Oil-in-water silicone emulsion composition and its uses
The oil-in-water silicone emulsion composition addresses the issues of film strength and tackiness by using a specific formulation of polyorganosiloxane, colloidal silica, and emulsifiers, resulting in a uniform, tack-free film with improved adhesion and friction reduction.
Patent Information
- Application Number
- JP2021528192
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-21
- Filing Date
- 2020-06-12
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-06-12
AI Technical Summary
Existing oil-in-water silicone emulsion compositions face issues with insufficient film strength, adhesion to substrates, and surface tackiness, particularly on smooth surfaces, limiting their application to substrates requiring good feel and friction-reducing properties.
An oil-in-water silicone emulsion composition containing a specific ratio of polyorganosiloxane, colloidal silica, and emulsifiers, including a polyoxyethylene-polyoxypropylene copolymer, to form a cured film with improved adhesion, reduced surface tackiness, and friction-reducing properties.
The composition forms a uniform, smooth, and tack-free cured film with excellent adhesion and rubber-like elasticity, suitable for various substrates, including those requiring friction reduction.
Smart Images

Figure 0007575180000001 
Figure 0007575180000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an oil-in-water silicone emulsion composition, in particular to an oil-in-water silicone emulsion composition which contains a relatively large amount of colloidal silica and uses thereof, and more particularly to an oil-in-water silicone emulsion composition which contains colloidal silica and which, upon removal of moisture, is capable of forming a friction-reducing cured coating which has rubber-like elasticity and a non-sticky surface.
[0002] Oil-in-water silicone emulsion compositions that form a cured film having releasability, peelability, water repellency, stain resistance, and heat resistance by removing water are used in paints, paper coating agents, release agents, stripping agents, fiber treatment agents, cosmetics, etc. As such a technique, a composition consisting of a hydroxyl group-containing diorganosiloxane, a silicone resin, and an aminoxy group-terminated diorganosiloxane (see, for example, Patent Document 1), a composition in which a hydroxyl group-containing diorganosiloxane and a compound selected from a linear siloxane having an aminoxy group on a side chain as a crosslinking agent, a cyclic aminoxysiloxane, an aminoxysilane, and a partial hydrolysis product thereof are mixed and emulsified (see, for example, Patent Document 2), etc. have been proposed. However, these compositions have problems in that the strength of the cured film and the adhesion of the cured film to the substrate are insufficient, and further, the adhesiveness remains on the substrate surface.
[0003] In order to solve this problem, oil-in-water silicone emulsion compositions containing colloidal silica have been proposed, for example as disclosed in Patent Documents 3 to 6, and the present applicants have also proposed in Patent Document 7 an oil-in-water silicone emulsion composition which does not require an organotin compound as a curing catalyst, has a low content of volatile siloxane oligomers, and is capable of forming a cured coating having rubber-like elasticity by removing moisture, and uses thereof.
[0004] However, these compositions still have room for improvement in terms of the strength of the cured coating and the adhesion of the cured coating to the substrate. In addition, the surface of the cured coating remains tacky, which means that these compositions cannot be used in applications requiring substrates that are particularly demanding a smooth surface / feel or a surface with reduced friction. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 06-73291 [Patent Document 2] Japanese Patent Application Publication No. 11-193349 [Patent Document 3] Japanese Patent Publication No. 56-16553 [Patent Document 4] Japanese Patent Publication No. 59-152972 [Patent Document 5] Japanese Patent Application Publication No. 09-165554 [Patent Document 6] Japanese Patent Application Publication No. 10-168393 [Patent Document 7] International Publication Pamphlet WO2012 / 002571 (Patent Registration No. 5848704) Summary of the Invention [Problem to be solved by the invention]
[0006] The object of the present invention is to provide an oil-in-water silicone emulsion composition which can be applied evenly to a substrate and which, by removing moisture, is capable of forming a cured coating which has little surface tack and which has excellent adhesion to the substrate and film strength, as well as uses and a production method for the same. [Means for solving the problem]
[0007] As a result of intensive research aimed at solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by an oil-in-water silicone emulsion composition comprising: (A) 100 parts by mass of a polyorganosiloxane having at least two hydroxyl groups or hydrolyzable groups bonded to silicon atoms in each molecule and having a viscosity at 25°C in the range of 100,000 to 20,000,000 mPa s; (B) 45 to 120 parts by mass of colloidal silica (converted to solids content); (C1) 1 to 100 parts by mass of an ionic emulsifier; and (D) 0 to 500 parts by mass of water (excluding the water content in the colloidal silica), preferably further containing 0.1 to 50 parts by mass of (C2) a polyoxyethylene-polyoxypropylene copolymer type nonionic emulsifier, and using the same as a surface treatment agent, thereby completing the present invention. Due to the above-mentioned configuration, the oil-in-water silicone emulsion composition is capable of forming a cured coating that has excellent adhesion to substrates and excellent coating strength, and because it contains a relatively large amount of colloidal silica (calculated on a solids basis) compared to component (A), the surface of the cured coating that is formed is smooth and tack-free, making it possible to form a cured coating that is smooth on the surface of the substrate and has excellent friction-reducing properties. Effect of the Invention
[0008] The oil-in-water silicone emulsion composition of the present invention can be applied uniformly to the surface of a substrate, and since it contains a relatively large amount of colloidal silica (solid content equivalent) relative to the component (A), it can form a cured film with low surface tackiness (tackiness) and excellent adhesion to the substrate and film strength by removing water.The oil-in-water silicone emulsion composition has rubber-like elasticity by removing water, and can form a cured film with no tackiness and friction reduction, so it can be suitably used as a surface treatment agent, and can provide a substrate with the cured film.
[0009] According to the method for producing the oil-in-water silicone emulsion composition of the present invention, the oil-in-water silicone emulsion composition of the present invention can be produced efficiently.In addition, according to the surface treatment method of the present invention, it is possible to efficiently form a cured coating film on the surface of a wide variety of substrates, which has sufficient strength, i.e., rubber-like elasticity and sufficient adhesion to the substrate, and has little surface tackiness (tack), is smooth, and has excellent friction reducing properties. BEST MODE FOR CARRYING OUT THEINVENTION
[0010] The oil-in-water silicone emulsion composition of the present invention will now be described in detail.
[0011] [Component (A)] Component (A) is a polyorganosiloxane having at least two groups selected from the group consisting of hydroxyl groups, alkoxy groups, and alkoxyalkoxy groups bonded to silicon atoms in each molecule, and having a viscosity of 100,000 to 20,000,000 mPa·s at 25°C, and is the main component of the oil-in-water silicone emulsion composition of the present invention. The molecular structure of the polyorganosiloxane of component (A) may be linear, cyclic, branched, dendritic, or network-like, but is preferably linear or partially branched linear. The group selected from the group consisting of hydroxyl groups, alkoxy groups, and alkoxyalkoxy groups may be present at the molecular chain terminals, side chains, or both. The alkoxy group is preferably an alkoxy group having 1 to 10 carbon atoms, such as a methoxy group, ethoxy group, n-propoxy group, isopropoxy group, n-butoxy group, t-butoxy group, hexyloxy group, cyclohexyloxy group, octyloxy group, or decyloxy group, and the alkoxyalkoxy group is preferably an alkoxyalkoxy group having 2 to 10 carbon atoms, such as a methoxymethoxy group, methoxyethoxy group, ethoxymethoxy group, or methoxypropoxy group.
