Manufacturing method of slide member

By manufacturing sliding members with ethylene-tetrafluoroethylene copolymer under ambient conditions, the inefficiencies of PTFE processing are overcome, enhancing manufacturing efficiency and maintaining sliding properties and strength.

JP7575403B2Active Publication Date: 2024-10-29SUMITOMO ELECTRIC INDUSTRIES LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021563829
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-13
Filing Date
2020-11-20
Publication Date
2024-10-29
Estimated Expiration
2040-11-20

AI Technical Summary

Technical Problem

Manufacturing sliding members using polytetrafluoroethylene (PTFE) requires significant equipment, energy, and time to maintain an oxygen-free atmosphere and molten state during electron beam irradiation, limiting manufacturing efficiency.

Method used

Manufacturing sliding members using ethylene-tetrafluoroethylene copolymer (ETFE) without an oxygen-free atmosphere and molten state during electron beam irradiation, utilizing injection molding and electron beam irradiation at room temperature in air, with a dose of 200 to 350 kGy.

Benefits of technology

Improves manufacturing efficiency and maintains excellent sliding properties while ensuring mechanical strength, reducing the need for specialized equipment and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575403000002
    Figure 0007575403000002
  • Figure 0007575403000003
    Figure 0007575403000003
  • Figure 0007575403000004
    Figure 0007575403000004
Patent Text Reader

Abstract

This method according to one mode of the present invention is for manufacturing a sliding member containing an ethylene-tetrafluoroethylene copolymer as a main component, and comprises: a step for processing a material containing the ethylene-tetrafluoroethylene copolymer as a main component; and a step for irradiating, with electron beams, a processed product obtained in the step for processing said material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a slide member and a slide member. This application claims priority to Japanese Application No. 2019-225660, filed on December 13, 2019, and incorporates by reference all of the contents of the above-mentioned Japanese application. [Background technology]

[0002] Sliding members are used, for example, in bearings for automobile engines and engines for other industrial machines, driving parts in the automobile field, piston packings, and the like. As such sliding members, those using fluororesins, particularly polytetrafluoroethylene (PTFE) on the surface layer are known (see JP 2018-185007 A). By using PTFE, the coefficient of dynamic friction with the mating material is reduced while maintaining wear resistance, and the sliding member can also be made excellent in mechanical strength, chemical resistance, easy slippage, heat resistance, weather resistance, non-flammability, and the like. In other words, sliding members using PTFE have excellent sliding properties.

[0003] The above-mentioned sliding member can be produced by laminating a material containing PTFE as a main component on a substrate by, for example, extrusion molding, and irradiating this material with an electron beam in an oxygen-free atmosphere in a molten state. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-185007 A Summary of the Invention

[0005] A method for producing a slide member according to one embodiment of the present disclosure is a method for producing a slide member containing an ethylene-tetrafluoroethylene copolymer as a main component, and includes the steps of processing a material containing an ethylene-tetrafluoroethylene copolymer as a main component, and irradiating an electron beam to a processed body obtained in the processing step.

[0006] A sliding member according to another embodiment of the present disclosure is a sliding member containing an ethylene-tetrafluoroethylene copolymer as a main component, in which the ethylene-tetrafluoroethylene copolymer is crosslinked by irradiation with an electron beam. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a schematic flow diagram showing a method for producing a slide member according to one embodiment of the present disclosure. [Diagram 2] FIG. 2 is a schematic side view showing a procedure for obtaining a processed body in the embodiment. [Diagram 3] FIG. 3 is an example of a DSC curve of an ethylene-tetrafluoroethylene copolymer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] [Problem that this disclosure aims to solve] In the case of a sliding member using PTFE, the excellent properties are exhibited by appropriately crosslinking the material by irradiating the material with an electron beam in an oxygen-free atmosphere and in a molten state. Therefore, when manufacturing the sliding member using the above-mentioned conventional PTFE, there is room for improvement in the manufacturing efficiency in terms of the equipment required for creating an oxygen-free atmosphere and in a molten state, as well as the energy and time required.

[0009] The present disclosure has been made in light of the above-mentioned circumstances, and has an object to provide a manufacturing method for a slide member that is excellent in slidability and can improve manufacturing efficiency, and the slide member.

[0010] [Effects of this disclosure] The manufacturing method of the slide member of the present disclosure and the slide member of the present disclosure have excellent sliding properties and can improve manufacturing efficiency.

