Manufacturing method for processed plastic film
By installing a conductor with a small radius near the plastic film and generating plasma, the method effectively neutralizes static charges, preventing discharge and adhesion problems during high-speed vacuum processing of laminated films.
Patent Information
- Application Number
- JP2021098726
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-06-14
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-06-14
AI Technical Summary
Existing methods for manufacturing laminated plastic films in a vacuum environment fail to effectively remove static charges at high speeds, leading to discharge damage and electrostatic adhesion issues, particularly in processes like vapor deposition where electrification is high.
Installation of a conductor with a radius of curvature of 1 mm or less near the plastic film, maintaining a pressure of 8 Pa to 800 Pa, and using grounded conductors and plasma generation to eliminate static charges, combined with a grounded metal roll to manage electrostatic adhesion.
Prevents discharge damage and unwinding issues by efficiently reducing surface potential and neutralizing static charges on the plastic film, ensuring smooth operation at high speeds.
Smart Images

Figure 0007574749000002 
Figure 0007574749000003 
Figure 0007574749000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a processed plastic film, which includes a step of removing electric charge that has built up on a plastic film traveling in a vacuum. [Background technology]
[0002] There are commercially available laminated films in which inorganic materials are laminated onto plastic films, such as magnetic recording tape, ITO film, aluminum vapor deposition film, and transparent vapor deposition film. These laminated films are manufactured using sputtering technology and vacuum vapor deposition technology. In these manufacturing methods, a long plastic film is placed in a vacuum device as a roll, and the plastic film is unwound while traveling through the vacuum to laminate inorganic thin film layers (see, for example, Patent Document 1).
[0003] When a plastic film is unwound or moved on a roll, the plastic film picks up electric charges due to peeling electrification, friction electrification, etc. When the potential becomes high due to the accumulation of many electric charges, a discharge occurs, destroying the surface of the plastic film, or discharging to a nearby conductor and creating holes in the plastic film. Furthermore, the plastic film may become electrostatically attracted to a roll in contact with the film and become wrapped around it, making it impossible for the film to move.
[0004] For this reason, static eliminators are installed to eliminate static electricity. For example, an electrostatic brush made of stainless steel fibers connected to earth is placed within 1 mm of the unwound plastic film, or an ion generator is used (see, for example, Patent Document 1). There is also a method of eliminating static electricity by blowing gas onto a charged plastic film (see, for example, Patent Document 2). There is also a method of applying a DC or AC voltage to electrodes and adjusting the pressure to generate a glow discharge to remove static electricity from a plastic film (see, for example, Patent Document 3).
[0005] When the electrostatic brush is placed within 1 mm as described in Patent Document 1, problems are unlikely to occur when the plastic film travels at a low speed (e.g., 10 m / min), but when the plastic film travels at a high speed (e.g., 100 m / min), the plastic film vibrates and comes into contact with the electrostatic brush, causing scratches on the plastic film. Generally, in a high vacuum, the electric field is concentrated and the movement of charges into space does not occur unless a high voltage is applied. In addition, when gas is present, the state of discharge changes depending on the pressure region, and at relatively high pressures, arc discharge occurs and damages the plastic film. The discharge start voltage also changes depending on the distance between the electrodes and the electrode shape. Therefore, the method of simply blowing gas as described in Patent Document 2 may not be able to remove static electricity or may cause arc discharge and damage the plastic film.
[0006] The neutralization by glow discharge described in Patent Document 3 is a method of neutralization using plasma generated by glow discharge, and neutralization is performed by electrons and ions present in the plasma. If the surface of the plastic film is charged with electrons, the ions that have moved to the boundary region in the plasma due to the potential difference between the boundary region of the plasma and the surface of the plastic film are accelerated and combine with the electrons to neutralize the film. Therefore, if the film is exposed to plasma for a sufficient period of time, it will be completely neutralized. However, as the running speed of the plastic film increases, the peeling electrification and frictional electrification of the plastic film increases, but the time of exposure to plasma becomes shorter, making it impossible to sufficiently remove the electricity.
