Resin-filled object and method of manufacturing same

The use of a magnetic field-induced heating method with a curable resin and magnetic powder addresses non-uniform curing and long curing times, achieving rapid, high-filling rate, and consistent hardness and insulation in narrow spaces within cylindrical objects like motor stators.

JP7574986B2Active Publication Date: 2024-10-29LG CHEM LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2021574908
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-02
Filing Date
2020-07-10
Publication Date
2024-10-29
Estimated Expiration
2040-07-10

AI Technical Summary

Technical Problem

Existing methods for curing curable resins face challenges such as non-uniform curing, long curing times, damage from excessive heat, and inconsistent thermal properties, particularly in narrow areas, leading to poor insulation and hardness properties.

Method used

A method involving a manufacturing apparatus with a solenoid coil that generates a magnetic field to induce heating, allowing for the use of a curable resin composition with magnetic powder to uniformly cure and fill narrow spaces within cylindrical objects, such as motor stators, by inductively heating the resin and magnetic powder.

Benefits of technology

The method achieves high filling rates with excellent hardness and insulation properties in narrow areas, ensuring rapid curing and maintaining consistent thermal properties, even in complex geometries like motor stators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574986000003
    Figure 0007574986000003
  • Figure 0007574986000004
    Figure 0007574986000004
  • Figure 0007574986000005
    Figure 0007574986000005
Patent Text Reader

Abstract

The present application relates to a method for producing a cured resin object. The method of the present application can rapidly produce a cured resin object having a high filling rate of a cured resin material with an excellent degree of cure even in a narrow internal space. The present application also relates to a cured resin object. The cured resin object of the present application can also have excellent voltage resistance properties.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Cross-reference to related applications This application claims the benefit of priority based on Korean Patent Application No. 10-2019-0083975 filed on July 11, 2019, Korean Patent Application No. 10-2019-0158213 filed on December 2, 2019, and Korean Patent Application No. 10-2019-0158214 filed on December 2, 2019, and all contents disclosed in the documents of the relevant Korean patent applications are incorporated herein by reference.

[0002] Technical Field FIELD OF THE DISCLOSURE This application relates to resin-filled bodies and methods of making same. [Background technology]

[0003] Curable resins can be used in a variety of applications. For example, curable resins can be used to form various adhesives and pressure sensitive adhesives, inks for 3D printing, or engineering plastics. Curable resins can also be used to form insulating materials such as insulating coating liquids, bearings, insulating coatings for motors, or insulating sealants. In addition, curable resins can also be used for insulation of transformers, generators, alternators, and the like.

[0004] Among hardening resins, a so-called thermosetting resin, which is hardened by heat, is hardened, for example, by applying heat from the outside, for example, by using hot air or a hot plate.

[0005] However, in the case of the above method, since the external heat cannot be sufficiently transferred to the inside of the composition, there is a problem that uneven curing is induced, and if an excessive amount of heat is required for complete curing, the resin may be damaged. In addition, the above method has a problem that the curing time is very long. In order to solve the problems of the above method, a method of applying heat at a relatively low temperature has been considered, but there is a problem that the material is not cured sufficiently and hardens naturally during storage or transportation, and the physical properties (e.g., insulating properties and heat resistance properties) are not maintained constant. In order to solve the problems of the above method, a method of enlarging the size of the heat application equipment has been considered, but the cost increases in the process of enlarging the equipment, and the curing efficiency is still poor compared to the enlarged size.

[0006] Therefore, a method of curing the curable resin by irradiating it with light such as ultraviolet light has been considered. Although this method allows for fast curing, the curing occurs smoothly only on the outside, which leads to uneven curing of the resin and leaves the curable resin inside. Therefore, this method still has the problem of requiring additional heat treatment.

[0007] In addition, a method has been considered in which a curable resin is applied onto a metal substrate, and an electromagnetic field is applied to the metal substrate to inductively heat the metal substrate. However, this method has problems in that it is difficult to control the degree of heating, and when two or more types of metal substrates are used, thermal conduction, expansion or contraction is induced between the metal substrates, and there is a large difference in the degree of curing of the resin between the portion adjacent to the substrate and the portion separated from the substrate.

[0008] Also, a method of curing the curable resin by irradiating it with infrared rays has been considered, but this method still cannot solve the problems associated with the above-mentioned method of applying hot air or a hot plate. Summary of the Invention [Problem to be solved by the invention]

[0009] The present application aims to provide a method capable of filling a filling portion having a small area with a hardenable resin at a high filling rate.

[0010] The present application aims to provide a method for filling a resin so that the resin has excellent hardness and excellent insulating properties even in a small area of ​​the filling portion.

[0011] The present application seeks to provide a method by which said filling can proceed within a fast time.

[0012] The present application seeks to provide a resin-filled object having excellent hardness and insulating properties even in a small area of ​​the filled portion, and having a resin filled at an excellent filling rate. [Means for solving the problem]

[0013] One aspect of the present application relates to a method for producing a resin-filled object. The resin-filled object includes an object having at least a filling space and a resin component filled in the filling space of the object. As described below, in the method of the present application, a curable resin can be used as the resin, so that the resin component in the resin-filled object can mean a resin in a cured state.

[0014] In the method of the present application, a manufacturing apparatus is used to manufacture a resin-filled object. Specifically, in the method of the present application, a manufacturing apparatus is used that includes a cylindrical object (see FIG. 1). The cylindrical object 10 includes at least a through space 2 and an edge portion 1. Specifically, in the cylindrical object, the through space is formed in the longitudinal direction. The edge portion has at least one slot 3 therein. Also, the slot is formed inside the edge portion in the longitudinal direction. The resin-filled object manufactured by the method of the present application includes a resin component filled in the slot.

[0015] In this application, the machine direction of a member may refer to the direction of the longest length among the directions of a plane parallel to the plane having the largest area of ​​the member, the transverse direction of a member may refer to the direction perpendicular to the machine direction within the plane direction, and the thickness direction of a member may refer to the normal direction of the plane formed by the axes of the machine direction and the transverse direction.

[0016] Among the terms defining angles in this application, vertical, parallel, orthogonal, horizontal, etc., mean substantially vertical, parallel, orthogonal, or horizontal within a range that does not impair the intended effect, and the range of vertical, parallel, orthogonal, or horizontal includes errors such as manufacturing errors or variations. For example, in each of the above cases, an error within about ±15 degrees, an error within about ±10 degrees, or an error within about ±5 degrees may be included.

[0017] As an example, the cross-sectional shape of the edge is not particularly limited, and may be, for example, a ring shape (circle), an ellipse, a polygon with more than one side, or an amorphous shape (as shown in FIG. 2). On the other hand, when considering the transmission efficiency of the magnetic field generated by the solenoid coil described later, it is appropriate that the shape is a ring shape (as shown in FIG. 2). In the above, the cross-sectional shape of the edge may refer to the shape of a cross section in the width direction of the cylindrical object (a cross section obtained when the cylindrical object is cut along any one direction perpendicular to the longitudinal direction).

[0018] The size of the cylindrical object is not particularly limited. For example, when the cross-sectional shape of the edge of the cylindrical object is ring-shaped, the inner diameter may be within a range of 50 mm to 150 mm. When the cross-sectional shape of the edge of the cylindrical object is ring-shaped, the outer diameter may be within a range of 100 mm to 250 mm (naturally, the outer diameter is larger than the inner diameter). When the cross-sectional shape of the edge of the cylindrical object is ring-shaped, the length may be within a range of 60 mm to 200 mm. When the cross-sectional shape of the edge of the cylindrical object is ring-shaped, the length of the through space may be shortened in the direction toward the center of the cylindrical object, and in this case, the length range may be within a range of 50 mm to 200 mm.

[0019] In one example, the manufacturing apparatus may further include a means for fixing, transporting, or rotating the cylindrical object together with the cylindrical object. The configuration of the means is not particularly limited, and various materials or shapes that can realize the above-mentioned functions may be applied. By providing the means, the magnetic field described below may be applied uniformly. In particular, the means for rotating the cylindrical object has the advantage that, when a precursor of a resin cured product, such as a resin composition, is in a liquid state, the composition may be prevented from flowing out of the slot into which it is injected through rotation.

