Substrate unit, method of manufacturing substrate unit, and method of manufacturing semiconductor device

The substrate unit with a support and warpage suppressing layer addresses manufacturing limitations by forming stable multilayer wiring and reducing warpage, enhancing semiconductor element mounting reliability and yield.

JP7574632B2Active Publication Date: 2024-10-29TOPPAN HOLDINGS INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020205343
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-10
Publication Date
2024-10-29
Estimated Expiration
2040-12-10

AI Technical Summary

Technical Problem

The manufacturing of silicon interposers for FC-BGA substrates is limited by the shape and size of silicon wafers, leading to high costs and deteriorated transmission characteristics, while methods like flattening FC-BGA substrates or forming fine wiring on supports face issues with manufacturing yield, warping, and mounting defects due to stress and deformation.

Method used

A substrate unit is created with a support and multiple first wiring boards separated by a release layer, incorporating a warpage suppressing layer and electrodes for bonding, and a method involving resin layer formation, electrolytic plating, and peeling to form stable multilayer wiring, followed by semiconductor element mounting and sealing.

Benefits of technology

This approach stabilizes the substrate unit against warpage, enabling reliable semiconductor element mounting with reduced defects and improved manufacturing yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574632000001
    Figure 0007574632000001
  • Figure 0007574632000002
    Figure 0007574632000002
  • Figure 0007574632000003
    Figure 0007574632000003
Patent Text Reader

Abstract

To provide a substrate unit with slight warpage, a stable manufacturing method for the same, and a manufacturing method for a semiconductor device using the same in a method for peeling off a support substrate and mounting on an FC-BGA substrate after forming a release layer and a fine wiring layer above a support and mounting and encapsulating a semiconductor element.SOLUTION: The substrate unit includes a support and a plurality of first wiring substrates placed above the support via a peeling layer. Electrodes for bonding at least one semiconductor element are provided on a first surface of each of the first wiring substrates. Electrodes for bonding with a second wiring substrate are provided on the other surface of each of the first wiring substrates. A warpage suppressing layer is formed below the support.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a substrate unit, a method for manufacturing a substrate unit, and a method for manufacturing a semiconductor device. [Background technology]

[0002] In recent years, as semiconductor devices become faster and more highly integrated, there is a demand for narrower pitches for the connection terminals with semiconductor elements and finer wiring within the board for FC-BGA (Flip Chip-Ball Grid Array) boards. On the other hand, there is a demand for connection between FC-BGA boards and motherboards with connection terminals at roughly the same pitch as before.

[0003] In order to accommodate the narrower pitch of the bonding terminals for semiconductor elements and the finer wiring within FC-BGA substrates, several countermeasures are being considered.

[0004] One of them is a method of creating a substrate (silicon interposer) for semiconductor element bonding, which has fine wiring formed on a silicon substrate, and bonding this to an FC-BGA substrate.

[0005] Furthermore, Patent Document 1 discloses a method of forming fine wiring on an FC-BGA substrate by planarizing the surface of the FC-BGA substrate by CMP (Chemical Mechanical Polishing) or the like without using a silicon interposer.

[0006] Furthermore, Patent Document 2 discloses a method in which a fine wiring layer is formed on a support, this is mounted on an FC-BGA substrate, and then the support substrate is peeled off to form a narrow-pitch wiring substrate. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2014-225671 A [Patent Document 2] International Publication No. 2018 / 047861 Summary of the Invention [Problem to be solved by the invention]

[0008] Silicon interposers are manufactured using silicon wafers with equipment for front-end semiconductor manufacturing. Silicon wafers are limited in shape and size, and only a small number of interposers can be manufactured from one wafer. In addition, the manufacturing equipment is expensive, so the interposers are also expensive. In addition, because silicon wafers are semiconductors, there is a problem of degradation of transmission characteristics.

[0009] In addition, in the method of flattening the surface of the FC-BGA substrate and forming a fine wiring layer on it, the deterioration of transmission characteristics seen in silicon interposers is small, but the manufacturing yield of the FC-BGA substrate itself and the difficulty of forming the fine wiring on the FC-BGA substrate are high, so the manufacturing yield of the fine wiring formation is an issue. Furthermore, there are also issues in mounting semiconductor elements due to warping and distortion of the FC-BGA substrate.

[0010] On the other hand, the method of forming a fine wiring layer on a support and mounting this on an FC-BGA substrate has the following problems: When the fine wiring layer formed on the support substrate is mounted on the FC-BGA substrate and then the support substrate is peeled off, the sealing resin material used to mount the fine wiring layer on the FC-BGA substrate wets up to the support substrate and prevents the support substrate from being peeled off;

[0011] Another method is to form a fine wiring layer on a support substrate, mount and seal a semiconductor element on the fine wiring layer, and then peel the fine wiring layer from the support substrate and mount the peeled fine wiring layer with the semiconductor element on an FC-BGA substrate. According to this method, the semiconductor element is mounted on the fine wiring layer held by the support substrate, so that the semiconductor element can be mounted with little deformation. However, since the fine wiring layer is formed on one side of the support, there is a problem that warping occurs due to the heat history when forming the wiring layer. In particular, there is a problem that the semiconductor element mounted on the fine wiring layer is prone to mounting defects even when there is a slight warping because the distance between the terminals is short.

