Lead alloy rolled foil, positive electrode for lead-acid battery, lead-acid battery, and energy storage system
A lead alloy with controlled crystal grain boundaries in the positive electrode lead layer addresses intergranular corrosion, ensuring low internal resistance and enhanced battery capacity in lead-acid batteries.
Patent Information
- Application Number
- JP2022541516
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-08-05
- Filing Date
- 2021-07-30
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-07-30
AI Technical Summary
Conventional lead-acid batteries face issues with intergranular corrosion of the positive electrode lead layer, particularly when thinned, leading to increased internal resistance and potential liquid junctions between electrodes, which can degrade battery performance and render it unusable.
A lead alloy with specific compositions, including 0.4-2% tin and 0.004% bismuth, with controlled crystal grain boundaries, forms a positive electrode lead layer that suppresses intergranular corrosion, maintaining electrical conductivity and reducing thickness to enhance battery capacity.
The solution prevents corrosion penetration, maintains low internal resistance, and allows for a thinner positive electrode, thereby increasing battery capacity and reducing weight, making it suitable for compact and efficient power storage systems.
Smart Images

Figure 0007575462000002 
Figure 0007575462000003 
Figure 0007575462000004
Abstract
Description
[Technical field]
[0001] The present invention relates to Lead alloy rolled foil The present invention relates to a positive electrode for a lead-acid battery, a lead-acid battery, and an electricity storage system. [Background technology]
[0002] The positive electrode of a lead-acid battery includes a positive-electrode lead layer made of a lead alloy and an active material disposed on the surface of the positive-electrode lead layer. Conventional positive electrodes for lead-acid batteries (see, for example, Patent Document 1) have been made of well-known lead or lead alloy. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2013 / 073420 Summary of the Invention [Problem to be solved by the invention]
[0004] However, when a lead-acid battery is used, the positive lead layer gradually corrodes. At this time, the corrosion progresses along the grain boundaries of the crystal grains of the lead alloy used in the positive lead layer, and there is a risk that the corrosion penetrates the positive lead layer in the thickness direction. In particular, when the positive lead layer is made thin in order to reduce the weight of the battery, improve the utilization rate of the volume in the battery, reduce the amount of lead used, etc., this problem becomes more prominent. When such penetration occurs, the electrical conduction path is cut off, and the internal resistance of the battery increases, and there is a concern that the battery cannot exhibit the desired characteristics. In addition, for example, in a bipolar lead-acid battery, the formation of a through hole in the positive lead layer causes further corrosion of other components, and the electrolytes on the positive and negative sides flow into each other, a phenomenon known as a liquid junction, causing deterioration of the battery characteristics and, in the worst case, making the battery unusable.
[0005] Therefore, the present invention can suppress the progress of intergranular corrosion. Lead alloy rolled foilThe present invention aims to provide a lead layer for a positive electrode that is resistant to penetration in the thickness direction due to corrosion even when the thickness is reduced, a positive electrode for a lead-acid battery using the same, and a lead-acid battery and an electricity storage system that are constructed using the positive electrode for a lead-acid battery and that are resistant to an increase in internal resistance and can have a long life. [Means for solving the problem]
[0006] A lead alloy according to one embodiment of the present invention contains 0.4% by mass or more and 2% by mass or less of tin and 0.004% by mass or less of bismuth, with the remainder being lead and unavoidable impurities, and is characterized in that when a crystal orientation distribution map created by analyzing the surface using electron backscatter diffraction is subjected to image analysis to extract intersections between misorientation boundaries between crystal grains having a crystal orientation misorientation of 5° or more and a line extending in a specific direction, and the distance between two adjacent intersections extracted from the intersections is measured, the average value of the distance is 50 μm or less.
[0007] In another embodiment of the present invention, the lead alloy contains 0.4% by mass or more and 2% by mass or less of tin, 0.004% by mass or less of bismuth, 0.1% by mass or less of calcium, 0.1% by mass or less of silver, and the remainder is lead and unavoidable impurities, and is characterized in that, when a crystal orientation distribution map created by analyzing the surface by electron backscatter diffraction is image-analyzed to extract intersections between crystal grains with a crystal orientation difference of 5° or more and a straight line extending in a specific direction, and the distance between two adjacent intersections among the extracted intersections is measured, the average value of the distance is 50 μm or less. More preferably, the average value of the distance is 30 μm or less.
