Method for forming boron nitride film

By forming an aminosilane seed layer and optionally using diborane, the method addresses non-uniform boron nitride film thickness issues on substrates with varying incubation times, enhancing film uniformity and deposition rate.

JP7575176B2Active Publication Date: 2024-10-29TOKYO ELECTRON LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021011396
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-27
Publication Date
2024-10-29
Estimated Expiration
2041-01-27

AI Technical Summary

Technical Problem

Existing methods for forming boron nitride films on substrates with different incubation times result in non-uniform film thickness due to variations in incubation times, leading to deteriorated in-plane uniformity.

Method used

A method involving the formation of an aminosilane seed layer on the substrate surface followed by the deposition of a boron nitride film using thermal CVD, which includes a step of supplying aminosilane gas to create uniform incubation conditions, and optionally adding a diborane supply step to further enhance adsorption sites.

Benefits of technology

The method significantly reduces the difference in incubation times between substrates with different base materials, improving in-plane uniformity and film thickness consistency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575176000001
    Figure 0007575176000001
  • Figure 0007575176000002
    Figure 0007575176000002
  • Figure 0007575176000003
    Figure 0007575176000003
Patent Text Reader

Abstract

To provide a method for depositing boron nitride films and a film deposition apparatus that allow uniform deposition of boron nitride films even on different primer coats with the uniformized incubation time.SOLUTION: The inventive method includes the steps in which: seed layers are formed on the surface of substrates by supplying them with an aminosilane gas, wherein the substrates have primer coats that are different in incubation time for depositing boron nitride films; and the boron nitride films are deposited on the seed layers.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for forming a boron nitride film. By law Regarding. [Background technology]

[0002] Conventionally, there has been known a method for forming a carbon film, in which a hydrocarbon carbon source gas is thermally decomposed to form a carbon film on a substrate to be processed, the carbon film formation temperature is set to a temperature lower than the thermal decomposition temperature of the hydrocarbon carbon source gas alone in an unassisted plasma state, the hydrocarbon carbon source gas and a thermal decomposition temperature lowering gas containing a halogen element are introduced into a processing chamber, and the film is formed by a non-plasma thermal CVD method (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-33186 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present disclosure provides a method and apparatus for depositing a uniform boron nitride film by aligning incubation times even when the substrates are different. [Means for solving the problem]

[0005] In order to achieve the above object, a method for forming a boron nitride film according to one aspect of the present invention includes: forming a boron nitride film on a surface of a substrate having an underlayer with a different incubation time when forming the boron nitride film; Without supplying nitrogen-containing gas supplying an aminosilane gas to form a seed layer; depositing a boron nitride film on the seed layer. death, The substrates with different incubation times include silicon and silicon dioxide. . Effect of the Invention

[0006] According to the present disclosure, it is possible to form a boron nitride film by eliminating differences in incubation time due to differences in undercoat films. [Brief description of the drawings]

[0007] [Figure 1] 1 is a cross-sectional view that illustrates an example of a film forming apparatus according to an embodiment of the present disclosure. [Diagram 2] FIG. 1 is a diagram showing the underlayer dependency in a conventional BN film formation process. [Diagram 3] FIG. 2 is a flow diagram showing an example of a method for forming a boron nitride film according to the present embodiment. [Figure 4] 1 is a diagram showing changes on a substrate caused by a BN film forming method according to an embodiment of the present invention. [Diagram 5] FIG. 13 is a diagram showing the experimental results of the difference in film thickness between the case where an aminosilane seed 30 is formed and the case where an aminosilane seed 30 is not formed, using DIPAS, which is a type of aminosilane gas. [Figure 6] FIG. 6 is a graph showing the experimental results shown in FIG. 5. [Figure 7] FIG. 1 is a model diagram of the behavior of the surface of a substrate 10 during aminosilane seed formation. [Figure 8] FIG. 1 is a model diagram showing a case where diborane (B2H6) is supplied after aminosilane gas is supplied. [Figure 9] FIG. 1 is a diagram showing an example of a conventional method for forming a BN film without forming an aminosilane seed. [Figure 10] 1A to 1C are diagrams showing a series of steps of a method for forming a BN film including a step of forming an aminosilane seed according to an embodiment of the present invention. [Figure 11] 1A to 1C are diagrams showing a series of steps of a method for forming a BN film including a step of forming an aminosilane seed and a step of supplying diborane according to an embodiment of the present invention. [Figure 12]FIG. 1 shows examples of a conventional BN film formation method, a BN film formation method according to the present embodiment including an aminosilane seed formation step, and a BN film formation method according to the present embodiment including both an aminosilane seed formation step and a diborane supply step. [Figure 13] This is a diagram showing the results of FIG. 12 reflected in terms of incubation time. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.

