Continuous synthesis of carbon nanotubes
The plasma-treated catalyst method addresses the challenges of uniformity and dispersibility in carbon nanotube synthesis, achieving high-yield, stable, and branched nanotubes suitable for electrochemical applications.
Patent Information
- Application Number
- JP2023551943
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-09
- Filing Date
- 2021-10-14
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2041-10-14
AI Technical Summary
Conventional methods for synthesizing carbon nanotubes face challenges in producing uniform-sized nanotubes with controlled diameter, require separate reducing agents, and struggle with the formation of branched structures, leading to issues with dispersibility and hydrophilicity, which are crucial for applications requiring two- or three-dimensional structures.
A method involving plasma treatment of metal salts to produce metal nanoparticles without a reducing agent, followed by controlled particle size synthesis of catalysts, and using pretreated carbon nanotubes as carriers to enhance hydrophilicity and specific surface area, allowing for the production of branched carbon nanotubes.
This method enables the production of carbon nanotubes with uniform size and improved reactivity, increased yield, and enhanced dispersibility and stability, particularly suitable for electrochemical applications.
Smart Images

Figure 0007575826000001 
Figure 0007575826000002 
Figure 0007575826000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for continuously synthesizing carbon nanotubes using a plasma-treated catalyst, and more particularly, to a method for continuously synthesizing carbon nanotubes by plasma-treating a metal salt to produce metal nanoparticles and reacting them with a carbon source in a gas phase to continuously synthesize carbon nanotubes, or by controlling the particle size of a catalytic metal supported on a supported catalyst used in the synthesis of carbon nanotubes, thereby producing carbon nanotubes of uniform size and performance, and improving the reactivity of the catalyst.
[0002] The present invention also provides a method for producing branched carbon nanotubes with improved hydrophilicity and specific surface area by using a catalyst that uses pretreated carbon nanotubes as a support. [Background technology]
[0003] Thermoplastic resins, especially high-performance plastics with excellent mechanical properties and heat resistance, are used in various applications. Depending on the field of application, such high-performance plastics are required to have antistatic properties such as antistatic and dust contamination to prevent malfunction and contamination of parts, and electrical conductivity is required in addition to the existing physical properties.
[0004] In order to impart such electrical conductivity to high-performance plastics, surfactants, metal powders, metal fibers, etc. have been added in the past, but these ingredients have problems such as low electrical conductivity or reducing physical properties, such as weakening mechanical strength, etc. For this reason, there is growing interest in carbon materials with electrical conductivity.
[0005] Conductive carbon black is generally used as a carbon material with electrical conductivity. However, in order to achieve high electrical conductivity using conductive carbon black, a large amount of carbon black must be added, and the carbon black structure may decompose during the melt mixing process, which may result in poor processability of the resin and a significant decrease in thermal stability and physical properties. Therefore, in order to improve electrical conductivity while reducing the amount of conductive filler added, active research is being conducted on carbon nanotube-resin composites that add carbon nanotubes instead of conductive carbon black.
[0006] Carbon nanotubes are a substance discovered in Japan in 1991. They consist of one carbon atom bonded to three adjacent carbon atoms, with the bonds between these carbon atoms forming hexagonal rings, and these rings are repeated in a honeycomb pattern, with the planes rolled up to form a cylindrical tube.
[0007] Carbon nanotubes are classified into single-walled carbon nanotubes (SW carbon nanotubes) with a diameter of about 1 nm, which are made up of a single wall, double-walled carbon nanotubes (DW carbon nanotubes) with two walls, and multiwalled carbon nanotubes (MW carbon nanotubes) with a diameter of about 5 to 100 nm, which are made up of three or more walls.
[0008] Such carbon nanotubes can be synthesized by various methods such as arc discharge, laser evaporation, thermal chemical vapor deposition (CVD), catalytic synthesis, and plasma synthesis. These methods synthesize carbon nanotubes at high temperatures ranging from several hundred to several thousand degrees or are performed under vacuum.
[0009] However, conventional methods have problems in that it is difficult to form a catalyst of uniform size, and therefore difficult to control the diameter of the carbon nanotubes produced uniformly. In addition, a separate reducing agent is required, which is disadvantageous in terms of the economics of the process.
[0010] In addition, the catalyst used is highly durable and the size of the catalytically active particles is uniform, so that carbon nanotubes with uniform size and excellent performance can be produced, and the synthesis yield of carbon nanotubes can be improved. Therefore, the development of such functional catalysts is being continuously carried out.
[0011] In addition, the existing conventional synthesis methods can only synthesize one-dimensional carbon nanotubes in the shape of a tube or rod. Currently, various applications using carbon nanotubes are being proposed, and each application requires characterized carbon nanotubes.
[0012] For example, when carbon nanotubes are used as electrode materials, polymer reinforcements, transistors, or electrochemical materials, branched carbon nanotubes having two- or three-dimensional structures may be more advantageous than linear, one-dimensional structures in the form of tubes or wires.
[0013] In particular, when used as an electrode material, two-dimensional or three-dimensional branched carbon nanotubes having a tree-like structure at the junction between carbon nanotubes or between a carbon nanotube and a current collector are expected to provide electrodes with excellent efficiency and stability.
[0014] In general, carbon nanotubes have a problem in that they are difficult to dissolve or disperse when used due to the strong van der Waals forces between the carbon nanotubes, and branched carbon nanotubes have a problem in that they are even more difficult to disperse because the carbon nanotubes are entangled and aggregated in the branched regions. Therefore, a method for producing carbon nanotubes is needed that can increase the hydrophilicity of branched carbon nanotubes and improve their dispersibility when used. Summary of the Invention [Problem to be solved by the invention]
[0015] One embodiment of the present invention relates to a method for continuously synthesizing carbon nanotubes using a plasma-treated catalyst, and relates to a method for continuously synthesizing carbon nanotubes, in which a metal salt is plasma-treated to produce metal nanoparticles without separately adding a reducing agent, and the metal nanoparticles are reacted with a carbon source in a gas phase to continuously produce carbon nanotubes.
[0016] A method for producing carbon nanotubes according to another embodiment of the present invention can produce carbon nanotubes of uniform size and performance by controlling the particle size of the catalytic metal supported on the supported catalyst used in the synthesis of carbon nanotubes, and can improve the reactivity of the catalyst.
[0017] Another embodiment of the present invention provides a method for producing branched carbon nanotubes with improved hydrophilicity and specific surface area by producing branched carbon nanotubes using a catalyst supported on pretreated carbon nanotubes. [Means for solving the problem]
[0018] One embodiment of the present invention for achieving the above object includes a plasma treatment step of plasma treating a metal salt in an H2 or NH3 atmosphere to produce metal nanoparticles, a first mixture preparation step of mixing a solvent and a surfactant to produce an emulsion mixture, a second mixture preparation step of mixing the emulsion mixture with a carrier gas to produce a second mixture, and a reaction step of introducing the second mixture and the metal nanoparticles into a heated reactor to form carbon nanotubes.
[0019] In the plasma treatment step, the plasma treatment may be performed in a gas atmosphere in which H2 or NH3 atmosphere further contains nitrogen gas and an inert gas of Group 18. In this case, H2 or NH3, nitrogen gas and an inert gas of Group 18 are preferably mixed in a volume ratio of about 1-5:5:0.01-1.0.
[0020] After the plasma treatment step, an oxygen plasma treatment step of performing plasma treatment in an oxygen atmosphere may be further included.
[0021] The plasma treatment step may be performed at a pressure of about 0.2-2.5 Torr, at a frequency range of about 15-30 kHz, and at a temperature of about 50-300°C.
[0022] In the first mixture preparation step, the solvent may be a solvent containing carbon or a solvent not containing carbon. In this case, when a solvent not containing carbon is used in the first mixture preparation step, a carbon source gas may be further included in the second mixture preparation step.
[0023] Another embodiment of the present invention relates to a method for producing carbon nanotubes, including a mixing step of mixing a solvent, a metal precursor and a support to produce a mixed solution, a first heating step of heating the mixed solution under vibration to produce a catalyst support, a dispersion step of dispersing the catalyst support in a reduction solution to produce a catalyst dispersion, an electron beam irradiation step of irradiating the catalyst dispersion with an electron beam, a second heating step of filtering the mixture obtained in the electron beam irradiation step and heating it to produce a functional catalyst support, and a synthesis step of reacting the functional catalyst support with a carbon source to produce carbon nanotubes.
[0024] The mixing step may be performed by mixing and dissolving 0.1 to 2.0 parts by weight of the metal precursor in 100 parts by weight of the solvent, and then mixing 0.5 to 5.0 parts by weight of the support.
[0025] The first heating step may be performed by a multi-stage heating method in which the mixture is vibrated, heated to a temperature range of 60 to 120°C, and then heated to a temperature range of 150 to 250°C after stopping the vibration.
[0026] The reducing solution may be an aqueous solution containing an alcohol having 1 to 3 carbon atoms and a reducing agent. The reducing agent may include at least one of hydrazine, LiBH4, NaBH4, ethylene oxide, formaldehyde, formic acid, and a polyol.
[0027] The electron beam has a current density of 100 to 500 A / cm 2 The acceleration voltage may be 300 to 600 keV, and the irradiation time of the electron beam may be 3 to 10 minutes.
