Electrochemical device and electronic device including same
By optimizing the negative electrode active material layer with a low contact angle and specific properties, the cycling characteristics of lithium-ion batteries are enhanced, addressing defects that cause capacity degradation.
Patent Information
- Application Number
- JP2022516386
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-12-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-12-25
AI Technical Summary
Lithium-ion batteries experience a decrease in charge/discharge capacity due to defects such as pinholes and pits in the active material layer, which degrade their performance and cycling characteristics, particularly in aqueous slurry compositions used to reduce environmental impact.
The negative electrode active material layer is designed with a contact angle of 60° or less to a nonaqueous solvent, porosity between 10% to 60%, and specific characteristics such as carbon material properties and the inclusion of auxiliary agents to improve interfacial stability, reducing defects and enhancing cycling characteristics.
The solution results in improved cycling characteristics by minimizing defects and maintaining stability during charge/discharge cycles, thereby enhancing the performance and longevity of lithium-ion batteries.
Smart Images

Figure 0007575448000001 
Figure 0007575448000002 
Figure 0007575448000003
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of energy storage, and in particular to electrochemical devices and electronic devices containing same, in particular lithium-ion batteries. [Background technology]
[0002] With the development of technology and the increasing demand for mobile devices, the demand for electrochemical devices (e.g., lithium-ion batteries) increases significantly. Lithium-ion batteries, which have high energy density and excellent life and cycle characteristics at the same time, are one of the research topics.
[0003] The theoretical capacity of a lithium-ion battery may vary depending on the type of negative electrode active material. As the cycle progresses, the charge / discharge capacity of the lithium-ion battery usually decreases, deteriorating its performance. In recent years, in the manufacture of lithium-ion batteries, aqueous slurry compositions using an aqueous medium as a dispersion medium have been attracting more and more attention in order to reduce the environmental load, but the aqueous slurry has many defects such as pinholes and pits in the active material layer due to the presence of bubbles in the slurry composition, which affects the cycle characteristics of the electrochemical device.
[0004] In view of this, there is a need to provide improved electrochemical devices and electronic devices containing the same that have excellent cycling characteristics. Summary of the Invention
[0005] SUMMARY OF THE PRESENT EMBODIMENTS Embodiments of the present invention seek to solve, at least in part, at least one problem in the related art by providing an electrochemical device and an electronic device including the same.
[0006] In one aspect of the present invention, there is provided an electrochemical device comprising a positive electrode, a negative electrode and an electrolyte, wherein the negative electrode comprises a negative electrode active material layer, and a contact angle of the negative electrode active material layer with a non-aqueous solvent measured by a contact angle measurement method is 60° or less.
[0007] According to some embodiments of the present invention, a droplet diameter of the non-aqueous solvent on the negative electrode active material layer is 30 mm or less, as measured by contact angle measurement.
[0008] According to some embodiments of the present invention, the contact angle measurement method refers to dropping a 3 microliter droplet of diethyl carbonate on the surface of the negative electrode active material layer, and then measuring the contact angle of the droplet on the surface of the negative electrode active material layer within 100 seconds.
[0009] According to some embodiments of the present invention, the porosity of the negative electrode active material layer is 10% to 60%.
[0010] According to some embodiments of the present invention, the negative electrode active material layer includes a carbon material, and the carbon material is (a) Specific surface area is 5 m 2 / g or less; (b) the median diameter is 5 μm to 30 μm; The present invention has at least one of the following characteristics.
[0011] According to some embodiments of the present invention, the negative electrode active material layer includes at least one of artificial graphite, natural graphite, mesocarbon microbeads, soft carbon, hard carbon, amorphous carbon, a silicon-containing material, a tin-containing material, and an alloy material.
[0012] According to some embodiments of the present invention, the negative electrode active material layer further contains at least one metal selected from the group consisting of molybdenum, iron and copper, and the content of the at least one metal is less than or equal to 0.05 wt % based on the total weight of the negative electrode active material layer.
[0013] According to some embodiments of the present invention, the negative electrode active material layer further includes an auxiliary agent, and the auxiliary agent is (a) an oxidation potential of 4.5 V or more and a reduction potential of 0.5 V or less; (b) The surface tension is 30 mN / m or less; (c) comprising a nonionic surfactant; (d) the content of the auxiliary is 3000 ppm or less based on the total weight of the negative electrode active material layer; and The present invention has at least one of the following characteristics.
[0014] According to some embodiments of the present invention, the coagent comprises a non-ionic surfactant, the non-ionic surfactant comprising at least one of polyoxyethylene ethers, polyol esters, amides, and block polyethers.
[0015] According to some embodiments of the present invention, the non-ionic surfactant is polyoxyethylene alkanolamide (polyoxyethylene alkanolamide), polyoxyethylene octylphenol ether, polyoxyethylene nonylphenol ether, polyoxyethylene aliphatic higher alcohol ether, polyoxyethylene fatty acid ester, polyoxyethylene amine, alkanolamide, polyoxyethylene lauryl ether, polyoxyethylene primary alcohol ether having 12 to 14 carbon atoms, polyoxyethylene secondary alcohol ether having 12 to 14 carbon atoms, polyoxyethylene branched Guerbet alcohol ether having 13 carbon atoms, polyoxyethylene branched Guerbet alcohol having 10 carbon atoms, polyoxyethylene linear alcohol ether having 10 carbon atoms, polyoxyethylene linear octyl alcohol ether having 8 carbon atoms, polyoxyethylene isooctyl alcohol ether having 8 carbon atoms, fatty acid monoglyceride, monoglyceride, sorbitan fatty acid, silicon-polyether complex, polysorbate, polyoxyethylene fatty acid ester, polyoxyethylene aliphatic alcohol ether, polyoxyethylene-polyoxypropylene block copolymer, polyether-modified trisiloxane, and polyether-modified silicon polyether siloxane.
[0016] According to some embodiments of the present invention, the electrolyte contains ethylene carbonate, and the content of the ethylene carbonate in the electrolyte is X mg and the reaction area of the negative electrode active material layer is Y m 2The relationship 10≦(X / Y)≦100 is satisfied.
[0017] According to some embodiments of the present invention, the electrolyte further comprises a compound represented by formula 1, [ka] formula 1 where R is a linear or branched alkyl group having 1 to 5 carbon atoms or -SiR 2 R 3 R 4 where R 2 , R 3 and R 4 are each independently an alkyl group having 1 to 5 carbon atoms, and R 1 is an alkylene group having 2 to 3 carbon atoms and substituted with the following substituents, wherein the substituents are selected from at least one fluorine atom or an alkyl group containing at least one fluorine atom and having 1 to 3 carbon atoms:
[0018] According to some embodiments of the present invention, in Formula 1, R is -SiR 2 R 3 R 4 Also, R 1 is an alkylene group having 2 carbon atoms and substituted with the following substituents selected from at least one fluorine atom or an alkyl group containing at least one fluorine atom and having 1 to 3 carbon atoms:
[0019] According to some embodiments of the present invention, the compound represented by formula 1 includes at least one of the compounds represented by formulas 1a to 1h. [ka]
[0020] According to some embodiments of the present invention, the content of the compound represented by formula 1 is 0.001 wt % to 10 wt % based on the total weight of the electrolyte.
[0021] According to some embodiments of the present invention, the electrolyte further comprises a difluorophosphate salt and an iron group element, the iron group element comprising cobalt, nickel or a combination thereof, and the content of the iron group element is less than or equal to 0.05 wt % based on the total weight of the electrolyte.
[0022] According to a further aspect of the present invention there is provided an electronic device comprising an electrochemical device according to the present invention.
[0023] Other aspects and advantages of embodiments of the invention are described in part below, illustrated in part, or may be learned through the practice of embodiments of the invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Examples of the present invention will be described in detail below. The examples of the present invention should not be construed as limiting the present invention.
[0025] As used herein, the following terms have the meanings indicated below, unless otherwise specified.
[0026] In the detailed description and claims, a list of terms connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms can refer to any combination of the listed terms. For example, if terms A and B are listed, the statement "at least one of A and B" means A only, B only, or A and B. In another example, if terms A, B, and C are listed, the phrase "at least one of A, B, and C" means A only, B only, C only, A and B (excluding C), A and C (excluding B), B and C (excluding A), or all of A, B, and C. Term A may include a single element or multiple elements. Term B may include a single element or multiple elements. Term C may include a single element or multiple elements.
[0027] The term "alkyl group" is contemplated as a straight chain, saturated hydrocarbon structure having from 1 to 20 carbon atoms. An "alkyl group" is also contemplated as a branched or cyclic hydrocarbon structure having from 3 to 20 carbon atoms. When an alkyl group having a specific number of carbon atoms is specified, it is contemplated to include all geometric isomers having such number of carbon atoms. Thus, for example, "butyl group" is meant to include n-butyl group, s-butyl group, isobutyl group, t-butyl group, and cyclobutyl group. "Propyl group" includes n-propyl group, isopropyl group, and cyclopropyl group. Illustrative examples of alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, cyclopropyl, n-butyl, isobutyl, s-butyl, t-butyl, cyclobutyl, n-pentyl, isopentyl, neopentyl, cyclopentyl, methylcyclopentyl, ethylcyclopentyl, n-hexyl, isohexyl, cyclohexyl, n-heptyl, octyl, cyclopropyl, cyclobutyl, norbornyl, and the like.
[0028] The term "alkylene group" refers to a divalent saturated hydrocarbon group having a straight or branched chain. The alkylene group, unless otherwise defined, typically contains from 2 to 10 carbon atoms and includes (for example) -C 2-3 Alkylene group-C 2-6 Representative alkylene groups include (for example) methylene, ethane-1,2-diyl ("ethylene"), propane-1,2-diyl, propane-1,3-diyl, butane-1,4-diyl, pentane-1,5-diyl, and the like.
[0029] The theoretical capacity of an electrochemical device (e.g., lithium-ion battery) can vary depending on the type of negative electrode active material. As cycling progresses, lithium-ion batteries usually experience a decline in charge / discharge capacity. This is because the electrode active material does not function due to changes in the electrode interface during charging and / or discharging of the electrochemical device.
[0030] The present invention uses a specific negative electrode material to ensure interfacial stability during cycling of an electrochemical device, thereby improving the cycle characteristics of the electrochemical device. The specific negative electrode material of the present invention is realized by controlling the contact angle on the surface of the negative electrode active material layer. Methods for controlling the contact angle include a method of adding an auxiliary agent to the negative electrode slurry, and a method of providing an auxiliary agent coating layer on the surface of the negative electrode active material layer.
[0031] In one embodiment, the present invention provides an electrochemical device comprising a positive electrode, a negative electrode, and an electrolyte, as described below.
[0032] I, negative electrode The negative electrode includes a negative electrode current collector and a negative electrode active material layer provided on one or two surfaces of the negative electrode current collector.
[0033] 1, negative electrode active material layer The negative electrode active material layer includes a negative electrode active material. The negative electrode active material layer may be a single layer or a multi-layer. Each layer in the multi-layer negative electrode active material layer may include the same or different negative electrode active materials. The negative electrode active material is any material that can reversibly absorb and release metal ions, such as lithium ions. In some embodiments, the chargeable capacity of the negative electrode active material is greater than the discharge capacity of the positive electrode active material to prevent unintentional deposition of lithium metal on the negative electrode during charging.
[0034] (1) Contact angle The electrochemical device of the present invention is characterized in that the contact angle of the negative electrode active material layer with the non-aqueous solvent is 60° or less, as measured by a contact angle measurement method. In some embodiments, the contact angle of the negative electrode active material layer with the non-aqueous solvent is 50° or less, as measured by a contact angle measurement method. In some embodiments, the contact angle of the negative electrode active material layer with the non-aqueous solvent is 30° or less, as measured by a contact angle measurement method. When the negative electrode active material layer has such a contact angle with the non-aqueous solvent, defects at the interface of the negative electrode active material layer are relatively few, the interface of the negative electrode active material layer is stable during the charge / discharge cycle of the electrochemical device, and the cycle characteristics of the electrochemical device can be ensured.
[0035] The contact angle of the negative electrode active material layer with respect to the non-aqueous solvent indicates the surface characteristics of the negative electrode active material layer and is one of the physicochemical parameters that characterize the negative electrode active material layer. The smaller the contact angle, the smoother the surface of the negative electrode active material layer, and the fewer pinholes and pit defects there are, which can significantly improve the cycle characteristics of the electrochemical device. The contact angle of the negative electrode active material layer with respect to the non-aqueous solvent can be affected by various factors, including the porosity of the auxiliary agent and the negative electrode active material layer.
[0036] According to some embodiments of the present invention, the contact angle measurement method refers to dropping a 3 microliter droplet of diethyl carbonate on the surface of the negative electrode active material layer, and then measuring the contact angle of the droplet on the surface of the negative electrode active material layer within 100 seconds.
[0037] According to some embodiments of the present invention, the droplet diameter of the non-aqueous solvent on the negative electrode active material layer is 30 mm or less, as measured by contact angle measurement. In some embodiments, the droplet diameter of the non-aqueous solvent on the negative electrode active material layer is 20 mm or less, as measured by contact angle measurement. In some embodiments, the droplet diameter of the non-aqueous solvent on the negative electrode active material layer is 15 mm or less, as measured by contact angle measurement. In some embodiments, the droplet diameter of the non-aqueous solvent on the negative electrode active material layer is 10 mm or less, as measured by contact angle measurement. When the negative electrode active material layer has the above-mentioned contact angle with respect to the non-aqueous solvent and the non-aqueous solvent has the above-mentioned droplet diameter, the cycle characteristics of the electrochemical device are further improved.
[0038] The contact angle of the negative electrode active material layer to the non-aqueous solvent and the droplet diameter of the non-aqueous solvent can be measured by the following method. 3 microliters of diethyl carbonate is dropped onto the surface of the negative electrode active material layer, and the droplet diameter is measured within 100 seconds using a JC2000D3E contact angle meter. The diameter is then fitted by a five-point fitting method (i.e., first, the two left and right end points of the droplet are obtained, the liquid-solid interface is determined, and then three points are selected on the outline of the droplet) to obtain the contact angle of the negative electrode active material layer to the non-aqueous solvent. Each sample is measured at least three times, and at least three data with a difference of less than 5° are selected to obtain the average value, thereby obtaining the contact angle of the negative electrode active material layer to the non-aqueous solvent.
