Aqueous compositions for coating grain-oriented electrical steels
Aqueous compositions with aluminum, manganese, phosphate, and silica provide a stable, chromium-free coating for grain-oriented electrical steel, addressing corrosion and insulation issues, enhancing performance in transformers.
Patent Information
- Application Number
- JP2021545995
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-02-06
- Filing Date
- 2020-02-04
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-02-04
AI Technical Summary
Existing coatings for grain-oriented electrical steel suffer from corrosion issues due to micro- and macro-pores, and often contain environmentally harmful metals like chromium, leading to instability and inadequate protection.
Aqueous compositions comprising aluminum cations, manganese cations, dihydrogen phosphate, hydrogen phosphate, and colloidal silica, with specific molar ratios, are applied to form a stable, chromium-free coating that seals pores and provides electrical insulation.
The coating offers superior corrosion resistance, electrical insulation, and stability, maintaining quality over time without the use of harmful metals, ensuring consistent performance in transformers and other applications.
Smart Images

Figure 0007575386000001 
Figure 0007575386000002 
Figure 0007575386000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an aqueous composition suitable for coating grain oriented electrical steel ("GO") steel, for example as used in transformers. [Background technology]
[0002] The prior art describes numerous methods for producing grain-oriented electrical steel sheets (see, i.e., US 5,288,736, US 3,159,511, US 5,643,370, JP 2002-2112639, JP 56-158816, DE 1226129, DE 1252220, DE 19745445, DE 60219158, EP 0484904, EP 1752548, EP 2022874, EP 2264220). Grain-oriented electrical steel sheets are used in transformers, generators and high-performance generators to ensure the required soft magnetic properties.
[0003] Grain-oriented electrical steels are essentially low carbon steels (carbon content of about 0.01% to about 0.1%) that have a high silicon content of about 2.5% to about 7.0%. Grain orientation is achieved through selected rolling, annealing and tempering steps. The steel sheets are finally dipolar oriented in the rolling direction and may be magnetized. Such steel sheets are often produced as steel strips with a thickness of about 0.2 to about 0.4 mm. To protect them against corrosion until processing (transport, blanking, etc.), the sheets are usually provided with a layer of about 1 to 2 μm of Mg silicate ("forsterite") already in the factory, i.e. immediately after production. This is achieved by coating with MgO, which reacts with the surface silicon from the steel during the annealing process ("batch annealing") to become silicate. This coating is hereinafter referred to as "base coating".
[0004] Methods for applying a "base coat" are described, for example, in DE 19816200, DE 60219158 and DE 2743859 and essentially comprise the following steps: - applying an aqueous MgO dispersion of about 10%; - Complete drying at 100℃; - annealing in a hydrogen gas atmosphere at 1000-1350°C; - cooling, and - Cleaning step: Brush off excess MgO.
[0005] The underlying coating provides sufficient temporary protection against corrosion and is essentially electrically insulating.
[0006] Depending on the type of coating, this can cause irregularities in the underlying coating, especially the finest pores, which may go unnoticed initially but cause delayed corrosion.
[0007] US 4,120,702 discloses a method for coating steel sheets having a protective silicate layer by first coating their surface with an aqueous solution containing phosphate ions, silica particles, iron and / or manganese ions and negative ions. During the coating method, the steel sheets are then heated to a temperature between 400°C and 1100°C for about 4 to 10 minutes, thereby forming a protective phosphate layer.
[0008] It is the object of the present invention to provide methods and means which make it possible to improve the corrosion resistance of grain-oriented electrical steels and to electrically insulate their surface, and in addition these means should not contain environmentally harmful metals such as chromium, which are present in many current coating means for grain-oriented electrical steels.
[0009] It is a further object of the present invention to provide a composition for coating grain-oriented electrical steel which can be used as is without mixing several components to ensure user convenience and which can be stored for long periods without quality limitations. Summary of the Invention
[0010] The present invention relates to - aluminum cations, - manganese cations, dihydrogen phosphate, hydrogen phosphate and / or phosphate anions, - Colloidal silica and - Optionally, iron cations wherein the aluminum cation is Al 2 O 3 The manganese cation is represented as MnO, and the dihydrogen phosphate, hydrogen phosphate and / or phosphate anions are represented as P 2 O 5 and colloidal silica is SiO 2 and optionally the iron cation is represented as FeO, which are represented as (Al 2 O 3 ) 2 (MnO) 1 . 8-2 . 4 (FeO) 0-0 . 2 (P 2 O 5 ) 5-7 (SiO 2 ) ≧30 The present invention relates to an aqueous composition for coating grain-oriented electrical steel, the aqueous composition being present in a composition represented by the sum formula:
[0011] Surprisingly, it has been shown that the problem discussed at the beginning can be solved by means of the aqueous solution according to the invention. The storage-stable composition according to the invention makes it possible to make grain-oriented electrical steel corrosion-resistant and to protect it and to electrically insulate it, said composition being free of any environmentally harmful metals such as chromium. Thereby, the composition according to the invention can be painted directly on the steel or on a steel substrate coated with forsterite.