[0012] The present invention has been made in consideration of the above problems, and has an object to provide a substrate unit that is less prone to deformation and can be stably manufactured, a method for manufacturing a substrate unit, and a method for manufacturing a semiconductor device.

[0013] Problems and advantages other than those described above will be described in the following embodiments of the invention. [Means for solving the problem]

[0014] In order to solve the above problems, one of the representative substrate units of the present invention is A substrate unit including a support and a plurality of first wiring substrates mounted on the support via a release layer, an electrode for bonding at least one semiconductor element is provided on a first surface of the first wiring board; an electrode for joining to a second wiring board is provided on a second surface of the first wiring board; A warp suppressing layer is formed below the support.

[0015] Furthermore, one of the representative methods for producing a substrate unit according to the present invention is to forming a release layer on an upper surface of the support; forming a resin layer above the release layer; forming a warp suppressing layer on the lower surface of the support; forming an opening in the resin layer; forming a seed layer over the resin layer and the opening; forming an electrolytic plating layer above the seed layer; a step of polishing the electrolytic plating layer and the seed layer until the resin layer is exposed, and forming an electrode for bonding to a second wiring board; a step of repeatedly forming a resin layer and a conductor layer on the upper surface of the exposed resin layer and the electrode to obtain a multilayer wiring; forming an electrode for bonding a semiconductor element to the outermost surface of the multilayer wiring; Includes.

[0016] Furthermore, one of the representative methods for manufacturing a semiconductor device according to the present invention includes the steps of: a step of bonding a semiconductor element to a first wiring board; a step of sealing a gap between the first wiring board and the semiconductor element with a first sealing resin; sealing the side surfaces of the first wiring board and the semiconductor element with a second sealing resin; peeling the first wiring substrate from the support; obtaining an assembly in which a semiconductor element is bonded to a first wiring substrate; a step of dividing the assembly into individual first wiring substrates; A step of joining the first wiring board to the second wiring board; sealing a gap between the first wiring board and the second wiring board with a third sealing resin; Includes. Effect of the Invention

[0017] According to the present invention, it is possible to manufacture a board unit that is less prone to warping, and a semiconductor element can be mounted with less warping. Problems and advantages other than those described above will be described in the following embodiments. [Brief description of the drawings]

[0018] [Figure 1] 13 is a diagram showing a state in which a release layer and a first wiring substrate are formed above the support body, and a warp suppressing layer is formed below the support body. FIG. [Diagram 2] FIG. 2 is a plan view showing a state in which a plurality of first wiring substrates are placed above a supporting body. [Diagram 3] 1 is a cross-sectional view showing a state in which a release layer and an insulating resin layer are formed above a support body, and a warp suppressing layer is formed below the support body. [Figure 4] 4A to 4C are cross-sectional views showing a step of forming an insulating resin layer and a conductor layer. [Figure 5A] 10 is a cross-sectional view showing a process of forming an insulating resin layer in a via portion and then forming a conductor layer. FIG. [Figure 5B] 10 is a cross-sectional view showing a step of removing the resist pattern and etching away unnecessary seed layer. FIG. [Figure 6] FIG. 2 is a cross-sectional view showing a state in which multi-layer wiring is formed. [Figure 7] 4 is a cross-sectional view showing a state in which an electrode for bonding to a semiconductor element has been formed. FIG. [Figure 8] FIG. 4 is a cross-sectional view showing a state in which a surface treatment layer is formed and a first wiring board is completed on a support body. [Figure 9] 5A to 5C are cross-sectional views showing a process of mounting a semiconductor element on a first wiring board. [Figure 10] 10A to 10C are cross-sectional views showing a step of removing the release layer. [Figure 11] 5A to 5C are process diagrams showing the formation of solder joints on the first wiring board. [Figure 12] 1 is a cross-sectional view showing a state in which a first wiring board on which a semiconductor element is mounted is mounted on an FC-BGA substrate. [Figure 13] 1 is a cross-sectional view showing an example of a semiconductor device of the present invention. [Figure 14] FIG. 11 is a cross-sectional view showing an example of a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the following description of the drawings, the same or similar parts are denoted by the same or similar reference numerals. However, it should be noted that the drawings are schematic, and the relationship between thickness and planar dimensions, the thickness ratio of each layer, etc., differ from the actual ones. Therefore, the specific thickness and dimensions should be determined with reference to the following description. In addition, it goes without saying that the drawings include parts with different dimensional relationships and ratios.

[0020] In addition, the embodiments shown below are merely examples of devices and methods for embodying the technical idea of ​​the present invention, and the technical idea of ​​the present invention does not specify the materials, shapes, structures, arrangements, etc. of the components to those described below. The technical idea of ​​the present invention can be modified in various ways within the technical scope defined by the claims.

[0021] <Embodiments of the present invention> Hereinafter, an example of a manufacturing process for a wiring board using a support according to an embodiment of the present invention will be described with reference to the drawings. In the present disclosure, a "support" refers to an object having a surface. Additionally, the term "upper surface" refers to the surface in the normal direction of a surface or layer, and the term "lower surface" refers to the reverse surface in the normal direction of a surface or layer. Additionally, "upper" refers to the vertically upward direction when the surface or layer is placed horizontally. Additionally, "below" refers to the direction vertically below when the surface or layer is placed horizontally. Moreover, the term "planar shape" refers to the shape when a surface or layer is viewed from above.