[0007] Sputtering is a method for forming an inorganic thin film layer on a plastic film. In this method, the raw material of the film to be formed is prepared as a target, plasma is generated, and ions are bombarded against the target, which is placed at a negative potential, to knock out the atoms and molecules of the raw material, depositing the atoms and molecules on the plastic film. In addition, the thin film formation speed in this method is generally several meters per minute, and the amount of electrostatic charge is relatively small. Electrostatic charge is also reduced in the sense that it is exposed to plasma.
[0008] Another method is chemical vapor deposition (CVD), in which a raw material gas is introduced between electrodes, plasma is generated, and the gas is chemically changed to form a film. In this method, the plastic film is usually moved at a speed of several tens of meters per minute, and since the plastic film travels through the plasma, the amount of charge is small.
[0009] In the vacuum deposition method, the temperature of the film raw material is raised and evaporated to form a film on a plastic film, and the plastic film is manufactured at a running speed of several hundred meters per minute. This results in more charging than other methods. In particular, in the electron beam heating deposition method, in which the raw material is irradiated with an electron beam to heat and evaporate it, a large amount of electrons are charged onto the plastic film during deposition due to some of the electron beam bouncing off the raw material and secondary electrons being generated.
[0010] Compared to inorganic lamination methods such as sputtering and CVD, deposition methods produce a larger amount of charge, making static elimination more difficult. Also, existing static elimination methods may not be able to eliminate static electricity when using deposition methods that use electron beams. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Japanese Unexamined Patent Publication No. 2-281420 [Patent Document 2] JP 2000-54151 A [Patent Document 3] Japanese Patent Application Publication No. 62-56567 Summary of the Invention [Problem to be solved by the invention]
[0012] The present invention has been made against the background of the problems of the prior art. That is, the object of the present invention is to provide a method for producing a processed plastic film, which includes a static elimination step for preventing damage to the plastic film caused by abnormal discharge and eliminating problems with the running of the plastic film caused by electrostatic adhesion by removing the electric charge from the charged plastic film with a simple device and lowering the surface potential. [Means for solving the problem]
[0013] As a result of extensive investigations, the present inventors have found that the above problems can be solved by the means described below, and have arrived at the present invention. That is, the present invention has the following configuration. This is a method for manufacturing processed plastics, which is characterized by including a step (Step 1) of placing a conductor with a radius of curvature of 1 mm or less in the width direction of the plastic film near the plastic film as a method for reducing the amount of static electricity on a plastic film traveling in a vacuum, setting the closest distance between the plastic film surface and the conductor to between 2 mm and 10 mm, and maintaining the pressure between them at between 8 Pa and 800 Pa, and performing static electricity removal using a static elimination method using a grounded conductor.
[0014] The method for producing processed plastics further includes a step (step 2) of connecting a negative potential or a high-frequency AC potential to the plate electrode following step 1, flowing gas between the plate electrode and the plastic film to generate plasma, and installing a device for eliminating electricity using the generated plasma to eliminate electricity from the plastic film.
[0015] Furthermore, the method for producing processed plastics includes a step in which a metal roll is installed on the opposite side of the plastic film from the side on which the conductor is installed, the metal roll is grounded, and static electricity is removed while the plastic film runs over the metal roll.
[0016] Furthermore, there is provided a method for producing a processed plastic film, which comprises the above-mentioned step of providing a vapor deposition layer on a plastic film. Effect of the Invention
[0017] According to the present invention, the electric charge on the plastic film can be removed and the surface potential can be brought closer to the ground potential, thereby preventing damage to the plastic film due to unintended arc discharge, etc. Also, it is possible to avoid running problems caused by the plastic film wrapping around the roll during running due to electrostatic adhesion. [Brief description of the drawings]
[0018] [Figure 1] Schematic diagram of an example of a static eliminator [Diagram 2] An example of the tip of a conductor [Diagram 3] An example of the tip of a conductor: Square [Figure 4] An example of a conductor: Comb-shaped [Diagram 5] An example of the tip of a comb-shaped conductor [Figure 6] An example of the tip of a comb-shaped conductor [Figure 7] An example of the tip of a comb-shaped conductor [Figure 8] An example of a conductor placed on a roll [Figure 9] An example of a manufacturing method using static elimination (roll-to-roll electron beam deposition) [Figure 10] An example of combining a static elimination method using a conductor followed by a static elimination method using plasma with a plate electrode DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The manufacturing method of the present invention is a method for producing processed plastics, which is characterized by including a step of removing static electricity by placing a grounded conductor with a radius of curvature of 1 mm or less under a certain pressure near the plastic film as a method for reducing the amount of static electricity on the plastic film traveling in a vacuum.