[0012] A further aspect of the invention relates to a method for producing an aqueous composition for coating grain-oriented electrical steel, comprising the step of mixing a compound liberating aluminium cations, a compound liberating manganese cations, a compound liberating dihydrogen phosphate, hydrogen phosphate and / or phosphate anions, colloidal silica and optionally a compound liberating iron cations, as defined in the present patent application (see claim 1).
[0013] To prepare the composition of the present invention, the individual compounds are dissolved in water as described above.The method of mixing such compounds with water is well described in the prior art.By mixing these components, it is possible to prepare a storage stable composition.
[0014] Another aspect of the invention relates to a method for coating grain oriented electrical steel comprising applying an aqueous composition according to the invention or an aqueous composition which can be produced according to the method according to the invention.
[0015] A further aspect of the present invention relates to grain oriented electrical steel, preferably grain oriented electrical steel sheet, obtainable by the coating method according to the present invention.
[0016] Another further aspect of the present invention relates to a grain oriented electrical steel, preferably a grain oriented electrical steel sheet, comprising a coating obtainable by painting the aqueous composition according to the present invention or the aqueous composition that can be produced according to the method according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The aqueous composition according to the invention comprises, in addition to water, aluminum cations, manganese cations, dihydrogen phosphate, hydrogen phosphate and / or phosphate anions, colloidal silica and optionally iron cations in a specific molar ratio to one another. This ratio is represented by the chemical formula (Al 2 O 3 ) 2 (MnO) 1 . 8-2 . 4 (FeO) 0-0 .2 (P 2 O 5 ) 5-7 (SiO 2 ) ≧30 where the aluminum cation contained in the composition is Al 2 O 3 The manganese cation is represented as MnO, and the dihydrogen phosphate, hydrogen phosphate and / or phosphate anions are represented as P 2 O 5 and colloidal silica is SiO 2 and the optional iron cation is expressed as FeO. The metal cations are preferably added to the aqueous composition as metal hydroxides, metal oxides or metal salts. The dihydrogen phosphate, hydrogen phosphate and / or phosphate anions may be mixed into the composition either as phosphoric acid or as phosphate salts.
[0018] According to a preferred embodiment of the present invention, the above-mentioned components are added to the aqueous composition of the present invention, which has the chemical formula (Al 2 O 3 ) 2 (MnO) 1 . 8-2 . 4 (FeO) 0-0 . 2 (P 2 O 5 ) 5-7 (SiO 2 ) 30-100 , preferably (Al 2 O 3 ) 2 (MnO) 1 . 8-2 . 4 (FeO) 0-0 . 2 (P 2 O 5 ) 5-7 (SiO 2 ) 30-80 , more preferably (Al 2 O 3 ) 2 (MnO) 1 . 8-2 . 4 (FeO) 0-0 . 2 (P2 O 5 ) 5-7 (SiO 2 ) 30-70 is added in an amount such that
[0019] The aqueous composition according to the invention may also contain, in addition to or instead of the iron cations, other metal cations (apart from the aluminum and manganese cations), the molar ratio of these metal cations to the other components in the composition, expressed as oxides, corresponding to the sum of the iron cations (see in this respect claim 1).
[0020] This aqueous composition can be used to coat grain-oriented electrical steel, in particular grain-oriented electrical steel sheet. After its production, grain-oriented electrical steel sheet is prone to corrosion and is therefore coated with a base coating (generally an aqueous MgO dispersion). This base coating can usually only insufficiently protect the steel sheet against corrosion due to the micro- and macro-pores in the coating, so it is necessary to provide the base-coated steel sheet with an additional coating. This (additional) coating can be obtained by the aqueous composition according to the invention.
[0021] Pores in the underlying coating can be detected, for example, by applying a dilute permanganate solution. Depending on the degree of porosity, such a solution will fade in a time- and concentration-dependent manner, triggered by the access of Mn VIII ions to the selectively exposed steel surface and their oxidation products (occurring simultaneously with the reduction of Mn VII to Mn II / III). If such porosity is determined in such a test, this defect can also be repaired by the coating or composition according to the invention, respectively. Thereby, the pores are closed in the first coating and at the same time a sustainable protection against corrosion is established, which protection is also evident on the basis of the excellent electrical insulation.
