IGZO sputtering target

The IGZO sputtering target with controlled ΔL*, density, and grain size addresses uniformity issues, enhancing the quality of IGZO films by minimizing processing damage and improving film characteristics.

JP7576019B2Active Publication Date: 2024-10-30JX NIPPON MINING & METALS CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2021209835
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-01-13
Filing Date
2021-12-23
Publication Date
2024-10-30
Estimated Expiration
2041-12-23

AI Technical Summary

Technical Problem

The uniformity of characteristics such as microcracks, pores, and surface roughness in IGZO sputtering targets is compromised during the cutting process, leading to increased particle generation and reduced quality of the IGZO film.

Method used

The IGZO sputtering target is designed with an oxide sintered body having specific properties, including a lightness difference (ΔL*) of less than 3.0 between the edge and center, a relative density of 97.0% or more, and controlled grain size, achieved through optimized firing conditions and cutting techniques to minimize processing damage.

Benefits of technology

This design improves the uniformity of microcracks, pores, and surface roughness, resulting in a higher quality IGZO film production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576019000001
    Figure 0007576019000001
  • Figure 0007576019000002
    Figure 0007576019000002
Patent Text Reader

Abstract

To provide IGZO sputtering target capable of improving uniformity for at least one characteristic selected from the number of micro cracks in tissue, the number of pores in sintered body structure, and surface roughness.SOLUTION: The present IGZO sputtering target is a sputtering target having an oxide sintered body comprising indium (In), gallium (Ga), zinc (Zn) and inevitable impurities. On a surface of the oxide sintered body, ΔL* determined by subtracting brightness Lc* in a central part of the surface from brightness Le* at a position of 10 mm from the end of the surface to the central side satisfies ΔL*<3.0, and a relative density of the oxide sintered body is 97.0% or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an IGZO sputtering target. [Background technology]

[0002] Traditionally, α-Si (amorphous silicon) has been used for the TFT (thin film transistor) of the backplane of FPD (flat panel display). However, α-Si does not provide sufficient electron mobility, and in recent years, research and development has been conducted on TFTs using In-Ga-Zn-O oxide (IGZO), which has higher electron mobility than α-Si. Some next-generation high-performance flat panel displays using IGZO-TFTs have been put into practical use and are attracting attention.

[0003] Here, IGZO films can be obtained primarily by DC sputtering a sputtering target made from an IGZO sintered body, and sputtering targets capable of obtaining higher quality IGZO films are under study (e.g., Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2017 / 131111 Summary of the Invention [Problem to be solved by the invention]

[0005] The IGZO sintered body of the sputtering target can be manufactured by sintering a molded body obtained by mixing and molding the desired metal oxides to produce an oxide sintered body, and then cutting it to the desired shape and dimensions. However, even if the oxide sintered body after sintering the molded body has high uniformity, the oxide sintered body after cutting to the desired shape and dimensions in the process of manufacturing the sputtering target may have reduced uniformity in at least one characteristic selected from the number of microcracks in the structure, the number of voids in the sintered body structure, and surface roughness. In such cases, there is a concern that the amount of particles generated during sputtering using the sputtering target will increase, making it difficult to obtain a high-quality IGZO film.

[0006] Therefore, an object of the present invention is to provide an IGZO sputtering target that can improve the uniformity of at least one property selected from the number of microcracks in the structure, the number of voids in the sintered compact structure, and surface roughness. [Means for solving the problem]

[0007] The present inventors have conducted extensive research to solve the problems of the conventional technology described above, and have found that in an oxide sintered body obtained by firing and cutting, differences in properties, particularly differences in the lightness L* of the surface of the sintered body, can occur depending on the position in the sintered body. The inventors have found that this is because at least one of the number of microcracks in the structure or the number of voids in the structure of the sintered body increases locally at the edge of the oxide sintered body due to processing damage during cutting of the oxide sintered body after firing, or the surface roughness increases. Furthermore, the inventors have found that as a result of the change at the edge, the lightness L* at the edge increases relative to the lightness L* at the center. The inventors have also found that if the density of the oxide sintered body is reduced too much in order to reduce the amount of cracks present in the oxide sintered body, nodules that are generated on the oxide sintered body and lead to a deterioration in the quality of the IGZO film are more likely to occur, and have completed the present invention. That is, the present invention is as follows.