[0012] Examples of organic groups bonded to silicon atoms other than groups selected from the group consisting of hydroxyl groups, alkoxy groups, and alkoxyalkoxy groups include unsubstituted monovalent hydrocarbon groups and substituted monovalent hydrocarbon groups. From the viewpoint of emulsification-assisting action, the unsubstituted monovalent hydrocarbon group is preferably one having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, or an alkenyl group having 2 to 10 carbon atoms, and particularly preferably a methyl group or a phenyl group.
[0013] Examples of the substituted monovalent hydrocarbon group include the above-mentioned unsubstituted monovalent hydrocarbon groups, particularly groups in which some or all of the hydrogen atoms of an alkyl group or phenyl group having 1 to 10 carbon atoms have been substituted with a substituent such as a halogen atom such as fluorine or chlorine; an epoxy functional group; a methacryl functional group; an acrylic functional group; an amino functional group; a sulfur-containing functional group; an alkoxy group; a hydroxycarbonyl group; or an alkoxycarbonyl group.
[0014] From the standpoint of the strength of the cured coating obtained by removing water from the oil-in-water silicone emulsion composition of the present invention, its adhesion to the substrate, and the reduction in surface tack and friction of the cured coating containing component (B), the viscosity of component (A) at 25°C is in the range of 100,000 mPa·s to 20,000,000 mPa·s, more preferably in the range of 300,000 mPa·s to 10,000,000 mPa·s, even more preferably in the range of 500,000 mPa·s to 5,000,000 mPa·s, and most preferably in the range of 750,000 mPa·s to 3,500,000 mPa·s. If the viscosity of component (A) is less than the lower limit, even if the amount of component (B) is within the range described below, the strength of the cured film obtained by removing water from the oil-in-water silicone emulsion composition and its adhesion to the substrate may be insufficient, and the surface of the cured film may become tacky, making it impossible to achieve a smooth surface. On the other hand, if the viscosity of component (A) exceeds the upper limit, synthesis by emulsion polymerization is difficult, and problems arise in that it is difficult to obtain a stable emulsion by conventional methods.
[0015] The component (A) is preferably a diorganopolysiloxane blocked at both molecular chain terminals with hydroxyl groups. Examples of such diorganopolysiloxanes blocked at both molecular chain terminals with hydroxyl groups include those represented by the general formula: HO(R 1 2SiO) m An example of the polyorganosiloxane is represented by the formula: 1 is the same as the unsubstituted or substituted monovalent hydrocarbon group bonded to a silicon atom other than a hydroxyl group or a hydrolyzable group described above, and is preferably an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, or an alkenyl group having 2 to 10 carbon atoms, and is particularly preferably a methyl group or a phenyl group. m is an integer of 2 or more, and is preferably a number that results in a viscosity at 25°C in the above-mentioned viscosity range of 100,000 mPa s to 20,000,000 mPa s.
[0016] As such component (A), a polyorganopolysiloxane having the above structure can be used, and there are no particular limitations on the production method thereof. A polyorganopolysiloxane obtained by a known production method such as an equilibrium polymerization method may be emulsified in water with an emulsifier such as component (C1) described below. However, from the standpoint of handling during production and particle size and stability during emulsion dispersion, it is preferable to use an organopolysiloxane obtained by emulsion polymerization using an organopolysiloxane with a lower degree of polymerization, which is the precursor of component (A).
[0017] Particularly preferred is a polyorganosiloxane obtained by emulsion polymerization of precursors of component (A), namely (a) a polyorganosiloxane having at least two hydroxyl groups or hydrolyzable groups bonded to silicon atoms per molecule, and (b) an aminoxy group-containing organosilicon compound having an average of two aminoxy groups bonded to silicon atoms per molecule, in the presence of component (C1) described below, or more preferably in the presence of component (C2).
[0018] The precursor of component (A), (a) polyorganosiloxane having at least two hydroxyl groups or hydrolyzable groups bonded to silicon atoms in each molecule, is a raw material component constituting the above-mentioned component (A), and is preferably a linear polyorganosiloxane having hydroxyl groups or hydrolyzable groups bonded to silicon atoms at both ends of the molecular chain, and having a lower viscosity than component (A). More specifically, component (a) is a diorganopolysiloxane capped with hydroxyl groups at both molecular chain ends, and having a viscosity at 25°C lower than that of component (A), particularly 100,000 mPa·s or less, preferably 50 to 50,000 mPa·s, and most preferably HO(R 1 2SiO) n H, and n is a number that gives the viscosity of component (a) at 25°C in the above-mentioned viscosity range, preferably in the range of 50 to 50,000 mPa s. 1 is the same as the above-mentioned unsubstituted or substituted monovalent hydrocarbon group bonded to a silicon atom other than a hydroxyl group or a hydrolyzable group, and is particularly preferably a methyl group or a phenyl group.
[0019] (b) Aminoxy group-containing organosilicon compounds, which have an average of two aminoxy groups bonded to silicon atoms per molecule, are components that promote the reaction and crosslinking of components (a) with each other, thereby promoting the formation of a cured coating that has good surface hardness and rubber-like elasticity without a tacky feel.
[0020] Component (b) contains an average of two aminoxy groups bonded to silicon atoms per molecule, and the aminoxy groups may be present only on the side chains of the molecular chain, or only on both ends of the molecular chain, or an average of one each on both the end and the side chain of the molecular chain. If component (b) contains an average of three or more aminoxy groups per molecule, gelation of the mixture is likely to occur inside the emulsification equipment during emulsification or in the pre-mixing step before emulsification, and the gel may adhere to the production equipment and the elongation of the resulting cured coating may be poor.
[0021] Examples of such aminoxy group-containing organosilicon compounds include polydiorganosiloxanes capped with aminoxy groups at both molecular chain terminals, diorganosiloxane-organoaminooxysiloxane copolymers capped with aminoxy groups at one molecular chain terminal, diorganosiloxane-organoaminooxysiloxane copolymers capped with triorganosilyl groups at both molecular chain terminals, cyclic diorganosiloxane-organoaminooxysiloxane copolymers, and diaminooxydiorganosilanes. Among these, polydiorganosiloxanes capped with aminoxy groups at both molecular chain terminals are preferred. The blending amount of component (b) is 0.1 to 100 parts by mass, preferably 0.5 to 50 parts by mass, and more preferably 1 to 20 parts by mass, per 100 parts by mass of component (a).