[0008] Furthermore, a positive electrode for a lead-acid battery according to yet another aspect of the present invention comprises a positive electrode lead layer formed from the lead alloy according to the one aspect or the other aspect, and an active material disposed on a surface of the positive electrode lead layer, and the positive electrode lead layer has a thickness of 0.5 mm or less. Furthermore, a lead-acid battery according to yet another aspect of the present invention includes the lead-acid battery positive electrode according to the yet another aspect. Furthermore, a power storage system according to yet another aspect of the present invention is an power storage system including the lead-acid battery according to the yet another aspect described above, for storing electricity in the lead-acid battery. Effect of the Invention
[0009] According to the present invention, even if the thickness is reduced, corrosion penetrating the positive electrode lead layer in the thickness direction is unlikely to occur. Lead alloy rolled foil , applicable Lead alloy rolled foil and a lead-acid battery and an electricity storage system that are configured using the lead-acid battery positive electrode and that are less susceptible to an increase in internal resistance. [Brief description of the drawings]
[0010] [Figure 1] 1 is a cross-sectional view illustrating a structure of a bipolar lead-acid battery which is one embodiment of the lead-acid battery according to the present invention. [Diagram 2] FIG. 1 is a diagram illustrating an embodiment of a power storage system according to the present invention. [Diagram 3] FIG. 2 is a diagram illustrating the size of crystal grains and corrosion in the lead alloy of the conventional example and the lead alloy of the present invention. [Figure 4] FIG. 1 is a diagram for explaining a method for performing image analysis of a crystal orientation distribution map created by analyzing the surface of a lead alloy by electron backscatter diffraction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] An embodiment of the present invention will be described. Note that the embodiment described below is merely an example of the present invention. In addition, various modifications and improvements can be made to this embodiment, and such modifications and improvements can also be included in the present invention. The structure of a lead-acid battery 1 according to one embodiment of the present invention will be described with reference to Fig. 1. The lead-acid battery 1 shown in Fig. 1 is a bipolar type lead-acid battery, and has a first plate unit in which a negative electrode 110 is fixed to a flat first plate 11, a second plate unit in which an electrolytic layer 105 is fixed to a frame-shaped second plate 12, a third plate unit in which a positive electrode 120, a substrate 111, and a negative electrode 110 are fixed in this order to a frame-shaped third plate 13, and a fourth plate unit in which the positive electrode 120 is fixed to a flat fourth plate 14, and has a structure that presents a substantially rectangular shape by combining them together.
[0012] A negative electrode terminal 107 is fixed to the first plate 11 in a state of being electrically connected to a negative electrode 110 fixed to the first plate 11 . A positive electrode terminal 108 is fixed to the fourth plate 14 in a state of electrical connection with a positive electrode 120 fixed to the fourth plate 14 . The second plate units and the third plate units can be provided alternately in any number of stages depending on the desired storage capacity. The first to fourth plates 11, 12, 13, and 14 and the substrate 111 are made of, for example, a known molding resin.
[0013] The electrolytic layer 105 is formed of a glass fiber mat or the like impregnated with an electrolyte such as sulfuric acid. The negative electrode 110 is composed of a negative electrode lead layer 102 made of, for example, well-known lead foil, and a negative electrode active material layer 104 . The positive electrode 120 is composed of a positive electrode lead layer 101 made of a foil of a lead alloy according to this embodiment, which will be described later, and a positive electrode active material layer 103 .
[0014] The positive electrode 120 and the negative electrode 110 are fixed to the front and back surfaces of the substrate 111, respectively, and are electrically connected by an appropriate method. Alternatively, the positive electrode 120 and the negative electrode 110 may be fixed to one surface of each of the two substrates 111, and the other surfaces may be electrically connected and fixed to each other. The plates 11 to 14 are fixed to each other in an appropriate manner so that the inside is sealed and the electrolyte does not leak out.
[0015] In the lead-acid battery 1 of this embodiment having such a configuration, a bipolar electrode 130, which is an electrode for a lead-acid battery, is configured by the substrate 111, the positive electrode lead layer 101, the positive electrode active material layer 103, the negative electrode lead layer 102, and the negative electrode active material layer 104. A bipolar electrode is an electrode that functions as both a positive electrode and a negative electrode in one sheet. The lead-acid battery 1 of this embodiment has a battery configuration in which the cells are connected in series by alternately stacking and assembling multiple cells each having an electrolytic layer 105 interposed between a positive electrode 120 having a positive electrode active material layer 103 and a negative electrode 110 having a negative electrode active material layer 104.
