 mL round-bottom flask, and 1.1 parts by mass of phenylphosphinic acid (0.5 molar equivalent relative to dimethylaminopropyl methacrylamide), which is a salt-forming component, was added. The mixture was stirred at a reaction temperature of 30°C for 20 hours, and PGMAc was added to adjust the content, thereby obtaining a dispersion resin (F-2) solution with a non-volatile content of 30%.
[0259] <Production of near infrared absorbent (G)> (Near infrared absorbing agent (G-1)) 400 parts of toluene were mixed with 40.0 parts of 1,8-diaminonaphthalene, 32.2 parts of 3,5-dimethylcyclohexanone, and 0.087 parts of p-toluenesulfonic acid monohydrate, and the mixture was heated and stirred in a nitrogen gas atmosphere and refluxed for 3 hours. Water generated during the reaction was removed from the reaction system by azeotropic distillation. After the reaction was completed, the dark brown solid obtained by distilling toluene was extracted with acetone and purified by recrystallization from a mixed solvent of acetone and ethanol. The obtained brown solid was dissolved in a mixed solvent of 240 parts of toluene and 160 parts of n-butanol, and 13.8 parts of 3,4-dihydroxy-3-cyclobutene-1,2-dione was added, and the mixture was heated and stirred in a nitrogen gas atmosphere and refluxed for 8 hours. Water generated during the reaction was removed from the reaction system by azeotropic distillation. After the reaction was completed, the solvent was distilled, and 200 parts of hexane was added while stirring the resulting reaction mixture. The resulting black-brown precipitate was filtered off, washed with hexane, ethanol, and acetone, and dried under reduced pressure to obtain a near-infrared absorbent (G-1) represented by the following chemical formula (6). 50 parts of the obtained near-infrared absorbent (G-1), 500 parts of sodium chloride, and 60 parts of diethylene glycol were charged into a stainless steel gallon kneader (manufactured by Inoue Seisakusho) and kneaded at 60 ° C for 12 hours. Next, the kneaded mixture was poured into hot water, heated to about 80 ° C and stirred for 1 hour to form a slurry, filtered and washed with water to remove sodium chloride and diethylene glycol, and then dried and pulverized at 80 ° C for one day and night to obtain a finely divided near-infrared absorbent (G-1).
[0260] Chemical formula (6) [ka]
[0261] <Preparation of Dispersion> (Dispersion 1) The following raw materials were mixed and stirred until uniform, then dispersed for 3 hours in an Eiger mill (Eiger Japan's "Mini Model M-250 MKII") using zirconia beads with a diameter of 0.5 mm, and then filtered through a filter with a pore size of 1.0 μm to produce black dispersion 1. The organic solvent (Q-1) was PGMAc. Carbon black (Mitsubishi Chemical #850): 15.0 parts Dispersion resin (F-1) solution: 20.0 parts The following dye derivative (E-1): 1.0 part Organic solvent (Q-1): 64.0 parts
[0262] Mitsubishi Chemical's #850 has an average primary particle size of 17 nm and a specific surface area of 220 m 2 / g of carbon black.