[0009] [Film forming equipment] FIG. 1 is a cross-sectional view that illustrates a schematic example of a film forming apparatus according to an embodiment of the present disclosure.

[0010] 1, the film forming apparatus 100 is configured as a vertical batch-type film forming apparatus, and includes a cylindrical outer wall 101 with a ceiling, and a cylindrical inner wall 102 provided inside the outer wall 101. The outer wall 101 and the inner wall 102 are made of, for example, quartz, and the area inside the inner wall 102 forms a processing chamber S in which a plurality of semiconductor wafers (hereinafter simply referred to as wafers) W, which are objects to be processed, are processed at once.

[0011] The outer wall 101 and the inner wall 102 are separated from each other in the horizontal direction with an annular space 104 between them, and their lower ends are joined to a base material 105. The upper end of the inner wall 102 is separated from the ceiling of the outer wall 101, so that the upper part of the processing chamber S is in communication with the annular space 104. The annular space 104 in communication with the upper part of the processing chamber S serves as an exhaust path. The gas supplied to and diffused in the chamber S flows from below the processing chamber S to above the processing chamber S and is sucked into the annular space 104. An exhaust pipe 106 is connected to, for example, the lower end of the annular space 104, and the exhaust pipe 106 is connected to an exhaust device 107. The exhaust device 107 is configured to include a vacuum pump and the like, and exhausts the processing chamber S and adjusts the internal pressure of the processing chamber S to a pressure appropriate for processing.

[0012] A heating device 108 is provided outside the outer wall 101 so as to surround the periphery of the processing chamber S. The heating device 108 adjusts the temperature inside the processing chamber S to a temperature appropriate for processing, and heats a plurality of wafers W at once.

[0013] The lower part of the processing chamber S is in communication with an opening 109 provided in the base material 105. A manifold 110 formed in a cylindrical shape from, for example, stainless steel is connected to the opening 109 via a seal member 111 such as an O-ring. The lower end of the manifold 110 is opened, and a boat 112 is inserted into the processing chamber S through this opening. The boat 112 is made of, for example, quartz, and has a plurality of support columns 113. The support columns 113 are formed with grooves (not shown), and the grooves support a plurality of substrates to be processed at once. This allows the boat 112 to mount a plurality of substrates to be processed, for example, 50 to 150 wafers W, in multiple stages. By inserting the boat 112 on which the plurality of wafers W are mounted into the processing chamber S, the processing chamber S can accommodate a plurality of wafers W.

[0014] The boat 112 is placed on a table 115 via a thermal insulation tube 114 made of quartz. The table 115 is supported on a rotating shaft 117 that penetrates a lid 116 made of, for example, stainless steel. The lid 116 opens and closes an opening at the lower end of the manifold 110. A magnetic fluid seal 118, for example, is provided at the penetration part of the lid 116, and rotatably supports the rotating shaft 117 while sealing it airtight. In addition, a seal member 119 made of, for example, an O-ring is interposed between the peripheral part of the lid 116 and the lower end of the manifold 110, and maintains the sealing property of the inside of the processing chamber S. The rotating shaft 117 is attached to the tip of an arm 120 supported by a lifting mechanism (not shown) such as a boat elevator. As a result, the wafer boat 112 and the lid 116 are vertically raised and lowered together to be inserted into and removed from the processing chamber S.