[0022] First, an example will be described in which a support 1, which is a rectangular plate-like member, is used, as shown in Fig. 1. Fig. 1 is a cross-sectional view showing a state in which a release layer 2 is formed on the upper surface of the support 1, a plurality of first wiring substrates 12 are formed on the upper surface of the release layer 2, and a warp suppressing layer 3 is formed on the lower surface of the support 1.

[0023] In this embodiment, as shown in FIG. 2, a plurality of first wiring boards 12 are placed above the support body 1 to form a board unit 12A.

[0024] In this embodiment, the support 1 will be described as a panel that is a rectangular plate-like member, but the support 1 may be, for example, a circular wafer.

[0025] The support 1 is advantageously light-transmitting since light may be irradiated onto the peeling layer 2 through the support 1, and for example, a rectangular glass plate may be used. Rectangular glass is suitable for large size, and glass has excellent flatness and high rigidity, making it suitable for forming a fine pattern on the support.

[0026] In addition, glass has a small coefficient of thermal expansion (CTE) and is not easily distorted, and is therefore excellent in terms of ensuring pattern placement accuracy and flatness. When glass is used as the support 1, the thickness of the glass is preferably large in order to suppress the occurrence of warping during the manufacturing process, and is, for example, 0.7 mm or more, and preferably 1.1 mm or more.

[0027] Furthermore, the CTE of the glass is preferably 3 ppm or more and 15 ppm or less, and from the viewpoint of compatibility with the CTE of the FC-BGA substrate (second wiring substrate) 12 and the semiconductor element 11, it is more preferably about 9 ppm.

[0028] As the type of glass, for example, quartz glass, borosilicate glass, alkali-free glass, soda glass, sapphire glass, or the like can be used.

[0029] On the other hand, in cases where light transmittance is not required for the support 1 when peeling off the support 1, for example, when a resin that foams when heated is used for the peel-off layer 2, a material with less distortion, such as metal or ceramics, can be used for the support 1.

[0030] The release layer 2 may be made of, for example, a resin that absorbs light such as UV light and generates heat or changes in quality to become peelable, or may be made of a resin that foams when heated to become peelable.

[0031] Specifically, the release layer 2 can be selected from organic resins such as epoxy resin, polyimide resin, polyurethane resin, silicone resin, polyester resin, oxetane resin, maleimide resin, and acrylic resin, and inorganic layers such as amorphous silicon, gallium nitride, and metal oxide layers. Furthermore, the release layer 2 may contain additives such as a photodecomposition promoter, a light absorber, a sensitizer, and a filler.

[0032] Furthermore, the release layer 2 may be composed of multiple layers, and for example, for the purpose of protecting the multilayer wiring layer formed on the support 1 in a later step, a protective layer may be further provided on the release layer 2, or a layer for improving adhesion to the support 1 may be provided under the release layer 2. Furthermore, a laser light reflecting layer or a metal layer may be provided between the release layer 2 and the multilayer wiring layer, and the configuration is not limited to this embodiment.

[0033] In addition, when a resin that can be peeled off by light such as laser light is used as the peel-off layer 2, if the support 1 is translucent, the direction in which light is irradiated onto the peel-off layer 2 may be the side opposite to the side on which the peel-off layer 2 is provided, i.e., the side on which the warp suppression layer 3 is formed.

[0034] The warp suppression layer 3 may be, for example, a resin that transmits light such as laser light. Specifically, the warp suppression layer 3 may be, for example, an organic resin such as an epoxy resin, a polyimide resin, a polybenzoxazole resin, or a benzocyclobutene resin. The warp suppression layer 3 may be made of the same resin as the insulating resin of the first wiring board 12, and may have photosensitivity.

[0035] The thickness of the warp suppression layer 3 is preferably 5 μm or more and 50 μm or less. If it is 5 μm or less, the warp suppression effect may not be obtained. If it is 50 μm or more, the warp suppression effect may be excessive, and warp may occur in the opposite direction. In addition, the thickness of the warp suppression layer 3 is preferably thinner than that of the first wiring board. If the warp suppression layer 3 is thicker than the first wiring board 12, the warp suppression effect may be excessive, and warp may occur in the opposite direction (convex toward the first wiring board 12).

[0036] In the following, an embodiment of the present invention will be described using an example in which a resin that transmits IR (infrared) laser light is used for the warp suppression layer 3, glass is used for the support 1, and a resin that absorbs IR laser light and becomes peelable is used for the peel-off layer 2.

[0037] Next, an example of a process for manufacturing the first wiring board 12 on the support 1 according to one embodiment of the present invention will be described with reference to FIGS.

[0038] First, as shown in FIG. 3(a), a release layer 2 is formed on the upper surface of a support 1.

[0039] Next, as shown in FIG. 3(b), an insulating resin layer 4 is formed on the upper surface of the release layer 2, and a warp suppressing layer 3 is formed on the lower surface of the support 1.

[0040] In this embodiment, the insulating resin layer is formed by, for example, spin-coating a photosensitive epoxy resin. Photosensitive epoxy resin can be cured at a relatively low temperature, shrinks little due to curing after formation, and is excellent for subsequent fine pattern formation.

