Manufacturing method for high strength steel slabs

A method for high-strength steel slabs with controlled cooling and stacking techniques addresses cracking and holes by managing internal and external stresses, enhancing production stability.

JP7575365B2Active Publication Date: 2024-10-29KOBE STEEL LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021155953
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-09-24
Publication Date
2024-10-29
Estimated Expiration
2041-09-24

AI Technical Summary

Technical Problem

High-strength steel slabs with high carbon content are prone to cracking, holes, and stubs during rolling due to internal and external stresses, which existing methods fail to adequately address.

Method used

A method involving specific carbon, silicon, and manganese content, controlled cooling rates, and stacking slabs to manage internal and external stresses, along with surface defect removal processes, to prevent cracking and holes during rolling.

Benefits of technology

Effectively suppresses cracking and holes in high-strength steel slabs by managing internal and external stresses through controlled cooling and surface defect management, ensuring stable production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575365000015
    Figure 0007575365000015
  • Figure 0007575365000016
    Figure 0007575365000016
  • Figure 0007575365000017
    Figure 0007575365000017
Patent Text Reader

Abstract

To suppress the occurrence of placing cracks and to suppress the occurrence of holes and scabs during rolling in a steel type where placing cracks are likely to occur.SOLUTION: Within 50 minutes of a slab passing through a final roll of a casting machine, the slab is stacked and another slab cast by another casting machine is placed above and below the stacked slab. The state is maintained for 8 hours or more. While the state is maintained, for a slab having an internal crack length of 23 mm or less, the cooling rate difference between the upper and lower surfaces is controlled to 0.5°C / min or less, and for a slab having an internal crack length longer than 23 mm and 50 mm or less, the cooling rate difference between the upper and lower surfaces is controlled to 0.25°C / min or less. Then, the depth of the surface defect present in the slab is measured, and when the depth of the surface defect exceeds the pre-calculated critical defect depth, the surface defect is removed.SELECTED DRAWING: Figure 15
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a slab of high strength steel. [Background technology]

[0002] In recent years, carbon (C), chromium (Cr), titanium (Ti), boron (B), etc. have been added to steel in order to increase its strength. The addition of these elements makes the steel more susceptible to cracks (hereinafter referred to as "delayed cracks") when it is cooled after being cast.

[0003] In order to further increase the strength of steel, the amount of carbon (C) added may be increased. However, as the amount of carbon (C) added increases, the frequency of thermal cracking increases. Patent Document 1 describes a method for suppressing the occurrence of thermal cracking even in steel types with a large amount of carbon (C) added. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-139209 A Summary of the Invention [Problem to be solved by the invention]

[0005] Research by the present inventors has revealed that steel types with a large amount of added carbon (C) are prone to developing cracks during rolling, and are also prone to holes and scabs during rolling. In steel types with a large amount of added carbon (C), it is desirable to be able to suppress the development of cracks during rolling, as well as to suppress the development of holes and scabs during rolling.

[0006] An object of the present invention is to provide a method capable of suppressing the occurrence of lap cracks even in a steel type in which lap cracks are likely to occur, and capable of suppressing the occurrence of holes and scabs during rolling. [Means for solving the problem]

[0007] The method for producing a high-tensile steel slab disclosed in the present specification includes casting a slab of high-tensile steel having a carbon content of 0.16 mass% or more and 0.35 mass% or less, a silicon content of 1.0 mass% or more and 2.5 mass% or less, and a manganese content of 1.2 mass% or more and 4.0 mass% or less, Within 50 minutes after the slab passes the final roll of the casting machine, stack the cut slabs and place other slabs cast by a different casting machine above and below the stacked slabs, and maintain the above state for 8 hours or more. While maintaining the above state, excluding the other slabs, for slabs with internal cracks of 23 mm or less in length, the difference in cooling rate between the top and bottom surfaces of the slab is kept to 0.5°C / min. or less, and for slabs with internal cracks of more than 23 mm and 50 mm or less in length, the difference in cooling rate between the top and bottom surfaces of the slab is kept to 0.25°C / min. or less, The depth of any surface defects present in the slab is then measured and the depth of the surface defects is then used to determine the surface stresses that arise during subsequent heating and / or rolling. σc(MPa) Based on From the formula below Pre-calculated critical defect depth cm) If the defect exceeds this limit, treatment is carried out to remove the surface defect.

number

[0008] According to the above-described method, even in a steel type in which the aging crack is likely to occur, the occurrence of the aging crack can be suppressed, and the occurrence of holes and scabs during rolling can be suppressed. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a perspective view of a cut slab X. [Diagram 2] FIG. 2 is a diagram showing a cross section taken along line II in FIG. [Diagram 3] FIG. 1 is a diagram showing the results of a fracture toughness test. [Figure 4]FIG. 1 is a diagram showing the relationship between stress (the sum of internal stress and external stress) and the length of an internal crack. [Diagram 5] FIG. 1 is a diagram showing the relationship between stress and internal crack length. [Figure 6] FIG. 2 is a graph showing the relationship between the temperature of a slab and the time after the slab has passed the final roll of a continuous casting machine. [Figure 7] FIG. 2 is a schematic diagram showing the state in which slabs are stacked. [Figure 8] FIG. 2 is a schematic diagram showing an example of a warped slab. [Figure 9] FIG. 2 is a schematic diagram for explaining how to determine the amount of warping of a slab. [Figure 10] FIG. 1 is a schematic diagram for explaining how to obtain an external stress. [Figure 11] FIG. 13 is a diagram showing experimental results. [Figure 12] FIG. 13 is a diagram showing the relationship between external stress and slab length. [Figure 13] FIG. [Figure 14] FIG. 1 is a diagram showing the relationship between stress and internal crack length. [Figure 15] FIG. 1 is a diagram showing the relationship between surface defect depth and surface stress. [Figure 16] FIG. 13 is a diagram showing experimental results. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Preferred embodiments of the present invention will now be described.

