DEPOSITION TOOLS AND METHODS FOR DEPOSITING METAL OXIDE FILMS ON ORGANIC MATERIALS - Patent application

Highly reactive organometallic precursors in ALD cycles address the slow growth and degradation issues of conventional ALD, enabling uniform metal oxide spacers for advanced multi-patterning, reducing costs and complexity in semiconductor manufacturing.

JP7575953B2Active Publication Date: 2024-10-30LAM RES CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020572887
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-08-01
Filing Date
2019-06-05
Publication Date
2024-10-30
Estimated Expiration
2039-06-05

AI Technical Summary

Technical Problem

Conventional atomic layer deposition (ALD) precursors result in slow growth rates and significant loss of organic layers, leading to non-uniform metal oxide films unsuitable for advanced multi-patterning processes in semiconductor manufacturing, which increases cost and complexity.

Method used

Employing highly reactive organometallic precursors in ALD cycles to rapidly deposit metal oxide layers, effectively sealing organic photoresists and enabling uniform metal oxide spacers for multi-patterning, reducing the number of lithography-etch cycles.

Benefits of technology

Achieves highly uniform and dense feature patterns with fewer processing steps, lowering the cost and complexity of semiconductor manufacturing while improving accuracy and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575953000001
    Figure 0007575953000001
  • Figure 0007575953000002
    Figure 0007575953000002
  • Figure 0007575953000003
    Figure 0007575953000003
Patent Text Reader

Abstract

An atomic layer deposition (ALD) tool configured to deposit a metal oxide layer over an organic photoresist on a substrate using highly reactive organometallic precursors is disclosed. The use of highly reactive metal precursors results in a very fast growth rate of the metal oxide layer, forming a "seal" that effectively protects the organic photoresist from loss and decomposition due to subsequent exposure to oxygen species during subsequent ALD cycles. The ability to deposit a metal oxide layer means that metal oxide spacers can be utilized in multi-patterning, resulting in highly uniform, dense lines and reduced photolithography-etching steps. [Selected figure] Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Background technology]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority to U.S. Provisional Application No. 62 / 690,210, filed June 26, 2018, and U.S. Provisional Application No. 16 / 052,286, filed August 1, 2018, both of which are incorporated by reference herein for all purposes.

[0002] Atomic layer deposition (ALD) is a deposition method that allows the thickness of thin films formed on semiconductor substrates to be controlled to the order of one atomic monolayer.

[0003] Plasma-enhanced ALD (PEALD) is a further improvement that allows for improved film properties at lower temperatures. PEALD uses chemical precursors (similar to ALD precursors) in an RF-induced plasma to trigger the chemical reactions necessary to form thin films in a highly controlled manner. PEALD offers many advantages, including low-temperature processing, excellent conformality and thickness control of the deposited layer, and the ability for in-situ processing before and after deposition.

[0004] Multiple patterning is a technique for increasing the feature density of integrated circuits (ICs) beyond the limits of photolithography. Such multiple patterning techniques include, for example, pitch division, sidewall image transfer, self-aligned contact, via patterning, layout division, self-aligned double or quadruple patterning, to name a few. Multiple patterning is expected to be required for semiconductor processing at the 10 nm and 7 nm nodes and beyond.

[0005] Self-Aligned Quadruple Patterning (SAQP) is essentially two cycles of a double patterning technique (often called Self-Aligned Double Patterning (SADP)). DPBoth require a substrate having multiple layers formed thereon. For example, from the bottom up, the layers on the substrate may include a first carbon film called an ashable hardmask (AHM) or spin-on carbon layer (SOC), a silicon oxide SiO2 layer, a second carbon AHM / SOC layer, and an antireflective layer (ARL).

[0006] SA DP defines features such as spacers on the substrate using photolithography and further etching steps. In SADP processing, the first step is to deposit a resist material, followed by photolithography to pattern "mandrels" on the top ARL layer on the substrate. The mandrels typically have a pitch at or near the limit of photolithography. The mandrels are then covered with a deposition layer such as silicon oxide (SiO2). A "spacer etch" is then performed to remove (a) the horizontal surfaces of the SiO2 layer and (b) the photoresist. As a result, only vertical surfaces of SiO2 remain on the ARL layer. These vertical surfaces define the "spacers", which have a finer pitch than can be achieved with conventional photolithography.

