Core-shell structured porous carbon material, its manufacturing method, sulfur-carbon composite containing same, and lithium secondary battery

A core-shell structured porous carbon material with laminated carbon sheets addresses the elution of lithium polysulfide, enhancing the capacity and stability of lithium-sulfur batteries by facilitating lithium ion transport and suppressing polysulfide loss.

JP7575467B2Active Publication Date: 2024-10-29LG ENERGY SOLUTION LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2022547749
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-23
Filing Date
2021-10-21
Publication Date
2024-10-29
Estimated Expiration
2041-10-21

AI Technical Summary

Technical Problem

Existing lithium-sulfur secondary batteries face challenges in maintaining high energy density and stability due to the elution of lithium polysulfide, which affects reactivity and lifetime characteristics, despite efforts to improve conductivity and suppress elution through carbon materials and graphene composites.

Method used

A porous carbon material with a core-shell structure is developed, comprising laminated carbon sheets for easy lithium ion entry and exit, and a shell to suppress lithium polysulfide elution, produced using a carbon precursor, basic zinc carbonate as a template, and heat treatment to form a core-shell structure.

Benefits of technology

The core-shell structure effectively suppresses lithium polysulfide elution, enhancing the capacity, charge/discharge, and life characteristics of lithium ion batteries, improving the performance of lithium-sulfur secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575467000003
    Figure 0007575467000003
  • Figure 0007575467000004
    Figure 0007575467000004
  • Figure 0007575467000005
    Figure 0007575467000005
Patent Text Reader

Abstract

The present invention provides a core-shell porous carbon material including a core having a structure in which carbon sheets are laminated and a shell containing carbon surrounding the core, a method for producing the same, a sulfur-carbon composite including the same, and a lithium secondary battery including the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0138507 filed on October 23, 2020, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.

[0002] The present invention relates to a core-shell porous carbon material, a method for producing the same, a sulfur-carbon composite containing the same, and a lithium secondary battery. [Background technology]

[0003] The application of secondary batteries is expanding to electric vehicles (EVs) and energy storage systems (ESSs), and as a result, lithium-sulfur secondary batteries, which theoretically realize an energy storage density (~2,600Wh / kg) compared to their high weight, are attracting attention as a next-generation secondary battery technology.

[0004] Lithium-sulfur secondary batteries are battery systems that use sulfur-based materials with sulfur-sulfur bonds as the positive electrode active material and lithium metal as the negative electrode active material. Sulfur, the main material of the positive electrode active material in such lithium-sulfur secondary batteries, has the advantages of being abundant worldwide, non-toxic, and having a low weight per unit atom.

[0005] When a lithium-sulfur secondary battery is discharged, lithium, the negative electrode active material, gives up electrons and is oxidized while being ionized, and the positive electrode active material, a sulfur-based material, receives electrons and is reduced. The lithium oxidation reaction is the process in which lithium metal gives up electrons and is converted into lithium cations. The sulfur reduction reaction is the process in which a sulfur-sulfur bond receives two electrons and is converted into sulfur anions. The lithium cations produced by the lithium oxidation reaction are transferred to the positive electrode through the electrolyte and combine with the sulfur anions produced by the sulfur reduction reaction to form a salt. Specifically, sulfur before discharge has a ring-shaped S8 structure, which is converted into lithium polysulfide (Li2S) by a reduction reaction. x , x = 8, 6, 4, 2), and if such lithium polysulfides are completely reduced, lithium sulfide (LiS) is ultimately produced.

[0006] Sulfur, which is a positive electrode active material, has low electrical conductivity and is therefore difficult to react with electrons and lithium ions in a solid-state form. In order to improve the reactivity of sulfur, existing lithium-sulfur secondary batteries use Li2S x The reactivity is improved by generating intermediate polysulfide of the lithium polysulfide type and inducing a liquid-state reaction. In this case, ether solvents such as dioxolane and dimethoxyethane, which have high solubility in lithium polysulfide, are used as the electrolyte solvent. In addition, in order to improve the reactivity, a catholyte type lithium-sulfur secondary battery system is constructed in the existing lithium-sulfur secondary battery. In this case, due to the characteristics of lithium polysulfide that easily dissolves in the electrolyte, the reactivity and life characteristics of sulfur are affected by the content of the electrolyte. In addition, in order to build a high energy density, a low content of electrolyte must be injected, but as the content of the electrolyte decreases, the concentration of lithium polysulfide in the electrolyte increases, making it difficult to operate the battery normally due to the decrease in the fluidity of the active material and the increase in side reactions.

[0007] Since the elution of lithium polysulfide has a detrimental effect on the capacity and life characteristics of a battery, various techniques have been proposed to suppress the elution of lithium polysulfide.

