Method for recovering active metals from lithium secondary batteries
The method addresses the inefficiencies of existing lithium recovery processes by employing a controlled dry reduction process to achieve high-purity and high-yield recovery of lithium and transition metals from lithium secondary batteries, minimizing environmental impact.
Patent Information
- Application Number
- JP2022548614
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Priority Date
- 2020-02-10
- Filing Date
- 2021-01-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-01-25
AI Technical Summary
Existing methods for recovering valuable metals from lithium secondary batteries, particularly lithium transition metal oxides, face challenges in selectivity, efficiency, and environmental impact, especially in dry-based processes.
A method involving a dry reduction process using a reducing reaction gas to convert lithium-transition metal oxides into pre-precursor mixtures with controlled transition metal reduction, followed by selective recovery of lithium and transition metals through controlled reaction conditions and fluidized bed reactors.
Achieves high-purity and high-yield recovery of lithium and transition metals without environmental pollution, reducing the need for wet processes and by-products.
Smart Images

Figure 0007575468000002 
Figure 0007575468000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for recovering active metals from lithium secondary batteries, and more particularly to a method for recovering active metals from used positive electrodes of lithium secondary batteries. [Background technology]
[0002] In recent years, secondary batteries have been widely applied and developed as power sources for portable electronic communication devices such as camcorders, mobile phones, and notebook computers, and for vehicles such as hybrid cars, electric cars, etc. As secondary batteries, lithium secondary batteries have been actively developed and applied because of their high operating voltage and energy density per unit weight, as well as their advantages in terms of charging speed and weight reduction.
[0003] The positive electrode active material of the lithium secondary battery may be a lithium metal oxide, which may further contain a transition metal such as nickel, cobalt, or manganese.
[0004] Since the positive electrode active material contains the expensive valuable metals, the production of the positive electrode material accounts for more than 20% of the production cost. In addition, in recent years, with the growing interest in environmental protection, research into recycling methods for the positive electrode active material has been progressing.
[0005] Conventionally, a method has been used in which waste cathode active material is leached in a strong acid such as sulfuric acid to recover valuable metals, but the wet process has disadvantages in terms of regeneration selectivity, regeneration time, etc., and can cause environmental pollution. Therefore, a method of recovering valuable metals using a dry-based reaction has been researched.
[0006] For example, a method for regenerating or recovering lithium by dry reduction reaction has been studied, and precise control of reaction equipment and reaction conditions is required to increase the lithium recovery rate.
[0007] For example, Korean Patent No. 10-0709268 discloses an apparatus and method for recycling waste manganese batteries and alkaline batteries, but does not provide a dry-based method for recovering valuable metals with high selectivity and high yield. Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a method for recovering active metals of lithium secondary batteries with high efficiency and high purity. [Means for solving the problem]
[0009] In a method for recovering active metals from a lithium secondary battery according to an embodiment of the present invention, a positive electrode active material mixture containing lithium-transition metal oxide is prepared from a waste positive electrode of a lithium secondary battery. The positive electrode active material mixture is reacted with a reducing reactant gas to form a preliminary precursor mixture defined by the following formula 1 and having a transition metal reduction degree in the range of 0.24 to 1.6. A lithium precursor is recovered from the preliminary precursor mixture.
[0010] [Formula 1] Degree of transition metal reduction = (MeO phase fraction + lithium-transition metal oxide phase fraction) / (Me phase fraction)
[0011] (In formula 1, Me includes Ni and Co, and the MeO phase fraction and the Me phase fraction are measured by Rietveld crystal structure analysis of the X-ray diffraction (XRD) analysis peaks of the preliminary precursor mixture.)
[0012] In some embodiments, the lithium-transition metal oxide can be represented by Formula 1:
[0013] [Chemical formula 1] Li x Ni a Co b Mn c O y
[0014] (0 in chemical formula 1 <x≦1.1、2≦y≦2.02、0<a<1、0<b<1、0<c<1、0<a+b+c≦1である。)
[0015] In some embodiments, the reducing reactant gas includes hydrogen and a carrier gas, and the concentration of hydrogen in the reducing reactant gas may be 10 to 40% by volume.