[0039] The non-aqueous solvent used in the contact angle measurement can be selected from commonly used electrolyte solvents such as diethyl carbonate, methyl ethyl carbonate, dimethyl carbonate, methyl propyl carbonate, or methyl isopropyl carbonate.
[0040] (2) Porosity According to some embodiments of the present invention, the porosity of the negative electrode active material layer is 10% to 60%. In some embodiments, the porosity of the negative electrode active material layer is 15% to 50%. In some embodiments, the porosity of the negative electrode active material layer is 20% to 40%. In some embodiments, the porosity of the negative electrode active material layer is 25% to 30%. In some embodiments, the porosity of the negative electrode active material layer is 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, or within a range formed by any two of the above values.
[0041] The porosity of the negative electrode active material layer can be measured by the following method. It is measured using a true density measuring device AccuPyc II 1340, and each sample is measured at least three times, and at least three data are selected to calculate an average value. The porosity of the negative electrode active material layer is calculated by the following formula: Porosity = (V1 - V2) / V1 x 100%, where V1 is the apparent volume, V1 = surface area of sample x thickness of sample x number of samples, and V2 is the true volume.
[0042] (3) Carbon materials According to some embodiments of the present invention, the negative electrode active material layer includes a carbon material.
[0043] According to some embodiments of the present invention, the negative electrode active material layer includes at least one of artificial graphite, natural graphite, mesocarbon microbeads, soft carbon, hard carbon, and amorphous carbon.
[0044] According to some embodiments of the present invention, the carbon material has amorphous carbon on a surface thereof.
[0045] According to some embodiments of the present invention, the shape of the carbon material includes, but is not limited to, fibrous, spherical, granular, and scaly shapes.
[0046] According to some embodiments of the present invention, the carbon material comprises: (a) Specific surface area (BET) is 5m2 / g or less; (b) The median diameter (D50) is 5 μm to 30 μm; The present invention has at least one of the following characteristics.
[0047] Specific surface area (BET) In some embodiments, the carbon material is 5 m 2 In some embodiments, the carbon material has a specific surface area of less than 3 m 2 In some embodiments, the carbon material has a specific surface area of less than 1 m 2 In some embodiments, the carbon material has a specific surface area of less than 0.1 m 2 In some embodiments, the carbon material has a specific surface area of more than 0.7 m 2 In some embodiments, the carbon material has a specific surface area of less than 0.5 m 2 / g. In some embodiments, the specific surface area of the carbon material is within the range defined by any two of the above values. When the specific surface area of the carbon material is within the above range, deposition of lithium on the surface of the electrode can be suppressed, and gas generation due to a reaction between the negative electrode and the electrolyte can be suppressed.
[0048] The porosity of the negative electrode active material layer can be measured by the following method. It is measured using a true density measuring device AccuPyc II 1340, and each sample is measured at least three times, and at least three data are selected to calculate an average value. The porosity of the negative electrode active material layer is calculated by the following formula: Porosity = (V1 - V2) / V1 x 100%, where V1 is the apparent volume, V1 = surface area of sample x thickness of sample x number of samples, and V2 is the true volume.
[0049] Median diameter (D50) The median diameter (D50) of the carbon material refers to the volume-based average particle diameter obtained by a laser diffraction / scattering method. In some embodiments, the carbon material has a median diameter (D50) of 5 μm to 30 μm. In some embodiments, the carbon material has a median diameter (D50) of 10 μm to 25 μm. In some embodiments, the carbon material has a median diameter (D50) of 15 μm to 20 μm. In some embodiments, the carbon material has a median diameter (D50) of 1 μm, 3 μm, 5 μm, 7 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, or a range formed by any two of the above values. When the median diameter of the carbon material is within the above range, the irreversible capacity of the electrochemical device is relatively small, and the negative electrode is easily coated uniformly.
[0050] The median diameter (D50) of the carbon material can be measured by the following method: the carbon material is dispersed in a 0.2 wt % aqueous solution (10 mL) of polyoxyethylene (20) sorbitan monolaurate, and the measurement is performed using a laser diffraction / scattering particle size distribution analyzer (LA-700 manufactured by Horiba, Ltd.).
[0051] X-ray diffraction pattern parameters According to some embodiments of the present invention, in an X-ray diffraction pattern by the Gakushin method, the interlayer distance of the lattice plane (002 plane) of the carbon material is in the range of 0.335 nm to 0.360 nm, in the range of 0.335 nm to 0.350 nm, or in the range of 0.335 nm to 0.345 nm.
[0052] According to some embodiments of the present invention, the crystallite size (Lc) of the carbon material is greater than 1.0 nm or greater than 1.5 nm in an X-ray diffraction pattern measured by the Gakushin method.
[0053] Raman Spectral Parameters In some embodiments, the carbon material has a Raman R value greater than 0.01, greater than 0.03, or greater than 0.1. In some embodiments, the carbon material has a Raman R value less than 1.5, less than 1.2, less than 1.0, or less than 0.5. In some embodiments, the carbon material has a Raman R value within a range formed by any two of the above values.
[0054] 1580 cm of the carbon material -1 The Raman half-width around 1580 cm of the carbon material is not particularly limited. -1 The Raman half-width in the vicinity is 10 cm -1 Over or 15cm -1 In some embodiments, the carbon material has a -1 The Raman half-width in the vicinity is 100 cm -1 Less than 80cm -1 Less than 60cm -1 Less than or equal to 40cm -1 In some embodiments, the carbon material has a surface area of less than 1580 cm -1 The Raman half-width in the vicinity is within the range formed by any two of the above values.
[0055] The Raman R value and the Raman half-width are indicators of the crystallinity of the surface of a carbon material. If the surface of a carbon material has a suitable crystallinity, the interlayer sites that accommodate lithium in the carbon material can be maintained and not lost during charging and discharging, which is advantageous for the chemical stability of the carbon material.
[0056] When the Raman R value and / or the Raman half-width are within the above-mentioned ranges, the carbon material can form an appropriate coating on the surface of the negative electrode, which is advantageous for improving the storage characteristics, cycle characteristics, load characteristics, etc. of the electrochemical device, and can also suppress a decrease in efficiency and gas generation due to a reaction between the carbon material and the electrolyte.
[0057] The Raman R value or Raman half-width can be measured by argon ion laser Raman spectroscopy. The measurement is performed by using a Raman spectrometer (Raman spectrometer manufactured by JASCO Corporation) to fill a sample into a measurement cell by gravity dropping, and rotating the cell in a plane perpendicular to the laser light while irradiating the sample surface in the cell with argon ion laser light. -1 The intensities of peaks PA and IA near 1360 cm -1 The intensity IB of the nearby peak PB is measured, and their intensity ratio R (R=IB / IA) is calculated.
[0058] The measurement conditions for the above-mentioned Raman spectroscopy are as follows. Argon ion laser wavelength: 514.5nm Laser power on sample: 15-25mW ·Resolution: 10~20cm -1 Measurement range: 1100cm -1 ~1730cm -1 Raman R value, Raman half-width analysis: background processing Smoothing process: Simple average, convolution 5 points
[0059] Circularity "Circularity" is defined by the following formula: Circularity = (perimeter of an equivalent circle having the same area as the projected shape of a particle) / (actual perimeter of the projected shape of a particle). A circularity of 1.0 is a theoretical perfect sphere.
[0060] In some embodiments, the carbon material has a particle size of 3 μm to 40 μm and a circularity of greater than 0.1, greater than 0.5, greater than 0.8, greater than 0.85, greater than 0.9, or 1.0.
[0061] Regarding high current density charge / discharge characteristics, the greater the circularity of the carbon material, the higher the packing property becomes, which is advantageous in suppressing resistance between particles, and therefore improves the high current density charge / discharge characteristics of the electrochemical device.
[0062] The circularity of the carbon material can be measured by a flow particle image analyzer (FPIA manufactured by Sysmex Corp.). Specifically, 0.2 g of a sample is dispersed in a 0.2 wt% aqueous solution (50 mL) of polyoxyethylene (20) sorbitan monolaurate, and ultrasonic waves of 28 kHz and output of 60 W are irradiated for 1 minute. Then, the detection range is set to 0.6 μm to 400 μm, and particles with particle diameters in the range of 3 μm to 40 μm are measured.
[0063] The method for improving the circularity is not particularly limited. The spheroidization treatment can be carried out in order to make the shape of the voids between the carbon material particles uniform when the carbon material is made into an electrode. The spheroidization treatment may be carried out by a mechanical method such as applying a shearing force or a compressive force, or may be carried out by a mechanical / physical method such as granulating a plurality of fine particles with a binder or by the adhesive force of the particles themselves. By carrying out the spheroidization treatment, the carbon material particles are made almost perfectly spherical.
[0064] Tap Density In some embodiments, the tap density of the carbon material is less than 0.1 g / cm 3 Super, 0.5g / cm 3 Super, 0.7g / cm 3 Over 1g / cm 3 In some embodiments, the tap density of the carbon material is greater than 2 g / cm 3 Less than 1.8g / cm 3 Less than or equal to 1.6g / cm 3 In some embodiments, the tap density of the carbon material is within a range formed by any two of the above values. When the tap density of the carbon material is within the above range, the capacity of the electrochemical device can be ensured and an increase in resistance between the carbon material particles can be suppressed.
[0065] The tap density of the carbon material can be measured by the following method. Specifically, a sample is passed through a sieve with an opening of 300 μm and then filtered for 20 cm. 3The sample is dropped into a tapping cell, filling the cell up to the top surface of the cell, and then tapping is performed 1,000 times with a stroke length of 10 mm using a powder density measuring device (e.g., Seishin Tap densor), and the tap density is calculated from the volume and mass of the sample at this time.
[0066] Orientation Ratio In some embodiments, the orientation ratio of the carbon material is greater than 0.005, greater than 0.01, or greater than 0.015. In some embodiments, the orientation ratio of the carbon material is less than 0.67. In some embodiments, the orientation ratio of the carbon material is within a range formed by any two values described above. When the orientation ratio of the carbon material is within the above range, the electrochemical device can have excellent high-density charge and discharge characteristics.
[0067] The orientation ratio of carbon materials can be measured by X-ray diffraction after pressing the sample. Specifically, 0.47 g of the sample was filled into a press with a diameter of 17 mm, and the orientation ratio was measured at 58.8 MN m -2 The compact obtained by compressing in step 1 is set using clay so that it is flush with the surface of the measurement sample holder, and X-ray diffraction measurement is performed. From the peak intensities of the (110) diffraction and (004) diffraction of the obtained carbon, the ratio expressed as the (110) diffraction peak intensity / (004) diffraction peak intensity is calculated.
[0068] The conditions for the X-ray diffraction measurement are as follows. Target: Cu (Kα line) graphite monochromator Slits: Divergence slit = 0.5 degrees, receiving slit = 0.15 mm, scattering slit = 0.5 degrees Measurement range and step angle / measurement time ("2θ" stands for the diffraction angle): (110) plane: 75 degrees≦2θ≦80 degrees 1 degree / 60 seconds (004) plane: 52 degrees ≦2θ≦57 degrees 1 degree / 60 seconds
[0069] Aspect Ratio In some embodiments, the aspect ratio of the carbon material is greater than 1, greater than 2, or greater than 3. In some embodiments, the aspect ratio of the carbon material is less than 10, less than 8, or less than 5. In some embodiments, the aspect ratio of the carbon material is within a range consisting of any two of the above values.
[0070] When the aspect ratio of the carbon material is within the above range, more uniform application can be achieved, so that the electrochemical device can have excellent high current density charge / discharge characteristics.
[0071] (4) Trace elements According to some embodiments of the present invention, the negative electrode active material layer further includes at least one metal selected from the group consisting of molybdenum, iron, and copper, which reacts with a portion of the poorly conductive organic matter in the negative electrode active material to promote the formation of a coating on the surface of the negative electrode active material.
[0072] According to some embodiments of the present invention, the above metal elements are present in the negative electrode active material layer in trace amounts, and excessive metal elements tend to form non-conductive by-products and adhere to the surface of the negative electrode. In some embodiments, the content of the at least one metal is 0.05 wt% or less based on the total weight of the negative electrode active material layer. In some embodiments, the content of the at least one metal is 0.03 wt% or less. In some embodiments, the content of the at least one metal is 0.01 wt% or less.
[0073] (5) Auxiliaries According to some embodiments of the present invention, the negative electrode active material layer further includes an auxiliary agent.
[0074] According to some embodiments of the present invention, the auxiliary agent is (a) an oxidation potential of 4.5 V or more and a reduction potential of 0.5 V or less; (b) The surface tension is 30 mN / m or less; (c) comprising a nonionic surfactant; (d) the content of the auxiliary is 3000 ppm or less based on the total weight of the negative electrode active material layer; and The present invention has at least one of the following characteristics.
[0075] Oxidation / Reduction Potential In some embodiments, the auxiliary has an oxidation potential of 4.5 V or more and a reduction potential of 0.5 V or less. In some embodiments, the auxiliary has an oxidation potential of 5 V or more and a reduction potential of 0.3 V or less. An auxiliary having the above-mentioned oxidation / reduction potential has stable electrochemical performance and is advantageous in improving the cycle characteristics of an electrochemical device.
[0076] surface tension In some embodiments, the surface tension of the auxiliary agent is 30 mN / m or less. In some embodiments, the surface tension of the auxiliary agent is 25 mN / m or less. In some embodiments, the surface tension of the auxiliary agent is 20 mN / m or less. In some embodiments, the surface tension of the auxiliary agent is 15 mN / m or less. In some embodiments, the surface tension of the auxiliary agent is 10 mN / m or less. The surface tension of the auxiliary agent is measured under the condition of an auxiliary agent aqueous solution with a solid content of 1%. An auxiliary agent having such a surface tension provides a good interface with the negative electrode active material layer, which is advantageous in improving the cycle characteristics of the electrochemical device.