[0028] The heating temperature in the second heating step may be 500 to 1000°C.
[0029] Between the second heating step and the synthesis step, a plasma treatment step may be further carried out to plasma treat the functional catalyst support.
[0030] Another embodiment of the present invention relates to a method for producing branched carbon nanotubes with improved hydrophilicity, comprising: a pretreatment step of discharging an acidic solution mixed with carbon nanotubes in water; a heat treatment step of heat treating the carbon nanotubes obtained in the pretreatment step to produce a support; a catalyst structure production step of mixing the support, a solvent and a catalyst precursor and then reducing the catalyst precursor to produce a catalyst structure in which a catalyst is supported on a support; and a carbon nanotube synthesis step of reacting the catalyst structure with a carbon source to produce branched carbon nanotubes.
[0031] The pretreatment step may include a first pretreatment step of mixing carbon nanotubes with an acidic solution and then ultrasonicating the mixture, and a second pretreatment step of subjecting the mixture that has undergone the first pretreatment step to underwater plasma discharge.
[0032] The heat treatment step may be a step of heat treating the pretreated carbon nanotubes in an oxygen atmosphere at a temperature range of 280 to 550° C. for 20 to 80 minutes.
[0033] The catalyst structure production step may include a first step of mixing the support, a solvent and a catalyst precursor to produce a precursor mixture, a second step of drying the precursor mixture at a temperature of 90 to 120°C to produce a supported catalyst, a third step of mixing the supported catalyst with a reducing liquid and then stirring to produce a catalyst structure, and a fourth step of filtering and washing the catalyst structure.
[0034] The third step may be carried out at a temperature of 20 to 200°C.
[0035] The reducing solution may contain at least one selected from the group consisting of hydrazine, LiBH4, NaBH4, ethylene oxide, formaldehyde, formic acid, and a polyol. Effect of the Invention
[0036] The continuous synthesis method of carbon nanotubes of the present invention can produce a catalyst by reducing a metal salt at a relatively low temperature in a shorter time, increase the yield of carbon nanotubes, and economically produce a large amount of carbon nanotubes by uniformly controlling the diameter of the carbon nanotubes.
[0037] According to another embodiment of the method for producing carbon nanotubes of the present invention, the particle size of the catalytic metal supported on the supported catalyst used in the synthesis of carbon nanotubes can be controlled to produce carbon nanotubes of uniform size and performance, and the reactivity of the catalyst can be improved, thereby improving the synthesis yield of carbon nanotubes.
[0038] According to another embodiment of the method for producing branched carbon nanotubes of the present invention, a number of Y junctions can be formed on a straight carbon nanotube to synthesize carbon nanotubes having a tree-like structure. The carbon nanotubes synthesized in this manner have improved hydrophilicity and specific surface area, and therefore excellent dispersibility. In addition, when used as an electrochemical material, they have the advantage of being excellent in stability and electrochemical efficiency. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0039] Before describing in detail preferred embodiments of the present invention below, it will be made clear that the terms and words used in the claims of this specification should not be interpreted limitedly to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept consistent with the technical ideas of the present invention.
[0040] Throughout this specification, when a part "comprises" a certain element, this means that it can further include other elements, rather than excluding other elements, unless specifically stated to the contrary.
[0041] Throughout this specification, "%" used to indicate the concentration of a particular substance means % (w / w) in the case of solid / solid, % (w / vol) in the case of solid / liquid, and % (vol / vol) in the case of liquid / liquid and gas / gas, respectively, unless otherwise specified.
[0042] Generally, a colloid means anything whose particle size is smaller than 0.45 μm (or 0.2 μm) and larger than 1000 Da (Dalton, mass of one molecule); however, in the specification of the present invention, the term "colloid" means a solution containing particles whose particle size is several to several hundred nanometers, and sometimes includes their precursors.
[0043] Hereinafter, an embodiment of the present invention will be described. However, the scope of the present invention is not limited to the following preferred embodiment, and a person skilled in the art can implement various modifications of the contents described in this specification within the scope of the present invention.
[0044] A method for continuously synthesizing carbon nanotubes according to one embodiment of the present invention relates to a method for continuously synthesizing carbon nanotubes, the method including: a plasma treatment step of plasma treating a metal salt in an H2 or NH3 atmosphere to produce metal nanoparticles; a first mixture preparation step of mixing a solvent and a surfactant to produce an emulsion mixture; a second mixture preparation step of mixing the emulsion mixture with a carrier gas to produce a second mixture; and a reaction step of introducing the second mixture and the metal nanoparticles into a heated reactor to form carbon nanotubes.
[0045] The plasma treatment step is a step of plasma treating a metal salt in an H2 or NH3 atmosphere to produce metal nanoparticles.
[0046] The plasma state is called the fourth state of matter other than solid, liquid, and gas, and is composed of molecules, atoms, ions, electrons, and quanta, and is in an electrically neutral state known as quasi-neutral as a whole. Plasma is classified into high-temperature plasma (equilibrium plasma) and low-temperature plasma (non-equilibrium plasma), and high-temperature plasma is mainly used in fields such as arc welding as it induces high temperatures of over 1000°C.
[0047] There is no particular restriction on the power for generating the plasma, but a high-frequency AC or high-frequency pulse generator can be used, and preferably a high-frequency anode DC pulse generator can be used.
[0048] The plasma treatment is preferably carried out in an H2 or NH3 atmosphere, and more preferably in a gas atmosphere in which nitrogen gas and an inert gas of Group 18 are further contained in the H2 or NH3 atmosphere.
[0049] In this case, H2 or NH3, nitrogen gas, and Group 18 inert gas are preferably mixed in a volume ratio of about 1-5:5:0.01-1.0, more preferably about 2:5:0.5. If H2 or NH3 is contained in an amount less than 1 v / v, the ratio of hydrogen radicals generated in the plasma treatment is reduced, which may result in small sizes of metal nanoparticles and reduced yields of carbon nanotubes.
[0050] On the other hand, if H2 or NH3 is mixed at more than 5 v / v, the ratio of hydrogen radicals becomes high, making the gas phase atmosphere unstable, making it difficult to control the size of the metal nanoparticles used as catalysts, and the diameter of the produced carbon nanotubes may not be uniform.
[0051] At this time, NH3 is decomposed into hydrogen and nitrogen while passing through the plasma, and the generated hydrogen radicals reduce metal salts to produce metal nanoparticles, while the nitrogen provides a stable reaction environment, thereby increasing the production rate of metal nanoparticles.
[0052] The nitrogen gas and the 18th group inert gas in the H2 or NH3 atmosphere serve to prevent impurities from being generated due to the high reactivity of hydrogen radicals generated during plasma treatment, to prevent hydrogen gas from being generated again due to reactions between hydrogen radicals, thereby increasing the production rate of metal nanoparticles, and to stably maintain the pressure before and after plasma treatment.
[0053] The Group 18 inert gas facilitates plasma generation, and is preferably helium (He), neon (Ne), argon (Ar), or the like, and is most preferably argon (Ar), but is not limited to these.
[0054] Meanwhile, after the plasma treatment step in the H2 or NH3 atmosphere, an oxygen plasma treatment step may be further included in which plasma treatment is performed in an oxygen atmosphere. At this time, nitrogen oxides such as O2, H2O, O3, N2O, or NO, NO2 may be supplied as the oxygen atmosphere plasma forming gas, and it is preferable to use O2 or H2O, but it is not limited thereto. By preventing the generation of other elements other than hydrogen, nitrogen, and oxygen by the plasma treatment, it is possible to prevent the generation of impurities and maintain the reactivity of the plasma treatment.
[0055] The plasma-forming gas not only helps generate and maintain the plasma, but also increases the production rate of metal nanoparticles by further converting metal salts that did not react in the plasma treatment step into metal nanoparticles using oxygen radicals generated from the oxygen gas.
[0056] In addition, by forming an oxide film on a certain portion of the surface of the metal nanoparticles formed in the plasma treatment step in an H2 or NH3 atmosphere, the metal nanoparticles can be prevented from agglomerating together.
[0057] Such oxygen gas is preferably supplied at a flow rate of about 50 to 300 sccm (standal cubic centimeter per minute), and more preferably mixed at a flow rate of about 100 to 150 sccm. If oxygen gas is mixed at a flow rate lower than 50 sccm, an oxide film cannot be sufficiently formed on the surface of the metal nanoparticles, and the aggregation rate of the metal nanoparticles may increase.
[0058] On the other hand, if the mixture is mixed at a flow rate higher than 300 sccm, the excess oxygen radicals will undergo an oxidation reaction, causing a widespread oxide film to form on the surface of the metal nanoparticles, which may reduce the reactivity of the metal nanoparticles as a catalyst for producing carbon nanotubes.
[0059] The plasma treatment step is preferably performed at a pressure of about 0.2 to 2.5 Torr, and more preferably at a pressure of about 0.5 to 1.5 Torr. At a pressure lower than 0.2 Torr, gas is not densely packed around the plasma, resulting in a shortage of radicals for forming metal nanoparticles, while at a pressure higher than 2.5 Torr, the kinetic energy of gas molecules is high, and excess hydrogen or oxygen radicals are generated to form water or hydrogen gas, reducing the possibility of reducing the metal salt, which may result in a low yield of carbon nanotubes.