[0016] In some embodiments, the reaction temperature with the reducing reactant gas may be 400 to 600°C.
[0017] In some embodiments, the preliminary precursor mixture includes preliminary lithium precursor particles and transition metal-containing particles, and the transition metal-containing particles can include Ni, Co, NiO, CoO, and MnO.
[0018] In some embodiments, the reserve lithium precursor particles may include at least one of lithium hydroxide, lithium oxide, or lithium carbonate.
[0019] In some embodiments, in recovering the lithium precursor, the preliminary lithium precursor particles can be subjected to a water washing process.
[0020] In some embodiments, the transition metal-containing particles can be selectively treated with an acid solution to recover the transition metal precursor in the form of an acid salt.
[0021] In some embodiments, the pre-precursor mixture may have a transition metal reduction degree of 0.24 to 1.0.
[0022] In some embodiments, the cathode active material mixture can be reacted with the reducing reactant gas in a fluidized bed reactor to form the pre-precursor mixture. Effect of the Invention
[0023] According to the above exemplary embodiment, the lithium precursor can be recovered from the waste cathode active material by a dry-based process utilizing a dry reduction process, thereby obtaining a lithium precursor with high purity without the additional process brought about by the wet-based process.
[0024] According to an exemplary embodiment, a suitable reduction degree for lithium recovery can be achieved by adjusting the ratio of the fraction of the transition metal oxide phase to the fraction of the transition metal phase after the dry reduction process, thereby preventing metal aggregation while efficiently extracting lithium from the lithium transition metal oxide, and increasing the recovery rate of the desired lithium precursor. [Brief description of the drawings]
[0025] [Figure 1] FIG. 1 is a schematic flow chart illustrating a method for recovering active metals from a lithium secondary battery according to an exemplary embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] An embodiment of the present invention provides a method for recovering active metals from lithium secondary batteries in high purity and high yield by dry reduction reaction.
[0027] Hereinafter, embodiments of the present invention will be described in more detail with reference to the drawings. However, these embodiments are merely illustrative of the present invention and are not intended to limit the present invention.
[0028] As used herein, the term "precursor" is used to refer collectively to a compound containing a specific metal to provide the specific metal contained in the electrode active material.
[0029] 1 is a schematic flow chart for explaining a method for recovering active metals from a lithium secondary battery according to an exemplary embodiment. For convenience of explanation, FIG. 1 shows a schematic diagram of a reactor together with the process flow.
[0030] Referring to FIG. 1, a positive electrode active material mixture (eg, a waste positive electrode active material mixture) can be prepared from a waste positive electrode of a lithium secondary battery (eg, step S10).
[0031] The lithium secondary battery may include an electrode assembly including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, and the positive electrode and the negative electrode may include a positive electrode active material layer and a negative electrode active material layer coated on a positive electrode current collector and a negative electrode current collector, respectively.
[0032] For example, the positive electrode active material contained in the positive electrode active material layer can include an oxide containing lithium and a transition metal.
[0033] In some embodiments, the positive electrode active material may include a compound represented by Formula 1:
[0034] [Chemical formula 1] Li x M1 a M2 b M3 c O y
[0035] In Chemical Formula 1, M1, M2, and M3 may be a transition metal selected from Ni, Co, Mn, Na, Mg, Ca, Ti, V, Cr, Cu, Zn, Ge, Sr, Ag, Ba, Zr, Nb, Mo, Al, Ga, or B. <x≦1.1、2≦y≦2.02、0<a<1、0<b<1、0<c<1、0<a+b+c≦1であってもよい。
[0036] In some embodiments, the active cathode material may be an NCM-based lithium oxide containing nickel, cobalt, and manganese.