[0041] When a liquid photosensitive resin is used, the method of forming the photosensitive resin can be selected from slit coating, curtain coating, die coating, spray coating, electrostatic coating, inkjet coating, gravure coating, screen printing, gravure offset printing, spin coating, and doctor coating. When a film-like photosensitive resin is used, lamination, vacuum lamination, vacuum pressing, and the like can be applied. For the insulating resin layer, for example, a photosensitive polyimide resin, a photosensitive benzocyclobutene resin, a photosensitive epoxy resin and its modified product, and a photosensitive polybenzoxazole resin can also be used.

[0042] The method of forming the warp suppression layer 3 can be selected from slit coating, curtain coating, die coating, spray coating, electrostatic coating, inkjet coating, gravure coating, screen printing, gravure offset printing, spin coating, and doctor coating when a liquid resin is used. When a film-like resin is used, lamination, vacuum lamination, vacuum pressing, and the like can be applied. The warp suppression layer 3 may have photosensitivity, and for example, photosensitive polyimide resin, photosensitive benzocyclobutene resin, photosensitive epoxy resin and its modified product, and photosensitive polybenzoxazole resin can be used.

[0043] The warp suppressing layer 3 may be made of the same resin as the insulating resin layer 4. By using the same resin as the insulating resin layer 4, processing in a single process becomes possible.

[0044] There is no problem in the order in which the insulating resin layer 4 and the warp suppressing layer 3 are formed. Furthermore, it is also possible to form the release layer 2 and the insulating resin layer 4 after forming the warp suppressing layer 3 on the lower surface of the support 1.

[0045] Furthermore, it is also possible to use a resin different from that of the insulating resin layer 4 for the warp suppressing layer 3. For example, by using a resin having a higher Young's modulus and a larger CTE than the insulating resin layer 4, it is possible to obtain the warp suppressing effect even if the warp suppressing layer 3 is made thin.

[0046] The warp suppression layer 3 may contain a resin different from that of the insulating resin layer 4 of the first wiring board 12. When the warp suppression layer 3 contains a resin different from that of the insulating resin layer 4, the number of resins that can be selected increases, increasing the degree of freedom in design. For example, it is possible to use a photosensitive epoxy resin for the insulating resin layer 4 of the first wiring board 12, and a non-photosensitive, thermosetting polyimide resin for the warp suppression layer 3.

[0047] The Young's modulus × thickness × CTE of the warp suppression layer 3 is preferably 0.9 to 1.1 times the Young's modulus × thickness × CTE of the insulating resin (insulating resin layer 4) of the first wiring board. If the Young's modulus × thickness × CTE of the warp suppression layer 3 is less than 0.9 times the Young's modulus × thickness × CTE of the insulating resin of the first wiring board, the warp suppression effect may not be obtained. If the Young's modulus × thickness × CTE of the warp suppression layer 3 is more than 1.1 times the Young's modulus × thickness × CTE of the insulating resin of the first wiring board, the warp suppression effect may be excessive, and warping in the opposite direction may occur.

[0048] Young's modulus reflects the elastic properties of a material and is a value that indicates how difficult a material is to deform. It is also called the longitudinal elastic modulus or modulus of longitudinal elasticity. Young's modulus can be obtained by measurement using a universal material testing machine, a thin film hardness meter, a dynamic viscoelasticity measuring device, etc. It is desirable to use values ​​for the Young's modulus of the warp suppression layer 3 and the Young's modulus of the insulating resin layer 4 at the same measurement method and temperature.

[0049] CTE is the rate of change in length per unit temperature change, and is also called the coefficient of thermal expansion or linear expansion. CTE can be obtained by measurement using a thermomechanical analyzer or the like. It is also possible to use an average CTE within a certain temperature range. It is desirable to use the same measurement method and temperature or temperature range for the CTE of the warp suppression layer 3 and the CTE of the insulating resin layer 4.

[0050] In the following, an embodiment of the present invention will be described taking as an example a case where the warp suppressing layer 3 is made of the same resin as the insulating resin layer 4 and is formed to a thickness of 15 μm.

[0051] Next, as shown in FIG. 3(c), openings are provided in the insulating resin layer by photolithography. The openings may be subjected to plasma treatment in order to remove residues from development. The thickness of the insulating resin layer 4 is set according to the thickness of the conductor layer to be formed in the openings, and is set to, for example, 7 μm in one embodiment of the present invention. The shape of the openings in plan view is set according to the pitch and shape of the bonding electrodes of the FC-BGA substrate, and in one embodiment of the present invention, the opening shape is set to, for example, φ80 μm, with a pitch of 150 μm.

[0052] Next, steps for manufacturing first wiring board 12 above the surface of support 1 will be described with reference to Fig. 4 to Fig. 8. Note that Fig. 4 to Fig. 8 use enlarged views of a portion of the central region of support 1 to describe an example of a step of forming multilayer wiring and a step of forming electrodes for bonding of the first wiring board of the present invention.

[0053] In Figure 4(a), as explained in Figure 3(c), a release layer 2 and an insulating resin layer 4 are formed above the surface of the support 1, and a warp suppression layer 3 is formed below the support 1.

