Resin composition for paint and paint

The resin composition with minimized reactive groups in an amino group-containing acrylic resin and siloxane oligomer, combined with a polyepoxide, addresses the issue of crack resistance and impact resistance in outdoor coatings by allowing independent polymer formation, resulting in a durable and flexible film with high gloss retention.

JP7576075B2Active Publication Date: 2024-10-30NIPPON PAINT CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2022208693
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-12-26
Publication Date
2024-10-30
Estimated Expiration
2042-12-26

AI Technical Summary

Technical Problem

Existing hybrid coating films for outdoor use suffer from inferior crack resistance and impact resistance due to insufficient chemical bonding between organic and inorganic components, leading to issues like microcracks and chalking.

Method used

A resin composition comprising an amino group-containing acrylic resin and a siloxane oligomer, with a polyepoxide as a curing agent, where the reactive groups are minimized to prevent cross-linking between components, allowing for independent polymer formation, thereby enhancing flexibility and resistance to environmental factors.

Benefits of technology

The coating film exhibits excellent impact resistance and maintains gloss retention, suppressing cracks and chalking even after prolonged outdoor exposure, with a gloss retention rate of 80% or more after one and a half years.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576075000001
    Figure 0007576075000001
  • Figure 0007576075000002
    Figure 0007576075000002
  • Figure 0007576075000003
    Figure 0007576075000003
Patent Text Reader

Abstract

To provide a resin composition from which a coated film excellent in suppression of cracking under outdoor environment and impact resistance can be obtained.SOLUTION: A resin composition for coating contains a main agent (A) containing an amino group-containing acrylic resin (a1) and a siloxane oligomer (a2), and a curing agent (B) containing a polyepoxide (b1) and a curing catalyst (b2), wherein (a1) has an amine value of 8 mgKOH / g or more and 90 mgKOH / g or less, (b1) has an epoxy equivalent of 100 g / eq or more and 1,500 g / eq or less, in (a1), a reactive group capable of reacting with a silanol group does not exist or the number of the reactive groups is less than 11% of the number of the amino groups in (a1), and in (b1), the reactive group does not exist, or the number of the reactive groups is less than 10% of the number of the epoxy groups in (b1).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition for paint and a paint. [Background technology]

[0002] Weather resistance is required for paints for buildings installed outdoors. Therefore, hybrid coating films in which organic components and inorganic components such as polysiloxane are chemically bonded have been proposed. Hybrid coating films are formed, for example, by the coatings described in Patent Documents 1 to 4. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-145268 A [Patent Document 2] JP 2018-145371 A [Patent Document 3] International Publication No. 2019 / 107124 [Patent Document 4] JP 2020-164583 A Summary of the Invention [Problem to be solved by the invention]

[0004] Patent Documents 1 and 2 disclose resin compositions in which a vinyl polymer (a1) and a polysiloxane (a2) are chemically bonded. Patent Document 3 discloses a coating composition containing (B) a compound having one or more functional groups capable of undergoing a Michael addition reaction with an acryloyloxy group and an alkoxy group, (C) an aliphatic urethane acrylate oligomer having three or more functional groups, and (A) a silicone resin having reactive groups that react with the above (B) and (C). Patent Document 4 discloses a coating composition containing a polyorganosiloxane and an acrylic resin having a hydroxyl group or a reactive silicon group. All of these compositions form a hybrid coating film. However, such a hybrid coating film is inferior in crack suppression and impact resistance in an outdoor environment.

[0005] The present invention has been made in view of the above, and an object of the present invention is to provide a resin composition which is capable of suppressing the occurrence of cracks in outdoor environments and giving a coating film which is excellent in impact resistance. [Means for solving the problem]

[0006] In order to solve the above problems, the present invention provides the following aspects. [1] Contains a base agent (A) and a hardener (B), The main component (A) contains an amino group-containing acrylic resin (a1) and a siloxane oligomer (a2), The curing agent (B) contains a polyepoxide (b1) and a curing catalyst (b2), The amino group-containing acrylic resin (a1) has an amine value of 8 mgKOH / g or more and 90 mgKOH / g or less, The polyepoxide (b1) has an epoxy equivalent of 100 g / eq or more and 1,500 g / eq or less, In the amino group-containing acrylic resin (a1), there is no reactive group capable of reacting with a silanol group, or the number of the reactive groups is less than 11% of the number of amino groups in the amino group-containing acrylic resin (a1); In the polyepoxide (b1), the reactive groups capable of reacting with silanol groups are absent or the number of the reactive groups is less than 10% of the number of epoxy groups in the polyepoxide (b1); The siloxane oligomer (a2) is represented by the following general formula (x): [ka] (In the formula, R 3 represents independently in each structural unit a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a single bond, R 4 represents independently in each structural unit an alkyl group having 1 to 5 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aralkyl group having 7 to 15 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or -O-; m is an integer from 0 to 200. and a structural unit X represented by the following general formula (y): [ka] (In the formula, R 5 and R 6 each independently in each repeating unit represents an alkyl group having 1 to 5 carbon atoms, an aryl group having 6 to 10 carbon atoms, or an aralkyl group having 7 to 15 carbon atoms; n is an integer from 0 to 200. A structural unit Y represented by has, as an end group, at least one selected from the group consisting of a hydrogen atom, a hydroxyl group, an alkyl group having 1 to 5 carbon atoms, and an alkoxy group having 1 to 5 carbon atoms; m+n is an integer from 2 to 200, A resin composition for paint, which satisfies n / (m+n)≧0.19, A coating film formed from the coating resin composition is subjected to an outdoor exposure test in Miyakojima for one and a half years in accordance with JIS K5600-7-6, with the coating film facing the equatorial plane at an angle of 20° to the horizontal plane, and after that, the gloss retention rate in accordance with JIS K5659 7.21 is 80% or more. [2] The resin composition for paint according to the above [1], wherein the reactive group is at least one selected from the group consisting of a hydroxyl group, an alkoxy group, an alkoxysilyl group and a silanol group. [3] The coating resin composition according to the above [1] or [2], wherein the mass ratio of the siloxane oligomer (a2) to the total solid content of the amino group-containing acrylic resin (a1), the siloxane oligomer (a2) and the polyepoxide (b1) is 10 mass % or more and 90 mass % or less. [4] A paint comprising the paint resin composition according to [1] or [2] above. [5] In addition, the paint mentioned above in [4] contains a Class 3 organic solvent as specified in the Industrial Safety and Health Act. Effect of the Invention

[0007] According to the present invention, there are provided a resin composition which can give a coating film which is excellent in impact resistance and suppresses the occurrence of cracks in outdoor environments, and a coating material containing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] It is said that coating films formed from polysiloxanes have excellent weather resistance. However, when exposed to moisture and heat for a long period of time, polysiloxanes condense, causing non-uniform shrinkage in the coating film. The hybrid coating film aims to alleviate the above-mentioned shrinkage of the coating film caused by the condensation of polysiloxanes by chemically bonding (typically covalently bonding) an organic component to polysiloxane to impart flexibility to the coating film. However, it has been found that chemically bonding polysiloxanes to an organic component results in insufficient weather resistance of polysiloxanes against substances other than moisture, and insufficient shrinkage alleviation action due to the flexibility of the organic component. Hereinafter, weather resistance refers to resistance to ultraviolet light, heat, and moisture.

[0009] In the present disclosure, both the amino group-containing acrylic resin (a1) and polyepoxide (b1), which are organic components, do not react with the siloxane oligomer (a2), which is an inorganic component, or the reaction is suppressed. Therefore, in the resulting coating film, the first polymer portion formed by the reaction product of the amino group-containing acrylic resin (a1) and polyepoxide (b1) and the second polymer portion formed by the polymer of the siloxane oligomer (a2) (or the polymer of the siloxane oligomer (a2) containing the curing catalyst (b2). The same applies below.) are substantially independent of each other. This allows the coating film to exhibit both the properties of the organic component (e.g., flexibility) and the properties of the inorganic component (e.g., resistance to ultraviolet light and heat).

[0010] When the functions of both the first polymer (organic component) and the second polymer (inorganic component) are fully exerted, the first polymer can exist in the coating film without shrinking in accordance with the shrinkage caused by the condensation of the second polymer. Therefore, the shrinkage of the entire coating film is mitigated, and for example, the occurrence of microcracks is suppressed. In addition, the resistance to ultraviolet light and heat by the second polymer suppresses the occurrence of chalking, for example.