[0022] The aqueous compositions of the invention form a highly effective protection against corrosion on the basis of a dense layer of silicates and phosphates. The coatings further have the following properties: hydrolysis resistance, annealing resistance up to 1000° C., electrical insulation, good adhesion to the underlying coating (forsterite layer) or directly to the steel surface, respectively, non-stickiness under processing conditions, attenuation of sound waves caused by magnetically limited vibrations (in transformers, "transformer noise") in subsequent painting operations. The coating means described in the prior art are mostly mixed immediately before their use and are not available as ready-to-use compositions, but they are superior due to their comparable properties, even if they result in significantly inferior quality in terms of the above-mentioned properties compared to the coatings according to the invention. As an example in this respect, reference should be made to DE 2247269, in which such coating means are disclosed. It is a particular feature of the compositions described therein that they contain chromium in order to ensure the desired corrosion-inhibiting properties of the silicate / phosphate matrix used. However, Cr VI compounds are increasingly legally undesirable due to their harmful effects on human health and the environment.
[0023] It is therefore necessary to provide compositions that are free of chromium without adversely affecting the advantageous properties mentioned. However, obvious variants of substituting tin, vanadium, titanate, zirconium complexes for chromium have been unsuccessful, since such compounds are also either toxic, entail poor stability of the compositions, or are not available in larger quantities at low cost. In particular, the poor stability of such compositions is particularly disadvantageous as the individual components therefore have to be stored separately and can only be mixed immediately before their use.
[0024] The aqueous compositions of the present invention are characterized in that they are chromium-free, storage stable (at least 3 months at room temperature of 22° C.), consist of only one component, and that the coatings that can be produced with them have the required physical properties listed above.
[0025] Al2 O 3 It has been shown that if the ratio of Al:MnO is reduced below 1:0.9, then the stability of the composition is significantly reduced, and at 1:0.75 it is further reduced or absent. In contrast, a ratio above 1:1.2 leads to increased stability problems (turbidity, emissions) in the liquid preparation, resulting in inclusions, turbidity, undesirable color effects and pores in the final cured coating. According to a particularly preferred embodiment of the present invention, Al is added to the composition. 2 O 3 The ratio of MnO to MnO is from 1:1 to 1:1.2, more preferably from 1:1.1 to 1:1.2.
[0026] SiO 2 :P 2 O 5 The ratio of SiO should preferably exceed 4.3. However, according to a preferred embodiment of the present invention, this ratio is greater than 4.3 and less than 16.7, more preferably greater than 4.3 and less than 13.3. 2 :P 2 O 5 If the ratio is less than 4.3, then this may result in problems with hydrolysis and / or corrosion resistance of the coating which may occur with the composition according to the invention.
[0027] Al 2 O 3 :P 2 O 5 The ratio of SiO 2 To ensure colloid resistance, it should preferably exceed 1:2.5. Depending on the concentration of further cations, especially manganese, P 2 O 5 The portion should be adjusted stoichiometrically.
[0028] In a particular embodiment of the invention, if pores are detected in the underlying coating (forsterite, see above), part of the manganese moieties may be replaced or supplemented by or with iron oxide in a second coating (which may be produced with the composition of the invention).
[0029] According to the prior art, MnFe mixed phosphates are poorly soluble and therefore contribute advantageously to the homogeneity of the undercoat (pore closure) as well as to the stability of the second coating (hydrolysis resistance). Surprisingly, this can occur optimally with the use of iron II oxalate, which is known to undergo reductive pyrolysis at temperatures above about 600° C., thus replenishing the impurities in the undercoat with iron oxide or iron phosphate, respectively, as well as reducing the already anoxidized steel surface.
[0030] According to a preferred embodiment of the present invention, the SiO 2 The number is from 30 to 100, preferably from 30 to 80, and more preferably from 30 to 70.
[0031] According to a further preferred embodiment of the present invention, P in the formula 2 O 5 is from 5.4 to 6.8, preferably from 5.6 to 6.6, and more preferably from 5.8 to 6.4.
[0032] The aluminum cations, manganese cations, dihydrogen phosphate, hydrogen phosphate and / or phosphate anions and optional iron cations present in the compositions according to the invention may be introduced therein by mixing different salts, hydroxides, oxides and / or salts with water. Thus, according to a preferred embodiment of the invention, the compositions according to the invention comprise aluminum hydroxide and / or aluminum phosphate.
[0033] Manganese cations are preferably added to the aqueous composition according to the invention as manganese(II) oxide, manganese(II) oxalate and / or manganese(II) hydroxide.
[0034] According to a preferred embodiment of the invention, the iron cations are added to the aqueous composition according to the invention as iron(II) oxide and / or iron(II) oxalate, with iron(II) oxalate being particularly preferred.
[0035] Instead of or in addition to the iron cation, the composition of the invention may further comprise other or further respective metal cations capable of forming sparingly soluble phosphates or pyrophosphates, respectively. In the composition according to the invention, the metal cations expressed as metal oxides are present in the same stoichiometric ratio to each other as shown in the chemical formula according to claim 1, with the exception of the aluminum and manganese cations, relative to the iron cation expressed as iron oxide.
