Polishing composition, polishing method, and method for producing substrate
The polishing composition with modified silica abrasive grains and controlled pH enhances the polishing speed and uniformity of resin-containing substrates, addressing the need for high-speed polishing of semiconductor substrates with patterned structures.
Patent Information
- Application Number
- JP2021509462
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-27
- Filing Date
- 2020-03-24
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2040-03-24
AI Technical Summary
There is a lack of effective polishing compositions capable of polishing resin-containing substrates at high speed, particularly for semiconductor substrates with patterned structures.
A polishing composition comprising silica abrasive grains modified with specific metal cations, a pH adjuster, and a dispersion medium, optimized to operate within a pH range of 2 to 7, which enhances the polishing rate of resin materials while maintaining stability and reducing metal corrosion.
The composition significantly increases the polishing rate of resin materials, reduces the step difference between resin and metal removal rates, and improves surface flatness by minimizing scratches and corrosion, suitable for substrates with patterned resin and metal structures.
Smart Images

Figure 0007576023000003 
Figure 0007576023000004 
Figure 0007576023000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a polishing composition, a polishing method using the polishing composition, and a method for producing a substrate. [Background technology]
[0002] In the semiconductor industry, planarization techniques are usually used to increase the flatness of the surface of a semiconductor substrate (e.g., a wafer). Chemical mechanical polishing (CMP) is one of the commonly used planarization techniques. Chemical mechanical polishing is a method of planarizing the surface of an object to be polished (a polished object) such as a semiconductor substrate by using a polishing composition containing abrasive grains such as silica, alumina, or ceria, an anticorrosive agent, a surfactant, and the like.
[0003] Furthermore, substrates containing resin materials (sometimes abbreviated as "resin-containing substrates" in this specification) are becoming more widespread. Therefore, the need for polishing compositions applicable to polishing resin-containing substrates is gradually increasing.
[0004] Patent Document 1 discloses a chemical mechanical polishing composition containing alumina, a complexing agent, and an oxidizing agent. The chemical mechanical polishing composition of Patent Document 1 is applicable to chemical mechanical polishing of a resin layer and a conductor layer. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Taiwan Patent Application Publication No. 200535218 A1 Summary of the Invention [Problem to be solved by the invention]
[0006] However, there has been no polishing composition capable of polishing a resin-containing substrate at high speed. Therefore, an object of the present invention is to provide a polishing composition capable of polishing a resin-containing substrate at high speed. [Means for solving the problem]
[0007] In order to achieve the above-mentioned object, some embodiments of the present invention disclose a polishing composition having a pH of more than 2 and not more than 7, the polishing composition comprising an abrasive grain containing silica, in which at least a portion of the hydrogen atoms constituting silanol groups located on the surface of the silica have been substituted with cations of a metal atom M that is at least one selected from the group consisting of aluminum, chromium, titanium, zirconium, iron, zinc, tin, scandium and gallium, a pH adjuster, and a dispersion medium.
[0008] Furthermore, some other embodiments of the present invention disclose a polishing method comprising a step of polishing an object to be polished using the above-mentioned polishing composition, wherein the surface of the object to be polished comprises a patterned structure, and the patterned structure comprises a resin material.
[0009] Some further embodiments of the present invention disclose a method for manufacturing a substrate, the method including the steps of: preparing a substrate, the surface of which includes a pattern structure and the pattern structure includes a resin material; and polishing the substrate using the polishing composition described above. Effect of the Invention
[0010] According to the present invention, it is possible to provide a polishing composition capable of polishing a resin-containing substrate at high speed. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is an illustration of the surface modification step of the abrasive grains according to some embodiments of the present invention. [Diagram 2] FIG. 2 is a schematic diagram of the surface of an unmodified silica abrasive grain. [Diagram 3] FIG. 2 is a schematic diagram of the surface of a silica abrasive grain showing that some silicon atoms have been replaced with aluminum atoms. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] In order to make the above and other objects, features and advantages of the present invention more clear and understandable, preferred embodiments are given below and described in detail.
[0013] The following describes embodiments of the present invention, but the present invention is not limited to these embodiments.
[0014] One embodiment of the present invention is a polishing composition having a pH greater than 2 and not greater than 7, the polishing composition comprising an abrasive grain containing silica, in which at least a portion of the hydrogen atoms constituting silanol groups located on the surface of the silica have been substituted with cations of a metal atom M that is at least one selected from the group consisting of aluminum, chromium, titanium, zirconium, iron, zinc, tin, scandium and gallium, a pH adjuster, and a dispersion medium.
[0015] In this embodiment, the polishing composition contains colloidal silica as an abrasive, the surface of which is modified with a specific metal cation, but not the inside. When a polishing object including a patterned structure formed of a material containing a resin is polished using the polishing composition of this embodiment, the removal rate of the resin material (also referred to as the polishing rate in this specification) can be significantly increased.
[0016] However, the polishing object to which the polishing composition of the present invention is applied is not particularly limited, and it can be applied to any general semiconductor substrate. Examples of the polishing object include silicon-containing substrates such as amorphous silicon, crystalline silicon, silicon oxide, and silicon nitride. The polishing composition of the present invention is particularly suitable for polishing a substrate including a patterned structure formed from a material containing a resin, and the technical effect of the present invention is fully exhibited when polishing such a substrate.
[0017] Specific examples of resin materials include polyethylene terephthalate (PET) (melting point: 260°C), polybenzoxazole (PBO) (melting point: 200°C or higher), polybutylene terephthalate (PBT) (melting point: 223°C), polyimide (PI) (melting point: 200°C or higher), polyamide (PA) (melting point: 187°C), epoxy resin (melting point: 200°C or higher), urethane acrylate resin (melting point: 200°C or higher), unsaturated polyester resin (melting point: 200°C or higher), phenol resin (melting point: 200°C or higher), polynorbornene resin, polyacetal (POM) (melting point: 175°C), polycarbonate (PC) (melting point: 120°C), and the like. ℃), modified polyphenylene ether (m-PPE) (melting point: 300 ° C or more), ultra-high molecular weight polyethylene (UHMWPE) (melting point: 136 ° C), syndiotactic polystyrene (SPS) (melting point: 270 ° C), amorphous polyarylate (PAR) (melting point: 250 ° C), polysulfone (PSF) (melting point: 185 ° C), polyethersulfone (PES), polyphenylene sulfide (PPS) (melting point: 288 ° C), polyetheretherketone (PEEK) (melting point: 343 ° C), polyetherimide (PEI) (melting point: 217 ° C), fluororesin (melting point: about 200 ° C or more), liquid crystal polymer (LCP) can be mentioned. Among them, those with a relatively high melting point are preferable, and resins with a melting point of 200 ° C or more are preferable. The upper limit of the melting point of such resins is preferably 300 ° C or less.
[0018] Therefore, polyethylene terephthalate (PET) (melting point: 260°C), polybenzoxazole (PBO) (melting point: 200°C or higher), polybutylene terephthalate (PBT) (melting point: 223°C), polyimide (PI) (melting point: 200°C or higher), epoxy resin (melting point: 200°C or higher), urethane acrylate resin (melting point: 200°C or higher), unsaturated polyester resin (melting point: 200°C or higher), phenolic resin (melting point: 200°C or higher), modified polyphenylene ether (m-PP E) (melting point: 300°C or higher), syndiotactic polystyrene (SPS) (melting point: 270°C), amorphous polyarylate (PAR) (melting point: 250°C), polyphenylene sulfide (PPS) (melting point: 288°C), polyether ether ketone (PEEK) (melting point: 343°C), polyetherimide (PEI) (melting point: 217°C), and fluororesin (melting point: about 200°C or higher) are more preferred, and polyimide (PI), epoxy resin, and urethane acrylate resin are particularly preferred. The melting point is measured in accordance with JIS K 0064:1992, Method for Measuring Melting Point and Melting Range of Chemical Products. The mechanism by which the melting point is 200°C or higher can efficiently achieve the desired effect of the present invention is not clear. Therefore, according to one embodiment of the present invention, the melting point of the resin is 200°C or higher. The above resin materials can be used alone or in combination of two or more types. According to one embodiment of the present invention, the resin contains nitrogen atoms. By including a nitrogen atom, the desired effect of the present invention can be efficiently achieved. According to one embodiment of the present invention, the repeating unit constituting the resin includes a nitrogen atom. By adopting such an embodiment, the desired effect of the present invention can be efficiently achieved.