[0015] The film forming apparatus 100 includes a process gas supply mechanism 130 inside the process chamber S for supplying gas used in the process.

[0016] The process gas supply mechanism 130 of this embodiment includes a boron-containing gas source 131a, a nitrogen-containing gas source 131b, an aminosilane gas source 131c, and an inert gas source 131d, and may further include a carbon-containing gas source 131e and a halogen gas source 131f, as necessary.

[0017] The boron-containing gas supply source 131a is connected to the gas supply port 134a via a flow rate controller (MFC) 132a and an on-off valve 133a. Similarly, the nitrogen-containing gas supply source 131b is connected to the gas supply port 134b via a flow rate controller (MFC) 132b and an on-off valve 133b, the aminosilane gas supply source 131c is connected to the gas supply port 134c via a flow rate controller (MFC) 132c and an on-off valve 133c, and the inert gas supply source 131d is connected to the gas supply port 134d via a flow rate controller (MFC) 132d and an on-off valve 133d. In addition, the carbon-containing gas supply source 131e is connected to the gas supply port 134e via a flow rate controller (MFC) 132e and an on-off valve 133e, and the halogen gas supply source 131f is connected to the gas supply port 134f via a flow rate controller (MFC) 132f and an on-off valve 133f.

[0018] The gas supply ports 134a to 134f are provided so as to penetrate the sidewall of the manifold 110 in the horizontal direction, and diffuse the supplied gas toward the inside of the processing chamber S located above the manifold 110.

[0019] The boron-containing gas supplied from the boron-containing gas supply source 131a is a gas for forming a boron nitride film by CVD, and various gases can be used as long as they contain boron. For example, diborane (B2H6) gas or boron trichloride (BCl3) may be used as the boron-containing gas. Furthermore, BCl3 (trichlorosilane), TEB ( BirdAlternatively, ethylborane, TMB (trimethylborane), or DMAB (dimethylaminoborane) may be used.

[0020] The nitrogen-containing gas supplied from the nitrogen-containing gas supply source 131b is a gas for forming a boron nitride film by CVD, and various gases containing nitrogen can be used. For example, ammonia (NH3) gas or nitrogen (N2) gas may be used as the nitrogen-containing gas.

[0021] The aminosilane gas supplied from the aminosilane gas supply source 131c is a gas for forming an aminosilane seed film on the wafer W, and various aminosilane gases can be used. As the aminosilane gas, for example, diisopropylaminosilane (DIPAS) gas can be used.

[0022] The inert gas supplied from the inert gas supply source 131d is used as a purge gas or a dilution gas. As the inert gas, for example, N2 gas or a rare gas such as Ar gas or He gas can be used.

[0023] The carbon-containing gas supplied from the carbon-containing gas supply source 131e provided as necessary is a gas for forming a carbon film by low-pressure CVD, and various gases containing carbon can be used, for example, a hydrocarbon-based carbon source gas can be used.

[0024] Examples of hydrocarbon carbon source gases include: C n H 2n+2 C m H 2m C m H 2m-2 (where n is a natural number of 1 or more, and m is a natural number of 2 or more).

[0025] In addition, examples of hydrocarbon carbon source gases include Benzene gas (C6H6) may be included.

[0026] Molecular formula C n H 2n+2 Examples of the hydrocarbon represented by the formula: Methane gas (CH4) Ethane gas (C2H6) Propane gas (C3H8) Butane gas (C4H 10 :Other isomers are also included) Pentane gas (C5H 12 :Other isomers are also included) Some examples include:

[0027] Molecular formula C m H 2m Examples of the hydrocarbon represented by the formula: Ethylene gas (C2H4) Propylene gas (C3H6: including other isomers) Butylene gas (C4H8: including other isomers) Pentane gas (C5H 10 :Other isomers are also included) Some examples include:

[0028] Molecular formula C m H 2m-2 Examples of the hydrocarbon represented by the formula: Acetylene gas (C2H2) Propyne gas (C3H4: including other isomers) Butadiene gas (C4H6: including other isomers) Isoprene gas (C5H8: including other isomers) Some examples include:

[0029] Halogen Gas Source 131 f A gas containing a halogen element is used as the halogen gas supplied from the source gas supplying unit 1. The gas containing a halogen element has a catalytic function to lower the thermal decomposition temperature of the hydrocarbon carbon source gas, thereby lowering the deposition temperature of the carbon film by the thermal CVD method.