[0008] For example, Patent Document 1 discloses that the use of a three-dimensional carbon nanotube aggregate coated with graphene as a carbon material can prevent lithium polysulfide from dissolving out and improve the electrical conductivity of a sulfur-carbon nanotube composite.

[0009] In addition, Patent Document 2 discloses that a graphene composite containing sulfur, which is manufactured by treating graphene with hydrofluoric acid to form pores on the graphene surface and growing sulfur particles in the pores, can be used as a positive electrode active material to suppress lithium polysulfide elution and minimize the capacity reduction of a battery.

[0010] The above patents have improved the performance degradation problem of lithium-sulfur secondary batteries to some extent by preventing the elution of lithium polysulfide by changing the structure or material of the sulfur-carbon composite used in the positive electrode active material, but the effect is not sufficient. Therefore, in order to construct a high energy density lithium-sulfur secondary battery, a battery system capable of driving electrodes with high loading and low porosity is required, and research into such a battery system is being continuously conducted in the relevant technical field. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] Korean Patent Publication No. 10-2016-0037084 [Patent Document 2] Korean Patent No. 1379716 Summary of the Invention [Problem to be solved by the invention]

[0012] The present invention aims to provide a core-shell structured porous carbon material having a core part in which carbon sheets are laminated to allow easy ingress and egress of lithium ions and a shell part that suppresses the elution of lithium polysulfide.

[0013] Another object of the present invention is to provide a method for preparing the core-shell porous carbon material, a sulfur-carbon composite including the core-shell porous carbon material, and a lithium secondary battery including the same. [Means for solving the problem]

[0014] In order to achieve the above object, the present invention provides A porous carbon material having a core-shell structure is provided, which includes a core having a structure in which carbon sheets are laminated, and a shell containing carbon surrounding the core.

[0015] The present invention also provides a method for producing a semiconductor device comprising the steps of: a) mixing a carbon precursor having a melting point of 130 to 350°C with one or more particles selected from basic zinc carbonazate (BZC), zinc(II) metal-organic frameworks, and porous ZnO as a template; b) heating the mixture at 120 to 350° C. to allow the carbon precursor to infiltrate into the mold; c) heating the structure infiltrated with the carbon precursor inside the template at 600 to 900° C. to remove the template, forming a core-shell structure; and d) heating the core-shell structure at 800 to 1500° C. to vaporize and remove zinc impurities.

[0016] The present invention also provides a method for producing a semiconductor device comprising the steps of: A sulfur-carbon composite containing the core-shell structured porous carbon material and a sulfur component is provided.

[0017] The present invention also provides a method for producing a semiconductor device comprising the steps of: A lithium secondary battery including the sulfur-carbon composite is provided. Effect of the Invention

[0018] The core-shell porous carbon material of the present invention is composed of a core portion in which carbon sheets are laminated to facilitate the inflow and outflow of lithium ions, and a shell portion that inhibits the elution of lithium polysulfide. This allows the inflow and outflow of lithium ions to be facilitated and effectively inhibits the elution of lithium polysulfide, thereby providing the effect of significantly improving the capacity, charge / discharge, and life characteristics of lithium ion batteries.

[0019] In addition, the sulfur-carbon composite of the present invention contains the carbon material, and thus can significantly improve the capacity, charge-discharge, and life characteristics of a lithium-ion battery. A lithium-sulfur battery containing the sulfur-carbon composite can also significantly improve the capacity, charge-discharge, and life characteristics.

[0020] In addition, the method for producing a porous carbon material having a core-shell structure according to the present invention provides a method for efficiently producing the porous carbon material having a core-shell structure. [Brief description of the drawings]

[0021] [Figure 1] 1 shows a scanning electron microscope (SEM) photograph of the structure of a core-shell porous carbon material of the present invention. [Diagram 2] 1 shows a scanning electron microscope (SEM) photograph of the structure of a conventional porous carbon material. [Diagram 3] 1 shows a scanning electron microscope (SEM) photograph and an energy dispersive spectroscopy (EDS) element mapping photograph of the sulfur-carbon composite produced in Example 8 of the present invention. [Figure 4] 1 shows a scanning electron microscope (SEM) photograph and an energy dispersive spectroscopy (EDS) element mapping photograph of the conventional sulfur-carbon composite produced in Comparative Example 2. [Diagram 5] 1 is a graph showing the specific surface area of ​​a core-shell porous carbon material prepared in Example 1 of the present invention. [Figure 6] 1 is a graph showing the life characteristics of lithium-sulfur batteries prepared in Example 9 of the present invention and Comparative Example 3. [Figure 7] 1 is a graph showing discharge capacity versus voltage for lithium-sulfur batteries prepared in Example 9 and Comparative Example 3 of the present invention. [Figure 8] 1 is a diagram illustrating a method for producing a core-shell porous carbon material according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The present invention will be described in detail below.