[0007] SAQP is an extension of the double patterning process described above. In SAQP, the SiO2 spacers are used as a mask in an etch step that removes the underlying ARL and second AHM layers except under the masked areas. The SiO2 spacers are then removed, leaving the second mandrels formed in the AHM layer. Another SiO2 layer is then deposited, followed by another "spacer etch" that removes (a) the horizontal portions of the SiO2 layer and (b) the second mandrels. The result is a structure with SiO2 spacers formed on top of the underlying SiO2 layer. In the SAQP process, the pitch of the second SiO2 spacers is finer than the first spacers, significantly exceeding the limits of conventional lithography.

[0008] Although multiple patterning offers great benefits and helps extend the utility of conventional photolithography to next generation integrated circuits, it has various process limitations. In particular, multiple patterning requires many deposition, photolithography, and etching steps to form spacers. Finer spacer pitches require more photolithography-etching cycles. These additional steps significantly increase the cost and complexity of semiconductor manufacturing. Therefore, a more cost-effective and simple solution is required to implement multiple patterning processes (SADP and SAQP and beyond). Summary of the Invention

[0009] Systems and methods are disclosed for depositing a metal oxide layer over an organic photoresist on a substrate using metalorganic precursors. In a non-exclusive embodiment, the systems and methods are performed in an atomic layer deposition (ALD) tool, with each ALD cycle comprising (1) a first half cycle using a metalorganic precursor to deposit a metal oxide layer over an organic photoresist layer on a substrate, and (2) a second half cycle including a plasma containing oxygen species that tend to decompose the organic photoresist. By using a highly reactive precursor in the first half cycle, the metal oxide layer is deposited at a rate that is so fast that it is sufficient to seal and protect the organic photoresist from decomposition and loss during the second half cycle of the subsequent ALD cycle. In a preferred but non-exclusive embodiment, the organic photoresist is effectively sealed by the metal oxide layer in three or fewer ALD cycles.

[0010] In various non-exclusive embodiments, (a) the metal oxide layer is deposited at a rate of 1.0 angstrom or greater per ALD cycle, and (b) the organometallic precursor is amino(c) the organic photoresist is a carbon photoresist, a polymer photoresist, a carbon ashable hardmask film, or a carbon antireflective layer (ARL); and (d) the metal oxide layer is tin oxide (SnO2).

[0011] In yet another embodiment, the deposited metal oxide layer is used to form spacers on a substrate in a multiple patterning process flow. The use of metal oxide spacers provides many advantages, such as highly uniform spacers, resulting in denser feature patterns, smaller line widths, and fewer photolithography-etch steps. As a result, multiple patterning is greatly simplified, reducing the cost and complexity of semiconductor manufacturing while improving the precision and performance of semiconductor devices.

[0012] In yet another embodiment, the ALD tool is a plasma-enhanced ALD tool (PEALD). [Brief description of the drawings]

[0013] The present application and its advantages are best understood by referring to the following description taken in conjunction with the accompanying drawings.

[0014] [Figure 1] FIG. 1 is a block diagram illustrating an atomic layer deposition (ALD) tool in accordance with a non-exclusive embodiment of the present invention.

[0015] [Figure 2A] 1A-1C are a series of cross-sections of a semiconductor substrate illustrating processing steps in a self-aligned quadruple patterning (SAQP) process in accordance with a non-exclusive embodiment of the present invention. [Figure 2B] 1A-1C are a series of cross-sections of a semiconductor substrate illustrating processing steps in a self-aligned quadruple patterning (SAQP) process in accordance with a non-exclusive embodiment of the present invention. [Figure 2C]1A-1C are a series of cross-sections of a semiconductor substrate illustrating processing steps in a self-aligned quadruple patterning (SAQP) process in accordance with a non-exclusive embodiment of the present invention. [Figure 2D] 1A-1C are a series of cross-sections of a semiconductor substrate illustrating processing steps in a self-aligned quadruple patterning (SAQP) process in accordance with a non-exclusive embodiment of the present invention. [Figure 2E] 1A-1C are a series of cross-sections of a semiconductor substrate illustrating processing steps in a self-aligned quadruple patterning (SAQP) process in accordance with a non-exclusive embodiment of the present invention.

[0016] [Diagram 3] 1 is a flow chart illustrating process steps for implementing SAQP in accordance with a non-exclusive embodiment of the present invention.

[0017] [Figure 4] FIG. 1 is a block diagram illustrating a system controller utilized to control an ALD tool in accordance with a non-exclusive embodiment of the present invention.