[0016] In this embodiment, a bipolar lead-acid battery having a bipolar electrode that functions as both a positive electrode and a negative electrode has been shown as an example of a lead-acid battery. However, the lead-acid battery of this embodiment may be a lead-acid battery having an electrode that functions as a positive electrode and an electrode that functions as a negative electrode, and in which the separate positive and negative electrodes are arranged alternately.
[0017] A power storage system can be configured using the lead-acid battery 1 of the present embodiment shown in Fig. 1. An example of the power storage system is shown in Fig. 2. The power storage system of Fig. 2 includes an assembled battery consisting of a plurality of (four in the example of Fig. 2) lead-acid batteries 1, 1, ... connected in series, an AC / DC converter 6 that performs AC / DC conversion (exchange between AC power and DC power) when the assembled battery is charged and discharged, a current sensor 3 that is installed between the assembled battery and the AC / DC converter 6 and measures a charge / discharge current when the assembled battery is charged and discharged, a voltage sensor 4 that measures the voltage of the assembled battery, a power storage state monitoring device 2 that receives measurement data transmitted from the current sensor 3 and the voltage sensor 4 and performs a state determination and an alarm determination of the assembled battery based on the received measurement data, and an energy management system 5 that receives power storage state information transmitted by the power storage state monitoring device 2 based on the results of the performed state determination and alarm determination, and determines whether to charge or discharge the assembled battery based on the received power storage state information.
[0018] The energy management system 5 determines whether to charge or discharge the battery pack based on the power storage state information received from the power storage state monitoring device 2, and transmits a signal to the AC / DC converter 6 commanding charging or discharging. When a signal commanding discharging is received, the AC / DC converter 6 converts the DC power discharged from the battery pack into AC power and outputs it to the commercial power system 7. On the other hand, when a signal commanding charging is received, the AC / DC converter 6 converts the AC power input from the commercial power system 7 into DC power and charges the battery pack. The number of lead-acid batteries 1 in series is determined by the input voltage range of the AC / DC converter 6.
[0019] <About the lead alloy constituting the positive electrode lead layer 101> In this embodiment, the thickness of the positive electrode lead layer 101 is set to 0.5 mm or less. In order to prevent the growth problem from occurring even with such a thickness, the positive electrode lead layer 101 is formed of a lead alloy that satisfies the following two conditions A and B.
[0020] (Condition A) A lead alloy containing 0.4% by mass or more and 2% by mass or less of tin (Sn) and 0.004% by mass or less of bismuth (Bi), with the balance being lead (Pb) and unavoidable impurities, or a lead alloy containing 0.4% by mass or more and 2% by mass or less of tin and 0.004% by mass or less of bismuth, as well as 0.1% by mass or less of calcium and 0.1% by mass or less of silver, with the balance being lead and unavoidable impurities.
[0021] (Condition B) When a crystal orientation distribution map is created by analyzing the surface of the lead alloy by electron backscatter diffraction, image analysis is performed to extract intersections between crystal grains with a crystal orientation difference of 5° or more and a straight line extending in a specific direction, and the distance between two adjacent intersections among the extracted intersections is measured, the average value of the distance is 50 μm or less. More preferably, the average value of the distance is 30 μm or less.
[0022] In the lead storage battery 1 and the power storage system of this embodiment, the positive electrode lead layer 101 is formed of the above-mentioned lead alloy, so that an increase in internal resistance is unlikely to occur. That is, since the positive electrode lead layer 101 is formed of the above-mentioned lead alloy, the progress of intergranular corrosion is suppressed and penetration in the thickness direction is unlikely to occur. This prevents the electrical conduction path from being cut off. Therefore, when used as a battery, it is possible to achieve the effect of preventing an increase in internal resistance. This will be described in more detail below.
[0023] [Regarding condition A] When the lead alloy contains tin, the adhesion between the positive electrode lead layer 101 and the positive electrode active material layer 103 formed of the lead alloy is improved. When the lead alloy contains calcium, the crystal grains of the lead alloy become fine. When the lead alloy contains silver, the crystal grains of the lead alloy become fine. Therefore, when the lead alloy contains tin and at least one of calcium and silver, the crystal grains of the lead alloy become small, making it difficult for the electrolyte to penetrate, and thus the progress of grain boundary corrosion can be effectively suppressed.
[0024] The tin content is more preferably 0.7% by mass or more, further preferably 1.0% by mass or more, particularly preferably 1.3% by mass or more, and most preferably 1.6% by mass or more. If the tin content is within this range, misorientation boundaries are easily formed in the lead alloy. In order to further suppress the occurrence of corrosion penetrating the positive electrode lead layer in the thickness direction, the calcium content is more preferably 0.07 mass % or less, even more preferably 0.04 mass % or less, and particularly preferably 0.02 mass % or less.