[0023] The present invention relates to a porous carbon material having a core-shell structure, which includes a core having a structure in which carbon sheets are laminated, and a shell containing carbon surrounding the core.

[0024] The core-shell porous carbon material of the present invention is characterized by being composed of a core portion in which carbon sheets are laminated to facilitate the ingress and egress of lithium ions and a shell portion that inhibits the elution of lithium polysulfide, thereby facilitating the ingress and egress of lithium ions and effectively inhibiting the elution of lithium polysulfide.

[0025] In one embodiment of the present invention, the carbon sheet is a graphene sheet.

[0026] In one embodiment of the present invention, the structure in which the carbon sheets are laminated is a hierarchical porous structure.

[0027] In one embodiment of the present invention, the porous carbon material has a specific surface area of ​​300 m 2 / g to 2000m 2 / g.

[0028] The core-shell porous carbon material contains variable pores therein, the average diameter of the pores being in the range of 1 to 1000 nm, and the porosity or void ratio being in the range of 10 to 90% of the total volume of the porous carbon material.

[0029] In one embodiment of the present invention, the core-shell structure is formed by infiltrating a carbon precursor having a melting point of 130 to 350°C into one or more template particles selected from basic zinc carbonazate (BZC), zinc(II) metal-organic frameworks, and porous ZnO, followed by heat treatment.

[0030] If the melting point of the carbon precursor is less than 130°C, it is not preferable because the carbon precursor is in a solid phase and cannot be injected into the mold shape, and if it exceeds 350°C, it is not preferable because a decomposition reaction will proceed before the carbon precursor can be injected into the mold shape.

[0031] The carbon precursor is one or more selected from glucose, sucrose, lactose, fructose, starch, tannic acid, and the like.

[0032] The heat-treated carbon precursor forms a core comprising a laminated structure of carbon sheets, and the heat-treated template forms a shell.

[0033] The heat treatment is a carbonization or graphitization treatment, and specifically, for example, the heat treatment of the carbon precursor and the mold may be performed at 600 to 900°C as a first step and at 800 to 1500°C as a second step.

[0034] The present invention also provides a method for producing a semiconductor device comprising the steps of: a) mixing a carbon precursor having a melting point of 130 to 350°C with one or more particles selected from basic zinc carbonazate (BZC), zinc(II) metal-organic frameworks, and porous ZnO as a template; b) heating the mixture at 120 to 350° C. to allow the carbon precursor to infiltrate into the mold; c) heating the structure infiltrated with the carbon precursor inside the template at 600 to 900° C. to remove the template, forming a core-shell structure; and d) heating the core-shell structure at 800 to 1500° C. to vaporize and remove zinc impurities.

[0035] The above-described core-shell structured porous carbon material may be applied to the preparation method, and the preparation method may be illustrated diagrammatically in FIG.

[0036] In step b), the heating is preferably performed at 130 to 180° C., more preferably 140 to 160° C., for 0.2 to 3 hours, preferably 0.5 to 2 hours, more preferably 0.5 to 1.5 hours. The heating may be performed in air or in an inert atmosphere.

[0037] In step c), the heating is preferably performed at 650 to 850° C., more preferably 700 to 800° C., for 0.5 to 4 hours, preferably 1 to 3 hours, more preferably 1.5 to 2.5 hours. The heating may be performed in air or in an inert atmosphere.

[0038] In step d), the heating is preferably performed at 850 to 1200° C., more preferably 900 to 1000° C., for 0.2 to 3 hours, preferably 0.5 to 2 hours, more preferably 0.5 to 1.5 hours. The heating may be performed in an inert atmosphere. The inert atmosphere may be formed using a gas such as argon, nitrogen, or an argon / nitrogen mixed gas, but is not limited thereto.

[0039] The carbon precursor is one or more selected from glucose, sucrose, lactose, fructose, starch, tannic acid, and the like.

[0040] In one embodiment of the present invention, the carbon precursor and the template may be mixed at a weight ratio of 1:1 to 1:10. If the weight ratio of the carbon precursor and the template is outside the above range, the amount of carbon sheet laminated on the core part is too small, or the shell is not properly formed, which is undesirable. The weight ratio of the carbon precursor and the template is more preferably 1:4 to 1:8.

[0041] In one embodiment of the present invention, the core-shell structured porous carbon material may be prepared in a one-pot manner.

[0042] The present invention also provides a method for producing a method for manufacturing a semiconductor device comprising the steps of: The present invention relates to a sulfur-carbon composite comprising the porous carbon material having the core-shell structure and a sulfur component.

[0043] In the sulfur-carbon composite, except for the porous carbon material having the core-shell structure, any technique known in the art may be applied without limitation.