[0020] The manufacturing apparatus further includes a solenoid coil together with the cylindrical object. The solenoid coil is formed so as to be inserted into the cylindrical through-space and generate a magnetic field. In the present application, a solenoid coil having a generally known shape can be applied. For example, the solenoid coil may be a coil in the form of a cylindrically wound conductor made of copper or the like, or a coil in the form of a cylindrical rod made of a ferromagnetic metal wound with a conductor. The cylindrical object can be inductively heated by the magnetic field formed by the solenoid coil. In addition, as described later, when a component containing a magnetic powder, such as the resin composition applied in the method of the present application, is injected into the slot of the cylindrical object, the magnetic field formed by the solenoid coil can also inductively heat the magnetic powder.

[0021] The manufacturing apparatus of the present application may include a magnetic field generator configured to apply an alternating current to the solenoid coil together with the cylindrical object, i.e., the alternating current applied by the magnetic field generator enables the solenoid coil to generate a magnetic field, and the magnetic field thus generated can inductively heat the cylindrical object, and in some cases the cylindrical object and the magnetic powder in the resin composition.

[0022] In the present application, as the device configuration such as the fixing means, any element known in the art that can embody the function can be applied as it is.

[0023] The manufacturing apparatus of the present application may further include other known means necessary for the configuration of the apparatus in addition to the above-mentioned means, the solenoid coil, and the magnetic field generator. Examples of the other means include a temperature control unit that detects the temperature inside the cylindrical object or the through-space, a resin supply unit that supplies a hardening resin or the like to the slot, and an integrated control unit that detects and controls the overall drive.

[0024] The method of the present application includes a step of introducing (or injecting) a resin composition into the cylindrical object. Specifically, the method includes a step of introducing a resin composition into the slot of the cylindrical object. The resin composition includes a resin and a magnetic powder. The method of the present application also includes a step of inserting a solenoid coil into the through space of the cylindrical object in which the resin composition has been introduced into the slot. The method of the present application then includes a step of generating a magnetic field with the solenoid coil inserted into the through space, and hardening the resin in the composition. Specifically, the cylindrical object can be inductively heated by the magnetic field generated by the solenoid coil. In addition, the magnetic field can also generate heat in the magnetic powder of the resin composition, so that the resin can be hardened using the heat. The magnetic powder does not generate heat due to so-called eddy current or hysteresis loss, and the hysteresis loss of the powder itself is small, and only a saturation magnetization value is substantially present, so that it can be designed to generate vibration heat. Specifically, when a magnetic field is applied as described above, the magnetic powder vibrates due to its coercive force, and as a result, heat can be released.

[0025] The resin composition supplied to the slot of the cylindrical object includes at least a resin and a magnetic powder. The resin may be a curable resin. Thus, the composition supplied to the slot may be a curable resin composition. The curable resin means a resin that can be cured by application of heat or irradiation of light. The magnetic powder means fine particles that can vibrate and generate Joule heat when a magnetic field is applied. That is, the magnetic powder can generate heat by the magnetic field generated by the solenoid coil. The resin can be cured by the heat generated by the magnetic powder to fill the slot of the cylindrical object.

[0026] Normally, a slot in a cylindrical object has a small area, and therefore the internal space is also small. However, in the manufacturing method of the present application, the above-mentioned device is used, and the magnetic field applied by the device is used to harden and fill the resin in the slot, so that the resin can be filled with an excellent filling rate even in the narrow slot.

[0027] In one example, the resin composition, specifically the resin therein, can be cured by applying a magnetic field within a predetermined range to the cylindrical object and the resin composition by the solenoid coil. The magnetic field applied in the resin composition curing step may be a magnetic field generated by an alternating current applied to a solenoid coil by a magnetic field generator described below.

[0028] In the method of the present application, the conditions for curing the resin composition are not particularly limited, and can be appropriately adjusted so that the resin composition can be cured within a short time to form a resin-filled object having an excellent resin filling rate and degree of curing, as described below, and excellent heat transfer properties, etc.

[0029] For example, the resin composition can be cured by applying a current of 100 A or more. In other examples, the current may be about 105 A or more, 110 A or more, 115 A or more, 120 A or more, or 125 A or more, and the upper limit is not particularly limited and may be appropriately adjusted as long as the resin is not overheated, and may be, for example, 500 A or less, 400 A or less, 350 A or less, 300 A or less, 250 A or less, 200 A or less, or 150 A or less.

[0030] In addition, the curing of the resin composition can be performed with an output of 5000 W or more. The output may refer to the output of a magnetic field generating device described later. In other examples, the output may be 5500 W or more, 6000 W or more, 6500 W or more, 7000 W or more, 7500 W or more, or 8000 W or more, and the upper limit is not particularly limited and may be appropriately adjusted as long as the resin is not overheated, and may be, for example, 10000 W or less, 9500 W or less, 9000 W or less, or 8500 W or less.

[0031] In one example, the resin composition can be cured by applying a current at a frequency in the range of 100 kHz to 1000 kHz. The frequency may be 110 kHz or more, 120 kHz or more, 130 kHz or more, 140 kHz or more, or 150 kHz or more, and may be 950 kHz or less, 900 kHz or less, 850 kHz or less, 800 kHz or less, 750 kHz or less, 700 kHz or less, 650 kHz or less, or 600 kHz or less.

[0032] In one example, the curing of the resin composition can be performed within 30 minutes. That is, the method of the present application can quickly produce the resin-filled object by applying the above-mentioned manufacturing apparatus and resin composition. In another example, the curing time can be 25 minutes or less, 20 minutes or less, 15 minutes or less, or 10 minutes or less, and the lower limit is not particularly limited, and the lower the value, the better, but it can be, for example, 10 seconds or more, 20 seconds or more, 30 seconds or more, 40 seconds or more, 50 seconds or more, or 60 seconds or more.

[0033] The method for producing a resin-filled object of the present application may further include a preheating step of preheating the cylindrical object before introducing the resin composition into the slot. The preheating may be performed by generating a magnetic field with a solenoid coil inserted into the through-space of the cylindrical object. The magnetic field thus applied may inductively heat the cylindrical object, thereby allowing the resin composition to be more efficiently introduced into the slot of the heated cylindrical object. Specifically, the inductively heated cylindrical object may reduce the viscosity of the resin composition, allowing the composition to be more efficiently filled into the slot.

[0034] In one example, the preheating is performed to ensure the fluidity of the resin composition so that the composition can be filled more smoothly into the slot, so it is preferable that a magnetic field of lower strength is applied than the magnetic field applied to harden the resin.

[0035] For example, the temperature in the preheating step, specifically, the temperature of the cylindrical object in the preheating step, may be lower than the curing start temperature of the resin composition. In the present application, a thermosetting resin that is cured by application of heat may be applied, and since the curing reaction of such a resin is usually an exothermic reaction, the curing start temperature of the resin composition may mean a temperature at which an exothermic reaction is observed when the resin composition is heated and cured. The curing start temperature may be measured using a known measuring device, for example, a differential scanning calorimetry (DSC) device. Specifically, the curing start temperature of the resin composition may mean a temperature at which an exothermic reaction is observed when the resin composition is injected into a differential scanning calorimeter and heated from a temperature of 25° C. to a temperature of 300° C. at a heating rate of 10° C. / min.

[0036] As described above, the preheating step may be performed to reduce the viscosity of the resin composition so that the composition can be better filled in the slots. However, in order to maintain a proper mixture of the resin and magnetic powder in the composition, the viscosity of the composition must also be properly adjusted. Therefore, in the method of the present application, the preheating of the cylindrical object may be performed by adjusting the temperature of the cylindrical object so that the viscosity of the resin composition at that temperature is maintained at more than 1 / 100 of the viscosity at room temperature. The viscosity may be, for example, at a shear ratio of 100s -1 The measurement can be performed using known measuring equipment under the above conditions.

[0037] In the present application, the term "room temperature" may mean a natural temperature without any particular heating or cooling, for example, a temperature within a range of about 20°C to 30°C, about 23°C, or about 25°C.

[0038] The preheating step is performed to more smoothly supply the resin composition into the slot, and is not performed to promote curing of the composition, and therefore may be performed by applying a magnetic field having a lower strength than the magnetic field applied in the curing step of the composition.

[0039] For example, the preheating can be performed by applying a current of less than 100 A. In other examples, the current may be 99 A or less, 98 A or less, 97 A or less, 96 A or less, or 95 A or less, and the lower limit is not particularly limited, and it is sufficient as long as the current is at least sufficient to heat the cylindrical object, and may be, for example, 50 A or more, 60 A or more, 70 A or more, 80 A or more, 85 A or more, or 90 A or more.