[0011] Furthermore, the coating film formed by the resin composition according to the present disclosure has a gloss retention rate of 80% or more according to JIS K5659 7.21 after one and a half years of outdoor exposure testing (hereinafter, sometimes simply referred to as outdoor exposure testing) at an angle of 20° to the horizontal plane toward the equatorial plane in Miyakojima in accordance with JIS K5600-7-6. The gloss retention rate may be 83% or more, or may be 85% or more.

[0012] The outdoor exposure test may be carried out, for example, by an external testing organization (typically, the Japan Weathering Test Center (JWTC), a general incorporated foundation, Miyakojima Exposure Test Site (Miyakojima City, Okinawa Prefecture)).

[0013] The gloss retention rate represents the change in the surface condition of the coating film (e.g., change in surface unevenness and surface roughness). In outdoor exposure tests, the coating film is exposed to ultraviolet rays, heat, and moisture (e.g., rain, snow, frost), etc. Even after this outdoor exposure test, a gloss retention rate of 80% or more means that the change in the surface condition is extremely small even when exposed to ultraviolet rays, heat, water, etc. Usually, ultraviolet rays, heat, and moisture deteriorate the organic component (first polymer) and promote the shrinkage of the inorganic component (second polymer).

[0014] In outdoor exposure tests, the surface state changes, for example, due to deterioration of the first polymer and / or shrinkage of the second polymer. Small changes in the surface state (i.e., the gloss retention rate of the coating film after outdoor exposure tests is 80% or more) indicates, in other words, that the functions of both the first polymer and the second polymer are fully exerted. If the first polymer and the second polymer are substantially independent from each other, the gloss retention rate of the coating film after outdoor exposure tests is likely to be 80% or more.

[0015] Degradation of the first polymer and shrinkage of the second polymer manifests itself as the development of microcracking and / or chalking, reduced adhesion, and discoloration.

[0016] The organic component is a component that contains a carbon-carbon bond in the main chain, and may refer to the first polymer as well as the material of the first polymer (i.e., the amino group-containing acrylic resin (a1) and the polyepoxide (b1)) in this specification. The inorganic component is a component that contains a bond other than a carbon-carbon bond in the main chain (herein, Si-O), and may refer to the second polymer as well as the material of the second polymer (i.e., the siloxane oligomer (a2)) in this specification.

[0017] "The first and second polymer portions are substantially independent of each other" means that a bond between the amino group-containing acrylic resin and / or polyepoxide and the siloxane oligomer is permitted when the ratio R1 is 0% or less than 11% and the ratio R2 is 0% or less than 10%. The amino group-containing acrylic resin and / or polyepoxide and the siloxane oligomer may or may not be bonded to each other within the above-mentioned permitted range. The bond between the two may or may not be via another compound.

[0018] In addition, in the resin composition according to the present disclosure, the siloxane oligomer (a2) satisfies n / (m+n)≧0.19, where m is the number of repetitions of the structural unit X that can form a second polymer having a three-dimensional structure, and n is the number of repetitions of the structural unit Y that can form a linear second polymer. In other words, the siloxane oligomer (a2) has relatively few crosslinking points that can form a three-dimensional structure. Therefore, when the siloxane oligomer (a2) self-condenses, the formation of a branched three-dimensional structure is suppressed, and the structure is easily close to linear, and the flexibility of the formed second polymer is improved. This improves the impact resistance of the resulting coating film, making it less susceptible to damage by external forces.

[0019] [Resin composition] The coating film is formed from the following resin composition. The resin composition according to the present disclosure includes a base agent (A) and a curing agent (B). The base agent (A) includes an amino group-containing acrylic resin (a1) as an organic component and a siloxane oligomer (a2) as an inorganic component. The curing agent (B) includes a polyepoxide (b1) and a curing catalyst (b2).

[0020] The amino group-containing acrylic resin (a1) reacts with the polyepoxide (b1) to crosslink and form a first polymer. In the amino group-containing acrylic resin (a1), there is no reactive group (hereinafter referred to as the first reactive group) capable of reacting with a silanol group, or the number of the first reactive groups is less than 11% of the number of amino groups in the amino group-containing acrylic resin (a1). Therefore, the amino group-containing acrylic resin (a1) does not react with the siloxane oligomer (a2), or reacts with little reaction.

[0021] The siloxane oligomer (a2) crosslinks by forming a siloxane bond through self-condensation to form a second polymer. On the other hand, the siloxane oligomer (a2) does not react with the organic component because it does not have a group (typically an epoxy group) that reacts with an amino group or a group (typically an amino group) that reacts with an epoxy group, as described below.

[0022] As described above, the polyepoxide (b1) reacts with the amino group-containing acrylic resin (a1) to crosslink and form a first polymer. Since the polyepoxide (b1) does not have a first reactive group or the number of the first reactive groups is less than 10% of the number of epoxy groups in the polyepoxide (b1), the polyepoxide (b1) does not react or hardly reacts with the siloxane oligomer (a2).

[0023] The curing catalyst (b2) promotes the condensation reaction of the siloxane oligomer (a2) and the reaction between the amino group-containing acrylic resin (a1) and the polyepoxide (b1). Furthermore, when the curing catalyst (b2) is an organometallic compound, the central metal of the organometallic compound is incorporated into the second polymer and fixed. This reduces the catalytic activity of the organometallic compound and stabilizes it. Therefore, the condensation reaction of the siloxane oligomer during outdoor exposure is further suppressed.

[0024] (Amino group-containing acrylic resin (a1)) The amino group-containing acrylic resin (a1) is one of the organic components and contains one or more amino groups. The amino group-containing acrylic resin (a1) reacts with the polyepoxide (b1) to form a first polymer.

[0025] In the amino group-containing acrylic resin (a1), there is no reactive group (first reactive group) capable of reacting with a silanol group, or the number of the first reactive groups is less than 11% of the number of amino groups in the amino group-containing acrylic resin (a1). In this way, the amount of the first reactive groups present in the amino group-containing acrylic resin (a1) is small, so that the amino group-containing acrylic resin (a1) does not react with the siloxane oligomer (a2), or reacts with little reaction.

[0026] The first reactive group may be at least one selected from the group consisting of a hydroxyl group, an alkoxy group, an alkoxysilyl group, and a silanol group.

[0027] The ratio R1 of the number of first reactive groups to the number of amino groups in the amino group-containing acrylic resin (a1) can be calculated from the structural formula of the amino group-containing acrylic resin (a1). The ratio R1 is calculated by dividing the number of first reactive groups in the structural formula by the number of amino groups and multiplying the result by 100.

[0028] The ratio R1 may be calculated from the number of amino groups and the number of first reactive groups obtained by component analysis of the amino group-containing acrylic resin. 1 The number of hydroxyl groups as the first reactive groups is determined by measuring the hydroxyl value of the amino group-containing acrylic resin. The number of alkoxy groups is determined by measuring the peak integral value ratio of the spectrum obtained by H-NMR measurement, or the amine value of the amino group-containing acrylic resin. 1 The number of silanol groups and alkoxysilyl groups is calculated from the peak integral ratio of the spectrum obtained by H-NMR measurement. 1 H-NMR or 29It can be determined from the peak integral ratio of the spectrum obtained by Si-NMR measurement, or the Si concentration obtained by ICP atomic emission spectrometry.

[0029] The amine value can be determined by the following method in accordance with ASTM D2073. (1) Accurately weigh 500 mg of amino group-containing acrylic resin (a1) into a 200 ml Erlenmeyer flask. (2) Add approximately 50 ml of tetrahydrofuran (THF) and dissolve uniformly. (3) Add 5 to 6 drops of indicator (methyl violet solution) and stir evenly. (4) Titrate with 0.2N hydrochloric acid-ethanol solution, and the endpoint is when the solution turns bright green. (The above (3) and (4) may be replaced by potentiometric titration.)

[0030] The ratio R1 may be calculated from the mass ratio and molecular weight of the raw material monomers used in the synthesis of the amino group-containing acrylic resin (a1) by the following formula: In the formula, WR11, WR12... represent the amount (g) of each monomer containing a first reactive group, n11, n12... represent the number of first reactive groups in one monomer molecule, and MR11, MR12 represent the molecular weight of each monomer, WA11, WA12... represent the amount (g) of each monomer containing an amino group, m11, m12... represent the number of amino groups in one monomer molecule, and MA11, MA12... represent the molecular weight of each monomer. TIFF0007576075000003.tif12150

[0031] The ratio R1 may be 10% or less, may be 5% or less, may be 2% or less, or may be 0%.

