Highly plastic hot-formed steels and hot-formed processes for automobiles with oxidation resistance
A high plasticity hot-formed steel with a tailored chemical composition and process introduces ferrite and retained austenite, addressing production challenges by enhancing strength and anti-oxidation, thus improving mechanical properties and reducing costs without protective atmospheres or shot peening.
Patent Information
- Application Number
- JP2023519094
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-11-19
- Filing Date
- 2021-11-25
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2041-11-25
AI Technical Summary
Existing hot-formed steels for automobiles face challenges with high production costs, complex processes, and the need for protective atmospheres and shot peening treatments due to issues like decarbonization and oxidation, limiting their strength and plasticity, especially for ultra-high-strength applications.
A high plasticity hot-formed steel with a specific chemical composition (C: 0.18% to 0.28%, Si: 0.20% or less, Mn: 1.20% to 2.0%, P: 0.030% to 0.080%, S: 0.004% or less, Als: 0.02% to 0.06%, Nb: 0.02% to 0.06%, Ti: 0.025% to 0.045%, V: 0.05% to 0.15%, Cr: 0.5% to 2.50%, Mo: 0.10% to 0.30%, B: 0.0015% to 0.0035%, N: 0.005% or less) and a hot forming process that includes heating, air cooling, and deformation to introduce ferrite and retained austenite, allowing for improved plasticity and anti-oxidation without protective atmospheres or shot peening.
The steel achieves tensile strengths of 1400 MPa to 1700 MPa, elongation of 18% or more, and anti-oxidation rates of 0.1g/(m²·h) or less, reducing production costs and simplifying the process by eliminating the need for protective atmospheres and shot peening, while maintaining high mechanical properties.
Smart Images

Figure 0007576167000001 
Figure 0007576167000002 
Figure 0007576167000003
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of automotive steels, in particular to oxidation-resistant, highly plastic hot-formed automotive steels and hot-forming processes. [Background technology]
[0002] In recent years, new materials for car bodies have been continuously developed and applied to car bodies, but ultra-high strength steel sheets for cold press processing exceeding 1000 MPa are usually used to manufacture parts with simple shapes due to problems such as being prone to cracking and having a large rebound. In contrast, hot-formed steel is formed in the austest region by the hot forming process, so it has a small rebound amount and can meet the requirements for assembly precision, and ultra-high strength parts with a strength of 1500 MPa or more can be obtained by quenching under pressure, which effectively simplifies the design of car body structures and parts and significantly reduces the weight of vehicles.
[0003] At present, hot-formed steels on the market are divided into painted hot-formed steels and unpainted hot-formed steels according to their surface state, among which, unpainted steels have mill scales formed on the steel surface during heating in a heating furnace, which easily causes decarbonization and affects the performance of the steel, so it is necessary to use a protective atmosphere during heating and to perform shot peening after hot forming, which increases the cost and process. On the other hand, painted steels are steel sheets coated with aluminum silicon or zinc, which can effectively prevent the decarbonization and oxidation of the steel surface during heating and can omit the shot peening after hot forming, but the cost of painted hot-formed steels is higher than that of unpainted steels. At present, hot-formed steel mass-produced and used by conventional technology has a strength level of 1500 MPa, but its elongation rate after hot forming is only 6-9%, which does not meet the development demand of the automobile field. There is still no good technology that can realize low-cost hot forming of steel, solve the problems of surface oxidation and decarbonization, avoid shot peening treatment, and at the same time ensure that the steel after hot forming has good plasticity.
[0004] Patent Document 1 discloses a method for producing ultra-high strength hot-formed steel for automobiles, the composition of which is, in mass%, C: 0.5%-0.6%, Mn: 0.5%-2.0%, Si: 1.5%-2.5%, Cr: 1.0%-3.0%, Al: 1.0%-2.0%, Nb: 0.01%-0.03%, B: 0.001%-0.005%, and the steel sheet after hot forming has a strength of 1500-2000 MPa and an elongation rate of 10%-20%. The steel sheet disclosed in Patent Document 1 has good strength and plasticity matching, but its composition contains high contents of Cr and Al elements, which increases the cost and difficulty of smelting. In addition, the production process is complicated, the existing production equipment cannot meet the production requirements, and protective atmosphere and shot peening treatment are also required during production.