[0036] It has been shown by the present invention that it is particularly advantageous for the colloidal silica contained in the aqueous solution to have no charge, i.e. colloidal silica or the like that contains charged metal ions, respectively, is less preferred or desired, for this reason the colloidal silica in the aqueous composition according to the invention is essentially free of a surface charge.
[0037] According to a preferred embodiment of the present invention, the colloidal silica comprises silica particles, preferably spherical silica particles, with a size between 5 and 80 nm, preferably between 5 and 60 nm, more preferably between 5 and 40 nm.
[0038] The silica particles in the composition according to the invention have a size of 5 nm and a diameter of 400 to 450 nm. 2 / g, 180 to 200 m at 15 nm size 2 / g, 130 to 150 m at 20 nm size 2 / g specific surface area, 100 to 120 m at 25 nm size 2 / g specific surface area, 90 to 110 m at 30 nm size 2 / g specific surface area, 60 to 70 m at 35 nm size 2 / g specific surface area, 40 to 50 m at 40 nm size 2 / g.
[0039] Since only the hydroxyl groups of the colloidal silica that are present at the surface and therefore freely available for reaction and condensation are available due to the compactness of the matrix formed, the size of the spheres, their specific surface area as well as the free availability of hydroxyl groups (e.g. not blocked by "stabilization" of sodium ions) are important for the durability of the liquid preparation as well as for the required quality of the final coating that can be produced from the composition.
[0040] According to a preferred embodiment of the present invention, the ratio of the total specific surface area of the colloidal silica particles to the total number of moles of all metal oxides is from 1:10000 to 1:200000, preferably from 1:20000 to 1:150000, more preferably from 1:25000 to 1:100000, even more preferably from 1:30000 to 1:80000.
[0041] According to a further preferred embodiment of the present invention, the total of metal ions expressed as oxides in the composition, in particular Al 2 O 3 and manganese cations, expressed as MnO, to silica is from 1:6.5 to 1:26.5, preferably from 1:6.8 to 1:20, more preferably from 1:7.5 to 1:18, more preferably from 1:8 to 1:16.
[0042] According to a particularly preferred embodiment of the invention, if the surface is coated with the aqueous composition with a layer thickness of less than 1.5 μm, preferably less than 1 μm, the sum of the metal ions, expressed as oxides, in the composition, in particular Al 2 O 3 The molar ratio of the sum of aluminum cations, expressed as aluminium cations, and manganese cations, expressed as MnO, to silica is preferably from 1:9 to 1:13, more preferably from 1:10 to 1:12.
[0043] According to a particularly preferred embodiment of the invention, if the surface is coated with the aqueous composition having a layer thickness of 2 to 10 μm, preferably 2 to 5 μm, the total amount of metal ions, expressed as oxides, in the composition, in particular Al 2 O 3 The molar ratio of the sum of aluminum cations, expressed as aluminium cations, and manganese cations, expressed as MnO, to silica is preferably from 1:10 to 1:14, more preferably from 1:11 to 1:13.
[0044] According to another preferred embodiment of the invention, the aqueous composition according to the invention has a solids content of between 10 and 70%, preferably from 20 to 60%, more preferably from 25 to 40%.
[0045] A further aspect of the invention relates to a method for producing an aqueous composition for coating grain oriented electrical steel, comprising the step of mixing a compound liberating aluminium cations, a compound liberating manganese cations, a compound liberating dihydrogen phosphate, hydrogen phosphate and / or phosphate anions, a compound liberating colloidal silica and optionally iron cations as defined above.
[0046] An ion-releasing compound is a compound that is capable of liberating an ion in water (e.g., a metal ion such as aluminum). The ion-releasing compound may be a salt, oxide, oxalate or hydroxide.
[0047] Another further aspect of the present invention relates to a method for coating grain oriented electrical steel comprising applying the aqueous composition according to the present invention or the aqueous composition producible by the method according to the present invention.
[0048] According to another preferred embodiment of the present invention, the grain oriented electrical steel is undercoated with forsterite.
[0049] As mentioned earlier, the grain oriented electrical steel to be coated may include a base coating to protect against rapid corrosion after manufacture. The base coating preferably includes forsterite.
[0050] According to another preferred embodiment of the invention, the grain oriented electrical steel has the form of a steel sheet. Such a steel sheet may be used, for example, for manufacturing a transformer.
[0051] According to a particularly preferred embodiment of the invention, the aqueous composition is applied at a concentration of 1 to 50 g / m on grain oriented electrical steel. 2 , preferably from 2 to 40 g / m 2 , more preferably from 3 to 30 g / m 2 , more preferably 4 to 20 g / m 2 is applied in an amount of
[0052] The water-based composition is preferably applied onto the grain oriented electrical steel by dipping, rolling or spraying.
[0053] According to a preferred embodiment of the present invention, the grain oriented electrical steel coated with the aqueous composition is treated at a temperature of 500°C to 900°C, preferably 600°C to 850°C.
