Polishing composition, polishing method, and method for producing semiconductor substrate

The polishing composition with positive zeta potential abrasive grains and amide group-containing polymer at pH 3.0 to 6.5 addresses the low selectivity issue, enhancing polysilicon polishing efficiency in semiconductor substrates by improving the polysilicon to silicon nitride ratio.

JP7575898B2Active Publication Date: 2024-10-30FUJIMI INCORPORATED
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020153888
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-14
Publication Date
2024-10-30
Estimated Expiration
2040-09-14

AI Technical Summary

Technical Problem

Existing polishing compositions have a low selectivity ratio for polishing polysilicon relative to silicon nitride, necessitating improved polishing rate control for polysilicon in semiconductor substrates containing both materials.

Method used

A polishing composition comprising abrasive grains with positive zeta potential and an amide group-containing polymer, maintained at a pH of 3.0 to 6.5, enhances the polishing rate of polysilicon while reducing the polishing rate of silicon nitride.

Benefits of technology

The composition achieves a high selectivity ratio of polysilicon to silicon nitride polishing rates, ensuring efficient and selective polishing of polysilicon without significantly affecting silicon nitride, thereby improving the manufacturing process for semiconductor substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575898000001
    Figure 0007575898000001
  • Figure 0007575898000002
    Figure 0007575898000002
Patent Text Reader

Abstract

To provide a polishing composition in which the ratio of the polishing rate of polysilicon to the polishing rate of silicon nitride is sufficiently high (that is, the selection ratio is high), and a polishing composition in which the polishing speed of polysilicon is sufficiently high.SOLUTION: A polishing composition includes an abrasive grain having a positive zeta potential and an amide group-containing polymer having a pH greater than 3.0 and less than 6.5.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polishing composition, a polishing method, and a method for producing a semiconductor substrate. [Background technology]

[0002] In recent years, new microfabrication technologies have been developed to accompany the high integration and high performance of LSI (Large Scale Integration). Chemical mechanical polishing (CMP) is one of these technologies, and is frequently used in the LSI manufacturing process, especially in the multi-layer wiring formation process, for planarizing interlayer insulating films, forming metal plugs, and forming buried wiring (damascene wiring).

[0003] CMP has been applied to various processes in semiconductor manufacturing, and one example of such application is the gate formation process in transistor fabrication. When fabricating a transistor, Si-containing materials such as silicon, silicon oxide film (silicon oxide), polycrystalline silicon (polysilicon), and silicon nitride (silicon nitride) may be polished, and depending on the transistor structure, it is necessary to control the polishing rate of each Si-containing material.

[0004] For example, Patent Document 1 discloses an abrasive for polysilicon, which contains aluminum oxide as abrasive grains and water, and has a pH of 10.5 to 11.5. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2006-344786 A Summary of the Invention [Problem to be solved by the invention]

[0006] Recently, substrates containing both polysilicon and silicon nitride have come to be used, and there is an increasing demand for selective polishing of polysilicon in such substrates. However, the technique of Patent Document 1 has a problem in that the ratio (selectivity) of the polishing speed of polysilicon to the polishing speed of silicon nitride is low.

[0007] Therefore, an object of the present invention is to provide a means for improving the ratio of the polishing rate of polysilicon to the polishing rate of silicon nitride (ie, the selectivity).

[0008] Another object of the present invention is to provide a polishing composition having a sufficiently high removal rate of polysilicon. [Means for solving the problem]

[0009] In order to solve the above problems, the present inventors have conducted extensive research and have found that at least one of the above problems can be solved by a polishing composition that contains abrasive grains having a positive zeta potential and an amide group-containing polymer and has a pH of more than 3.0 and less than 6.5, thereby completing the present invention. Effect of the Invention

[0010] According to the present invention, the ratio of the polishing rate for polysilicon to the polishing rate for silicon nitride can be improved. Also, according to the present invention, a polishing composition having a sufficiently high polishing rate for polysilicon is provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention relates to a polishing composition comprising an abrasive having a positive zeta potential and an amide group-containing polymer, and having a pH of more than 3.0 and less than 6.5. The polishing composition of the present invention having such a constitution has the effect of providing a sufficiently high ratio of the polishing rate of polysilicon to the polishing rate of silicon nitride (high selectivity). The polishing composition of the present invention also has the effect of providing a sufficiently high polishing rate of polysilicon.

[0012] The mechanism by which the above-mentioned effects are obtained is believed to be as follows: However, the following mechanism is merely speculation, and the scope of the present invention is not limited thereto.

[0013] The main chain of the amide group-containing polymer contained in the polishing composition is electron donative, and the electron density of the nitrogen atom contained in the amide group of the side chain is high, and the nucleophilicity of the unshared electron pair of the nitrogen atom is enhanced. This unshared electron pair undergoes a nucleophilic reaction with the polysilicon surface, weakening the silicon-silicon bond of the polysilicon. This makes the polysilicon film surface (i.e., the polishing surface) brittle, making it easier to scrape off with abrasive grains, and improving the polishing rate of the polysilicon. In addition, when the object to be polished contains silicon oxide as well as polysilicon, the ratio of the polishing rate of polysilicon to the polishing rate of silicon oxide (selectivity) approaches 1.

[0014] Furthermore, when the object to be polished contains silicon nitride as well as polysilicon, nucleophilic addition to silicon nitride hardly occurs, so the polishing rate of silicon nitride remains low, and therefore the ratio (selectivity) of the polishing rate of polysilicon to the polishing rate of silicon nitride is thought to improve.

[0015] In addition, when using the polishing composition of the present invention to polish polysilicon, the zeta potential of the polysilicon surface is negative. Since the zeta potential of the abrasive grains contained in the polishing composition of the present invention is positive, an attractive force is generated between the abrasive grains and the polysilicon surface, and the abrasive grains are likely to adhere to the polysilicon surface, which is the polishing surface. This allows the abrasive grains to be significantly closer to the polysilicon surface, making it easier for the abrasive grains to scrape off the polysilicon surface, and it is presumed that more efficient polishing of polysilicon can be achieved. Therefore, it is considered that the ratio (selectivity) of the polishing speed of polysilicon to the polishing speed of silicon nitride is improved.