[0032] The amino group-containing acrylic resin (a1) has an amine value of 8 mgKOH / g or more and 90 mgKOH / g or less. When the amine value is 8 mgKOH / g or more, the number of crosslinking points with the polyepoxide (b1) increases, and the water resistance and weather resistance of the resulting coating film are improved. When the amine value is 90 mgKOH / g or less, excessive crosslinking is suppressed, and a decrease in flexibility is suppressed. The amine value of the amino group-containing acrylic resin (a1) may be 10 mgKOH / g or more, or 12 mgKOH / g or more. The amine value of the amino group-containing acrylic resin (a1) may be 89 mgKOH / g or less, or 36 mgKOH / g or less.

[0033] The weight average molecular weight Mw of the amino group-containing acrylic resin (a1) is, for example, 5,000 or more and 200,000 or less. When the Mw of the amino group-containing acrylic resin (a1) is 5,000 or more, decomposition of the first polymer by ultraviolet light is easily suppressed. When the Mw of the amino group-containing acrylic resin (a1) is 200,000 or less, a decrease in flexibility of the coating film is easily suppressed. The Mw of the amino group-containing acrylic resin (a1) may be 10,000 or more, 20,000 or more, or 25,000 or more. The Mw of the amino group-containing acrylic resin (a1) may be 100,000 or less, 70,000 or less, or 50,000 or less.

[0034] The amino group-containing acrylic resin (a1) is mixed with the siloxane oligomer (a2) as a polymer. The resin composition may contain two or more kinds of amino group-containing acrylic resins (a1). The two or more kinds of amino group-containing acrylic resins (a1) are mixed with the siloxane oligomer (a2) as a polymer, respectively. The two or more kinds of amino group-containing acrylic resins (a1) may be mixed with the siloxane oligomer (a2) as a mixture of two or more polymers.

[0035] The mass ratio of the amino group-containing acrylic resin (a1) to the total solid content of the amino group-containing acrylic resin (a1), the siloxane oligomer (a2) and the polyepoxide (b1) is, for example, 10% by mass or more and 80% by mass or less. When the mass ratio of the amino group-containing acrylic resin (a1) is 10% by mass or more, the characteristics of the first polymer are easily exhibited. When the mass ratio of the amino group-containing acrylic resin (a1) is 80% by mass or less, the characteristics of the second polymer are easily exhibited. The mass ratio of the amino group-containing acrylic resin (a1) may be 20% by mass or more, 30% by mass or more, 40% by mass or more, or 50% by mass or more. The mass ratio of the amino group-containing acrylic resin (a1) may be 77% by mass or less, 73% by mass or less, or 70% by mass or less.

[0036] The amino group may be primary, secondary, or tertiary. The amino group-containing acrylic resin (a1) may have at least one tertiary amino group in one molecule. This increases the crosslink density of the organic component, and improves durability. The number of tertiary amino groups may be two or more, or three or more.

[0037] The amino group-containing acrylic resin (a1) is usually a copolymer of raw material monomers including an amino group-containing polymerizable monomer (m1) and another polymerizable monomer (m2) copolymerizable with the amino group-containing polymerizable monomer (m1). By using a polymerizable monomer containing a tertiary amino group, one or more tertiary amino groups can be introduced into the amino group-containing acrylic resin (a1).

[0038] The amino group-containing polymerizable monomer (m1) may be at least one selected from the group consisting of tertiary amino group-containing monomers such as N,N-dimethylaminoethyl (meth)acrylate (DMAEMA), N,N-diethylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylate, N,N-dimethylaminobutyl (meth)acrylate, and N,N-dimethylaminopropyl (meth)acrylamide; and secondary amino group-containing monomers such as Nt-butylaminoethyl (meth)acrylate. "(Meth)acrylate" is a concept that includes both acrylate and methacrylate.

[0039] Examples of other polymerizable monomers (m2) include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, dodecyl (meth)acrylate, lauryl (meth)acrylate, ) acrylate), tridecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, cyclododecyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, tricyclodecanyl (meth)acrylate, and other alkyl (meth)acrylates; benzyl (meth)acrylate, Aromatic ring-containing polymerizable monomers such as styrene, α-methylstyrene, and vinyltoluene; perfluoroalkyl (meth)acrylates such as perfluorobutylethyl (meth)acrylate and perfluorooctylethyl (meth)acrylate; polymerizable monomers having a fluorinated alkyl group such as fluoroolefin; polymerizable monomers having a photopolymerizable functional group such as a maleimide group; vinyl compounds such as N-vinylpyrrolidone, ethylene, butadiene, chloroprene, vinyl propionate, and vinyl acetate; carboxy group-containing polymerizable monomers such as (meth)acrylic acid, maleic acid, crotonic acid, and β-carboxyethyl acrylate; nitrogen-containing polymerizable monomers such as (meth)acrylonitrile and (meth)acrylamide; epoxy group-containing polymerizable monomers such as glycidyl (meth)acrylate, β-methylglycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, 3,4-epoxycyclohexylethyl (meth)acrylate, 3,4-epoxycyclohexylpropyl (meth)acrylate, and allyl glycidyl ether;Examples of the alkoxy group-containing polymerizable monomer include N-methoxymethyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, alkoxyalkyl (meth)acrylates such as methoxyethyl (meth)acrylate, methoxypropyl (meth)acrylate, ethoxyethyl (meth)acrylate, and ethoxypropyl (meth)acrylate, and polyalkylene glycol monoalkoxy (meth)acrylates such as polyethylene glycol monomethoxy (meth)acrylate; and carbonyl group-containing polymerizable monomers such as acrolein, diacetone acrylamide, diacetone methacrylamide, acetoacetoxyethyl methacrylate, formyl styrene, and vinyl alkyl ketones having 4 to 7 carbon atoms (for example, vinyl methyl ketone, vinyl ethyl ketone, vinyl butyl ketone). The other polymerizable monomers (m2) may be used alone or in combination of two or more.;

[0040] A polymerizable monomer having a first reactive group may be further used as the raw material monomer, provided that the polymerizable monomer containing the first reactive group is used so that the above-mentioned ratio R1 is less than 11%.

[0041] Examples of the polymerizable monomer containing a first reactive group include polymerizable monomers having an alkoxysilyl group, such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(2-methoxyethoxy)silane, γ-(meth)acryloyloxypropyltrimethoxysilane, and γ-(meth)acryloyloxypropyltriethoxysilane; 2-hydroxyethyl(meth)acrylate, 2-hydroxypropyl(meth)acrylate, 3-hydroxypropyl(meth)acrylate, and 4-hydroxybutyl(meth)acrylate. monoesters of (meth)acrylic acid and dihydric alcohols having 2 to 8 carbon atoms, ε-caprolactone-modified products of the monoesters of (meth)acrylic acid and dihydric alcohols having 2 to 8 carbon atoms, other hydroxyl-containing polymerizable monomers such as N-hydroxymethyl(meth)acrylamide, allyl alcohol, (meth)acrylates having a polyoxyethylene chain whose molecular terminal is a hydroxyl group, and silanol-containing polymerizable monomers such as dimethylvinylsilanol and methylphenylvinylsilanol. The monomers having a first reactive group may be used alone or in combination of two or more.

[0042] (Polyepoxide (b1)) The polyepoxide (b1) is one of the organic components and has at least two epoxy groups (oxirane rings) in one molecule. The polyepoxide (b1) reacts with the amino group-containing acrylic resin (a1) to form a first polymer.

[0043] In the polyepoxide (b1), there is no first reactive group capable of reacting with the above-mentioned silanol group, or the number of the first reactive groups is less than 10% of the number of epoxy groups in the polyepoxide (b1). In this way, the amount of the first reactive groups present in the polyepoxide (b1) is small, so that the polyepoxide (b1) does not react with the siloxane oligomer (a2) or reacts with the siloxane oligomer (a2) with difficulty.

[0044] The ratio R2 of the number of first reactive groups to the number of epoxy groups in the polyepoxide (b1) can be determined from the structural formula of the polyepoxide (b1). The ratio R2 is calculated by dividing the number of first reactive groups in the structural formula by the number of epoxy groups and multiplying the result by 100.

[0045] The ratio R2 may be calculated from the number of epoxy groups and the number of first reactive groups obtained by component analysis of the polyepoxide. 1 It is obtained by measuring the peak integral ratio of the spectrum obtained by H-NMR measurement, or the epoxy equivalent of the polyepoxide. The number of the first reactive groups is obtained in the same manner as above. The epoxy equivalent is obtained, for example, in accordance with JIS K 7236:2001.