[0054] Next, as shown in Fig. 4(b), a seed layer 5 is formed on the release layer 2 in a vacuum. The seed layer 5 acts as a power supply layer for electrolytic plating in forming wiring. The seed layer 5 is formed by, for example, a sputtering method or a CVD method, and may be made of, for example, Cu, Ni, Al, Ti, Cr, Mo, W, Ta, Au, Ir, Ru, Pd, Pt, AlSi, AlSiCu, AlCu, NiFe, ITO, IZO, AZO, ZnO, PZT, TiN, Cu3N4, or a combination of these.

[0055] In this embodiment, taking into consideration the electrical characteristics, ease of manufacture, and cost, a titanium layer and then a copper layer are formed in this order by sputtering. The total thickness of the titanium and copper layers is preferably 1 μm or less as a power supply layer for electrolytic plating. In one embodiment of the present invention, Ti: 50 nm, Cu: 300 nm are used.

[0056] 4(c), a conductor layer 6 is formed above the seed layer 5 by electrolytic plating. This conductor layer 6 will later become an electrode for bonding to the FC-BGA substrate 13. Types of electrolytic plating include nickel electrolytic plating, copper electrolytic plating, chromium electrolytic plating, Pd electrolytic plating, gold electrolytic plating, rhodium electrolytic plating, and iridium electrolytic plating, among which copper electrolytic plating is preferable because it is simple, inexpensive, and has good electrical conductivity.

[0057] Considering that the conductor layer 6 serves as an electrode for bonding to the FC-BGA substrate 13 and is soldered, it is desirable that the thickness of the electrolytic copper plating is 1 μm or more and 30 μm or less from the viewpoint of productivity. In one embodiment of the present invention, the openings of the insulating resin layer 4 are electrolytically plated with Cu to a thickness of 9 μm, and the upper part of the insulating resin layer 4 is electrolytically plated with Cu to a thickness of 2 μm.

[0058] 4(d), the copper layer is polished by CMP (chemical mechanical polishing) or the like to remove the conductor layer 6 and the seed layer 5. In one embodiment of the present invention, the Cu:2 μm of the conductor layer 6 on the upper part of the insulating resin layer 4 and the seed layer 5 are removed by polishing. The conductor layer 6 remaining after polishing becomes an electrode for bonding to the FC-BGA substrate 13. That is, in this embodiment, an electrode for bonding to the FC-BGA substrate 13 is formed by a damascene method.

[0059] Next, a wiring layer is formed. In one embodiment of the present invention, the wiring layer is formed by a semi-additive process (SAP). First, as shown in FIG. 5A(a), an insulating resin layer 4 is formed on the upper surface of the plane formed in FIG. 4(d) in the same manner as described in FIG. 4(a). The thickness of the insulating resin layer 4 is set according to the thickness of the conductor layer to be formed in the opening, and is set to, for example, 2 μm in one embodiment of the present invention.

[0060] The opening in the insulating resin layer 4 is formed so as to be bonded to the conductor layer 6, and in one embodiment of the present invention, is formed as an opening having a diameter of, for example, φ10 μm. This opening has the shape of a via portion connecting the upper and lower layers of the multilayer wiring.

[0061] Next, as shown in FIG. 5A(b), a seed layer 5 is formed in a vacuum in the same manner as described in FIG. 4(b).

[0062] Next, as shown in Fig. 5A(c), a resist pattern 7 is formed on the upper surface of the seed layer 5. Thereafter, as shown in Fig. 5A(d), a conductor layer 6 is formed by electrolytic plating. The conductor layer 6 becomes the via portion and the wiring portion.

[0063] Examples of types of electrolytic plating include electrolytic nickel plating, electrolytic copper plating, electrolytic chromium plating, electrolytic Pd plating, electrolytic gold plating, electrolytic rhodium plating, and electrolytic iridium plating. Of these, electrolytic copper plating is preferred because it is simple, inexpensive, and has good electrical conductivity.

[0064] The thickness of the electrolytic copper plating is desirably 0.5 μm or more from the viewpoint of electrical resistance of the wiring portion, and 30 μm or less from the viewpoint of productivity. In one embodiment of the present invention, Cu: 4 μm is formed in the opening of the insulating resin layer 4, and Cu: 2 μm is formed on the upper part of the insulating resin layer 4.

[0065] Thereafter, the resist pattern 7 is removed as shown in Fig. 5B(e), and then the unnecessary seed layer 5 is etched away as shown in Fig. 5B(f).

[0066] 5A and 5B are repeated, a multi-layered wiring structure can be formed above the release layer 2. In the example of Fig. 6, two wiring layers are formed.

[0067] If the warping of the substrate unit increases due to the multi-layering process, it is also possible to increase the thickness of the warp suppressing layer 3 as appropriate.

[0068] Next, as shown in FIG. 7, a conductor layer 6 is formed to serve as an electrode for bonding to a semiconductor element 11, to form a substrate unit. The method for forming the electrode for bonding is the same as the method for forming the wiring layer described above, but the thickness of the electrolytic copper plating is different between the electrode for bonding and the wiring layer. It is desirable that the thickness of the electrolytic copper plating of the electrode for bonding is 1 μm or more from the viewpoint of solder bonding, and 30 μm or less from the viewpoint of productivity. In one embodiment of the present invention, Cu: 9 μm is formed in the opening of the insulating resin layer 4, and Cu: 7 μm is formed on the upper part of the insulating resin layer 4.