[0008] In one embodiment, the IGZO sputtering target of the present invention is a sputtering target having an oxide sintered body composed of indium (In), gallium (Ga), zinc (Zn) and unavoidable impurities, wherein ΔL*, which is obtained by subtracting the lightness Lc* at the center of the surface from the lightness Le* at a position 10 mm from the edge of the surface toward the center, satisfies ΔL*<3.0, and the relative density of the oxide sintered body is 97.0% or more. Effect of the Invention

[0009] According to one embodiment of the present invention, it is possible to provide an IGZO sputtering target that is capable of improving the uniformity of at least one property selected from the number of microcracks in the structure, the number of voids in the sintered compact structure, and surface roughness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail, but the present invention is not limited to the present embodiment.

[0011] The IGZO sputtering target of this embodiment (hereinafter also referred to as "sputtering target") is an IGZO sputtering target having an oxide sintered body made of indium (In), gallium (Ga), zinc (Zn) and unavoidable impurities. The sputtering target of this embodiment can be used to form a semiconductor film, specifically, it can be used to form TFTs (thin film transistors) for FPDs (flat panel displays) such as organic electroluminescence (EL) and flexible displays, transparent semiconductor films for semiconductor products, etc.

[0012] Here, the oxide sintered body of the sputtering target of this embodiment is composed of a composite oxide containing In2O3-Ga2O3-ZnO as a main component. More specifically, for example, in a composition in which the target Ga content and the target Zn content are each 100 when the In content in the oxide sintered body is taken as 100, it is preferable that the atomic ratio of Ga is 100±30 and that of Zn is 100±30. The contents of In, Ga, and Zn in the oxide sintered body can be measured by a method such as fluorescent X-ray or ICP-AES.

[0013] In this embodiment, the oxide sintered body may further contain other additive elements in addition to indium (In), gallium (Ga), and zinc (Zn), and may specifically contain at least one selected from the group consisting of Sn, Zr, Mg, Al, Si, Y, and Ti. The total amount of these other additive elements is preferably 50 to 1000 mass ppm, and more preferably 100 to 500 mass ppm. By setting the total amount of these other additive elements to 1000 mass ppm or less, a sintered body having a desired grain size and sintered body density can be obtained, and by setting the total amount to 50 mass ppm or more, the effect of adding the additive elements can be sufficiently obtained. The additive elements here also include unavoidable impurities due to grinding media wear. In this embodiment, when the oxide sintered body further contains other additive elements, it is preferable that the oxide sintered body contains at least tin (Sn), which can control the grain size and the resistance to microcracks in the structure. When the oxide sintered body contains at least tin, the content of tin is preferably 1000 mass ppm or less, more preferably 500 mass ppm or less.

[0014] In addition, inevitable impurities are generally those that are present in raw materials or are inevitably mixed in the manufacturing process of metal or metal oxide products, such as media used in grinding raw powder. Although they are essentially unnecessary, they are permitted because they are present in trace amounts and do not affect the properties of metal or metal oxide products. In the sputtering target according to this embodiment, the total amount of inevitable impurities is generally 1000 ppm by mass or less, typically 500 ppm by mass or less, and more typically 200 ppm by mass or less.

[0015] In this embodiment, when the lightness at a position 10 mm from the edge of the surface of the oxide sintered body of the sputtering target is Le*, the lightness at the center of the surface of the oxide sintered body is Lc*, and the lightness difference obtained by subtracting Lc* from lightness Le* is ΔL*, the lightness difference ΔL* satisfies ΔL*<3.0. Here, lightness (L*) belongs to one of the three elements of the color system defined in JIS Z 8729, and as lightness increases, the color becomes brighter and closer to white. In other words, the greater the lightness of the surface of the oxide sintered body, the greater the diffuse reflection of visible light, indicating that at least one of microcracks in the sintered body structure and voids in the sintered body structure is present in large numbers, or that the surface roughness is large. In this embodiment, the sputtering target satisfies the lightness difference ΔL* of ΔL*<3.0, so that there is no significant difference between the end and center of the oxide sintered body of the sputtering target in at least one characteristic selected from the number of microcracks in the structure, the number of voids in the sintered body structure, and the surface roughness. Therefore, the sputtering target of this embodiment has an oxide sintered body with less processing damage during cutting and improved uniformity. It is presumed that a high-quality IGZO film can be formed by sputtering using a sputtering target having such an oxide sintered body. From the same viewpoint, in this embodiment, the sputtering target preferably satisfies the difference in brightness ΔL*<2.5, and more preferably ΔL*<2.0.

