Sinter manufacturing method
By adjusting the blending ratio of low-nitrogen anthracite with sintered ore production, the method stabilizes NOx emissions in response to varying crystallization water content in iron ores, addressing the inconsistency in NOx levels during sintered ore production.
Patent Information
- Application Number
- JP2021028474
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-25
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2041-02-25
AI Technical Summary
Existing methods for producing sintered ore fail to effectively suppress the variation in nitrogen oxide (NOx) emissions due to fluctuations in the crystallization water content of iron ore, despite efforts to maintain constant blending ratios.
A method involving blending low-nitrogen anthracite with sintered ore production to counteract increases in NOx emissions by adjusting the ratio based on changes in the crystallization water content of mixed iron ores, using a specific ratio adjustment formula to maintain NOx levels.
Effectively suppresses NOx emissions by correlating crystallization water content changes with low-nitrogen anthracite blending, ensuring stable NOx concentrations in sintering exhaust gases.
Smart Images

Figure 0007575680000009 
Figure 0007575680000001 
Figure 0007575680000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing sintered ore. [Background technology]
[0002] Currently, the main raw material in the blast furnace ironmaking process is sintered ore. The raw materials for sintered ore are new raw materials consisting of iron ore (several brands of iron ore), miscellaneous raw materials (recycled raw materials containing iron, such as scale and steelmaking dust), and auxiliary raw materials (raw materials used to adjust the CaO and MgO content in the sintered ore, such as limestone and olivine), carbonaceous materials (also called agglomeration materials, raw materials that serve as the heat source for the sintering reaction, such as coke powder and anthracite), and return ore (recycling the undersieve product).
[0003] Sintered ore is usually manufactured as follows. First, raw materials are mixed in a predetermined ratio to form a blended raw material, and the blended raw materials are granulated to form raw granules. Next, the raw granules are loaded onto the pallet of a downward suction type Dwight Lloyd (DL) sintering machine from a hopper to form a raw material packed bed. The carbonaceous material in the raw material packed bed is ignited from the top (surface layer) of the formed raw material packed bed. Then, while the pallet is continuously moved, air is sucked from below the pallet to supply oxygen, and the carbonaceous material in the raw material packed bed is burned from the top to the bottom, and is sintered sequentially by the combustion heat of the carbonaceous material. The obtained sintered part (sinter cake) is crushed to a predetermined grain size, sized by sieving, etc., to become sintered ore, which is a raw material for a blast furnace.
[0004] Sintering exhaust gas (hereinafter simply referred to as exhaust gas) discharged from the sintering machine contains nitrogen oxides NOx (NO and NO2). Most of the nitrogen oxides NOx in the exhaust gas are fuel NOx, which are generated when the carbonaceous fuel burns in the sintering bed. Fuel NOx is generated when the nitrogen contained in the carbonaceous fuel reacts with oxygen.
[0005] Nitrogen oxides (NOx) are one of the causes of air pollution, and reducing their emissions is important. Because the NOx concentration in exhaust gas varies with changes in the daily operation of sintering machines, such as changes to the raw material mix ratio, steelworks constantly monitor the NOx concentration and operate so as not to exceed the control value. This control value is set for each steelworks at a value lower than the regulatory value for NOx emissions in each operating area (such as the standard value set by ordinance).