[0016] On the other hand, when using the polishing composition of the present invention to polish silicon nitride, the zeta potential of silicon nitride surface is positive, and a repulsive force occurs between the abrasive grains having positive zeta potential, so that the abrasive grains are difficult to approach the silicon nitride surface.As a result, the abrasive grains are difficult to scrape off the silicon nitride surface, and the polishing speed of silicon nitride remains low.Therefore, it is considered that the ratio (selectivity) of the polishing speed of polysilicon to the polishing speed of silicon nitride is improved.

[0017] Hereinafter, embodiments of the present invention will be described. Note that the present invention is not limited to the following embodiments.

[0018] In this specification, unless otherwise specified, operations and measurements of physical properties are performed under conditions of room temperature (20° C. or higher and 25° C. or lower) and relative humidity of 40% RH or higher and 50% RH or lower.

[0019] In addition, in this specification, "(meth)acrylic" is meant to collectively refer to acrylic and methacrylic, and "(meth)acrylate" is meant to collectively refer to acrylate and methacrylate.

[0020] [Polished object] The object to be polished according to the present invention is not particularly limited, and examples thereof include polysilicon, silicon nitride, silicon carbonitride (SiCN), silicon oxide, metal, SiGe, and the like.

[0021] Examples of objects to be polished that contain silicon oxide include a TEOS-type silicon oxide surface (hereinafter simply referred to as "TEOS") produced using tetraethyl orthosilicate as a precursor, a high density plasma (HDP) film, an undoped silicate glass (USG) film, a phosphorus silicate glass (PSG) film, a boron-phosphorus silicate glass (BPSG) film, and a rapid thermal oxidation (RTO) film.

[0022] Examples of the metal include tungsten, copper, aluminum, cobalt, hafnium, nickel, gold, silver, platinum, palladium, rhodium, ruthenium, iridium, and osmium.

[0023] Among these, an object to be polished containing polysilicon is preferred. Therefore, according to a preferred embodiment of the present invention, the polishing composition is used for polishing an object to be polished containing polysilicon.

[0024] In addition, as described above, when the polishing composition of the present invention is applied to a polishing object that contains polysilicon and silicon nitride, the ratio (selectivity) of the polishing speed of polysilicon to the polishing speed of silicon nitride is improved.Therefore, according to another preferred embodiment of the present invention, the polishing composition is used for selective polishing of polysilicon with respect to silicon nitride.

[0025] [Abrasive grain] The abrasive grains contained in the polishing composition of the present invention have the effect of mechanically polishing an object to be polished, and improve the polishing rate of the object to be polished by the polishing composition.

[0026] The abrasive grains according to the present invention have a positive zeta potential in a polishing composition having a pH of more than 3.5 and less than 6.5. When using an abrasive grains having a zeta potential of 0 or less in a polishing composition having a pH of more than 3.5 and less than 6.5, the ratio (selectivity) of the polishing rate of polysilicon to the polishing rate of silicon nitride decreases. Also, the polishing rate of polysilicon decreases.

[0027] The lower limit of the zeta potential of the abrasive grain in the polishing composition is preferably 10mV or more, more preferably more than 10mV, even more preferably 20mV or more, and particularly preferably more than 20mV.The upper limit of the zeta potential of the abrasive grain in the polishing composition is preferably 40mV or less, more preferably less than 40mV, even more preferably 35mV or less, and particularly preferably less than 35mV.In other words, the zeta potential of the abrasive grain in the polishing composition is preferably 10mV or more and 40mV or less, more preferably more than 10mV and less than 40mV, even more preferably 20mV or more and 35mV or less, and particularly preferably more than 20mV and less than 35mV.

[0028] Abrasive grains having the above-mentioned zeta potential can further improve the ratio (selectivity) of the polishing speed of polysilicon to the polishing speed of silicon nitride. Also, abrasive grains having the above-mentioned zeta potential can further improve the ratio (selectivity) of the polishing speed of polysilicon to the polishing speed of silicon nitride.

[0029] In this specification, the zeta potential of the abrasive grains is a value measured by the method described in the Examples. The zeta potential of the abrasive grains can be adjusted by the amount of cationic groups contained in the abrasive grains, the pH of the polishing composition, etc.

[0030] In the polishing composition of the present invention, the type of abrasive grains may be, for example, metal oxides such as cation-modified silica grains, alumina grains, zirconia grains, titania grains, ceria grains, etc. The abrasive grains may be used alone or in combination of two or more kinds. The abrasive grains may be either commercially available or synthetic.

[0031] The abrasive grains are preferably cation-modified silica particles (silica particles having a cationic group), and more preferably cation-modified colloidal silica particles (colloidal silica particles having a cationic group).

[0032] The colloidal silica can be produced by a sodium silicate method or a sol-gel method, and colloidal silica produced by either method can be suitably used as the abrasive grain of the present invention. However, from the viewpoint of reducing metal impurities, colloidal silica produced by the sol-gel method is preferred. Colloidal silica produced by the sol-gel method is preferred because it contains less metal impurities that are diffusible in semiconductors and less corrosive ions such as chloride ions. Colloidal silica can be produced by the sol-gel method using a conventionally known method, and specifically, colloidal silica can be obtained by hydrolysis and condensation reaction using a hydrolyzable silicon compound (e.g., alkoxysilane or its derivative) as a raw material.

[0033] Here, cationically modified means a state in which a cationic group (e.g., an amino group or a quaternary ammonium group) is bonded to the surface of silica (preferably colloidal silica). According to a preferred embodiment of the present invention, the cationically modified silica particles are amino group-modified silica particles, more preferably amino group-modified colloidal silica particles. According to this embodiment, the ratio (selectivity) of the polishing rate of polysilicon to the polishing rate of silicon nitride can be further improved. Also, according to this embodiment, the polishing rate of an object to be polished containing polysilicon can be increased.

[0034] To cationic modify silica (colloidal silica), a silane coupling agent having a cationic group (e.g., an amino group or a quaternary ammonium group) is added to silica (colloidal silica) and reacted at a predetermined temperature for a predetermined time. In a preferred embodiment of the present invention, the abrasive grains are formed by immobilizing a silane coupling agent having an amino group or a silane coupling agent having a quaternary ammonium group on the surface of silica (more preferably colloidal silica).