[0025] The silver content is more preferably 0.03 mass % or less in order to suppress separation of the silver phase and improve the corrosion resistance of the lead alloy. Although calcium and silver may be actively added to lead alloys, they may also be included as unavoidable impurities due to inclusion from the base metal, etc. The maximum amount that can be included as an unavoidable impurity is 0.012 mass% for both calcium and silver.
[0026] On the other hand, when the lead alloy contains bismuth, the formability of the lead alloy by rolling or the like tends to decrease. That is, bismuth is one of the impurities that is preferably not contained in the lead alloy of this embodiment as much as possible. Therefore, the bismuth content in the lead alloy needs to be 0.004 mass% or less, and is most preferably 0 mass%. However, considering the cost of the lead alloy, the bismuth content is preferably 0.0004 mass% or more.
[0027] On the other hand, lead alloys may contain elements other than lead, tin, calcium, silver, and bismuth. These elements are impurities inevitably contained in lead alloys, and the total content of elements other than lead, tin, calcium, silver, and bismuth in the lead alloy is preferably 0.01% by mass or less, and most preferably 0% by mass.
[0028] As described above, the lead alloy of the present embodiment forming the positive electrode lead layer 101 is a lead alloy containing 0.4% by mass or more and 2% by mass or less of tin and 0.004% by mass or less of bismuth, with the balance being lead and unavoidable impurities, or a lead alloy containing 0.4% by mass or more and 2% by mass or less of tin and 0.004% by mass or less of bismuth, and further containing at least one of 0.1% by mass or less of calcium and 0.1% by mass or less of silver, with the balance being lead and unavoidable impurities. The lead alloy of the present embodiment preferably does not contain bismuth as an impurity, but if it does contain bismuth, its content must be 0.004% by mass or less. In addition, if the lead alloy of the present embodiment contains elements other than lead, tin, calcium, silver, and bismuth as unavoidable impurities, the total content is preferably 0.01% by mass or less.
[0029] [Regarding condition B] In general metals, lattice defects are introduced by deformation, and the introduced lattice defects are rearranged to form misorientation boundaries. On the other hand, in lead and lead alloys, lattice defects have low thermal stability and do not accumulate, so recrystallization occurs at room temperature to generate coarse crystal grains. Therefore, conventional rolled foils of lead alloys (foils produced by rolling lead alloys) have coarse crystal grains, as shown in the column of the conventional example before the corrosion resistance test in Figure 3. Therefore, when the rolled foil corrodes, the grain boundaries of the coarse crystal grains in the lead alloy corrode, and corrosion that penetrates the rolled foil in the thickness direction (left and right direction on the paper in Figure 3) is likely to occur (see the column of the conventional example after the corrosion resistance test in Figure 3).
[0030] Therefore, when the thickness of the positive lead layer formed of a conventional lead alloy is thinned to increase the amount of active material on the surface, the grain boundaries of the coarse crystal grains corrode when the positive lead layer corrodes, and the corrosion easily penetrates the positive lead layer in the thickness direction. As a result, there is a risk of the internal resistance of the lead-acid battery increasing. In addition, there is a risk of the liquid junction between the positive and negative electrodes.
[0031] As a result of the inventors' research, it was found that by extracting the intersections between misorientation boundaries between crystal grains having a crystal orientation difference of 5° or more and a straight line extending in a specific direction, and measuring the distance between two adjacent ones of the extracted intersections, the progression of such corrosion can be suppressed and penetration can be prevented by making the average value of said distances 50 μm or less. In other words, since lattice defects are dense at grain boundaries between particles with a crystal orientation difference of 5° or more, it is thought that less noble elements such as Sn tend to concentrate there and become corrosion initiation sites. Therefore, conversely, if multiple corrosion initiation sites are created, the concentration of less noble elements at each corrosion initiation site can be kept low, and the progress of corrosion from each corrosion initiation site can be suppressed.
[0032] As a result of thorough investigation based on this assumption, it was found that the progression of corrosion can be suppressed by extracting the intersections between misorientation boundaries between crystal grains where the crystal orientation difference is 5° or more and a straight line extending in a specific direction, and measuring the distance between two adjacent ones of the extracted intersections, and keeping the average value of this distance to 50 μm or less.