[0040] Also, the preheating can be performed with an output of less than 5000 W. The output may refer to the output of a magnetic field generating device described later. In other examples, the output may be 4950 W or less, 4900 W or less, 4850 W or less, 4800 W or less, 4750 W or less, 4700 W or less, 4650 W or less, 4600 W or less, 4550 W or less, or 4500 W or less, and the lower limit is not particularly limited and may be appropriately adjusted to at least the output level at which the cylindrical object can be heated, for example, 1000 W or more, 1500 W or more, 2000 W or more, 2500 W or more, 3000 W or more, 3500 W or more, or 4000 W or more.

[0041] In one example, the preheating can also be performed by applying a current with a frequency in the range of 100 kHz to 1000 kHz. The frequency may be 110 kHz or more, 120 kHz or more, 130 kHz or more, 140 kHz or more, or 150 kHz or more, or 950 kHz or less, 900 kHz or less, 850 kHz or less, 800 kHz or less, 750 kHz or less, 700 kHz or less, 650 kHz or less, or 600 kHz or less.

[0042] In one example, the preheating is performed to appropriately reduce the viscosity of the resin composition, and it is sufficient to perform the preheating to a degree that ensures the above-mentioned degree of viscosity. Therefore, the preheating (preheating of the cylindrical object) may be performed within a time shorter than the curing (curing of the resin composition, specifically, the resin in the composition). For example, the preheating may be performed for a time of 10 minutes or less. In another example, the preheating time may be 9 minutes or less, 8 minutes or less, 7 minutes or less, 6 minutes or less, 5 minutes or less, 4 minutes or less, 3 minutes or less, 2 minutes or less, or 1 minute or less, and the lower limit is not particularly limited, and may be, for example, 10 seconds or more, 20 seconds or more, 30 seconds or more, 40 seconds or more, or 50 seconds or more.

[0043] In this manner, in the present application, the resin composition can be introduced after the cylindrical object is heated. However, in the method of the present application, the introduction of the composition can also proceed while a magnetic field is generated by the solenoid coil. In this manner, when the introduction of the composition is also performed while the magnetic field is generated, the composition can be introduced while the temperature in the preheating step is maintained. As a result, the resin composition can be filled more smoothly into the slot. That is, when the resin composition is introduced by generating a magnetic field from a solenoid coil and heating the cylindrical object to a predetermined temperature, the temperature of the cylindrical object during the process may be within a range of ±10°C or less, ±5°C or less, ±3°C or less, or ±1°C or less based on the temperature in the preheating step.

[0044] When the introduction of the resin composition is performed together with the application of a magnetic field, the conditions for applying the magnetic field are not particularly limited and can be appropriately adjusted within the range that maintains the temperature of the cylindrical object in the preheating step within the above-mentioned range. For example, the preheating step can be performed by applying a magnetic field of lower strength for a predetermined time.

[0045] In one embodiment, the resin composition is introduced by applying a current of less than 50 A. The current may be 45 A or less, 40 A or less, or 35 A or less, and the lower limit is not particularly limited as long as the current is at least capable of maintaining the temperature of the preheated cylindrical object, and may be, for example, 10 A or more, 15 A or more, 20 A or more, 25 A or more, or 30 A or more.

[0046] In one example, the introduction of the resin composition can be performed at an output of 500 W or less. The output may refer to the output of a magnetic field generating device described later. In other examples, the output may be 450 W or less, 400 W or less, 350 W or less, 300 W or less, or 250 W or less, and the lower limit is not particularly limited, and may be, for example, 100 W or more, 150 W or more, 200 W or more, 210 W or more, 220 W or more, or 230 W or more.

[0047] In one example, the introduction of the resin composition can be performed by applying a current at a frequency in the range of 100 kHz to 1000 kHz. The frequency may be 110 kHz or more, 120 kHz or more, 130 kHz or more, 140 kHz or more, or 150 kHz or more, or 950 kHz or less, 900 kHz or less, 850 kHz or less, 800 kHz or less, 750 kHz or less, 700 kHz or less, 650 kHz or less, or 600 kHz or less.

[0048] When applying a magnetic field when introducing the resin composition, the application time of the magnetic field is not particularly limited as long as the temperature in the preheating step can be maintained. For example, the application time of the magnetic field can be 10 minutes or less. In addition, the application time of the magnetic field may be 9 minutes or less, 8 minutes or less, 7 minutes or less, 6 minutes or less, 5 minutes or less, 4 minutes or less, 3 minutes or less, 2 minutes or less, or 1 minute or less, and the lower limit is not particularly limited, and may be, for example, 10 seconds or more, 20 seconds or more, 30 seconds or more, 40 seconds or more, or 50 seconds or more.

[0049] The manufacturing method of the present application may further include a step of maintaining the temperature at the time of curing even after the resin composition is cured (hereinafter, sometimes referred to as an additional temperature maintaining step). That is, by generating a magnetic field of appropriate strength by the solenoid coil for a predetermined time even after the resin composition is cured, the temperature at the time of curing of the resin composition is maintained, so that the resin component that does not fill the slot and remains uncured can be additionally cured. Such an additional curing step may be performed multiple times, whereby the uncured resin component may be additionally cured and the degree of curing of the resin in the slot may be improved.

[0050] In one example, the additional temperature maintaining step can be performed by applying a current of less than 50 A. In another example, the current can be 45 A or less, and the lower limit is not particularly limited as long as the current is at least capable of maintaining the temperature of the preheated cylindrical object, and can be, for example, 10 A or more, 15 A or more, 20 A or more, 25 A or more, or 30 A or more.

[0051] In one example, the additional temperature maintaining step can be performed at an output of 1000 W or less. The output may refer to the output of a magnetic field generating device described below. In other examples, the output may be 950 W or less, 900 W or less, 850 W or less, 800 W or less, 750 W or less, 700 W or less, 650 W or less, 600 W or less, 550 W or less, or 500 W or less, or may be 100 W or more, 150 W or more, 200 W or more, 210 W or more, 220 W or more, or 230 W or more.

[0052] In one embodiment of the method of the present application, the additional temperature maintenance may also be performed by applying a current at a frequency in the range of 100 kHz to 1000 kHz. The frequency may be 110 kHz or more, 120 kHz or more, 130 kHz or more, 140 kHz or more, or 150 kHz or more, or may be 950 kHz or less, 900 kHz or less, 850 kHz or less, 800 kHz or less, 750 kHz or less, 700 kHz or less, 650 kHz or less, or 600 kHz or less.

[0053] The time for which the additional temperature maintaining step is performed is not particularly limited as long as it is a time during which the temperature in the curing step can be maintained. For example, the time during which the temperature can be maintained may be 10 minutes or less. In addition, the time during which the temperature can be maintained may be, for example, 9 minutes or less, 8 minutes or less, 7 minutes or less, 6 minutes or less, 5 minutes or less, 4 minutes or less, 3 minutes or less, 2 minutes or less, or 1 minute or less, and the lower limit is not particularly limited, and may be, for example, 10 seconds or more, 20 seconds or more, 30 seconds or more, 40 seconds or more, or 50 seconds or more.

[0054] In one example, the method of introducing the resin composition into the slot is not particularly limited. For example, the resin composition may be introduced into the slot by a liquid dipping method, a solid phase dipping method, or a trickling method. In the above, the liquid dipping method may mean a method of immersing a cylindrical object (including a preheated object) in a liquid resin composition and then removing it after a predetermined time has elapsed. In addition, the solid phase dipping method may mean a method of immersing the cylindrical object (including a preheated object) in a solid resin, for example, a tube containing the powder when the resin is in powder form, so that a curable resin is introduced into the slot. In addition, the trickling method may mean a method of injecting a certain amount of the resin composition into the slot using a known injection device such as a dispenser onto the rotating cylindrical object while rotating the cylindrical object.

[0055] As described above, the magnetic field generated from the solenoid coil may be generated by applying an alternating current to the solenoid coil using a magnetic field generating device.

[0056] In the manufacturing method of a resin-filled object of the present application, a resin composition is injected into the above-mentioned slot, an alternating current is applied to the solenoid coil by a magnetic field generating device, and the magnetic field generated by the solenoid coil induces heating of the cylindrical object and the magnetic powder contained in the resin composition, and the resin composition can be hardened by the heating, so that the slot can be filled with resin, specifically a hardened resin.