[0011] [Description of the embodiments of the present disclosure] The present inventors have discovered that by using ethylene-tetrafluoroethylene copolymer (ETFE) obtained by polymerization of ethylene and tetrafluoroethylene instead of polytetrafluoroethylene (PTFE) obtained by polymerization of tetrafluoroethylene, a sliding member having excellent sliding properties can be obtained even without an oxygen-free atmosphere and a molten state during irradiation with electron beams, and have completed the present invention.

[0012] That is, the manufacturing method of a slide member according to one embodiment of the present disclosure is a manufacturing method of a slide member containing an ethylene-tetrafluoroethylene copolymer as a main component, and includes a step of processing a material containing an ethylene-tetrafluoroethylene copolymer as a main component, and a step of irradiating an electron beam to the processed body obtained in the processing step.

[0013] The method for producing a sliding member uses an ethylene-tetrafluoroethylene copolymer, which is a fluororesin, as the main component of the sliding member, and therefore can obtain a sliding member having excellent sliding properties. Moreover, the method for producing a sliding member does not require an oxygen-free atmosphere and the processed body to be in a molten state during electron beam irradiation, thereby improving production efficiency.

[0014] The exposure dose of the electron beam in the step of irradiating the electron beam is preferably 200 kGy or more. By setting the exposure dose of the electron beam to the lower limit or more, the sliding properties of the obtained slide member can be more reliably improved.

[0015] The exposure dose of the electron beam in the step of irradiating the electron beam is preferably 350 kGy or less. By setting the exposure dose of the electron beam to the above upper limit or less, it is easy to ensure the mechanical strength of the obtained sliding member.

[0016] It is preferable that the conditions of the electron beam irradiation step are not an oxygen-free atmosphere and the processed body is not in a molten state. By irradiating the electron beam under such conditions that are not an oxygen-free atmosphere and are not in a molten state, the manufacturing efficiency can be more reliably improved.

[0017] The atmospheric temperature in the electron beam irradiation step is preferably room temperature. By setting the atmospheric temperature at room temperature in this manner, no equipment or energy for heating or cooling is required, and therefore production efficiency can be further improved.

[0018] The electron beam irradiation step is preferably performed in an air atmosphere, which can further increase the production efficiency since no equipment or energy is required for adjusting the atmosphere.

[0019] The processing method in the processing step is preferably injection molding. By using injection molding as the processing method in the processing step, the processed body can be preliminarily shaped into the desired shape of the sliding member. Therefore, there is no need to process or adjust the processed body into the desired shape after the electron beam irradiation step, which further improves manufacturing efficiency.

[0020] A sliding member according to another embodiment of the present disclosure is a sliding member containing an ethylene-tetrafluoroethylene copolymer as a main component, in which the ethylene-tetrafluoroethylene copolymer is crosslinked by irradiation with an electron beam.

[0021] The sliding member has high production efficiency because it is mainly composed of ethylene-tetrafluoroethylene copolymer, and has excellent sliding properties because the ethylene-tetrafluoroethylene copolymer is crosslinked by electron beam irradiation.

[0022] The endothermic curve peak of the ethylene-tetrafluoroethylene copolymer is present on a DSC curve by differential scanning calorimetry, and the endothermic curve peak is shifted to the low temperature side relative to the endothermic curve peak of an uncrosslinked ethylene-tetrafluoroethylene copolymer, and the amount of shift is preferably 11° C. or more and 20° C. or less. By setting the amount of shift within the above range, the sliding properties can be improved while ensuring the mechanical strength of the sliding member.

[0023] The ratio of the endothermic heat of the ethylene-tetrafluoroethylene copolymer to that of an uncrosslinked ethylene-tetrafluoroethylene copolymer, as determined by a DSC curve obtained by differential scanning calorimetry, is preferably 0.8 to 0.9. By setting the endothermic heat ratio within the above range, the sliding properties of the sliding member can be improved while ensuring the mechanical strength of the sliding member.

[0024] Here, "main component" refers to the component with the highest content, for example, a component with a content of 50% by mass or more. Also, "room temperature" refers to a natural temperature without heating or cooling, and generally refers to a temperature between 15°C and 35°C.