[0037] The positive electrode can be separated from the used lithium secondary battery to recover the used positive electrode. The used positive electrode includes a positive electrode current collector (e.g., aluminum (Al)) and a positive electrode active material layer as described above, and the positive electrode active material layer can include a conductive material and a binder in addition to the positive electrode active material.
[0038] The conductive material may include, for example, a carbon-based material such as graphite, carbon black, graphene, carbon nanotubes, etc. The binder may include, for example, a resin material such as vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, etc.
[0039] According to an exemplary embodiment, the recovered waste positive electrodes may be pulverized to produce a positive electrode active material mixture, whereby the positive electrode active material mixture may be manufactured in a powder form.
[0040] The positive electrode active material mixture includes a lithium-transition metal oxide powder as described above, for example, an NCM-based lithium oxide powder (e.g., Li(NCM)O2). In this case, in the NCM-based lithium oxide powder, M1, M2, and M3 in the following Chemical Formula 1 may be Ni, Co, and Mn, respectively.
[0041] The term "positive electrode active material mixture" as used herein may refer to a raw material input to a reductive reaction process described below after the positive electrode current collector is substantially removed from the waste positive electrode. In one embodiment, the positive electrode active material mixture may include positive electrode active material particles such as the NCM-based lithium oxide. In one embodiment, the positive electrode active material mixture may also include a component derived from the binder or the conductive material. In one embodiment, the positive electrode active material mixture may be substantially composed of the positive electrode active material particles.
[0042] In some embodiments, the average particle size (D 50 ) may be 5 to 100 μm. Within this range, the lithium-transition metal oxide to be recovered, such as Li(NCM)O2, can be easily separated from the positive electrode current collector, conductive material, and binder contained in the positive electrode active material mixture.
[0043] In some embodiments, the cathode active material mixture may be heat-treated before being introduced into a reducing reactor described below. The heat treatment may remove or reduce impurities, such as the conductive material and binder, contained in the waste cathode active material mixture, and the lithium-transition metal oxide may be introduced into the reducing reactor in high purity.
[0044] The temperature of the heat treatment may be, for example, about 100 to 500° C., preferably about 350 to 450° C. Within this range, the impurities are substantially removed, and decomposition and damage of the lithium-transition metal oxide can be prevented.
[0045] For example, in step S20, the positive electrode active material mixture may be reacted in a reducing reactor 100 to form a pre-precursor mixture 80.
[0046] 1, the reducing reactor 100 can be divided into a reactor body 130, a reactor lower part 110, and a reactor upper part 150. The reactor body 130 can include a heating means such as a heater or can be integrated with a heating means.
[0047] The positive electrode active material mixture may be supplied into the reactor body 130 through the supply passages 106a and 106b. The positive electrode active material mixture may be dropped through a first supply passage 106a connected to the upper part 150 of the reactor or may be added through a second supply passage 106b connected to the bottom of the reactor body 130. In one embodiment, the waste positive electrode active material mixture may be supplied using both the first and second supply passages 106a and 106b.
[0048] For example, the powder of the waste positive electrode active material mixture may be fixed by disposing a support 120 between the reactor body 130 and the reactor lower portion 110. The support 120 may include holes or nozzles for passing a reducing reaction gas and / or a carrier gas, which will be described later.
[0049] A reducing reactant gas for converting the positive active material mixture into a pre-precursor may be supplied into the reactor body 130 through a reactant gas passage 102 connected to the reactor lower portion 110. According to an exemplary embodiment, the reducing reactant gas may include hydrogen (H2). The reducing reactant gas may further include a carrier gas such as nitrogen (N2) or argon (Ar).
[0050] The reducing reactant gas is supplied from the lower part of the reducing reactor 100 and contacts the positive active material mixture, and the positive active material mixture may react with the reducing reactant gas while moving to the upper part 150 of the reactor or while remaining in the reactor body 130, and may be converted into the pre-precursor.