[0263] Dye derivative (E-1) [ka]
[0264] (Dispersion 2) The following raw materials were mixed and stirred until uniform, then dispersed in an Eiger mill (Eiger Japan, "Mini Model M-250 MKII") for 3 hours using zirconia beads with a diameter of 0.5 mm. The mixture was then filtered through a filter with a pore size of 1.0 μm to produce black dispersion 2. Finely divided blue organic pigment (A-1): 8.75 parts Finely divided yellow organic pigment (A-2): 8.75 parts Finely divided purple organic pigment (A-3): 7.5 parts Dispersion resin (F-1) solution: 23.0 parts The following dye derivative (E-2): 1.5 parts Organic solvent (Q-1): 50.5 parts
[0265] Dye derivative (E-2)
[0266] [ka]
[0267] (Dispersion 3) The raw materials listed below were mixed and stirred until uniform, and then dispersed in an Eiger mill (Eiger Japan's "Mini Model M-250 MKII") for 3 hours using zirconia beads with a diameter of 0.5 mm. The mixture was then filtered through a filter with a pore size of 1.0 μm to produce Dispersion 3. Near infrared absorbing agent (G-1): 25.0 parts Alkali-soluble resin (B-6) solution: 35.0 parts Dispersion resin (F-4) solution: 15.0 parts Organic solvent (Q-1): 25.0 parts
[0268] <Production of Photosensitive Coloring Composition> [Example 1] (Photosensitive coloring composition 1) The following raw materials were mixed and stirred, and filtered through a filter having a pore size of 1.0 μm to obtain a photosensitive coloring composition 1. Dispersion 1: 25.0 parts Alkali-soluble resin (B) solution: 40.0 parts Polymerizable compound (C-1-1): 4.0 parts Polymerizable compound (C-4-1): 6.0 parts Photopolymerization initiator (D-1): 0.5 parts Epoxy compound (I-1): 1.0 part Thiol chain transfer agent (J): 0.1 parts Polymerization inhibitor (K): 0.01 parts UV absorber (L): 0.1 parts Antioxidant (M): 0.1 parts Leveling agent (N): 1.0 part Storage stabilizer (O): 0.2 parts Organic solvent (Q): 21.99 parts
[0269] [Examples 2 to 31, Comparative Examples 1 to 4] (Photosensitive composition 2-35) Photosensitive coloring compositions 2 to 35 were prepared in the same manner as in Example 1, except that the photosensitive coloring composition 1 in Example 1 was changed to the raw materials and amounts described in Tables 2-1 to 2-4. It was visually confirmed that the coatings formed from the photosensitive coloring compositions of Examples 1 to 31 had sufficient light-shielding properties. In this specification, Examples 1 to 12 and 29 are reference examples.
[0270] [Table 2-1]
[0271] [Table 2-2]
[0272] [Table 2-3]
[0273] [Table 2-4]
[0274] The respective raw materials listed in Tables 2-1 to 2-4 are as follows.
[0275] [Alkali-soluble resin (B) solution] The alkali-soluble resin (B-2) to (B-6) solutions were mixed in equal amounts to prepare an alkali-soluble resin (B) solution.
[0276] [Polymerizable compound (C)] (Polymerizable compound (C-1) having a 9,9-bisarylfluorene structure) C-1-1: OGSOL EA-0200 (Osaka Gas Chemicals Co., Ltd., compound with Tg of 211°C represented by chemical formula (4), non-volatile content 100%) C-1-2: OGSOL EA-0300 (Osaka Gas Chemicals Co., Ltd., R in general formula (1) 1 and R 3 is a hydrogen atom, R 2 and R4 Compound with ethylene group, m+n=20, Tg17℃, non-volatile content 100%) C-1-3: OGSOL GA-5060P (Osaka Gas Chemicals Co., Ltd., R in general formula (2) 5 and R 6 A compound with a Tg of 228°C and a hydrogen atom (100% non-volatile content) C-1-4: OGSOL GA-2800 (Osaka Gas Chemicals Co., Ltd., R in general formula (3) 7 and R 8 Compound with Tg7℃ and hydrogen atom (100% non-volatile content) (Polymerizable compound having a urethane bond (C-2)) C-2-5: EBECRY220 (manufactured by Daicel-Allnex, aromatic urethane acrylate with 6 polymerizable unsaturated groups, non-volatile content 100%) C-2-6: EBECRY4513 (manufactured by Daicel-Allnex, aliphatic urethane acrylate with three polymerizable unsaturated groups, non-volatile content 100%) C-2-7: U-15HA (manufactured by Shin-Nakamura Chemical Co., Ltd., an aliphatic urethane acrylate with 15 polymerizable unsaturated groups, non-volatile content 100%) (Polymerizable compound having an acid group (C-3)) C-3-1: Aronix M-520 (manufactured by Toagosei Co., Ltd., 100% non-volatile content) (Other polymerizable compounds (C-4)) C-4-1: KAYARAD DPHA (manufactured by Nippon Kayaku Co., Ltd., a mixture of dipentaerythritol hexaacrylate and dipentaerythritol pentaacrylate, 100% non-volatile content) C-4-2: NK Ester ABE-300 (manufactured by Shin-Nakamura Chemical Co., Ltd., ethoxylated bisphenol A diacrylate, 100% non-volatile content) C-4-3: EBECRY130 (manufactured by Daicel-Allnex, tricyclodecane dimethanol diacrylate, non-volatile content 100%)
[0277] [Photopolymerization initiator (D)] D-1: ADEKA Cruise NCI-831 (ADEKA) D-2: Irgacure OXE02 (BASF Japan) D-3: Irgacure 907 (BASF Japan)
[0278] [Sensitizer (H)] H-1: Kayacure DETX-S (manufactured by Nippon Kayaku Co., Ltd.) H-2:CHEMARK DEABP (manufactured by Chemark Chemical) The above (H-1) and (H-2) were mixed in equal amounts to prepare sensitizer (H).