[0025] The "endothermic curve peak on the DSC curve by differential scanning calorimetry" refers to the temperature (P in FIG. 3) at which the absolute value of the endothermic amount is maximum in the DSC curve. Also, the "endothermic amount defined by the DSC curve" corresponds to the area S surrounded by the DSC curve near the endothermic curve peak and the baseline BL, as shown in FIG. 3. Also, the "uncrosslinked ethylene-tetrafluoroethylene copolymer" can be recovered by dissolving it in a solvent from the ethylene-tetrafluoroethylene copolymer irradiated with an electron beam.

[0026] [Details of the embodiment of the present invention] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, a method for producing a slide member and an embodiment of the slide member according to the present invention will be described in detail with reference to the drawings.

[0027] [Method of manufacturing slide member] A method for producing a slide member according to one embodiment of the present disclosure is a method for producing a slide member mainly composed of an ethylene-tetrafluoroethylene copolymer, which includes a step S1 of processing a material mainly composed of an ethylene-tetrafluoroethylene copolymer, and a step S2 of irradiating an electron beam to the processed body obtained in the processing step S1, as shown in FIG.

[0028] <Processing process> In the processing step S1, the material containing an ethylene-tetrafluoroethylene copolymer as a main component is processed as described above.

[0029] The main component of the above material, ethylene-tetrafluoroethylene copolymer (ETFE), is ethylene (C 2 H 4 ) and tetrafluoroethylene (C 2 F 4 ETFE is a fluororesin polymerized with PTFE. ETFE has superior mechanical strength and chemical resistance compared to PTFE.

[0030] The lower limit of the ETFE content in the material is preferably 60% by mass, more preferably 85% by mass, and even more preferably 98% by mass, based on the processed body after processing. It is particularly preferable that the ETFE content is 100% by mass, that is, the processed body after processing is composed only of ETFE. If the ETFE content is less than the lower limit, the sliding properties of the resulting sliding member may be reduced.

[0031] ETFE may contain polymerization units derived from other copolymerizable monomers within the range that does not impair the effects of the present invention. Examples of the polymerization units include perfluoro(alkyl vinyl ether), hexafluoropropylene, (perfluoroalkyl)ethylene, and chlorotrifluoroethylene. The upper limit of the content of the polymerization units may be, for example, 3 mol%.

[0032] The material may contain other optional components. Examples of the optional components include solid lubricants and reinforcing agents. By containing the solid lubricants and reinforcing agents, the lubricity can be improved. Examples of the solid lubricants include molybdenum disulfide. Examples of the reinforcing agents include glass fillers such as glass fiber (glass fiber) and spherical glass, carbon fiber, calcium carbonate, talc, silica, alumina, aluminum hydroxide, and other inorganic fillers.

[0033] The method for processing the above-mentioned material is not particularly limited, and in addition to the well-known extrusion molding and injection molding, powder coating, welding or adhesion to a substrate, etc. can be used.

[0034] As a processing method in the processing step S1, injection molding is preferable. Conventional sliding members using PTFE are easily deformed because they are in a molten state during manufacturing, and are manufactured by laminating them on the surface of a base material to prevent this deformation. For this reason, it is difficult to configure a sliding member only from a material mainly composed of PTFE by injection molding. In contrast, the manufacturing method of the sliding member uses ETFE as the main component, so there is no need to put the processed body in a molten state during manufacturing, and the processed body is less likely to deform. Therefore, in the manufacturing method of the sliding member, the processed body can be made into a desired part shape of the sliding member in advance. In addition, since the manufacturing method of the sliding member can prevent deformation in the step of irradiating the electron beam, there is no need to process or adjust it into a desired shape after the step of irradiating the electron beam, and manufacturing efficiency can be further improved.

[0035] The shape of the processed body obtained in the processing step S1 is appropriately selected depending on the application and processing method of the obtained slide member, such as the shape of a part or a roll of material to be used as a slide member, but it is preferable to have a part shape from the viewpoint of production efficiency as described above.

[0036] The processed body may be a single body made of a material mainly composed of ETFE, or may be a laminated body made of a surface layer containing ETFE laminated on the surface of a substrate. When the processed body is a laminated body, the substrate may be made of metal, ceramics, rubber material, heat-resistant resin, or the like. Examples of the metal include aluminum, iron, copper, stainless steel, and the like. Examples of the ceramic include aluminum oxide, silicon nitride, silicon carbide, tungsten carbide, and the like. Examples of the rubber material include fluororubber, silicone rubber, thermoplastic elastomer, and the like. Examples of the heat-resistant resin include polyimide resin, polyamideimide resin, polyether ether ketone resin, and the like. The surface layer may be made of the material mainly composed of ETFE. The surface layer may cover the entire substrate, or may be laminated on a part of the substrate.