[0019] As described above, the polishing composition according to the embodiment of the present invention is used to polish an object to be polished that contains a resin. In addition, according to the embodiment of the present invention, the application (use) of the polishing composition containing specific abrasive grains to polish a resin material is provided.
[0020] According to one embodiment of the present invention, the object to be polished includes a metal material. Here, according to a general polishing composition, the removal rate of the metal material is higher than the removal rate of the resin material. In other words, when a patterned structure including a resin material and a metal material is polished, the removal rate of the metal material is different from the removal rate of the resin material, so that a step difference is likely to occur. According to the polishing composition of the present invention, a resin material, which generally has a low polishing rate, can be polished at a high speed. Then, in the chemical mechanical polishing process, the removal rate of the metal material and the removal rate of the resin material can be made the same (i.e., the removal rate of the resin material relative to the removal rate of the metal material is made 1.0) or can be made close to each other (i.e., the removal rate of the resin material relative to the removal rate of the metal material is made close to 1.0). Therefore, the occurrence of a step can be avoided or suppressed. According to one embodiment of the present invention, at least one of a metal polishing accelerator, a metal corrosion inhibitor, and an oxidizing agent may be contained in the polishing composition in order to make the removal rate of the resin material relative to the removal rate of the metal material closer to 1.0, or for another purpose. The metal polishing accelerator, the metal corrosion inhibitor, and the oxidizing agent will be described later.
[0021] Specific examples of the metal material include transition metals (particularly those in Group 11) and metals in Group 13, such as copper, aluminum, cobalt, and tungsten. The above metal materials can be used alone or in combination of two or more kinds.
[0022] Hereinafter, various components contained in the polishing composition according to this embodiment will be described.
[0023] [Abrasive grain] The polishing composition of the present embodiment contains silica as an abrasive. In some embodiments, the abrasive is colloidal silica. The abrasive in the present embodiment is surface-modified with a specific metal cation. More specifically, the abrasive contains colloidal silica, and at least a part of the hydrogen atoms constituting the silanol groups located on the silica surface is substituted with a cation of a metal atom M, and the metal atom M is at least one selected from the group consisting of aluminum, chromium, titanium, zirconium, iron, zinc, tin, scandium, and gallium.
[0024] Since the zeta potential of general colloidal silica is close to zero under acidic conditions, electrostatic repulsion does not occur between colloidal silica particles under acidic conditions, and aggregation is likely to occur. In this embodiment, the colloidal silica particles are surface-modified so that the colloidal silica particles have a relatively large positive zeta potential (for example, greater than 40 mV; upper limit is about 100 mV) under acidic conditions. This allows the abrasive grains to strongly repel each other under acidic or neutral conditions and disperse well. As a result, the storage stability of the polishing composition is improved. The surface-modified silica of the present invention can be produced by the method disclosed in JP-B-47-26959. Alternatively, the surface-modified silica of the present invention can be produced by the method described in the Examples.
[0025] In one embodiment of the present invention, the zeta potential of the abrasive grains in the polishing composition is preferably 20 mV or more, more preferably 25 mV or more, and preferably 30 mV or more. In one embodiment of the present invention, the zeta potential of the abrasive grains in the polishing composition may be 80 mV or less, 70 mV or less, 60 mV or less, 50 mV or less, or 40 mV or less.
[0026] The step of surface modification of the abrasive grains may mainly include a step of mixing a salt compound of a metal atom M, such as aluminum, chromium, titanium, zirconium, iron, zinc, tin, scandium, or gallium, with colloidal silica particles, and a step of substituting at least a part of the hydrogen atoms constituting the silanol groups located on the surface of the colloidal silica with the cation of the metal atom M. Examples of the salt compound of the metal atom M include halides, hydroxides, sulfates, and nitrates of the metal atom M. Specific examples of the salt compound of the metal atom M include aluminum chloride, aluminum bromide, aluminum iodide, aluminum hydroxide, aluminum sulfate, aluminum nitrate, chromium chloride, chromium bromide, chromium iodide, chromium hydroxide, chromium sulfate, chromium nitrate, titanium chloride, titanium bromide, titanium iodide, titanium hydroxide, titanium sulfate, titanium nitrate, zirconium chloride, zirconium bromide, zirconium iodide, zirconium hydroxide, zirconium sulfate, zirconium nitrate, and zirconium chloride. Examples of the metal atom M include arsenic, iron chloride, iron bromide, iron iodide, iron hydroxide, iron sulfate, iron nitrate, zinc chloride, zinc bromide, zinc iodide, zinc hydroxide, zinc sulfate, zinc nitrate, tin chloride, tin bromide, tin iodide, tin hydroxide, tin sulfate, tin nitrate, scandium chloride, scandium bromide, scandium iodide, scandium hydroxide, scandium sulfate, scandium nitrate, gallium chloride, gallium bromide, gallium iodide, gallium hydroxide, gallium sulfate, and gallium nitrate. The above salt compounds of the metal atom M can be used alone or in combination of two or more.
[0027] In one embodiment of the present invention, in order to perform surface modification of the abrasive grains, 1 m of the abrasive grains is added to a dispersion liquid in which the abrasive grains are dispersed. 2 To the total amount of the salt compound of the metal atom M, 0.0001 to 0.0010 g is preferably added, 0.0002 to 0.0008 g is more preferably added, and 0.0003 to 0.0006 g is further preferably added.
[0028] The present inventors speculate as follows about the mechanism of surface modification of abrasive grains with specific metal cations in this embodiment. Note that the mechanism described below is based on speculation, and whether this mechanism is accurate or not does not affect the technical content and claims of the present invention. In this specification, the mechanism of surface modification will be explained using the example of modifying colloidal silica with aluminum ions.
[0029] FIG. 1 is an explanatory diagram of the steps of surface modification of abrasive grains according to some embodiments of the present invention. Please refer to FIG. 1. The surface state of colloidal silica particles 102 dissolved (dispersed) in water is shown in the upper left square of FIG. 1. The main body of the colloidal silica particles 102 is a tetrahedral network structure composed of silica. One end of the oxygen atoms located on the surface of the colloidal silica particles is bonded to a silicon atom, and the other end is bonded to a hydrogen atom to form a silanol group. After modifying the colloidal silica particles 102 with an aluminum chloride modifier 104, modified colloidal silica particles 112 are formed. The surface state of the modified colloidal silica particles 112 is as shown in the upper right square of FIG. 1. The main body of the modified colloidal silica particles 112 is also a tetrahedral network structure composed of silica, but some of the hydrogen atoms in the silanol groups located on the surface of the colloidal silica particles are replaced with aluminum ions. As shown in FIG. 1, each aluminum ion is bonded to two oxygen atoms on the surface of the modified colloidal silica particles 112. Therefore, the surface of the modified colloidal silica particle 112 is positively charged, and the negatively charged chloride ions serve as counter ions.
[0030] In some embodiments, all hydrogen atoms in the silanol groups located on the surface of the colloidal silica particles are replaced with aluminum ions. In such embodiments, the dispersibility of the colloidal silica particles is improved. In other embodiments, only a portion of the hydrogen atoms in the silanol groups located on the surface of the colloidal silica particles are replaced with aluminum ions.