[0044] The sulfur contained in the sulfur-carbon composite may be at least one selected from the group consisting of elemental sulfur (S8) and sulfur compounds. For example, inorganic sulfur, Li2S n (n≧1), disulfide compounds, organic sulfur compounds and carbon-sulfur polymers ((C2S x ) n , x=2.5 to 50, n≧2), and the like may be used.

[0045] Since sulfur does not have electrical conductivity by itself, it is used in combination with a conductive material such as the core-shell structured porous carbon material of the present invention.

[0046] The core-shell porous carbon material provides a framework in which sulfur can be uniformly and stably fixed, and complements the low electrical conductivity of sulfur to facilitate smooth electrochemical reactions.

[0047] In addition, in the core-shell structured porous carbon material of the present invention, the core including the laminated carbon sheets can facilitate the ingress and egress of lithium ions, and the shell can suppress the elution of lithium polysulfide.

[0048] The core-shell structured porous carbon material contains variable pores, the average diameter of the pores is in the range of 1 to 1000 nm, and the porosity or void ratio is in the range of 10 to 90% of the total volume of the porous carbon material. If the average diameter of the pores is less than the range, the size of the pores is merely at the molecular level, making it impossible to impregnate with sulfur, and conversely, if it exceeds the range, the mechanical strength of the porous carbon material is weakened, making it unsuitable for use in the manufacturing process of an electrode.

[0049] The sulfur-carbon composite of the present invention may further include one or more carbon materials commonly used in this field in addition to the core-shell porous carbon material. The carbon materials may include, but are not limited to, one or more selected from the group consisting of graphite, graphene, carbon black such as denka black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black, carbon nanotubes (CNTs) such as single-walled carbon nanotubes (SWCNTs) and multi-walled carbon nanotubes (MWCNTs), carbon fibers such as graphite nanofibers (GNFs), carbon nanofibers (CNFs), and activated carbon fibers (ACFs), graphite such as natural graphite, artificial graphite, and expanded graphite, and activated carbon.

[0050] In the sulfur-carbon composite, the weight ratio of sulfur to the porous carbon material is 9:1 to 7:3, preferably 9:1 to 7.5:2.5. If the sulfur content is less than 70 wt% based on 100 wt% of the total sulfur-carbon composite, the content of the porous carbon material increases relatively, and the specific surface area increases, so that the content of the binder required for manufacturing the positive electrode increases. Such an increase in the amount of binder used may ultimately increase the surface resistance of the positive electrode and act as an insulator that prevents electron transfer, thereby reducing the performance of the battery. On the other hand, if the content exceeds 90 wt%, the sulfur compounds that cannot be bonded to the porous carbon material may form a lump or be re-eluted on the surface of the porous carbon material, making it difficult for them to receive electrons and therefore unable to directly participate in the electrochemical reaction, which may cause a loss of capacity in the battery.

[0051] In addition, in the sulfur-carbon composite, the sulfur is located at least in one of the inner and outer surfaces of the porous carbon material, and may be present in an area of ​​less than 100%, preferably 1 to 95%, more preferably 60 to 90% of the entire inner and outer surfaces of the porous carbon material. When the sulfur is present in the inner and outer surfaces of the porous carbon material within the above range, it can exhibit the maximum effect in terms of electron transfer area and wettability with the electrolyte. Specifically, in the above range, the sulfur is thinly and uniformly impregnated in the inner and outer surfaces of the porous carbon material, so that the electron transfer contact area during charging and discharging can be increased. If the sulfur is located in 100% of the entire inner and outer surfaces of the porous carbon material, the carbon material is completely covered with sulfur, which reduces wettability with the electrolyte and reduces contact with the conductive material contained in the electrode, making it impossible to transfer electrons and participate in the electrochemical reaction.

[0052] In one embodiment of the present invention, the diameter of the sulfur-carbon composite is not particularly limited in the present invention, but is preferably 0.1 to 20 μm, more preferably 1 to 10 μm. When the diameter satisfies the above range, it is advantageous in that a high loading electrode can be manufactured.

[0053] The method for preparing the sulfur-carbon composite is not particularly limited in the present invention and may be performed by a method commonly used in this field. For example, the sulfur and the porous carbon material may be simply mixed and then heat-treated to prepare a composite.

[0054] The present invention also provides a method for producing a method for manufacturing a semiconductor device comprising the steps of: A lithium secondary battery including the core-shell structured porous carbon material is provided.

[0055] The present invention also provides a lithium secondary battery including the sulfur-carbon composite.

[0056] The lithium secondary battery of the present invention may employ known structures commonly applied to lithium-sulfur batteries in this field, except for the core-shell structured porous carbon material and / or sulfur-carbon composite.

[0057] The following description will be given taking the lithium secondary battery as an example.

[0058] The lithium secondary battery of the present invention may include a negative electrode; a positive electrode; a separator disposed between the positive electrode and the negative electrode; and an electrolyte.