[0279] [Epoxy compound (I-1)] I-1-1: EHPE-3150 (manufactured by Daicel) I-1-2: Denacol EX611 (Nagase ChemteX Corporation) I-1-3: Triglycidyl isocyanurate The above (I-1-1) to (I-1-3) were mixed in equal amounts to obtain the epoxy compound (I-1).
[0280] [Thiol-based chain transfer agents (J)] J-1: Trimethylolethane tris(3-mercaptobutyrate) J-2: Trimethylolpropane tris(3-mercaptobutyrate) J-3: Pentaerythritol tetrakis(3-mercaptopropionate) J-4: Trimethylolpropane tris(3-mercaptopropionate) J-5: Tris[(3-mercaptopropionyloxy)-ethyl]-isocyanurate The above (J-1) to (J-5) were mixed in equal amounts to prepare a thiol-based chain transfer agent (J).
[0281] [Polymerization inhibitor (K)] K-1: 4-Methylcatechol K-2: Methylhydroquinone K-3: t-Butylhydroquinone The above (K-1) to (K-3) were mixed in equal amounts to prepare a polymerization inhibitor (K).
[0282] [Ultraviolet absorber (L)] L-1: TINUVIN400 (BASF Japan) L-2: TINUVIN900 (BASF Japan) The above (L-1) and (L-2) were mixed in equal amounts to prepare an ultraviolet absorber (L).
[0283] [Antioxidants (M)] M-1: Pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate M-2: Dioctadecyl 3,3'-thiodipropanoate M-3: Tris[2,4-di-(t)-butylphenyl]phosphine M-4: Bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate M-5: p-Octylphenyl salicylate The above (M-1) to (M-5) were mixed in equal amounts to prepare an antioxidant (M).
[0284] [Leveling agent (N)] N-1: BYK-330 (manufactured by BYK-Chemie) N-2: Megafac F-551 (DIC) One part each of (N-1) and (N-2) was mixed and dissolved in 98 parts of PGMAc to prepare a mixed solution, which was used as a leveling agent (N).
[0285] [Storage stabilizer (O)] O-1: 2,6-bis(1,1-dimethylethyl)-4-methylphenol O-2: Triphenylphosphine The above (O-1) and (O-2) were mixed in equal amounts to prepare a storage stabilizer (O).
[0286] [Organic solvent (Q)] Q-1: Propylene glycol monomethyl ether acetate 30 parts Q-2: Cyclohexanone 30 parts Q-3: 10 parts of ethyl 3-ethoxypropionate Q-4: Propylene glycol monomethyl ether 10 parts Q-5: Cyclohexanol acetate 10 parts Q-6: Dipropylene glycol methyl ether acetate 10 parts The above (Q-1) to (Q-6) were mixed in the above-mentioned parts by mass to obtain organic solvent (Q).
[0287] <Evaluation of Photosensitive Coloring Composition> The obtained photosensitive coloring composition was evaluated for optical density, reflectance, adhesion, pattern shape, and surface wrinkles by the following methods. The evaluation results are shown in Table 3.