[0030] Halogen elements include fluorine (F), chlorine (Cl), bromine (Br), and iodine (I). The gas containing halogen elements may be a halogen element alone, i.e., a fluorine (F2) gas alone, a chlorine (Cl2) gas alone, a bromine (Br2) gas alone, and an iodine (I2) gas alone, or a compound containing these. However, halogen elements alone have the advantage that heat is not required for thermal decomposition and that the effect of lowering the thermal decomposition temperature of a hydrocarbon-based carbon source gas is high. Among the above halogen elements, fluorine is highly reactive and may impair the surface roughness and flatness of the carbon film to be formed. For this reason, chlorine, bromine, and iodine are preferable as halogen elements, except for fluorine. Among these, chlorine is preferable from the viewpoint of handling.

[0031] The film forming apparatus 100 has a control unit 150. The control unit 150 includes a process controller 151 formed of, for example, a microprocessor (computer), and the process controller 151 controls each component of the film forming apparatus 100. A user interface 152 and a storage unit 153 are connected to the process controller 151.

[0032] The user interface 152 includes an input section including a touch panel display and a keyboard for an operator to input commands to manage the film forming apparatus 100, and a display section including a display that visualizes and displays the operating status of the film forming apparatus 100.

[0033] The storage unit 153 stores so-called process recipes, which include control programs for implementing various processes executed in the film forming apparatus 100 under the control of the process controller 151, and programs for causing each component of the film forming apparatus 100 to execute processes according to processing conditions. The process recipes are stored in a storage medium in the storage unit 153. The storage medium may be a hard disk or a semiconductor memory, or may be a portable medium such as a CD-ROM, a DVD, or a flash memory. The process recipes may also be appropriately transmitted from another apparatus, for example, via a dedicated line.

[0034] The process recipe is read out from the storage unit 153 as required, for example, in response to an instruction from an operator via a user interface 152, and the process controller 151 causes the film forming apparatus 100 to perform processing in accordance with the read process recipe.

[0035] [Film forming method] When a boron nitride film is formed on a wafer W, silicon (Si) and silicon dioxide (SiO2) may be mixed on the surface of the wafer W.

[0036] When forming a boron nitride film (hereinafter referred to as a "BN film") on such a wafer W, the time from the start of the film formation process to the actual start of film formation (incubation time) may differ between silicon and silicon dioxide.

[0037] Figure 2 shows the dependence of the thickness on the substrate in the conventional BN film formation process. In Figure 2, the horizontal axis shows time (min) and the vertical axis shows film thickness (Å). Also, A shows the change in thickness over time for BN film formation on a silicon substrate, and B shows the change in thickness over time for BN film formation on a silicon dioxide substrate.

[0038] 2, when the substrate is silicon, there is no incubation time, as shown by characteristic A, and the BN film is deposited on the wafer W immediately after the BN film formation process begins. On the other hand, when the substrate is silicon dioxide, there is an incubation time of 17 minutes, as shown by characteristic B.

[0039] If such base materials with different incubation times exist on the same wafer W, it becomes impossible to form a BN film with a uniform thickness, and a thick BN film is formed on the silicon and a thin BN film is formed on the silicon dioxide, resulting in poor in-plane uniformity.

[0040] Therefore, in the method for forming a boron nitride film according to this embodiment, an aminosilane seed layer is first formed on the surface of the wafer W, and the surface of the wafer W is brought into a state approximating that of a silicon substrate before the BN film is formed.

[0041] 3 is a flow diagram showing an example of a method for forming a boron nitride film according to this embodiment, in which the diagram on the left shows the behavior on a silicon underlayer, and the diagram on the right shows the behavior on a silicon dioxide underlayer.

