Melting method of molten iron using converter type refining furnace
By adjusting CaO-based auxiliary material calculations based on the rate of change in slag surface height, the method addresses slag mass estimation inaccuracies, optimizing raw material use and maintaining effective P removal in molten iron smelting processes.
Patent Information
- Application Number
- JP2021044757
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-18
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2041-03-18
AI Technical Summary
Existing methods for smelting molten iron in converter-type furnaces face challenges in accurately estimating the mass of slag to be removed during the intermediate slag removal process, leading to variations that require excessive addition of CaO sources to maintain proper P removal, resulting in inefficiencies and increased costs.
The method adjusts the calculation of CaO-based auxiliary materials by considering the rate of change in slag surface height during the hot metal pretreatment process, using the equation W' CaO = a·(1/h foam -1/h' foam ) + W CaO + E CaO to determine the exact amount needed for decarburization, thereby accounting for variations in slag density.
This approach reduces the excessive addition of CaO sources, maintaining effective P removal while optimizing raw material usage and minimizing operational issues.
Smart Images

Figure 0007575684000002 
Figure 0007575684000003 
Figure 0007575684000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for smelting molten iron using a converter-type refining furnace, in which molten iron is refined by successively carrying out a molten iron pretreatment process, an intermediate slag removal process, and a decarburization process using the converter-type refining furnace. [Background technology]
[0002] In converter-type refining furnaces, oxygen is supplied to the molten iron to decarbonize it and produce steel through blowing. Prior to this decarbonization process, it is common to perform pretreatment of the molten iron to remove silicon and phosphorus from the molten iron, and the process up to decarbonization is called primary refining. Methods for pretreatment of molten iron include desiliconization in a torpedo car, which is a vessel for transporting molten iron, and using a converter-type refining furnace exclusively for dephosphorization, but the most widely used method is to perform desiliconization, dephosphorization, and decarbonization in a single converter-type refining furnace.
[0003] Patent Document 1 discloses a technique in which, as a first step, scrap iron and molten iron are charged into a top and bottom blowing converter, as a second step (molten iron pretreatment step), dephosphorization is performed by adding flux and blowing acid, as a third step (intermediate slag removal step), the converter is turned over on its side to remove the slag generated in the second step, as a fourth step (decarburization step), decarbonization and dephosphorization are performed to a predetermined [C] and [P] by adding flux and blowing acid, as a fifth step, steel is tapped while leaving the slag generated in the fourth step, as a sixth step, the furnace is turned upright, and carbonaceous material is added while performing bottom blowing stirring to reduce the amount of FeO in the slag, and the process returns to the first step, and the process is repeated up to the sixth step. This technology is widely used as a primary refining method because it enables hot recycling of slag, allows for large amounts of scrap to be input, and reduces the amount of slag generated.
[0004] When refining molten iron using the above-mentioned method, the slag removal rate of the slag discharged in the intermediate slag removal process (=mass of slag removed / mass of slag in the furnace before removal) has a large effect on the refining performance in the decarburization process and after. In the deP reaction, the ratio of P in the molten iron to P in the slag (hereinafter referred to as P distribution) is determined according to the ratio of CaO to SiO2 in the slag (CaO / SiO2 mass ratio, hereinafter referred to as basicity C / S). Therefore, in the final deP process in the decarburization process, the higher the slag removal rate in the intermediate slag removal process, the less slag generated in the converter during the hot metal pretreatment process will remain in the furnace, and the more CaO source can be saved in the subsequent decarburization process.
[0005] Prior to the intermediate slag-removal process, in the hot metal pretreatment process, the C in the hot metal reacts with the FeO in the slag, unavoidably generating CO gas, which causes the slag to foam, a phenomenon known as foaming. In the intermediate slag-removal process, the converter-type refining furnace is tilted to discharge the foamed slag outside the furnace. By making the slag foam as much as possible in the hot metal pretreatment process without interfering with operation, the slag volume in the converter before intermediate slag-removal can be increased, and the amount of slag to be removed can be increased. However, since it is difficult to directly observe the inside of a converter-type refining furnace during blowing, a technology has been developed to grasp the height of the top surface of the slag (hereinafter referred to as the slag surface) using microwaves.