[0011] The high tensile steel of the present embodiment has the following composition. Carbon (C) content: 0.16mass% or more and 0.35mass% or less Silicon (Si) content: 1.0 mass% to 2.5 mass% Manganese (Mn) content: 1.2 mass% to 4.0 mass%

[0012] The upper limit of the carbon content of the high tensile steel of the present embodiment is higher than the upper limit of the carbon content of general high tensile steel, and the present embodiment also targets steels with higher strength than general high tensile steel.

[0013] A slab of high tensile steel having the above composition is cast by a casting machine. The size of the slab is, for example, 230 mm to 270 mm thick and 800 mm to 1,400 mm wide. After casting, the slab is cut to a predetermined length.

[0014] [Cracked] The present inventors have studied the cause of the occurrence of staggered cracks when the cut slab is cooled after casting, and have found the following.

[0015] FIG. 1 shows an example of a cut slab (slab X). The width direction, thickness direction, and longitudinal direction shown in FIG. 1 are perpendicular to each other. When slab X is cooled, internal stress is generated in slab X. When the magnitude of the internal stress is compared in the width direction, thickness direction, and longitudinal direction of slab X, it is found that the stress in the longitudinal direction is the largest. It is also found that this stress in the longitudinal direction is the main stress that causes temporary cracks.

[0016] FIG. 2 shows an example of a cut surface along the longitudinal direction of slab X. The cut surface shown in FIG. 2 is the cut surface II in FIG. 1. As shown in FIG. 2, internal cracks may occur in slab X. The internal cracks occur in a direction perpendicular to the longitudinal direction of the slab, where the internal stress is greatest. When stress acts on the internal crack, a crack occurs starting from the internal crack.

[0017] The internal stress that occurs when Slab X is cooled is the result of the combination of thermal stress due to thermal expansion and contraction, and transformation stress due to transformation expansion and contraction. Thermal stress is caused by the difference between the surface temperature and the internal temperature of Slab X, and can be controlled by controlling the cooling rate using water cooling or air cooling.

[0018] Since the high-tensile steel targeted in this embodiment has a higher carbon content than conventional steels, it was found that the occurrence of thermal cracks cannot be suppressed by only reducing thermal stress in some cases. Therefore, the present invention focuses on transformation stress in addition to thermal stress.

[0019] The transformation stress varies depending on the difference in the timing of transformation between the surface and the interior of the slab, and the strength (structure) of the material after transformation. If the structure of the slab during cooling transforms from austenite to ferrite, pearlite, or a structure containing both, the transformation stress is small. However, if the structure of the slab changes to bainite or martensite, the transformation stress becomes large.

[0020] In the high-tensile steel targeted in this embodiment, it was found that the transformation stress may be reduced if transformation (transformation to ferrite structure or pearlite structure) occurs when the slab is at 500°C or higher and 700°C or lower. From this, it is considered that the transformation stress can be reduced by controlling the cooling rate when the slab is at 500°C or higher and 700°C or lower. If the transformation stress can be reduced, the internal stress, which is the sum of thermal stress and transformation stress, becomes smaller, so that the internal (residual) stress at room temperature that generates cracks when the slab is cooled to room temperature can be reduced. Therefore, it is important to control the cooling rate within this temperature range. On the other hand, in a temperature range higher than the above range, the structure of the slab does not transform, so that no transformation stress occurs. In addition, if transformation occurs in a temperature range lower than the above range, a bainite structure or martensite structure occurs, and the strength of the material increases, so that the transformation stress increases.

[0021] From the above, in the high tensile steel targeted in this embodiment, it is considered important to control the cooling rate of the slab after casting from when the slab temperature reaches 700°C to when it drops to 500°C (when the temperature is 500°C or higher and 700°C or lower) in order to suppress the occurrence of thermal cracks. Note that the cooling rate when the slab temperature is below 500°C and the cooling rate when the slab temperature exceeds 700°C contribute to changes in thermal stress, but the degree of contribution is small and they are not a direct cause of thermal cracks.

[0022] As a result of further research, the present inventors have obtained the following findings. It has been found that the high tensile steel targeted in this embodiment warps after casting and cooling. When correcting the warp, an external stress is generated. It has been found that this external stress acts as the starting point of the stabilization crack.

[0023] From the above, it was found that in the high tensile steel targeted in this embodiment, in addition to internal stress, external stress acts on the starting point of the lattice crack. It was also found that the internal stress and external stress acting on the starting point of the lattice crack are the cause of the occurrence of the lattice crack. From this, it was thought that the occurrence of the lattice crack could be suppressed by reducing the external stress as well as the internal stress occurring in the slab, and by reducing the sum of the internal stress and the external stress. It was also thought that there is a limit value of the stress (sum of the internal stress and the external stress) at which the lattice crack does not occur, and the following experiment was carried out to investigate this limit value.

[0024] Slabs of the steel types shown in Table 1 were cast using a vertical bending type continuous casting machine (machine length 39.0 m, bending radius 8.8 m). Steel types A and B shown in Table 1 are high tensile steels targeted in this embodiment. The casting conditions are shown in Table 2. After casting the slabs, samples were taken from the slabs and subjected to fracture toughness testing in accordance with ISO12737 Metallic materials - Plane strain fracture toughness testing method. [Table 1] [Table 2]

[0025] The results of the fracture toughness test are shown in Figure 3. The vertical axis of Figure 3 is the fracture stress at room temperature, and the horizontal axis of Figure 3 is the fracture starting point (notch length). The curve shown in Figure 3 shows the fracture toughness characteristics. It was found that the slab fractures above the curve, but does not fracture on or below the curve.