[0037] <Electron beam irradiation process> In the electron beam irradiating step S2, the processed body obtained in the above-described processing step S1 is irradiated with an electron beam.

[0038] The ETFE constituting the processed body is irradiated with the electron beam. This irradiation with the electron beam promotes cross-linking of the ETFE, thereby improving the sliding properties of the resulting sliding member.

[0039] The conditions for irradiating the electron beam are such that the atmosphere is not oxygen-free and the processed body is not in a molten state. By irradiating the electron beam under such conditions that the atmosphere is not oxygen-free and the processed body is not in a molten state, the equipment, energy, and time required for creating an oxygen-free atmosphere and a molten state can be reduced, and therefore the manufacturing efficiency can be more reliably improved.

[0040] In particular, it is preferable that the atmospheric temperature in step S2 of irradiating the electron beam is room temperature. By setting the atmospheric temperature to room temperature in this manner, no equipment or energy is required for heating or cooling. In addition, since deformation of the processed body due to heat can be suppressed, there is no need to adjust the shape of the processed body after irradiating the electron beam. This further improves the manufacturing efficiency of the manufacturing method for the slide member.

[0041] In addition, the electron beam irradiation step may be performed in an air atmosphere, which can further increase the production efficiency since no equipment or energy is required for adjusting the atmosphere.

[0042] The lower limit of the electron beam irradiation dose in the step S2 of irradiating with electron beams is preferably 200 kGy, more preferably 220 kGy, and even more preferably 240 kGy. On the other hand, the upper limit of the electron beam irradiation dose is preferably 350 kGy, and more preferably 320 kGy. If the electron beam irradiation dose is less than the lower limit, the sliding properties of the obtained slide member may not be sufficiently improved. Conversely, if the electron beam irradiation dose exceeds the upper limit, the mechanical strength of the obtained slide member may be reduced.

[0043] If the shape of the processed body obtained in the processing step S1 is the shape of a part to be used as a sliding member, and the conditions for irradiating the electron beam in the electron beam irradiating step S2 are not in a molten state, a desired sliding member can be obtained by this electron beam irradiation. On the other hand, in cases other than the above, processing or adjustment to a desired shape is performed as necessary after the electron beam irradiating step.

[0044] <Advantages> The method for producing a sliding member uses an ethylene-tetrafluoroethylene copolymer, which is a fluororesin, as the main component of the sliding member, and therefore can obtain a sliding member having excellent sliding properties. Moreover, the method for producing a sliding member does not require an oxygen-free atmosphere and the processed body to be in a molten state during electron beam irradiation, thereby improving production efficiency.

[0045] [Sliding member] A sliding member according to another embodiment of the present invention is a sliding member containing an ethylene-tetrafluoroethylene copolymer as a main component, the ethylene-tetrafluoroethylene copolymer being crosslinked by irradiation with an electron beam.

[0046] The slide member is used, for example, in bearings for automobile engines and other industrial machine engines, driving parts in the automobile field, piston packing, etc. The slide member can be manufactured, for example, by using the above-mentioned manufacturing method for a slide member of the present invention.

[0047] The sliding member may be a single body made of a material mainly composed of ethylene-tetrafluoroethylene copolymer (ETFE), or may be a laminate having a structure in which a surface layer containing ETFE is laminated on the surface of a substrate. When the sliding member is a single body rather than a laminate, the material mainly composed of ETFE may be a solidified material described in the above-mentioned method for producing a sliding member. When the sliding member is a laminate, the substrate and surface layer may be the substrate and surface layer described in the above-mentioned method for producing a sliding member.