[0005] Patent Document 2 discloses a hot-formed steel sheet with high strength and high toughness for automobiles and a manufacturing method thereof, in which the chemical components of the steel sheet are, in mass%, C: 0.1-0.5%, Si: 0.5-1.5%, Mn: 1.2%-2.4%, Ti: 0.01%-0.05%, B: 0.001%-0.005%, S: 0.01% or less, and P: 0.01% or less, and the steel sheet after hot forming has a tensile strength of 1600 MPa and an elongation rate of 16%, with good overall performance and low alloy cost. However, in order to obtain the final structure and mechanical properties, the steel sheet needs to be deformed in a heating process and quenched twice, and the hot forming process is complicated and cannot be realized with existing equipment, and a protective atmosphere during heating and a shot peening treatment after hot forming are also required.
[0006] Based on the above, the development of highly plastic hot-formed steel with excellent oxidation resistance and hot-forming process for automobiles is expected to be applied. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Chinese Patent No. 107354385 [Patent Document 2] Chinese Patent No. 103255340 Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in view of the above technical problems, and provides a hot forming process and a highly plastic hot forming steel for automobiles having oxidation resistance. [Means for solving the problem]
[0009] The technical means of the present invention are as follows: The highly plastic hot-formed steel for automobiles having oxidation resistance of the present invention has chemical components, in mass %, of the hot-formed steel: C: 0.18% to 0.28%, Si: 0.20% or less, Mn: 1.20% to 2.0%, P: 0.030% to 0.080%, S: 0.004% or less, Als: 0.02% to 0.06%, Nb: 0.02% to 0.06%, Ti: 0.025% to 0.045%, V: 0.05% to 0.15%, Cr: 0.5% to 2.50%, Mo: 0.10% to 0.30%, B: 0.0015% to 0.0035%, N: 0.005% or less, with the balance being Fe and unavoidable impurities.
[0010] The structure of hot-formed steel consists of ferrite, martensite and retained austenite.
[0011] The volume fraction of ferrite is 5% to 12%, the volume fraction of martensite is 78% to 89%, and the volume fraction of retained austenite is 6% to 10%.
[0012] Hot-formed steel has a tensile strength of 1400MPa to 1700MPa and an oxidation resistance rate of 0.1g / (m 2 ·h) or less, the yield strength is 900MPa to 1450MPa, the elongation is 18.0% or more, the surface of the steel is not completely decarburized, the thickness of the decarburized layer is 15μm or less, and the thickness of the hot-formed steel plate is 0.8mm to 12.0mm.
[0013] The components of the hot forming steel according to the present invention have the following effects: C: C is advantageous in ensuring the strength of steel and improving the hardenability of steel. If the carbon content is too low, the strength of the steel after hot stamping will not reach the desired target, while if the carbon content is too high, the strength of the hot-formed steel will be too high and the plasticity will decrease. In addition, increasing the C content can lower the phase transition temperature of the steel and lower the austenitizing temperature, which is advantageous in obtaining a surface that does not require shot peening, and the increase in the C content allows the steel to generate a sufficient amount of supercooled austenite during the heating pressure holding process, thereby improving the plasticity. Therefore, the optimal range of C in the present invention is 0.18% to 0.28%.
[0014] Si: Si is an element that does not precipitate carbides in steel, and it has the effect of suppressing the precipitation of carbides during the cooling and pressure holding process of hot forming, and ensuring the amount and stability of retained austenite. However, if the Si content is too high, defects such as a large amount of mill scale and color difference will occur on the surface of the hot formed substrate, which will affect the surface quality of the hot formed parts, and if the Si element is too high, the two-phase region will expand, the austenitization temperature will increase, and the steel will be kept at a high temperature, which will make the steel surface easily deteriorate. Therefore, the Si content in the steel of the present invention is set to 0.20% or less.