[0006] Patent Document 2 discloses a technique for measuring the slag height in a refining furnace using a microwave radar-type slag level meter. This technique makes it possible to grasp the time-varying behavior of the slag surface during blowing in a converter in real time, and therefore makes it possible to take action such as changing the blowing conditions, such as the oxygen supply rate, according to the slag surface height (hereinafter also referred to as the slag level), and by stopping blowing when the slag surface height reaches the top of the converter-type refining furnace, it is possible to increase the amount of slag to be discharged.
[0007] In the hot metal pretreatment process, when the slag level in the converter-type refining furnace reaches a certain level, there is a concern that the slag will overflow from the refining furnace, and therefore the deP treatment cannot be continued any further. For this reason, Patent Document 3 discloses a technique in which "the slag level in the hot metal ladle is measured, and at the same time, the weight of the hot metal in the hot metal ladle is measured, and the level of the hot metal is calculated from the obtained values, and when the difference between the measured value and the calculated value exceeds a predetermined value, a predetermined amount of foaming inhibitor is added to the hot metal ladle to advance the desiliconization reaction of the hot metal." This technique utilizes the measured slag level itself.
[0008] On the other hand, when considering increasing the mass of slag removed in the intermediate slag removal process, the volume of the converter-type refining furnace does not change, the volume of molten pig iron in the furnace is almost constant, and the critical slag surface height that does not cause operational trouble is also determined, so the volume of the slag that has risen to the critical slag surface height in the converter before intermediate slag removal is constant. If the tilting angle of the refining furnace during slag removal is also constant, the volume of slag remaining in the converter during intermediate slag removal is also constant, so the volume of the removed slag is also constant. Therefore, in order to increase the mass of the removed slag, it is necessary to create foamed slag with the highest possible density as the removed slag.
[0009] As a technique for adjusting the density of foamed slag, Patent Document 4 discloses a technique for adjusting the density of slag in a converter-type refining furnace by changing the generation rate of CO gas generated in the furnace during refining treatment. According to this technique, the degree of slag foaming can be changed by the generation rate of CO gas generated by the reaction of a gaseous oxygen source and a solid oxygen source supplied into the furnace with carbon in the molten iron, and the slag density tends to decrease as the CO gas generation rate increases. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Japanese Patent Application Publication No. 05-140627 [Patent Document 2] Japanese Patent Application Publication No. 03-281717 [Patent Document 3] Japanese Patent Application Publication No. 08-143925 [Patent Document 4] JP 2015-218338 A Summary of the Invention [Problem to be solved by the invention]
[0011] When treating molten iron using the method of Patent Document 1, the initial slag mass and composition in the molten iron pretreatment process can be calculated from the slag mass and composition in the previous ch and the mass and composition of the auxiliary materials added before the molten iron pretreatment process. Since almost all of the Si in the molten iron is oxidized in the molten iron pretreatment process, the slag mass and composition at the end of the molten iron pretreatment process can be calculated from the mass and composition of the auxiliary materials added in the molten iron pretreatment process, and when the mass of the slag removed during the intermediate process is known, the mass of the auxiliary materials containing CaO to be added in the decarburization process can be calculated according to the target P concentration.
[0012] The problem at this time is the variation in the mass of the slag discharged in the intermediate slag discharge process. When the slag surface height in the furnace at the end of the hot metal pretreatment process is constant and the tilting angle of the converter-type refining furnace in the intermediate slag discharge process is kept constant, the volume of the discharged foamed slag can be estimated as a constant value, as described above. The mass of the discharged slag can be estimated by multiplying the volume of the discharged foamed slag by the apparent density of the discharged foamed slag. However, when the mass of the slag discharged in the intermediate slag discharge process is measured with a weighing machine, it was found that the mass of the discharged slag varies even if the slag that has been foamed to the same height by the slag level meter is discharged at the same tilting angle, i.e., even if the same volume of slag is discharged. This variation is large, and if the mass of slag to be discharged is estimated to be less than the actual mass to be discharged, auxiliary materials will be added in a state where a larger mass of slag than calculated actually remains in the converter-type refining furnace, resulting in a lower slag basicity C / S than the slag basicity C / S set according to the target P concentration, resulting in poor deP. In order to avoid poor deP, the problem was that there was no choice but to add an excess of CaO source to make the basicity C / S higher than the basicity set according to the target P concentration, taking the variation into account.