[0020] The plastic film referred to in the present invention is a plastic film obtained by melt-extruding an organic polymer, and stretching it in the longitudinal direction and / or the transverse direction, cooling, and heat setting as necessary. Examples of the organic polymer include polyethylene, polypropylene, polyethylene terephthalate, polyethylene-2,6-naphthalate, nylon 6, nylon 4, nylon 66, nylon 12, polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, wholly aromatic polyamide, polyamideimide, polyimide, polyetherimide, polysulfone, polyphenylene sulfide, polyphenylene oxide, etc. Furthermore, these organic polymers may be copolymerized or blended with a small amount of other organic polymers.
[0021] In view of recent global environmental problems, it is also possible to use organic polymers which are prepared in whole or in part from organic matter derived from biomass.
[0022] Furthermore, the plastic film may be subjected to a surface treatment such as a corona treatment.
[0023] Furthermore, a laminate in which different organic materials are laminated together is also called a plastic film. A laminate in which a plastic film is coated with another organic material and laminated is also called a plastic film. A laminate in which a plastic film or a laminate in which a plastic film is coated with an organic material is coated with a metal layer such as aluminum or an inorganic material such as ITO or a metal oxide such as aluminum oxide and laminated is also called a plastic film. The thickness of the plastic film of the present invention is preferably in the range of 5 to 500 μm, more preferably in the range of 8 to 300 μm.
[0024] The processed plastic film referred to in the present invention refers to a plastic film which has been subjected to processing such as laminating an organic layer or an inorganic layer onto the plastic film, or treating the surface with plasma or the like to change the surface properties.
[0025] The conductor (1) of the present invention having a radius of curvature of 1 mm or less is a metal or carbon having a conductivity of 1×10 3 It refers to a molded product made of conductive materials with a resistance of S / m or higher. It also refers to resins made conductive by kneading these conductive materials in fibrous or powder form into the resin, etc., or resins with metal or carbon layers laminated on the surface. In the present invention, a radius of curvature of 1 mm or less means, for example, in the case of the conductor (1) for static elimination installed in Fig. 1, that the tip of the conductor facing the plastic film (2) has a radius of curvature smaller than a circle with a radius of 1 mm as shown in Fig. 2. The surface for which this radius of curvature is sought is the surface with the smallest radius of curvature when viewed in cross section on any plane passing through the tip. Also, the tip may have a corner with a radius of curvature smaller than the circle with a radius of 1 mm as shown by the dotted line in FIG. Furthermore, in the case of a comb-like or brush-like shape as shown in Fig. 4, if the tip of the part corresponding to the teeth of the comb or the part corresponding to the bristles of the brush has the shape shown in Fig. 5, the minimum value of the radius of curvature obtained at any cross section passing through the tip is 1 mm or less. The shape is not particularly limited as shown in Fig. 6 and Fig. 7, and it is sufficient that the tip has a radius of curvature of 1 mm or less.
[0026] The radius of curvature is preferably 1 mm or less. If it exceeds 1 mm, the electric field lines from the charges on the plastic film will be less concentrated on the conductor, and the force for ionizing the gas and extracting the charges will be insufficient.
[0027] Specific examples of conductors that satisfy the requirements of the conductor (1) of the present invention include copper strips having a thickness of 1 mm or less, thin carbon or metal threads that are generally sold as anti-static brushes, anti-static cloth woven with organic fibers and metal threads, or woven fabric with fibers laminated with a conductive material.