[0031] When colloidal silica particles are surface-modified using other metal ions with different valences, the number of oxygen atoms bonded to the metal atom M (or the cation of the metal atom M) may also change. In some embodiments, as shown in FIG. 1, the number of oxygen atoms bonded to the metal atom M is two. In other embodiments, the number of oxygen atoms bonded to the metal atom M is one. In still other embodiments, the number of oxygen atoms bonded to the metal atom M is three. In other words, one metal atom M is bonded to one oxygen atom of one silanol group; one metal atom M is bonded to two oxygen atoms of two silanol groups; or one metal atom M is bonded to three oxygen atoms of three silanol groups. For reference, FIG. 2 shows a schematic diagram of the surface of an unmodified silica abrasive grain. In this way, the surface of the unmodified silica abrasive grain is covered only with silanol groups. In addition, the abrasive grain that should be recognized as being structurally distinct from the specific abrasive grain of the present invention is the abrasive grain shown in FIG. 3. Fig. 3 is a schematic diagram of the surface of a silica abrasive grain showing that some silicon atoms have been replaced with aluminum atoms. In the abrasive grain of the present invention, at least some of the hydrogen atoms constituting the silanol groups located on the silica surface have been replaced with aluminum or the like. In contrast, in the abrasive grain of Fig. 3, the silicon atoms located inside the silica have been replaced with aluminum atoms.
[0032] The abrasive grains of the present invention may be synthetic products or commercially available products, such as Ludox (registered trademark) CL (Sigma-Aldrich; aluminum ion-modified colloidal silica, counter ion is chlorine).
[0033] When the total amount of the polishing composition is 100% by weight, the content of the abrasive grains in the polishing composition is preferably 0.1% by weight or more, more preferably 0.5% by weight or more, and even more preferably 1% by weight or more. When the content of the abrasive grains is the above-mentioned lower limit, the polishing rate for the polishing object containing a resin material or a metal material is generally increased. On the other hand, according to an embodiment of the present invention, the content of the abrasive grains in the polishing composition is more than 1% by weight (or 1.5% by weight or more). In this way, by using abrasive grains that have been surface-modified with a specific metal cation and the content of the abrasive grains is more than 1% by weight (or 1.5% by weight or more), the polishing rate of the metal can be increased without excessively increasing the polishing rate of the resin. Therefore, the removal rate of the resin material relative to the removal rate of the metal material becomes closer to 1.0.
[0034] When the total amount of the polishing composition is 100% by weight, the content of the abrasive grains in the polishing composition is preferably 10% by weight or less, more preferably 8% by weight or less, even more preferably 5% by weight or less, and particularly preferably 3% by weight or less. When the content of the abrasive grains is the above upper limit, when the polishing composition is used to polish an object to be polished, a polished surface with fewer scratches can be easily obtained, and agglomeration of the abrasive grains is less likely to occur.
[0035] According to one embodiment of the present invention, the content of the abrasive grains is 0.1 to 10% by weight based on the total weight of the polishing composition. This embodiment increases the polishing speed for a polishing object containing a resin material or a metal material, and easily obtains a polished surface with fewer scratches, while also making it difficult for abrasive grains to aggregate.
[0036] The average primary particle size of the abrasive grains is preferably more than 30 nm, more preferably 40 nm or more, and particularly preferably 50 nm or more. As the average primary particle size of the abrasive grains increases, the polishing speed for the polishing object containing resin or metal material increases. The specific surface area of the abrasive grains can be measured by the BET method, and the value of the average primary particle size of the abrasive grains can be calculated based on the measured specific surface area. The average primary particle size of the abrasive grains is preferably 150 nm or less, more preferably 130 nm or less, even more preferably 110 nm or less, even more preferably 90 nm or less, and most preferably 70 nm or less. As the average primary particle size of the abrasive grains decreases, a polished surface with fewer scratches can be easily obtained when polishing an object to be polished using the polishing composition.
[0037] Therefore, according to one embodiment of the present invention, the primary particle size of the abrasive grains is 40 to 150 nm. This embodiment makes it possible to increase the polishing speed for a polishing target containing a resin or metal material, and to easily obtain a polished surface with fewer scratches.
[0038] The average secondary particle size of the abrasive grains is preferably 60 nm or more, more preferably 80 nm or more, even more preferably 100 nm or more, and even more preferably 110 nm or more. As the average secondary particle size of the abrasive grains increases, the polishing speed for polishing objects including resin or metal materials increases.
[0039] The average secondary particle diameter of the abrasive grains is preferably 300nm or less, more preferably 250nm or less, even more preferably 200nm or less, even more preferably 150nm or less, and particularly preferably 135nm or less. As the average secondary particle diameter of the abrasive grains becomes smaller, when the polishing composition is used to polish an object to be polished, it becomes easier to obtain a polished surface with fewer scratches. The value of the average secondary particle diameter of the abrasive grains can be measured by a suitable method, for example, a laser light scattering method.
[0040] [pH adjuster] The polishing composition of this embodiment may contain a pH adjuster. From another perspective, a pH adjuster used for adjusting the pH value of the polishing composition to a range of more than 2 and not more than 7 may be included. The pH adjuster can adjust the pH value of the polishing composition to a range of more than 2 and not more than 7. Examples of pH adjusters include known acids and bases. When the pH of the polishing composition is 2.0 or less, or exceeds 7.0, the polishing rate of the resin material is significantly reduced (Comparison between Example 2 and Comparative Example 1, Comparison between Example 13 and Comparative Example 2). In other words, the present invention is also characterized in that it was created by finding the critical points related to the polishing rate of the resin material at pH 2.0 and 7.0.
[0041] The acid used as the pH adjuster in the polishing composition of this embodiment may be an inorganic acid or an organic acid, or may be a chelating agent.Specific examples of inorganic acids that can be used as pH adjusters include hydrochloric acid (HCl), sulfuric acid (H2SO4), nitric acid (HNO3), hydrofluoric acid (HF), boric acid (H3BO3), carbonic acid (H2CO3), hypophosphorous acid (H3PO2), phosphorous acid (H3PO3) and phosphoric acid (H3PO4).Preferred among these inorganic acids are hydrochloric acid, sulfuric acid, nitric acid and phosphoric acid.
[0042] Specific examples of organic acids that can be used as pH adjusters include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylpentanoic acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, hydroxyacetic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, lactic acid, glyoxylic acid, and the like. Examples of suitable organic acids include 2-furan carboxylic acid, 2,5-furandicarboxylic acid, 3-furan carboxylic acid, 2-tetrahydrofuran carboxylic acid, methoxyacetic acid, methoxyphenylacetic acid, and phenoxyacetic acid. Organic sulfuric acids such as methanesulfonic acid, ethanesulfonic acid, and isethionic acid (2-hydroxyethanesulfonic acid) may also be used. Among these organic acids, preferred are dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, and tartaric acid, and tricarboxylic acids such as citric acid.
[0043] In one embodiment of the present invention, the acid used as the pH adjuster in the polishing composition is different from the metal polishing accelerator. In one embodiment of the present invention, the acid used as the pH adjuster in the polishing composition does not contain an amino acid.
[0044] Examples of the base used as a pH adjuster in the polishing composition of this embodiment include hydroxides or salts of alkali metals, hydroxides or salts of Group 2 elements, quaternary ammonium hydroxides or salts thereof, ammonia, amines, etc. Specific examples of alkali metals include potassium, sodium, etc.