[0042] 3, in step 10, wafers W are loaded into the processing chamber S. Specifically, a plurality of wafers W made of silicon, for example 50 to 150 wafers W, are loaded onto a wafer boat 112, and the wafer boat 112 is inserted into the processing chamber S in the film forming apparatus 100 from below, thereby loading the plurality of wafers W into the processing chamber S (step 10). Then, the lower end opening of the manifold 110 is closed with the lid 116 to make the processing chamber S into an airtight space. In this state, the processing chamber S is evacuated to maintain a predetermined reduced pressure atmosphere, and the power supplied to the heating device 108 is controlled to raise the wafer temperature and maintain it at the process temperature, while the wafer boat 112 is rotated.

[0043] In step 20, in this state, first, aminosilane gas (eg, DIPAS) is supplied as a seed gas from the aminosilane gas supply source 131c and adsorbed onto the wafer surface to form aminosilane seeds for improving the incubation time.

[0044] In step 30, a boron-containing gas such as a borane-based gas typified by diborane (B2H6) gas or boron trichloride (BCl3) gas is supplied from the boron-containing gas supply source 131a, and a nitrogen-containing gas such as ammonia or nitrogen (N2) is supplied from the nitrogen-containing gas supply source 131b. At this time, the inside of the processing chamber S is heated, and a BN film is deposited on the aminosilane seed by thermal CVD. Note that, as the boron-containing gas and the nitrogen-containing gas, various gases can be used as long as they can deposit a BN film, but the most preferable gas is B2H6 gas as the boron-containing gas, and the most preferable gas is NH3 gas as the nitriding gas.

[0045] The temperature of the wafer W during the formation of the BN film in step 30 is preferably 200 to 300° C., from the viewpoints of enabling film formation and having good controllability.

[0046] In step 40, it is determined whether the BN film is an undercoat film or not. If it is not an undercoat film, the BN film is grown to a predetermined thickness, and the process flow ends.

[0047] On the other hand, when the BN film is used as an undercoat film, for example an undercoat film for a carbon film, the process proceeds to step 50 .

[0048] In step 50, after the BN film is formed in step 30, the processing chamber S is purged, and a carbon film 50 is formed by thermal CVD without using plasma assistance.

[0049] In the carbon film formation process by thermal CVD in step 50, carbonA hydrocarbon-based carbon source gas containing a hydrocarbon, for example, C4H6 gas, is supplied to the processing chamber S as a carbon-containing gas from the containing gas supply source 131e, and a halogen gas, for example, Cl2 gas, is supplied from the halogen gas supply source 131f. The hydrocarbon-based carbon source gas is heated to a predetermined temperature lower than its thermal decomposition temperature to be thermally decomposed, and a carbon film is formed on the surface of the wafer W by thermal CVD.

[0050] FIG. 4 is a diagram showing changes on a substrate caused by the BN film forming method according to this embodiment.

[0051] The left side of Fig. 4(a) is a cross-sectional view showing an exposed portion of a silicon substrate 10 having a silicon surface with no incubation time. The right side of Fig. 3(a) is a cross-sectional view showing an area where a silicon dioxide film 20 with an incubation time is formed on a silicon substrate 10.

[0052] In this state, there is no incubation time in the area where the silicon substrate 10 is the underlying material, but there is an incubation time in the area where the silicon dioxide film 20 is the underlying material. Therefore, if a BN film is formed in this state, there will be a difference in film thickness.

[0053] 4(b) is a diagram showing a state in which aminosilane gas is supplied to the substrate 10 and aminosilane seeds 30 are formed on the silicon substrate 10. In this state, both the surface of the silicon substrate 10 and the surface of the silicon dioxide film 20 are covered with the aminosilane seeds 30.

[0054] 4(c) shows the state in which a BN film is formed on an aminosilane seed. In this case, the entire base is the aminosilane seed 30, so the BN film depends on the incubation time on the aminosilane seed 30. It is considered that there will be no difference in incubation time between the case of a silicon base and the case of a silicon dioxide base.

[0055] FIG. 5 is a diagram showing the experimental results of the difference in film thickness between the case where the aminosilane seed 30 is formed and the case where it is not formed, using DIPAS, which is a type of aminosilane gas.

