Etching Composition
A selective etching composition for TaN in semiconductor devices using an oxidizing agent, hydroxycarboxylic acid, and anionic surfactant addresses the issue of substrate damage, achieving efficient and cost-effective TaN etching.
Patent Information
- Application Number
- JP2021572089
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-03
- Filing Date
- 2020-05-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-05-27
AI Technical Summary
Existing etching processes for tantalum nitride (TaN) in semiconductor devices are not selective enough, leading to damage of gate insulating layers and semiconductor substrates, and often require additional protective steps that increase costs.
An etching composition comprising an oxidizing agent, hydroxycarboxylic acid with at least two carboxy groups, an anionic surfactant, and water, with a pH of about 7 to 10, which selectively etches TaN without significantly etching other materials like copper and low-k dielectrics.
The composition achieves high TaN etch rates with low etching and corrosion rates for other semiconductor materials, minimizing substrate damage and reducing additional processing costs.
Smart Images

Figure 0007575407000001 
Figure 0007575407000002 
Figure 0007575407000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to etching compositions and processes using the etching compositions. In particular, the present disclosure relates to etching compositions capable of selectively etching tantalum nitride (TaN) in the presence of other exposed or underlying materials, such as metal conductors (e.g., copper), barrier materials, and insulating materials (e.g., low-k dielectric materials). [Background technology]
[0002] In the semiconductor industry, the size of electronic circuits and electronic components in microelectronic devices, silicon chips, liquid crystal displays, MEMS (Micro Electro Mechanical Systems), printed wiring boards, etc. is rapidly decreasing and the density is increasing. The thickness of the insulating layers between the circuit layers in which integrated circuits are stacked or overlapped is constantly decreasing, and the feature size is becoming smaller. As the feature size decreases, the patterns become smaller and the device performance parameters become more stringent and robust. As a result, various problems that were previously tolerable are no longer tolerable or become more of a problem as the feature size decreases.
[0003] In the manufacture of advanced integrated circuits, both high-k and low-k dielectric films, as well as a variety of barrier layer materials, are used to minimize density problems and optimize performance.
[0004] Tantalum nitride (TaN) is used in semiconductor devices, liquid crystal displays, MEMS (Micro Electro Mechanical Systems), printed wiring boards, etc., and as a ground layer and cap layer for precious metal wiring, aluminum (Al) wiring, and copper (Cu) wiring. In semiconductor devices, it is also used as a barrier metal, hard mask, or gate material.
[0005] In fabricating devices for these applications, it is often necessary to etch the TaN. In various applications and device environments for TaN, other layers are in contact with or otherwise exposed at the same time as the TaN is etched. High selectivity etching of the TaN in the presence of these other materials (e.g., metal conductors, dielectrics, and hard marks) is generally necessary for device yield and longevity. The etching process for TaN may be a plasma etching process. However, using a plasma etching process on the TaN layer may damage either or both the gate insulating layer and the semiconductor substrate. Furthermore, the etching process may remove portions of the semiconductor substrate by etching the gate insulating layer exposed by the gate electrode. This may have a negative impact on the electrical properties of the transistor. To avoid such etching damage, additional protective device fabrication steps may be used, but this involves significant costs.
[0006] Wet etching methods for TaN are known. Such methods may involve the use of etchants in combination with other reagents. However, they lack sufficient selectivity to silicon-based dielectrics and metals (e.g., Cu), and other exposed metals in the device may also be attacked or etched.
[0007] Therefore, there is a need for an etchant that has a high etch rate for TaN, but has low etch and corrosion rates for other semiconductor materials that are exposed or in contact with the Ta or TaN during the etching process. Summary of the Invention [Problem to be solved by the invention]
[0008] The present disclosure is based on the unexpected discovery that certain etching compositions are capable of selectively etching TaN relative to metal conductor layers, hard mask layers, and low-k dielectric layers present in semiconductor devices. More specifically, the present disclosure relates to compositions and processes for selectively etching TaN relative to copper, cobalt, and / or ruthenium. [Means for solving the problem]
[0009] In one aspect, the present disclosure features an etching composition that includes (1) an oxidizing agent, (2) a hydroxycarboxylic acid having at least two carboxy groups, (3) an anionic surfactant, and (4) water, the etching composition being abrasive-free and having a pH of about 7 to about 10.
[0010] In another aspect, the disclosure features an etching composition that includes (1) an oxidizing agent, (2) a hydroxycarboxylic acid having at least two carboxy groups, and (3) water, the etching composition being abrasive-free and having a pH of about 7 to about 10.
[0011] In another aspect, the disclosure features a method that includes contacting a semiconductor substrate including a TaN feature with an etching composition disclosed herein to remove at least a portion of the TaN feature.
[0012] In yet another aspect, the disclosure features an article formed by the above method, the article being a semiconductor device (eg, an integrated circuit). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] As defined herein, unless otherwise specified, all percentages expressed are to be understood as percentages by weight based on the total weight of the composition. Ambient temperature is defined as between about 16 and about 27° C. unless otherwise specified.
[0014] As defined herein, a "water-soluble" substance (e.g., a water-soluble alcohol, ketone, ester, ether, etc.) refers to a substance that has a solubility of 0.5% by weight or more (e.g., 1% by weight or more, or 5% by weight or more) in water at 25°C.
[0015] Tautomerization is defined herein as the formal migration of a hydrogen atom or proton with a single bond and the interchange of the adjacent double bond. Because of the low activation energy for tautomerization in the triazole ring system, references, descriptions and claims to triazole compounds include the tautomers of triazole compounds.
[0016] In general, the present disclosure features an etching composition (e.g., an etching composition for selectively removing TaN) that contains (e.g., contains, consists essentially of, or consists of) (1) an oxidizing agent, (2) a hydroxycarboxylic acid having at least two carboxy groups, (3) an anionic surfactant, and (4) water, the etching composition being abrasive-free and having a pH of about 7 to about 10.
[0017] The etching compositions of the present disclosure can include at least one (e.g., two, three, or four) oxidizing agents suitable for use in microelectronic applications. Examples of suitable oxidizing agents include oxidizing acids or salts thereof (e.g., nitric acid, permanganic acid, or potassium permanganate), peroxides (e.g., hydrogen peroxide, dialkyl peroxides, urea hydrogen peroxide), persulfonic acids (e.g., hexafluoropropanepersulfonic acid, methanepersulfonic acid, trifluoromethanepersulfonic acid, or p-toluenepersulfonic acid) and salts thereof, ozone, peroxycaboxylic acids (e.g., peracetic acid) and salts thereof, perphosphoric acid, and the like. Examples of oxidizing agents include, but are not limited to, ammonium persulfate and its salts, persulfuric acid and its salts (e.g., ammonium persulfate or tetramethylammonium persulfate), perchloric acid and its salts (e.g., ammonium perchlorate, sodium perchlorate, or tetramethylammonium perchlorate), and periodic acid and its salts (e.g., periodic acid, ammonium periodate, or tetramethylammonium periodate). These oxidizing agents can be used alone or in combination.