[0026] The fracture, fracture origin (notch length), and fracture stress of the sample in the fracture toughness test can be considered as the slab crack, the internal crack (internal crack length) that is the origin of the crack, and the stress applied to the slab, respectively. This "stress applied to the slab" was considered to be the sum of the internal stress and the external stress.

[0027] When the fracture, fracture origin (notch length), and fracture stress of the sample in the fracture toughness test were respectively substituted for the slab's pre-crack, internal crack (internal crack length), and stress applied to the slab (total of internal and external stress), the diagram shown in Figure 4 was obtained. The vertical axis of Figure 4 is stress (total of internal and external stress) δ, and the horizontal axis of Figure 4 is internal crack length L. The curve shown in Figure 4 can be considered the maximum stress at which pre-cracks do not occur. The range above the curve is the "range in which pre-cracks occur," and the range on and below the curve is the "range in which pre-cracks do not occur."

[0028] The fracture toughness value Kc (MPa√m) was obtained from the fracture toughness test described above. The fracture limit stress σc is expressed by equation (1) using the fracture toughness value Kc (MPa√m), the notch length a (m), and the correction coefficient F of the stress intensity factor.

number

number

number

[0029] Figure 5 shows formula (3) when the horizontal axis is "stress" and the vertical axis is "internal crack length." The curve of formula (3) is the limit value where no cracking occurs, and the area above the curve of formula (3), in other words, when the sum of internal stress and external stress exceeds the curve, is the "range where cracking occurs," and the area on the curve of formula (3) and below the curve of formula (3), in other words, when the sum of internal stress and external stress does not exceed the curve, is the "range where cracking does not occur."

[0030] From the above, it is believed that the occurrence of thermal cracks can be suppressed by controlling the cooling so that the sum of the internal and external stresses generated in the slab is within the "range in which thermal cracks do not occur" shown in Figure 5 during the period from when the slab temperature reaches 700°C to when it falls to 500°C (when the temperature is between 500°C and 700°C).

[0031] To confirm the above findings, the following experiment was carried out.

[0032] First, the following experiment was carried out to investigate the time it takes for the temperature of the slab to reach 700° C. after casting.

[0033] A slab (thickness 230 mm × width 1230 mm) of steel type B shown in Table 1 was cast using a vertical bending type continuous casting machine (machine length 39.0 m, bending radius 8.8 m). When the slab started to be drawn, it was drawn at 0.2 m / min for about 100 seconds. Cut out Then, 0.12m / min. 2 The casting speed was gradually increased to the target casting speed at an acceleration rate of 1.3 m / min. The specific water amount was 1.0 g / kg-steel. The surface temperature of the slab was measured after it passed the last roll of the continuous casting machine. The last roll of the continuous casting machine is the roll located at the farthest position from the mold of the continuous casting machine along the casting path.

[0034] As mentioned above, it is known that latent cracks originate from internal cracks. As shown in Figure 2, internal cracks are defects that exist inside the slab (near the axis), and are known to occur frequently, particularly in slabs with a thickness of t, at a position about t / 4 from the surface in the thickness direction. Therefore, we investigated the temperature at the slab axis near the position where internal cracks are likely to occur, at which the temperature at the slab axis reaches 700°C. The slab axis refers to the position at the center of the slab in the width direction, thickness direction, and length direction.

[0035] The axial temperature of the slab was calculated using the heat transfer coefficient of the slab (steel) and the slab surface temperature as the boundary condition. In this experiment, CASTEM (heat transfer solidification calculation) was used. In this experiment, the surface temperature of the slab was measured, and the heat transfer coefficient in CASTEM was fitted to match the surface temperature (measured value) to calculate the axial temperature.

[0036] In Figure 6, in a graph with the vertical axis representing "slab temperature" and the horizontal axis representing "time since the slab passed the final roll of the continuous casting machine," the slab's central axis temperature is indicated by a "◯." Figure 6 also shows curve A, which indicates the lower limit of the slab's central axis temperature (◯). For reference, the slab's surface temperature is indicated by a "◆." Also shown is curve B, which indicates the lower limit of the slab's surface temperature (◆).

[0037] In curve A, the slab's central axis temperature reaches 700°C approximately 50 minutes after the slab passes through the final roll of the casting machine. Curve A is a line that indicates the lower limit of the slab's central axis temperature (◯), and it is believed that the actual central axis temperature is higher than curve A. Therefore, it is believed that the actual central axis temperature reaches 700°C approximately 50 minutes after the slab passes through the final roll of the casting machine.

[0038] From the above, it was found that it took more than 50 minutes for the slab's core temperature to reach 700°C after the slab had passed through the final roll of the casting machine.

[0039] The temperature of the slab drops below 700°C after 50 minutes have passed since the slab passed the final roll of the casting machine. By keeping the sum of the internal and external stresses generated in the slab within the "range in which thermal cracking does not occur" shown in Figure 5 during the period from when the slab temperature drops below 700°C until it reaches 500°C, the occurrence of thermal cracking can be suppressed.

[0040] Based on the above findings, an experiment was conducted to confirm the findings shown in Fig. 5 by comparing slabs with different cooling conditions after 50 minutes or more had elapsed since passing through the final roll of the casting machine.

[0041] A slab (thickness 230 mm x width 1230 mm) of steel type B in Table 1 was cast using a vertical bending type continuous casting machine (machine length 39.0 m, bending radius 8.8 m). When the slab started to be drawn, it was drawn at 0.2 m / min for about 100 seconds. Cut out Then, 0.12m / min. 2 The casting speed was gradually increased to the target casting speed at an acceleration rate of 100 / s. The casting speed and specific water amount are shown in Table 2. After casting, the slab was cut to a specified length (5.5 to 11.0 m).