[0013] Therefore, an object of the present invention is to provide a method for producing molten iron using a converter-type refining furnace, which is capable of producing molten iron without adding an excessive amount of CaO source. [Means for solving the problem]
[0014] As a result of intensive research by the present inventors in order to solve the above-mentioned problems, it was found that the cause of the variation in the mass of the slag discharged is the difference in density of the foamed slag discharged, and that even if the height of the slag surface in the converter-type refining furnace at the end of the hot metal pretreatment process is the same, the mass of the slag discharged differs depending on the rising speed of the slag surface height. That is, the apparent density of the slag discharged when estimating the mass of the slag discharged was conventionally treated as a constant value, but it was found that when the rising speed of the slag surface height is slow, the bubbles in the foamed slag are small and the apparent density of the foamed slag discharged is large, and conversely, when the rising speed of the slag surface height is fast, the bubbles in the foamed slag are large and the apparent density of the foamed slag discharged is small. In intermediate slag discharge, the slag in the upper layer of the slag in the converter-type refining furnace is preferentially discharged. When the rate at which the slag surface height rises is slow compared to when the rate at which the slag surface height rises is fast, it can be estimated that the density of the slag in the upper layer of the slag in the converter-type refining furnace before intermediate slag removal is relatively high.
[0015] Based on this knowledge, even if the volume of slag discharged in the intermediate slag discharge process after the hot metal pretreatment process is constant, the density of the discharged slag changes depending on the rate of rise of the slag surface height, so that the apparent density used to estimate the mass of the discharged slag can be adjusted according to the rate of rise of the slag surface height, thereby improving the accuracy of estimating the mass of the discharged slag. In addition, the relationship between the rate of rise of the slag surface height and the mass of the auxiliary material added in the decarburization process can be obtained, and the amount of the auxiliary material added can be directly adjusted. It would seem that the above-mentioned operations would be unnecessary if the mass of the slag discharged was directly measured using a weighing machine; however, since the discharged slag contains iron particles that were scattered into the slag during the blowing process in the hot metal pretreatment process, an error would occur if the slag mass measured by the weighing machine was directly used. In addition, the mass of the slag discharged by the weighing machine is determined after the intermediate slag discharge process, which means that it will be too late to prepare the auxiliary materials to be added in the first half of the decarburization process.
[0016] The present invention was conceived based on the above-mentioned considerations, and was completed by clarifying the relationship between the rate of rise of the slag surface height and the mass of the added auxiliary material. The specific means are as follows. [1] A method for producing molten iron, comprising the steps of: a molten iron pretreatment process in which slag and molten iron are blown into a converter-type refining furnace to remove silicon and phosphorus; an intermediate slag removal process in which the furnace is tilted to remove the slag from the converter-type refining furnace; and a decarburization process in which CaO-based auxiliary materials are added to the converter-type refining furnace and blown into the furnace to remove carbon and final phosphorus, the method comprising the steps of measuring the slag surface height at the end of the molten iron pretreatment process and determining the CaO consumption rate in the auxiliary materials to be added in the decarburization process according to the rate of change of the slag surface height. [2] A method for producing molten iron, characterized in that, when producing molten iron by the method for producing molten iron described in the above item [1], a basic unit of CaO in the auxiliary raw materials to be added is determined according to formula (1). W' CaO =a (1 / h foam -1 / h' foam )+W CaO +E CaO (1) W' CaO : CaO unit consumption in added auxiliary material (kg / ton) h' foam : Actual change rate of slag surface height (m / s) a: constant h foam : Average speed of change of slag surface height (m / s) W CaO : The rate of change of the slag surface height is h foam Under the above conditions, the thermodynamically necessary CaO consumption unit (kg / ton) in the auxiliary raw material is determined according to the target P concentration and temperature. E CaO : Unit of CaO content in auxiliary materials added to reduce deP defects and variations (kg / ton) Effect of the Invention
[0017] According to the present invention, it is possible to reduce the amount of auxiliary materials added in excess in the decarburization process, and also to reduce the rate of deP defects in the decarburization process. [Brief description of the drawings]
[0018] [Figure 1] Processing flow [Diagram 2] Relationship between CaO unit consumption in added auxiliary materials and [%P] after decarburization treatment DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] [Terminology definition] In the present invention, molten iron refers to molten pig iron and molten steel. In the decarburization process, the C content in the molten pig iron decreases to turn into molten steel, but in the present invention, the molten iron in the furnace is generally referred to as molten iron.