[0006] NOx concentration is generally monitored using the value of "NOx concentration (O2 = 15% corrected value)". NOx concentration (O2 = 15% corrected value) is the NOx concentration C after oxygen concentration correction, which is corrected so that the standard oxygen concentration remaining in the exhaust gas is 15%. NOx concentration C (O2 = 15% corrected value) is calculated using the following formula (1) based on the measured NOx concentration (actual value Cs) and oxygen concentration Os. The NOx concentration (actual value) and oxygen concentration (actual value) in the exhaust gas are continuously measured, for example, by an analyzer (NOx analyzer (chemiluminescence method), zirconia analyzer, etc.) installed between the main blower that performs downward suction and the chimney. C=(21-On) / (21-Os)×Cs...(1) C: NOx concentration after oxygen concentration correction (ppm) Os: Oxygen concentration in exhaust gas (20% if the concentration exceeds 20%) On: Standard oxygen concentration (%) *15% for sintering machines Cs: Actual measured value of NOx in exhaust gas (ppm)
[0007] In steelworks, the calculated NOx concentration C (O2=15% corrected value) is constantly monitored, and if it exceeds the control value, measures are taken to reduce NOx emissions. For example, one reduction measure is to change the brand of carbon material. In addition, the following technologies have been proposed:
[0008] Patent Document 1 discloses a method for producing sintered ore, which comprises granulating sintering raw materials with a granulation moisture content of 4.0-6.0%, supplying the sintering raw materials to a continuous downward suction sintering machine, and supplying 5.0-90.0 l / t of raw material moisture to the surface of the sintering bed during the coke combustion reaction. Patent Document 2 discloses a method for producing sintered ore, which comprises blending, as sintering raw materials, iron ore containing high water of crystallization iron ore containing 4.0 mass% or more of water of crystallization, auxiliary materials, and solid fuel containing 10 mass% or more of low-temperature combustion solid fuel whose combustion reaction initiation temperature is less than 450°C, so that the high water of crystallization iron ore is contained in the sintering raw materials at 30 mass% or more.
[0009] The technology described in Patent Document 1 reduces the amount of NOx generated by spraying water on the surface of the sintered bed to optimize the ratio between the amount of water sprayed and the amount of water in the blended raw materials, while the technology described in Patent Document 2 reduces the amount of NOx generated by combining high water of crystallization ore with solid fuel (char) and setting the blending ratio of the solid fuel (char) to the high water of crystallization ore to a predetermined amount or more. Note that the technology described in Patent Document 2 is based on the premise that H2 is generated in the calcination zone and NO is reduced there, but it is known that the reduction of NO does not occur in the calcination zone (low temperature) but in the coke gas boundary film (combustion zone). [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Japanese Patent Application Publication No. 61-204342 [Patent Document 2] International Publication No. 2010 / 106756 Summary of the Invention [Problem to be solved by the invention]
[0011] The inventors conducted repeated sintering experiments using a small pot test apparatus and found that even if the blending ratio of carbonaceous material used as sintering fuel is constant, the amount of NOx generated during sintering varies greatly when different brands of iron ore are used. The inventors then discovered that there is a correlation between the crystal water content (average value) of the iron ore in the sintering raw material and the amount of NOx generated. This finding shows the opposite result to the technology disclosed in Patent Document 2, which reduces the amount of NOx generated by using a specified amount or more of high crystal water ore.
[0012] The present invention has been created based on such knowledge, and has an object to provide a new method for producing sintered ore that can suppress an increase in the amount of NOx contained in the sintering exhaust gas. [Means for solving the problem]