[0015] Mn: The main role of Mn in the present invention is to improve the hardenability of steel, lower the phase transition temperature, and realize austenitization at a lower temperature. If the Mn content is too high, it deteriorates the uniformity of the steel structure, and serious band-like structural defects tend to occur in the structure. Therefore, in the present invention, the Mn content is selected to be 1.20% to 2.0%.
[0016] P: The role of P in the present invention is similar to that of Si, and it can suppress the formation of cementite and improve the stability of retained austenite. In addition, P refines and uniformly distributes lath martensite slabs, improving toughness. The content of P in the present invention is 0.030% to 0.080%.
[0017] S: In the present invention, S is a harmful element that forms MnS impurities and deteriorates the microstructure and mechanical properties of the steel sheet. Therefore, in the present invention, S is limited to 0.004% or less.
[0018] Als: Als (acid-soluble aluminum) plays a role in deoxidizing and fixing nitrogen in the smelting process, but if there is too much Als, the amount of aluminum-based impurities increases. Therefore, in the present invention, the range of Als is 0.020% to 0.060%.
[0019] Cr: Cr is an element that improves the hardenability of steel. In the present invention, the main role of Cr element is to improve the high temperature oxidation resistance of steel, improve the tempering stability of steel, and ensure that tempered martensite does not occur in the steel within the holding temperature range. The optimum Cr content is 0.50%~2.50%.
[0020] Mo: Mo is a medium-strength carbide forming element, which improves the strength and toughness of steel. In the present invention, Mo can lower the martensite transition temperature and significantly improve the stability of retained austenite, and at the same time, the addition of Mo element improves the oxidation resistance of steel. In the present invention, the content of Mo is 0.10%-0.30%.
[0021] Nb, V: Nb and V mainly play a role in fine grain strengthening and precipitation strengthening of steel. In the present invention, both of them are dispersed and precipitated as nano-scale fine carbides, thereby effectively pinning the original austenite grain boundaries, further refining the structure of each phase of the hot-formed steel sheet, and improving the overall performance. At the same time, the dispersed and precipitated carbides function as hydrogen traps, pinning diffusible hydrogen in the steel, and improving the delayed fracture resistance. In addition, the precipitation of VN formed from V and N can suppress the precipitation of BN and prevent the decrease in strength due to the precipitation of B. In the present invention, the content of Nb is 0.020% to 0.060%, and the content of V is 0.050% to 0.15%.
[0022] Ti: Ti is mainly used in boron steel to fix nitrogen, ensuring the hardening effect of boron. In addition, Ti is precipitated as fine carbides with C element, reducing the hardness and strength of martensite in the structure after hot forming, which is advantageous for improving the plasticity and toughness of steel. In the present invention, the Ti content is 0.025% to 0.045%.
[0023] B: Adding boron to steel can significantly improve the hardenability of the steel and ensure the stability of the strength of the steel after hardening. If the B content is too low, the effect is not significant, and if the B content is too high, it is easy to form a compound of B together with N in the steel, which reduces the performance of the steel sheet. Therefore, in the present invention, the B content is 0.0015% to 0.0035%.
[0024] N: The lower the N content, the better, but if it is too low, production becomes difficult and costs increase. Therefore, in the present invention, the N content is 0.005% or less.
[0025] In the present invention, by adding alloy elements such as C, Mn, Cr, and Mo, the austenitizing temperature is lowered, the hardenability of the steel is improved, the oxidation of the steel is inhibited, and the critical cooling rate of the hot forming of the steel is decreased, so that hot forming steel of a thickness standard can be manufactured. In addition, by combining the chemical composition and the hot forming process, a certain amount of ferrite is obtained in the air cooling stage, and a certain amount of stable retained austenite is obtained in the pressure holding stage after cooling, so that the plasticity of the steel is improved. By adding the elements Si and P to the composition, the precipitation of carbides is inhibited, the content of the retained austenite in the steel is ensured, and the mechanical properties of the steel are improved. In addition, since the elements Cr and Mo in the composition of the steel have an antioxidant effect, the steel can be heated and kept warm under non-protective atmosphere conditions, and the subsequent processes can be directly carried out after hot forming without shot peening.