[0042] From the above experiment, it was found that the axial temperature of the slab reaches 700°C 50 minutes after the slab passes the final roll of the continuous casting machine, so the slabs were stacked so that they reached the cooling state shown in Table 3 within 50 minutes after the slab passes the final roll of the continuous casting machine. The slabs were left in the cooling state shown in Table 3 for 96 hours to cool to room temperature, and then it was confirmed whether or not the slabs in the stacking positions shown in Table 3 had developed cracks (whether or not the slabs were broken). The results are shown in Table 3.

[0043] [Table 3]

[0044] The items shown in Table 3 are explained below.

[0045] <Cooling state> As shown in Figure 7, eight cut slabs were stacked with their wide faces overlapping. The wide face of a slab is the face that is nearly horizontal in the width and length directions of the slab. In this experiment, slabs with wide faces of nearly the same size were stacked in layers. Eight slabs were stacked so that the centres of all the slabs in the width and length directions were aligned on the same vertical line (eight slabs stacked). In this state, the slabs were left at room temperature for 96 hours. In this state, the slabs were left at room temperature for 96 hours, and the slabs were allowed to reach room temperature.

[0046] "Cooling rate" in Table 3, "Cooling of the upper surface-lower surface of the slab" speed The "difference in strength," "internal crack length L," "presence or absence of cracking," "internal stress," "amount of warping," and "external stress" are for the following slabs out of the eight stacked slabs. No.1: Top slab No.2: Second slab No.3: above The third slab from

[0047] <Cooling rate> As shown in Figure 7, after the slabs were stacked, K-type thermocouples were set on the top and bottom surfaces of the slabs No. 1 to 3, and the "cooling rate at the top surface" and "cooling rate at the bottom surface" of the slabs were measured for 96 hours. Laid cracks often occur at the longitudinal center and width center of the slab. Furthermore, calculations of internal stress, which will be described later, show that stress is greatest at the longitudinal center and width center of the slab. Therefore, in the case of No. 1, as shown in the enlarged view of Figure 7, K-type thermocouples were set at the longitudinal center and width center (C 1 ) and the longitudinal center and transverse center of the bottom surface of the slab (C 2 ) and C 1 "Cooling rate of the upper surface" and C 2 The "cooling rate of the bottom surface" of the slab was measured. Similarly, for No. 2 and No. 3, a K-type thermocouple was placed at the center of the length and width of the top surface of the slab (C 1 ) and the longitudinal center and transverse center of the bottom surface of the slab (C 2 ) and C 1 "Cooling rate of the upper surface" and C 2 The "cooling rate of the lower surface" was measured.

[0048] <Difference in cooling rate between top and bottom of slab> The "cooling rate difference between the top and bottom surfaces of the slab" shown in Table 3 is the absolute value of the difference between the "cooling rate at the top surface" and the "cooling rate at the bottom surface" of the slab.

[0049] table 3 Although not shown in the figure, the axial cooling rate of the slab was calculated using CASTEM (heat transfer solidification calculation). For the calculation, the heat transfer coefficients of the slab surface, mist, air, and rolls were given as a function of temperature based on the physical properties (specific heat, latent heat of solidification, thermal conductivity, density, etc.) collected by various tests of slab samples with the components shown in Table 3, and based on the cooling conditions of the continuous casting machine (casting speed, specific water amount) and the cooling conditions after casting shown in Table 3. In addition, the slab surface temperature immediately after passing through the final roll of the continuous casting machine and the slab surface temperature during cooling after casting were measured, and the heat transfer coefficient of the slab surface was corrected so that the surface temperature history obtained by the calculation matched the actual measured value. In addition, in the analysis of internal stress described later, the internal stress was maximum at the center of the width direction, center of the thickness direction, and center of the length direction of the slab (axial center), so the cooling rate was obtained at the center of the width direction, center of the thickness direction, and center of the length direction of the slab (axial center). The axial cooling rate of No. 1 was 0.7°C / min., and the axial cooling rate of No. 2 and No. 3 was 0.44°C / min.

[0050] <Internal crack length L> After casting, the slab was cut to a specified length, and then cut longitudinally at the center of the width (see Figures 1 and 2). A sample was taken from the cut surface, and acid was applied to the sample. The length of the part corroded by the acid in the thickness direction of the slab was measured and taken as the internal crack length L. When there were multiple corroded parts, the longest corroded part was taken as the internal crack length L. The lower limit of detection with this method is 10 mm. All cracks less than 10 mm in length were treated as 10 mm. In addition, since it is difficult to distinguish between parts with large microsegregation (less than 10 mm) and internal cracks between dendrite trees, parts with large microsegregation were also treated as 10 mm cracks.

[0051] <Whether or not cracks have occurred> The cooling conditions shown in Table 3 were maintained for 96 hours, and after the slabs reached room temperature, it was checked whether or not cracks had occurred in the slabs (whether or not the slabs had broken). In addition, when it was checked whether or not cracks had occurred in the slabs other than No. 1 to No. 3 in Table 3 (excluding the bottom row), it was confirmed that no cracks had occurred in the slabs other than No. 1 to No. 3 in Table 3 (excluding the bottom row).

[0052] <Internal stress> The internal stress was calculated when the slab was maintained in the cooling state shown in Table 3. In this experiment, the internal stress was calculated by numerical analysis using the general-purpose software ABAQUS. When calculating the internal stress, the temperature distribution of the slab calculated in advance by CASTEM, which was used to calculate the axial center temperature of the slab, was given, and the physical property values ​​(stress-strain relationship, linear expansion coefficient) corresponding to that temperature and cooling rate were sequentially given to calculate the stress distribution within the slab. This analysis showed that the internal stress is greatest in the longitudinal direction of the slab among the width, thickness, and longitudinal directions. It was also found that the internal stress in the width, thickness, and longitudinal directions of the slab is greatest at the center of the width, thickness, and longitudinal directions, respectively.