[0018] In the drawings, like numerals may be used to designate like structural elements. It should also be understood that the depictions in the figures are schematic and are not necessarily to scale. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present application will now be described in detail with reference to some non-exclusive embodiments illustrated in the accompanying drawings. In the following description, numerous specific details are set forth to facilitate a thorough understanding of the present disclosure. However, it will be apparent to one skilled in the art that the present disclosure can be practiced without some or all of these specific details. Additionally, detailed descriptions of well-known process steps and / or structures have been omitted to avoid unnecessarily obscuring the present disclosure.

[0020] Referring to FIG. layer depositionA block diagram of an ALD tool 10 is shown. The tool 10 comprises a process chamber 12, a showerhead 14, a substrate holder 16 for positioning / holding a substrate 18, an optional RF source 20, and a system controller 22. During operation, one or more reactant gases or "precursors" are supplied one at a time to the process chamber 12 through the showerhead 14. Within the showerhead 14, the precursors are distributed into the chamber 12 via one or more plenums (not shown) throughout the area above the surface of the substrate 18.

[0021] A two-part ALD cycle is used to form a film on the upper surface of substrate 18: (1) In the first half of an ALD cycle, a first precursor is introduced into processing chamber 12 via showerhead 14. The first precursor reacts with substrate 18 to deposit a first layer of first particles on the surface. Processing chamber 12 is then purged. (2) In the second half of the ALD cycle, a second precursor is introduced into the process chamber. The second precursor also reacts with the substrate 18 to form a second layer of second particles on the surface.

[0022] The reactions of both the first and second precursors are self-limiting, meaning that once a particular area of ​​the surface of substrate 18 is covered by particles, further particles do not accumulate in that same area. As a result, each reactant forms an atomic monolayer on the surface of substrate 18.

[0023] The above ALD cycle may be performed multiple times in succession to produce alternating monolayers of the first and second particles. Once a film of a desired thickness is achieved, the ALD cycle is stopped and the process is complete.

[0024] In a non-exclusive embodiment, the ALD tool 10 is a plasma-enhanced ALD or "PEALD" tool. In a PEALD tool, an RF potential generated by an optional RF generator 20 is applied to the showerhead 14, the substrate holder 16, and the like. 16(also not shown), or the showerhead 14 and the substrate holder 16 Regardless of how it is applied, the RF potential creates a plasma 24 within the process chamber 12.

[0025] During an ALD cycle in a PEALD tool, a first precursor is introduced into the process chamber 12 and an RF potential is applied. The resulting plasma 24 causes excited electrons to ionize or dissociate (i.e., "crack") from the first precursor to generate chemically reactive radicals. As these radicals react, particles are deposited on the substrate 18 to form an atomic monolayer. Once the atomic monolayer is complete, the process chamber is purged. A second precursor is then introduced into the process chamber 12 and a plasma is generated by the RF potential, and another monolayer of second particles is formed on the surface of the substrate 18. The above-described two-part ALD cycle may be repeated multiple times until the film formed from alternating monolayers of first and second particles is of a desired thickness.

[0026] In various non-exclusive embodiments, the RF generator 20 may be a single RF generator or multiple RF generators capable of generating high, medium, and / or low RF frequencies. For example, for high frequencies, the RF generator 20 may generate frequencies in the range of 2-100 MHz, preferably 13.56 MHz or 27 MHz. For low frequencies generated, the range is 50 KHz-2 MHz, preferably 350-600 KHz. In yet another embodiment, the RF source 20 may be inductively or passively coupled to one or more RF generating electrodes provided on the showerhead 14 and / or substrate holder 16 as described above.

[0027] In multiple patterning, the ability to deposit metal oxides is advantageous for several reasons: such metal oxide films offer the advantages of (1) improved etch selectivity, and (2) simplified multiple patterning processing, potentially reducing the number of photoresist and etch steps required.

[0028] However, deposition of such thin metal films on organic carbon layers using conventional ALD precursors is problematic for several reasons. Conventional precursors used in the first half of the ALD cycle (such as tetramethyltin) result in very slow growth rates (e.g., on the order of 0.1-0.2 Angstroms) per ALD cycle. As a result, during the second half of the ALD cycle, significant loss and decomposition occurs in the organic carbon layer upon exposure to oxygen species.