[0020] Auxiliary materials are refining agents added to converter-type refining furnaces mainly for the purpose of slag formation during the hot metal pretreatment process, decarburization process, and before and after these processes. They include quicklime, limestone, dephosphorization slag, decarburization slag, iron ore, sintered ore, dust, dolomite, calcium ferrite, silica, manganese ore, and recycled products containing oxides generated in the ironmaking process, including blast furnaces. The components of the auxiliary materials are analyzed in advance, so the mass of each component can be calculated according to the amount added. CaO-based auxiliary materials refer to auxiliary materials with a Ca content of 50% or more calculated as CaO. The CaO unit consumption refers to the amount of CaO per mass of molten iron, calculated by multiplying the mass of auxiliary materials containing CaO by the CaO concentration, and dividing the result by the mass of molten iron. It is often expressed in units of kg / ton.
[0021] [Processing Procedure] The present invention is intended to refine molten iron by successively carrying out a hot metal pretreatment process using a converter-type refining furnace, which performs desiliconization and phosphorus removal by blowing in a state where slag and molten iron coexist, an intermediate slag removal process in which the furnace is tilted to remove the slag from the furnace, and a decarburization process in which CaO-based auxiliary materials are added to the furnace and blown therein to perform decarbonization and final dephosphorization, and is intended to be carried out mainly from the end of the hot metal pretreatment process to the beginning of the decarburization process among a series of processes for desiliconization, dephosphorization, and decarbonization. The following will be explained with reference to Fig. 1. In Fig. 1, (A) shows the hot metal charging process, (B) shows the hot metal pretreatment process, (C) shows the intermediate slag removal process, (D) shows the decarburization process, and (E) shows the steel tapping.
[0022] When molten iron is produced using one converter-type refining furnace 1, after the decarburization process of the front charge is completed, the molten iron 3 is tapped (see FIG. 1(E)), and the furnace body is tilted to discharge the slag (not shown) so that some of the slag remains in the furnace. The volume of the slag remaining in the front charge can be calculated according to the tilt angle of the furnace body. Since the slag in the converter-type refining furnace at this time is not foamed, it can be converted to the slag mass by multiplying it by the slag density obtained in advance.
[0023] After that, to refine the molten iron in the ch, the molten iron is charged from the pouring ladle 2 into a converter-type refining furnace 1 as shown in Figure 1(A), and in addition, iron sources such as scrap and auxiliary materials for slag production are added. The amount of CaO-based auxiliary materials required in the hot metal pretreatment process shown in Figure 1(B) can be calculated from information such as the Si in the molten iron, the molten iron temperature, the blast furnace hot metal blending ratio, and the mass of slag carried over from the previous ch. Since almost all of the Si in the molten iron is oxidized by blowing using the oxygen supply lance 5 in the hot metal pretreatment process, the slag basicity C / S at the end of the hot metal pretreatment can be calculated. At the end of the hot metal pretreatment, Si in the hot metal is oxidized, and the reaction between the oxygen blown from the oxygen supply lance 5 and the C in the hot metal as well as between FeO in the slag and the C in the hot metal becomes active, causing foaming of the slag 4 in the furnace. If the foamed slag 4 is blown directly from the top of the furnace, it will hinder operation. In addition, if the furnace body is tilted after reaching the top of the furnace, the slag removed during tilting may burn the auxiliary equipment of the converter. Therefore, when the top surface (slag surface) of the foamed slag 4 reaches a predetermined height, blowing in the hot metal pretreatment is usually stopped and the intermediate slag removal process is started. In the present invention, the measurement result of the slag surface height at the end of the hot metal pretreatment using the slag surface meter 6 is used to determine the completion of the hot metal pretreatment process as well as to calculate the amount of auxiliary materials to be added in the decarburization process. The rate of change in the slag surface height used in calculating the amount of auxiliary raw materials to be added is calculated by measuring the slag surface height multiple times within about one minute before the blowing is stopped, and using a method such as the least squares method.