[0060] Meanwhile, plasma generation is preferably performed in a frequency range of about 15-30 kHz at a temperature of about 50-300° C., and more preferably in a frequency range of about 20-30 kHz at a temperature of about 70-150° C. If the frequency is less than 15 kHz, plasma may not be generated or the generated plasma may not be sustained for long and may easily disappear, whereas if the frequency exceeds 30 kHz, it may transition to arc plasma.
[0061] Furthermore, if the temperature is below 50°C, radicals are not generated, which may cause a problem that the metal salt is not reduced, whereas if the temperature exceeds 300°C, there is a risk of transition to arc plasma.
[0062] The metal salt is a precursor of metal nanoparticles, which are a catalyst for forming carbon nanotubes, and is formed into fine particles with a metal particle size of 300 nm or less through a plasma treatment step, which may result in different physical properties and performance compared to larger particle sizes. In particular, the surface area per unit mass increases significantly, improving functionality, and physical property changes such as a decrease in the melting point of the particles and discoloration occur. Such nanometer-sized fine metal particles are highly reactive and can exist in a suspended state in the gas phase, and can be used as a catalyst for synthesizing carbon nanotubes in the gas phase.
[0063] The metal salt can be at least one of oxides, nitrides, borides, fluorides, bromides, sulfides, chlorides, and carbonates of one or more metals selected from the group consisting of iron (Fe), cobalt (Co), nickel (Ni), platinum (Pt), palladium (Pd), molybdenum (Mo), and vanadium (V).
[0064] The metal salt, either as it is or in the form of a metal oxide, can be reduced by contacting with radicals formed by plasma treatment to produce metal nanoparticles. The metal nanoparticles are small in size, and can be formed in a gas phase by themselves or by mixing with other gases, and then sprayed into the reactor in a colloidal form. In this case, the carrier gas can be an inert gas such as argon, neon, helium, nitrogen, or a hydrocarbon, and the flow rate is preferably about 30 to 450 sccm.
[0065] If the flow rate is outside the above range, the metal nanoparticles may not be uniformly dispersed or diffused in the gas phase, which may result in a reduced yield of carbon nanotubes, and the amount of catalyst that does not participate in the reaction may increase, which may result in problems such as a decrease in economic viability or process efficiency.
[0066] Meanwhile, the first mixture preparation step is a step of preparing an emulsion mixture by mixing a solvent and a surfactant.
[0067] The surfactant prevents the aggregation of metal nanoparticles that are sprayed in a colloidal state in the subsequent reaction step, and adheres to the oxide film on the surface of the metal nanoparticles that have undergone a plasma treatment step that further contains oxygen gas, thereby improving the reactivity of the metal nanoparticles as a catalyst.
[0068] As such a surfactant, at least one of a nonionic surfactant, an anionic surfactant, a cationic surfactant and an amphoteric surfactant can be used, and preferably a nonionic surfactant or an anionic surfactant can be used.
[0069] As the nonionic surfactant, polyoxyethylene, alkyl glucoside, alkyl polyglucoside, polyhydroxy fatty acid amide, alkoxylated fatty acid ester, sucrose ester, amine oxide, alcohol ethoxylate, amide ethoxylate, amine oxide, alkyl glucoside, etc. can be used. For example, cocamide methyl, C8-C14 glucose amide, C8-C14 alkyl polyglucoside, sucrose cocoate, sucrose laurate, lauramine oxide, cocoamine oxide, etc. can be appropriately used according to need by ordinary skilled artisans, but are not limited thereto.
[0070] Examples of the anionic surfactant that can be used include alkyl sulfates, ethoxylated alkyl sulfates, alkyl ethoxy carboxylates, alkyl glyceryl ether sulfonates, ethoxy ether sulfonates, methyl acyltaurates, alkyl sulfosuccinates, alkyl ethoxy sulfosuccinates, alpha-sulfonated fatty acids, alkyl phosphate esters, ethoxylated alkyl phosphate esters, linear alkyl benzene sulfonates, paraffin sulfonates, alpha-olefin sulfonates, and alkyl alkoxy sulfates. Examples of the anionic surfactant that can be used include, but are not limited to, sodium lauryl sulfate, sodium laureth sulfate, and sodium coco sulfate.
[0071] The cationic surfactant may be at least one selected from the group consisting of cetyltrimethylammonium bromide, decyltrimethylammonium bromide, dodecyltrimethylammonium bromide, didecyldimethylammonium bromide, cetyldimethylammonium chloride, lauryldimethylammonium chloride, stearyldimethylammonium chloride, tallow dimethylammonium chloride, ditallow dimethylammonium methyl sulfate, coconut ammonium chloride, stearamidopropyl PG-dimonium chloride phosphate, and stearamidopropyl ethyldimonium ethosulfate, but is not limited thereto.
[0072] Examples of the amphoteric surfactant that can be used include, but are not limited to, alkyl betaines, amido betaines, sulfo betaines, hydroxysulfo betaines, amido sulfo betaines, phospho betaines, imidazolinium betaines, aminopropionic acid surfactants, and amino acid surfactants.
[0073] The surfactant can be used in an amount of 5 to 13 parts by weight per 100 parts by weight of the solvent, and if the surfactant content is less than 5 parts by weight, the metal nanoparticles may aggregate with each other, making it difficult to synthesize carbon nanotubes of uniform size. On the other hand, if the surfactant content exceeds 13 parts by weight, the excess surfactant may rather reduce the function of the metal nanoparticles as a catalyst, resulting in a reduced yield of carbon nanotubes.
[0074] The solvent may be a solvent that does not contain carbon or may be a solvent that contains carbon, such as aromatic hydrocarbons, aliphatic hydrocarbons, and alcohol compounds. Preferably, water is used as the solvent, or ethanol (C2H6O), benzene (C6H6), toluene (C7H8), or xylene (C8H 10 ) can be used, but is not limited thereto.
[0075] The second mixture preparation step is a step of preparing a second mixture by mixing the emulsion mixture with a carrier gas. In this case, the carrier gas may be an inert gas such as argon, neon, helium, or nitrogen, or a hydrocarbon, and the flow rate is preferably about 30 to 450 sccm. If the flow rate is less than 30 sccm, the content of the carrier gas in the second mixture is too low, so that the second mixture may not be easily introduced into the reactor thereafter, and if the flow rate is more than 450 sccm, the amount of carrier gas used increases too much, so that the process is not economical.
[0076] In this case, when water is used as the solvent, the second mixture preparation step may further include a carbon source gas, and in consideration of the yield of carbon nanotubes, minimization of unreacted materials, improvement of economy and productivity, etc., it is preferable that the supply flow rate of the carbon source gas is about 35 to 280 sccm.
[0077] The carbon source gas may be an organic compound selected from the group consisting of carbon monoxide, saturated or unsaturated aliphatic hydrocarbons having 1 to 6 carbon atoms, or aromatic hydrocarbons having 6 to 10 carbon atoms. Such a carbon source gas may contain about 1 to 3 heteroatoms selected from the group consisting of oxygen, nitrogen, chlorine, fluorine, and sulfur. In this case, a gas characterized by H2, H2S, NH3, etc. may be supplied together with the carbon source gas.
[0078] Meanwhile, the reacting step is a step of forming carbon nanotubes by introducing the second mixture and metal nanoparticles into a heated reactor.
[0079] The second mixture and the metal nanoparticles may be formed into a gas phase by a method such as spraying or injection and then introduced into the reactor, and are preferably injected in a colloidal form.
[0080] Meanwhile, depending on the temperature of the reactor, single-walled carbon nanotubes (SWNT) or multi-walled carbon nanotubes (MWNT) can be mainly produced. The temperature of the reactor is preferably maintained at about 600 to 1500°C, but the temperature of the reactor can be appropriately adjusted depending on the characteristics of the carbon nanotubes to be produced. In this case, the process of producing multi-walled carbon nanotubes (MWNT) can be performed at a temperature of about 600°C to less than 1000°C, more preferably about 800°C to less than 1000°C. At a temperature lower than 600°C, the amount of reactants that do not participate in the reaction increases, and the growth of carbon nanotubes is sluggish, which may reduce the yield.
[0081] Single-walled carbon nanotubes (SWNTs) are preferably produced at a temperature range of about 1000° C. to 1500° C., more preferably about 1000° C. to 1200° C. If the temperature is outside the above range, problems may occur, such as slow growth of single-walled carbon nanotubes resulting in a reduced yield, reduced selectivity of carbon nanotubes, or difficulty in controlling the diameter of carbon nanotubes.
[0082] The following description will focus on specific examples of the present invention. However, the scope of the present invention is not limited to the following examples, and these examples are merely presented for illustrative purposes to more specifically explain the present invention. It will be apparent to those skilled in the art that various modifications of the contents described herein can be made within the scope of the present invention.
[0083] [Experimental Example 1] Metal nanoparticles were produced by reducing FeCl3 in a gas atmosphere containing hydrogen gas, nitrogen gas or argon gas according to the conditions in Table 1 below, with the pressure maintained at about 1.0 Torr and plasma generated at a temperature of 100°C using a high frequency anode DC pulse generator at a frequency of 22 kHz. With the frequency, temperature, pressure, etc. maintained as they were, an oxygen plasma treatment step was carried out in an oxygen atmosphere where O2 was supplied at a flow rate of 110 sccm for about 10 minutes. The number concentration (number / cm) of metal nanoparticles with a size of about 15 to 100 nm was measured using a portable CPC (Condensation Particle Counter, Kanomax Model 3800). 3 ) was measured for about 20 minutes, and then the production rate (%) of metal nanoparticles was calculated according to the following formula 1.