[0016] In this specification, the lightness can be measured by polishing the surface of the oxide sintered body of the sputtering target with a grindstone of #80 to #800, and then measuring with a simplified spectrophotometer (manufactured by Nippon Denshoku Industries Co., Ltd., model number: NF333). The surface of the oxide sintered body of the sputtering target, which is the object of measurement of lightness Le* and Lc*, is the surface of the oxide sintered body on the side to be sputtered when the sputtering target is used. Specifically, if the oxide sintered body is, for example, disk-shaped or rectangular, the surface is, for example, the surface (flat surface) of the oxide sintered body on the opposite side to the bonding surface with the backing plate, and if the oxide sintered body is cylindrical, the outer peripheral surface of the cylinder. More specifically, the lightness Le* is the arithmetic average of values ​​measured at three positions on the surface of the oxide sintered body of the sputtering target, the positions being 10 mm away from the end of the oxide sintered body toward the center, and the end of the oxide sintered body refers to the end formed by cutting the oxide sintered body after firing, among the ends of the oxide sintered body of the sputtering target. Moreover, from the end to the center refers to the direction perpendicular to the outline of the end. More specifically, the lightness Lc* is the arithmetic average of values ​​measured at three locations in the center of the surface of the oxide sintered body of the sputtering target, and the center of the surface of the oxide sintered body refers to a region of the surface of the oxide sintered body of the sputtering target that is more than 10 mm away from the end of the oxide sintered body (including an end formed by cutting the oxide sintered body after firing and an end that has not been cut) toward the center.

[0017] In the present embodiment, a method for making the difference ΔL* in lightness of the oxide sintered body in the sputtering target satisfy ΔL*<3.0 includes reducing processing damage during cutting of the oxide sintered body, specifically, reducing the cutting speed during cutting and using finer grindstones. However, from the viewpoint of ensuring the productivity of the sputtering target, it is also preferable that the oxide sintered body itself has strength against such processing damage during cutting. An oxide sintered body having strength against processing damage during cutting can be obtained by adjusting the firing temperature of the oxide sintered body, the holding time at the maximum firing temperature, and the atmosphere during firing. Specifically, when the firing temperature is relatively high, microcracks may occur throughout the structure of the oxide sintered body. In this case, the residual stress in the sintered body structure is relaxed, and the microcracks tend not to progress significantly due to damage during cutting, so the difference ΔL* between the lightness Le* near the edge of the oxide sintered body and the lightness Lc* at the center of the oxide sintered body is unlikely to become large. On the other hand, when the firing temperature is relatively low, the particles in the structure of the oxide sintered body can be made strong, so that microcracks that may occur due to processing damage during cutting can be reduced throughout the structure, and the difference ΔL* between the lightness Le* near the edge of the oxide sintered body and the lightness Lc* at the center of the oxide sintered body tends to be small even after cutting. Also, when the grain size in the structure at this time is small, the structure itself becomes even stronger, microcracks due to damage during cutting hardly progress, and the difference ΔL* between the lightness Le* near the edge of the oxide sintered body and the lightness Lc* at the center of the oxide sintered body tends to be smaller. Furthermore, when the sintering temperature is moderate, there may be no cracks in the entire structure of the oxide sintered body after sintering, or if there are any, they may be very few. However, in this case, it is believed that there is residual stress in the sintered body structure generated during the sintering process, and microcracks are likely to progress due to damage during cutting, which may result in a large difference ΔL* between the lightness Le* near the target edge and the lightness Lc* at the center.