[0024] In the intermediate slag removal process shown in Fig. 1(C), the furnace body of the converter-type refining furnace 1 is tilted to remove slag so that the amount of CaO added in the decarburization process can be reduced and the maximum amount of slag is removed without discharging molten iron. A slag removal ladle 7 is placed on a cart 8, and the slag 4 discharged from the converter-type refining furnace 1 is stored in the slag removal ladle 7.
[0025] The volume of the discharged slag is determined by the height of the foamed slag at the end of the hot metal pretreatment and the tilting angle of the furnace body, but as mentioned above, the density of the discharged foamed slag varies, so the mass of the discharged slag changes even if the volume is constant. Therefore, the mass of the slag remaining in the furnace after intermediate slag discharge, which is necessary for calculating the amount of CaO to be added in the decarburization process, also changes, so the amount of CaO required to obtain the target P concentration changes even if the volume of the discharged slag is the same.
[0026] In the conventional process, the CaO unit D in the auxiliary material added in the decarburization process shown in Figure 1(D) is CaO (kg / ton) can be determined as follows. Since the molten iron after decarburization is vigorously stirred in the high-temperature environment of a converter-type refining furnace, the P distribution, which is the ratio of the P concentration in the slag to the P concentration in the molten iron, is determined largely by the temperature and slag composition, particularly the basicity C / S, at the end of the decarburization process. P distribution is one of the indices that includes thermodynamic elements, and is greatly influenced by the basicity C / S in the slag. Once the P distribution is determined, the P concentration in the molten iron and the P2O5 concentration in the slag can be calculated according to the amounts of molten iron and slag. Since the thermodynamically required basicity C / S is determined according to the target P concentration and target temperature at the end of the decarburization process, the thermodynamically required CaO consumption unit W in the auxiliary raw materials can be determined according to the slag condition after the intermediate slag removal process. CaO (kg / ton) is determined. D CaO W CaO The CaO basic unit E in the auxiliary material added to reduce variation CaO (kg / ton) is added.
[0027] In the present invention, the rate of change in the slag surface height, h', measured at the end of the hot metal pretreatment process foam According to the speed (m / s), the CaO consumption unit W' in the auxiliary material is calculated from the following formula (1). CaO (kg / ton) can be calculated. CaO Compared to the E CaO The feature of the present invention is that it is possible to reduce W' CaO =a (1 / h foam -1 / h' foam )+WCaO +E CaO (1)
[0028] Derivation of Equation (1) Here, the derivation of formula (1) will be explained. The mass of slag in the hot metal pretreatment process (mass of slag in the furnace before intermediate slag removal) is W1 (kg), the basicity C / S of the slag is B1 (-), the CaO concentration in the slag is %CaO, the SiO2 concentration is %SiO2, and the volume of foamed slag removed in the intermediate slag removal process is V1 (m 3 ), and the density of the discharged foamed slag is ρ1 (kg / m 3 ), the mass of slag remaining in the furnace after intermediate slag draining is W2 (kg), and the slag basicity C / S during the decarburization process is B2 (-). The volume V1 of the foamed slag to be drained can be estimated by estimating the slag volume before slag draining from the height of the slag surface in the furnace at the end of the molten iron pretreatment process, and the volume of slag remaining in the furnace can be estimated from the tilting angle of the slag draining during intermediate slag draining, so V1 can be obtained as the difference between the two volumes. The basicity B2 should be determined in advance for each type of slag being produced. The amount of CaO to be added during the decarburization process is A CaO (kg). In this case, equations (2) and (3) hold. B1 = %CaO / %SiO2 (2) B2 = (W2 × %CaO / 100 + A CaO ) / (W2×%SiO2 / 100) (3) Furthermore, when considering mass balance, equation (4) holds true. W2 = W1 - V1 × ρ1 (4)
[0029] Here, the greater the rate of change in the slag surface height, the smaller the density of the foamed slag that is discharged. Based on this, the average rate of change in the slag surface height h foam In terms of m / s, ρ1=b1 / h foam Experiments have shown that the rate of change of the average slag surface height can be expressed as follows: where b1 is a constant. Also, the rate of change of the average slag surface height h foamcan be calculated by averaging several charges using the actual rate of change in slag surface height under similar refining conditions, i.e., the Si concentration in the molten iron before treatment, the amount of slag carried over from the previous charge, the amount of auxiliary materials added in the molten iron pretreatment process, and conditions close to the target C / S basicity.