[0057] The resin composition may contain at least a curable (=curable) resin as described above. In addition, since the device of the present application can at least cure the resin by heating, it is appropriate to apply a thermosetting resin as the curable resin.

[0058] Meanwhile, since the method of the present application is particularly suitable for insulating an object, the resin of the resin composition injected into the slot may be an insulating resin. In the above, "insulating" means a property of not conducting electricity, as is well known.

[0059] As an example, the thermosetting resin is not particularly limited in type as long as it can be cured by application of heat, and examples thereof include polysilicon resins; imide-based resins such as polyetherimide, polyimide, and polyesterimide; polyurethane-based resins; isocyanate-based resins; acrylic-based resins; polyester-based resins; phthalonitrile-based resins; and polyolefin-based resins.

[0060] The phase of the thermosetting resin is not particularly limited. For example, the thermosetting resin may be a solid, semi-solid, or liquid resin.

[0061] In addition, the resin composition may contain a resin, specifically, a thermosetting resin, as a main component. In the present application, when a composition contains a certain component as a main component, the content of the component may be 50 wt% or more, 55 wt% or more, 60 wt% or more, 65 wt% or more, 70 wt% or more, 75 wt% or more, 80 wt% or more, 85 wt% or more, 90 wt% or more, or 95 wt% or more based on the total weight of the composition, and the upper limit is not particularly limited, and may be, for example, less than 100 wt%, 99 wt% or less, 98 wt% or less, or 97 wt% or less.

[0062] In the manufacturing apparatus of the present application, the resin, specifically, the thermosetting resin, is cured by heat generated by the magnetic field generated by the magnetic field generator and the solenoid coil. At this time, if the curable resin composition containing the resin and the cured resin formed therefrom contain magnetic powder, it is possible to manufacture a resin-filled object in which a large number of slots having a small area and narrow space are more effectively filled, as described above.

[0063] As the magnetic powder, any known component capable of generating vibrational heat by the magnetic field can be used without limitation. Specifically, the magnetic powder can be selected in consideration of the properties of the resin-filled object (e.g., insulation, voltage resistance, degree of hardening, or filling rate) that are to be obtained by dispersing the magnetic powder in the resin composition with an appropriate degree of dispersion.

[0064] In this application, the terms "crystal," "magnetic particle," "magnetic material," and "magnetic powder" are used to describe a substance that can generate heat by application of an electromagnetic field. Below, we will first define their meanings and then provide a specific explanation.

[0065] In this application, the term "magnetic particles" may refer to particles in the form of aggregated "crystals" that exhibit magnetism. In addition, the term "magnetic material" is used to distinguish the magnetic particles from additional components (e.g., surface treatment agents) when the magnetic particles are present together. In one example, an object including magnetic particles and a surface treatment agent introduced on the surface of the particles may be referred to as a magnetic material. In addition, "magnetic powder" may refer to a state in which one or more magnetic materials are mixed together.

[0066] That is, the resin composition applied in the present application includes a resin and a magnetic powder, and in one example, the magnetic powder includes one or more magnetic materials, the magnetic materials may include magnetic particles and a surface treatment agent introduced onto the surfaces of the magnetic particles, and the magnetic particles may have a morphology in which a plurality of crystals are aggregated.

[0067] As the magnetic particles, it may be advantageous to select multi-domain magnetic particles in which a plurality of crystals, specifically, two or more magnetic domains, are formed. In such magnetic particles, the magnetic domains are randomly arranged when there is no external magnetic field, and when an external magnetic field is applied, the magnetic particles may be magnetized according to the direction of the applied magnetic field. The magnetic domains being randomly arranged may mean that the magnetic directions of the magnetic domains are different and not aligned, and in this case, the net value of the magnetic domains may be substantially close to 0, and thus there may be no magnetism. When an external electromagnetic field is applied, the magnetic directions of the magnetic domains are aligned, and magnetization may occur. Such magnetic particles may be, but are not limited to, super-paramagnetic particles.

[0068] Whether or not a magnetic particle has multi-domains can usually be confirmed through the particle size of the magnetic particle.

[0069] For example, the particle diameter D of the magnetic particles satisfies the following formula 1. sWhen the magnetic particles have a particle size of this size or larger, the magnetic particles can be determined to have multi-domains.

[0070] [Formula 1]

number

[0071] In formula 1, μ0 is the magnetic permeability constant in vacuum (1.26X -6 H / m), Ms is the saturation magnetization of the magnetic particle (units: A / m or emu / g), A is the exchange stiffness of the magnetic particle (units: J / m), and a is the lattice constant of the magnetic particle (units: m).

[0072] In Equation 1, the variables other than the magnetic permeability constant under vacuum, i.e., the saturation magnetization, exchange hardness, and lattice constant of the magnetic particles, vary depending on the type of the magnetic particles. Therefore, after confirming each value for the magnetic particles to be applied, the D s By controlling the size of the magnetic particles as described above, magnetic particles having multi-domains can be formed.

[0073] Generally, D calculated by the above formula s From the above, the magnetic particles are multi-domained, and therefore, the magnetic particles applied in the present application have a particle size D s The magnetic particles may have a particle size of D or more. There is no particular upper limit to the particle size of the magnetic particles. s If the diameter exceeds this range, the coercivity of the magnetic particles tends to decrease, but the magnetic particles used in the present application can have a particle diameter within a range that allows them to have the coercivity described below.

[0074] When the magnetic particles described above are used, the particles behave similarly to a non-magnetic state in the absence of an external magnetic field, and therefore can exist in a uniformly dispersed state without agglomeration within the composition.

[0075] The magnetic particles do not generate heat due to so-called eddy current or hysteresis loss, but have a small hysteresis loss and only a saturation magnetization value, so that they can be selected to generate vibration heat. For example, the magnetic particles can be selected to generate heat by vibrating due to the coercive force of the magnetic particles when an external electromagnetic field is applied.

[0076] As described above, the magnetic particles may include two or more magnetic domains. The term "magnetic domain" generally refers to regions inside a magnetic particle that are divided so that the directions of magnetization are different from each other. In the present application, the magnetic particles having two or more magnetic domains are strongly magnetized by an external AC magnetic field to generate vibration heat, and when the magnetic field is removed, the magnetic domains return to their original state, thereby providing magnetic particles with low residual magnetization of hysteresis loss.

[0077] In one example, the magnetic particles may have a coercive force in the range of 1 kOe to 200 kOe, 10 kOe to 150 kOe, 20 kOe to 120 kOe, 30 kOe to 100 kOe, 40 kOe to 95 kOe, or 50 kOe to 95 kOe. In other examples, the coercive force may be about 10 kOe or more, 15 kOe or more, 20 kOe or more, 25 kOe or more, 30 kOe or more, 35 kOe or more, 40 kOe or more, 45 kOe or more, 50 kOe or more, 55 kOe or more, 60 kOe or more, 65 kOe or more, 70 kOe or more, 75 kOe or more, 80 kOe or more, 85 kOe or more, or 90 kOe or more, or about 190 kOe or less, 180 kOe or less, 170 kOe or less, 160 kOe or less, 150 kOe or less, 140 kOe or less, 130 kOe or less, 120 kOe or less, 110 kOe or less, or 100 kOe or less. The term "coercive force" may refer to the strength of a critical magnetic field required to reduce the magnetization of a magnetic particle to zero. Magnetic particles magnetized by an external magnetic field maintain a certain level of magnetization even after the magnetic field is removed, and the strength of the magnetic field that can reduce the magnetization to 0 by applying a magnetic field in the opposite direction to such magnetized magnetic particles is called coercivity. The coercivity of magnetic particles can be a criterion for distinguishing soft magnetic particles from hard magnetic particles, and the magnetic particles of the present application may be soft magnetic particles. In the present application, the coercivity of the magnetic particles is controlled within the above range to more easily realize magnetic conversion of the magnetic particles, and the vibration heat of the present application is generated to the extent desired in the present application, thereby satisfying the desired curing properties through uniform curing of the resin.