[0018] Next, a method for improving strength against damage caused by cutting by adjusting the holding time of the maximum firing temperature will be described. In an oxide sintered body, the longer the holding time of the maximum firing temperature, the more likely it is that microcracks will occur throughout the structure after firing. However, when the holding time is relatively long, even if microcracks develop due to damage caused by cutting, the difference ΔL* between the lightness Le* near the edge of the oxide sintered body and the lightness Lc* at the center of the oxide sintered body is unlikely to become large. In addition, when the holding time is relatively short, the occurrence of cracks throughout the structure can be reduced, and even when cutting is performed, the difference ΔL* between the lightness Le* near the end of the oxide sintered body and the lightness Lc* at the center of the oxide sintered body tends to be small. Furthermore, when the holding time is medium, there are no cracks in the entire structure of the oxide sintered body after sintering, or if there are any, they are very few. However, in this case, it is thought that there is residual stress in the sintered body structure generated during the sintering process, and microcracks are likely to progress due to damage during cutting, so as a result, the difference ΔL* between the lightness Le* near the target edge and the lightness Lc* at the center can become large.

[0019] Next, the sintering atmosphere for obtaining the oxide sintered body is preferably an oxygen atmosphere, which improves sinterability and tends to increase the difference in lightness ΔL* compared to sintering in an air atmosphere.

[0020] Furthermore, an oxide sintered body that has the strength to withstand processing damage during cutting can also be obtained by adjusting the density (relative density) of the sintered body structure. Generally, if the density of a sputtering target is low, it can cause nodules to form, but if the density of the oxide sintered body of an IGZO target is too high, local stress within the structure is not alleviated and cracks tend to progress, although the mechanism is not clear. On the other hand, if the density is too low, microcracks are less likely to progress, but there is a higher concern about nodule formation.

[0021] That is, in this embodiment, from the viewpoint of suppressing the generation of nodules, the relative density is 97.0% or more, and preferably 98.0% or more, whereas from the viewpoint of suppressing the growth of microcracks, the relative density is preferably 99.3% or less. The relative density is determined by the ratio of the Archimedes density to the theoretical density, which is determined by the composition.

[0022] Here, the theoretical density is a density value calculated from the theoretical density of the oxide of each of the constituent elements of the oxide sintered body of the sputtering target, excluding oxygen. The oxide sintered body is subjected to a component analysis, and the theoretical density is calculated using the oxide mass ratio (mass%) calculated by converting the atomic ratio (at%) of each of the constituent elements In, Ga, and Zn to the total of 100 at% of In, Ga, and Zn, obtained by the analysis, and the simple substance densities of In2O3, Ga2O3, and ZnO. Specifically, the simple substance density of In2O3 is set to 7.18 (g / cm 3 ), and the density of Ga2O3 is 5.95 (g / cm 3 ), and the density of ZnO is 5.61 (g / cm 3 ) and the mass ratio of In2O3 is W In2O3 (mass%), the mass ratio of Ga2O3 is W Ga2O3 (mass%), the mass ratio of ZnO is W ZnO (mass%), theoretical density (g / cm 3 )=(7.18×W In2O3 +5.95×W Ga2O3 +5.61×W ZnO ) / 100.

[0023] Note that this relative density is based on the theoretical density calculated by assuming that the sintered body of the sputtering target is a mixture of In2O3, Ga2O3, and ZnO. Since the true density of the target sintered body may be higher than the theoretical density, the relative density referred to here may exceed 100%.

[0024] The relative density of the oxide sintered body of the sputtering target of this embodiment can be controlled within the above range by adjusting the maximum firing temperature, firing holding time, firing atmosphere, and the like.

[0025] In this embodiment, the grain size of the oxide sintered body is preferably 1.5 μm or more and 15 μm or less, more preferably 3.0 μm or more and 10 μm or less. If the grain size is large, that is, if it exceeds 15 μm, there is a concern that coarse particles will be generated during sputtering. If the grain size is less than 1.5 μm, there is a concern that sintering will be insufficient and sufficient density will not be obtained.

[0026] The grain size is measured by the code method. The grain size is measured by cutting a sample for observation from the target, mirror-polishing the surface of the sample, taking a structural photograph of the mirror-polished sample surface from five fields of view at 1000 times magnification with a scanning electron microscope (SEM), drawing two straight lines on the photographed image, and measuring the arithmetic mean value of the lengths at which each line intersects with the crystal grains, and the arithmetic mean value is taken as the grain size (crystal grain size). The grain size of the oxide sintered body measured by the cord method can be controlled by adjusting the maximum sintering temperature, sintering holding time, sintering atmosphere, and the like.