[0288] [Optical density (OD value) evaluation] The obtained photosensitive coloring composition was applied by spin coating to a glass substrate (Corning Eagle 2000) measuring 100 mm in length, 100 mm in width, and 0.7 mm in thickness so that the film thickness after drying would be 2.0 μm. The coating was then dried on a hot plate at 70° C. for 1 minute, and then irradiated with 250 mJ / cm 2 using an ultra-high pressure mercury lamp. 2 The entire surface was exposed to light. After that, the substrate was spray-developed using an organic alkaline developer (NMD-3, manufactured by Tokyo Ohka Kogyo Co., Ltd.) at 23°C, washed with ion-exchanged water, air-dried, and heated (post-baked) in a clean oven at 230°C for 30 minutes to obtain a cured film. The optical density (OD value) of the obtained cured film was measured using a Macbeth densitometer (GretagMacbeth D200-II). The evaluation criteria are as follows, with 2 or more being practical. 3:OD value is 2.0 or more 2:OD value is 1.8 or more and less than 2.0 1:OD value is less than 1.8
[0289] [Reflectance evaluation] The cured film prepared by the optical density measurement was measured for reflectance (SCI value and SCE value) of the color matching function Y using a colorimeter CM-2002 (measurement conditions: C light source, viewing angle 2°) manufactured by Konica Minolta, Inc. The evaluation criteria are as follows, with 3 or more being practical. The SCI value is an abbreviation for Specular Component Include, which is the total reflectance value, and the SCE value is an abbreviation for Specular Component Exclude, which is the total reflectance value excluding the specular reflected light component. 5: SCI value is less than 3.0 and SCE value is less than 0.15 4: SCI value is 3.0 or more but less than 3.5, and SCE value is 0.15 or more but less than 0.2 3: SCI value is 3.5 or more and less than 4.0, and SCE value is 0.2 or more and less than 0.25 2: SCI value is 4.0 or more but less than 4.5, and SCE value is 0.25 or more but less than 0.3 1: SCI value is 4.5 or more and SCE value is 0.3 or more
[0290] [Adhesion evaluation] The obtained photosensitive coloring composition was applied by spin coating to a glass substrate (Corning Eagle 2000) measuring 100 mm in length, 100 mm in width, and 0.7 mm in thickness so that the film thickness after drying would be 2.0 μm, and then dried on a hot plate at 70° C. for 1 minute. Next, after cooling the substrate to room temperature, a high-pressure mercury lamp was used to illuminate the substrate through a photomask with a stripe pattern of 100 μm width (pitch 200 μm) and 10 μm width (pitch 20 μm) at an illumination intensity of 30 mW / cm. 2 , 250mJ / cm 2 The substrate was then spray-developed using an organic alkaline developer (NMD-3, manufactured by Tokyo Ohka Kogyo Co., Ltd.) at 23°C, washed with ion-exchanged water, air-dried, and heated at 230°C for 30 minutes in a clean oven to obtain a substrate for evaluating adhesion. The spray development was carried out for the shortest time possible for forming a pattern without leaving any residual development on the coating of each photosensitive coloring composition, and this was determined as the appropriate development time. Of the patterns on the substrate for evaluating adhesion, fine line patterns with widths of 6 to 25 μm were observed under an optical microscope to confirm the minimum line width of the remaining fine line patterns. 5: Fine lines of 10 μm or less remain. 4: Fine lines of 15 μm or less remain. 3: Fine lines of 20 μm or less remain. 2: Fine lines of 25 μm or less remain. 1: No fine lines remain.
[0291] [Pattern shape evaluation] The substrate prepared for the adhesion evaluation was evaluated by measuring the maximum and minimum line widths of 10 stripe patterns using a Nikon ECLIPSE LV100POL Model optical microscope and calculating the average. The evaluation criteria are as follows, with 3 or more being practical. 5: The difference between the maximum and minimum line widths is less than 0.5 μm 4: The difference between the maximum and minimum line widths is 0.5 μm or more and less than 1.0 m 3: The difference between the maximum and minimum line widths is 1.0 μm or more and less than 1.5 m 2: The difference between the maximum and minimum line widths is 1.5 μm or more and less than 2.0 m 1: The difference between the maximum and minimum line widths is 2.0 μm or more
[0292] [Surface wrinkle evaluation] The pattern surface of the substrate prepared for the adhesion evaluation was observed using an optical microscope (Olympus Optical Co., Ltd. "BX-51", magnification: 200 times). The evaluation criteria are as follows, with 3 or more being practical. 5: No wrinkles are observed on the surface of the pattern. 4: Very slight wrinkles are observed on the pattern surface. 3: Slight wrinkles are observed on the pattern surface. 2: Wrinkles are observed on the surface of the pattern. 1: Severe wrinkles are observed on the pattern surface.