[0077] The surface tension of the auxiliary can be measured by the following method: Specifically, a JC2000D3E contact angle meter is used to measure an aqueous solution of the auxiliary with a solid content of 1%, and each sample is measured at least three times, and at least three data are selected and averaged to obtain the surface tension of the auxiliary.
[0078] Nonionic Surfactants In some embodiments, the coagent comprises a non-ionic surfactant, and the non-ionic surfactant comprises at least one of a polyoxyethylene ether, a polyol ester, an amide, or a block polyether.
[0079] In some embodiments, the nonionic surfactant is a polyoxyethylene alkanolamide, polyoxyethylene octylphenol ether, polyoxyethylene nonylphenol ether, polyoxyethylene aliphatic higher alcohol ether, polyoxyethylene fatty acid ester, polyoxyethylene amine, alkanolamide, polyoxyethylene lauryl ether, polyoxyethylene primary alcohol ether having 12 to 14 carbon atoms, polyoxyethylene secondary alcohol ether having 12 to 14 carbon atoms, polyoxyethylene branched Guerbet alcohol ether having 13 carbon atoms, polyoxyethylene The polyoxyethylene fatty acid esters include at least one of C10 branched Guerbet alcohols, polyoxyethylene C10 linear alcohol ethers, polyoxyethylene C8 linear octyl alcohol ethers, polyoxyethylene C8 isooctyl alcohol ethers, fatty acid monoglycerides, monoglycerides, sorbitan fatty acids, silicon-polyether complexes, polysorbates, polyoxyethylene fatty acid esters, polyoxyethylene aliphatic alcohol ethers, polyoxyethylene-polyoxypropylene block copolymers, polyether-modified trisiloxanes, and polyether-modified silicon polyether siloxanes.
[0080] Auxiliary agent content In some embodiments, the content of the auxiliary is 2500 ppm or less, based on the total weight of the negative electrode active material layer. In some embodiments, the content of the auxiliary is 2000 ppm or less, based on the total weight of the negative electrode active material layer. In some embodiments, the content of the auxiliary is 1500 ppm or less, based on the total weight of the negative electrode active material layer. In some embodiments, the content of the auxiliary is 1000 ppm or less, based on the total weight of the negative electrode active material layer. In some embodiments, the content of the auxiliary is 500 ppm or less, based on the total weight of the negative electrode active material layer. In some embodiments, the content of the auxiliary is 200 ppm or less, based on the total weight of the negative electrode active material layer. When the auxiliary is contained in the above-mentioned amount, it is advantageous to improve the output characteristics, load characteristics, low temperature characteristics, cycle characteristics, and high temperature storage characteristics of the electrochemical device.
[0081] (6) Other ingredients Silicon and / or tin containing materials According to some embodiments of the present invention, the negative electrode active material layer further comprises at least one of a silicon-containing material, a tin-containing material, and an alloy material. According to some embodiments of the present invention, the negative electrode active material layer further comprises at least one of a silicon-containing material and a tin-containing material. In some embodiments, the negative electrode active material layer further comprises one or more of a silicon-containing material, a silicon-carbon composite material, a silicon-oxygen material, an alloy material, and a lithium-containing metal composite oxide material. In some embodiments, the negative electrode active material layer further comprises one or more other types of negative electrode active materials, for example, metal elements and metalloid elements that can form an alloy with lithium. In some embodiments, examples of the metal elements and metalloid elements include, but are not limited to, Mg, B, Al, Ga, In, Si, Ge, Sn, Pb, Bi, Cd, Ag, Zn, Hf, Zr, Y, Pd, and Pt. In some embodiments, examples of the metal elements and metalloid elements include Si, Sn, or a combination thereof. Si and Sn have excellent lithium ion releasing ability and can provide high energy density to lithium ion batteries. In some embodiments, other types of negative electrode active materials may include one or more of metal oxides and polymer compounds. In some embodiments, the metal oxides include, but are not limited to, iron oxide, ruthenium oxide, and molybdenum oxide. In some embodiments, the polymer compounds include, but are not limited to, polyacetylene, polyaniline, and polypyrrole.
[0082] Negative electrode conductive material In some embodiments, the negative electrode active material layer further includes a negative electrode conductive material. The conductive material may include any conductive material as long as it does not cause a chemical change. Non-limiting examples of the conductive material include carbon-based materials (e.g., natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon fiber, etc.), conductive polymers (e.g., polyphenylene derivatives), and mixtures thereof.
[0083] Negative electrode binder In some embodiments, the negative electrode active material layer further includes a negative electrode binder. The negative electrode binder can improve the bonding between particles of the negative electrode active material and between the negative electrode active material and the current collector. The type of the negative electrode binder is not particularly limited, and may be any material that is stable against the electrolyte or the solvent used in the manufacture of the electrode.
[0084] Examples of the negative electrode binder include resin-based polymers such as polyethylene, polypropylene, polyethylene terephthalate, polymethyl methacrylate, aromatic polyamide, polyimide, cellulose, and nitrocellulose; rubber-like polymers such as styrene-butadiene rubber (SBR), isoprene rubber, butadiene rubber, fluororubber, acrylonitrile-butadiene rubber (NBR), and ethylene-propylene rubber; styrene-butadiene-styrene block copolymers or hydrogenated products thereof; ethylene-propylene-diene terpolymers (EPDM), and styrene-ethylene-butadiene-styrene. Thermoplastic elastomer-like polymers such as copolymers, styrene-isoprene-styrene block copolymers or hydrogenated products thereof; soft resin-like polymers such as syndiotactic-1,2-polybutadiene, polyvinyl acetate, ethylene-vinyl acetate copolymers, and propylene-α-olefin copolymers; fluorine-based polymers such as polyvinylidene fluoride, polytetrafluoroethylene, fluorinated polyvinylidene fluoride, and polytetrafluoroethylene-ethylene copolymers; polymer compositions having ionic conductivity for alkali metal ions (especially lithium ions), but are not limited to these. The above-mentioned negative electrode binders may be used alone or in any combination.
[0085] In some embodiments, the content of the negative electrode binder is more than 0.1 wt%, more than 0.5 wt%, or more than 0.6 wt%, based on the total weight of the negative electrode active material layer. In some embodiments, the content of the negative electrode binder is less than 20 wt%, less than 15 wt%, less than 10 wt%, or less than 8 wt%, based on the total weight of the negative electrode active material layer. In some embodiments, the content of the negative electrode binder is within a range formed by any two of the above values. When the content of the negative electrode binder is within the above range, the capacity of the electrochemical device and the strength of the negative electrode can be sufficiently ensured.
[0086] When the anode active material layer contains a rubbery polymer (e.g., SBR), in some embodiments, the content of the anode binder is greater than 0.1 wt%, greater than 0.5 wt%, or greater than 0.6 wt%, based on the total weight of the anode active material layer. In some embodiments, the content of the anode binder is less than 5 wt%, less than 3 wt%, or less than 2 wt%, based on the total weight of the anode active material layer. In some embodiments, the content of the anode binder is within a range formed by any two of the above values, based on the total weight of the anode active material layer.
[0087] When the negative electrode active material layer contains a fluorine-based polymer (e.g., polyvinylidene fluoride), in some embodiments, the content of the negative electrode binder is greater than 1 wt%, greater than 2 wt%, or greater than 3 wt%, based on the total weight of the negative electrode active material layer. In some embodiments, the content of the negative electrode binder is less than 15 wt%, less than 10 wt%, or less than 8 wt%, based on the total weight of the negative electrode active material layer. The content of the negative electrode binder is within a range consisting of any two of the above values, based on the total weight of the negative electrode active material layer.
[0088] solvent The type of solvent for forming the negative electrode slurry is not particularly limited, and may be any solvent capable of dissolving or dispersing the negative electrode active material, the negative electrode binder, the thickener used as necessary, and the conductive material. In some embodiments, the solvent for forming the negative electrode slurry may be any one of an aqueous solvent and an organic solvent. Examples of the aqueous solvent include, but are not limited to, water, alcohol, and the like. Examples of the organic solvent include, but are not limited to, N-methylpyrrolidone (NMP), dimethylformamide, dimethylacetamide, ethyl methyl ketone, cyclohexanone, methyl acetate, methyl acrylate, diethylenetriamine, N,N-dimethylaminopropylamine, tetrahydrofuran (THF), toluene, acetone, diethyl ether, hexamethylphosphatamide, dimethylsulfoxide, benzene, xylene, quinoline, pyridine, methylnaphthalene, hexane, and the like. The above-mentioned solvents may be used alone or in any combination.
[0089] Thickener A thickener is usually used to adjust the viscosity of the negative electrode slurry. The type of thickener is not particularly limited, and examples thereof include, but are not limited to, carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein, and salts thereof. The above-mentioned thickeners may be used alone or in any combination.
[0090] In some embodiments, the content of the thickener is more than 0.1 wt%, more than 0.5 wt%, or more than 0.6 wt%, based on the total weight of the negative electrode active material layer. In some embodiments, the content of the thickener is less than 5 wt%, less than 3 wt%, or less than 2 wt%, based on the total weight of the negative electrode active material layer. When the content of the thickener is within the above range, the decrease in capacity and the increase in resistance of the electrochemical device can be suppressed, and good coating properties of the negative electrode slurry can be ensured.
[0091] Surface Coating In some embodiments, a material different from the composition of the negative electrode active material layer may be attached to the surface of the negative electrode active material layer. Examples of the material attached to the surface of the negative electrode active material layer include, but are not limited to, oxides such as aluminum oxide, silicon dioxide, titanium dioxide, zirconium oxide, magnesium oxide, calcium oxide, boron oxide, antimony oxide, and bismuth oxide; sulfates such as lithium sulfate, sodium sulfate, potassium sulfate, magnesium sulfate, calcium sulfate, and aluminum sulfate; carbonates such as lithium carbonate, calcium carbonate, and magnesium carbonate.
[0092] (7) Content of negative electrode active material In some embodiments, the content of the anode active material is greater than 80 wt%, greater than 82 wt%, or greater than 84 wt%, based on the total weight of the anode active material layer. In some embodiments, the content of the anode active material is less than 99 wt% or less than 98 wt%, based on the total weight of the anode active material layer. In some embodiments, the content of the anode active material is within a range formed by any two of the above values, based on the total weight of the anode active material layer.
[0093] (8) Thickness of the negative electrode active material layer The thickness of the negative electrode active material layer refers to the thickness of the negative electrode active material layer on any one side of the negative electrode current collector. In some embodiments, the thickness of the negative electrode active material layer is greater than 15 μm, greater than 20 μm, or greater than 30 μm. In some embodiments, the thickness of the negative electrode active material layer is less than 300 μm, less than 280 μm, or less than 250 μm. In some embodiments, the thickness of the negative electrode active material layer is within the range formed by any two of the values listed above.
[0094] (9) Density of negative electrode active material In some embodiments, the density of the negative electrode active material in the negative electrode active material layer is less than 1 g / cm 3 Super, 1.2g / cm 3 Over 1.3g / cm 3 In some embodiments, the density of the negative electrode active material in the negative electrode active material layer is greater than 2.2 g / cm 3 Less than 2.1g / cm 3Less than 2.0g / cm 3 Less than or equal to 1.9g / cm 3 In some embodiments, the density of the negative electrode active material in the negative electrode active material layer is within the range formed by any two of the above values.
[0095] When the density of the negative electrode active material is within the above-mentioned range, damage to the negative electrode active material particles can be prevented, and deterioration of the high current density charge / discharge characteristics due to an increase in the initial irreversible capacity of the electrochemical device or a decrease in the permeability of the electrolyte in the vicinity of the negative electrode current collector / negative electrode active material interface can be suppressed, and further a decrease in the capacity and an increase in the resistance of the electrochemical device can be suppressed.
[0096] 2, negative electrode current collector Any known current collector may be used as the current collector that holds the negative active material. Examples of the negative current collector include, but are not limited to, metal materials such as aluminum, copper, nickel, stainless steel, and nickel-plated steel. In some embodiments, the negative current collector is copper.
[0097] When the negative electrode current collector is a metal material, the form of the negative electrode current collector includes, but is not limited to, a metal foil, a metal cylinder, a metal coil, a metal plate, a metal thin film, an expanded metal, a punched metal, a foamed metal, etc. In some embodiments, the negative electrode current collector is a metal thin film. In some embodiments, the negative electrode current collector is a copper foil. In some embodiments, the negative electrode current collector is a rolled copper foil by a rolling method or an electrolytic copper foil by an electrolytic method.
[0098] In some embodiments, the thickness of the negative electrode current collector is greater than 1 μm or greater than 5 μm. In some embodiments, the thickness of the negative electrode current collector is less than 100 μm or less than 50 μm. In some embodiments, the thickness of the negative electrode current collector is within the range formed by any two of the values listed above.
[0099] The thickness ratio of the negative electrode current collector to the negative electrode active material layer refers to the ratio of the thickness of the negative electrode active material layer on one side before the electrolyte is injected to the thickness of the negative electrode current collector, and the value is not particularly limited. In some embodiments, the thickness ratio of the negative electrode current collector to the negative electrode active material layer is less than 150, less than 20, or less than 10. In some embodiments, the thickness ratio of the negative electrode current collector to the negative electrode active material layer is greater than 0.1, greater than 0.4, or greater than 1. In some embodiments, the thickness ratio of the negative electrode current collector to the negative electrode active material layer is within a range consisting of any two values described above. When the thickness ratio of the negative electrode current collector to the negative electrode active material layer is within the above range, the capacity of the electrochemical device can be ensured and heat generation of the negative electrode current collector during high current density charge and discharge can be suppressed.
[0100] II, electrolyte The electrolytic solution used in the electrochemical device of the present invention includes an electrolyte and a solvent that dissolves the electrolyte. In some embodiments, the electrolytic solution used in the electrochemical device of the present invention further includes an additive.
[0101] According to some embodiments of the present invention, the electrolyte contains ethylene carbonate, and the content of the ethylene carbonate in the electrolyte is X mg and the reaction area of the negative electrode active material layer is Y m 2 and X and Y satisfy the relationship 10≦(X / Y)≦100. In some embodiments, X and Y satisfy the relationship 10≦(X / Y)<100. In some embodiments, X and Y satisfy the relationship 20≦(X / Y)<70.