[0059] The negative electrode may include a negative electrode active material, a binder, and a conductive material, and may further include a dispersant. The negative electrode active material may be any material known in the art, and may include, for example, LiTi2(PO4)3, Li3V2(PO4)3, LiVP2O7, LiFeP2O7, LiVPO4F, LiVPO4O, and LiFeSO4F. The negative electrode active material has a carbon coating layer formed on its surface.

[0060] The negative electrode active material, binder, conductive material, and / or dispersant may form a negative electrode active material layer, and the negative electrode active material layer may be included in the negative electrode by preparing a slurry containing the above components by a conventional method, coating the slurry on a current collector, and drying the same. Non-limiting examples of the current collector include foils made of copper, gold, nickel, copper alloys, or combinations thereof.

[0061] The conductive material is not particularly limited, and conductive materials such as graphite-based materials such as KS6, carbon-based materials such as Super-P, Denka Black, and carbon black, and conductive polymers such as polyaniline, polythiophene, polyacetylene, and polypyrrole can be used alone or in combination.

[0062] The method for manufacturing the negative electrode is not particularly limited, and the negative electrode may be manufactured in a form in which the negative electrode active material is bound to the current collector by a conventional method known in the art.

[0063] The positive electrode may include a positive electrode active material, a binder, a conductive material, and may further include a dispersant. The positive electrode active material may be a known positive electrode active material, such as lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, lithium iron oxide, or a three-component positive electrode material, such as LiNi x Mn y Co z O2(NMC), or a lithium composite oxide combining these, etc. When the lithium secondary battery is a lithium-sulfur battery, the sulfur-carbon composite may be included as a positive electrode active material.

[0064] The positive electrode active material, binder, conductive material, and / or dispersant may form a positive electrode active material layer, and the positive electrode active material layer may be included in the positive electrode by preparing a slurry containing the above components by a conventional method, coating the slurry on a current collector, and drying the same. Non-limiting examples of the current collector include foils made of aluminum, nickel, or a combination thereof.

[0065] Examples of the conductive material that can be used include carbon black such as Super-P, denka black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon black; carbon derivatives such as carbon nanotubes and fullerene; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; and conductive polymers such as polyaniline, polythiophene, polyacetylene, and polypyrrole.

[0066] The method for manufacturing the positive electrode is not particularly limited, and the positive electrode may be manufactured in a form in which the positive electrode active material is bound to the current collector by a conventional method known in the art.

[0067] The separator between the positive electrode and the negative electrode separates or insulates the positive electrode and the negative electrode from each other and allows lithium ions to be transported between the positive electrode and the negative electrode. The separator used in the present invention may be any porous polymer substrate commonly used in this field, for example, a polyolefin-based porous polymer membrane or nonwoven fabric, but is not limited thereto.

[0068] Examples of the polyolefin-based porous polymer membrane include membranes formed of polyolefin-based polymers such as polyethylene (e.g., high density polyethylene, linear low density polyethylene, low density polyethylene, ultra-high molecular weight polyethylene), polypropylene, polybutylene, and polypentene, either alone or in combination.

[0069] The nonwoven fabric may be a polyolefin nonwoven fabric, or may be a nonwoven fabric formed of a polymer such as polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyether ether ketone, polyether sulfone, polyphenylene oxide, polyphenylene sulfide, or polyethylene naphthalene, either alone or in combination. The nonwoven fabric may be a spunbonded or meltblown nonwoven fabric made of long fibers.

[0070] The thickness of the porous polymer substrate is not particularly limited, but is 5 to 50 μm, and the size and porosity of the pores present in the porous polymer substrate are also not particularly limited, but are 0.01 to 50 μm and 10 to 95%, respectively.

[0071] In addition, in order to improve the mechanical strength of the separator and the safety of the lithium secondary battery, a porous coating layer including inorganic particles and a polymer binder may be further included on at least one surface of the porous polymer substrate.

[0072] In the lithium-sulfur battery of the present invention, the electrolyte may be any electrolyte known in the art without limitation. For example, a non-aqueous electrolyte solution containing a lithium salt, an organic solid electrolyte, an inorganic solid electrolyte, etc. may be used.

[0073] The non-aqueous electrolyte containing a lithium salt is composed of a lithium salt and a solvent, and the solvent may be a non-aqueous organic solvent, an organic solid electrolyte, or an inorganic solid electrolyte.

[0074] The lithium salt is a material that can be easily dissolved in a non-aqueous organic solvent, for example, LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiB(Ph) 4、 The compound may be one or more selected from the group consisting of LiC4BO8, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, LiSO3CH3, LiSO3CF3, LiSCN, LiC(CF3SO2)3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(SO2F)2, lithium chloroborane, lithium lower aromatic carboxylates, lithium tetraphenylborate, and lithium imide.