[0018] In some embodiments, the at least one oxidizing agent may be about 10 wt% or more (e.g., about 12 wt% or more, about 14 wt% or more, about 15 wt% or more, about 16 wt% or more, about 18 wt% or more, or about 20 wt% or more) to about 30 wt% or less (e.g., about 28 wt% or less, about 26 wt% or less, about 25 wt% or less, about 24 wt% or less, about 22 wt% or less, or about 20 wt% or less) of the total weight of the etching composition of the present disclosure. Without wishing to be bound by theory, it is believed that the oxidizing agent can facilitate and enhance the removal of TaN on the semiconductor substrate (e.g., by forming a TaOx-type material that is soluble in the etching composition).
[0019] In some embodiments, the etching compositions of the present disclosure may include at least one (e.g., two, three, or four) hydroxycarboxylic acid. In some embodiments, the hydroxycarboxylic acid may include at least two (e.g., three or four) carboxy groups (COOH) and / or at least one (e.g., two or three) hydroxy groups (OH). In some embodiments, the hydroxycarboxylic acid may be non-aromatic and / or acyclic (e.g., without a ring structure). For example, the hydroxycarboxylic acid may include citric acid or tartaric acid. In some embodiments, the hydroxycarboxylic acids described herein exclude hydroxycarboxylic acids that include only one carboxy group (e.g., lactic acid or glycolic acid).
[0020] In some embodiments, the at least one hydroxy carboxylic acid may be about 1 wt % or more (e.g., about 2 wt % or more, about 3 wt % or more, about 4 wt % or more, or about 5 wt % or more) to about 10 wt % or less (e.g., about 9 wt % or less, about 8 wt % or less, about 7 wt % or less, about 6 wt % or less, or about 5 wt % or less) of the total weight of the etching composition of the present disclosure. Without wishing to be bound by theory, it is believed that the hydroxy carboxylic acid can facilitate the removal of TaN on the semiconductor substrate.
[0021] In some embodiments, the etching compositions of the present disclosure may optionally include at least one (e.g., two, three, or four) anionic surfactant. In some embodiments, the anionic surfactant may be an alkyl ethoxylated carboxylic acid or a salt thereof. In some embodiments, the anionic surfactant may be a compound of formula (I) or a salt thereof: [ka] Here, R is C1 to C14 alkyl (e.g., C2, C4, C6, C8, C10, or C12 alkyl), and n is an integer ranging from 1 to 14 (e.g., 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, or 13). Specific examples include poly(oxy-1,2-ethanediyl)-α-(carboxymethyl)-ω-(hexyloxy) (e.g., a compound of formula (I) in which R is hexyl and n is 3), poly(oxy-1,2-ethanediyl)-α-(carboxymethyl)-ω-(octoxy) (e.g., a compound of formula (I) in which R is octyl and n is 8), or a salt thereof or a combination thereof. Commercially available examples of suitable anionic surfactants include AKYPO series products (e.g., AKYPO LF 1, AKYPO LF 2, AKYPO LF 4, AKYPO LF 6, AKYPO RLM 25, AKYPO RLM 45 CA, or AKYPO RLM 100) available from Kao Corporation, SA (Barcelona, Spain), or EMPICOL series products (e.g., EMPICOL CBJ, or EMPICOL CED5) available from Huntsman Performance Products, Inc. (The Woodlands, Texas, USA). In some embodiments, the anionic surfactant may be polyacrylic acid. Without wishing to be bound by theory, it is believed that the carboxylic acid group and polyacrylic acid in the compound of formula (I) can be deprotonated under basic conditions to form an anionic surfactant.
[0022] In some embodiments, the at least one anionic surfactant may be about 0.001 wt% or more (e.g., about 0.005 wt% or more, about 0.008 wt% or more, about 0.01 wt% or more, about 0.02 wt% or more, about 0.05 wt% or more, or about 0.1 wt% or more) to about 5 wt% or less (e.g., about 4 wt% or less, about 3 wt% or less, about 2 wt% or less, about 1 wt% or less, about 0.5 wt% or less, about 0.1 wt% or less, or about 0.05 wt% or less) of the total weight of the etching composition of the present disclosure. Without wishing to be bound by theory, it is believed that the anionic surfactant can reduce or minimize the corrosion or removal of copper on a semiconductor substrate exposed to the etching composition during the etching process.
[0023] In some embodiments, the etching compositions of the present disclosure may include water as a solvent (e.g., as the only solvent). In some embodiments, the water may be deionized and ultra-pure, free of organic contaminants, and have a minimum resistivity of about 4 to about 17 megaohms, or about 17 megaohms or greater. In some embodiments, the amount of water is about 50 wt% or greater (e.g., about 55 wt% or greater, about 60 wt% or greater, about 65 wt% or greater, about 70 wt% or greater, about 75 wt% or greater, about 80 wt% or greater, or about 85 wt% or greater) to about 90 wt% or less (e.g., about 85 wt% or less, about 80 wt% or less, about 75 wt% or less, about 70 wt% or less, about 65 wt% or less, about 60 wt% or less, or about 55 wt% or less) of the total weight of the etching composition. While not wishing to be bound by theory, it is believed that if the amount of water is greater than 90 wt% of the composition, it will adversely affect the TaN etch rate and reduce the removal of TaN during the etching process. On the other hand, while not wishing to be bound by theory, it is believed that the etching compositions of the present disclosure should contain a certain amount of water (e.g., about 50 wt% or more) to keep other components in solution and avoid degrading the etching performance.
[0024] In some embodiments, the etching compositions of the present disclosure may include at least one (e.g., two, three, or four) organic solvents. In other embodiments, the etching compositions of the present disclosure do not include any organic solvents.
[0025] In some embodiments, the etching composition of the present disclosure may optionally further include at least one (e.g., two, three, or four) metal corrosion inhibitor. Examples of suitable corrosion inhibitors include azole compounds (e.g., substituted or unsubstituted azole compounds) or salts thereof. Examples of azole compounds include triazole compounds, imidazole compounds, thiadiazole compounds, and tetrazole compounds. Examples of triazole compounds include triazole, benzotriazole, substituted triazole, and substituted benzotriazole. Examples of triazole compounds include 1,2,4-triazole, 1,2,3-triazole, or triazoles substituted with substituents such as C1-C8 alkyl groups (e.g., 5-methyltriazole), amino groups, thiol groups, mercapto groups, imino groups, carboxy groups, and nitro groups. Specific examples of substituted triazole compounds include, but are not limited to, tolyltriazole, 5-methyl-1,2,4-triazole, 3-amino-5-mercapto-1,2,4-triazole, 1-amino-1,2,4-triazole, 4-amino-1,2,4-triazole, 1-amino-1,2,3-triazole, 1-amino-5-methyl-1,2,3-triazole, 3-amino-1,2,4-triazole, 3-amino-1,2,4-triazole-5-thiol, 3-mercapto-1,2,4-triazole, and 3-isopropyl-1,2,4-triazole.