[0056] 5(a) is a diagram showing the difference between the film thickness A on the silicon underlayer when there is no aminosilane seed 30 and the film thickness B on the silicon dioxide underlayer. As shown in FIG. 4(a), the difference between the two is large.

[0057] Fig. 5(b) is a diagram showing the difference between the film thickness A on the silicon underlayer and the film thickness B on the silicon dioxide underlayer when the aminosilane seed 30 is formed. As shown in Fig. 4(b), the difference between the two is very small, indicating that the incubation time has improved.

[0058] Fig. 6 is a graph showing the experimental results shown in Fig. 5. In Fig. 6, the horizontal axis shows the position coordinate from the center to the outer periphery of the wafer, and the vertical axis shows the film thickness.

[0059] In FIG. 6, A is the reference value for the silicon substrate, and B is the reference value for the silicon dioxide film substrate without aminosilane seed.

[0060] D is the case where DIPAS was flowed at a flow rate of 500 sccm for 5 minutes on a silicon substrate before BN film formation.

[0061] E is a case where DIPAS was flowed at a flow rate of 200 sccm for 10 minutes on a silicon substrate, and then a BN film was formed.

[0062] F is the case where DIPAS was flowed at a flow rate of 500 sccm for 5 minutes on a silicon dioxide substrate, and then a BN film was formed.

[0063] G is a case where DIPAS was flowed at a flow rate of 200 sccm for 10 minutes on a silicon dioxide substrate, and then a BN film was formed.

[0064] In either case, it can be seen that by forming a DIPAS seed, the result is much closer to A, which is a silicon underlayer without a DIPAS seed, compared to B, which is a silicon dioxide underlayer without a DIPAS seed.

[0065] In the cases of D and E, where a DIPAS seed was formed on the silicon underlayer, the film thickness was thicker than in the case of a silicon underlayer where a DIPAS seed was not formed, and the film thickness in the case of E, where a DIPAS seed was supplied for 10 minutes at a flow rate of 200 sccm, was the largest.

[0066] In addition, F and G, in which a DIPAS seed was formed on a silicon dioxide substrate, improved to a level that was much closer to the film thickness of the silicon substrate, with little difference being observed.

[0067] In this way, by forming a DIPAS seed layer over the entire surface of the substrate 10, it is possible to reduce dependency on the underlying material and improve the in-plane uniformity, as shown in FIG.

[0068] FIG. 7 is a model diagram of the behavior of the surface of the substrate 10 during the formation of aminosilane seeds.

[0069] Figure 7(a) is a model diagram of a silicon dioxide surface, with each H-terminator present on the surface.

[0070] Figure 7(b) shows a model of the state after aminosilane flow has been performed. The aminosilane flow can increase the number of H-terminators.

[0071] Figure 7(c) shows a model of BN film formation. As shown in Figure 7(c), the number of H terminations, which are boron adsorption sites, is increased, making it easier for BN to form a film.

[0072] In this way, by supplying aminosilane gas, many H terminations are formed on the silicon dioxide underlayer, creating conditions that facilitate the deposition of a BN film.

[0073] Figure 8 is a model diagram of the case where diborane (B2H6) is supplied after aminosilane gas is supplied. It was confirmed that adding a process of supplying diborane after aminosilane gas supply can further eliminate the difference in incubation time. Details of this point will be described later.

[0074] Figure 8(a) shows the state in which aminosilane gas is supplied onto a silicon dioxide substrate, which is the same state as Figure 7(b).

[0075] Figure 8(b) is a model diagram of the diborane supplying process. It is believed that when diborane is supplied, it is possible to form H-terminated adsorption sites in the most electronically balanced state.

[0076] Figure 8(c) is a model diagram of the BN film formation process. BN bonds without imbalance, and H-terminators can be formed in good electronic states, which is believed to reduce the incubation time difference even more than when only aminosilane flow is used.

[0077] 9 to 11 are diagrams showing a comparison of the BN film forming methods described above.