[0026] The present invention further provides a hot forming process for hot forming high plasticity automotive steel with oxidation resistance, comprising the steps of: Step (1): A hot-formed substrate containing the above components is C3 -A C Heat in a heating oven at 3+15℃ and keep warm for 180s-300s. Step (2): The heated hot-formed substrate is removed from the heating furnace and r3 After air-cooling to temperature, after 5s to 8s, it is placed in a hot forming mold to be deformed, cooled to 180℃ to 250℃ at a cooling rate of 18℃ / s or more, and then held at pressure for 40s to 80s. After that, the formed part is taken out and air-cooled to room temperature to obtain hot-formed steel.
[0027] The steel according to the present invention does not require a protective atmosphere during hot forming, does not require shot peening treatment after hot forming, and subsequent processes can be carried out directly, so the overall process cost is lower than that of conventional hot formed products.
[0028] The hot-formed substrate is obtained through smelting, hot rolling and cold rolling. The composition and mass% of the smelting are the composition and mass% of the hot-formed high-plasticity steel for automobiles having the above-mentioned oxidation resistance. Effect of the Invention
[0029] Compared with the prior art, the present invention has the following advantages: (1) By combining chemical components and hot forming processes to introduce a certain amount of ferrite and retained austenite into the conventional fully martensite structure, the plasticity of the steel can be improved, and an elongation rate of 18% or more can be achieved while ensuring a tensile strength of 1,400 MPa or more. (2) The addition of Cr and other elements improves the oxidation resistance of steel at high temperatures, and the oxidation resistance rate of steel is 0.1 g / (m 2 h), and the oxidation resistance level reaches level 1. Therefore, no protective atmosphere is required during hot forming of the steel, and no shot peening treatment is required after hot forming, and the subsequent processes can be carried out directly. (3) The manufacturing of the provided hot-formed steel and the hot-forming process can be carried out using existing equipment, eliminating the need for equipment modification and enabling low-cost implementation. For the above reasons, the present invention can be widely used in fields such as automotive steel. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] In the absence of conflict, the embodiments of the present invention and the features of the embodiments can be combined with each other. The described embodiments are only some of the embodiments of the present invention, and not all of the embodiments. The following description of at least one exemplary embodiment is illustrative in nature and does not limit the present invention and its application or use. All other embodiments obtained based on the embodiments of the present invention without the creative labor of those skilled in the art should be included in the scope of the claims of the present invention.
[0031] The present invention provides a hot-formed steel having high plasticity and oxidation resistance for automobiles, and the chemical components of the hot-formed steel are, in mass%, C: 0.18% to 0.28%, Si: 0.20% or less, Mn: 1.20% to 2.0%, P: 0.030% to 0.080%, S: 0.004% or less, Als: 0.02% to 0.06%, Nb: 0.02% to 0.06%, Ti: 0.025% to 0.045%, V: 0.05% to 0.15%, Cr: 0.5% to 2.50%, Mo: 0.10% to 0.30%, B: 0.0015% to 0.0035%, N: 0.005% or less, and the balance being Fe and unavoidable impurities.
[0032] The structure of hot-formed steel consists of ferrite, martensite and retained austenite.
[0033] The volume fraction of ferrite is 5% to 12%, the volume fraction of martensite is 78% to 89%, and the volume fraction of retained austenite is 6% to 10%.
[0034] Hot-formed steel has a tensile strength of 1400MPa to 1700MPa and an oxidation resistance rate of 0.1g / (m 2·h) or less, the yield strength is 900MPa to 1450MPa, the elongation is 18.0% or more, the surface of the steel is not completely decarburized, the thickness of the decarburized layer is 15μm or less, and the thickness of the hot-formed steel is 0.8mm to 12.0mm.
[0035] The hot-formed steel with high strength and excellent oxidation resistance according to the present embodiment is smelted, hot-rolled and cold-rolled to obtain a hot-formed plate having a thickness of 0.8 mm to 12.0 mm, and then a hot-forming process is carried out, which specifically includes the following steps:
[0036] Step (1): Place the hot-formed substrate in A C3 -A C3 Heat in a furnace at +15℃ and keep at this temperature for 180s-300s. The purpose is to make the hot-formed substrate completely austenitized and have the original small size of austenite grains. The low austenitizing temperature can also reduce the oxidation of the surface of the hot-formed substrate.