[0026] In some embodiments, the at least one metal corrosion inhibitor may include a benzotriazole optionally substituted with at least one substituent selected from the group consisting of an alkyl group, an aryl group, a halogen group, an amino group, a nitro group, an alkoxy group, and a hydroxy group.Examples include benzotriazole (or 1H-benzotriazole), 5-aminobenzotriazole, hydroxybenzotriazole (e.g., 1-hydroxybenzotriazole), 5-phenylthiol-benzotriazole, halo-benzotriazoles (halo = F, Cl, Br or I) (e.g., 5-chlorobenzotriazole, 4-chlorobenzotriazole, 5-bromobenzotriazole, 4-bromobenzotriazole, 5-fluorobenzotriazole, and 4-fluorobenzotriazole), naphthotriazole, 5-phenyl-benzotriazole, 5-nitrobenzotriazole, 4-nitrobenzotriazole, 2-(5-amino-pentyl)-benzotriazole, 1-amino-benzotriazole, 5-methyl-1H-benzotriazole, 1H-benzotriazole-1-methanol, benzotriazole-5-carboxylic acid, 4-methylbenzotriazole, 4-ethylbenzotriazole, 5-ethylbenzotriazole, 4-propylbenzotriazole, benzotriazole, 5-propylbenzotriazole, 4-isopropylbenzotriazole, 5-isopropylbenzotriazole, 4-n-butylbenzotriazole, 5-n-butylbenzotriazole, 4-isobutylbenzotriazole, 5-isobutylbenzotriazole, 4-pentylbenzotriazole, 5-pentylbenzotriazole, 4-hexylbenzotriazole, 5-hexylbenzotriazole, 5,6-dimethyl-1H-benzotriazole, 5-methoxybenzotriazole, 5-hydroxybenzotriazole, dihydroxypropylbenzotriazole, 1-[N,N-bis(2-ethylhexyl)aminomethyl]-benzotriazole, 5-t-butylbenzotriazole, 5-(1',1'-dimethylpropyl)benzotriazole, 5-(1',1',3'-trimethylbutyl)benzotriazole, 5-n-octylbenzotriazole, and 5-(1',1',3',3'-tetramethylbutyl)benzotriazole.
[0027] Examples of imidazole compounds include, but are not limited to, 2-alkyl-4-methylimidazole, 2-phenyl-4-alkylimidazole, 2-methyl-4(5)-nitroimidazole, 5-methyl-4-nitroimidazole, 4-imidazolemethanol hydrochloride, and 2-mercapto-1-methylimidazole.
[0028] An example of a thiadiazole compound is 2-amino-1,3,4-thiadiazole.
[0029] Examples of tetrazole compounds include 1H-tetrazole, 5-methyl-1H-tetrazole, 5-phenyl-1H-tetrazole, 5-amino-1H-tetrazole, 1-phenyl-5-mercapto-1H-tetrazole, 5,5'-bis-1H-tetrazole, 1-methyl-5-ethyltetrazole, 1-methyl-5-mercaptotetrazole, and 1-carboxymethyl-5-mercaptotetrazole, and the like.
[0030] In some embodiments, the at least one metal corrosion inhibitor may be about 0.01 wt% or more (e.g., about 0.02 wt% or more, about 0.05 wt% or more, about 0.1 wt% or more, about 0.2 wt% or more, about 0.3 wt% or more, about 0.4 wt% or more, or about 0.5 wt% or more) to about 10 wt% or less (e.g., about 8 wt% or less, about 5 wt% or less, about 3 wt% or less, about 2.5 wt% or less, about 2 wt% or less, about 1.5 wt% or less, about 1 wt% or less, about 0.8 wt% or less, or about 0.5 wt% or less) of the total weight of the etching composition of the present disclosure. Without wishing to be bound by theory, it is believed that the metal corrosion inhibitor can inhibit or minimize the corrosion or removal of copper on a semiconductor substrate exposed to the etching composition during the etching process.
[0031] In some embodiments, the etching compositions of the present disclosure may optionally further comprise at least one (e.g., two, three, or four) chelating agent. In some examples, the chelating agent may include a phosphonic acid or a salt thereof. Specific examples of such chelating agents include hexamethylenediaminetetra(methylenephosphonic acid) or its hexapotassium salt, 1-hydroxyethane-1,1-diphosphonic acid, aminotris(methylenephosphonic acid), ethylenediaminetetra(methylenephosphonic acid), tetramethylenediaminetetra(methylenephosphonic acid), diethylenetriaminepenta(methylenephosphonic acid), or a salt thereof.
[0032] In some embodiments, the chelating agent may include a polyaminopolycarboxylic acid or a salt thereof. The polyaminopolycarboxylic acid may include at least two (e.g., three or four) amino groups and at least two (e.g., three or four) carboxy groups. Specific examples of such chelating agents include butylenediaminetetraacetic acid, diethylenetriaminepentaacetic acid (DTPA), ethylenediaminetetrapropionic acid, triethylenetetraminehexaacetic acid, 1,3-diamino-2-hydroxypropane-N,N,N',N'-tetraacetic acid, propylenediaminetetraacetic acid, ethylenediaminetetraacetic acid, trans-1,2-diaminocyclohexanetetraacetic acid, ethylenediaminediacetic acid, ethylenediaminedipropionic acid, 1,6-hexamethylenediamine-N,N,N',N'-tetraacetic acid, N,N-bis(2-hydroxybenzyl)ethylenediamine-N,N-diacetic acid, diaminopropanetetraacetic acid, 1,4,7,10-tetraazacyclododecane-tetraacetic acid, diaminopropanoltetraacetic acid, and (hydroxyethyl)ethylenediaminetriacetic acid.
[0033] In some embodiments, the at least one chelating agent may be present in an amount of about 0.01 wt% or more (e.g., about 0.02 wt% or more, about 0.05 wt% or more, about 0.1 wt% or more, about 0.2 wt% or more, about 0.3 wt% or more, about 0.4 wt% or more, or about 0.5 wt% or more) to about 10 wt% or less (e.g., about 8 wt% or less, about 5 wt% or less, about 3 wt% or less, about 2.5 wt% or less, about 2 wt% or less, about 1.8 wt% or less, about 1.5 wt% or less, about 1 wt% or less, about 0.8 wt% or less, or about 0.5 wt% or less) of the total weight of the etching composition of the present disclosure. Without wishing to be bound by theory, it is believed that the chelating agent can form a complex with a metal (e.g., copper) on the semiconductor substrate and inhibit or minimize the removal of such metal exposed to the etching composition during the etching process. It is also believed that chelating agents may assist in stabilizing oxidizing agents (eg, peroxides).
[0034] In some embodiments, the etching compositions of the present disclosure may optionally further comprise at least one (e.g., two, three, or four) pH adjusters (e.g., acids or bases). In some embodiments, the pH adjuster may be a base that contains a metal ion (e.g., an alkali ion). Examples of such metal-containing bases include alkali hydroxides such as NaOH or KOH. In some embodiments, the pH adjuster may be a base that does not contain a metal ion, such as ammonium hydroxide (i.e., NH4OH). In some embodiments, when the etching compositions of the present disclosure include at least two basic pH adjusters, the primary pH adjuster may be an alkali hydroxide or ammonium hydroxide as described above, and the secondary basic pH adjuster may be a quaternary ammonium hydroxide (e.g., a tetraalkylammonium hydroxide such as tetramethylammonium hydroxide (TMAH) or tetrabutylammonium hydroxide (TBAH)) or an amidine (e.g., 1,8-diazabicyclo[5.4.0]-7-undecene (DBU) or 1,5-diazabicyclo[4.3.0]-5-nonene (DBN)).