[0051] In some embodiments, the reducing reactant gas is injected to form a fluidized bed in the reactor body 130. Therefore, the reducing reactor 100 may be a fluidized bed reactor. In the fluidized bed, the positive electrode active material mixture and the reducing reactant gas come into contact with each other, and the reaction contact time is increased by repeating rising, staying, and falling, and the dispersion of particles is enhanced, thereby obtaining a pre-precursor mixture 80 with a uniform size.
[0052] However, the concept of the present invention is not necessarily limited to a fluidized bed reaction. For example, a fixed-bed reaction may be carried out by preloading a mixture of positive active materials into a batch reactor or a tubular reactor and then supplying a reducing reactant gas.
[0053] As the reducing reactant gas is supplied from the lower part of the reducing reactor 100 and contacts the positive active material mixture, the positive active material mixture moves to the upper part 150 of the reactor to expand the reaction area and may be converted into the pre-precursor.
[0054] In some embodiments, the lithium-transition metal oxide may be reduced by the reducing reactant gas to produce, for example, lithium hydroxide (LiOH), a lithium oxide (e.g., LiO2) and a pre-lithium precursor, including a transition metal or transition metal oxide. For example, the reducing reaction may produce Ni, Co, NiO, CoO and MnO along with the lithium oxide.
[0055] For example, as the reduction process proceeds, the crystal structure of Li(NCM)O2 may collapse and Li may leave the crystal structure from which NiO and CoO may form, and as the reduction process continues, Ni and Co phases may form together.
[0056] This can form a preliminary precursor mixture 80 including preliminary lithium precursor particles 60 and transition metal-containing particles 70 (e.g., the transition metal or transition metal oxide) within the reactor body 130. The preliminary lithium precursor particles 60 can include, for example, lithium hydroxide (LiOH), lithium oxide (LiO2), and / or lithium carbonate (LI2CO3).
[0057] The transition metal-containing particles 70 can include Ni, Co, NiO, CoO, and MnO as previously described.
[0058] According to an exemplary embodiment, the degree of transition metal reduction of pre-precursor mixture 80, as measured by X-ray diffraction analysis (XRD) and defined by Equation 1 below, may be between 0.24 and 1.6.
[0059] [Formula 1] Degree of transition metal reduction = (MeO phase fraction + lithium-transition metal oxide phase fraction) / (Me phase fraction)
[0060] In the above formula 1, Me includes Ni and Co. For example, the MeO phase may be the mole fraction of NiO and CoO phases in the pre-precursor mixture produced by the reduction process. The Me phase may be the mole fraction of Ni and Co in the pre-precursor mixture produced by the reduction process.
[0061] The lithium-transition metal oxide phase fraction shown in formula 1 may represent, for example, the fraction of lithium-transition metal oxide that is unreacted or undecomposed by the reduction process. The lithium-transition metal oxide may represent an NCM-based lithium oxide, and may be represented by the following formula 1-1.
[0062] [Chemical formula 1-1] Li x Ni a Co b Mn c O y
[0063] (0 in chemical formula 1-1 <x≦1.1、2≦y≦2.02、0<a<1、0<b<1、0<c<1、0<a+b+c≦1である。)
[0064] The above fractions are obtained by crystal structure analysis using the Rietveld method for peaks obtained from XRD analysis.
[0065] If the transition metal reduction degree is less than 0.24, the transition metal may be excessively reduced, and excessive metal agglomerates may be generated, which may prevent a sufficient fluidized bed from being generated in the reactor body 130, and the metal agglomerates may stick to the inner wall of the reactor body 130, thereby preventing the generation of preliminary lithium precursor particles 60.
[0066] If the transition metal reduction degree exceeds 1.6, the collapse of the crystal structure of the lithium-transition metal compound may not be sufficiently induced, and therefore, the release of Li ions may not occur sufficiently, resulting in a decrease in the recovery rate of the lithium precursor.
[0067] The degree of reduction of the transition metal can be finely adjusted by adjusting process conditions such as the hydrogen concentration in the reducing reaction gas, the flow rate of the reducing reaction gas, the reaction temperature, and the reduction reaction time.