[0102] According to some embodiments of the present invention, the electrolyte further comprises a compound represented by formula 1, [ka] formula 1 where R is a linear or branched alkyl group having 1 to 5 carbon atoms or -SiR 2 R 3 R 4 where R 2 , R 3 and R 4are each independently an alkyl group having 1 to 5 carbon atoms, and R 1 is an alkylene group having 2 to 3 carbon atoms and substituted with the following substituents, wherein the substituents are selected from at least one fluorine atom or an alkyl group containing at least one fluorine atom and having 1 to 3 carbon atoms:
[0103] According to some embodiments of the present invention, in Formula 1, R is -SiR 2 R 3 R 4 Also, R 1 is an alkylene group having 2 carbon atoms and substituted with the following substituents selected from at least one fluorine atom or an alkyl group containing at least one fluorine atom and having 1 to 3 carbon atoms:
[0104] According to some embodiments of the present invention, the compound represented by formula 1 includes at least one of the compounds represented by formulas 1a to 1h. [ka]
[0105] According to some embodiments of the present invention, the content of the compound represented by formula 1 is 0.001 wt% to 10 wt% based on the total weight of the electrolyte. In some embodiments, the content of the compound represented by formula 1 is 0.005 wt% to 9 wt% based on the total weight of the electrolyte. In some embodiments, the content of the compound represented by formula 1 is 0.01 wt% to 8 wt% based on the total weight of the electrolyte. In some embodiments, the content of the compound represented by formula 1 is 0.05 wt% to 7 wt% based on the total weight of the electrolyte. In some embodiments, the content of the compound represented by formula 1 is 0.1 wt% to 6 wt% based on the total weight of the electrolyte. In some embodiments, the content of the compound represented by formula 1 is 0.5 wt% to 5 wt% based on the total weight of the electrolyte. In some embodiments, the content of the compound represented by formula 1 is 1 wt% to 4 wt% based on the total weight of the electrolyte. In some embodiments, the content of the compound represented by formula 1 is 2 wt % to 3 wt % based on the total weight of the electrolyte solution.
[0106] According to some embodiments of the present invention, the electrolyte further comprises a difluorophosphate and an iron group element, the iron group element comprising cobalt, nickel or a combination thereof, and the content of the iron group element is 0.05 wt% or less based on the total weight of the electrolyte. In some embodiments, the content of the iron group element is 0.03 wt% or less based on the total weight of the electrolyte. In some embodiments, the content of the iron group element is 0.02 wt% or less based on the total weight of the electrolyte. In some embodiments, the content of the iron group element is 0.01 wt% or less based on the total weight of the electrolyte. In some embodiments, the content of the iron group element is 0.005 wt% or less based on the total weight of the electrolyte. In some embodiments, the content of the iron group element is 0.004 wt% or less based on the total weight of the electrolyte. In some embodiments, the content of the iron group element is 0.002 wt% or less based on the total weight of the electrolyte.
[0107] In some embodiments, the electrolyte further comprises any non-aqueous solvent known in the art for use as a solvent for the electrolyte.
[0108] In some embodiments, the non-aqueous solvent may include, but is not limited to, one or more of cyclic carbonates, linear carbonates, cyclic carboxylic acid esters, linear carboxylic acid esters, cyclic ethers, linear ethers, phosphorus-containing organic solvents, sulfur-containing organic solvents, and aromatic fluorine-containing solvents.
[0109] In some embodiments, examples of the cyclic carbonate include, but are not limited to, one or more of ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate. In some embodiments, the cyclic carbonate has 3 to 6 carbon atoms.
[0110] In some embodiments, examples of the linear carbonate include, but are not limited to, one or more of linear carbonates such as dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate (DEC), methyl-n-propyl carbonate, ethyl-n-propyl carbonate, di-n-propyl carbonate, etc. Examples of fluorine-substituted linear carbonate include, but are not limited to, one or more of bis(fluoromethyl)carbonate, bis(difluoromethyl)carbonate, bis(trifluoromethyl)carbonate, bis(2-fluoroethyl)carbonate, bis(2,2-difluoroethyl)carbonate, bis(2,2,2-trifluoroethyl)carbonate, 2-fluoroethylmethylcarbonate, 2,2-difluoroethylmethylcarbonate, and 2,2,2-trifluoroethylmethylcarbonate.
[0111] In some embodiments, examples of the cyclic carboxylic acid ester include, but are not limited to, one or more of γ-butyrolactone and γ-valerolactone. In some embodiments, a portion of the hydrogen atoms of the cyclic carboxylic acid ester may be replaced with fluorine.
[0112] In some embodiments, examples of the chain carboxylic acid ester include, but are not limited to, one or more of methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, butyl acetate, sec-butyl acetate, isobutyl acetate, t-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, isopropyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, methyl isobutyrate, ethyl isobutyrate, methyl valerate, ethyl valerate, methyl pivalate, and ethyl pivalate. In some embodiments, some of the hydrogen atoms of the chain carboxylic acid ester may be substituted with fluorine. In some embodiments, examples of the chain carboxylic acid ester substituted with fluorine include, but are not limited to, methyl trifluoroacetate, ethyl trifluoroacetate, propyl trifluoroacetate, butyl trifluoroacetate, and 2,2,2-trifluoroethyl trifluoroacetate.
[0113] In some embodiments, examples of the cyclic ether include, but are not limited to, one or more of tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, 2-methyl-1,3-dioxolane, 4-methyl-1,3-dioxolane, 1,3-dioxane, 1,4-dioxane, and dimethoxypropane.
[0114] In some embodiments, examples of the linear ether include, but are not limited to, one or more of dimethoxymethane, 1,1-dimethoxyethane, 1,2-dimethoxyethane, diethoxymethane, 1,1-diethoxyethane, 1,2-diethoxyethane, ethoxymethoxymethane, 1,1-ethoxymethoxyethane, and 1,2-ethoxymethoxyethane.
[0115] In some embodiments, examples of the phosphorus-containing organic solvent include, but are not limited to, one or more of trimethyl phosphate, triethyl phosphate, dimethylethyl phosphate, methyldiethyl phosphate, ethylenemethyl phosphate, ethyleneethyl phosphate, triphenyl phosphate, trimethyl phosphite, triethyl phosphite, triphenyl phosphite, tris(2,2,2-trifluoroethyl)phosphate, and tris(2,2,3,3,3-pentafluoropropyl)phosphate, and the like.
[0116] In some embodiments, examples of the sulfur-containing organic solvent include, but are not limited to, one or more of sulfolane, 2-methylsulfolane, 3-methylsulfolane, dimethylsulfone, diethylsulfone, ethylmethylsulfone, methylpropylsulfone, dimethylsulfoxide, methyl methanesulfonate, ethyl methanesulfonate, methyl ethanesulfonate, ethyl ethanesulfonate, dimethyl sulfate, diethyl sulfate, and dibutyl sulfate. In some embodiments, some of the hydrogen atoms of the sulfur-containing organic solvent may be replaced with fluorine.
[0117] In some embodiments, the aromatic fluorine-containing solvent includes, but is not limited to, one or more of fluorobenzene, difluorobenzene, trifluorobenzene, tetrafluorobenzene, pentafluorobenzene, hexafluorobenzene, and trifluoromethylbenzene.
[0118] In some embodiments, the solvent used in the electrolyte of the present invention includes cyclic carbonates, linear carbonates, cyclic carboxylic acid esters, linear carboxylic acid esters, and combinations thereof. In some embodiments, the solvent used in the electrolyte of the present invention includes at least one of ethylene carbonate, propylene carbonate, diethyl carbonate, ethyl propionate, propyl propionate, n-propyl acetate, and ethyl acetate. In some embodiments, the solvent used in the electrolyte of the present invention includes ethylene carbonate, propylene carbonate, diethyl carbonate, ethyl propionate, propyl propionate, γ-butyrolactone, and combinations thereof.
[0119] After adding the chain carboxylate and / or the cyclic carboxylate to the electrolyte, the chain carboxylate and / or the cyclic carboxylate form a passivation film on the surface of the electrode, thereby improving the capacity retention rate after intermittent charging cycles of the electrochemical device. In some embodiments, the electrolyte contains 1 wt% to 60 wt% of the chain carboxylate, the cyclic carboxylate, and combinations thereof. In some embodiments, the electrolyte contains ethyl propionate, propyl propionate, γ-butyrolactone, and combinations thereof, and the content of the combination is 1 wt% to 60 wt%, 10 wt% to 60 wt%, 10 wt% to 50 wt%, or 20 wt% to 50 wt% based on the total weight of the electrolyte. In some embodiments, the electrolyte contains 1 wt%-60 wt%, 10 wt%-60 wt%, 20 wt%-50 wt%, 20 wt%-40 wt%, or 30 wt% propyl propionate, based on the total weight of the electrolyte.
[0120] In some embodiments, examples of the additives include, but are not limited to, one or more of fluorinated carbonates, ethylene carbonate containing a carbon-carbon double bond, compounds containing sulfur-oxygen double bonds, and acid anhydrides.
[0121] In some embodiments, the content of the additive is 0.01% to 15%, 0.1% to 10%, or 1% to 5%, based on the total weight of the electrolyte.
[0122] According to an embodiment of the present invention, the content of the propionate is 1.5 to 30 times, 1.5 to 20 times, 2 to 20 times, or 5 to 20 times that of the additive, based on the total weight of the electrolyte.
[0123] In some embodiments, the additive comprises one or more fluorinated carbonates, which together with the propionate can form a stable protective film on the surface of the negative electrode during charging / discharging of the lithium ion battery, thus inhibiting the decomposition reaction of the electrolyte.
[0124] In some embodiments, the fluorinated carbonate has the formula C=O(OR 1 )(OR 2 ), where R 1 and R 2 are each independently selected from an alkyl group or a halogenated alkyl group having 1 to 6 carbon atoms, where R 1 and R 2 At least one of R is selected from fluoroalkyl groups having 1 to 6 carbon atoms, and 1 and R 2 optionally form a 5- to 7-membered ring together with the atoms to which they are attached.
[0125] In some embodiments, examples of the fluorinated carbonate ester include, but are not limited to, one or more of fluoroethylene carbonate, cis-4,4-difluoroethylene carbonate, trans-4,4-difluoroethylene carbonate, 4,5-difluoroethylene carbonate, 4-fluoro-4-methylethylene carbonate, 4-fluoro-5-methylethylene carbonate, trifluoromethyl methyl carbonate, trifluoroethyl methyl carbonate, and trifluoroethyl ethyl carbonate.
[0126] In some embodiments, the additive comprises one or more ethylene carbonates containing carbon-carbon double bonds, examples of which include, but are not limited to, vinylene carbonate, methylvinylene carbonate, ethylvinylene carbonate, 1,2-dimethylvinylene carbonate, 1,2-diethylvinylene carbonate, fluorovinylene carbonate, trifluoromethylvinylene carbonate; vinylethylene carbonate, 1-methyl-2-vinylethylene carbonate, 1-ethyl-2-vinylethylene carbonate, 1-n-propyl-2-vinylethylene carbonate, 1-methyl-2-vinylethylene carbonate, 1,1-divinylethylene carbonate, 1,2-divinylethylene carbonate, 1,1-dimethyl-2-methyleneethylene carbonate, and 1,1-diethyl-2-methyleneethylene carbonate. In some embodiments, the ethylene carbonate containing carbon-carbon double bonds includes vinylene carbonate, which is readily available and provides additional advantages.
[0127] In some embodiments, the additive comprises one or more compounds containing a sulfur-oxygen double bond, examples of which include, but are not limited to, one or more of cyclic sulfates, linear sulfates, linear sulfonates, cyclic sulfonates, linear sulfites, and cyclic sulfites.
[0128] Examples of the cyclic sulfate include, but are not limited to, one or more of 1,2-ethylene sulfate, 1,2-propylene sulfate, 1,3-propylene sulfate, 1,2-butylene sulfate, 1,3-butylene sulfate, 1,4-butylene sulfate, 1,2-pentylene sulfate, 1,3-pentylene sulfate, 1,4-pentylene sulfate, and 1,5-pentylene sulfate.
[0129] Examples of the chain sulfate ester include, but are not limited to, one or more of dimethyl sulfate, ethyl methyl sulfate, and diethyl sulfate.
[0130] Examples of the chain sulfonate ester include, but are not limited to, one or more of fluorosulfonate esters such as methyl fluorosulfonate and ethyl fluorosulfonate, methyl methanesulfonate, ethyl methanesulfonate, butyl dimethanesulfonate, methyl 2-(methanesulfonyloxy)propionate, and ethyl 2-(methanesulfonyloxy)propionate.
[0131] Illustrative examples of the cyclic sulfonic acid ester include 1,3-propane sultone, 1-fluoro-1,3-propane sultone, 2-fluoro-1,3-propane sultone, 3-fluoro-1,3-propane sultone, 1-methyl-1,3-propane sultone, 2-methyl-1,3-propane sultone, 3-methyl-1,3-propane sultone, 1-propylene-1,3-sultone, 2-propylene-1,3-sultone, 1-fluoro-1-propylene-1,3-sultone, 2-fluoro-1-propylene-1,3-sultone, 3-fluoro-1-propylene-1,3-sultone, 1-fluoro-2-propylene-1,3-sultone, and 1-fluoro-2-propylene-1,3-sultone. The polysulfones include, but are not limited to, one or more of sultone, 2-fluoro-2-propylene-1,3-sultone, 3-fluoro-2-propylene-1,3-sultone, 1-methyl-1-propylene-1,3-sultone, 2-methyl-1-propylene-1,3-sultone, 3-methyl-1-propylene-1,3-sultone, 1-methyl-2-propylene-1,3-sultone, 2-methyl-2-propylene-1,3-sultone, 3-methyl-2-propylene-1,3-sultone, 1,4-butane sultone, 1,5-pentane sultone, methylene methane disulfonate, and ethylene methane disulfonate.
[0132] Examples of the chain sulfite ester include, but are not limited to, one or more of dimethyl sulfite, ethyl methyl sulfite, and diethyl sulfite.