[0048] The lower limit of the limit PV value of the sliding member is preferably 500 MPa·m / min, more preferably 700 MPa·m / min. If the limit PV value is less than the lower limit, the sliding property of the sliding member may be insufficient. On the other hand, the upper limit of the limit PV value is not particularly limited, but may be, for example, 3000 MPa·m / min. The "limit PV value" is the product of the surface contact pressure (P) and the speed (V), and is a value measured in accordance with the "Sliding Wear Test Method for Plastics" of JIS-K-7218:1986. Under conditions close to the limit PV value, both the friction coefficient and the amount of wear increase, making it difficult for the material to maintain its function. For this reason, the limit PV value is used as an index for judging the sliding property of the sliding member. The measurement conditions for the limit PV value are as follows: the surface roughness of the mating material is Ra=0.28μm based on JIS-B-0601:2001, the surface contact pressure (P) is fixed at 10MPa, and the speed is changed. The test piece for the sliding member is a 45 mm square cold-rolled steel plate (SPCC material) substrate with a thickness of 4.5 mm and a 50 mm square ETFE film with a thickness of 50 μm welded to the substrate.

[0049] The upper limit of the dynamic friction coefficient of the sliding member is preferably 0.15, more preferably 0.1. If the dynamic friction coefficient exceeds the upper limit, the sliding property of the sliding member may be insufficient. The lower limit of the dynamic friction coefficient of the sliding member is not particularly limited, and may be 0.

[0050] When the sliding member is subjected to differential scanning calorimetry, the endothermic curve peak of the ethylene-tetrafluoroethylene copolymer is present on the DSC curve (see FIG. 3). The endothermic curve peak is shifted to the lower temperature side relative to the endothermic curve peak of the uncrosslinked ethylene-tetrafluoroethylene copolymer. The lower limit of the shift amount is preferably 11° C., more preferably 12° C., and even more preferably 13° C. On the other hand, the upper limit of the shift amount is preferably 20° C., and more preferably 18° C. If the shift amount is less than the lower limit, the sliding properties may be insufficient. Conversely, if the shift amount exceeds the upper limit, the mechanical strength may be reduced.

[0051] The lower limit of the ratio of the endothermic heat of the ethylene-tetrafluoroethylene copolymer to the endothermic heat of the uncrosslinked ethylene-tetrafluoroethylene copolymer as determined by the DSC curve by differential scanning calorimetry is preferably 0.8, more preferably 0.83. On the other hand, the upper limit of the endothermic heat ratio is preferably 0.9, more preferably 0.89, and even more preferably 0.88. If the endothermic heat ratio is less than the lower limit, the mechanical strength may decrease. On the other hand, if the endothermic heat ratio exceeds the upper limit, the sliding properties may become insufficient.

[0052] <Advantages> The sliding member has high production efficiency because it is mainly composed of ethylene-tetrafluoroethylene copolymer, and has excellent sliding properties because the ethylene-tetrafluoroethylene copolymer is crosslinked by electron beam irradiation.

[0053] [Other embodiments] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present disclosure is not limited to the configurations of the above-described embodiments, but is indicated by the scope of the claims, and is intended to include all modifications within the meaning and scope equivalent to the scope of the claims.

[0054] In the above embodiment, the conditions for irradiating the electron beam in the step of irradiating the electron beam are not an oxygen-free atmosphere and the workpiece is not in a molten state, but the above conditions can be an oxygen-free atmosphere and a molten state, or an oxygen-free atmosphere but not a molten state, or conversely, a non-oxygen-free atmosphere but a molten state. EXAMPLES

[0055] Hereinafter, the manufacturing method of the slide member and the slide member according to the present disclosure will be specifically described based on examples, but the present disclosure is not limited to these examples.

[0056] [No.1] As shown in Figure 2, a cold-rolled steel plate (SPCC material) substrate 1 and an ETFE film 2 were overlapped. The substrate 1 was 4.5 mm thick and had a square shape with sides of 45 mm, while the ETFE film 2 was 50 mm thick and had a square shape with sides of 50 mm. In addition, a rectangular PTFE film 3 and a SUS plate 4 were overlapped on the surface of the ETFE film 2, and the whole was sandwiched between a pair of welding jigs 5 so that they were in contact with the substrate 1 and the SUS plate 4. In this state, the pair of welding jigs 5 were fastened together with a pair of screws 6 as shown in Figure 2, and the screws 6 were tightened so that a pressure of 3 N·m was applied between the substrate 1 and the ETFE film 2.