[0078] In one example, the magnetic particles may have a saturation magnetization value at room temperature in the range of 20 emu / g to 150 emu / g, 30 emu / g to 130 emu / g, 40 emu / g to 100 emu / g, 50 emu / g to 90 emu / g, or 60 emu / g to 85 emu / g. In another example, the saturation magnetization value may be about 20 emu / g or more, 30 emu / g or more, 40 emu / g or more, 50 emu / g or more, 60 emu / g or more, 70 emu / g or more, or 75 emu / g or more, or about 150 emu / g or less, 140 emu / g or less, 130 emu / g or less, 120 emu / g or less, 110 emu / g or less, 100 emu / g or less, or 90 emu / g or less. In this application, the saturation magnetization value of the magnetic particles can be controlled relatively large, and heat is generated by vibration between the magnetic particles, not eddy current, and the resin can be cured uniformly to satisfy the curing properties. In this application, the physical properties of the magnetic particles can be measured by VSM (Vibrating Sample Magnetometer). VSM is a device that records the applied magnetic field by Hall probe, and records the electromotive force obtained when the sample is vibrated according to Faraday's law to measure the magnetization value of the sample. Faraday's law shows that if the north pole of a bar magnet is pushed toward the coil so that it faces the coil, the galvanometer moves and a current flows in the coil. The current that appears as a result of this is called induced current, and is said to be created by induced electromotive force. VSM is a method that detects the induced electromotive force generated when the sample is vibrated according to this basic operating principle with a search coil, and measures the magnetization value of the sample based on this electromotive force. It can easily measure the magnetic properties of materials as a function of magnetic field, temperature, and time, and is capable of fast measurements of magnetic forces up to 2 Tesla and temperatures ranging from 2K to 1273K.

[0079] The above-mentioned properties such as coercivity and saturation magnetization can be adjusted according to the properties related to the particle size of the magnetic particles. Specifically, when the magnetic particles have the crystal size described below and the average particle size described below, the magnetic body and magnetic powder using the magnetic particles can exhibit the above-mentioned magnetic properties such as coercivity and saturation magnetization.

[0080] In one example, the average particle size of the magnetic particles may be within a range of 20 nm to 300 nm. In another example, the average particle size may be within a range of 30 nm to 250 nm, 40 nm to 230 nm, or 45 nm to 220 nm. In another example, the average particle size of the magnetic particles may be approximately 30 nm or more, 40 nm or more, 50 nm or more, 60 nm or more, 70 nm or more, 80 nm or more, 90 nm or more, or 95 nm or more, or 290 nm or less, 280 nm or less, 270 nm or less, 260 nm or less, 250 nm or less, 240 nm or less, 230 nm or less, 220 nm or less, 210 nm or less, 200 nm or less, 190 nm or less, 180 nm or less, 170 nm or less, 160 nm or less, 150 nm or less, 140 nm or less, 130 nm or less, 120 nm or less, or 110 nm or less.

[0081] The magnetic domains of the magnetic particles, specifically the average size of the crystals that the magnetic particles have, may be within a range of 10 nm to 50 nm, or 20 nm to 30 nm.

[0082] In the present application, by applying a magnetic powder that satisfies the above range of particle size or size, heat capable of uniformly curing the resin in the composition can be generated. In the present application, by controlling the average size of the magnetic particles to 20 nm or more, sufficient vibration heat can be generated during curing through low coercivity and multiple magnetic domains, and by controlling the average size to 300 nm or less, the hysteresis loss of the magnetic particles themselves can be reduced and only the saturation magnetization value can be present, thereby realizing uniform and stable curing.

[0083] In addition, in the present application, from the viewpoint of realizing the above-mentioned characteristics such as coercivity and saturation magnetization value, the coefficient of variation of the particle size of the magnetic particles may be adjusted to be within a specific range. Specifically, the coefficient of variation of the particle size of the magnetic particles may be within a range of 5% to 30%. In the above, the coefficient of variation of a certain factor may mean a ratio of the standard deviation of the factor to the average of the factor, expressed as a percentage. That is, in the magnetic powder, the ratio of the standard deviation of the particle size of the magnetic particles to the average of the particle size of the magnetic particles may be within a range of 5% to 30%. The coefficient of variation may be estimated through an electron microscope photograph obtained for the magnetic material or the magnetic powder containing the magnetic material.

[0084] The magnetic particles of the present application are not particularly limited in material as long as they can generate heat through electromagnetic induction heating. In one example, the magnetic particles may be particles represented by the following chemical formula 1:

[0085] [Chemical formula 1] MX a O b

[0086] In Formula 1, M is a metal or metal oxide, and X is Fe, Mn, Co, Ni, or Zn, satisfying |aXc|=|bXd|, where c is the cation charge of X, and d is the anion charge of oxygen. In one example, M may be Fe, Mn, Mg, Ca, Zn, Cu, Co, Sr, Si, Ni, Ba, Cs, K, Ra, Rb, Be, Li, Y, B, or an oxide thereof. For example, X a O b is Fe2O3, c may be +3 and d may be -2. a O b is Fe3O4, it can be expressed as FeOFe2O3, so that c can be +2 and +3, respectively, and d can be -2. The magnetic particles of the present application are not particularly limited as long as they satisfy the above Chemical Formula 1, and may be, for example, MFe2O3.

[0087] In one example, the composition of the present application may contain, as magnetic particles, the compound of Chemical Formula 1 alone, a mixture of compounds of Chemical Formula 1, or a compound in which an inorganic substance is doped into the compound of Chemical Formula 1. The inorganic substance may contain monovalent to trivalent cationic metals or oxides thereof, and two or more types of cationic metals may be used.

[0088] In one example, the magnetic particles may be present in the form of magnetic particle thrusts within the magnetic body, which prevents aggregation between the magnetic particles and improves dispersibility, thereby allowing the resin to be effectively cured by vibration heat.

[0089] If necessary, the magnetic particles may be surface-treated with a suitable surface treatment agent within the magnetic body.

[0090] As one example, the ratio of the magnetic material in the resin composition is not particularly limited, and can be appropriately adjusted within a range that can ensure an appropriate degree of curing or filling rate of the resin cured product. The ratio may be, for example, within a range of 1 part by weight to 30 parts by weight relative to 100 parts by weight of the curable resin. As another example, the ratio may be 2 parts by weight or more, 3 parts by weight or more, 4 parts by weight or more, or 5 parts by weight or more, and may be 25 parts by weight or less, 20 parts by weight or less, 15 parts by weight or less, or 10 parts by weight or less.

[0091] The cylindrical object of the manufacturing apparatus used in the manufacturing method of the resin-filled object of the present application can be an apparatus generally known as a motor stator. That is, in the present application, a resin-filled object in which the slots of a motor stator are filled with a cured resin can be manufactured.

[0092] As mentioned above, a motor is a device that can obtain a rotational force from electric energy. For example, the motor can include a so-called stator and a rotor, and the stator can be applied to the cylindrical object, and the cross-sectional shape of the stator can be a ring shape. Here, the rotor is configured to electromagnetically interact with the stator and can rotate by the force acting between the magnetic field and the current flowing in the coil.

[0093] As in the case of the cylindrical object, the stator may have a number of slots. A wire is wound in the slots, and each wire is connected to a lead wire to receive power. Known examples of the wire wound in the slots include a general winding type wire and a hairpin winding type wire.

[0094] The general winding method involves winding a number of relatively thin wires into slots, which creates less skin effect at high speeds. The hairpin winding method involves inserting a relatively thick wire into a slot. With the hairpin winding method, there is no wasted space between the coils, which maximizes the space factor, and therefore reduces resistance and can be expected to improve output.

[0095] Therefore, the resin-filled object of the present application may include, as the cylindrical object, at least a stator having one or more slots formed therein, and a winding present in the slot of the stator. The stator may have a structure including a steel plate made of a material such as iron (Fe) laminated in a cylindrical shape, and in this case, the slots are arranged radially along the circumferential direction of the stator, but the type of stator that may be applied in the present application is not limited thereto.

[0096] In addition, the type of the windings applied in the present application is not particularly limited. Usually, windings are manufactured by applying an insulating coating to a material such as copper (Cu), and in addition to such a conventional winding, other types of windings may also be applied in the present application. In addition, all types of winding methods, such as the general winding method and the hairpin winding method, may be applied.

[0097] 3 and 4 are diagrams showing an exemplary form of the cylindrical object when the cylindrical object is the motor stator described above. The stator illustrated in Figs. 3 and 4 is the cylindrical (cylinder-shaped) stator mentioned above, with Fig. 3 showing the stator 100 observed from the surface direction in which the slots 101 are formed, and Fig. 4 showing the stator 100 observed from the side. Fig. 5 is a side view of the stator 100 with the windings 102 introduced into the slots. The above description of the cylindrical object can be applied to the motor stator as it is, so a more detailed description will be omitted.