[0035] In this case, the silane coupling agent used may be, for example, that described in JP-A-2005-162533.Specific examples of the silane coupling agent include N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, γ-aminopropyltriethoxysilane ((3-aminopropyl)triethoxysilane), γ-aminopropyltrimethoxysilane, γ-triethoxysilyl-N-(α,γ-dimethyl-butylidene)propylamine, N-phenyl-γ-aminopropyltrimethoxysilane, N-(vinylbenzyl)-β-aminoethyl-γ-aminopropyltriethoxysilane hydrochloride, octadecyldimethyl-(γ-trimethoxysilylpropyl)-ammonium chloride, and N-trimethoxysilylpropyl-N,N,N-trimethylammonium chloride. Among them, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, γ-aminopropyltriethoxysilane, and γ-aminopropyltrimethoxysilane are preferably used because of their good reactivity with colloidal silica. In the present invention, the silane coupling agent may be used alone or in combination of two or more kinds.

[0036] The silane coupling agent can be added to silica (colloidal silica) as it is or after diluting with a hydrophilic organic solvent or pure water. By diluting with a hydrophilic organic solvent or pure water, the formation of aggregates can be suppressed. When diluting the silane coupling agent with a hydrophilic organic solvent or pure water, the silane coupling agent may be diluted in the hydrophilic organic solvent or pure water so that the concentration of the silane coupling agent is about 0.01 to 1 g, preferably about 0.1 to 0.7 g, per 1 L of the hydrophilic organic solvent or pure water. The hydrophilic organic solvent is not particularly limited, but examples thereof include lower alcohols such as methanol, ethanol, isopropanol, and butanol.

[0037] In addition, it is considered that the amount of cationic groups introduced to the surface of silica (colloidal silica) can be adjusted by adjusting the pH of the silica raw material and the amount of silane coupling agent added. The amount of silane coupling agent used is not particularly limited, but is preferably 0.01% by mass or more and 3.0% by mass or less, more preferably 0.05% by mass or more and 1.0% by mass or less, based on silica (colloidal silica).

[0038] The treatment temperature when the silica (colloidal silica) is cationically modified with the silane coupling agent is not particularly limited, and may be from room temperature (e.g., 25°C) to a temperature about the boiling point of the dispersion medium in which the silica (colloidal silica) is dispersed, specifically, from 0°C to 100°C, and preferably from room temperature (e.g., 25°C) to 90°C.

[0039] The shape of the abrasive grains is not particularly limited, and may be spherical or non-spherical. Specific examples of non-spherical shapes include polygonal prisms such as triangular prisms and square prisms, cylinders, bales in which the center of a cylinder is bulged out more than the ends, donut shapes in which the center of a disk is penetrated, plates, so-called cocoon shapes with a constriction in the center, so-called association-type spheres in which multiple particles are integrated, so-called confetti shapes with multiple protrusions on the surface, and rugby ball shapes, and various other shapes are not particularly limited.

[0040] The size of the abrasive grains is not particularly limited. For example, the average primary particle diameter of the abrasive grains is preferably 10 nm or more, more preferably 15 nm or more, and even more preferably 20 nm or more. As the average primary particle diameter of the abrasive grains increases, the polishing speed of the object to be polished by the polishing composition increases. In addition, the average primary particle diameter of the abrasive grains is preferably 300 nm or less, more preferably 100 nm or less, even more preferably 50 nm or less, and most preferably 30 nm or less. As the average primary particle diameter of the abrasive grains decreases, it becomes easier to obtain a surface with fewer defects by polishing with the polishing composition. That is, the average primary particle diameter of the abrasive grains is preferably 10 nm or more and 300 nm or less, more preferably 15 nm or more and 100 nm or less, even more preferably 20 nm or more and 50 nm or less, and most preferably 20 nm or more and 30 nm or less. The average primary particle diameter of the abrasive grains can be calculated, for example, based on the specific surface area (SA) of the abrasive grains calculated by the BET method, assuming that the shape of the abrasive grains is a true sphere. In this specification, the average primary particle size of the abrasive grains is a value measured by the method described in the Examples.

[0041] In addition, the average secondary particle diameter of the abrasive grains is preferably 20 nm or more, more preferably 30 nm or more, and even more preferably 35 nm or more. As the average secondary particle diameter of the abrasive grains increases, the resistance during polishing decreases, and stable polishing becomes possible. In addition, the average secondary particle diameter of the abrasive grains is preferably 400 nm or less, more preferably 250 nm or less, even more preferably 100 nm or less, and most preferably 70 nm or less. As the average secondary particle diameter of the abrasive grains decreases, the surface area per unit mass of the abrasive grains increases, the contact frequency with the object to be polished increases, and the polishing rate increases. That is, the average secondary particle diameter of the abrasive grains is preferably 20 nm or more and 400 nm or less, more preferably 30 nm or more and 250 nm or less, even more preferably 35 nm or more and 100 nm or less, and particularly preferably 35 nm or more and 70 nm or less. The average secondary particle diameter of the abrasive grains is a value measured by the method described in the Examples.

[0042] The average degree of association of the abrasive grains is preferably 5.0 or less, more preferably 4.0 or less, even more preferably 3.0 or less, even more preferably 2.5 or less, and most preferably 2.3 or less. As the average degree of association of the abrasive grains decreases, defects can be reduced more. The average degree of association of the abrasive grains is also preferably 1.0 or more, more preferably 1.5 or more, and even more preferably 2.0 or more. This average degree of association is obtained by dividing the value of the average secondary particle diameter of the abrasive grains by the value of the average primary particle diameter. As the average degree of association of the abrasive grains increases, there is an advantageous effect that the polishing speed of the object to be polished by the polishing composition is improved.

[0043] The upper limit of the aspect ratio of the abrasive grains in the polishing composition is not particularly limited, but is preferably less than 2.0, more preferably 1.8 or less, and even more preferably 1.5 or less. In such a range, defects on the surface of the object to be polished can be further reduced. The aspect ratio is the average value obtained by taking the smallest rectangle that circumscribes the image of the abrasive grains by a scanning electron microscope, and dividing the length of the long side of the rectangle by the length of the short side of the same rectangle, and can be determined using general image analysis software. The lower limit of the aspect ratio of the abrasive grains in the polishing composition is not particularly limited, but is preferably 1.0 or more.