[0013] The gist of the present invention is as follows. (1) A method for producing sintered ore in which a mixture of multiple brands of iron ore in a predetermined composition ratio is defined as total iron ore, and the total iron ore is mixed with new raw materials in a predetermined ratio, A method for producing sintered ore, in which, when changing the composition ratio of two or more brands of iron ore in the total iron ore, if the crystal water content of the total iron ore after the change increases compared to before the change, the blending ratio of low-nitrogen anthracite is increased in accordance with the increase in the crystal water content so that the NOx concentration in the exhaust gas does not increase compared to before the composition ratio was changed. (2) calculating a coefficient of increase in NOx concentration Ccw (dNOx / dCW) relative to an increase in the amount of water of crystallization of the total iron ore; A reduction coefficient Cans(dNOx / dAns) of NOx concentration with respect to an increase in the blending ratio of the low nitrogen anthracite is obtained in advance, The method for producing sintered ore according to (1), wherein when the increase in the crystal water content of the total iron ore is Δx, the increase in the blending ratio of the low nitrogen anthracite is (Ccw / Cans)×Δx or more. (3) The method for producing sintered ore according to (2), wherein the unit of the increase in the crystal water content of the total iron ore, Δx, is mass %, and Ccw / Cans is 0.5. Here, low-nitrogen anthracite is anthracite having a nitrogen content lower than that of coke breeze, which is a typical carbon material for sintering. Effect of the Invention
[0014] According to the present invention, when an operational action is taken to change the composition ratio of two or more brands of iron ore in the total iron ore, if the crystallization water content of the total iron ore increases, the blending ratio of low-nitrogen anthracite can be increased in accordance with the increase, thereby suppressing the increase in the amount of NOx in the sintering machine exhaust gas. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a diagram showing the relationship between the crystallization water content of each brand of iron ore and the NOx concentration in the sintering exhaust gas (O2=15% corrected value). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The inventors of the present invention have conducted extensive research to reduce NOx emissions, and have found a correlation that, even if the blending ratio of iron ore in new raw materials is constant, the amount of NOx generated is large when iron ore with a high content of crystal water is used, and the amount of NOx generated is small when iron ore with a low content of crystal water is used. Based on this finding, the inventors of the present invention have devised a method for producing sintered ore by using the average amount of crystal water contained in all iron ores in the blended raw materials (the crystal water content of all iron ores) as an index for managing the NOx emissions in the sintering exhaust gas. Below, we will first explain an experiment that supports the above finding and its results.
[0017] <Basic studies that led to the invention> In order to confirm the NOx emission tendency specific to each brand of iron ore, five experiments (Experiment 1 to Experiment 5) were conducted using a raw material blend in which five brands of iron ore (Iron Ore A to Iron Ore E) were blended together. Experiments 1 to 5 were conducted using a small sintering pot test (100 mm diameter) that mimicked the sintering phenomenon in a sintering machine.
[0018] (Raw material blend) Table 1 shows the blending ratio of each raw material for sintering used in Experiments 1 to 5. As shown in Table 1, the blending ratios of the return ore and the carbonaceous material were set to 15.0 mass% and 4.5 mass%, respectively, with the new raw materials excluding the return ore and the carbonaceous material being taken as 100 mass%.
[0019] [Table 1]
[0020] Table 2 shows the main component amounts (mass%) of each of iron ore A to iron ore E used in experiments 1 to 5. In each of experiments 1 to 5, one iron ore type (one brand) was used alone as the raw iron ore shown in Table 1. For example, in experiment 1, only iron ore A was used as the raw iron ore. As shown in Table 2, iron ore A and iron ore B are pisolite-based iron ores with a high content of combined water of crystallization (CW), and iron ore D and iron ore E are hematite-based ores with a low content of combined water of crystallization. Iron ore C is a Marra Mamba-based iron ore with a lower content of combined water of crystallization than iron ore A and iron ore B, and a higher content than iron ore D and iron ore E.
[0021] [Table 2]
[0022] Table 3 shows the particle size distribution of the iron ore and carbonaceous material used as raw materials. This particle size distribution was obtained by classifying the materials using sieves with mesh sizes of 5.0 mm, 3.0 mm, 1.0 mm, 0.5 mm, and 0.25 mm. For example, the particle size classification "1 mm-0.5 mm" means that the material is on the sieve when sieved using a sieve with 0.5 mm mesh and is on the sieve when sieved using a sieve with 1 mm mesh. The particle size conditions were the same in each of Experiments 1 to 5, and iron ore and carbonaceous material with the particle size distribution shown in Table 3 were used.
[0023] [Table 3]
[0024] (Experimental conditions) Each sintering raw material was mixed in the ratio shown in Table 1, granulated, and the granulated raw material was fired. The main experimental equipment is shown in Table 4.