[0053] <Warpage amount> It was found that the slab warps due to the difference in cooling rate between the top and bottom surfaces. The slab was left in the cooling state shown in Table 3, and after it had cooled to room temperature, the amount of warping in the longitudinal direction of the slab was measured using the following method. As shown in the upper diagram of Figure 8, when the slab is aligned so that it is convex upward in the longitudinal direction, the shortest distance from the center of the bottom surface of the slab to the line connecting both ends of the bottom surface of the slab in the longitudinal direction is the amount of warping (maximum value) x 1 It was decided. As shown in the lower diagram of Figure 8, when the slab is aligned so that it is convex downward, the shortest distance from one end of the slab's underside in the longitudinal direction to the tangent line at the center of the slab's underside is the amount of warping (maximum value) x 2 The maximum warpage x(x 1 or x 2) is expressed by the following formula using the slab warp radius (the radius of the warped part of the slab) R, the angle θ, and the slab length l, as shown in Figure 9.

number

[0054] <External stress> In this experiment, the force to straighten the warp of the slab after cooling it to room temperature was defined as the external stress. The external stress was calculated by the following method. In the slab with thickness t shown in Fig. 10, it is known that the external stress is greatest at a position of thickness t / 4 from the inner circumference. When the center of the slab thickness is used as the reference, the radius R at the position of thickness t / 4 from the inner circumference 1 is expressed by the following formula: R 1 =R-t / 4 (a) where R is the radius at the centre of the slab thickness. Slab length l at thickness t / 4 from the inner circumference 1 is expressed by the following formula: l 1 =R 1 ×θ (b) When the warp of a slab is corrected, the strain ε that occurs at the position of thickness t / 4 from the inner circumference is 1 is expressed by the following formula:

number

[0055] Figure 11 shows No. 1 to No. 3 plotted on the graph in Figure 5. As shown in Figure 11, No. 1, where cracking occurred, exceeds the curve of formula (3) and is in the "range where cracking occurs." No. 2 and No. 3, where cracking did not occur, are in the "range where cracking does not occur."

[0056] From the above experiment, it was confirmed that the range exceeding the curve of formula (3) is the "range in which storage cracking occurs," and the range not exceeding the curve of formula (3) is the "range in which storage cracking does not occur."

[0057] From the above, it was found that the occurrence of thermal cracking can be suppressed by ensuring that the sum of internal stress and external stress is within the "range in which thermal cracking does not occur" shown in Figure 5 while the slab temperature is dropping from 700°C to 500°C (in the range of 500°C to 700°C) 50 minutes after the slab has been cast and passed through the final roll of the continuous casting machine.

[0058] Next, we investigated a method for keeping the sum of the internal stress and external stress within the "range in which no thermal cracking occurs" shown in Figure 5.

[0059] Figure 12 shows the relationship between external stress and slab length when the amount of warping (x) is changed, with the vertical axis representing "external stress" and the horizontal axis representing "slab length." "External stress" is the external stress at a position that is t / 4 thickness from the inner circumference of the slab, as shown in Figure 10, and is calculated using formula (d) above. "Slab length" is the longitudinal length (l) of the center of the thickness direction of the slab, as shown in Figure 10. As shown in Figure 12, the smaller the amount of warping (x), the smaller the external stress. For the same amount of warping (x), the longer the slab length, the smaller the external stress.

[0060] Figure 13 shows the table 313 shows the amount of warpage of No. 1 to No. 3 in the table. In FIG. 13, the maximum amount of warpage of the 10 tests is shown as "max", and the average amount of warpage of the 10 tests is shown as "ave". From FIG. 13, the maximum amount of warpage was 20 mm in No. 2 and No. 3, which did not have any placement cracks. From FIG. 12, when the amount of warpage was 20 mm (x=20 mm), the maximum external stress was about 50 MPa. From Table 3, in No. 2, which had a warpage of 20 mm, the external stress was 50 MPa, and this external stress was the maximum external stress (about 50 MPa) when the amount of warpage shown in FIG. 12 was 20 mm (x=20 mm).

[0061] The warpage of slab No. 3 (the third slab from the top) was 0 mm (Fig. 13). From Table 3, the warpage of slab No. 3 was 0 mm, and the external stress at this time was 0 MPa. The slabs below the third row from the top are cooled in almost the same way as the third row from the top, or are cooled more slowly than the third row from the top, so it is presumed that they have the same warpage (0 mm) and external stress (0 MPa) as the third row from the top (No. 3).

[0062] In addition, the bottom slab will be in a cooling state different from the other slabs in the stacking position, and as described below, it is thought that there is a high possibility of cracks occurring due to the large internal stress. The second slab from the bottom is considered to be in a similar cooling state to the second slab from the top (for example, the difference in cooling rate between the top and bottom surfaces of the slab is the same as shown in Table 3), but since there are many slabs placed above the second slab from the bottom, it is less likely to warp than the second slab from the top. Therefore, the amount of warping of the second slab from the bottom is smaller than that of the top slab. and others The amount of warping of the second slab is thought to be smaller than that of the first slab. Also, the external stress generated in the second slab from the bottom is smaller than that of the first slab. and others It is considered to be smaller than the external stress of the second slab (50 MPa).

[0063] From the above, it is considered that the maximum warp amount of the slab without occurrence of cracks is 20 mm, and the external stress at this time is 50 MPa.

[0064] Regarding internal stress, Table 3 shows that the internal stress of the topmost slab (No. 1) is large at 198 MPa, while the internal stress of the second and third slabs from the top (No. 2 and No. 3) was 125 MPa. It is believed that the cooling state of the slabs from the fourth row from the top to the second row from the bottom is the same as or more difficult to cool than that of the second and third rows from the top, so it is estimated that the internal stress generated in the slabs from the fourth row from the top to the second row from the bottom is 125 MPa or less.

[0065] In addition, the bottom slab is easily cooled because there is no slab below it. Therefore, the internal stress of the bottom slab is large. In fact, the internal stress of the bottom slab was calculated to be 310 MPa.