[0045] If the polishing composition is alkaline (i.e., pH is greater than 7), the zeta potential of the abrasive grain surface is shifted in the negative direction, weakening the repulsion with the resin material, which causes a decrease in the polishing rate of the resin material. The pH value of the polishing composition of this embodiment is acidic or neutral, so that the polishing rate of the resin material can be effectively improved. More specifically, the upper limit of the pH value of the polishing composition of this embodiment is preferably less than 7, more preferably 6.5 or less, and even more preferably 6.2 or less, and may be less than 6, 5 or less, or less than 5. If the pH value of the polishing composition is too low, it becomes difficult to effectively increase the removal rate of the resin material. In addition, if the pH value of the polishing composition is too low, the burden of waste liquid treatment increases. The lower limit of the pH value of the polishing composition of this embodiment is preferably greater than 2, preferably 3 or more, more preferably greater than 3, more preferably 4 or more, even more preferably greater than 4, even more preferably more than 5, even more preferably 5.5 or more, and even more preferably 5.8 or more. Since the pH value of the polishing composition of the present invention is acidic or neutral, it can inhibit the corrosion of metal materials, and thus improve the surface flatness and quality of metal structures.
[0046] In one embodiment of the present invention, from the viewpoint of eliminating the step, it is preferably 6.5 or less, more preferably 6.2 or less, even more preferably less than 6, even more preferably 5 or less, and even more preferably less than 5. In one embodiment of the present invention, from the viewpoint of eliminating the step, it is preferably greater than 2 and preferably 3 or more, more preferably greater than 3, even more preferably 4 or more, and even more preferably greater than 4.
[0047] [Dispersion medium] The polishing composition of this embodiment contains a dispersion medium (which may also be referred to as a "solvent"). The dispersion medium can be used to disperse or dissolve each component in the polishing composition. In this embodiment, the polishing composition may contain water as a dispersion medium. From the viewpoint of suppressing inhibition of the action of other components, water that contains as few impurities as possible is preferred. More specifically, pure water or ultrapure water from which impurity ions have been removed with an ion exchange resin and foreign matter has been removed through a filter, or distilled water is preferred.
[0048] [Oxidizing agent] The polishing composition used in the polishing method of the present invention may further contain an oxidizing agent, if necessary. There is no particular restriction on the type of oxidizing agent contained in the polishing composition, but it is preferable that the oxidizing agent has a standard electrode potential of 0.5V or more. Compared with the use of an oxidizing agent having a standard electrode potential of less than 0.5V, the use of an oxidizing agent having a standard electrode potential of 0.5V or more is useful for further increasing the polishing speed of the metal material part using the polishing composition. This can shorten the time required for the polishing process, and improve the efficiency of the polishing process. Specific examples of oxidizing agents having a standard electrode potential of 0.5 V or more include, for example, hydrogen peroxide (1.7 V), sodium peroxide, barium peroxide, organic oxidizing agents, ozone water, salts of silver (II), salts of iron (III), and permanganic acid, chromic acid, dichromic acid, peroxophosphoric acid, perboric acid, performic acid, peracetic acid, perbenzoic acid, perphthalic acid, hypochlorous acid, hypobromous acid, hypoiodous acid, chloric acid, chlorous acid, perchloric acid, bromic acid, iodic acid, and periodic acid. Examples of oxidizing agents include isocyanuric acid (1.6V), persulfuric acid (2.0V), dichloroisocyanuric acid, trichloroisocyanuric acid, and salts thereof. These oxidizing agents may be used alone or in combination of two or more.
[0049] Among the above-mentioned oxidizing agents, from the viewpoint of effectively increasing the polishing rate of metal parts using the polishing composition, hydrogen peroxide, periodic acid or a salt thereof, persulfuric acid or a salt thereof, dichloroisocyanuric acid or a salt thereof, and trichloroisocyanuric acid or a salt thereof are preferred, and at least one selected from the group consisting of hydrogen peroxide, periodic acid or a salt thereof, and persulfuric acid and a salt thereof is particularly preferred.
[0050] The standard electrode potential refers to the electrode potential when all chemical species involved in the oxidation reaction are in a standard state, and is expressed by the following formula 1.
[0051]
number
[0052] In formula 1, E0 is the standard electrode potential, ΔG0 is the standard Gibbs energy change of the oxidation reaction, K is the equilibrium constant, F is the Faraday constant, T is the absolute temperature, and n is the number of electrons involved in the oxidation reaction. As can be seen from formula 1, the standard electrode potential varies with temperature, so in this specification, the standard electrode potential at 25°C is used. The standard electrode potential of an aqueous solution system is described, for example, in Revised 4th Edition Chemistry Handbook (Basics) II, pp. 464-468 (edited by the Chemical Society of Japan).
[0053] When the polishing composition of the present embodiment contains an oxidizing agent, the content of the oxidizing agent is preferably 0.001% by weight or more, and more preferably 0.01% by weight or more, based on the total amount of the polishing composition being 100% by weight. End When the content of the oxidizing agent is within the above lower limit, the polishing rate of the metal material portion by the polishing composition can be further increased.
[0054] When the polishing composition of the present embodiment contains an oxidizing agent, the content of the oxidizing agent is preferably 10% by weight or less, more preferably 5% by weight or less, even more preferably 1% by weight or less, and even more preferably 0.5% by weight or less, when the total amount of the polishing composition is 100% by weight. When the content of the oxidizing agent is the upper limit described above, excessive oxidation of the surface of the object to be polished by the polishing composition is unlikely to occur, and a polished surface with less surface roughness can be obtained, and the burden of processing the polishing composition after polishing (i.e., the burden of waste liquid processing) can also be reduced.
[0055] [Metal polishing accelerator] The polishing composition of the present embodiment may further contain a metal polishing accelerator as necessary.When the metal polishing accelerator is added to the polishing composition, the etching effect of the metal polishing accelerator can further increase the polishing speed of the metal material part by the polishing composition, which is advantageous.This can shorten the time required for the polishing process, and thus improve the efficiency of the polishing process.
[0056] Examples of the metal polishing accelerator that can be used include inorganic acids, organic acids, amino acids, nitrile compounds, and chelating agents.
[0057] Specific examples of inorganic acids include sulfuric acid, nitric acid, boric acid, and carbonic acid. Specific examples of organic acids include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylpentanoic acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, and lactic acid. Organic acids such as methanesulfonic acid, ethanesulfonic acid, and isethionic acid can also be used. Instead of or in combination with inorganic or organic acids, salts of inorganic or organic acids, such as alkali metal salts, may be used.
[0058] Specific examples of amino acids include glycine, α-alanine, β-alanine, N-methylglycine, N,N-dimethylglycine, 2-aminobutyric acid, norvaline, valine, leucine, norleucine, isoleucine, phenylalanine, proline, sarcosine, ornithine, lysine, taurine, serine, threonine, homoserine, tyrosine, bicine, tricine, 3,5-diiodo-tyrosine, β-(3,4-dihydroxyphenyl)-alanine, thyroxine, 4-hydroxy-proline, cysteine, methionine, ethionine, lanthionine, cystathionine, cystine, and cysteic acid. Examples of such acids include glycine, histidine, alanine, malic acid, tartaric acid, citric acid, glycolic acid, isethionic acid, and salts thereof.
[0059] Specific examples of the nitrile compound include acetonitrile, aminoacetonitrile, propionitrile, butyronitrile, isobutyronitrile, benzonitrile, glutarodinitrile, and methoxyacetonitrile. Specific examples of the chelating agent include nitrilotriacetic acid, diethylenetriaminepentaacetic acid, ethylenediaminetetraacetic acid, N,N,N-trimethylenephosphonic acid, ethylenediamine-N,N,N',N'-tetramethylenesulfonic acid, transcyclohexanediaminetetraacetic acid, 1,2-diaminopropanetetraacetic acid, glycol ether diaminetetraacetic acid, ethylenediamine orthohydroxyphenylacetic acid, ethylenediamine disuccinic acid (SS form), N-(2-carboxylate ethyl)-L-aspartic acid, β-alanine diacetic acid, 2-phosphonobutane-1,2,4-tricarboxylic acid, 1-hydroxyethylidene-1,1-diphosphonic acid, N,N'-bis(2-hydroxybenzyl)ethylenediamine-N,N'-diacetic acid, and 1,2-dihydroxybenzene-4,6-disulfonic acid.