[0025] [Table 4]
[0026] In the above sintering experiment, the blended raw materials were mixed (dry mixed) for 1 minute at 32 rpm using a drum mixer. After mixing, 7.0% by mass of moisture was added to the blended raw materials and granulated for 4 minutes to produce raw granulated material. First, Kaowool was placed on the grate inside the sintering pot. Next, the raw granulated material was charged into the sintering pot so that the layer thickness was 445 mm. After charging, the raw material surface was heated and ignited in an ignition furnace for 60 [sec], and the air volume (constant) in the wind box was 0.08 [Nm 3 / min].
[0027] (measurement) Gas analysis was performed using a portable gas analyzer PG-350 manufactured by Horiba, Ltd. NOx concentration was measured using a chemiluminescence analysis unit, and oxygen concentration was measured using a zirconia analysis unit.
[0028] (Experimental Results) The rightmost column of Table 5 shows the NOx concentration (O2=15% corrected value) calculated from the measured NOx concentration and oxygen concentration. Also, Figure 1 is a graph showing the relationship between the crystal water content and the NOx concentration (O2=15% corrected value) in Table 5. As shown in Figure 1, there is a correlation between the crystal water content and the NOx concentration (O2=15% corrected value), and it was confirmed that the lower the crystal water content in iron ore, the lower the NOx concentration (NOx emission amount) generated by calcination tends to be.
[0029] [Table 5]
[0030] The NOx concentration increase coefficient Ccw, which indicates the correlation between the crystallization water content and the NOx concentration (O2 = 15% corrected value) derived from Figure 1, is shown in the following formula (2). As shown in formula (2), it was found that when the crystallization water content in iron ore increases by 1% (mass%), the NOx concentration (O2 = 15% corrected value) increases by about 5 ppm. Increase coefficient of NOx concentration Ccw = 5 ppm / increase in crystal water content 1 mass% (2)
[0031] <Embodiment> (The present invention and its features) The present invention was invented by combining the above findings with a method for reducing the amount of NOx using low-nitrogen anthracite (details will be described later). In a method for producing sintered ore in which a mixture of iron ores of multiple brands in a predetermined composition ratio is defined as total iron ore, and the total iron ore is mixed with new raw materials in a predetermined ratio, the present invention is characterized in that, when changing the composition ratio of two or more brands of iron ore in the total iron ore, if the crystal water content of the total iron ore after the change increases compared to before the change, the mixing ratio of low-nitrogen anthracite is increased according to the increase so that the amount of NOx (NOx concentration) in the exhaust gas does not increase compared to before the composition ratio change operation.
[0032] (Change in iron ore composition) The iron ore blended raw material is usually a mixture of multiple brands of iron ore blended in a predetermined ratio. Since the incoming amount and price of each brand of iron ore are not constant but fluctuate, the blending ratio of each brand of iron ore is changed as appropriate. Specifically, the blending ratio (mass%) of the total iron ore in the new raw material (the total of multiple brands of iron ore blended in a predetermined ratio) is not changed, and an operational action is taken to change part or all of the composition ratio of each brand of iron ore in the total iron ore. This operational action is called an operation to change the composition ratio of iron ore. In the following explanation, the total of multiple brands of iron ore blended in a predetermined ratio is called total iron ore or equal iron ore.
[0033] (Water of crystallization content of ore) The crystal water content of the average iron ore is calculated by the following formula (3). Formula (3) shows that the crystal water content CW of the average iron ore is the average crystal water content of all brands of iron ore, and the crystal water content CWi of each brand is calculated by weighting it by the composition ratio of each brand in the average iron ore. CW = Σ(Xi × CWi) / 100 (3) CW: Water of crystallization content of the ore (mass%) Xi: Composition ratio of iron ore type i in the ore balance (mass%) CWi: Water of crystallization content of iron ore grade i (mass%)
[0034] (Low nitrogen anthracite) Next, we will explain low-nitrogen anthracite and the method for reducing NOx amounts using it. In the present invention, low-nitrogen anthracite is defined as anthracite with a lower nitrogen content than coke breeze (nitrogen content is about 1% by mass), which is a typical carbonaceous material for sintering. Since low-nitrogen anthracite has a low nitrogen content, it generates less NOx during combustion than coke breeze. In order to achieve a large NOx reduction effect, it is desirable to use anthracite with a nitrogen content of 0.6% by mass or less. Table 6 shows an example of the properties of coke breeze and low-nitrogen anthracite.