[0046] The ratio R2 may be calculated from the mass ratio and molecular weight of the raw material monomers used in the synthesis of polyepoxide (b1) by the following formula: In the formula, WR21, WR22... represent the amount (g) of each monomer containing a first reactive group, n21, n22... represent the number of first reactive groups in one monomer molecule, and MR21, MR22 represent the molecular weight of each monomer, WE11, WE12... represent the amount (g) of each monomer containing an epoxy group, m21, m22... represent the number of epoxy groups in one monomer molecule, and ME11, ME12... represent the molecular weight of each monomer. TIFF0007576075000004.tif12150

[0047] The ratio R2 may be 9.5% or less, may be 5% or less, may be 2% or less, or may be 0%.

[0048] The polyepoxide (b1) has an epoxy equivalent of 100 g / eq or more and 1,500 g / eq or less. When the epoxy equivalent is 100 g / eq or more, the number of crosslinking points with the amino group-containing acrylic resin (a1) increases, and the water resistance and weather resistance of the resulting coating film are improved. When the epoxy equivalent is 1,500 g / eq or less, excessive crosslinking is suppressed, and a decrease in flexibility is suppressed. The epoxy equivalent of the polyepoxide (b1) may be 120 g / eq or more, or 130 g / eq or more. The epoxy equivalent of the polyepoxide (b1) may be 1,450 g / eq or less, 500 g / eq or less, or 400 g / eq or less.

[0049] The weight average molecular weight Mw of the polyepoxide (b1) is, for example, 200 or more and 100,000 or less. When the Mw of the polyepoxide (b1) is 200 or more, decomposition of the first polymer by ultraviolet light is easily suppressed. When the Mw of the polyepoxide (b1) is 100,000 or less, a decrease in flexibility of the coating film is easily suppressed. The Mw of the polyepoxide (b1) may be 250 or more. The Mw of the polyepoxide (b1) may be 50,000 or less, or 30,000 or less.

[0050] The mass ratio of the polyepoxide (b1) to the total solid content of the amino group-containing acrylic resin (a1), the siloxane oligomer (a2) and the polyepoxide (b1) is, for example, 0.8 mass% or more and 80 mass% or less. When the mass ratio of the polyepoxide (b1) is 0.8 mass% or more, the properties of the first polymer are easily exhibited. When the mass ratio of the polyepoxide (b1) is 80 mass% or less, the properties of the second polymer are easily exhibited. The mass ratio of the polyepoxide (b1) may be 1.0 mass% or more. The mass ratio of the polyepoxide (b1) may be 60 mass% or less, 40 mass% or less, 20 mass% or less, 18 mass% or less, or 5 mass% or less.

[0051] The polyepoxide (b1) may have at least one glycidyl group in one molecule. The number of glycidyl groups in one molecule of the polyepoxide (b1) may be 2 or more. All of the epoxy groups in one molecule of the polyepoxide (b1) may be glycidyl groups.

[0052] Examples of the polyepoxide (b1) include glycidyl group-containing acrylic resins, glycidyl ether-type polyepoxides, glycidyl ester-type polyepoxides, glycidyl amine-type polyepoxides, and alicyclic polyepoxides. Among them, in terms of flexibility and weather resistance, glycidyl group-containing acrylic resins and glycidyl ether-type polyepoxides may be used.

[0053] The glycidyl group-containing acrylic resin is a copolymer of raw material monomers including an epoxy group-containing polymerizable monomer and another polymerizable monomer copolymerizable with the epoxy group-containing polymerizable monomer. A specific example of the epoxy group-containing polymerizable monomer is given as one of the raw material monomers of the amino group-containing acrylic resin (a1). The epoxy group-containing polymerizable monomer is used alone or in combination of two or more kinds. A specific example of the other polymerizable monomer is the raw material monomer of the amino group-containing acrylic resin (a1) other than the epoxy group-containing polymerizable monomer. The other polymerizable monomer is used alone or in combination of two or more kinds. However, the polymerizable monomer containing the first reactive group is used so that the above ratio R2 is less than 10%.

[0054] Examples of glycidyl ether type polyepoxides include ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, trimethylolpropane polyglycidyl ether, glycerol polyglycidyl ether, diglycerol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, and sorbitol polyglycidyl ether.

[0055] Examples of the glycidyl ester type polyepoxides include diglycidyl phthalate, diglycidyl tetrahydrophthalate, diglycidyl hexahydrophthalate, diglycidyl-p-oxybenzoate, glycidyl ether-glycidyl ester of salicylic acid, and glycidyl ester of dimer acid.

[0056] Examples of the glycidylamine type polyepoxide include triglycidyl isocyanurate, N,N'-diglycidyl derivatives of cyclic alkylene ureas, N,N,O-triglycidyl derivatives of p-aminophenol, and N,N,O-triglycidyl derivatives of m-aminophenol.

[0057] Examples of alicyclic polyepoxides include 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, 3,4-epoxy-2-methylcyclohexylmethyl-3,4-epoxy-2-methylcyclohexanecarboxylate, bis(3,4-epoxycyclohexyl)adipate, bis(3,4-epoxycyclohexylmethyl adipate, bis(3,4-epoxy-6-methylcyclohexylmethyl)adipate, 2-(3,4-epoxycyclohexyl-5,5-spiro-3,4-epoxycyclohexanone-meta-dioxane, and bis(2,3-epoxycyclopentyl)ether.

[0058] The resin composition may contain two or more polyepoxides (b1).

[0059] (Siloxane oligomer (a2)) The siloxane oligomer (a2) is an inorganic component that self-condenses to form a second polymer.

[0060] The siloxane oligomer (a2) is represented by the following general formula (x): [ka] (In the formula, R 3 represents independently in each structural unit a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a single bond, R 4 represents independently in each structural unit an alkyl group having 1 to 5 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aralkyl group having 7 to 15 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or -O-; m is an integer from 0 to 200. and a structural unit X represented by the following general formula (y): [ka] (In the formula, R 5 and R 6 each independently in each repeating unit represents an alkyl group having 1 to 5 carbon atoms, an aryl group having 6 to 10 carbon atoms, or an aralkyl group having 7 to 15 carbon atoms; n is an integer from 0 to 200. A structural unit Y represented by The terminal group has at least one selected from the group consisting of a hydrogen atom, a hydroxyl group, an alkyl group having 1 to 5 carbon atoms, and an alkoxy group having 1 to 5 carbon atoms.

[0061] As can be understood from the above general formulas (x) and (y), the siloxane oligomer (a2) does not have a second reactive group (typically an amino group) that reacts with an epoxy group and a third reactive group (typically an epoxy group) that reacts with an amino group. Therefore, the reaction between the siloxane oligomer (a2) and the amino group-containing acrylic resin (a1) and the polyepoxide (b1) is further suppressed. Examples of the second reactive group include an amino group and a carboxy group. Examples of the third reactive group include an epoxy group and a halogen group.

[0062] m+n is an integer of 2 to 200. When m+n is 2 or more, the second polymer exhibits its properties as an inorganic component. When m+n is 200 or less, the molecular weight of the second polymer is prevented from becoming excessively large, and the second polymer is easily mixed with the first polymer, improving compatibility. m+n may be 3 or more, or 5 or more. m+n may be 150 or less, 60 or less, or 30 or less.

[0063] m+n is determined from the weight average molecular weight of the siloxane oligomer (a2) and the ratio of the structural units X and Y constituting the polymer and their molecular weights. The weight average molecular weight can be measured, for example, by gel permeation chromatography (GPC). The ratio of the structural units X and Y constituting the polymer and their molecular weights can be determined by the formulation or 29 It can be calculated from the peak integral value of the spectrum obtained by Si-NMR measurement.

[0064] The resin composition may contain two or more kinds of siloxane oligomers (a2). In this case, m+n is calculated as the average value of the mixture of two or more kinds of siloxane oligomers.

[0065] When m≧1, the siloxane oligomer (a2) has at least a structural unit X. In the structural unit X, R 3 When R is a single bond, the siloxane oligomer (a2) has a branched three-dimensional structure. 3 The oxygen atom bonded to is bonded to a Si atom of another structural unit X.

[0066] When m≧1, the siloxane oligomer (a2) has at least a structural unit X. In the structural unit X, R 4 When R is -O-, the siloxane oligomer (a2) has a branched three-dimensional structure. 4 The oxygen atom of is bonded to the Si atom of another structural unit X.

[0067] When n≧1, the siloxane oligomer (a2) has at least a structural unit Y. When n≧1 and m=0, the siloxane oligomer (a2) has a linear structure.