[0033] As described above, the lead alloy of this embodiment has fine crystal grains, for example, with a grain size of 0.1 μm to 50 μm, due to the alloy composition and manufacturing method (see the diagram shown in the column before the corrosion resistance test of the example of the present invention in FIG. 3), so that even if the rolled foil of the lead alloy of this embodiment corrodes and the grain boundaries of the crystal grains corrode, corrosion penetrating the rolled foil in the thickness direction is unlikely to occur (see the diagram shown in the column after the corrosion resistance test of the example of the present invention in FIG. 3). Therefore, if the positive electrode lead layer of the positive electrode of a lead-acid battery is formed from the lead alloy of this embodiment, a lead-acid battery in which the internal resistance is unlikely to increase can be obtained.
[0034] In addition, if the lead alloy of this embodiment is used to form the positive electrode lead layer 101 of the positive electrode of a lead storage battery, even if the thickness of the positive electrode lead layer is thin, corrosion penetrating the positive electrode lead layer in the thickness direction is unlikely to occur. Therefore, if the lead alloy of this embodiment is used to form the positive electrode lead layer, the thickness of the positive electrode lead layer can be reduced to 0.5 mm or less, and the battery capacity can be increased accordingly. For example, if a positive electrode is conventionally constructed by applying an active material of 1 mm thickness to a positive electrode lead layer of 1 mm thickness, if a positive electrode is constructed by applying an active material of 1.8 mm thickness to a positive electrode lead layer of 0.2 mm thickness, the amount of active material increases by 1.8 times, and the battery capacity can be increased by about 1.8 times compared to the conventional case with the same positive electrode thickness.
[0035] Furthermore, if the lead-acid battery is a bipolar lead-acid battery, the bipolar lead-acid battery has a low internal resistance and can therefore be used at a higher C-rate than a conventional lead-acid battery with a high internal resistance. This allows the size of the lead-acid battery to be reduced. If the size of the lead-acid battery is small, the size of the container can be reduced when it is used as an industrial battery. This is particularly advantageous when the lead-acid battery is buried underground. In addition, when it is used in mobility such as automobiles, the weight of the automobile can be reduced, leading to improved fuel efficiency and reducing the space required for mounting the lead-acid battery in the automobile.
[0036] Furthermore, since the positive electrode lead layer can be made thinner, the lead storage battery can be made lighter, which makes it easier to install the lead storage battery. If the thickness of the positive electrode lead layer 101 is 0.37 mm or less, more preferably 0.25 mm or less, the effect of the present invention that the internal resistance is less likely to increase can be more easily achieved.
[0037] The average grain size of the crystal grains in the lead alloy, i.e., the average spacing of the orientation difference boundaries between the crystal grains, can be evaluated by image analysis of a crystal orientation distribution map created by analyzing the surface of the lead alloy by electron backscatter diffraction. The method for evaluating the average grain size of the crystal grains in the lead alloy will be described with reference to FIG. 4, taking as an example a case where the rolled surface of a rolled foil produced by rolling a lead alloy is analyzed by electron backscatter diffraction. In FIG. 4, RD means the rolling direction of the rolled foil, and TD means the direction perpendicular to the rolling (width direction) of the rolled foil.
[0038] First, the rolled surface of the rolled foil produced by rolling a lead alloy is analyzed by electron backscatter diffraction to create a crystal orientation distribution map as shown in Figure 4. Figure 4 is a black and white image, in which crystal grains with different crystal orientations are displayed in different shades of gray (grayscale), and misorientation boundaries are shown between crystal grains with a crystal orientation difference of 5° or more.
[0039] Next, the crystal orientation distribution map is subjected to image analysis. In this image analysis, a straight line extending in a specific direction (hereinafter, sometimes referred to as a "specific straight line") is set on the crystal orientation distribution map, and the intersection points between the specific straight line and the misorientation boundary between crystal grains with a crystal orientation difference of 5° or more are extracted. The intersection points are extracted for one or more specific straight lines, and the distance between two adjacent intersection points on the same specific straight line among the extracted intersection points is measured. Then, the average value of the measured distances is calculated. Since a large number of intersection points are usually extracted, there are many combinations of two adjacent intersection points, but the average value may be calculated using all combinations, or the average value may be calculated using some combinations.
[0040] The direction in which the specific straight line extends is not particularly limited, and may be set in advance to a desired direction during image analysis. For example, the direction may be the same as the rolling direction of the rolled foil, or may be the same as the direction perpendicular to the rolling direction of the rolled foil. In the example of FIG. 4, the direction in which the specific straight line extends and the rolling direction of the rolled foil are the same. That is, the straight line extending in the rolling direction at approximately the center in the vertical direction of the paper surface of FIG. 4 is the specific straight line. In addition, when performing image analysis using multiple specific straight lines, the directions in which all the specific straight lines extend are the same.