[0044] In the particle size distribution of abrasive grains obtained by laser diffraction scattering method, the lower limit of D90 / D50, which is the ratio of particle diameter (D90) when the cumulative particle weight from the fine particle side reaches 90% of the total particle weight and particle diameter (D50) when the cumulative particle weight from the fine particle side reaches 50% of the total particle weight of all particles, is not particularly limited, but is preferably 1.1 or more, more preferably 1.2 or more, and even more preferably 1.3 or more. In addition, in the particle size distribution of abrasive grains in a polishing composition obtained by laser diffraction scattering method, the upper limit of the ratio D90 / D50, which is the ratio of particle diameter (D90) when the cumulative particle weight from the fine particle side reaches 90% of the total particle weight and particle diameter (D50) when the cumulative particle weight from the fine particle side reaches 50% of the total particle weight of all particles, is not particularly limited, but is preferably 2.0 or less, more preferably 1.7 or less, and even more preferably 1.5 or less. Within such a range, defects on the surface of the object to be polished can be further reduced.

[0045] The size of the abrasive grains (average primary particle size, average secondary particle size, aspect ratio, D90 / D50, etc.) can be appropriately controlled by selecting the manufacturing method of the abrasive grains, etc.

[0046] The content (concentration) of the abrasive grains is not particularly limited, but is preferably 0.1 mass% or more, more preferably 0.2 mass% or more, even more preferably 0.5 mass% or more, and particularly preferably more than 0.5 mass% based on the total mass of the polishing composition. The upper limit of the content of the abrasive grains is preferably 20 mass% or less, more preferably 10 mass% or less, even more preferably 5 mass% or less, and particularly preferably less than 5 mass% based on the total mass of the polishing composition. That is, the content of the abrasive grains is preferably 0.1 mass% or more and 20 mass% or less, more preferably 0.2 mass% or more and 10 mass% or less, even more preferably 0.5 mass% or more and 5 mass% or less, and particularly preferably more than 0.5 mass% and less than 5 mass% based on the total mass of the polishing composition. Within such a range, the polishing rate of silicon nitride can be kept low while keeping costs down. Therefore, the ratio (selectivity) of the polishing rate of polysilicon to the polishing rate of silicon nitride can be further improved. In addition, within such a range, the balance between the polishing rate of polysilicon and the polishing rate of silicon nitride can be further improved. In addition, the polishing rate of polysilicon and the polishing rate of silicon oxide can be made more equivalent (the ratio (selectivity) of the polishing rate of polysilicon to the polishing rate of silicon oxide can be made closer to 1). When the polishing composition contains two or more types of abrasive grains, the content of the abrasive grains refers to the total amount of these. When the polishing composition contains two or more types of abrasive grains, the content of the abrasive grains refers to the total amount of these.

[0047] [Amide group-containing polymer] The polishing composition of the present invention contains an amide group-containing polymer. The main chain of the amide group-containing polymer is electron donating, and the electron density of the nitrogen atom contained in the amide group of the side chain is high. The nucleophilic action of the nitrogen atom with high electron density weakens the silicon-silicon bond of the polysilicon, and it is believed that the polishing speed of the polysilicon is improved. In addition, when the object to be polished contains silicon nitride as well as polysilicon, the above action is unlikely to act on silicon nitride, and therefore the ratio (selectivity) of the polishing speed of polysilicon to the polishing speed of silicon nitride is thought to be improved.

[0048] The amide group-containing polymer used in the present invention is a polymer containing structural units derived from amide group-containing monomers at a ratio of more than 50% by mass based on the total structural units. The content of structural units derived from amide group-containing monomers in the polymer is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. Particularly preferably, the content is 100% by mass, i.e., a homopolymer of amide group-containing monomers.

[0049] Examples of the amide group-containing monomer include (meth)acrylamide; N-alkyl (meth)acrylamides such as N-methyl (meth)acrylamide, N-ethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, Nn-butyl (meth)acrylamide, N-sec-butyl (meth)acrylamide, and N-tert-butyl (meth)acrylamide; N,N-dialkyl (meth)acrylamides such as N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N,N-dipropyl (meth)acrylamide, N,N-diisopropyl (meth)acrylamide, N,N-di(n-butyl) (meth)acrylamide, and N,N-di(tert-butyl) (meth)acrylamide; N-vinyl carboxylic acid amides such as N-vinyl formamide and N-vinyl acetamide; N-(2-hydroxyphenyl)-2-propanediol; N-vinyl carboxylic acid amides such as N-vinyl carboxylate and N-vinyl carboxylate; ... N-hydroxyalkyl (meth)acrylamides such as N-hydroxyethyl (meth)acrylamide, N-(2-hydroxypropyl) (meth)acrylamide, N-(1-hydroxypropyl) (meth)acrylamide, N-(3-hydroxypropyl) (meth)acrylamide, N-(2-hydroxybutyl) (meth)acrylamide, N-(3-hydroxybutyl) (meth)acrylamide, and N-(4-hydroxybutyl) (meth)acrylamide; N-alkoxyalkyl (meth)acrylamides such as N-methoxymethyl (meth)acrylamide, N-methoxyethyl (meth)acrylamide, and N-butoxymethyl (meth)acrylamide; N,N-dimethylaminopropyl (meth)acrylamide, N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, and N-vinyl-2-caprolactam.

[0050] These amide group-containing monomers may be used alone or in combination of two or more.

[0051] The amide group-containing polymer may contain, as necessary, a structural unit derived from another copolymerizable monomer that is copolymerizable with the amide group-containing monomer.