[0084] Metal nanoparticle generation rate (%) = {(R2-R1) / R1} x 100 (Equation 1) (In the formula, R2 is the number concentration of metal nanoparticles after the reaction, and R1 is the number concentration of metal nanoparticles before the reaction.)
[0085] [Table 1]
[0086] As can be seen from Table 1, the production rate of metal nanoparticles exceeded 90% under the conditions of Examples 1 to 9, in which hydrogen gas, nitrogen gas, and argon gas were mixed in a volume ratio (v / v) of about 2:5:0.01 to 1.0.
[0087] In contrast, in Comparative Example 1, which contained only hydrogen gas, and Comparative Example 2, which contained hydrogen and nitrogen gas, the production rate of metal nanoparticles did not reach 80%, and in Comparative Examples 3 to 6, in which the contents of hydrogen, nitrogen, and argon gas were outside the above range, the production rate of metal nanoparticles was less than 90%.
[0088] Therefore, it was found that when hydrogen gas, nitrogen gas, and argon gas are mixed in a volume ratio (v / v) of about 2:5:0.01 to 1.0, the production rate of metal nanoparticles is excellent, and when mixed in a volume ratio (v / v) of about 2:5:0.5, the production rate of metal nanoparticles is the best.
[0089] [Experimental Example 2] The results of producing carbon nanotubes using the metal nanoparticles produced in Examples 1 to 9 and Comparative Examples 1 to 6 of Experimental Example 1 as catalysts are shown in Table 2 below.
[0090] Metal nanoparticles were supplied by injecting argon as a carrier gas at a flow rate of 100 sccm into the reactor. In addition, 6 parts by weight of alkyl glucoside was mixed with 100 parts by weight of benzene as a solvent, and then argon as a carrier gas was injected at a flow rate of 100 sccm into the reactor. At this time, the temperature of the reactor was maintained at 800°C. The produced carbon nanotubes were observed by a scanning electron microscope (SEM) to measure their diameters, and the yield (%) of carbon nanotubes was calculated according to the following Equation 2.
[0091] Yield (%) = {amount of carbon nanotubes produced (g) / amount of metal salt provided (g)} x 100 (Equation 2)
[0092] [Table 2]
[0093] As can be seen from Table 2, in the cases of Examples 1 to 9, the yield of carbon nanotubes exceeded 2,000%, and the diameter of the produced carbon nanotubes was constant at about 70 nm, with the standard deviation maintained between about 74 and 90. In contrast, in the cases of Comparative Examples 1 to 6, the yield of carbon nanotubes was less than 2,000%, and the diameter of the produced carbon nanotubes was in the range of about 62 to 69 nm, with the standard deviation calculated to be about 11 to 22, confirming that it was difficult to control the produced carbon nanotubes to a constant size.
[0094] Comparative Examples 1 and 2 showed that the addition of nitrogen gas increased the yield of carbon nanotubes by more than two times, and Comparative Examples 2 and 3 showed that the addition of argon gas increased both the yield of carbon nanotubes and the diameter of the carbon nanotubes.
[0095] In addition, from Comparative Examples 3 to 6 and Examples 1 to 9, it was confirmed that when the volume ratio of hydrogen gas and nitrogen gas is 2:5, the range of the argon gas content that can simultaneously adjust the yield and diameter of carbon nanotubes by increasing the argon gas content is 0.01 to 1.0 v / v, and the most preferable argon gas content is 0.5 It was found to be v / v.
[0096] [Experimental Example 3] Metal nanoparticles and carbon nanotubes were produced in the same manner as in Experimental Examples 1 and 2 under the conditions in Table 3 below, and the production rate of metal nanoparticles and the yield of carbon nanotubes were calculated according to Equations 1 and 2. The produced carbon nanotubes were observed with a scanning electron microscope (SEM) to measure their diameters.
[0097] [Table 3]
[0098] As can be seen from Table 3, the yield of carbon nanotubes produced in Comparative Example 7, in which the hydrogen gas content was less than 1 v / v, was less than 2000%, and the diameter of the carbon nanotubes was not controlled.
[0099] In contrast, in Comparative Examples 8 and 9, where the hydrogen gas content was greater than 5 v / v, the production rate of metal nanoparticles was quite high at approximately 995% or more, but the yield of carbon nanotubes was less than 2000%, and it was confirmed that the diameter of the produced carbon nanotubes could not be smoothly controlled.
[0100] Therefore, taking into consideration all of the control aspects of the production rate of metal nanoparticles, the yield of carbon nanotubes, and the diameter of carbon nanotubes, it was found that the measurement results were excellent when the hydrogen gas content was about 1 to 5 v / v, as in the case of Examples 5 and 10 to 12, and it was confirmed that the measurement results were best when the volume ratio (v / v) of hydrogen gas, nitrogen gas and argon gas was about 2:5:0.5, as in the case of Example 5.
[0101] A method for producing carbon nanotubes according to another embodiment of the present invention includes a mixing step of mixing a solvent, a metal precursor and a support to produce a mixed solution, a first heating step of heating the mixed solution under vibration to produce a catalyst support, a dispersion step of dispersing the catalyst support in a reduction solution to produce a catalyst dispersion solution, an electron beam irradiation step of irradiating the catalyst dispersion solution with an electron beam, a second heating step of filtering the mixture obtained in the electron beam irradiation step and heating it to produce a functional catalyst support, and a synthesis step of reacting the functional catalyst support with a carbon source to produce carbon nanotubes.
[0102] First, the mixing step is a step of mixing a solvent, a metal precursor, and a support to adsorb the metal precursor to the support. In this step, the mixture is obtained by mixing 0.1 to 2.0 parts by weight of the metal precursor in 100 parts by weight of the solvent to uniformly disperse the metal precursor, and then mixing 0.5 to 5.0 parts by weight of the support. When performed in this order, the metal precursor can be more uniformly dispersed and adsorbed on the support.
[0103] At this time, after mixing the supports together, stirring may be performed at a stirring speed of 300 to 600 rpm for 30 minutes to 2 hours.
[0104] The solvent is used as a dispersion medium for uniformly dispersing the support and the metal precursor to adsorb and support the metal precursor on the support, and may be at least one selected from the group consisting of aromatic hydrocarbons, aliphatic hydrocarbons, alcohol compounds, and water. For example, benzene, toluene, xylene, etc. may be used as the aromatic hydrocarbon, hexane, heptane, octane, etc. may be used as the aliphatic hydrocarbon, and ethanol, propyl alcohol, polyethylene glycol, etc. may be used as the alcohol compound.
[0105] In particular, it is preferable to use an alcohol compound as the solvent, and more preferably, polyethylene glycol can be used. In this case, the metal precursor can be uniformly dispersed in the solvent without using a separate surfactant, which prevents the decrease in the accessibility between the metal precursor and the support caused by the surfactant, and does not require a post-process to remove the surfactant, which is more effective in terms of reaction efficiency and process efficiency.
[0106] The metal precursor is a metal salt that is a precursor of a catalyst for forming carbon nanotubes, and at least one metal salt selected from the group consisting of iron (Fe), cobalt (Co), nickel (Ni), platinum (Pt), palladium (Pd), molybdenum (Mo), and vanadium (V) can be used, which is at least one metal salt selected from the group consisting of oxides, nitrides, borides, fluorides, bromides, sulfides, chlorides, and carbonates.
[0107] Such metal precursors can be mixed in an amount of 0.1 to 2.0 parts by weight per 100 parts by weight of the solvent. When the content of the metal precursor is less than 0.1 part by weight, the amount of metal salt supported on the support is small, and when it exceeds 2.0 parts by weight, there is no additional increase in the amount supported, resulting in a decrease in the support efficiency. Therefore, it is preferable that the metal precursor is mixed in the above content in the mixing step.
[0108] The support is a carrier on which the metal precursor is adsorbed, and the type thereof is not particularly limited, but may be a carbon-based support, for example, at least one selected from the group consisting of carbon black, activated carbon powder, carbon nanotubes, carbon nanowires, and fullerenes.
[0109] Such a support may be porous, and preferably has a specific surface area of 200 to 600 m in order to increase the efficiency of supporting the metal precursor and the efficiency of synthesizing carbon nanotubes. 2 / g of porous support.
[0110] The porous support may preferably be a carbon-based support whose specific surface area has been increased by ozone treatment. When a carbon-based support is subjected to ozone treatment in this manner, not only is the specific surface area increased by the ozone, but there is also an advantage in that the introduction of oxygen-based functional groups improves the loading efficiency when a metal catalyst is subsequently loaded.
[0111] Specifically, it is preferable to supply ozone to the above-mentioned carbon-based support at a temperature of 250 to 380°C and a flow rate of 80 to 250 mg / min for 1 to 4 hours for ozone treatment. In this case, if the flow rate of ozone is less than 80 mg / min, the treatment time increases excessively and workability decreases, whereas if the flow rate exceeds 250 mg / min, the pressure in the reactor increases rapidly, making it difficult to store the porous support powder.