[0027] Here, in this embodiment, the oxide sintered body can be a part of a sputtering target, and can be bonded to a backing plate with a bonding material as necessary, and the oxide sintered body in the sputtering target can be in the shape of a circular plate, a rectangular plate, or a cylindrical shape. The thickness of the oxide sintered body in the sputtering target can be 18 mm or less, preferably 15 mm or less. The thickness is preferably 3 mm or more, more preferably 6 mm or more. By making the thickness 3 mm or more, the usage period of the target can be extended, the downtime of the sputtering device can be reduced, and the productivity can be improved. If the thickness of the target is too thick, there is a tendency that sufficient density cannot be obtained during sintering, so the thickness is preferably 18 mm or less.

[0028] Next, a method for producing the sputtering target of this embodiment will be described. The sputtering target of this embodiment can be produced through the steps of mixing and pulverizing raw materials, a granulating step, a molding step, and a firing step. In the mixing and grinding process, indium oxide (In2O3) powder, gallium oxide (Ga2O3) powder, and zinc oxide (ZnO) powder are prepared as raw material powders. Indium oxide powder has a median diameter (D50): 0.5 to 3 μm and a specific surface area: 4 to 10 m 2 / g, and the gallium oxide powder has a median diameter (D50): 0.5 to 4 μm and a specific surface area: 6 to 30 m 2 / g, and the zinc oxide powder has a median diameter (D50): 0.1 to 2 μm and a specific surface area: 2 to 20 m 2 It is preferred to use / g.

[0029] Next, the raw material powders are weighed to obtain the desired composition ratio, and then mixed and pulverized. There are various pulverization methods depending on the desired particle size and the material to be pulverized, and wet or dry ball mills, vibration mills, bead mills, etc. can be used. To obtain uniform and fine crystal particles, the bead mill mixing method is preferred, which has high efficiency in disintegrating aggregates in a short time and also provides good dispersion of additives.

[0030] Next, in the granulation process, the finely ground slurry is granulated. This is to improve the fluidity of the powder by granulation, so that the powder can be filled evenly into a mold during the next process of press molding, and a homogeneous molded body can be obtained. There are various methods for granulation, but one method for obtaining granulated powder suitable for press molding is to use a spray drying device (spray dryer). This method makes the powder into a slurry, disperses it as droplets in hot air, and dries it instantly, and it is possible to continuously obtain spherical granulated powder of 10 to 500 μm.

[0031] When drying with a spray dryer, it is important to control the inlet and outlet temperatures of the hot air. If the temperature difference between the inlet and outlet is large, the amount of dry material per unit time increases, improving productivity. However, if the inlet temperature is too high, the powder and added binder may be altered by the heat, and the desired characteristics may not be obtained. Also, if the outlet temperature is too low, the granulated powder may not be dried sufficiently.

[0032] In addition, the strength of the molded body can be improved by adding a binder such as polyvinyl alcohol (PVA) to the slurry and incorporating it into the granulated powder. The amount of PVA added can be 50 to 250 cc / kg of an aqueous solution containing 6% by mass of PVA relative to the raw material powder. Furthermore, the crushing strength of the granulated powder during press molding can be adjusted by adding a plasticizer suitable for the binder. There is also a method of improving the strength of the molded body by adding a small amount of water to the obtained granulated powder to moisten it.

[0033] Next, in the molding process, the granulated powder is pressed by a mold or cold isostatic press (CIP) at a pressure of, for example, 1 ton / cm 2 The pressure is maintained at the above level for 1 to 3 minutes to obtain a molded body.

[0034] In the subsequent sintering step, for example, an electric furnace may be used, and in addition to atmospheric sintering, pressure sintering methods such as hot pressing, oxygen pressure, and hot isostatic pressing may also be used. However, from the viewpoints of reducing manufacturing costs, the possibility of mass production, and the ease of manufacturing large sintered bodies, it is preferable to use atmospheric sintering.

[0035] The firing atmosphere in the firing step preferably contains oxygen, and more preferably is an oxygen atmosphere. By containing oxygen, the bulk resistance of the oxide sintered body can be easily adjusted to a desired range. In the normal pressure sintering method, the molded body is usually sintered by firing in the air, and when oxygen is introduced for firing, the flow rate of oxygen is preferably 5 to 2000 L / min.