[0035] In some embodiments, the pH adjuster may be an organic acid, such as a sulfonic acid (e.g., methanesulfonic acid, trifluoromethanesulfonic acid, and p-toluenesulfonic acid) or a carboxylic acid (e.g., a hydroxycarboxylic acid such as citric acid). In some embodiments, the pH adjuster is not an inorganic acid (e.g., a hydrogen halide).
[0036] Generally, the amount of pH adjuster in the etching composition of the present disclosure can be sufficient to adjust the pH of the etching composition to a desired value. In some embodiments, the pH adjuster can be about 1 wt% or more (e.g., about 1.5 wt% or more, about 2 wt% or more, about 2.5 wt% or more, about 3 wt% or more, about 3.5 wt% or more, about 4 wt% or more, about 4.5 wt% or more, or about 5 wt% or more) to about 10 wt% or less (e.g., about 9 wt% or less, about 8 wt% or less, about 7.5 wt% or less, about 7 wt% or less, about 6 wt% or less, or about 5 wt% or less) of the total weight of the etching composition.
[0037] In some embodiments, the etching compositions of the present disclosure may optionally further comprise at least one (e.g., two, three, or four) quaternary ammonium salt, such as a tetraalkylammonium salt. Examples of suitable quaternary ammonium salts include (lauryldimethylammonio)acetate, dodecyltrimethylammonium chloride, or benzyldodecyldimethylammonium bromide.
[0038] In general, the quaternary ammonium salt in the etching composition of the present disclosure may be about 0.01 wt% or more (e.g., about 0.02 wt% or more, about 0.04 wt% or more, about 0.05 wt% or more, about 0.06 wt% or more, about 0.08 wt% or more, about 0.1 wt% or more, about 0.2 wt% or more, about 0.3 wt% or more, about 0.4 wt% or more, or about 0.5 wt% or more) to about 1 wt% or less (e.g., about 0.9 wt% or less, about 0.8 wt% or less, about 0.75 wt% or less, about 0.7 wt% or less, about 0.6 wt% or less, or about 0.5 wt% or less) of the total weight of the etching composition. Without wishing to be bound by theory, it is believed that the quaternary ammonium salt can inhibit or minimize the removal of metal exposed to the etching composition during the etching process.
[0039] In some embodiments, the pH of the etching composition of the present disclosure may be about 7 or more (e.g., about 7.2 or more, about 7.4 or more, about 7.5 or more, about 7.6 or more, about 7.8 or more, about 8 or more, about 8.2 or more, about 8.4 or more, about 8.5 or more, or about 9 or more) and / or about 10 or less (e.g., about 9.8 or less, about 9.6 or less, about 9.5 or less, about 9.4 or less, about 9.2 or less, about 9 or less, about 8.5 or less, or about 8 or less). Without wishing to be bound by theory, it is believed that an etching composition having a pH lower than 7 does not have a sufficient TaN etch rate. Furthermore, it is believed that an etching composition having a pH higher than 10 may result in excessive Cu etching, prevent certain components in the composition from functioning, and / or decompose certain components in the composition due to its strong basicity.
[0040] Additionally, in some embodiments, the etching compositions of the present disclosure may contain optional additives such as additional corrosion inhibitors, surfactants, additional organic solvents, biocides, and antifoaming agents. Examples of suitable antifoaming agents include polysiloxane antifoaming agents (e.g., polydimethylsiloxane), polyethylene glycol methyl ether polymers, ethylene oxide / propylene oxide copolymers, and glycidyl ether capped acetylenic diol ethoxylates (e.g., those described in U.S. Pat. No. 6,717,019, which is incorporated herein by reference). Examples of suitable surfactants may be cationic, anionic, nonionic, or amphiphilic.
[0041] In general, the etching compositions of the present disclosure may have a relatively high TaN / metal (e.g., copper) etch selectivity (i.e., a high ratio of the TaN etch rate to the metal etch rate). In some embodiments, the TaN / metal etch selectivity of the etching composition may be about 2 or more (e.g., about 3 or more, about 4 or more, about 5 or more, about 6 or more, about 7 or more, about 8 or more, about 9 or more, about 10 or more, about 15 or more, about 20 or more, about 30 or more, about 40 or more, or about 50 or more) and / or about 500 or less (e.g., about 100 or less).
[0042] In some embodiments, the etching compositions of the present disclosure may be specifically free of one or more (any combination of more than one) of the additive components listed above. Such ingredients are selected from the group consisting of organic solvents, pH adjusters, polymers (e.g., cationic or anionic polymers), oxygen scavengers, quaternary ammonium salts or quaternary ammonium hydroxides, amines, alkaline bases (such as CsOH and RbOH), surfactants other than antifoaming agents, antifoaming agents, fluorine-containing compounds, abrasives (e.g., cationic or anionic abrasives), silicates, hydroxycarboxylic acids (e.g., those containing more than two hydroxy groups), carboxylic acids and polycarboxylic acids (e.g., those with or without amino groups), silanes (e.g., alkoxysilanes), cyclic compounds (e.g., azoles, such as diazoles, triazoles, or tetrazoles), triazines, and cyclic compounds containing at least two rings (e.g., substituted or unsubstituted naphthalenes, or substituted or unsubstituted biphenyl ethers), buffers, non-azole corrosion inhibitors, and salts (e.g., halogen salts or metal salts, such as metal halides).
[0043] The etching compositions of the present disclosure can be prepared by simply mixing the components together or by blending two compositions in a kit. The first composition in the kit can be an aqueous solution of an oxidizing agent (e.g., H2O2). The second composition in the kit can contain the remaining components of the etching compositions of the present disclosure in concentrated form in a predetermined ratio such that blending the two compositions provides the desired etching composition of the present disclosure.
[0044] In some embodiments, the present disclosure features a method of etching a semiconductor substrate including at least one TaN feature (e.g., a TaN film or layer). In some embodiments, the TaN feature may be a liner or barrier (e.g., about 1 nm thick) around a via or trench filled with Cu, Co, and / or Ru, or a film coating the sidewall of a via or trench filled with Cu, Co, and / or Ru. Examples of features having materials including TaN arranged in the fill metal / liner / barrier sequence include Cu / TaN / TaN, Cu / Ta / TaN, Cu / Co / TaN, and Co / Ru / TaN. Examples of features having materials including TaN arranged in the fill metal / barrier sequence include Co / TaN.
[0045] In some embodiments, the method may include contacting the semiconductor substrate including at least one TaN feature with an etching composition of the present disclosure to remove at least a portion of the TaN feature. The method may further include rinsing the semiconductor substrate with a rinsing solution after the contacting step and / or drying the semiconductor substrate after the rinsing step. In some embodiments, one advantage of the methods described herein is that they do not substantially remove metal (e.g., Cu) on the semiconductor substrate that is exposed to the etching composition during the etching process.