[0028] In the present invention, "installed in the width direction of the plastic film (2)" means installed so as to cover the entire width or substantially the entire width of the plastic film (2) as shown in FIG.
[0029] In the present invention, the shortest distance between the surface of the plastic film (2) and the conductor (1) is 2 mm or more and 10 mm or less means that the length from the tip of the conductor (1) to the surface of the plastic film (2) on a normal line that passes through the tip of the conductor (1) and connects the surface of the plastic film (2) is 2 mm or more and 10 mm or less. If it is closer than 2 mm, the running plastic film will vibrate and come into contact with the conductor, causing scratches or tears. On the other hand, if the distance is greater than 10 mm, the potential gradient between the plastic film and the conductor will be gentle, and the force of ionizing the gas and extracting the charge will be insufficient.
[0030] One method for maintaining the distance between the surface of a traveling plastic film and the conductor is to fix the surface position of the plastic film by running it under tension between at least two rolls (3), as shown in Fig. 1. However, with thin plastic films of 25 μm or less, wrinkles may occur due to the influence of the flatness and thickness uniformity, making it difficult to maintain the distance.
[0031] A preferred method is to run a plastic film (2) over a metal roll (3) as shown in FIG. 8, place a conductor (1) on the side opposite the metal roll (3), and maintain a distance between the conductor (1) and the plastic film (2).
[0032] The pressure in the present invention refers to the pressure in the space between the tip of the conductor and the plastic film. The pressure may be maintained by residual gas, but is usually adjusted by introducing gas from the outside. It is preferable to adjust and maintain the pressure by introducing argon as the gas. A pressure of about 1 Pa is effective for eliminating static electricity, but to obtain a more preferable static elimination effect, a pressure of 8 Pa or more is necessary. If the pressure is 800 Pa or more, the static elimination effect starts to decrease due to self-discharge, which is not preferable.
[0033] When introducing gas from outside, it is preferable to install a nozzle (4) for blowing gas between the tip of the conductor (1) and the plastic film (2) near the conductor. This allows for efficient adjustment of the pressure between the conductor and the plastic film. It is also preferable to surround the conductor (1) and the nozzle (4) with a wall (5). This allows for more efficient pressure adjustment and reduces pressure increases in other areas. It is preferable for the wall (5) to be made of a conductive material such as metal and to be grounded.
[0034] It is preferable that the metal roll (3) installed on the opposite side of the plastic film from the side on which the conductor (1) is installed is also grounded by being connected to the grounded vacuum chamber (6) or to a metal structure inside the vacuum chamber that is at ground potential.
[0035] The static elimination method of the present invention can efficiently eliminate the charge on the plastic film (2). It can prevent damage caused by the discharge of the charged charge, winding around the roll, etc. However, since static elimination utilizes the potential difference with the ground potential of the conductor, it is not possible to eliminate the charge on the plastic film to the ground potential. Therefore, as shown in Figure 10, it is preferable to have a step (step 2) of connecting a negative potential or a high-frequency AC potential to the plate electrode (7) following static elimination using a grounded conductor, flowing gas under the plate electrode (7) to generate plasma, and installing a device that eliminates static electricity using the generated plasma to eliminate static electricity.
[0036] The plate electrode (7) is preferably made of a metal, particularly titanium or stainless steel, which is resistant to sputtering by ions in the plasma. Carbon, which is conductive, is also preferable. The plasma that contributes to static elimination is generated by essentially maintaining the plate electrode (7) at a negative potential. Commonly used methods include lowering the potential using a DC power source, or applying a high-frequency alternating current (RF) to create a substantially negative potential. The potential reference is based on ground.
[0037] To generate plasma stably, it is preferable to use the magnetron method, which uses a magnetic field to confine electrons in the vicinity of the electrode. The magnetic field can be generated by placing a magnet or the like on the opposite side of the plate electrode where the plasma is generated. To efficiently generate a confining magnetic field, the plate electrode (7) is preferably made of a non-magnetic material. Based on this condition, the plate electrode (7) is preferably made of a non-magnetic metal such as titanium or stainless steel, or carbon.