[0029] In multi-patterning, the uniformity of the spacer sidewall is crucial. However, with conventional precursors used in ALD processes, the resulting spacer sidewalls are substantially non-uniform due to losses and decomposition experienced during ALD cycles. Sidewall spacer defects generally make conventional precursors incompatible with patterning metal oxide films, such as tin oxide (SnO2), in multi-patterning processes.

[0030] Applicants have defined an ALD cycle that relies on one of several highly reactive precursors. By using the highly reactive precursors, the growth rate of the metal oxide is much faster in the first half of the ALD cycle, even at the low temperatures typically used in PEALD tools. As a result, the metal oxide effectively "seals" the underlying organic layer. Thus, the organic layer is substantially protected from significant loss / decomposition due to exposure to oxygen species during the second half of the ALD cycle.

[0031] In a non-exclusive embodiment, the metal oxide layer is tin oxide (SnO2) that is deposited on the organic photoresist during one or more ALD cycles. For tin oxide, the first half cycle uses a first precursor that includes tin (Sn) and a second precursor that includes an oxygen (O2) species for the second half cycle. Each ALD cycle includes: (1) a first half cycle using a highly reactive organometallic precursor containing tin to deposit a metal oxide layer on an organic photoresist layer on a substrate; and (2) A second half cycle containing oxygen (O2) species, however, a side effect of the oxygen species is to decompose the organic photoresist.

[0032] Using highly reactive organometallic precursors, the deposited metal oxide layer effectively seals the organic photoresist within three ALD cycles. For example, if each first half cycle results in a metal oxide layer thickness of 1.0 angstrom or greater, the organic photoresist is effectively sealed from exposure to oxygen species during the second half of the ALD cycle.

[0033] In a non-exclusive embodiment, the organometallic precursor is a metal organotin precursor ( amino (e.g., methoxy-type precursors or methoxy-type precursors). amino Examples of precursors are (a) dimethylaminodimethyltin (Me2Sn( N Me2)2), (b) dimethylaminotrimethyltin (Me3Sn( N Me2), or (c) tetrakis(dimethylamino)tin (Sn(N M e2)4 ) , (d) tetrakis(diethylamino)tin (Sn(N E t2)4). Examples of methoxy-type precursors include: (a) Dibutyldimethoxytin (Bu2Sn(OMe)2), and , (b) aminotin and methoxymetalorganotin precursors.

[0034] In yet another non-exclusive embodiment, the organic photoresist is a carbon photoresist, a polymer photoresist, a carbon hardmask film, and / or an antireflective layer (ARL).

[0035] In comparison, applicants have found that conventional precursors result in slow growth rates of the metal oxide layer, on the order of 0.1-0.2 angstroms per ALD cycle, and loss of the carbon layer in the range of more than 25 nanometers. By contrast, with one of the highly reactive precursors described above, which accelerates growth to the order of 1.0-2.0 angstroms per ALD cycle, loss is reduced to less than 0.5 nanometers per ALD cycle. This significant reduction in loss makes the deposition of oxide thin films, such as tin oxide (SnO2), suitable for multi-patterning processes.

[0036] ALD cycle details In a non-exclusive embodiment, process parameters for an example of a first and second half cycle of an ALD cycle for depositing a metal oxide layer, such as tin oxide (SnO2), onto an organic photoresist, such as carbon, using an organometallic precursor are provided below.

[0037] The process parameters for the first half cycle include (a) one of the organometallic precursors listed above at a flow rate of 0.1-0.5 liters per minute, (b) a temperature ranging from room or ambient temperature to 125° C., (c) an RF frequency of 13.5 MHz and a potential ranging from 50-1250 Watts, a chamber pressure ranging from 1.0-6.0 Torr, and a duration of 1.0-3.0 seconds.

[0038] The process parameters for the second half cycle include (a) a plasma including oxygen, nitrous oxide, carbon dioxide, ozone, or other oxygen species at a flow rate of 0.1-2 liters per minute, (b) a temperature ranging from room or ambient temperature to 125° C., (c) an RF frequency of 13.5 MHz and a potential ranging from 50-1200 Watts, a chamber pressure ranging from 1.0-6.0 Torr, and a duration of 1.0-3.0 seconds. In yet another embodiment, argon and helium may be included with the oxygen species in the second half of the cycle. The presence of argon and helium helps to create a more uniform plasma in the chamber.

[0039] Multi-Patterning Processing The ability to deposit metal oxides on organic layers offers the opportunity to significantly improve and simplify multi-patterning by reducing (1) the number of layers involved and (2) the number of lithography-etch cycles required. These advantages are realized by introducing or forming spacers formed from metal oxides, which were previously unsuitable due to non-uniformity issues as discussed above.