[0036] The maximum firing temperature in the firing step can be 1200 to 1500° C., and preferably 1220 to 1360° C. By setting the maximum firing temperature within this range, the difference in lightness ΔL* satisfies ΔL*<3.0, and the relative density of the oxide sintered body can be easily set within a predetermined range. The holding time at the maximum firing temperature can be 5 to 100 hours, preferably 10 to 100 hours, and more preferably 20 to 80 hours. By setting the holding time at the maximum firing temperature within this range, the difference in lightness ΔL* satisfies ΔL*<3.0, and the relative density of the oxide sintered body can be easily set within a predetermined range.

[0037] Furthermore, the heating rate during sintering is preferably 0.1 to 5°C / min, more preferably 0.3 to 3°C / min, and even more preferably 0.5 to 2°C / min, in the temperature range of 1000°C or higher. A heating rate of 5°C / min or higher in this temperature range is not preferred from the viewpoint of process stability during mass production. Also, a heating rate of 0.1°C / min or lower in this temperature range is not preferred from the viewpoint of productivity. Furthermore, the rate of temperature increase outside the above-mentioned predetermined temperature range is not particularly limited and can be any rate of temperature increase.

[0038] Furthermore, the temperature of the molded body (sintered body) after sintering can be decreased at a rate of 10°C / min or less in a temperature range of 600°C or more. By decreasing the rate of temperature decrease to 10°C / min or less, cracking of the sintered body due to thermal stress can be suppressed. The reason why the temperature range for which the rate of temperature decrease is 10°C / min or less is set to 600°C or more is that thermal stress tends to increase in sintered bodies at 600°C or more when the temperature of the sintered body is decreased. The temperature drop rate is preferably 5° C. / min or less, more preferably 3° C. / min or less, and from the viewpoint of productivity, is preferably 0.1° C. / min or more, more preferably 0.5° C. / min or more. Furthermore, the temperature decreasing rate outside the above-mentioned predetermined temperature range is not particularly limited and can be any desired temperature decreasing rate.

[0039] In the method for producing a sputtering target of this embodiment, the sintered body obtained through the above-mentioned firing process can be processed into a desired shape by a processing machine such as a surface grinder, a cylindrical grinder, or a machining machine, as necessary, to produce a sputtering target. There is no particular restriction on the shape of the sputtering target. For example, it can be disk-shaped, rectangular, cylindrical, etc. The sputtering target may be bonded to a backing plate using a bonding material as necessary.

[0040] The oxide sintered body can be cut using a cutting wheel. The wheel is preferably made of a metal material, and has a grain size of #60 to #400, more preferably #80 to #280. When the oxide sintered body has a cylindrical shape, the cutting can be performed by cutting the oxide sintered body from the outer circumferential surface at a speed of 0.1 to 10 mm / min while rotating the oxide sintered body around its axis at, for example, 5 to 200 rpm. When the oxide sintered body has a disk or rectangular shape, the cutting can be performed by cutting the oxide sintered body from the surface at a speed of 0.1 to 100 mm / min.

[0041] Although the embodiments of the present invention have been described above, the sputtering target of the present invention is not limited to the above examples and can be modified as appropriate. EXAMPLES

[0042] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.

[0043] (Preparation of sputtering targets) As raw material powders of oxide sintered bodies for the sputtering targets of Examples 1 to 31 and Comparative Examples 1 to 9, indium oxide (In2O3) powder, gallium oxide (Ga2O3) powder, and zinc oxide (ZnO) powder were prepared. In the sputtering targets of Examples 1, 3 to 7, 9, 11, 13 to 20, and 22 to 30 and Comparative Examples 1, 2, 4, 5, 8, and 9, the indium oxide powder had a median diameter (D50): 1.6 μm and a specific surface area: 4.2 m 2 / g, as gallium oxide powder, median diameter (D50): 1.7 μm, specific surface area: 11.7 m 2 / g, as zinc oxide powder, median diameter (D50): 0.6 μm, specific surface area: 3.9 m 2 / g was used. In the sputtering targets of Examples 2, 8, 10, 12, 21, and 31 and Comparative Examples 3, 6, and 7, the indium oxide powder had a median diameter (D50): 1.4 μm and a specific surface area: 5.0 m 2 / g, as gallium oxide powder, median diameter (D50): 1.7 μm, specific surface area: 11.7 m 2 / g, as zinc oxide powder, median diameter (D50): 0.6 μm, specific surface area: 3.9 m 2 In Examples 2, 8, 10, 12, 21, and 31 and Comparative Examples 3, 6, and 7, tin oxide (SnO2) powder was also used as a raw material in the amount shown in Table 1 (Table 1 shows the content of tin atoms). The tin oxide powder had a median diameter (D50): 1.5 μm and a specific surface area: 5.7 m 2 / g was used.