[0133] Examples of the cyclic sulfite include, but are not limited to, one or more of 1,2-ethylene sulfite, 1,2-propylene sulfite, 1,3-propylene sulfite, 1,2-butylene sulfite, 1,3-butylene sulfite, 1,4-butylene sulfite, 1,2-pentylene sulfite, 1,3-pentylene sulfite, 1,4-pentylene sulfite, and 1,5-pentylene sulfite.
[0134] In some embodiments, the additive comprises one or more acid anhydrides. Examples of the acid anhydrides include, but are not limited to, one or more of phosphonic acid cyclic anhydrides, carboxylic acid anhydrides, disulfonic acid anhydrides, and carboxylic acid sulfonic acid anhydrides. Examples of the phosphonic acid cyclic anhydrides include, but are not limited to, one or more of trimethylphosphonic acid cyclic anhydride, triethylphosphonic acid cyclic anhydride, and tripropylphosphonic acid cyclic anhydride. Examples of the carboxylic acid anhydrides include, but are not limited to, one or more of succinic anhydride, glutaric anhydride, and maleic anhydride. Examples of the disulfonic acid anhydrides include, but are not limited to, one or more of ethane disulfonic acid anhydride and propane disulfonic acid anhydride. Examples of the carboxylic acid sulfonic acid anhydrides include, but are not limited to, one or more of sulfobenzoic acid anhydride, sulfopropionic acid anhydride, and sulfobutyric acid anhydride.
[0135] In some embodiments, the additive is a combination of a fluorinated carbonate and ethylene carbonate containing a carbon-carbon double bond. In some embodiments, the additive is a combination of a fluorinated carbonate and a compound containing a sulfur-oxygen double bond. In some embodiments, the additive is a combination of a fluorinated carbonate and a compound having 2 to 4 cyano groups. In some embodiments, the additive is a combination of a fluorinated carbonate and a cyclic carboxylic acid ester. In some embodiments, the additive is a combination of a fluorinated carbonate and a phosphonic acid cyclic anhydride. In some embodiments, the additive is a combination of a fluorinated carbonate and a carboxylic acid anhydride. In some embodiments, the additive is a combination of a fluorinated carbonate and a sulfonic acid anhydride. In some embodiments, the additive is a combination of a fluorinated carbonate and a carboxylic acid sulfonic acid anhydride.
[0136] The electrolyte is not particularly limited, and any substance known as an electrolyte may be used. In the case of a lithium secondary battery, a lithium salt is usually used. An example of the electrolyte is LiPF 6 , LiBF 4 , LiClO 4 , LiAlF 4 , LiSbF 6 , LiTaF 6 , LiWF 7 Inorganic lithium salts such as LiWOF 5 Lithium tungstates such as HCO 2 Li, C.H. 3 CO 2 Li, C.H. 2 FCO 2 Li, C.H.F. 2 CO 2 Li, C.F. 3 CO 2 Li, C.F. 3 CH 2 CO 2 Li, C.F. 3 CF 2 CO 2 Li, C.F. 3 CF2 CF 2 CO 2 Li, C.F. 3 CF 2 CF 2 CF 2 CO 2 Lithium carboxylates such as Li;FSO 3 Li, C.H. 3 SO 3 Li, C.H. 2 FSO 3 Li, C.H.F. 2 SO 3 Li, C.F. 3 SO 3 Li, C.F. 3 CF 2 SO 3 Li, C.F. 3 CF 2 CF 2 SO 3 Li, C.F. 3 CF 2 CF 2 CF 2 SO 3 Lithium sulfonates such as Li; LiN(FCO) 2 , LiN(FCO)(FSO 2 ), LiN(FSO 2 ) 2 , LiN(FSO 2 )(CF 3 SO 2 ), LiN(CF 3 SO 2 ) 2 , LiN(C 2 F 5 SO 2 ) 2 , lithium cyclic 1,2-perfluoroethane disulfonylimide, lithium cyclic 1,3-perfluoropropane disulfonylimide, LiN(CF 3 SO 2 )(C 4 F 9 SO 2 Lithium imide salts such as LiC(FSO 2 ) 3 , LiC(CF 3 SO 2 ) 3 , LiC(C 2 F5 SO 2 ) 3 Lithium methylate salts such as lithium bis(malonato)borate, lithium difluoro(malonato)borate, and the like; lithium malonato)borate salts such as lithium tris(malonato)phosphate, lithium difluorobis(malonato)phosphate, lithium tetrafluoro(malonato)phosphate, and the like; and LiPF 4 (CF 3 ) 2 , LiPF 4 (C 2 F 5 ) 2 , LiPF 4 (CF 3 SO 2 ) 2 , LiPF 4 (C 2 F 5 SO 2 ) 2 , LiBF 3 CF 3 , LiBF 3 C 2 F 5 , LiBF 3 C 3 F 7 , LiBF 2 (CF 3 ) 2 , LiBF 2 (C 2 F 5 ) 2 , LiBF 2 (CF 3 SO 2 ) 2 , LiBF 2 (C 2 F 5 SO 2 ) 2lithium oxalatoborate salts such as lithium difluoro(oxalato)borate, lithium bis(oxalato)borate; lithium (oxalato)phosphate salts such as lithium tetrafluoro(oxalato)phosphate, lithium difluorobis(oxalato)phosphate, lithium tris(oxalato)phosphate, and the like.
[0137] In certain embodiments, the electrolyte is LiPF 6 , LiSbF 6 , LiTaF 6 , FSO 3 Li, C.F. 3 SO 3 Li, LiN(FSO 2 ) 2 , LiN(FSO 2 )(CF 3 SO 2 ), LiN(CF 3 SO 2 ) 2 , LiN(C 2 F 5 SO 2 ) 2 , Lithium cyclic 1,2-perfluoroethane disulfonylimide, Lithium cyclic 1,3-perfluoropropane disulfonylimide, LiC(FSO 2 ) 3 , LiC(CF 3 SO 2 ) 3 , LiC(C 2 F 5 SO 2 ) 3 , LiBF 3 CF 3 , LiBF 3 C 2 F 5 , LiPF 3 (CF 3 ) 3 , LiPF 3 (C 2 F 5 ) 3, lithium difluoro(oxalato)borate, lithium bis(oxalato)borate, or lithium difluorobis(oxalato)phosphate. They contribute to improving the output characteristics, high-rate charge / discharge characteristics, high-temperature storage characteristics, and cycle characteristics of electrochemical devices.
[0138] The content of the electrolyte is not particularly limited as long as it does not impair the effect of the present invention. In some embodiments, the total molar concentration of lithium in the electrolyte is more than 0.3 mol / L, more than 0.4 mol / L, or more than 0.5 mol / L. In some embodiments, the total molar concentration of lithium in the electrolyte is less than 3 mol / L, less than 2.5 mol / L, or less than 2.0 mol / L. In some embodiments, the total molar concentration of lithium in the electrolyte is within a range consisting of any two values described above. When the concentration of the electrolyte is within the above range, lithium, which is a charged particle, is sufficient, and the viscosity can be kept within an appropriate range, making it easy to ensure good electrical conductivity.
[0139] When two or more electrolytes are used in combination, the electrolyte comprises at least one salt selected from the group consisting of monofluorophosphate, borate, oxalate, and fluorosulfonate. In some embodiments, the electrolyte comprises a salt selected from the group consisting of monofluorophosphate, oxalate, and fluorosulfonate. In some embodiments, the electrolyte comprises a lithium salt. In some embodiments, the content of the salt selected from the group consisting of monofluorophosphate, borate, oxalate, and fluorosulfonate is greater than 0.01 wt% or greater than 0.1 wt% based on the total weight of the electrolyte. In some embodiments, the content of the salt selected from the group consisting of monofluorophosphate, borate, oxalate, and fluorosulfonate is less than 20 wt% or less than 10 wt% based on the total weight of the electrolyte. In some embodiments, the content of the salt selected from the group consisting of monofluorophosphate, borate, oxalate, and fluorosulfonate is within the range consisting of any two of the above values.
[0140] In some embodiments, the electrolyte comprises one or more materials selected from the group consisting of monofluorophosphates, borates, oxalates, and fluorosulfonates, and one or more other salts, such as the lithium salts exemplified above, and in some embodiments, the other salts are LiPF 6 , LiN(FSO 2 )(CF 3 SO 2 ), LiN(CF 3 SO 2 ) 2 , LiN(C 2 F 5 SO 2 ) 2 , Lithium cyclic 1,2-perfluoroethane disulfonylimide, Lithium cyclic 1,3-perfluoropropane disulfonylimide, LiC(FSO 2 ) 3 , LiC(CF 3 SO 2 ) 3 , LiC(C 2 F 5 SO 2 ) 3 , LiBF 3 CF 3 , LiBF 3 C 2 F 5 , LiPF 3 (CF 3 ) 3 , LiPF 3 (C 2 F 5 ) 3 In some embodiments, the other salt is LiPF 6 It is.
[0141] In some embodiments, the content of the other salt is more than 0.01 wt% or more than 0.1 wt% based on the total weight of the electrolyte. In some embodiments, the content of the other salt is less than 20 wt%, less than 15 wt%, or less than 10 wt% based on the total weight of the electrolyte. In some embodiments, the content of the other salt is within a range consisting of any two of the above values. The other salt having the above content contributes to balancing the electrical conductivity and viscosity of the electrolyte.
[0142] In addition to the above-mentioned solvent, additives, and electrolyte salt, the electrolyte may contain other additives such as an anode film forming agent, a cathode protector, and an overcharge inhibitor, if necessary. As the additive, an additive that is usually used in a non-aqueous electrolyte secondary battery can be used, and examples thereof include, but are not limited to, vinylene carbonate, succinic anhydride, biphenyl, cyclohexylbenzene, 2,4-difluoroanisole, propane sultone, propene sultone, and the like. These additives may be used alone or in any combination. The content of these additives in the electrolyte is not particularly limited, and may be appropriately set depending on the type of the additive. In some embodiments, the content of the additive is less than 5 wt%, in the range of 0.01 wt% to 5 wt%, or in the range of 0.2 wt% to 5 wt%, based on the total weight of the electrolyte.
[0143] III, positive electrode The positive electrode includes a positive electrode current collector and a positive electrode active material layer disposed on one or two surfaces of the positive electrode current collector.
[0144] 1. Positive electrode active material layer The positive electrode active material layer includes a positive electrode active material. The positive electrode active material layer may be a single layer or a multi-layer. Each layer in the multi-layer positive electrode active material may include the same or different positive electrode active materials. The positive electrode active material is a material that can reversibly absorb and release any metal ion such as lithium ion.
[0145] The type of the positive electrode active material is not particularly limited, and may be any material capable of absorbing and releasing metal ions (e.g., lithium ions) in an electrochemical manner. In some embodiments, the positive electrode active material is a material containing lithium and at least one transition metal. Examples of the positive electrode active material include, but are not limited to, lithium transition metal composite oxides and lithium-containing transition metal phosphate compounds.
[0146] In some embodiments, the transition metal in the lithium transition metal composite oxide includes V, Ti, Cr, Mn, Fe, Co, Ni, Cu, etc. In some embodiments, the lithium transition metal composite oxide is LiCoO 2 Lithium-cobalt composite oxides such as LiNiO 2 Lithium-nickel composite oxides such as LiMnO 2 , LiMn 2 O 4 , Li 2 MnO 4 Lithium manganese composite oxides such as LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O 2 , LiNi 0.5 Mn 0.3 Co 0.2 O 2 Lithium transition metal oxides include lithium nickel manganese cobalt composite oxides such as LiNi, where some of the transition metal atoms, which are the main part of these lithium transition metal composite oxides, are replaced by other elements such as Na, K, B, F, Al, Ti, V, Cr, Mn, Fe, Co, Li, Ni, Cu, Zn, Mg, Ga, Zr, Si, Nb, Mo, Sn, and W. An example of a lithium transition metal composite oxide is LiNi 0.5 Mn 0.5 O 2 , LiNi 0.85 Co 0.10 Al 0.05 O 2 , LiNi 0.33 Co 0.33 Mn 0.33 O 2 , LiNi 0.45 Co 0.10 Al 0.45 O 2 , LiMn1.8 Al 0.2 O 4 and LiMn 1.5 Ni 0.5 O 4 Examples of lithium transition metal oxide combinations include, but are not limited to, LiCoO 2 and LiMn 2 O 4 and combinations thereof, including, but not limited to, LiMn 2 O 4 A part of Mn in may be replaced by a transition metal (e.g., LiNi 0.33 Co 0.33 Mn 0.33 O 2 ), LiCoO 2 A part of Co in the above may be substituted with a transition metal.
[0147] In some embodiments, the transition metal in the lithium-containing transition metal phosphate compound includes V, Ti, Cr, Mn, Fe, Co, Ni, Cu, etc. In some embodiments, the lithium-containing transition metal phosphate compound is LiFePO 4 , Li 3 Fe 2 (PO 4 ) 3 , LifeP 2 O 7 Iron phosphates such as LiCoPO 4 and the like, in which some of the transition metal atoms that are the major part of these lithium-containing transition metal phosphate compounds are replaced with other elements, such as Al, Ti, V, Cr, Mn, Fe, Co, Li, Ni, Cu, Zn, Mg, Ga, Zr, Nb, Si, and the like.
[0148] In some embodiments, the positive electrode active material includes lithium phosphate, which can improve the continuous charging characteristics of the electrochemical device. The use of lithium phosphate is not limited. In some embodiments, the positive electrode active material and lithium phosphate are used in combination. In some embodiments, the content of lithium phosphate is greater than 0.1 wt%, greater than 0.3 wt%, or greater than 0.5 wt%, based on the total weight of the positive electrode active material and lithium phosphate. In some embodiments, the content of lithium phosphate is less than 10 wt%, less than 8 wt%, or less than 5 wt%, based on the total weight of the positive electrode active material and lithium phosphate. In some embodiments, the content of lithium phosphate is within a range consisting of any two of the values described above.