[0040] 2A-2E, a series of cross sections of a substrate 18 are shown illustrating processing steps in a self-aligned quadruple patterning (SAQP) sequence using metal oxide spacers.

[0041] In Figure 2A, the cross section includes an organic ashable hardmask (AHM) 40 and an organic antireflective layer (ARL) 42 formed on a substrate 18. Mandrels 44 are formed by a photolithographic process and provided on the organic ARL layer 42. In certain embodiments, the mandrels 44 typically, but not necessarily, have a pitch that is equal to or close to the limit of conventional lithography. In other embodiments, the mandrels 44 have a pitch that is greater than that limit. In yet other embodiments, the organic layers 42, 44 can be carbon and / or polymer materials.

[0042] In FIG. 2B, a metal oxide layer 46 is formed over the mandrel 44 and the ARL layer 42. The metal oxide layer 46 is formed using up to three ALD cycles in the tool 10, as described above. In other words, a metal oxide layer having a thickness of at least 1.0 Angstrom is deposited in each half cycle. These layers function to effectively seal the underlying organic mandrel 44 and the ARL layer 42 from decomposition and loss during the second half of each ALD cycle. In a non-exclusive embodiment, the metal oxide layer is tin oxide (SnO2).

[0043] 2C, substrate 18 is shown after a "spacer etch" that removes (a) the horizontal portions of metal oxide layer 46 and (b) mandrels 44. The resulting structure defines a plurality of metal oxide spacers 48. Metal oxide spacers 48 effectively function as second mandrels having a significantly smaller pitch than mandrels 44.

[0044] In FIG. 2D, a silicon oxide (SiO 2 ) layer 50 is formed on the metal oxide spacers 48.

[0045] 2E, a second spacer etch is performed that removes (a) the horizontal portions of silicon oxide layer 50 and (b) the second mandrels (e.g., metal oxide spacers 48). The resulting structure comprises a plurality of silicon oxide spacers 52 on substrate 18 having a pitch that is significantly smaller than that of metal oxide spacers 48.

[0046] By way of example, certain embodiments of the first mandrels 44 may have a pitch in the range of 32-128 nanometers, the metal oxide spacers 48 may have a pitch in the range of 16-32 nanometers, and the silicon oxide spacers 52 may have a pitch in the range of 8-16 nanometers. Thus, the SAQP process described above results in lines and features having dimensions that are significantly smaller than are possible with conventional precursors. It should be understood that these ranges are exemplary and should not be construed as limiting. As semiconductor manufacturing processes improve and feature sizes become smaller and smaller, these ranges may become smaller and smaller.

[0047] The use of highly reactive precursors allows for the formation of highly uniform metal oxide spacers, which offers many advantages. First, the uniformity of the metal oxide spacers allows for very dense lines, leading to very small feature sizes. Second, the metal oxide spacers have high elasticity. Third, the metal oxide spacers also provide a reduction in the number of photoresist etch steps compared to traditional multi-patterning that relies on traditional reactive precursors. The reduction in processing steps reduces the cost and complexity of multi-patterning while improving accuracy and performance.

[0048] In the above embodiments, tin oxide (SnO2) is the only metal oxide mentioned, however, it should be understood that other metal oxides may be used, such as titanium dioxide, hafnium dioxide, zirconium dioxide, tantalum oxide, etc.

[0049] Referring to FIG. 3, a flow chart 300 is shown illustrating the process steps for implementing a SAQP sequence as described above.

[0050] At step 302, mandrels 44 are formed on substrate 18 using photolithography to pattern an organic layer (such as a carbon or polymer material).

[0051] A metal oxide layer 46 is deposited over the mandrel 44 and the underlying organic layer at step 304. The metal oxide layer 46 is deposited using a highly reactive organometallic precursor, such as one of those described above.

[0052] At step 306, a spacer etch is performed that removes (a) the horizontal portions of metal oxide layer 46 and (b) mandrels 44. As a result of the spacer etch, metal oxide spacers 48 are formed. Metal oxide spacers 48 effectively define second mandrels having a finer pitch than first mandrels 44.

[0053] At step 308, a layer of silicon oxide (SiO2) 50 is deposited over the substrate 18, which comprises silicon oxide (SiO2).