[0066] From the above, it is considered that the maximum internal stress of the slab where no cracks occur is 125 MPa.

[0067] From the above, the maximum warpage (x) of the slab where cracks do not occur is 20mm or less, and the maximum stress generated in the slab at this time is 175MPa, which is the sum of the internal stress (125MPa) and the external stress (50MPa). Figure 14 shows formula (3) shown in Figure 5, the "range where cracks occur" and the "range where cracks do not occur". In the "range where cracks do not occur" shown in Figure 14, the stress becomes 175MPa when the internal crack length is about 23mm. From this, it is considered that cracks do not occur when the internal crack length is 23mm or less and the warpage is 20mm or less. From Table 3, it is considered that the warpage becomes 20mm or less, in other words, the maximum internal stress becomes 175MPa or less when the cooling rate difference between the top and bottom surfaces of the slab is 0.50℃ / min or less.

[0068] In addition, among the slabs in which no cracks occurred, the slabs from the third row onwards (excluding the bottom row) (No. 3) had a warpage of 0 mm, and the maximum stress generated in the slab at this time was the sum of the internal stress (125 MPa) and the external stress (0 MPa), which was 125 MPa. In the "range in which cracks do not occur" shown in Figure 14, the stress reaches 125 MPa when the internal crack length is around 50 mm. From this, it is considered that no cracks will occur if the internal crack length is 50 mm or less and the warpage is 0 mm or less. From Table 3, it is considered that the warpage is 0 mm or less, in other words, the maximum internal stress is 125 MPa or less, when the cooling rate difference between the top and bottom surfaces of the slab is 0.25°C / min or less.

[0069] From the above, when the length of the internal crack in the slab is 23 mm or less, 50 minutes after the slab passes through the final roll of the continuous casting machine, the slab is cooled so that the difference in cooling rate between the top and bottom surfaces is 0.50°C / min or less. This keeps the amount of warping to 20 mm or less, and prevents the occurrence of cracks during placement. In addition, when the length of the internal crack of the slab is greater than 23 mm and less than 50 mm, the difference in the cooling rate between the top and bottom surfaces of the slab is 0.25 or less after 50 minutes have elapsed since the slab passed through the final roll of the continuous casting machine. ℃ / min. or less. This will result in a warpage of 0 mm and prevent cracks from occurring when placed on the floor.

[0070] There is no particular limitation on the method for making the cooling temperature difference between the upper and lower surfaces of a slab 0.5°C / min or less, in other words, for making the amount of warping of the slab 20 mm or less. For example, as in the above experiment, within 50 minutes after the slab passes through the final roll of the casting machine, multiple cut slabs are stacked, and other slabs cast by other casting machines are placed above and below the stacked slabs (stacking). As a result, the cooling temperature difference between the upper and lower surfaces of the slab is 0.5°C / min or less for all slabs except the top and bottom tiers, and the amount of warping of the slab is 20 mm or less.

[0071] The conditions for stacking are not particularly limited, but suitable conditions include, for example, stacking slabs and other slabs with approximately the same size of broad faces. Also, stacking all slabs so that the widthwise center and the longitudinal center are located on a vertical line. Note that the broad faces of all slabs, including the top and bottom tiers, may be different in size. Also, the widthwise center and the longitudinal center of all slabs, including the top and bottom tiers, may be slightly shifted from the vertical line. Also, at least Except for the top and bottom rows Kus The ratio of the total area of ​​one wide surface of the slab in contact with the slab placed above it and the total area of ​​the other wide surface of the slab in contact with the slab placed below it to the total area of ​​one wide surface of the slab and the other wide surface of the slab may be 60% or more. It has been found that in a slab with this ratio of 60% or more, the cooling temperature difference between the upper and lower surfaces of the slab is 0.5°C / min. or less, and the warp of the slab after cooling is within 20 mm. There is no particular restriction on the number of slabs to be stacked, as long as it is 3 or more, including the top and bottom layers.

[0072] The conditions for the top and bottom separate slabs are not particularly limited. For example, it is preferable to place the top and bottom separate slabs above and below the slab of this embodiment within 4 hours after passing through the final roll of the separate casting machine. In this case, when stacked in layers using the method exemplified above, it was found that the cooling temperature difference between the top and bottom surfaces of the slabs is 0.5°C / min or less for the slabs other than the top and bottom layers, and the amount of warping of the slab is 20 mm or less. The steel type of the separate slabs is not particularly limited.

[0073] Furthermore, the method for making the cooling temperature difference between the upper and lower surfaces of the slab 0.25°C / min or less, in other words, the method for making the warpage of the slab 0 mm or less, is not particularly limited. For example, the above-mentioned method for making the cooling temperature difference between the upper and lower surfaces of the slab 0.5°C / min or less, and the method similar to the method exemplified as the method for making the warpage of the slab 20 mm or less can be mentioned. As a result, for slabs other than the topmost slab, the second slab from the top, the bottommost slab, and the second slab from the bottom, 50 minutes or more after the slab passes through the final roll of the casting machine, the cooling temperature difference between the upper and lower surfaces of the slab becomes 0.25°C / min or less, and the warpage of the slab after cooling becomes 0 mm or less. Also, for at least the slabs excluding the top and bottom slabs, the ratio of the total area of ​​one broad surface of the slab in contact with the slab placed above it and the total area of ​​the other broad surface of the slab in contact with the slab placed below it to the total area of ​​the one broad surface and the other broad surface of the slab may be 60% or more. As a result, it has been found that the cooling temperature difference between the upper surface and the lower surface of the slab is 0.25°C / min or less for the slabs excluding the top slab, the second slab from the top, the bottom slab, and the second slab from the bottom, and the warpage of the slab after cooling is 0 mm. The conditions for the separate slab are not particularly limited, but for example, the same conditions as those described above can be adopted. For example, it is preferable to arrange the top and bottom separate slabs as the top and bottom within 4 hours after passing through the final roll of the separate casting machine. In this case, when the slabs were stacked in layers using the method exemplified above, it was found that the cooling temperature difference between the top and bottom surfaces of the slabs was 0.25°C / min or less for all slabs except for the top slab, the second slab from the top, the bottom slab, and the second slab from the bottom, and the warping of the slabs after cooling was 0 mm.