[0075] The concentration of the lithium salt is 0.1 to 4.0M, preferably 0.5 to 2.0M, depending on many factors such as the exact composition of the electrolyte mixture, the solubility of the salt, the conductivity of the dissolved salt, the charge and discharge conditions of the battery, the operating temperature, and other factors known in the lithium-sulfur battery field. If the concentration of the lithium salt is below this range, the conductivity of the electrolyte may decrease, resulting in a decrease in battery performance, and if it exceeds this range, the viscosity of the electrolyte may increase, resulting in a decrease in the amount of lithium ions (Li + Since the mobility of the ion exchange polymer may be decreased, it is preferable to select an appropriate concentration within the above range.

[0076] The non-aqueous organic solvent is a material that can dissolve lithium salts well, and is preferably N-methyl-2-pyrrolidone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-2-methoxyethane, tetraethylene glycol dimethyl ether, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, 4-methyl Aprotic organic solvents such as 1,3-dioxane, diethyl ether, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ether, methyl propionate, and ethyl propionate can be used, and one or more of these can be used in the form of a mixed solvent.

[0077] Examples of the organic solid electrolyte that can be used include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyagitate lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and polymers containing ionic dissociation groups.

[0078] In the inorganic solid electrolyte of the present invention, for example, nitrides, halides, and sulfates of Li, such as Li3N, LiI, Li5NI2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH, and Li3PO4-Li2S-SiS2, can be used.

[0079] The non-aqueous electrolyte for a lithium-sulfur battery according to the present invention may further include a nitric acid or nitrite-based compound as an additive, which has the effect of forming a stable coating on the lithium electrode and improving charge / discharge efficiency. The nitric acid or nitrite compound is not particularly limited in the present invention, but may be one selected from the group consisting of inorganic nitric acid or nitrite compounds such as lithium nitrate (LiNO3), potassium nitrate (KNO3), cesium nitrate (CsNO3), barium nitrate (Ba(NO3)2), ammonium nitrate (NH4NO3), lithium nitrite (LiNO2), potassium nitrite (KNO2), cesium nitrite (CsNO2), and ammonium nitrite (NH4NO2); organic nitric acid or nitrite compounds such as methyl nitrate, dialkylimidazolium nitrate, guanidine nitrate, imidazolium nitrate, pyridinium nitrate, ethyl nitrate, propyl nitrate, butyl nitrate, pentyl nitrate, and octyl nitrate; and organic nitro compounds such as nitromethane, nitropropane, nitrobutane, nitrobenzene, dinitrobenzene, nitropyridine, dinitropyridine, nitrotoluene, and dinitrotoluene, and combinations thereof. Preferably, lithium nitrate can be used.

[0080] In addition, the non-aqueous electrolyte may further contain other additives for the purpose of improving charge / discharge characteristics, flame retardancy, etc. Examples of the additives include pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, aluminum trichloride, fluoroethylene carbonate (FEC), propene sultone (PRS), vinylene carbonate (VC), etc.

[0081] The lithium secondary battery may be constructed by applying techniques known in the art, except for the characteristic techniques of the present invention.

[0082] The lithium secondary battery may be manufactured by stacking, lamination, folding, and stacking / folding processes of a separator and an electrode in addition to the general winding process. The shape of the lithium secondary battery is not particularly limited, and may be cylindrical, rectangular, pouch-shaped, or coin-shaped using a can.

[0083] In the following, preferred examples are presented to facilitate understanding of the present invention. However, the following examples are merely illustrative of the present invention, and it will be obvious to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical idea of ​​the present invention, and it is natural that such changes and modifications fall within the scope of the attached claims.

[0084] Manufacturing example 1: Manufacturing basic zinc carbonate (BZC) Zn(NO3)2·6H2O, urea, and L-asparagine were mixed and stirred in a molar ratio of 1:5:1, and then subjected to a hydrothermal reaction at 120℃ for 3 hours, followed by filtering and drying to produce BZC. The molar ratio can be selected from the range of 1:1:1 to 1:10:1.

[0085] The BZC can also be purchased and used (eg, Sigma-Arich, alfa, product name: Zinc carbonate basic).

[0086] Examples 1 to 5: Preparation of porous carbon materials with core-shell structure Glucose (CH) was used as the carbon precursor. 12O6) and BZC as a template were mixed in the weight ratios shown in Table 1 below. The mixture was then heated at 150°C for 1 hour to allow glucose to infiltrate into the BZC template. The BZC with glucose infiltrated into the core was then heated at 750°C for 2 hours, and the template was removed to form a core-shell porous carbon material morphology (morphology imprinting). The core-shell porous carbon material was then heated at 950°C for 1 hour in an inert atmosphere to vaporize and remove zinc impurities, thereby producing a core-shell porous carbon material.