[0041] In the example of Fig. 4, the number of intersections between the specific straight line and the misorientation boundary between crystal grains with a crystal orientation misorientation of 5° or more is 13. Short horizontal lines (short lines extending in the direction perpendicular to the rolling direction) perpendicular to the specific straight line indicate the positions of the intersections between the specific straight line and the misorientation boundary. Therefore, in the example of Fig. 4, there are 12 pairs of combinations of two adjacent intersections on the specific straight line, and the distances between the two intersections for these 12 pairs are measured and their average value is calculated.
[0042] The average value of the distance calculated as above is the average value of the interval between the orientation difference boundaries between the crystal grains, so that the average grain size of the crystal grains of the lead alloy can be evaluated by this. That is, when the average value of the distance is small, it means that the average grain size of the crystal grains of the lead alloy is small, and when the average value of the distance is large, it means that the average grain size of the crystal grains of the lead alloy is large.
[0043] If the average value of the distance is 50 μm or less, the average grain size of the crystal grains of the lead alloy forming the rolled foil is small, so that corrosion penetrating the rolled foil in the thickness direction is unlikely to occur. Therefore, if the positive electrode lead layer of the lead-acid battery electrode is formed from such a rolled foil, the internal resistance of the lead-acid battery is unlikely to increase. The average value of the distance must be 50 μm or less, but is preferably 30 μm or less, and more preferably 20 μm or less.
[0044] The average value of the distance may be, for example, about 20 μm immediately after the production of the rolled foil, but may gradually decrease to, for example, 50 μm, since recrystallization of crystal grains may occur during use of the lead-acid battery. When the lead-acid battery is used in a high-temperature environment, recrystallization is likely to occur, and the average value of the distance is likely to be large.
[0045] [Method for refining crystal grains of lead alloys] Hereinafter, a method of refining crystal grains by rolling will be described as an example of a method of refining crystal grains in the lead alloy of this embodiment (a method of reducing the average value of the above distances). Lattice defects such as dislocations introduced by rolling are rearranged to form low-angle misorientation boundaries. Therefore, a certain amount of strain is required in rolling, so the reduction during rolling is preferably more than 5%, more preferably 10% or more, and even more preferably 20% or more.
[0046] However, if the rolling reduction is too high, the density of lattice defects becomes too high, which may cause thermal instability and recrystallization. In addition, the surface roughness of the lead alloy after rolling may become rough. Therefore, the rolling reduction is preferably 99% or less, more preferably 90% or less, and even more preferably 70% or less. In order to further actively refine the crystal grains of the lead alloy, it is preferable to subject the lead alloy to a heat treatment (intermediate heat treatment) at 300°C or higher before rolling to homogenize the solute elements. In addition, the rolling and intermediate heat treatment may each be repeated multiple times, and in this case, it is preferable to perform the intermediate heat treatment at 300°C or higher two or more times.
[0047] [Example] The present invention will be described in more detail below with reference to examples and comparative examples. An alloy plate made of a lead alloy having the alloy composition shown in Table 1 was manufactured by melting and casting. This alloy plate was subjected to heat treatment and rolling to produce a rolled foil. The detailed manufacturing method is as follows.
[0048] In Examples 1 to 7, an alloy plate having a thickness of 1 mm was rolled at a reduction rate of 70% to obtain a thickness of 0.3 mm. Next, the rolled foil having a thickness of 0.3 mm was subjected to an intermediate heat treatment at a temperature of 315°C for 30 minutes, and then further rolled at a reduction rate of 50% to obtain a rolled foil having a thickness of 0.15 mm.
[0049] For Examples 8 to 10, an alloy plate having a thickness of 2 mm was subjected to an intermediate heat treatment (first intermediate heat treatment) at a temperature of 315°C for 30 min, and then rolled at a reduction rate of 55% to a thickness of 0.9 mm. Next, the rolled plate having a thickness of 0.9 mm was subjected to an intermediate heat treatment (second intermediate heat treatment) at a temperature of 315°C for 30 min, and then further rolled at a reduction rate of 50% to obtain a rolled foil having a thickness of 0.45 mm.