[0069] Next, as shown in FIG. 8, in order to prevent oxidation of the surface of the conductor layer 6 and improve wettability of the solder bumps, the substrate unit may be provided with a surface treatment layer 8. In the embodiment of the present invention, an electrolytic Ni / SnAg plating film is formed as the surface treatment layer 8. Note that an OSP (Organic Soiderability Preservative, surface treatment with a water-soluble preflux) film may be formed on the surface treatment layer 8. In addition, surface treatments such as Sn, SnAg, Ni / Sn, Ni / SnAg, Ni / Cu / Sn, Ni / Cu / SnAg, Ni / Au, and Ni / Pd / Au may be appropriately selected according to the application as electrolytic plating, and Ni / Au, Ni / Pd / Au, and Sn may be appropriately selected as electroless plating.

[0070] As a result, as shown in FIG. 1, first wiring board 12 is completed on the support body, and board unit 12A in which a plurality of first wiring boards 12 are attached to the support body can be obtained.

[0071] The wiring layer can be formed by the SAP (Semi Additive Process) method shown in Figs. 5 to 8, or by the Damascene method. In the case of the Damascene method, after laminating an insulating resin layer, a pattern is formed by photolithography, and a seed layer is formed, followed by electrolytic copper plating. After electrolytic copper plating, a planarization process can be performed by CMP (Chemical Mechanical Polishing). The number of layers of the wiring layer is at least one, and may be set appropriately depending on the line width of the first wiring board.

[0072] Next, an example of a method for manufacturing a semiconductor device according to an embodiment of the present invention, which includes a mounting step of a semiconductor element, a removing step of the support and the peeling layer, and a mounting step on an FC-BGA substrate, will be described with reference to Figures 9 to 13. Figures 9 to 13 are cross-sectional views limited to the region of first wiring board 12 after singulation, in order to explain the details of the multiple first wiring boards placed above support 1.

[0073] First, the mounting process of the semiconductor element 11 shown in Fig. 9(a) will be described. In Fig. 9(a), 9 is an electrode for mounting the semiconductor element, 10 is an electrode for bonding with the FC-BGA substrate, 12 is a first wiring board, and 14 is a solder joint between the semiconductor element and the first wiring board.

[0074] The semiconductor element 11 is mounted on the first wiring board 12 by using mount & reflow, TCB (Thermal Compression Bonding), etc. For TCB, a TC-CUF (Thermal Compression Capillary Underfill) method in which the first sealing resin 16 is injected by capillary action after solder bonding, a film-like bonding material (NCF), or a non-conductive paste (NCP) in which a liquid resin is placed before bonding and fills spaces during bonding may be used.

[0075] In the present invention, TC-CUF is used for sealing with the first sealing resin 16 after solder bonding as shown in Fig. 9(b), which is injected by capillary action. The mounting method of the semiconductor element 11 may be changed as appropriate from the viewpoint of the size of the semiconductor element 11 and the equipment used for mounting. However, when the bonding pitch between the first wiring board 12 and the semiconductor element 11 is fine, it is preferable to select one of the TCB methods.

[0076] Next, as shown in FIG. 9(c), the semiconductor element 11 is sealed with a second sealing resin 17 to protect the side surface. The material used for the second sealing resin 17 is in the form of granules, liquid, or tablets, and is formed by compression molding or transfer molding, using one of epoxy resin, silicon resin, acrylic resin, urethane resin, polyester resin, and oxetane resin, or a mixture of two or more of these resins, to which silica, titanium oxide, aluminum oxide, magnesium oxide, zinc oxide, or the like is added as a filler. The shape, composition, and forming method of the resin may be appropriately set according to the manner in which the first wiring board 12 is placed on the support 1. In the present invention, a liquid epoxy resin is used, and molding is performed by compression molding.

[0077] 9(d), the second sealing resin 17 is removed from the upper surface of the semiconductor element 11 with respect to the first wiring board 12 sealed with the second sealing resin 17. If the second sealing resin 17 remains on the semiconductor element 11, warping may occur due to the influence of the CTE of the second sealing resin 17, and in some cases, peeling may occur at the interface between the first wiring board 12 and the second sealing resin 17. The second sealing resin 17 on the semiconductor element 11 can be removed by CMP, grinding, or the like. In the present invention, the second sealing resin 17 on the semiconductor element 11 is removed by grinding.

[0078] Next, a process of separating the first wiring board and the semiconductor element from the support 1 will be described with reference to Fig. 10. Note that in Fig. 10, the support 1 and the first wiring board 12 to which the semiconductor element after singulation shown in Fig. 9 is bonded are shown upside down.