[0052] Examples of other copolymerizable monomers include carboxy group-containing monomers such as acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid; acid anhydride group-containing monomers such as maleic anhydride and itaconic anhydride; alkyl (meth)acrylate monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, t-butyl (meth)acrylate, n-propyl (meth)acrylate, n-hexyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; and (meth)acrylates having an alicyclic structure such as cyclohexyl (meth)acrylate, cyclohexyloxyalkyl (meth)acrylate, t-butylcyclohexyloxyethyl (meth)acrylate, isobornyl (meth)acrylate, and dicyclopentanyl (meth)acrylate. acrylate monomers containing an alkoxy group or an oxyalkylene group, such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, methoxydiethylene glycol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, and polypropylene glycol mono(meth)acrylate; cyano group-containing monomers, such as acrylonitrile and methacrylonitrile; olefins, such as ethylene, propylene, butadiene, isoprene, and isobutylene; styrene, α-methylstyrene, vinyl acetate, vinyl propionate, vinyl stearate, alkyl vinyl ethers, vinyl toluene, vinyl pyridine, dialkyl itaconate esters, dialkyl fumarate esters, allyl alcohol, methyl vinyl ketone, allyl trimethyl ammonium chloride, and dimethyl allyl vinyl ketone.

[0053] These other copolymerizable monomers may be used either individually or in combination of two or more.

[0054] More specific examples of the amide group-containing polymer include polyacrylamide, polymethacrylamide, poly N-vinylformamide, poly N-vinylacetamide, etc. Among these amide group-containing polymers, polyacrylamide and poly N-vinylacetamide are preferred from the viewpoint of availability, and polyacrylamide is more preferred.

[0055] The amide group-containing polymer may be used alone or in combination of two or more kinds. The amide group-containing polymer may be a commercially available product or a synthetic product.

[0056] The synthesis method for synthesizing the amide group-containing polymer is not particularly limited, and known polymerization methods such as solution polymerization, emulsion polymerization, bulk polymerization, suspension polymerization, and photopolymerization can be appropriately adopted. The initiator used for polymerization can be appropriately selected from conventionally known thermal polymerization initiators and photopolymerization initiators according to the polymerization method. The polymerization initiator can be used alone or in combination of two or more kinds.

[0057] The lower limit of the weight average molecular weight (Mw) of the amide group-containing polymer is not particularly limited, but is preferably 1000 or more, more preferably more than 1000, even more preferably 1500 or more, even more preferably more than 1500, particularly preferably 5000 or more, and most preferably more than 5000. The upper limit of the weight average molecular weight of the amide group-containing polymer is not particularly limited, but is preferably 100,000 or less, more preferably less than 100,000, even more preferably 90,000 or less, even more preferably less than 90,000, even more preferably 80,000 or less, particularly preferably less than 80,000, and most preferably 55,000 or less.

[0058] That is, the weight average molecular weight of the amide group-containing polymer is preferably 1000 or more and 100000 or less, more preferably more than 1000 and less than 100000, even more preferably 1500 or more and 90000 or less, even more preferably more than 1500 and less than 90000, even more preferably 5000 or more and 80000 or less, particularly preferably more than 5000 and less than 80000, and most preferably more than 5000 and 55000 or less. If the amide group-containing polymer has a weight average molecular weight in the above range, it has excellent solubility and can further improve the ratio (selectivity) of the polishing speed of polysilicon to the polishing speed of silicon nitride. In addition, if the amide group-containing polymer has a weight average molecular weight in the above range, it can further improve the polishing speed of polysilicon.

[0059] The weight average molecular weight of the amide group-containing polymer can be measured by gel permeation chromatography (GPC).

[0060] The content (concentration) of the amide group-containing polymer is not particularly limited, but is preferably 0.0001 mass% or more, more preferably 0.0005 mass% or more, even more preferably 0.001 mass% or more, and particularly preferably 0.01 mass% or more, based on the total mass of the polishing composition. The upper limit of the content of the amide group-containing polymer is preferably 10 mass% or less, more preferably 1 mass% or less, even more preferably 0.5 mass% or less, and particularly preferably 0.1 mass% or less, based on the total mass of the polishing composition. That is, the content of the amide group-containing polymer is preferably 0.0001 mass% or more and 10 mass% or less, more preferably 0.0005 mass% or more and 1 mass% or less, even more preferably 0.001 mass% or more and 0.5 mass% or less, and particularly preferably 0.01 mass% or more and 0.1 mass% or less, based on the total mass of the polishing composition. If the content is within such a range, the ratio (selectivity) of the polishing speed of polysilicon to the polishing speed of silicon nitride can be further improved while suppressing costs. In addition, within such a content range, the polishing rate of polysilicon can be further improved. When the polishing composition contains two or more kinds of amide group-containing polymers, the content of the amide group-containing polymers refers to the total amount thereof.

[0061] [Dispersion medium] The polishing composition of the present invention preferably contains a dispersion medium for dispersing each component. Examples of the dispersion medium include water; alcohols such as methanol, ethanol, and ethylene glycol; ketones such as acetone, and mixtures thereof. Of these, water is preferred as the dispersion medium. That is, according to a more preferred embodiment of the present invention, the dispersion medium contains water. According to a further preferred embodiment of the present invention, the dispersion medium is substantially composed of water. Note that the above "substantially" means that a dispersion medium other than water may be included as long as the objective effect of the present invention can be achieved, and more specifically, the dispersion medium is preferably composed of 90% by mass or more and 100% by mass or less of water and 0% by mass or more and 10% by mass or less of a dispersion medium other than water, and more preferably composed of 99% by mass or more and 100% by mass or less of water and 0% by mass or more and 1% by mass or less of a dispersion medium other than water. As described above, more preferably, the dispersion medium is composed of only water.

[0062] From the viewpoint of not inhibiting the action of the components contained in the polishing composition, it is preferable for the dispersion medium to be water that contains as few impurities as possible. Specifically, pure water or ultrapure water from which impurity ions have been removed with an ion exchange resin and then foreign matter has been removed through a filter, or distilled water is more preferable.

[0063] [pH] The pH of the polishing composition of the present invention is more than 3.0 and less than 6.5. When the pH is 3.0 or less, the difference in zeta potential between the abrasive grains and the object to be polished (particularly silicon oxide) becomes small, the attraction between the abrasive grains and the object to be polished (particularly silicon oxide) becomes weak, and the polishing speed of the object to be polished (particularly silicon oxide) decreases. On the other hand, when the pH is 6.5 or more, the high electron donative property (nucleophilicity) of the unshared electron pair present in the nitrogen atom of the amide group-containing polymer decreases excessively, and the polishing speed of polysilicon or silicon oxide (hence the ratio (selectivity) of the polishing speed of polysilicon to the polishing speed of silicon nitride) decreases excessively.