[0054] According to another preferred embodiment of the invention, the aqueous composition is applied on the grain-oriented electrical steel with a layer thickness of 100 nm to 20 μm, preferably 200 nm to 10 μm.
[0055] A further aspect of the present invention relates to a grain oriented electrical steel, preferably a grain oriented electrical steel sheet, obtainable by the method according to the present invention.
[0056] Another further aspect of the present invention relates to a grain oriented electrical steel, preferably a grain oriented electrical steel sheet, comprising a coating obtainable by painting the aqueous composition according to the present invention or the aqueous composition which can be produced according to the process according to the present invention.
[0057] The present invention relates inter alia to the following embodiments: 1. An aqueous composition for coating grain-oriented electrical steel, - aluminum cations, - manganese cations, dihydrogen phosphate, hydrogen phosphate and / or phosphate anions, - Colloidal silica and optionally an iron cation, and wherein the Al is present in the composition. 2 O 3 aluminum cations represented as MnO; manganese cations represented as MnO; P 2 O 5 dihydrogen phosphate, hydrogen phosphate and / or phosphate anion, SiO 2 and optionally, iron cations represented as FeO, collectively represented as (Al 2 O 3 ) 2 (MnO) 1 . 8-2 . 4 (FeO) 0-0 . 2 (P 2 O 5 ) 5-7 (SiO 2 ) ≧30 The aqueous composition has the formula:
[0058] 2. SiO in the chemical formula 2 is from 30 to 100, preferably from 30 to 80, more preferably from 30 to 70.
[0059] 3. P in the chemical formula 2 O 5 The aqueous composition according to embodiment 1 or 2, wherein the number is from 5.4 to 6.8, preferably from 5.6 to 6.6, more preferably from 5.8 to 6.4.
[0060] 4. An aqueous composition according to any of embodiments 1 to 3, comprising aluminum hydroxide and / or aluminum phosphate.
[0061] 5. An aqueous composition according to any of embodiments 1 to 4, comprising manganese(II) oxide, manganese(II) oxalate and / or manganese(II) hydroxide.
[0062] 6. An aqueous composition according to any of embodiments 1 to 5, comprising iron oxide, iron(II) oxide and / or iron(II) oxalate.
[0063] 7. The aqueous composition according to any of the preceding embodiments, wherein the colloidal silica has no surface charge.
[0064] 8. The aqueous composition according to any of the preceding embodiments, wherein the colloidal silica comprises silica particles, preferably spherical silica particles, having a size between 5 nm and 80 nm, preferably between 5 nm and 60 nm, more preferably between 5 nm and 40 nm.
[0065] 9. An aqueous composition according to any of the preceding embodiments, wherein the specific surface area of the colloidal silica has a ratio of 1:25000 to 1:100000, preferably 1:30000 to 1:80000, relative to the total number of moles of all metal oxides contained in the composition.
[0066] 10. The silica particles in the composition according to the invention have a size of 5 nm and a particle size of 400 to 450 nm. 2 / g, 180 to 200 m at 15 nm size 2 / g, 130 to 150 m at 20 nm size 2 / g specific surface area, 100 to 120 m at 25 nm size 2 / g specific surface area, 90 to 110 m at 30 nm size 2 / g specific surface area, 60 to 70 m at 35 nm size 2 / g specific surface area, 40 to 50 m at 40 nm size 2 10. The aqueous composition according to embodiment 8 or 9, having a specific surface area of 100 / g.
[0067] 11. The aqueous composition according to any of the preceding embodiments, wherein the ratio of the sum of the specific surface area of the particles of colloidal silica to the sum of the moles of all metal oxides is from 1:10000 to 1:200000, preferably from 1:20000 to 1:150000, more preferably from 1:25000 to 1:100000, and even more preferably from 1:30000 to 1:80000.
[0068] 12. The aqueous composition according to any of the preceding embodiments, wherein the molar ratio of the sum of metal ions, expressed as oxides, in the composition to silica is from 1:6.5 to 1:26.5, preferably from 1:6.8 to 1:20, more preferably from 1:7.5 to 1:18, more preferably from 1:8 to 1:16.
[0069] 13. An aqueous composition according to any of the preceding embodiments, in which the molar ratio of the sum of metal ions, expressed as oxides, to silica in the composition is preferably from 1:9 to 1:13, more preferably from 1:10 to 1:12, if the surface is coated with the aqueous composition with a layer thickness of less than 1.5 μm, preferably less than 1 μm.
[0070] 14. An aqueous composition according to any of the preceding embodiments, in which the molar ratio of the sum of metal ions, expressed as oxides, to silica in the composition is preferably from 1:10 to 1:14, more preferably from 1:11 to 1:13, if the surface is coated with the aqueous composition with a layer thickness of from 2 to 10 μm, preferably from 2 to 5 μm.