[0044] Next, each raw material powder was weighed to have the composition ratio (atomic ratio) shown in Table 1, and then wet mixed and pulverized in a bead mill. Note that the particle size of each raw material powder in the slurry after pulverization was 0.6 μm. Next, the pulverized slurry was granulated. In the granulation, the powder was made into a slurry, dispersed as droplets in hot air using a spray dryer, and instantly dried to continuously obtain 49 μm spherical granulated powder.

[0045] Next, for Examples 5, 11 to 14, 16 to 21, 23, 25 to 31, and Comparative Examples 3 to 7, the granulated powder was filled into a mold and compressed under a pressure of 1800 kgf / cm 2The pressure was maintained for 1 minute to obtain a disk-shaped molded body having a diameter of 130 mm and a thickness of 21 mm. In addition, in Examples 3, 15, and 24 and Comparative Examples 1, 2, and 9, the granulated powder was filled into a mold and a pressure of 1800 kgf / cm was applied. 2 The pressure was maintained for 1 minute to obtain a cylindrical molded body having an axial length of 1600 mm, an outer diameter of 197 mm, and an inner diameter of 157 mm. In addition, for Examples 1, 2, 4, 6 to 10, and 22 and Comparative Example 8, the granulated powder was filled into a mold and cold pressed, and then the pressure was increased to 1800 kgf / cm. 2 The pressure was maintained for 1 minute to form a rectangular molded body having a width of 550 mm, a length of 595 mm, and a thickness of 16 mm. These molded bodies were then fired in an electric furnace under the atmosphere of Table 1 to obtain oxide sintered bodies. Specifically, the molded bodies were heated under the conditions shown in Table 1, and then fired at the sintering temperature and time shown in Table 1. The heating rate from 1000°C to the maximum temperature was 1°C / min, and after the maximum temperature was maintained, the temperature was lowered to 600°C at a rate of 1.5°C / min.

[0046] Next, for Examples 5, 11 to 14, 16 to 21, 23, 25 to 31 and Comparative Examples 3 to 7, the obtained oxide sintered bodies were processed into disks having a diameter of 100 mm and a thickness of 15 mm. The oxide sintered bodies were cut by applying a metal #140 cutting wheel grindstone to the surface of the oxide sintered bodies at a speed of 50 mm / min. In addition, for Examples 3, 15, and 24 and Comparative Examples 1, 2, and 9, the obtained oxide sintered bodies were processed into a cylindrical shape with an axial length of 50 mm, an outer diameter of 153 mm, and an inner diameter of 135 mm. The oxide sintered bodies were cut by applying a metal #140 cutting wheel grindstone to the surface of the oxide sintered body at a speed of 1 mm / min while rotating the oxide sintered body in the axial direction at 20 rpm. In addition, for Examples 1, 2, 4, 6 to 10, and 22 and Comparative Example 8, the obtained oxide sintered bodies were processed into a rectangular shape with a width of 450 mm, a length of 450 mm, and a thickness of 10 mm. The oxide sintered bodies were cut by applying a metal #140 cutting wheel grindstone to the surface of the oxide sintered bodies at a speed of 50 mm / min. The oxide sintered body processed as described above was subjected to surface finishing with an abrasive having a grain size shown in Table 1. The oxide sintered body subjected to surface finishing was subjected to the evaluation described below.

[0047] The firing of each molded body was carried out in a furnace with a volume of 2.2 m 3 (in Table 1, it is referred to as "furnace (large)"), with a furnace volume of 0.06 m 3 An electric furnace (referred to as "small furnace" in Table 1) was used.