[0112] Furthermore, when the ozone treatment time is less than 1 hour, the increase in the specific surface area and the effect of introducing functional groups by ozone are negligible, whereas when the ozone treatment time exceeds 4 hours, there is a risk that the micropores on the surface of the carbon-based support are closed, resulting in a decrease in the specific surface area. Therefore, it is preferable to carry out the ozone treatment under the above-mentioned conditions.
[0113] Next, the first heating step is a step of producing a catalyst support by applying vibration to the mixture obtained in the previous mixing step and heating it.
[0114] In this step, heating under vibration prevents aggregation between the metal precursor and the support or between the supports during the process of adsorption of the metal precursor onto the support, so that the metal precursor is uniformly dispersed and adsorbed onto the support, making it possible to form a catalyst support of a more consistent size. Thereafter, carbon nanotubes having a consistent size and consistent physical properties are synthesized during the synthesis of carbon nanotubes, which has the advantage of improving the reliability of the carbon nanotubes.
[0115] This step can be performed by a multi-stage heating method, specifically, by vibrating the mixture, heating it at a temperature range of 60 to 120°C for 10 to 80 minutes, and then stopping the vibration and heating it at 150 to 250°C for 1 to 30 hours.
[0116] By first applying vibration and then heating at a relatively low temperature, the metal precursor can be uniformly dispersed and adsorbed on the support. In addition, by heating to the above-mentioned temperature range, the solvent loss can be minimized and the efficiency of adsorption of the metal precursor to the support by heat can be improved.
[0117] Thereafter, the solvent can be completely removed by heating to a relatively high temperature while removing vibration, thereby forming a particulate catalyst support. Since there is no vibration, damage to the supports due to collisions between supports and falling off of the metal precursor can be prevented.
[0118] At this time, the vibration can be applied by vibrating the reactor containing the mixed liquid in the vertical or horizontal direction, and the vibration is preferably applied with an amplitude of 0.5 to 5 mm and a frequency of 0.5 to 5 kHz. When the strength of the vibration is small, the dispersion effect obtained by applying the vibration is insignificant, and particularly when the frequency exceeds 5 kHz, the supports collide with each other in the mixed liquid, resulting in damage to the supports due to the collision energy generated, and there is a problem that the size of the supports becomes non-uniform, so it is preferable to apply the vibration under the above conditions.
[0119] Next, a dispersion step is performed in which the catalyst support obtained in the first heating step is dispersed in a reduction solution to prepare a catalyst dispersion, which can reduce the metal precursor to a metal and improve the catalytic activity.
[0120] The reducing solution is an aqueous solution containing an alcohol having 1 to 3 carbon atoms and a reducing agent, where the alcohol having 1 to 3 carbon atoms may be at least one selected from the group consisting of methanol, ethanol, and propanol, and the reducing agent may be at least one of hydrazine, LiBH4, NaBH4, ethylene oxide, formaldehyde, formic acid, and polyol.
[0121] The reduction solution may contain 1 to 30 parts by weight of alcohol and 0.01 to 1 part by weight of a reducing agent per 100 parts by weight of water. Since an aqueous alcohol solution is used as a solvent for the reduction solution instead of water, the catalyst support can be uniformly dispersed in the reduction solution without a separate surfactant. In addition, the alcohol controls active species generated in the subsequent electron beam irradiation step, thereby preventing damage to the catalyst support, and since no separate impurities are generated, a catalyst support with higher purity can be produced.
[0122] Next, an electron beam irradiation step is performed in which the catalyst dispersion is irradiated with an electron beam. This step is a step for controlling the particle size of the reduced metal and the particle size of the support by irradiating the catalyst dispersion with an electron beam in order to form carbon nanotubes of a uniform size and properties in a subsequent carbon nanotube synthesis step. In addition, the molecular bonds of the support connected by weak bonds are strengthened by the irradiation of the electron beam, thereby improving the strength of the support itself.
[0123] In this step, the electron beam irradiated to the catalyst dispersion liquid has a current density of 100 to 500 A / cm 2 The acceleration voltage may be 300 to 600 keV, and the irradiation time may be 3 to 10 minutes.
[0124] If the density current, acceleration voltage, and irradiation time of the electron beam are below the above ranges, it is difficult to obtain the above-mentioned effects by irradiating the electron beam. If they exceed the above ranges, excessive irradiation of the electron beam may cause problems such as breaking the bond between the metal and the support or damaging the support. Therefore, it is preferable to irradiate the electron beam under conditions within the above ranges.
[0125] Next, the mixture obtained in the electron beam irradiation step is filtered, and then heated in a second heating step to produce a functional catalyst support.
[0126] The second heating step is a step of producing a functional catalyst support in which the surface and voids of the support are coated with metal particles as a catalyst by heating the catalyst support particles obtained by filtering the mixture obtained in the electron beam irradiation step.
[0127] In this step, the heating temperature may be 500 to 1000°C, preferably 800 to 1000°C. By heating in such a temperature range, the crystallinity of the support itself is increased, improving the strength of the support, and the functional catalyst support of the above-mentioned form can be obtained. At this time, if the heating temperature exceeds 1000°C, excessive crystallization may rather close the voids, and the specific surface area of the support may decrease, so it is preferable to perform the heat treatment in the above-mentioned temperature range.
[0128] In the second heating step, the heating may be carried out for 1 to 18 hours, preferably 2 to 10 hours.
[0129] Thereafter, a synthesis step may be performed in which the functional catalyst support obtained through the second heating step is reacted with a carbon source to synthesize carbon nanotubes. At this time, a plasma treatment step may be further performed between the second heating step and the synthesis step in which the functional catalyst support is plasma treated. When plasma treated in this manner, the strength of the support itself may be improved, and the bonding strength between the metal and the support may be improved.
[0130] In this case, the plasma treatment is preferably carried out in a nitrogen or inert gas atmosphere under a vacuum of 1 to 100 Torr and at a temperature of 200 to 500°C. When carried out under such conditions, it is possible to obtain a performance improvement effect without damaging the support or metal.
[0131] Finally, the synthesis step is a step of reacting the functional catalyst support obtained in the above-mentioned process with a carbon source and synthesizing carbon nanotubes using the metal supported on the functional catalyst support as a catalyst. Through this synthesis step, carbon nanotubes with uniform particle size and physical properties can be synthesized.
[0132] The method for synthesizing carbon nanotubes in this step is not particularly limited, and can be, for example, an arc discharge method, a laser vaporization method, a CVD method, a catalytic synthesis method, a plasma synthesis method, a continuous gas phase synthesis method, etc., but is not limited to these.
[0133] For example, the functional catalyst support can be placed in a quartz boat and placed inside a reactor to produce carbon nanotubes.
[0134] For example, the functional catalyst support may be dispersed in a solvent and continuously supplied into a reactor while the carbon nanotube synthesis reaction proceeds, thereby allowing the carbon nanotubes to be continuously produced.
[0135] In this case, the functional catalyst support is prepared in the form of a colloidal solution in a solvent such as water or an organic solvent, and is finely dispersed or sprayed inside a reactor to suspend the colloidal solution particle droplets in a gas, where they exist as gas-phase colloids for a certain period of time, thereby allowing two- or three-dimensional carbon nanotubes to be continuously synthesized in the gas phase.
[0136] The method for converting the dispersion or colloidal solution obtained by dispersing the functional catalyst support in a solvent into a gas phase or suspending it in a gas is not particularly limited, and may be performed by a method commonly used in the art, such as direct spraying, siphon spraying, atomization, etc.
[0137] On the other hand, when dispersing the functional catalyst support in a solvent such as water or an organic solvent, a surfactant can be added in an amount that does not adversely affect the carbon nanotube synthesis reaction in order to prevent aggregation and uniformly disperse the functional catalyst support. In this case, the type of surfactant used is not particularly limited.
[0138] The carbon source in the carbon nanotube synthesis step may be, for example, an organic compound selected from the group consisting of carbon monoxide, saturated or unsaturated aliphatic hydrocarbons having 1 to 6 carbon atoms, or aromatic hydrocarbons having 6 to 10 carbon atoms, and such a carbon source may have 1 to 3 heteroatoms selected from the group consisting of oxygen, nitrogen, chlorine, fluorine, and sulfur. Such a carbon source may partially or entirely replace the solvent of the colloidal solution, or may be additionally mixed. In the case of additional mixing, the carbon source may be introduced into the reactor together with the colloidal solution when the colloidal solution is sprayed into the reactor to carry out the reaction.
[0139] In particular, when water is used as a solvent for the colloidal solution, a separate carbon source must be supplied during the reaction.
[0140] [Production Example 1] Manufacturing of functional catalyst carriers
[0141] 100 parts by weight of polyethylene glycol and 0.5 parts by weight of FeCl3 as a metal precursor were mixed, and 1.0 part by weight of a support was mixed therewith and stirred at a speed of 380 rpm for 90 minutes to adsorb the metal precursor onto the support. At this time, the support was a 370 m2 BET specific surface area support treated with ozone at 280°C for 200 minutes at a flow rate of 100 mg / min. 2 / g of carbon nanotubes were used.