[0078] FIG. 9 is a diagram showing an example of a conventional method for forming a BN film without forming an aminosilane seed.

[0079] 9(a) is a diagram showing the surface state of the silicon dioxide film 20. As shown in FIG. 9(a), OH groups 50 are formed on the surface of the silicon dioxide film 20.

[0080] 9B shows a state in which the BN film 40 is formed on the surface of the OH groups 50 of the silicon dioxide film 20. BN is adsorbed to the H terminals of the OH groups 50, and the BN film is formed.

[0081] FIG. 10 is a diagram showing a series of steps of a method for forming a BN film, including a step of forming an aminosilane seed according to this embodiment.

[0082] Fig. 10(a) is a diagram showing the surface state of the silicon dioxide film 20. As shown in Fig. 10(a), OH groups 50 are formed on the surface of the silicon dioxide film 20.

[0083] 10(b) is a diagram showing the surface state after the aminosilane seed formation step. Aminosilane is adsorbed to the H terminal of the OH group 50, and SiH group 60 is formed on the surface. This functions as an adsorption site for the BN film.

[0084] 10(c) shows the surface state after the BN film formation process. BN is adsorbed to the H terminal of the SiH group, and a BN film 40 is formed. In this way, the SiH group is formed on the surface by the aminosilane seed flow, and the incubation time on the silicon dioxide film 20 can be reduced.

[0085] FIG. 11 is a diagram showing a series of steps of a method for forming a BN film, including a step of forming an aminosilane seed and a step of supplying diborane, according to this embodiment.

[0086] 11(a) and (b) show the same steps as those in FIG. 10(a) and (b), and therefore the description thereof will be omitted.

[0087] 11(c) is a diagram showing the surface state after the diborane supplying step. The surface of the SiH groups 60 is replaced by SiBH groups 70. The SiBH groups 70 function as even better adsorption sites for BN than the SiH groups 60.

[0088] 11(d) is a diagram showing the surface state after the BN film formation process. BN is adsorbed to the H termination of the SiBH group 70, and the BN film can be formed with a reduced incubation time.

[0089] The diborane supply process uses boron used in the BN film formation process. Contains When diborane is supplied from the gas supply source 131a, boron is also supplied in the diborane supply step. Contains Diborane may be supplied from the gas supply source 131a.

[0090] In the BN film formation process, when a boron-containing gas other than diborane is to be supplied, a diborane supply source may be provided separately and diborane may be supplied from there.

[0091] In this way, by adding a diborane supplying step to the aminosilane supplying step, better adsorption sites can be formed, and the difference in incubation time between the silicon underlayer and the silicon dioxide underlayer can be further reduced.

[0092] [Example] FIG. 12 shows examples of a conventional BN film formation method, a BN film formation method according to this embodiment including an aminosilane seed formation step, and a BN film formation method according to this embodiment including both an aminosilane seed formation step and a diborane supply step.

[0093] The leftmost graph in Fig. 12 shows the difference in film thickness between the silicon underlayer and the silicon dioxide underlayer in a conventional BN film formation method. The center graph in Fig. 12 shows the difference in film thickness between the silicon underlayer and the silicon dioxide underlayer in a BN film formation method according to this embodiment, which includes an aminosilane seed formation process. The rightmost graph in Fig. 12 shows the difference in film thickness between the silicon underlayer and the silicon dioxide underlayer in a BN film formation method according to this embodiment, which includes an aminosilane seed formation process and a diborane supply process.

[0094] As shown in FIG. 12, compared with the conventional BN film formation method shown on the far left, the film thickness of the BN film formed by the method according to this embodiment shown in the center is much closer to the film thickness of the silicon dioxide underlying portion than the silicon underlying portion.

[0095] Moreover, in the process shown on the right side of FIG. 12, in which a diborane supplying step was further added, the film thickness difference was significantly reduced and the film thickness itself was significantly increased.

[0096] Thus, according to this embodiment, it was shown that the difference in incubation time can be significantly reduced by performing an aminosilane seed formation process, and that by additionally performing a diborane supply process, the difference in incubation time can be reduced and the deposition rate can be significantly improved.