[0074] In the above experiment, 3 The cooling state shown in FIG. 1 (slabs stacked in layers) was maintained for 96 hours. However, the slabs may be stacked for a period shorter than 96 hours. 3The axial cooling rates of slabs No. 1 to 3 were calculated. The axial cooling rate of slab No. 1 (top) was 0.7°C / min, and the axial cooling rates of slabs No. 2 (second from the top) and No. 3 (third from the top) were 0.44°C / min. From this, it is considered that the axial cooling rate of slabs other than the top and bottom slabs is about 0.44°C / min. When the axial cooling rate is 0.44°C / min, it takes (700-500) / 0.44=455 minutes (<8 hours) for the axial temperature of the slab to drop from 700°C to 500°C. Therefore, it is recommended to keep the slabs stacked for 8 hours or more.

[0075] In view of the above, after the slab of high tensile steel that is the subject of this embodiment is cast, it is cooled by the following method. Within 50 minutes after the slab passes the final roll of the casting machine, the cut slabs are stacked, and other slabs cast by a different casting machine are placed above and below the stacked slabs. This state is maintained for 8 hours or more, and while this state is maintained, the difference in cooling rate between the top and bottom surfaces of the slab is kept to 0.5°C / min or less for slabs with internal cracks of 23 mm or less in length, and the difference in cooling rate between the top and bottom surfaces of the slab is kept to 0.25°C / min or less for slabs with internal cracks of more than 23 mm and 50 mm or less in length.

[0076] For example, when stacking slabs in the manner exemplified above, slabs with internal cracks of 23 mm or less in length are placed in positions other than the top tier (another slab) and the bottom tier (another slab).When stacking slabs in the manner exemplified above, slabs with internal cracks of more than 23 mm and 50 mm or less in length are placed in positions other than the top tier (another slab), the second tier from the top, the bottom tier (another slab), and the second tier from the bottom.

[0077] As a result of the above, it is possible to prevent the occurrence of stabilization cracks in the high tensile steel slab that is the subject of this embodiment.

[0078] In the above experiment, the actual value measured on the cut surface of the slab after casting was used as the "internal crack length". However, instead of the actual value, for example, an internal crack length estimated based on the casting conditions of the slab (casting speed, specific water amount, slab size, roll stand usage status, etc.) may be used. In addition, when an estimated length exists as the "internal crack length L", when the slab is cast under the same casting conditions as the casting conditions used to estimate the length, the "internal crack length L" of the slab may be the already existing estimated length. For example, when an actual measurement value of the "internal crack length L" exists, when the slab is cast under the same casting conditions as the casting conditions under which the actual measurement value was obtained, the "internal crack length L" of the slab may be the above-mentioned actual measurement value. In addition, when the "internal crack length L" is the actual measurement value, if multiple internal cracks occur, the longest internal crack length is adopted as the "internal crack length".

[0079] [Hole, dent] In the case of a slab of high tensile steel, which is the subject of this embodiment, it was found that the occurrence of staging cracks could be suppressed by the above method, but it was also found that when the slab was subsequently rolled, holes and spalling were likely to occur in the product. Therefore, a method for suppressing the occurrence of holes and spalling during rolling was investigated.

[0080] It is believed that holes and scabs that occur during rolling are caused by surface defects (cracks) that propagate in the depth direction due to surface stresses that occur during heating and / or rolling of the slab. The following study was carried out using equation (1) that expresses the fracture limit stress σc, which was adopted in the above-mentioned study of temporary cracks.

[0081] The critical fracture stress σc is expressed by equation (1).

number

number

number

[0082] Figure 15 shows equation (5) when the vertical axis is "surface defect depth" and the horizontal axis is "surface stress." The curve in equation (5) is the "limit value of surface stress at which holes and scabs do not occur" and is also the "maximum surface defect depth (critical defect depth) at which holes and scabs do not occur." The area above the curve in equation (5), in other words, when the surface defect depth exceeds the curve, is the "range in which holes and scabs occur," and the area on and below the curve in equation (5), in other words, when the surface defect depth does not exceed the curve, is the "range in which holes and scabs do not occur."

[0083] From the above, if the "surface defect depth" is measured before rolling, and if the "surface defect depth" before rolling exceeds the curve of formula (5) shown in Figure 15 and exists in the "range where holes and scabs occur", it is considered that the occurrence of holes and scabs can be prevented by performing a process to remove the surface defect of that depth before rolling (for example, grinder maintenance). Specifically, the surface stress generated during heating and / or rolling is calculated, and the "maximum surface defect depth (critical defect depth) at which holes and scabs do not occur" is obtained from formula (5) using the calculated surface stress. The depth of the surface defect of the slab is measured before rolling, and if the depth of the surface defect (measured value) exceeds the previously obtained "maximum surface defect depth (critical defect depth) at which holes and scabs do not occur", it exists in the "range where holes and scabs occur" shown in Figure 15, so a process to remove the surface defect of that depth before rolling (for example, grinder maintenance) is performed. It is considered that the occurrence of holes and scabs can be prevented.

[0084] To confirm the above findings, the following experiment was carried out.