[0068] In the non-terminal structural unit X, R 3 is a single bond and R 4 When m is -O-, each of the four bonds of the Si atom can be bonded to an oxygen atom. Such a Si atom is said to be tetrafunctional. When m≧1, the siloxane oligomer (a2) can contain a structural unit having a tetrafunctional Si atom (hereinafter, sometimes referred to as a Q unit). The siloxane oligomer (a2) containing a Q unit can be obtained by using a silane compound having a Si atom bonded to four alkoxy groups (e.g., carbon number 1 to 5) as one of the raw material monomers.

[0069] In the non-terminal structural unit X, R 3 is a single bond or R 4 When m is -O-, three of the bonds of the Si atom can be bonded to an oxygen atom. Such a Si atom is said to be trifunctional. When m≧1, the siloxane oligomer (a2) can contain a structural unit having a trifunctional Si atom (hereinafter, sometimes referred to as a T unit). The siloxane oligomer (a2) containing a T unit can be obtained by using a silane compound having a Si atom bonded to three alkoxy groups (e.g., carbon number 1 to 5) as one of the raw material monomers.

[0070] In the structural unit Y that is not at a terminal, two of the bonds of the Si atom can be bonded to an oxygen atom. Such a Si atom is called bifunctional. When n≧1, the siloxane oligomer (a2) can contain a structural unit having a bifunctional Si atom (hereinafter, sometimes referred to as a D unit). The siloxane oligomer (a2) containing a D unit can be obtained by using a silane compound having a Si atom bonded to two alkoxy groups (e.g., carbon number 1 to 5) as one of the raw material monomers.

[0071] In the structural unit Y at the terminal, one of the bonds of the Si atom may be bonded to an oxygen atom. Such a Si atom is called monofunctional. When n≧1, the siloxane oligomer (a2) may contain a structural unit having a monofunctional Si atom (hereinafter, sometimes referred to as an M unit). The Si atom in the M unit is bonded to an alkyl group having 1 to 5 carbon atoms as a terminal group.

[0072] In the siloxane oligomer (a2), n / (m+n) is 0.19 or more (n / (m+n)≧0.19). n is the repeat number of the structural unit Y. As described above, the structural unit Y is a structural unit having a bifunctional Si atom (D unit) or a structural unit having a monofunctional Si atom (M unit). m is the repeat number of the structural unit X. As described above, the structural unit X is a structural unit having a tetrafunctional Si atom (Q unit) or a structural unit having a trifunctional Si atom (T unit). When the ratio of the number of D units and / or M units is 19% or more of the total number of Q, T, D, and M units, the formation of a branched three-dimensional structure is suppressed when the siloxane oligomer (a2) self-condenses, and the structure is likely to be close to linear. Therefore, the second polymer formed becomes flexible, and the impact resistance of the coating film is improved.

[0073] n / (m+n) may be 0.20 or more, or 0.25 or more. n / (m+n) may be 1.5 or less, or 1.2 or less, or 1.0 or less.

[0074] n / (m+n) is calculated in the same manner as (m+n).

[0075] The mass ratio of the siloxane oligomer (a2) to the total solid content of the amino group-containing acrylic resin (a1), the siloxane oligomer (a2) and the polyepoxide (b1) is, for example, 10% by mass or more and 90% by mass or less. When the mass ratio of the siloxane oligomer (a2) is 10% by mass or more, the properties of the second polymer are easily exhibited. When the mass ratio of the siloxane oligomer (a2) is 90% by mass or less, the properties of the first polymer are easily exhibited. The mass ratio of the siloxane oligomer (a2) may be 15% by mass or more, 20% by mass or more, or 25% by mass or more. The mass ratio of the siloxane oligomer (a2) may be 70% by mass or less, 50% by mass or less, or 40% by mass or less.

[0076] (Curing catalyst (b2)) The curing catalyst (b2) promotes the condensation reaction of the siloxane oligomer (a2) and the reaction of the amino group-containing acrylic resin (a1) with the polyepoxide (b1).

[0077] Examples of the curing catalyst (b2) include organometallic compounds, aliphatic amines, amine catalysts, metal (e.g., lead, tin, zinc) complexes of carboxylic acids, and boric acid compounds. These may be used alone or in combination of two or more.

[0078] Examples of the organometallic compounds include organotin compounds such as diacetyltin diacetate, dibutyltin dilaurate, dibutyltin diacetate, dioctyltin dilaurate, diacetyltin dioctoate, tin octoate, dibutyltin diacetate, and dibutyltin dioctoate; organoaluminum compounds such as aluminum trimethoxide, aluminum tris(acetylacetonate), aluminum tri-n-butoxide, aluminum tris(ethyl acetoacetate), aluminum diisopropoxy(ethyl acetoacetate), and aluminum acetylacetonate; and titanium tetraacetate. Examples of suitable organic titanium compounds include titanium tetra(monoethyl ethoxide), titanium tetra(monoethyl ethoxide), titanium tetra(monobutyl ethoxide), titanium tetrakis(acetylacetonate), and tetra normal butyl titanate; organic zirconium compounds include zirconium tetra(monomethyl ethoxide), zirconium tetra(monoethyl ethoxide), zirconium tetra(monobutyl ethoxide), zirconium normal propylate, zirconium normal butylate, and zirconium tetrakis(acetylacetonate); and organic zinc compounds include zinc naphthenate.

[0079] Examples of aliphatic amines include trimethylamine, triethylamine, 2-(dimethylamino)ethyl methacrylate, 1,4-diazabicyclo[2.2.2]octane, 1,8-diazabicyclo[5.4.0]-7-undecene, 1,5-diazabicyclo[4.3.0]-5-nonene, 1-methylpiperidine, and 1-methylpyrrolidine.

[0080] Examples of the amine catalyst include pyridine, 4-dimethylaminopyridine, 4-(1-piperidyl)pyridine, N-methylimidazole, and N,N-dimethylaniline.

[0081] Examples of the boric acid compound include boric acid esters such as trimethyl borate, triethyl borate, tripropyl borate, tributyl borate, triphenyl borate, tri(4-chlorophenyl) borate, and trihexafluoroisopropyl borate.

[0082] The curing catalyst (b2) may be an organometallic compound. The organometallic compound promotes the condensation reaction of the siloxane oligomer (a2), and the central metal is incorporated and fixed in the second polymer. This reduces the catalytic action of the organometallic compound and stabilizes it. Therefore, the condensation reaction of the siloxane oligomer during outdoor exposure is further suppressed.

[0083] The mass ratio of the curing catalyst (b2) to the total solid content of the amino group-containing acrylic resin (a1), the siloxane oligomer (a2) and the polyepoxide (b1) may be 0.1 mass% or more and 30 mass% or less. The mass ratio of the curing catalyst (b2) may be 0.5 mass% or more and 1 mass% or more. The mass ratio of the curing catalyst (b2) may be 10 mass% or less and 8 mass% or less.

[0084] The weight average molecular weight Mw of the amino group-containing acrylic resin (a1), the siloxane oligomer (a2) and the polyepoxide (b1) can be measured using GPC (e.g., Tosoh Corporation, product name: HLC-8220GPC column, Tosoh Corporation, product names: TSK-GEL SUPER HZM-H, TSK-GEL SUPER HZ3000, TSK-GEL SUPER HZ2000) using tetrahydrofuran or chloroform as a solvent, and can be calculated in terms of polystyrene.

[0085] [paint] The present disclosure includes a coating material containing the above-mentioned resin composition. According to the coating material of the present disclosure, a coating film that suppresses crack generation in outdoor environments and has excellent impact resistance can be obtained. Therefore, the coating material of the present disclosure is suitable for coating of objects that are mainly used or installed outdoors. Examples of such objects include bridges, buildings, tanks, plants, towers, roads, tunnels, ships, vehicles, and roofs. Examples of the material of the object include metals (e.g., steel such as steel plate, zinc plating, stainless steel, and aluminum), ceramic materials (e.g., concrete, mortar, slate, slate), plastics, vinyl sheets, paper, wood, and glass.

[0086] (Organic solvent) The paint may contain a third-class organic solvent as specified in the Industrial Safety and Health Act. Third-class organic solvents are also called weak solvents and generally have low dissolving power. The third-class organic solvent adjusts the paint to a desired viscosity. The solid content of the paint is appropriately set depending on the application, coating method, etc.

[0087] Class 3 organic solvents include gasoline, coal tar naphtha (including solvent naphtha), petroleum ether, petroleum naphtha, petroleum benzine, turpentine oil, and mineral spirits (including mineral thinner, petroleum spirits, white spirits, and mineral turpentine). These may be used alone or in combination of two or more.