[0097] Figure 13 shows the results of Figure 12 reflected in the incubation time. Figure 13(a) shows the incubation time for a silicon substrate and a silicon dioxide substrate in a conventional BN film formation method. In Figure 13(a), H indicates the change in film thickness over time on a silicon substrate with a surface treatment, I indicates the change in film thickness over time on a silicon substrate without a surface treatment, and J indicates the change in film thickness over time on a silicon dioxide substrate.

[0098] As shown in FIG. 13(a), the difference in incubation time between the film thickness time change characteristic H on the surface-treated silicon base and the film thickness time change characteristic J when the base is a silicon dioxide film is large, being 14 minutes.

[0099] FIG. 13B shows the change over time in the thickness of the BN film in the method for forming a BN film according to this embodiment, which includes the aminosilane seed formation step.

[0100] As shown in FIG. 13(b), the difference in incubation time between the film thickness time change characteristic H on the surface-treated silicon base and the film thickness time change characteristic J when the base is a silicon dioxide film is significantly reduced to 4 minutes.

[0101] FIG. 13C shows the change over time in the thickness of the BN film in the method for forming a BN film according to this embodiment, which includes an aminosilane seed forming step and a diborane supplying step.

[0102] As shown in FIG. 13(c), the difference in incubation time between the film thickness time change characteristic H on the surface-treated silicon base and the film thickness time change characteristic J when the base is a silicon dioxide film is almost zero, at 0.5 minutes.

[0103] In this way, the difference in actual incubation time was also significantly improved, and this example demonstrated that the BN film formation method according to this embodiment can significantly reduce the dependency of the incubation time on the underlying film.

[0104] Although the preferred embodiments and examples of the present disclosure have been described in detail above, the present disclosure is not limited to the above-described embodiments and examples, and various modifications and substitutions can be made to the above-described embodiments and examples without departing from the scope of the present disclosure. [Explanation of symbols]

[0105] 10 Substrate (silicon) 20 Silicon dioxide film 30 Aminosilane Seed 40 Boron nitride film 50 OH group 60 SiH group 70 SiBH group 100 Film deposition equipment 107 Exhaust system 112 Wafer Boat 130 Processing gas supply mechanism 131a Boron-containing gas source 131b Nitrogen-containing gas source 131c Aminosilane Gas Source 131d Inert gas supply source 131e Carbon-containing gas sources 131f Halogen gas source 150 Control section S Processing Room W Semiconductor wafer

Claims

1. A step of forming a seed layer by supplying an aminosilane gas without supplying a nitrogen-containing gas onto a surface of a substrate having an underlayer with a different incubation time when forming a boron nitride film; depositing a boron nitride film on the seed layer; The substrates having different incubation times include silicon and silicon dioxide. A method for forming a boron nitride film.

2. 2. The method for forming a boron nitride film according to claim 1, wherein the aminosilane gas is diisopropylaminosilane gas.

3. 3. The method for forming a boron nitride film according to claim 1, wherein the step of depositing a boron nitride film on the seed layer comprises the step of supplying a boron-containing gas and a nitrogen-containing gas to perform CVD film formation on the seed layer.

4. The boron-containing gas is B 2 H 6 (Diborane), BCl 3 (trichlorosilane), TEB (triethylborane), TMB (trimethylborane) or DMAB (dimethylaminoborane); 4. The method for forming a boron nitride film according to claim 3, wherein the nitrogen-containing gas is ammonia.

5. 5. The method for forming a boron nitride film according to claim 1, further comprising the step of depositing a carbon film on the boron nitride film.

6. The method for forming a boron nitride film according to any one of claims 1 to 5, further comprising the step of supplying a boron-containing gas to the substrate between the step of forming the seed layer and the step of depositing the boron nitride film.

Citation Information

Patent Citations

  • Boron film interface technology

    JP2012531045A

  • Carbon film deposition method and deposition device

    JP2014033186A

  • Film forming method and film forming apparatus

    JP2017175106A

  • Remote plasma based deposition of boron nitride, boron carbide, and boron carbonitride films