[0064] The lower limit of pH is preferably 3.5 or more, more preferably more than 3.5, even more preferably 3.7 or more, and particularly preferably more than 3.7.The upper limit of pH is preferably 5.5 or less, more preferably less than 5.5, even more preferably 5.0 or less, and particularly preferably less than 5.0.That is, the pH of the polishing composition is preferably 3.5 or more and 5.5 or less, more preferably more than 3.5 and less than 5.5, even more preferably 3.7 or more and 5.0 or less, and particularly preferably more than 3.7 and less than 5.0.

[0065] The pH of the polishing composition can be measured with a pH meter (manufactured by Horiba, Ltd., model number: LAQUA).

[0066] In the polishing composition of the present invention, a pH adjuster may be added to adjust the pH within a range that does not impair the effects of the present invention.

[0067] The pH adjuster may be either an acid or a base, and may be either an inorganic compound or an organic compound. The pH adjuster may be used alone or in combination of two or more kinds.

[0068] Specific examples of acids used as pH adjusters include inorganic acids such as sulfuric acid, nitric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid, and phosphoric acid; carboxylic acids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylpentanoic acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, and lactic acid; and organic acids such as organic sulfuric acids such as methanesulfonic acid, ethanesulfonic acid, and isethionic acid.

[0069] Specific examples of the base used as the pH adjuster include hydroxides or salts of Group 1 elements, hydroxides or salts of Group 2 elements, quaternary ammonium hydroxide or its salt, etc. Specific examples of the salts include carbonates, hydrogen carbonates, sulfates, acetates, etc.

[0070] The amount of the pH adjuster added is not particularly limited, and may be appropriately adjusted so that the polishing composition has a desired pH.

[0071] [Electrical conductivity (EC) of polishing composition] The lower limit of the electrical conductivity (EC) of the polishing composition of the present invention is preferably 0.01 mS / cm or more, more preferably 0.1 mS / cm or more. The upper limit of the electrical conductivity (EC) of the polishing composition of the present invention is preferably 10 mS / cm or less, more preferably 3 mS / cm or less. Within the above range, the repulsion between the abrasive grains can be appropriately adjusted to ensure sufficient polishing speed and stability (especially for polysilicon). The electrical conductivity of the polishing composition can be adjusted by the type and amount of the amide group-containing polymer, the pH of the polishing composition, the type and amount of the pH adjuster, etc. The electrical conductivity of the polishing composition is a value measured by a tabletop electrical conductivity meter (manufactured by Horiba, Ltd., model number: DS-71).

[0072] [Other ingredients] The polishing composition of the present invention may further contain, as necessary, known additives that can be used in polishing compositions, such as complexing agents, preservatives, and anti-mold agents, to the extent that the effects of the present invention are not significantly impeded.

[0073] The polishing composition according to the present invention preferably does not substantially contain an oxidizing agent. If an oxidizing agent is contained in the polishing composition, the surface of the object to be polished (e.g., polysilicon) is oxidized to generate an oxide film, which may lengthen the polishing time. Specific examples of the oxidizing agent include hydrogen peroxide (H2O2), sodium persulfate, ammonium persulfate, and sodium dichloroisocyanurate. The polishing composition substantially does not contain an oxidizing agent means that the oxidizing agent is not intentionally contained at least. Therefore, a polishing composition that inevitably contains a small amount of an oxidizing agent due to raw materials, manufacturing method, etc. is included in the concept of a polishing composition that does not substantially contain an oxidizing agent. For example, the concentration of the oxidizing agent in the polishing composition is preferably 0.001% by mass or less, more preferably 0.0001% by mass or less, and even more preferably 0.00001% by mass or less (lower limit: 0% by mass).

[0074] [Method of manufacturing the polishing composition] The method for producing the polishing composition of the present invention is not particularly limited, and can be obtained, for example, by stirring and mixing abrasive grains, amide group-containing polymer, and other additives as necessary in a dispersion medium (for example, water). The details of each component are as described above. Therefore, the present invention provides a method for producing a polishing composition, comprising the step of mixing abrasive grains and amide group-containing polymer.

[0075] The temperature at which the components are mixed is not particularly limited, but is preferably 10° C. to 40° C., and may be heated to increase the dissolution rate. The mixing time is also not particularly limited as long as the components can be mixed uniformly.

[0076] [Polishing method and semiconductor substrate manufacturing method] As described above, the polishing composition of the present invention is suitable for use in polishing an object to be polished that contains polysilicon. Thus, the present invention provides a polishing method for polishing an object to be polished that contains polysilicon with the polishing composition of the present invention.

[0077] Furthermore, the present invention provides a method for producing a semiconductor substrate, comprising the step of polishing a semiconductor substrate containing polysilicon by the above-mentioned polishing method.

[0078] As a polishing device, a general polishing device can be used that is equipped with a holder for holding a substrate or the like having an object to be polished, a motor whose rotation speed can be changed, and a polishing platen onto which a polishing pad (polishing cloth) can be attached.

[0079] The polishing pad may be made of any material, including, without particular limitation, a general nonwoven fabric, polyurethane, porous fluororesin, etc. The polishing pad is preferably provided with grooves for storing the polishing liquid.

[0080] Regarding the polishing conditions, for example, the rotation speed of the polishing platen was 10 rpm (0.17 s -1 ) or more 500rpm(8.3s -1 ) or less. The pressure (polishing pressure) applied to the substrate having the object to be polished is preferably 0.5 psi (3.4 kPa) or more and 10 psi (68.9 kPa) or less. The method of supplying the polishing composition to the polishing pad is not particularly limited, and for example, a method of continuously supplying the composition using a pump or the like is used. There is no limit to the amount of supply, but it is preferable that the surface of the polishing pad is always covered with the polishing composition of the present invention.

[0081] After polishing, the substrate is washed with running water, and water droplets adhering to the substrate are removed by a spin dryer or the like, followed by drying to obtain a substrate having a metal-containing layer.