[0038] Moreover, since the plate electrode (7) is heated by the plasma, it is preferable to cool it. The gas for generating plasma is preferably argon gas. It is also preferable to enclose the chamber with a wall (8) to stabilize the pressure. The pressure is preferably in the range of 0.1 Pa to 10 Pa.
[0039] Although the plate electrode (7) has a plate shape, when it is placed on the roll (5), it may be curved in order to keep the distance from the roll (5) constant.
[0040] An example of a manufacturing method that uses this static elimination method is the production of alumina transparent barrier film by deposition using an electron beam heating method. Alumina transparent barrier film is a plastic film that has barrier properties imparted by laminating an aluminum oxide layer onto a plastic film made of polyethylene terephthalate (PET), polyamide resin, or generally known as nylon (Ny)(2).
[0041] The manufacturing process will be explained using the schematic diagram of the manufacturing device shown in Figure 9. The roll of plastic film (2) that serves as the substrate is set on the unwinding roll (9). The plastic film (2) runs along the guide roll (10) and then over the coating roll (11). The aluminum in the crucible (12) is heated and evaporated by an electron beam emitted from an electron gun (19). The aluminum turns into gas and flies upward. Oxygen gas is blown in from a nozzle (13) along the way to cause a reaction, forming an alumina layer on the plastic film (2) traveling on the coating roll (11).
[0042] A large amount of reflected electrons and secondary electrons are emitted from the crucible (12) along with aluminum vapor. Some of the emitted electrons charge the plastic film (2) on the coating roll (11). When the plastic film is peeled off from the coating roll (11) in this state, the charged electrons are discharged, damaging the alumina layer and the plastic film.
[0043] A static eliminator (14) using the conductor of the present invention and a static eliminator (15) using a plate electrode are installed on the coating roll (11) to eliminate the charged electrons. Also, in order to reduce the charge caused by peeling when the plastic film (2) is peeled off from the coating roll (11), a negative electrode (16) is installed near the peeling point to generate plasma.
[0044] The plastic film (2) that leaves the coating roll (11) is passed through an optical thickness gauge (17) and wound onto a take-up roll (18). The optical thickness gauge (17) measures the light transmittance of the passing plastic film (2) to measure the thickness of the laminated alumina layer. To control the thickness to the target thickness, the electron beam output from the electron gun (13) is controlled to control the amount of aluminum evaporated from the crucible.
[0045] The coating roll (11) in this description corresponds to the metal roll (3) placed on the opposite side of the plastic film with respect to the side on which the conductor is placed. EXAMPLES
[0046] The present invention will be specifically described below by showing examples, but the present invention is not limited to these examples. Example 1 A transparent barrier film was produced using a roll-to-roll electron beam heating reactive deposition apparatus shown in the schematic diagram of the production apparatus in Figure 9. As the plastic film (2), Toyobo Ester (R) film E5100 12 μm thick manufactured by Toyobo Co., Ltd. was used. Aluminum (purity 3N) was placed in an alumina crucible (12) and evaporated by heating with an electron beam. Oxygen gas was introduced from a nozzle (13) at 16,800 sccm to react with the aluminum vapor, thereby laminating an alumina layer on the plastic film (2) traveling on the coating roll (11) set at -20°C. The plastic film was run at 8 m / sec.
[0047] After laminating the alumina layer, the plastic film (2) is neutralized by a static eliminator (14) using a conductor (1), and is then further neutralized by a static eliminator (15) using a plate electrode (7) before being separated from the coating roll (11). A negative electrode (16) was installed at the position where the plastic film (2) separated from the coating roll (11) to prevent peeling electrification. The conditions for neutralization are shown in Table 1. The conductor (1) is a woven fabric made of spun short fibers of several tens of micrometers laminated with metal and woven with chemical fibers, with the fibers protruding from the plastic film in a blind-like shape of about 5 mm. The distance between the plastic film and the tip of the blind fiber was kept 3 mm. The radius of curvature is less than 100 μm because the fibers used are made from short fibers spun together to a size of several tens of μm. The plate electrode (7) is made of stainless steel, and a magnet is installed on the back side to confine the plasma. Water is also run on the back side to cool it. The power source is a DC power source, and the positive side is grounded and the negative side is connected to the plate electrode. The negative electrode (16) is a stainless steel cylinder that is cooled by running water inside. The power source is a DC power supply, the positive side of which is grounded and the negative side is connected to the cylindrical electrode.