[0087] [Table 1]

[0088] Examples 6-10: Preparation of porous carbon materials with core-shell structure Sucrose (C) was used as the carbon precursor. 12 H 22 O 11 , T m Sucrose (180°C) and BZC as a template were mixed in the weight ratios shown in Table 2 below. The mixture was then heated at 200°C for 1 hour to infiltrate sucrose into the BZC as a template. The BZC with the sucrose infiltrated into the core was then heated at 750°C for 2 hours, and the template was removed to form a core-shell structured porous carbon material morphology (morphology imprinting). The core-shell structured porous carbon material was then heated at 950°C for 1 hour in an inert atmosphere to vaporize and remove zinc impurities, thereby producing a core-shell structured porous carbon material.

[0089] [Table 2]

[0090] Comparative Example 1: Production of porous carbon material 1.6g of BZC was dispersed in 140ml of deionized water, and then 6.9g of CTAB, 1.05g of resorcinol, 84.6ml of ethanol, and 0.2ml of ammonia were added and mixed at 35°C for 30 minutes, and then 1.5ml of formalin was added and stirred for 6 hours. The mixture was then aged without stirring for 12 hours, centrifuged, washed several times with water and ethanol, and dried.

[0091] Then, the carbon precursor (resorcinol-formaldehyde polymer resin) and the BZC mixture were heat-treated at 150°C for 1 hour, at 300°C for 30 minutes, and at 800°C for 2 hours. The heat treatment was performed in an inert atmosphere, and the obtained sample was washed with 1M HCl and dried to prepare a porous carbon material F2SMC.

[0092] Experimental Example 1: Measurement of the specific surface area of ​​core-shell structured porous carbon material The specific surface area of ​​the core-shell porous carbon material prepared in Example 1 was measured by the Brunauer-Emmett-Teller method using N2 sorption (MicrotracBEL, product name: BELSORP-max) at 77K, and the results are shown in FIG. 5. As can be seen in FIG. 5, the specific surface area of ​​the core-shell porous carbon material of the present invention is 1050 m 2 / g. In Figure 5, Ads indicates adsorption and Des indicates desorption.

[0093] Example 8: Preparation of sulfur-carbon composite The core-shell structured carbon material prepared in Example 1 and sulfur (S8) were uniformly mixed in a weight ratio of 2.5:7.5, and then heated in an oven at 155° C. for 30 minutes to prepare a sulfur-carbon composite.

[0094] Comparative Example 2: Preparation of sulfur-carbon composite The carbon material prepared in Comparative Example 1 and sulfur (S8) were uniformly mixed in a weight ratio of 2.5:7.5, and then heated in an oven at 155° C. for 30 minutes to prepare a sulfur-carbon composite.

[0095] Experimental Example 2: Structure confirmation of porous carbon material and sulfur-carbon composite In order to confirm the structures of the porous carbon materials prepared in Example 1 and Comparative Example 1, a scanning electron microscope (SEM) was used to photograph and compare the morphologies of the core-shell structured porous carbon materials prepared in Example 1 and Comparative Example 1 (FIGS. 1 and 2). In addition, a scanning electron microscope (SEM) and an energy dispersive spectroscopy (EDS) were used to take and compare SEM photographs and element mapping photographs of the sulfur-carbon composites prepared in Example 8 and Comparative Example 2 (FIGS. 3 and 4).

[0096] Specifically, Figure 1 shows a scanning electron microscope (SEM) image of the core-shell porous carbon material prepared in Example 1. It can be seen from Figure 1 that the core-shell porous carbon material of the present invention includes a structure in which a carbon sheet is laminated on a core, and includes a shell containing carbon surrounding the core.

[0097] Figure 2 shows a scanning electron microscope (SEM) image of the porous carbon material prepared in Comparative Example 1. It can be seen from Figure 2 that the porous carbon material prepared in Comparative Example 1 has a flower-type open structure without a shell.

[0098] 3 shows a scanning electron microscope (SEM) photograph and an energy dispersive spectroscopy (EDS) elemental mapping photograph of the sulfur-carbon composite prepared in Example 8. As can be seen from FIG. 3, in the sulfur-carbon composite including the core-shell structured porous carbon material prepared in Example 8 of the present invention, carbon was detected in the shell and sulfur was detected in the core, and it was confirmed that the sulfur contained in the core was not aggregated or precipitated as crystals but was uniformly supported.

[0099] Fig. 4 shows a scanning electron microscope (SEM) photograph and an energy dispersive spectroscopy (EDS) elemental mapping photograph of the sulfur-carbon composite prepared in Comparative Example 2. From Fig. 4, it was confirmed that the sulfur-carbon composite prepared in Comparative Example 1 did not have a shell structure, and sulfur precipitated as a single crystal in the mesoporous structure was also observed.