[0068] In a preferred embodiment, the transition metal reduction degree defined by the above formula 1 may be 0.24 to 1.0.
[0069] In one embodiment, the concentration of hydrogen in the reducing reaction gas may be about 10 to 40 volume percent (vol%). As described above, the reducing reaction gas may be a mixed gas of hydrogen and a carrier gas, and the concentration of hydrogen may be the vol% of hydrogen in the total volume of the mixed gas.
[0070] The temperature of the reduction reaction can be adjusted within the range of about 400 to 800°C, preferably within the range of about 400 to 600°C, and more preferably within the range of about 400 to 500°C.
[0071] The pre-precursor mixture 80 obtained by the aforementioned dry reduction process can be collected for a subsequent recovery process.
[0072] In one embodiment, the transition metal-containing particles 70, including nickel, cobalt, or manganese, are relatively heavier than the reserve lithium precursor particles 60, so the reserve lithium precursor particles 60 may be collected first via the outlets 160a, 160b.
[0073] In one embodiment, the spare lithium precursor particles 60 can be discharged through a first outlet 160a connected to the reactor upper portion 150. In this case, selective recovery of the spare lithium precursor particles 60 by a weight gradient can be facilitated.
[0074] In one embodiment, the preliminary precursor mixture 80 including the preliminary lithium precursor particles 60 and the transition metal-containing particles 70 can be collected via the second outlet 160b connected to the reactor body 130. In this case, the preliminary precursor mixture 80 can be directly recovered from the fluidized bed formation region to increase the yield.
[0075] In one embodiment, the pre-precursor mixture 80 may be collected via both the first and second outlets 160a, 160b.
[0076] The preliminary lithium precursor particles 60 collected via the outlet 160 can be recovered as lithium precursors (eg, step S30).
[0077] In some embodiments, the preliminary lithium precursor particles 60 can be subjected to a water washing process, whereby the preliminary lithium precursor particles in the form of lithium hydroxide (LiOH) can be substantially dissolved in water and preferentially recovered separately from the transition metal precursor. A lithium precursor substantially composed of lithium hydroxide can be obtained, such as by a crystallization process of the lithium hydroxide dissolved in water.
[0078] In one embodiment, the reserve lithium precursor particles in the form of lithium oxide and lithium carbonate can be substantially removed by said water washing process, hi one embodiment, the reserve lithium precursor particles in the form of lithium oxide and lithium carbonate can be at least partially converted to lithium hydroxide by said water washing process.
[0079] In some embodiments, the preliminary lithium precursor particles 60 can be reacted with a carbon-containing gas, such as carbon monoxide (CO), carbon dioxide (CO2), etc., to obtain lithium carbonate (e.g., Li2CO3) as the lithium precursor. The reaction with the carbon-containing gas can provide a crystallized lithium precursor. For example, a carbon-containing gas can be co-injected during the water washing process and lithium carbonate can be collected.
[0080] The temperature of the crystallization reaction by the carbon-containing gas may be, for example, in the range of about 60 to 150° C. In this temperature range, highly reliable lithium carbonate can be produced without damaging the crystal structure.
[0081] As mentioned above, according to an exemplary embodiment, lithium precursors can be recovered from spent cathodes by a continuous dry process.
[0082] In the comparative example, a wet process such as a strong acid leaching process can be used to recover lithium or transition metals from waste secondary batteries. However, the wet process has limitations in selectively separating lithium. In addition, a water washing process is required to remove solution residues, and the generation of by-products such as hydrates due to contact with the solution may increase.
[0083] In contrast, according to an embodiment of the present invention, the lithium precursor is collected by a dry reduction reaction that eliminates the use of a solution, so that by-products are reduced, yields are increased, and no wastewater treatment is required, making it possible to design an environmentally friendly process.
[0084] In addition, the degree of reduction of the transition metal can be adjusted to promote the extraction of lithium and prevent the aggregation of the metal, thereby making it possible to recover a lithium precursor with high purity and high yield.