[0048] The light transmittance of the plastic film (2) laminated with the alumina layer was measured at around 365 nm using an optical thickness meter (17), and was controlled to the target light transmittance of 83%.
[0049] The laminated plastic film (2) was taken up by a take-up roll (18). A sample was taken from the take-up roll and observed from the alumina layer side with a differential interference microscope to confirm the presence or absence of discharge marks. The results are shown in Table 1.
[0050] Example 2 In Example 1, the distance between the tip of the conductive fabric blind and the plastic film was changed to 5 mm. The pressure between the conductive material and the plastic film was also changed as shown in Table 1. The presence or absence of discharge marks on the evaporated alumina transparent barrier film was confirmed.
[0051] [Table 1]
[0052] Comparative Example 1 Except for not introducing Ar gas into the static eliminator using a conductor, deposition was carried out under the same conditions as in Example 1. The presence or absence of discharge marks on the deposited alumina transparent barrier film was confirmed.
[0053] Comparative Example 2 In Example 1, the pressure between the conductor and the plastic film was changed as shown in Table 1. The presence or absence of discharge marks on the evaporated alumina transparent barrier film was confirmed.
[0054] Comparative Example 3 Deposition was carried out without installing a static eliminator using a conductor. To facilitate peeling of the plastic film from the coating roll, the discharge current of the static eliminator using a negative electrode was set to 0.65 A. The presence or absence of discharge marks on the deposited alumina transparent barrier film was confirmed. [Industrial Applicability]
[0055] The present invention makes it possible to provide a method for producing processed plastic films that includes a static elimination method that can easily eliminate static electricity when processing a plastic film by running it in a vacuum, and prevents damage to the plastic film due to discharge. [Explanation of symbols]
[0056] 1: Conductor 2: Plastic film 3: Roll 4: Nozzle 5: Wall 6: Vacuum chamber 7: Plate electrode 8: Wall 9: Unwinding roll 10: Guide roll 11: Coating roll 12: Crucible 13: Nozzle 14: Static electricity eliminator using conductive material 15: Static electricity eliminator using plate electrodes 16: Negative electrode 17: Optical thickness gauge 18: Winding roll 19: Electron gun
Claims
1. A method for producing processed plastic film, comprising the steps of: placing a conductor having a radius of curvature of 1 mm or less in the width direction of the plastic film near the plastic film as a method for reducing the amount of static electricity on a plastic film traveling in a vacuum; setting the closest distance between the plastic film surface and the conductor to 2 mm or more and 10 mm or less; maintaining the pressure between them at 8 Pa or more and 800 Pa or less; and performing static electricity removal using a static elimination method using a grounded conductor (Step 1).
2. The method for producing a processed plastic film as described in claim 1, further comprising the step (step 2) of connecting a negative potential or a high-frequency AC potential to the plate electrode, flowing a gas between the plate electrode and the plastic film to generate plasma, and installing a device for eliminating electricity using the generated plasma to eliminate electricity from the plastic film.
3. A method for producing a processed plastic film as described in claim 1 or 2, which includes a step of discharging electricity while the plastic film is running over a metal roll that is grounded and a metal roll that is installed on the opposite side of the plastic film from the side on which the conductor is installed, the metal roll being installed on the opposite side of the plastic film from the side on which the conductor is installed, and the plastic film being grounded.
4. A method for producing a processed plastic film, comprising the steps of providing a vapor deposition layer on a plastic film, comprising the steps of claim 1, 2 or 3.
Citation Information
Patent Citations
Production of metallic thin film
JP1987056567A
Vacuum film forming device
JP2000054151A
Static elimination method
JP2002367796A
Plastic film static eliminator and heating carrier device for plastic film
JP2009181938A
Method for manufacturing laminate
JP2013125205A