[0293] [Table 3] [Explanation of symbols]
[0294] 10 LCD display device 11 Transparent substrate 12 TFT array 13 Transparent electrode layer 14 Alignment layer 15 Polarizing plate 21 Transparent substrate 22 Color Filter 23 Transparent electrode layer 24 Alignment layer 25 Polarizing Plate 30 Backlight unit 31 White LED light source LC Liquid Crystal 200 Solid-state imaging device 201 Solid-state image sensor 202 Imaging unit 203 Cover Glass 204 Spacer 205 Laminated Board 206 Chip Substrate 207 Circuit Board 208 Electrode Pad 209 External connection terminal 210 Through electrode 211 Lens layer 212 Lens material 213 Support 214 Cured film (light shielding) 215 Cured film (light shielding) 300 Infrared Sensor 310 Solid-state imaging element 311 Infrared absorbing filter 312 Color Filter 313 Infrared absorbing and transmitting filter 314 Resin Film 315 Micro Lens 316 Flat membrane
Claims
1. A photosensitive coloring composition comprising a colorant (A), an alkali-soluble resin (B), a polymerizable compound (C), and a photopolymerization initiator (D), the polymerizable compound (C) contains a polymerizable compound (C-1) having a 9,9-bisarylfluorene structure and a polymerizable compound (C-2) having a urethane bond, The photosensitive coloring composition, wherein the polymerizable compound (C-1) having a 9,9-bisarylfluorene structure is any one of the compounds represented by the following general formulas (1) to (3). General formula (1) 【Chemistry 1】 (In general formula (1), R 1 and R 3 each independently represent a hydrogen atom or a methyl group, R 2 and R 4 each independently represent an alkylene group, and m and n each independently represent an integer of 1 to 10.) General formula (2) 【Chemistry 2】 (In formula (2), R 5 and R 6 each independently represent a hydrogen atom or a methyl group.) General formula (3) 【Chemistry 3】 (In formula (3), R 7 and R 8 each independently represent a hydrogen atom or a methyl group.)
2. 2. The photosensitive coloring composition according to claim 1, wherein the polymerizable compound (C-1) having a 9,9-bisarylfluorene structure has a glass transition temperature of 200° C. or higher.
3. The photosensitive coloring composition according to claim 1 or 2, wherein the content of the polymerizable compound (C-1) having a 9,9-bisarylfluorene structure is 10% by mass or more in 100% by mass of the polymerizable compound (C).
4. The photosensitive coloring composition according to any one of claims 1 to 3, wherein the mass ratio of the polymerizable compound (C-1) having the 9,9-bisarylfluorene structure to the polymerizable compound (C-2) having the urethane bond is 80:20 to 20:
80.
5. The photosensitive coloring composition contains the polymerizable compound (C) in an amount of 1 to 60% by mass in the nonvolatile content thereof, The total content of the polymerizable compound (C-1) having the 9,9-bisarylfluorene structure and the polymerizable compound (C-2) having the urethane bond is 40 mass% or more in 100 mass% of the polymerizable compound (C), the photosensitive coloring composition according to any one of claims 1 to 4.
6. The photosensitive coloring composition according to any one of claims 1 to 5, which contains carbon black as the colorant (A) and exhibits a black color.
7. The photosensitive coloring composition according to any one of claims 1 to 5, comprising at least two or more organic pigments selected from a red organic pigment, a yellow organic pigment, a blue organic pigment, and a purple organic pigment as the colorant (A), and exhibiting a black color.
8. The photosensitive coloring composition according to claim 7, further comprising a near-infrared absorbing agent (G).
9. A cured film which is a cured product of the photosensitive coloring composition according to any one of claims 1 to 8.
10. A light-shielding filter comprising the cured film according to claim 9.
11. A color filter comprising the cured film according to claim 9.
12. An image display device comprising the cured film according to claim 9 .
13. A solid-state imaging device comprising the cured film according to claim 9 .
14. An infrared sensor comprising the cured film according to claim 9.
Citation Information
Patent Citations
Light-shielding film forming composition, light-shielding film for solid-state imaging element using same, and solid-sate imaging element
JP2006156801A
Photosensitive coloring composition and color filter
JP2006259716A
Photosensitive resin composition and laminate, and electromagnetic wave shield and transparent conductive substrate using the same
JP2011048064A
Photosensitive composition for forming partition wall of optical element, black matrix using the same, method for producing the black matrix, and method for producing color filter on array
JP2011048195A
Composition, infrared transmitting filter, manufacturing method therefor, and infrared sensor
JP2014130338A