[0100] Example 9 and Comparative Example 3: Fabrication of Lithium-Sulfur Battery A positive electrode slurry composition was prepared by mixing 88 wt % of the sulfur-carbon composites prepared in Example 8 and Comparative Example 2 as a positive electrode active material, 5 wt % of carbon nanotubes as a conductive material, 7 wt % of polyacrylic acid as a binder, and 7 wt % of polyvinyl alcohol (PAA:PVA=6.5:0.5 wt %) as a thickener.

[0101] The prepared positive electrode slurry composition was coated on an aluminum current collector, dried at 50° C. for 12 hours, and pressed with a roll press to prepare a positive electrode for a lithium-sulfur battery.

[0102] Together with the positive electrodes prepared above, a 45μm-thick lithium metal thin film was used as the negative electrode, and a mixture of 1M lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and 1% by weight lithium nitrate (LiNO3) dissolved in an organic solvent consisting of 1,3-dioxolane and dimethyl ether (DOL:DME=1:1 (volume ratio)) was used as the electrolyte.

[0103] Specifically, the prepared positive and negative electrodes were placed facing each other, and a separator made of polyethylene having a thickness of 16 μm and a porosity of 45% was placed therebetween, and then the prepared electrolyte was injected to prepare lithium-sulfur batteries of Example 9 and Comparative Example 3, respectively.

[0104] Experimental Example 3: Performance evaluation of lithium-sulfur batteries The lithium-sulfur batteries prepared in Example 9 and Comparative Example 3 were charged and discharged at current densities of 0.1 C, 0.2 C, and 0.5 C, respectively, using a charge / discharge measuring device (LAND CT-2001A, Wuhan, China), and the discharge capacity and coulombic efficiency were measured to evaluate the battery characteristics. The results are shown in FIGS. 6 and 7.

[0105] As shown in Figures 6 and 7, the initial 0.1C discharge capacity of the battery of Comparative Example 3 (using the existing carbon material S75 F2SMC composite (Comparative Example 1)) was calculated to be 725mAh / g, but thereafter, a charge delay phenomenon occurred and it was not possible to drive any further. This is believed to be due to the limitations of the existing open structure mesoporous carbon material. Meanwhile, in the case of the battery of Example 9 of the present invention (using the core-shell structured porous carbon material of Example 1), the initial 0.1C discharge capacity was calculated to be 1036mAh / g, and it was confirmed that the reaction continued reversibly thereafter, resulting in a clear improvement in the capacity and life characteristics of the battery.

Claims

1. A sulfur-carbon composite comprising a core-shell structured porous carbon material and a sulfur component, The diameter of the sulfur-carbon composite is 0.1 to 20 μm; The core-shell porous carbon material includes a core having a structure in which carbon sheets are laminated, and a shell including carbon surrounding the core; The carbon sheet laminated structure is a hierarchical porous structure, The porous carbon material includes pores therein, and the average diameter of the pores is in the range of 1 to 1000 nm.

2. The sulfur-carbon composite according to claim 1, wherein the carbon sheet is a graphene sheet.

3. The porous carbon material has a specific surface area of ​​300 m 2 / g to 2000m 2 The sulfur-carbon composite according to claim 1 or 2, wherein the sulfur-carbon composite has a molecular weight of 1.0 to 1.0 g.

4. a) mixing a carbon precursor having a melting point of 130 to 350° C. with one or more particles selected from basic zinc carbonate (BZC) and porous structure ZnO as a template; b) heating the mixture obtained in step a) at 120 to 350° C. to allow the carbon precursor to infiltrate into the mold; c) heating the structure infiltrated with the carbon precursor inside the template at 600 to 900° C. to remove the template, thereby forming a core-shell structure; and d) heating the core-shell structure at 800 to 1500° C. to vaporize and remove zinc impurities.

5. 5. The method for producing a core-shell porous carbon material according to claim 4, wherein the carbon precursor is at least one selected from the group consisting of glucose, sucrose, lactose, fructose, starch, and tannic acid.

6. 6. The method for preparing a core-shell porous carbon material according to claim 4, wherein the carbon precursor and the template are mixed in a weight ratio of 1:1 to 1:

10.

7. The method for producing a porous carbon material according to any one of claims 4 to 6, wherein the core-shell structured porous carbon material is produced in a one-pot manner.

8. A lithium secondary battery comprising the sulfur-carbon composite according to claim 1.

Citation Information

Patent Citations

  • Carbon molecular material and method for manufacturing it

    JP2003034516A

  • Method for producing porous carbon material

    JP2009143786A

  • Porous carbon product having a layered bonding structure, method for producing the same, and method for using the same.

    JP2014511816A

  • Surface-modified carbon hybrid particles, their fabrication methods, and applications

    JP2015525184A

  • Sulfur-Carbon Composites Containing Highly Graphitic Carbon Materials for Lithium-Sulfur Batteries and Their Fabrication Process

    JP2018535915A