[0030] Furthermore, by modifying equations (2), (3), and (4), the amount of CaO added in the decarburization process, A CaO Factoring out (kg), we get equation (5). (Reference: Intermediate formula) B2 = (W2 × %CaO / 100 + A CaO ) / (W2×%SiO2 / 100) (3) W2×%SiO2 / 100×B2=W2×%SiO2 / 100×B1+A CaO Transform equation (3) and substitute equation (2) A CaO =W2×%SiO2 / 100×B2-W2×%SiO2 / 100×B1 A CaO = W2 × % SiO2 / 100 × (B2-B1) A CaO =(W1-V1×b1 / h foam )×%SiO2 / 100×(B2-B1) ···(5) A in equation (5) CaO The value obtained by dividing the amount of molten iron (kg) by the amount of molten iron (tons) is the W CaO (kg / ton), and the average rate of change of the slag surface height h foam It can be seen that B2 is the CaO consumption rate added in the decarburization process under the condition of (m / s). Also, B2 is the set basicity C / S thermodynamically required to obtain the target P concentration.
[0031] (5) A shown in Eq. CaO (kg) is the rate of change of the average slag surface height h foam (m / s), the amount of CaO required is h' foam (m / s), ρ1 changes according to the rate of change, and the mass of slag remaining in the furnace changes, so it is necessary to add an amount of CaO that corresponds to the change.foam Based on the formula, the rate of change of the slag surface height h' foam (m / s) CaO amount A' required CaO (kg) can be expressed by equation (6). A' CaO =(W1-V1×b1 / h' foam )×%SiO2 / 100×(B2-B1) ···(6) Equation (6) - Equation (5) A' CaO -A CaO =(1 / h foam -1 / h' foam )×V1×b1×%SiO2 / 100×(B2-B1) A' CaO =(1 / h foam -1 / h' foam )×V1×b1×%SiO2 / 100×(B2-B1)+A CaO Where: V1×b1×%SiO2 / 100×(B2-B1)=b2 (8) If we replace it with A' CaO =b2×(1 / h foam -1 / h' foam )+A CaO (7)
[0032] A' shown in equation (7) CaO The rate of change of the slag surface height is h' foam (m / s), which is the amount of CaO required under conditions that have changed from 0.01 to 0.1 (m / s); dividing this by the amount of molten iron (tons), and replacing b2 in equation (8) above with a, results in the first and second terms on the right-hand side of equation (1) above. The left-hand side of equation (8) is a function with variables V1, %SiO2, B2, and B1, but these variables can be treated as approximately constants if the same type of material is being refined, so a can also be treated as a constant if the same type of material is being melted.
[0033] (1) E on the right side of Eq. CaOIn addition to the CaO described above, CaO is added so that deP is not insufficient in response to variations in the deP ability and P concentration of the slag, and can be determined based on the actual results of the slag composition and P concentration at the end of the decarburization process. Generally, a value of up to about 3 kg / ton is sufficient, and it is often set to about 1 to 2 kg / ton. In the present invention, since the rate of change of the slag surface height is taken into consideration, it is possible to set the amount of CaO to a smaller amount than the amount added in excess in the conventional manufacturing method, which is affected by variations in the density of the foamed slag.