[0022] Component (b) preferably has the general formula: R 2 R 1 2SiO(R 1 R 3 SiO) n (R 1 2SiO) p SiR 1 2R 2 In the above formula, R 1 is the same as above, and among them, an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, or an alkenyl group having 2 to 10 carbon atoms is preferable, and a methyl group or a phenyl group is particularly preferable. 3 is an aminoxy group. When n is 0, R 2 is an aminoxy group; when n is 1, R 2 One of the R 2 is a group selected from the group consisting of unsubstituted monovalent hydrocarbon groups having 1 to 10 carbon atoms, halogen-substituted monovalent hydrocarbon groups having 1 to 10 carbon atoms, hydroxyl groups, alkoxy groups having 1 to 10 carbon atoms, and alkoxyalkoxy groups having 2 to 10 carbon atoms; when n is 2, R 2 is a group selected from the group consisting of unsubstituted monovalent hydrocarbon groups having 1 to 10 carbon atoms, halogen-substituted monovalent hydrocarbon groups having 1 to 10 carbon atoms, hydroxyl groups, alkoxy groups having 1 to 10 carbon atoms, and alkoxyalkoxy groups having 2 to 10 carbon atoms.
[0023] Examples of the unsubstituted monovalent hydrocarbon include the same groups as those mentioned above, among which alkyl groups having 1 to 10 carbon atoms, aryl groups having 6 to 10 carbon atoms, and alkenyl groups having 2 to 10 carbon atoms are preferred, and in particular, methyl or phenyl groups are preferred. Examples of the halogen-substituted monovalent hydrocarbon group include the unsubstituted monovalent hydrocarbon group described above, in which some or all of the hydrogen atoms are substituted with halogen atoms, and halogen-substituted alkyl groups such as chloromethyl, 3,3,3-trifluoropropyl, 3,3,4,4,5,5,5-heptafluoropentyl, and difluoromonochloropropyl are preferred. Examples of the alkoxy group and alkoxyalkoxy group include the same groups as those mentioned above.
[0024] The aminoxy group is -ON(R 4 ) 2 and groups represented by the following formulas: [ka] R in the formula 4 is a linear or branched alkyl group having 1 to 5 carbon atoms. 5is a divalent hydrocarbon group having 2 to 15 carbon atoms or a divalent organic group having a molecular chain main chain consisting of 3 to 17 carbon atoms and 1 to 3 nitrogen atoms or 1 to 2 oxygen atoms, and examples thereof include -(CH2)2-, -(CH2)5-, -(CH2)6-, -(CH2)7-, -(CH2)2-O-(CH2)2-, -(CH=CH)-(CH=CH)-, -(CH=N)-(CH=CH)-, and -(C6H4)-(CH2)2-. Among these, -(CH2)6- and -(CH2)2-O-(CH2)2- are preferred. Among these, a dialkylaminoxy group in which an alkyl group having 1 to 5 carbon atoms is bonded to a nitrogen atom is preferable, and preferable examples of the aminoxy group include a dimethylaminoxy group, a diethylaminoxy group, a dipropylaminoxy group, a dibutylaminoxy group, a diheptylaminoxy group, an ethylmethylaminoxy group, a propylmethylaminoxy group, a propylethylaminoxy group, a butylmethylaminoxy group, a butylethylaminoxy group, a butylpropylaminoxy group, a heptylmethylaminoxy group, a heptylethylaminoxy group, a heptylpropylaminoxy group, and a heptylbutylaminoxy group, and a diethylaminoxy group is preferable.
[0025] In the above formula, n is 0, 1 or 2, preferably 0 or 2, and more preferably 0. When n is 0, R 2 is an aminoxy group, and when n is 1, R 2 At least one of the above formulas is an aminoxy group. 2 is preferably an aminoxy group from the viewpoint of availability.
[0026] In the formula, p is an integer of 0 or more. There is no particular upper limit to the upper limit of p. However, in terms of ease of emulsification, p is preferably an integer in the range of 0 to 1000, more preferably an integer in the range of 2 to 200, and most preferably an integer in the range of 4 to 140.
[0027] Examples of such aminoxy group-containing organosilicon compounds include those represented by the following formula: In the formula, Me represents a methyl group, Et represents an ethyl group, and Pr represents a propyl group. (Et2NO)Me2SiOSiMe2(ONEt2) (Et2NO)Me2SiO(Me2SiO) 12 SiMe2(ONEt2) (Et2NO)Me2SiO(Me2SiO) 40 SiMe2(ONEt2) (Et2NO)Me2SiO(Me2SiO) 80 SiMe2(ONEt2) Me2Si(ONEt2)2 Me3SiO(MeSi(ONEt2)O)2SiMe3 Me3SiO(Me2SiO)4(MeSi(ONEt2)O)2SiMe3 Me3SiO(Me2SiO) 15 (MeSi(ONEt2)O)2SiMe3 Me3SiO(Me2SiO)3(MeSi(ONEt2)O)7SiMe3
[0028] Furthermore, when component (b) remains in the oil-in-water silicone emulsion composition, it is a component that contributes to the reaction and crosslinking of component (A) and component (B), making it possible to form a cured coating that has good surface hardness and rubber-like elasticity without a tacky feel.
[0029] [(B) Component] (B) Colloidal silica is a component that improves the strength of the cured coating and its adhesion to the substrate. When the composition of the present invention contains a relatively large amount of colloidal silica, calculated as solids, compared to component (A), it is a component that can form a cured coating on the substrate surface that has little surface adhesion (tack) and is smooth and has excellent friction-reducing properties.
[0030] Colloidal silica is available as an aqueous dispersion in which 5 to 40% by mass of silica particles are colloidally dispersed in water, has many silanol groups on the surface, and generally has a particle diameter of about 1 nm to 1 μm. Such colloidal silica is preferably a basic aqueous dispersion stabilized by sodium ions or ammonium ions. The pH of colloidal silica as a basic aqueous dispersion is preferably 7.0 or more, more preferably more than 9.0. The shape of the silica fine particles of colloidal silica is not particularly limited, and is generally spherical, but elongated or pearl necklace-shaped ones may also be used.
[0031] In the present invention, the blending amount of the (B) component, calculated as the solid content, must be within the range of 45 to 120 parts by mass per 100 parts by mass of the (A) component, is preferably within the range of 50 to 110 parts by mass, and particularly preferably within the range of 55 to 100 parts by mass.
[0032] Here, the solid content of colloidal silica refers to the non-volatile silica particle content, and when the blending amount of component (B) is within the above range, the cured film surface obtained by removing water from the oil-in-water silicone emulsion composition of the present invention and mainly consisting of component (A) or its crosslinking reaction product can be given smoothness. On the other hand, when the blending amount of component (B) is less than the above lower limit, the cured film surface may become sticky (tacky). On the other hand, when the blending amount of component (B) exceeds the above upper limit, the flexibility, rubber elasticity, and conformability and adhesion to the substrate surface of the cured film may become insufficient, and the obtained cured film may crack or peel off, and furthermore, the cured film surface may become sticky (tacky).