[0050] For Example 11, an alloy plate having a thickness of 4 mm was subjected to an intermediate heat treatment (first intermediate heat treatment) at a temperature of 315°C for 30 min, and then rolled at a rolling reduction of 25% to a thickness of 3 mm. Next, the rolled plate having a thickness of 3 mm was subjected to an intermediate heat treatment (second intermediate heat treatment) at a temperature of 315°C for 30 min, and then further rolled at a rolling reduction of 95% to obtain a rolled foil having a thickness of 0.15 mm.
[0051] For Example 12, an alloy plate having a thickness of 2 mm was subjected to an intermediate heat treatment (first intermediate heat treatment) at a temperature of 315°C for 30 min, and then rolled at a rolling reduction of 50% to a thickness of 1 mm. Next, the rolled plate having a thickness of 1 mm was subjected to an intermediate heat treatment (second intermediate heat treatment) at a temperature of 315°C for 30 min, and then further rolled at a rolling reduction of 85% to obtain a rolled foil having a thickness of 0.15 mm.
[0052] In Example 13, an alloy plate having a thickness of 1 mm was subjected to an intermediate heat treatment (first intermediate heat treatment) at a temperature of 315°C for 30 min, and then rolled at a rolling reduction of 40% to a thickness of 0.6 mm. Next, the rolled plate having a thickness of 0.6 mm was subjected to an intermediate heat treatment (second intermediate heat treatment) at a temperature of 315°C for 30 min, and then further rolled at a rolling reduction of 75% to obtain a rolled foil having a thickness of 0.15 mm.
[0053] For Example 14, an alloy plate having a thickness of 0.4 mm was subjected to an intermediate heat treatment (first intermediate heat treatment) at a temperature of 315° C. for 30 min, and then rolled at a reduction rate of 50% to a thickness of 0.2 mm. Next, the rolled plate having a thickness of 0.2 mm was subjected to an intermediate heat treatment (second intermediate heat treatment) at a temperature of 315° C. for 30 min, and then further rolled at a reduction rate of 25% to obtain a rolled foil having a thickness of 0.15 mm.
[0054] For Example 15, an alloy plate having a thickness of 0.4 mm was subjected to intermediate heat treatment (first intermediate heat treatment) at a temperature of 315° C. for 30 min, and then rolled at a reduction rate of 55% to a thickness of 0.18 mm. Next, the rolled plate having a thickness of 0.18 mm was subjected to intermediate heat treatment (second intermediate heat treatment) at a temperature of 315° C. for 30 min, and then further rolled at a reduction rate of 17% to obtain a rolled foil having a thickness of 0.15 mm.
[0055] In addition, for Comparative Examples 1 to 4, rolled foils were manufactured according to a conventional manufacturing method. That is, a 1 mm thick alloy plate was rolled at a rolling reduction rate of 5% in one pass to obtain a thickness of 0.15 mm. Next, the rolled foil with a thickness of 0.15 mm was subjected to a heat treatment at a temperature of 315°C for 30 min and an aging heat treatment at a temperature of 60°C for 30 min in the order described, to obtain a rolled foil. For Comparative Example 4, a defect called edge cracking occurred at the end of the plate during rolling, so that a rolled foil could not be manufactured.
[0056] For Comparative Examples 5 to 8, rolled foils were produced according to a method with low processing costs among conventional manufacturing methods. That is, a 1 mm thick alloy plate was rolled at a rolling reduction rate of 5% in one pass to obtain a rolled foil with a thickness of 0.15 mm. For Comparative Examples 5 to 8, no heat treatment was performed. For Comparative Example 5, a defect called edge cracking occurred at the end of the plate during rolling, so that rolled foil could not be produced.
[0057] [Table 1]
[0058] Next, the surface (rolled surface) of each of the rolled foils of Examples 1 to 15 and Comparative Examples 1 to 3 and 6 to 8 was analyzed by electron backscatter diffraction, and a crystal orientation distribution map was created from the results. Next, the crystal orientation distribution map was subjected to the same image analysis as described above. Then, the intersection points between the orientation difference boundaries between crystal grains with a crystal orientation difference of 5° or more and the specific straight line were extracted, and the distance between two adjacent intersection points on the same specific straight line among the extracted intersection points was measured. The extension direction of the specific straight line was the same as the rolling direction. In addition, the total length of the specific straight lines used to extract the intersection points was 10 mm. Next, the average value (unit: μm) of all the measured distances was calculated. This average value of the distances means the average value of the spacing between the misorientation boundaries between the crystal grains. The calculation results of the average spacing between the misorientation boundaries between the crystal grains are shown in Table 1.