[0060] The metal polishing accelerator may be used alone or in combination of two or more kinds. Among the above metal polishing accelerators, inorganic acids, organic acids, or amino acids are preferred from the viewpoint of effectively increasing the polishing rate of the metal material part by the polishing composition, more preferably carboxylic acids or amino acids, particularly preferably glycine or histidine, and most preferably histidine. Therefore, in one embodiment of the present invention, the metal polishing accelerator is at least one selected from the group consisting of carboxylic acids and amino acids. By adopting such an embodiment, the technical effect of being able to easily dissolve metals and improve the polishing rate is obtained. According to one embodiment of the present invention, the number of nitrogen atoms of the amino acid is 3 to 4, or the amino acid has a heterocyclic ring in the structure. By adopting such an embodiment, the desired effect of the present invention is efficiently achieved. According to one embodiment of the present invention, the heterocyclic rings each independently have 1 to 3, 1 to 2, or 1 nitrogen atom, oxygen atom, or sulfur atom.
[0061] When the polishing composition of the present embodiment contains a metal polishing accelerator, the content of the metal polishing accelerator in the polishing composition is preferably 0.01% by weight or more, more preferably 0.05% by weight or more, and particularly preferably 0.1% by weight or more, when the total amount of the polishing composition is 100% by weight. When the content of the metal polishing accelerator is the lower limit, the polishing rate of the polishing composition for the metal material part can be further increased.
[0062] When the polishing composition of this embodiment contains a metal polishing accelerator, the content of the metal polishing accelerator in the polishing composition is preferably 10% by weight or less, more preferably 5% by weight or less, particularly preferably 3% by weight or less, particularly preferably 1% by weight or less, and also preferably 0.4% by weight or less, assuming that the total amount of the polishing composition is 100% by weight. When the content of the metal polishing accelerator is the above upper limit, excessive etching of the metal material of the polishing object can be avoided, and the burden of waste liquid treatment after polishing can be reduced. Note that, according to one embodiment of the present invention, the content of the metal polishing accelerator is 0.3 weight % or less, and according to this embodiment, the polishing rate of the resin material can be further increased. weight %, and according to such an embodiment, the removal rate of the metal material can be further increased.
[0063] [Metal corrosion inhibitor] The polishing composition of this embodiment may further contain a metal corrosion inhibitor as necessary. By adding a metal corrosion inhibitor to the polishing composition, it is possible to further suppress the occurrence of dents beside wiring during polishing using the polishing composition. Furthermore, it is possible to suppress or avoid the occurrence of corrosion of metal materials, and thus to improve the surface flatness and quality of metal structures. In addition, when polishing an object to be polished that includes a patterned structure formed of resin and metal materials, it is possible to improve the surface flatness of the object to be polished, and further reduce the steps that are generated on the surface of the object to be polished by polishing.
[0064] The metal corrosion inhibitor that can be used is not particularly limited, but is preferably a heterocyclic compound or a surfactant. The number of members of the heterocycle in the heterocyclic compound is not particularly limited. The heterocyclic compound may be a monocyclic compound or a polycyclic compound having a condensed ring. The metal corrosion inhibitor may be used alone or in combination of two or more kinds. The metal corrosion inhibitor may be a commercially available product or a synthetic product.
[0065] Specific examples of heterocyclic compounds that can be used as metal corrosion inhibitors include nitrogen-containing heterocyclic compounds such as pyrrole compounds, pyrazole compounds, imidazole compounds, triazole compounds, tetrazole compounds, pyridine compounds, pyrazine compounds, pyridazine compounds, pyrindine compounds, indolizine compounds, indole compounds, isoindole compounds, indazole compounds, purine compounds, quinolizine compounds, quinoline compounds, isoquinoline compounds, naphthyridine compounds, phthalazine compounds, quinoxaline compounds, quinazoline compounds, cinnoline compounds, buteridine compounds, thiazole compounds, isothiazole compounds, oxazole compounds, isoxazole compounds, and furazan compounds.
[0066] More specifically, examples of pyrazole compounds include 1H-pyrazole, 4-nitro-3-pyrazolecarboxylic acid, 3,5-pyrazolecarboxylic acid, 3-amino-5-phenylpyrazole, 5-amino-3-phenylpyrazole, 3,4,5-tribromopyrazole, 3-aminopyrazole, 3,5-dimethylpyrazole, 3,5-dimethyl-1-hydroxymethylpyrazole, 3-methylpyrazole, 1-methylpyrazole, 3-amino-5-methylpyrazole, 4-amino-pyrazolo[3,4-d]pyrimidine, allopurinol, 4-chloro-1H-pyrazolo[3,4-D]pyrimidine, 3,4-dihydroxy-6-methylpyrazolo(3,4-B)-pyridine, and 6-methyl-1H-pyrazolo[3,4-b]pyridin-3-amine.
[0067] Examples of the imidazole compound include imidazole, 1-methylimidazole, 2-methylimidazole, 4-methylimidazole, 1,2-dimethylpyrazole, 2-ethyl-4-methylimidazole, 2-isopropylimidazole, benzimidazole, 5,6-dimethylbenzimidazole, 2-aminobenzimidazole, 2-chlorobenzimidazole, 2-methylbenzimidazole, 2-(1-hydroxyethyl)benzimidazole, 2-hydroxybenzimidazole, 2-phenylbenzimidazole, 2,5-dimethylbenzimidazole, 5-methylbenzimidazole, 5-nitrobenzimidazole, and 1H-purine.
[0068] Examples of the triazole compound include, for example, 1,2,3-triazole, 1,2,4-triazole, 1-methyl-1,2,4-triazole, methyl-1H-1,2,4-triazole-3-carboxylate, 1,2,4-triazole-3-carboxylic acid, methyl 1,2,4-triazole-3-carboxylate, 1H-1,2,4-triazole-3-thiol, 3,5-diamino-1H-1,2,4-triazole, 3-amino-1,2,4-triazole-5-thiol, 3-amino-1H-1,2,4-triazole, 3-amino-5-benzyl-4H-1,2,4-triazole, 3 -Amino-5-methyl-4H-1,2,4-triazole, 3-nitro-1,2,4-triazole, 3-bromo-5-nitro-1,2,4-triazole, 4-(1,2,4-triazol-1-yl)phenol, 4-amino-1,2,4-triazole, 4-amino-3,5-dipropyl-4H-1,2,4-triazole, 4-amino-3,5-dimethyl-4H-1,2,4-triazole, 4-amino-3,5-dipeptyl-4H-1,2,4-triazole, 5-methyl-1,2,4-triazole-3,4-diamine, 1H-benzotriazole , 1-hydroxybenzotriazole, 1-aminobenzotriazole, 1-carboxybenzotriazole, 5-chloro-1H-benzotriazole, 5-nitro-1H-benzotriazole, 5-carboxy-1H-benzotriazole, 5-methyl-1H-benzotriazole, 5,6-dimethyl-1H-benzotriazole, 1-(1',2'-dicarboxyethyl)benzotriazole, 1-[N,N-bis(hydroxyethyl)aminomethyl]benzotriazole, 1-[N,N-bis(hydroxyethyl)aminomethyl]-5-methylbenzotriazole, 1-[N,N-bis(hydroxyethyl)aminomethyl]-4-methylbenzotriazole, and the like.