[0071] 15. The aqueous composition according to any of the preceding embodiments, having a solids content between 10% and 70%, preferably between 20% and 60%, more preferably between 25% and 40%.
[0072] 16. A method for producing an aqueous composition as defined in one of embodiments 1 to 15 for coating grain-oriented electrical steel, comprising mixing a compound liberating aluminum cations, a compound liberating manganese cations, a compound liberating dihydrogen phosphate, hydrogen phosphate and / or phosphate anions, a compound liberating colloidal silica and optionally iron cations.
[0073] 17. A method for coating grain-oriented electrical steel, comprising applying an aqueous composition according to any of embodiments 1 to 15 or an aqueous composition that can be produced according to the method according to embodiment 16.
[0074] 18. The method according to embodiment 17, wherein the grain-oriented electrical steel is undercoated with forsterite.
[0075] 19. The method according to embodiment 17 or 18, wherein the grain-oriented electrical steel has the form of a sheet.
[0076] 20. The aqueous composition is applied to grain-oriented electrical steel at a rate of 1 to 50 g / m 2 , preferably from 2 to 40 g / m 2 , more preferably from 3 to 30 g / m 2 , more preferably 4 to 20 g / m 2 The method according to any of embodiments 17 to 19, wherein the coating is applied in an amount of
[0077] 21. The method according to one of embodiments 17 to 20, wherein the aqueous composition is applied onto the grain-oriented electrical steel by dipping, rolling or spraying.
[0078] 22. The method according to any of embodiments 17 to 20, wherein the grain-oriented electrical steel coated with the aqueous composition is treated at a temperature of 500°C to 900°C, preferably 600°C to 850°C.
[0079] 23. The method according to any of embodiments 17 to 22, wherein the aqueous composition is applied onto the grain-oriented electrical steel with a layer thickness of 100 nm to 20 μm, preferably 200 nm to 10 μm.
[0080] 24. Grain-oriented electrical steel, preferably a grain-oriented electrical steel sheet, obtainable by a method according to any of embodiments 17 to 23.
[0081] 25. A grain-oriented electrical steel, preferably a grain-oriented electrical steel sheet, comprising a coating obtainable by painting the aqueous composition according to any of embodiments 1 to 15 or the aqueous composition which can be produced according to the method according to embodiment 16. EXAMPLES
[0082] [Example 1] Preparation of an aqueous composition for coating grain-oriented electrical steel Into a mixture of 400 g of 75% phosphoric acid and 135 ml of water, 78 g of aluminum hydroxide, followed by dissolving 40 g of manganese(II) oxide and 7 g of iron(II) oxalate, was made a clear, viscous phosphate-containing solution. The resulting solution had a total weight of 660 g. To 200 g of the phosphate-containing solution, 800 g of charge-free silica sol (colloidal silica) with a solid content of 30% (SiO 2 with an average diameter of 35 nm) was added. 2 The calculated composition was (Al 2 O 3 ) 2 (MnO) 2 . 2 (FeO) 0 . 2 (SiO 2 ) 53 (P 2 O 5 ) 6 . 3 (Composition 1).
[0083] 5 g / m on pre-coated GO steel sheet (i.e., grain-oriented electrical steel sheet coated with forsterite) 2 This was then briefly dried in air and the layer cured at 820° C. for 60 seconds.
[0084] By adjusting the stoichiometric ratios of the above components, it was possible to prepare the following further compositions (Compositions 2 to 9): Composition 2 (Al 2 O 3 ) 2 (MnO) 2 . 1 (FeO) 0 . 18 (SiO 2 ) 75 (P 2 O 5 ) 6 . 2 Composition 3 (Al 2 O 3 ) 2 (MnO) 2 . 2 (FeO) 0 . 18 (SiO 2 ) 49 (P 2 O 5 ) 6 . 3 Composition 4 (Al 2 O 3 ) 2 (MnO) 2 . 0 (FeO) 0 . 2 (SiO 2 ) 32 (P 2 O 5 ) 6 . 5 Composition 5 (iron oxide free) (Al 2 O 3 ) 2 (MnO) 2 . 2 (SiO 2 ) 55 (P 2 O 5 ) 6 . 1 Composition 6 (Al 2 O 3 )2 (MnO) 1 . 75 (FeO) 0 . 15 (SiO 2 ) 55 (P 2 O 5 ) 6 . 2 Composition 7 (iron oxide instead of iron oxalate in phosphate-containing solutions) (Al 2 O 3 ) 2 (MnO) 2 . 2 (FeO) 0 . 2 (SiO 2 ) 53 (P 2 O 5 ) 7
[0085] Compositions 2 to 7 were also applied to GO steel sheets with a base coat of 5 g / m 2 The coating was applied in an amount of 0.01g / g, briefly dried in air and then cured at 820°C for 60 seconds.