[0057] After the welding jig 5 was fixed as described above, the temperature was kept at 300°C for 1.5 hours to weld the ETFE film 2 to the substrate 1. Then, the welding jig 5, the PTFE film 3, and the SUS plate 4 were removed to obtain a processed body in which the ETFE film 2 was laminated on the surface of the substrate 1. In No. 1, this processed body was used as a sliding member. In other words, No. 1 is an iron plate welded with a non-crosslinked ETFE film.

[0058] [No.2~No.13] A processed body was obtained in the same manner as No. 1. The ETFE film 2 of this processed body was irradiated with an electron beam at the dose shown in Table 1. The electron beam was irradiated in an air atmosphere at room temperature without heating or cooling. In this way, sliding members No. 2 to No. 13 were obtained. No. 2 to No. 13 are cross-linked ETFE film-welded iron plates.

[0059] <Evaluation method> The obtained sliding members No. 1 to No. 13 were evaluated for limit PV, tensile strength, tensile elongation, tensile modulus, tear strength and dynamic friction coefficient. The evaluation methods are shown below. The evaluation results are shown in Table 1.

[0060] (Limit PV) The limit PV was measured using a ring-on-disk abrasion tester (testing device: EFM-III 1010 manufactured by A&D) in accordance with JIS-K-7218:1986 "Method of testing sliding abrasion of plastics". A cylinder (outer diameter: 11.6 mm, inner diameter: 7.4 mm) made of S45C was used as the ring-shaped mating material, and the surface roughness based on JIS-B-0601:2001 was set to 0.28 μm. The test conditions were dry (no oil), pressure was kept constant at 10 MPa, and the speed was increased.

[0061] (Tensile strength, tensile elongation and tensile modulus) The measurements of tensile strength, tensile elongation and tensile modulus were performed based on JIS-K-7161-1:2014 "Plastics - Determination of tensile properties - Part 1: General rules."

[0062] (tear strength) The tear strength was measured based on JIS-K-7128-1:1998 "Tear strength of plastic films and sheets".

[0063] (Kinematic friction coefficient) The dynamic friction coefficient was measured from the reaction torque generated in the cylinder, which is the mating ring material, in the above-mentioned measurement of the limit PV.

[0064] [Table 1]

[0065] The results in Table 1 show that by using an ethylene-tetrafluoroethylene copolymer as the main component, a sliding member with excellent sliding properties, a large limiting PV and a low dynamic friction coefficient, can be obtained even when the electron beam is irradiated under conditions other than an oxygen-free atmosphere and when the processed body is not in a molten state.

[0066] In particular, the sliding members Nos. 6 to 9, which have an electron beam irradiation dose of 200 kGy or more and 350 kGy or less, have a large limit PV and are less likely to have a decrease in mechanical strength such as tensile strength. Therefore, it can be seen that by setting the electron beam irradiation dose within the above range, the sliding properties can be improved while ensuring the mechanical strength of the sliding members. [Explanation of symbols]

[0067] 1 Base material 2 ETFE film 3. PTFE film 4 SUS board 5 Welding jig 6 Screws P Peak BL Baseline S area (absorption amount)

Claims

1. A method for producing a sliding member containing an ethylene-tetrafluoroethylene copolymer as a main component, comprising the steps of: processing a material based on ethylene-tetrafluoroethylene copolymer; a step of irradiating the processed body obtained in the processing step with an electron beam; Equipped with The processing method in the above processing step is injection molding, The electron beam irradiation dose in the electron beam irradiation step is 350 kGy or less, The method for producing a sliding member, wherein the condition of the step of irradiating with electron beams is not a molten state.

2. 2. The method for producing a sliding member according to claim 1, wherein the electron beam is irradiated at a dose of 200 kGy or more in the step of irradiating with the electron beam.

3. 3. The method for producing a sliding member according to claim 1, wherein the step of irradiating the electron beam is not carried out in an oxygen-free atmosphere.

4. 4. The method for producing a sliding member according to claim 3, wherein the atmospheric temperature in the step of irradiating the electron beam is room temperature.

5. 5. The method for producing a slide member according to claim 3, wherein the atmosphere in the step of irradiating the electron beam is air.

Citation Information

Patent Citations

  • Production of modified fluororesin

    JP1999349711A

  • Seal material for reciprocation

    JP2003049950A

  • Seal ring

    JP2003049951A

  • Sliding component and method of manufacturing the same

    JP2011074938A

  • Method of manufacturing transparent fluororesin molded product and transparent fluororesin molded product

    JP2013043413A