[0069] Examples of the tetrazole compound include 1H-tetrazole, 5-methyltetrazole, 5-aminotetrazole, and 5-phenyltetrazole.
[0070] Examples of indazole compounds include 1H-indazole, 5-amino-1H-indazole, 5-nitro-1H-indazole, 5-hydroxy-1H-indazole, 6-amino-1H-indazole, 6-nitro-1H-indazole, 6-hydroxy-1H-indazole, and 3-carboxy-5-methyl-1H-indazole.
[0071] Examples of indole compounds include 1H-indole, 1-methyl-1H-indole, 2-methyl-1H-indole, 3-methyl-1H-indole, 4-methyl-1H-indole, 5-methyl-1H-indole, 6-methyl-1H-indole, 7-methyl-1H-indole, 4-amino-1H-indole, 5-amino-1H-indole, 6-amino-1H-indole, 7-amino-1H-indole, 4-hydro-1H-indole, 5-amino-1H-indole, 6-amino-1H-indole, 7-amino-1H-indole, 4-hydro-1H-indole, 5-amino-1H-indole, 6-hydro ... 1H-indole, 5-hydroxy-1H-indole, 6-hydroxy-1H-indole, 7-hydroxy-1H-indole, 4-methoxy-1H-indole, 5-methoxy-1H-indole, 6-methoxy-1H-indole, 7-methoxy-1H-indole, 4-chloro-1H-indole, 5-chloro-1H-indole, 6-chloro-1H-indole, 7-chloro-1H-indole, 4-carboxy-1H- Indole, 5-carboxy-1H-indole, 6-carboxy-1H-indole, 7-carboxy-1H-indole, 4-nitro-1H-indole, 5-nitro-1H-indole, 6-nitro-1H-indole, 7-nitro-1H-indole, 4-nitrile-1H-indole, 5-nitrile-1H-indole, 6-nitrile-1H-indole, 7-nitrile-1H-indole, 2,5-dimethyl-1H-indole Indole, 1,2-dimethyl-1H-indole, 1,3-dimethyl-1H-indole, 2,3-dimethyl-1H-indole, 5-amino-2,3-dimethyl-1H-indole, 7-ethyl-1H-indole, 5-(aminomethyl)indole, 2-methyl-5-amino-1H-indole, 3-hydroxymethyl-1H-indole, 6-isopropyl-1H-indole, 5-chloro-2-methyl-1H-indole, and the like.
[0072] Among these, the preferred heterocyclic compounds are triazole compounds, and in particular, 1H-benzotriazole, 5-methyl-1H-benzotriazole, 5,6-dimethyl-1H-benzotriazole, 1-[N,N-bis(hydroxyethyl)aminomethyl]-5-methylbenzotriazole, 1-[N,N-bis(hydroxyethyl)aminomethyl]-4-methylbenzotriazole, 1,2,3-triazole, and 1,2,4-triazole are preferred. These heterocyclic compounds have a high chemical or physical adsorption power to the surface of the object to be polished, so that they can form a stronger protective film on the surface of the object to be polished, and thus can effectively suppress the corrosion of metal materials. This is advantageous in improving the flatness of the surface of the object to be polished after polishing with the polishing composition of the present invention.
[0073] When the polishing composition of the present embodiment contains a metal corrosion inhibitor, the content of the metal corrosion inhibitor in the polishing composition is preferably 0.001% by weight or more, more preferably 0.005% by weight or more, and particularly preferably 0.01% by weight or more, when the total amount of the polishing composition is 100% by weight. When the content of the metal corrosion inhibitor is the above-mentioned lower limit, the corrosion of the metal material can be effectively suppressed.
[0074] When the polishing composition of this embodiment contains a metal corrosion inhibitor, the content of the metal corrosion inhibitor in the polishing composition is preferably 5% by weight or less, more preferably 1% by weight or less, particularly preferably 0.5% by weight or less, and most preferably 0.1% by weight or less, when the total amount of the polishing composition is 100% by weight. When the content of the metal corrosion inhibitor is the above upper limit, it is possible to avoid an excessive decrease in the polishing speed of the metal material of the polishing object. This makes it possible to reduce the step that is generated on the surface of the polishing object by polishing. Furthermore, it is also possible to reduce the burden of waste liquid treatment after polishing.
[0075] In view of the above, in one embodiment of the present invention, a polishing composition further containing an oxidizing agent having a standard electrode potential of 0.5 V or more, a metal polishing accelerator, and a metal corrosion inhibitor is preferable. By adopting such an embodiment, the intended effect of the present invention is efficiently achieved. In one embodiment of the present invention, a polishing composition is provided which further contains an oxidizing agent having a standard electrode potential of 0.5 V or more, a metal polishing accelerator, and at least one of a metal corrosion inhibitor and an oxidizing agent.
[0076] [Other ingredients] The polishing composition used in the polishing method of the present invention may further contain other components such as a chelating agent, a water-soluble polymer, a preservative, and an antifungal agent, if necessary.
[0077] [Polishing method and substrate manufacturing method] As described above, the polishing composition according to the present invention is particularly suitable for polishing a substrate including a patterned structure formed of a resin material and a metal material. Thus, the present invention provides a polishing method for polishing an object to be polished including a patterned structure formed of a resin material and, if necessary, a metal material with the polishing composition according to the present invention. For example, such an object to be polished can be a substrate including a patterned structure formed of polyimide and copper. The present invention also provides a method for manufacturing a substrate, comprising a step of polishing a substrate including a patterned structure formed of a resin and, if necessary, a metal material, using the polishing composition according to the present invention. Such a substrate can include, for example, a patterned structure formed of polyimide and copper. When polishing an object to be polished including a patterned structure formed of a resin material and a metal material, in order to effectively reduce the step formed on the surface of the object to be polished by polishing, the closer the ratio of the removal rate of the resin material to the removal rate of the metal material is to 1.0, the better. More specifically, when polishing an object to be polished including a patterned structure formed of a resin material and a metal material at a specific polishing pressure (e.g., 5 psi), the closer the ratio (R1 / R2) of the removal rate of the resin material R1 to the removal rate of the metal material R2 is to 1.0, the better. In some embodiments, when the polishing pressure is 5 psi, the removal rate of the polishing composition for the resin material is defined as a first removal rate R1, and the removal rate of the polishing composition for the metal material is defined as a second removal rate R2, and the ratio of the first removal rate to the second removal rate (R1 / R2) is 0.5 to 6.0. In other embodiments, the ratio of the first removal rate to the second removal rate (R1 / R2) is 0.5 to 4.0. In still other embodiments, the ratio of the first removal rate to the second removal rate (R1 / R2) is 0.8 to 3.0 (or 0.8 to 1.5).
[0078] The polishing apparatus used in the polishing step may be a polishing apparatus used in a general chemical mechanical polishing process. Such a polishing apparatus is equipped with a carrier for holding the object to be polished, a motor capable of changing the rotation speed, and the like, and also includes a polishing platen on which a polishing pad (or a polishing cloth) can be attached.
[0079] There is no particular limitation on the polishing pad, and it is possible to use a general nonwoven fabric, a polyurethane resin pad, a porous fluororesin pad, etc. Furthermore, if necessary, the polishing pad can be grooved, so that the polishing composition can be accumulated in the grooves of the polishing pad.
[0080] The parameter conditions of the polishing step are not particularly limited, and can be adjusted according to actual needs.For example, the rotation speed of the polishing platen can be 10 to 500 rpm, the rotation speed of the carrier can be 10 to 500 rpm, and the flow rate of the polishing composition can be 10 to 500 ml / min.The method of supplying the polishing composition to the polishing pad is also not particularly limited, and for example, a method of continuous supply using a pump or the like can be adopted.