[0054] Process 310 Then, a second spacer etch is performed that removes (a) the horizontal portions of silicon oxide (SiO2) 50 and (b) silicon oxide (SiO2). The end result is the formation of spacers 52 that have a pitch that is significantly smaller than the mandrels 44.

[0055] System Controller Referring now to Figure 4, a block diagram of the system controller 22 is shown in accordance with a non-exclusive embodiment of the present invention. 22 are used to generally control the overall operation of the ALD (or PEALD) tool 10 and manage processing conditions during deposition, post-deposition, and / or other processing operations.

[0056] System Controller 22 The computer system 24 may take many physical forms, ranging from integrated circuits to printed circuit boards, small handheld devices, personal computers, servers, and supercomputers (any of which may have one or more processors). The computer system 24 may further include an electronic display device 404 (for displaying images, text, and other data), a non-transitory main memory 406 (e.g., random access memory (RAM)), a storage device 408 (e.g., a hard disk drive), a removable storage device 410 (e.g., an optical disk drive), a user interface device 412 (e.g., a keyboard, touch screen, keypad, mouse, or other pointing device, etc.), and a communications interface 414 (e.g., a wireless network interface). The communications interface 414 may link to the system controller 420, which may include a processor 422, a ROM 424, and a memory 426. 22 and external devices. 22may further comprise a communications infrastructure 216 (eg, a communications bus, crossover bar, or network) to which the above-mentioned devices / modules are connected.

[0057] The term "non-transitory computer-readable medium" is used generally to refer to media such as main memory, secondary memory, removable storage, and storage devices (such as hard disks, flash memory, disk drive memory, CD-ROMs, and other forms of persistent memory), and should not be construed to cover transitory objects, such as carrier waves or signals.

[0058] In certain embodiments, the system controller 22 executes or executes system software or code to control all or at least most of the operation of the tool 10, including operations such as controlling the timing of processing operations, the frequency and power of operation of the RF generator 20, the pressure within the processing chamber 12, the flow rates of reactants, concentrations and temperatures within the processing chamber 12, the timing of purging the processing chamber, etc.

[0059] Information transferred through communications interface 414 may be in the form of signals, such as electronic, electromagnetic, optical, or other signals that may be received by communications interface 414 over a communications link carrying the signals, which may be implemented using electrical wires or cables, optical fibers, telephone lines, cellular phone links, radio frequency links, and / or communications channels. Using such communications interfaces, it is contemplated that one or more processors 402 may receive information from a network or output information to a network. Additionally, method embodiments may be performed solely by the processor or may be performed over a network, such as the Internet, in cooperation with a remote processor that shares some of the processing.

[0060] It should be understood that the embodiments provided herein are merely illustrative and should not be construed as limiting in any respect. In general, the present application is intended to cover any showerhead having at least two sets of holes defining two helical patterns and two plenums for the two patterns.

[0061] Although only a few embodiments have been described in detail, it should be understood that the present application can be embodied in many other forms without departing from the spirit or scope of the disclosure provided herein For example, the substrate can be a semiconductor wafer, another semiconductor device, a flat panel display, or any other type of workpiece.