[0046] In some embodiments, the etching method includes the steps of: (A) providing a semiconductor substrate including a TaN feature; (B) contacting the semiconductor substrate with an etching composition described herein; (C) rinsing the semiconductor substrate with one or more suitable rinsing solvents; and (D) optionally drying the semiconductor substrate (e.g., by any suitable means that removes the rinsing solvent but does not destroy the integrity of the semiconductor substrate).
[0047] The semiconductor substrates (e.g., wafers) described herein are typically composed of silicon, silicon germanium, III-V compounds (e.g., GaAs), or any combination thereof. The semiconductor substrate may additionally include exposed integrated circuit structures (e.g., metal lines and dielectric materials), such as interconnect features. Metals and metal alloys used in the interconnect features include, but are not limited to, aluminum, aluminum alloyed with copper, copper, titanium, tantalum, cobalt, silicon, titanium nitride, tantalum nitride, and tungsten. The semiconductor substrate may also include layers of interlayer dielectric (ILD), polysilicon, silicon oxide, silicon nitride, silicon carbide, titanium oxide, and carbon-doped silicon oxide.
[0048] The semiconductor substrate may be contacted with the etching composition by any suitable method, such as placing the etching composition in a tank and dipping and / or submerging the semiconductor substrate in the etching composition, spraying the etching composition onto the semiconductor substrate, flowing the etching composition onto the semiconductor substrate, or any combination thereof.
[0049] Etching compositions of the present disclosure can be effectively used at temperatures up to about 85° C. (e.g., about 20° C. to about 80° C., about 55° C. to about 65° C., or about 60° C. to about 65° C.). Within this range, the etch rate of TaN increases with temperature, so that processes at higher temperatures can be completed in shorter times. Conversely, lower etch temperatures typically require longer etch times.
[0050] Etching times can vary widely depending on the particular etching method, thickness, and temperature used. When etching is performed in an immersion batch type process, suitable time ranges are, for example, about 10 minutes or less (e.g., about 1 minute to about 7 minutes, about 1 minute to about 5 minutes, or about 2 minutes to about 4 minutes). Etching times for a single wafer process may range from about 30 seconds to about 5 minutes (e.g., about 30 seconds to about 4 minutes, about 1 minute to about 3 minutes, or about 1 minute to about 2 minutes).
[0051] Mechanical agitation means can be used to further enhance the etching ability of the etching composition of the present disclosure. Examples of suitable agitation means include circulating the etching composition over the substrate, flowing or spraying the etching composition over the substrate, and ultrasonic or megasonic agitation during the etching process. The orientation of the semiconductor substrate with respect to the ground can be at any angle. A horizontal or vertical orientation is preferred.
[0052] Following etching, the semiconductor substrate may be rinsed with a suitable rinsing solvent for about 5 seconds to about 5 minutes with or without agitation. Multiple rinsing steps using different rinsing solvents may be used. Examples of suitable rinsing solvents include, but are not limited to, deionized (DI) water, methanol, ethanol, isopropyl alcohol, N-methylpyrrolidinone, γ-butyrolactone, dimethylsulfoxide, ethyl lactate, and propylene glycol monomethyl ether acetate. Alternatively or additionally, an aqueous rinse agent with a pH>8 may be used, such as a dilute aqueous ammonium hydroxide solution. Examples of rinsing solvents include, but are not limited to, a dilute aqueous ammonium hydroxide solution, DI water, methanol, ethanol, and isopropyl alcohol. The rinsing solvent may be applied using a similar means to those used to apply the etching compositions described herein. The etching composition may be removed from the semiconductor substrate before the rinsing step begins, or may still be in contact with the semiconductor substrate at the beginning of the rinsing step. In some embodiments, the temperature used in the rinsing step is between 16°C and 27°C.
[0053] Optionally, the semiconductor substrate is dried after the rinsing step. Any suitable drying means known in the art can be used. Examples of suitable drying means include spin drying, flowing a drying gas across the semiconductor substrate, heating the semiconductor substrate with a heating means such as a hot plate or an infrared lamp, Marangoni drying, Rotagoni drying, isopropyl alcohol (IPA) drying, or any combination thereof. The drying time depends on the specific method used, but is typically on the order of 30 seconds to several minutes.
[0054] In some embodiments, the etching methods described herein further include forming a semiconductor device (eg, an integrated circuit device such as a semiconductor chip) from the semiconductor substrate obtained by the above-described method. EXAMPLES
[0055] The present disclosure will now be described in more detail with reference to the following examples, which are for illustrative purposes and should not be construed as limiting the scope of the present disclosure.
[0056] All percentages listed are by weight (wt%) unless otherwise noted. Controlled stirring during testing was performed with a 1 inch stir bar at 300 rpm unless otherwise noted.
[0057] <Basic Step 1> [Blending of ingredients] The etching composition samples were prepared by adding the remaining ingredients of the formulation to the calculated amount of solvent with stirring. After a homogeneous solution was achieved, optional additives, if used, were added.
[0058] <Basic Step 2> Materials and Methods The blanket test coupons were evaluated for etching and materials compatibility in the test solutions prepared according to General Procedure 1, following the procedures described in General Procedure 3.
[0059] Blanket film etch rate measurements on films were performed using commercially available unpatterned 300 mm diameter wafers diced into 0.5 inch by 1.0 inch evaluation test coupons. The blanket film materials tested were: (1) a tantalum nitride (TaN) film approximately 500 Å thick deposited on a silicon substrate, (2) a copper (Cu) film approximately 1500 Å thick deposited on a silicon substrate, (3) a tantalum oxide (TaOx) film approximately 200 or 350 Å thick deposited on a silicon substrate, (4) a ruthenium (Ru) film approximately 350 Å thick deposited on a silicon substrate, and (5) a cobalt (Co) film approximately 2000 Å thick deposited on a silicon substrate.
[0060] Blanket film test coupons were measured for thickness before and after processing to determine blanket film etch rates. A CDE-RESMAP 4-point probe was used to measure the thickness of TaN, Cu, Co, and Ru films before and after processing. An ESM-300 ellipsometer (JA Woolam, Lincoln, Nebraska) was used to measure the thickness of TaOx films before and after processing. Further film thickness measurements were collected by X-ray reflectometry using a Rigaku SmartLab X-ray diffractometer.
[0061] The patterned test coupons were evaluated for etching and materials compatibility in the test solutions prepared according to General Procedure 1, following the procedures described in General Procedure 3.
[0062] Patterned test coupons Cu / Ta(3 nm) / TaN(3 nm) / ILD were evaluated for material compatibility and / or etch response. The processed test coupons were then evaluated by scanning electron microscopy (SEM). SEM images from the processed coupons were compared to a set of previously captured pre-processing SEM images to evaluate the material compatibility and etch response of each test formulation on the patterned test device features.