[0081] After the polishing step is completed, the object to be polished is washed in a water stream and dried in a rotary dryer or the like to remove water droplets adhering to the object to be polished, thereby obtaining a substrate having a flat surface without any steps. EXAMPLES
[0082] [Example] The present invention will be described in more detail with reference to the following examples and comparative examples, but the technical scope of the present invention is not limited to the following examples. In this specification, unless otherwise specified, operations and measurements of physical properties are performed under the conditions of room temperature (20 to 25°C) and relative humidity of 40 to 50% RH.
[0083] [Preparation of polishing composition] According to the composition shown in Table 1 below, abrasive grains, pH adjuster, metal polishing accelerator, metal corrosion inhibitor, and oxidizer were mixed in a dispersion medium (ultrapure water) (mixing temperature: about 25°C, mixing time: about 10 minutes) to prepare a polishing composition. The abrasive grains shown in Table 1 can be commercially available products, or can be obtained by adding a chemical for modifying the surface (e.g., aluminum chloride, APTES, sulfonic acid, etc., aluminum chloride in this embodiment) to abrasive grains whose surface is not modified. The pH of the polishing composition was confirmed using a pH meter (LAQUA manufactured by Horiba, Ltd.) (the temperature of the polishing composition when measuring the pH value was 25°C). In addition, "-" in Table 1 indicates that the component was not added. Details of each component in Table 1 are as follows.
[0084] Abrasive A: Colloidal silica with the surface modified with aluminum ions (primary particle size: 60 nm; secondary particle size: 120 nm) Abrasive B: Colloidal silica with unmodified surface (primary particle size: 30 nm; secondary particle size: 60 nm) Grain C: Grain B whose surface was modified with aminopropyltriethoxysilane (APTES) (Primary particle size: 30 nm; Secondary particle size: 60 nm; APTES modifier concentration: 1.3 M) Grain D: Grain B with the surface modified with sulfonic acid (primary particle size: 30 nm; secondary particle size: 60 nm) Abrasive E: Colloidal silica with unmodified surface (primary particle size: 60 nm; secondary particle size: 120 nm) Grain F: Grain E with its surface modified with aminopropyltriethoxysilane (primary particle size: 60 nm; secondary particle size: 120 nm; APTES modifier concentration: 1.3 M) Grain G: Grain E whose surface was modified with aminopropyltriethoxysilane (primary particle size: 60 nm; secondary particle size: 120 nm; APTES modifier concentration: 3.7 M) Abrasive H: Abrasive E whose surface has been modified with aminopropyltriethoxysilane (primary particle size: 60 nm; secondary particle size: 120 nm; APTES modifier concentration: 5.0 M).
[0085] H2O2: Hydrogen peroxide (concentration: 31%): Standard electrode potential 1.7V, Hydrochloric acid: (concentration: 37%) Succinic acid: (purity: 99.9%) Gly: glycine (purity: 100%), L-His: L-histidine (purity: 98%), BTA: Benzotriazole (purity: 99.9%).
[0086] [How to make abrasive grains A, C, D, F to H] Abrasive grain A: 1 L of silica sol (similar to abrasive grain E) in which fine silica particles are dispersed at a silica concentration of 20 mass % was maintained at a temperature in the range of 0 to 15° C., and 4.0 g of aluminum chloride was added while stirring or circulating.
[0087] Abrasive C: A colloidal silica dispersion containing 20 mass% colloidal silica (same as abrasive B) in pure water as a dispersion medium was prepared. 1.3 mmol (3.7 mmol, 5.0 mmol) of (3-aminopropyl)triethoxysilane (APTES) was slowly added (1 drop per about 5 seconds, 1 drop about 0.03 g) to 1 L of the colloidal silica dispersion. During the addition, the colloidal silica dispersion was stirred at a speed of 300 to 400 rpm with a stirrer. After the addition of APTES was completed, stirring was continued for 5 hours at room temperature (25°C).
[0088] Abrasive grain D: A colloidal silica dispersion containing 20% by mass of colloidal silica (same as abrasive grain B) in pure water as a dispersion medium was prepared. 1.2 g of 3-mercaptopropyltrimethoxysilane was added as a silane coupling agent to 1 L of the colloidal silica dispersion, and the mixture was refluxed at the boiling point to perform thermal aging. Thereafter, in order to keep the volume constant, pure water was added while replacing methanol and ammonia with water, and when the pH became 8 or less, the liquid temperature of the silica sol was temporarily lowered to room temperature. Next, 10.7 g of 35% hydrogen peroxide water was added and heated again, and the reaction was continued for 8 hours. After cooling to room temperature, a sulfonic acid-modified aqueous anionic silica sol was obtained.
[0089] Abrasives F, G, and H: A colloidal silica dispersion containing 20 mass% colloidal silica (similar to abrasive E) in pure water was prepared as a dispersion medium. 1.3 mmol (3.7 mmol, 5.0 mmol) of (3-aminopropyl)triethoxysilane (APTES) was slowly added (1 drop every 5 seconds, 1 drop approximately 0.03 g). During the addition, the colloidal silica dispersion was stirred at a speed of 300 to 400 rpm with a stirrer. After the addition of APTES was completed, stirring was continued at room temperature (25°C) for 5 hours.
[0090] [Measurement of surface zeta potential] The surface zeta potential of the abrasive grains contained in the polishing composition was measured by a multiple frequency electro-acoustic method using an interfacial potential analyzer (Zeta Probe Analyzer, manufactured by Colloidal Dynamics).
[0091] [Measurement of removal rate] The polishing rate was measured when a polyimide substrate (manufactured by SVM: film thickness 50,000 Å) and a copper substrate (manufactured by SVM: film thickness 40,000 Å) were polished using the polishing composition obtained above under the following polishing conditions.
[0092] Polishing equipment: Single-sided CMP polishing equipment (FREX 300E: manufactured by Ebara Corporation) Polishing pad: Polyurethane pad Plate rotation speed: 110 rpm Carrier rotation speed: 110 rpm Flow rate of polishing composition: 300 mL / min Polishing time: 60sec Grinding pressure: 2 psi (approx. 13.8 kPa) or 5 psi (34.5 kPa ).
[0093] The thickness of the polished object before and after polishing was measured by an optical interference film thickness measurement system (KLA-Tencor, ASET-F5X) for the polyimide substrate, and a sheet resistor (KLA-Tencor, OmniMap RS-100) for the copper substrate. The removal rate was calculated by the following formula.
[0094] Removal rate = {[Thickness before polishing] - [Thickness after polishing]} / [Processing time] where thickness is in Å, treatment time is in minutes, and removal rate is in (Å / min).
[0095] [Calculation of removal rate ratio value] The polishing step is performed under the above polishing pressure (i.e., 2 psi or 5 psi), and the removal rate R of the polyimide substrate at this polishing pressure is calculated according to the above formula. PI Similarly, the polishing step was performed under the above polishing pressure (i.e., 5 psi), and the removal rate R of the copper substrate at this polishing pressure was calculated using the above formula. Cu The removal rate R of the polyimide substrate at a polishing pressure of 5 psi was calculated. PI Removal rate of copper substrate R Cu The ratio value (R PI / R Cu The ratio of the removal rates (R PI / R Cu ) can be used to represent the ratio of the removal rate of the resin material (i.e., PI) to the removal rate of the metal material (i.e., copper) under this particular polishing pressure (i.e., 5 psi). The value of the removal rate ratio (R PI / R Cu The larger the ratio of the removal rate of the resin material to the removal rate of the metal material, the greater the removal rate R PI , the removal rate of the copper substrate R Cu and / or the removal rate R of the polyimide substrate PI Removal rate of copper substrate R Cu The ratio value (R PI / R Cu ) are shown in Table 1.