[0059] Next, bipolar electrodes for bipolar lead-acid batteries were prepared using the rolled foils of Examples 1 to 15 and Comparative Examples 1 to 3 and 6 to 8 as positive electrode lead layers. Then, bipolar lead-acid batteries were manufactured using the electrodes. The structures of the electrodes and bipolar lead-acid batteries were almost the same as those shown in FIG. 1. The active material forming the positive electrode active material layer was lead dioxide, and the thickness of the positive electrode active material layer was 1.8 mm. The active material forming the negative electrode active material layer was lead, and the thickness of the negative electrode active material layer was 1.8 mm.
[0060] A charge-discharge cycle test was conducted on the manufactured bipolar lead-acid battery by repeatedly charging and discharging. The charge-discharge C rate was 0.2C, and the number of charge-discharge cycles was 1000. If the internal resistance measured after the charge-discharge cycle test was 120% or less of the initial internal resistance measured before the charge-discharge cycle test, the battery was determined to be one in which the internal resistance is unlikely to increase, and was marked as "OK" in Table 1. If the internal resistance exceeded 120%, the battery was determined to be one in which the internal resistance is likely to increase, and was marked as "NG" in Table 1.
[0061] From the results shown in Table 1, it is found that the lead-acid batteries of Examples 1 to 15 are lead-acid batteries in which the internal resistance is unlikely to increase because the average value of the distance is 50 μm or less. In contrast, the lead-acid batteries of Comparative Examples 1 to 3 and 6 to 8 are lead-acid batteries in which the internal resistance is likely to increase because the average value of the distance exceeds 50 μm. [Explanation of symbols]
[0062] 1...lead acid battery 101...Lead layer for positive electrode 102...Lead layer for negative electrode 103...Active material layer for positive electrode 104...Active material layer for negative electrode 105...electrolytic layer 111... Substrate
Claims
1. A rolled foil of a lead alloy containing 0.4% by mass or more and 2% by mass or less of tin and 0.004% by mass or less of bismuth, with the remainder being lead and unavoidable impurities, A crystal orientation distribution map prepared by analyzing a rolled surface by an electron backscatter diffraction method is subjected to image analysis to extract intersections between orientation mismatch boundaries between crystal grains having a crystal orientation mismatch of 5° or more and a straight line extending in a specific direction, and when the distance between two adjacent ones of the extracted intersections is measured, the average value of the distance is 50 μm or less; The misorientation boundaries are formed by rearrangement of lattice defects in the lead alloy rolled foil.
2. A rolled foil of a lead alloy containing 0.4% by mass or more and 2% by mass or less of tin, 0.004% by mass or less of bismuth, 0.1% by mass or less of calcium, 0.1% by mass or less of silver, or both, with the remainder being lead and unavoidable impurities, A crystal orientation distribution map prepared by analyzing a rolled surface by an electron backscatter diffraction method is subjected to image analysis to extract intersections between orientation mismatch boundaries between crystal grains having a crystal orientation mismatch of 5° or more and a straight line extending in a specific direction, and when the distance between two adjacent ones of the extracted intersections is measured, the average value of the distance is 50 μm or less; the misorientation boundary is formed by rearrangement of lattice defects, The thickness of the rolled foil is 0.37 mm or less.
3. The lead alloy rolled foil according to claim 1 or 2, wherein the bismuth content is 0.0004 mass% or more and 0.004 mass% or less.
4. The lead alloy rolled foil according to any one of claims 1 to 3, wherein the average value of the distance is 30 µm or less.
5. A positive electrode for a lead-acid battery, comprising: a positive electrode lead layer formed of the rolled lead alloy foil according to any one of claims 1 to 4; and an active material disposed on a surface of the positive electrode lead layer, wherein the thickness of the positive electrode lead layer is 0.37 mm or less.
6. 6. The positive electrode for a lead-acid battery according to claim 5, which is for a bipolar lead-acid battery.
7. A lead-acid battery comprising the lead-acid battery positive electrode according to claim 5 or 6.
8. An electricity storage system comprising the lead-acid battery according to claim 7, for storing electricity in the lead-acid battery.
Citation Information
Patent Citations
Lead storage battery
JP2008210698A
Method for manufacturing positive electrode lattice substrate
JP2014207087A
Improved battery and assembly method
JP2014507774A
Method of manufacturing positive electrode lattice body for lead storage battery, positive electrode lattice body for storage battery, and lead storage battery
JP2019067522A
Lead storage battery
WO2013073420A1