[0142] Next, the mixed liquid of the polyethylene glycol, metal precursor and support was heated to 78°C and subjected to vibration with an amplitude of 2 mm and a frequency of 2.3 kHz for 30 minutes to disperse uniformly, after which the vibration was stopped and the temperature was raised to 180°C and heated for 8 hours to obtain a catalyst support in which the metal precursor was uniformly adsorbed on the support.
[0143] Then, the catalyst carrier was mixed in a reducing solution of 100 parts by weight of water, 5 parts by weight of methanol, and 40.05 parts by weight of LiBH4 as a reducing agent in a weight ratio of 100:5, and a current density of 230 A / cm 2The sample was irradiated with an electron beam at an accelerating voltage of 400 keV for 7 minutes.
[0144] The mixture was then filtered and the powder components were heated at 850° C. for 4 hours to produce a functional catalyst support.
[0145] Synthesis of Carbon Nanotubes
[0146] 0.25 g of the catalyst structure prepared above was placed in a quartz boat and placed in the center of a quartz tube with a diameter of 27 mm in an electric furnace. Argon (Ar) gas was then supplied at a flow rate of 100 ml / min, and the temperature of the electric furnace was increased to 800°C. Thereafter, argon (Ar) gas containing 2 vol % of vaporized benzene was injected into the reactor while synthesizing carbon nanotubes for 30 minutes.
[0147] [Experimental Example 4] Carbon nanotubes were synthesized using the same method as in Preparation Example 1, but the electron beam irradiation conditions during the production of the functional catalyst support were changed as shown in Table 4 below, and carbon nanotubes were synthesized using each functional catalyst support in the same manner as in Preparation Example 1. The diameter distribution diagram and BET specific surface area of each carbon nanotube were then measured to calculate the synthesis yield, and the results are shown in Table 4. At this time, Comparative Example 11 in Table 4 is a case in which a functional catalyst support produced without the electron beam irradiation step was used.
[0148] The diameter distribution diagram was prepared by taking a scanning electron microscope (SEM) photograph of each synthesized carbon nanotube, measuring the diameters of 10 random strands, including the thinnest and thickest carbon nanotube strands in the photograph, and calculating the average value and standard deviation, which are listed in Table 4.
[0149] Synthesis yield (%)=[amount of carbon nanotubes produced (g) / amount of catalyst structure provided (g)]×100 (Equation 3)
[0150] [Table 4]
[0151] Referring to the experimental results in Table 4, it can be seen that in Examples 11 to 13, carbon nanotubes having a high specific surface area and a uniform diameter distribution were obtained.
[0152] On the other hand, in the cases of Comparative Examples 11 to 15, the diameter distribution diagrams are non-uniform, the synthesis yield is low, and in the cases of Comparative Examples 11, 13 and 15, the specific surface area is significantly lower than that of the other samples.
[0153] In particular, when Example 12 and Comparative Example 15 are taken together, it can be seen that when the density current amount is the same and the irradiation time exceeds 10 minutes, the specific surface area is rapidly reduced, the uniformity of the diameter distribution diagram is reduced, and the synthesis yield is significantly reduced. This is believed to be due to problems such as damage to the support and changes in the bonding structure of the catalyst metal caused by the excessively long electron beam irradiation time.
[0154] In addition, when Example 13 and Comparative Example 14 are taken together, it can be seen that even when the irradiation time is less than 3 minutes, the diameter distribution and synthesis yield are significantly reduced. This is believed to be due to the fact that the particle size of the reduced metal is not controlled by electron beam irradiation because the electron beam irradiation time is too short.
[0155] Therefore, from the results of this experiment, in order to improve the specific surface area of carbon nanotubes, to uniformize the diameter distribution, and to improve the synthesis yield, the electron beam is irradiated at a density current of 100 to 500 A / cm in the electron beam irradiation step in the carbon nanotube manufacturing method according to one embodiment of the present invention. 2 It can also be confirmed that irradiation is preferably performed for 3 to 10 minutes under conditions of an acceleration voltage of 300 to 600 keV.
[0156] Another embodiment of the present invention includes a method for producing branched carbon nanotubes with improved hydrophilicity, which results in the formation of multiple Y junctions on a straight central carbon nanotube, and at such Y junctions, branched carbon nanotubes are formed extending from the central carbon nanotube, resulting in the formation of branched carbon nanotubes having an overall tree-like structure.
[0157] Such branched carbon nanotubes have the advantage of being very stable and highly efficient when used as electrochemical materials because they have a plurality of Y-junctions.
[0158] A method for producing branched carbon nanotubes according to one embodiment of the present invention includes a pretreatment step of immersing carbon nanotubes in an acidic solution, a heat treatment step of heat treating the carbon nanotubes obtained in the pretreatment step to produce a support, a catalyst structure production step of mixing the support, a solvent and a catalyst precursor and reducing the catalyst precursor to produce a catalyst structure in which a catalyst is bonded to a support, and a carbon nanotube synthesis step of reacting the catalyst structure with a carbon source to produce branched carbon nanotubes.
[0159] First, the pretreatment step is a step performed to generate physical defects on the surface of the carbon nanotubes used as catalyst supports by immersing the carbon nanotubes in an acidic solution, and in a subsequent step, to adsorb metal catalyst particles to the defect sites and induce the growth of branched carbon nanotubes.
[0160] Specifically, this step includes a first pretreatment step of immersing the carbon nanotubes in an acidic solution and ultrasonically treating them, and a second pretreatment step of subjecting the mixture that has undergone the first pretreatment step to underwater plasma discharge.
[0161] The first pretreatment step is a step for uniformly dispersing the carbon nanotubes in the acidic solution by immersing the carbon nanotubes in the acidic solution and subjecting them to ultrasonic treatment. At this time, the acidic solution that can be used is an aqueous weak acid solution containing at least one weak acid selected from the group consisting of acetic acid, formic acid, lactic acid, benzoic acid, propionic acid, citric acid, malonic acid, adipic acid, and tartaric acid.
[0162] If the acidic solution used in the first pretreatment step is a strong acid aqueous solution containing sulfuric acid, hydrochloric acid, nitric acid, or phosphoric acid, etc., physical defects in the carbon nanotubes can be induced by the first pretreatment step alone. However, there is a problem that the strong acidity can excessively increase the amount of physical defects, resulting in the formation of brush-like carbon nanotubes centered on a central carbon nanotube rather than branched carbon nanotubes. Therefore, it is preferable to use the above-mentioned weak acid aqueous solution as the acidic solution in this case.
[0163] The first pretreatment step can be carried out at 80 to 130°C for 1 to 5 hours. Through this step, the carbon nanotubes are uniformly dispersed, and hydrophilic functional groups are bonded to the carbon nanotubes by the simultaneous action of heat and weak acid, thereby imparting hydrophilicity to the carbon nanotubes.
[0164] The second pretreatment step is a step of generating radicals by applying a pulsed underwater plasma discharge to the weak acid aqueous solution in which the carbon nanotubes are immersed, and generating more physical defects in the carbon nanotubes by the radicals thus generated. At the same time, the radicals generated by the plasma discharge bind to the sites of the carbon nanotubes where physical defects have occurred, hydrophilizing the carbon nanotubes used as carriers, thereby improving the hydrophilicity of the branched carbon nanotubes obtained as a final product and improving the dispersibility in various solvents.
[0165] In addition, various contaminants contained in the mixture used in the reaction are removed through plasma discharge, which has the advantage that a carrier with higher purity and stability can be produced.
[0166] In this step, the underwater plasma discharge can be applied at a frequency of 3-6 kHz, a pulse width of 3-5 seconds, and a power of 600-1200 W. These plasma discharge conditions are for inducing plasma generation while forming physical defects in the carbon nanotubes due to the plasma discharge, and for forming the final branched carbon nanotube into a branched type with multiple Y junctions rather than a brush type or integrated type. Therefore, it is preferable to maintain these discharge conditions during the underwater plasma discharge.
[0167] The second pretreatment step can be carried out at a temperature range of 10 to 60°C for 30 minutes to 2 hours. If the process is carried out at a temperature lower than the above-mentioned temperature conditions or for a shorter period of time, the rate of physical defect formation is low. If the process is carried out at a temperature higher than the above-mentioned temperature conditions or for a longer period of time, excessive defects are generated, and instead a branched structure is not formed, resulting in a deterioration in the physical and electrical properties of the final carbon nanotubes. Therefore, it is preferable to carry out a plasma treatment during the above-mentioned process time.
[0168] Next, a heat treatment step is performed to heat treat the carbon nanotubes obtained in the pretreatment step to produce a support. The carbon nanotubes obtained in the pretreatment step can be used in the heat treatment step after filtering and washing, and the heat treatment step removes contaminants and amorphous carbon present on the surface of the carbon nanotubes to obtain carbon nanotubes with higher purity. The carbon nanotubes obtained here are used as supports for supporting catalysts in the subsequent steps.
[0169] This step is a step of heat-treating the pretreated carbon nanotubes in an oxygen atmosphere for 20 to 80 minutes at a temperature range of 280 to 550°C, where the oxygen atmosphere means oxygen alone or a gas containing oxygen, such as air. Since the heat treatment is performed in an oxygen atmosphere, the functional groups that impart hydrophilicity to the surface of the carbon nanotubes are maintained as they are, and the hydrophilicity of the carbon nanotubes used as carriers can be maintained even in the subsequent steps.