[0037] Step (2): The heated hot-formed substrate is removed from the heating furnace and r3 After air-cooling to temperature, after 5s to 8s, it is placed in a hot forming mold to be deformed, cooled to 180℃ to 250℃ at a cooling rate of 18℃ / s or more, and then held at pressure for 40s to 80s. After that, the formed part is taken out and air-cooled to room temperature to obtain hot-formed steel.
[0038] The components, hot forming process parameters, and the structure and properties of the steel sheets after hot forming in the examples of the present invention are shown in Tables 1 to 3.
[0039] [Table 1]
[0040] [Table 2]
[0041] [Table 3]
[0042] In this embodiment, by combining chemical components and a hot forming process, a certain amount of ferrite and retained austenite are introduced into the conventional fully martensite structure to improve the plasticity of the steel, and the elongation rate can be 18% or more under the condition that the tensile strength can be secured at 1400 MPa or more. The addition of elements such as Cr and Mo improves the oxidation resistance of the steel, and the oxidation resistance rate of the steel is 0.1 g / (m 2 h), the level of oxidation resistance reaches level 1, the steel does not need a protective atmosphere during hot forming, does not need shot peening treatment after hot forming, and subsequent processes can be carried out directly. The cost of the provided hot formed steel and the whole process of the hot forming process is lower than the production cost of traditional hot formed parts, and can be realized with existing equipment without equipment modification.
[0043] Finally, the following should be mentioned: the above embodiments are only for explaining the technical means of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the above embodiments, it is also possible to modify the technical means described in the above embodiments, or to carry out equivalent replacements for part or all of the technical features, and it is understood by those skilled in the art that such modifications and replacements do not depart from the essence of the corresponding technical means of the embodiments of the present invention.
[0044] (Additional Note) (Appendix 1) A hot-formed steel having high plasticity and oxidation resistance for automobiles, the chemical components of the hot-formed steel being, in mass%, C: 0.18% to 0.28%, Si: 0.20% or less, Mn: 1.20% to 2.0%, P: 0.030% to 0.080%, S: 0.004% or less, Als: 0.02% to 0.06%, Nb: 0.02% to 0.06%, Ti: 0.025% to 0.045%, V: 0.05% to 0.15%, Cr: 0.5% to 2.50%, Mo: 0.10% to 0.30%, B: 0.0015% to 0.0035%, N: 0.005% or less, the balance being Fe and unavoidable impurities. A hot-formed, highly plastic, oxidation-resistant steel for automobiles.
[0045] (Appendix 2) The structure of the hot-formed steel is composed of ferrite, martensite and retained austenite. 2. A hot-formed, highly plastic, oxidation-resistant steel for automobiles according to claim 1.
[0046] (Appendix 3) The ferrite has a volume fraction of 5% to 12%, the martensite has a volume fraction of 78% to 89%, and the retained austenite has a volume fraction of 6% to 10%. 3. A hot-formed, highly plastic, oxidation-resistant steel for automobiles according to claim 2.
[0047] (Appendix 4) The tensile strength of the hot-formed steel is 1400 MPa to 1700 MPa. 2. A hot-formed, highly plastic, oxidation-resistant steel for automobiles according to claim 1.
[0048] (Appendix 5) The oxidation resistance rate of the hot-formed steel is 0.1 g / (m 2 h) is less than or equal to 2. A hot-formed, highly plastic, oxidation-resistant steel for automobiles according to claim 1.
[0049] (Appendix 6) The yield strength of the hot-formed steel is 900 MPa to 1450 MPa. 2. A hot-formed, highly plastic, oxidation-resistant steel for automobiles according to claim 1.
[0050] (Appendix 7) The elongation ratio of the hot-formed steel is 18.0% or more; 2. A hot-formed, highly plastic, oxidation-resistant steel for automobiles according to claim 1.
[0051] (Appendix 8) The surface of the hot-formed steel is not completely decarburized, and the thickness of the decarburized layer is 15 μm or less; 2. A hot-formed, highly plastic, oxidation-resistant steel for automobiles according to claim 1.