[0034] The constant a in equation (1) can be calculated from the rate of change of the slag surface height, the CaO consumption rate, and the actual value of the P concentration in the molten iron after the decarburization process. By using equation (1), the h' foam When the CaO consumption rate W' in the auxiliary raw material is found, CaO It is possible to calculate the amount of wastewater (kg / ton) and proceed with the extraction of auxiliary materials during intermediate slag removal.
[0035] The above describes formula (1) for calculating the unit CaO consumption to be added in the decarburization process from the rate of change of the slag surface height. However, the method for calculating the unit CaO consumption is not limited to this. The relationship between the rate of change of the slag surface height and the density of the foamed slag may be obtained, and the CaO unit consumption may be calculated using the density of the foamed slag corresponding to the rate of change of the slag surface height. Alternatively, the relationship between the rate of change of the slag surface height and the mass of the slag discharged may be obtained, and the CaO unit consumption may be calculated using the amount of slag discharged corresponding to the rate of change of the slag surface height.
[0036] [How to check the effect] The effect of the invention was confirmed by comparing the P concentration achieved after decarburization treatment when the same steel type was melted and confirmed that when the amount of CaO added was reduced, the P concentration achieved did not change, but when the amount of CaO added was increased, the P concentration achieved decreased. EXAMPLES
[0037] According to the flow shown in Figure 1, the hot metal was desiliconized, dephosphorized, and decarbonized in the same converter-type refining furnace. The amount of processing in the converter-type refining furnace 1 was about 420 tons, including iron sources such as scrap, and auxiliary materials such as quicklime, limestone, and iron ore were added in the first half of the hot metal pretreatment as auxiliary materials for adjusting the basicity C / S and for cooling. The calculated slag amount at the end of the hot metal pretreatment shown in Figure 1(B) was about 30 tons, and the basicity C / S was about 1.1. During the hot metal pretreatment, the slag level in the furnace was measured using a slag level gauge 6 attached to the top of the furnace body while blowing. In the second half of the hot metal pretreatment, slag foaming occurred, and blowing was stopped when the slag level reached a predetermined critical height. The invention example and the comparative example each had 8 channels, and in order to match the conditions, the channel with a P concentration of 0.077% in the analysis results of a sample taken after the hot metal pretreatment was selected.
[0038] In the comparative example, the CaO consumption rate D required to adjust the basicity to C / S=3.0 during the decarburization process is determined in advance assuming that the target P concentration at the end of the decarburization process is 0.015%, the temperature is 1630°C, and the slag discharge amount is constant. CaO In all comparative examples, the auxiliary materials satisfying the thermodynamic requirement of CaO consumption W CaO The CaO unit E in the auxiliary raw material added to reduce dephosphorization and variation is 19.5 kg / ton. CaO was calculated at 1.5kg / ton. As a result, D CaO =W CaO +E CaO =21.0kg / ton.
[0039] On the other hand, in the example of the present invention, the CaO consumption rate W CaO and the rate of change in slag surface height h' obtained from the time-dependent change in slag surface height during the final 60 seconds of hot metal pretreatment. foam The average slag surface height change rate h, which was previously obtained from the time-dependent change in the slag surface height under similar refining conditions, foam = 0.06m / s. Substituting these values into equation (1), we obtain the CaO consumption unit W' required to adjust the basicity to C / S during decarburization. CaO The standard average slag surface height change rate h foamAt 0.06 m / s, the thermodynamically necessary CaO consumption unit W CaO The CaO unit E in the auxiliary raw material added to reduce dephosphorization and variation is 19.5 kg / ton. CaO It was found that it could be handled at a constant value of 0.50 kg / ton, so these values were adopted for calculation. The constant a was calculated by referring to past performance data and calculating the correlation between the amount of CaO added and the rate of change in the slag surface height when [%P] at the end of the decarburization process was 0.015%, and the constant a was set to 0.15 for these refining conditions.
[0040] In the decarburization process shown in Figure 1(D), prepared auxiliary materials containing CaO were added in the first half of the process and blown, followed by finish deP and deC treatment. After the treatment, molten iron samples were taken and the [%P] concentration in the molten iron was analyzed. Table 1 shows the rate of change in slag surface height, the CaO consumption rate in the added auxiliary materials, and the [%P] concentration in the molten iron after decarburization treatment for the present invention and comparative examples.