[0149] Surface Coating A substance having a different composition from the positive electrode active material may be attached to the surface of the positive electrode active material. Examples of the surface-attached substance include, but are not limited to, oxides such as aluminum oxide, silicon dioxide, titanium dioxide, zirconium oxide, magnesium oxide, calcium oxide, boron oxide, antimony oxide, and bismuth oxide; sulfates such as lithium sulfate, sodium sulfate, potassium sulfate, magnesium sulfate, calcium sulfate, and aluminum sulfate; carbonates such as lithium carbonate, calcium carbonate, and magnesium carbonate; and carbon.
[0150] These surface-attaching substances can be attached to the surface of the positive electrode active material by a method of dissolving or suspending the surface-attaching substance in a solvent, impregnating and adding it to the positive electrode active material, and drying it; a method of dissolving or suspending a precursor of the surface-attaching substance in a solvent, impregnating and adding it to the positive electrode active material, and then reacting it by heating or the like; and a method of adding it to a precursor of the positive electrode active material and simultaneously baking it, etc. When attaching carbon, a method of mechanically attaching a carbon material (e.g., activated carbon, etc.) can also be used.
[0151] In some embodiments, the content of the surface attachment material is greater than 0.1 ppm, greater than 1 ppm, or greater than 10 ppm, based on the total weight of the positive electrode active material layer. In some embodiments, the content of the surface attachment material is less than 20%, less than 10%, or less than 10%, based on the total weight of the positive electrode active material layer. In some embodiments, the content of the surface attachment material is within a range formed by any two of the above values, based on the total weight of the positive electrode active material layer.
[0152] The surface-attached substance of the positive electrode active material can suppress the oxidation reaction of the electrolyte on the surface of the positive electrode active material, thereby improving the life of the electrochemical device. If the amount of the surface-attached substance is too small, the effect is not fully exerted, and if the amount of the surface-attached substance is too large, the ingress and egress of lithium ions is inhibited, which may increase the resistance.
[0153] In the present invention, a positive electrode active material having a substance with a different composition from the positive electrode active material attached to its surface is also referred to as a "positive electrode active material".
[0154] shape In some embodiments, the shape of the particles of the positive electrode active material includes, but is not limited to, agglomerates, polyhedrons, spheres, ellipsoids, plates, needles, columns, etc. In some embodiments, the particles of the positive electrode active material include primary particles, secondary particles, or combinations thereof. In some embodiments, the primary particles may aggregate to form secondary particles.
[0155] Tap Density In some embodiments, the tap density of the positive electrode active material is 0.5 g / cm 3 Super, 0.8g / cm 3 Over 1.0g / cm 3When the tap density of the positive electrode active material is within the above range, the amount of dispersion medium, conductive material, and positive electrode binder required during the formation of the positive electrode active material layer can be reduced, so that the packing rate of the positive electrode active material and the capacity of the electrochemical device can be ensured. By using a complex oxide powder with a high tap density, a high density positive electrode active material layer can be formed. Generally, the higher the tap density, the more preferable it is, and there is no particular upper limit. In some embodiments, the tap density of the positive electrode active material is 4.0 g / cm or less. 3 Less than 3.7g / cm 3 Less than or equal to 3.5g / cm 3 When the tap density of the positive electrode active material has the above upper limit, it is possible to suppress a decrease in the load characteristics.
[0156] The tap density of the positive electrode active material is determined as the powder packing density (tap density) when 5 g to 10 g of the positive electrode active material powder is placed in a 10 mL glass measuring cylinder and tapped 200 times with a stroke of 20 mm.
[0157] Median diameter (D50) When the particles of the positive electrode active material are primary particles, the median diameter (D50) of the particles of the positive electrode active material refers to the primary particle diameter of the particles of the positive electrode active material. When the primary particles of the particles of the positive electrode active material are aggregated to form secondary particles, the median diameter (D50) of the particles of the positive electrode active material refers to the secondary particle diameter of the particles of the positive electrode active material.
[0158] In some embodiments, the median diameter (D50) of the particles of the positive electrode active material is greater than 0.3 μm, greater than 0.5 μm, greater than 0.8 μm, or greater than 1.0 μm. In some embodiments, the median diameter (D50) of the particles of the positive electrode active material is less than 30 μm, less than 27 μm, less than 25 μm, or less than 22 μm. In some embodiments, the median diameter (D50) of the particles of the positive electrode active material is within a range consisting of any two values described above. When the median diameter (D50) of the particles of the positive electrode active material is within the above range, a positive electrode active material with a high tap density can be obtained, and the deterioration of the characteristics of the electrochemical device can be suppressed. Meanwhile, during the preparation process of the positive electrode of the electrochemical device (i.e., when the positive electrode active material, the conductive material, the binder, etc. are slurried with a solvent and applied in a thin film), problems such as the occurrence of streaks can be prevented. Here, by mixing two or more positive electrode active materials having different median diameters, the filling property during the preparation of the positive electrode can be further improved.
[0159] The particle median diameter (D50) of the positive electrode active material can be measured by a laser diffraction / scattering type particle size distribution analyzer. Specifically, when using HORIBA's LA-920 as a particle size distribution analyzer, a 0.1 wt% sodium hexametaphosphate aqueous solution is used as the dispersion medium for the measurement, and the measurement is performed after ultrasonic dispersion for 5 minutes with a measurement refractive index set to 1.24.
[0160] Average primary particle size When the primary particles of the positive electrode active material aggregate to form secondary particles, in some embodiments, the average primary particle size of the positive electrode active material is greater than 0.05 μm, greater than 0.1 μm, or greater than 0.5 μm. In some embodiments, the average primary particle size of the positive electrode active material is less than 5 μm, less than 4 μm, less than 3 μm, or less than 2 μm. In some embodiments, the average primary particle size of the positive electrode active material is within a range consisting of any two values described above. When the average primary particle size of the positive electrode active material is within the above range, powder packing and specific surface area can be ensured, deterioration of battery characteristics can be suppressed, and appropriate crystallinity can be obtained, so that the reversibility of charge and discharge of the electrochemical device can be ensured.
[0161] The average primary particle diameter of the positive electrode active material is obtained by observing an image taken with a scanning electron microscope (SEM). Specifically, in an SEM image with a magnification of 10,000 times, the longest intercept of the horizontal line at the left and right boundaries of the primary particles is calculated for any 50 primary particles, and the average value is calculated to obtain the average primary particle diameter.
[0162] Specific surface area (BET) In some embodiments, the specific surface area (BET) of the positive electrode active material is less than 0.1 m 2 / g, 0.2m 2 / g or greater than 0.3m 2 In some embodiments, the specific surface area (BET) of the positive electrode active material is greater than 50 m 2 / g, less than 40m 2 / g or less than 30m 2 / g. In some embodiments, the specific surface area (BET) of the positive electrode active material is within a range formed by any two values described above. When the specific surface area (BET) of the positive electrode active material is within the above range, the positive electrode active material can have good coating properties while ensuring the characteristics of the electrochemical device.
[0163] The specific surface area (BET) of the positive electrode active material can be measured by the following method: Using a surface area meter (e.g., a fully automatic surface area measuring device manufactured by Ohkura Riken), nitrogen gas is passed through the sample, and the sample is pre-dried at 150°C for 30 minutes, and then the specific surface area is measured by the nitrogen adsorption BET one-point method using a gas flow method, using a nitrogen-helium mixed gas precisely adjusted so that the relative pressure of the nitrogen gas to the atmospheric pressure is 0.3.
[0164] Positive electrode conductive material The type of the positive electrode conductive material is not limited, and any known conductive material can be used. Examples of the positive electrode conductive material include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black; carbon materials such as amorphous carbon such as needle coke; carbon nanotubes; graphene, etc. The above-mentioned positive electrode conductive materials may be used alone or in any combination.
[0165] In some embodiments, the content of the positive electrode conductive material is greater than 0.01 wt%, greater than 0.1 wt%, or greater than 1 wt%, based on the total weight of the positive electrode active material layer. In some embodiments, the content of the positive electrode conductive material is less than 50 wt%, less than 30 wt%, or less than 15 wt%, based on the total weight of the positive electrode active material layer. When the content of the positive electrode conductive material is within the above range, sufficient conductivity and capacity of the electrochemical device can be ensured.
[0166] Positive electrode binder The type of positive electrode binder used in the manufacture of the positive electrode active material layer is not particularly limited, and in the case of a coating method, any material may be used as long as it is soluble or dispersible in the liquid medium used in the manufacture of the electrode. Examples of positive electrode binders include resin-based polymers such as polyethylene, polypropylene, polyethylene terephthalate, polymethyl methacrylate, polyimide, aromatic polyamide, cellulose, and nitrocellulose; rubber-like polymers such as styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber (NBR), fluororubber, isoprene rubber, butadiene rubber, and ethylene-propylene rubber; styrene-butadiene-styrene block copolymers or their hydrogenated products, ethylene-propylene-diene terpolymers (EPDM), styrene-ethylene-butadiene-ethylene copolymers, styrene-propylene-diene terpolymers (EPDM), styrene-ethylene-butadiene-ethylene copolymers, and styrene-propylene-diene terpolymers. The positive electrode binder may include, but is not limited to, one or more of the following: thermoplastic elastomeric polymers such as ethylene-isoprene-styrene block copolymers or hydrogenated products thereof; soft resinous polymers such as syndiotactic-1,2-polybutadiene, polyvinyl acetate, ethylene-vinyl acetate copolymers, and propylene-α-olefin copolymers; fluorine-based polymers such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene, fluorinated polyvinylidene fluoride, and polytetrafluoroethylene-ethylene copolymers; and polymer compositions having ionic conductivity for alkali metal ions (especially lithium ions). The positive electrode binders described above may be used alone or in any combination.
[0167] In some embodiments, the content of the positive electrode binder is more than 0.1 wt%, more than 1 wt%, or more than 1.5 wt%, based on the total weight of the positive electrode active material layer. In some embodiments, the content of the positive electrode binder is less than 80 wt%, less than 60 wt%, less than 40 wt%, or less than 10 wt%, based on the total weight of the positive electrode active material layer. When the content of the positive electrode binder is within the above range, the capacity of the electrochemical device can be secured while the positive electrode has good electrical conductivity and sufficient mechanical strength.
[0168] solvent The type of solvent for forming the positive electrode slurry is not limited, and may be any solvent capable of dissolving or dispersing the positive electrode active material, the conductive material, the positive electrode binder, and the thickener used as needed. Examples of the solvent for forming the positive electrode slurry may include any one of an aqueous solvent and an organic solvent. Examples of the aqueous solvent include, but are not limited to, water, and a mixture of alcohol and water. Examples of organic solvents include, but are not limited to, aliphatic hydrocarbons such as hexane; aromatic hydrocarbons such as benzene, toluene, xylene, and methylnaphthalene; heterocyclic compounds such as quinoline and pyridine; ketones such as acetone, ethyl methyl ketone, and cyclohexanone; esters such as methyl acetate and methyl acrylate; amines such as diethylenetriamine and N,N-dimethylaminopropylamine; ethers such as diethyl ether, propylene oxide, and tetrahydrofuran (THF); amides such as N-methylpyrrolidone (NMP), dimethylformamide, and dimethylacetamide; and aprotic polar solvents such as hexamethylphosphamide and dimethylsulfoxide.
[0169] Thickener A thickener is usually used to adjust the viscosity of the slurry. When a water-based solvent is used, a thickener and a styrene-butadiene rubber (SBR) latex may be used to form a slurry. The type of thickener is not particularly limited, and examples thereof include, but are not limited to, carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein, and salts thereof. The above-mentioned thickeners may be used alone or in any combination.
[0170] In some embodiments, the content of the thickener is more than 0.1 wt%, more than 0.2 wt%, or more than 0.3 wt%, based on the total weight of the positive electrode active material layer. In some embodiments, the content of the thickener is less than 5 wt%, less than 3 wt%, or less than 2 wt%, based on the total weight of the positive electrode active material layer. In some embodiments, the content of the thickener is within a range formed by any two of the above values, based on the total weight of the positive electrode active material layer. When the content of the thickener is within the above range, the positive electrode slurry has good coating properties and the capacity decrease and the resistance increase of the electrochemical device can be suppressed.
[0171] Positive electrode active material content In some embodiments, the content of the positive electrode active material is more than 80 wt%, more than 82 wt%, or more than 84 wt%, based on the total weight of the positive electrode active material layer. In some embodiments, the content of the positive electrode active material is less than 99 wt% or less than 98 wt%, based on the total weight of the positive electrode active material layer. In some embodiments, the content of the positive electrode active material is within a range formed by any two values described above, based on the total weight of the positive electrode active material layer. When the content of the positive electrode active material is within the above range, the strength of the positive electrode can be maintained while ensuring the electric capacity of the positive electrode active material in the positive electrode active material layer.
[0172] Density of the positive electrode active material The positive electrode active material layer obtained by coating and drying may be subjected to a compaction treatment using a hand press, a roller press, or the like in order to increase the packing density of the positive electrode active material. In some embodiments, the density of the positive electrode active material layer is 1.5 g / cm 3 Super, 2g / cm 3 Over 2.2g / cm 3 In some embodiments, the density of the positive electrode active material layer is greater than 5 g / cm 3 Less than 4.5g / cm 3 Less than or equal to 4g / cm 3 In some embodiments, the density of the positive electrode active material layer is within a range formed by any two values described above. When the density of the positive electrode active material layer is within the above range, the electrochemical device can have good charge / discharge characteristics while suppressing an increase in resistance.
[0173] Thickness of the positive electrode active material layer The thickness of the positive electrode active material layer refers to the thickness of the positive electrode active material layer on any one side of the positive electrode current collector. In some embodiments, the thickness of the positive electrode active material layer is greater than 10 μm or greater than 20 μm. In some embodiments, the thickness of the positive electrode active material layer is less than 500 μm or less than 450 μm.
[0174] Method for producing positive electrode active material The positive electrode active material may be manufactured by a general method for manufacturing an inorganic compound. In order to prepare a spherical or elliptical positive electrode active material, the following manufacturing method may be adopted. Specifically, the raw material of the transition metal is dissolved or crushed and dispersed in a solvent such as water, and the pH is adjusted while stirring to prepare a spherical precursor, which is then recovered and dried as necessary, and then LiOH, Li 2 CO 3 , LiNO 3 A Li source such as the above is added and calcined at high temperature to obtain the positive electrode active material.