[0082] The polishing composition of the present invention may be a one-liquid type or a multi-liquid type such as a two-liquid type. The polishing composition of the present invention may be prepared by diluting the stock solution of the polishing composition, for example, 10 times or more, with a diluent such as water.

[0083] (polishing speed, selectivity) In an embodiment of the present invention, the polishing speed of polysilicon is preferably 500 Å / min or more, more preferably 600 Å / min or more, and even more preferably 700 Å / min or more. Also, in an embodiment of the present invention, the polishing speed of silicon nitride is preferably 60 Å / min or less, more preferably 50 Å / min or less, and even more preferably 40 Å / min or less.

[0084] When a polishing object containing polysilicon and silicon nitride is polished using the polishing composition of the present invention, a high ratio of the polishing speed of polysilicon to the polishing speed of silicon nitride (high selectivity of polysilicon to silicon nitride) can be achieved. Specifically, in the embodiment of the present invention, the ratio (selectivity) of the polishing speed of polysilicon to the polishing speed of silicon nitride is preferably 10 or more, more preferably 15 or more, even more preferably 20 or more, and particularly preferably 30 or more. The higher the ratio (selectivity) of the polishing speed of polysilicon to the polishing speed of silicon nitride, the more preferable it is, so the upper limit is not particularly limited, but is usually 50 or less.

[0085] In addition, when an object to be polished containing polysilicon and silicon oxide is polished using the polishing composition of the present invention, polysilicon and silicon oxide can be polished at substantially the same polishing rate. Specifically, in an embodiment of the present invention, the ratio (selectivity) of the polishing rate of polysilicon to the polishing rate of silicon oxide is preferably 0.5 or more and 2 or less, more preferably 0.55 or more and 1.5 or less, and even more preferably 0.65 or more and 1.2 or less.

[0086] In this specification, the polishing rates of polysilicon, silicon nitride, and silicon oxide are calculated by the method described in the Examples. In this specification, the ratio of the polishing rate of polysilicon to the polishing rate of silicon nitride (selectivity of polysilicon to silicon nitride) and the ratio of the polishing rate of polysilicon to the polishing rate of silicon oxide (selectivity of polysilicon to silicon oxide) are calculated by the method described in the Examples. EXAMPLES

[0087] The present invention will be described in more detail with reference to the following examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. In addition, unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively.

[0088] The following commercially available amide group-containing polymers were used: Polyacrylamide A (weight average molecular weight: 1500) Polyacrylamide B (weight average molecular weight: 10,000) Polyacrylamide C (weight average molecular weight: 70,000) ·Poly N-vinylacetamide (weight average molecular weight: 50,000).

[0089] (Measurement of Electrical Conductivity of Polishing Composition) The electrical conductivity (EC) of the polishing composition was measured with a tabletop electrical conductivity meter (manufactured by Horiba, Ltd., model number: DS-71).

[0090] (Measurement of Zeta Potential of Abrasive Grains) The prepared polishing composition was provided to ELS-Z2 manufactured by Otsuka Electronics Co., Ltd., and measured by the laser Doppler method (electrophoretic light scattering measurement method) using a flow cell at a measurement temperature of 25° C. The obtained data was analyzed by the Smoluchowski formula to calculate the zeta potential of the abrasive grains in the polishing composition.

[0091] (Measurement of abrasive grain size) The average primary particle size of the abrasive grains was calculated from the specific surface area of ​​the abrasive grains measured by the BET method using a Micromeritics "Flow SorbII 2300" and the density of the abrasive grains. The average secondary particle size of the abrasive grains was measured using a Nikkiso Co., Ltd. dynamic light scattering particle size and particle size distribution analyzer UPA-UTI151.

[0092] (Preparation of abrasive grains) In the same manner as described in Example 1 of JP 2005-162533 A, γ-aminopropyltriethoxysilane was used as a silane coupling agent at a concentration of 2 mmol per 1 L of a methanol solution of silica sol (silica concentration = 20 mass%) to prepare a cocoon-shaped cation-modified colloidal silica having an average primary particle diameter of 23 nm, an average secondary particle diameter of 50 nm, an aspect ratio of 1.2, D90 / D50 of about 1.4, and an average degree of association of 2.17. In addition, a sulfonic acid-modified colloidal silica (prepared by the method described in “Sulfonic acid-functionalized silica through quantitative oxidation of thiol groups”, Chem. Commun. 246-247 (2003), an average primary particle diameter of 20 nm, an average secondary particle diameter of 40 nm, and an average degree of association of 2) was prepared as an anion-modified silica.

[0093] Example 1 The cation-modified colloidal silica obtained above as the abrasive grains and polyacrylamide A as the amide group-containing polymer were added to pure water as the dispersion medium at room temperature (25° C.) to a final concentration of 1 mass % to obtain a mixed liquid.

[0094] Thereafter, nitric acid was added to the mixture as a pH adjuster so that the pH was 4.0, and the mixture was stirred and mixed at room temperature (25°C) for 30 minutes to prepare a polishing composition. The pH of the polishing composition (liquid temperature: 25°C) was confirmed with a pH meter (manufactured by Horiba, Ltd., model number: LAQUA). The zeta potential of the cation-modified colloidal silica in the obtained polishing composition was measured according to the above (measurement of the zeta potential of the abrasive grains), and was +30 mV. The particle diameter of the cation-modified colloidal silica in the polishing composition was the same as the particle diameter of the cation-modified colloidal silica used. The electrical conductivity of the obtained polishing composition was measured according to the above (measurement of the electrical conductivity of the polishing composition), and was 0.8 mS / cm.

[0095] (Examples 2 to 7, Comparative Examples 1 to 7) Polishing compositions of Examples 2 to 7 and Comparative Examples 1 to 7 were prepared in the same manner as in Example 1, except that the type of abrasive grains, the type of amide group-containing polymer, and the pH of the polishing composition were changed as shown in the following Table 1. In the following Table 1, "-" indicates that the agent was not contained.