[0088] The paint may contain organic solvents other than the third organic solvent. Examples of other organic solvents include hydrocarbon solvents such as n-butane, n-hexane, n-heptane, n-octane, cyclopentane, cyclohexane, and cyclobutane; aromatic solvents such as toluene and xylene; ethylene glycol monoisopropyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol mono-n-butyl ether, ethylene glycol mono-t-butyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, propylene glycol mono-n-butyl ether, and propylene glycol monomethyl ether. Examples of the solvent include ether solvents such as glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, and dioxane; ester solvents such as methyl acetate, ethyl acetate, n-butyl acetate, isobutyl acetate, methyl acetoacetate, ethylene glycol monomethyl ether acetate, and butyl carbitol acetate; ketone solvents such as acetone, acetylacetone, diacetone alcohol, methyl ethyl ketone, methyl isobutyl ketone, and diisobutyl ketone; and alcohol solvents such as methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, isobutanol, and n-pentanol. These may be used alone or in combination of two or more.

[0089] (Pigments) The paint may contain a pigment. Examples of the pigment include color pigments, anti-rust pigments, and extender pigments. These may be used alone or in combination of two or more.

[0090] (Additives) The coating material may contain various additives as necessary. Examples of the additives include ultraviolet absorbers, viscosity modifiers, antioxidants, defoamers, surface conditioners, pinhole inhibitors, silane coupling agents, and pigment dispersants. These may be used alone or in combination of two or more.

[0091] <Second compound> It is desirable that the second compound containing both the first reactive group and the second reactive group in one molecule is not contained in the resin composition and the coating material, or the content thereof is small. The mass ratio of the second compound to the total solid content of the amino group-containing acrylic resin (a1), the siloxane oligomer (a2) and the polyepoxide (b1) may be 1 mass% or less, 0.8 mass% or less, 0.5 mass% or less, or 0 mass%.

[0092] Examples of the second compound include an amino group-containing silane coupling agent and a carboxy group-containing silane coupling agent.

[0093] In order to have little effect on the reactivity between the amino group-containing acrylic resin (a1) and the polyepoxide (b1), the number of second reactive groups in the second compound may be less than 11% of the number of amino groups in the amino group-containing acrylic resin (a1).

[0094] The ratio R3 of the number of second reactive groups in the second compound to the number of amino groups in the amino group-containing acrylic resin (a1) can be determined in the same manner as the ratio R1.

[0095] When the ratio R3 is calculated using the mass ratio and molecular weight of the raw material monomers used in the synthesis of the amino group-containing acrylic resin (a1), the following formula can be referred to. In the formula, WR31, WR32... represent the respective amounts (g) of the second compounds, n31, n32... represent the number of second reactive groups in one molecule of the second compound, and MR31, MR32 represent the respective molecular weights of the second compounds. WA11, WA12..., m11, m12..., MA11, MA12... are the same as the formula for calculating the ratio R1. TIFF0007576075000007.tif12150

[0096] <Third compound> It is desirable that the third compound containing both the first reactive group and the third reactive group in one molecule is not contained in the resin composition and the coating material, or the content thereof is small. The mass ratio of the third compound to the total solid content of the amino group-containing acrylic resin (a1), the siloxane oligomer (a2) and the polyepoxide (b1) may be 1 mass% or less, 0.8 mass% or less, 0.5 mass% or less, or 0 mass%.

[0097] Examples of the third compound include an epoxy-containing silane coupling agent and a halogen-containing silane coupling agent.

[0098] The number of third reactive groups in the third compound may be less than 10% of the number of epoxy groups in the polyepoxide (b1), since this has little effect on the reactivity between the amino group-containing acrylic resin (a1) and the polyepoxide (b1).

[0099] The ratio R4 of the number of third reactive groups in the third compound to the number of epoxy groups in the polyepoxide (b1) can be determined in the same manner as the ratio R1.

[0100] When the ratio R4 is calculated using the mass ratio and molecular weight of the raw material monomers used in the synthesis of the polyepoxide (b1), the following formula can be referred to. In the formula, WR41, WR42... represent the respective amounts (g) of the third compounds, n41, n42... represent the number of third reactive groups in one molecule of the third compound, and MR41, MR42 represent the respective molecular weights of the third compounds. WE11, WE12..., m21, m22..., ME11, ME12... are the same as the formula for calculating the ratio R2. TIFF0007576075000008.tif12150

[0101] <4th compound> The resin composition and the coating material do not contain any of the first, second, and third reactive groups, and may contain a fourth compound other than the amino group-containing acrylic resin (a1), the siloxane oligomer (a2), and the polyepoxide (b1). The resin composition and the coating material do not have to contain a fourth compound.

[0102] The mass proportion of the fourth compound to the total solid content of the amino group-containing acrylic resin (a1), the siloxane oligomer (a2) and the polyepoxide (b1) may be 30 mass% or less, 10 mass% or less, 5 mass% or less, or 0 mass%.

[0103] Examples of the fourth compound include olefin resins, urethane resins, and fluororesins.

[0104] (Paint preparation method) The coating material according to the present disclosure can be prepared by a method commonly used by those skilled in the art. The base agent (A) is prepared by mixing the above-mentioned amino group-containing acrylic resin (a1) and siloxane oligomer (a2) with other components as necessary. The curing agent (B) is separately prepared by mixing at least the above-mentioned polyepoxide (b1) and curing catalyst (b2) with other components as necessary. The coating material is prepared by mixing the base agent (A) and curing agent (B) with other components as necessary. For mixing, a commonly used mixing device such as a paint shaker or mixer is used.

[0105] (Painting method) The coating method is appropriately selected depending on the shape of the object to be coated, etc. Examples of the coating method include brush coating, roller coating, spray coating, and flow coating.

[0106] [Paint film] A coating film obtained from the resin composition or paint of the present disclosure comprises a first polymer portion formed by a reaction product of an amino group-containing acrylic resin (a1) and a polyepoxide (b1), and a second polymer portion formed by a polymer of a siloxane oligomer (a2) (or a polymer of a siloxane oligomer (a2) containing a curing catalyst (b2); the same applies below).

[0107] The first polymer portion is an organic component and is formed by the first polymer. The second polymer portion is an inorganic component and is formed by the second polymer. The coating film has a gloss retention of 80% or more according to JIS K5659 7.21 after an outdoor exposure test in Miyakojima, facing the equatorial plane at an angle of 20° to the horizontal plane, for one and a half years according to JIS K5600-7-6. Furthermore, the first and second polymer portions are substantially independent of each other. Therefore, the coating film can exhibit both the properties of an organic component (e.g., flexibility) and the properties of an inorganic component (e.g., resistance to ultraviolet light and heat). This suppresses the occurrence of cracks in an outdoor environment.

[0108] The first and second polymer parts are formed in the same system, although they are substantially independent of each other. Therefore, the two polymer parts are at least partially entangled with each other, and the first polymer part and the second polymer part are compatible without being separated. Therefore, the properties of the organic component and the inorganic component are exhibited throughout the entire coating film, not only partially, and the durability and impact resistance of the coating film are further improved. Furthermore, the appearance of the resulting coating film is also improved. The two polymer parts are entangled with each other, for example, in a mesh-like shape. The formed network structure may be a semi-interpenetrating polymer network or an interpenetrating polymer network.

[0109] According to the Glossary of Fundamental Terms in Polymer Science by the International Union of Pure and Applied Chemistry (IUPAC) Commission on Macromolecular Nomenclature, a "semi-interpenetrating polymer network (SIPN)" is "a polymer (see Definition 2.2) consisting of one or more networks (see Definition 1.58) and one or more linear (see Definition 1.32) or branched polymers (see Definition 1.33), at least some of the linear or branched polymers penetrating at least one of the networks on a molecular scale." "(Note) Semi-interpenetrating polymer networks are distinguished from interpenetrating polymer networks because, in principle, the constituent linear or branched polymers can be separated from the constituent polymer networks without breaking chemical bonds. That is, semi-interpenetrating polymer networks are polymer blends."

[0110] Similarly, an "interpenetrating polymer network (IPN)" is "a polymer (see Definition 2.2) in which two or more networks (see Definition 1.58) are at least partially interwoven on the molecular scale and are not covalently connected to one another but cannot be separated without breaking chemical bonds." Note: "A mixture of two or more preformed polymer networks is not an IPN."

[0111] The compatibility of the first polymer portion and the second polymer portion can be confirmed, for example, by the Tg of the coating film, the number of peaks of the loss tangent (tan δ) of the coating film, or a transmission electron microscope (TEM) image of the coating film surface. (Method 1) When the Tg of the coating film is a value between Tg1 of the coating film formed only from the first polymer and Tg2 of the coating film formed only from the second polymer, and the number of tan δ peaks is one, or (Method 2) When no sea-island structure is confirmed in the TEM image, the first polymer portion and the second polymer portion can be considered to be compatible. The compatibility of the first polymer portion and the second polymer portion may be confirmed by at least one of the above two methods.