[0085] In some embodiments, a transition metal precursor can be obtained from the collected transition metal-containing particles 70 (eg, step S40).
[0086] For example, the preliminary lithium precursor particles 60 can be collected via the outlets 160a, 160b, followed by recovery of the transition metal-containing particles 70. The transition metal-containing particles 70 can then be treated with an acid solution to form precursors of the acid salt forms of the respective transition metals.
[0087] In one embodiment, the preliminary lithium precursor particles 60 and the transition metal-containing particles 70 can be collected together and subjected to a water washing step, where the preliminary lithium precursor particles 60 can be converted to a lithium precursor, such as lithium hydroxide, and dissolved, and the transition metal-containing particles 70 can be precipitated. The precipitated transition metal-containing particles 70 can again be collected and treated with an acid solution.
[0088] In one embodiment, sulfuric acid can be used as the acid solution, in which case NiSO4, MnSO4, and CoSO4 can be recovered as the transition metal precursors, respectively.
[0089] As described above, after the lithium precursor is collected by the dry process, the transition metal precursor is selectively extracted using an acid solution, thereby improving the purity and selectivity of each metal precursor, reducing the load of the wet process, and reducing the increase in wastewater and by-products.
[0090] In the following, preferred examples are presented to aid in understanding the present invention, but these examples are merely illustrative of the present invention and do not limit the scope of the appended claims. It is clear to those skilled in the art that various changes and modifications can be made to these examples within the scope of the scope and technical ideas of the present invention, and it is natural that these changes and modifications fall within the scope of the appended claims.
[0091] Example 1 1 kg of the cathode material separated from the waste lithium secondary batteries was heat-treated at 450°C for 1 hour. The heat-treated cathode material was cut into small units and pulverized by milling to obtain a Li-Ni-Co-Mn oxide cathode active material sample. 20 g of the cathode active material sample was placed in a fluidized bed reactor, and while maintaining the temperature inside the reactor at 455°C, a mixed gas of 20 vol% hydrogen / 80 vol% nitrogen was injected from the bottom of the reactor at a flow rate of 400 mL / min for 4 hours to obtain a preliminary precursor mixture.
[0092] The transition metal reduction degree of the obtained pre-precursor mixture was measured by XRD analysis, and then the pre-precursor mixture and water (19 times by weight) were added together and stirred. The concentration of lithium dissolved in water was analyzed, and the lithium recovery rate was calculated from the ratio of the weight of lithium dissolved in water to the weight of lithium in the initial positive electrode active material sample.
[0093] Example 2 The same process as in Example 1 was carried out, except that the reaction time was changed to 3 hours.
[0094] Example 3 2 g of the same positive electrode active material sample as in Example 1 was placed in a tubular reactor. The temperature in the reactor was maintained at 450° C., and a mixed gas of 40 vol% hydrogen / 60 vol% nitrogen was injected at a flow rate of 50 mL / min for 3 hours to obtain a preliminary precursor mixture. Thereafter, the transition metal reduction degree and lithium recovery rate were measured in the same manner as in Example 1.
[0095] Example 4 The process was carried out in the same manner as in Example 3, except that the reaction temperature was adjusted to 430° C. and a mixed gas of 20 vol % hydrogen / 80 vol % nitrogen was injected at a flow rate of 50 mL / min for 5 hours.
[0096] Example 5 The process was carried out in the same manner as in Example 2, except that a mixed gas of 15 vol % hydrogen / 80 vol % nitrogen was used.
[0097] Comparative Example 1 The process was carried out in the same manner as in Example 1, except that the reaction temperature was changed to 470° C. and the reaction time was changed to 3 hours.
[0098] Comparative Example 2 The process was carried out in the same manner as in Example 3, except that the reaction temperature was maintained at 450° C. and a mixed gas of 12.5 vol % hydrogen / 87.5 vol % nitrogen was injected at a flow rate of 50 mL / min for 5 hours.