[0170] If the heat treatment temperature or time in this step is below the above range, the purification effect will be negligible, and if it exceeds the above range, excessive heat treatment may actually reduce the physical properties and hydrophilicity of the carbon nanotubes used as a support, so it is preferable to carry out the heat treatment within the above process conditions.
[0171] The catalyst structure preparation step is a step of mixing the carbon nanotubes obtained through the heat treatment step, i.e., the carrier, with a solvent and a catalyst precursor to form a catalyst structure in which the catalyst is bonded to the carrier. Through this step, the catalyst precursor is bonded and reduced to the area where physical defects occur in the carbon nanotubes, and this area acts as a Y-junction formation area, making it possible to manufacture branched carbon nanotubes.
[0172] This step is carried out in a multi-step manner, specifically including a first step of mixing the support, a solvent and a catalyst precursor to prepare a precursor mixture, a second step of drying the precursor mixture at a temperature range of 90 to 120°C to prepare a supported catalyst, a third step of mixing the supported catalyst with a reducing liquid and stirring to prepare a catalyst structure, and a fourth step of filtering and washing the catalyst structure.
[0173] The first step is to prepare a precursor mixture by mixing the support, the solvent and the catalyst precursor. The support is the carbon nanotubes obtained by the previous heat treatment step.
[0174] The solvent is used as a dispersion medium for uniformly dispersing the carrier and the catalyst precursor to adsorb and support the catalyst precursor on the carrier, and may be at least one selected from the group consisting of aromatic hydrocarbons, aliphatic hydrocarbons, alcohol compounds, and water. For example, benzene, toluene, xylene, etc. can be used as the aromatic hydrocarbon, hexane, heptane, octane, etc. can be used as the aliphatic hydrocarbon, and ethanol, propyl alcohol, polyethylene glycol, etc. can be used as the alcohol compound.
[0175] In particular, it is preferable to use an alcohol compound, especially polyethylene glycol, as the solvent. In this case, the catalyst precursor can be uniformly dispersed in the solvent without using a separate surfactant. This prevents the decrease in the accessibility between the catalyst precursor and the support caused by the surfactant, and does not require a post-process to remove the surfactant, which is more effective in terms of reaction efficiency and process efficiency.
[0176] The catalyst precursor is a metal salt that is a precursor of a catalyst for forming carbon nanotubes, and at least one metal salt selected from the group consisting of iron (Fe), cobalt (Co), nickel (Ni), platinum (Pt), palladium (Pd), molybdenum (Mo), and vanadium (V) can be used, which is at least one metal salt selected from the group consisting of oxides, nitrides, borides, fluorides, bromides, sulfides, chlorides, and carbonates.
[0177] In this step, the precursor mixture may contain 0.1-10 parts by weight of the carrier and 0.1-1.2 parts by weight of the catalyst precursor with respect to 100 parts by weight of the solvent. If the content of the carrier in the precursor mixture is less than 0.1 parts by weight, the productivity of the supported catalyst decreases, and if it exceeds 10 parts by weight, even if the content of the catalyst precursor is increased, the catalyst adsorption efficiency to the carrier decreases, so it is preferable that it is contained within the above-mentioned weight range. At this time, in order to maximize such effects, it is more preferable that the carrier is contained in an amount of 0.5-3 parts by weight.
[0178] The content of the catalyst precursor is also within a range for maximizing the supporting efficiency on the support, so the precursor mixture preferably contains components within the above-mentioned content ranges.
[0179] This step can be performed by first mixing the solvent and catalyst precursor, then mixing the carrier with the mixture and stirring for 2 to 4 hours at a stirring speed of 300 to 600 rpm. Through this step, physical defects are induced by underwater plasma discharge, and the metal salt as the catalyst precursor is adsorbed to the radicals formed at the physical defect sites, so that the catalyst metal can be bonded to the physical defect areas in the subsequent reduction process.
[0180] In this step, the precursor mixture may further include a catalyst function improver, which helps the metal precursor to be adsorbed on the support in a uniform and consistent size in a solvent environment without a separate surfactant, and prevents excessive aggregation of metal particles during the reduction process. Therefore, when a catalyst function improver is added, carbon nanotubes with uniform physical properties can be grown, and the yield of branched carbon nanotubes can be increased.
[0181] Such catalyst function improvers include at least one of indole, imidazole and hectorite compounds, and the hectorite compounds that can be used include dihydrogenated tallow benzylmonium hectorite, disteardimonium hectorite, quaternium-18 hectorite and stearalkonium hectorite.
[0182] Such a catalyst function improver can be mixed together with the solvent in the step of mixing the catalyst precursor, and can be included in an amount of 17 to 58 parts by weight based on 100 parts by weight of the catalyst precursor.
[0183] Preferably, at least one first compound selected from the group consisting of indole and imidazole can be used together with the second compound, which is a hectorite compound, because when used together in this manner, the above-mentioned effects are more excellent than when the first compound and the second compound are used alone.
[0184] In this case, the first and second compounds are 1: 0.3~0.7 If they are used outside this mixing ratio, the catalyst function improvement effect is rather poor due to factors such as reduced stability, making it difficult to obtain an effect of improving the yield of carbon nanotubes. Therefore, it is preferable to use them together within the above weight range.
[0185] Next, the second step is a step of filtering and drying the mixture obtained through the first step to obtain a supported catalyst. Drying in this step can be performed at a temperature range of 90 to 120°C for 2 to 10 hours, and by going through this step, adsorption of the catalyst precursor to areas of the support where no physical defects occur is minimized, and branched carbon nanotubes can be grown only in areas where physical defects occur, and a dry powder supported catalyst can be obtained through this step.
[0186] Next, the third step is a step of producing a catalyst structure by mixing the supported catalyst obtained through the second step with a reduction liquid and stirring the mixture to reduce the catalyst precursor to a catalyst metal.
[0187] In this step, the reduction liquid is mixed with a supported catalyst, and the mixture is heated and stirred at a temperature range of 20 to 200° C. and a stirring speed of 300 to 600 rpm for 1 to 4 hours.
[0188] In this step, the reducing solution includes a solvent and a reducing agent, and the reducing agent may include at least one of hydrazine, LiBH4, NaBH4, ethylene oxide, formaldehyde, formic acid, and polyol.
[0189] The reducing solution may contain 0.01 to 0.5 parts by weight of a reducing agent per 100 parts by weight of the solvent. If the content of the reducing agent is outside the above weight range, there may be a problem that the metal salt is not sufficiently reduced or that the economic efficiency is reduced. Therefore, it is preferable that the content of the reducing agent is within the above weight range.
[0190] The fourth step is a step of filtering the catalyst structure with the mixture obtained in the third step and washing it with a solvent to remove the unreacted reducing agent. In this case, the solvent used for the reducing solution can be used as the solvent used for washing.
[0191] On the other hand, the carbon nanotube synthesis step is a step in which the previously obtained catalyst structure is reacted with a carbon source to synthesize carbon nanotube branches from physical defect regions of the catalyst structure, and through this step, branched carbon nanotubes having multiple Y junctions can be synthesized.
[0192] The method for synthesizing carbon nanotubes in this step is not particularly limited, and can be, for example, an arc discharge method, a laser vaporization method, a CVD method, a catalytic synthesis method, a plasma synthesis method, a continuous gas phase synthesis method, etc., but is not limited to these.
[0193] For example, the catalyst structure can be placed in a quartz boat and placed inside a reactor to produce carbon nanotubes.
[0194] As an example, the catalyst structure is dispersed in a solvent and continuously supplied into a reactor while the carbon nanotube synthesis reaction is carried out, whereby two-dimensional or three-dimensional Y-branch carbon nanotubes can be continuously produced.
[0195] In this case, the catalyst structure is prepared in the form of a colloidal solution in a solvent such as water or an organic solvent, and when it is finely dispersed or sprayed inside a reactor to suspend the colloidal solution particle droplets in a gas, they exist as gas-phase colloids for a certain period of time, thereby allowing two- or three-dimensional carbon nanotubes to be continuously synthesized in the gas phase.
[0196] The method for converting the dispersion or colloidal solution obtained by dispersing the catalyst structure in a solvent into a gas phase or suspending it in a gas is not particularly limited, and may be performed by a method commonly used in the art, such as direct spraying, siphon spraying, atomization, etc.
[0197] Meanwhile, when dispersing the catalyst structure in a solvent such as water or an organic solvent, a surfactant may be added in an amount that does not adversely affect the carbon nanotube synthesis reaction in order to prevent aggregation and uniformly disperse the catalyst structure. In this case, the type of the surfactant used is not particularly limited.
[0198] The carbon source in the carbon nanotube synthesis step may be, for example, an organic compound selected from the group consisting of carbon monoxide, saturated or unsaturated aliphatic hydrocarbons having 1 to 6 carbon atoms, or aromatic hydrocarbons having 6 to 10 carbon atoms, and such a carbon source may have 1 to 3 heteroatoms selected from the group consisting of oxygen, nitrogen, chlorine, fluorine, and sulfur. Such a carbon source may partially or entirely replace the solvent of the colloidal solution, or may be additionally mixed. In the case of additional mixing, the carbon source may be introduced into the reactor together with the colloidal solution when the colloidal solution is sprayed into the reactor, and the reaction may be carried out. In particular, when water is used as the solvent of the colloidal solution, a separate carbon source must be supplied during the reaction.