[0063] <Basic Step 3> (Etching evaluation in beaker test) All blanket film etching tests were performed in a 250 mL glass beaker containing 100 g of sample solution with continuous stirring at 300 rpm between 20° C. and 85° C. with a Parafilm® cover at all times to minimize evaporation losses. All blanket test coupons with blanket metal or dielectric film exposed to the test solution on one side were diced with a diamond scribe to test coupon size for beaker scale testing, approximately 0.5 inch by 1 inch rectangular. Each individual test coupon was held in place using one 4 inch long plastic locking tweezer clip. The test coupons held by the locking tweezer clip on one end were suspended in the 250 mL glass beaker and immersed in 100 g of test solution with continuous stirring at 300 rpm at process temperature. Immediately after placing each test coupon in the stirring solution, the top of the 250 mL glass beaker was covered and resealed with Parafilm®. The test coupons were held statically in the stirring solution until the treatment time (described in General Procedure 3A) had elapsed. After the treatment time in the test solution had elapsed, the sample coupons were quickly removed from the 250 mL glass beaker and rinsed according to General Procedure 3A. After the final DI rinse step, all test coupons were subjected to a filtered nitrogen gas blowing step using a hand held nitrogen gas blower to force out any DI water residuals and produce a final dry sample for test measurements.
[0064] <Basic Procedure 3A (Blanket Test Coupon)> Immediately following the treatment period according to General Procedure 3 (i.e., 5 or 6 minutes for TaN, 10 or 20 minutes for Cu, Ru, Co, and TaOx), the coupons were immersed in a volume of 1000 mL of ultra-high purity deionized (DI) water at an overflow rate of approximately 1 liter / min at 20° C. for 30 seconds and then 30 seconds with gentle agitation. This treatment was completed according to General Procedure 3.
[0065] <Basic Procedure 3B (Patterned Test Coupon)> Immediately after a treatment period of 2.5 to 3 minutes (depending on the experiment), the patterned test coupons were post-treated by immersion in isopropyl alcohol (IPA) or ultra-high purity deionized water with gentle agitation for 20 seconds at 20 °C. This treatment was completed according to General Procedure 3.
[0066] <Example 1> Formulation Examples 1-47 (FE-1 to FE-47) were prepared according to General Procedure 1 and evaluated using blanket test coupons according to General Procedures 2 and 3, except that the etching temperatures were 56-67° C. A summary of the formulations is shown in Table 1, and a summary of the test results is shown in Table 2.
[0067] Table 1 [Table 1-1] [Table 1-2]
[0068] [Table 2]
[0069] As shown in Table 2, formulations FE-1 to FE-47 exhibited relatively high TaN etch rates and / or TaN / Cu etch selectivities under the test conditions. Also, most of these formulations were clear (i.e., free of precipitate) before H2O2 was added, were clear after H2O2 was added, and were still clear at the process temperature. Furthermore, most of these formulations produced no or low foaming when used to etch TaN and Cu films.
[0070] <Example 2> Formulation Examples 48-50 (FE-48 to FE-50) were prepared according to General Procedure 1 and evaluated using blanket test coupons according to General Procedures 2 and 3, except that the etching temperature was 65° C. A summary of the formulations and test results is shown in Table 3.
[0071] [Table 3]
[0072] As shown in Table 3, FE-48 (containing KOH as a pH adjuster) exhibited a relatively high TaN etch rate and a relatively low Cu etch rate (i.e., a relatively high TaN / Cu etch selectivity) under the test conditions, while FE-49 and FE-50 (containing the metal-free bases TMAH and DBU as pH adjusters) both exhibited relatively low TaN etch rates under the test conditions.
[0073] <Example 3> Formulation Examples 51-55 (FE-51-FE-55) were prepared according to General Procedure 1 and evaluated using blanket test coupons according to General Procedures 2 and 3, except that the etching temperature was 60° C. A summary of the formulations and test results is shown in Table 4.
[0074] [Table 4]
[0075] As shown in Table 4, FE-51, FE-54, and FE-55 (containing KOH, NAOH, and NH4OH as pH adjusters) exhibited relatively high TaN etch rates and relatively low Cu etch rates (i.e., relatively high TaN / Cu etch selectivities) under the test conditions, although Cu was oxidized by FE-55. In addition, the other two formulations tested, FE-52 and FE-53, exhibited relatively high TaN / Cu etch selectivities under the test conditions.
[0076] <Example 4> Formulation Examples 56-58 (FE-56-FE-58) were prepared according to General Procedure 1 and evaluated using blanket test coupons according to General Procedures 2 and 3, except that the etching temperature was 65° C. A summary of the formulations and test results is shown in Table 5.
[0077] [Table 5]
[0078] As shown in Table 5, FE-56 (which had a relatively low pH) exhibited a relatively low TaN etch rate and a relatively high Cu etch rate (i.e., a relatively low TaN / Cu etch selectivity) under the conditions tested. In contrast, the other two formulations tested, FE-57 and FE-58, exhibited a relatively high TaN etch rate and a relatively low Cu etch rate (i.e., a relatively high TaN / Cu etch selectivity) under the conditions tested.
[0079] <Example 5> Formulation Examples 59-63 (FE-59 to FE-63) were prepared according to General Procedure 1 and evaluated using blanket test coupons according to General Procedures 2 and 3, except that the etching temperature was 65° C. A summary of the formulations and test results is shown in Table 6.
[0080] [Table 6]
[0081] As shown in Table 6, FE-59 and FE-61 (containing α-hydroxycarboxylic acids with two or more carboxy groups) exhibited relatively high TaN etch rates and relatively low Cu etch rates (i.e., relatively high TaN / Cu etch selectivity) under the test conditions.
[0082] <Example 6> Formulation Examples 64-67 (FE-64 to FE-67) were prepared according to General Procedure 1 and evaluated using blanket test coupons according to General Procedures 2 and 3, except that the etching temperature was 65° C. A summary of the formulations and test results is shown in Table 7.
[0083] [Table 7]
[0084] As shown in Table 7, FE-65 to FE-67 (containing citric acid) exhibited relatively high TaN etch rates and relatively low Cu etch rates (i.e., relatively high TaN / Cu etch selectivity) under the test conditions, while FE-64 (not containing citric acid) exhibited relatively low TaN etch rates and relatively low TaN / Cu etch selectivity under the test conditions.
[0085] <Example 7> Formulation Examples 68-70 (FE-68 through FE-70) were prepared according to General Procedure 1 and evaluated using blanket test coupons according to General Procedures 2 and 3, except that the etching temperature was 65° C. A summary of the formulations and test results is shown in Table 8.
[0086] [Table 8]
[0087] As shown in Table 8, FE-69 and FE-70 (containing anionic surfactant) exhibited higher TaN etch rates and lower Cu etch rates (i.e., higher TaN / Cu etch selectivity) compared to FE-68 (not containing anionic surfactant).
[0088] <Example 8> Formulation Examples 71-73 (FE-71-FE-73) were prepared according to General Procedure 1 and evaluated using blanket test coupons according to General Procedures 2 and 3, except that the etching temperature was 65° C. A summary of the formulations and test results is shown in Table 9.
[0089] [Table 9]
[0090] As shown in Table 9, FE-71 to FE-73 (all containing anionic surfactants) exhibited relatively high TaN etch rates and relatively low Cu etch rates (ie, relatively high TaN / Cu etch selectivity).