[0099] Comparative Example 3 The process was carried out in the same manner as in Example 3, except that the reaction temperature was maintained at 465° C. and a mixed gas of 30 vol % hydrogen / 70 vol % nitrogen was injected at a flow rate of 30 mL / min for 1.5 hours.
[0100] Comparative Example 4 The process was carried out in the same manner as in Comparative Example 3, except that the injection time of the mixed gas was changed to 1 hour.
[0101] In the examples and comparative examples, the transition metal reduction degree according to formula 1 was measured by Rietveld refinement of the XRD peak of the preliminary precursor mixture, and the lithium recovery rate after mixing with water was measured. The evaluation results are shown in Table 1 below.
[0102] [Table 1]
[0103] Referring to Table 1, when the transition metal reduction degree was adjusted within the range according to the above-described embodiment of the present invention, a significantly higher lithium recovery rate was obtained compared to the comparative example.
Claims
1. Preparing a positive electrode active material mixture containing lithium-transition metal oxide from a used positive electrode of a lithium secondary battery; reacting the positive electrode active material mixture with a reducing reactant gas to form a pre-precursor mixture defined by the following formula 1 and having a transition metal reduction degree in the range of 0.24 to 1.6; and recovering a lithium precursor from said preliminary precursor mixture. [Formula 1] Degree of transition metal reduction=(MeO phase fraction+lithium-transition metal oxide phase fraction) / (Me phase fraction) (In formula 1, Me includes Ni and Co, and the MeO phase fraction, the lithium-transition metal oxide phase fraction, and the Me phase fraction are measured by Rietveld crystal structure interpretation of X-ray diffraction (XRD) analysis peaks of the pre-precursor mixture.)
2. 2. The method of claim 1, wherein the lithium-transition metal oxide is represented by the following Chemical Formula 1: [Chemical formula 1] Li x Ni a Co b Mn c O y (In chemical formula 1, 0<x≦1.1, 2≦y≦2.02, 0<a<1, 0<b<1, 0<c<1, and 0<a+b+c≦1.)
3. 2. The method for recovering active metals from a lithium secondary battery according to claim 1, wherein the reducing reaction gas contains hydrogen and a carrier gas, and the concentration of hydrogen in the reducing reaction gas is 10 to 40% by volume.
4. 2. The method for recovering active metals from a lithium secondary battery according to claim 1, wherein the reaction temperature with the reducing reaction gas is 400 to 600° C.
5. the preliminary precursor mixture comprises preliminary lithium precursor particles and transition metal-containing particles; 2. The method for recovering active metals from a lithium secondary battery according to claim 1, wherein the transition metal-containing particles contain Ni, Co, NiO, CoO and MnO.
6. 6. The method for recovering active metals of a lithium secondary battery according to claim 5, wherein the reserve lithium precursor particles include at least one of lithium hydroxide, lithium oxide, or lithium carbonate.
7. The method for recovering an active metal of a lithium secondary battery according to claim 5 , wherein the step of recovering the lithium precursor includes a step of washing the spare lithium precursor particles with water.
8. 6. The method for recovering active metals of a lithium secondary battery according to claim 5, further comprising the step of selectively treating the transition metal-containing particles with an acid solution to recover a transition metal precursor in the form of an acid salt.
9. 2. The method for recovering active metals of a lithium secondary battery according to claim 1, wherein the transition metal reduction degree of the preliminary precursor mixture is 0.24 to 1.
0.
10. 2. The method for recovering active metals of a lithium secondary battery according to claim 1, wherein the step of forming the preliminary precursor mixture comprises reacting the positive electrode active material mixture with the reducing reactant gas in a fluidized bed reactor.
Citation Information
Patent Citations
Reducible granulation evaluation method of sintered ore
JP2018179692A
Regeneration of cathode material of lithium-ion batteries
US20150052739A1
Process for the recycling of spent lithium ion cells
WO2020011765A1