[0199] [Production Example 2] Fabrication of the catalyst structure
[0200] First, the carbon nanotubes were immersed in a propionic acid solution, heated to 90°C, and ultrasonically treated for 2 hours. The temperature was then lowered to 35°C, and underwater plasma was generated for a total of 50 minutes at a frequency of 5 kHz, a pulse width of 4 seconds, and a power of 800 W to induce physical defects in the carbon nanotubes. The carbon nanotubes were then filtered and washed with water to produce carbon nanotubes with physical defects, which were then heat-treated in an oxygen atmosphere at 450°C for 60 minutes to produce a carrier.
[0201] Next, 0.5 parts by weight of FeCl3 as a catalyst precursor was mixed with 100 parts by weight of polyethylene glycol as a solvent, and 4.5 parts by weight of the carrier was mixed, and the mixture was stirred at a stirring speed of 400 rpm for 3 hours to prepare a precursor mixture.
[0202] Next, the precursor mixture was filtered and dried at 105°C for 4 hours to obtain a supported catalyst. This was mixed with a reducing solution and stirred at 120°C and 400 rpm for 2 hours to reduce the catalyst precursor, thereby producing a catalyst structure. At this time, a reducing solution containing 40.2 parts by weight of LiBH4 as a reducing agent for 100 parts by weight of polyethylene glycol was used as the reducing solution.
[0203] Then, the catalyst structure was filtered from the mixture and washed with polyethylene glycol to produce the final catalyst structure.
[0204] Synthesis of Carbon Nanotubes
[0205] 0.25 g of the catalyst structure prepared above was placed in a quartz boat and placed in the center of a quartz tube with a diameter of 27 mm in an electric furnace. Helium gas was then supplied at a flow rate of 100 ml / min to raise the temperature of the electric furnace to 1000°C.
[0206] Thereafter, carbon nanotubes were synthesized for 30 minutes while hydrogen gas containing 2 vol % of vaporized benzene was injected into the reactor.
[0207] [Experimental Example 5] The catalyst structure was manufactured using the same method as in Manufacturing Example 2, but the underwater plasma application conditions in the catalyst structure manufacturing step were changed as shown in Table 5 below to manufacture the catalyst structure. Thereafter, the catalyst structures of each Example and Comparative Example were used as catalysts to synthesize carbon nanotubes using the same method as in Manufacturing Example 2, and the synthesis yield, surface resistance, BET specific surface area, and water dispersibility of the carbon nanotubes were measured, and the results are shown in Table 5.
[0208] The synthesis yield was confirmed by calculation according to the following formula 4. Synthesis yield (%)=[amount of carbon nanotubes produced (g) / amount of catalyst structure provided (g)]×100 (Equation 4)
[0209] The surface resistance was measured by mixing 27 wt% of the produced carbon nanotubes, 96.5 wt% of polycarbonate polymer, and 0.8 wt% of additives including stabilizers, lubricants, and antioxidants, and heating and molding the mixture to produce test pieces with a thickness of 3.0 mm and a length of 11.4 mm. The surface resistance of each test piece was then measured using SRM-110 (Pinion).
[0210] Water dispersibility was evaluated by mixing each carbon nanotube in water at a concentration of 0.1 wt%, dispersing it for 1 minute with ultrasonic waves at 20 KHz and 110 W output, and then checking whether or not a precipitate was generated. If a precipitate was generated, it was rated as X, and if no precipitate was generated, it was rated as O.
[0211] [Table 5]
[0212] From the experimental results in Table 5, it was confirmed that Examples 21 and 22 had significantly lower surface resistance than the Comparative Example, and also had excellent synthesis yields and specific surface areas.
[0213] In particular, when considering the experimental results of Example 21, Example 22, Comparative Example 21 and Comparative Example 22, respectively, the result values of Comparative Example 21 and Comparative Example 22 are significantly lower than those of the Examples. This is believed to be due to the fact that the frequency of the plasma applied when manufacturing the catalyst structure for synthesizing the carbon nanotubes of the comparative examples is excessively low or high, resulting in insufficient formation of physical defects in the catalyst structure by the plasma, resulting in a decrease in the adsorption efficiency of the metal catalyst precursor, or excessive formation of physical defects, resulting in damage to the shape of the central pillar of the branched carbon nanotube.
[0214] In addition, in the case of Comparative Example 21, it was confirmed that precipitation occurred during dispersion in water, resulting in lower water dispersibility than the other carbon nanotubes.
[0215] On the other hand, even when the results of Example 21, Comparative Example 23 and Comparative Example 24 are taken together, it can be seen that Example 21 shows significantly superior results. However, this is considered to be due to the problem of the plasma pulse width being too short or too long, similar to the above reasons.
[0216] Therefore, from the results of this experiment, it can be confirmed that, when manufacturing the catalyst structure, it is preferable to apply plasma under the conditions of a frequency of 3 to 6 kHz and a pulse width of 3 to 5 seconds.
[0217] [Experimental Example 6] The catalyst structure and carbon nanotubes were prepared using the same method as in Preparation Example 2, but the catalyst function improver was further added when preparing the precursor mixture during the catalyst structure preparation step.
[0218] At this time, the catalyst function improver was added in the weight shown in Table 2. At this time, the weight shown in Table 6 is the weight relative to 100 parts by weight of the catalyst precursor. The synthesis yield of carbon nanotubes produced in each example was calculated using the same method as in Experimental Example 5, and the results are also shown in Table 6.
[0219] [Table 6]
[0220] From the experimental results in Table 6, it can be seen that the synthesis yield increases when a catalyst function improver is added during the preparation of the precursor mixture.
[0221] From the results of Examples 23 to 29 in Table 6, it can be seen that the synthesis yield is further increased when indole or hectorite compound is used together as a catalyst function improver than when it is used alone, and it was confirmed that the synthesis yield is particularly increased significantly in Examples 26 and 28.
[0222] From these results, it can be confirmed that the synthesis yield of carbon nanotubes increases when a catalyst function improver is used in the preparation of the precursor mixture. In particular, when indole and hectorite compounds are used as catalyst function improvers in a ratio of 1: 0.3~0.7 When the weight ratio of the precursor mixture is 0.1 to 0.5, it can be confirmed that the stability of the precursor mixture is increased and the catalyst function is improved, thereby obtaining a more significant yield improvement effect. [Industrial Applicability]
[0223] The present invention relates to a method for continuously synthesizing carbon nanotubes using a plasma-treated catalyst, and the method involves plasma-treating a metal salt to produce metal nanoparticles without adding a separate reducing agent, and reacting the metal nanoparticles with a carbon source in the gas phase to continuously produce carbon nanotubes, and thus has industrial applicability.
Claims
1. H 2 or NH 3 a plasma treatment step of plasma treating a metal salt in an atmosphere to produce metal nanoparticles; a first mixture preparation step of preparing an emulsion mixture by mixing a solvent and a surfactant; a second mixture producing step of mixing the emulsion mixture with a carrier gas to produce a second mixture; and reacting the second mixture with metal nanoparticles in a heated reactor to form carbon nanotubes. The metal salt is at least one metal salt selected from the group consisting of oxides, nitrides, borides, fluorides, bromides, sulfides, chlorides, and carbonates of one or more metals selected from the group consisting of iron (Fe), cobalt (Co), nickel (Ni), platinum (Pt), palladium (Pd), molybdenum (Mo), and vanadium (V); A method for continuous synthesis of carbon nanotubes.
2. In the plasma treatment step, the plasma treatment is performed by using H 2 or NH 3 2. The method for continuously synthesizing carbon nanotubes according to claim 1, wherein the method is carried out in a gas atmosphere further containing nitrogen gas and an inert gas of Group 18.
3. H 2 or NH 3 3. The method for continuously synthesizing carbon nanotubes according to claim 2, wherein the nitrogen gas and the Group 18 inert gas are mixed in a volume ratio of 1-5:5:0.01-1.
0.
4. After the plasma treatment step, 3. The method for continuously synthesizing carbon nanotubes according to claim 1, further comprising an oxygen plasma treatment step in which plasma treatment is performed in an oxygen atmosphere.
5. 2. The method for continuously synthesizing carbon nanotubes according to claim 1, wherein the plasma treatment step is performed at a pressure of 0.2 to 2.5 Torr.
6. 2. The method for continuously synthesizing carbon nanotubes according to claim 1, wherein the plasma treatment step is carried out at a frequency in the range of 15 to 30 kHz and at a temperature in the range of 50 to 300°C.
7. In the first mixture preparation step, a solvent containing carbon or a solvent not containing carbon is used as the solvent; 2. The method of claim 1, wherein when a solvent not containing carbon is used in the first mixture preparation step, a carbon source gas is further included in the second mixture preparation step.
Citation Information
Patent Citations
Method for producing carbon nanotubes
JP2004534715A
Fabrication of y-branched carbon nanotubes
JP2007528339A
Method of growing carbon nanotube, and carbon nanotube bundle-formed substrate
JP2010163331A
Pretreatment method and method of forming carbon nanotube
JP2013027843A
Method for mass synthesis of carbon nanotube and carbon nanotube synthesized from it
KR1020200084572A