[0096] In addition, for each of the above polishing compositions, the zeta potential of the abrasive grains in the polishing composition and the electrical conductivity of the polishing composition were measured in the same manner as in Example 1, and the results are shown in the following Table 1. The particle size of the abrasive grains in each polishing composition was the same as the particle size of the abrasive grains used.

[0097] In Comparative Example 6, urea (manufactured by Tokyo Chemical Industry Co., Ltd.) was used instead of the amide group-containing polymer, and in Comparative Example 7, biurea (manufactured by Tokyo Chemical Industry Co., Ltd.) was used instead of the amide group-containing polymer.

[0098] <Evaluation> Each of the polishing compositions obtained above was used to measure the removal rate when polishing any of the following objects to be polished under the following polishing conditions.

[0099] (Polishing equipment and polishing conditions) Polishing equipment: Applied Materials 200mm CMP single-sided polishing equipment Mirra Polishing pad: Nitta Haas Corporation hard polyurethane pad IC1010 Polishing pressure: 3 psi (1 psi = 6894.76 Pa) Polishing platen rotation speed: 97 rpm Head (carrier) rotation speed: 43 rpm Supply of polishing composition: free-flowing Polishing composition supply amount: 200mL / min Polishing time: 60 seconds.

[0100] (Object to be polished) Silicon wafers (200 mm, blanket wafer, Advantec Co., Ltd.) with a film of the object to be polished formed on the surface were prepared. (1) A silicon wafer (poly-Si) with a 5000 Å thick polysilicon film formed on its surface (2) A silicon wafer (TEOS) with a 10,000 Å thick silicon oxide (TEOS) film formed on its surface. (3) A silicon wafer (SiN) with a 2000 Å thick silicon nitride film formed on its surface. The above three types of substrates were polished under the above polishing conditions using each of the polishing compositions obtained above.

[0101] (polishing speed) The polishing speed (polishing rate) was calculated by the following formula.

[0102]

number

[0103] The film thickness was measured using an optical film thickness measuring device (ASET-f5x: manufactured by KLA-Tencor Corporation), and the polishing speed (polishing rate) (Å / min) was evaluated by dividing the difference in film thickness before and after polishing by the polishing time. In Table 1 below, the polishing speeds for polysilicon, silicon nitride, and silicon oxide are shown in the "poly-Si", "SiN", and "TEOS" columns, respectively.

[0104] Regarding the selectivity ratio, the value obtained by dividing the polishing speed of polysilicon by the polishing speed of silicon nitride is shown in the "poly-Si / SiN" column, and the value obtained by dividing the polishing speed of polysilicon by the polishing speed of silicon oxide is shown in the "poly-Si / TEOS" column.

[0105] The evaluation results are shown in Table 1 below.

[0106] [Table 1]

[0107] As is clear from Table 1 above, the polishing compositions of Examples 1 to 7 were found to have a sufficiently high polishing rate for polysilicon compared to the polishing compositions of Comparative Examples 1 to 7. Also, the polishing compositions of Examples 1 to 7 were found to have a sufficiently high ratio of the polishing rate for polysilicon to the polishing rate for silicon nitride (poly-Si / SiN) compared to the polishing compositions of Comparative Examples 1 to 7. In particular, the polishing composition of Example 3 was excellent in both the polishing rate for polysilicon and the selectivity (poly-Si / SiN).

[0108] Moreover, it was found that the polishing compositions of Examples 1 to 7 exhibited a ratio of the polishing rate of polysilicon to the polishing rate of silicon oxide (TEOS) (poly-Si / TEOS) closer to 1 than the polishing compositions of Comparative Examples 1 to 7. This indicates that the polishing compositions of Examples 1 to 7 can polish silicon oxide at the same polishing rate as polysilicon.

Claims

1. an abrasive having a positive zeta potential; an amide group-containing polymer; Including, A polishing composition used for selective polishing of polysilicon relative to silicon nitride, having a pH of more than 3.0 and less than 6.5, comprising: The amide group-containing polymer includes (meth)acrylamide, N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-n-butyl(meth)acrylamide, N-sec-butyl(meth)acrylamide, N-tert-butyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, N,N-di(n-butyl)(meth)acrylamide, N,N-di(tert-butyl)(meth)acrylamide, N-vinylformamide, N-vinylacetamide, N-(2-hydroxyethyl)(meth)acrylamide, The polishing composition is a homopolymer of any one amide group-containing monomer selected from the group consisting of N-(2-hydroxypropyl)(meth)acrylamide, N-(1-hydroxypropyl)(meth)acrylamide, N-(3-hydroxypropyl)(meth)acrylamide, N-(2-hydroxybutyl)(meth)acrylamide, N-(3-hydroxybutyl)(meth)acrylamide, N-(4-hydroxybutyl)(meth)acrylamide, N-methoxymethyl(meth)acrylamide, N-methoxyethyl(meth)acrylamide, N-butoxymethyl(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, N-methylvinylpyrrolidone, and N-vinyl-2-caprolactam.

2. The polishing composition described in claim 1, wherein the amide group-containing polymer is at least one selected from the group consisting of polyacrylamide, polymethacrylamide, poly N-vinylformamide, and poly N-vinylacetamide.

3. The polishing composition according to claim 1 or 2, wherein the amide group-containing polymer has a weight average molecular weight of more than 1,000 and less than 100,000.

4. The polishing composition according to any one of claims 1 to 3, wherein the pH is 3.5 or more and 5.5 or less.

5. 5. The polishing composition according to claim 1, wherein the abrasive grains are cation-modified silica particles.

6. 6. A polishing method comprising polishing an object containing silicon nitride and polysilicon with the polishing composition according to claim 1.

7. A method for manufacturing a semiconductor substrate, comprising polishing a semiconductor substrate containing silicon nitride and polysilicon by the polishing method described in claim 6.

Citation Information

Patent Citations

  • Polishing material for polysilicon and polishing method thereof

    JP2006344786A

  • Polishing liquid, polishing liquid set and substrate polishing method

    JP2016199659A

  • Composition for chemical mechanical polishing and chemical mechanical polishing method using the same

    JP2017114966A

  • Aqueous dispersion for chemical mechanical polishing and chemical mechanical polishing method

    WO2016067923A1

  • Polishing solution and polishing method

    WO2019030865A1