[0112] Tan δ is measured in accordance with the tensile vibration non-resonant method of JIS-K7244-4:1999. The measurement is performed under conditions of a temperature rise rate of 2°C / min and a frequency of 8 Hz. Tan δ can be measured using a dynamic viscoelasticity measuring device (for example, manufactured by UBM Corporation, product name: Rheogel E-4000).

[0113] Tangent delta is used as an index of Tg. In a graph with temperature on the horizontal axis and tan delta on the vertical axis, the temperature at which tan delta reaches its peak is regarded as Tg.

[0114] The thickness of the coating film is appropriately set depending on the type of substrate, the environment of use, etc. The dry thickness of the coating film is, for example, 20 μm or more and 1,000 μm or less.

[0115] In one embodiment, a coating film formed by the paint resin composition according to the present disclosure comprises a first polymer portion formed by a reaction product of an amino group-containing acrylic resin (a1) and a polyepoxide (b1), and a second polymer portion formed by a polymer of a siloxane oligomer (a2) polymerized in the presence of a curing catalyst (b2) containing an organometallic compound and independent of the first polymer portion, wherein at least a portion of the first polymer portion and at least a portion of the second polymer portion are entangled, and the second polymer portion contains a metal derived from the organometallic compound. EXAMPLES

[0116] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples. In the examples, "parts" and "%" are based on mass unless otherwise specified.

[0117] [Synthesis example of amino group-containing acrylic resin (a1)] A reaction vessel equipped with a thermometer, a thermostat, a stirrer, a reflux condenser and a dropping device was charged with 35 parts of a third organic solvent (A Solvent (trade name), manufactured by ENEOS Corporation), and the temperature was raised to 115°C while aerating nitrogen gas. Separately, a monomer mixture was prepared by mixing the raw material monomers shown in Table 1. In addition, an initiator mixture was prepared by mixing 1.5 parts of t-butylperoxy-2-ethylhexanoate (polymerization initiator) and 18 parts of A Solvent. The monomer mixture and the initiator mixture were dropped in parallel into the reaction vessel over a period of 3 hours. After the reaction was carried out by a standard method, the resin solid content was adjusted to 65% with A Solvent. In this way, an amino group-containing acrylic resin (a1) Ac1 was obtained.

[0118] Details of the monomers in Table 1 are as follows: ·DMAEMA: N,N-Dimethylaminoethyl methacrylate MMA: Methyl methacrylate ·NBA: normal butyl methacrylate IBMA: Isobutyl methacrylate ·EHA: 2-Ethylhexyl acrylate

[0119] [Table 1]

[0120] [Synthesis example of polyepoxide (b1) Ep2] A reaction vessel equipped with a thermometer, a thermostat, a stirring device, a reflux condenser and a dropping device was charged with 94 parts of A solvent, and the temperature was raised to 130°C under stirring while passing nitrogen gas through. Separately, the raw material monomers shown in Table 2 were mixed to prepare a monomer mixture. In addition, 6.16 parts of t-butylperoxy-2-ethylhexanoate and 7 parts of A solvent were mixed to prepare an initiator mixture. The monomer mixture and the initiator mixture were dropped in parallel into the reaction vessel over a period of 3 hours. After the reaction was carried out by a standard method, the solid content was adjusted to 50% with A solvent. In this way, polyepoxide (b1) Ep2 was obtained.

[0121] Details of the monomers in Table 2 are as follows: EMA: Ethyl methacrylate ·HEMA: Hydroxyethyl methacrylate EHMA: 2-Ethylhexyl methacrylate GMA: Glycidyl methacrylate ·NBA: n-Butyl acrylate

[0122] [Table 2]

[0123] [Synthesis examples of siloxane oligomers (a2) S1 to S6] A silane compound shown in Table 3 and 10 parts of methanol were added and mixed in a reaction vessel equipped with a thermometer, a thermostat, a stirrer, a reflux condenser, and a dropping device. Then, a mixture of ion-exchanged water in the amount shown in Table 3 and 0.78 parts of sulfuric acid was dropped into the reaction vessel over a period of 1 hour while the temperature was raised to 65°C. The reaction was carried out for 4.5 hours while maintaining the temperature at 65°C. After the reaction was completed, the solvent was removed under reduced pressure (100 Torr) to obtain siloxane oligomers (a2) S1 to S6.

[0124] n and m+n were calculated from the weight average molecular weight Mw of the siloxane oligomer (a2) and the amounts of the silane compounds 1 to 4 charged.

[0125] Details of the silane compounds in Table 3 are as follows: Silane compound 1: Methyltrimethoxysilane Silane compound 2: Dimethyldimethoxysilane Silane compound 3: Phenyltrimethoxysilane Silane compound 4: Diphenyldimethoxysilane

[0126] [Table 3]

[0127] [Example 1] The base resin and curing agent prepared as described below were mixed to obtain a coating material.

[0128] (1) Preparation of the base agent Half of 31.11 parts of amino group-containing acrylic resin (a1) Ac1, 33.42 parts of titanium oxide (product name: CR-95, Ishihara Sangyo Kaisha, Ltd., pigment), and 20.31 parts of A-solvent were charged into a tin container and stirred for about 30 minutes. The contents were transferred to a dispersion vessel, and an appropriate amount of glass beads were charged, and then mixed with a sand grinding mill at 2000 rpm for about 1 hour. After removing the glass beads, the remaining amount of amino group-containing acrylic resin (a1) Ac1 and 10.65 parts of siloxane oligomer (a2) S3 were added to the obtained white dispersion paste, and mixed for 15 minutes. In this way, the main agent was obtained.

[0129] (2) Preparation of hardener 0.47 parts of polyepoxide (b1) Ep1 (trade name: Epolite 70P, Kyoeisha Chemical Co., Ltd., glycidyl ether type, epoxy equivalent 142, weight average molecular weight 284, ratio R2: 0%), 2.5 parts of dibutyltin dilaurate (curing catalyst (b2)), and 4.1 parts of A solvent were charged into a tin container and mixed with a disperser for about 15 minutes. In this way, a curing agent was obtained.

[0130] [Examples 2-4, Comparative Example 1] The base resin and the curing agent were obtained in the same manner as in Example 1, except that the amounts of each component were changed as shown in Table 4.

[0131] [Example 5] Except for not adding titanium oxide, the base agent and the curing agent were obtained in the same manner as in Example 2. In preparing the base agent, 68.18 parts of the amino group-containing acrylic resin (a1) Ac1 and 23.35 parts of the siloxane oligomer (a2) S4 were charged in a tin container and stirred for about 30 minutes.

[0132] [Reference example 1] A base resin and a curing agent were prepared in the same manner as in Example 1, except that the siloxane oligomer (a2) S2 was used, and a coating material was obtained.

[0133] [Reference example 2] A base resin and a curing agent were prepared in the same manner as in Example 5, except that the siloxane oligomer (a2) S2 was used, and a coating material was obtained.

[0134] [evaluation] The obtained base agent and curing agent were mixed to obtain a paint, and test panels were prepared using the paint, and the following evaluations were performed. The evaluation results are shown in Table 4. The test panels were prepared as follows.

[0135] (Preparation of test panels) The paint was applied to an aluminum-treated plate (A1050P Alodine #1200, 150 mm x 70 mm x 0.8 mm) using a doctor blade (coating thickness 10 mil), and then cured for 7 days under conditions of 23°C and 50% RH to obtain a test plate.

[0136] The initial 60 degree specular gloss of the coating films using the coating materials of the Examples, Comparative Examples and Reference Examples, measured in accordance with JIS K5600-4-7, was 70 to 85.

[0137] (i) Gloss retention after outdoor exposure test The test panels were installed in Miyakojima, facing south (equatorial plane) at an angle of 20° to the horizontal plane for one and a half years in accordance with JIS K5600-7-6. After that, the gloss retention of the coating was evaluated in accordance with JIS K5659 7.21.

[0138] (ii) Suppression of microcracks after outdoor exposure tests After the outdoor exposure test, the surface of the coating film on the test plate was visually observed and evaluated according to the following criteria. Good: No microcracks observed Poor: Microcracks are observed

[0139] (iii) Resistance to falling weights A weight drop test was performed on the test plate in accordance with JIS K5659 7.13, varying the weight and / or the height from which the weight was dropped. The coating film was visually observed for cracks and peeling due to impact deformation, and was evaluated according to the following criteria.