[0033] When the polyorganosiloxane of the (A) component is obtained by emulsion polymerization, the colloidal silica of the (B) component can be added during or after polymerization. Specifically, an aqueous dispersion of colloidal silica particles containing water may be added to an emulsion containing the polyorganosiloxane of the (A) component, or an aqueous dispersion of colloidal silica particles may be added to an emulsion containing the (a) component, which is a precursor of the (A) component, to proceed with emulsion polymerization reaction.
[0034] Examples of such colloidal silica include Snowtex 20, Snowtex 30, etc. manufactured by Nissan Chemical Industries, Ltd.; Adelite AT-20, etc. manufactured by Asahi Denka Kogyo Co., Ltd.; Crebosol 30R9, etc. manufactured by Clariant Japan K.K.; Ludox (trademark) HS-40, etc. manufactured by DuPont; Cataloid S-20L, etc. manufactured by Catalysts and Chemicals Industry Co., Ltd.; and Silicadol-20 manufactured by Nippon Chemical Industry Co., Ltd.
[0035] [(C1) component] The ionic emulsifier of component (C1) is a component that stably emulsifies component (A) and, if necessary, component (F) in component (D). The blending amount of component (C1) is 1 to 100 parts by mass, preferably 1 to 50 parts by mass, and more preferably 1 to 20 parts by mass, per 100 parts by mass of component (A).
[0036] The ionic emulsifier of component (C1) can be an anionic surfactant, a cationic surfactant, or an amphoteric surfactant. As the ionic emulsifier, one of these surfactants may be used alone, or two or more different types of surfactants may be used in combination.
[0037] Examples of anionic surfactants include alkylbenzene sulfonates, alkyl ether sulfates, polyoxyethylene alkyl ether sulfates, polyoxyethylene alkyl phenyl ether sulfates, alkyl naphthyl sulfonates, unsaturated aliphatic sulfonates, and hydroxylated aliphatic sulfonates.
[0038] Examples of cationic surfactants include alkyltrimethylammonium salts such as octadecyltrimethylammonium chloride and hexadecyltrimethylammonium chloride; and quaternary ammonium salt surfactants such as dialkyldimethylammonium salts such as dioctadecyldimethylammonium chloride, dihexadecyldimethylammonium chloride and didecyldimethylammonium chloride.
[0039] Examples of amphoteric surfactants include alkylbetaines and alkylimidazolines.
[0040] From the standpoint of stability, it is preferable to use the ionic emulsifier (C1) in the oil-in-water silicone emulsion composition of the present invention in combination with other nonionic emulsifiers.
[0041] As the nonionic emulsifier usable in the present invention, a known nonionic surfactant can be used. Examples of the nonionic surfactant include glycerin fatty acid ester, sorbitan fatty acid ester, polyoxyalkylene alkyl ether, polyoxyalkylene alkylphenyl ether, polyoxyalkylene sorbitan fatty acid ester, polyoxyalkylene glycerin fatty acid ester, and polyoxyethylene-polyoxypropylene copolymer type nonionic emulsifier.
[0042] [(C2) component] In particular, the oil-in-water silicone emulsion composition of the present invention preferably further comprises (C2) polyoxyethylene-polyoxypropylene copolymer type nonionic emulsifier as a nonionic emulsifier.By using the above-mentioned (C1) component and (C2) component in combination, the (A) component and the (F) component can be stably emulsified in the (D) component, which is a dispersion medium, with small particle size, and in particular, when the (A) component is formed by emulsion polymerization, the emulsion polymerization reaction can be stably progressed, and the emulsion of the (A) component, which is a highly stable emulsion polymerization reaction product, can be obtained.
[0043] The polyoxyethylene-polyoxypropylene copolymer nonionic emulsifier, which is the component (C2), is usually a compound represented by the following general formula (1) or general formula (2). HO(CH2CH2O) a (CH(CH3)CH2O) b (CH2CH2O) C H (1) HO(CH(CH3)CH2O) d (CH2CH2O) e (CH(CH3)CH2O) f H (2) In the general formulas (1) and (2), a, b, c, d, e, and f are the average number of moles of ethylene oxide or propylene oxide added, and are each independently a number from 1 to 350. The weight average molecular weight of the component (C2) is preferably from 1,000 to 18,000, and more preferably from 1,500 to 10,000. When the component (C2) is in a solid state, it can be used in the form of an aqueous solution.
[0044] More specifically, examples of the compound which is component (C2) include the "Pluronic (registered trademark) L" series, "Pluronic (registered trademark) P" series, "Pluronic (registered trademark) F" series, and "Pluronic (registered trademark) TR" series manufactured by ADEKA CORPORATION; Emulgen PP-290 manufactured by Kao Corporation; and Newcol 3240 manufactured by Nippon Nyukazai Co., Ltd., which are available on the market.
[0045] The amount of component (C2) blended is 0.1 to 50 parts by mass, and preferably 1 to 20 parts by mass, per 100 parts by mass of component (A). When component (C2) is used in combination with component (C1) to emulsify component (A) or its precursor component, and other optional components such as component (F), the particle size of the resulting emulsion particles can be made smaller than that of each component alone, and the stability of the emulsion composition can be improved.
[0046] The total amount of components (C1) and (C2) is generally preferably 1 to 30% by mass, more preferably 2 to 20% by mass, of the total amount of component (A) and optional component (F). The ratio of the amount of component (C1) to the amount of component (C2) is preferably in the range of 3:1 to 100:1.
[0047] It is also possible to use the above emulsifiers for components (C1) and (C2) to emulsify and disperse in water cyclic siloxanes, diorganopolysiloxanes capped with hydroxyl groups at both molecular chain terminals, organoalkoxysilanes, etc., and then, if necessary, add a catalyst such as an acid or alkaline substance to carry out a polymerization reaction. It is also possible to use the above emulsifiers to emulsify and disperse in water a polyorganosiloxane having per molecule at least two groups selected from the group consisting of hydroxyl groups, alkoxy groups and alkoxyalkoxy groups bonded to silicon atoms, and an aminoxy group-containing organosilicon compound having per molecule an average of two aminoxy groups bonded to silicon atoms, and this is particularly suitable in that it is possible to obtain a stable emulsion containing the highly viscous component (A).
[0048] [(D) component] The amount of water used as component (D) is not particularly limited as long as it is sufficient to maintain a stable aqueous emulsion state, but it is usually 0 to 500 parts by mass, and preferably 10 to 200 parts by mass, per 100 parts by mass of component (A).
[0049] In this composition, the component (D) is water added independently of the component (B). Here, water is an essential component in the oil-in-water emulsion composition of the present invention, but the colloidal silica of the component (B) is in the form of an aqueous dispersion as described above, and the amount of water in the component (D) may be 0 parts by mass if there is moisture contained when the component (B) is blended (for example, an aqueous dispersion of colloidal silica with a solid content of 30% by mass contains 70% by mass of moisture). In addition, when the entire emulsion composition is taken as 100% by mass, the amount of water derived from the components (B) and (D) is generally in the range of 5 to 95% by mass of the entire composition.