[0091] <Example 9> Formulation Examples 74-77 (FE-74 to FE-77) were prepared according to General Procedure 1 and evaluated according to General Procedures 2 and 3, except that the etching temperature was 65° C. A summary of the formulations and test results is shown in Table 10.
[0092] [Table 10]
[0093] As shown in Table 10, FE-74 to FE-77 (all containing polyacrylic acid as an anionic surfactant) exhibited relatively high TaN etch rates and relatively low Cu etch rates (i.e., relatively high TaN / Cu etch selectivity).
[0094] <Example 10> Formulation Examples 78-91 (FE-78-FE-91) were prepared according to General Procedure 1 and evaluated using blanket test coupons according to General Procedures 2 and 3, except that the etching temperature was 65°C. FE-78-FE-91 contained 0.7% DTPA, 5.5% citric acid, 0.3% AKYPO LF4, KOH, 20% H2O2, 0-2 azole additives, and the balance was water. A summary of the azole additives and test results is shown in Table 11.
[0095] [Table 11]
[0096] As shown in Table 11, FE-79 to FE-91 (containing at least one triazole) exhibited higher TaN etch rates and lower Cu etch rates (i.e., higher TaN / Cu etch selectivities) than FE-78 (containing no triazole) under the conditions tested. Furthermore, FE-83 to FE-91 (containing two triazoles) generally exhibited higher TaN / Cu etch selectivities than FE-79 to FE-82 (containing one triazole) under the conditions tested.
[0097] <Example 11> Formulation Examples 92-95 (FE-92 through FE-95) were prepared according to General Procedure 1 and evaluated using blanket test coupons according to General Procedures 2 and 3, except that the etching temperature was 65° C. A summary of the formulations and test results is shown in Table 12.
[0098] [Table 12]
[0099] As shown in Table 12, FE-93 through FE-95 (all containing tetraalkylammonium salts) exhibited higher TaN / Cu etch selectivity than FE-92 (which did not contain tetraalkylammonium salts) under the test conditions.
[0100] <Example 12> Formulation Examples 96-98 (FE-96 to FE-98) were prepared according to General Procedure 1 and evaluated using blanket and patterned test coupons according to General Procedures 2 and 3, except that the etching temperature was 65° C. A summary of the formulations and test results is shown in Table 13.
[0101] [Table 13]
[0102] Although the invention has been described in detail with reference to specific embodiments, it will be understood that modifications and variations are encompassed within the spirit and scope of what is described and claimed.
[0103] <Reference to Related Applications> This application claims priority to U.S. Provisional Application No. 62 / 856,213, filed June 3, 2019, the contents of which are incorporated by reference in their entirety. The aspects of the present disclosure also include the following aspects. <1> An etching composition comprising: (1) an oxidizing agent; (2) a hydroxycarboxylic acid having at least two carboxy groups; (3) an anionic surfactant; and (4) water; the composition does not contain an abrasive; and has a pH of about 7 to about 10. <2> The pH is about 7 to about 9.5. <1> The composition described in <3> The oxidizing agent includes peroxide, persulfonic acid or a salt thereof, ozone, peroxycarboxylic acid or a salt thereof, perphosphoric acid or a salt thereof, persulfuric acid or a salt thereof, perchloric acid or a salt thereof, or periodic acid or a salt thereof; <1> The composition described in <4> The oxidizing agent comprises hydrogen peroxide or persulfuric acid; <1> The composition described in <5> The amount of the oxidizing agent is about 10% to about 30% by weight of the composition. <1> The composition described in <6> The hydroxycarboxylic acid is citric acid or tartaric acid. <1> The composition described in <7> the amount of the hydroxycarboxylic acid is about 1% to about 10% by weight of the composition; <1> The composition described in <8> The anionic surfactant is an alkyl ethoxylated carboxylic acid or a salt thereof; <1> The composition described in <9> The anionic surfactant is a compound represented by the following formula (I) or a salt thereof: <1> The composition according to the present invention comprises: [ka] In formula (I), R is C 1 ~C 14 and n is an integer ranging from 1 to 14. <10> The amount of the surfactant is about 0.001% to about 5% by weight of the composition. <1> The composition described in <11> The amount of water is about 50% to about 90% by weight of the composition. <1> The composition described in <12> Further comprising a metal corrosion inhibitor, <1> The composition described in <13> The metal corrosion inhibitor comprises an azole or a salt thereof; <12> The composition described in <14> the metal corrosion inhibitor comprises 1,2,3-triazole, 1,2,4-triazole, 4-amino-1,2,4-triazole, 3-amino-1,2,4-triazole-5-thiol, 1H-benzotriazole, 5-methyl-1H-benzotriazole, 1H-benzotriazole-1-methanol, 5,6-dimethyl-1H-benzotriazole, 2-amino-1,3,4-thiadiazole, 1H-tetrazole, 5-phenyl-1H-tetrazole, 5-amino-1H-tetrazole, or a combination thereof; <12> The composition described in <15> The amount of the metal corrosion inhibitor is about 0.01% to about 10% by weight of the composition. <12> The composition described in <16> Further comprising a chelating agent, <1> The composition described in <17> The chelating agent is a phosphonic acid or a salt thereof; <16> The composition described in <18> The chelating agent is hexamethylenediaminetetra(methylenephosphonic acid), 1-hydroxyethane-1,1-diphosphonic acid, aminotris(methylenephosphonic acid), ethylenediaminetetra(methylenephosphonic acid), tetramethylenediaminetetra(methylenephosphonic acid), diethylenetriaminepenta(methylenephosphonic acid), or a salt thereof; <16> The composition described in <19> the chelating agent comprises a polyaminopolycarboxylic acid; <16> The composition described in <20> the chelating agent comprises butylenediaminetetraacetic acid, diethylenetriaminepentaacetic acid, ethylenediaminetetrapropionic acid, triethylenetetraminehexaacetic acid, 1,3-diamino-2-hydroxypropane-N,N,N',N'-tetraacetic acid, propylenediaminetetraacetic acid, ethylenediaminetetraacetic acid, trans-1,2-diaminocyclohexanetetraacetic acid, ethylenediaminediacetic acid, ethylenediaminedipropionic acid, 1,6-hexamethylene-diamine-N,N,N',N'-tetraacetic acid, N,N-bis(2-hydroxybenzyl)ethylenediamine-N,N-diacetic acid, diaminopropanetetraacetic acid, 1,4,7,10-tetraazacyclododecane-tetraacetic acid, diaminopropanoltetraacetic acid, or (hydroxyethyl)ethylenediaminetriacetic acid; <16> The composition described in <21> The amount of the chelating agent is about 0.01% to about 10% by weight of the composition. <16> The composition described in <22> Further comprising a pH adjuster, <1> The composition described in <23> The pH adjuster comprises a base or an acid. <22> The composition described in <24> The base is an alkali hydroxide or ammonium hydroxide. <23> The composition described in <25> The amount of the pH adjuster is about 1% to about 10% by weight of the composition. <20> The composition described in <26> Further comprising a quaternary ammonium salt, <1> The composition described in <27> The quaternary ammonium salt is (lauryldimethylammonio)acetic acid, dodecyltrimethylammonium chloride, or benzyldodecyldimethylammonium bromide; <26> The composition described in <28> The amount of the quaternary ammonium salt is about 0.01% to about 1% by weight of the composition. <26> The composition described in <29> An etching composition comprising: (1) an oxidizing agent; (2) a hydroxycarboxylic acid having at least two carboxy groups; and (3) water; and wherein the etching composition does not contain an abrasive and has a pH of about 7 to about 10. <30> A semiconductor substrate including TaN features is <1> removing at least a portion of the TaN feature by contacting the TaN feature with a composition of formula (I). <31> Further comprising rinsing the semiconductor substrate with a rinsing solvent after the contacting step. <30> The method described above. <32> Further comprising drying the semiconductor after the rinsing step. <31> The method described above. <33> the method does not substantially remove copper in the semiconductor substrate; <30> The method described above. <34> <30> 2. An article formed by the method of claim 1, which is a semiconductor device. <35> the semiconductor device is an integrated circuit; <34> The article described in
Claims
1. An etching composition for removing at least a portion of a TaN feature by contacting a semiconductor substrate including the TaN feature with the etching composition, comprising: The etching composition comprises: (1) an oxidizing agent, (2) a hydroxycarboxylic acid having at least two carboxy groups; (3) an anionic surfactant, and (4) Water Including, the etching composition is abrasive-free and has a pH of 7 to 10; The anionic surfactant is an alkyl ethoxylated carboxylic acid or a salt thereof; The etching composition.