[0086] [Table 1]
[0087] [Example 2] Comparative composition: In order to illustrate the advantages of the compositions according to the invention over other compositions according to the prior art, respective tests were carried out using comparative compositions. Comparative Composition 1 (Example B1 (Al, Mn) of WO2014 / 180610) (Al 2 O 3 ) 8 (MnO) 2 (SiO 2 ) 20 (P 2 O 5 ) 27 Comparative composition 2 (Example 1 of EP2264220Al (KMnO4 )) (Al 2 O 3 ) 5 (MnO 2 )(K 2 O) 0 . 5 (SiO 2 ) 29 (P 2 O 5 ) 5 . 5 Comparative composition 3 (Example 3 (Al, Cr) of DE 2247269) (Al 2 O 3 ) 2 (CrO 3 ) 2 . 4 (SiO 2 ) 12 (P 2 O 5 ) 6 Comparative composition 4 (Example B3 (Al, Mn, Zn, Mg) of WO2014 / 180610) (Al 2 O 3 ) 1 . 6 (MnO) 0 . 6 (ZnO) 0 . 2 (MgO) 2 (SiO 2 ) 16 (P 2 O 5 ) 5
[0088] Comparative compositions 1 to 4 were then applied at 5 g / m2 onto the precoated GO steel sheets as described in Example 1. 2 The coating was applied in an amount of 0.01g / g, briefly dried in air and then cured at 820°C for 60 seconds.
[0089] [Table 2]
[0090] [Example 3] Testing of the Compositions and Coatings of Examples 1 and 2 Several tests were carried out to determine or evaluate the quality of the compositions according to Examples 1 and 2 and their suitability for coating grain oriented electrical steel, respectively.
[0091] Stability of the composition It is the goal of the present invention to provide a storage stable aqueous composition to ensure sufficient user convenience.For this reason, the stability of the aqueous composition is evaluated.In this regard, it is observed whether the aqueous composition remains stirrable and whether particles are deposited over a long period of time.Both properties are important for the storage stability of the composition.
[0092] Visual appearance of steel surfaces (corrosion appearance / hydrolysis resistance) A crucial quality criterion for a composition used to coat grain-oriented electrical steel is its ability to protect the coated steel against corrosion. For this assertion, the central part of coated steel sheet samples was wetted with water and their undercoating containing Mg silicate (forsterite) was coated with the compositions according to examples 1 and 2, tightly packed in a water- and steam-resistant film and stored at 90° C. in a heating box for 8 hours. The surface of the coated steel sheet was then optically evaluated.
[0093] Cured Coating Color The compositions were painted onto GO steel sheets, subsequently heated (see above), and the color was then visually evaluated.
[0094] Coating inclusions (solid) Inclusions in the final coating can also represent a relevant criterion for the quality of the composition according to the invention. Any inclusions were determined and evaluated visually.
[0095] Pore and bubble formation The formation of bubbles in the final coating on the steel sheet is generally undesirable as the bubbles are precursors to the subsequent appearance of corrosion. The formation of bubbles can be assessed visually.
[0096] result The results of the above tests are shown in the table below.
[0097] [Table 3]
[0098] The results impressively show that the compositions according to the invention (compositions 1 to 5 and 7) have a high storage stability of more than 3 months and therefore the coatings produced therewith have high hydrolysis resistance and extremely low susceptibility to corrosion. The comparative compositions from the prior art have low storage stability in the ready-to-use mixtures. The hydrolysis stability of the coatings produced therewith is also not optimal. Composition 6, in addition, has a low Al content in the composition. 2 O 3 It is shown that a lower molar ratio between MnO and MnO (2:1.75) would result in lower storage stability.
Claims
1. 1. An aqueous composition for coating grain oriented electrical steel, comprising: - aluminum cations, - manganese cations, dihydrogen phosphate, hydrogen phosphate and / or phosphate anions, colloidal silica, and - optionally, iron cations and wherein Al is present in the composition. 2 O 3 aluminum cations represented as MnO; manganese cations represented as P 2 O 5 dihydrogen phosphate, hydrogen phosphate and / or phosphate anion, SiO 2 and optionally an iron cation represented as FeO, 2 O 3 ) 2 (MnO) 1.8-2.4 (FeO) 0-0.2 (P 2 O 5 ) 5-7 (SiO 2 ) ≧ 30 The aqueous composition has the following chemical formula:
2. In the above formula, SiO 2 The aqueous composition of claim 1 , wherein the number of is from 30 to 100.
3. The aqueous composition of claim 1, wherein the number of SiO 2 s in said chemical formula is from 30 to 80.
4. The aqueous composition of claim 1, wherein the number of SiO 2 s in said chemical formula is from 30 to 70.
5. In the above chemical formula, P 2 O 5 The aqueous composition according to any one of claims 1 to 4, wherein the number is from 5.4 to 6.