[0098] In addition, insulating paper may be injected between the slot and the resin composition during the process of introducing the resin composition into the slot of the cylindrical object (stator). That is, the method of the present application may further include a step of introducing insulating paper into the slot before introducing the resin composition into the slot.

[0099] Therefore, in one example, the resin hardened through induction heating by the magnetic field generated by the magnetic field generator and the solenoid coil may be an insulating resin hardened product in which insulation properties are imparted or improved by the insulating paper.

[0100] Also, as described above, since a winding is formed in the slot, the method of the present application may further include the step of introducing a winding into the slot before introducing insulating paper into the slot.

[0101] In the present application, particularly when the cylindrical object is a stator for a motor, as long as the above-mentioned cured resin has a form that fills the inside of a slot, all commonly known parts of an electric motor may be applied as other elements or parts to the cylindrical object.

[0102] The present application also relates to a resin-filled object. The resin-filled object includes a cylindrical object having an edge and a resin filler. The through space may be formed along the longitudinal direction within the cylindrical object, and the interior of the edge may include one or more slots formed along the longitudinal direction. The resin filler may fill the slot. The resin filler can be formed by curing the above-mentioned resin composition, and therefore includes a component derived from the resin (resin component) and a magnetic powder.

[0103] The cured resin fills the slot with an excellent filling rate. Thus, the filling rate of the cured resin in the slot is 90% or more. The filling rate may refer to the percentage of the volume of the cured resin present in the slot with respect to the internal volume of the slot, excluding the volume occupied by other elements that may be included outside the cured resin (if the cylindrical object is a stator for a motor and the slot of the stator is wound, the winding). The higher the filling rate, the more advantageous it is, so there is no particular upper limit. Exemplarily, the filling rate may be about 100% or less, 99% or less, 98% or less, 97% or less, 96% or less, 95% or less, 94% or less, or 93% or less.

[0104] In addition, the resin-filled object of the present application may include a resin cured product having a high degree of curing. For example, the relative degree of curing of the resin cured product may be 95% or more. The relative degree of curing may mean the ratio (Hb / Ha) of the enthalpy (Ha) of the resin cured product before curing, for example, the curable resin composition, to the enthalpy (Hb) of the resin cured product, and each enthalpy may be measured using DSC (Differentiation Scanning Calorimetry). The relative degree of curing is not an absolute value, so the upper limit may exceed 100%. In other examples, the relative degree of curing may be 95% or more, 97% or more, 99% or more, or 102% or more, and the upper limit is not particularly limited, and may be, for example, 150% or less, 140% or less, 130% or less, 125% or less, 120% or less, or 115% or less.

[0105] The resin-filled object of the present application has excellent voltage resistance characteristics. For example, the resin-filled object may have a line resistance within a predetermined range, and an insulation resistance and leakage current at a specific voltage that are equal to or greater than a specific value. Specifically, the resin-filled object of the present application may have a line resistance within a range of 18 mΩ to 21 mΩ. Furthermore, the resin-filled object of the present application may have an insulation resistance of 20 mΩ or more at 1000V, for example. And, the resin-filled object of the present application may have a leakage current of 20 mA or less at 1,900V.

[0106] The measurement methods of the line resistance, insulation resistance, and leakage current are well known, and in this application, any of the well-known methods may be used for measurement. For example, the line resistance and insulation resistance may be measured using a commercially available insulation resistance meter, which is the resistance value when an AC voltage of 60 Hz and 1,000 V is applied to the resin-filled object for about one minute. In addition, the leakage current refers to the current value leaking from the resin-filled object measured under the above conditions by a well-known method using a high-voltage (Hipot) tester.

[0107] The line resistance, insulation resistance, and leakage current may be measured when the cylindrical object has a ring-shaped edge and is a cylindrical object with a perforated interior. Specifically, the line resistance, insulation resistance, and leakage current may be measured when the cylindrical object is a cylindrical object with a perforated interior, an inner diameter of about 130 mm, an outer diameter of about 210 mm, and a length of about 160 mm.

[0108] In one example, the area of ​​the opening of the slot in the edge of the cylindrical object (area of ​​the cross-sectional surface in the width direction) is 0.5 cm 2 ~10cm 2 In other words, the area of ​​the opening of the slot is considerably narrow. Also, since four or more slots are formed in the edge portion, a resin-filled object having a resin cured material filled with an excellent filling rate even in a large number of narrow filling spaces (slots) can be manufactured.

[0109] In other examples, the number of slots may be 10 or more, 15 or more, 20 or more, 30 or more, 40 or more, or 50 or more, and since a larger number of slots can increase the amount of the cured resin filled, the number is not particularly limited, and may be, for example, 100 or less, 90 or less, 80 or less, 70 or less, or 64 or less. However, the number of slots may vary depending on the design of the equipment to be insulated.

[0110] As described above, in the resin-filled object of the present application, the resin is filled at an excellent filling rate even in a narrow slot.

[0111] The resin-filled object of the present application can be manufactured by the above-mentioned manufacturing method, and therefore all the contents described in the above-mentioned manufacturing method are also applicable to the resin-filled object.

[0112] For example, as described above, the cylindrical object may be a motor stator or a transformer. Specifically, the cylindrical object may be a stator for a DC-driven or AC-driven motor. Therefore, in the slot of the motor stator, insulating paper may be introduced between the precursor of the resin filler (resin composition) and the inner wall of the slot, so that in the resin-filled object, the resin filler may be an insulating resin filler.

[0113] In another example, if a winding is introduced into the slot and part of the winding is damaged by external impact, the insulating properties of the resin-filled body can be maintained by applying the resin in powder form. Effect of the Invention

[0114] The method of the present application can fill a hardenable resin at a high filling rate even in a filling portion having a small area.

[0115] The method of the present application can fill a resin so that it has excellent hardness even in a small area of ​​filling and at the same time has excellent insulating properties.

[0116] The method of the present application allows the above filling to proceed in a fast time.

[0117] The resin-filled object of the present application has excellent hardness and insulating properties and has a resin filled at an excellent filling rate even within a small area of ​​the filled portion. [Brief description of the drawings]

[0118] [Figure 1] FIG. 2 is a schematic diagram of a cylindrical object to which the method of the present application is applied. [Diagram 2] 1 is an exemplary cross-sectional view of a cylindrical object applied with the method of the present application; [Diagram 3] FIG. 1 is a diagram showing an example of a cylindrical object. [Figure 4] FIG. 1 is a diagram showing an example of a cylindrical object. [Diagram 5] FIG. 1 is a diagram showing an example of a cylindrical object. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0119] Hereinafter, the present application will be described in detail with reference to examples. However, the scope of the present application is not limited to the following examples.

[0120] <1. Measurement of relative degree of cure>

[0121] The enthalpy (Hb) of the resin-filled objects prepared in the Examples and Comparative Examples and the enthalpy (Ha) of the curable resin composition before curing were measured using DSC, and the ratio (Hb / Ha) was converted into a percentage and reported as the relative degree of curing.

[0122] <2. Measurement of filling rate>

[0123] The filling rate was determined by cutting the resin-filled objects prepared in the Examples and Comparative Examples in a direction perpendicular to the longitudinal direction, measuring the amount of the cured resin filled in the slot, and calculating the percentage of the volume of the cured resin to the entire volume of the slot.

[0124] <3. Evaluation of voltage resistance characteristics>

[0125] The inter-line resistance, insulation resistance, and leakage current of the resin-filled objects manufactured in the examples and comparative examples were measured, and the objects were rated as Pass only if the inter-line resistance was within the range of 18mΩ to 21mΩ, the insulation resistance at 1000V was 20mΩ or more, and the leakage current at 1900V was 20mA or less, and otherwise rated as Fail.

[0126] Specifically, the line resistance and insulation resistance are resistances measured using a known insulation resistance meter after applying an AC voltage of 60 Hz and 1,000 V to the resin-filled object for about one minute, and the leakage current is the value of the leaked current when a voltage of 1,900 V is applied using a known method using a high voltage (HIPOT) tester.