[0079] When the peeling layer 2 can be peeled off by irradiation with a laser beam 19, since the support 1 is light-transmitting, the laser beam 19 is irradiated onto the warp suppression layer 3 from the side of the warp suppression layer 3 as shown in FIG. 10(a). The laser beam 19 passes through the warp suppression layer 3 and the support 1 and is irradiated onto the peeling layer 2, and the support 1 can be removed as shown in FIG. 10(b). In one embodiment of the present invention, an IR laser beam of 1064 nm is used as the laser beam 19. In one embodiment of the present invention, the support 1 is made of glass and is light-transmitting, and the resins used in the warp suppression layer 3, such as epoxy resin, polyimide resin, polybenzoxazole resin, and benzocyclobutene resin, have the property of transmitting an IR laser, so that the laser beam passes through the warp suppression layer and the support and is irradiated onto the peeling layer.

[0080] Next, as shown in FIG. 10(c), the release layer 2 is completely removed by dry etching, solvent cleaning, ultrasonic cleaning, or the like to expose the electrodes 10 for bonding to the FC-BGA substrate 13. When dry etching is used, the etching is performed using a gas containing at least one of gas species such as O2, Ar, and CF4. When solvent cleaning is used, a solvent such as acetone, toluene, MEK, or methanol is used. When ultrasonic cleaning is used, the removal is performed with an oscillation frequency in the range of 28 kHz to 1 MHz. The removal of the release layer 2 may be performed by combining any one or more of these removal methods.

[0081] Next, solder is formed on the electrodes 10 for bonding to the FC-BGA substrate 13 of the first wiring substrate 12 shown in Fig. 11. The solder is formed by forming Ni / Au, Ni / Pd / Au, or Sn on the electrodes 10 for bonding to the FC-BGA substrate 13 by an OSP (Organic Solderability Preservative, surface treatment with a water-soluble preflux) film or electroless plating, then printing the flux, mounting a solder ball, and then reflowing, or by forming Sn, SnAg, Ni / Sn, Ni / SnAg, Ni / Cu / Sn, Ni / Cu / SnAg, or Sn by electrolytic plating, then printing the flux, and then mounting a solder ball, or by forming Sn, SnAg, Ni / Sn, Ni / SnAg, Ni / Cu / Sn, or Ni / Cu / SnAg by electrolytic plating, then reflowing, or by directly printing a solder paste and then reflowing. In the embodiment of the present invention, after forming Ni / Pd / Au by electroless plating, flux printing is performed, solder balls are mounted, and reflow is performed. This forms solder joints 15 between the first wiring board and the FC-BGA board, and completes an assembly of the first wiring board 12 in which the semiconductor element 11 is fixed with the first sealing resin and the second sealing resin.

[0082] Next, the first wiring board 12 as an assembly after the balls are mounted is diced into pieces according to the shape of the support or wafer. Examples of the dicing method include blade dicing, laser dicing, plasma dicing, etc., and the method may be set appropriately. In the present invention, the dicing is performed into pieces by using blade dicing.

[0083] 12, first wiring board 12 carrying individual semiconductor elements 11 is mounted on FC-BGA substrate 13. First wiring board 12 carrying semiconductor elements 11 is mounted on FC-BGA substrate 13 using mount & reflow, TCB, or the like.

[0084] In this embodiment, first wiring board 12 carrying semiconductor element 11 is mounted on FC-BGA substrate 13, and solder bonding between FC-BGA substrate 13 and first wiring board 12 carrying semiconductor element 11 is performed by a mount & reflow method, and third sealing resin 18 is injected by capillary action into the gap between FC-BGA substrate 13 and first wiring board 12. As a result, a semiconductor device 20 of the present invention can be obtained as shown in Fig. 13.

[0085] While one embodiment of the present invention has been exemplified above, the present invention is not limited to the above embodiment, and it goes without saying that, as long as the technical idea of ​​the embodiment of the present invention is not deviated from, other layers and structures can be formed as desired for the purpose of improving other required physical properties such as rigidity, strength, and impact resistance, taking into account the use as a wiring board.

[0086] <Action and effect> Next, the effects of using the above-described configuration of the substrate unit and the manufacturing method thereof will be described.

[0087] According to one aspect of the present invention, a method for forming a release layer and a fine wiring layer on a support, mounting and sealing a semiconductor element, and then peeling off the support substrate and mounting the semiconductor element on an FC-BGA substrate includes the steps of: This makes it possible to suppress warping of the board unit and mount the semiconductor element with minimal warping.

[0088] <Comparative Example> A configuration in which a substrate unit is manufactured without forming a warp suppression layer 3 below the support body will be described as a comparative example with reference to Fig. 14. Fig. 14 is a cross-sectional view showing a state in which a release layer 2 is formed on the upper surface of the support body 1, and a plurality of first wiring substrates 12 are formed on the upper surface of the release layer 2. No warp suppression layer 3 is formed on the lower surface of the support body 1.

[0089] At this time, there is a risk of warping in the substrate unit 12B because the warp suppressing layer 3 is not formed. Warping in the substrate unit 12B may cause mounting defects of the semiconductor element. Recent high-performance semiconductor elements have a large area, and semiconductor elements with a large area are more likely to cause mounting defects.

[0090] <Confirmation of action and effect> To confirm the effect of this embodiment, a simulation model of the board unit 12A of the example and the board unit 12B of the comparative example was created. The size of the board unit was 300 mm square in both the example and the comparative example. A material with a Young's modulus of 1.5 GPa and a CTE of 65 ppm was used for the insulating resin of the first wiring board. The thickness of the insulating resin layer of the first wiring board was 17 μm in both the example and the comparative example. In the example, a warp suppressing layer 3 of 15 μm was formed on the lower surface of the support using the same material as the insulating resin of the first wiring board.