[0062] Therefore, these embodiments are to be considered as illustrative and not restrictive, and should not be limited to the details given herein, but may be modified within the scope of the appended claims and their equivalents. Application example 1: 1. An atomic layer deposition (ALD) tool configured to deposit a metal oxide layer over an organic photoresist on a substrate using an organometallic precursor. Application example 2: 2. The ALD tool of claim 1, wherein the metal oxide layer is deposited on the organic photoresist during one or more ALD cycles, each ALD cycle comprising: a first half cycle using the organometallic precursor to deposit the metal oxide layer over the organic photoresist on the substrate; a second half cycle including an oxygen species that decomposes the organic photoresist; An ALD tool equipped with Application example 3: The ALD tool of application example 2, wherein the organometallic precursor is sufficiently reactive to seal the organic photoresist with the deposited metal oxide layer in no more than three of the ALD cycles. Application example 4: 3. The ALD tool of application example 2, wherein the metal oxide layer is deposited at a rate of 1.0 angstroms or greater per ALD cycle. Application example 5: The ALD tool of application example 1, wherein the organometallic precursor is a metal organotin precursor. Application example 6: The ALD tool of application example 1, wherein the organometallic precursor is an amino 10 type precursor. Example 7: The ALD tool of application example 6, wherein the amino 10 type precursor is (a) Dimethylaminodimethyltin (Me 2 Sn(NMe 2 ) 2 、 (b) Dimethylaminotrimethyltin (Me 3 Sn(MMe 2 )、 (c) Tetrakis(dimethylamino)tin (Sn(Nme 2 ) 4 、 (d) Tetrakis(diethylamino)tin (Sn(Net 2 )) 4 ,or, (e) other aminometalorganotin precursors; The ALD tool is selected from the group comprising: Application example 8: 2. The ALD tool of claim 1, wherein the organometallic precursor is a methoxy-type precursor. Example 9: The ALD tool of application example 8, wherein the methoxy-type precursor is (a) Dibutyldimethoxytin (Bu 2 Sn(OMe) 2 ),or, (b) any methoxy or ethoxy tin precursor; The ALD tool is selected from the group comprising: Example 10: 2. The ALD tool of application example 1, wherein the organic photoresist is a carbon photoresist. Example 11: 2. The ALD tool of claim 1, wherein the organic photoresist is a polymer photoresist. Application example 12: 2. The ALD tool of claim 1, wherein the organic photoresist is a carbon mask film. Application example 13: 2. The ALD tool of application example 1, wherein the organic photoresist is an antireflective layer (ARL). Example 14: In the ALD tool of application example 1, the metal oxide layer is a tin oxide (SnO 2 ) wherein the organic photoresist is a carbon photoresist. Application example 15: In the ALD tool of application example 1, the metal oxide layer is a tin oxide (SnO 2 ) and the organic photoresist is a carbon antireflective layer (ARL). Application example 16: The ALD tool of application example 2, further comprising: a processing chamber; a substrate pedestal for supporting the substrate within the processing chamber; Equipped with An ALD tool, wherein the one or more ALD cycles are performed in the processing chamber. Example 17: The ALD tool of Application Example 16, wherein the ALD tool is a plasma-enhanced ALD tool (PEALD) equipped with an RF source for generating a plasma in the processing chamber. Application example 18: 2. The ALD tool of claim 1, wherein the deposited metal oxide layer is used to form spacers on the substrate in a multi-patterning process flow. Example 19: A multi-patterning method performed on a substrate, the method comprising forming metal oxide spacers on an organic photoresist on the substrate using an organometallic precursor. Example 20: In the multi-patterning method of Application Example 19, the step of forming a metal oxide spacer further includes: patterning the organic photoresist using photolithography to define mandrels on the substrate; depositing a layer of metal oxide over the mandrels on the substrate; removing the substantially horizontal surface of the layer of metal oxide and the mandrel from the substrate to form the metal oxide spacers on the substrate; A method comprising: Example 21: The multi-patterning method of Application Example 20, further comprising: The metal oxide spacer on the substrate is then formed on silicon oxide (SiO 2 ) layer; The silicon oxide (SiO 2 ) layer and the metal oxide spacers are removed to deposit a SiO 2 forming a spacer; A method comprising: Example 22: 22. The multi-patterning method of claim 21, wherein the metal oxide spacers have a smaller pitch than the mandrels, and the SiO 2 The method, wherein the spacers have a smaller pitch than the metal oxide spacers. Application example 23: The multi-patterning method of Application Example 20, wherein the step of depositing a metal oxide layer further comprises performing up to three atomic layer deposition (ALD) cycles on the substrate, each ALD cycle resulting in a metal oxide film having a thickness of 1.0 angstrom or greater. Application 24: In the multi-patterning method of Application Example 23, each ALD cycle further comprises: depositing the metal oxide film during a first half cycle to form the metal oxide layer; exposing the substrate to oxygen species during a second half cycle; Including, The method, wherein the metal oxide film deposited during the first half cycle serves to prevent the oxygen species from decomposing the mandrel during the second half cycle. Example 25: 22. The multi-patterning method of application example 21, wherein the organometallic precursor is a metal organotin precursor. Example 26: The multi-patterning method of Application Example 25, wherein the organometallic precursor is an amino 10 type precursor. Example 27: In the multi-patterning method of Application Example 26, the amino 10 type precursor is (a) Dimethylaminodimethyltin (Me 2 Sn(NMe 2 ) 2 、 (b) Dimethylaminotrimethyltin (Me 3 Sn(MMe 2 )、 (c) Tetrakis(dimethylamino)tin Sn(Nme 2 ) 4 、 (d) Tetrakis(diethylamino)tin (Sn(Net 2 )4) or (e) any metal organoaminotin precursor; The method is selected from the group comprising: Application example 28: 22. The multi-patterning method of application example 21, wherein the organometallic precursor is a methoxy-type precursor. Example 29: In the multi-patterning method of Application Example 28, the methoxy type precursor is (a) Dibutyldimethoxytin (Bu 2 Sn(OMe) 2 )、 (b) any other methoxy or ethoxy tin precursor; The method is selected from the group comprising: Example 30: In the multi-patterning method of Application Example 21, the organic photoresist is (a) carbon photoresist; (b) a polymer photoresist; (c) a carbon mask film, or (d) carbon antireflection layer (ARL), This is one of the methods. Example 31: In the multi-patterning method of Application Example 19, the metal oxide layer is made of tin oxide (SnO 2 ) wherein the organic photoresist is a carbon photoresist. Example 32: In the multi-patterning method of Application Example 19, the metal oxide layer is made of tin oxide (SnO 2 ) wherein the photoresist is a carbon antireflective layer (ARL). Application 33: The multi-patterning method of Application Example 23, wherein each ALD cycle is performed at a temperature ranging from room temperature to 125° C. Example 34: A multi-patterning method according to Application Example 23, wherein during the first half cycle, depositing the metal oxide film further comprises introducing an organometallic precursor into the processing chamber at a flow rate in the range of 0.1 to 0.5 liters per minute. Application 35: A multi-patterning method according to Application Example 34, further comprising the step of setting the duration of the first half cycle to within the range of 1.0 to 3.0 seconds. Example 36: The ALD tool of application example 1, wherein the metal oxide layer is (a) tin oxide, (b) titanium dioxide, (c) hafnium dioxide, (d) zirconium dioxide, or (e) tantalum oxide, The ALD tool is selected from the group comprising: Example 37: In the multi-patterning method of Application Example 19, the metal oxide spacer is (a) tin oxide, (b) titanium dioxide, (c) hafnium dioxide, (d) zirconium dioxide, or (e) tantalum oxide, The method includes one of the following:

Claims

1. 1. A method comprising: depositing a metal layer over an organic photoresist on a substrate using an organometallic precursor during the first half of one atomic layer deposition (ALD) cycle; exposing the substrate, on which the metal layer is deposited on the organic photoresist, to oxygen species during the second half of the single ALD cycle to form a deposited metal oxide layer; depositing the metal layer and exposing the substrate in a manner such that the deposited metal layer seals the organic photoresist from decomposition by the oxygen species within three or fewer ALD cycles; The method, wherein the organometallic precursor is a metal organotin precursor.

2. 10. The method of claim 1, further comprising depositing the metal oxide layer at a thickness of 1.0 Angstrom or greater per ALD cycle.

3. 10. The method of claim 1, wherein the organometallic precursor is an amino-type precursor.

4. 4. The method of claim 3, wherein the amino type precursor is (a) Dimethylaminotrimethyltin (Me 3 Sn(NMe 2 ), (b) Tetrakis(dimethylamino)tin (Sn(NMe 2 ) 4 ), (c) Tetrakis(diethylamino)tin (Sn(NEt 2 ) 4 ),or, (d) other aminometalorganotin precursors; The method is selected from the group comprising:

5. 2. The method of claim 1, wherein the organic photoresist comprises: (a) a carbon photoresist; (b) a polymer photoresist; (c) a carbon mask film, or (d) antireflection layer (ARL), This method is one of the above.

6. 2. The method of claim 1, wherein the metal oxide layer is tin oxide (SnO 2 ) wherein the organic photoresist is either a carbon photoresist or a carbon antireflective layer (ARL).

7. 10. The method of claim 1 further comprising: using the deposited metal oxide layer to form spacers on the substrate in a multi-patterning process flow.

8. The method of claim 1, comprising: The method according to claim 1, wherein said organometallic precursor is dibutyldimethoxytin.

Citation Information

Patent Citations

  • Copolymer, composition for buffer membrane, pattern forming method using the same and method for producing capacitor by using the same

    JP2007056262A

  • Method of forming hard mask of metal oxide

    JP2012142574A

  • Soft landing nanolaminate for advanced patterning

    JP2015111668A

  • Tin oxide thin film spacers in semiconductor device manufacturing

    JP2018006742A

  • Semiconductor light-emitting element, illuminating device, head light, movable body, illuminating device, video device, projection type image display device and projector

    JP2018064061A