[0096] [Cu etching rate] (Test conditions) In Examples 1 to 13 and Comparative Examples 1 to 9, a silicon wafer (200 mm, blanket wafer) having a copper film of 10,000 Å formed on the surface was used as a test piece. Each silicon wafer was cut into a coupon of 30 mm×30 mm chip, and the coupon was immersed in 200 ml of each polishing composition under the following conditions.
[0097] Soaking time: 10 minutes Soaking temperature: 60℃ Stirrer rotation speed: 300 rpm.
[0098] (Etching rate evaluation) The thickness of the copper layer before and after immersion was measured using a sheet resistor meter (OmniMap RS-100, manufactured by KLA-Tencor), and the amount of copper etched was determined as (thickness before immersion) - (thickness after immersion).
[0099] The results obtained are shown in Table 1.
[0100] The lower this value, the more the dissolution that is expected to occur during polishing of the copper layer is suppressed, which is to say, it can be said to be a favorable result in suppressing the formation of steps.
[0101] [Table 1]
[0102] See Example 1 and Comparative Examples 3 to 9 in Table 1. Other than the different abrasive grains used, the other experimental conditions in Example 1 and Comparative Examples 3 to 9 are the same or similar. In Example 1, colloidal silica with its surface modified with aluminum ions was used as the abrasive grain (i.e., abrasive grain A), and the removal rate R of the polyimide substrate was 1.0 μm. PI The removal rate R of the polyimide substrate in Comparative Examples 3 to 9 was 2867 Å / min. In contrast, the abrasive grains used in Comparative Examples 3 to 9 (i.e., abrasive grains B to H) were all different from the abrasive grains according to the present invention. PI are the removal rates R of the polyimide substrate in Example 1.PI As can be seen from this, the polishing composition of the present invention can significantly increase the removal rate of polyimide.
[0103] Please refer to Examples 2 to 4 and Comparative Examples 1 and 2 in Table 1. Except for the different pH values of the polishing compositions, the other experimental conditions are all the same or similar. The pH value of the polishing composition in Comparative Example 2 is 8.0, and the removal rate R PI The flow rate was 118 Å / min. comparison In Example 1, the pH value of the polishing composition was 2.0, and the removal rate of the polyimide substrate R PI but 30 In Examples 2 to 4, the pH values of the polishing compositions were 3.0, 5.0, and 6.0, respectively, and the removal rates R PI were 5079 Å / min, 6489 Å / min and 6721 Å / min, respectively. As can be seen from these, the polishing composition of the present invention can significantly increase the removal rate of polyimide in a specific pH range (e.g., pH greater than 2.0 and equal to or less than 7).
[0104] See Example 5 to Example 12 in Table 1. The polishing compositions used in each of Examples 5 to 12 contain the abrasive grains according to the present invention (i.e., abrasive grains A), a metal polishing accelerator, an oxidizing agent, and (in some Examples) a metal corrosion inhibitor. In Examples 5 to 12, when the polishing pressure is 5 psi, the removal rate R of the polyimide substrate is PI Removal rate of copper substrate R Cu The ratio value (R PI / R Cu ) were 2.9, 3.5, 0.8, 1.2, 1.3, 1.3, 1.4 and 2.1, respectively. As can be seen from this, when a polishing object including a patterned structure formed of polyimide and copper is polished with the polishing composition used in each of Examples 5 to 12, the ratio of the removal rate of polyimide to the removal rate of copper can be made extremely close to 1.0.
[0105] In summary, the polishing composition according to the present invention contains abrasive grains having a specific structure, and can significantly increase the removal rate of resin materials under a specific pH environment. When a polishing object including a patterned structure formed of a resin material and a metal material is polished using the polishing composition according to the present invention, the ratio of the removal rate of the resin material to the removal rate of the metal material can be reduced. Therefore, the step formed on the surface of the polishing object by polishing can be effectively reduced. In addition, the polishing composition according to the present invention may further contain at least one selected from the group consisting of an oxidizing agent, a metal polishing accelerator, and a metal corrosion inhibitor, which can further adjust the removal rate of the metal material and reduce the corrosion of the metal material. When a polishing object including a patterned structure formed of a resin material and a metal material is polished using such a polishing composition, the step formed on the surface of the polishing object by polishing can be more effectively reduced.
[0106] In addition, the polishing composition according to the present invention can be used in a chemical mechanical polishing process and is useful for obtaining a substrate having a flat surface, and therefore has industrial applicability.
[0107] Although the present invention has been disclosed above by several preferred embodiments, these are not intended to limit the present invention, and those skilled in the art may of course make any changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be determined by the following claims.
[0108] This application is based on Japanese Patent Application No. 2019-061636 filed on March 27, 2019, the disclosure of which is incorporated herein by reference in its entirety. [Explanation of symbols]
[0109] 102...Colloidal silica particles, 104...Aluminum chloride modifier, 112...Modified colloidal silica particles.
Claims
1. A polishing composition comprising: an abrasive grain comprising silica, in which at least a portion of the hydrogen atoms constituting silanol groups located on the surface of the silica are substituted with cations of a metal atom M which is at least one selected from the group consisting of aluminum, chromium, titanium, zirconium, iron, zinc, tin, scandium and gallium; A pH adjuster; and A dispersion medium; An oxidant having a standard electrode potential of 0.5 V or more; A metal polishing accelerator; and a pH of from 4 to 7, the composition being used for polishing an object to be polished that contains a resin.
2. 2. The polishing composition according to claim 1, wherein one metal atom M is bonded to one oxygen atom of one silanol group, one metal atom M is bonded to two oxygen atoms of two silanol groups, or one metal atom M is bonded to three oxygen atoms of three silanol groups.
3. 3. The polishing composition according to claim 1, wherein the abrasive grains have a primary particle size of 40 to 150 nm.
4. 4. The polishing composition according to claim 1, wherein the content of the abrasive grains is 0.1 to 10 wt % based on the total weight of the polishing composition.
5. 5. The polishing composition according to claim 1, wherein the metal polishing accelerator is at least one selected from the group consisting of carboxylic acids and amino acids.
6. 6. The polishing composition according to claim 5, wherein the amino acid has 3 to 4 nitrogen atoms or has a heterocycle in its structure.
7. 7. The polishing composition according to claim 1, wherein the resin has a melting point of 200° C. or higher.
8. The polishing composition according to claim 7 , wherein the resin has a nitrogen atom.
9. A polishing method comprising a step of polishing an object to be polished with the polishing composition according to any one of claims 1 to 8, wherein a surface of the object to be polished includes a patterned structure, and the patterned structure includes a resin.
10. 10. The polishing method according to claim 9, wherein the patterned structure further comprises a metallic material, the metallic material comprising at least one selected from the group consisting of copper, aluminum, cobalt, tungsten, and combinations thereof.
11. 11. The polishing method according to claim 10, wherein, when a polishing pressure is 5 psi, a removal rate of the polishing composition for the resin is defined as a first removal rate R1, and a removal rate of the polishing composition for the metal material is defined as a second removal rate R2, a ratio R1 / R2 of the first removal rate to the second removal rate is 0.5 to 6.
0.
12. providing a substrate; A step of polishing the substrate using the polishing composition according to any one of claims 1 to 8; Including, A method for manufacturing a substrate, wherein a surface of the substrate includes a pattern structure, and the pattern structure includes a resin and a metal material.
Citation Information
Patent Citations
Polishing liquid composition
JP2006026885A
Organic insulating material, polishing material for copper film compound material, and polishing method
JP2007150264A
Metal polishing composition, and chemical-mechanical polishing method using it
JP2007299942A
Polishing liquid for CMP, storage liquid for polishing liquid for CMP, polishing method, semiconductor substrate and electronic apparatus
JP2014022511A
Polishing composition
JP2015189898A