8.
6. The aqueous composition according to claim 1, wherein the number of P 2 O 5 in the chemical formula is from 5.6 to 6.
6.
7. The aqueous composition according to claim 1, wherein the number of P 2 O 5 in the chemical formula is from 5.8 to 6.
4.
8. An aqueous composition according to any one of claims 1 to 7, comprising aluminium hydroxide and / or aluminium phosphate.
9. 9. The aqueous composition according to any one of claims 1 to 8, comprising manganese(II) oxide, manganese(II) oxalate and / or manganese(II) hydroxide.
10. 10. The aqueous composition according to any one of claims 1 to 9, comprising iron oxide, iron(II) oxide and / or iron(III) oxalate.
11. The aqueous composition according to any one of claims 1 to 10, wherein the colloidal silica has no surface charge.
12. 12. The aqueous composition of any one of claims 1 to 11, wherein the colloidal silica comprises silica particles with a size between 5 and 80 nm.
13. The aqueous composition of claim 1, wherein the colloidal silica comprises silica particles having a size between 5 and 60 nm.
14. The aqueous composition of claim 1, wherein the colloidal silica comprises silica particles having a size between 5 and 40 nm.
15. The aqueous composition according to claim 12, wherein the silica particles are spherical silica particles.
16. 16. An aqueous composition according to any one of the preceding claims, wherein in said composition the molar ratio of the sum of metal ions, expressed as oxides, to silica is from 1:6.5 to 1:26.
5.
17. An aqueous composition according to any one of claims 1 to 15, wherein the molar ratio of the sum of metal ions, expressed as oxides, in the composition to silica is from 1:6.8 to 1:
20.
18. An aqueous composition according to any one of claims 1 to 15, wherein the molar ratio of the sum of metal ions, expressed as oxides, in the composition to silica is from 1:7.5 to 1:
18.
19. An aqueous composition according to any one of claims 1 to 15, wherein the molar ratio of the sum of metal ions, expressed as oxides, to silica in the composition is from 1:8 to 1:
16.
20. 20. Aqueous composition according to any one of the preceding claims, in which, if a surface is coated with said aqueous composition with a layer thickness of less than 1.5 μm, the molar ratio of the sum of metal ions, expressed as oxides, to silica in the composition is from 1:9 to 1:
13.
21. An aqueous composition described in any one of claims 1 to 19, in which if a surface is coated with the aqueous composition with a layer thickness of less than 1.5 μm, the molar ratio of the sum of metal ions, expressed as oxides, in the composition to silica is from 1:10 to 1:
12.
22. An aqueous composition described in any one of claims 1 to 19, in which if a surface is coated with the aqueous composition with a layer thickness of less than 1 μm, the molar ratio of the sum of metal ions, expressed as oxides, in the composition to silica is from 1:9 to 1:
13.
23. An aqueous composition described in any one of claims 1 to 19, in which if a surface is coated with the aqueous composition with a layer thickness of less than 1 μm, the molar ratio of the sum of metal ions, expressed as oxides, in the composition to silica is from 1:10 to 1:
12.
24. 24. Aqueous composition according to any one of the preceding claims, in which, if a surface is coated with said aqueous composition with a layer thickness of from 2 to 10 μm, the molar ratio of the sum of metal ions, expressed as oxides, to silica in the composition is from 1:10 to 1:
14.
25. An aqueous composition described in any one of claims 1 to 23, in which if a surface is coated with the aqueous composition with a layer thickness of 2 to 10 μm, the molar ratio of the sum of metal ions, expressed as oxides, in the composition to silica is 1:11 to 1:
13.
26. An aqueous composition described in any one of claims 1 to 23, in which if a surface is coated with the aqueous composition with a layer thickness of 2 to 5 μm, the molar ratio of the sum of metal ions, expressed as oxides, in the composition to silica is from 1:10 to 1:
14.
27. An aqueous composition described in any one of claims 1 to 23, in which if a surface is coated with the aqueous composition with a layer thickness of 2 to 5 μm, the molar ratio of the sum of metal ions, expressed as oxides, in the composition to silica is 1:11 to 1:
13.
28. A method of coating grain oriented electrical steel comprising applying an aqueous composition according to any one of claims 1 to 27.
29. 30. The method of claim 28, wherein the grain oriented electrical steel is undercoated with forsterite.
Citation Information
Patent Citations
Method of treating silicon steel article
JP1978086647A
Method of forming top coating insulation film of tension addition type without containing chromium oxide on directional silicone steel plate
JP1981075579A
Grain oriented magnetic steel sheet for magnetic shielding having excellent film adhesion property and corrosion resistance
JP2004143564A
Grain oriented silicon steel sheet and method for producing the same
JP2014095129A
Chromium-Free Coating for the Electrical Insulation of Grain-Oriented Electrical Steel Strip
US20160060465A1