[0050] [(E) component] The oil-in-water emulsion composition of the present invention preferably further contains one or more (E) thickeners from the viewpoint of improving the workability such as the coating property and the storage stability of the composition, particularly the dispersion stability of the (B) component. In particular, by using a thickener containing a water-soluble organic polymer such as a water-soluble acrylic resin or an inorganic thickener such as a clay mineral, the viscosity of water can be increased, and there is an advantage that the coating property and workability of the oil-in-water emulsion composition of the present invention or the surface treatment agent containing the same to the substrate can be improved without substantially impairing the technical effect of the present invention and the heat resistance / flame retardancy of the cured coating. The amount of the (E) thickener to be added is arbitrary, and when a thickener is used, it is preferable to appropriately select an amount that makes the entire composition have a viscosity range described below (1,000 mPas or more at 25 ° C.).
[0051] The thickener used in the present invention is not particularly limited, but preferred examples of the thickener include one or more types selected from (E1) thickeners containing clay minerals and (E2) thickeners containing water-soluble organic polymers.
[0052] The clay mineral may be either a natural or synthetic product, and examples thereof include natural or synthetic smectite clays such as bentonite, which are mainly composed of clay minerals, and hydrophilic composites made of such smectite clays and anionic polymers such as polyacrylic acid and carboxyvinyl polymers. In other words, component (E) may and preferably contains a thickener made of a water-soluble organic polymer other than a clay mineral.
[0053] Specifically, examples of thickeners containing natural or synthetic clay minerals (E1) include natural or synthetic smectite clays such as bentonite, montmorillonite, hectorite, saponite, sauconite, beidellite, and nontronite; magnesium aluminum silicate; and composites of these with water-soluble organic polymers such as carboxyvinyl polymers, with smectite clays such as bentonite and montmorillonite being preferred. As such smectite clays, for example, Sumecton SA (manufactured by Kunimine Kogyo Co., Ltd.), which is a hydrothermal synthesis product, and Bengel (manufactured by Hojun Co., Ltd.), which is a natural refined product, are available.
[0054] When imparting heat resistance and flame retardancy to a substrate (such as airbag fabric or building material) coated with the oil-in-water silicone emulsion composition of the present invention, the pH of the smectite clay is preferably within the range of pH 5.0 to 9.0.
[0055] (E2) Examples of thickeners containing water-soluble organic polymers include water-soluble organic polymers such as polymeric polysaccharides and water-soluble acrylic resins, which may be used alone or in the form of a hydrophilic complex with clay minerals. In particular, the use of water-soluble organic polymers containing carboxylate groups is preferred, and examples thereof include polyacrylic acids, which are carboxyl-containing addition polymers such as sodium polyacrylate or sodium polymethacrylate. If the amount of thickeners made of these water-soluble organic polymers is excessive, the heat resistance and flame retardancy of the cured coating obtained by removing water from the oil-in-water silicone emulsion composition of the present invention may be impaired, so it is preferable to select the amount used according to the application.
[0056] Component (E) may be in the form of an aqueous dispersion of a thickener made of the above-mentioned clay mineral or water-soluble organic polymer. In particular, the content of the inorganic thickener which is a clay mineral is preferably within the range of 0.1 to 10 parts by mass, or within the range of 0.5 to 5 parts by mass, per 100 parts by mass of water.
[0057] [Component (F)] In order to improve the strength and adhesion of the cured coating, the oil-in-water silicone emulsion composition of the present invention further comprises (F) a compound represented by the general formula: R 1 a Six 4-a In the formula, R is the same as above, and among them, it is preferable that it is an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, or an alkenyl group having 2 to 10 carbon atoms, and in particular, it is preferable that it is a methyl group or a phenyl group. X is an alkoxy group having 1 to 10 carbon atoms or an alkoxyalkoxy group having 2 to 10 carbon atoms, and examples thereof include the same groups as above. a is 0, 1, or 2, and is preferably 0 or 1. In particular, the component (F) is preferably a tetraalkoxysilane, an alkyltrialkoxysilane, a tetraalkoxyalkoxysilane, or an alkyltrialkoxyalkoxysilane, and more preferably a tetraalkoxysilane or an alkylalkoxysilane.
[0058] The component (F) may be a partial hydrolysis condensate of the above-mentioned organoalkoxysilane, organoalkoxyalkoxysilane, tetraalkoxysilane, or tetraalkoxyalkoxysilane.
[0059] From the standpoint of improving the strength of the cured film and adhesion to the substrate, the (F) component is preferably blended in an amount of 0.1 to 50 parts by weight, and more preferably 1 to 15 parts by weight, per 100 parts by weight of the (A) component. If the blending amount of the (F) component is less than 0.1 part by weight per 100 parts by weight of the (A) component, the strength of the cured film obtained by removing water from the aqueous silicone emulsion composition produced may not be sufficiently improved, while if the blending amount exceeds 50 parts by weight, the amount of alcohol produced as a by-product increases, which may have adverse effects on the environment and human body and may change in the formability of the cured film over time, which is not preferable.
[0060] [(G) component] The oil-in-water silicone emulsion composition of the present invention preferably contains an amine compound (G) as a pH adjuster. The amine compound is preferably diethylamine. These components (G) also function as a curing catalyst (described later) when removing moisture, and therefore promote the condensation reaction of each component, making it possible to realize curing reactivity free of heavy metals such as tin.
[0061] The blend amount of component (G) as a pH adjuster is preferably in the range of 0.01 to 5 mass %, and more preferably in the range of 0.1 to 2 mass %, based on the total mass of the oil-in-water silicone emulsion composition of the present invention.
[0062] [Other optional ingredients] The oil-in-water silicone emulsion composition of the present invention may be appropriately blended with other components as necessary, such as pigments, antifoaming agents, penetrating agents, antistatic agents, inorganic powders, preservatives, rust inhibitors, silane coupling agents other than component (F) such as bis(trimethoxysilylpropyl)-disulfide, pH adjusters other than component (G), buffers, ultraviolet absorbers, curing catalysts, water-soluble resins, organic resin emulsions, pigments and solid lubricants, dyes, flame retardants, etc. When the oil-in-water silicone emulsion composition of the present invention is used for coating purposes, it is particularly preferable in practice to blend components selected from curing catalysts, pigments and solid lubricants, and flame retardants.