[0035] [Table 6]
[0036] When the crystallization water content of the total iron ore increases due to the change in the composition ratio of iron ore by brand, the amount of NOx in the sintering exhaust gas also increases. In the present invention, the increase in the amount of NOx in the sintering exhaust gas is suppressed by increasing the blending ratio of low-nitrogen anthracite according to the increase in the amount of crystallization water. Preferred embodiments of the present invention will now be described.
[0037] First, the correlation between the amount of NOx in the sintering exhaust gas (NOx) and the content of water of crystallization in the iron ore (CW) is obtained by experiments, regression analysis of operation data, etc., and the increase coefficient Ccw (d1NOx / dCW) is obtained, which indicates the increase in the amount of NOx in the sintering exhaust gas (d1NOx) relative to the increase in the amount of water of crystallization in the iron ore (dCW). In addition, the correlation between the amount of NOx in the sintering exhaust gas and the amount of anthracite used (Ans) is obtained by experiments, regression analysis of operation data, etc., and the reduction coefficient Cans (d2NOx / dAns) is also obtained, which indicates the reduction in the amount of NOx in the sintering exhaust gas (d2NOx) relative to the increase in the blending ratio of anthracite (dAns). Furthermore, when the crystal water content of all iron ore (average crystal water content of all iron ore brands) increases (ΔCW) as a result of changing the composition ratio of iron ore, the blending ratio of low-nitrogen anthracite is increased (ΔAns) in accordance with the increase in the crystal water content so that the amount of NOx (NOx concentration) in the exhaust gas does not increase compared to before the composition ratio change operation. In other words, the increase in the blending ratio of low nitrogen anthracite (ΔAns) should satisfy the following formula (4). ΔAns≧ΔCW×((d1NOx / dCW) / (d2NOx / dAns)) = ΔCW × (Ccw / Cans) (4)
[0038] In the above embodiment, a specific example of the increase coefficient Ccw (d1NOx / dCW) indicating the increase in NOx in the sintering exhaust gas relative to the increase in the amount of crystallization water of iron ore has already been shown as formula (2). Below, a specific example of the reduction coefficient Cans (d2NOx / dAns) indicating the decrease in NOx in the sintering exhaust gas relative to the increase in the amount of anthracite used is shown.
[0039] (Method of reducing NOx using low-nitrogen anthracite) In the present invention, as a measure for reducing the amount of NOx (NOx concentration) in the sintering exhaust gas, the above-mentioned low nitrogen anthracite is used in large amounts as the carbonaceous material instead of coke breeze. The inventors newly conducted an experiment similar to the above-mentioned small sintering pot test to confirm the effect of reducing the amount of NOx when low nitrogen anthracite was used. Specifically, in the above-mentioned small sintering pot test, the NOx amount when coke breeze was used alone as the carbonaceous material blended at an additional 4.5 mass% was first confirmed, and then the NOx amount when the coke breeze was gradually replaced with low nitrogen anthracite in equal amounts was recorded, and the relationship between the amount of replacement with low nitrogen anthracite and the amount of reduction in NOx concentration was quantified. As a result, as shown in the following formula (5), the amount of NOx generation was reduced by 10 ppm per 1 mass% of replacement with low nitrogen anthracite. For the iron ore in Table 1, a mixture of iron ores of multiple brands was used as shown in Table 7. NOx concentration reduction coefficient Cans = 10 ppm / amount of low-nitrogen anthracite replaced by 1 mass% (5)
[0040] [Table 7]