[0175] 2, Positive electrode current collector The type of the positive electrode current collector is not particularly limited, and may be any known material that is applied to a positive electrode current collector. Examples of the positive electrode current collector include, but are not limited to, metal materials such as aluminum, stainless steel, nickel plating, titanium, and tantalum; and carbon materials such as carbon cloth and carbon paper. In some embodiments, the positive electrode current collector is a metal material. In some embodiments, the positive electrode current collector is aluminum.
[0176] The form of the positive electrode current collector is not particularly limited. When the positive electrode current collector is a metal material, the form of the positive electrode current collector includes, but is not limited to, a metal foil, a metal cylinder, a metal coil, a metal plate, a metal thin film, an expanded metal, a punched metal, a foamed metal, and the like. When the positive electrode current collector is a carbon material, the form of the positive electrode current collector includes, but is not limited to, a carbon plate, a carbon thin film, a carbon cylinder, and the like. In some embodiments, the positive electrode current collector is a metal thin film. In some embodiments, the metal thin film is in the form of a mesh. The thickness of the metal thin film is not particularly limited. In some embodiments, the thickness of the metal thin film is greater than 1 μm, greater than 3 μm, or greater than 5 μm. In some embodiments, the thickness of the metal thin film is less than 1 mm, less than 100 μm, or less than 50 μm. In some embodiments, the thickness of the metal thin film is within the range consisting of any two values described above.
[0177] In order to reduce the electrical contact resistance between the positive electrode current collector and the positive electrode active material layer, a conductive additive may be included on the surface of the positive electrode current collector. Examples of the conductive additive include, but are not limited to, carbon and precious metals such as gold, platinum, and silver.
[0178] The thickness ratio of the positive electrode collector to the positive electrode active material layer refers to the ratio of the thickness of the positive electrode active material layer on one side before the electrolyte is injected to the thickness of the positive electrode collector, and the value is not particularly limited. In some embodiments, the thickness ratio of the positive electrode collector to the positive electrode active material layer is less than 20, less than 15, or less than 10. In some embodiments, the thickness ratio of the positive electrode collector to the positive electrode active material layer is greater than 0.5, greater than 0.8, or greater than 1. In some embodiments, the thickness ratio of the positive electrode collector to the positive electrode active material layer is within a range consisting of any two values described above. When the thickness ratio of the positive electrode collector to the positive electrode active material layer is within the above range, the heat dissipation of the positive electrode collector during high current density charging and discharging can be suppressed, and the capacity of the electrochemical device can be ensured.
[0179] 3. Positive electrode structure and manufacturing method The positive electrode is produced by forming a positive electrode active material layer containing a positive electrode active material and a binder on a current collector. The positive electrode using the positive electrode active material can be produced by a conventional method. That is, the positive electrode active material and the binder, as well as the conductive material and thickener used as necessary, are mixed in a dry state to form a sheet, which is then pressed onto the positive electrode current collector; or these materials are dissolved or dispersed in a liquid medium to form a slurry, which is then applied to the positive electrode current collector and dried to form a positive electrode active material layer on the current collector, thereby obtaining a positive electrode.
[0180] IV, separator A separator is usually provided between the positive electrode and the negative electrode to prevent short circuiting, and in this case, the electrolyte of the present invention is usually impregnated into the separator before use.
[0181] The material and shape of the separator are not particularly limited as long as they do not significantly impair the effects of the present invention. The separator may be a resin, glass fiber, inorganic material, etc., made of a material stable to the electrolyte of the present invention. In some embodiments, the separator includes a porous sheet or nonwoven fabric-like material having excellent liquid retention. Examples of materials for the resin or glass fiber separator include, but are not limited to, polyolefin, aromatic polyamide, polytetrafluoroethylene, polyethersulfone, glass filter, etc. In some embodiments, the material for the separator is a glass filter. In some embodiments, the polyolefin is polyethylene or polypropylene. In some embodiments, the polyolefin is polypropylene. The above-mentioned separator materials may be used alone or in any combination.
[0182] The separator may be a material formed by laminating the above-mentioned materials, and examples thereof include, but are not limited to, a three-layer separator formed by laminating polypropylene, polyethylene, and polypropylene in this order.
[0183] Examples of inorganic materials include, but are not limited to, oxides such as aluminum oxide, silicon dioxide, etc.; nitrides such as aluminum nitride, silicon nitride, etc.; sulfates (e.g., barium sulfate, calcium sulfate, etc.). The form of the inorganic material includes, but is not limited to, particulate or fibrous.
[0184] The separator is in the form of a thin film, examples of which include, but are not limited to, nonwoven fabric, woven fabric, microporous film, etc. In the thin film form, the pore size of the separator is 0.01 μm to 1 μm, and the thickness is 5 μm to 50 μm. In addition to the above-mentioned independent thin film separator, a separator formed by forming a composite porous layer containing the above-mentioned inorganic particles on the surface of a positive electrode and / or a negative electrode using a resin binder, for example, a separator formed by forming a porous layer of aluminum oxide with a 90% particle size of less than 1 μm on both sides of a positive electrode using a fluororesin as a binder, can also be used.
[0185] The thickness of the separator is arbitrary. In some embodiments, the thickness of the separator is more than 1 μm, more than 5 μm, or more than 8 μm. In some embodiments, the thickness of the separator is less than 50 μm, less than 40 μm, or less than 30 μm. In some embodiments, the thickness of the separator is within a range formed by any two of the above values. When the thickness of the separator is within the above range, the rate characteristics and energy density of the electrochemical device can be ensured while ensuring insulation and mechanical strength.
[0186] When a porous material such as a porous sheet or nonwoven fabric is used as the separator, the porosity of the separator is arbitrary. In some embodiments, the porosity of the separator is more than 20%, more than 35%, or more than 45%. In some embodiments, the porosity of the separator is less than 90%, less than 85%, or less than 75%. In some embodiments, the porosity of the separator is within a range formed by any two of the above values. When the porosity of the separator is within the above range, the resistance of the membrane can be suppressed while ensuring insulation and mechanical strength, and the electrochemical device has good rate characteristics.
[0187] The average pore size of the separator is also arbitrary. In some embodiments, the average pore size of the separator is less than 0.5 μm or less than 0.2 μm. In some embodiments, the average pore size of the separator is greater than 0.05 μm. In some embodiments, the average pore size of the separator is within a range formed by any two values described above. If the average pore size of the separator exceeds the above range, a short circuit is likely to occur. If the average pore size of the separator is within the above range, it is possible to prevent a short circuit while suppressing the membrane resistance, and to provide the electrochemical device with good rate characteristics.
[0188] V. Components of electrochemical devices The components of the electrochemical device include an electrode group, a current collecting structure, an outer case, and a protective element.
[0189] electrode group The electrode group may have any one of a laminated structure formed by stacking the above-mentioned positive electrode and negative electrode with the above-mentioned separator interposed therebetween, and a structure in which the above-mentioned positive electrode and negative electrode are spirally wound with the above-mentioned separator interposed therebetween. In some embodiments, the ratio of the volume of the electrode group to the internal volume of the battery (electrode group occupancy rate) is more than 40% or more than 50%. In some embodiments, the electrode group occupancy rate is less than 90% or less than 80%. In some embodiments, the electrode group occupancy rate is within a range formed by any two values described above. When the electrode group occupancy rate is within the above-mentioned range, the capacity of the electrochemical device can be secured while suppressing deterioration of characteristics such as charge / discharge cycle characteristics and high-temperature storage characteristics caused by an increase in internal pressure, and thus the operation of the gas release valve can be prevented.
[0190] Current collection structure The current collecting structure is not particularly limited. In some embodiments, the current collecting structure is a structure that reduces the resistance of the wiring portion and the joint portion. When the electrode group has the above-mentioned laminated structure, a structure formed by bundling the metal core portions of the electrode layers and welding them to a terminal is preferably used. Since the internal resistance increases when the electrode area is large, it is also preferable to provide two or more terminals in the electrode to reduce the resistance. When the electrode group has the above-mentioned wound structure, the internal resistance can be reduced by providing two or more lead structures on each of the positive electrode and the negative electrode and bundling them to a terminal.
[0191] Outer case The material of the outer case is not particularly limited as long as it is a material that is stable against the electrolyte used. The outer case is made of metals such as nickel-plated steel, stainless steel, aluminum or aluminum alloy, magnesium alloy, or a laminate film of resin and aluminum foil, but is not limited thereto. In some embodiments, the outer case is made of metal such as aluminum or aluminum alloy, or a laminate film.
[0192] The metal exterior case includes, but is not limited to, a sealed structure formed by welding metals together by laser welding, resistance welding, or ultrasonic welding; or a crimped structure formed by using the above-mentioned metals via a resin gasket. The above-mentioned exterior case using the laminate film includes, but is not limited to, a sealed structure formed by heat-sealing resin layers together. In order to improve the sealing property, a resin different from the resin used in the laminate film may be interposed between the above-mentioned resin layers. When the resin layer is heat-sealed via the current collecting terminal to form a sealed structure, the metal and the resin are bonded, so that a resin having a polar group or a modified resin into which a polar group has been introduced is used as the interposed resin. The shape of the exterior case is also arbitrary, and may be, for example, any one of a cylindrical shape, a rectangular shape, a laminate type, a button type, a large size, etc.
[0193] Protection Device The protective element may be a positive temperature coefficient (PTC) whose resistance increases when abnormal heat is generated or an excessive current flows, a thermal fuse, a thermistor, a valve (current cutoff valve) that cuts off the current flowing in the circuit due to a sudden increase in the internal pressure or temperature of the battery when abnormal heat is generated, etc. The above-mentioned protective elements may be selected so that they do not operate under conditions of normal use at high current, or a design may be used in which abnormal heat generation or thermal runaway does not occur even without the protective element.
[0194] VI. Application The electrochemical device of the present invention includes any device in which an electrochemical reaction occurs, and specific examples thereof include all kinds of primary batteries, secondary batteries, fuel cells, solar cells, or capacitors. In particular, the electrochemical device is a lithium secondary battery, including a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, and a lithium ion polymer secondary battery.
[0195] The present invention further provides an electronic device comprising an electrochemical device according to the present invention.
[0196] The application of the electrochemical device of the present invention is not particularly limited, and can be used in any electronic device known in the existing technology. In some embodiments, the electrochemical device of the present invention is used in notebook computers, pen-input personal computers, mobile personal computers, electronic book players, mobile phones, mobile fax machines, mobile copiers, mobile printers, headphone stereos, video movie machines, liquid crystal televisions, handy cleaners, portable CDs, mini discs, transceivers, electronic organizers, calculators, memory cards, portable tape recorders, radios, backup power sources, motors, automobiles, motorcycles, assisted bicycles, bicycles, lighting equipment, toys, game equipment, watches, power tools, strobes, cameras, large-scale household storage batteries, and lithium ion capacitors, but is not limited thereto.
[0197] Hereinafter, the preparation of a lithium ion battery will be described with reference to specific examples, and those skilled in the art should understand that the preparation method described in the present invention is merely exemplary, and any other suitable preparation method is within the scope of the present invention.
[0198] Working Example Examples and comparative examples of the lithium ion battery according to the present invention will be described below, and performance evaluation will be performed.
[0199] 1. Preparation of lithium-ion batteries 1. Preparation of the negative electrode Artificial graphite, styrene-butadiene rubber, and sodium carboxymethylcellulose were mixed with deionized water and auxiliary agents in a mass ratio of 96%:2%:2%, and stirred uniformly to obtain anode slurry. The anode slurry was applied onto a 12 μm copper foil. The anode was dried, cold pressed, punched, and tab welded to obtain anode. The anode was set according to the conditions of the following examples and comparative examples to have the corresponding parameters.
[0200] 2. Preparation of the positive electrode Lithium cobalt oxide (LiCoO 2), conductive material (Super-P), and polyvinylidene fluoride (PVDF) were mixed with N-methylpyrrolidone (NMP) in a mass ratio of 95%:2%:3% and stirred uniformly to obtain a positive electrode slurry. This positive electrode slurry was applied onto 12 μm aluminum foil, dried, cold pressed, punched, and tabs were welded to obtain a positive electrode.
[0201] 3. Preparation of electrolyte EC, PC, and DEC (weight ratio 1:1:1) were mixed in a dry argon gas atmosphere, and LiPF 6 The concentration of LiPF was adjusted to 1.15 mol / L. 6 The basic electrolyte solution was prepared by adding different amounts of additives to the basic electrolyte solution to obtain different examples and comparative examples of electrolyte solutions.
[0202] 4. Preparation of the separator A polyethylene (PE) porous polymer thin film was used as the separator.
[0203] 5. Preparation of Lithium-ion Battery The obtained positive electrode, separator, and negative electrode were wound in order and placed in an exterior foil, leaving an inlet through which an electrolyte was injected, and the battery was sealed. After going through processes such as formation and capacity measurement, a lithium-ion battery was obtained.
[0204] 2.Measurement method 1. Method for measuring the contact angle of the negative electrode active material layer with a non-aqueous solvent Three microliters of diethyl carbonate was dropped onto the surface of the negative electrode active material layer, and within 100 seconds, the contact angle was measured using a JC2000D3E contact angle meter, and the contact angle was fitted using a five-point fitting method (i.e., first, the left and right end points of the droplet were obtained, the liquid-solid interface was determined, and then three points were selected on the outline of the droplet) to obtain the contact angle of the negative electrode active material layer with respect to the non-aqueous solvent. Each sample was measured at least three times, and at least three data with a difference of less than 5° were selected and averaged to obtain the contact angle of the negative electrode active material layer with respect to the non-aqueous solvent.
[0205] 2. Method for measuring droplet diameter of non-aqueous solvent Three microliters of diethyl carbonate was dropped onto the surface of the negative electrode active material layer, and the droplet diameter was measured within 100 seconds using a JC2000D3E contact angle measuring instrument.