[0085] A slab (thickness 230 mm × width 1230 mm) of steel type A in Table 1 was cast using a vertical bending type continuous casting machine (machine length 39.0 m, bending radius 8.8 m). When the slab started to be drawn, it was drawn at 0.2 m / min for about 100 seconds. Cut out Then, 0.12m / min. 2 The casting speed was gradually increased to the target casting speed at an acceleration rate of 100 / s. The casting speed and specific water amount are shown in Table 4. After casting, the slab was cut to a specified length (5.5 to 11.0 m).

[0086] Within 50 minutes after the slabs passed the final roll of the continuous casting machine, the eight cut slabs were stacked as shown in Figure 7. The eight slabs were left in this stacked state for 96 hours, after which the slabs reached room temperature. The second slab from the top (No. 4), the third slab from the top (No. 5), and the fourth slab from the top (No. 6) were checked for surface defects, and if any were present, the depth of the surface defects was measured by ultrasonic testing. Table 4 shows the surface defect depths (actual measurements).

[0087] The slab was then rolled and the product (coil) was checked for holes or chipping. 4 The results are shown in.

[0088] [Table 4]

[0089] The "surface stress" shown in Table 4 is the surface stress that occurs during subsequent heating and / or rolling, calculated in the same manner as the calculation of internal stress. The "critical defect depth c" shown in Table 4 is the "maximum surface defect depth (critical defect depth) at which holes and scabs do not occur" calculated from the "surface stress" and the above formula (5).

[0090] In Figure 16, No. 4 to 6As shown in Figure 16, No. 4, where holes and scabs occurred, exceeds the curve of formula (5) and is in the "range where holes and scabs occur." No. 5 and No. 6, where no holes or scabs occurred, are in the "range where holes and scabs do not occur."

[0091] From the above experiment, it was confirmed that the range exceeding the curve of equation (5) is the "range in which holes and scabs occur," and the range not exceeding the curve of equation (5) is the "range in which holes and scabs do not occur."

[0092] From the above, the "surface defect depth" of the slab is measured before rolling. If the "surface defect depth" exceeds the "maximum surface defect depth (critical defect depth) at which holes and scabs do not occur" calculated from the surface stress during heating and / or rolling and formula (5), the surface defect is in the "range at which holes and scabs occur" shown in Figure 15, so a process to remove the surface defect of that depth (for example, grinder cleaning) is performed before rolling. This can prevent holes and scabs from occurring during rolling. If the measured "surface defect depth" is less than the "maximum surface defect depth (critical defect depth) at which holes and scabs do not occur," a process to remove the surface defect of that depth may be performed. If the measured "surface defect depth" is less than the "maximum surface defect depth (critical defect depth) at which holes and scabs do not occur," it is considered that holes and scabs do not occur at that location, so a process to remove the surface defect of that depth is not required.

[0093] It was found that in steels other than the high-tensile steel targeted in this embodiment, for example, conventional steels with a low carbon content, the curve of "maximum surface defect depth (critical defect depth) at which holes and scabs do not occur" shown in formula (5) is completely different from the curve shown in FIG. 15. In conventional steels with a low carbon content, the "maximum surface defect depth (critical defect depth) at which holes and scabs do not occur" is larger than in the case of the high-tensile steel targeted in this embodiment. Therefore, in conventional steels with a low carbon content, the "range at which holes and scabs do not occur" is wider than the "range at which holes and scabs do not occur" shown in FIG. 15. Therefore, it is considered that holes and scabs do not occur even if the surface defects are somewhat deep.

[0094] In the high tensile steel targeted in this embodiment, the "maximum surface defect depth (critical defect depth) at which holes or scabs do not occur" is small, and the "range at which holes or scabs do not occur" is narrow, as shown in Figure 15. For this reason, in the high tensile steel of this embodiment in which plateau cracks are likely to occur, the above-mentioned method of measuring the "surface defect depth" before rolling, predicting whether holes or scabs will occur based on the measured "surface defect depth," and performing processing to remove surface defects before rolling is effective.

[0095] Although the embodiments of the present invention have been described above with reference to the drawings, the specific configuration should not be considered to be limited to these embodiments. The scope of the present invention is indicated by the claims rather than the above description, and includes all modifications within the meaning and scope of the claims. [Explanation of symbols]

[0096] X Slab

Claims

[Claim 1] A slab of high tensile steel having a carbon content of 0.16 mass% or more and 0.35 mass% or less, a silicon content of 1.0 mass% or more and 2.5 mass% or less, and a manganese content of 1.2 mass% or more and 4.0 mass% or less is cast; Within 50 minutes after the slab passes the final roll of the casting machine, stack the cut slabs and place other slabs cast by another casting machine above and below the stacked slabs, and maintain said state for 8 hours or more. While maintaining said state, excluding the other slabs, for slabs with internal cracks of 23 mm or less in length, the difference in cooling rate between the top and bottom surfaces of the slab is 0.5°C / min. or less, and for slabs with internal cracks of more than 23 mm and 50 mm or less in length, the difference in cooling rate between the top and bottom surfaces of the slab is 0.25°C / min. or less, The method for manufacturing a slab of high tensile steel is characterized in that the depth of surface defects present in the slab is then measured, and when the depth of the surface defects exceeds a critical defect depth c (m) calculated from the following formula based on the surface stress σc (MPa) generated during subsequent heating and / or rolling, a process for removing the surface defects is carried out. [Number A] Here, Kc is the fracture toughness value.

Citation Information

Patent Citations

  • Method for removing surface defect of slab

    JP1989157770A

  • Method for reducing surface flaw of steel sheet in hot rolling

    JP1997024401A

  • Method for preventing delayed failure in continuous cast slab of high tension steel

    JP2007083274A

  • Method for repairing surface of hot-state slab

    JP2008238259A

  • Method for cooling slab for high-strength steel sheet, method for producing high-strength hot-rolled steel sheet, method for producing high-strength hot-dip galvanized steel sheet, and method for producing high-strength alloyed hot-dip galvanized steel sheet

    JP2019167560A