[0140] JIS K5659 7.13 specifies that the weight mass is 300g±1g and the height from which the weight is dropped is 500mm. Tests were started using a load significantly smaller than the JIS standard, and the load was increased stepwise in accordance with the following criteria. When cracks in the coating were confirmed with a load of 500g and a drop height of 500mm, but no cracks in the coating were confirmed with a load of 300g and a drop height of 500mm, the test was judged to be "good."

[0141] Best: No cracks or peeling of the coating film is observed even when a load significantly greater than the JIS standard (mass 500g, drop height 500mm) is applied. Good: No cracks or peeling of the coating film is observed even when a load according to the JIS standard (mass 300g, drop height 500mm) is applied. Poor: No cracks or peeling of the coating was observed when a load smaller than the JIS standard (mass 300g, drop height 300mm) was applied. Worst case: Cracks and peeling of the coating were observed when a load smaller than the JIS standard (mass 300g, drop height 300mm) was applied.

[0142] [Table 4]

[0143] The coating films of Examples 1 to 5 all had excellent resistance to falling weight. This is believed to be due to the fact that the flexibility of the second polymer portion was increased because the siloxane oligomer (a2) of Examples 1 to 5 had a large n / (m+n). Furthermore, the occurrence of cracks was suppressed in all of the coating films of Examples 1 to 5. This is believed to be due to the fact that the functions of both the first polymer and the second polymer were fully exerted, as can be seen from the fact that the gloss retention rate of the coating films after the outdoor exposure test was 80% or more.

[0144] The coating film of Comparative Example 1 showed microcracks in the outdoor exposure test. This is believed to be because the proportion of the first reactive group in the polyepoxide (b1) Ep2 was high, and it reacted with the siloxane oligomer (a2), preventing the flexibility provided by the organic component, resulting in the microcracks. Furthermore, the resistance to a falling weight was also poor. This is believed to be because, since n / (m+n)=0 in the siloxane oligomer (a2), crosslinking proceeded excessively, making the formed second polymer portion hard and brittle.

[0145] In both of the coating films of Reference Examples 1 and 2, the occurrence of cracks was suppressed, but the resistance to the falling weight was insufficient compared to the Examples.

[0146] The present invention includes the following aspects. [1] Contains a base agent (A) and a hardener (B), The main component (A) contains an amino group-containing acrylic resin (a1) and a siloxane oligomer (a2), The curing agent (B) contains a polyepoxide (b1) and a curing catalyst (b2), The amino group-containing acrylic resin (a1) has an amine value of 8 mgKOH / g or more and 90 mgKOH / g or less, The polyepoxide (b1) has an epoxy equivalent of 100 g / eq or more and 1,500 g / eq or less, In the amino group-containing acrylic resin (a1), there is no reactive group capable of reacting with a silanol group, or the number of the reactive groups is less than 11% of the number of amino groups in the amino group-containing acrylic resin (a1); In the polyepoxide (b1), the reactive groups capable of reacting with silanol groups are absent or the number of the reactive groups is less than 10% of the number of epoxy groups in the polyepoxide (b1); The siloxane oligomer (a2) is represented by the following general formula (x): [ka] (In the formula, R 3 represents independently in each structural unit a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a single bond, R 4 represents independently in each structural unit an alkyl group having 1 to 5 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aralkyl group having 7 to 15 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or -O-; m is an integer from 0 to 200. and a structural unit X represented by the following general formula (y): [ka] (In the formula, R 5 and R 6 each independently in each repeating unit represents an alkyl group having 1 to 5 carbon atoms, an aryl group having 6 to 10 carbon atoms, or an aralkyl group having 7 to 15 carbon atoms; n is an integer from 0 to 200. A structural unit Y represented by has, as an end group, at least one selected from the group consisting of a hydrogen atom, a hydroxyl group, an alkyl group having 1 to 5 carbon atoms, and an alkoxy group having 1 to 5 carbon atoms; m+n is an integer from 2 to 200, A resin composition for paint, which satisfies n / (m+n)≧0.19, A coating film formed from the coating resin composition is subjected to an outdoor exposure test in Miyakojima for one and a half years in accordance with JIS K5600-7-6, with the coating film facing the equatorial plane at an angle of 20° to the horizontal plane, and after that, the gloss retention rate in accordance with JIS K5659 7.21 is 80% or more. [2] The resin composition for paint according to the above [1], wherein the reactive group is at least one selected from the group consisting of a hydroxyl group, an alkoxy group, an alkoxysilyl group and a silanol group. [3] The coating resin composition according to the above [1] or [2], wherein the mass ratio of the siloxane oligomer (a2) to the total solid content of the amino group-containing acrylic resin (a1), the siloxane oligomer (a2) and the polyepoxide (b1) is 10 mass % or more and 90 mass % or less. [4] A paint comprising the paint resin composition according to any one of [1] to [3] above. [5] In addition, the paint mentioned above in [4] contains a Class 3 organic solvent as specified in the Industrial Safety and Health Act. [Industrial Applicability]

[0147] The coating material according to the present invention provides a coating film that is excellent in impact resistance and suppresses the occurrence of cracks in outdoor environments. The coating material according to the present invention is suitable for coating of objects that are used or installed mainly outdoors.

Claims

1. Contains a base agent (A) and a curing agent (B), The base material (A) contains an amino group-containing acrylic resin (a1) and a siloxane oligomer (a2), The curing agent (B) contains a polyepoxide (b1) and a curing catalyst (b2), The amino group-containing acrylic resin (a1) has an amine value of 10 mgKOH / g or more and 88 mgKOH / g or less, The polyepoxide (b1) has an epoxy equivalent of 100 g / eq or more and 1,500 g / eq or less, in the amino group-containing acrylic resin (a1), at least one first reactive group selected from the group consisting of a hydroxyl group, an alkoxy group, an alkoxysilyl group, and a silanol group is not present, or the number of the first reactive groups is less than 11% of the number of amino groups in the amino group-containing acrylic resin (a1); In the polyepoxide (b1), the first reactive group is absent or the number of the first reactive groups is less than 10% of the number of epoxy groups in the polyepoxide (b1). The siloxane oligomer (a2) is represented by the following general formula (x): 【Chemistry 1】 (In the formula, R 3 represents independently in each structural unit a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a single bond, R 4 represents independently in each structural unit an alkyl group having 1 to 5 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aralkyl group having 7 to 15 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or -O-; m is an integer from 0 to 200. and a structural unit X represented by the following general formula (y): 【Chemistry 2】 (In the formula, R 5 and R 6 each independently in each repeating unit represents an alkyl group having 1 to 5 carbon atoms, an aryl group having 6 to 10 carbon atoms, or an aralkyl group having 7 to 15 carbon atoms; n is an integer from 0 to 200. A structural unit Y represented by the formula: has, as an end group, at least one selected from the group consisting of a hydrogen atom, a hydroxyl group, an alkyl group having 1 to 5 carbon atoms, and an alkoxy group having 1 to 5 carbon atoms; m+n is 2 to 200; A coating resin composition (excluding the case where the coating resin composition contains a reaction product of a hydrolyzable silyl group-containing silicone resin and a hydroxyl group-containing ultraviolet absorber and / or a hydroxyl group-containing light stabilizer), which satisfies n / (m+n)≧0.19, does not contain a third compound containing both the first reactive group and at least one third reactive group selected from an epoxy group and a halogen group in one molecule, or contains the third compound in an amount of 1 mass % or less based on the total solid content of the amino group-containing acrylic resin (a1), the siloxane oligomer (a2), and the polyepoxide (b1); A coating film formed from the coating resin composition is subjected to an outdoor exposure test in Miyakojima for one and a half years in accordance with JIS K5600-7-6, with the coating film facing the equatorial plane at an angle of 20° to the horizontal plane, and the gloss retention rate in accordance with JIS K5659 7.21 after the test is 80% or more.

2. 2. The coating resin composition according to claim 1, wherein the mass ratio of the siloxane oligomer (a2) to the total solid content of the amino group-containing acrylic resin (a1), the siloxane oligomer (a2), and the polyepoxide (b1) is 10 mass % or more and 90 mass % or less.

3. A paint comprising the paint resin composition according to claim 1 or 2.

4. The paint according to claim 3, further comprising a third type organic solvent as specified in the Industrial Safety and Health Law.

5. A coating film formed from the paint resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Formation of coating film

    JP1996120215A

  • Curable liquid resin composition

    JP1996333440A

  • Curable resin composition for water-based coating

    JP1997194762A

  • Cold cure non-aqueous dispersion type resin composition

    JP1999131009A

  • Ordinary temperature curable weather resistant coating composition

    JP2016141711A