[0206] 3. Method for measuring the porosity of the negative electrode active material layer The measurements were performed using a density measuring device AccuPyc II 1340, and each sample was measured at least three times, and at least three pieces of data were selected to calculate the average value. The porosity of the negative electrode active material layer was calculated by the following formula. Porosity=(V1-V2) / V1×100% where V1 is the apparent volume, V1 = surface area of sample x thickness of sample x number of samples; V2 is the true volume.
[0207] 4. Measurement method of specific surface area (BET) Using a surface area meter (e.g., a fully automatic surface area measuring device manufactured by Ohkura Riken), nitrogen gas was passed through the sample, and the sample was pre-dried for 15 minutes at 350°C. Then, the surface area was measured by the nitrogen adsorption BET one-point method using a gas flow method, using a nitrogen-helium mixed gas precisely adjusted so that the relative pressure of nitrogen to atmospheric pressure was 0.3.
[0208] 5. How to measure the median diameter (D50) The carbon material was dispersed in a 0.2 wt % aqueous solution (10 mL) of polyoxyethylene (20) sorbitan monolaurate, and the particle size distribution was measured using a laser diffraction / scattering type particle size distribution analyzer (LA-700 manufactured by Horiba Manufacturing Co., Ltd.).
[0209] 6. Method for measuring the surface tension of auxiliary agents A JC2000D3E contact angle meter was used to measure the aqueous solution of the auxiliary agent with a solid content of 1%, and each sample was measured at least three times. At least three data were selected and averaged to obtain the surface tension of the auxiliary agent.
[0210] 7. Method for measuring the reaction area of the negative electrode active material layer The specific surface area of the negative electrode active material layer was measured by the above-mentioned "method of measuring specific surface area (BET)". The specific surface area of the negative electrode active material layer refers to the specific surface area of the entire negative electrode active material layer containing the negative electrode active material and additives (binder, conductive agent, thickener, filler, etc.). The weight of the negative electrode active material layer, that is, the total weight of the entire negative electrode active material layer containing the negative electrode active material and additives (binder, conductive agent, thickener, filler, etc.), was measured. The reaction area of the negative electrode active material layer was calculated from the following formula. Reaction area = specific surface area of negative electrode active material layer × weight of negative electrode active material layer
[0211] 8. Measurement method for capacity retention rate of lithium-ion batteries after cycling At 45°C, the lithium-ion battery was charged to 4.45V at 1C using a constant current method, then charged to 4.45V using a constant voltage method until the current reached 0.05C, and then discharged to 3.0V using a constant current method at 1C, which was the first cycle. Under the above conditions, the lithium-ion battery was cycled 200 times. "1C" refers to the current value at which the lithium-ion battery capacity was completely discharged within 1 hour. The capacity retention rate of the lithium-ion battery after cycling was calculated using the following formula. Capacity retention rate after cycling = (discharge capacity of corresponding cycle number / discharge capacity of first cycle) x 100%
[0212] 9. Measurement method for cycle expansion rate of lithium-ion batteries After leaving the lithium-ion battery at 25°C for 30 minutes, it was charged to 4.45V at a constant current rate of 0.5C, then charged to 0.05C at 4.45V at a constant voltage rate of 0.05C, left to stand for 5 minutes, and the thickness was measured. The cycle test was performed again, and the thickness of the battery was measured after 100 cycles. The thickness expansion rate of the lithium-ion battery after 100 cycles was calculated using the following formula. Cyclic thickness expansion rate = [(thickness after cycling - thickness before cycling) / thickness before cycling] x 100%
[0213] 3. Measurement results Table 1 shows the contact angle of the negative electrode active material layer with respect to the non-aqueous solvent, the porosity, and the auxiliary used, as well as the cycle characteristics of the lithium ion battery in each of the examples and comparative examples. Auxiliary used in the examples 1: 1000 ppm trisiloxane surfactant (CAS No. 3390-61-2; 28855-11-0).
[0214] [Table 1]
[0215] The results show that when the contact angle of the negative electrode active material layer to the non-aqueous solvent is 60° or less, the capacity retention rate and the cycle thickness expansion rate of the lithium ion battery after cycling can be significantly improved. When the contact angle of the negative electrode active material layer to the non-aqueous solvent is 60° or less, the capacity retention rate and the cycle thickness expansion rate of the lithium ion battery after cycling can be further improved by making the negative electrode active material layer have a porosity of 10% to 60%.
[0216] Table 2 shows the effect of the specific surface area (BET) and median diameter (D50) of carbon materials on the cycle characteristics of lithium-ion batteries. The examples in Table 2 are improvements based on Example 4, and the only differences between them are the parameters listed in Table 2.
[0217] [Table 2]
[0218] The results showed that the specific surface area (BET) of the carbon material was 5m 2 / g and / or the median diameter (D50) is in the range of 5 μm to 30 μm, the capacity retention rate after cycling and the cycle thickness expansion rate of the lithium ion battery are further improved.
[0219] Table 3 shows the effect of trace metals in the negative electrode active material layer on the cycle characteristics of a lithium-ion battery. The examples in Table 3 are improvements based on Example 4, and the only differences between them are the parameters listed in Table 3.
[0220] [Table 3]
[0221] The results show that when the negative electrode active material layer contains a trace metal element (eg, iron, molybdenum, or copper), the capacity retention rate and cycle thickness expansion rate of the lithium ion battery after cycling can be further improved.
[0222] The effect of the auxiliary agent on the cycle characteristics of the lithium ion battery is shown in Table 4. The only difference between Examples 21 to 25 and Example 4 in Table 4 is the type of auxiliary agent.
[0223] [Table 4]
[0224] As shown in Comparative Example 1, when no auxiliary agent is added, the capacity retention rate and cycle thickness swelling rate of the lithium ion battery after cycling are poor. As shown in Examples 4 and 21 to 25, the capacity retention rate and cycle thickness swelling rate of the lithium ion battery after cycling can be significantly improved by adding an auxiliary agent. When the oxidation potential of the auxiliary agent is 4.5V or more and the reduction potential is 0.5V or less, the capacity retention rate and cycle thickness swelling rate of the lithium ion battery after cycling are further improved. Compared to ethanol and acetone (as shown in Examples 24 and 25), nonionic surfactants (as shown in Examples 21 to 23) have a lower surface tension (30mN / m or less), so that the capacity retention rate and cycle thickness swelling rate of the lithium ion battery after cycling can be further improved.
[0225] Table 5 shows the EC content (Xmg) in the electrolyte and the reaction area (Ym2 ) shows the effect on the cycling characteristics of lithium-ion batteries. The examples in Table 5 are improvements based on Example 4, and the only differences between them are the parameters listed in Table 5.
[0226] [Table 5]
[0227] From the results, the EC content in the electrolyte (Xmg) and the reaction area of the negative electrode active material layer (Ym 2 ) satisfies 10≦(X / Y)≦100, the capacity retention rate and the cycle thickness expansion rate of the lithium ion battery are further improved.
[0228] Table 6 shows the effect of electrolyte components on the cycling performance of lithium-ion batteries. The examples in Table 6 are improvements based on Example 4, and the only differences between them are the compounds listed in Table 6 and their contents.
[0229] [Table 6]
[0230] The results show that when the negative electrode of the embodiment of the present invention is used, adding the compound represented by formula 1 to the electrolyte is advantageous for forming an SEI film on the surface of the electrode, improving the interface stability, and improving the capacity retention rate and cycle thickness expansion rate of the lithium ion battery after cycling. When the content of the compound represented by formula 1 is 0.001wt% to 10wt%, the capacity retention rate and cycle thickness expansion rate of the lithium ion battery after cycling are significantly improved.
[0231] Table 7 shows the effect of iron group metals in electrolyte on the cycling performance of lithium-ion batteries. The examples in the table are improvements based on Example 4, with the only differences being the iron group metals and their contents listed in Table 7.
[0232] [Table 7]
[0233] From the results, when the negative electrode of the embodiment of the present invention is used, the inclusion of a trace amount of iron group metal (e.g., cobalt and nickel) in the electrolyte is advantageous in improving the capacity retention rate and cycle thickness expansion rate of the lithium ion battery after cycling.
[0234] Throughout the specification, references to "in some embodiments," "in one embodiment," "another example," "example," "embodiment," or "examples" mean that at least one embodiment or example of the invention includes a particular feature, structure, material, or characteristic described in that embodiment or example. Thus, the appearances of, for example, "in some embodiments," "in an embodiment," "in another example," "in one example," "in a particular example," or "example" in various places throughout the specification do not necessarily refer to the same embodiment or example of the invention. Furthermore, particular features, structures, materials, or characteristics herein may be combined in any suitable manner in one or more embodiments or examples.
[0235] Although exemplary embodiments have been described and illustrated, those skilled in the art should understand that the above-described embodiments are not to be construed as limiting the present invention, and that modifications, substitutions, and alterations to the embodiments are possible without departing from the spirit, principle, and scope of the present invention.
Claims
1. A positive electrode, a negative electrode, and an electrolyte solution are included, The negative electrode includes a negative electrode active material layer, a contact angle of the negative electrode active material layer with respect to a non-aqueous solvent, as measured by a contact angle measurement method, is 60° or less; the negative electrode active material layer further contains at least one metal selected from the group consisting of molybdenum, iron, and copper, and the content of the at least one metal is 0.05 wt % or less based on the total weight of the negative electrode active material layer; the negative electrode active material layer further includes an auxiliary, and the content of the auxiliary is 2500 ppm or less based on the total weight of the negative electrode active material layer; The auxiliary is (a) an oxidation potential of 4.5 V or more and a reduction potential of 0.5 V or less; (b) the surface tension is 30 mN / m or less; (c) comprising a nonionic surfactant; At least one of the following characteristics is provided: The contact angle measurement method refers to dropping a 3 microliter droplet of diethyl carbonate on the surface of the negative electrode active material layer, and then measuring the contact angle of the droplet on the surface of the negative electrode active material layer within 100 seconds.
2. 2. The electrochemical device according to claim 1, wherein a droplet diameter of the non-aqueous solvent on the negative electrode active material layer, as measured by contact angle measurement, is 30 mm or less.
3. 2. The electrochemical device according to claim 1, wherein the porosity of the negative electrode active material layer is 10% to 60%.
4. The negative electrode active material layer contains a carbon material, (a) Specific surface area is 5 m 2 / g or less; (b) the median diameter is 5 μm to 30 μm; 13. The electrochemical device of claim 1, comprising at least one of the following features:
5. 10. The electrochemical device of claim 1, wherein the negative electrode active material layer comprises at least one of artificial graphite, natural graphite, mesocarbon microbeads, soft carbon, hard carbon, amorphous carbon, silicon-containing materials, tin-containing materials, and alloy materials.
6. 2. The electrochemical device of claim 1, wherein the co-agent comprises a non-ionic surfactant, the non-ionic surfactant comprising at least one of a polyoxyethylene ether, a polyol ester, an amide, and a block polyether.
7. The auxiliary comprises a nonionic surfactant, The nonionic surfactants include polyoxyethylene alkanolamides, polyoxyethylene octylphenol ethers, polyoxyethylene nonylphenol ethers, polyoxyethylene aliphatic higher alcohol ethers, polyoxyethylene fatty acid esters, polyoxyethylene amines, alkanolamides, polyoxyethylene lauryl ethers, polyoxyethylene primary alcohol ethers having 12 to 14 carbon atoms, polyoxyethylene secondary alcohol ethers having 12 to 14 carbon atoms, polyoxyethylene branched Guerbet alcohol ethers having 13 carbon atoms, and polyoxyethylene branched Guerbet alcohols having 10 carbon atoms. , polyoxyethylene linear alcohol ether having 10 carbon atoms, polyoxyethylene linear octyl alcohol ether having 8 carbon atoms, polyoxyethylene isooctyl alcohol ether having 8 carbon atoms, fatty acid monoglyceride, monoglyceride, sorbitan fatty acid, silicon-polyether complex, polysorbate, polyoxyethylene fatty acid ester, polyoxyethylene aliphatic alcohol ether, polyoxyethylene-polyoxypropylene block copolymer, polyether-modified trisiloxane, and polyether-modified silicon polyether siloxane. The electrochemical device of claim 1, comprising at least one of the following:
8. The electrolytic solution contains ethylene carbonate, and the content of the ethylene carbonate in the electrolytic solution is X mg and the reaction area of the negative electrode active material layer is Y m 2 The electrochemical device according to claim 1 , wherein the relational expression 10≦(X / Y)≦100 is satisfied.
9. The electrolyte solution further contains a compound represented by formula 1, 【Chemistry 1】 Formula 1 where R is a linear or branched alkyl group having 1 to 5 carbon atoms or -SiR 2 R 3 R 4 where R 2 , R 3 and R 4 are each independently an alkyl group having 1 to 5 carbon atoms, and R 1 is an alkylene group having 2 to 3 carbon atoms and substituted with the following substituents selected from at least one fluorine atom or an alkyl group containing at least one fluorine atom and having 1 to 3 carbon atoms:
10. In formula 1, R is -SiR 2 R 3 R 4 and R 1 is an alkylene group having 2 carbon atoms and substituted with the following substituents selected from at least one fluorine atom or an alkyl group containing at least one fluorine atom and having 1 to 3 carbon atoms:
11. 10. The electrochemical device according to claim 9, wherein the compound represented by formula 1 includes at least one of the compounds represented by formulas 1a to 1h. 【Chemistry 2】
12. 10. The electrochemical device according to claim 9, wherein the content of the compound represented by formula 1 is 0.001 wt % to 10 wt % based on the total weight of the electrolyte.
13. 2. The electrochemical device according to claim 1, wherein the electrolyte further contains an iron group element, the iron group element including cobalt, nickel, or a combination thereof, and the content of the iron group element is 0.05 wt % or less with respect to a total weight of the electrolyte.
14. An electronic device comprising an electrochemical device according to any one of claims 1 to 13.
Citation Information
Patent Citations
Nonaqueous electrolyte secondary battery
JP1998092436A
Manufacturing method of electrode plate for negative electrode of nonaqueous secondary battery
JP2006107896A
Aqueous paste for forming anode active material layer of nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery anode and manufacturing method thereof, and nonaqueous electrolyte secondary battery
JP2012038597A
Lithium ion secondary battery
JP2019175657A