[0048] [Table 1]

[0049] The obtained oxide sintered body was evaluated as follows. The evaluation results are shown in Table 2. (1) Density and relative density of oxide sintered bodies In accordance with JIS R 1634, the bulk density was calculated from the volume and dry weight of the sintered body calculated by the Archimedes method using the following formula, and the bulk density was divided by the theoretical density to obtain the relative density. Volume of sintered body = (weight of sintered body containing water - weight of sintered body in water) / density of water The theoretical density of the sintered body is the mass ratio W of In2O3 calculated from the atomic ratio (at%) of each of the constituent elements In, Ga, and Zn to 100 at%. In2O3 (mass%), mass ratio of Ga2O3 W Ga2O3 (mass%), mass ratio of ZnO W ZnO (mass%), and the density of In2O3 is 7.18 (g / cm 3 ), and the density of Ga2O3 is 5.95 (g / cm 3 ), and the density of ZnO is 5.61 (g / cm 3 ) was used to calculate the following formula: Theoretical density (g / cm 3 )=(7.18×W In2O3 +5.95×W Ga2O3 +5.61×W ZnO ) / 100

[0050] (2) Grain size of oxide sintered body measured by cord method The grain size of the oxide sintered body measured by the code method was obtained by cutting out an observation sample from the oxide sintered body after surface finishing with an abrasive having the grain size shown in Table 1, and mirror-polishing the surface of the cut sample. Photographs of the grain size of the mirror-polished sample surface were taken in five fields of view at 1000x magnification using a scanning electron microscope (SEM), and the crystal grain size (grain size of the grain) of the multiple fields of view (five fields) was calculated as the arithmetic average value using the code method evaluation method. In the code method, two straight lines of arbitrary length were drawn on each surface grain photograph, the length of the lines was divided by the number of grains that the lines crossed, and this value was converted by applying it to the scale of the surface grain photograph, and the arithmetic average grain size was calculated based on the value obtained from a total of 10 straight lines.

[0051] (3) Lightness Le* and Lc* The lightness Le* and Lc* of the oxide sintered bodies that had been surface-finished with the abrasives having the grain sizes shown in Table 1 were measured using a simplified spectrophotometer (NF333, manufactured by Nippon Denshoku Industries Co., Ltd.).

[0052] [Table 2]

[0053] As shown in Table 2, the lightness Le*, lightness Lc*, lightness difference ΔL*, and relative density of the oxide sintered body could be adjusted to the desired range by sintering the raw material molded body to obtain the oxide sintered body under a high oxygen partial pressure, adjusting the sintering temperature, sintering time, sintering atmosphere, and temperature increase / decrease rate, annealing treatment after sintering, fine-tuning the composition, etc. Furthermore, in Examples 1 to 31, in which the lightness difference ΔL* and relative density of the oxide sintered body are set within a predetermined range, it is possible to provide an IGZO sputtering target with improved uniformity in at least one property selected from the number of microcracks in the structure, the number of voids in the sintered body structure, and surface roughness, and it is presumed that this will enable the production of a high-quality IGZO film. [Industrial Applicability]

[0054] According to the present invention, it is possible to provide an IGZO sputtering target that is capable of improving the uniformity of at least one property selected from the number of microcracks in the structure, the number of voids in the sintered compact structure, and surface roughness.

Claims

1. A sputtering target having an oxide sintered body composed of indium (In), gallium (Ga), zinc (Zn) and inevitable impurities and cut after sintering, In the surface of the oxide sintered body, ΔL* obtained by subtracting the lightness Lc* at the center of the surface from the lightness Le* at a position 10 mm from the end of the surface toward the center satisfies ΔL*<3.0, The relative density of the oxide sintered body is 97.0% or more, The IGZO sputtering target, wherein the surface of the oxide sintered body is flat.

2. The IGZO sputtering target according to claim 1, wherein the grain size of the oxide sintered body is 1.5 to 15 μm.

3. The IGZO sputtering target according to claim 1 or 2, wherein the oxide sintered body has a relative density of 99.3% or less.

4. The IGZO sputtering target according to any one of claims 1 to 3, wherein the oxide sintered body has a circular plate shape or a rectangular plate shape.

5. The IGZO sputtering target according to any one of claims 1 to 4, wherein when the In content in the oxide sintered body is 100, Ga is 100 ± 30 and Zn is 100 ± 30 in atomic ratio.

6. The IGZO sputtering target according to any one of claims 1 to 5, wherein the oxide sintered body has a thickness of 15 mm or less.

Citation Information

Patent Citations

  • Cylindrical ceramic-based sputtering target material and cylindrical ceramic-based sputtering target configured by joining one or more cylindrical ceramic-based sputtering target materials to backing tube

    WO2017131111A1