[0127] <4. Evaluation of thermal shock properties>

[0128] The resin-filled objects prepared in the Examples and Comparative Examples were introduced into a commercially available thermostatic / variable temperature chamber. Then, the resin-filled objects were subjected to thermal shock by repeatedly increasing the temperature of the thermostatic / variable temperature chamber from -30°C to 180°C about 300 times. The number of cracks (crack count, unit: ea) generated in the resin-filled object and the number of peel-offs (peel-off count, unit: ea) of the cured resin were measured.

[0129] <Production example 1. Resin composition>

[0130] A curable resin composition was prepared by mixing 100 parts by weight of epoxy resin (a mixture of KUKDO Chemical YD128 and nadic anhydride in a weight ratio of 60:40) and 5 parts by weight of magnetic particles. A liquid epoxy resin was used as the epoxy resin. Fe3O4 particles were used as the magnetic particles. The magnetic particles had an average particle size of about 100 nm, a coercive force of about 94 kOe, and a saturation magnetization value of about 80 emu / g when measured by FESEM (Field Effect Scanning Electron Microscope) and DLS (Dynamic Light Scattering). The coercive force and saturation magnetization values ​​were measured using a HS curve (VSM curve) with a vibrating sample magnetometer (SQUID-Vibrating Sample Magnetometer, Ministry of Basic Science and Technology, Republic of Korea) under an external magnetic field of 1 Tesla.

[0131] <Production example 2. Resin composition>

[0132] A curable resin composition was produced in the same manner as in Production Example 1, except that a solid-phase epoxy resin (3M, Scotchcast 255) was used as the epoxy resin.

[0133] <Production Example 3. Resin composition>

[0134] A curable resin composition was produced in the same manner as in Production Example 1, except that no magnetic particles were mixed.

[0135] Example 1. Preparation of a resin-filled object

[0136] A cylindrical motor stator (inner diameter: about 130 mm, outer diameter: about 210 mm, total length: 160 mm) as shown in Fig. 3 was prepared. The slots were formed radially in the stator as shown in Fig. 3, and the openings were rectangular with a horizontal length of about 5 mm and a vertical length of about 20 mm. Windings 102 (copper wire) were introduced into the slots as shown in Fig. 5. The windings used had a circular cross section with a diameter of about 4.5 mm, and five of the windings were introduced into each slot.

[0137] A solenoid coil electrically connected to a magnetic field generator was inserted into the through space formed in the motor stator, and an AC magnetic field of about 4500 W output, about 307 kHz frequency, and 95 A was applied from the magnetic field generator for about 1 minute to preheat the stator until the temperature of the stator reached about 60° C. (preheating step).

[0138] After preheating the stator, the curable resin composition according to Preparation Example 1 was injected into the slots of the stator using a known nozzle. The curable resin composition was injected while applying an AC magnetic field of about 230 W output, about 306 kHz frequency, and 35 A for about 5 minutes from the magnetic field generator so that the temperature of the preheated stator was maintained at about 60° C. (resin composition introduction step).

[0139] Thereafter, an AC magnetic field of about 8000 W output, about 306 kHz frequency, and 125 A was applied from the magnetic field generator for about 10 minutes to heat the stator until the temperature of the stator reached about 150° C., thereby producing a resin cured product (curing step).

[0140] Additionally, to maintain the temperature during the curing step, an AC magnetic field with an output of about 500 W, a frequency of about 305 kHz, and 45 A was applied by the magnetic field generator for about 7 minutes to prepare a resin-filled object.

[0141] Example 2. Production of resin-filled objects

[0142] A resin-filled object was manufactured in the same manner as in Example 1, except that in the curing step, an AC magnetic field of about 9,800 W output, about 305 kHz frequency, and 130 A was applied for about 5 minutes by the magnetic field generator, and the stator was heated until its temperature reached about 170°C.

[0143] Example 3. Preparation of resin-filled objects

[0144] A resin-filled object was manufactured using the same motor stator as that prepared in Example 1.

[0145] A solenoid coil electrically connected to a magnetic field generator was inserted into the through space formed in the motor stator, and the magnetic field generator applied an AC magnetic field of about 4500 W output, about 307 kHz wave number, and 95 A for about 1 minute to preheat the stator until the temperature of the stator reached about 130° C. (preheating step).

[0146] The preheated stator was immersed in the curable resin composition of Preparation Example 2 by a transfer means for about 1 minute, and then removed so that the curable resin composition of Preparation Example 2 was injected into the slots of the stator. Then, an AC magnetic field with an output of about 8000 W, a frequency of about 306 kHz, and 125 A was applied by the magnetic field generator for about 10 minutes to heat the stator until the temperature of the stator reached about 150° C., thereby producing a resin-filled object.

[0147] Thereafter, a magnetic field was generated by the magnetic field generator, and the stator was heated until the temperature of the stator reached about 150° C., thereby producing a cured resin material.

[0148] Additionally, to maintain the temperature during the curing step, an AC magnetic field with an output of about 500 W, a frequency of about 305 kHz, and 45 A was applied by the magnetic field generator for about 7 minutes to prepare a resin-filled object.

[0149] <Comparative Example 1. Production of resin-filled object>

[0150] A resin-filled object was produced in the same manner as in Example 1, except that the curable resin composition of Production Example 3 was used as the curable resin composition.

[0151] <Comparative Example 2. Production of resin-filled object>

[0152] A resin-filled object was manufactured using the same motor stator as that prepared in Example 1.

[0153] Specifically, heat was applied in an oven for about 30 minutes to preheat the motor stator to about 60°C.

[0154] After the stator was preheated, the curable resin composition according to Preparation Example 1 was injected into the slots of the stator using a known nozzle.

[0155] Thereafter, the stator was heat-treated for 40 minutes in an oven heated to about 150° C. to produce a resin-filled object (hardening step).

[0156] Comparative Example 3: Resin-filled object

[0157] A resin-filled object was manufactured in the same manner as in Comparative Example 1, except that in the curing step, the stator was heat-treated in an oven heated to about 170° C. for 40 minutes.

[0158] <Comparative Example 4. Resin-filled object>

[0159] A resin-filled object was manufactured in the same manner as in Comparative Example 1, except that the curable resin composition of Preparation Example 3 was injected.

[0160] Comparative Example 5: Resin-filled object

[0161] A resin-filled object was manufactured in the same manner as in Comparative Example 1, except that the curable resin composition of Preparation Example 2 was injected and the stator was heat-treated in an oven heated to about 130° C. for about 30 minutes.

[0162] The physical properties of the resin-filled objects produced in Examples 1 to 3 and Comparative Examples 1 to 5 were evaluated and are shown in Table 1 below.

[0163] [Table 1]

[0164] In Examples 1 and 2, which used the curable resin composition and method defined in the present application, it was confirmed that a resin-filled object having a high filling rate and relative degree of curing, and excellent thermal shock resistance and voltage resistance characteristics, could be produced in a short time. However, in Example 3 and Comparative Example 5, the resin composition of Preparation Example 2 is a mixed powder that is not in a liquid form, and this is only applied to the windings exposed from the slots, so it is difficult to directly confirm the filling rate and voltage resistance characteristics, but it can at least be confirmed that fast curing is possible, as the curing time is shorter in Example 3 (magnetic powder applied) than in Comparative Example 5 (magnetic powder not applied).

[0165] On the other hand, in the case of Comparative Example 1, in which the method applied in the present application was applied but a curable resin composition not containing a magnetic material was used, a resin-filled object could be produced within a short time, but there were problems with the degree of curing, filling rate, thermal shock resistance and voltage resistance characteristics being inferior.