[0091] In the simulation model of the embodiment, the first wiring board was disposed above the support, and the height of the convex portion was calculated to be 50 μm, resulting in a downward convex warp. On the other hand, in the simulation model of the comparative example, the first wiring board was disposed above the support, and the height of the convex portion was calculated to be 400 μm, resulting in a downward convex warp. It was confirmed that the formation of the warp suppressing layer 3 has the effect of reducing warp.

[0092] The above-described embodiment is merely an example, and it goes without saying that other specific details such as structure can be modified as appropriate. [Industrial Applicability]

[0093] The present invention can be used in a substrate unit used for mounting a semiconductor element on an FC-BGA substrate. [Explanation of symbols]

[0094] 1 Support 2. Peel layer 3. Anti-warping layer 4 Insulating resin layer 5 Seed layer 6 Conductor Layer 7 Resist Pattern 8 Surface treatment layer 9. Electrodes for mounting semiconductor elements 10 Electrode for bonding with FC-BGA substrate 11 Semiconductor elements 12 First wiring board 12A Substrate unit of the present invention 12B Comparative example board unit 13 FC-BGA board (second wiring board) 14 Solder joint between semiconductor element and first wiring board 15 Solder joint between first wiring board and FC-BGA board 16 First sealing resin 17 Second sealing resin 18 Third sealing resin 19 Laser Light 20 Semiconductor Devices

Claims

1. Support and A substrate unit in which a plurality of first wiring substrates are placed above the support via a release layer, an electrode for bonding at least one semiconductor element is provided on a first surface of the first wiring board; an electrode for joining the first wiring board to a second wiring board is provided on a second surface of the first wiring board; A substrate unit comprising a warp suppressing layer formed below the support body.

2. The substrate unit according to claim 1 , wherein the warp suppressing layer is made of a resin.

3. 3. The substrate unit according to claim 1, wherein the warp suppressing layer has a thickness of 5 μm or more and 50 μm or less.

4. 4. The substrate unit according to claim 1, wherein the warp suppressing layer contains the same resin as an insulating resin of the first wiring substrate.

5. 5. The substrate unit according to claim 1, wherein the warp suppressing layer is thinner than the first wiring substrate.

6. 4. The substrate unit according to claim 1, wherein the warp suppressing layer contains a resin different from an insulating resin of the first wiring substrate.

7. A substrate unit as described in any one of claims 1, 2, 3, and 6, characterized in that the Young's modulus x thickness x CTE of the warp suppression layer is 0.9 to 1.1 times the Young's modulus x thickness x CTE of the insulating resin of the first wiring substrate.

8. 8. The substrate unit according to claim 1, wherein the support body is made of glass.

9. 4. The substrate unit according to claim 3, wherein the resin of the warp suppressing layer is one or a mixture of two or more resins selected from the group consisting of epoxy resin, polyimide resin, polybenzoxazole resin and benzocyclobutene resin.

10. A method for manufacturing a substrate unit in which a plurality of first wiring substrates are placed above a support, comprising the steps of: forming a release layer on an upper surface of the support; forming a resin layer above the release layer; forming a warp suppressing layer on the lower surface of the support; forming an opening in the resin layer; forming a seed layer over the resin layer and the opening; forming an electrolytic plating layer above the seed layer; a step of polishing the electrolytic plating layer and the seed layer until the resin layer is exposed, and forming an electrode for bonding to a second wiring board; a step of repeatedly forming a resin layer and a conductor layer on the exposed upper surfaces of the resin layer and the electrodes to obtain a multilayer wiring; forming an electrode for bonding a semiconductor element to an outermost surface of the multilayer wiring; A method for manufacturing a substrate unit, comprising:

11. A method for manufacturing a semiconductor device using the substrate unit according to any one of claims 1 to 9, bonding the semiconductor element to the first wiring substrate; sealing a gap between the first wiring substrate and the semiconductor element with a first sealing resin; sealing the first wiring substrate and the side surfaces of the semiconductor element with a second sealing resin; peeling the first wiring substrate from the support; obtaining an assembly in which the semiconductor element is bonded to the first wiring substrate; dividing the assembly into individual first wiring substrates; bonding the first wiring substrate to the second wiring substrate; sealing a gap between the first wiring substrate and the second wiring substrate with a third sealing resin; 2. A method for manufacturing a semiconductor device comprising the steps of:

12. In the step of peeling off the first wiring substrate from the support, 12. The method for manufacturing a semiconductor device according to claim 11, further comprising the step of irradiating the warp suppression layer with laser light.

13. 13. The method for manufacturing a semiconductor device according to claim 12, wherein the laser light is an IR laser light.

Citation Information

Patent Citations

  • Semiconductor package and method for manufacturing the same

    JP2012129419A

  • Manufacturing method of semiconductor package

    JP2013118364A

  • Wiring board and semiconductor device

    JP2014225671A

  • Semiconductor element built-in substrate

    JP2017199705A

  • Coreless substrate with fine wiring layer, semiconductor package and semiconductor device, and method of manufacturing coreless substrate with fine wiring layer and semiconductor package

    JP2019169559A