[0063] [Curing catalyst] The incorporation of a curing catalyst is optional, but can be incorporated in order to rapidly crosslink and cure the components of the composition of the present invention through a condensation reaction. Specific examples of the curing catalyst include organic tin compounds such as dibutyltin dilaurate, dibutyltin diacetate, tin octenate, dibutyltin dioctate, tin laurate, dioctyltin diversatate, dioctyltin diacetate, and dibutyltin bisoleyl maleate; organic tin compounds such as tetrabutyl titanate, tetrapropyl titanate, and dibutoxybis(ethylacetoacetate)titanium; Others include: acidic compounds such as hydrochloric acid, sulfuric acid, and dodecylbenzenesulfonic acid; alkaline compounds such as ammonia and sodium hydroxide; amine compounds such as n-hexylamine, guanidine, 1,8-diazabicyclo[5.4.0]undecene (DBU), and 1,4-diazabicyclo[2.2.2]octane (DABCO); organic zirconium esters such as zirconium tetrapropylate and zirconium tetrabutylate; and zirconium tributoxyacetylacetonate. zirconium-based condensation promoters such as organic zirconium chelates, zirconium butoxyacetylacetonate bisethylacetoacetate, zirconium tetraacetylacetonate, and the like; oxozirconium compounds, such as zirconium bis(2-ethylhexanoate)oxide, zirconium acetylacetonate(2-ethylhexanoate)oxide, and the like; aluminum alcoholates, such as aluminum triethylate, aluminum triisopropylate, aluminum tri(sec-butylate), and the like; aluminum chelate compounds, such as diisopropoxyaluminum(ethylacetoacetate), aluminum tris(ethylacetoacetate), and aluminum tris(acetylacetonate), and the like; aluminum-based condensation promoters, such as aluminum acyloxy compounds, such as hydroxyaluminum bis(2-ethylhexanoate), and the like; and condensation reaction catalysts such as organic acid metal salts, such as zinc stearate, zinc octylate, zinc acetate, and iron octylate, and the like. Except when the curing catalyst is water-soluble, it is preferable to prepare the curing catalyst in advance in the form of an emulsion by emulsifying and dispersing the catalyst in water using a surfactant.In addition, the above amine compounds are components common to the (G) component, and by using these components, it is possible to design a composition that does not contain a curing catalyst containing metals such as tin, which is preferable from the viewpoint of reducing environmental impact. In the composition of the present invention, the amount of the condensation reaction catalyst used is not particularly limited, and can be any amount within the range in which the purpose of promoting the condensation reaction is achieved. In addition, the use of the condensation reaction catalyst is optional, and it is not necessary to use it in this composition.
[0064] [Pigments and solid lubricants] The oil-in-water silicone emulsion composition of the present invention may and preferably contains a pigment or a solid lubricant.In particular, by containing a solid lubricant such as phyllosilicate, also known as layered silicate, the obtained cured coating film can be given antifriction properties that reduce friction and / or blocking, and the friction reducing properties can be further improved.
[0065] Specifically, examples of phyllosilicates suitable for use as solid lubricants in the present invention include mica, talc, e.g., talc microspheres, kaolinite, smectite, sericite, and chlorite.
[0066] As the pigment, for example, inorganic pigments such as aluminum hydroxide, heavy calcium carbonate, light calcium carbonate, titanium oxide, barium sulfate, activated clay, magnesium carbonate, alumina, and aluminum oxide, and organic pigments such as polystyrene resin particles, urea-formalin resin particles, and polyolefin particles can be selected.
[0067] [Flame retardant] When the oil-in-water silicone emulsion composition of the present invention is applied to applications such as airbag coating, it may further contain a flame retardant in practical use. For example, the composition according to the present invention is suitable for surface coating of airbags and the like because it forms a lubricating dry coating film that reduces friction and / or blocking on the substrate surface, but it is important that substrates such as airbags are difficult to ignite and do not support combustion by their nature, and the addition of a flame retardant is generally required to pass the strict flammability test that can be applied to the application. When the oil-in-water silicone emulsion composition of the present invention is applied (=topcoat) on a substrate such as an airbag coated with silicone rubber, flammability is generally suppressed, but when a topcoat that does not contain a flame retardant is applied to an airbag coated with an organic resin, it may not pass a flammability test such as the US Federal Motor Vehicles Safety Standards Test FMVSS#302 (hereinafter referred to as "FMVSS#302"), and the addition of a flame retardant is practically important.
[0068] In particular, the composition according to the present invention is suitable for use as a coating agent for applications requiring non-flammability / flame retardancy, such as the topcoat of an airbag or a covering fabric that is subsequently formed into an airbag, and the flame retardant is often most effective when present in the topcoat. An example of a preferred flame retardant is aluminum trihydrate, preferably not surface-treated. Flame retardants include other metal hydroxides such as magnesium hydroxide, metal oxides such as ferrite oxide and titanium oxide, carbonates such as zinc carbonate, and carbon black. The content of these flame retardant components may be in the range of 2 to 40% by mass, preferably 5 to 25% by mass, based on the total composition, and a component at least partly made of aluminum trihydrate may be selected as the flame retardant, and is preferred.
[0069] [Total viscosity of composition and viscosity measurement method] From the viewpoint of uniform application and workability, the viscosity of the oil-in-water silicone emulsion composition of the present invention is preferably 1000 mPa·s or more. The viscosity is measured at 25°C at a shear rate of 1 s-1 using a Wells-Brookfield Cone / Plate Viscometer equipped with a 2° tapered cone with a diameter of 20 mm (ASTM D4287). Unless otherwise indicated, the viscosity described in this specification is measured by the same method as above. In addition, the above viscosity is the total viscosity of the oil-in-water silicone emulsion composition including solid lubricants, thickeners, etc. as necessary.
[0070] The average particle size (average primary particle size) of the silicone emulsion particles in the oil-in-water silicone emulsion composition of the present invention may be in the range of 50 to 600 nm, preferably 300 nm or less, and particularly preferably 250 nm or less, from the viewpoints of storage stability, formability of a cured film, and stability when diluted with water. The average particle size of the emulsion particles can be measured by a dynamic light scattering method or the like.
[0071] [Manufacturing method] The oil-in-water silicone emulsion composition of the present invention comprises: Step (I): A step of emulsifying and dispersing component (A), component (C1), and, if necessary, a part of component (C2) and component (D) using an emulsifier such as a homomixer, a homogenizer, a colloid mill, a combimixer, an in-line continuous emulsifier, a vacuum emulsifier, an ultrasonic emulsifier, or a continuous mixer; and Step (II): A step of blending and dispersing component (B) and the remaining component (D) in the emulsion obtained in the previous step. The present invention can be produced by a production method including the steps of:
[0072] Here, the components (B), (E), (F) and (G) may be mixed in any of the above steps, or may be mixed in portions in both steps, as necessary.
[0073] In the production of the oil-in-water silicone emulsion composition of the present invention, the polyorganosiloxane, which is the component (A), may be obtained by emulsion polymerization. Specifically, the production method of the oil-in-water silicone emulsion composition of the present invention may include a step of obtaining a polyorganosiloxane by emulsion polymerization of (a) a polyorganosiloxane having at least two hydroxyl groups or hydrolyzable groups bonded to silicon atoms in one molecule, which is a precursor of the component (A), and (b) an aminoxy group-containing organosilicon compound having an average of two aminoxy groups bonded to silicon atoms in one molecule, in the presence of the component (C1) and, optionally, the component (C2). In this case, the aqueous dispersion containing the component (A), which is the polyorganosiloxane after emulsion polymerization, is an emulsion in which the component (A), the component (C1), the optional component (C2), and a part of the water (D) are emulsified and dispersed, and may be carried out simultaneously with the above-mentioned step (I) or as a part of the step (I). Subsequently, the above-mentioned step (II) may be carried out, and the components (B), (E), (F) and (G) may be added to the emulsion before the emulsion polymerization reaction, if necessary.