[0041] (Adjustment of NOx amount in exhaust gas based on increase in total iron ore water of crystallization content) According to the above formula (2), when the increase in the crystal water content is 1 mass%, the NOx concentration increases by 5 ppm. Furthermore, according to the above formulas (4) and (5), in order to suppress the increase in the NOx concentration, the low-nitrogen anthracite replacement amount should be 0.5 mass%. That is, in order to prevent the NOx concentration from increasing after the composition ratio change operation of the iron ore, the low-nitrogen anthracite replacement amount should be (0.5 x Δx) mass% or more for the increase in the crystal water content Δx mass%, and the suppression effect coefficient for suppressing the increase in the NOx concentration is 0.5. EXAMPLES
[0042] Using the raw materials having the blending ratios shown in Table 8, an experiment similar to the above-mentioned small sintering pot test was carried out to verify the effects of the above-mentioned invention. As shown in Table 8, the NOx concentration in the sintering exhaust gas was measured before and after changing the composition ratio of multiple brands of iron ore. The crystallization water content in the total iron ore was increased after the change compared to before the change in the composition ratio of multiple brands of iron ore, so the blending ratio of low-nitrogen anthracite, which is a carbonaceous material, was increased. Specifically, since the crystallization water content in the total iron ore increased by 1.5 mass% compared to before the change, based on the above-mentioned inhibition effect coefficient value (0.5), the fine coke was replaced with low-nitrogen anthracite at an amount of 0.75 mass% of the new raw material.
[0043] [Table 8]
[0044] As shown in the rightmost column of Table 8, it was confirmed that the NOx concentration in the sintering exhaust gas did not increase even after the composition ratio of the iron ore was changed.
[0045] In this embodiment, the relationship between the amount of low-nitrogen anthracite replaced with low-nitrogen anthracite and the amount of NOx concentration reduction was determined for the low-nitrogen anthracite and powdered coke shown in Table 6. However, when using other low-nitrogen anthracite with a different nitrogen content and / or other powdered coke with a different nitrogen content, it is desirable to conduct a new sintering pot test and determine the relationship between the amount of low-nitrogen anthracite replaced with low-nitrogen anthracite and the amount of NOx concentration reduction (NOx concentration reduction coefficient Cans).
Claims
1. In a method for producing sintered ore, a mixture of iron ores of a plurality of brands in a predetermined composition ratio is defined as total iron ore, and the total iron ore is mixed with new raw materials in a predetermined ratio, A method for producing sintered ore, in which, when changing the composition ratio of two or more brands of iron ore in the total iron ore, if the crystal water content of the total iron ore after the change increases compared to before the change, the blending ratio of low-nitrogen anthracite is increased in accordance with the increase in the crystal water content so that the NOx concentration in the exhaust gas does not increase compared to before the composition ratio was changed.
2. The increase coefficient Ccw (d 1 NOx / dCW) was calculated, The NOx concentration reduction coefficient Cans (d 2 NOx / dAns) was calculated, 2. The method for producing sintered ore according to claim 1, wherein when the increase in the crystal water content of the total iron ore is Δx, the increase in the blending ratio of the low nitrogen anthracite is (Ccw / Cans)×Δx or more. however, d1NOx: Increase in NOx in sintering exhaust gas dCW: Increase in the amount of crystal water in iron ore d2NOx: reduction amount of NOx in sintering exhaust gas dAns: Increase in the blend ratio of anthracite
3. The method for producing sintered ore according to claim 2, wherein the unit of the increase amount Δx of the crystal water content of the total iron ore is mass %, and Ccw / Cans is 0.5.
Citation Information
Patent Citations
Manufacture of sintered ore
JP1986204342A
Operating method for sintering low in NOX
JP1990085324A
Method for reducing NOX of sintering exhaust gas
JP2021031749A
Carbonaceous material for sintering iron ore
WO2010087468A1
Process for producing sintered ore
WO2010106756A1