[0166] In addition, in the case of Comparative Examples 2 to 5, which used an oven heating method that is not the method applied in the present application, it was found that the cured resin did not fill the slots at a satisfactory filling rate, despite the long curing time required. Here, examples of the invention according to this embodiment will be described as items. [Item 1] 1. A method of making a resin filled object using a tubular object including an edge having a longitudinally extending through space and one or more slots formed therein, the method comprising: introducing a resin composition into the slot, the resin composition including a resin and a magnetic powder; Inserting a solenoid coil into the through space of the cylindrical object having the resin composition introduced into the slot; and A method for producing a resin-filled object, comprising the step of generating a magnetic field with the solenoid coil to harden the resin. [Item 2] 2. The method for producing a resin-filled object according to claim 1, wherein the resin is an insulating resin. [Item 3] The magnetic powder includes one or more magnetic materials, 3. The method for producing a resin-filled object according to claim 1 or 2, wherein the magnetic material comprises magnetic particles and a surface treatment agent introduced onto the surfaces of the magnetic particles. [Item 4] The average particle size of the magnetic particles is within a range of 20 nm to 300 nm; 4. The method for producing a resin-filled object according to item 3, wherein the crystal size of the magnetic particles is within a range of 10 nm to 40 nm. [Item 5] The method for producing a resin-filled object according to item 3 or 4, wherein the surface treatment agent is a polyol-based compound, a polysiloxane-based compound, an alkyl phosphoric acid-based surface treatment agent, an alkyl carboxylic acid-based surface treatment agent, a sulfonic acid-based surface treatment agent, an acid compound containing a long-chain alkyl group, an acrylic copolymer containing an acidic functional group or an amino group, an aromatic acid-based surface treatment agent, or a block copolymer containing an acidic functional group or an amino group. [Item 6] 6. The method for producing a resin-filled object according to any one of items 3 to 5, wherein the coefficient of variation of the particle size of the magnetic particles is within a range of 5% to 30%. [Item 7] 7. The method of claim 1, further comprising the step of introducing insulating paper into the slot before introducing a resin composition into the slot. [Item 8] 8. The method of claim 7, further comprising the step of introducing a winding into the slot before introducing insulating paper into the slot. [Item 9] 9. The method for producing a resin-filled object according to any one of claims 1 to 8, further comprising the step of inserting a solenoid coil into the through space of the cylindrical object before introducing a resin composition into the slot, and then preheating the cylindrical object by generating a magnetic field with the solenoid coil. [Item 10] 10. The method for producing a resin-filled object according to item 9, wherein the cylindrical object is preheated by adjusting the temperature of the cylindrical object to be lower than a curing initiation temperature of the resin composition. [Item 11] Item 11. The method for producing a resin-filled object according to item 9 or 10, wherein the preheating of the cylindrical object is performed by adjusting the temperature of the cylindrical object so that the viscosity of the resin composition at the temperature is maintained at 1 / 100 or more of the viscosity at room temperature. [Item 12] 12. The method for producing a resin-filled object according to any one of claims 9 to 11, wherein the resin composition is introduced while a magnetic field is generated by the solenoid coil. [Item 13] 13. The method for producing a resin-filled object according to any one of claims 1 to 12, wherein the introduction of the resin composition is carried out by a liquid dipping method, a solid phase dipping method, or a trickling method. [Item 14] Item 14. A method for producing a resin-filled object according to any one of items 1 to 13, comprising applying an alternating current to the solenoid coil using a magnetic field generating device to generate a magnetic field to harden the resin. [Item 15] a cylindrical object including an edge having a through space formed in a longitudinal direction and one or more slots formed therein in the longitudinal direction; and a resin filler filling the interior of the slots, the resin filler including a resin component and a magnetic powder; The filling rate of the resin filler in the slot is 90% or more, The line resistance is within the range of 18mΩ to 21mΩ. Insulation resistance at 1000V is 20mΩ or more. A resin-filled object with a leakage current of 20mA or less at 1,900V. [Item 16] The cross-sectional area of ​​the slot in the width direction is 0.01 cm 2 ~10cm 2 Item 16. The resin-filled body according to item 15, wherein the resin-filled body has a diameter in the range of 100 mm to 150 mm. [Item 17] Item 17. The resin-filled body according to item 15 or 16, wherein the edge has between 2 and 100 slots. [Item 18] Item 18. The resin-filled object according to any one of items 15 to 17, wherein the cylindrical object is a stator for a motor, and the resin component is a component derived from an insulating resin. [Item 19] 19. The resin filled body of any one of claims 15 to 18, further comprising insulating paper present in the slot between the resin filling and an inner wall of the slot. [Item 20] 20. The resin filled body of any one of claims 15 to 19, further comprising a winding present in the slot. [Explanation of symbols]

[0167] 1: Edge 2:Through space 3:Slots on the edges 10: Cylindrical object 100: Motor stator 101: Stator slot 102: Winding in slot

Claims

1. 1. A method of making a resin filled object using a tubular object including an edge having a longitudinally extending through space and one or more slots formed therein, the method comprising: a step of inserting a solenoid coil into the through-space of the cylindrical object before introducing a resin composition into the slot, and then preheating the cylindrical object by generating a magnetic field with the solenoid coil; introducing a resin composition into the slot, the resin composition including a resin and a magnetic powder; and A method for producing a resin-filled object, comprising the step of generating a magnetic field with the solenoid coil to harden the resin.

2. The method for producing a resin-filled object according to claim 1 , wherein the resin is an insulating resin.

3. The magnetic powder includes one or more magnetic materials, The method for producing a resin-filled object according to claim 1 or 2, wherein the magnetic material comprises magnetic particles and a surface treatment agent introduced onto the surfaces of the magnetic particles.

4. The average particle size of the magnetic particles is within a range of 20 nm to 300 nm; The method for producing a resin-filled object according to claim 3, wherein the crystal size of the magnetic particles is within the range of 10 nm to 40 nm.

5. 5. The method for producing a resin-filled object according to claim 3 or 4, wherein the surface treatment agent is a polyol-based compound, a polysiloxane-based compound, an alkyl phosphoric acid-based surface treatment agent, an alkyl carboxylic acid-based surface treatment agent, a sulfonic acid-based surface treatment agent, an acid compound containing a long-chain alkyl group, an acrylic copolymer containing an acidic functional group or an amino group, an aromatic acid-based surface treatment agent, or a block copolymer containing an acidic functional group or an amino group.

6. The method for producing a resin-filled object according to any one of claims 3 to 5, wherein the coefficient of variation of the particle size of the magnetic particles is within a range of 5% to 30%.

7. A method for producing a resin filled body according to any one of claims 1 to 6, further comprising the step of introducing insulating paper into the slot prior to introducing a resin composition into the slot.

8. The method of claim 7 further comprising the step of introducing a winding into said slot prior to introducing insulating paper into said slot.

9. The method for producing a resin-filled object according to claim 1 , wherein the cylindrical object is preheated by adjusting the temperature of the cylindrical object to be lower than a curing initiation temperature of the resin composition.

10. The method for producing a resin-filled object described in any one of claims 1 to 9, wherein the cylindrical object is preheated by adjusting the temperature of the cylindrical object so that the viscosity of the resin composition at that temperature is maintained at more than 1 / 100 of the viscosity at room temperature.

11. The method for producing a resin-filled object according to claim 1 , wherein the resin composition is introduced while a magnetic field is being generated by the solenoid coil.

12. The method for producing a resin-filled object according to any one of claims 1 to 11, wherein the introduction of the resin composition is carried out by a liquid dipping method, a solid phase dipping method or a trickling method.

13. The method for manufacturing a resin-filled object according to any one of claims 1 to 12, further comprising using a magnetic field generating device to apply an alternating current to the solenoid coil to generate a magnetic field to harden the resin.

14. the filling rate of the cured resin material containing the resin and the magnetic powder in the slot is 90% or more, The resin-filled object has a line resistance in the range of 18 mΩ to 21 mΩ; The insulation resistance of the resin-filled object at 1000 V is 20 mΩ or more; A method for producing a resin-filled object, the resin-filled object having a leakage current of 20 mA or less at 1,900 V, comprising the steps of: the filling rate is a percentage of the volume of the cured resin present inside the slot with respect to the internal volume of the slot, excluding the volume of other elements contained outside the cured resin, The cured resin is obtained through the step of curing the resin. A method of making a resin filled body according to any one of claims 1 to 13.

15. The cross-sectional area of ​​the slot in the width direction is 0.01 cm 2 ~10cm 2 15. The method of claim 14, wherein the thickness of the resin-filled body is in the range of

16. The method of claim 14 or 15, wherein there are between 2 and 100 slots in the edge.

17. 17. The method for manufacturing a resin-filled object according to claim 14, wherein the cylindrical object is a stator for a motor, and the resin is an insulating resin.

18. 18. A method for producing a resin filled body as claimed in any one of claims 14 to 17, further comprising insulating paper present in said slot between said resin and said magnetic powder and an inner wall of said slot.

19. 19. A method of making a resin filled body as claimed in any one of claims 14 to 18, further comprising windings present in said slots.

Citation Information

Patent Citations

  • 3D printing compositions

    JP2019506499A

  • Scroll compressor

    WO2020188738A1