[0074] In the oil-in-water silicone emulsion composition of the present invention, the total content of siloxane oligomers consisting of 4 to 5 siloxane units may be reduced to 2% by mass or less, 1% by mass or less, or 0.5% by mass or less, if necessary. Examples of siloxane oligomers consisting of 4 to 5 siloxane units include cyclic siloxane oligomers having a 4 to 5 molar ratio, such as octaorganotetracyclosiloxane and decaorganopentacyclosiloxane; and linear siloxane oligomers having a 4 to 5 molar ratio, such as tetraorganodisiloxanes capped at both ends of the molecular chain with hydroxydiorganosiloxy groups, and hexaorganotrisiloxanes capped at both ends of the molecular chain with hydroxydiorganosiloxy groups. The content of siloxane oligomers in the oil-in-water silicone emulsion composition of the present invention can be measured by gas chromatography.
[0075] [Use of the above oil-in-water silicone emulsion composition: Surface treatment agent / surface modifier] The oil-in-water silicone emulsion composition described above can be applied to the surface of a substrate and the water removed by evaporation / heating or the like to form a cured coating that has rubber-like elasticity, is non-sticky on the surface, and has friction-reducing properties, and can therefore be used as a surface treatment agent for the purpose of modifying the surface of a substrate.
[0076] That is, the surface treatment method of the present invention is characterized by treating a substrate surface with a surface treatment agent containing the above-mentioned oil-in-water silicone emulsion composition, and at least a portion of the substrate surface is covered with the above-mentioned cured film, thereby modifying the surface condition. Here, the surface treatment agent may be the above-mentioned oil-in-water silicone emulsion composition or a water dilution thereof, and may optionally contain other additives.
[0077] The substrate to which the surface treatment agent of the present invention can be applied is not particularly limited, and examples thereof include metals, ceramics, concrete, cement, mortar, paper, fiber, natural fiber fabric, synthetic fiber fabric, nonwoven fabric, cloth, plastic, glass, rubber, wood, stone, and composite materials of other substrates. In particular, the surface treatment agent of the present invention can form a cured film having rubber-like elasticity and no adhesion on the surface and having friction reduction properties on the substrate surface by removing moisture, and therefore can be used for surface treatment of functional cloth such as airbags, emergency chutes of aircraft and hot air balloons, and building materials such as concrete to improve their functions. In addition, the silicone elastomer can impart water repellency, weather resistance, chemical resistance, soft texture, etc. to the surface of various substrates as required, and further, the silicone elastomer is expected to improve heat resistance and flame retardancy.
[0078] The method for treating a substrate surface with the oil-in-water silicone emulsion composition preferably comprises the steps of (I) applying the oil-in-water silicone emulsion composition to the substrate surface, and (II) removing water from the oil-in-water silicone emulsion composition on the substrate surface to form a cured coating.
[0079] As a specific means for step (I), coating methods and application methods used for paints and coating agents can be used without any particular limitation, and examples thereof include brush coating, spray coating, immersion (dipping), flow coater, dispenser coating, roller coating such as gravure roller, knife coating, spin coating, etc., and not only one coat but also multiple coats may be applied. Furthermore, before coating, the surface of the object to be coated / coated may be cleaned, dried, and coated with a primer. In addition, the amount of application / coating is not particularly limited, and the coating may be applied thinly to a functional fabric such as an airbag or its silicone rubber-coated surface to reduce weight, or applied thickly to the surface of a substrate to form a thick, durable cured film.
[0080] The moisture removal in step (II) may be carried out by leaving the material at room temperature to air dry, by leaving the material in an atmosphere adjusted to a temperature of 20 to 200° C., or by irradiating the material with infrared rays, ultraviolet rays, or other high-energy rays. EXAMPLES
[0081] The present invention will be described in detail below with reference to examples and comparative examples. In the examples, the viscosity is a value measured at 25° C., the parts expressing the blend amount mean parts by mass, and the % expressing the content means % by mass. In the formulas, Me represents a methyl group, and Et represents an ethyl group.
[0082] The average particle size of the emulsion particles was measured by dynamic light scattering at 25° C. using a submicron particle analyzer (COULTER MODEL N4 MD, manufactured by Coulter Electronics), and calculated by monodispersion mode analysis.
[0083] The viscosity of the emulsion compositions was measured at 25°C using a Wells-Brookfield Cone / Plate Viscometer equipped with a 20 mm diameter 2° tapered cone at a shear rate of 1 s (ASTM D4287).
[0084] [Evaluation of cured film] The oil-in-water silicone emulsion composition (film-forming composition) of each example was applied to the coated surface of a woven nylon airbag fabric by gravure roller coating, heat cured at 140°C, and evaluated for the following items: Uniformity: The uniformity of the coating film when the coating composition was applied at 20 g / m2 was evaluated visually. Antifriction properties: As an index of initial antifriction properties, evaluation was performed by measuring the dynamic friction coefficient when the coating composition was applied at 25 g / m2. Antifriction after scrubbing: After scrubbing 10 times with a finger, the surface was evaluated by touch with a finger.
[0085] [Example 1] (a) 92.5 parts of a polydimethylsiloxane terminated at both ends with a hydroxydimethylsiloxy group and having a viscosity of 2,400 mPa·s, (b) 7.5 parts of an aminoxy group-containing polysiloxane represented by the formula (1): Et2NO(Me2SiO)7NEt2, (C2) 7.5 parts of a polyoxyethylene-polyoxypropylene copolymer type nonionic emulsifier (manufactured by ADEKA, product name Pluronic (registered trademark) F108) that had been mixed uniformly in advance was mixed uniformly with (C1) a dispersion of 12.5 parts of a 40% aqueous solution of sodium alkanesulfonate, and emulsified using an emulsifier. 86 parts of water (D), 44.0 parts of colloidal silica (Nissan Chemical's Snowtex 30, 30% active ingredient, pH 10, colloidal silica whose surface is stabilized with sodium) (B-1), and 1.25 parts of diethylamine (G) were added to the obtained emulsion and mixed uniformly. 2.5 parts of methyltriethoxysilane (F) were added and mixed uniformly, and the mixture was left at room temperature for 2 weeks. Then, 125 parts of colloidal silica (Nissan Chemical's Snowtex 30, 30% active ingredient, pH 10, colloidal silica whose surface is stabilized with sodium) (B-2) were added and mixed uniformly to prepare an oil-in-water silicone emulsion (No. 1). The total amount of silica particles was 50.7 parts.