[0052] (Appendix 9) The thickness of the hot-formed steel is 0.8 mm to 12.0 mm; 2. A hot-formed, highly plastic, oxidation-resistant steel for automobiles according to claim 1.
[0053] (Appendix 10) A hot-formed substrate comprising the chemical composition according to any one of claims 1 to 9. C3 -A C3 Heat in a +15℃ oven and keep warm for 180s-300s; The heated hot-formed substrate is removed from the heating furnace and r3 After cooling to room temperature, the hot-formed steel is deformed after 5 s to 8 s, and then cooled to 180 ° C to 250 ° C at a cooling rate of 18 ° C / s or more, and then held for 40 s to 80 s. Then, the formed part is removed and cooled to room temperature to obtain the hot-formed steel. 1. A hot forming process for hot forming high plasticity automotive steel with oxidation resistance, characterized in that
Claims
1. A hot-formed steel having high plasticity and oxidation resistance for automobiles, the chemical components of the hot-formed steel being, in mass%, C: 0.18% to 0.28%, Si: 0.20% or less, Mn: 1.20% to 2.0%, P: 0.030% to 0.080%, S: 0.004% or less, Als: 0.02% to 0.06%, Nb: 0.02% to 0.06%, Ti: 0.025% to 0.045%, V: 0.05% to 0.15%, Cr: 0.5% to 2.50%, Mo: 0.10% to 0.30%, B: 0.0015% to 0.0035%, N: 0.005% or less, the balance being Fe and unavoidable impurities; The structure of the hot-formed steel is composed of ferrite, martensite and retained austenite, The ferrite has a volume fraction of 5% to 12%, the martensite has a volume fraction of 78% to 89%, and the retained austenite has a volume fraction of 6% to 10%. A hot-formed, highly plastic, oxidation-resistant steel for automobiles.
2. The tensile strength of the hot-formed steel is 1400 MPa to 1700 MPa; 2. Highly plastic hot forming steel for automobiles with oxidation resistance according to claim 1.
3. The oxidation resistance rate of the hot-formed steel is 0.1 g / (m 2 h) is equal to or less than 2. Highly plastic hot forming steel for automobiles with oxidation resistance according to claim 1.
4. The yield strength of the hot formed steel is 900 MPa to 1450 MPa; 2. Highly plastic hot forming steel for automobiles with oxidation resistance according to claim 1.
5. The elongation rate of the hot-formed steel is 18.0% or more; 2. Highly plastic hot forming steel for automobiles with oxidation resistance according to claim 1.
6. The surface of the hot-formed steel is not completely decarburized, and the thickness of the decarburized layer is 15 μm or less.
2. Highly plastic hot forming steel for automobiles with oxidation resistance according to claim 1.
7. The thickness of the hot-formed steel is 0.8 mm to 12.0 mm; 2. Highly plastic hot forming steel for automobiles with oxidation resistance according to claim 1.
8. A hot-formed substrate containing the chemical component according to any one of claims 1 to 7 is C3 -A C3 Heating in a heating oven at +15°C and keeping the temperature for 180s-300s; The heated hot-formed substrate is removed from the heating furnace and r3 After air-cooling to a temperature of 180°C to 250°C for 5s to 8s, the hot-formed steel is deformed in a hot-formed mold, cooled to 180°C to 250°C at a cooling rate of 18°C / s or more, and then held for 40s to 80s. The formed part is then removed and air-cooled to room temperature to obtain the hot-formed steel.
1. A hot forming process for hot forming high plasticity automotive steel with oxidation resistance, characterized in that
Citation Information
Patent Citations
Vehicle high strength and toughness hot-forming steel plate and preparation method thereof
CN103255340A
Hot-stamping forming process of 22MnB5 high-strength thin steel plate
CN104384283A
Hot forming steel directly rolled through medium and thin slab and having tensile strength larger than or equal to 1500 MPa and production method
CN106119692A
Preparation method for ultrahigh-strength thermoforming steel for car
CN107354385A
1600MPa-grade high strength and high plasticity hot stamping steel and preparation method thereof
CN110029274A