2. The composition of claim 1, having a pH of from 7 to 9.
5.
3. 2. The composition of claim 1, wherein the oxidizing agent comprises a peroxide, a persulfonic acid or a salt thereof, ozone, a peroxycarboxylic acid or a salt thereof, a perphosphoric acid or a salt thereof, a persulfuric acid or a salt thereof, a perchloric acid or a salt thereof, or a periodic acid or a salt thereof.
4. The composition of claim 1 , wherein the oxidizing agent comprises hydrogen peroxide or persulfuric acid.
5. The composition of claim 1, wherein the amount of said oxidizing agent is from 10% to 30% by weight of said composition.
6. The composition of claim 1 , wherein the hydroxycarboxylic acid is citric acid or tartaric acid.
7. The composition of claim 1, wherein the amount of said hydroxycarboxylic acid is from 1% to 10% by weight of said composition.
8. 2. The composition of claim 1, wherein the anionic surfactant is a compound of formula (I) or a salt thereof: 【Chemistry 1】 In formula (I), R is C 1 ~C 14 and n is an integer ranging from 1 to 14.
9. The composition of claim 1, wherein the amount of said anionic surfactant is from 0.001% to 5% by weight of the composition.
10. The composition of claim 1, wherein the amount of water is from 50% to 90% by weight of the composition.
11. The composition of claim 1 further comprising a metal corrosion inhibitor.
12. 12. The composition of claim 11, wherein the metal corrosion inhibitor comprises an azole or a salt thereof.
13. 12. The composition of claim 11, wherein the metal corrosion inhibitor comprises 1,2,3-triazole, 1,2,4-triazole, 4-amino-1,2,4-triazole, 3-amino-1,2,4-triazole-5-thiol, 1H-benzotriazole, 5-methyl-1H-benzotriazole, 1H-benzotriazole-1-methanol, 5,6-dimethyl-1H-benzotriazole, 2-amino-1,3,4-thiadiazole, 1H-tetrazole, 5-phenyl-1H-tetrazole, 5-amino-1H-tetrazole, or a combination thereof.
14. The composition of claim 11, wherein the amount of said metal corrosion inhibitor is from 0.01% to 10% by weight of said composition.
15. The composition of claim 1 further comprising a chelating agent.
16. The composition of claim 15, wherein the chelating agent is a phosphonic acid or a salt thereof.
17. 16. The composition of claim 15, wherein the chelating agent is hexamethylenediaminetetra(methylenephosphonic acid), 1-hydroxyethane-1,1-diphosphonic acid, aminotris(methylenephosphonic acid), ethylenediaminetetra(methylenephosphonic acid), tetramethylenediaminetetra(methylenephosphonic acid), diethylenetriaminepenta(methylenephosphonic acid), or a salt thereof.
18. The composition of claim 15 , wherein the chelating agent comprises a polyaminopolycarboxylic acid.
19. 16. The composition of claim 15, wherein the chelating agent comprises butylenediaminetetraacetic acid, diethylenetriaminepentaacetic acid, ethylenediaminetetrapropionic acid, triethylenetetraminehexaacetic acid, 1,3-diamino-2-hydroxypropane-N,N,N',N'-tetraacetic acid, propylenediaminetetraacetic acid, ethylenediaminetetraacetic acid, trans-1,2-diaminocyclohexanetetraacetic acid, ethylenediaminediacetic acid, ethylenediaminedipropionic acid, 1,6-hexamethylene-diamine-N,N,N',N'-tetraacetic acid, N,N-bis(2-hydroxybenzyl)ethylenediamine-N,N-diacetic acid, diaminopropanetetraacetic acid, 1,4,7,10-tetraazacyclododecane-tetraacetic acid, diaminopropanoltetraacetic acid, or (hydroxyethyl)ethylenediaminetriacetic acid.
20. The composition of claim 15, wherein the amount of said chelating agent is from 0.01% to 10% by weight of the composition.
21. The composition of claim 1 further comprising a pH adjuster.
22. 22. The composition of claim 21, wherein the pH adjuster comprises a base or an acid.
23. 23. The composition of claim 22, wherein the base is an alkali hydroxide or ammonium hydroxide.
24. The composition of claim 21, wherein the amount of said pH adjuster is from 1% to 10% by weight of the composition.
25. The composition of claim 1 further comprising a quaternary ammonium salt.
26. 26. The composition of claim 25, wherein the quaternary ammonium salt is (lauryldimethylammonio)acetic acid, dodecyltrimethylammonium chloride, or benzyldodecyldimethylammonium bromide.
27. 26. The composition of claim 25, wherein the amount of said quaternary ammonium salt is from 0.01% to 1% by weight of the composition.
28. 13. A method comprising contacting a semiconductor substrate including a TaN feature with the composition of claim 1 to remove at least a portion of said TaN feature.
29. 30. The method of claim 28, further comprising rinsing the semiconductor substrate with a rinsing solvent after the contacting step.
30. 30. The method of claim 29, further comprising drying the semiconductor substrate after the rinsing step.
31. The method of claim 28, wherein copper in the semiconductor substrate is removed at a rate that is slower than the rate at which the TaN features are removed.
Citation Information
Patent Citations
Etchant, etching method using the same, and method of manufacturing semiconductor element
JP2014093407A
Compositions and methods for selectively etching titanium nitride
JP2016527707A
Etchant composition for tantalum-containing layer, and etching method
JP2017162967A
Etching agent, etching method and liquid for preparing etching agent
US20110230053A1
Compositions and methods for selectively etching titanium nitride
US20160130500A1