[0086] The viscosity of organopolysiloxane (A) obtained by emulsion polymerization after reaction was measured by the following procedure. (a) 92.5 parts of a polydimethylsiloxane with a viscosity of 2,400 mPa·s and terminated at both ends of the molecular chain with hydroxydimethylsiloxy groups, (b) 7.5 parts of an aminoxy group-containing polysiloxane represented by formula (1): Et2NO(Me2SiO)7NEt2, were mixed uniformly with (C2) 7.5 parts of a polyoxyethylene-polyoxypropylene copolymer type nonionic emulsifier (manufactured by ADEKA, product name Pluronic (registered trademark) F108) that had been mixed and homogenized in advance, and (C1) a dispersion of 12.5 parts of a 40% aqueous solution of sodium alkanesulfonate, and emulsified using an emulsifier. After leaving to stand for one week, 10 g of the prepared emulsion was added with stirring to 10 g of isopropyl alcohol, and only the precipitated dimethylsiloxane was dried at 105°C for 3 hours and measured using a Brookfield type viscometer. The viscosity at 25°C was 1,800,000 mPas.
[0087] (E) 73 parts of a 1.5% anionic polymer composite refined bentonite (product name: Bengel W100U: Hojun Co., Ltd.) aqueous solution and 15 parts of talc powder were mixed into a dispersion, and 12 parts of the silicone emulsion (No. 1) obtained above was uniformly mixed to obtain an oil-in-water silicone emulsion composition (=coating composition) of the present invention.
[0088] The resulting oil-in-water silicone emulsion was left at 25°C for six months, after which no separation was observed and the dispersion was stable. When evaluated using the method described above, it was found to be able to form a cured film. The evaluation results are shown in Table 1.
[0089] [Example 2] Except for changing the total amount of silica particles to 65.7 parts, a silicone emulsion (No. 2) and a coating composition were prepared in the same manner as in Example 1, and evaluations were carried out in the same manner as in Example 1. The evaluation results are shown in Table 1.
[0090] [Example 3] Except for changing the total amount of silica particles to 73.2 parts, a silicone emulsion (No. 3) and a coating composition were prepared in the same manner as in Example 1, and evaluations were carried out in the same manner as in Example 1. The evaluation results are shown in Table 1.
[0091] [Comparative Example 1] Except for changing the total amount of silica particles to 24.75 parts, a silicone emulsion (No. C1) and a coating composition were prepared in the same manner as in Example 1, and evaluations were carried out in the same manner as in Example 1. The evaluation results are shown in Table 1.
[0092] [Comparative Example 2] A silicone emulsion (No. C2) and a coating composition were prepared in the same manner as in Example 1, except that the total amount of silica particles was changed to 35.7 parts, and evaluations were carried out in the same manner as in Example 1.
[0093] [Table 1]
[0094] [Summary] The oil-in-water silicone emulsion compositions (=coating compositions) of Examples 1 to 3 had colloidal silica solids within the range of the present invention, formed coatings with excellent uniformity, and had excellent anti-friction properties from the initial stage to after scrubbing, and were able to form smooth cured films on the substrate. On the other hand, in Comparative Examples 1 and 2, compared to the Examples, the coatings were insufficient in uniformity and had inferior anti-friction properties, and it was not possible to reduce the surface tackiness of the coating. [Industrial Applicability]
[0095] The oil-in-water silicone emulsion composition of the present invention has good storage stability even when it contains colloidal silica, and when it is applied to or impregnated into a substrate and then the water is removed, it forms a cured film that has rubber-like elasticity, i.e., excellent strength, and is therefore useful as a paper coating agent used in water-based paints and inks, thermal paper, inkjet paper, etc., a release agent for molds and rubber, a resin coating agent used in automobile weather strips, gaskets, rubber hoses, etc., a fiber treatment agent used in clothing and airbags, a release agent, cosmetics, building materials, etc.
Claims
1. (A) 100 parts by mass of a polyorganosiloxane having at least two hydroxyl groups or hydrolyzable groups bonded to silicon atoms in each molecule and having a viscosity at 25° C. in the range of 100,000 to 20,000,000 mPa s; (B) 45 to 120 parts by mass of colloidal silica (solid content equivalent) in the form of an aqueous dispersion in which 5 to 40% by mass of silica particles are colloidally dispersed in water, (C1) 1 to 100 parts by mass of an ionic emulsifier, (C2) 0.1 to 50 parts by mass of a polyoxyethylene-polyoxypropylene copolymer nonionic emulsifier, and (D) Water: 0 to 500 parts by mass (excluding water in colloidal silica) 1. An oil-in-water silicone emulsion composition comprising:
2. 2. The oil-in-water silicone emulsion composition according to claim 1, wherein the viscosity of the entire composition at 25° C. is 1,000 mPa·s or greater.
3. 3. The oil-in-water silicone emulsion composition according to claim 1 or 2, further comprising (E) a thickener.
4. 4. The oil-in-water silicone emulsion composition according to claim 3, wherein component (E) is at least one member selected from the group consisting of (E1) a thickener containing a clay mineral and (E2) a thickener containing a water-soluble organic polymer.
5. Furthermore, (F)R 1 a Six 4-a (In the formula, R 1 is an unsubstituted monovalent hydrocarbon group or a substituted monovalent hydrocarbon group, X is an alkoxy group or an alkoxyalkoxy group, and a is 0, 1, or 2), or 0.1 to 50 parts by mass of a partial hydrolysis condensate of said alkoxysilane or alkoxyalkoxysilane.
6. The oil-in-water silicone emulsion composition according to any one of claims 1 to 5, further comprising (G) an amine compound.
7. 7. The oil-in-water silicone emulsion composition according to any one of claims 1 to 6, wherein the average primary particle size of the emulsion particles is in the range of 50 to 600 nm.
8. 8. The oil-in-water silicone emulsion composition according to any one of claims 1 to 7, wherein component (A) is a polyorganosiloxane obtained by emulsion polymerization of precursors of component (A), namely (a) a polyorganosiloxane having at least two hydroxyl groups or hydrolyzable groups bonded to silicon atoms per molecule, and (b) an aminoxy group-containing organosilicon compound having an average of two aminoxy groups bonded to silicon atoms per molecule, in the presence of component (C1) and component (C2).
9. A surface treatment agent comprising the oil-in-water silicone emulsion composition according to any one of claims 1 to 8.
10. A surface treatment method, comprising treating a surface of a substrate with the oil-in-water silicone emulsion composition according to any one of claims 1 to 8 or with a surface treatment agent according to claim 9 that contains the same.
11. 9. A substrate which has been surface-treated with the oil-in-water silicone emulsion composition according to any one of claims 1 to 8, or with a surface treatment agent according to claim 9 which contains the same.
Citation Information
Patent Citations
Silicone emulsion
JP1981016553A
Controlling system for governor of feed water pump in turbine
JP1983048704A
Water-resistant coating composition
JP1984152972A
Aqueous silicone emulsion composition