[0041] [Table 1]
[0042] CaO unit consumption W' obtained in the present invention CaO As a comparison example, CaO The relationship between the CaO consumption rate in the auxiliary raw material and [%P] after decarburization treatment when D is added is shown in Figure 2. CaO As a result of adding 21.0 kg / ton, the [%P] after treatment was 0.013% to 0.015%. (All of the targets for [%P]≦0.015 were met, but some showed a tendency to remove excess P.)
[0043] On the other hand, the CaO basic unit E in the auxiliary raw material added to reduce deP defects and variations CaO to 0.50 kg / ton, and the CaO consumption unit W' calculated using equation (1) CaO In the invention example where W' was added (white circle in Figure 2), the [%P] after treatment was 0.014% to 0.015%. CaOHowever, the D added in the comparative example CaO =21.0kg / ton. W' under the condition where the rate of change in slag surface height due to forming was the largest (Example 18) CaO The amount of SiO2 added was 20.9 kg / ton, which was close to that of the comparative example. This is thought to be because the rate of change in the slag surface height due to foaming was large, so the apparent density of the slag discharged in the intermediate slag discharge process was small and the amount of SiO2 remaining in the furnace was large. In addition, W' under the condition (invention example 1) in which the rate of change in the slag surface height due to foaming was the smallest was CaO The rate of change in the slag surface height due to foaming was small, so the apparent density of the slag discharged in the intermediate slag discharge process was large and the amount of SiO2 remaining in the furnace was small. As mentioned above, the rate of change in the slag surface height at the end of the hot metal pretreatment, h' foam According to the formula (1), the CaO consumption rate W' CaO It was found that by optimizing the above, it was possible to reduce the CaO consumption rate while maintaining the deP capacity.
[0044] In the embodiment, the constant a is 0.15, and the average slag surface height change rate h foam = 0.06m / s, CaO consumption rate W required to adjust basicity C / S during decarburization treatment CaO = 19.5 kg / ton, CaO unit E in auxiliary materials added to reduce deP defects and variations CaO However, these values can be adjusted according to the refining conditions such as the target P concentration and temperature, and are not limited to the examples described in the examples. [Explanation of symbols]
[0045] 1: Converter-type refining furnace 2: Pouring pot 3: Molten iron 4: Slug 5: Oxygen supply lance 6: Slag level gauge 7: Slag pan 8: Cart
Claims
1. A method for producing molten iron, comprising the steps of: a molten iron pretreatment process using a converter-type refining furnace to perform desiliconization and dephosphorization by blowing in a state in which slag and molten iron coexist; an intermediate slag removal process in which the furnace is tilted to remove the slag from the converter-type refining furnace; and a decarburization process in which CaO-based auxiliary materials are added to the converter-type refining furnace and then blown thereinto to perform decarbonization and finish dephosphorization, characterized in that the slag surface height at the end of the molten iron pretreatment process is measured and the CaO basic unit of the auxiliary materials to be added in the decarburization process is determined in accordance with the rate of change of the slag surface height.
2. 2. A method for producing molten iron according to claim 1, characterized in that, in producing molten iron, a basic unit of CaO in the auxiliary raw materials to be added is determined according to formula (1). W' CaO =a・(1 / h foam -1 / (' foam )+W CaO +E CaO (1) W' CaO : CaO unit content in added auxiliary raw material (kg / ton) h' foam :Actual change rate of slag surface height (m / s) a: constant h foam : Average slag surface height change rate (m / s) W CaO : The rate of change of the slag surface height is h foam Under the conditions, the thermodynamically necessary CaO consumption unit (kg / ton) in the auxiliary raw material is determined according to the target P concentration and temperature. E CaO : CaO basic unit (kg / ton) in auxiliary raw material added to reduce deP failure and variation
Citation Information
Patent Citations
Method and instrumetn for measuring slag level in converter
JP1991281717A
Steelmaking method in converter
JP1993140627A
Method for desiliconizing molten iron
JP1996143925A
Slag sampling method during blowing
JP2013104069A
Molten iron refining method by converter type refining furnace
JP2015218338A